Alloy steel
The vanadium alloy steel with coherent phase interfacial precipitates addresses the need for improved fire and structural resistance, enhancing elastic modulus and structural integrity for construction and automotive applications.
Patent Information
- Application Number
- JP2024521241
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2021-10-06
- Publication Date
- 2024-10-23
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The challenge lies in developing steel materials with improved fire resistance, buckling resistance, and deflection resistance to meet the demands of the construction and automotive industries while aligning with decarbonization goals, as existing technologies often fail to balance these requirements effectively.
A vanadium alloy steel is developed with specific carbon and vanadium compositions, featuring coherent phase interfacial precipitates that enhance the elastic modulus, providing improved buckling and deflection resistance, and includes additional elements like nitrogen, molybdenum, copper, silicon, chromium, and manganese to optimize microstructure and properties.
The vanadium alloy steel exhibits enhanced elastic modulus, particularly at high temperatures, leading to improved structural integrity and resistance to buckling and deflection, enabling the construction of taller structures and lighter automotive components.
Smart Images

Figure 2024538742000001_ABST
Abstract
Description
[Technical field]
[0001] The present disclosure relates to steel alloys and methods of making the same, and more particularly to vanadium steel alloys having improved elastic modulus. [Background technology]
[0002] Given the trend towards decarbonisation towards the use of stronger and lighter structural steels, there is a need to develop steels with improved properties such as fire resistance, buckling resistance and flexure resistance.
[0003] The development and use of fire-resistant structural steels in civil engineering is of particular concern in the construction industry, and there is a strong trend in the steel industry to reduce the use of solid carbon.
[0004] The development of lean-alloy high-strength steels with superior fire resistance would provide significant economic benefits, enable the use of thinner column and beam designs, and accelerate progress towards global decarbonization targets. However, fire performance requirements and decarbonization goals are often incompatible.
[0005] Furthermore, providing steel with enhanced resistance to buckling and bending would be beneficial in both the automotive industry and in the construction of wind power towers, for example. Summary of the Invention [Problem to be solved by the invention]
[0006] It is an object of the present disclosure to address or at least alleviate problems associated with the prior art. [Means for solving the problem]
[0007] In a first aspect, there is provided a vanadium alloy steel comprising, preferably consisting essentially of, and more preferably consisting of carbon and vanadium, carbon and vanadium, wherein the microstructure of the steel comprises coherent interphase precipitates comprising vanadium.
[0008] In some embodiments, there is provided a vanadium alloy steel comprising, preferably consisting essentially of, more preferably consisting of, carbon, vanadium, and balance iron, wherein the microstructure of the steel comprises coherent phase interfacial precipitates comprising vanadium.
[0009] In some embodiments, the vanadium alloy steel comprises: Carbon in the range of about 0.06% by weight to about 1.1% by weight; Vanadium in the range of about 0.1% to about 1.5% by weight; comprising, preferably consisting essentially of, more preferably consisting of, The microstructure of the steel contains coherent interphase precipitates containing vanadium.
[0010] In some embodiments, the vanadium alloy steel comprises: Carbon in the range of about 0.06% by weight to about 1.1% by weight; Vanadium in the range of about 0.1% to about 1.5% by weight; The remaining iron comprising, preferably consisting essentially of, more preferably consisting of, The microstructure of the steel contains coherent interphase precipitates containing vanadium.
[0011] In some embodiments, the vanadium alloy steel comprises, preferably consists essentially of, and more preferably consists of vanadium and carbon, optionally one or more of nitrogen, molybdenum, copper, silicon, chromium, and / or manganese, with the balance iron, and the microstructure of the steel comprises coherent phase interfacial precipitates comprising vanadium.
[0012] In some embodiments, the vanadium alloy steel comprises: Carbon in the range of about 0.06% by weight to about 1.1% by weight; Vanadium in the range of about 0.1% to about 1.5% by weight; Optionally, about 0.015% by weight or less of nitrogen; about 1.6% by weight or less of molybdenum; about 1% by weight or less of copper; about 1.2% by weight or less silicon; about 0.3% by weight or less of chromium, and / or Approximately 1.6% by weight or less of manganese and one or more of The remaining iron comprising, preferably consisting essentially of, more preferably consisting of, The microstructure of the steel contains coherent interphase precipitates containing vanadium.
[0013] As explained below, the steels disclosed herein improve the average elastic modulus (i.e., Young's modulus) of the steel. It is believed that the coherent vanadium precipitates create large strain fields in the steel, which can result in a change in the lattice parameter and thus a change in the bulk modulus of the steel.
[0014] It is believed that the increased elastic modulus is applicable at higher temperatures due to the increased stability of the coherent precipitates against tempering and coarsening, thereby improving the buckling resistance of the steel. In this manner, improved fire performance is achieved, for example, using the lower alloyed embodiments.
[0015] Providing higher modulus steels as disclosed herein may also be beneficial in providing enhanced structural benefits, such as higher buckling resistance, for example using more highly alloyed embodiments, which may allow for the construction of taller wind turbines.
[0016] Providing higher modulus steels as disclosed herein, for example using more highly alloyed embodiments, can also be beneficial in providing enhanced resistance to flexure, which can be beneficial in creating lighter and stiffer automotive structures.
[0017] As shown in Figure 1, the lattice parameter change effect is believed to be a direct result of matrix expansion and contraction caused by elastic accommodation of precipitates in the surrounding steel matrix. The vanadium-containing precipitates 2 have a different lattice parameter than the surrounding steel (e.g., ferritic) matrix 4. In other words, there is a lattice parameter misfit between the vanadium-containing precipitates and the surrounding steel, which results in the generation of a large strain field (indicated by the shaded area denoted by reference number 6 in Figure 1) when vanadium-containing coherent precipitates form. This results in a change in the average lattice parameter of the entire steel, which in turn changes the bulk modulus of the steel. In contrast, no such strain field is observed when incoherent precipitates form.
[0018] This change in lattice parameter is thought to be anisotropic, but as would be expected in a polycrystalline material such as steel, random crystal orientation can counteract this anisotropy, facilitating an enhancement of the macroscale elastic modulus.
[0019] Combined with this physical effect, the electron distribution near the coherent interface is altered, further contributing to the enhancement of the bulk modulus.
[0020] Figure 2 illustrates the uniqueness of vanadium in that the misfit between the lattice parameters of vanadium-containing precipitates is relatively small, as compared to, for example, ferrite and austenite. Data points for the ferrite misfit are shown as filled circles and triangles, and data points for the austenite misfit are shown as open circles and triangles. Additionally, Figure 2 illustrates the high limit size of vanadium-containing coherent precipitates (in this case in ferrite) compared to precipitates containing other elements commonly used in steels. This is believed to encourage the creation of coherent precipitate formation, with the effect that a larger coherence limit makes it easier to maintain coherence by established steelmaking methods.
[0021] Looking at Figure 3, this shows the relationship between strengthening effect and precipitate size. As can be seen, the shear strength increases with increasing grain size up to a critical grain size. This is due to coherent strain hardening as discussed above. Once the grain size exceeds the critical grain size, incoherent precipitates form and the modulus strengthening effect disappears.
[0022] Vanadium containing precipitates are believed to be very efficient in increasing the elastic modulus of steel by virtue of their high coherence limit and high shear modulus compared to other precipitates.
[0023] When precipitates are small and coherent with the surrounding matrix, the dislocation mechanism transitions from the well-established Ashby-Orowan looping mechanism (applicable to incoherent precipitates) to a grain shear mechanism. The strengthening mechanism resulting from dislocations shearing ordered coherent grains results in the action of ordering and modulus strengthening mechanisms. The resulting increase in modulus strengthening can be explained by the Knowles-Kelly equation (1):
number
[0024] This indicates that there is a direct relationship between the number density of vanadium-containing precipitates (e.g., carbides), their average size, their shear modulus (which depends on the V:C ratio of the vanadium precipitates), and the subsequent modulus strengthening.
[0025] By way of example, Figure 5a shows a simulation of a ferritic steel as disclosed herein, illustrating the elastic strain fields associated with vanadium-containing coherent interphase precipitates, which in this embodiment form as nano-sized platelets. The platelets are arranged in rows with spacing between the rows indicated at 22. For clarity, only two rows of interphase precipitates are shown.
[0026] In vanadium-containing precipitates such as vanadium carbide and / or vanadium carbonitride, large relative differences in the parallel and perpendicular components of atomic misfit occur depending on the orientation of the precipitate. Parallel to the surfaces of the platelet precipitates, very low misfit exists, which leads to a large coherence critical size limit and dilation effects. Perpendicular to the precipitates, relatively large misfit and low coherence size limits are observed, which results in a contraction effect on the lattice spacing perpendicular to the broad platelet surfaces of the precipitates. This contraction reduces the average lattice spacing, i.e., the Burgers vector, resulting in an increase in the elastic modulus of the unit cell, which, when applied to multiple grains at the macroscale, leads to a significant increase in the Young's modulus at the macrolevel.
[0027] The change in lattice parameters is shown along line AA, which indicates a reduction in the average lattice spacing and a change in bulk modulus as a result of the anisotropic misfit strain.
[0028] In some embodiments, the steel is a fire-resistant steel. Such improved modulus can also be applied at high temperatures due to the increased stability of the coherent precipitates against tempering and coarsening, thereby improving the buckling resistance of the fire-resistant steel.
[0029] The stability of buildings and other structures in fire depends on the extent to which steel structures soften when heated to temperatures produced by fire. Steel is generally considered to be fire-resistant if its short-term strength when heated to such temperatures is about 0.6 to 0.7 of its strength at room temperature.
[0030] In an exemplary embodiment, the average elastic modulus is greater than or equal to 120 GPa at a temperature in the range of about 600°C to about 700°C.
[0031] In some embodiments, the steel comprises vanadium in the range of about 0.1 to about 0.3 (wt%), for example, the steel is a ferritic steel (eg, a refractory alloy HSLA (high strength low alloy)).
[0032] In some embodiments, the steel comprises vanadium in the range of about 0.3 to about 1.5 wt %, for example, the steel is a ferritic steel (eg, AHSS (advanced high strength steel)).
[0033] In some embodiments, the steel comprises vanadium in the range of about 0.1 to about 1.5 (wt%), for example, the steel is a ferritic steel (eg, a hydrogen resistant steel).
[0034] In some embodiments, the steel comprises vanadium in the range of about 0.1 to about 1 (wt%), for example, the steel is pearlitic steel.
[0035] The use of vanadium to form interphase precipitates is believed to be advantageous compared to other alloying elements such as niobium and titanium because vanadium has a relatively low effect on the transformation temperature (i.e., the temperature at which the steel transforms from austenite to ferrite). Lowering the transformation temperature has the detrimental effect of increasing the probability of random precipitation rather than interphase precipitation. Thus, the use of vanadium is beneficial in maintaining the transformation temperature in the desired range.
[0036] The presence of carbon contributes to the hardness, strength and hardenability of steel. Carbon also acts as an austenite stabilizer.
[0037] In some embodiments, the steel comprises carbon in the range of about 0.06 to about 0.2 (wt%), for example, the steel is a ferritic steel (eg, a refractory alloy HSLA (high strength low alloy)).
[0038] In some embodiments, the steel comprises carbon in the range of about 0.06 to about 0.3 weight percent, for example, the steel is a ferritic steel (eg, AHSS (advanced high strength steel)).
[0039] In some embodiments, the steel comprises about 0.06 to about 0.3 weight percent carbon, for example, the steel is a ferritic steel (eg, a hydrogen resistant steel).
[0040] In some embodiments, the steel comprises carbon in the range of about 0.6 to about 1.1 (wt%), for example, the steel is pearlitic steel.
[0041] In some embodiments, the steel is a modulus-strengthened steel with an average modulus (i.e., measured bulk modulus) greater than about 210 Pa, e.g., greater than about 220 GPa, e.g., in the range of about 210 GPa to about 300 GPa, e.g., in the range of about 220 GPa to about 300 GPa.
[0042] The elastic modulus can be measured using the dynamic resonance method. Steel specimens with uniform cross-sections (e.g., circular, square, or rectangular) are prepared and the natural vibration frequency of the steel is determined and related to the elastic modulus using known equations. ASTM Standard C1259 specifies the standard test method for dynamic Young's modulus, shear modulus, and Poisson's ratio of advanced ceramics by vibration impulse excitation for rectangular and circular cross-section bars.
[0043] Optionally, the steel is a modulus enhanced AHSS steel. Optionally, the steel is a fire resistant steel (e.g., HSLA steel) with an average modulus of elasticity of about 120 GPa or greater at a temperature in the range of about 600° C. to about 700° C.
[0044] Optionally, the coherent phase interface precipitates have a grain size of about 9 nm or less, optionally in the range of about 5 nm to about 9 nm, and optionally greater than about 5 nm, as can be measured by high resolution transmission electron microscopy, x-ray diffraction, or other suitable methods.
[0045] The grain size of the coherent phase interface precipitates is taken as the average of the maximum grain dimension of a representative sample of the grains.
[0046] In the case of coherent phase interface precipitates in ferrite, lamellar samples are typically prepared using a focused ion beam (FIB) microscope. Analysis of thin lamellae is also typically performed in situ using a cold field emission gun with a probe-corrected high-resolution scanning transmission electron microscope (HRSTEM). This method allows high-angle annular dark field (HAADF) images to be acquired at appropriate collection angles. The size, morphology and number density of the coherent precipitates can be obtained from such HAADF and STEM micrographs, whereby the average number density is derived from the average values obtained from the various grains. Concentration profiles can also be obtained from such HAADF data, validating the nature of the bonded nanoparticles. Atom probe tomography can also be used to validate the atomic concentration profile within the core-shell nanoparticles (from the HAADF micrographs) and improve its 3D spatial resolution.
[0047] As shown in Figure 2 and previously discussed, this is relatively large compared to precipitates formed from other commonly used elements and is believed to contribute to an increase in the elastic modulus of the bulk steel (as shown in Figure 3).
[0048] Optionally, the coherent phase interface precipitates include vanadium carbide, and optionally the coherent phase interface precipitates have the chemical formula V x C y (e.g., coherent phase interface precipitates include V4C3, V6C5, and / or V5C3) where x>y. During the transition from coherent to incoherent grains, the precipitate-matrix interfacial energy increases so that more vacancies are required for precipitate stability, resulting in a slight gradual decrease in the carbon-to-vanadium ratio, thus improving stability.
[0049] It is also believed that a slight increase in the vanadium content in ferritic steels reduces the carbon to vanadium ratio in the precipitates, which serves to enhance the shear modulus of the precipitates, resulting in an enhanced elastic modulus.
[0050] In some embodiments, the steel is a hydrogen resistant steel, for example using high alloy embodiments. Vanadium carbides within the steel are believed to act as hydrogen traps capable of irreversibly trapping hydrogen.
[0051] By increasing the V:C ratio of the interphase precipitates, a large amount of carbon vacancies are generated at the coherent interfaces of the lattice matrix of the steel (e.g., ferrite). These vacancies act as hydrogen traps, leading to improved resistance to hydrogen embrittlement.
[0052] This is illustrated in Figures 4a and 4b. Figure 4b shows a 3D view of a hydrogen atom 8 occupying a carbon vacancy in a V4C3 coherent phase interface precipitate 2. Figure 4a shows the potential energy wells associated with a TiC precipitate 14, a NbC precipitate 12, and a V4C3 precipitate 10. As can be seen, the potential energy well associated with the V4C3 precipitate 10 is deeper than the potential energy wells of the other precipitates, and therefore acts as a more effective hydrogen trap.
[0053] Additionally, vanadium carbide precipitates containing enhanced vanadium are believed to contain carbon vacancies which are inherently more thermally stable under fire exposure conditions.
[0054] Optionally, the steel comprises a ferrite phase, and coherent phase interface precipitates are formed within the ferrite phase, for example forming nodular or knotted ferrite.
[0055] In some embodiments, coherent phase interface precipitates form when the austenite phase transforms into the ferrite phase, in other words, at conditions that correspond to a mobile phase boundary between austenite and ferrite.
[0056] Upon cooling, it is believed that spheroidal ferrite (NF) forms and changes its orientation during growth in order to accommodate the accumulated elastic strain caused by the formation of coherent phase interface precipitates. Spheroidal ferrite has been identified so far only in eutectic cast steels and is caused by the misfit of lattice parameters due to iron carbides (i.e., those in cementite). It has been found that spheroidal ferrite can also be generated by the misfit generated by coherent alloy carbides. Spheroidal ferrite is characterized by disordered crystal orientation and disordered misorientation of grain boundaries. The grains are not isomorphic but resemble a nodular appearance. The ferrite transformation with phase interface precipitation is a kind of eutectoid transformation similar to modified pearlite in high carbon steels, where alloy carbides are formed instead of iron carbides, cementite. This spheroidal or nodular ferrite can therefore be considered similar to the pearlite observed in high carbon steels.
[0057] This bifurcation of NFs, and thus the alteration of the ferrite / austenite interface for interphase precipitation, is believed to optimize the microstructural organization to enhance hydrogen embrittlement resistance. It is believed that lower angle grain boundaries and coincidence site lattices (CSLs), which indicate lower relative grain boundary energy, can significantly enhance the hydrogen embrittlement resistance of ferritic steels. One possible mechanism for this is that the number of atoms located at the CSL grain boundaries (e.g., between Σ5 and Σ13) increases, which reduces the vacancy density and can further mitigate the segregation of hydrogen atoms at the grain boundaries.
[0058] In some embodiments, the steel composition includes Mo, Cr, and / or Cu. In this manner, it is believed that the steel may benefit from core-shell nanoparticles that exhibit higher capillary-driven coarsening resistance and lattice parameter contraction. With reference to FIG. 7b, in some exemplary embodiments, the core-shell nanoparticle 16 may include a core 18 of VN. For example, the core-shell nanoparticle may include a shell 20 that includes Mo, Cr, and / or Cu.
[0059] Capillary-driven grain coarsening is hindered by the interfacial segregation of Mo, Cr, and / or Cu, which reduces the driving force for further grain coarsening due to the lowering of the interfacial energy. The anti-coarsening aids in grain refinement during austenitization and prior austenite grain size control. The developed core-shell nanoparticles are inherently resistant to coarsening and exert a Zener pinning mechanism at the austenite grain boundaries to restrict the grain size.
[0060] Thus, improved toughness is achieved.
[0061] It is believed that copper, due to its low misfit with the ferrite lattice, can contribute to the elastic misfit strain by forming a high density of coherent phase interfacial grains. The low magnetic moment of Cu is believed to play a positive role in increasing the number density of the complex nanoparticles. Without being bound to a particular theory, it is believed that the application of a magnetic field increases the Gibbs free energy of the system. The increase in Gibbs free energy promotes the precipitation of alloying elements, including Cu, and because Cu has a low magnetic moment, the precipitation is not hindered by the magnetic field.
[0062] In some embodiments, the steel comprises copper in the range of greater than 0 to about 0.5 (wt %). For example, the steel is a ferritic steel (e.g., a refractory alloy HSLA (high strength low alloy)).
[0063] In some embodiments, the steel comprises copper in the range of greater than 0 to about 1 (by weight). For example, the steel is a ferritic steel (e.g., AHSS (advanced high strength steel)).
[0064] In some embodiments, the steel comprises copper in the range of greater than 0 to about 1 (by weight). For example, the steel is a ferritic steel (e.g., a hydrogen resistant steel).
[0065] In some embodiments, the steel comprises copper in the range of greater than 0 to about 0.5 (wt %). For example, the steel is a pearlitic steel.
[0066] The presence of manganese is believed to contribute to ferrite grain refinement, for example when higher coiling temperatures are used.
[0067] In some embodiments, the steel comprises manganese in the range of about 0.4 to about 1.6 wt %, for example, the steel is a ferritic steel (eg, a refractory alloy HSLA (high strength low alloy)).
[0068] In some embodiments, the steel comprises manganese in the range of greater than 0 to about 0.8 (wt %). For example, the steel is a ferritic steel (e.g., AHSS (advanced high strength steel)).
[0069] In some embodiments, the steel comprises manganese in the range of greater than 0 to about 1.6 (wt %), for example, the steel is a ferritic steel (e.g., a hydrogen resistant steel).
[0070] In some embodiments, the steel comprises manganese in the range of about 0.6 to about 1.6 wt %, for example, the steel is pearlitic steel.
[0071] The presence of silicon is believed to increase the number density of coherent interfacial precipitates, for example when higher coiling temperatures are used. Silicon may retard the formation of pearlite and allow slower cooling rates, promoting the formation of coherent interfacial precipitates.
[0072] In some embodiments, the steel comprises silicon in the range of greater than 0 to about 0.5 (wt%). For example, the steel is a ferritic steel (e.g., a refractory alloy HSLA (high strength low alloy)).
[0073] In some embodiments, the steel comprises silicon in the range of greater than 0 to about 0.5 (wt%). For example, the steel is a ferritic steel (e.g., AHSS (advanced high strength steel)).
[0074] In some embodiments, the steel comprises silicon in the range of greater than 0 to about 1.5 (wt%). For example, the steel is a ferritic steel (e.g., a hydrogen resistant steel).
[0075] In some embodiments, the steel comprises silicon in the range of greater than 0 to about 1.2 (wt%), for example, the steel is pearlitic steel.
[0076] The presence of chromium is believed to increase the solid solubility of the other microalloying elements and reduce the size of the precipitates, thus keeping the average precipitate size below the coherent size limit, thereby increasing the proportion of coherent precipitates.
[0077] In some embodiments, the steel comprises chromium in the range of greater than 0 to about 0.3 (wt %). For example, the steel is a ferritic steel (e.g., a refractory alloy HSLA (high strength low alloy)).
[0078] In some embodiments, the steel comprises chromium in the range of greater than 0 to about 0.3 (wt %). For example, the steel is a ferritic steel (e.g., AHSS (advanced high strength steel)).
[0079] In some embodiments, the steel comprises chromium in the range of greater than 0 to about 0.3 (wt %). For example, the steel is a ferritic steel (e.g., a hydrogen resistant steel).
[0080] In some embodiments, the steel comprises chromium in the range of greater than 0 to about 0.1 (wt %). For example, the steel is a pearlitic steel.
[0081] The presence of molybdenum is believed to contribute to an increase in the number density of coherent phase interface grains by forming complexes with the precipitates that can improve the diffusion rate of the precipitates.
[0082] Optionally, the coherent phase interface precipitates include Mo, and optionally, the coherent phase interface precipitates have the formula (Mo,V) x C ywhere x>y, for example, (Mo,V)C / (Mo,V)C.
[0083] This is believed to have the effect of reducing the lattice mismatch between the interphase precipitates and the ferrite phase, resulting in improved coherence.
[0084] In addition, the presence of Mo is believed to reduce the rate of migration from the austenite to the ferrite phase interface during transformation, allowing more interphase precipitates to form.
[0085] In some embodiments, the steel comprises molybdenum in the range of greater than 0 to about 0.2 (wt %). For example, the steel is a ferritic steel (e.g., a refractory alloy HSLA (high strength low alloy)).
[0086] In some embodiments, the steel comprises molybdenum in the range of greater than 0 to about 0.5 (wt %). For example, the steel is a ferritic steel (e.g., AHSS (advanced high strength steel)).
[0087] In some embodiments, the steel comprises molybdenum in the range of greater than 0 to about 0.5 (wt %). For example, the steel is a ferritic steel (e.g., a hydrogen resistant steel).
[0088] In some embodiments, the steel comprises molybdenum in the range of greater than 0 to about 0.2 (wt %). For example, the steel is a pearlitic steel.
[0089] Optionally, the ferrite phase includes grains having an average size of less than about 20 μm. For example, the average grain size is in the range of about 5 μm to about 20 μm. The grain size can be measured by any suitable method, for example, using a scanning electron microscope and electron backscatter diffraction. The average grain size can then be calculated using an intercept method. In this method, a line is drawn on the micrograph and the number of grain boundaries that intersect with the line are counted. The average grain size is determined by dividing the number of intersections by the length of the actual line.
[0090] Optionally, the microstructure of the steel includes VN precipitates, and optionally the microstructure includes intragranular VN nucleated acicular ferrite (e.g., V(C,N)). Optionally, the VN precipitates form in austenite as an intragranular nucleating agent for the formation of acicular ferrite. This is believed to be due to the low solid solubility of VN in austenite compared to vanadium carbide.
[0091] The intragranular VN nucleated acicular ferrite structure is believed to improve the alignment of phase interface grains and refine the ferrite grains, resulting in benefits to the elastic modulus and toughness of the steel.
[0092] In this way, an acicular microstructure is formed simultaneously with a system of nanoscale interphase precipitates, which is shown diagrammatically in Figure 7a.
[0093] In some embodiments, the steel comprises nitrogen in the range of greater than 0 to about 0.015 (wt %). For example, the steel is a ferritic steel (e.g., a refractory alloy HSLA (high strength low alloy)).
[0094] In some embodiments, the steel comprises nitrogen in the range of greater than 0 to about 0.015 (wt %). For example, the steel is a ferritic steel (e.g., AHSS (advanced high strength steel)).
[0095] In some embodiments, the steel comprises nitrogen in the range of greater than 0 to about 0.015 (wt %). For example, the steel is a ferritic steel (e.g., a hydrogen resistant steel).
[0096] In some embodiments, the steel comprises nitrogen in the range of greater than 0 to about 0.01 (wt %), for example, the steel is pearlitic steel.
[0097] In some embodiments, if not all of the nitrogen is used to form VN precipitates as intragranular nucleating agents for acicular ferrite formation, interphase vanadium carbonitrides may form as coherent interphase precipitates. Nitrogen is also beneficial in further increasing the driving force for precipitation and obtaining high number density of interphase precipitates.
[0098] Optionally, the steel comprises a single phase ferritic steel (eg, HSLA, AHSS, and / or hydrogen resistant steel).
[0099] Optionally, the steel comprises a pearlitic steel, thus comprising a ferrite phase and a cementite phase, the elastic modulus of the ferrite phase being enhanced by the presence of coherent phase interface particles and the above mechanisms.
[0100] Optionally, the pearlitic steel comprises a vanadium strengthened cementite phase, which optionally comprises vanadium dissolved in cementite, for example forming Fe2VC and / or FeV2C.
[0101] The average lattice spacing of the ferrite phase shrinks as a result of misfit strain from both the vanadium-containing coherent interphase precipitates and cementite. Vanadium can also readily dissolve in cementite given an appropriate isothermal holding regime, which may cause misfit-induced lattice strain due to the change in the lattice parameter of cementite.
[0102] Cementite is notable for its anisotropy, which also applies to the anisotropy of the elastic modulus components as a function of crystallographic orientation. When vanadium is dissolved in cementite, this anisotropy is reduced. This is thought to evolve as a function of isothermal holding time, as the composition of cementite changes with age.
[0103] Lattice strains associated with the elastic misfit of alloyed carbides or V-strengthened cementite can be examined using high-resolution scanning transmission electron microscopy (HRSTEM) and X-ray diffraction (XRD), respectively. Atom probe tomography can also be used as an additional method to quantify atomic concentrations in three dimensions.
[0104] The formation of lattice strains associated with iron carbides and strains induced by V-strengthening cementite in high carbon pearlitic steels can be characterized using electron backscatter diffraction (XRD). Elastic strains are quantified from the full width at half maximum (FWHM) of the ferrite diffraction peaks measured by XRD. Lattice strains in lamellar ferrite quantified by XRD measurements will also correlate with yield strength. The improved elastic modulus will also contribute to the yield strength obtainable by conventional tensile testing equipment.
[0105] Referring to Figure 5b, an exemplary embodiment is shown in which the steel includes cementite colonies, showing the additional strain imposed on the ferrite lattice by the cementite, which reduces the average lattice spacing of the ferrite matrix in the region proximate to the cementite colonies.
[0106] The change in lattice parameters along line AA is shown, indicating that the average lattice spacing contracts as a result of misfit strain from both the coherent vanadium alloy carbides and cementite, resulting in a change in bulk modulus.
[0107] Figure 5b also shows a schematic diagram of the pearlite microstructure containing V-strengthening cementite.
[0108] Optionally, the steel has a tensile strength in the range of about 690 MPa to about 2000 MPa, such as in the range of about 690 MPa to about 1800 MPa.
[0109] Tensile strength can be measured by gripping the ends of a properly prepared standard specimen in a tensile testing machine and then applying a continuously increasing uniaxial load up to the point where failure occurs. ASTM E8 / E8M-13: Standard Test Methods for Tensile Testing of Metallic Materials can be used.
[0110] The end result of greater number density and optimized precipitation composition may clearly impact the applicability of the steels disclosed herein for refractory or hydrogen transport / storage applications.
[0111] The structure of the steel alloys described herein may be determined by conventional microstructural evaluation techniques such as, for example, optical microscopy, TEM, SEM, AP-FIM, and X-ray diffraction (including combinations of two or more of these techniques).
[0112] In another aspect, there is provided a method for preparing a vanadium alloy steel as disclosed herein, comprising the steps of: Providing a starting steel; Heating the starting steel to at least partially austenitize the steel; holding the temperature of the steel at 650°C ± 200°C for about 25 minutes or less; Including, A method is provided in which the vanadium alloy steel comprises coherent interphase precipitates comprising vanadium.
[0113] Optionally, the starting steel comprises, preferably consists essentially of, and more preferably consists of vanadium and carbon.
[0114] Optionally, the starting steel comprises, preferably consists essentially of, and more preferably consists of vanadium, carbon, and balance iron.
[0115] Optionally, the starting steel comprises: Carbon in the range of about 0.06% by weight to about 1.1% by weight; Vanadium in the range of about 0.1% to about 1.5% by weight; comprises, preferably consists essentially of, more preferably consists of.
[0116] Optionally, the starting steel comprises: Carbon in the range of about 0.06% by weight to about 1.1% by weight; Vanadium in the range of about 0.1% to about 1.5% by weight; The remaining iron, comprises, preferably consists essentially of, more preferably consists of.
[0117] Optionally, the starting steel comprises vanadium and carbon, one or more of nitrogen, molybdenum, copper, silicon, chromium, and / or manganese, with the balance being iron.
[0118] Optionally, the starting steel comprises: Carbon in the range of about 0.06 to about 1.1; Vanadium in the range of about 0.1 to about 1.5; Nitrogen less than about 0.015, Molybdenum, less than about 1.6; Copper below approx. Silicon less than about 1.2; Chromium up to about 0.3; and / or Manganese below approx. 1.6 and one or more of The remaining iron, comprises, preferably consists essentially of, more preferably consists of.
[0119] Optionally, heating the starting steel to at least partially austenitize the steel includes increasing the temperature to at least about 900°C, optionally to a temperature in the range of about 920°C to about 1300°C, such as a temperature in the range of about 1100°C to about 1300°C.
[0120] In some embodiments, the starting steel may be provided in the form of a billet, a slab, a bloom, or any other suitable form.
[0121] In some embodiments, the heating may be performed by induction heating and / or a roller hearth furnace.
[0122] Holding the temperature of the steel at 650°C ± 200°C for up to about 25 minutes (i.e., isothermal holding) increases the number density of coherent phase interface precipitates, which in turn improves the elastic modulus (according to equation (1) above).
[0123] It has been found that the rapid advancement of the ferrite / austenite interface prevents the formation of precipitates at the ferrite / austenite interface, and thus such isothermal holding promotes interphase precipitation (e.g., vanadium carbide and / or vanadium carbonitride precipitation), resulting in improved properties of the steel.
[0124] The sheet spacing between the rows of interphase precipitates decreases with increasing transformation time. Thus, isothermal holding has the effect of decreasing the spacing between the rows of interphase precipitates, thereby increasing their number density.
[0125] Furthermore, such isothermal holding is believed to have the effect of increasing the V:C ratio in the interphase precipitates such that a large number of carbon vacancies are generated at the coherent interphase interfaces of the lattice matrix of the steel (e.g., ferrite). These vacancies act as hydrogen traps, leading to improved resistance to hydrogen embrittlement (see, e.g., Figures 4a and 4b).
[0126] In some embodiments, the temperature is maintained at 650° C.±200° C. for about 20 minutes or less.
[0127] In some embodiments, the temperature is maintained by placing the steel in an insulated thermal box.
[0128] In some embodiments, batch annealing is performed using, for example, an insulated thermal box to control the temperature applied to the steel. For example, a bell-type furnace can be used to apply the heat treatment to the entire coil.
[0129] In some embodiments, the temperature is maintained by using an induction heating system (eg, an induction furnace).
[0130] Optionally, the temperature is held at 650° C.±200° C. for about 15 minutes or less. In some embodiments, the temperature is held at 650° C.±200° C. for about 5 minutes to about 20 minutes, such as about 10 minutes to about 20 minutes. Optionally, following the isothermal hold, the steel is air cooled. Optionally, the temperature is held at 650°C ± 100°C.
[0131] Optionally, the steel is cooled at a cooling rate in the range of about 2°C / sec to about 80°C / sec, optionally at a cooling rate in the range of about 2°C / sec to about 50°C / sec, before holding the temperature at 650°C ± 200°C.
[0132] It has been found that rapid advancement of the ferrite / austenite interface prevents the formation of precipitates at the ferrite / austenite interface, and thus controlling the cooling rate in this way promotes interphase precipitation (e.g., vanadium carbide and / or vanadium carbonitride precipitation), which in turn improves the properties of the steel.
[0133] Furthermore, such rapid cooling of the steel prevents or hinders the formation of undesirable phases and / or promotes the formation of acicular ferrite.
[0134] In some embodiments, cooling is performed by air cooling, forced air cooling, laminar cooling, and / or any other suitable cooling method.
[0135] When Mn is present in the steel composition, this can promote higher number densities at faster cooling rates.
[0136] In some embodiments, after heating the starting steel, the steel is hot rolled above the recrystallization stop temperature (RST), optionally by recrystallization-controlled rolling and / or V(C,N) precipitation-controlled rolling.
[0137] By carrying out hot rolling at temperatures above the RST, grain deformation is limited, thereby promoting the formation of interphase precipitates.
[0138] Optionally, hot rolling of the steel is carried out before cooling it to 650°C ± 200°C.
[0139] In some embodiments, the hot rolling is carried out at one or more temperatures in the range of about 820°C to about 1200°C.
[0140] In some embodiments, hot rolling includes a roughing step, an intermediate step, and / or a finishing step.
[0141] Optionally, for compositions containing relatively high amounts of nitrogen, V(C,N) precipitation controlled rolling may be used to achieve low grain deformation levels.
[0142] In some embodiments, hot rolling the steel comprises hot rolling at substantially the V(C,N) precipitation temperature time nose.
[0143] For example, if V(C,N) precipitation controlled rolling is used, this may be carried out at substantially the V(C,N) precipitation temperature time nose.
[0144] At the precipitation temperature-time nose of V(C,N), the system has optimal free energy for VN to precipitate. Therefore, hot rolling at this temperature promotes the formation of acicular ferrite.
[0145] The precipitation temperature-time nose of V(C,N) varies with the specific composition of the steel, but is typically around 850°C.
[0146] In some embodiments, a magnetic field is applied to the steel composition during or after the temperature hold.
[0147] Optionally, the magnetic field is a static magnetic field in the range of about 0.2 T to about 16 T. Optionally, the magnetic field is a variable magnetic field, for example, applied by an induction heating system. In some embodiments, the variable magnetic field is applied by an induction heating system that also controls the temperature of the steel (e.g., used to maintain the temperature at 650° C.±200° C.).
[0148] The application of a magnetic field promotes an increase in the number density of coherent precipitates and also optimizes the composition of the constituent nano-sized precipitates.
[0149] In practice, long isothermal holds can have a detrimental effect on productivity. A proposed environmentally friendly method to accelerate this isothermal hold is to utilize a magnetic field, which can act to slow down the rate of austenite to ferrite transformation (thereby adjusting the spacing between precipitates and maximizing the number density of interphase precipitates). This can also lead to a wider range of carbides with higher V:C ratios due to paramagnetic effects.
[0150] Vanadium in solution acts to increase the Curie temperature Tc before precipitation (but with a small effect on the magnetic moment and a smaller energy of interaction with an external magnetic field), thus increasing the temperature range between Tc and a given transformation temperature below the Curie point, and therefore the magnetization at the transformation point becomes greater. The external magnetization energy acts to significantly increase the Gibbs free energy of the system, thus increasing the overall free energy for nucleation of nanoparticles, which subsequently increases the nucleation rate and the quantitative number density of the coherent phase interface vanadium precipitates.
[0151] In steel compositions containing higher amounts of carbon (i.e., pearlitic steels), the application of a magnetic field also acts to refine the interlamellar spacing of the pearlite (by increasing the nucleation rate of cementite), which may further contribute to the lattice strain and improved elastic modulus as a result of straining the ferrite lattice in regions close to the cementite colonies, as discussed above.
[0152] Optionally, the temperature is held at 650° C.±200° C. for up to about 25 minutes, after which the steel is reheated to at least partially austenitize the steel.
[0153] Optionally, this reheating step includes increasing the temperature to a range of about 920°C to about 1150°C.
[0154] Optionally, after reheating the steel, the temperature is again held at 650°C ± 200°C for up to about 25 minutes.
[0155] In some embodiments, the temperature is maintained at 650° C.±200° C. for about 20 minutes or less. Optionally, the temperature is maintained at 650° C.±200° C. for about 15 minutes or less. In some embodiments, the temperature is maintained at 650° C.±200° C. for a period ranging from about 5 minutes to about 20 minutes, such as from about 10 minutes to about 20 minutes. Optionally, following the isothermal hold, the steel is air cooled.
[0156] Optionally, the temperature is held at 650°C ± 100°C.
[0157] Isothermal holding in this manner promotes interphase precipitation (eg, precipitation of vanadium carbide and / or vanadium carbonitride), as previously described.
[0158] Optionally, the steel is reheated and then cooled at a cooling rate in the range of about 2°C / sec to about 80°C / sec, optionally to a temperature of 650°C±200°C.
[0159] Optionally, the cooling rate is in the range of about 2° C. / sec to 50° C. / sec. Controlled cooling promotes interphase precipitation (e.g., vanadium carbide and / or vanadium carbonitride precipitation) and inhibits the formation of undesirable phases, as discussed above.
[0160] Reheating leaves at least a portion of the previously formed precipitates in the steel, so that the reheating, subsequent cooling and / or subsequent isothermal holding steps result in an increase in the number density of precipitates in the final steel. [Brief description of the drawings]
[0161] [Figure 1] FIG. 1 shows a schematic diagram illustrating the interaction of coherent and incoherent precipitates with the surrounding ferrite lattice matrix. [Diagram 2] A comparison of the lattice parameter misfit and limited coherent precipitate size for precipitates containing Ti, V, Zr, or Nb is shown. [Diagram 3] The relationship between strength and precipitate grain size is shown. [Figure 4a] FIG. 1 is a schematic diagram illustrating the ability of coherent phase interface precipitates to act as hydrogen traps. [Figure 4b] FIG. 1 is a schematic diagram illustrating the ability of coherent phase interface precipitates to act as hydrogen traps. [Figure 5a] The effect of the strain field in the ferrite matrix on the average lattice parameter of ferritic steel is shown. [Figure 5b] The effect of the strain field of the ferrite matrix on the average lattice parameter of pearlitic steel is shown. [Figure 6] Three typical beam configurations (according to Eurocode 3) are shown. [Figure 7a] A schematic diagram of the VN nucleated acicular ferrite structure is shown. [Figure 7b] FIG. 1 shows a schematic diagram of a core-shell nanoparticle. [Figure 8] FIG. 1 shows a process diagram illustrating a steel manufacturing process according to the present disclosure. [Figure 9] 9 shows a flow chart illustrating additional steps that can be applied to the process of FIG. 8. [Figure 10] FIG. 1 shows a process diagram illustrating a process for producing modulus enhanced hot rolled high carbon wire steel according to the present disclosure. [Figure 11] 11 shows a flow chart illustrating additional steps that can be applied to the process of FIG. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0162] The vanadium alloy steels and manufacturing processes disclosed herein will now be described with reference to the following non-limiting examples. EXAMPLES
[0163] Four exemplary steel compositions according to the present disclosure are set forth in Table 1. Each composition also includes a balance amount of iron. [Table 1]
[0164] The ferrite compositions shown in Table 1 have been determined to have the characteristics and properties shown in Table 2. [Table 2] EXAMPLES
[0165] A typical composition for a high modulus AHSS steel is shown in Table 3. Such a composition also includes a balance of iron, which in this case is 97.6955 wt. %. [Table 3] EXAMPLES
[0166] A conventional steel of grade S690MC (according to EN10051) was compared with a nanostructured enhanced modulus steel as disclosed herein. The conventional S690MC steel is considered to have a nominal modulus of elasticity of 210 GPa (according to European Standard EN1993-1-1: Eurocode 3: Design of steel structures, and European Standard EN1993-1-12: General - High tensile steels). The modulus-enhanced steel is considered to have an average modulus of elasticity of 230 GPa, i.e. an increase of 20 GPa.
[0167] Figure 6 shows three typical beam configurations (according to Eurocode 3). The results regarding the reduction in deflection due to the increase in elastic modulus are shown in Table 4. These results were obtained by computer simulation. [Table 4] EXAMPLES
[0168] With reference to FIG. 8, an exemplary method for producing the enhanced modulus steel disclosed herein will now be described.
[0169] A slab (or alternatively a billet) of cast steel is heated to a reheat temperature (Treh) in the range of about 1100 to about 1300°C. This is shown by reference numeral 102 in Figure 8. This temperature is maintained until the steel slab is fully heated throughout its thickness (i.e., at Teq as shown in Figure 8). By heating the steel slab in this manner, the steel is heated to form austenite (γ) having a grain microstructure as shown in the schematic diagram shown at reference numeral 104.
[0170] The heated steel is then hot rolled at a temperature ranging from about 820° C. to about 1200° C., first in a roughing mill, indicated at 106, and then in a finishing mill, indicated at 108. During hot rolling, the temperature of the steel is cooled under standard air cooling, for example at about 0.7° C. / sec.
[0171] Hot rolling in the finishing mill 108 can be performed using conventional recrystallization controlled rolling. Alternatively, V(C,N) precipitation controlled rolling can be performed, especially if the steel has a composition with a relatively high amount of nitrogen. This is performed at a V(C,N) precipitation time temperature nose 110 where there is optimal free energy for VN to precipitate. The V(C,N) precipitation time temperature nose varies depending on the composition of the particular steel, but is typically around 850°C.
[0172] When the steel is hot rolled, especially in the finishing mill, VN precipitates in the austenite as an intragranular nucleating agent for the formation of acicular ferrite. At this stage the steel has a microstructure as shown diagrammatically at 112.
[0173] Before the recrystallization stop temperature (RST) is reached and after hot rolling is completed, the steel is quenched (114) at a cooling rate in the range of about 2°C / sec to about 80°C / sec until a temperature of 650±100°C is reached. This can be done by forced air cooling, laminar cooling, or other suitable cooling means. Cooling the steel rapidly in this manner prevents or hinders the formation of undesirable phases and / or promotes the formation of acicular ferrite, as shown generally at 116.
[0174] Once the temperature of 650±100°C is reached, the steel is formed into a coil. The temperature of the steel is then held at 650±100°C for a time ranging from about 10 minutes to about 20 minutes (118), after which the steel is air cooled. As noted above, this isothermal hold promotes the formation of interphase precipitates.
[0175] In this way, nanostructured steels with improved elastic modulus are produced.
[0176] Optionally, the method may further include the step shown in FIG. 9 to increase the number density of interphase precipitates.
[0177] After the isothermal hold step 118, the coiled steel is cooled and then blanks are stamped or cut from the decoiled strip 120. Optionally, this step can be omitted.
[0178] The steel may then be austenitized a second time by heating it to a temperature in the range of about 920° C. to about 1150° C. (122), for example, using a roller hearth furnace and / or an induction heating device. The reheated steel is then cooled at a rate in the range of about 2° C. / sec to about 50° C. / sec until it reaches a temperature of 650±40° C. (124). Cooling may be performed using forced air cooling, laminar cooling, or other suitable methods.
[0179] A static magnetic field ranging from about 0.2 T to about 16 T can then be applied to the steel (26). While the magnetic field is applied, the temperature is held at 650 ± 40 °C for no more than about 15 minutes. For example, this may be performed using an insulated thermal box.
[0180] Alternatively, after the blank is stamped or cut (120) from the decoiled strip, a variable magnetic field is applied (128) to the steel. For example, this may be applied using an induction heating system. While the variable magnetic field is applied, the temperature is held at 650±100°C for no more than 15 minutes.
[0181] In an alternative embodiment, a magnetic field is applied to the steel during the isothermal hold step (118), using either a static magnetic field or a variable magnetic field.
[0182] The resulting modulus enhanced nanostructured steel is then air cooled (130) and ready for cold stamping and / or forming as desired.
[0183] Alternatively, instead of decoiling and stamping a blank from the steel, the entire coil can be reheated (i.e., austenitized) (122), cooled (124), and then held at 650±100° C. for the required time. This can be done as a batch annealing process using an insulated thermal box (e.g., a bell-type furnace suitable for applying heat treatment to the entire coil).
[0184] This method is applicable to both ferritic and pearlitic steels. EXAMPLES
[0185] 10 illustrates a method for producing modulus enhanced hot rolled high carbon wire steel. A billet of cast steel is heated (202) to a reheat temperature as described in connection with Example 4.
[0186] The heated steel is then hot rolled (206) at temperatures ranging from about 840° C. to about 1200° C. using roughing, intermediate, finishing, and / or twistless V-block mills. Hot rolling is performed above the recrystallization stop temperature so that grain distortion is minimized.
[0187] After hot rolling is completed, the steel is quenched at a cooling rate in the range of about 2°C / sec to about 80°C / sec until a temperature of 650±100°C is reached (214).
[0188] The temperature is then held at 650±100° C. (218), for example, using an in-line induction heating coil. Referring to FIG. 11, the steel is then air cooled (230).
[0189] Optionally, the steel can then be cold drawn (132). In this process, the steel wire is induction heated to austenitization, fan cooled to 600 ± 50 °C, and then the temperature is held at 650 ± 200 °C for less than 5 minutes. These steps are applied in successive, slow motions. Optionally, a static magnetic field can be applied at this stage to refine the interlamellar spacing of the pearlite, which can further contribute to the lattice strain and improved elastic modulus.
[0190] Unless otherwise specified, each integer described herein can be used in combination with any other integer, as will be understood by those skilled in the art. Furthermore, it is specifically contemplated that all aspects of the invention, while preferably "comprising" the features described in connection with that aspect, can "consist" or "consist essentially" of the features outlined in the claims. Also, unless otherwise defined herein, all terms are intended to be given the meanings commonly understood in the art.
[0191] Furthermore, in the discussion of the present invention, unless otherwise indicated, the disclosure of alternative values at the upper or lower limits of an acceptable range of a parameter is to be construed as an implicit statement that each intermediate value of that parameter between the lower and upper alternatives is also itself disclosed as a possible value of the parameter.
[0192] Additionally, unless otherwise specified, all numerical values set forth in this application should be understood as being modified by the term "about."
Claims
1. A vanadium alloy steel comprising carbon and vanadium, the microstructure of the vanadium alloy steel comprising coherent phase interfacial precipitates comprising vanadium.
2. carbon in the range of about 0.06% to about 1.1% by weight; Vanadium in the range of about 0.1% to about 1.5% by weight; The vanadium alloy steel of claim 1 , comprising:
3. 3. The vanadium alloy steel of claim 1 or 2, wherein the vanadium alloy steel is a modulus strengthened steel with an average modulus of elasticity greater than about 210 GPa, optionally the vanadium alloy steel has an average modulus of elasticity up to about 300 GPa.
4. The vanadium alloy steel according to any one of claims 1 to 3, wherein the coherent phase interfacial precipitates have a grain size of about 9 nm or less.
5. The vanadium alloy steel of claim 4, wherein the coherent phase interfacial precipitates have a grain size ranging from about 5 nm to about 9 nm.
6. The vanadium alloy steel according to any one of claims 1 to 5, wherein the coherent phase interfacial precipitates comprise vanadium carbides.
7. The coherent phase interface precipitate has the formula V x C y (wherein x>y) (e.g., the coherent phase interface precipitates include precipitates having high levels of vanadium, 4 C 3 The vanadium alloy steel of claim 6.
8. The coherent phase interface precipitates are V 6 C 5 and / or V 5 C 3 The vanadium alloy steel of claim 7, comprising:
9. The composition of the vanadium alloy steel is about 0.015% by weight or less of nitrogen; up to about 1.6 weight percent molybdenum; about 1% by weight or less copper; up to about 1.2 wt. % silicon; % by weight or less of chromium, and / or Up to about 1.6% by weight manganese The vanadium alloy steel according to any one of claims 1 to 8, comprising at least one of the following:
10. The composition of the vanadium alloy steel is Carbon in the range of about 0.06% to about 1.1% by weight; Vanadium in the range of about 0.1% to about 1.5% by weight; about 0.015% by weight or less of nitrogen; up to about 1.6 weight percent molybdenum; about 1% by weight or less copper; up to about 1.2 wt. % silicon; % by weight or less of chromium, and Up to about 1.6% by weight manganese The vanadium alloy steel according to any one of claims 1 to 9, comprising:
11. The coherent phase interface precipitates include Mo, and optionally the coherent phase interface precipitates have the formula (Mo,V) x C y (wherein x>y), for example, (Mo,V) 4 C 3 11. The vanadium alloy steel according to claim 9 or 10, comprising precipitates having the formula: / (Mo,V)C.
12. The vanadium alloy steel according to any one of claims 9 to 11, wherein the microstructure of the vanadium alloy steel comprises VN precipitates, and optionally the microstructure comprises intragranular VN nucleated acicular ferrite.
13. The vanadium alloy steel according to any one of claims 1 to 12, wherein the vanadium alloy steel comprises a ferrite phase, and the coherent phase interface precipitates are formed in the ferrite phase to form spheroidal ferrite or nodular ferrite.
14. The vanadium alloy steel of claim 13, wherein the ferritic phase comprises grains having an average size of less than about 20 μm, such as in the range of about 5 μm to about 20 μm.
15. The vanadium alloy steel of any one of claims 1 to 14, wherein the vanadium alloy steel comprises a single phase ferritic steel (e.g. HSLA, AHSS).
16. The vanadium alloy steel according to any one of the preceding claims, wherein the vanadium alloy steel comprises a pearlite phase, and optionally the vanadium alloy steel comprises vanadium strengthened cementite.
17. The vanadium-strengthened cementite contains vanadium dissolved in the cementite, for example Fe. 2 VC and / or FeV 2 17. The vanadium alloy steel of claim 16, forming C.
18. The vanadium alloy steel of any one of claims 1 to 17, wherein the vanadium alloy steel comprises a tensile strength in the range of about 360 MPa to about 2000 MPa.
19. A method for preparing the vanadium alloy steel according to any one of claims 1 to 18, comprising the steps of: Providing a starting steel; heating the starting steel to at least partially austenitize the starting steel; holding the temperature at 650° C.±200° C. for about 25 minutes or less; A method comprising:
20. The starting steel is carbon in the range of about 0.06% to about 1.1% by weight; Vanadium in the range of about 0.1% to about 1.5% by weight; Optionally, about 0.015% by weight or less of nitrogen; Up to about 1.6% by weight molybdenum about 1% by weight or less copper; up to about 1.2 wt. % silicon; up to about 0.3% by weight chromium, and / or Up to about 1.6% by weight manganese One or more of 20. The method of claim 18 having a composition comprising:
21. 21. The method of claim 19 or 20, wherein the starting steel is cooled at a cooling rate in the range of about 2°C / s to about 80°C / s, optionally to a temperature of 650°C±200°C, before holding the temperature at 650°C±200°C.
22. 22. The method according to any one of claims 19 to 21, wherein after heating the starting steel, the starting steel is hot rolled above a recrystallization stop temperature (RST), optionally by recrystallization controlled rolling and / or V(C,N) precipitation controlled rolling.
23. 23. The method of claim 22, wherein hot rolling the starting steel comprises hot rolling at substantially a V(C,N) precipitation temperature time nose.
24. A method according to any one of claims 19 to 23, wherein a magnetic field is applied to the starting steel composition during or after holding at temperature.
25. 25. The method of any one of claims 19 to 24, wherein after holding the temperature at 650°C ± 200°C for about 25 minutes or less, the starting steel is reheated to at least partially austenitize the starting steel.
26. 26. The method of claim 25, wherein after reheating the starting steel, the temperature is again held at 650°C ± 200°C for no more than about 25 minutes.
27. 27. The method of claim 25 or 26, wherein after reheating the starting steel, the starting steel is cooled at a cooling rate in the range of about 2°C / sec to about 80°C / sec, optionally to a temperature of 650°C±200°C.
Citation Information
Patent Citations
Low cr ferritic heat resistant steel and production method therefor
JP2002180178A
High-rigidity high-strength thin steel sheet and method for producing same
JP2005314792A
High-rigidity high-strength thin steel sheet and method for producing same
JP2005314793A
High-rigidity / high-strength thin steel sheet and manufacturing method therefor
JP2006183130A
High-rigidity / high-strength thin steel sheet and manufacturing method therefor
JP2006183131A