Cold-rolled heat-treated steel sheet and its manufacturing method

A cold rolled heat-treated steel sheet with a specific composition and microstructure, combined with controlled annealing and tempering, achieves high strength and formability, ensuring weldability and coating compatibility, addressing the balance of strength and formability in automotive parts.

JP2024538819AInactive Publication Date: 2024-10-23ARCELORMITTAL SA
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2024525321
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2021-10-29
Publication Date
2024-10-23
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing high-strength and high-formability steel sheets lack one or both properties, failing to achieve a balance between strength and formability, and are not weldable without liquid metal embrittlement, which is a challenge in automotive parts requiring improved fuel efficiency and crashworthiness.

Method used

A cold rolled heat-treated steel sheet with a specific chemical composition and microstructure, including carbon, manganese, silicon, and other alloying elements, achieving a microstructure of at least 75% tempered martensite, 3-20% ferrite, and controlled amounts of bainite and fresh martensite, with a method that includes controlled annealing and tempering processes.

Benefits of technology

The steel sheet achieves ultimate tensile strength over 1500 MPa, yield strength over 1100 MPa, total elongation over 6%, and 90°V bendability of 2.5t or less, with good weldability and coating compatibility, addressing the balance of strength and formability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024538819000001
    Figure 2024538819000001
  • Figure 2024538819000002
    Figure 2024538819000002
  • Figure 2024538819000003
    Figure 2024538819000003
Patent Text Reader

Abstract

Cold rolled heat treated steel sheet, containing the following elements expressed in weight percent: 0.2%≦C≦0.35%, 0.2%≦Mn≦1.2%, 0.1%≦Si≦0.9%, 0%≦Al≦0.1%, 0.2%≦Cr≦0.8%, 0.01%≦Nb≦0.1%, 0.1%≦Ni≦0.9%, 0.1%≦Mo≦0.9%, 0.01%≦Ti≦0.1%, 0%≦P≦0.02%, 0%≦S≦0.03%, 0%≦N≦0.09%, 0.0001%≦B≦0.0 A cold rolled heat treated steel sheet comprising, by area percentage, at least 75% tempered martensite, 0% to 10% fresh martensite, 3 to 20% ferrite and 0 to 5% bainite, with the remainder consisting of iron and unavoidable impurities resulting from processing.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a cold-rolled steel sheet suitable for use as a steel sheet for vehicles. [Background technology]

[0002] Automotive parts must meet two contradictory needs: ease of forming and strength. Recently, however, due to environmental concerns, automobiles have been given a third requirement: improved fuel economy. Thus, automotive parts must now be made from materials with high formability to meet the criteria of ease of fitting into complex automotive assemblies, while at the same time improving strength for vehicle crashworthiness and durability while reducing vehicle weight for improved fuel economy. Additionally, steel parts must be weldable without the drawback of liquid metal embrittlement.

[0003] Therefore, there is a strong research and development effort to reduce the amount of material used in the vehicle interior by increasing the strength of the material. Conversely, increasing the strength of steel sheets reduces their formability, so there is a need to develop materials that have both high strength and high formability.

[0004] Previous research and development in the field of high strength and highly formable steel plates has led to several methods for producing high strength and highly formable steel plates, some of which are listed here for a final understanding of the present invention.

[0005] EP3486346 presents a steel sheet having a specific chemical composition and a manufacturing method thereof. The steel sheet has a microstructure including martensite and bainite. The total area fraction of martensite and bainite in the entire microstructure is 95% or more and 100% or less. The remainder of the microstructure is at least one of ferrite and retained austenite. The microstructure includes specific inclusion clusters, and the content of the inclusion clusters in the microstructure is mm 2The microstructure contains prior austenite grains with an average size of more than 5 μm. The steel plate has a tensile strength of more than 1320 MPa. However, the steel of EP 3486346 cannot reach a bendability of less than 2.5t.

[0006] Known prior art techniques for producing high strength and high formability steel sheets suffer from the deficiencies of one or the other. Thus, there is a need for cold rolled steel sheets having strengths in excess of 1500 MPa and methods for producing same. [Prior art documents] [Patent documents]

[0007] [Patent Document 1] European Patent Application Publication No. 3486346 Summary of the Invention

[0008] The object of the present invention is to provide the following: - an ultimate tensile strength of at least 1500 MPa, preferably more than 1600 MPa; - a yield strength of more than 1100 MPa, preferably more than 1130 MPa, - Total elongation of 6% or more, - Hole expansion ratio of 10% or more, - Bendability of 2.5t or less when measuring 90° V-bend The object of the present invention is to solve the above problems by making available a cold-rolled, heat-treated steel sheet having the above properties at the same time.

[0009] In a preferred embodiment, the cold rolled heat treated steel sheet exhibits a YS / TS ratio of greater than 0.60.

[0010] Preferably, such a steel should also have good suitability for forming, especially rolling, together with good weldability and coatability.

[0011] Another object of the invention is also to make available a manufacturing method for these plates that is compatible with conventional industrial applications while being robust to shifts in manufacturing parameters.

[0012] The cold rolled, heat treated steel sheet of the present invention may optionally be coated with zinc or a zinc alloy, or with aluminum or an aluminum alloy, to improve its corrosion resistance. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0013] Other features and advantages of the present invention will become apparent from the following detailed description of the invention.

[0014] Carbon is present in the steel in an amount of 0.2% to 0.35%. Carbon is an element necessary to retard the formation of ferrite and bainite during cooling after annealing, thereby increasing the strength of the steel sheet. At a content of less than 0.2%, the steel of the present invention will not have sufficient tensile strength and ductility. On the other hand, if the carbon content exceeds 0.35%, the welds and heat-affected zones will be significantly hardened, and the mechanical properties of the welds will be impaired. The preferred limit of carbon is 0.22% to 0.35%, and the more preferred limit is 0.22% to 0.34%.

[0015] The manganese content of the steel of the present invention is between 0.2% and 1.2%. Manganese is a strength imparting element and an amount of at least 0.2% manganese is necessary to impart strength and hardenability to the steel sheet by retarding the formation of ferrite. Thus, the manganese percentage is preferably between 0.3% and 1.1%, more preferably between 0.4% and 1%. However, if the manganese content exceeds 1.2%, it will have adverse effects such as retarding the transformation from austenite to martensite, which will reduce the ductility of the final product. Also, if the manganese content exceeds 1.2%, central segregation will occur and the weldability of the steel will be reduced. Furthermore, a high manganese content is detrimental in terms of hydrogen delayed fracture, which is an important criterion for steel manufacturers and the automotive industry.

[0016] The silicon content of the steel of the present invention is between 0.1% and 0.9%. Silicon is an element that contributes to the strength improvement by solid solution strengthening. Silicon is a constituent that can delay the precipitation of carbides during cooling after annealing, therefore silicon promotes the formation of martensite. However, silicon is also a ferrite former and also increases the Ac3 transformation point, which pushes the annealing temperature to a higher temperature range, which is why the silicon content is kept at a maximum of 0.9%. A silicon content above 0.9% can also strengthen the embrittlement, in addition silicon also impairs the coatability. The preferred limit of silicon presence is between 0.2% and 0.8%, more preferably between 0.3% and 0.7%.

[0017] The aluminum content of the steel of the present invention is 0-0.1%. Aluminum can be added during steelmaking to deoxidize the steel and capture oxygen. Above 0.1%, the Ac3 point becomes high and productivity decreases. Also, within such ranges, aluminum combines with nitrogen in the steel to form aluminum nitrides, reducing the grain size, and aluminum also retards the precipitation of cementite, but in the present invention, when the aluminum content exceeds 0.1%, the amount and size of aluminum nitrides are detrimental to hole expansion and bending, and also pushes Ac3 into a higher temperature range that is industrially very expensive to achieve, and further causes grain coarsening during annealing and soaking. The preferred limit of aluminum is 0%-0.06%, more preferably 0%-0.05%.

[0018] Chromium is an essential element of the steel of the present invention and is present in an amount between 0.2% and 0.8%. Chromium provides strength and hardening to the steel, but if used in excess of 0.8%, it will impair the surface finish of the steel. The preferred limits for chromium are 0.2% to 0.7%, more preferably 0.2% to 0.6%.

[0019] Niobium is an essential element and may be present in an amount of 0.01% to 0.1%, preferably 0.01% to 0.09%, more preferably 0.01% to 0.07%. The formation of carbonitrides is suitable for imparting strength to the steel according to the invention by precipitation hardening during the annealing soaking temperature range, which leads to hardening of the product. However, when the niobium content exceeds 0.1%, the consumption of carbon by niobium by forming a large amount of carbonitrides is not preferred for the invention, since a large amount of carbonitrides tends to reduce the ductility of the steel.

[0020] Nickel is an essential element and is present in an amount of 0.1% to 0.9% in order to increase the strength of the steel of the present invention and improve its toughness. A minimum of 0.01% is preferred to obtain such effects. The preferred limits of nickel are 0.2% to 0.7%, more preferably 0.3% to 0.6%.

[0021] Molybdenum is an essential element and is present in the steel of the present invention in an amount of 0.01% to 0.9%. Molybdenum plays an effective role in improving hardenability and hardness, and when added in an amount of at least 0.01%, it retards the formation of ferrite and bainite during cooling after annealing. Mo is also beneficial for the toughness of hot-rolled products, making them easier to manufacture. However, the addition of molybdenum excessively increases the cost of adding alloying elements, so for economic reasons, its content is limited to 0.9%. The preferred limit for molybdenum is 0.01% to 0.7%, more preferably 0.01% to 0.6%.

[0022] Titanium is an essential element added to the steel of the invention in an amount of 0.01% to 0.1%, preferably 0.01% to 0.09%. The formation of carbides, nitrides and carbonitrides is suitable for imparting strength to the steel according to the invention by precipitation hardening during the annealing soaking temperature range, resulting in hardening of the product. However, titanium contents exceeding 0.1% are not preferred for the invention, since titanium consumes carbon by forming a large amount of precipitates, which tend to reduce the ductility of the steel. The preferred limit for titanium is 0.01% to 0.08%, more preferably 0.01% to 0.06%.

[0023] The phosphorus content of the steel of the invention is limited to 0.02%. Phosphorus is a hardening element in solid solution. Small amounts of phosphorus, at least 0.002%, can therefore be advantageous, but phosphorus also has its negative effects, such as reduced spot weldability and hot rollability, due in particular to its tendency to segregate at grain boundaries or co-segregate with manganese. For these reasons, its content is preferably limited to a maximum of 0.015%.

[0024] Sulfur is not an essential element, but may be present in the steel as an impurity. The lower the sulfur content, the better, but from the viewpoint of production costs, it is 0.03% or less, preferably 0.005% at most. Furthermore, if higher sulfur is present in the steel, it will combine with Mn and Ti to form sulfides, which are particularly detrimental to bending, hole expansion and elongation of the steel of the present invention.

[0025] Nitrogen is limited to 0.09% to avoid ageing of the material and to minimize the precipitation of nitrides during solidification, which are detrimental to the mechanical properties of the steel.

[0026] Boron is an optional element and can be added in the range of 0% to 0.010%, preferably 0.001% to 0.004%, to harden the steel. Boron traps nitrides to form boron nitrides, which impart strength to the steel of the present invention. Boron also imparts hardenability to the steel of the present invention. However, it has been found that the addition of more than 0.010% boron significantly reduces the rollability of the steel sheet. Further boron segregation can occur at grain boundaries, which is detrimental to formability.

[0027] Vanadium is an optional element that may be added to the steel of the present invention in a range of 0% to 0.1%, preferably 0.001% to 0.1%. Like niobium, vanadium plays a role in hardening, since it participates in carbonitrides. But it also participates in forming VN, which appears during solidification of the cast product. The amount of V is limited to 0.1% to avoid coarse VN, which is detrimental to hole expansion. If the vanadium content is less than 0.001%, vanadium does not have any effect on the steel of the present invention.

[0028] In order to increase the strength and improve the corrosion resistance of the steel of the present invention, 0% to 2% copper may be added as an optional element. To obtain such effects, a minimum of 0.01% copper is preferable. However, if the copper content exceeds 2%, the surface morphology may deteriorate.

[0029] Calcium is an optional element that may be added to the steel of the present invention in an amount of 0% to 0.005%, preferably 0.001% to 0.005%. Calcium is added to the steel of the present invention as an optional element, especially during inclusion treatment. Calcium contributes to the refinement of the steel by capturing the harmful sulfur content in the spheroidization of the steel.

[0030] Other elements such as cerium, magnesium or zirconium can be added individually or in combination in the following proportions: Ce≦0.1%, Mg≦0.05% and Zr≦0.05%. Up to the maximum content levels indicated, these elements make it possible to refine the inclusion particles during solidification.

[0031] The balance of the steel composition consists of iron and unavoidable impurities resulting from processing.

[0032] The microstructure of the steel sheet according to the present invention comprises, by area fraction, at least 75% tempered martensite, 3% to 20% ferrite, 0% to 5% bainite, and 0% to 10% fresh martensite.

[0033] The surface fraction of the phases in the microstructure is determined by the following method: a sample is cut from the steel sheet, polished and etched with reagents known per se to reveal the microstructure. The cross section is then examined using a scanning electron microscope, for example a scanning electron microscope equipped with a field emission gun ("FEG-SEM"), in secondary electron mode at a magnification of more than 5000 times.

[0034] The ferrite fraction is determined by SEM observation after etching with nital or picral / nital reagents.

[0035] The determination of the fraction of martensite or tempered martensite is carried out by dilatometric studies carried out according to SMCVan Bohemen and J. Sietsma in the publication Metallurgical and Materials transactions, Volume 40A, May 2009-1059.

[0036] The tempered martensite constitutes at least 75% of the microstructure by area fraction. The tempered martensite is formed during cooling after annealing, in particular from martensite occurring below the Ms temperature, more particularly below Ms-10°C. Such martensite is then tempered while being maintained at a tempering temperature Ttemper between 180°C and 320°C. The tempered martensite of the present invention imparts ductility and strength to such steel. Preferably, the content of tempered martensite is between 75% and 95%, more preferably between 78% and 90%.

[0037] The ferrite constitutes 3% to 20% of the microstructure in terms of area fraction of the steel of the present invention. The ferrite imparts strength and elongation to the steel of the present invention. The ferrite of the present steel may include polygonal ferrite, lath ferrite, acicular ferrite, plate ferrite or epitaxial ferrite. The ferrite of the present invention is formed during cooling after annealing. However, if the content of ferrite is more than 20% in the steel of the present invention, the hardness difference with hard phases such as tempered martensite, martensite, bainite, etc. becomes large, the local ductility decreases, and the total elongation and yield strength decrease, so that both the yield strength and the total elongation cannot be obtained at the same time. The preferred limit of the ferrite of the present invention is 5% to 20%, more preferably 5% to 15%.

[0038] Bainite is present in an amount of 0% to 5%. In the framework of the present invention, bainite may include carbide-free bainite and / or lath bainite and granular bainite. When present, lath bainite is in the form of laths with a thickness of 1 micron to 5 microns. When present, carbide-free bainite has a very low density of carbides and is less than 100 μm.2 Bainite having less than 100 carbides per area unit and possibly containing austenite islands. When present, granular bainite is a grain form with carbides present intragranularly. Bainite provides improved elongation. The preferred presence of bainite is 0%-3%.

[0039] Fresh martensite constitutes 0% to 10% of the microstructure by area fraction. In the steel of the present invention, fresh martensite is formed by cooling the cold rolled steel sheet after overaging. Martensite imparts ductility and strength to the steel of the present invention. However, if the presence of fresh martensite exceeds 10%, it imparts excess strength but reduces elongation beyond the allowable limit of the steel of the present invention. Fresh martensite contains a large amount of carbon and is therefore brittle and hard. Therefore, the preferred limit of fresh martensite for the steel of the present invention is 0% to 8%, more preferably 0% to 6%.

[0040] In addition to the above microstructure, the microstructure of the cold rolled heat treated steel sheet does not contain microstructural components such as pearlite, cementite and retained austenite without impairing the mechanical properties of the steel sheet.

[0041] The cold rolled steel sheet according to the invention can be produced by any suitable method. A preferred method consists in providing a semi-finished casting of steel having the chemical composition according to the invention. Casting can be carried out in ingots or continuously in the form of thin slabs or thin strip, i.e. with thicknesses ranging from about 220 mm for slabs to several tens of millimeters for thin strip.

[0042] For example, a slab is considered a semi-finished product. The slab having the above chemical composition is produced by continuous casting, and the slab is preferably subjected to a soft reduction directly during casting to ensure the elimination of center segregation and porosity reduction. The slab provided by the continuous casting process can be used directly at high temperature after continuous casting, or it can be first cooled to room temperature and then reheated for hot rolling.

[0043] The temperature of the slabs subjected to hot rolling should preferably be at least 1000°C, preferably above 1150°C and below 1300°C. If the temperature of the slab is below 1150°C, excessive loads will be applied to the rolling mill and the temperature of the steel may drop to the ferrite transformation temperature during the finish rolling, so that the steel is rolled with transformed ferrite in its structure. Moreover, the temperature should not exceed 1300°C, as this is industrially expensive.

[0044] The temperature of the slab is preferably high enough to allow hot rolling to be completed entirely in the austenitic field and for the final hot rolling temperature to remain above 850° C. It is necessary that the final rolling be carried out above 850° C., because below this temperature the rollability of the steel sheet decreases significantly.

[0045] The sheet thus obtained is then cooled to a temperature of 560°C or less at a cooling rate of at least 5°C / s. Preferably, the cooling rate is less than or equal to 100°C / s and more than 10°C / s. The hot rolled steel sheet is then coiled at a coiling temperature of 560°C to 500°C, preferably 500°C to 550°C, more preferably 510°C to 540°C. The coiled hot rolled steel sheet is then cooled, preferably to room temperature. The hot rolled sheet can then be subjected to an optional descaling process, such as pickling, to remove scale formed during hot rolling and ensure that the surface of the hot rolled steel sheet is free of scale before the hot rolled steel sheet is subjected to an optional hot band annealing.

[0046] The hot rolled sheet may be subjected to an optional hot band annealing at a temperature between 350°C and 750°C for 1 to 96 hours. The temperature and time of such hot band annealing are selected to ensure softening of the hot rolled sheet and to facilitate cold rolling of the hot rolled steel sheet. The hot rolled sheet may then be subjected to an optional descaling process, such as pickling, to remove scale formed during the hot band annealing.

[0047] Next, the hot-rolled steel sheet is cooled to room temperature, and then cold-rolled at a rolling reduction of 35 to 90% to obtain a cold-rolled steel sheet.

[0048] The cold rolled steel sheet is then annealed to impart the desired microstructure and mechanical properties to the steel of the present invention.

[0049] In the annealing, the cold rolled steel sheet is heated from room temperature to a soaking temperature TA of Ac3+10°C to Ac3+150°C at a heating rate HR1 of 1°C / sec to 30°C / sec. It is preferable to have an HR1 rate of 1°C / sec to 20°C / sec, more preferably 1°C / sec to 10°C / sec. The preferred TA temperature is 800°C to 900°C.

[0050] The cold rolled steel sheet is then held at the annealing soaking temperature TA for 100-1000 seconds to ensure sufficient transformation to form at least 80% austenite at the end of the soaking. The cold rolled steel sheet is then cooled at an average cooling rate CR1 of 5°C / s-200°C / s, preferably 8°C / s-100°C / s, more preferably 10°C / s-70°C / s, to a cooling stop temperature range CS1 of Ms-150°C-Ms-300°C, preferably 50°C-210°C, more preferably 100°C-210°C. During this cooling step, the martensite of the present invention is formed. If the CS1 temperature is higher than Ms-150°C, the steel of the present invention has too much austenite, which is detrimental to the total elongation.

[0051] The cold rolled steel sheet is then brought to a tempering temperature TT of 180°C to 320°C and held at the TT temperature for 1 to 500 seconds. A preferred tempering temperature TT is 190°C to 310°C. During this tempering step, the martensite formed during the cooling step is tempered to form tempered martensite. The duration of the tempering is selected such that no residual austenite remains in the cold rolled steel sheet at the end of the tempering.

[0052] The cold-rolled steel sheet is then cooled to room temperature at a cooling rate of at least 1° C. / sec to obtain a cold-rolled heat-treated steel sheet.

[0053] The resulting cold rolled heat treated steel sheet can then be optionally coated by any of the known methods. The coating can be made with zinc or a zinc-based alloy, or with aluminum or an aluminum-based alloy.

[0054] To ensure degassing of the coated product, an optional post-batch annealing, preferably at 170-210°C for 12-30 hours, can be performed after coating the product, followed by cooling to room temperature to obtain the cold-rolled coated steel sheet. EXAMPLES

[0055] The following tests and examples presented herein are non-limiting in nature and must be considered for illustrative purposes only, showing the advantageous features of the invention, explaining the importance of the parameters selected by the inventors after extensive experimentation, and further establishing the properties that may be achieved by the steel according to the invention.

[0056] Steel samples according to the invention and some comparative grades were prepared using the compositions summarized in Table 1 and the processing parameters collected in Table 2. The corresponding microstructures of these steel samples are summarized in Table 3 and the properties are summarized in Table 4.

[0057] Table 1 lists steels having compositions expressed in weight percent, and also lists the Ac3 and Ms for each steel, where the Ac3 and Ms temperatures are calculated from the formula derived by Andrews published in Journal of the Iron and Steel Institute, 203, 721-727, 1965.

[0058] Ac3(℃)=910-203×(%C)^(1 / 2)-15.2×(%Ni)+44.7×(%Si)+104×(%V)+31.5×(%Mo)+13.1 ×(%W)-30×(%Mn)-11×(%Cr)-20×(%Cu)+700×(%P)+400×(%Al)+120×(%As)+400×(%Ti).

[0059] Ms(℃)=539-423×(%C)-30.4×(%Mn)-12.1×(%Cr)-17.7×(%Ni)-7.5×(%Mo)

[0060] [Table 1]

[0061] Table 2 summarizes the annealing process parameters performed on the steels in Table 1.

[0062] Furthermore, before the annealing treatment of the steels of the present invention and the reference examples, the samples were heated to a temperature of 1150° C. to 1300° C. and hot rolled. All trials were cold rolled with a cold rolling reduction of 56%.

[0063] [Table 2]

[0064] Table 3 summarizes the results of tests carried out according to standards with different microscopes, such as a scanning electron microscope, to determine the microstructural composition of the specimens.

[0065] Table 3

[0066] From the above table it can be seen that all trials according to the present invention meet the microstructure goals.

[0067] Table 4 summarizes the mechanical and surface properties of the steels.

[0068] Table 4: Mechanical properties of the trials. The yield strength YS, tensile strength TS and total elongation TE are measured according to the ISO standard ISO 6892-1 published in October 2009.

[0069] [Table 3]

Claims

1. 2. A cold rolled heat treated steel sheet comprising the following elements expressed in weight percent: 0.2%≦C≦0.35%, 0.2%≦Mn≦1.2%, 0.1%≦Si≦0.9%, 0%≦Al≦0.1%, 0.2%≦Cr≦0.8%, 0.01%≦Nb≦0.1%, 0.1%≦Ni≦0.9%, 0.1%≦Mo≦0.9%, 0.01%≦Ti≦0.1%, 0%≦P≦0.02%, 0%≦S≦0.03%, 0%≦N≦0.09% and any of the following elements: 0.0001%≦B≦0.010%, 0%≦V≦0.1%, 0%≦Cu≦2%, 0%≦Ca≦0.005%, 0%≦Ce≦0.1%, 0%≦Mg≦0.05%, 0%≦Zr≦0.05% and the remainder of the composition consists of iron and unavoidable impurities resulting from processing, and the microstructure of the steel comprises, in area percent, at least 75% tempered martensite, 0% to 10% fresh martensite, 3 to 20% ferrite, and 0 to 5% bainite.

2. 2. The cold rolled heat treated steel sheet according to claim 1, wherein said composition comprises 0.22% to 0.35% carbon.

3. 3. The cold rolled heat treated steel sheet according to claim 1, wherein the composition contains 0.3% to 1.1% manganese.

4. The cold rolled heat treated steel sheet according to any one of claims 1 to 3, wherein the composition comprises 0% to 0.06% aluminum.

5. The cold rolled heat treated steel sheet according to any one of claims 1 to 4, wherein the composition comprises 0.2% to 0.8% silicon.

6. The cold rolled heat treated steel sheet according to any one of claims 1 to 5, which does not contain retained austenite.

7. The cold rolled heat treated steel sheet according to any one of claims 1 to 7, wherein the tempered martensite is 75% to 95%.

8. The cold rolled heat treated steel sheet according to any one of claims 1 to 8, having an ultimate tensile strength of 1500 MPa or more and a yield strength of 1100 MPa or more.

9. The following consecutive steps: - providing a steel composition according to any one of claims 1 to 5, - reheating said semi-finished product to a temperature between 1000°C and 1300°C, - rolling said semi-finished product in the austenitic range with a hot rolling finishing temperature above 850 ° C to obtain a hot rolled steel sheet; - cooling the sheet at a cooling rate of at least 5 ° C / s to a coiling temperature of not more than 560 ° C and coiling the hot rolled sheet; - cooling the hot rolled sheet to room temperature; - optionally subjecting said hot rolled steel plate to a descaling process; - optionally subjecting the hot rolled steel sheet to annealing; - optionally subjecting said hot rolled steel plate to a descaling process; - cold rolling the hot rolled steel sheet at a rolling reduction of 35 to 90% to obtain a cold rolled steel sheet; - then, starting heating the cold-rolled steel sheet from room temperature to a temperature TA of Ac3+10 ° C. to Ac3+150 ° C. at a heating rate HR1 of 1 ° C. / s to 30 ° C. / s and holding for 100 to 1000 seconds; - then starting to cool the cold-rolled steel sheet from TA to a temperature CS1 of Ms-150 ° C. to Ms-300 ° C. at a cooling rate CR1 of 5 ° C. / s to 200 ° C. / s; - then subjecting said cold-rolled steel sheet to a tempering temperature TT of 180 ° C. to 320 ° C. and holding for 1 to 500 seconds; - Then, cooling to room temperature at a cooling rate of at least 1 ° C. / sec to obtain a cold-rolled heat-treated steel sheet. A method for producing a cold-rolled heat-treated steel sheet comprising the steps of:

10. The method of claim 9, wherein the coiling temperature is from 560°C to 500°C.

11. The method according to claim 9 or 10, wherein CS1 is from 50°C to 210°C.

12. The method according to any one of claims 9 to 11, wherein TT is between 190°C and 310°C.

13. The method according to any one of claims 9 to 12, wherein TA is between 800°C and 900°C.

14. Use of a steel sheet obtained according to any one of claims 1 to 8 or produced by the method according to any one of claims 9 to 13 for producing structural parts of a vehicle.

Citation Information

Patent Citations

  • Hollow member and method for producing the same

    JP2018095899A

  • Process for manufacturing steel sheets for press hardening, and parts obtained by means of this process

    JP2019035149A

  • Bonded component and method for producing same

    WO2021162101A1

  • Steel sheet and production method therefor

    EP3486346A1