CATALYST FOR GAS PHASE OXIDATION OF 1,2,4,5-TETRAALKYLBENZENE, METHOD FOR PREPARATION THEREOF AND USE THEREOF, AND METHOD FOR PREPARATION OF 1,2,4,5-BENZENETTETRACARBOXYLIC ANHYDRIDE
A dual-coating catalyst with controlled titanium-to-vanadium mass ratios in each layer enhances the yield of 1,2,4,5-benzenetetracarboxylic anhydride by optimizing the catalytic activity, addressing the low yield issue in conventional vanadium-based catalysts.
Patent Information
- Application Number
- JP2024524388
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2021-11-01
- Filing Date
- 2022-10-28
- Publication Date
- 2024-10-28
- Estimated Expiration
- 2042-10-28
AI Technical Summary
Conventional vanadium-based catalysts for producing pyromellitic dianhydride by gas-phase oxidation of 1,2,4,5-tetraalkylbenzene have low actual yields, despite controlling elemental composition and loading the catalyst in stages, indicating a need for further improvement in yield optimization.
A catalyst with a dual coating structure is developed, where the first coating near the surface and the second coating further away from the surface have distinct titanium-to-vanadium mass ratios, with a controlled difference within a specific range, enhancing the catalytic activity and yield.
The dual-coating catalyst significantly improves the yield of 1,2,4,5-benzenetetracarboxylic anhydride by optimizing the titanium-to-vanadium mass ratio in each coating, achieving higher product yields compared to single-coating catalysts.
Smart Images

Figure 2024539251000001 
Figure 2024539251000002 
Figure 2024539251000003
Abstract
Description
Detailed Description of the Invention
[0001] [CROSS REFERENCE TO RELATED APPLICATIONS] This application claims the benefit of Chinese patent application No. 202111282786.7, filed on November 01, 2021, the contents of which are incorporated herein by reference.
[0002] [Technical field] The present invention relates to a catalyst, in particular to a catalyst for preparing 1,2,4,5-benzenetetracarboxylic anhydride by vapor phase oxidation of 1,2,4,5-tetraalkylbenzene, the present invention also relates to a method for preparing and using said catalyst, the present invention further relates to a method for preparing 1,2,4,5-benzenetetracarboxylic anhydride.
[0003] [Background technology] Pyromellitic dianhydride (1,2,4,5-benzenetetracarboxylic dianhydride, hereafter referred to as pyromellitic dianhydride) is a very important chemical raw material. Pyromellitic dianhydride and its derivatives are very important and have a wide range of applications, and pyromellitic dianhydride in particular is useful as one of the main monomers for producing polyimide. Polyimide has comprehensive performance under high temperatures, and is a new engineering material that can be used at the widest range of temperatures among current organic polymer materials, and has good dimensional stability, radiation resistance, mechanical properties, electrical properties, and corrosion resistance under high temperatures.
[0004] In the early days, the production of pyromellitic dianhydride using durene as a raw material mainly involved the liquid-phase oxidation method, in which the raw material was oxidized in the liquid phase to produce an acid, which was then dehydrated to produce an anhydride. Currently, the process that is commonly used is the gas-phase oxidation method, in which 1,2,4,5-tetraalkylbenzene is used as a raw material to produce 1,2,4,5-benzenetetracarboxylic dianhydride in one step by air oxidation. The gas-phase oxidation method is characterized by its simple process, the absence of a step of dehydrating the acid to produce the anhydride, the use of air as an oxidizing agent, the absence of the catalyst separation step required in the liquid-phase oxidation process, the possibility of continuous production, and ease of automation.
[0005] The production of pyromellitic dianhydride by oxidation of 1,2,4,5-tetraalkylbenzene is a reaction process in which selective oxidation generates relatively high heat, so that the theoretical yield of pyromellitic dianhydride is high but the actual yield is low.
[0006] Controlling the elemental composition of the catalyst is one of the technical means for increasing the yield of pyromellitic dianhydride that is mainly adopted in the prior art.CN107866241A is a catalyst for producing pyromellitic dianhydride by oxidizing durene, which uses an inert carrier and contains at least one of vanadium element, titanium element, VA group element and alkali metal element as an active component, andCN107866257A is a catalyst for producing pyromellitic dianhydride from durene, which uses α-Al2O3, silicon carbide, ceramic ring or a mixture thereof as a carrier and contains at least one of vanadium element, iron-based element, IIB group element and alkali metal element as an active component.
[0007] Staged catalyst loading is another prior art means of increasing the yield of pyromellitic dianhydride. CN1116197A discloses a method for producing 1,2,4,5-benzenetetracarboxylic anhydride, which comprises filling a reactor with catalysts in stages to form a multi-stage catalyst, and filling a first catalyst containing vanadium (a) and at least one metal (b) selected from molybdenum and tungsten, with the atomic ratio of the metal (b) to the vanadium (a) being 0.01-2 on the outlet side of the product gas of the reactor, and at least one other catalyst selected from a second catalyst containing vanadium (a) and at least one metal (b) selected from molybdenum and tungsten, with the atomic ratio of the metal (b) to the vanadium (a) being smaller than that of the first catalyst, and a third catalyst containing vanadium (a) and an alkali metal (c), with the atomic ratio of the alkali metal (c) to the vanadium (a) being 0.2-2.5 on the inlet side of the raw material mixed gas of the reactor.
[0008] Controlling the elemental composition of catalyst and loading catalyst stepwise have achieved a certain effect in increasing the yield of pyromellitic dianhydride, but there is still a relatively large difference between the actual yield and the theoretical yield of pyromellitic dianhydride, and how to further increase the actual yield of pyromellitic dianhydride remains a technical problem to be solved.
[0009] [Summary of the Invention] [Problem to be solved by the invention] Most of the conventional vanadium catalysts for producing pyromellitic dianhydride by the gas phase oxidation of 1,2,4,5-tetraalkylbenzene are formed with a coating containing catalytically active components on the surface of the carrier, but the present inventors have intensively studied the problem of the conventional technology that the yield of the product is low when producing pyromellitic dianhydride by the gas phase oxidation of durene, and as a result, have found that when forming a coating containing catalytically active components on the surface of the carrier of the vanadium catalyst, the mass ratio of titanium / vanadium in the coating close to the carrier is lower than the mass ratio of titanium / vanadium in the coating away from the carrier, and the difference between the two is within a predetermined range, by controlling the mass ratio of titanium / vanadium in the radial direction of the coating. Based on the above findings, the present invention has been completed.
[0010] [Means for solving the problem] According to a first aspect of the present invention, there is provided a method for producing ... composition comprising the steps of: The present invention comprises a carrier and a catalytically active component coating supported on the carrier, the catalytically active component coating comprising a first coating and a second coating, the first coating being close to a surface of the carrier and the second coating being distant from the surface of the carrier, the first coating and the second coating each independently containing vanadium element and titanium element, and a mass ratio of titanium element calculated as Ti to vanadium element calculated as V in the first coating is Ti / V 1 The mass ratio of titanium element (calculated as Ti) to vanadium element (calculated as V) in the second coating is Ti / V2 Then, Ti / V 2 = Ti / V 1 +ΔTi / V, and ΔTi / V is within the range of 3 to 9.
[0011] According to a second aspect of the present invention, there is provided a method for producing ... composition comprising the steps of: (1) applying a first slurry containing a first dispersing medium, a first vanadium source, and a first titanium source to a surface of a support to form a first coating; (2) applying a second slurry containing a second dispersing medium, a second vanadium source, a second titanium source, and a pore expander onto the first coated surface of the carrier to form a second coating; The mass of the vanadium source introduced into the first coating in terms of V is C V 12 The mass of the titanium source introduced into the first coating in terms of Ti is C Ti 12 The mass of the vanadium source introduced into the second coating in terms of V is C V 22 The mass of the titanium source introduced into the second coating in terms of Ti is C Ti 22 Then, Ti / V 12 =C Ti 12 / C V 12 , Ti / V 22 =C Ti 22 / C V 22 , Ti / V 22 = Ti / V 12 +ΔTi / V 2 and ΔTi / V 2 The present invention provides a method for preparing a catalyst for the gas phase oxidation of 1,2,4,5-tetraalkylbenzene, wherein the molar ratio of the catalyst is in the range of 3 to 9.
[0012] According to a third aspect of the invention, the present invention provides a catalyst prepared by the method according to the second aspect of the invention.
[0013] According to a fourth aspect of the invention, the present invention provides the use of a catalyst according to the first or third aspect of the invention as a catalyst for a reaction for preparing 1,2,4,5-benzenetetracarboxylic acid anhydride by oxidation of a 1,2,4,5-tetraalkylbenzene.
[0014] According to a fifth aspect of the present invention, there is provided a method for producing ... composition comprising the steps of: There is provided a process for preparing 1,2,4,5-benzenetetracarboxylic anhydride, comprising the step of contacting a gas comprising 1,2,4,5-tetraalkylbenzene and oxygen gas with a catalyst according to the first or third aspect of the present invention to obtain a product stream comprising 1,2,4,5-benzenetetracarboxylic anhydride.
[0015] When the catalyst according to the present invention is used as a catalyst for the reaction of preparing 1,2,4,5-benzenetetracarboxylic anhydride by oxidation of 1,2,4,5-tetraalkylbenzene, it exhibits improved catalytic activity and can effectively improve the yield of 1,2,4,5-benzenetetracarboxylic anhydride.
[0016] [Mode for carrying out the invention] The endpoints of the ranges and any values disclosed herein are not intended to be limited to the exact ranges or values, and these ranges or values should be understood to include values close to these ranges or values. In the case of numerical ranges, the endpoints of each range, and the individual point values and the individual point values can be combined with each other to obtain one or more new numerical ranges, and these numerical ranges should be considered to be specifically disclosed herein.
[0017] In the present invention, unless otherwise specified, the terms "first" and "second" appearing before the names of materials or steps do not indicate a sequence or limit the individual materials or steps, but are used simply to distinguish the names of the materials or steps. For example, in "first coating" and "second coating", "first" and "second" are used to distinguish two types of coatings. In the present invention, the term "optional" means that the term following "optional" is not required, and can be understood to contain, not contain, or include or not include the term.
[0018] In the present invention, the 1,2,4,5-tetraalkylbenzene may be one or more selected from the compounds shown in formula I: [ka] In formula I, R1, R2, R3, and R4 are the same or different and each independently represent C1 to C5 alkyl. In the present invention, C1 to C5 alkyl includes C1 to C5 linear alkyl and C3 to C5 branched alkyl, specific examples of which include, but are not limited to, methyl, ethyl, n-propyl, isopropyl, n-butyl, sec-butyl, isobutyl, tert-butyl, n-pentyl, isopentyl, tert-pentyl, and vineopentyl.
[0019] Preferably, the 1,2,4,5-tetraalkylbenzene is 1,2,4,5-tetramethylbenzene (ie, durene).
[0020] According to a first aspect of the present invention, there is provided a catalyst for the gas phase oxidation of 1,2,4,5-tetraalkylbenzenes, comprising a support and a catalytically active component coating supported on the support, the catalytically active component coating comprising a first coating and a second coating, the first coating being proximate to a surface of the support and the second coating being remote from the surface of the support.
[0021] According to the catalyst of the present invention, the first coating and the second coating each independently contain vanadium and titanium. According to the catalyst of the present invention, the mass ratio of titanium to vanadium in the first coating and the second coating (i.e., the mass ratio of Ti / V) is different, and the Ti / V in the second coating is 2 The mass ratio of Ti / V in the first coating is 1 The inventors have found that the mass ratio of Ti / V in the first coating, which is the inner coating close to the surface of the support, is higher than that of Ti / V in the first coating, which is the inner coating close to the surface of the support. 1 The mass ratio of Ti / V in the second coating, which is the outer coating away from the surface of the support, is 2 The mass ratio of titanium element calculated as Ti to vanadium element calculated as V in the first coating is controlled to be lower than Ti / V. 1 The mass ratio of titanium element (calculated as Ti) to vanadium element (calculated as V) in the second coating is Ti / V 2 Then, Ti / V 2 = Ti / V 1 +ΔTi / V, where ΔTi / V is within the range of 3 to 9. Specifically, ΔTi / V may be 3, 3.1, 3.2, 3.3, 3.4, 3.5, 3.6, 3.7, 3.8, 3.9, 4, 4.1, 4.2, 4.3, 4.4, 4.5, 4.6, 4.7, 4.8, 4.9, 5, 5.1, 5.2, 5.3, 5.4, 5.5, 5.6, 5.7, 5.8, 5.9, 6, 6.1, 6.2, 6.3, 6.4, 6.5, 6.6, 6.7, 6.8, 6.9, 7, 7.1, 7.2, 7.3, 7.4, 7.5, 7.6, 7.7, 7.8, 7.9, 8, 8.1, 8.2, 8.3, 8.4, 8.5, 8.6, 8.7, 8.8, 8.9, or 9. Preferably, ΔTi / V is within the range of 3.5 to 8.5.
[0022] According to the catalyst of the present invention, the mass ratio Ti / V of titanium element in the first coating calculated as Ti to vanadium element in the first coating calculated as V is1 may be 7 to 8.5:1, for example, 7:1, 7.1:1, 7.2:1, 7.3:1, 7.4:1, 7.5:1, 7.6:1, 7.7:1, 7.8:1, 7.9:1, 8:1, 8.1:1, 8.2:1, 8.3:1, 8.4:1, or 8.5:1.
[0023] According to the catalyst of the present invention, the mass ratio Ti / V of titanium element calculated as Ti in the second coating to vanadium element calculated as V in the second coating is 2 is 12~15.5:1, for example, 12:1, 12.1:1, 12.2:1, 12.3:1, 12.4:1, 12.5:1, 12.6:1, 12.7:1, 12.8:1, 12.9:1, 13:1, 13.1:1, 13.2:1, 13.3:1, 13.4:1, 13.5:1, 13.6:1, 13. It may be 7:1, 13.8:1, 13.9:1, 14:1, 14.1:1, 14.2:1, 14.3:1, 14.4:1, 14.5:1, 14.6:1, 14.7:1, 14.8:1, 14.9:1, 15:1, 15.1:1, 15.2:1, 15.3:1, 15.4:1, or 15.5:1.
[0024] According to the catalyst of the present invention, the content C of titanium element calculated as Ti in the first coating Ti 1 may be within a range of 40% by mass to 60% by mass, for example, 40, 41, 42, 43, 44, 45, 46, 47, 48, 49, 50, 51, 52, 53, 54, 55, 56, 57, 58, 59, or 60%. Preferably, the content C of titanium element in terms of Ti in the first coating is Ti 1 is in the range of 45 to 55 mass %.
[0025] According to the catalyst of the present invention, the content C of titanium element calculated as Ti in the second coating Ti 2may be in the range of 45 to 65 mass%, for example, 45, 46, 47, 48, 49, 50, 51, 52, 53, 54, 55, 56, 57, 58, 59, 60, 61, 62, 63, 64, or 65%. Preferably, the content C of titanium element in terms of Ti in the second coating Ti 2 may be in the range of 50 to 60 mass %.
[0026] In the present invention, the mass ratio of titanium element to vanadium element in the first coating and the second coating (i.e., mass ratio of Ti / V) is measured by scanning electron microscope-energy spectrometer, and the specific test method is as follows: After cooling the catalyst particle with liquid nitrogen, cut it along the longitudinal direction from the side without coating to obtain a catalyst semi-particle with an exposed cross section, fix the catalyst semi-particle to a conductive tape, and coat its surface with gold, platinum or carbon to improve its conductivity to obtain a test sample. The test sample is placed on the sample stage of the scanning electron microscope, and the cross section of the catalyst semi-particle is observed by the scanning electron microscope, and the mass ratio of Ti / V at various thicknesses of the coating (also called "longitudinal direction") is measured by the energy spectrometer. Here, the measurement method of the mass ratio of Ti / V at the same coating thickness is as follows: Three adjacent points along the horizontal direction of the coating (i.e., a direction perpendicular or nearly perpendicular to the thickness direction of the coating) are randomly selected, magnified by the same factor (generally 500 to 1000 times), and the mass ratio of Ti / V at the points is measured by an energy spectrometer. The values measured at the three points are averaged to obtain the mass ratio of Ti / V in the horizontal direction. In the present invention, the first coating and the second coating are distinguished according to the difference in the mass ratio of Ti / V between two adjacent points along the thickness direction of the coating. If the difference in the mass ratio of Ti / V between the two adjacent points is within the range of ΔTi / V defined in the present invention, the two points belong to the first coating and the second coating, respectively, and if the difference in the mass ratio of Ti / V between the two adjacent points is below the range of ΔTi / V defined in the present invention (including the two end points), the two points belong to the same coating.
[0027] According to the catalyst of the present invention, the catalytically active component coating may further contain a trace amount of an adjustment element. In one preferred embodiment, the catalytically active component coating further contains at least one element selected from the group consisting of VA group nonmetal elements, alkali metal elements, and auxiliary metal elements, and the auxiliary metal elements are at least one selected from the group consisting of rare earth elements, VIB group elements, VIII group elements, IIIA group metal elements, VA group metal elements, and IVB group elements other than titanium element.
[0028] According to the catalyst of the present invention, the Group VA non-metallic element is preferably phosphorus (P). In the first coating, the content of the Group VA non-metallic element in elemental terms is 0.1-0.5 mass%, preferably 0.3-0.4 mass%. According to the catalyst of the present invention, the second coating may contain the Group VA non-metallic element or may not contain the Group VA non-metallic element. Preferably, the second coating does not contain the Group VA non-metallic element.
[0029] According to the catalyst of the present invention, the alkali metal element is preferably cesium (Cs). In the first coating, the content of the alkali metal element in elemental terms may be 0.1-0.3 mass%, preferably 0.15-0.2 mass%. In the second coating, the content of the alkali metal element in elemental terms may be 0.1-0.7 mass%, preferably 0.3-0.5 mass%.
[0030] According to the catalyst of the present invention, specific examples of the auxiliary metal element include at least one selected from the group consisting of rubidium (Rb), cerium (Ce), niobium (Nb), chromium (Cr), tungsten (W), silver (Ag), cobalt (Co), gallium (Ga), indium (In), antimony (Sb), bismuth (Bi), zirconium (Zr), and erbium (Er), but are not limited thereto. In one preferred embodiment, the auxiliary metal element is at least one selected from the group consisting of niobium, zirconium, and antimony.
[0031] According to the catalyst of the present invention, the content of the auxiliary metal element in the first coating calculated as an oxide may be 1-6 mass%, but is preferably 1.5-5 mass%, more preferably 2-4.5%, and even more preferably 3-4 mass%. In one preferred embodiment, the auxiliary metal elements in the first coating are niobium, zirconium, and antimony. In this preferred embodiment, the content of the niobium element-containing compound in the first coating calculated as Nb2O5 may be 0.15-0.2 mass%, the content of the zirconium element-containing compound in the first coating calculated as ZrO2 may be 0.4-0.45 mass%, and the content of the antimony element-containing compound in the first coating calculated as Sb2O3 may be 2.8-3.2 mass%.
[0032] In the second coating, the content of the auxiliary metal element calculated as an oxide may be 1 to 6 mass%, preferably 1.2 to 5%, and more preferably 1.5 to 3%. In one preferred embodiment, the auxiliary metal element in the second coating is niobium and antimony. In this preferred embodiment, the content of the niobium element-containing compound calculated as Nb2O5 in the second coating may be 0.12 to 0.18 mass%, and the content of the antimony element-containing compound calculated as Sb2O3 in the second coating may be 1.5 to 2 mass%.
[0033] In the present invention, the amounts of titanium, Group VA non-metallic elements, alkali metal elements, and auxiliary metal elements in the coating are calculated based on the total amount (in oxide terms) of the raw materials forming the coating, which do not include the dispersion medium.
[0034] According to the catalyst of the present invention, the first coating is closer to the support than the second coating, i.e., the first coating is closer to the surface of the support than the second coating. In one preferred embodiment, the second coating is attached to the surface of the first coating. In one more preferred embodiment, the second coating is attached to the surface of the first coating, and the first coating is attached to the surface of the support. In this more preferred embodiment, the second coating is exposed to the environment as an outer coating, and the first coating connects the support and the second coating as an inner coating.
[0035] According to the catalyst of the present invention, the weight ratio of the first coating, the second coating, and the support may be 5.5-6.8:1.9-3.5:100, but is preferably 5.8-6.7:1.9-2.9:100.
[0036] According to the catalyst of the present invention, the total pore volume of the catalyst is 0.03 to 0.08 mL / g.
[0037] In the present invention, the total catalytic pore volume is measured by the BET specific surface method.
[0038] According to the catalyst of the present invention, the support is used to support a catalytically active coating, and the support is an inert inorganic support, which may be at least one selected from the group consisting of alumina, talc, silicon carbide, aluminum silicate, quartz, and ceramics.
[0039] According to the catalyst of the present invention, the shape of the catalyst may be cylindrical, spherical, annular, or granular. Preferably, the shape of the catalyst is annular. In one preferred embodiment, the catalyst is annular, and the outer diameter of the catalyst (i.e., the diameter of the outer ring) may be 3 to 13 mm, for example, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, or 13 mm. Preferably, the outer diameter of the catalyst is 5 to 9 mm. In this preferred embodiment, the thickness of the catalyst (i.e., the difference between the diameter of the outer ring and the diameter of the inner ring / 2) is 0.1 to 10 mm, preferably 0.1 to 5 mm, and more preferably 1 to 3 mm. In this preferred embodiment, the height of the catalyst may be 2 to 12 mm, for example, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, or 12 mm, but is preferably 3 to 8 mm.
[0040] According to a second aspect of the present invention, there is provided a process for the preparation of a catalyst for the gas phase oxidation of 1,2,4,5-tetraalkylbenzenes, comprising the steps of: (1) applying a first slurry containing a first dispersing medium, a first vanadium source, and a first titanium source to a surface of a support to form a first coating; and (2) applying a second slurry containing a second dispersing medium, a second vanadium source, a second titanium source, and a pore expander onto the first coated surface of the carrier to form a second coating.
[0041] According to the method of the present invention, the mass of the vanadium source introduced into the first coating is calculated as V and is C V 12 The mass of the titanium source introduced into the first coating in terms of Ti is C Ti 12 The mass of the vanadium source introduced into the second coating in terms of V is C V 22 The mass of the titanium source introduced into the second coating in terms of Ti is C Ti 22 Then, Ti / V 12 =C Ti 12 / C V 12 , Ti / V22 =C Ti 22 / C V 22 , Ti / V 22 = Ti / V 12 +ΔTi / V 2 and ΔTi / V 2 is in the range of 3 to 9. Specifically, ΔTi / V 2 may be 3, 3.1, 3.2, 3.3, 3.4, 3.5, 3.6, 3.7, 3.8, 3.9, 4, 4.1, 4.2, 4.3, 4.4, 4.5, 4.6, 4.7, 4.8, 4.9, 5, 5.1, 5.2, 5.3, 5.4, 5.5, 5.6, 5.7, 5.8, 5.9, 6, 6.1, 6.2, 6.3, 6.4, 6.5, 6.6, 6.7, 6.8, 6.9, 7, 7.1, 7.2, 7.3, 7.4, 7.5, 7.6, 7.7, 7.8, 7.9, 8, 8.1, 8.2, 8.3, 8.4, 8.5, 8.6, 8.7, 8.8, 8.9, or 9. Preferably, ΔTi / V 2 is in the range of 3.5 to 8.5.
[0042] According to the method for preparing the catalyst of the present invention, the content C of the titanium source in terms of Ti introduced into the first coating is Ti 12 may be in the range of 40% by mass to 60% by mass, for example, 40, 41, 42, 43, 44, 45, 46, 47, 48, 49, 50, 51, 52, 53, 54, 55, 56, 57, 58, 59, or 60% by mass. Preferably, the content C of titanium element in terms of Ti introduced into the first coating is Ti 12 is in the range of 45 to 55 mass %.
[0043] According to the catalyst of the present invention, the content C of the titanium source introduced into the second coating in terms of Ti Ti 22 may be in the range of 45 to 65 mass%, for example 45, 46, 47, 48, 49, 50, 51, 52, 53, 54, 55, 56, 57, 58, 59, 60, 61, 62, 63, 64, or 65%. Preferably, the content C of titanium element, calculated as Ti, introduced into the second coating is Ti22 is in the range of 50 to 60 mass %.
[0044] According to the catalyst preparation method of the present invention, the first vanadium source and the second vanadium source may be the same or different. The first vanadium source and the second vanadium source may each independently be at least one selected from the group consisting of ammonium metavanadate, vanadium pentoxide, and sodium vanadate. Preferably, the first vanadium source and the second vanadium source are ammonium metavanadate.
[0045] According to the catalyst preparation method of the present invention, the first titanium source and the second titanium source may be the same or different. The first titanium source and the second titanium source may each independently be titanium dioxide and / or a precursor of titanium dioxide. In one preferred embodiment, the first titanium source and the second titanium source each independently are at least one selected from the group consisting of titanium dioxide and metatitanic acid. The titanium dioxide is preferably anatase type TiO2. The specific surface area of the anatase type TiO2 is 10 to 30 m 2 / g.
[0046] According to the method for preparing a catalyst of the present invention, the mass ratio of titanium element (calculated as Ti) introduced into the first coating to vanadium element (calculated as V) introduced into the first coating is Ti / V 12 may be 7 to 8.5:1, for example, 7:1, 7.1:1, 7.2:1, 7.3:1, 7.4:1, 7.5:1, 7.6:1, 7.7:1, 7.8:1, 7.9:1, 8:1, 8.1:1, 8.2:1, 8.3:1, 8.4:1, or 8.5:1.
[0047] According to the method for preparing a catalyst of the present invention, the mass ratio Ti / V of titanium element (calculated as Ti) introduced into the second coating to vanadium element (calculated as V) introduced into the second coating is 22is 12~15.5:1, for example, 12:1, 12.1:1, 12.2:1, 12.3:1, 12.4:1, 12.5:1, 12.6:1, 12.7:1, 12.8:1, 12.9:1, 13:1, 13.1:1, 13.2:1, 13.3:1, 13.4:1, 13.5:1, 13.6:1, 13. It may be 7:1, 13.8:1, 13.9:1, 14:1, 14.1:1, 14.2:1, 14.3:1, 14.4:1, 14.5:1, 14.6:1, 14.7:1, 14.8:1, 14.9:1, 15:1, 15.1:1, 15.2:1, 15.3:1, 15.4:1, or 15.5:1.
[0048] According to the catalyst preparation method of the present invention, the first slurry and the second slurry may each independently comprise at least one selected from the group consisting of a compound containing a non-metallic element of Group VA, a compound containing an alkali metal element, and a compound containing an auxiliary metal element, whereby the first coating and the second coating each independently comprise at least one selected from the group consisting of a compound containing a non-metallic element of Group VA, a compound containing an alkali metal element, and a compound containing an auxiliary metal element. The auxiliary metal element is at least one selected from the group consisting of a rare earth element, a group VIB element, a group VIII element, a group IIIA metal element, a group VA metal element, and a group IVB element other than titanium element. In one embodiment, the first slurry contains a compound containing a non-metallic element of Group VA, a compound containing an alkali metal element, and a compound containing an auxiliary metal element. The second slurry contains a compound containing an alkali metal element, a compound containing an auxiliary metal element, and a compound containing any non-metallic element of Group VA.
[0049] According to the catalyst preparation method of the present invention, the Group VA nonmetallic element is preferably phosphorus (P). Preferably, the compound containing the Group VA nonmetallic element is at least one selected from the group consisting of ammonium dihydrogen phosphate, triammonium phosphate, and phosphorus pentoxide. The content of the compound containing the Group VA nonmetallic element introduced into the first coating in elemental terms may be 0.1-0.5 mass %, but is preferably 0.3-0.4 mass %. According to the catalyst preparation method of the present invention, the second coating may contain a compound containing a Group VA nonmetallic element, or may not contain a compound containing a Group VA nonmetallic element. The second slurry may contain a Group VA nonmetallic element, or may not contain a Group VA nonmetallic element. Preferably, the second slurry does not contain a Group VA nonmetallic element.
[0050] According to the catalyst preparation method of the present invention, the alkali metal element is preferably cesium (Cs). Preferably, the compound containing an alkali metal element is at least one selected from the group consisting of MNO3, M2SO4, MCl, and M2CO3, where M is an alkali metal element. The content of the compound containing an alkali metal element in elemental conversion introduced into the first coating may be 0.1-0.3 mass%, more preferably 0.15-0.2 mass%. The content of the compound containing an alkali metal element in elemental conversion introduced into the second coating may be 0.1-0.7 mass%, more preferably 0.3-0.5 mass%.
[0051] According to the catalyst preparation method of the present invention, specific examples of the auxiliary metal element may include at least one selected from the group consisting of rubidium (Rb), cerium (Ce), niobium (Nb), chromium (Cr), tungsten (W), silver (Ag), cobalt (Co), gallium (Ga), indium (In), antimony (Sb), bismuth (Bi), zirconium (Zr), and erbium (Er), but are not limited thereto. In one preferred embodiment, the auxiliary metal element is at least one selected from the group consisting of niobium, zirconium, and antimony. Preferably, the compound containing the auxiliary metal element is at least one selected from the group consisting of an oxide of the auxiliary metal and a water-soluble salt containing the auxiliary metal. The water-soluble metal salt refers to a substance having a solubility in water of 1 g / 100 g water or more, and may be at least one selected from the group consisting of nitrates, carbonates, sulfates, oxalates, and chlorides.
[0052] According to the catalyst preparation method of the present invention, the content of the compound containing the auxiliary metal element in terms of oxide introduced into the first coating may be 1 to 6 mass%, but is preferably 1.5 to 5 mass%, more preferably 2 to 4.5 mass%, and even more preferably 3 to 4 mass%. The content of the compound containing the auxiliary metal element in terms of oxide introduced into the second coating may be 1 to 6 mass%, but is preferably 1.2 to 5 mass%, and more preferably 1.5 to 3 mass%.
[0053] According to the catalyst preparation method of the present invention, in one preferred embodiment, the auxiliary metal elements in the first slurry are niobium, zirconium, and antimony. In this preferred embodiment, the content of the niobium element-containing compound in terms of Nb2O5 introduced into the first coating may be 0.15-0.2 mass%, the content of the zirconium element-containing compound in terms of ZrO2 introduced into the first coating may be 0.4-0.45 mass%, and the content of the antimony element-containing compound in terms of Sb2O3 introduced into the first coating may be 2.8-3.2 mass%.
[0054] According to the catalyst preparation method of the present invention, in one preferred embodiment, the auxiliary metal elements in the second coating are niobium and antimony. In this preferred embodiment, the content of the niobium element-containing compound calculated as Nb2O5 introduced into the second coating may be 0.12-0.18 mass%, and the content of the antimony element-containing compound calculated as Sb2O3 introduced into the second coating may be 1.5-2 mass%.
[0055] In the preparation method of the catalyst of the present invention, the content of each element introduced into the first coating and the second coating is calculated by the input amount and is calculated based on the total amount (in oxide equivalent) of the raw materials forming the coating, the raw materials not containing the dispersion medium.
[0056] According to the catalyst preparation method of the present invention, the first slurry and the second slurry may each independently contain oxalic acid, and the mass ratio of the oxalic acid to the vanadium source in the first slurry and the second slurry may each be 2 to 2.5:1.
[0057] According to the catalyst preparation method of the present invention, the first slurry and the second slurry may each independently contain a binder. The binder is at least one selected from the group consisting of vinyl acetate-acrylate copolymer emulsion, vinyl acetate-ethylene copolymer emulsion, vinyl acetate-maleic acid ester copolymer emulsion, and acrylic acid-maleic acid copolymer emulsion. Based on the total amount of the first slurry, the content of the binder may be 4 to 4.3 mass %. In the second slurry, the content of the binder may be 4.3 to 4.6 mass %.
[0058] According to the catalyst preparation method of the present invention, the second slurry contains a pore expander. The pore expander may be at least one selected from the group consisting of stearic acid and sodium stearate. Based on the total amount of the second slurry, the content of the pore expander may be 3.9 to 4.2 mass %. According to the catalyst preparation method of the present invention, the first slurry preferably does not contain a pore expander.
[0059] According to the catalyst preparation method of the present invention, the first dispersion medium and the second dispersion medium each independently contain water and an aqueous organic solvent. Preferably, the aqueous organic solvent is at least one selected from the group consisting of methanol, ethanol, formamide, and N,N-dimethylamide. According to the catalyst preparation method of the present invention, the mass ratio of water to aqueous organic solvent in the first dispersion medium and the second dispersion medium each independently may be 1:0.1-1, but is preferably 1:0.3-0.8, and more preferably 1:0.4-0.7.
[0060] According to the method for preparing a catalyst of the present invention, the first slurry and the second slurry can be obtained by uniformly mixing the components.
[0061] In one embodiment, the first slurry may be prepared by a method comprising the following steps.
[0062] (1-1) Mixture A is obtained by mixing oxalic acid, a vanadium source, a compound containing a Group VA non-metallic element, a compound containing an alkali metal element, and a first dispersion medium.
[0063] (1-2) The mixed solution A is mixed with a titanium source, a compound containing an auxiliary metal element, and a binder to obtain a first slurry.
[0064] The mixing in step (1-1) and step (1-2) may each be performed at a temperature of 20 to 90° C. The mixing in step (1-2) may be performed in a ball mill, and the ball milling time may be 1 to 5 hours, but is preferably 2 to 4 hours.
[0065] In one embodiment, the second slurry may be prepared by a method comprising the following steps.
[0066] (2-1) Mixture B is obtained by mixing oxalic acid, a vanadium source, an arbitrary compound containing a Group VA nonmetallic element, a compound containing an alkali metal element, and a first dispersion medium.
[0067] (2-2) The mixed solution B is mixed with a titanium source, a compound containing an auxiliary metal element, and a binder to obtain a second slurry.
[0068] The mixing in step (2-1) and step (2-2) may each be carried out at a temperature of 20 to 90° C. The mixing in step (2-2) may be carried out in a ball mill, and the ball milling time may be 1 to 5 hours, but is preferably 2 to 4 hours.
[0069] According to the catalyst preparation method of the present invention, the carrier is an inert inorganic carrier and may be at least one selected from the group consisting of alumina, talc, silicon carbide, aluminum silicate, quartz, and ceramics. According to the catalyst preparation method of the present invention, the shape of the carrier may be cylindrical, spherical, annular, or granular. Preferably, the shape of the carrier is annular. In one preferred embodiment, the carrier is an annular carrier, and the outer diameter of the carrier (i.e., the diameter of the outer ring) may be 3 to 13 mm, for example, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, or 13 mm. Preferably, the outer diameter of the carrier is 5 to 9 mm. In this preferred embodiment, the wall thickness of the carrier (i.e., the difference between the diameter of the outer ring and the diameter of the inner ring / 2) is 0.1 to 10 mm, preferably 0.1 to 5 mm, and more preferably 1 to 3 mm. In this preferred embodiment, the height of the carrier may be 2-12 mm, for example 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, or 12 mm, but is preferably 3-8 mm.
[0070] According to the method for preparing the catalyst of the present invention, the weight ratio of the first coating, the second coating, and the support may be 5.5-6.8:1.9-3.5:100, but is preferably 5.8-6.7:1.9-2.9:100.
[0071] According to the catalyst preparation method of the present invention, the coating temperature of the first slurry is higher than the coating temperature of the second slurry. In the present invention, the coating temperature refers to the temperature of the support at the time of spraying. Preferably, when the coating temperature of the first slurry is T1 and the coating temperature of the second slurry is T2, T1-T2 (the difference between T1 and T2) is within the range of 70 to 150°C, preferably within the range of 80 to 120°C, more preferably within the range of 85 to 105°C. In one preferred embodiment, the coating temperature of the first slurry may be 200 to 250°C, for example, 200, 205, 210, 215, 220, 225, 230, 235, 240, 245, or 250°C. In another preferred embodiment, the coating temperature of the second slurry may be 100 to 130°C, for example, 100, 105, 110, 115, 120, 125, or 130°C.
[0072] According to the method for preparing the catalyst of the present invention, the first slurry layer formed on the surface of the carrier by a conventional method may be cured to form the first coating. In the present invention, the term "curing" refers to the slurry layer losing fluidity and changing from a liquid to a solid. In one embodiment, the first slurry layer may be dried with a first airflow to form the first coating. The temperature of the first airflow is such that the first slurry layer can lose fluidity to form a coating. The temperature of the first airflow may be 200 to 250°C, for example, 200, 205, 210, 215, 220, 225, 230, 235, 240, 245, or 250°C.
[0073] According to the method for preparing the catalyst of the present invention, the second slurry is applied onto the surface on which the first coating is formed to form a second slurry layer, and after the application is completed, the second coating may be formed by directly purging with a purge gas, or the second coating may be formed by first drying with a second airflow and then purging with a purge airflow. The temperature of the purge airflow may be preferably 380-450°C, for example, 380, 385, 400, 405, 410, 415, 420, 425, 430, 435, 440, 445, or 450°C. The temperature of the second airflow may be preferably 100-150°C, for example, 100, 105, 110, 115, 120, 125, 130, 135, 140, 145, or 150°C.
[0074] According to the catalyst preparation method of the present invention, the first slurry and the second slurry may be applied onto the carrier by a conventional method. In one embodiment, the first slurry and the second slurry are applied onto the carrier by spraying. In this embodiment, the spraying speed of the first slurry and the second slurry per 2000 g of carrier may be independently 30 to 60 mL / min, for example, 30 mL / min, 35 mL / min, 40 mL / min, 45 mL / min, 50 mL / min, 55 mL / min, or 60 mL / min, but is preferably 35 to 50 mL / min.
[0075] The spraying may be performed by a common spraying device. As an example, the spraying device may include a hot air blower, a coating body, an exhaust fan, a slurry spraying system, a control system, and a high-power power cabinet. The coating body may include a coating drum and its power mechanism, and the coating drum is housed in the coating body and the rotation speed is adjustable. The coating drum adopts a horizontal hollow columnar structure, which can increase the probability of contact between the active ingredient and the inactive carrier material. The horizontal hollow columnar structure is perforated with a round mesh with a hole diameter of 1 to 8 mm, preferably a round mesh with a hole diameter of 3 to 4 mm, so that hot air can be put into the coating drum, and after evaporating the solvent in the slurry on the carrier, the volatilized solvent is removed from the coating drum, and the rotation speed of the coating drum is preferably 5 to 10 rpm. The slurry spraying system includes a nozzle and a supply system, and the supply system includes a tank, an agitator, a supply pump, and a transport pipeline. The feed pump can adjust the spray speed, and the nozzle is used to spray the slurry fed by the feed pump evenly onto the surface of the carrier.
[0076] According to a third aspect of the invention, the present invention provides a catalyst prepared by the method according to the second aspect of the invention.
[0077] The catalyst prepared by the method according to the second aspect of the present invention comprises a support and a catalytically active component coating supported on the support, the catalytically active component coating comprising a first coating and a second coating, the first coating being close to a surface of the support and the second coating being distant from the surface of the support, wherein the mass ratio of titanium element calculated as Ti to vanadium element calculated as V in the first coating is Ti / V 1 The mass ratio of titanium element (calculated as Ti) to vanadium element (calculated as V) in the second coating is Ti / V 2 Then, Ti / V 2 = Ti / V 1 +ΔTi / V, where ΔTi / V is within the range of 3 to 9. Preferably, ΔTi / V is within the range of 3.5 to 8.5.
[0078] According to a fourth aspect of the present invention, there is provided the use of a catalyst according to the first aspect of the present invention, or a catalyst according to the third aspect of the present invention, as a catalyst for the preparation of 1,2,4,5-benzenetetracarboxylic acid anhydride by oxidation of 1,2,4,5-tetraalkylbenzene.
[0079] The 1,2,4,5-tetraalkylbenzene is preferably 1,2,4,5-tetramethylbenzene (ie, durene).
[0080] According to a fifth aspect of the present invention there is provided a process for the preparation of 1,2,4,5-benzenetetracarboxylic anhydride comprising contacting a gas comprising 1,2,4,5-tetraalkylbenzene and oxygen gas with a catalyst according to the first or third aspect of the present invention to obtain a product stream comprising 1,2,4,5-benzenetetracarboxylic anhydride.
[0081] According to the preparation method of 1,2,4,5-benzenetetracarboxylic anhydride of the present invention, the 1,2,4,5-tetraalkylbenzene is preferably 1,2,4,5-tetramethylbenzene (ie, durene).
[0082] According to the method for preparing 1,2,4,5-benzenetetracarboxylic anhydride of the present invention, the concentration of 1,2,4,5-tetraalkylbenzene is 1 to 50 g / m 3 However, preferably, the thickness is 10 to 30 g / m 3 The concentration of 1,2,4,5-tetraalkylbenzene refers to the grams of 1,2,4,5-tetraalkylbenzene contained in a unit volume of gas containing oxygen gas, and the higher the value, the higher the durene content in the gas containing oxygen gas.
[0083] According to the method for preparing 1,2,4,5-benzenetetracarboxylic anhydride of the present invention, the temperature at which the raw material mixed gas comes into contact with the catalyst may be 300 to 400°C, preferably 320 to 360°C, and more preferably 330 to 350°C.
[0084] According to the preparation method of 1,2,4,5-benzenetetracarboxylic anhydride of the present invention, the mixed gas of raw materials containing 1,2,4,5-tetraalkylbenzene and oxygen gas may be carried out in a general reactor. In one embodiment, the reactor is a fluidized bed reactor. In one preferred embodiment, the reactor is a fixed bed reactor. In a more preferred embodiment, the reactor is a fixed bed single tube reactor. In this more preferred embodiment, the fixed bed single tube reactor may have a tube length of 3000 to 4800 mm and an inner diameter of 20 to 30 mm. The outside of the reaction tube of the fixed bed single tube reactor may be forcibly exchanged for reaction heat by circulating a molten salt. In this preferred embodiment, the catalyst may be a single stage (i.e., one stage of catalyst is packed in the reaction tube of the fixed bed single tube reactor) or two or more stages (i.e., two or more stages of catalyst are packed in the reaction tube of the fixed bed single tube reactor).
[0085] According to the method for preparing 1,2,4,5-benzenetetracarboxylic anhydride of the present invention, the volumetric space velocity of the gas containing oxygen gas is 1500 to 5000 h -1 However, it is preferable that the time is 2000 to 4000 h. -1 It is.
[0086] The present invention will now be described in detail with reference to examples, but the scope of the present invention is not limited thereto.
[0087] In the following examples and comparative examples, the mass ratio of titanium element to vanadium element (Ti / V) in the first coating and the second coating of the catalyst is 1 and Ti / V 2) is measured by a scanning electron microscope (HITACHI-4800) equipped with an energy spectrometer (EDAX GENESIS XM2 SYSTEM 60x), and the test method is specifically as follows. The test is performed under the same test conditions as the scanning electron microscope by an EDAX energy spectrometer (TEAM Octane Super), and the catalyst particles are cooled with liquid nitrogen, then cut along the longitudinal direction from the side without the coating to obtain a catalyst semi-particle with an exposed cross section, and the catalyst semi-particle is fixed to a conductive tape, and its surface is coated with gold, platinum or carbon to improve its conductivity, to obtain a test sample. The test sample is placed on the sample stage of the scanning electron microscope, and the cross section of the catalyst semi-particle is observed with the scanning electron microscope, and the mass ratio of Ti / V at various thicknesses of the coating (also called the "longitudinal direction") is measured using an energy spectrometer. Here, the measurement method of the mass ratio of Ti / V at the same coating thickness is as follows. Three adjacent points along the horizontal direction of the coating (i.e., perpendicular or nearly perpendicular to the coating thickness direction) are randomly selected, and the images are magnified by the same factor (generally 500 to 1000 times), and the mass ratio of Ti / V, vanadium content, and titanium content at the points are measured by an energy spectrometer, and the values measured at the three points are averaged to obtain the mass ratio of Ti / V in the horizontal direction. The first coating and the second coating are distinguished according to the difference in the mass ratio of Ti / V between two adjacent points along the thickness direction of the coating. If the difference in the mass ratio of Ti / V between the two adjacent points is within the range of ΔTi / V defined in the present invention, the two points belong to the first coating and the second coating, respectively, and if the difference in the mass ratio of Ti / V between the two adjacent points is below the range of ΔTi / V defined in the present invention (including the two end point values), the two points belong to the same coating. As for the test conditions of the energy spectrometer, the excitation source is a high-energy electron beam with an energy of 15 kv.
[0088] In the following examples and comparative examples, the total pore volume of the catalyst is measured by BET specific surface method using a fully automatic chemical adsorption analyzer manufactured by Micromeritics, Inc., USA, and the specific test method is as follows: A certain amount of sample is placed in a sample tube, heated to 350°C at 10°C / min, and vacuum-suctioned for 4 hours to degas the sample tube, then the sample tube is placed in an analyzer to perform pore isothermal SEM analysis, and the specific surface area of the catalyst is calculated by BET method.
[0089] In the following Examples and Comparative Examples, the preparation of the slurry is carried out at room temperature (25° C.).
[0090] In the following examples and comparative examples, the titanium dioxide is anatase type titanium dioxide having a specific surface area of 20 to 30 m 2 / g.
[0091] Examples 1 to 4 prepare catalysts according to the present invention. Example 1
[0092] 1. Preparation of the first slurry (1-i) 123.23 g of ammonium metavanadate, 275.36 g of oxalic acid, 2.11 g of cesium sulfate, 10.23 g of ammonium dihydrogen phosphate, formamide, and 350 g of water were mixed to prepare a solution A-1 having a formamide to water weight ratio of 0.7:1. (1-ii) Solution A-1 was placed in a ball mill together with 630 g of titanium dioxide, 6.12 g of niobium oxalate, 7.24 g of zirconium sulfate, and 23.1 g of antimony trioxide, and then 70 g of vinyl acetate / ethylene copolymer emulsion was added thereto and ball milled for 4 hours to obtain a first slurry. 2. Preparation of the second slurry (2-i) 69.82 g of ammonium metavanadate, 161.3 g of oxalic acid, 4.57 g of cesium sulfate, formamide, and 350 g of water were mixed to prepare a solution B-1 having a formamide to water weight ratio of 0.7:1. (2-ii) Solution B-1 was placed in a ball mill together with 630 g of titanium dioxide, 4.86 g of niobium oxalate, 13.96 g of antimony trioxide, and 63 g of stearic acid, and then 70 g of vinyl acetate / ethylene copolymer emulsion was added and ball milled for 4 hours to obtain a second slurry. 3. Preparation of catalyst (1-iii) 2000g of carrier ceramic ring (outer diameter 8mm, height 6mm, thickness 1.5mm, material talc ring) was placed in a drum, and the drum speed was controlled at 10rpm. The first slurry was placed in the stirring can of the liquid material spraying system and stirred. The hot air blower was started to pass 100℃ hot air through the drum to preheat the carrier ceramic ring, and when the temperature of the carrier ceramic ring reached 210℃, the supply nozzle was opened, the spraying speed of the first slurry was controlled at 30mL / min, and the first slurry was sprayed from the nozzle onto the surface of the carrier and quickly dried with 220℃ hot air. When the content of the inner coating reached 6.2wt% of the weight of the carrier, the spraying was completed to obtain a catalyst intermediate. (2-iii) The second slurry was placed in the stirring can of the liquid material spraying system and stirred. The hot air blower was started to pass 100°C hot air through the drum, and when the temperature of the support reached 120°C, the supply nozzle was opened, the spraying speed of the second slurry was controlled to 30mL / min, and the second slurry was sprayed from the nozzle onto the surface of the catalyst intermediate and quickly dried with 120°C hot air. When the content of the outer coating reached 2.3wt% of the weight of the support, the spraying was completed and purged with 400°C hot air for 2h to obtain catalyst S1. The composition and total pore volume of this catalyst are shown in Table 1. Catalyst S1 included a support and a first coating (i.e., inner coating) and a second coating (i.e., outer coating) sequentially supported on the support, and in catalyst S1, the weight ratio of the first coating, the second coating, and the support was 6.2:2.3:100. Example 2
[0093] 1. Preparation of the first slurry (1-i) 123.23 g of ammonium metavanadate, 275.36 g of oxalic acid, 2.11 g of cesium sulfate, 10.23 g of ammonium dihydrogen phosphate, formamide, and 350 g of water were mixed to prepare a solution A-1 having a formamide to water weight ratio of 0.7:1. (1-ii) Solution A-1 was placed in a ball mill together with 630 g of titanium dioxide, 6.12 g of niobium oxalate, 7.24 g of zirconium sulfate, and 23.1 g of antimony trioxide, and then 70 g of vinyl acetate / ethylene copolymer emulsion was added and ball milled for 4 hours to obtain a first slurry. 2. Preparation of the second slurry (2-i) 57.31 g of ammonium metavanadate, 123.89 g of oxalic acid, 3.77 g of cesium sulfate, formamide, and 350 g of water were mixed to prepare a solution B-2 having a formamide to water weight ratio of 0.7:1. (2-ii) Solution B-2 was placed in a ball mill together with 630 g of titanium dioxide, 3.92 g of niobium oxalate, 11.29 g of antimony trioxide, and 63 g of stearic acid, and then 70 g of vinyl acetate / ethylene copolymer emulsion was added and ball milled for 4 hours to obtain a second slurry. 3. Preparation of catalyst (1-iii) 2000g of carrier ceramic ring (outer diameter 8mm, height 6mm, thickness 1.5mm, material talc ring) was placed in a drum, and the drum speed was controlled at 10rpm. The first slurry was placed in the stirring can of the liquid material spraying system and stirred. The hot air blower was started to pass 100℃ hot air through the drum to preheat the carrier ceramic ring, and when the temperature of the carrier ceramic ring reached 210℃, the supply nozzle was opened, the spraying speed of the first slurry was controlled at 30mL / min, and the first slurry was sprayed from the nozzle onto the surface of the carrier and quickly dried with 220℃ hot air. When the content of the inner coating reached 5.8wt% of the weight of the carrier, the spraying was completed to obtain a catalyst intermediate. (2-iii) The second slurry was placed in the stirring can of the liquid material spraying system and stirred. The hot air blower was started to pass 100°C hot air through the drum, and when the temperature of the support reached 120°C, the supply nozzle was opened, the spraying speed of the second slurry was controlled to 30mL / min, and the second slurry was sprayed from the nozzle onto the surface of the catalyst intermediate and quickly dried with 120°C hot air. When the content of the outer coating reached 1.9wt% of the weight of the support, the spraying was completed and purged with 400°C hot air for 2h to obtain catalyst S2. The composition and total pore volume of this catalyst are shown in Table 1. Catalyst S2 included a support and a first coating (i.e., inner coating) and a second coating (i.e., outer coating) sequentially supported on the support, and in catalyst S2, the weight ratio of the first coating, the second coating, and the support was 5.8:1.9:100. Example 3
[0094] 1. Preparation of the first slurry (1-i) 102.55 g of ammonium metavanadate, 230.27 g of oxalic acid, 1.72 g of cesium sulfate, 8.76 g of ammonium dihydrogen phosphate, formamide, and 350 g of water were mixed to prepare a solution A-3 having a formamide to water weight ratio of 0.7:1. (1-ii) Solution A-3 was placed in a ball mill together with 630 g of titanium dioxide, 5.83 g of niobium oxalate, 7.15 g of zirconium sulfate, and 21.8 g of antimony trioxide, and then 70 g of vinyl acetate / ethylene copolymer emulsion was added and ball milled for 4 hours to obtain a first slurry. 2. Preparation of the second slurry (2-i) 69.82 g of ammonium metavanadate, 161.3 g of oxalic acid, 4.57 g of cesium sulfate, formamide, and 350 g of water were mixed to prepare a solution B-1 having a formamide to water weight ratio of 0.7:1. (2-ii) Solution B-1 was placed in a ball mill together with 630 g of titanium dioxide, 4.86 g of niobium oxalate, 13.96 g of antimony trioxide, and 63 g of stearic acid, and then 70 g of vinyl acetate / ethylene copolymer emulsion was added and ball milled for 4 hours to obtain a second slurry. 3. Preparation of catalyst (1-iii) 2000g of carrier ceramic ring (outer diameter 8mm, height 6mm, thickness 1.5mm, material talc ring) was placed in a drum, and the drum speed was controlled at 10rpm. The first slurry was placed in the stirring can of the liquid material spraying system and stirred. The hot air blower was started to pass 100℃ hot air through the drum to preheat the carrier ceramic ring, and when the temperature of the carrier ceramic ring reached 210℃, the supply nozzle was opened, the spraying speed of the first slurry was controlled at 30mL / min, and the first slurry was sprayed from the nozzle onto the surface of the carrier and quickly dried with 220℃ hot air. When the content of the inner coating reached 6.5wt% of the weight of the carrier, the spraying was completed to obtain a catalyst intermediate. (2-iii) The second slurry was placed in the stirring can of the liquid material spraying system and stirred. The hot air blower was started to pass 100°C hot air through the drum, and when the temperature of the support reached 120°C, the supply nozzle was opened, the spraying speed of the second slurry was controlled to 30mL / min, and the second slurry was sprayed from the nozzle onto the surface of the catalyst intermediate and quickly dried with 120°C hot air. When the content of the outer coating reached 2.7wt% of the weight of the support, the spraying was completed and purged with 400°C hot air for 2h to obtain catalyst S3. The composition and total pore volume of this catalyst are shown in Table 1. Catalyst S3 included a support and a first coating (i.e., inner coating) and a second coating (i.e., outer coating) sequentially supported on the support, and in catalyst S3, the weight ratio of the first coating, the second coating, and the support was 6.5:2.7:100. Example 4
[0095] 1. Preparation of the first slurry (1-i) 102.55 g of ammonium metavanadate, 230.27 g of oxalic acid, 1.72 g of cesium sulfate, 8.76 g of ammonium dihydrogen phosphate, formamide, and 350 g of water were mixed to prepare a solution A-3 having a formamide to water weight ratio of 0.7:1. (1-ii) Solution A-3 was placed in a ball mill together with 630 g of titanium dioxide, 5.83 g of niobium oxalate, 7.15 g of zirconium sulfate, and 21.8 g of antimony trioxide, and then 70 g of vinyl acetate / ethylene copolymer emulsion was added and ball milled for 4 hours to obtain a first slurry. 2. Preparation of the second slurry (2-i) 57.31 g of ammonium metavanadate, 123.89 g of oxalic acid, 3.77 g of cesium sulfate, formamide, and 350 g of water were mixed to prepare a solution B-2 having a formamide to water weight ratio of 0.7:1. (2-ii) Solution B-2 was placed in a ball mill together with 630 g of titanium dioxide, 3.92 g of niobium oxalate, 11.29 g of antimony trioxide, and 63 g of stearic acid, and then 70 g of vinyl acetate / ethylene copolymer emulsion was added and ball milled for 4 hours to obtain a second slurry. 3. Preparation of catalyst (1-iii) 2000g of carrier ceramic ring (outer diameter 8mm, height 6mm, thickness 1.5mm, material talc ring) was placed in a drum, and the drum speed was controlled at 10rpm. The first slurry was placed in the stirring can of the liquid material spraying system and stirred. The hot air blower was started to pass 100℃ hot air through the drum to preheat the carrier ceramic ring, and when the temperature of the carrier ceramic ring reached 210℃, the supply nozzle was opened, the spraying speed of the first slurry was controlled at 30mL / min, and the first slurry was sprayed from the nozzle onto the surface of the carrier and quickly dried with 220℃ hot air. When the content of the inner coating reached 6.7wt% of the weight of the carrier, the spraying was completed to obtain a catalyst intermediate. (2-iii) The second slurry was placed in the stirring can of the liquid material spraying system and stirred. The hot air blower was started to pass 100°C hot air through the drum, and when the temperature of the support reached 120°C, the supply nozzle was opened, the spraying speed of the second slurry was controlled to 30mL / min, and the second slurry was sprayed from the nozzle onto the surface of the catalyst intermediate and quickly dried with 120°C hot air. When the content of the outer coating reached 1.9wt% of the weight of the support, the spraying was completed and purged with 450°C hot air for 2h to obtain catalyst S4. The composition and total pore volume of this catalyst are shown in Table 1. Catalyst S4 included a support and a first coating (i.e., inner coating) and a second coating (i.e., outer coating) sequentially supported on the support, and in catalyst S4, the weight ratio of the first coating, the second coating, and the support was 6.7:1.9:100. Comparative Example 1
[0096] In Comparative Example 1, the catalyst was prepared by the same method as in Example 1, except that the second slurry was not prepared and the prepared catalyst did not contain the second coating. The specific operation is as follows: The first slurry was prepared by the same method as in Example 1, and 2000g of the carrier ceramic ring (similar to Example 1) was placed in a drum, and the drum speed was controlled at 10 rpm. The first slurry was placed in the stirring can of the liquid material spraying system and stirred. The hot air blower was started to pass 100°C hot air through the drum to preheat the carrier ceramic ring, and when the temperature of the carrier ceramic ring reached 210°C, the supply nozzle was opened, the spraying speed of the first slurry was controlled at 30mL / min, and the first slurry was sprayed from the nozzle onto the surface of the carrier and quickly dried with 220°C hot air. When the content of the inner coating reached 8.3wt% of the weight of the carrier, the spraying was completed to obtain catalyst DS1. Catalyst DS1 included a support and a coating carried on the support, and in catalyst DS1 the weight ratio of the coating to the support was 8.3:100. Comparative Example 2
[0097] In Comparative Example 2, the first slurry was not prepared, and the catalyst prepared did not contain the first coating. The catalyst was prepared by the same method as in Example 1, except that the second slurry prepared by the same method as in Example 1 was directly sprayed onto the surface of the carrier to form a coating. The specific operation is as follows: The second slurry was prepared by the same method as in Example 1, 2000g of the carrier ceramic ring (similar to Example 1) was placed in a drum, the drum speed was controlled at 10 rpm, and the first slurry was placed in the stirring can of the liquid material spraying system and stirred. The hot air blower was started to pass 100°C hot air through the drum to preheat the carrier ceramic ring. When the temperature of the carrier ceramic ring reached 210°C, the supply nozzle was opened, the spraying speed of the first slurry was controlled to 30mL / min, and the first slurry was sprayed onto the surface of the carrier from the nozzle and quickly dried with 220°C hot air. When the content of the inner coating reached 8.8wt% of the weight of the carrier, the spraying was completed to obtain catalyst DS2. Catalyst DS2 included a support and a coating carried on the support, and in catalyst DS2 the weight ratio of the coating to the support was 8.8:100. Comparative Example 3
[0098] In Comparative Example 3, the first slurry was not prepared, and the catalyst prepared did not contain the first coating. The catalyst was prepared by the same method as in Example 2, except that the second slurry prepared by the same method as in Example 2 was directly sprayed onto the surface of the carrier to form a coating. The specific operation is as follows: The second slurry was prepared by the same method as in Example 2, 2000g of the carrier ceramic ring (similar to Example 2) was placed into a drum, the drum speed was controlled at 10 rpm, and the second slurry was placed into the stirring can of the liquid material spraying system and stirred. The hot air blower was started to pass 100°C hot air through the drum to preheat the carrier ceramic ring, and when the temperature of the carrier ceramic ring reached 210°C, the supply nozzle was opened, the spraying speed of the second slurry was controlled at 30mL / min, and the second slurry was sprayed onto the surface of the carrier from the nozzle and quickly dried with 220°C hot air. When the content of the inner coating reached 8.7wt% of the weight of the carrier, the spraying was completed to obtain catalyst DS3. Catalyst DS3 included a support and a coating carried on the support, and in catalyst DS3 the weight ratio of the coating to the support was 8.7:100. Comparative Example 4
[0099] 1. Preparation of the first slurry (1-i) 102.55 g of ammonium metavanadate, 230.27 g of oxalic acid, 1.72 g of cesium sulfate, 8.76 g of ammonium dihydrogen phosphate, formamide, and 350 g of water were mixed to prepare a solution A-3 having a formamide to water weight ratio of 0.7:1. (1-ii) Solution A-3 was placed in a ball mill together with 630 g of titanium dioxide, 5.83 g of niobium oxalate, 7.15 g of zirconium sulfate, and 21.8 g of antimony trioxide, and then 70 g of vinyl acetate / ethylene copolymer emulsion was added and ball milled for 4 hours to obtain a first slurry. 2. Preparation of the second slurry (2-i) 90.28 g of ammonium metavanadate, 218.12 g of oxalic acid, 5.97 g of cesium sulfate, formamide, and 350 g of water were mixed to prepare a solution B-4 having a formamide to water weight ratio of 0.7:1. (2-ii) Solution B-4 was placed in a ball mill together with 630 g of titanium dioxide, 6.51 g of niobium oxalate, 17.85 g of antimony trioxide, and 63 g of stearic acid, and then 70 g of vinyl acetate / ethylene copolymer emulsion was added and ball milled for 4 hours to obtain a second slurry. 3. Preparation of catalyst (1-iii) 2000g of the carrier ceramic ring (same as in Example 3) was placed in a drum, and the drum speed was controlled at 10 rpm. The first slurry was placed in the stirring can of the liquid material spraying system and stirred. The hot air blower was started to pass 100°C hot air through the drum to preheat the carrier ceramic ring, and when the temperature of the carrier ceramic ring reached 210°C, the supply nozzle was opened, the spraying speed of the first slurry was controlled at 30 mL / min, and the first slurry was sprayed from the nozzle onto the surface of the carrier and quickly dried with 220°C hot air. When the content of the inner coating reached 6.8 wt% of the weight of the carrier, the spraying was completed to obtain a catalyst intermediate. (2-iii) The second slurry was placed in the stirring can of the liquid material spraying system and stirred. The hot air blower was started to pass 100°C hot air through the drum, and when the temperature of the support reached 120°C, the supply nozzle was opened, the spraying speed of the second slurry was controlled to 30mL / min, and the second slurry was sprayed from the nozzle onto the surface of the catalyst intermediate and quickly dried with 120°C hot air. When the content of the outer coating reached 1.9wt% of the weight of the support, the spraying was completed and purged with 400°C hot air for 2h to obtain catalyst DS4. The composition and total pore volume of this catalyst are shown in Table 1. Catalyst DS4 included a support and a first coating and a second coating supported on the support in sequence, and in catalyst DS4, the weight ratio of the first coating, the second coating, and the support was 6.8:1.9:100. Comparative Example 5
[0100] 1. Preparation of the first slurry (1-i) 102.55 g of ammonium metavanadate, 230.27 g of oxalic acid, 1.72 g of cesium sulfate, 8.76 g of ammonium dihydrogen phosphate, formamide, and 350 g of water were mixed to prepare a solution A-3 having a formamide to water weight ratio of 0.7:1. (1-ii) Solution A-3 was placed in a ball mill together with 630 g of titanium dioxide, 5.83 g of niobium oxalate, 7.15 g of zirconium sulfate, and 21.8 g of antimony trioxide, and then 70 g of vinyl acetate / ethylene copolymer emulsion was added and ball milled for 4 hours to obtain a first slurry. 2. Preparation of the second slurry (2-i) 40.19 g of ammonium metavanadate, 84.32 g of oxalic acid, 2.33 g of cesium sulfate, formamide, and 350 g of water were mixed to prepare a solution B-5 having a formamide to water weight ratio of 0.7:1. (2-ii) Solution B-5 was placed in a ball mill together with 630 g of titanium dioxide, 2.48 g of niobium oxalate, 7.32 g of antimony trioxide, and 63 g of stearic acid, and then 70 g of vinyl acetate / ethylene copolymer emulsion was added and ball milled for 4 hours to obtain a second slurry. 3. Preparation of catalyst (1-iii) 2000g of the carrier ceramic ring (same as in Example 3) was placed in a drum, and the drum speed was controlled at 10 rpm. The first slurry was placed in the stirring can of the liquid material spraying system and stirred. The hot air blower was started to pass 100°C hot air through the drum to preheat the carrier ceramic ring, and when the temperature of the carrier ceramic ring reached 210°C, the supply nozzle was opened, the spraying speed of the first slurry was controlled at 30 mL / min, and the first slurry was sprayed from the nozzle onto the surface of the carrier and quickly dried with 220°C hot air. When the content of the inner coating reached 6.9 wt% of the weight of the carrier, the spraying was completed to obtain a catalyst intermediate. (2-iii) The second slurry was placed in the stirring can of the liquid material spraying system and stirred. The hot air blower was started to pass 100°C hot air through the drum, and when the temperature of the support reached 120°C, the supply nozzle was opened, the spraying speed of the second slurry was controlled to 30mL / min, and the second slurry was sprayed from the nozzle onto the surface of the catalyst intermediate and quickly dried with 120°C hot air. When the content of the outer coating reached 2.1wt% of the weight of the support, the spraying was completed and purged with 400°C hot air for 2h to obtain catalyst DS5. The composition and total pore volume of this catalyst are shown in Table 1. Catalyst DS5 included a support and a first coating and a second coating supported on the support in sequence, and in catalyst DS5, the weight ratio of the first coating, the second coating, and the support was 6.9:2.1:100. Comparative Example 6
[0101] A catalyst was prepared in the same manner as in Example 1, except that the second slurry was used in step 3 (1-iii) and the first slurry was used in step (2-iii), i.e., the second slurry was used to form the first coating (i.e., the inner coating) and the first slurry was used to form the second coating (i.e., the outer coating) to obtain catalyst DS6. The composition and total pore volume of this catalyst are shown in Table 1. Catalyst DS6 includes a support and a first coating (i.e., the inner coating) and a second coating (i.e., the outer coating) sequentially supported on the support, and in catalyst DS6, the weight ratio of the first coating, the second coating, and the support was 6.2:2.3:100.
[0102] [Table 1]
[0103] 1: Mass ratio of titanium / vanadium in the first coating (Ti / V 1 ) and the mass ratio of titanium / vanadium in the second coating (Ti / V 2 ) was measured by scanning electron microscopy-energy spectroscopy and the Ti / V 1is the mass ratio of titanium element (converted into Ti) to vanadium element (converted into V) in the first coating, Ti / V 2 is the mass ratio of titanium element (converted into Ti) to vanadium element (converted into V) in the second coating, Ti / V 2 = Ti / V 1 +ΔTi / V.
[0104] 2: The contents of titanium (Ti), phosphorus (P), cesium (Cs) and auxiliary agents are calculated based on the input amounts and are calculated based on the total amount of raw materials forming the coating (in oxide terms), which do not include the dispersion medium, the titanium (Ti) content is in elemental titanium terms, the phosphorus (P) content is in P terms, the cesium (Cs) content is in Cs terms, and the auxiliary agents content is in oxide terms. Test Examples and Comparative Test Examples
[0105] The catalytic performance was evaluated using a fixed-bed single-tube reactor simulating industrial production conditions. The fixed-bed single-tube reactor had an inner diameter of 29 mm and a tube length of 4,400 mm, and heat transfer was performed by circulating molten salt on the outside of the reaction tube. The outlet of the reactor was connected to an analysis system and a reaction product collection system. The catalyst adopts a single-stage (i.e., one stage of a single tube) or two-stage (i.e., two stages of a single tube) packing method, and the total catalyst packing height is 2000 mm. When packing in two stages, the first stage is packed at the inlet end of the reaction tube, and the second stage is packed at the outlet end of the reaction tube, with the packing height of the first stage being 1200 mm and the packing height of the second stage being 800 mm. In the test examples and comparative test examples, the catalysts were activated in an oxidizing atmosphere at a temperature of 410° C. for 4 hours before the reaction.
[0106] In the test examples and the comparative test examples, the gas phase oxidation reaction method was the same, the reaction pressure was normal pressure (i.e., 1 standard atmospheric pressure), air was used as the oxygen-containing gas, and the space velocity of air was 2000 h -1During the reaction, the feed concentration of durene was gradually increased, and sampling analysis was performed at the outlet of the reactor under each condition to evaluate the durene conversion and the pyromellitic dianhydride yield at the maximum catalyst load (i.e., the maximum feed concentration of durene, i.e., the durene concentration shown in Table 2), and at the molten salt temperature and maximum load shown in Table 2. The test results are shown in Table 2.
[0107] [Table 2]
[0108] Comparing Test Example 1, Test Comparative Example 1, and Test Comparative Example 2, it was found that Test Example 1 can effectively improve the yield of pyromellitic dianhydride by using the catalyst on which the first coating and second coating of the present invention are formed, compared to forming a single layer of catalytically active coating on the surface of the carrier. Comparing Test Example 1 and Test Comparative Example 6, it was found that forming the first coating and second coating on the surface of the carrier using the method of the present invention is effective in improving the yield of pyromellitic dianhydride.
[0109] Comparing Test Example 3, Test Example 4 and Test Example 5, it was found that controlling the mass ratio of the titanium content calculated as Ti and the vanadium content calculated as V in the first coating and the second coating within the range defined in the present invention can effectively improve the catalytic activity and obtain a significantly improved selectivity for pyromellitic dianhydride.
[0110] Comparing Test Example 5 with Test Comparative Example 3, it can be seen that when two stages of catalysts are packed in one reaction tube, the catalyst according to the present invention can not only operate at a higher durene concentration, but also improve the conversion rate of durene and the selectivity of pyromellitic dianhydride.
Claims
1. A catalyst for the gas phase oxidation of 1,2,4,5-tetraalkylbenzene, comprising: The present invention comprises a carrier and a catalytically active component coating supported on the carrier, the catalytically active component coating comprising a first coating and a second coating, the first coating being close to a surface of the carrier and the second coating being distant from the surface of the carrier, the first coating and the second coating each independently containing vanadium element and titanium element, and a mass ratio of titanium element calculated as Ti to vanadium element calculated as V in the first coating is Ti / V. 1 The mass ratio of titanium element calculated as Ti to vanadium element calculated as V in the second coating is Ti / V 2 Then, Ti / V 2 = Ti / V 1 +ΔTi / V, where ΔTi / V is in the range of 3 to 9.
2. a mass ratio Ti / V of titanium element in the first coating calculated as Ti to vanadium element in the first coating calculated as V; 1 The catalyst of claim 1, wherein the molar ratio is 7-8.5:
1.
3. a mass ratio Ti / V of titanium element in the second coating calculated as Ti to vanadium element in the second coating calculated as V; 2 The catalyst of claim 1, wherein the molar ratio is 12-15.5:
1.
4. The content C of titanium element in the first coating calculated as Ti Ti 1 is in the range of 40 to 60% by weight, and / or The content C of titanium element in the second coating calculated as Ti Ti 2 The catalyst according to any one of claims 1 to 3, wherein the content of the catalyst is in the range of 45 to 65 mass%.
5. The catalytically active component coating further contains at least one selected from the group consisting of a Group VA non-metallic element, an alkali metal element, and an auxiliary metal element, the auxiliary metal element being at least one selected from the group consisting of a rare earth element, a Group VIB element, a Group VIII element, a Group IIIA metal element, a Group VA metal element, and a Group IVB element other than titanium; Preferably, the Group VA non-metallic element is phosphorus; Preferably, the alkali metal element is cesium; The catalyst according to any one of claims 1 to 4, wherein the auxiliary metal element is at least one selected from the group consisting of niobium, zirconium, and antimony.
6. the second coating is applied to a surface of the first coating; The catalyst according to any one of claims 1 to 5, wherein the first coating is preferably applied to a surface of the support.
7. The catalyst according to any one of claims 1 to 6, wherein the total pore volume of the catalyst is from 0.03 to 0.08 mL / g.
8. The catalyst according to any one of claims 1 to 7, wherein the support is at least one selected from the group consisting of alumina, talc, silicon carbide, aluminum silicate, quartz, and ceramics.
9. A process for preparing a catalyst for the gas phase oxidation of 1,2,4,5-tetraalkylbenzene, comprising the steps of: (1) applying a first slurry containing a first dispersing medium, a first vanadium source, and a first titanium source to a surface of a support to form a first coating; (2) applying a second slurry containing a second dispersing medium, a second vanadium source, a second titanium source, and a pore expander onto the first coated surface of the carrier to form a second coating; The mass of the vanadium source introduced into the first coating in terms of V is C V 12The mass of the titanium source introduced into the first coating in terms of Ti is C Ti 12 The mass of the vanadium source introduced into the second coating in terms of V is C V 22 The mass of the titanium source introduced into the second coating is expressed as Ti. Ti 22 Then, Ti / V 12 = C Ti 12 / C V 12 , Ti / V 22 = C Ti 22 / C V 22 , Ti / V 22 = Ti / V 12 +ΔTi / V 2 and ΔTi / V 2 is in the range of 3 to 9.
10. The content C of the titanium source introduced into the first coating in terms of Ti Ti 12 is in the range of 40 to 60 mass %; or The content C of the titanium source introduced into the second coating in terms of Ti Ti 22 The method according to claim 9, wherein the content of the cellulose acetate layer is in the range of 45 to 65% by weight.
11. the first vanadium source and the second vanadium source are each independently at least one selected from the group consisting of ammonium metavanadate, vanadium pentoxide, and sodium vanadate; Preferably, the first titanium source and the second titanium source are each independently at least one selected from the group consisting of titanium dioxide and metatitanic acid; The method according to claim 9 or 10, wherein the support is at least one selected from the group consisting of alumina, talc, silicon carbide, aluminum silicate, quartz, and ceramics.
12. The method according to any one of claims 9 to 11, wherein the weight ratio of the first coating, the second coating and the carrier is 5.5-6.8:1.9-3.5:
100.
13. the first slurry further contains at least one compound selected from the group consisting of a compound containing a Group VA non-metallic element, a compound containing an alkali metal element, and a compound containing an auxiliary metal element, the auxiliary metal element being at least one element selected from the group consisting of a rare earth element, a Group VIB element, a Group VIII element, a Group IIIA metal element, a Group VA metal element, and a Group IVB element other than titanium; Preferably, the content of the compound containing a Group VA non-metallic element introduced into the first coating is 0.1 to 0.5 mass % in terms of element; Preferably, the content of the compound containing an alkali metal element introduced into the first coating is 0.1 to 0.3 mass% in terms of element, Preferably, the content of the compound containing the auxiliary metal element introduced into the first coating is 1 to 6 mass % in terms of oxide, Preferably, the VA group non-metallic element is phosphorus, the alkali metal element is cesium, and the auxiliary metal element is at least one element selected from the group consisting of niobium, zirconium, and antimony; Preferably, the compound containing a Group VA nonmetallic element is at least one selected from the group consisting of ammonium dihydrogen phosphate, triammonium phosphate, and phosphorus pentoxide; Preferably, the compound containing an alkali metal element is MNO 3 , M. 2 SO 4 , MCl, and M 2 CO 3 wherein M is an alkali metal element; Preferably, the compound containing the auxiliary metal element is at least one selected from the group consisting of an oxide of the auxiliary metal and a water-soluble salt containing the auxiliary metal. The method according to any one of claims 9 to 12.
14. the second slurry further contains a compound containing an alkali metal element, a compound containing an auxiliary metal element, and a compound containing any Group VA non-metallic element, the auxiliary metal element being at least one selected from the group consisting of rare earth elements, Group VIB elements, Group VIII elements, Group IIIA metal elements, Group VA metal elements, and Group IVB elements other than titanium; Preferably, the content of the compound containing an alkali metal element introduced into the second coating is 0.1 to 0.7 mass% in terms of element, Preferably, the content of the compound containing the auxiliary metal element introduced into the second coating is 1 to 6 mass % in terms of oxide, Preferably, the VA group nonmetallic element is phosphorus, the alkali metal element is cesium, and the auxiliary metal element is at least one selected from the group consisting of niobium, zirconium, and antimony; Preferably, the compound containing a Group VA nonmetallic element is at least one selected from the group consisting of ammonium dihydrogen phosphate, triammonium phosphate, and phosphorus pentoxide; Preferably, the compound containing an alkali metal element is MNO 3 , M. 2 SO 4 , MCl, and M 2 CO 3 wherein M is an alkali metal element; Preferably, the compound containing the auxiliary metal element is at least one selected from the group consisting of an oxide of the auxiliary metal and a water-soluble salt containing the auxiliary metal. The method according to any one of claims 9 to 13.
15. Based on the total amount of the second slurry, the content of the pore expander is 3.9 to 4.2 mass %; The method according to any one of claims 9 to 14, wherein the pore expander is at least one selected from the group consisting of stearic acid and sodium stearate.
16. The application temperature of the first slurry is higher than the application temperature of the second slurry, Preferably, the application temperature of the first slurry is T 1 The application temperature of the second slurry is T 2 Then, T 1 -T 2 is in the range of 70 to 150°C, preferably in the range of 80 to 120°C, more preferably in the range of 85 to 105°C, Preferably, the application temperature of the first slurry is 200 to 250° C.; Preferably, the application temperature of the second slurry is 100 to 130° C.; Preferably, the method of forming the second coating comprises purging the second slurry applied onto the first coated surface of the carrier with a purge airflow, the temperature of the purge airflow being preferably between 380 and 450°C.
17. A catalyst prepared by the method according to any one of claims 9 to 16.
18. 20. Use of the catalyst according to any one of claims 1 to 8 and 17 as a catalyst for the reaction for preparing 1,2,4,5-benzenetetracarboxylic anhydride by oxidation of 1,2,4,5-tetraalkylbenzene.
19. A process for preparing 1,2,4,5-benzenetetracarboxylic anhydride, comprising the steps of:
20. A process for preparing 1,2,4,5-tetraalkylbenzene and oxygen gas comprising contacting a gas with the catalyst of any one of claims 1 to 8 and 17 to obtain a product stream containing 1,2,4,5-benzenetetracarboxylic acid anhydride.
Citation Information
Patent Citations
Catalyst for catalytic oxidation
JP1999104497A
Multilayer shell-type catalyst for gas-phase oxidation of aromatic hydrocarbons
JP2002523232A
Process for the preparation of catalysts for gas-phase oxidation by coating a support material in a fluidized bed apparatus