Process for recovering dialkyl terephthalates from feedstocks - Patents.com
The method addresses the inefficiencies of conventional polyester recycling by using depolymerization and alcoholysis at reduced temperatures to produce high-purity dialkyl terephthalates with reduced energy and resource use, promoting sustainable recycling.
Patent Information
- Application Number
- JP2024525066
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2021-10-25
- Filing Date
- 2022-10-25
- Publication Date
- 2024-10-28
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Conventional glycolysis and methanolysis processes for recycling polyesters require substantial amounts of resources and energy, leading to inefficient production of dialkyl terephthalates.
A method involving depolymerization of a feedstock composition with glycols and a catalyst under controlled conditions, followed by alcoholysis at reduced temperatures to produce high-yield and high-purity dialkyl terephthalates, with the option to reuse glycols in subsequent processes.
The method reduces energy and resource consumption while achieving high purity and yield of dialkyl terephthalates, minimizing side reactions and impurities, and allows for the recycling of glycols, thereby enhancing the efficiency and sustainability of the process.
Smart Images

Figure 2024539305000010 
Figure 2024539305000001 
Figure 2024539305000002
Abstract
Description
[Technical field]
[0001] The present disclosure relates to methods for recycling one or more polyesters in a feedstock composition. More particularly, the present disclosure relates to recovering dialkyl terephthalates from a feedstock composition. [Background technology]
[0002] Certain conventional systems may utilize glycolysis and / or methanolysis processes in an attempt to recycle polyesters, however, certain conventional glycolysis and / or methanolysis processes may require substantial amounts of resources and energy to arrive at a product suitable for use in a subsequent production process, such as a production process to make recycled polyester or other compositions. Summary of the Invention
[0003] In one aspect, a method for recovering one or more dialkyl terephthalates from a feedstock composition is provided. The method may include exposing a feedstock composition including one or more polyesters and one or more contaminants to one or more glycols and a depolymerization catalyst in a first reaction vessel under depolymerization conditions to provide a first mixture. The first mixture may include one or more depolymerization products. The method may also include exposing at least a portion of the first mixture to an alcohol composition and an alcoholysis catalyst under alcoholysis conditions to provide a second mixture. The second mixture may include one or more dialkyl terephthalates. The alcoholysis conditions may include a temperature of 23° C. to 70° C. for 0.5 hours to 10 hours. The method may also include isolating at least a portion of the one or more dialkyl terephthalates from the second mixture. [Brief description of the drawings]
[0004] [Figure 1]1 is an exemplary system for recovering one or more dialkyl terephthalates from a feedstock composition according to an embodiment of the present disclosure. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0005] overview The present disclosure may be more readily understood by reference to the following detailed description of certain aspects and examples of the disclosure. In accordance with the purposes of this disclosure, certain aspects of the disclosure are described in the Summary of the Invention and further described herein below. Other aspects of the disclosure are also described herein.
[0006] Aspects herein relate to methods for recovering one or more dialkyl terephthalates from a feedstock composition. As described herein, an exemplary method may include exposing a feedstock composition to one or more glycols under depolymerization conditions to produce one or more depolymerization products, which are then exposed to an alcoholysis process, followed by isolating the dialkyl terephthalates.
[0007] As discussed above, certain conventional glycolysis and / or methanolysis processes may require substantial amounts of resources and energy to arrive at a product suitable for use in a downstream production process, such as a production process for making recycled polyester or other compositions.
[0008] The methods and systems disclosed herein can alleviate one or more of the above problems. For example, in certain embodiments, the methods disclosed herein can include exposing a polyester composition to depolymerization conditions with one or more glycols to provide one or more depolymerized products. In various embodiments, the one or more depolymerized products can include monomers, oligomers, or combinations thereof. In embodiments, the one or more depolymerized products can be exposed to alcoholysis conditions to obtain high yields and high purity dialkyl terephthalate products. As discussed herein, the alcoholysis conditions include reduced temperatures compared to certain conventional systems, which reduces the overall energy and resources required. In embodiments, as discussed herein, the depolymerization and alcoholysis conditions described herein are substantially milder than certain conventional processes, resulting in less ethylene glycol yield loss, for example, due to fewer side reactions or decomposition reactions that convert ethylene glycol to various impurities. Additionally, in certain embodiments discussed further below, the glycols present in the resulting alcoholysis liquid component can be separated from at least a portion of the alcohol composition utilized in the alcoholysis, and these recycled glycols may be reused in subsequent series of dialkyl terephthalate recovery attempts, again reducing resource consumption.
[0009] Feedstock Composition In various embodiments, the feedstock composition for the processes disclosed herein comprises one or more polyesters and one or more contaminants.
[0010] The term "polyester" may refer to a synthetic polymer prepared by the reaction of one or more difunctional carboxylic acids and / or polyfunctional carboxylic acids with one or more difunctional hydroxyl compounds and / or polyfunctional hydroxyl compounds. The difunctional carboxylic acids may be dicarboxylic acids and the difunctional hydroxyl compounds may be dihydric alcohols such as glycols. Additionally, as used herein, the term "diacid" or "dicarboxylic acid" includes polyfunctional acids such as branching agents. As used herein, the term "glycol" or "diol" includes but is not limited to diols, glycols, and / or polyfunctional hydroxyl compounds. The dicarboxylic acid residue may be derived from a dicarboxylic acid monomer or its associated acid halide, ester, salt, anhydride, or mixtures thereof. Thus, as used herein, the term dicarboxylic acid is intended to include dicarboxylic acids and any derivatives of dicarboxylic acids including their associated acid halides, esters, half esters, salts, half salts, anhydrides, mixed anhydrides, or mixtures thereof that are useful in the reaction process with diols to create polyesters. As used herein, the term "polyester" should be understood to also refer to copolyesters.
[0011] As used herein, the term "residue" refers to a monomeric or repeating unit in a polymer, oligomer, or dimer. For example, a polymer may be made from the condensation of the following monomers: terephthalic acid ("TPA") and cyclohexyl-1,4-dimethanol ("CHDM"). The condensation reaction results in the loss of a water molecule. The residue in the resulting polymer comes from either terephthalic acid or cyclohexyl-1,4-dimethanol. Formula (I) below illustrates a non-limiting example of a polyester.
[0012] [ka] In embodiments, the polyesters exhibit an intrinsic viscosity of from about 0.1 dL / g to about 1.2 dL / g, as determined in accordance with ASTM D2857-70, from about 0.2 dL / g to about 1.2 dL / g, as determined in accordance with ASTM D2857-70, from about 0.3 dL / g to about 1.2 dL / g, as determined in accordance with ASTM D2857-70, or from about 0.4 dL / g to about 1.2 dL / g, as determined in accordance with ASTM D2857-70.
[0013] In various embodiments, the one or more polyesters may include terephthalate polyesters. Terephthalate polyesters are polyesters that include residues of terephthalic acid or any derivative of terephthalic acid, including its associated acid halides, esters, half esters, salts, half salts, anhydrides, mixed anhydrides, and / or mixtures or residues thereof, that are useful in the reaction process with diols to make copolyesters. In various embodiments, the polyester may include polyethylene terephthalate (PET). In one or more embodiments, the polyester may include glycol modified PET. In certain aspects, the polyester may comprise polyethylene terephthalate (PET), 1,4-cyclohexanedimethanol (CHDM) modified PET, isophthalic acid (IPA) modified PET, diethylene glycol (DEG) modified PET, glycol modified PET, neopentyl glycol (NPG) modified PET, propanediol (PDO) modified PET, butanediol (BDO) modified PET, heaxanediol (HDO) modified PET, 2-methyl-2,4-pentanediol (MP diol) modified PET, isosorbide modified PET, poly(tetramethylene ether) glycol (PTMG) modified PET, poly(ethylene) glycol (PEG) modified PET, polycyclohexylene dimethylene terephthalate (PCT), cyclohexanedimethanol (CHDM) containing copolyesters, isosorbide containing copolyesters, or combinations thereof. In the same or alternative embodiment, the polyester composition may include polyethylene terephthalate (PET) containing CHDM, IPA, DEG, NPG, PDO, BDO, HDO, MP diol, isosorbide, PTMG, PEG, or combinations thereof.
[0014] In various embodiments, the polyester may comprise CHDM. In one embodiment, the polyester may comprise from about 0 mol% to about 100 mol% CHDM, from about 1 mol% to about 100 mol% CHDM, from about 1 mol% to about 90 mol% CHDM, from about 1 mol% to about 80 mol% CHDM, from about 1 mol% to about 70% CHDM, from about 1 mol% to about 60 mol% CHDM, from about 1 mol% to about 50 mol% CHDM, from about 1 mol% to about 40 mol% CHDM, from about 1 mol% to about 35 mol% CHDM, from about 1 mol% to about 30 mol% CHDM, from about 1 mol% to about 25 mol% CHDM, from about 1 mol% to about 20 mol% CHDM, from about 1 mol% to about 10 mol% CHDM, or from about 1 mol% to about 5 mol% CHDM. In an embodiment, the mol% of CHDM refers to the mol% of CHDM relative to all diol equivalents in the polyester. In various embodiments, the polyester may include DEG. In embodiments, the polyester may include about 0 mol % to about 100 mol % DEG, about 1 mol % to about 100 mol % DEG, about 1 mol % to about 90 mol % DEG, about 1 mol % to about 80 mol % DEG, about 1 mol % to about 70 mol % DEG, about 1 mol % to about 60 mol % DEG, about 1 mol % to about 50 mol % DEG, about 1 mol % to about 40 mol % DEG, about 1 mol % to about 35 mol % DEG, about 1 mol % to about 30 mol % DEG, about 1 mol % to about 20 mol % DEG, about 1 mol % to about 10 mol % DEG, about 1 mol % to about 5 mol % DEG, or about 1 mol % to about 3 mol % DEG. In embodiments, the mol % of DEG refers to the mol % of DEG relative to all diol equivalents in the polyester. In an embodiment, the polyester may include isophthalic acid. In an embodiment, the polyester may include about 0 mol% to about 30 mol% isophthalic acid, about 1 mol% to about 30 mol% isophthalic acid, about 1 mol% to about 25 mol% isophthalic acid, about 1 mol% to about 20 mol% isophthalic acid, about 1 mol% to about 15 mol% isophthalic acid, about 1 mol% to about 10 mol% isophthalic acid, about 1 mol% to about 7.5 mol% isophthalic acid, about 1 mol% to about 5 mol% isophthalic acid, about 1 mol% to about 3 mol% isophthalic acid, about 10 mol% or less isophthalic acid, about 7.5 mol% or less isophthalic acid, about 5 mol% or less isophthalic acid, or about 3 mol% or less isophthalic acid.In embodiments, the mole % of isophthalic acid refers to the mole % of isophthalic acid relative to the total diacid equivalents in the polyester. In certain embodiments, the polyester may comprise from about 0 mole % to about 100 mole % CHDM, from about 0 mole % to about 100 mole % DEG, from about 0 mole % to about 30 mole % isophthalic acid, or a combination thereof. In certain embodiments, the polyester may comprise from about 1 mole % to about 100 mole % CHDM, from about 1 mole % to about 100 mole % DEG, from about 1 mole % to about 30 mole % isophthalic acid, or a combination thereof. In various embodiments, the polyester may comprise other glycols, such as those other than those mentioned above. For example, in embodiments, the polyester may include, but is not limited to, neopentyl glycol (NPG), 2-methyl-2,4-pentanediol (MP diol), butanediol (BDO), propanediol (PDO), hexanediol (HDO), isosorbide, poly(tetramethylene ether) glycol (PTMG), poly(ethylene) glycol (PEG), or combinations thereof. In certain embodiments, each of NPG, MP diol, BDO, PDO, HDO, isosorbide, PTMG and PEG may be present in the polyester in an amount of 0 mol % to about 100 mol %, about 1 mol % to about 100 mol %, about 1 mol % to about 90 mol %, about 1 mol % to about 80 mol %, about 1 mol % to about 70 mol %, about 1 mol % to about 60 mol %, about 1 mol % to about 50 mol %, about 1 mol % to about 40 mol %, about 1 mol % to about 35 mol %, about 1 mol % to about 30 mol %, about 1 mol % to about 25 mol %, about 1 mol % to about 20 mol %, about 1 mol % to about 10 mol %, or about 1 mol % to about 5 mol %. In embodiments, the mole % of each of NPG, MP diol, BDO, PDO, HDO, isosorbide, PTMG, and PEG refers to the mole % of each of NPG, MP diol, BDO, PDO, HDO, isosorbide, PTMG, and PEG, respectively, relative to the total diol equivalents in the polyester. In various embodiments, the polyester may include CHDM, DEG, NPG, MP diol, BDO, PDO, HDO, isosorbide, PTMG, PEG, isophthalic acid, or combinations thereof, each component being present in any of the amounts for such components described in this paragraph.
[0015] In embodiments, the polyester composition or one or more polyesters present in the polyester composition may be recycled polyester. In various embodiments, recycled polyester may include materials recovered as manufacturing scrap, post-industrial waste, post-consumer waste, or combinations thereof. In embodiments, recycled polyester may be used and / or discarded post-consumer products. In embodiments, the polyester composition and / or recycled polyester may be obtained from various sources and / or in various forms, including, but not limited to, textiles, carpets, thermoforming materials, bottles, pellets, and films.
[0016] In various embodiments, as discussed above, the feedstock composition may include one or more foreign materials. In certain embodiments, the foreign material may be any non-polyester material. In one or more embodiments, the one or more foreign materials may include, but are not limited to, polyesters other than polyethylene terephthalate, polyvinyl chloride (PVC), polyvinyl acetal, polyvinyl butyral (PVB), polyvinyl alcohol (PVOH), ethylene vinyl alcohol (EVOH), cotton, polyolefins, polyethylene, polypropylene, polystyrene, polycarbonate, spandex, natural fibers, cellulose esters, polyacrylates, polymethacrylates, polyamides, nylons, poly(lactic acid), polydimethylsiloxanes, polysilanes, calcium carbonate, titanium dioxide, inorganic fillers, dyes, pigments, color toners, colorants, plasticizers, adhesives, flame retardants, metals, aluminum and iron, or combinations thereof. In various embodiments, the one or more contaminants may be present in the feedstock composition in an amount of from about 0.01 wt.% to about 50 wt.%, from about 0.01 wt.% to about 40 wt.%, from about 0.01 wt.% to about 30 wt.%, from about 0.01 wt.% to about 20 wt.%, from about 0.01 wt.% to about 15 wt.%, from about 0.01 wt.% to about 10 wt.%, from about 0.01 wt.% to about 7.5 wt.%, from about 0.01 wt.% to about 5 wt.%, from about 0.01 wt.% to about 2.5 wt.%, or from about 0.01 wt.% to about 1.0 wt.%, based on the weight of the one or more polyesters in the polyester composition.
[0017] In embodiments, the feedstock composition may be in a solid form, liquid form, melt form, or solution. In certain embodiments, the solution may include one or more polyesters pre-dissolved in a solvent, such as DMT, EG, DEG, TEG, or combinations thereof.
[0018] Optional Pretreatment of the Polyester Composition In certain embodiments, optional treatment of the feedstock composition may be performed prior to glycolysis and / or methanolysis. In various embodiments, the optional pretreatment may include any type of treatment that aids in removing a portion of any contaminants from the feedstock composition and / or aids in recovering one or more polyesters from a mixed feedstock, such as a feedstock containing the contaminants discussed above. For example, in one embodiment, the optional pretreatment may include exposing the feedstock composition to one or more solvents to selectively dissolve the polyesters in the feedstock composition (or at least a portion of the contaminants in the feedstock composition) and allow separation between at least a portion of the contaminants and one or more polyesters in the feedstock composition. In one example embodiment, the optional pretreatment may include exposing the feedstock composition to one or more solvents, such as one or more solvents that can cause dissolution of the polyesters in the feedstock composition. For example, the one or more solvents may include, but are not limited to, 4-methylcyclohexanemethanol (MCHM), ethylene glycol (EG), diethylene glycol (DEG), triethylene glycol (TEG), 1,4-cyclohexanedimethanol (CHDM), poly(ethylene glycol) (PEG), neopentyl glycol (NPG), propanediol (PDO), butanediol (BDO), 2-methyl-2,4-pentanediol (MP diol), poly(tetramethylene ether) glycol (PTMG), dibutyl terephthalate (DBT), dioctyl terephthalate (DOTP), ethylene carbonate (EC), dimethyl carbonate (DMC), dimethyl sulfoxide (DMSO), dimethylformamide (DMF), or combinations thereof. In the same or alternative embodiment, the feedstock composition may be exposed to one or more solvents at a particular temperature to effect dissolution of one or more components. In various embodiments, the pretreatment process may include one or more dissolution and separation steps using various solvents and / or temperatures to achieve a desired level of contaminant removal and / or purity level of PET.For example, in one embodiment, dissolution and separation can be utilized using one solvent at a particular temperature, e.g., to remove one or more contaminants, followed by subsequent dissolution and separation of the polyester fraction using another solvent at a particular temperature, e.g., to remove one or more other contaminants. The dissolution and / or separation in this optional pretreatment step can utilize any suitable system, reactor, vessel, and / or separation technique to achieve the desired pretreated feedstock composition.
[0019] Glycolysis of Feedstock Compositions As discussed above, in various embodiments, the methods disclosed herein may include exposing the feedstock composition to depolymerization conditions to depolymerize at least a portion of the one or more polyesters into one or more depolymerized products. In various embodiments, the one or more depolymerized products may include monomers, oligomers, or combinations thereof. In certain embodiments, the oligomers may exhibit a degree of polymerization of 2-10, 2-8, 2-6, or 2-4. In embodiments, the one or more polyesters may be depolymerized into one or more depolymerized products that may include monomers and terephthalate oligomers having a degree of polymerization of 2-10, 2-8, 2-6, or 2-4. In embodiments, liquid chromatography may be performed to identify the degree of polymerization of the oligomers, and / or gel permeation chromatography may be utilized to identify the molecular weight of the oligomers.
[0020] In an embodiment, the term degree of polymerization (DP) may refer to the number of residues in an oligomer. As used herein, degree of polymerization (DP) refers to the number of difunctional carboxylic acid residues and / or polyfunctional carboxylic acid residues in an oligomer. For example, in one exemplary embodiment, a DP of 1 refers to a residue that contains one terephthalic acid residue or one isophthalic acid residue. In such an exemplary embodiment, a DP of 1 may also be referred to as a monomer. A non-limiting example of a DP of 1 is shown in the following formula (II):
[0021] [ka]
[0028] Formulas (III)-(V) below show non-limiting examples of oligomers having DP's of 2, 3, and n, respectively, in embodiments.
[0022] [ka] In an embodiment, this depolymerization may be carried out via a glycolysis process. In general, in an embodiment, the glycolysis process may include exposing the feedstock composition to one or more glycols, which react with the polyester, optionally in the presence of a transesterification catalyst, to form a mixture of bis(hydroxyethyl) terephthalate (BHET) and low molecular weight terephthalate oligomers. Some representative examples of the glycolysis process are disclosed in U.S. Patent Nos. 3,257,335; 3,907,868; 6,706,843; and 7,462,649, which are incorporated herein by reference.
[0023] In one embodiment of the glycolysis process, one or more polyesters, such as one or more recycled polyesters, and one or more glycols can be fed to a glycolysis reactor, where the one or more recycled polyesters are dissolved and depolymerized under depolymerization conditions.
[0024] In embodiments, any amount of one or more glycols suitable for use in a glycolysis process can be utilized. In various embodiments, the weight ratio of one or more glycols to the amount of polyester composition can be 12:1 to 1:12, 8:1 to 1:9, 6:1 to 1:9, 4:1 to 1:9, 4:1 to 1:7, 4:1 to 1:4, 4:1 to 1:2, 3:1 to 1:9, 3:1 to 1:7, 3:1 to 1:4, 3:1 to 1:2, 2:1 to 1:9, 2:1 to 1:7, 2:1 to 1:4, 2:1 to 1:2, 4:1 to 2:7, 3:1 to 1:4, 3:1 to 1:3, 2:1 to 1:2, 2:1 to 3:7, 1:1 to 3:7, 4:1 to 3:7, 4:1 to 4:7, 4:1 to 5:7, or 3:1 to 3:7.
[0025] In certain embodiments, the one or more glycols may include any glycol suitable for use in the glycolysis process. As used herein, the term "glycol" refers to aliphatic, cycloaliphatic, and aralkyl glycols. Exemplary glycols include ethylene glycol, 1,2-propanediol (also known as propylene glycol), 1,3-propanediol, 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol, 2,2-dimethyl-1,3-propanediol, 1,2-cyclohexanedimethanol, 1,3-cyclohexanedimethanol, 1,4-cyclohexanedimethanol, 2,2,4,4-tetramethyl-1,3-cyclobutanediol, isosorbide, p-xylylenediol, and the like. These glycols may also include ether linkages, such as in the case of diethylene glycol, triethylene glycol, and tetraethylene glycol. Additional embodiments of glycols include the higher molecular weight homologs known as polyethylene glycols, such as those produced by Dow Chemical Company under the trade name Carbowax™. In one embodiment, the polyethylene glycol has a molecular weight of greater than 200 to about 10,000 Daltons (M n ) These glycols also include higher alkyl analogs such as dipropylene glycol, dibutylene glycol, etc. Similarly, additional glycols have molecular weights of about 200 to about 10,000 Daltons (M n) (also referred to as g / mol) range, and higher polyalkylene ether diols such as polypropylene glycol and polytetramethylene glycol. In one aspect, the glycol can be selected from aliphatic, cycloaliphatic and aralkyl glycols. In the same or alternative aspect, the glycol can be selected from polyalkylene ether diols selected from ethylene glycol; 1,2-propanediol; 1,3-propanediol; 1,4-butanediol; 1,5-pentanediol; 1,6-hexanediol; 2,2-dimethyl-1,3-propanediol; 1,2-cyclohexanedimethanol; 1,3-cyclohexanedimethanol; 1,4-cyclohexanedimethanol; 2,2,4,4-tetramethyl-1,3-cyclobutanediol; isosorbide; p-xylylenediol; diethylene glycol; triethylene glycol; tetraethylene glycol; polyethylene glycol; dipropylene glycol; dibutylene glycol; polypropylene glycol and polytetramethylene glycol.
[0026] In various embodiments, the one or more glycols may include ethylene glycol (EG), diethylene glycol (DEG), triethylene glycol (TEG), 1,4-cyclohexanedimethanol (CHDM), poly(ethylene glycol) (PEG), neopentyl glycol (NPG), propanediol (PDO), butanediol (BDO), 2-methyl-2,4-pentanediol (MP diol), poly(tetramethylene ether) glycol (PTMG), or combinations thereof. In one embodiment, the one or more glycols may include about 0 wt.% to about 100 wt.% EG, or about 1 wt.% to about 100 wt.% EG, based on the total weight of the one or more glycols. In certain embodiments, the one or more glycols may include about 0 wt.% to about 100 wt.% DEG, or about 1 wt.% to about 100 wt.% DEG, based on the total weight of the one or more glycols. In certain embodiments, the one or more glycols may comprise about 0 wt.% to about 100 wt.% TEG, or about 1 wt.% to about 100 wt.% TEG, based on the total weight of the one or more glycols. In certain embodiments, the one or more glycols may comprise about 0 wt.% to about 100 wt.% PEG, or about 1 wt.% to about 100 wt.% PEG, based on the total weight of the one or more glycols. In certain embodiments, the one or more glycols may comprise about 0 wt.% to about 100 wt.% NPG, or about 1 wt.% to about 100 wt.% NPG, based on the total weight of the one or more glycols. In certain embodiments, the one or more glycols may comprise about 0 wt.% to about 100 wt.% PDO, or about 1 wt.% to about 100 wt.% PDO, based on the total weight of the one or more glycols. In certain embodiments, the one or more glycols may comprise from about 0 wt.% to about 100 wt.% BDO, or from about 1 wt.% to about 100 wt.% BDO, based on the total weight of the one or more glycols. In certain embodiments, the one or more glycols may comprise from about 0 wt.% to about 100 wt.% MP diol, or from about 1 wt.% to about 100 wt.% MP diol, based on the total weight of the one or more glycols.In certain embodiments, the one or more glycols may comprise from about 0 wt.% to about 100 wt.% PTMG, or from about 1 wt.% to about 100 wt.% PTMG, based on the total weight of the one or more glycols. In embodiments, the one or more glycols may comprise from about 0 wt.% to about 50 wt.% CHDM, or from about 1 wt.% to about 50 wt.% CHDM, based on the total weight of the one or more glycols. In one embodiment, the one or more glycols may include 0 wt.% to about 100 wt.% EG, 0 wt.% to about 100 wt.% DEG, 0 wt.% to about 100 wt.% TEG, 0 wt.% to about 100 wt.% PEG, 0 wt.% to about 100 wt.% NPG, 0 wt.% to about 100 wt.% PDO, 0 wt.% to about 100 wt.% BDO, 0 wt.% to about 100 wt.% MP diol, 0 wt.% to about 100 wt.% PTMG, and 0 wt.% to about 50 wt.% CHDM, based on the total weight of the one or more glycols. In one embodiment, the one or more glycols may include 1 wt.% to about 100 wt.% EG, 1 wt.% to about 100 wt.% DEG, 1 wt.% to about 100 wt.% TEG, 1 wt.% to about 100 wt.% PEG, 1 wt.% to about 100 wt.% NPG, 1 wt.% to about 100 wt.% PDO, 1 wt.% to about 100 wt.% BDO, 1 wt.% to about 100 wt.% MP diol, 1 wt.% to about 100 wt.% PTMG, and 1 wt.% to about 50 wt.% CHDM, based on the total weight of the one or more glycols. In certain embodiments, as discussed in detail below, the one or more glycols may be recycled glycols recovered from prior glycolysis and methanolysis processes to recover one or more dialkyl terephthalates, as disclosed herein.
[0027] In various embodiments, as discussed above, the glycolysis process may include one or more catalysts, such as a transesterification catalyst. In certain embodiments, the catalyst may be present in an amount of 0.1 wt.% to 10 wt.% based on the weight of the polyester composition. In embodiments, any suitable catalyst may be utilized. In one embodiment, the catalyst may include a carbonate catalyst, such as, but not limited to, Li2CO3, K2CO3, Na2CO3, Cs2CO3, ZrCO3, or combinations thereof. In one embodiment, the catalyst may include a hydroxide catalyst, such as, but not limited to, LiOH, NaOH, KOH, tetrabutylammonium hydroxide (TBAH), or combinations thereof. In one embodiment, the catalyst may include an alkoxide catalyst, such as, but not limited to, sodium methoxide (NaOMe), lithium methoxide (LiOMe), magnesium methoxide, potassium t-butoxide, ethylene glycol monosodium salt, ethylene glycol disodium salt, or combinations thereof. In one embodiment, the catalyst may include tetraisopropyl titanate (TIPT), butyltin tris-2-ethylhexanoate (FASCAT 4102), 1,8-diazabicyclo[5.4.0]undec-7-ene (DBU), zinc acetylacetonate hydrate (Zn(acac)2), zinc acetate (Zn(OAc)2), and manganese(II) acetate (Mn(OAc)2)), or combinations thereof. In certain embodiments, the catalyst may include LiOH, NaOH, KOH, tetraisopropyl titanate (TIPT), butyltin tris-2-ethylhexanoate (FASCAT 4102), ZrCO3, 1,8-diazabicyclo[5.4.0]undec-7-ene (DBU), sodium methoxide (NaOMe), lithium methoxide (LiOMe), and zinc acetylacetonate hydrate (Zn(acac)2), or combinations thereof. In one embodiment, the catalyst may include LiOH, NaOH, KOH, sodium methoxide (NaOMe), and lithium methoxide (LiOMe).In certain embodiments, the catalyst may include Li2CO3, K2CO3, CaCO3, Na2CO3, Cs2CO3, ZrCO3, LiOH, NaOH, KOH, tetrabutylammonium hydroxide (TBAH), sodium methoxide (NaOMe), lithium methoxide (LiOMe), magnesium methoxide (Mg(OMe)2, potassium t-butoxide, ethylene glycol monosodium salt, ethylene glycol disodium salt, tetraisopropyl titanate (TIPT), butyltin tris-2-ethylhexanoate (FASCAT 4102), 1,8-diazabicyclo[5.4.0]undec-7-ene (DBU), zinc acetylacetonate hydrate (Zn(acac)2), zinc acetate (Zn(OAc)2), manganese(II) acetate (Mn(OAc)2), hydrotalcite, zeolite, lithium chloride, or combinations thereof.
[0028] Depolymerization conditions may include temperatures of 150°C to 260°C for 0.5 hours to 10 hours in an agitated reactor and absolute pressures of 1 atmosphere (atm) to 15 atm, or 1 atm to 2 atm. Higher temperatures may be used to increase the rate of depolymerization, but may require a reactor system capable of withstanding high pressures. One or more reactors may be used to react the polyester with one or more glycols. For example, the reaction mixture may be continuously withdrawn from a first stage and introduced, along with additional glycol, into a second stage maintained under pressure, where depolymerization continues to the desired degree of completion. In various embodiments, any type of vessel, reactor, and / or reactor system may be utilized for the depolymerization or glycolysis of the polyester composition. In one embodiment, a continuous stirred tank reactor or vessel, a fixed bed reactor, or a melt extruder. In the same or alternative embodiments, the depolymerization or glycolysis of the polyester composition may be a batch or continuous process.
[0029] In various embodiments, by exposing the feedstock composition to the depolymerization conditions described herein, one or more components in the feedstock composition, such as one or more contaminants, may melt and / or form a gel-like layer in the reaction vessel and may float on or near the top of the solvent or glycol in the reaction vessel. In one exemplary embodiment, contaminants including polyolefins, polyethylene, polypropylene, polystyrene, or combinations thereof may float on or near the top of the solvent or glycol in the reaction vessel under the depolymerization conditions described herein. In such embodiments, these contaminants may be removed from the glycolysis reaction vessel using any suitable removal process, for example, via a pump or other process.
[0030] As discussed further below, the liquid component is further subjected to at least a methanolysis process to recover one or more dialkyl terephthalates. In various embodiments, prior to exposing the mixture resulting from the depolymerization or glycolysis process to the alcoholysis process described below, the resulting mixture may be optionally cooled to a temperature of about 150° C. or less, or from about 50° C. to about 150° C. In embodiments, the resulting mixture may be cooled to the desired temperature in the glycolysis reactor or transferred to a different vessel to reduce the temperature. Alcoholysis of one or more of the depolymerization products As discussed above, in embodiments, one or more depolymerized products produced in the glycolysis process described above may be subjected to an alcoholysis process. In certain embodiments, the glycolysis process may result in a first mixture that may include one or more depolymerized products, such as monomers and / or oligomers having a degree of polymerization of 2 to 10, along with one or more glycols, catalysts, at least a portion of the foreign matter, or combinations thereof. In one embodiment, the first mixture from the glycolysis process may be subjected to the alcoholysis process without a separation process.
[0031] Generally, in a typical alcoholysis process, a polyester is reacted with an alcohol, such as methanol, to produce a depolymerized mixture that includes oligomers, terephthalate monomers, such as dimethyl terephthalate (DMT), and one or more glycols. In other embodiments, depending on the composition of the polyester, other monomers may also be produced, such as, for example, CHDM, DEG, and dimethyl isophthalate (DMI). In one embodiment, during the alcoholysis process, terephthalate oligomers are reacted with methanol to produce a depolymerized polyester mixture that includes polyester oligomers, DMT, CHDM, and / or EG.
[0032] Some representative examples of the methanolysis of PET are described in U.S. Patent Nos. 3,321,510; 3,776,945; 5,051,528; 5,298,530; 5,414,022; 5,432,203; 5,576,456; and 6,262,294, which are incorporated herein by reference.
[0033] In an embodiment, the alcoholysis process may include exposing a first mixture containing one or more depolymerization products obtained from the glycolysis process to an alcohol composition under conditions that produce one or more dialkyl terephthalates. As discussed above, in an embodiment, the one or more depolymerization products may be present in a liquid component obtained from the glycolysis process. Without being bound to any particular theory, it is believed that because the glycolysis process is carried out using a smaller amount of glycol (or a weight ratio of glycol to the amount of polyester composition of 3:1 to 1:9) compared to certain conventional processes, this allows the liquid component obtained from the glycolysis process to be directly utilized in the alcoholysis process, for example, without requiring further processing to concentrate the one or more depolymerization products obtained and / or remove a portion of the glycol.
[0034] The alcohol composition may comprise any suitable alcohol known in the art for use in an alcoholysis process to obtain a particular dialkyl terephthalate. In one embodiment, the alcohol composition may be methanol. In an embodiment, when methanol is utilized as the alcohol composition, it may be the methanolysis product that results in DMT.
[0035] In certain embodiments, the amount of the alcohol composition may be any amount that is in excess by weight relative to the amount or weight of the polyester composition. In certain embodiments, the weight ratio of the amount of the alcohol composition to the amount of the polyester composition may be from about 2:1 to about 10:1. In such embodiments, the amount of the polyester composition refers to the amount or weight of the polyester composition utilized in the glycolysis process described above.
[0036] In embodiments, the alcoholysis reaction may be carried out at a temperature of about 90° C. or less, about 80° C. or less, about 70° C. or less, about 60° C. or less, about 50° C. or less, about 40° C. or less, or about 30° C. or less. In the same or alternative embodiments, the alcoholysis reaction may be carried out at a temperature of about 20° C. to about 90° C., about 20° C. to about 80° C., about 20° C. to about 70° C., about 20° C. to about 60° C., about 20° C. to about 50° C., about 20° C. to about 40° C., or about 20° C. to about 30° C. In various embodiments, without being bound by any particular theory, it is believed that in the methods disclosed herein, because the polyester in the polyester composition has already undergone at least a partial depolymerization process, for example, in the glycolysis step discussed above, the methanolysis process can be carried out at a relatively reduced temperature as compared to certain other conventional processes. Additionally or alternatively, without being bound to any particular theory, it is believed that the alcoholysis process can be carried out at the reduced temperatures described above because one or more depolymerized products produced in the glycolysis process are separated from waste or insoluble materials prior to the alcoholysis process.
[0037] In embodiments, the alcoholysis process may be carried out in any suitable reactor and / or vessel. In embodiments, the alcoholysis reactor may be in fluid communication with the reactor utilized in the glycolysis process described above. In certain embodiments, the alcoholysis reactor is a different reactor than the vessel used for glycolysis. Alternatively, in various embodiments, the alcoholysis process may be carried out in the same vessel as the glycolysis process and / or filtration process described above. In certain embodiments, the alcoholysis process may be carried out at ambient pressure, e.g., about 1 atm, or about 1 atm to about 5 atm, or about 1 atm to about 3 atm. In various embodiments, the alcoholysis reaction may be carried out at pressures above ambient pressure, e.g., greater than 1 atm, or about 5 atm or less, about 3 atm or less, when the alcoholysis reaction temperature is high relative to the process conditions disclosed herein, e.g., about 50° C. or more, about 60° C. or more, about 70° C. or more, about 80° C. or more, or about 90° C. or more.
[0038] In various embodiments, an alcoholysis catalyst can be utilized in the alcoholysis process. In embodiments, the alcoholysis catalyst may be present in an amount of about 0.1 wt.% to about 20 wt.% based on the weight of the polyester composition, or about 0.1 wt.% to about 10 wt.% based on the weight of the polyester composition, or about 0.1 wt.% to about 5 wt.% based on the weight of the polyester composition, or about 0.1 wt.% to about 2 wt.% based on the weight of the polyester composition, or about 0.1 wt.% to about 1 wt.% based on the weight of the polyester composition, or about 0.1 wt.% to about 0.5 wt.% based on the weight of the polyester composition. In such embodiments, the amount of polyester composition refers to the amount or weight of the polyester composition utilized in the above-mentioned alcoholysis process. In various embodiments, the amount of alcoholysis catalyst disclosed in this paragraph refers to the amount of alcoholysis catalyst present in the alcoholysis reaction. In various embodiments, the amount of alcoholysis catalyst disclosed in this paragraph refers to the amount of alcoholysis catalyst added to one or more depolymerization products and one or more alcohols to promote the alcoholysis reaction. In certain embodiments, a reduced or smaller amount of alcoholysis catalyst can be added to one or more depolymerization products and one or more alcohols to promote the alcoholysis reaction, for example, about 0.1 wt.% to about 10 wt.% by weight of the polyester composition, or about 0.1 wt.% to about 5 wt.% by weight of the polyester composition, or about 0.1 wt.% to about 2 wt.% by weight of the polyester composition, or about 0.1 wt.% to about 1 wt.% by weight of the polyester composition, or about 0.1 wt.% to about 0.5 wt.% by weight of the polyester composition. In embodiments, such a smaller amount of alcoholysis catalyst can be added, at least in part, because the alcoholysis catalyst is already present in one or more depolymerization products and / or one or more alcohols. In such embodiments, as discussed below, the alcohol and / or glycol may be recycled and reused in subsequent glycolysis and alcoholysis processes disclosed herein, which may include at least a portion of the alcoholysis catalyst from the preceding alcoholysis and / or glycolysis process.
[0039] In various embodiments, the alcoholysis catalyst may include carbonate catalysts, such as, but not limited to, K2CO3, Na2CO3, Li2CO3, Cs2CO3; hydroxide catalysts, such as, but not limited to, KOH, LiOH, NaOH; alkoxide catalysts, such as, but not limited to, NaOMe, Mg(OMe)2, KOMe, KOt-Bu, ethylene glycol monosodium salt, ethylene glycol disodium salt, or combinations thereof. In certain embodiments, the alcoholysis catalyst may include KOH, NaOH, LiOH, or combinations thereof. In certain embodiments, the alcoholysis catalyst may include NaOMe, KOMe, Mg(OMe)2, KOt-Bu, ethylene glycol monosodium salt, ethylene glycol disodium salt, or combinations thereof. In various embodiments, the alcoholysis catalyst may be in solid form, in solution form in water, methanol, or ethylene glycol, or combinations thereof. In certain embodiments, an alcoholysis catalyst may be added to the one or more depolymerization products and the alcohol composition once the alcohol composition and the one or more depolymerization products reach the desired reaction temperature or temperature range disclosed above.
[0040] The one or more depolymerization products may be exposed to the alcohol composition and optionally the alcoholysis catalyst under the above-mentioned temperature and pressure conditions for a time to achieve a desired yield of the resulting dialkyl terephthalate. In certain embodiments, the one or more depolymerization products may be exposed to the alcohol composition and optionally the alcoholysis catalyst under the above-mentioned temperature and pressure conditions for a time of about 5 minutes to about 5 hours, or about 5 minutes to about 2 hours, or about 5 minutes to about 1 hour, or about 5 minutes to about 30 minutes, or about 5 minutes to about 15 minutes, or about 5 minutes to about 10 minutes.
[0041] In an embodiment, the alcoholysis process results in a mixture comprising one or more dialkyl terephthalates. In various embodiments, the alcoholysis process results in a mixture in which the dialkyl terephthalates are insoluble and / or solid components, and the mixture may also include one or more contaminants. Isolation of DMT is further discussed below. In an embodiment, the liquid component of the mixture obtained from the glycolysis process may include glycol, alcohol composition, DEG, CHDM, or combinations thereof. In one embodiment, the glycol may be the glycol utilized in the glycolysis process and present with the one or more depolymerization products at the beginning of the alcoholysis process. In various embodiments, the crude dialkyl terephthalate product may be isolated from the mixture using any known separation technique, such as filtration, centrifugation, precipitation, sedimentation, or a combination of one or more separation techniques. In an embodiment, the filtration may include washing the solid components with additional alcohol composition or other solvents. The resulting liquid components may include the filtrate and the wash liquid.
[0042] As discussed above, the resulting crude dialkyl terephthalate product may include not only the dialkyl terephthalate, but also one or more contaminants or other insoluble materials generated in the depolymerization and alcoholysis processes described herein. In an embodiment, the dialkyl terephthalate may be isolated using any suitable isolation process. In an embodiment, the dialkyl terephthalate may be isolated using a distillation process, a dissolution process, or both. In certain embodiments, optionally, prior to the distillation process and / or the dissolution process, the crude product may be subjected to melting, filtration, washing, or a combination thereof. In certain embodiments, the crude product may be exposed to any suitable distillation conditions to isolate the dialkyl terephthalate. The distillation may be carried out in any vessel or distillation system suitable for use in the processes and systems described herein. In various embodiments, the distillation process of the crude product may result in a pot residue that may include one or more contaminants from the feedstock. In the same or alternative embodiments, the crude product may be subjected to one or more dissolution processes using a solvent, where the solvent is δT The solvent has a Hansen Solubility Parameter (HSP) of 16±3, total solubility parameter. In such an embodiment, the solvent may be, but is not limited to, ethyl acetate, isopropyl acetate, isobutyl acetate, n-butyl acetate, n-propyl acetate, butyl propionate, Eastman PM acetate, isobutyl isobutyrate, n-pentyl propionate, mixed hexyl acetate esters, 2-ethylhexyl acetate, Eastman EB acetate, ethylene glycol acetate, and Eastman Texanol™. In an embodiment, the solvent may be a linear and / or cyclic ether, including, but not limited to, 1,4-dioxane, Eastman EB solvent, Eastman EP solvent. In an embodiment, the solvent may be a ketone and / or a hydrocarbon, including, but not limited to, toluene, methyl ethyl ketone. In an embodiment, more than one dissolution and solid-liquid separation may be utilized to remove one or more contaminants to obtain a purer product. In certain embodiments, dissolution may be performed at 150° C. or less, 120° C. or less, 100° C. or less, 80° C. or less, or 60° C. or less. In certain embodiments, the weight ratio of solvent to crude DMT may be 50% or less, 40% or less, 30% or less, 20% or less, or 10% or less. In some embodiments, the solvent may be recycled and reused by distillation. In various embodiments, the DMT product may be isolated as a solid.
[0043] In various embodiments, the isolated dialkyl terephthalate may comprise about 90 wt.% or more dialkyl terephthalate, e.g., DMT, about 93 wt.% or more dialkyl terephthalate, e.g., DMT, or about 95 wt.% or more dialkyl terephthalate, e.g., DMT, based on the weight of the isolated component. In the same or alternative embodiments, the dialkyl terephthalate, e.g., DMT, in the resulting isolated dialkyl terephthalate component may be about 90% or more pure, about 93% or more pure, or about 95% or more pure. In various embodiments, the resulting isolated dialkyl terephthalate component may also comprise dimethyl isophthalate (DMI). In such embodiments, DMI may be present in an amount of about 1000 ppm or less, or about 500 ppm or less, or about 1 ppm to about 1000 ppm, or about 1 ppm to about 500 ppm. In one or more embodiments, the resulting isolated dialkyl terephthalate component may also comprise bisphenol A (BPA). In such embodiments, BPA may be present in an amount of about 1000 ppm or less, or about 500 ppm or less, or from about 1 ppm to about 1000 ppm, or from about 1 ppm to about 500 ppm.
[0044] The processes described herein, e.g., glycolysis and / or alcoholysis processes, are substantially milder than certain conventional processes, e.g., high temperature one-step glycolysis or methanolysis processes. For example, certain conventional one-step processes may utilize a glycolysis process at a temperature of 240° C. or higher in the presence of a Lewis acid catalyst, e.g., Zn(OAc) 2 or KOAc. Such harsh conditions may result in reduced EG yield from depolymerization due to EG being converted in various side reactions to various impurity compounds, including, but not limited to, diethylene glycol (DEG), triethylene glycol (TEG), acetaldehyde, 1,1-dimethoxyethane, 1,2-dimethoxyethane, dioxane, 2-methoxyethanol, 1-methoxyethanol, and dimethyl ether. In an embodiment, the processes described herein are substantially milder than such conventional processes, and further result in less EG yield loss, e.g., due to fewer side reactions that convert EG to various impurities. In one embodiment, the process described herein results in a yield loss of about 5% or less of EG, a yield loss of about 2% or less of EG, or a yield loss of about 1% or less of EG, or a yield loss of about 0.5% or less of EG. In such an embodiment, the yield loss of EG is the percentage of EG formed into impurities, e.g., DEG, relative to the combined amount of EG from the polyester composition feed and EG added in the glycolysis process. In the same or alternative embodiment, the process described herein produces minimal glycol impurities. For example, in one aspect, the processes described herein can result in a net generation of about 5 wt.% or less DEG, about 2 wt.% or less DEG, or about 1 wt.% or less DEG, or about 0.5 wt.% or less DEG, or about 0.01 wt.% to about 5 wt.% DEG, about 0.01 wt.% to about 2 wt.% DEG, or about 0.01 wt.% to about 1 wt.% DEG, or about 0.01 wt.% to about 0.5 wt.% DEG, or about 0.01 wt.% to about 0.2 wt.% DEG when EG is used as one or more glycols in the glycolysis process.In an embodiment, the processes described herein can result in a net generation of about 5 wt.% or less DEG and / or other impurities, about 2 wt.% or less DEG and / or other impurities, or about 1 wt.% or less DEG and / or other impurities, or about 0.5 wt.% or less DEG and / or other impurities, or about 0.01 wt.% to about 5 wt.% DEG and / or other impurities, about 0.01 wt.% to about 2 wt.% DEG and / or other impurities, or about 0.01 wt.% to about 1 wt.% DEG and / or other impurities, or about 0.01 wt.% to about 0.5 wt.% DEG and / or other impurities, or about 0.01 wt.% to about 0.2 wt.% DEG and / or other impurities when EG is used as one or more glycols in the glycolysis process. In an embodiment, the net generation of DEG (or other impurities) is the weight percent of the amount of DEG or other impurities present relative to the amount of DEG or other impurities present in the polyester composition feed. In an embodiment, the DEG produced may be produced in a glycolysis process described herein and / or an alcoholysis process described herein. In certain embodiments, when EG is used as one or more glycols in the glycolysis process, EG such as DEG and / or any glycol impurities may be present in the liquid component resulting from the alcoholysis step. In certain embodiments, the utilization of a Lewis base catalyst, e.g., a hydroxide-based or carbonate-based catalyst, in the glycolysis process may also facilitate or contribute to the reduction of EG decomposition and / or the reduction of glycol impurities.
[0045] Glycol Recycling As discussed above, in various embodiments, the glycol utilized in the glycolysis process can be reused in a subsequent series of process runs to recover one or more dialkyl terephthalates disclosed herein. In embodiments, at a high level, the liquid components resulting from the alcoholysis process can be processed for reuse, for example, for reuse in a subsequent series of glycolysis runs of a subsequent polyester composition to recover one or more dialkyl terephthalates.
[0046] In embodiments, as discussed above, the liquid component resulting from the alcoholysis process may include glycols, alcohol compositions, DEG, CHDM, or combinations thereof. In embodiments, the glycols in the liquid component may be glycols utilized in the glycolysis process and present with one or more depolymerization products at the start of the alcoholysis process. In various embodiments, the liquid component may be subjected to a separation process, for example, to remove or separate at least a portion of the alcohol composition, for example, methanol, or a mixture of methanol and ethylene glycol. In certain embodiments, the liquid component may be exposed to distillation or short path distillation to remove at least a portion of the alcohol composition. In such embodiments, the distillation conditions may include exposing the liquid component to a temperature of about 220° C. or less, about 200° C. or less, about 180° C. or less, about 160° C. or less, about 150° C. or less, about 130° C. or less, about 60° C. or more, about 70° C. or more, about 60° C. to about 220° C., about 70° C. to about 220° C., about 60° C. to about 180° C., or about 60° C. to about 160° C. In the same or alternative embodiments, the distillation conditions may include a pressure of about 1 Torr (133.3 Pa) to about 800 Torr (106,657 Pa), or about 30 Torr (3999 Pa) to about 500 Torr (66,661 Pa). In embodiments, the liquid component may be exposed to the distillation conditions until all or a substantial portion of the alcoholic composition is removed from the liquid component, e.g., vaporized. In certain embodiments, at least a portion of the alcohol composition, if present with the recycle glycol, may be removed during the subsequent glycolysis process, e.g., removed or vaporized by the glycolysis conditions.
[0047] In embodiments, distillation of the liquid components may be carried out in any vessel or distillation system suitable for use in the methods and systems described herein. In one embodiment, the distillation vessel can be in fluid communication with the alcoholysis reaction vessel and / or any component of the filtration process utilized subsequent to alcoholysis, for example, to isolate the dialkyl terephthalate solid or insoluble components. In the same or alternative embodiments, the distillation vessel can be in fluid communication with the glycolysis vessel.
[0048] In various embodiments, distillation of the liquid component can vaporize the alcohol composition and leave a pot residue. In embodiments, the pot residue includes glycol and any other heavies, such as non-vaporizable compounds, present in the liquid component. In embodiments, the glycol in the pot residue may be referred to as recycled glycol and / or the glycol from the non-vaporizable portion of the continuous distillation process using the distillation conditions described herein may be referred to as recycled glycol.
[0049] In an embodiment, as discussed above, the recycled glycol may be utilized in a subsequent series of process trials described herein to recover one or more dialkyl terephthalates from the polyester composition. Furthermore, in an embodiment, the recycled glycol may be recycled again using the processes described herein after this subsequent series of dialkyl terephthalate recovery trials. In an embodiment, the recycled glycol may be recovered and reused at least two times, at least three times, at least four times, or at least five times. In certain embodiments, when the recycled glycol is used in a subsequent series of dialkyl terephthalate recovery trials, the addition of a catalyst in the subsequent glycolysis step may be omitted since the recycled glycol may contain used catalyst.
[0050] In embodiments, it has been unexpectedly discovered that when recycled glycol is recovered and reused, the resulting recovered dialkyl terephthalate exhibits a purity comparable to that of dialkyl terephthalate recovered using glycol that was not recovered and reused. In embodiments, this comparable purity of dialkyl terephthalate exists after reusing recycled glycol at least two, at least three, at least four, or at least five times, resulting in the recovery of dialkyl terephthalate having a purity of at least about 90%, at least about 93%, or at least about 95%.
[0051] As discussed above, in embodiments, the processes described herein are substantially milder than certain conventional processes and result in less EG yield loss, for example, due to fewer side reactions that convert EG to various impurities. In one example with three EG recycle runs, the yield loss of EG to DEG is about 5% or less, about 2% or less, about 1% or less, or about 0.5% or less. In one example with four EG recycle runs, the yield loss of EG to DEG is about 5% or less, about 2% or less, about 1% or less, or about 0.5% or less. In the same or alternative embodiments, the processes described herein produce minimal glycol impurities. In certain embodiments, when EG is used as one or more glycols in the glycolysis process, any glycol impurities, such as EG and / or DEG, may be present in the liquid component resulting from the alcoholysis process discussed above. In such embodiments, DEG or any glycol impurities may be recovered and / or may be present in the recycled glycol described herein. In such embodiments, the recycled glycol may contain about 5 wt.% or less DEG and / or other impurities, about 2 wt.% or less DEG and / or other impurities, or about 1 wt.% or less DEG and / or other impurities, or about 0.5 wt.% or less DEG and / or other impurities, or about 0.01 wt.% to about 5 wt.% DEG and / or other impurities, about 0.01 wt.% to about 2 wt.% DEG and / or other impurities, or about 0.01 wt.% to about 1 wt.% DEG and / or other impurities, or about 0.01 wt.% to about 0.5 wt.% DEG and / or other impurities, or about 0.01 wt.% to about 0.2 wt.% DEG and / or other impurities when EG is used as one or more glycols in the glycolysis process.
[0052] Use of Recovered Dialkyl Terephthalates to Form Polyesters or Other Products As discussed above, the methods disclosed herein can result in high purity dialkyl terephthalates such as DMT. For example, in certain embodiments, the recovered DMT may be utilized to form one or more polyesters, including but not limited to PET and TMCD-containing polyesters. In various embodiments, the products formed using the recovered DMT may be indistinguishable from similar products formed from virgin DMT. In such embodiments, any suitable process for forming PET and TMCD-containing polyesters may be utilized, since the DMT is of sufficient purity.
[0053] In the same or alternative embodiments, the recovered DMT may be utilized to form CHDM. In various embodiments, the CHDM formed using the recovered DMT may be indistinguishable from CHDM formed from virgin DMT due to the high purity of the recovered DMT. In such embodiments, the CHDM may be formed from the recovered DMT using any suitable process. Exemplary System FIG. 1 illustrates generally one exemplary system and / or method for recovering one or more dialkyl terephthalates from a feedstock composition. System 100 includes a source 110 of a feedstock composition, such as the feedstock composition described above. Vessel 120 represents a glycolysis vessel, in which the feedstock composition is received and exposed to one or more glycols under depolymerization conditions, as discussed in detail above. In an embodiment, vessel 120 can be in fluid communication with source 110. In various embodiments, the feedstock composition is converted to one or more depolymerized products after being exposed to depolymerization conditions in vessel 120, as discussed above. In various embodiments, the one or more depolymerized products may include monomers and / or oligomers having a degree of polymerization of 2-10, 2-8, 2-6, or 2-4, as discussed above. As discussed, in certain embodiments, one or more foreign materials may be removed from the glycolysis vessel, for example, foreign materials that may melt in the glycolysis vessel and / or float to the top of the glycol or solvent. In the embodiment shown in FIG. 1, one or more depolymerization products and / or the mixture resulting from the glycolysis process may be exposed to alcoholysis conditions in vessel 130. In embodiments, one or more depolymerization products and / or liquid components may be directly utilized in the alcoholysis process. Alcoholysis conditions are discussed in detail above. In embodiments, as discussed above, alcoholysis of one or more depolymerization products and / or liquid components may result in a mixture including an insoluble or solid component comprising the crude dialkyl terephthalate, and a liquid component comprising the alcohol composition, glycol, and potentially other soluble components as described herein. As discussed above, the resulting alcoholysis reaction mixture may be exposed to a solid-liquid separation device 140, for example, a filtration system, to separate the solid component comprising the crude dialkyl terephthalate product. In embodiments, as discussed above, the filtrate or liquid components may be subjected to one or more distillations or other processes in system 150 to recover glycol and / or methanol, which may optionally be returned to the glycolysis or alcoholysis reactors, respectively.As mentioned above, the crude dialkyl terephthalate product may undergo one or more isolation processes, such as distillation and / or dissolution, in system 160 to provide a high purity dialkyl terephthalate product. In certain embodiments, the methods described herein relating to system 100 may be implemented as continuous, batch, or semi-continuous methods. It is understood that system 100 is merely an example system, and other configurations of system components are contemplated by the disclosure herein. For example, one or more components of system 100 may not be physically separated or distinct from one or more other components of system 100. It is further understood that system 100 is merely illustrated diagrammatically to highlight aspects of the methods disclosed herein.
[0054] The present disclosure can be further illustrated by the following examples of its aspects, although it will be understood that these examples are included for illustrative purposes only and are not intended to limit the scope of the disclosure unless specifically indicated otherwise. EXAMPLES
[0055] material The solid blend (SSB) contains 84.265% TPA and 1.599% IPA by LC analysis. The TPA of the PET sample is 86.4% of theoretical.
[0056] The 25% PCR contains 82.103% TPA and 1.563% IPA by LC analysis. FDST-251 contains 77.157% TPA and 1.511% IPA by LC analysis.
[0057] Ethylene glycol, methanol, potassium carbonate and 50% aqueous sodium hydroxide were obtained from Sigma Aldrich. All chemicals and reagents were used as received unless otherwise stated.
[0058] Analytical procedures Gas Chromatography (GC) Analysis. GC analysis was performed on an Agilent Model 7890B Gas Chromatograph equipped with a 7693A autosampler and two G4513A towers. The GC was equipped with two columns, a 60m x 0.32mm x 1.0 micron DB-1701™ (J&W123-0763) and a 60m x 0.32 x 1 micron DB-1™ (J&W123-1063), and samples were injected simultaneously onto both columns. A common oven temperature program was used and sample components were detected by flame ionization detection (FID). A five-point calibration was performed for components of interest. The gas chromatograph was interfaced to an EZChrom Elite Chromatography Data System. Methanolysis product samples were prepared by adding a known volume of pyridine-based internal standard solution to a known mass of sample, followed by derivatization with N,O-bis(trimethylsilyl)trifluoroacetamide (BSTFA).
[0059] Gel Permeation Chromatography (GPC). Size Exclusion Chromatography GPC analysis was performed on an Agilent 1100 series GPC / SEC analytical system equipped with a UV-Vis detector. The column set used was a guarded Polymer Laboratories 5 μm Plgel, mixed C and oligopore. The eluent consisted of 95% methylene chloride and 5% hexafluoroisopropanol with tetraethylammonium nitrate (1 gram / 2 liters of solvent). The tests were performed at ambient temperature using a flow rate of 1.0 mL / min. The instrument was calibrated with linear PET oligomer standards. Samples were prepared by dissolving 10 mg of sample in 10 mL of methylene chloride / hexafluoroisopropanol (70 / 30). 10 μL of toluene was added as a flow rate marker. The injection volume was 10 μL. The GC wt.% of BHET (bis(hydroxyethyl) terephthalate), GC wt.% of MHT (4-(methoxycarbonyl)benzoic acid), GC wt.% of MHET (methyl-2-hydroxyethyl terephthalate), and GC wt.% of dimethyl isophthalate (DMI) are provided as readouts from the GC process software.
[0060] Liquid chromatography (LC). LC analysis of oligomers was performed on an HP 1100 series liquid chromatograph equipped with a diode array detector (DAD) with a range of 190-900 nm. The system was equipped with a Zorbax Poroshell 120 EC-C18 (4.6 × 50 mm, 2.7 μm) column at 40 °C. The flow rate was 1.0 mL / min. The mobile phase was water (25 nM ammonium acetate) (A) and acetonitrile (B). The elution gradient was as follows: 0 min, 95% A / 5% B; 2 min, 95% A / 5% B; 18 min, 0% A / 100% B; 28 min, 0% A / 100% B; 28.1 min, 95% A / 5% B; 33 min, 95% A / 5% B. Sample solutions were prepared by dissolving approximately 4 mg of sample in 1 mL of DMF / DMSO (50 / 50). The injection volume was 2 μL. Oligomer distributions were reported as area %.
[0061] LC analysis of TPA and IPA was performed on an HP1100 series liquid chromatograph equipped with a fluorescence detector using an excitation wavelength of 225 nm, an emission wavelength of 310 nm, an FLD PMT gain of 10, and a data frequency of 2.31 Hz. The system was equipped with an Agilent Poroshell EC-C18 (4.6 × 150 mm, 2.7 μm) column at 30 °C. The mobile phase was 0.14% phosphoric acid in water (A), acetonitrile (B), and THF (C). The elution gradient was as follows: 0 min, 79% A / 0% B / 21% C; 10 min, 79% A / 0% B / 21% C; 18 min, 34% A / 45% B / 21% C; 18.1 min, 14% A / 65% B / 21% C; 19 min, 14% A / 65% B / 21% C; 19.1 min, 79% A / 0% B / 21% C; 25 min, 79% A / 0% B / 21% C. The flow rate was 0.9 mL / min. TPA and IPA contents were reported as wt.%.
[0062] XRF Quantitative Metal Analysis. Quantitative XRF testing was performed using a Malvern Panalytical Zetium WDXRF. DMT and feedstock samples were prepared by pressing into chips. All samples were analyzed in helium mode with a 4 μm Mylar film attached. The method is capable of detecting 14 major elements with a quantitative range of a few ppm to hundreds of ppm w / w.
[0063] The % DMT yield was calculated as follows: (weight of final DMT) / (weight of theoretical DMT). * 100%. DMT GC purity % was calculated as follows: (wt.% DMT in final product by GC) / (total wt.% by GC). * 100%.
[0064] Measurement of Intrinsic Viscosity. The intrinsic viscosity (IV) of certain polymeric materials useful herein is determined according to the ASTM D2857-70 procedure on a LabGlass Wagner Viscometer with a 1 / 2 mL capillary valve using a polymer concentration of about 0.5 wt % in 60 / 40 phenol / tetrachloroethane by weight. The procedure is performed by heating the polymer / solvent system at 120° C. for 15 minutes, cooling the solution to 25° C., and measuring the flow time at 25° C. The IV is calculated from the following formula:
[0065]
number
[0066] In the following examples, viscosity was measured in tetrachloroethane / phenol (50 / 50, by weight) at 30° C. and calculated according to the following formula:
[0067]
number
[0068] Example 1: Direct low-temperature methanolysis of high molecular weight feedstock SSB to DMT In this Example 1, a three-necked, 1-liter round-bottom flask was equipped with a mechanical stirrer, reflux condenser, and thermocouple. The SSB dissolver sample (100.65 g) and methanol (401.37 g) were charged. The resulting mixture was heated to 64° C. with 500 rpm agitation. Once the reaction reached the set temperature, 50% aqueous NaOH (468 mg) was added. After 20 minutes, the mixture was cooled to 50° C. and a second dose of NaOH solution (468 mg) was added. After 1 hour, a third dose of NaOH solution was added. The resulting mixture was stirred for an additional hour. The flask was cooled to room temperature and the product was collected by filtration and washing. The insoluble solid was also isolated as a solid mass by carefully decanting the slurry. After drying overnight in air, 49.57 g of the product was obtained as a grey powder, which contained 49.9% DMT by GC analysis. The insoluble material was isolated (40.5 g). LC analysis showed that the insoluble solids contained 76.08% TPA, 1.387% IPA. GPC analysis showed Mn 1051, Mw 1525, and Mz 2002.
[0069] Example 2: Glycolysis and low-temperature methanolysis of high molecular weight feedstock SSB to DMT In this example, a three-necked 1-liter round-bottom flask was equipped with a mechanical stirrer, reflux condenser, and thermocouple. Charge the SSB dissolver sample (97.94 g from the pilot plant dissolver), EG (42.53 g), and K2CO3 (0.97 g). The resulting mixture was refluxed for 2 hours. After cooling the reaction mixture to 50° C., 50% aqueous NaOH solution (468 mg) and MeOH (400.29 g) were added. The mixture was then cooled to 50° C. and a second dose of NaOH solution (612 mg) was added. The resulting mixture was kept at 50° C. and stirred for 30 minutes. The flask was cooled to room temperature and the product was collected by filtration and washing. After drying overnight in air, 70.19 g of DMT product was obtained as a grey powder (GC purity 92.45%).
[0070] Example 3: Conversion of PCR feedstock to DMT by methanolysis at reflux A three-necked, 1-liter round-bottom flask was equipped with a mechanical stirrer, reflux condenser, and thermocouple. 25% PCR carpet dissolver sample (100.11 g) and methanol (408.95 g) were charged. The resulting mixture was heated to reflux. Once the reaction reached the set temperature, 50% aqueous NaOH solution (468 mg) was added and held for 1 hour. The mixture was then cooled to 50° C. and a second dose of NaOH solution (468 mg) was added. After 30 minutes, the flask was cooled to room temperature and the product was recovered by filtration and washing. The insoluble solid was isolated as a solid mass (65.94 g) by carefully decanting the slurry. The DMT product was obtained as a grey solid (24.83 g, GC purity 59.5%).
[0071] [Table 1] As can be seen in Table 1, direct methanolysis of the feedstocks in Examples 1 and 3 at low temperatures resulted in DMT products with poor mass balance and low GC purity. Additionally, in Examples 1 and 3, significant amounts of insoluble solids were isolated by careful decantation and analyzed to be high MW PET oligomers. The presence of high MW PET oligomers and broad MW distribution may contribute to the low yield and purity of the isolated DMT products in these examples. As in Example 2, a glycolysis step prior to methanolysis was demonstrated to improve yield and GC purity. The results confirmed the presence of high MW PET oligomers and that their conversion to lower MW oligomers may facilitate efficient methanolysis.
[0072] Example 4: Conversion of feedstock to DMT by glycolysis using a 7 / 3 PET / EG ratio A three-necked 1-liter round-bottom flask was equipped with a mechanical stirrer, reflux condenser, and thermocouple. SSB sample (87.51 g), EG (37.69 g), and K2CO3 (0.90 g) were charged. The resulting mixture was refluxed for 2 h. The reaction mixture was cooled to 50° C., followed by the addition of 50% aqueous NaOH (546 mg) and MeOH (350.8 g). The resulting mixture was kept at 50° C. and stirred for 30 min. The flask was cooled to room temperature, and the product was collected by filtration and washing. After drying overnight in air, 32.27 g of DMT product was obtained as a grey powder (GC purity 85.81%). A solid mass (51.01 g) was also isolated, consisting mainly of PET oligomers.
[0073] Example 5: Conversion of Feedstock to DMT by Glycolysis Using a 1 / 1 PET / EG Ratio Followed by Short Path Distillation A three-necked, 1-liter round-bottom flask was equipped with a mechanical stirrer, reflux condenser, and thermocouple. SSB sample (100.18 g), EG (103.38 g), and K2CO3 (1.01 g) were charged. The resulting mixture was refluxed for 3 h. After the reaction mixture was cooled to 50° C., 50% aqueous NaOH (546 mg) and MeOH (403.7 g) were added. The resulting mixture was kept at 50° C. and stirred for 30 min. The flask was cooled to room temperature and the product was collected by filtration and washing. After drying overnight in air, 90.07 g of DMT product was obtained as a grey powder (GC purity 95.73%).
[0074] A three-neck, 1 L round bottom flask was equipped with a magnetic stir bar, heating mantle, distillation head and air condenser, and thermocouple. Both the distillation head and air condenser were insulated with heat tape and thermocouple. 121.89 g of crude DMT was charged. DMT distillation was carried out at a vacuum of 44.4-46.3 torr and a take off temperature of 186.3°C. The DMT product was collected as white needles (112.15 g, GC purity 99.4%).
[0075] Example 6: Conversion of Feedstock to DMT by Glycolysis Using a 1 / 1 PET / EG Ratio Followed by Short Path Distillation A three-necked, 1-liter round-bottom flask was equipped with a mechanical stirrer, reflux condenser, and thermocouple. 25% PCR sample (120.13 g), EG (121.7 g), and K2CO3 (1.21 g) were charged. The resulting mixture was refluxed for 2 h. After the reaction mixture was cooled to 50° C., 50% aqueous NaOH (749 mg) and MeOH (480.0 g) were added. The resulting mixture was kept at 50° C. and stirred for 30 min. The flask was cooled to room temperature and the product was collected by filtration and washing. After drying overnight in air, 102.31 g of DMT product was obtained as a grey powder (GC purity 97.73%).
[0076] A 3-neck, 1 L round bottom flask was equipped with a magnetic stir bar, heating mantle, distillation head and air condenser, and thermocouple. Both the distillation head and air condenser were insulated with heat tape and thermocouple. 99.5 g of crude DMT was charged. The DMT product was collected as white needles (92.49 g, GC purity 99.7%).
[0077] Example 7: Conversion of Feedstock to DMT by Glycolysis Using a 1 / 1 PET / EG Ratio Followed by Short Path Distillation A three-necked 1-liter round-bottom flask was equipped with a mechanical stirrer, reflux condenser, and thermocouple. FDST-251 sample (120.01 g), EG (121.35 g), and K2CO3 (1.21 g) were charged. The resulting mixture was refluxed for 2 h. After the reaction mixture was cooled to 50° C., 50% aqueous NaOH (749 mg) and MeOH (483.17 g) were added. The resulting mixture was kept at 50° C. and stirred for 30 min. The flask was cooled to room temperature and the product was collected by filtration and washing. After drying overnight in air, 103.01 g of DMT product was obtained as a grey powder (GC purity 92.57%).
[0078] A 3-neck, 1 L round bottom flask was equipped with a magnetic stir bar, heating mantle, distillation head and air condenser, and thermocouple. Both the distillation head and air condenser were insulated with heat tape and thermocouple. 99.8 g of crude DMT was charged. The DMT product was collected as white needles (85.9 g, GC purity 99.1%).
[0079] [Table 2] As shown in Table 2, flash distillation significantly improved the quality of DMT as indicated by the reduction in impurity levels and the improvement in total accountable mass. Additionally, these processes demonstrated efficient separation of isophthalate from terephthalate.
[0080] Example 8: Metals analysis of distilled DMT and analysis of raw materials Metals analysis was performed on the distilled DMT products of Examples 5, 6 and 7, as well as the feedstock material. Metals analysis and feedstock description are provided above. Results are shown below in Tables 3 and 4. The wt% of IPA and TPA were determined using LC as described above.
[0081] Low levels of residual metals were observed in the distilled DMT product starting with the solids blend (SSB), 25% PCR, and FDST-251 textile and carpet. As shown in Tables 3 and 4, the methods described herein demonstrated efficient removal of a variety of elements including metals (Sb, Ca, Fe, Mn, Na, Ti), halogens (Br, Cl) and other elements (P and S).
[0082] [Table 3]
[0083] [Table 4] The present disclosure may also be described according to the following numbered sections:
[0084] Item 1. A method for recovering one or more dialkyl terephthalates from a feedstock composition, comprising: exposing a feedstock composition comprising one or more polyesters and one or more contaminants to one or more glycols and a depolymerization catalyst in a first reaction vessel under depolymerization conditions to prepare a first mixture, the first mixture comprising one or more depolymerization products; exposing at least a portion of the first mixture to an alcohol composition and an alcoholysis catalyst under alcoholysis conditions to prepare a second mixture, the second mixture comprising one or more dialkyl terephthalates, the alcoholysis conditions comprising a temperature of 23°C to 70°C for 0.5 hours to 10 hours; and isolating at least a portion of the one or more dialkyl terephthalates from the second mixture.
[0085] Item 2. The method according to item 1, wherein the one or more foreign substances include at least one element selected from the group consisting of polyesters other than polyethylene terephthalate, polyvinyl chloride (PVC), polyvinyl acetal, polyvinyl butyral (PVB), polyvinyl alcohol (PVOH), ethylene vinyl alcohol (EVOH), cotton, polyolefins, polyethylene, polypropylene, polystyrene, polycarbonate, spandex, natural fibers, cellulose esters, polyacrylates, polymethacrylates, polyamides, nylons, poly(lactic acid), polydimethylsiloxanes, polysilanes, calcium carbonate, titanium dioxide, inorganic fillers, dyes, pigments, color toners, colorants, plasticizers, adhesives, flame retardants, metals, aluminum, and iron.
[0086] Item 3. The method according to Items 1 to 2, further comprising a step of removing a first portion of one or more foreign substances from the first reaction vessel. Item 4. The method according to items 2-3, wherein a first portion of the one or more foreign substances is removed from the first reaction vessel via a pump.
[0087] Item 5. The method according to any one of items 2 to 4, wherein the first portion of the one or more foreign bodies comprises a polyolefin, a polyethylene, a polypropylene, a polystyrene, or a combination thereof. Item 6. The method according to any one of items 1 to 5, wherein the one or more foreign matter is present in the feedstock composition in an amount of 0.01 wt.% to 50 wt.% based on the weight of the one or more polyesters.
[0088] Item 7. The method according to any one of items 1 to 6, wherein the step of isolating at least a portion of the one or more dialkyl terephthalates from the second mixture comprises exposing at least a portion of the second mixture to distillation conditions to separate at least a portion of the one or more dialkyl terephthalates from a distillation pot residue.
[0089] Item 8. The method of item 7, wherein the distillation pot residue comprises a second portion of one or more foreign materials. Item 9. The method according to item 8, wherein the second portion of the one or more foreign bodies is selected from the group consisting of polyesters other than polyethylene terephthalate, polyvinyl chloride (PVC), polyvinyl acetal, polyvinyl butyral (PVB), polyvinyl alcohol (PVOH), ethylene vinyl alcohol (EVOH), cotton, polycarbonate, spandex, natural fibers, cellulose esters, polyacrylates, polymethacrylates, polyamides, nylons, poly(lactic acid), polydimethylsiloxanes, polysilanes, calcium carbonate, titanium dioxide, inorganic fillers, dyes, pigments, color toners, colorants, plasticizers, adhesives, flame retardants, metals, aluminum and iron.
[0090] Item 10. The method according to any one of items 1 to 9, wherein the depolymerization conditions include a temperature in the range of about 120° C. to about 260° C., a pressure in the range of about 0.013 atm (0.2 psig) to about 2 atm (30 psig), and a period in the range of about 0.5 hours to about 10 hours.
[0091] Item 11. The method of any one of items 1 to 10, wherein the one or more glycols include ethylene glycol (EG), diethylene glycol (DEG), triethylene glycol (TEG), 1,4-cyclohexanedimethanol (CHDM), poly(ethylene glycol) (PEG), neopentyl glycol (NPG), propanediol (PDO), butanediol (BDO), 2-methyl-2,4-pentanediol (MP diol), poly(tetramethylene ether) glycol (PTMG), or a combination thereof.
[0092] Item 12. The method according to any one of items 1 to 11, wherein the weight ratio of the one or more glycols to the feedstock composition is in the range of about 1:9 to about 9:1. Item 13. The method according to any one of claims 1 to 12, wherein the depolymerization catalyst comprises an element selected from the group consisting of Li2CO3, K2CO3, CaCO3, Na2CO3, Cs2CO3, ZrCO3, LiOH, NaOH, KOH, tetrabutylammonium hydroxide (TBAH), sodium methoxide (NaOMe), lithium methoxide (LiOMe), magnesium methoxide (Mg(OMe)2, potassium t-butoxide, ethylene glycol monosodium salt, ethylene glycol disodium salt, tetraisopropyl titanate (TIPT), butyltin tris-2-ethylhexanoate (FASCAT 4102), 1,8-diazabicyclo[5.4.0]undec-7-ene (DBU), zinc acetylacetonate hydrate (Zn(acac)2), zinc acetate (Zn(OAc)2), manganese(II) acetate (Mn(OAc)2), hydrotalcite, zeolite and lithium chloride.
[0093] Item 14. The method according to any one of items 1 to 13, wherein the one or more polyesters are polyethylene terephthalate (PET), 1,4-cyclohexanedimethanol (CHDM) modified PET, isophthalic acid (IPA) modified PET, diethylene glycol (DEG) modified PET, neopentyl glycol (NPG) modified PET, propanediol (PDO) modified PET, butanediol (BDO) modified PET, hexanediol (HDO) modified PET, 2-methyl-2,4-pentanediol (MP diol) modified PET, isosorbide modified PET, poly(tetramethylene ether) glycol (PTMG) modified PET, poly(ethylene glycol) (PEG) modified PET, polycyclohexylene dimethylene terephthalate (PCT), cyclohexanedimethanol (CHDM)-containing copolyester, isosorbide-containing copolyester, or a combination thereof.
[0094] Item 15. The method of any one of items 1 to 14, wherein the one or more polyesters comprise 0 mol% to 100 mol% CHDM, 0 mol% to 100 mol% DEG, 0 mol% to 100 mol% NPG, 0 mol% to 100 mol% PDO, 0 mol% to 100 mol% BDO, 0 mol% to 100 mol% HDO, 0 mol% to 100 mol% MP diol, 0 mol% to 100 mol% isosorbide, 0 mol% to 100 mol% PTMG, 0 mol% to 100 mol% PEG, and 0 mol% to 30 mol% isophthalic acid, wherein the total of the diol equivalents in the one or more polyesters is about 100 mol%, and the total of the diacid equivalents in the one or more polyesters is about 100 mol%.
[0095] Item 16. The method of any one of items 1 to 15, wherein at least one of the one or more polyesters has an intrinsic viscosity of about 0.1 dL / g to about 1.2 dL / g, as determined according to ASTM D2857-70.
[0096] Item 17. The method according to any one of items 1 to 16, wherein at least one of the one or more polyesters is a recycled polyester. Item 18. The method according to items 1 to 17, wherein the alcohol composition contains methanol.
[0097] Item 19. The method according to any one of items 1 to 18, wherein the alcoholysis catalyst is present in an amount of 0.1 wt.% to 20 wt.%, based on the weight of the one or more polyesters in the feedstock composition. Item 20. The method according to items 1 to 19, wherein the alcoholysis catalyst comprises K2CO3, Na2CO3, Li2CO3, Cs2CO3; KOH, LiOH, NaOH; NaOMe, Mg(OMe)2, KOMe, KOt-Bu, ethylene glycol monosodium salt, ethylene glycol disodium salt, or a combination thereof.
[0098] Item 21. The method according to any one of items 1 to 20, wherein at least a portion of the one or more dialkyl terephthalates comprises dimethyl terephthalate (DMT), and the DMT has a purity of at least 90%.
[0099] Item 22. At least a portion of the one or more dialkyl terephthalates further comprises dimethyl isophthalate (DMI) in an amount of 1000 ppm or less, or 500 ppm or less; bisphenol A (BPA) in an amount of 1000 ppm or less, or 500 ppm or less; or both. The method according to items 1 to 21.
[0100] Item 23. The method according to any one of items 1 to 22, wherein the step of isolating at least a portion of the one or more dialkyl terephthalates from the second mixture comprises exposing the second mixture to a solvent dissolution process.
[0101] Item 24. The method of items 1 to 23, carried out as a batch process, a semi-continuous process, or a continuous process. Item 25. The method of any one of items 1 to 24, wherein the one or more depolymerization products include monomers, oligomers, or combinations thereof.
[0102] Item 26. The method according to item 25, wherein the one or more oligomers have a degree of polymerization of 2 to 10.
Claims
1. 1. A method for recovering one or more dialkyl terephthalates from a feedstock composition, the method comprising: exposing a feedstock composition comprising one or more polyesters and one or more contaminants to one or more glycols and a depolymerization catalyst in a first reaction vessel under depolymerization conditions to provide a first mixture, the first mixture comprising one or more depolymerization products; exposing at least a portion of the first mixture to an alcohol composition and an alcoholysis catalyst under alcoholysis conditions to provide a second mixture, the second mixture comprising one or more dialkyl terephthalates, the alcoholysis conditions comprising a temperature of 23° C. to 70° C. for a period of 0.5 hours to 10 hours; and isolating at least a portion of the one or more dialkyl terephthalates from the second mixture.
2. 2. The method of claim 1, wherein the one or more foreign bodies comprise at least one member selected from the group consisting of polyesters other than polyethylene terephthalate, polyvinyl chloride (PVC), polyvinyl acetal, polyvinyl butyral (PVB), polyvinyl alcohol (PVOH), ethylene vinyl alcohol (EVOH), cotton, polyolefins, polyethylene, polypropylene, polystyrene, polycarbonate, spandex, natural fibers, cellulose esters, polyacrylates, polymethacrylates, polyamides, nylon, poly(lactic acid), polydimethylsiloxane, polysilanes, calcium carbonate, titanium dioxide, inorganic fillers, dyes, pigments, color toners, colorants, plasticizers, adhesives, flame retardants, metals, aluminum, and iron.
3. 10. The method of claim 1, further comprising removing a first portion of the one or more foreign bodies from the first reaction vessel.
4. 3. The method of claim 2, wherein the first portion of the one or more foreign bodies is removed from the first reaction vessel via a pump.
5. 3. The method of claim 2, wherein the first portion of the one or more foreign bodies comprises a polyolefin, a polyethylene, a polypropylene, a polystyrene, or a combination thereof.
6. 10. The method of claim 1, wherein the one or more contaminants are present in the feedstock composition in an amount of from 0.01 wt. % to 50 wt. %, based on the weight of the one or more polyesters.
7. 2. The method of claim 1 , wherein the step of isolating at least a portion of the one or more dialkyl terephthalates from the second mixture comprises exposing at least a portion of the second mixture to distillation conditions to separate at least a portion of the one or more dialkyl terephthalates from a distillation pot residue.
8. 8. The method of claim 7, wherein the distillation pot residue comprises a second portion of the one or more contaminants.
9. 9. The method of claim 8, wherein the second portion of the one or more foreign objects comprises at least one member selected from the group consisting of polyesters other than polyethylene terephthalate, polyvinyl chloride (PVC), polyvinyl acetal, polyvinyl butyral (PVB), polyvinyl alcohol (PVOH), ethylene vinyl alcohol (EVOH), cotton, polycarbonate, spandex, natural fibers, cellulose esters, polyacrylates, polymethacrylates, polyamides, nylon, poly(lactic acid), polydimethylsiloxane, polysilanes, calcium carbonate, titanium dioxide, inorganic fillers, dyes, pigments, color toners, colorants, plasticizers, adhesives, flame retardants, metals, aluminum, and iron.
10. 10. The method of claim 1, wherein the depolymerization conditions comprise a temperature in the range of about 120° C. to about 260° C., a pressure in the range of about 0.013 atm (0.2 psig) to about 2 atm (30 psig), and a time period in the range of about 0.5 hours to about 10 hours.
11. 2. The method of claim 1, wherein the one or more glycols comprise ethylene glycol (EG), diethylene glycol (DEG), triethylene glycol (TEG), 1,4-cyclohexanedimethanol (CHDM), poly(ethylene glycol) (PEG), neopentyl glycol (NPG), propanediol (PDO), butanediol (BDO), 2-methyl-2,4-pentanediol (MP diol), poly(tetramethylene ether) glycol (PTMG), or combinations thereof.
12. 10. The method of claim 1, wherein the weight ratio of the one or more glycols to the feedstock composition ranges from about 1:9 to about 9:
1.
13. The depolymerization catalyst is Li 2 CO 3 , K 2 CO 3 , CaCO 3 , Na 2 CO 3 , Cs 2 CO 3 , ZrCO3, LiOH, NaOH, KOH, tetrabutylammonium hydroxide (TBAH), sodium methoxide (NaOMe), lithium methoxide (LiOMe), magnesium methoxide (Mg(OMe) 2 , potassium t-butoxide, ethylene glycol monosodium salt, ethylene glycol disodium salt, tetraisopropyl titanate (TIPT), butyltin tris-2-ethylhexanoate (FASCAT 4102), 1,8-diazabicyclo[5.4.0]undec-7-ene (DBU), zinc acetylacetonate hydrate (Zn(acac) 2 ), zinc acetate (Zn(OAc) 2 ), Manganese(II) acetate (Mn(OAc) 2 ), hydrotalcite, zeolite and lithium chloride.
14. 2. The method of claim 1, wherein the one or more polyesters comprise polyethylene terephthalate (PET), 1,4-cyclohexanedimethanol (CHDM) modified PET, isophthalic acid (IPA) modified PET, diethylene glycol (DEG) modified PET, neopentyl glycol (NPG) modified PET, propanediol (PDO) modified PET, butanediol (BDO) modified PET, hexanediol (HDO) modified PET, 2-methyl-2,4-pentanediol (MP diol) modified PET, isosorbide modified PET, poly(tetramethylene ether) glycol (PTMG) modified PET, poly(ethylene glycol) (PEG) modified PET, polycyclohexylene dimethylene terephthalate (PCT), cyclohexanedimethanol (CHDM)-containing copolyesters, isosorbide-containing copolyesters, or combinations thereof.
15. 2. The method of claim 1, wherein the one or more polyesters comprise 0 mol% to 100 mol% CHDM, 0 mol% to 100 mol% DEG, 0 mol% to 100 mol% NPG, 0 mol% to 100 mol% PDO, 0 mol% to 100 mol% BDO, 0 mol% to 100 mol% HDO, 0 mol% to 100 mol% MP diol, 0 mol% to 100 mol% isosorbide, 0 mol% to 100 mol% PTMG, 0 mol% to 100 mol% PEG, and 0 mol% to 30 mol% isophthalic acid, the total of diol equivalents in the one or more polyesters is about 100 mol%, and the total of diacid equivalents in the one or more polyesters is about 100 mol%.
16. The method of claim 1 , wherein the alcohol composition comprises methanol.
17. The alcoholysis catalyst is present in an amount of 0.1 wt. % to 20 wt. %, based on the weight of the one or more polyesters in the feedstock composition, and the alcoholysis catalyst is selected from the group consisting of K 2 CO 3 , Na 2 CO 3 , Li 2 CO 3 , Cs 2 CO 3 ;KOH, LiOH, NaOH; NaOMe, Mg(OMe) 2 , KOMe, KOt-Bu, ethylene glycol monosodium salt, ethylene glycol disodium salt, or combinations thereof.
18. 2. The method of claim 1, wherein at least a portion of the one or more dialkyl terephthalates comprises dimethyl terephthalate (DMT), the DMT being at least 90% pure.
19. 10. The method of claim 1, wherein the step of isolating at least a portion of the one or more dialkyl terephthalates from the second mixture comprises exposing the second mixture to a solvent dissolution process.
20. 10. The method of claim 1 , wherein the one or more depolymerization products comprise monomers, oligomers, or combinations thereof, and the one or more oligomers exhibit a degree of polymerization of 2 to 10.