Polyether diacid or its salt surfactant and use thereof

Polyether diacid or its salt surfactants with specific structures address the need for environmentally friendly alternatives to PFOA by reducing surface tension and enhancing fluorine-containing polymer dispersion stability, enabling efficient production with lower agent usage.

JP2024539619AActive Publication Date: 2024-10-29ZHONGHAO CHENGUANG RES INST OF CHEMICALINDUSTRY CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2024522048
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2021-06-11
Filing Date
2021-09-28
Publication Date
2024-10-29
Estimated Expiration
2041-09-28

AI Technical Summary

Technical Problem

The environmental and health concerns associated with the use of perfluorooctanoic acid (PFOA) and its salts have led to the need for safe, environmentally friendly alternatives that maintain excellent surface properties and low toxicity, while also being easy to decompose.

Method used

The development of polyether diacid or its salt surfactants with specific structural formulas, including ether bonds and terminal groups like carboxylate or sulfonate, which reduce surface tension and improve the stability of fluorine-containing polymer dispersions, allowing for reduced usage amounts.

Benefits of technology

These surfactants significantly lower the surface tension of polymerization systems, enhance the stability of fluorine-containing polymer dispersions, and enable the production of fluorine-containing polymers with improved properties using less agent, thus addressing the need for safer and more sustainable alternatives to PFOA.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024539619000001
    Figure 2024539619000001
  • Figure 2024539619000002
    Figure 2024539619000002
  • Figure 2024539619000003
    Figure 2024539619000003
Patent Text Reader

Abstract

The present invention relates to the technical field of fluorine-containing polymers, in particular to a polyether diacid or its salt surfactant and its use. The polyether diacid or its salt surfactant has the general structural formula: XL-(O-CH 2 CHZ) a -(O-CR 1 R 2 CR 3 R 4 ) b -OLX, where Z is H or CH 3 L stands for C 1 ~C 5 represents an alkylene group represented by the formula: 3 M represents H + , N.H. 4 + Or Na + R 1 ~R 4 each independently represents a hydrogen atom, a fluorine atom, a non-fluorinated alkyl group or alkoxy group, a partially fluorinated alkyl group or alkoxy group, or a completely fluorinated alkyl group or alkoxy group, and a and b each independently represent a positive integer of 0 to 10. The polyether diacid or a salt thereof surfactant provided by the present invention can significantly reduce the surface tension of a polymerization system, improve the stability of an aqueous dispersion of a fluorine-containing polymer, and significantly reduce the amount of a fluorine-containing surfactant used.
Need to check novelty before this filing date? Find Prior Art

Description

cross reference

[0001] This application claims priority from Chinese Patent Application No. 202110653981.X, filed on June 11, 2021, entitled "Polyether diacid or its salt-based surfactant and its use," the entire contents of which are incorporated herein by reference. [Technical field]

[0002] The present invention relates to the technical field of fluorine-containing polymers, and in particular to polyether diacid or salt-based surfactants and their uses. [Background technology]

[0003] Among the many surfactants available, fluorine-containing surfactants have excellent performance, among which perfluorooctanoic acid (PFOA) and its salts (e.g., ammonium salt, sodium salt) are the most widely used types of fluorine-containing surfactants, and their main application is as an auxiliary in the production of fluorine-containing functional polymer materials. In recent years, as PFOA has been widely used, its potential problems of affecting the environment and health have gradually become apparent, and its production and use are being increasingly restricted.

[0004] In terms of molecular structure, fluorine-containing surfactants that can replace PFOA must not only have excellent surface performance that meets the requirements for water repellency, oil repellency, and high surface activity, but also have properties such as low toxicity and easy decomposition that meet the requirements for environmental protection and health. At present, the technical routes for developing PFOA substitutes at home and abroad are mainly divided into two categories: developing fluorocarbon surfactants containing short or branched chains, and introducing ether bonds and methylene groups or similar groups into the fluorocarbon chain.

[0005] In CN101535352A, a fluorine-containing polyether acid or its salt having a number average molecular mass of at least 800 g / mol is used as the main emulsifier, and [R1-O n -LA-] - Y+ Structure (wherein R1 is a linear or branched, partially or fully fluorinated aliphatic group which may contain an ether linkage, n is 0 or 1, L is a non-fluorinated, partially or fully fluorinated, linear or branched alkylene group which may contain an ether linkage, A- is an anion such as a carboxylate, sulfonate, sulfonamide or phosphonate group, and Y + is hydrogen, ammonium, or an alkali metal cation, and R n By using a compound having the formula (I) (wherein the chain length of -L- is 6 atoms or less) or a siloxane surfactant as an auxiliary emulsifier, an aqueous dispersion of a fluorine-containing polymer with good performance is produced, and the amount of the fluorine-containing emulsifier used is less than 0.03% (parts by mass) of the amount of the aqueous dispersion used.

[0006] CN101223228A discloses the use of a non-ionic non-fluorinated emulsifier to produce an aqueous dispersion of a fluorine-containing polymer. The emulsifier used is an emulsifier containing a polyethylene glycol and / or polypropylene glycol segment having 3 to 100 repeating units, and may have the same or different end groups at each end in terms of structure, such as hydroxyl groups, carboxylates, benzoates, acrylates, methacrylates, ethers, hydrocarbons, phenols, functionalized phenols, esters, fatty acid esters, etc.

[0007] The present invention has been made in view of the above. Summary of the Invention

[0008] The present invention provides a polyether diacid or a salt thereof-based surfactant, which is safe to use, environmentally friendly, and easily decomposable, and can replace the use of some fluorine-containing surfactants in fluorine-containing polymers. Another aspect of the present invention provides use of the polyether diacid or a salt thereof-based surfactant.

[0009] Specifically, the present invention provides the following technical solutions:

[0010] The present invention relates to a compound having the general structural formula: XL-(O-CH2CHZ) a -(O-CR 1 R 2 CR 3 R 4 ) b -OLX (In the formula, Z represents H or CH3, L represents a C1 to C5 alkylene group, X represents -COOM or -SO3M, and M represents H + , N.H. 4+ Or Na + R1 to R4 each independently represent a hydrogen atom, a fluorine atom, a non-fluorinated alkyl group or alkoxy group, a partially fluorinated alkyl group or alkoxy group, or a completely fluorinated alkyl group or alkoxy group, and a and b each independently represent a positive integer of 0 to 10. The present invention provides a polyether diacid or salt thereof surfactant represented by the formula:

[0011] In the present invention, it has been unexpectedly discovered that the polyether diacid or a salt thereof surfactant significantly reduces the surface tension of the polymerization system, improves the stability of the aqueous dispersion of the fluorine-containing polymer, and enables a significant reduction in the amount of the fluorine-containing surfactant used.

[0012] In the present invention, the polyether segment of the polyether diacid or its salt surfactant has any chain structure in which the oxygen atoms in the molecular backbone are separated by a saturated hydrocarbon group having two carbon atoms. In the structural formula of the polyether diacid or its salt surfactant, one or more fluorinated hydrocarbon groups may be present. A representative structure has the following repeating unit: -CH2-CH2-O- (2) -CH2-CF2-O- (3) -CF2-CF2-O- (4) -CH2-CCH3-O- (5) -CF2-CCF3-O- (6) -CH2-CH(OCH3)-O- (7) -CH2-CH(CH2OH)-O- (8);

[0013] The polyether diacid or salt thereof surfactant provided by the present invention has two end groups X which are carboxylate or sulfonate groups, and the carboxylate and sulfonate groups may be present in the form of an acid or a salt thereof, and has at least two ether bonds, preferably at least four ether bonds, and even more preferably at least six ether bonds.

[0014] In a preferred embodiment, Z represents H, L represents a C2 alkylene group, X represents -COOM, and M represents NH4 + R 1 ~R 4 each independently represents a hydrogen atom, and a and b each independently represent a positive integer of 1 to 5.

[0015] Furthermore, the polyether diacid or salt thereof surfactant is one or two selected from the following structural formulas: NH 4 OOC-CH2CH2-(O-CH2CH2)3-O-CH2CH2-COONH 4 NH 4 OOC-CH2CH2-(O-CH2CH2)5-O-CH2CH2-COONH 4

[0016] The present invention also provides the use of the polyether diacid or a salt thereof in the production of a fluorine-containing polymer, preferably in the production of an aqueous dispersion of a fluorine-containing polymer.

[0017] The present invention also provides a dispersant comprising the polyether diacid or a salt thereof surfactant, and a fluorine-containing surfactant.

[0018] When the polyether diacid or a salt thereof surfactant provided by the present invention is used as a dispersant, it becomes easy to separate the fluorine-containing polymer from the aqueous dispersion.

[0019] In a preferred embodiment, the fluorine-containing surfactant has the general structural formula: R f -O-CZ1Z2CZ3Z4-X (In the formula, R f represents a C1 to C5 perfluoroalkyl group or an alkoxy group, Z1 to Z4 represent a hydrogen atom or a fluorine atom, X represents -COOM or -SO3M, and M is H + , NH4 + Or Na + Represents.) It is expressed as follows.

[0020] In the present invention, the above-mentioned fluorine-containing surfactant is particularly suitable for use in combination with the polyether diacid or salt thereof surfactant according to the present invention.

[0021] Furthermore, the fluorine-containing surfactant is one or more selected from the following structural formulas: CF3-O-CF(CF3)CF2-O-CH2CH2COOM CF3OCF2OCF2CF2-O-CH2CH2COOM CF3-OCF(CF3)CF2-O-CH2CH2SO3M CF3OCF2OCF2CF2-O-CH2CH2SO3M (wherein M is H + or NH4 + Represents.)

[0022] Further, the fluorine-containing surfactant has the general structural formula: CF3-OCF(CF3)-CF2-O-CH2CH2COONH4 It is expressed as follows.

[0023] In a preferred embodiment, the amount of the fluorine-containing surfactant used is 5 to 50%, and preferably 10 to 30%, based on the total mass of the dispersant.

[0024] In the present invention, when the mass ratio of the polyether diacid or salt thereof surfactant to the fluorine-containing surfactant is within the above range, the surface tension when a mixture of the two is dissolved in water to give a concentration of 2000 ppm is at least 20% lower than the surface tension when the fluorine-containing surfactant is used alone at the same concentration.

[0025] The present invention also provides a method for producing an aqueous dispersion of a fluorine-containing polymer, which comprises using the above-mentioned dispersant as a dispersant and polymerizing at least one fluorine-containing monomer in an aqueous dispersion system.

[0026] In a preferred embodiment, the fluorine-containing monomer is one or more selected from tetrafluoroethylene (TFE), vinylidene fluoride (VDF), and chlorotrifluoroethylene (CTFE).

[0027] In the present invention, the fluorine-containing polymer obtained by polymerization contains one or more comonomers selected from hexafluoropropylene (HFP), perfluoroalkylethylene monomer, and fluorovinyl ether, wherein the perfluoroalkylethylene monomer is one or more selected from tetrafluoroethylene (TFE), hexafluoropropylene (HFP), and vinylidene fluoride (VDF), and the fluorovinyl ether is perfluoroalkylvinyl ether (PAVE), such as perfluoropropylvinyl ether (PPVE), perfluoroethylvinyl ether (PEVE), and perfluoromethylvinyl ether (PMVE).

[0028] In specific embodiments, the comonomers are tetrafluoroethylene and perfluoropropylene, tetrafluoroethylene and perfluoroalkoxyvinyl ether, tetrafluoroethylene, perfluoropropylene and vinylidene fluoride, vinylidene fluoride and perfluoropropylene, vinylidene fluoride and tetrafluoroethylene.

[0029] In a preferred embodiment, the content of the dispersant in water is 10 to 10,000 ppm, preferably 50 to 5,000 ppm, and more preferably 200 to 1,500 ppm.

[0030] In the above technical solution, the water refers to the water for polymerization.

[0031] In a preferred embodiment, the aqueous dispersion of the fluorine-containing polymer is an aqueous dispersion of polytetrafluoroethylene, an aqueous dispersion of polychlorotrifluoroethylene, or an aqueous dispersion of polyvinylidene fluoride.

[0032] Specifically, the above process can be used to produce polytetrafluoroethylene (PTFE) homopolymers and modified PTFE dispersions, which generally have a molecular weight of at least 1×10 8It has a melt viscosity of Pa·s, and at such a high melt viscosity, the flow of the polymer in the molten state is not significant, and it cannot be processed and molded by a melt processing method. Polytetrafluoroethylene homopolymer means a high molecular weight polymer obtained by polymerizing a high purity tetrafluoroethylene monomer, and does not contain a significant comonomer. Modified PTFE means a copolymer obtained by copolymerizing TFE with a low concentration of a second monomer, and the melting point of the resulting polymer is not significantly lower than the melting point of PTFE. The concentration of such comonomer is preferably less than 1 wt%, more preferably less than 0.5 wt%, and it is preferable to use a minimum amount of at least about 0.05 wt% to obtain a significant modification effect. Modified PTFE containing a small amount of comonomer has better film-forming properties in the sintering process. Suitable copolymerized modifying monomers include fluorine-containing olefins and fluorine-containing vinyl ethers, such as perfluoropropylene (HFP) or perfluoroalkyl vinyl ethers (PAVE), preferably perfluoroethyl vinyl ether (PEVE) and perfluoropropyl vinyl ether (PPVE). In addition, it may be modified with a monomer such as chlorotrifluoroethylene (CTFE) or perfluorobutylethylene (PFBE).

[0033] The above-mentioned manufacturing method can also be used to manufacture a dispersion of a melt-processible non-elastomeric fluorine-containing polymer. Examples of such melt-processible non-elastomeric fluorine-containing polymer include polychlorotrifluoroethylene (PCTFE) or copolymers of tetrafluoroethylene (TFE) and at least one fluorinated copolymerizable monomer (comonomer). The fluorinated copolymerizable monomer is present in the polymer in a sufficient amount to make the melting point of the copolymer significantly lower than that of polytetrafluoroethylene (PTFE) homopolymer, for example, to reduce the melting temperature to 315°C or less. Preferred melt-processible non-elastomeric copolymers produced by the process of the present invention contain at least about 40-99 mol % tetrafluoroethylene units and about 1-60 mol % of at least one other unit. Preferred comonomers with TFE are perfluoroolefins having 3-8 carbon atoms, such as hexafluoropropylene (HFP) and perfluoroalkyl vinyl ethers (PAVE).

[0034] The fluorine-containing polymer produced by the method according to the present invention comprises polymerized units from at least one fluorine-containing monomer, and preferably comprises copolymerized units from at least one fluorine-containing monomer and copolymerized units from a second different monomer. The fluorine-containing monomer includes, but is not limited to, a fluorine-containing olefin and a fluorine-containing vinyl ether.

[0035] The production method according to the present invention can also be used to synthesize polyvinylidene fluoride (PVDF) and copolymers of vinylidene fluoride, and also to synthesize polyvinyl fluoride (PVF) and copolymers of vinyl fluoride.

[0036] The present invention also provides an aqueous dispersion of a fluorine-containing polymer produced by the above process. Effect of the Invention

[0037] The polyether diacid or a salt thereof surfactant provided by the present invention significantly reduces the surface tension of a polymerization system, improves the stability of an aqueous dispersion of a fluorine-containing polymer, and enables a significant reduction in the amount of a fluorine-containing surfactant used. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0038] The following examples are intended to illustrate the present invention and are not intended to limit the scope of the invention.

[0039] In the examples, unless otherwise specified, all test means and devices used are common in the art, and those in which specific techniques and conditions are not specifically described in the examples are carried out in accordance with the techniques and conditions described in the literature in the art or the product instructions. Reagents and instruments for which the manufacturer is not specified are all common products that can be purchased through official channels.

[0040] The examples of the present invention were carried out in a vertical or horizontal reactor equipped with an agitator. The polymerization method was batch polymerization. In the polymerization, deionized water was used as a dispersion medium, and TFE in the gas phase was introduced into the water phase under stirring, and the polymerization reaction was caused by sufficient contact with the radical initiator in the water under the action of stirring and dispersing agent. In order to ensure the polymerization rate, it is necessary to ensure the pressure of the monomer in the reactor and to maintain the pressure in the polymerization reactor by replenishing the monomer after the reaction starts. The reactor further includes a cooling jacket surrounding the reactor for controlling the temperature of the polymerization reaction by removing the heat of polymerization with cooling water.

[0041] In a typical polymerization process of PTFE homopolymer and modified PTFE, first, the reactor was charged with deionized water as the polymerization medium and paraffin as the stabilizer. The reactor was sealed, and the oxygen gas in the reactor was replaced with nitrogen gas so that the oxygen content was less than 30 ppm. A part or all of the dispersant was added to disperse it in the deionized water. The agitator was turned on to heat the deionized water in the reactor to the polymerization temperature. After a part or all of the comonomer (e.g., HFP or perfluoroalkyl vinyl ether) was added, TFE was added to pressurize the reactor to the polymerization pressure. A radical initiator solution, e.g., ammonium persulfate solution, was added. Succinic acid was used to reduce the condensation of PTFE homopolymer and modified PTFE. A redox initiator system such as ammonium persulfate / sodium bisulfite may be used, in which case a lower polymerization temperature can be used. After the polymerization started, TFE was continuously added to maintain the stability of the polymerization pressure. At each stage of the polymerization, comonomers, chain transfer agents, and auxiliary agents such as some surfactants, as well as some initiators, can be added depending on the desired product performance.

[0042] When the amount of the monomers added reaches a predetermined value, the addition of TFE is stopped, the operation of the agitator is stopped, the unpolymerized monomers in the reactor are recovered, nitrogen gas is blown into the reactor to replace the atmosphere in the reactor, and the reactor is then emptied. The resulting aqueous dispersion of the fluorine-containing polymer is transferred to a storage tank and awaits further processing. The solid content of the aqueous dispersion of the fluorine-containing polymer produced by the method of the present invention is preferably at least about 10% by weight, more preferably at least about 20% by weight. The solid content of the fluorine-containing polymer produced by the method of the present invention is preferably in the range of about 20% by weight to about 40% by weight, more preferably about 25% by weight to about 35% by weight.

[0043] In a preferred process of the present invention, the total weight of undispersed fluorine-containing polymer (aggregate) produced during the polymerization process is less than 5% by weight, more preferably less than 1% by weight, and most preferably less than 0.5% by weight of the stable fluorine-containing polymer dispersed in water.

[0044] From the aqueous dispersion of the fluorine-containing polymer obtained by the polymerization of the present invention, a fine powder with an average particle size of about 500 μm can be obtained by the method of demulsification and aggregation. Through process flows such as washing and drying, a fluorine-containing dispersion resin product for use in the fields of manufacturing films, fibers, extruded tubes, etc. can be obtained.

[0045] The aqueous dispersion of the fluorine-containing polymer obtained by the polymerization of the present invention can also be sold in the form of an aqueous dispersion. Usually, the initial aqueous dispersion obtained by polymerization is concentrated, but before concentration, a nonionic surfactant is added to stabilize the aqueous dispersion, and then chemical concentration or vacuum concentration is required. The solid content of the aqueous dispersion of the fluorine-containing polymer after concentration is generally about 35% by weight to about 65% by weight.

[0046] The preparation of melt-processable fluorine-containing copolymer may adopt a similar polymerization process, but unlike PTFE homopolymer and modified PTFE, a large amount of comonomer is used. The comonomer may be added to the reactor in batches during the polymerization process, or may be mixed uniformly with TFE monomer and then added continuously to the reactor. In order to improve the melt flow rate of the melt-processable fluorine-containing copolymer, the molecular weight of the copolymer is usually controlled by a chain transfer agent. A stable concentrated aqueous dispersion of fluorine-containing polymer can be prepared by a concentration operation using the same aqueous dispersion of fluorine-containing polymer. The melt-processable fluorine-containing copolymer can also be processed into granules or thin sheets by processes such as flocculation, washing, and drying.

[0047] Example 1 In a 50 L stainless steel reactor equipped with an agitator, 30 kg of deionized water, 1,000 g of paraffin, and NH 4 OOC-CH2CH2-(O-CH2CH2)3-O-CH2CH2-COONH 48g of (surfactant A) and 2g of CF3-OCF(CF3)-CF2-O-CH2CH2COONH4 (fluorine-containing surfactant B) were added, the reactor was sealed, and the system was replaced with nitrogen gas three times so that the oxygen content in the reactor was less than 30 ppm, and the system was replaced with TFE gas twice. The reactor was heated, and when it reached 80°C, TFE was added so that the pressure in the reactor was 2.0 MPa, and an ammonium persulfate solution (aqueous solution obtained by dissolving 60 mg of ammonium persulfate in 100 ml of deionized water) was added by a metering pump, and the stirring speed was set to 100 rpm. After the polymerization reaction started, the internal pressure of the reactor was maintained at 2.0 ± 0.05 MPa by continuously adding TFE. The polymerization heat was removed by flowing cooling water into the reactor jacket, and the polymerization temperature in the reactor was kept stable. When the amount of added TFE reached 1.6 kg, 150 g of a mixed aqueous solution of surfactant A and fluorine-containing surfactant B (surfactant weight ratio 4:1, content 20 wt%) was added by a metering pump. When the amount of consumed TFE reached 13 kg, the addition of monomer and stirring were stopped, and the unreacted monomer in the reactor was collected until micro positive pressure was reached, and the reactor was emptied to terminate the polymerization reaction, and an aqueous dispersion A of PTFE was obtained. The polymer concentration was 29.9 wt%, and the particle size of the primary particles in the aqueous dispersion was 0.23 μm.

[0048] The resulting aqueous dispersion was coagulated with an aqueous solution of saturated ammonium bicarbonate. The polymer was washed several times with warm water and filtered to obtain a polymer powder with an average particle size of 506 μm. It was dried in an oven at 180° C. for 24 hours to obtain 12.85 kg of a white polymer. A standard specific gravity test was performed and the standard specific gravity of the polymer was 2.173.

[0049] Example 2 In a 50 L stainless steel reactor equipped with an agitator, 30 kg of deionized water, 1,000 g of paraffin, and NH 4 OOC-CH2CH2-(O-CH2CH2)3-O-CH2CH2-COONH 44g of (surfactant A) and 1g of CF3-OCF(CF3)-CF2-O-CH2CH2COONH4 (surfactant B) were added, the reactor was sealed, and the system was replaced with nitrogen gas three times so that the oxygen content in the reactor was less than 30 ppm, and the system was replaced with TFE gas twice. The reactor was heated, and when it reached 80°C, TFE was added so that the pressure in the reactor was 2.0 MPa, and an ammonium persulfate solution (aqueous solution obtained by dissolving 60 mg of ammonium persulfate in 100 ml of deionized water) was added by a metering pump, and the stirring speed was set to 100 rpm. After the polymerization reaction started, the internal pressure of the reactor was maintained at 2.0 ± 0.05 MPa by continuously adding TFE. The polymerization heat was removed by flowing cooling water into the reactor jacket, and the polymerization temperature in the reactor was kept stable. When the amount of added TFE reached 1.6 kg, 75 g of a mixed aqueous solution of surfactant A and fluorine-containing surfactant B (surfactant weight ratio 4:1, content 20 wt%) was added by a metering pump. When the amount of consumed TFE reached 13 kg, the addition of monomer and stirring were stopped, and the unreacted monomer in the reactor was collected until micro positive pressure was reached, and the reactor was emptied to terminate the polymerization reaction, and an aqueous dispersion A of PTFE was obtained. The polymer concentration was 29.6 wt%, and the particle size of the primary particles in the aqueous dispersion was 0.26 μm.

[0050] The resulting aqueous dispersion was coagulated with an aqueous solution of saturated ammonium bicarbonate. The polymer was washed several times with warm water and filtered to obtain a polymer powder with an average particle size of 557 μm. It was dried in an oven at 180° C. for 24 hours to obtain 12.72 kg of a white polymer. A standard specific gravity test was performed and the standard specific gravity of the polymer was 2.172.

[0051] Example 3 In a 50 L stainless steel reactor equipped with an agitator, 30 kg of deionized water, 1,000 g of paraffin, and NH 4 OOC-CH2CH2-(O-CH2CH2)5-O-CH2CH2-COONH 44g of (surfactant A) and 1g of CF3-OCF(CF3)-CF2-O-CH2CH2COONH4 (surfactant B) were added, the reactor was sealed, and the system was replaced with nitrogen gas three times so that the oxygen content in the reactor was less than 30 ppm, and the system was replaced with TFE gas twice. The reactor was heated, and when it reached 80°C, TFE was added so that the pressure in the reactor was 2.0 MPa, and an ammonium persulfate solution (aqueous solution obtained by dissolving 60 mg of ammonium persulfate in 100 ml of deionized water) was added by a metering pump, and the stirring speed was set to 100 rpm. After the polymerization reaction started, the internal pressure of the reactor was maintained at 2.0 ± 0.05 MPa by continuously adding TFE. The polymerization heat was removed by flowing cooling water into the reactor jacket, and the polymerization temperature in the reactor was kept stable. When the amount of TFE added reached 1.6 kg, 75 g of a mixed aqueous solution of surfactant A and fluorine-containing surfactant B (surfactant weight ratio 4:1, content 20 wt%) was added by a metering pump. When the amount of TFE consumed reached 13 kg, the addition of monomer and stirring were stopped, and the unreacted monomer in the reactor was collected until micro positive pressure was reached, and the reactor was emptied to terminate the polymerization reaction, obtaining an aqueous dispersion A of PTFE. The polymer concentration was 29.7 wt%, and the particle size of the primary particles in the aqueous dispersion was 0.25 μm.

[0052] The resulting aqueous dispersion was coagulated with an aqueous solution of saturated ammonium bicarbonate. The polymer was washed several times with warm water and filtered to obtain a polymer powder with an average particle size of 536 μm. It was dried in an oven at 180° C. for 24 hours to obtain 12.75 kg of a white polymer. A standard specific gravity test was performed to find that the standard specific gravity of the polymer was 2.170.

[0053] Example 4 In a 50 L stainless steel reactor equipped with an agitator, 30 kg of deionized water, 1,000 g of paraffin, and NH 4 OOC-CH2CH2-(O-CH2CH2)5-O-CH2CH2-COONH 44g of (surfactant A) and 1g of CF3-OCF(CF3)-CF2-O-CH2CH2COONH4 (surfactant B) were added, the reactor was sealed, and the system was replaced with nitrogen gas three times so that the oxygen content in the reactor was less than 30 ppm, and the system was replaced with TFE gas twice. 8g of perfluoropropylene was added, the reactor was heated, and when it reached 80°C, TFE was added so that the pressure in the reactor was 2.0 MPa, and an ammonium persulfate solution (aqueous solution obtained by dissolving 80mg of ammonium persulfate in 100ml of deionized water) was added by a metering pump, and the stirring speed was set to 80 rpm. After the polymerization reaction started, the internal pressure of the reactor was maintained at 2.0±0.05 MPa by continuously adding TFE. The polymerization heat was removed by flowing cooling water into the reactor jacket, and the polymerization temperature in the reactor was kept stable. When the amount of added TFE reached 1.6 kg, 75 g of a mixed aqueous solution of 20 wt% surfactant A and fluorine-containing surfactant B (surfactant weight ratio 4:1) was added by a metering pump. When the amount of TFE consumed reached 13 kg, the addition of monomer and stirring were stopped, and the unreacted monomer in the reactor was collected until micro positive pressure was reached, and the reactor was emptied to terminate the polymerization reaction, thereby obtaining an aqueous dispersion A of PTFE. The polymer concentration was 29.9 wt%, and the particle size of the primary particles in the aqueous dispersion was 0.25 μm.

[0054] The resulting aqueous dispersion was coagulated with an aqueous solution of saturated ammonium bicarbonate. The polymer was washed several times with warm water and filtered to obtain a polymer powder with an average particle size of 533 μm. It was dried in an oven at 180° C. for 24 hours to obtain 12.83 kg of a white polymer. A standard specific gravity test showed that the standard specific gravity of the polymer was 2.176 and the extrusion pressure was 23.2 MPa.

[0055] Example 5 In a 50 L stainless steel reactor equipped with an agitator, 30 kg of deionized water, 1,000 g of paraffin, and NH 4 OOC-CH2CH2-(O-CH2CH2)5-O-CH2CH2-COONH 44g of (surfactant A) and 1g of CF3-OCF(CF3)-CF2-O-CH2CH2COONH4 (surfactant B) were added, the reactor was sealed, and the system was replaced with nitrogen gas three times so that the oxygen content in the reactor was less than 30 ppm, and the system was replaced with TFE gas twice. 6g of perfluoropropyl vinyl ether (PPVE) was added, the reactor was heated, and when it reached 80°C, TFE was added so that the pressure in the reactor was 2.0 MPa, and an ammonium persulfate solution (aqueous solution obtained by dissolving 80 mg of ammonium persulfate in 100 ml of deionized water) was added by a metering pump, and the stirring speed was set to 80 rpm. After the polymerization reaction started, the internal pressure of the reactor was maintained at 2.0 ± 0.05 MPa by continuously adding TFE. The polymerization heat was removed by flowing cooling water into the reactor jacket, and the polymerization temperature in the reactor was kept stable. When the amount of added TFE reached 1.6 kg, 75 g of a mixed aqueous solution of 20 wt% surfactant A and fluorine-containing surfactant B (surfactant weight ratio 4:1) was added by a metering pump. When the amount of consumed TFE reached 13 kg, the addition of monomer and stirring were stopped, and the unreacted monomer in the reactor was collected until micro positive pressure was reached, and the reaction vessel was emptied to terminate the polymerization reaction, thereby obtaining an aqueous dispersion A of PTFE. The polymer concentration was 29.8 wt%, and the particle size of the primary particles in the aqueous dispersion was 0.24 μm.

[0056] The resulting aqueous dispersion was coagulated with an aqueous solution of saturated ammonium bicarbonate. The polymer was washed several times with warm water and filtered to obtain a polymer powder with an average particle size of 566 μm. It was dried in an oven at 180° C. for 24 hours to obtain 12.81 kg of a white polymer. A standard specific gravity test showed that the standard specific gravity of the polymer was 2.160 and the extrusion pressure was 24.1 MPa.

[0057] Comparative Example 1 In a 50L stainless steel reactor equipped with an agitator, 30 kg of deionized water, 1000 g of paraffin, and 410 g of CF3-OCF(CF3)-CF2-O-CH2CH2COONH were added, the reactor was sealed, and the system was replaced with nitrogen gas three times so that the oxygen content in the reactor was less than 30 ppm, and the system was replaced with TFE gas twice. The reactor was heated, and when it reached 80°C, TFE was added so that the pressure in the reactor was 2.0 MPa, and an ammonium persulfate solution (an aqueous solution obtained by dissolving 60 mg of ammonium persulfate in 100 ml of deionized water) was added by a metering pump, and the stirring speed was set to 100 rpm. After the polymerization reaction started, the internal pressure of the reactor was maintained at 2.0 ± 0.05 MPa by continuously adding TFE. The polymerization heat was removed by flowing cooling water into the reactor jacket, and the polymerization temperature in the reactor was kept stable. When the amount of TFE added reached 1.6 kg, 150 g of 20 wt% ammonium perfluorooctanoate aqueous solution was added by a metering pump. When the amount of TFE consumed reached 13 kg, the addition of monomer and stirring were stopped, and the unreacted monomer in the reactor was recovered until micro positive pressure was reached, and the reactor was emptied to terminate the polymerization reaction, obtaining an aqueous dispersion A of PTFE. The polymer concentration was 29.7 wt%, and the particle size of the primary particles in the aqueous dispersion was 0.25 μm.

[0058] The resulting aqueous dispersion was coagulated with an aqueous solution of saturated ammonium bicarbonate. The polymer was washed several times with warm water and filtered to obtain a polymer powder with an average particle size of 535 μm. It was dried in an oven at 180° C. for 24 hours to obtain 12.75 kg of a white polymer. A standard specific gravity test was performed and the standard specific gravity of the polymer was 2.169.

[0059] Comparative Example 2 In a 50L stainless steel reactor equipped with an agitator, 30 kg of deionized water, 1000 g of paraffin, and 410 g of CF3-OCF(CF3)-CF2-O-CH2CH2COONH were added, the reactor was sealed, and the system was replaced with nitrogen gas three times so that the oxygen content in the reactor was less than 30 ppm, and the system was replaced with TFE gas twice. 8 g of perfluoropropylene was added, the reactor was heated, and when it reached 80°C, TFE was added so that the pressure in the reactor was 2.0 MPa, and an ammonium persulfate solution (a solution obtained by dissolving 80 mg of ammonium persulfate in 100 ml of deionized water) was added by a metering pump, and the stirring speed was set to 80 rpm. After the polymerization reaction started, the internal pressure of the reactor was maintained at 2.0 ± 0.05 MPa by continuously adding TFE. The polymerization heat was removed by flowing cooling water into the reactor jacket, and the polymerization temperature in the reactor was kept stable. When the amount of TFE added reached 1.6 kg, 150 g of 20 wt% ammonium perfluorooctanoate aqueous solution was added by a metering pump. When the amount of TFE consumed reached 13 kg, the addition of monomer and stirring were stopped, and the unreacted monomer in the reactor was recovered until micro positive pressure was reached, and the reactor was emptied to terminate the polymerization reaction, obtaining an aqueous dispersion A of PTFE. The polymer concentration was 30.0 wt%, and the particle size of the primary particles in the aqueous dispersion was 0.23 μm.

[0060] The resulting aqueous dispersion was coagulated with an aqueous solution of saturated ammonium bicarbonate. The polymer was washed several times with warm water and filtered to obtain a polymer powder with an average particle size of 546 μm. It was dried in an oven at 180° C. for 24 hours to obtain 12.85 kg of a white polymer. A standard specific gravity test showed that the polymer had a standard specific gravity of 2.175 and an extrusion pressure of 23.5 MPa.

[0061] Comparative Example 3 In a 50L stainless steel reactor equipped with an agitator, 30 kg of deionized water, 1000 g of paraffin, and 410 g of CF3-OCF(CF3)-CF2-O-CH2CH2COONH were added, the reactor was sealed, and the system was replaced with nitrogen gas three times so that the oxygen content in the reactor was less than 30 ppm, and the system was replaced with TFE gas twice. 6.0 g of perfluoropropyl vinyl ether (PPVE) was added, the reactor was heated, and when it reached 80°C, TFE was added so that the pressure in the reactor was 2.0 MPa, and an ammonium persulfate solution (a solution obtained by dissolving 80 mg of ammonium persulfate in 100 ml of deionized water) was added by a metering pump, and the stirring speed was set to 80 rpm. After the polymerization reaction started, the internal pressure of the reactor was maintained at 2.0 ± 0.05 MPa by continuously adding TFE. The polymerization heat was removed by flowing cooling water into the reactor jacket, and the polymerization temperature in the reactor was kept stable. When the amount of TFE added reached 1.6 kg, 150 g of 20 wt% ammonium perfluorooctanoate aqueous solution was added by a metering pump. When the amount of TFE consumed reached 13 kg, the addition of monomer and stirring were stopped, and the unreacted monomer in the reactor was recovered until micro positive pressure was reached, and the reactor was emptied to terminate the polymerization reaction, obtaining an aqueous dispersion A of PTFE. The polymer concentration was 29.9 wt%, and the particle size of the primary particles in the aqueous dispersion was 0.25 μm.

[0062] The resulting aqueous dispersion was coagulated with an aqueous solution of saturated ammonium bicarbonate. The polymer was washed several times with warm water and filtered to obtain a polymer powder with an average particle size of 527 μm. It was dried in an oven at 180° C. for 24 hours to obtain 12.8 kg of a white polymer. A standard specific gravity test showed that the standard specific gravity of the polymer was 2.157 and the extrusion pressure was 25.2 MPa. Although the present invention has been described in detail above through a general description, a mode for carrying out the invention, and tests, it is obvious to those skilled in the art that some modifications or improvements may be made based on the present invention. Therefore, all of these modifications and improvements made within the scope of the present invention are included in the scope of protection that the present invention is intended to protect. [Industrial Applicability]

[0063] The present invention provides a polyether diacid or its salt surfactant and its use. The polyether diacid or its salt surfactant has the general structural formula: XL-(O-CH2CHZ) a -(O-CR 1 R 2 CR 3 R 4 ) b -OLX (wherein Z represents H or CH3, L represents a C1 to C5 alkylene group, X represents -COOM or -SO3M, and M represents H + , NH4 + Or Na + R 1 ~R 4 each independently represents a hydrogen atom, a fluorine atom, a non-fluorinated alkyl group or alkoxy group, a partially fluorinated alkyl group or alkoxy group, or a completely fluorinated alkyl group or alkoxy group, and a and b each independently represent a positive integer of 0 to 10. The polyether diacid or salt thereof surfactant provided by the present invention can significantly reduce the surface tension of a polymerization system, improve the stability of an aqueous dispersion of a fluorine-containing polymer, and significantly reduce the amount of a fluorine-containing surfactant used, and has good economic value and application prospects.

Claims

1. General structural formula: X-L-(O-CH 2 C.H.Z. a -(O-CR 1 R 2 CR 3 R 4 ) b -O-L-X (Wherein, Z is H or CH 3 L represents C 1 ~C 5 represents an alkylene group represented by the formula: 3 M, where M is H + , N.H. 4 + Or Na + represents R 1 ~R 4 each independently represents a hydrogen atom, a fluorine atom, a non-fluorinated alkyl group or alkoxy group, a partially fluorinated alkyl group or alkoxy group, or a completely fluorinated alkyl group or alkoxy group, and a and b each independently represent a positive integer of 0 to 10. A polyether diacid or a salt thereof surfactant, characterized in that:

2. Z represents H and L represents C 2 X represents -COOM, and M represents NH 4 + represents R 1 ~R 4 each independently represents a hydrogen atom; and a and b each independently represent a positive integer of 1 to 5. The polyether diacid or salt thereof surfactant according to claim 1 .

3. 3. The polyether diacid or salt thereof surfactant according to claim 2, wherein the polyether diacid or salt thereof surfactant is one or two selected from the following structural formulas: N.H. 4 OOC-CH 2 CH 2 -(O-CH 2 CH 2 ) 3 -O-CH 2CH 2 -COONH 4 N.H. 4 OOC-CH 2 CH 2 -(O-CH 2 CH 2 ) 5 -O-CH 2 CH 2 -COONH 4

4. Use of the polyether diacid or salt thereof surfactant according to any one of claims 1 to 3 in the production of a fluorine-containing polymer, preferably in the production of an aqueous dispersion of a fluorine-containing polymer.

5. A dispersant comprising the polyether diacid or salt thereof surfactant according to any one of claims 1 to 3 and a fluorine-containing surfactant, Preferably, the fluorine-containing surfactant has the general structural formula: R f -O-CZ 1 Z 2 CZ 3 Z 4 -X (In the formula, R f is C 1 ~C 5 represents a perfluoroalkyl group or an alkoxy group represented by the formula: 1 ~Z 4 represents a hydrogen atom or a fluorine atom, and X is -COOM or -SO 3 Represents M, M is H + , N.H. 4 + Or Na + Represents.) It is expressed by More preferably, the fluorine-containing surfactant is one or more selected from the following structural formulas: CF 3 -O-CF(CF 3 ) CF 2 -O-CH 2 CH 2 COOM CF 3 O.C.F. 2 O.C.F. 2 CF 2 -O-CH 2 CH 2 COOM CF 3 -OCF (CF 3 ) CF 2 -O-CH 2 CH 2 SO 3 M CF 3 O.C.F. 2 O.C.F. 2 CF 2 -O-CH 2 CH 2 SO 3 M (Wherein, M is H + or NH 4 + Represents.) Most preferably, the fluorine-containing surfactant has the structural formula: CF 3 -OCF (CF 3 )-CF 2 -O-CH 2 CH 2 COONH 4 A dispersant characterized by being represented by the formula:

6. The dispersant according to claim 5, characterized in that the amount of the fluorine-containing surfactant used is 5 to 50%, preferably 10 to 30%, based on the total mass of the dispersant.

7. A method for producing an aqueous dispersion of a fluorine-containing polymer, comprising polymerizing at least one fluorine-containing monomer in an aqueous dispersion system using the dispersant according to claim 5 or 6 as a dispersant.

8. The method according to claim 7, characterized in that the content of the dispersant in water is 10 to 10,000 ppm, preferably 50 to 5,000 ppm.

9. 9. The method according to claim 7, wherein the aqueous dispersion of a fluorine-containing polymer is an aqueous dispersion of polytetrafluoroethylene, an aqueous dispersion of polychlorotrifluoroethylene, or an aqueous dispersion of polyvinylidene fluoride.

10. An aqueous dispersion of a fluorine-containing polymer, which is produced by the method according to any one of claims 7 to 9.

Citation Information

Patent Citations

  • Fluoropolymer dispersion liquid

    JP2003286379A

  • Electrolytic capacitor and electrolyte therefor

    JP2004071727A

  • Dispersion including fluoropolymer particle

    JP2010159430A

  • Electrolyte for electrolytic capacitor

    JP2015019015A