High strength, highly elongated and highly thermally conductive aluminum casting alloy and its method of manufacture
A high-strength, high-elongation, and high-thermal-conductivity aluminum casting alloy is produced by controlling the phase transformation of β-Al5FeSi to α-AlFeSi through specific composition and cooling processes, addressing the challenges of existing alloys and enhancing mechanical and thermal properties.
Patent Information
- Application Number
- JP2024522558
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2022-10-17
- Filing Date
- 2022-10-18
- Publication Date
- 2024-10-29
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing aluminum casting alloys face challenges in achieving high strength, high elongation, and high thermal conductivity due to the formation of coarse, acicular β-Al5FeSi phases, which reduce ductility and conductivity, and there is a lack of effective methods to control these phases.
An aluminum casting alloy with a composition of 6.5% to 11.5% silicon, 0.2% to 0.4% magnesium, 0.32% to 0.85% iron, and a cubic crystal structure α-AlFeSi intermetallic compound, along with additives like manganese and cobalt, is produced by applying external energy at temperatures higher than the liquidus temperature and controlling the cooling rate to convert β-Al5FeSi to α-AlFeSi.
The method results in an alloy with improved strength, elongation, and thermal conductivity, achieving yield strengths of 100-140 MPa, ultimate tensile strengths of 180-220 MPa, elongation rates of 2.5%-8.5%, and thermal conductivity of 160-190 W/mK, while reducing the negative effects of β-Al5FeSi phases.
Smart Images

Figure 2024539658000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to an aluminum alloy and a method for producing the same, and more particularly to an aluminum casting alloy with high strength, high elongation and high thermal conductivity, and a method for producing the same. [Background technology]
[0002] Due to environmental regulations and the demand for improved fuel efficiency, the market for electric power-based automobiles is expanding rapidly. In the case of electric power-based automobiles, weight reduction technology is essential to ensure driving distance due to the increase in batteries, electrical components, and safety components. In particular, it is important to ensure the high heat dissipation properties of aluminum, which directly affects the performance and lifespan of the finished main electrical module. There is an absolute lack of material technology for high-performance aluminum casting that takes into account the properties of "high strength vs. high elongation," "high strength vs. high thermal conductivity," and "high fluidity vs. high thermal conductivity," which are generally in conflicting relationships in aluminum alloys.
[0003] Meanwhile, it has been reported that recycling aluminum can save about 95% of the energy required to make the metal from pure raw materials. Despite these strong economic and environmental advantages, aluminum alloys accumulate Fe as a major impurity at levels of 0.4-0.8 wt.%, during the recycling process, which acts as a cause of limiting scrap use in many automotive parts industries by reducing the ductility of the material.
[0004] It has been reported that if a small amount of Fe is present in an Al-Si alloy, the β-Al5FeSi phase, an Fe-based intermetallic compound that has low cohesive strength with the aluminum matrix and is hard and brittle, is formed. For example, when 0.4 wt% or more of Fe is added to an Al-7Si alloy, a coarse needle-like β-Al5FeSi phase reaching several hundred μm is formed before the Al-Si eutectic reaction during solidification. In actual practice, attempts have been made to improve the β-Al5FeSi intermetallic compound by using chemical additives (e.g., Mn, Co, Cr, Mo) to neutralize it. However, such research has been limited to reports on the phenomena, and there has been no research on the control mechanism of the formed phase and its relationship with physical / mechanical properties.
[0005] Related prior art documents include Korean Patent Publication No. 10-2016-0048777. Summary of the Invention [Problem to be solved by the invention]
[0006] The technical problem to be solved by the present invention is to provide an aluminum casting alloy with high strength, high elongation and high thermal conductivity, and to provide a manufacturing method thereof. As described above, the formation of coarse acicular β-Al5FeSi phases can have a detrimental effect on the strength, ductility and conductivity of the material, but by changing the concept, the present invention aims to provide an aluminum casting alloy that can increase 'strength and elongation' at the same time by controlling the formation phase of such Fe-based intermetallic compounds, and to provide a manufacturing method thereof. [Means for solving the problem]
[0007] In order to solve the above problems, one embodiment of the present invention provides an aluminum casting alloy with high strength, high elongation and high thermal conductivity, which contains 6.5 wt % to 11.5 wt % silicon (Si); 0.2 wt % to 0.4 wt % magnesium (Mg); 0.32 wt % to 0.85 wt % iron (Fe); and the balance being aluminum (Al) and unavoidable impurities, and contains an α-AlFeSi intermetallic compound having a cubic crystal structure in an aluminum matrix.
[0008] In the high strength, highly elongated and high thermal conductivity aluminum casting alloy, the α-AlFeSi intermetallic compound having a cubic crystal structure has the same crystal structure as the α-AlMnSi phase, but does not contain Mn and can undergo a phase change from the β-Al5FeSi intermetallic compound.
[0009] In the high strength, high elongation and high thermal conductivity aluminum casting alloy, the aluminum casting alloy is characterized in that it does not contain manganese (Mn), cobalt (Co), chromium (Cr) or molybdenum (Mo) as an additive for neutralizing the β-Al5FeSi intermetallic compound. Neutralizing the β-Al5FeSi intermetallic compound includes controlling the shape of the β-Al5FeSi intermetallic compound or reducing brittleness through phase transformation.
[0010] In the high-strength, highly elongated and highly thermally conductive aluminum casting alloy, the α-AlFeSi intermetallic compound may have a composition of Al: 74.9 to 86.7 at.%, Fe: 6.9 to 14.3 at.%, and Si: 6.2 to 11.3 at.%.
[0011] The high strength, high elongation and high thermal conductivity aluminum casting alloy may have a yield strength in the range of 100 MPa to 140 MPa, an ultimate tensile strength in the range of 180 MPa to 220 MPa, an elongation in the range of 2.5% to 8.5%, and a thermal conductivity in the range of 160 W / mK to 190 W / mK.
[0012] In order to solve the above problems, a method for producing an aluminum casting alloy having high strength, high elongation and high thermal conductivity according to one embodiment of the present invention includes a first step of providing a molten aluminum casting alloy containing 6.5 wt % to 11.5 wt % silicon (Si); 0.2 wt % to 0.4 wt % magnesium (Mg); 0.32 wt % to 0.85 wt % iron (Fe); and the balance being aluminum (Al) and unavoidable impurities; and a second step of applying external energy at a temperature higher than the liquidus temperature of the molten aluminum casting alloy, followed by cooling, so as to contain an α-AlFeSi intermetallic compound having a cubic crystal structure in an aluminum matrix.
[0013] In the manufacturing method of the high strength, highly elongated and high thermal conductivity aluminum casting alloy, the second step may include a step of maintaining the molten aluminum casting alloy at a temperature 200°C to 300°C higher than the liquidus temperature, and then cooling the molten aluminum casting alloy at a cooling rate of 1 K / sec or more.
[0014] In the manufacturing method of the high strength, highly elongated and high thermal conductivity aluminum casting alloy, the second step may include a step of maintaining the molten aluminum casting alloy at a temperature 100°C to 150°C higher than the liquidus temperature, and then cooling the molten aluminum casting alloy at a cooling rate of 10 K / sec or more.
[0015] The method for producing the high-strength, highly elongated and highly thermally conductive casting aluminum alloy may be characterized in that the molten aluminum casting alloy is maintained at a temperature higher than the liquidus temperature for 1 to 2 hours.
[0016] The method for producing the high-strength, highly elongated and high-thermal conductivity aluminum casting alloy may be characterized in that the molten aluminum casting alloy is maintained at a temperature higher than the liquidus temperature by applying ultrasonic waves for 1 to 2 minutes.
[0017] In the method for producing the high strength, high elongation and high thermal conductivity aluminum casting alloy, the second step may include a step of changing a phase from a β-AlFeSi intermetallic compound having a monoclinic crystal structure to an α-AlFeSi intermetallic compound having a cubic crystal structure.
[0018] In the manufacturing method of the high strength, highly elongated and high thermal conductivity aluminum casting alloy, in the second step, the generation of the β-Al5FeSi intermetallic compound occurs prior to the Al-Si eutectic reaction, and the α-Al phase, which is an aluminum matrix, can be generated prior to the generation of the β-Al5FeSi intermetallic compound.
[0019] In order to solve the above problems, a high-strength, highly elongated and highly thermally conductive aluminum casting alloy according to another embodiment of the present invention contains 6.5 wt % to 11.5 wt % silicon (Si); 0.2 wt % to 0.4 wt % magnesium (Mg); 0.2 wt % to 0.3 wt % iron (Fe); and the balance being aluminum (Al) and unavoidable impurities, and contains an α-AlFeSi intermetallic compound having a cubic crystal structure in an aluminum matrix.
[0020] In order to solve the above problems, a method for producing an aluminum casting alloy having high strength, high elongation and high thermal conductivity according to another embodiment of the present invention includes a first step of providing a molten aluminum casting alloy containing 6.5 wt % to 11.5 wt % silicon (Si); 0.2 wt % to 0.4 wt % magnesium (Mg); 0.2 wt % to 0.3 wt % iron (Fe); and the balance being aluminum (Al) and unavoidable impurities; and a second step of applying external energy at a temperature higher than the liquidus temperature of the molten aluminum casting alloy, followed by cooling, so as to contain an α-AlFeSi intermetallic compound having a cubic crystal structure in an aluminum matrix. Effect of the Invention
[0021] According to the embodiment of the present invention, it is possible to realize an aluminum casting alloy with high strength, high elongation and high thermal conductivity, and a manufacturing method thereof. According to the embodiment, it is possible to realize an aluminum casting alloy that improves strength while increasing the allowable iron (Fe) content level of the aluminum casting material, and a manufacturing method thereof without reducing the elongation rate. Specifically, it is possible to realize an aluminum casting alloy with high strength, high elongation and high thermal conductivity, and a manufacturing method thereof, which can simultaneously improve conflicting properties such as strength, conductivity, and ductility, by applying external energy that can disrupt the structure (e.g., bonding, clustering) of the aluminum liquid metal for casting to the liquid metal, to control the generated phase such as an intermetallic compound, and induce changes in the type, size, and distribution of the crystallized phase and intermetallic compound generated during solidification.
[0022] Of course, the scope of the present invention is not limited to such effects. [Brief description of the drawings]
[0023] [Figure 1] FIG. 1 is a diagram showing a liquidus projection of the Al-Si-Fe ternary system. [Diagram 2] FIG. 2 is a schematic diagram showing a step mold used to form an aluminum alloy casting according to an example of the present invention. [Diagram 3] 3 is a photograph showing the microstructure of an aluminum casting alloy according to a cooling rate in an experimental example of the present invention. [Figure 4] 3 is a photograph showing the microstructure of an aluminum casting alloy according to a cooling rate in an experimental example of the present invention. [Figure 5A] 4 is a graph showing the morphology of a microstructure according to the temperature and method of applying external energy and the cooling rate in an experimental example of the present invention. [Figure 5B] 1 is a graph showing the morphology of a microstructure of an aluminum casting alloy according to an experimental example of the present invention, depending on the time the alloy was kept at a molten temperature of 800° C. [Figure 5C] FIG. 2 is a diagram showing a backscattered electron image of an aluminum casting alloy heated to a molten temperature of 600 to 800° C. and solidified at a cooling rate of 0.8 K / s in an experimental example of the present invention. [Figure 6] FIG. 1 shows backscattered electron images and three-dimensional microstructures for the alloy solidified at a cooling rate of 2.2 K / s after each liquidus step. [Figure 7] FIG. 1 shows backscattered electron images and three-dimensional microstructures for the alloy solidified at a cooling rate of 2.2 K / s after each liquidus step. [Figure 8] FIG. 1 shows backscattered electron images and three-dimensional microstructures for the alloy solidified at a cooling rate of 2.2 K / s after each liquidus step. [Figure 9] FIG. 1 shows backscattered electron images and three-dimensional microstructures for the alloy solidified at a cooling rate of 2.2 K / s after each liquidus step. [Figure 10] FIG. 1 shows backscattered electron images and three-dimensional microstructures for the alloy solidified at a cooling rate of 2.2 K / s after each liquidus step. [Figure 11] FIG. 1 shows backscattered electron images and three-dimensional microstructures for the alloy solidified at a cooling rate of 2.2 K / s after each liquidus step. [Figure 12] FIG. 1 shows backscattered electron images and three-dimensional microstructures for the alloy solidified at a cooling rate of 2.2 K / s after each liquidus step. [Figure 13] 1 is a photograph showing an analysis of the crystal structure of a β-Al5FeSi intermetallic compound in a manufacturing method of an aluminum casting alloy according to the present invention. [Figure 14] 1 is a photograph showing an analysis of the crystal structure of an α-AlFeSi intermetallic compound in a manufacturing method of an aluminum casting alloy according to the present invention. [Figure 15] FIG. 2 is a diagram showing the physical properties of the casting aluminum alloy according to the above-mentioned experimental example A of the present invention. [Figure 16]FIG. 2 is a diagram showing the physical properties of the casting aluminum alloy according to the above-mentioned experimental example A of the present invention. [Figure 17] FIG. 2 is a diagram showing the physical properties of the casting aluminum alloy according to the above-mentioned experimental example A of the present invention. [Figure 18] FIG. 2 is a diagram showing the physical properties of the casting aluminum alloy according to the above-mentioned experimental example A of the present invention. [Figure 19] FIG. 2 is a diagram showing the physical properties of the casting aluminum alloy according to the above-mentioned experimental example A of the present invention. [Figure 20] FIG. 2 is a diagram showing the physical properties of the casting aluminum alloy according to the above-mentioned experimental example A of the present invention. [Figure 21] FIG. 2 is a diagram showing the physical properties of the casting aluminum alloy according to the above-mentioned experimental example A of the present invention. [Figure 22] FIG. 2 is a diagram showing the physical properties of the casting aluminum alloy according to the above-mentioned experimental example A of the present invention. [Figure 23] FIG. 2 is a diagram showing the physical properties of the casting aluminum alloy according to the above-mentioned experimental example A of the present invention. [Figure 24] FIG. 2 is a diagram showing the physical properties of the casting aluminum alloy according to the above-mentioned experimental example A of the present invention. [Diagram 25] FIG. 2 is a diagram showing the physical properties of the casting aluminum alloy according to the above-mentioned experimental example A of the present invention. [Figure 26] FIG. 2 is a diagram showing the physical properties of the casting aluminum alloy according to the above-mentioned experimental example A of the present invention. [Figure 27] FIG. 2 is a diagram showing the physical properties of the casting aluminum alloy according to the above-mentioned experimental example A of the present invention. [Figure 28] FIG. 2 is a diagram showing the physical properties of the casting aluminum alloy according to the above-mentioned experimental example A of the present invention. [Figure 29] FIG. 2 is a diagram showing the physical properties of the casting aluminum alloy according to the above-mentioned experimental example A of the present invention. [Diagram 30] FIG. 2 is a diagram showing the physical properties of the casting aluminum alloy according to the above-mentioned experimental example A of the present invention. [Diagram 31] FIG. 2 is a diagram showing the physical properties of the casting aluminum alloy according to the above-mentioned experimental example A of the present invention. [Diagram 32] FIG. 2 is a diagram showing the physical properties of the casting aluminum alloy according to the above-mentioned experimental example A of the present invention. [Diagram 33] 1 shows photographs of the microstructure of aluminum immediately after casting (as cast) depending on the cooling rate in Experimental Examples 11 to 13 of the present invention. [Diagram 34] 1 shows photographs of the microstructure of aluminum immediately after casting (as cast) depending on the cooling rate in Experimental Examples 11 to 13 of the present invention. [Diagram 35] 1 shows photographs of microstructures immediately after casting of aluminum at different cooling rates in Experimental Examples 14 to 16 of the present invention. [Diagram 36] 1 shows photographs of microstructures immediately after casting of aluminum at different cooling rates in Experimental Examples 14 to 16 of the present invention. [Figure 37] 1 is a graph comparing the tensile properties immediately after casting of aluminum depending on the cooling rate in Experimental Examples 14 to 16 of the present invention. [Figure 38] 1 is a graph comparing thermal conductivity characteristics immediately after casting of aluminum at different cooling rates in Experimental Examples 14 to 16 of the present invention. [Figure 39] 1 is a graph comparing thermal conductivity characteristics immediately after casting of aluminum at different cooling rates in Experimental Examples 14 to 16 of the present invention. [Diagram 40] 1 is a graph comparing thermal conductivity characteristics immediately after casting of aluminum at different cooling rates in Experimental Examples 14 to 16 of the present invention. [Diagram 41] FIG. 41 shows photographs of the microstructure of an aluminum casting alloy according to the cooling rate in another modified embodiment (Table 7) of the present invention. [Diagram 42] FIG. 42 shows the as-cast tensile properties of an aluminum casting alloy according to another modified embodiment of the present invention (Table 7). [Diagram 43] FIG. 43 shows the electrical conductivity characteristics of the aluminum casting alloy according to another modified embodiment of the present invention (Table 7) after T6 heat treatment. BEST MODE FOR CARRYING OUT THEINVENTION
[0024] A high strength, high elongation and high thermal conductivity aluminum casting alloy and a manufacturing method thereof according to an embodiment of the present invention will be described in detail. The terms used below are appropriately selected in consideration of the functions of the present invention, and the definitions of such terms should be based on the contents of the entire specification.
[0025] In the present invention, external energy capable of destroying the structure (e.g., bonding, clustering) of aluminum liquid metal for casting is applied to the liquid metal to control the generated phase such as intermetallic compounds. By inducing changes in the type, size, and distribution of the crystallized phase and intermetallic compounds generated during solidification, the present invention provides a high-strength, highly elongated, and highly thermally conductive aluminum casting alloy and a method for producing the same, which can simultaneously improve conflicting properties such as strength, conductivity, and ductility.
[0026] A high-strength, highly elongated and high thermal conductivity aluminum casting alloy according to one embodiment of the present invention contains 6.5 wt % to 11.5 wt % silicon (Si); 0.2 wt % to 0.4 wt % magnesium (Mg); 0.32 wt % to 0.85 wt % iron (Fe); and the balance being aluminum (Al) and unavoidable impurities, and contains an α-AlFeSi intermetallic compound having a cubic crystal structure in an aluminum matrix.
[0027] The aluminum casting alloy may further include strontium (Sr): 0.02% by weight or less, titanium (Ti): 0.15% by weight or less, or zirconium (Zr): 0.15% by weight or less.
[0028] In the high-strength, highly elongated, and high-thermal conductivity aluminum casting alloy, the α-AlFeSi intermetallic compound having a cubic crystal structure has the same crystal structure as the α-AlMnSi phase, but does not contain Mn and can undergo a phase change from the β-Al5FeSi intermetallic compound. The high-strength, highly elongated, and high-thermal conductivity aluminum casting alloy does not contain manganese, and therefore does not contain the α-AlMnSi phase in the final structure. However, this means that the α-AlFeSi intermetallic compound having a cubic crystal structure has the same crystal structure as the α-AlMnSi phase.
[0029] In the high strength, high elongation and high thermal conductivity aluminum casting alloy, the aluminum casting alloy is characterized in that it does not contain manganese (Mn), cobalt (Co), chromium (Cr) or molybdenum (Mo) as an additive for neutralizing the β-Al5FeSi intermetallic compound.
[0030] Table 1 shows the analysis results of the composition of the α-AlFeSi intermetallic compound embodied in the high strength, high elongation and high thermal conductivity aluminum casting alloy according to an embodiment of the present invention.
[0031] [Table 1]
[0032] In the high strength, highly elongated and highly thermally conductive aluminum casting alloy, the α-AlFeSi intermetallic compound may have a composition of Al: 74.9-86.7 at.%, Fe: 6.9-14.3 at.%, and Si: 6.2-11.3 at.%. Figure 1 shows a liquidus projection diagram of the Al-Si-Fe ternary system.
[0033] Referring to FIG. 1, a high-strength, highly elongated and highly thermally conductive aluminum casting alloy according to an embodiment of the present invention is an alloy in which Fe is added to an Al-Si based alloy, and may be limited to a composition range of Al, Si and Fe in which a β-Al5FeSi phase can be generated during a solidification path according to a liquidus projection phase diagram of an Al-Si-Fe ternary system.
[0034] In the high-strength, highly elongated, and high-thermal-conductivity aluminum casting alloy according to an embodiment of the present invention, the composition range of iron (Fe) may be 0.32 wt% or more to 0.85 wt% or less. If the iron (Fe) content is lower than 0.32 wt%, the Al-Si eutectic reaction may occur before the formation of the β-Al5FeSi phase during the solidification process of the Al-7Si-xFe alloy. On the other hand, if the iron (Fe) content is more than 0.85 wt%, the β-Al5FeSi phase may be formed before the α-Al phase, which is the base, during solidification. Therefore, in the high-strength, highly elongated, and high-thermal-conductivity aluminum casting alloy according to an embodiment of the present invention, the composition range of iron (Fe) is preferably controlled to 0.32 wt% or more to 0.85 wt% or less.
[0035] In the high strength, high elongation and high thermal conductivity aluminum casting alloy according to an embodiment of the present invention, the composition range of silicon (Si) may be 6.5 wt% to 11.5 wt%. If the silicon (Si) content is lower than 6.5 wt%, the fluidity of the molten metal may decrease, making it difficult to ensure castability. On the other hand, if the silicon (Si) content exceeds 11.5 wt%, the thermal conductivity of the aluminum casting alloy may decrease.
[0036] In the high strength, highly elongated and highly thermally conductive aluminum casting alloy according to an embodiment of the present invention, the magnesium (Mg) content may be in the range of 0.2 wt% to 0.4 wt%. If the magnesium (Mg) content is less than 0.2 wt%, the age hardening ability of the aluminum casting alloy may decrease, resulting in reduced strength. On the other hand, if the magnesium (Mg) content is more than 0.4 wt%, the ductility of the aluminum casting alloy may decrease.
[0037] Meanwhile, a manufacturing method of an aluminum casting alloy having high strength, high elongation and high thermal conductivity according to an embodiment of the present invention includes a first step of providing a molten aluminum casting alloy containing 6.5 wt % to 11.5 wt % silicon (Si); 0.2 wt % to 0.4 wt % magnesium (Mg); 0.32 wt % to 0.85 wt % iron (Fe); and the balance being aluminum (Al) and unavoidable impurities; and a second step of applying external energy at a temperature higher than a liquidus temperature of the molten aluminum casting alloy, and then cooling the molten aluminum casting alloy, so as to contain an α-AlFeSi intermetallic compound having a cubic crystal structure in an aluminum matrix.
[0038] In the manufacturing method of the high strength, high elongation and high thermal conductivity aluminum casting alloy, the second step may include a step of maintaining the molten aluminum casting alloy at a temperature 200°C to 300°C higher than the liquidus temperature, and then cooling the molten aluminum casting alloy at a cooling rate of 1 K / sec or more. For example, the cooling rate may be in the range of 1 K / sec to 100 K / sec.
[0039] In the manufacturing method of the high strength, highly elongated and high thermal conductivity aluminum casting alloy, the second step may include a step of maintaining the molten aluminum casting alloy at a temperature 100°C to 150°C higher than the liquidus temperature, and then cooling the molten aluminum casting alloy at a cooling rate of 10 K / sec or more. For example, the cooling rate may be in the range of 10 K / sec to 100 K / sec.
[0040] In the manufacturing method of the high-strength, highly elongated and high-thermal conductivity aluminum casting alloy, the temperature of the molten aluminum casting alloy in the second step is higher than the liquidus temperature, but it is necessary to control the cooling rate so that the smaller the difference between the temperature of the molten aluminum casting alloy and the liquidus temperature, the faster the cooling rate becomes.
[0041] The method for producing the high-strength, highly elongated and highly thermally conductive casting aluminum alloy may be characterized in that the molten aluminum casting alloy is maintained at a temperature higher than the liquidus temperature for 1 to 2 hours.
[0042] The method for producing the high-strength, highly elongated and high-thermal conductivity aluminum casting alloy may be characterized in that the molten aluminum casting alloy is maintained at a temperature higher than the liquidus temperature by applying ultrasonic waves for 1 to 2 minutes.
[0043] In the method for producing the high strength, high elongation and high thermal conductivity aluminum casting alloy, the second step may include a step of changing a phase from a β-AlFeSi intermetallic compound having a monoclinic crystal structure to an α-AlFeSi intermetallic compound having a cubic crystal structure.
[0044] In the manufacturing method of the high strength, highly elongated and high thermal conductivity aluminum casting alloy, in the second step, the generation of the β-Al5FeSi intermetallic compound occurs prior to the Al-Si eutectic reaction, and the α-Al phase, which is an aluminum matrix, can be generated prior to the generation of the β-Al5FeSi intermetallic compound.
[0045] Experimental Example
[0046] In the following, preferred experimental examples are presented to aid in understanding the present invention. However, the following experimental examples are merely intended to aid in understanding the present invention, and the present invention is not limited to the following experimental examples.
[0047] Composition and process design of aluminum alloy castings
[0048] Table 2 shows the composition and process conditions of the aluminum casting alloy according to Experimental Example A of the present invention. Experimental Example A was evaluated for the composition (unit: weight %) of a hypoeutectic Al-Si alloy.
[0049] [Table 2]
[0050] In this experimental example, in order to control the formation phase of Fe-based intermetallic compounds, the following two liquid phase processes (Thermal Rate (TR) and Ultrasonic treatment (UST)) were performed in addition to the normal casting method in the step of melting the liquid metal. Thermal Rate refers to a treatment method in which the molten metal is kept in an overheated state for a certain period of time. In Table 2, the "TR" item refers to a process in which the molten metal is kept at a set temperature for one hour, cooled to about 700°C, and then poured into a mold for casting, and the "UST" item refers to a process in which the molten metal at the set temperature is subjected to ultrasonic treatment for one minute, cooled to about 700°C, and then poured into a mold for casting.
[0051] In Table 2, 'Alloy 1' in Experimental Example 1 corresponds to A356.2 alloy, 'Alloy 2' in Experimental Example 2 corresponds to an alloy with an iron (Fe) content of about 0.3~0.4 wt% more than A356.2 alloy, 'Alloy 3' in Experimental Example 3 corresponds to a case where a molten alloy of Alloy 2 is maintained at a set temperature of 800℃ for 1 hour, cooled to about 700℃, and then poured into a mold for casting, and 'Alloy 4' in Experimental Example 4 corresponds to a case where a molten alloy of Alloy 2 is maintained at a set temperature of 800℃ for 1 hour, cooled to about 700℃, and then poured into a mold for casting. In experimental example 5, 'Alloy 5', a molten alloy of alloy 2 was subjected to ultrasonic treatment at 800°C for 1 minute, cooled to about 700°C, and then poured into a mold for casting. In experimental example 6, 'Alloy 6', a molten alloy of alloy 2 was subjected to remelting after maintaining the molten alloy at a set temperature of 900°C for 1 hour. Meanwhile, 'Alloy 7' in Experimental Example 7 corresponds to an alloy with an iron (Fe) content that is about 0.5~0.6% higher by weight than A356.2 alloy, 'Alloy 8' in Experimental Example 8 corresponds to a case where a molten alloy of Alloy 7 is ultrasonically treated at 700℃ for 1 minute and then poured into a mold at a temperature of about 700℃ for casting, and 'Alloy 9' corresponds to a case where a molten alloy of Alloy 7 is maintained at a set temperature of 1100℃ for 1 hour, cooled to about 700℃, and then poured into a mold for casting.
[0052] FIG. 2 is a schematic diagram showing a step mold used to form an aluminum alloy casting according to an example of the present invention.
[0053] In the experimental examples of the present invention, a process was applied in which an alloy weighing about 8 kg was melted at a normal melting temperature of 700°C using an induction melting furnace and an electric resistance melting furnace, and the molten metal was poured into a step mold (cooling rate 2.2K / s to 40K / s) as shown in Figure 2 for casting. Alloys 1 to 6 were melted and degassed in an electric resistance melting furnace, and the pouring temperature was fixed at 700°C for all of them. On the other hand, Alloys 7 to 9 were melted in an induction melting furnace, but degassed, and the pouring temperature was fixed at 700°C for all of them.
[0054] 3 and 4 are photographs showing the microstructure of an aluminum casting alloy depending on the cooling rate in an experimental example of the present invention, and FIG. 5A is a graph showing the morphology of the microstructure depending on the temperature and method of applying external energy and the cooling rate in an experimental example of the present invention.
[0055] Meanwhile, Fig. 6 to Fig. 12 are photographs of the 2-dimensional or 3-dimensional form of the microstructure according to the experimental example of the present invention. Specifically, Fig. 6 is a scanning electron micrograph of the 2-dimensional form of the microstructure of alloy 9 in the experimental example of the present invention, Fig. 7 is an image photograph of the 3-dimensional form of the microstructure of alloy 9 in the experimental example of the present invention, Fig. 8 is a scanning electron micrograph of the 2-dimensional form of the microstructure of alloy 3 in the experimental example of the present invention, Fig. 9 is a scanning electron micrograph of the 2-dimensional form of the microstructure of alloy 4 in the experimental example of the present invention, Fig. 10 is an image photograph of the 3-dimensional form of the microstructure of alloy 4 in the experimental example of the present invention, Fig. 11 is a scanning electron micrograph of the 2-dimensional form of the microstructure of alloy 2 in the experimental example of the present invention, and Fig. 12 is an image photograph of the 3-dimensional form of the microstructure of alloy 2 in the experimental example of the present invention.
[0056] 3 to 12, in a process of applying external energy at a temperature higher than the liquidus temperature (about 600°C) of the molten aluminum casting alloy and then cooling, when the molten aluminum casting alloy is maintained at a temperature (about 800°C to 900°C) 200°C to 300°C higher than the liquidus temperature and then cooled at a cooling rate of 1K / sec or more, it can be seen that a phase change occurs from a β-Al5FeSi intermetallic compound having a plate-like shape to an α-AlFeSi intermetallic compound having a shape of Chinese script. The β-Al5FeSi intermetallic compound has a three-dimensional plate shape and can have a needle-like shape on a two-dimensional cross section.
[0057] In the experimental alloy 5 (Alloy 5), when a process was applied in which a molten alloy (A5) having the composition in Table 2 was maintained at a set temperature of 900°C for 1 hour, the pouring temperature was then lowered to 700°C, and the molten alloy was poured into a mold at a cooling rate of 1 K / sec or more (2.2 K / sec, 6.9 K / sec, 16 K / sec, 40 K / sec) and cast, it was confirmed that all of the plate-shaped β-Al5FeSi intermetallic compounds underwent a phase change to α-AlFeSi intermetallic compounds having the shape of Chinese characters.
[0058] In the experimental alloy 3 (Alloy 3), when a process was applied in which a molten alloy (A3) having the composition in Table 2 was maintained at a set temperature of 800°C for 1 hour, the pouring temperature was then lowered to 700°C, and the molten alloy was poured into a mold at a cooling rate of 1 K / sec or more (2.2 K / sec, 6.9 K / sec, 16 K / sec, 40 K / sec) and cast, it was confirmed that all of the plate-shaped β-Al5FeSi intermetallic compounds underwent a phase change to α-AlFeSi intermetallic compounds having the shape of Chinese characters.
[0059] In the experimental alloy 4 (Alloy4), when a process is applied in which a molten alloy (A4) having the composition in Table 2 is ultrasonically treated at 800°C for 1 minute, the pouring temperature is lowered to 700°C, and the molten alloy is poured into a mold at a cooling rate of 1K / sec or more (2.2K / sec, 6.9K / sec, 16K / sec, 40K / sec) and cast, it can be confirmed that at least a part of the β-Al5FeSi intermetallic compounds having a plate shape undergoes a phase change to an α-AlFeSi intermetallic compound having a shape of Chinese characters. Furthermore, when a process is applied in which the molten alloy is poured into a mold at a cooling rate of 10K / sec or more (16K / sec, 40K / sec) and cast, it can be confirmed that all of the β-Al5FeSi intermetallic compounds having a plate shape undergo a phase change to an α-AlFeSi intermetallic compound having a shape of Chinese characters.
[0060] Meanwhile, in the case of Alloy 9 of the experimental example, when a process was applied in which a molten alloy (A9) having the composition in Table 2 was maintained at a set temperature of 1100°C for 1 hour, the pouring temperature was then lowered to 700°C, and the molten alloy was poured into a mold at a cooling rate of 1 K / sec or more (2.2 K / sec, 6.9 K / sec, 16 K / sec, 40 K / sec) and cast, it was confirmed that all of the plate-shaped β-Al5FeSi intermetallic compounds underwent a phase change to α-AlFeSi intermetallic compounds having the shape of Chinese characters.
[0061] In addition, referring to Figs. 3 to 12, in a process of applying external energy at a temperature higher than the liquidus temperature (about 600°C) of the molten aluminum casting alloy and then cooling the molten aluminum casting alloy, when the molten aluminum casting alloy is maintained at a temperature (about 700°C to 750°C) 100°C to 150°C higher than the liquidus temperature and then cooled at a cooling rate of 10K / sec or more, it can be confirmed that a phase change occurs from a plate-shaped β-AlFeSi intermetallic compound to an α-AlFeSi intermetallic compound having the shape of Chinese characters.
[0062] In the case of alloy 8 (Alloy 8) of the experimental example, when a process is applied in which a molten alloy (A8) having the composition in Table 2 is ultrasonically treated at 700°C for 1 minute, the injection temperature is lowered to 700°C, and the molten alloy is poured into a mold at a cooling rate of 10K / sec or more (16K / sec, 40K / sec) and cast, it can be confirmed that at least a part of the β-Al5FeSi intermetallic compound having a plate shape undergoes a phase change to an α-AlFeSi intermetallic compound having the shape of Chinese characters. However, in the case of alloy 8 (Alloy 8) of the experimental example, when a molten alloy (A8) having the composition in Table 2 is ultrasonically treated at 700°C for 1 minute, the injection temperature is lowered to 700°C, and the molten alloy is poured into a mold at a cooling rate of less than 10K / sec (2.2K / sec, 6.9K / sec) and cast, it can be confirmed that the β-Al5FeSi intermetallic compound having a plate shape does not undergo a phase change to an α-AlFeSi intermetallic compound having the shape of Chinese characters.
[0063] Referring to Figure 4, it can be seen that ultrasonic treatment at each cooling rate refines the β-Al5FeSi phase without changing its shape, while thermal-rate changes the shape of the needle-like β-Al5FeSi to the shape of Chinese characters. As the cooling rate increases from 6.9 to a maximum of 40 K / s, the refinement effect of the generated phase by ultrasonic treatment (Alloy 8) and thermal-rate (Alloy 9) is more pronounced than that of the conventionally treated material (Alloy 7).
[0064] The Chinese character-shaped Fe-based intermetallic compounds are judged to be quasi-equilibrium phases that cannot be predicted by thermodynamic calculations, and are observed in all thermal-rate alloys regardless of the cooling rate. On the other hand, in the conventionally and ultrasonically treated alloys, the quasi-equilibrium phases are observed only in some cases when the cooling rate is fast (e.g., 40K / s).
[0065] As mentioned above, in order to derive the process conditions for the formation of such quasi-equilibrium phases, thermal-rate tests were conducted for A356.2+0.4~0.6Fe alloys at molten temperatures of 700~1100°C and cooling rates of 0.3~40K / s. The thermal-rate tests were conducted by superheating the molten metal to each target temperature, maintaining it for 1 hour, then lowering the pouring temperature to 700°C and casting it into a steel step mold as shown in Figure 2. In addition, ultrasonic treatment was also conducted. The experiment was conducted by ultrasonicating the molten metal at 700°C and 800°C for 1 minute, then lowering the pouring temperature to 700°C and casting it into the same steel step mold.
[0066] FIG. 5A shows a process map in which quasi-equilibrium phases may appear.
[0067] As can be seen from FIG. 5A, in the case of A356 alloy with about 0.4 wt.% Fe added, when the alloy is heated to a temperature of 800°C or higher and maintained for about 1 hour, it is possible to generate a quasi-equilibrium phase having the shape of Chinese characters during solidification. The important point is that, even though a liquid phase process that generates the quasi-equilibrium phase was performed, when the cooling rate during casting was very slow (e.g., 0.3 K / s), all of the phases were observed as needle-shaped β-Al5FeSi equilibrium phases. This is because it is believed that if the cooling rate is sufficiently slow, the Chinese character phases will all transform into needle-shaped β-Al5FeSi equilibrium phases due to a peritectic reaction. What is even more interesting is that when the liquid metal is ultrasonically treated for 1 minute without being maintained at a temperature of 800°C, a quasi-equilibrium phase having the shape of Chinese characters can be observed in part of the solidification structure. As can be seen from FIG. 5A, when the liquid metal is ultrasonically treated for 1 minute at 800°C and then cast at a high cooling rate of 16 K / s or higher, it is observed that all of the Fe-based intermetallic compounds are generated as quasi-equilibrium phases during solidification. On the other hand, when the cooling rate is 2.2 to 6.9 K / s, it is confirmed that Fe-based intermetallic compounds having the shapes of Chinese characters and needle-shaped ones are mixed. In particular, it is confirmed that the β-Al5FeSi equilibrium phase observed in the ultrasonically treated material is significantly finer than the needle-shaped ones observed in the normally treated material or the alloy maintained at 700°C for 1 hour.
[0068] 5B is a graph showing the morphology of the microstructure of an aluminum casting alloy according to an experimental example of the present invention, depending on the time the alloy was kept at a molten temperature of 800° C. The cooling rate during casting was about 10 K / s.
[0069] Referring to FIG. 5B, when the molten aluminum casting alloy is maintained at 800°C, which is a temperature higher than the liquidus temperature, for 1 to 2 hours, it can be seen that a phase change occurs from the β-AlFeSi intermetallic compound having a plate shape to the α-AlFeSi intermetallic compound having the shape of Chinese characters.
[0070] FIG. 5C is a diagram showing a backscattered electron image of an aluminum casting alloy heated to a molten temperature of 600 to 800° C. and solidified at a cooling rate of 0.8 K / s in an experimental example of the present invention.
[0071] Referring to FIG. 5C, it can be seen that when the cooling rate is slow (e.g., cooling rate less than 1 K / s), almost no phase change is observed due to the application of external energy (e.g., superheating).
[0072] 6 to 12 show backscattered electron images and 3D microstructures of the alloys solidified at a cooling rate of 2.2 K / s after each liquid phase process. As can be seen, when the liquid metal is maintained at 700°C for 1 hour, coarse needle-like β-Al5FeSi phases having a size of several hundred μm are generated during solidification, while when the liquid metal is maintained at 800°C for 1 hour, Fe-based intermetallic compounds exist in the form of a quasi-equilibrium phase. In addition, it is observed that the liquid metal subjected to ultrasonic treatment at 800°C for 1 minute has both the quasi-equilibrium phase and the fine needle-like β-Al5FeSi equilibrium phase coexisting during solidification.
[0073] FIG. 13 is a photograph showing an analysis of the crystal structure of the β-AlFeSi intermetallic compound in the manufacturing method of the casting aluminum alloy of the present invention, and FIG. 14 is a photograph showing an analysis of the crystal structure of the α-AlFeSi intermetallic compound in the manufacturing method of the casting aluminum alloy of the present invention.
[0074] Table 3 shows the results of analyzing the crystal structure of the Fe-based intermetallic compound in the manufacturing method of the aluminum casting alloy of the present invention.
[0075] [Table 3]
[0076] In this experimental example, it was confirmed that a quasi-equilibrium phase can be generated during solidification of A356.2 liquid metal containing a large amount of Fe by applying external energy such as superheating (heat) or UST (ultrasonic wave). In this case, the quasi-equilibrium phase is observed to have a clear change in shape of the thermodynamically equilibrium β-Al5FeSi phase, which is believed to be due to a crystallographic change in the phase.
[0077] To analyze the crystal structure of the resulting phases, thin foil samples for the regions containing each phase were prepared by focused ion beam (FIB) milling and subjected to transmission electron microscopy (TEM) analysis.
[0078] 13 and 14 show TEM photographs and diffraction pattern analysis results for the needle-like β-Al5FeSi phase and the quasi-equilibrium phase (hereinafter referred to as α-AlFeSi phase), which are equilibrium phases, respectively. As can be seen, the needle-like β-Al5FeSi phase was analyzed to have a monoclinic structure with typically low symmetry, and the lattice constants and angles of the unit cell were analyzed as shown in Table 3. On the other hand, in the case of the α-AlFeSi phase having the shape of Chinese characters, the diffraction pattern analysis confirmed that it has the same crystal structure as the α-AlMnSi phase, but does not contain Mn and has a cubic crystal structure with a 4-fold structure. In other words, it is determined that the change from an asymmetrical shape such as a needle to a radially symmetrical shape such as a Chinese character is due to the crystal structure of the generated phase.
[0079] A more important point in the mechanism of change in the product phase is that the application of external energy to the liquid metal is considered to affect the short range ordering (SRO) bonding structure, which absolutely affects the formation of intermetallic compounds. Considering the fact that accurate analysis of the liquid phase structure is still limited, it is obviously difficult to speculate on theoretical possibilities based on phenomenal changes. Nevertheless, it is understood that the application of such external energy can affect the internal bonding structure of the liquid metal (bonding structure forming Fe-based intermetallic compounds, e.g., Al-Fe or Fe-Si bonds) or quasi-crystalline cluster structure, thereby causing changes in the crystal structure and shape of the product phase crystallized during solidification.
[0080] As can be seen from Figure 5A above, the liquid phase process can induce changes in the crystal structure of the resulting phase through structural changes within the liquid phase, but it can also be seen that the sustainability of such quasi-equilibrium phases is also highly dependent on the cooling rate during casting that is performed after the liquid phase process.
[0081] That is, the α-AlFeSi phase, which is a quasi-equilibrium phase, may be generated during solidification by the liquid phase process, but as solidification proceeds, it may be partially or entirely transformed into the β-Al5FeSi phase by the peritectic reaction accompanied by the diffusion of Si. That is, if the α-AlFeSi phase (containing up to 10 at.%), which has a relatively low solid solubility of Si, is generated first, Si is concentrated in the remaining liquid phase during growth, and then, through the peritectic reaction between the liquid phase and the α-AlFeSi phase, it transforms into the β-Al5FeSi phase (containing 15 to 20 wt.%), which has a relatively high solid solubility of Si. At this time, the thinner the branch of the α-AlFeSi phase is, the smaller the size is, and when sufficient time for diffusion (e.g., a slow cooling rate) is given, the more likely it is that the quasi-equilibrium phase will all transform into the β-Al5FeSi phase.
[0082] According to the theoretical prediction of the reaction and transformation rate, together with the concept of the peritectic reaction of "Liquid + α-AlFeSi → α-Al + β-Al5FeSi", it is found that the peritectic reaction rate depends on both the formation rate of the β-Al5FeSi phase by the reaction of the liquid phase with the α-AlFeSi phase, and the transformation rate of α → β. In particular, it is determined that the formation rate of the β-Al5FeSi phase by the reaction of the liquid phase with the α-AlFeSi phase, which has a significantly slow reaction rate, is the controlling factor. According to the prediction results, it is predicted that at a cooling rate of 2.2 K / s, the α-AlFeSi phase, which has a theoretical maximum thickness of about 2.5 μm, can all be transformed into the β-Al5FeSi phase by the peritectic reaction during solidification. On the other hand, when the cooling rate is increased to 6.9 K / s or more, it is predicted that only the α-AlFeSi phase, which has a thickness of 1 μm or less, can be transformed into the β-Al5FeSi phase. In other words, as the cooling rate increases, it becomes impossible for the peritectic reaction to occur completely from the already formed quasi-equilibrium phase α-AlFeSi to the β-Al5FeSi phase. This coincides with the fact that, as confirmed when observing the actual solidification structure, the faster the cooling rate after the thermal rate of the molten metal, the higher the tendency for it to exist as a quasi-equilibrium phase. By considering this kinetics, the quasi-equilibrium-equilibrium mechanism can be elucidated and process variables for realizing the quasi-equilibrium phase can be derived.
[0083] 3 to 5A, it was found that the application of external energy to liquid metal can induce the generation of quasi-equilibrium phases of Fe-based intermetallic compounds. At a molten metal temperature of 700°C, almost no microstructural changes were observed due to thermal rate treatment. However, as the cooling rate increased, significant refinement of the acicular β-Al5FeSi phase was observed, and at a cooling rate of 40K / s, it was confirmed that some of the quasi-equilibrium phases did not completely transform into the equilibrium phase and remained as they were.
[0084] On the other hand, when the thermal rate is 1 hour at a molten metal temperature of 800°C or higher, all Fe-based intermetallic compounds are observed as α-AlFeSi quasi-equilibrium phases with the shape of Chinese characters over the entire range of cooling rates from 2.2 to 40 K / s. An interesting point is that in the case of UST treatment performed as part of the external energy application method, it is confirmed that treatment at 800°C for only 1 minute has the effect of refining the generated phase. However, although almost no change in shape was observed due to ultrasonic treatment, this cannot be simply interpreted as meaning that the external energy of ultrasonic waves is not effective in changing the structure of the liquid metal and inducing the quasi-equilibrium phase.
[0085] When UST (ultrasonic waves) is applied to liquid metal, it is accompanied by two main phenomena, namely, "cavitation" and "acoustic streaming." Here, cavitation is a concept that includes a series of processes of bubble generation, growth, and collapse. In particular, it is known that bubble collapse locally generates hot spots with high temperatures and pressures of 5000°C and 500atm, so ultrasonic waves are considered to be a sufficient energy application means that can cause changes in the internal structure of liquid metal.
[0086] Therefore, it is believed that even if sufficient external energy is applied to the molten metal at a high temperature of 800°C for just one minute, it can affect the bonding structure or cluster structure of the liquid metal, and in parallel, the homogenization effect of the molten metal due to acoustic streaming causes the quasi-equilibrium phase to be small and uniformly generated. Then, such fine quasi-equilibrium phase can be kinetically rapidly transformed into the β-Al5FeSi equilibrium phase during the solidification process, and as a result, it can be observed as fine needle-like β-Al5FeSi phase in the microstructure.
[0087] 15 to 32 are diagrams showing the physical properties of the aluminum casting alloy according to the above-mentioned Experimental Example A of the present invention.
[0088] Specifically, Fig. 15 is a graph showing the maximum tensile strength of the aluminum casting alloys (cooling rate 2.2K / s) according to Experimental Examples 1 to 6 of the present invention for T5 heat treatment (artificial aging 155°C, 8 hours), Fig. 16 is a graph showing the yield strength of the aluminum casting alloys (cooling rate 2.2K / s) according to Experimental Examples 1 to 6 of the present invention for T5 heat treatment (artificial aging 155°C, 8 hours), Fig. 17 is a graph showing the elongation of the aluminum casting alloys (cooling rate 2.2K / s) according to Experimental Examples 1 to 6 of the present invention for T5 heat treatment (artificial aging 155°C, 8 hours), and Fig. 18 is a graph showing the thermal conductivity of the aluminum casting alloys (cooling rate 2.2K / s) according to Experimental Examples 1 to 6 of the present invention for T5 heat treatment (artificial aging 155°C, 8 hours). In Figs. 15 to 18, a condition of a cooling rate of 2.2K / sec was applied.
[0089] Fig. 19 is a graph showing the maximum tensile strength of the aluminum casting alloys (cooling rate 6.9K / s) according to Experimental Examples 1 to 6 of the present invention for T5 heat treatment (artificial aging 155°C, 8 hours), Fig. 20 is a graph showing the yield strength of the aluminum casting alloys (cooling rate 6.9K / s) according to Experimental Examples 1 to 6 of the present invention for T5 heat treatment (artificial aging 155°C, 8 hours), Fig. 21 is a graph showing the elongation of the aluminum casting alloys (cooling rate 6.9K / s) according to Experimental Examples 1 to 6 of the present invention for T5 heat treatment (artificial aging 155°C, 8 hours), Fig. 22 is a graph showing the thermal conductivity of the aluminum casting alloys (cooling rate 6.9K / s) according to Experimental Examples 1 to 6 of the present invention for T5 heat treatment (artificial aging 155°C, 8 hours). In Figs. 19 to 22, the cooling rate was 6.9K / sec.
[0090] Fig. 23 is a graph showing the maximum tensile strength of the aluminum casting alloys (cooling rate 16K / s) according to Experimental Examples 1 to 6 of the present invention for T5 heat treatment (artificial aging 155°C, 8 hours), Fig. 24 is a graph showing the yield strength of the aluminum casting alloys (cooling rate 16K / s) according to Experimental Examples 1 to 6 of the present invention for T5 heat treatment (artificial aging 155°C, 8 hours), Fig. 25 is a graph showing the elongation of the aluminum casting alloys (cooling rate 16K / s) according to Experimental Examples 1 to 6 of the present invention for T5 heat treatment (artificial aging 155°C, 8 hours), Fig. 26 is a graph showing the thermal conductivity of the aluminum casting alloys (cooling rate 16K / s) according to Experimental Examples 1 to 6 of the present invention for T5 heat treatment (artificial aging 155°C, 8 hours). In Figs. 23 to 26, a condition of a cooling rate of 16K / sec was applied.
[0091] FIG. 27 is a graph showing the thermal conductivity and electrical conductivity of the aluminum casting alloys according to Experimental Examples 2 to 6 of the present invention, and FIG. 28 is a graph showing the thermal conductivity in the R1 region of FIG.
[0092] 15 to 28, it can be seen that the ultimate tensile strength and elongation properties of Alloys 3 to 6 are significantly improved compared to Alloy 2, and that the yield strength and thermal conductivity properties are at the same level or higher.
[0093] Tables 4 and 5 show the measured physical properties (T5 & as-cast) of the aluminum casting alloy according to the experimental examples of the present invention.
[0094] [Table 4]
[0095] [Table 5]
[0096] In Tables 4 and 5, it can be seen from Alloys 3 to 6 that the high-strength, high-elongation, and high-thermal conductivity aluminum casting alloys according to the embodiments of the present invention can achieve a yield strength in the range of 100 MPa to 140 MPa, a maximum tensile strength in the range of 180 MPa to 220 MPa, an elongation in the range of 2.5% to 8.5%, and a thermal conductivity in the range of 160 W / mK to 190 W / mK.
[0097] In this experimental example, we evaluated how the control of the product phase based on the liquid phase process ultimately affects the mechanical and physical properties. A356.2+0.4Fe alloy was melt-processed using the liquid phase process method presented above and cast at a cooling rate of 2.2 to 16 K / s. Tensile samples were then taken from the cast samples to evaluate the tensile properties. All samples were subjected to T5 treatment, which involves aging only without solution treatment, and the aging conditions were 155°C for 8 hours. It can be seen that the control of the product phase by the liquid phase process (e.g., realization and refinement of the quasi-equilibrium phase of Fe-based intermetallic compounds) increases the elongation rate by 2% to 6%, up to a maximum of 300%, compared to the TR@700°C condition where there is no change in the product phase. It is also evaluated that the yield strength and tensile strength increase slightly with the increase in elongation rate. In the case of UST-treated materials, the yield strength reached the target property of 130 MPa at some cooling rates, but it is estimated that the yield strength is at the level of 100 to 120 MPa at other liquid phase processes and cooling rates. It has been confirmed that such control of the product phase of the liquid phase process affects not only the tensile properties but also the thermal conductivity properties.
[0098] 27 and 28 are graphs showing the change in thermal conductivity depending on the liquid phase process and cooling rate presented above. In this experimental example, the room temperature thermal conductivity was measured for the T5 heat-treated material in the same manner as the tensile test.
[0099] As can be seen, the alloys used in the test have a thermal conductivity of over 160W / mK for the T5 treated material, regardless of the casting process (liquid phase process, cooling rate). Meanwhile, it can be seen that the thermal conductivity properties increase as the cooling rate increases, regardless of the liquid phase process conditions. When the cooling rate is increased to 40K / s, both Alloy 4 and Alloy 5 are evaluated to reach a thermal conductivity value of 190W / mK, demonstrating improved thermal conductivity compared to Alloy 2.
[0100] It is understood that as the cooling rate increases, the solid solubility increases due to the trapping behavior of solute elements in the matrix, and therefore the amount of aging precipitates is expected to increase proportionally even after T5 heat treatment. Considering this, we present the fact that in the case of the fastest cooling rate of 40K / s, the thermal conductivity does not decrease but increases compared to other cooling rate conditions, due to other microstructural factors rather than the solute-precipitation effect in the matrix. This result supports the hypothesis that not only the matrix precipitate phase but also the shape, size and distribution of the solidified crystallized phase can affect thermal conductivity.
[0101] Meanwhile, in the case of Fe-based intermetallic compounds observed at a cooling rate of 40 K / s, it is confirmed that the thermal-rate promotes the induction of quasi-equilibrium phases at temperatures above 800°C, while at the same time significantly refining the phases. It is also observed that the distribution of the resulting phases has become more uniform. Assuming that there are no changes in the other solidification crystallization phases, the eutectic Si and π-Al8FeMg3Si6 phases, the backscattered electron images indicate that the changes in the shape, size and distribution of these Fe-based intermetallic compounds directly affect the thermal conductivity.
[0102] FIG. 29 is a graph showing the size of Fe-based intermetallic compounds depending on the cooling rate of the aluminum casting alloys according to Experimental Examples 2 to 5 of the present invention, and FIG. 30 is a graph showing the volume fraction of Fe-based intermetallic compounds depending on the cooling rate of the aluminum casting alloys according to Experimental Examples 2 to 5 of the present invention.
[0103] 29 and 30, it can be seen that the size and fraction of the β-Al5FeSi phase are generally reduced by the liquid phase process, and when the cooling rate is 2.2 K / s, it can be seen that the size (46.5 μm→10.3 μm) and fraction (1.1%→0.7%) are reduced by the liquid phase process to the greatest extent.
[0104] The size and fraction of Fe-based intermetallic compounds observed in the samples cast over the entire range of liquid phase processes and cooling rates tested in this experimental example were quantitatively analyzed. Figures 29 and 30 show the results, which indicate that the size and fraction of Fe-based intermetallic compounds both decrease as the cooling rate increases, regardless of the liquid phase process variables. Meanwhile, it is confirmed that the size of Fe-based intermetallic compounds generally decreases in the alloy 4, alloy 3, and alloy 5 conditions compared to alloy 2 at each cooling rate. Such a difference in the size of Fe-based intermetallic compounds according to the casting process is the largest when the cooling rate is 2.2 K / s, and when the cooling rate is increased to 6.9 K / s or more, it is confirmed that the degree of refinement is similar for alloy 3, alloy 4, and alloy 5. Similar to the size, the fraction of Fe-based intermetallic compounds is also analyzed to be significantly decreased in the alloy 4 and alloy 5 conditions compared to alloy 2, but to be somewhat increased in the alloy 3 condition.
[0105] FIG. 31 is a graph showing the correlation between stress and deformation rate of aluminum casting alloys according to Experimental Examples 7 to 9 of the present invention at a cooling rate of 6.9 K / sec, and FIG. 32 is a graph showing the correlation between stress and deformation rate of aluminum casting alloys according to Experimental Examples 7 to 9 of the present invention at a cooling rate of 16 K / sec.
[0106] 31 and 32, it can be seen that the elongation rate is increased by refining the generated phase by ultrasonic treatment (Alloy 8). When the cooling rate is 16 K / s, it can be seen that the elongation rate increases by about 200% and the strength is also improved.
[0107] On the other hand, in the case of Alloy 9, which is heat-treated at 1100°C, it is confirmed that the magnesium volatilization problem and the increase in the degree of hydrogen trapping result in almost no improvement in properties. In other words, when superheating is performed at a temperature 300°C higher than the liquidus temperature, it is confirmed that the inherent properties of the alloy are deteriorated because highly reactive alloy elements such as magnesium are volatilized.
[0108] Table 6 shows the composition and process conditions of the aluminum casting alloy according to the experimental example B of the present invention. The experimental example B is an evaluation of the composition (unit: weight %) of the eutectic Al-Si alloy system.
[0109] [Table 6]
[0110] In this experimental example, in order to control the phase of the Fe-based intermetallic compound, the following two liquid phase processes (Thermal Rate (TR) and Ultrasonic treatment (UST)) were performed in addition to the normal casting method in the step of melting the liquid metal. In Table 6, the "TR" item means a process of maintaining the molten metal at a set temperature for one hour, cooling the molten metal to about 700°C, and then pouring the molten metal into a mold for casting; the "UST" item means a process of ultrasonically treating the molten metal at a set temperature for one minute, cooling the molten metal to about 700°C, and then pouring the molten metal into a mold for casting; and the "Mn-free" item means an alloy to which Mn is not added in order to control the phase of the Fe-based intermetallic compound in the A365 alloy.
[0111] In Table 6, 'Alloy 10' in Experimental Example 10 corresponds to A365 alloy, 'Alloy 11' in Experimental Example 11 corresponds to an alloy with about 0.4 wt% more iron (Fe) than A365 alloy, 'Alloy 12' in Experimental Example 12 corresponds to a case where molten alloy 11 is maintained at a set temperature of 800°C for 1 hour, cooled to about 700°C, and then poured into a mold for casting, and 'Alloy 13' in Experimental Example 13 corresponds to a case where molten alloy 11 is maintained at a set temperature of 800°C for 1 hour, cooled to about 700°C, and then poured into a mold for casting. 'Alloy 13', which is experimental example 13, is a case where a molten alloy of Alloy 11 is maintained at a set temperature of 900°C for 1 hour, the molten alloy is cooled to about 700°C, and then poured into a mold for casting. 'Alloy 14', which is experimental example 14, is an A365 alloy to which Mn is not added in order to control the formation phase of Fe intermetallic compounds. 'Alloy 15', which is experimental example 15, is a case where a molten alloy of Alloy 14 is maintained at a set temperature of 800°C for 1 hour, and then cooled to about 700°C. The molten alloy was cooled to about 700°C and then poured into a mold for casting. Experimental Example 16, 'Alloy 16', was a case where a molten alloy of Alloy 14 was maintained at a set temperature of 900°C for 1 hour, and then cooled to about 700°C and then poured into a mold for casting. Experimental Example 17, 'Alloy 17', was an A365 alloy to which Sr and Ti were added, but Mn was not added, in order to control the formation phase of Fe intermetallic compounds. Experimental Example 18, 'Alloy 18', was a case where a molten alloy of Alloy 17 was maintained at a set temperature of 800°C for 1 hour, and then cooled to about 700°C and then poured into a mold for casting. Experimental Example 19, 'Alloy 19', was a case where a molten alloy of Alloy 17 was subjected to ultrasonic treatment at a set temperature of 800°C for 1 minute, then cooled to about 700°C and then poured into a mold for casting.
[0112] Figures 33 and 34 are photographs of the microstructure of aluminum immediately after casting (as cast) depending on the cooling rate in Experimental Examples 11 to 13 of the present invention. Referring to Figure 33, it can be seen that the improvement phenomenon caused by the addition of Sr in eutectic Si is eliminated by the liquid phase process. Referring to Figure 34, it can be seen that Fe intermetallic compounds are present, and that when manganese is contained, α-AlMnSi phases having the shape of coarse Chinese characters are generated.
[0113] Figures 35 and 36 are photographs of the microstructures immediately after casting of aluminum according to the cooling rate in Experimental Examples 14 to 16 of the present invention. Referring to Figure 35, it can be seen that there is no change in the microstructure in eutectic Si. Referring to Figure 36, it can be seen that Fe intermetallic compounds are present, and in the alloy not containing manganese, it can be seen that the acicular structure of β-Al5FeSi having the existing monoclinic crystal structure changes to the shape of Chinese characters of α-AlFeSi having the cubic crystal structure.
[0114] FIG. 37 is a graph comparing the tensile properties immediately after casting of aluminum according to cooling rates in Experimental Examples 14 to 16 of the present invention.
[0115] Referring to FIG. 37, it can be seen that as the cooling rate increases, the ultimate tensile strength increases slightly and the yield strength decreases slightly.
[0116] Figures 38 to 40 are graphs comparing the thermal conductivity characteristics of aluminum immediately after casting depending on the cooling rate in Experimental Examples 14 to 16. Referring to Figures 38 to 40, it can be seen that the general inverse proportional relationship between yield strength and conductivity does not apply when the cooling rate is 4-6 K / s or more.
[0117] Hereinafter, a high strength, high elongation and high thermal conductivity aluminum casting alloy according to another modified embodiment of the present invention will be described.
[0118] In Al-Si alloys, not only the β-Al5FeSi phase, which is generally generated before the Al-Si eutectic reaction (Fe addition amount of 0.32 wt.% or more), but also the β-Al5FeSi phase, which is generated before the Al-Si eutectic reaction (Fe addition amount of less than 0.32 wt.%), can greatly reduce the ductility of the alloy. Therefore, we investigated whether the technical idea of the present invention can be additionally applied to alloys with 0.2 to 0.3 wt.% Fe addition, which is a level at which the β-Al5FeSi phase can be generated in the range before the Al-Si eutectic reaction, and confirmed that the technology can be implemented as follows.
[0119] A high-strength, highly elongated and high thermal conductivity aluminum casting alloy according to another modified embodiment of the present invention includes 6.5 wt % to 11.5 wt % silicon (Si); 0.2 wt % to 0.4 wt % magnesium (Mg); 0.2 wt % to 0.3 wt % iron (Fe); and the balance being aluminum (Al) and unavoidable impurities, and includes an α-AlFeSi intermetallic compound having a cubic crystal structure in an aluminum matrix.
[0120] The aluminum casting alloy may further include strontium (Sr): 0.02% by weight or less, titanium (Ti): 0.15% by weight or less, or zirconium (Zr): 0.15% by weight or less.
[0121] In the high strength, highly elongated and high thermal conductivity aluminum casting alloy, the α-AlFeSi intermetallic compound having a cubic crystal structure has the same crystal structure as the α-AlMnSi phase, but does not contain Mn and can undergo a phase change from the β-Al5FeSi intermetallic compound.
[0122] In the high strength, high elongation and high thermal conductivity aluminum casting alloy, the aluminum casting alloy is characterized in that it does not contain manganese (Mn), cobalt (Co), chromium (Cr) or molybdenum (Mo) as an additive for neutralizing the β-Al5FeSi intermetallic compound.
[0123] In the high-strength, highly elongated and highly thermally conductive aluminum casting alloy, the α-AlFeSi intermetallic compound may have a composition of Al: 74.9 to 86.7 at.%, Fe: 6.9 to 14.3 at.%, and Si: 6.2 to 11.3 at.%.
[0124] The high strength, high elongation and high thermal conductivity aluminum casting alloy may have a yield strength in the range of 100 MPa to 140 MPa, an ultimate tensile strength in the range of 180 MPa to 220 MPa, an elongation in the range of 2.5% to 8.5%, and a thermal conductivity in the range of 160 W / mK to 190 W / mK.
[0125] A method for producing an aluminum casting alloy having high strength, high elongation and high thermal conductivity according to another modified embodiment of the present invention includes a first step of providing a molten aluminum casting alloy containing 6.5 to 11.5 wt % silicon (Si); 0.2 to 0.4 wt % magnesium (Mg); 0.2 to 0.3 wt % iron (Fe); and the balance being aluminum (Al) and unavoidable impurities; and a second step of applying external energy at a temperature higher than a liquidus temperature of the molten aluminum casting alloy, followed by cooling, so as to contain an α-AlFeSi intermetallic compound having a cubic crystal structure in an aluminum matrix.
[0126] In the manufacturing method of the high strength, highly elongated and high thermal conductivity aluminum casting alloy, the second step may include a step of maintaining the molten aluminum casting alloy at a temperature 200°C to 300°C higher than the liquidus temperature, and then cooling the molten aluminum casting alloy at a cooling rate of 1 K / sec or more.
[0127] In the manufacturing method of the high strength, highly elongated and high thermal conductivity aluminum casting alloy, the second step may include a step of maintaining the molten aluminum casting alloy at a temperature 100°C to 150°C higher than the liquidus temperature, and then cooling the molten aluminum casting alloy at a cooling rate of 10 K / sec or more.
[0128] The method for producing the high-strength, highly elongated and highly thermally conductive casting aluminum alloy may be characterized in that the molten aluminum casting alloy is maintained at a temperature higher than the liquidus temperature for 1 to 2 hours.
[0129] The method for producing the high-strength, highly elongated and high-thermal conductivity aluminum casting alloy may be characterized in that the molten aluminum casting alloy is maintained at a temperature higher than the liquidus temperature by applying ultrasonic waves for 1 to 2 minutes.
[0130] In the method for producing the high strength, high elongation and high thermal conductivity aluminum casting alloy, the second step may include a step of changing a phase from a β-AlFeSi intermetallic compound having a monoclinic crystal structure to an α-AlFeSi intermetallic compound having a cubic crystal structure.
[0131] In the manufacturing method of the high strength, highly elongated and high thermal conductivity aluminum casting alloy, in the second step, the generation of the β-Al5FeSi intermetallic compound occurs prior to the Al-Si eutectic reaction, and the α-Al phase, which is an aluminum matrix, can be generated prior to the generation of the β-Al5FeSi intermetallic compound.
[0132] Table 7 shows the composition and process conditions of the aluminum casting alloy according to another modified embodiment of the present invention. The composition is evaluated based on the composition of the Al-Si alloy system (unit: weight %).
[0133] [Table 7]
[0134] In this experimental example, in order to control the formation phase of Fe-based intermetallic compounds, the following two liquid phase processes (Thermal Rate (TR) and Ultrasonic treatment (UST)) were performed in addition to the normal casting method in the step of melting the liquid metal. Thermal Rate refers to a treatment method in which the molten metal is kept in an overheated state for a certain period of time. In Table 7, the "TR" item refers to a process in which the molten metal is kept at a set temperature for one hour, cooled to about 700°C, and then poured into a mold for casting, and the "UST" item refers to a process in which the molten metal at the set temperature is subjected to ultrasonic treatment for one minute, cooled to about 700°C, and then poured into a mold for casting.
[0135] In Table 7, the item 'Alloy 20' in Experimental Example 20 corresponds to the base alloy, the item 'Alloy 21' in Experimental Example 21 corresponds to the case where the molten alloy of Alloy 20 is ultrasonically treated at 800°C for 1 minute, cooled to about 700°C, and then poured into a mold for casting, and the item 'Alloy 22' in Experimental Example 22 corresponds to the case where the molten alloy of Alloy 20 is maintained at a set temperature of 800°C for 1 hour, cooled to about 700°C, and then poured into a mold for casting. The casting process for forming the aluminum casting alloy according to the modified embodiment of the present invention was the casting process described with reference to FIG. 2. FIG. 41 is a photograph of the microstructure of the aluminum casting alloy according to the cooling rate in the modified embodiment of the present invention (Table 7). In FIG. 41, Step 1 shows a case where the cooling rate is 2.2 K / sec, Step 2 shows a case where the cooling rate is 6.9 K / sec, Step 3 shows a case where the cooling rate is 16 K / sec, and Step 4 shows a case where the cooling rate is 40 K / sec.
[0136] Referring to FIG. 41, it can be seen that in Alloy 20, β-Al5FeSi intermetallic compounds having a plate shape are observed, but α-AlFeSi intermetallic compounds having the shape of Chinese characters are not observed.
[0137] In Alloy 21, which is made by subjecting a molten alloy of Alloy 20 to ultrasonic treatment at 800°C for 1 minute, cooling to about 700°C, and then pouring it into a mold for casting, it can be confirmed that when the cooling rate is 10K / sec or more, a phase change occurs from β-Al5FeSi intermetallic compound having a plate shape to α-AlFeSi intermetallic compound having the shape of Chinese characters.
[0138] In the case of Alloy 22, which is produced by maintaining the molten alloy of Alloy 20 at a set temperature of 800°C for 1 hour, cooling the molten alloy to about 700°C, and then pouring it into a mold for casting, it can be confirmed that when the cooling rate is 1K / sec or more, a phase change occurs from β-Al5FeSi intermetallic compound having a plate shape to α-AlFeSi intermetallic compound having a shape of Chinese characters.
[0139] 42 and Table 8 show the tensile properties immediately after casting of the aluminum casting alloy according to another modified embodiment (Table 7) of the present invention. In Table 8, UTS is tensile strength, YS is yield strength, and EL is elongation.
[0140] [Table 8]
[0141] 41, 42 and Table 8, it can be seen that the phase change occurs from the β-Al5FeSi intermetallic compound having a plate shape to the α-AlFeSi intermetallic compound having the shape of Chinese characters, so that the fraction of the brittle β-Al5FeSi intermetallic compound decreases and the elongation increases.
[0142] Table 9 shows the tensile properties of the aluminum casting alloy according to another modified embodiment of the present invention (Table 7) after the T6 heat treatment. The T6 heat treatment refers to a heat treatment in which a solution treatment and an aging treatment are performed in sequence.
[0143] [Table 9]
[0144] Referring to Table 9, it can be seen that the phase change from the β-Al5FeSi intermetallic compound having a plate shape to the α-AlFeSi intermetallic compound having the shape of Chinese characters occurs, so that the fraction of the brittle β-Al5FeSi intermetallic compound decreases and the elongation increases, but the strength and elongation increase when the T6 heat treatment is performed, compared to immediately after casting.
[0145] 43 shows the electrical conductivity characteristics of the aluminum casting alloy according to another modified embodiment of the present invention (Table 7) after the T6 heat treatment. The cooling rate of the sample was 1 to 2 K / s.
[0146] Referring to FIG. 43, it can be seen that the electrical conductivity properties of Alloy 22 are significantly improved when the molten alloy of Alloy 20 is maintained at a set temperature of 800°C for 1 hour, cooled to about 700°C, and then poured into a mold for casting.
[0147] Although the present invention has been described above with reference to the preferred embodiment, various modifications and variations may be made by those skilled in the art. As long as such modifications and variations do not deviate from the scope of the present invention, they are considered to belong to the present invention. Therefore, the scope of the present invention should be determined by the appended claims.
Claims
1. 6.5% by weight or more and 11.5% by weight or less of silicon (Si); 0.2% to 0.4% by weight of magnesium (Mg); 0.32% to 0.85% by weight of iron (Fe), and The balance includes aluminum (Al) and inevitable impurities. A high strength, highly elongated and highly thermally conductive aluminum casting alloy comprising an α-AlFeSi intermetallic compound having a cubic crystal structure within an aluminum matrix.
2. The high strength, highly elongated and highly thermal conductive aluminum casting alloy according to claim 1, wherein the α-AlFeSi intermetallic compound having a cubic crystal structure has the same crystal structure as the α-AlMnSi phase, but does not contain Mn and is a phase change from the β-Al5FeSi intermetallic compound.
3. The high strength, high elongation and high thermal conductivity aluminum casting alloy according to claim 2, characterized in that the aluminum casting alloy does not contain manganese (Mn), cobalt (Co), chromium (Cr) or molybdenum (Mo) as an additive for neutralizing the β-Al5FeSi intermetallic compound.
4. The high-strength, highly elongated and highly thermally conductive aluminum casting alloy according to claim 2, characterized in that the α-AlFeSi intermetallic compound has a composition of Al: 74.9 to 86.7 at. %, Fe: 6.9 to 14.3 at. %, and Si: 6.2 to 11.3 at. %.
5. 2. The high strength, highly elongated and high thermal conductivity aluminum casting alloy of claim 1 having a yield strength in the range of 100 MPa to 140 MPa, an ultimate tensile strength in the range of 180 MPa to 220 MPa, an elongation in the range of 2.5% to 8.5%, and a thermal conductivity in the range of 160 W / mK to 190 W / mK.
6. A first step of providing a molten aluminum casting alloy, the molten aluminum casting alloy comprising 6.5% to 11.5% by weight of silicon (Si), 0.2% to 0.4% by weight of magnesium (Mg), 0.32% to 0.85% by weight of iron (Fe), and the balance being aluminum (Al) and unavoidable impurities; and a second step of applying external energy at a temperature higher than the liquidus temperature of the molten aluminum casting alloy, so as to include an α-AlFeSi intermetallic compound having a cubic crystal structure in the aluminum matrix, and then cooling the molten aluminum casting alloy.
7. 7. The method for producing a high strength, highly elongated and highly thermally conductive aluminum casting alloy according to claim 6, wherein the second step includes a step of maintaining the molten aluminum casting alloy at a temperature 200° C. to 300° C. higher than the liquidus temperature, and then cooling the molten aluminum casting alloy at a cooling rate of 1 K / sec or more.
8. 7. The method for producing a high strength, highly elongated and highly thermally conductive aluminum casting alloy according to claim 6, wherein the second step includes a step of maintaining the molten aluminum casting alloy at a temperature 100° C. to 150° C. higher than the liquidus temperature, and then cooling the molten aluminum casting alloy at a cooling rate of 10 K / sec or more.
9. 9. A method for producing a high strength, highly elongated and highly thermally conductive aluminum casting alloy according to claim 7 or 8, characterized in that the molten aluminum casting alloy is maintained at a temperature higher than the liquidus temperature for 1 hour to 2 hours.
10. 9. The method for producing a high-strength, highly elongated and highly thermally conductive aluminum casting alloy according to claim 7 or 8, characterized in that the molten aluminum casting alloy is maintained at a temperature higher than the liquidus temperature for 1 to 2 minutes by applying ultrasonic waves.
11. 9. The method for producing a high strength, highly elongated and high thermal conductivity aluminum casting alloy according to claim 7 or 8, wherein the second step includes a step of changing a phase from a β-Al5FeSi intermetallic compound having a monoclinic crystal structure to an α-AlFeSi intermetallic compound having a cubic crystal structure.
12. 9. The method for producing a high strength, highly elongated and highly thermal conductive aluminum casting alloy according to claim 7 or 8, characterized in that in the second step, generation of a β-Al5FeSi intermetallic compound occurs prior to an Al-Si eutectic reaction, and an α-Al phase, which is an aluminum matrix, is generated prior to the generation of the β-Al5FeSi intermetallic compound.
13. 6.5% by weight or more and 11.5% by weight or less of silicon (Si); 0.2% to 0.4% by weight of magnesium (Mg); 0.2% to 0.3% by weight of iron (Fe), and The balance includes aluminum (Al) and inevitable impurities. A high strength, highly elongated and highly thermally conductive aluminum casting alloy comprising an α-AlFeSi intermetallic compound having a cubic crystal structure within an aluminum matrix.
14. A first step of providing a molten aluminum casting alloy, the molten aluminum casting alloy comprising 6.5% to 11.5% by weight of silicon (Si), 0.2% to 0.4% by weight of magnesium (Mg), 0.2% to 0.3% by weight of iron (Fe), and the balance being aluminum (Al) and unavoidable impurities; and a second step of applying external energy at a temperature higher than the liquidus temperature of the molten aluminum casting alloy, so as to include an α-AlFeSi intermetallic compound having a cubic crystal structure in the aluminum matrix, and then cooling the molten aluminum casting alloy.
Citation Information
Patent Citations
Method for producing aluminum alloy
JP2011255392A
Thermally conductive aluminum alloys and their applications
JP2020500265A
Al-Si casting alloy and method for fabricating the same
KR1020170099345A
Die cast aluminum alloys for structural components
WO2021150604A1
Die-casting aluminum alloy, aluminum alloy die-cast material, and method for manufacturing same
WO2021199428A1