Aluminum matrix NbTi superconducting wire and preparation method thereof

Through extrusion processing and cold quenching treatment, the processing difficulties and performance problems of NbTi superconducting wires when using aluminum matrix are solved, and the efficient preparation and optimization of superconducting performance of NbTi superconducting wires of aluminum matrix are achieved, thereby improving the conductivity and criticality of NbTi superconducting wires of aluminum matrix are achieved. Current density.

CN118507144BActive Publication Date: 2024-11-29XIAN SUPERCONDUCTING WIRE TECHNOLOGIES CO LTD

Patent Information

Application Number
CN202410961289.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-18
Publication Date
2024-11-29
Estimated Expiration
2044-07-18

AI Technical Summary

Technical Problem

When using aluminum as a stabilized metal matrix, NbTi superconducting wires have difficulty in processing due to different material characteristics and high heat treatment temperature requirements, which affects superconducting performance and limits their wide application.

Method used

The NbTi/Cu single-core or multi-core wire was coated on the surface with an aluminum. By controlling the extrusion temperature, speed and pressure, combined with cold quenching treatment, an aluminum matrix NbTi superconducting wire is prepared. The processing difficulties when using aluminum as the matrix material are avoided.

Benefits of technology

The efficient preparation of aluminum matrix NbTi superconducting wire was achieved, the conductivity and critical current density were optimized, the superconducting current carrying capacity was maintained, the cost was reduced, and the processing problems and performance of aluminum matrix NbTi superconducting wire was solved. Poor problem.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118507144B_ABST
    Figure CN118507144B_ABST
Patent Text Reader

Abstract

The present invention belongs to the technical field of superconducting wires, and relates to an aluminum-based NbTi superconducting wire and a preparation method thereof. The present invention provides a preparation method of an aluminum-based NbTi superconducting wire, which comprises: extruding at least one NbTi / Cu single-core wire or NbTi / Cu multi-core wire, and covering the surface with aluminum to obtain an aluminum-based NbTi superconducting wire. The present invention covers the surface of the finished NbTi / Cu single-core wire or NbTi / Cu multi-core wire with an aluminum matrix by an extrusion method, thereby solving the technical problems of the difficulty in processing and poor performance of the aluminum-based NbTi superconducting wire.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of superconducting wires and relates to an aluminum-based NbTi superconducting wire and a preparation method thereof. Background Art

[0002] NbTi superconducting wires account for a major share of the entire superconducting material market due to their excellent superconducting properties in medium and low magnetic fields, good mechanical properties and processing properties, and price advantages. The stabilized metal matrix used by NbTi superconducting wires is mainly oxygen-free copper, and a few use aluminum as the stabilized metal matrix. Using aluminum as a stabilized metal matrix has many advantages over copper. For example, under the same geometric shape, the heat dissipation capacity of high-purity aluminum is several times higher than that of oxygen-free copper, the magnetic diffusion coefficient of high-purity aluminum is only 0.13 times that of oxygen-free copper, and the specific gravity of high-purity aluminum is only 0.5 times that of oxygen-free copper. Aluminum can anneal itself at room temperature to eliminate some stress, and the price of aluminum is lower than that of copper.

[0003] There are many problems in using aluminum as a stabilizing metal matrix in NbTi superconducting wires, which has led to the fact that NbTi / Al superconducting wires have not been widely used. For example, due to the great difference in the material properties (hardness, elongation, etc.) of NbTi superconducting materials and aluminum, it is extremely difficult to coordinate the deformation of the two during joint processing. Specific molds and lubrication conditions are required when NbTi superconducting materials and aluminum are drawn together; high extrusion temperatures are required when hot extrusion and heat treatment are used to generate superconducting phases. If the extrusion temperature is too high, the aluminum is too soft to withstand it. If the extrusion temperature is too low, the NbTi superconducting material cannot be extruded; when heat treatment is used to generate superconducting phases, the temperature is too high and the aluminum is too soft, resulting in the inability to stretch subsequently. If the temperature is too low, the superconducting pinning phase of the NbTi superconducting material is too little and the performance is low. Summary of the invention

[0004] The object of the present invention is to solve at least one of the above-mentioned technical problems. By using it, it is possible to achieve the stabilization of the metal matrix as aluminum outside the NbTi superconducting wire in a simple and cost-effective manner. To this end, the present invention provides an aluminum-based NbTi superconducting wire and a preparation method thereof to solve this need in the art.

[0005] The present invention is based on the prepared NbTi / Cu single-core wire or NbTi / Cu multi-core wire, and achieves the above-mentioned purpose by extrusion processing.

[0006] The manufacture of the NbTi / Cu single core wire or the NbTi / Cu multi-core wire of the present invention generally involves first manufacturing a preliminary conductor containing NbTi, and Cu as a matrix material. When only one preliminary conductor is placed in the matrix material, an α-Ti superconducting pinning phase is produced by reactive heat treatment, and when it is processed into a fully manufactured conductor, it is called a NbTi / Cu single core wire. When multiple preliminary conductors are placed in the matrix material, an α-Ti superconducting pinning phase is produced by reactive heat treatment, and when it is processed into a fully manufactured conductor, it is called a NbTi / Cu multi-core wire.

[0007] On the one hand, the present invention provides a method for preparing an aluminum-based NbTi superconducting wire, which comprises: subjecting at least one NbTi / Cu single-core wire or NbTi / Cu multi-core wire to an extrusion process, and covering the surface with aluminum to obtain an aluminum-based NbTi superconducting wire; the extrusion process is performed at a temperature of 350°C to 500°C, a speed of 10m / min to 80m / min, and a pressure of 70 to 500MPa.

[0008] Optionally, in order to meet different technical specifications, before extrusion, technicians in this field process multiple NbTi / Cu single-core wires or a single NbTi / Cu multi-core wire into various shapes such as round wires, flat wires, rectangles, etc. through various methods such as twisting, assembling, and arranging, which does not affect the implementation of the technical solution provided by the present invention.

[0009] Furthermore, in the method for preparing the aluminum-based NbTi superconducting wire provided by the present invention, a thermal insulation layer is coated on the surface of the NbTi / Cu single-core wire or the NbTi / Cu multi-core wire before the extrusion process, and / or cold quenching is performed immediately after the extrusion process is completed.

[0010] Furthermore, in the method for preparing the aluminum-based NbTi superconducting wire provided by the present invention, the thermal insulation layer is a metal having a higher thermal conductivity than copper, and the thickness of the thermal insulation layer is 0.0015 mm to 0.004 mm.

[0011] Furthermore, in the method for preparing the aluminum-based NbTi superconducting wire provided by the present invention, the thermal insulation layer is Ni or Cr.

[0012] Furthermore, in the method for preparing the aluminum-based NbTi superconducting wire provided by the present invention, the quenching is water quenching, the distance between the water quenching and the extrusion die is ≤15 cm, the length of the water pool is ≥1 m, and the cooling water temperature is ≤50°C.

[0013] Furthermore, in the method for preparing the aluminum-based NbTi superconducting wire provided by the present invention, the copper superconducting ratio of the NbTi / Cu single-core wire or the NbTi / Cu multi-core wire is 0.2-10.

[0014] On the other hand, the present invention relates to an aluminum-based NbTi superconducting wire, which is prepared by the above-mentioned preparation method.

[0015] Furthermore, in the aluminum-based NbTi superconducting wire provided by the present invention, the area ratio of aluminum to NbTi / Cu in the aluminum-based NbTi superconducting wire is 0.2-25.

[0016] Furthermore, in the aluminum-based NbTi superconducting wire provided by the present invention, the purity of aluminum used in the preparation of the aluminum-based NbTi superconducting wire is not less than 99.99%, and the RRR of aluminum is not less than 700 under the condition of 273K / 10K.

[0017] Furthermore, in the aluminum matrix NbTi superconducting wire provided by the present invention, the RRR of the aluminum matrix NbTi superconducting wire is not less than 300 under the condition of 273K / 10K.

[0018] Compared with the prior art, the technical solution provided by the present invention has the following beneficial effects or advantages:

[0019] The present invention uses NbTi / Cu single-core wire or NbTi / Cu multi-core wire, and is processed by extrusion, and aluminum is covered on the surface to obtain an aluminum-based NbTi superconducting wire. The method avoids many problems when aluminum is used as a matrix material in the assembly stage before the reactive heat treatment produces the NbTi superconducting phase, thereby optimizing the conductive properties (RRR value and critical current) of the superconducting wire in a simple and low-cost manner. The present invention further protects the microstructure in the NbTi core wire by electroplating and / or water quenching, which will not cause the superconducting current carrying capacity of the NbTi / Cu superconducting wire to decrease, and can maintain the original high superconducting current carrying capacity of the NbTi / Cu superconducting wire. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0021] Figure 1 It is an aluminum matrix NbTi superconducting wire made of a NbTi / Cu single core wire.

[0022] Figure 2 The invention is an aluminum-based NbTi superconducting wire made of multiple NbTi / Cu multi-core wires. DETAILED DESCRIPTION

[0023] The technical solution of the present invention is described below in conjunction with embodiments; however, the present invention is not limited to the following embodiments.

[0024] The experimental methods and detection methods described in the following embodiments are conventional methods unless otherwise specified; the reagents and materials are commercially available unless otherwise specified.

[0025] Example 1

[0026] This embodiment provides a method for preparing an aluminum-based NbTi superconducting wire.

[0027] The NbTi / Cu single core wire is extruded, and the area ratio of aluminum to NbTi / Cu in the aluminum matrix NbTi superconducting wire is 0.3, and the following is obtained: Figure 1 The aluminum matrix NbTi superconducting wire round wire is shown. The specific experimental plan is as follows:

[0028] A NbTi / Cu single core wire is prepared, the copper ratio of the single core wire is 0.3, the diameter is Φ0.50 mm, and the surface is electroplated as a heat insulation layer, the material of the heat insulation layer is Ni, and the thickness of the heat insulation layer is 0.0015 mm.

[0029] The NbTi / Cu single core wire is extruded and covered with aluminum on the surface to obtain an aluminum-based NbTi superconducting wire; the purity of the aluminum used is greater than 99.992%, and the residual resistance ratio (RRR) of the aluminum is 1000 under the condition of 273K / 10K. The extrusion temperature is 360°C, the speed is 18m / min, and the pressure is 80MPa. The diameter of the obtained aluminum-based NbTi superconducting wire is Φ0.57mm. The area ratio of aluminum to NbTi / Cu in the aluminum-based NbTi superconducting wire is 0.3. After extrusion, cold quenching is immediately carried out, and the cold quenching medium is water quenching. The distance between the water quenching and the extrusion die is 15cm, the length of the water pool is 1m, and the cooling water temperature is 50°C.

[0030] Example 2

[0031] This embodiment provides a method for preparing an aluminum-based NbTi superconducting wire.

[0032] The NbTi / Cu multi-core wires are twisted and then extruded, and the area ratio of aluminum to NbTi / Cu in the aluminum matrix NbTi superconducting wire is 10, and the following is obtained: Figure 2 The aluminum matrix NbTi superconducting wire (rectangle) is shown. The specific experimental plan is as follows:

[0033] A NbTi / Cu multi-core wire is prepared, the copper ratio of the multi-core wire is 2.6, and the diameter is Φ0.85 mm. Electroplating is performed on the surface as a heat insulation layer, the material of the heat insulation layer is Ni, and the thickness of the heat insulation layer is 0.002 mm.

[0034] The NbTi / Cu multi-core wire was used to prepare a 7-strand primary round cable, and the diameter of the primary round cable was Φ2.562mm. The NbTi / Cu primary round cable was used to prepare a 7-strand secondary round cable, and the diameter of the secondary round cable was Φ7.686mm.

[0035] Two strands of NbTi / Cu secondary round cables are extruded side by side, and aluminum is covered on the surface to obtain an aluminum-based NbTi superconducting wire; the purity of the aluminum used is greater than 99.999%, and the residual resistance ratio (RRR) of aluminum is 1200 under the condition of 273K / 10K. The extrusion temperature is 420°C, the speed is 26m / min, and the pressure is 210MPa. The size of the obtained aluminum-based NbTi superconducting wire is 17.686×36.059mm. The area ratio of aluminum to NbTi / Cu in the aluminum-based NbTi superconducting wire is 10. After extrusion, cold quenching is performed immediately, and the cold quenching medium is water quenching. The distance between the water quenching and the extrusion die is 10cm, the length of the water pool is 2m, and the cooling water temperature is 30°C.

[0036] Example 3

[0037] This embodiment provides a method for preparing an aluminum-based NbTi superconducting wire.

[0038] The NbTi / Cu multi-core wires were twisted and then extruded, and the area ratio of aluminum to NbTi / Cu in the aluminum matrix NbTi superconducting wire was 20, and a rectangular aluminum matrix NbTi superconducting wire was made. The specific experimental plan is as follows:

[0039] A NbTi / Cu multi-core wire is prepared, the copper ratio of the multi-core wire is 8, and the diameter is Φ1.00 mm. Electroplating is performed on the surface as a heat insulation layer, the material of the heat insulation layer is Cr, and the thickness of the heat insulation layer is 0.004 mm.

[0040] The NbTi / Cu multi-core wire was used to prepare a 19-strand primary round cable, and the diameter of the primary round cable was Φ4.29 mm. The NbTi / Cu primary round cable was used to prepare a 7-strand secondary round cable, and the diameter of the secondary round cable was Φ12.87 mm.

[0041] The three strands of NbTi / Cu secondary round cables were extruded side by side, and the aluminum matrix NbTi superconducting wire was covered with aluminum on the surface; the purity of the aluminum used was greater than 99.996%, and the residual resistance ratio (RRR) of the aluminum was 1100 under the condition of 273K / 10K. The extrusion temperature was 480°C, the speed was 70m / min, and the pressure was 460MPa. The size of the obtained aluminum matrix NbTi superconducting wire was 173.516×28.8mm. The area ratio of aluminum to NbTi / Cu in the aluminum matrix NbTi superconducting wire was 20. After extrusion, cold quenching was performed immediately, and the cold quenching medium was water quenching. The distance between the water quenching and the extrusion die was 5cm, the length of the water pool was 4m, and the cooling water temperature was 10°C.

[0042] Example 4

[0043] The preparation methods of the aluminum-based NbTi superconducting wires obtained in Examples 1 to 3 were processed according to Table 1, respectively. The test results are shown in Table 2.

[0044] Table 1: Experimental plan

[0045]

[0046] Table 2: Performance test results

[0047]

[0048] As can be seen from Table 1 and Table 2, the present invention provides a method for preparing an aluminum-based NbTi superconducting wire, and the extrusion process can be used to better prepare the aluminum-based NbTi superconducting wire, and its critical current density and RRR value are higher than those of commercially available aluminum-based NbTi superconducting wires, which effectively solves the technical problems of difficult processing and poor performance of aluminum-based NbTi superconducting wires. The present invention further protects the microstructure in the NbTi core wire by electroplating and / or water quenching during the preparation process, which can effectively improve the critical current and critical current density of the aluminum-based NbTi superconducting wire. Although the RRR value of the aluminum-based NbTi superconducting wire will be reduced, it is still far higher than that of commercially available aluminum-based NbTi superconducting wires.

[0049] As described above, the basic principle, main features and advantages of the present invention are well described. The above embodiments and descriptions are only descriptions of the preferred implementation modes of the present invention, and the present invention is not limited by the above embodiments. Without departing from the spirit and scope of the present invention, various changes and improvements made by ordinary technicians in this field to the technical solution of the present invention should fall within the protection scope determined by the present invention.

Claims

1. A method for preparing an aluminum-based NbTi superconducting wire, characterized in that: include: Extruding at least one NbTi / Cu single-core wire or NbTi / Cu multi-core wire and covering the surface with aluminum to obtain an aluminum-based NbTi superconducting wire; The extrusion process has a temperature of 350°C to 500°C, a speed of 10m / min to 80m / min, and a pressure of 70 to 500MPa; Before the extrusion process is performed, a heat insulation layer is coated on the surface of the NbTi / Cu single-core wire or the NbTi / Cu multi-core wire, and cold quenching is performed immediately after the extrusion process is completed; The heat insulation layer is Ni or Cr.

2. The method for preparing an aluminum-based NbTi superconducting wire according to claim 1, characterized in that: The heat insulation layer is a metal with a higher thermal conductivity than copper, and the thickness of the heat insulation layer is 0.0015 mm to 0.004 mm.

3. The method for preparing an aluminum-based NbTi superconducting wire according to claim 1, characterized in that: The cold quenching is water quenching, the distance between the water quenching and the extrusion die is ≤15cm, the length of the water pool is ≥1m, and the cooling water temperature is ≤50°C.

4. The method for preparing an aluminum-based NbTi superconducting wire according to claim 1, characterized in that: The copper excess ratio of the NbTi / Cu single-core wire or the NbTi / Cu multi-core wire is 0.2-10.

5. An aluminum-based NbTi superconducting wire, characterized in that: The method is prepared by the preparation method according to any one of claims 1 to 4.

6. The aluminum-based NbTi superconducting wire according to claim 5, characterized in that: The area ratio of aluminum to NbTi / Cu in the aluminum-based NbTi superconducting wire is 0.2-25.

7. The aluminum-based NbTi superconducting wire according to claim 5, characterized in that: The purity of aluminum used in the preparation of the aluminum-based NbTi superconducting wire is not less than 99.99%, and the residual resistance ratio of aluminum is not less than 700 under the condition of 273K / 10K.

8. The aluminum-based NbTi superconducting wire according to any one of claims 5 to 7, characterized in that: The aluminum-based NbTi superconducting wire has a residual resistance ratio of not less than 300 under the condition of 273K / 10K.

Citation Information

Patent Citations

  • Preparation method of ultralow-loss NbTi superconducting wire

    CN114783681A

  • Manufacture of aluminum stabilized superconducting wire

    JP2000164053A

Cited By

  • Layered structure MXenes aluminum-based composite wire and preparation method thereof

    CN120565152A