Polymerizable raw material containing regenerated bis(2-hydroxyethyl) terephthalate and its preparation method
By purifying BHET through depolymerization and crystallization, the method addresses impurity issues in recycled BHET, ensuring high-quality polymer production with maintained heat resistance.
Patent Information
- Application Number
- JP2024509428
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2022-09-30
- Filing Date
- 2023-09-25
- Publication Date
- 2024-10-31
- Estimated Expiration
- 2043-09-25
AI Technical Summary
Bis(2-hydroxyethyl) terephthalate (BHET) regenerated from waste polyester contains impurities such as acetic acid ester compounds and diethylene glycol ester compounds, which impair the quality and heat resistance properties of polymers, making it unsuitable for high-quality polymer production.
A method to purify BHET by depolymerizing waste polyester, followed by cooling crystallization and pressure filtration to remove low-weight organics, adjusting the content of acetic acid ester compounds and diethylene glycol ester compounds to specific levels, ensuring a purity of 95% BHET with impurities below 1.0% and 2.0% respectively.
The method ensures the production of high-quality polymerization raw materials with maintained heat resistance properties, suitable for producing polyester resins with improved thermal stability and reduced impurity content.
Smart Images

Figure 2024539816000001 
Figure 2024539816000002 
Figure 2024539816000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a polymerization raw material containing bis(2-hydroxyethyl) terephthalate (BHET) regenerated from waste polyester and a method for preparing the same. [Background technology]
[0002] Polyesters are excellent in mechanical strength, heat resistance, transparency, and gas barrier properties, and are therefore widely used as materials for beverage containers, packaging films, audio films, video films, etc. Polyesters are also widely produced worldwide as industrial materials for medical fibers, tire cords, etc. In particular, polyester sheets or plates have good transparency and excellent mechanical strength, and are therefore widely used as raw materials for cases, boxes, partitions, shelves, panels, packaging materials, building materials, interior and exterior materials, etc.
[0003] As a result, plastic waste, including polyester, is generated at unmanageable levels worldwide every year. In recent years, countries around the world have created regulations and plans for recycling waste plastic resources, including waste polyester. Physical and chemical methods are used to recycle waste polyester, but physical recycling methods are not widely used because purity cannot be guaranteed.
[0004] On the other hand, chemical recycling methods involve breaking the ester bonds of waste polyester and depolymerizing it. In particular, reactions such as glycolysis, hydrolysis, methanolysis, and aminolysis are used. In particular, glycolysis is the decomposition of waste polyester by adding glycols such as ethylene glycol or diethylene glycol at high temperatures. A reaction product containing mainly bis(2-hydroxyethyl) terephthalate (BHET) is obtained. The bis(2-hydroxyethyl) terephthalate contained in the reaction product can be used as a raw material for preparing unsaturated polyester or ester polyol after crystallization or purification.
[0005] However, in order to use bis(2-hydroxyethyl) terephthalate as the above-mentioned raw material, it is necessary to increase the purity of bis(2-hydroxyethyl) terephthalate by minimizing the formation of by-products such as diethylene glycol esters during the depolymerization process. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] Korean Patent Application Publication No. 2022-0068991 Summary of the Invention [Problem to be solved by the invention]
[0007] Generally, bis(2-hydroxyethyl) terephthalate regenerated by depolymerization of waste polyester resin contains oligomeric substances such as dimers and trimers in addition to by-products derived from diethylene glycol (DEG) formed at high depolymerization temperatures, which are factors that impair the quality of the product. In addition, acetate, which is mainly used as a catalyst for glycolysis, has a boiling point close to that of ethylene glycol, which is mainly used as a solvent, and therefore is not easy to filter out as an impurity during the recovery and reuse of ethylene glycol. As a result, it accumulates and forms by-products as the process is repeated.
[0008] In particular, the present inventors have noticed that among these by-products, acetic acid ester compounds and diethylene glycol ester compounds impair the purity and quality of the recycled bis(2-hydroxyethyl) terephthalate, thereby impairing the degree of polymerization and heat resistance properties when preparing a polymer from the recycled bis(2-hydroxyethyl) terephthalate. To solve this problem, the present inventors have been able to control the content of acetic acid ester compounds and diethylene glycol ester compounds in the final product to a specific level by removing these low-weight organic substances during the purification process. As a result, it has become possible to prevent the deterioration of heat resistance properties in the preparation of polymers.
[0009] Therefore, the object of the present invention is to provide a polymerization raw material containing recycled bis(2-hydroxyethyl) terephthalate that does not reduce heat resistance in the preparation of a polymer, and a preparation method thereof. [Means for solving the problem]
[0010] According to one embodiment of the present invention, there is provided a polymerization raw material obtained by depolymerization of waste polyester, which, when measured by high performance liquid chromatography (HPLC), has a peak area of bis(2-hydroxyethyl) terephthalate of 95% or more, a peak area of acetate ester compounds of 0.001% to 1.0% in total, and a peak area of diethylene glycol ester compounds of 0.001% to 2.0% in total.
[0011] According to another aspect of the present invention, there is provided a method for preparing a polymerization feedstock, comprising: (a) depolymerizing waste polyester by glycolysis to obtain a crude bis(2-hydroxyethyl) terephthalate solution; (b) cooling the crude bis(2-hydroxyethyl) terephthalate solution to crystallize it; and (c) separating the crystallized product into solid and liquid using a pressure filter. Effect of the Invention
[0012] In the present invention, the content of acetic acid ester compounds and diethylene glycol ester compounds in the polymerization raw material containing recycled bis(2-hydroxyethyl) terephthalate is adjusted to a specific level, thereby preventing the deterioration of heat resistance caused by these compounds during polymerization of recycled polyester resin.
[0013] In order to prepare such a polymerization raw material containing regenerated bis(2-hydroxyethyl) terephthalate, low-weight organic matters including acetic acid are removed by cooling crystallization and pressure filtration during the purification process, so that the content of by-products such as acetic acid-based ester compounds or diethylene glycol ester compounds can be effectively suppressed.
[0014] Therefore, the present invention not only makes it possible to depolymerize waste polyester to prepare a polymerization raw material, but also makes it possible to produce polyester resins and products having excellent qualities such as heat resistance by using the waste polyester as a raw material. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0015] In this specification, the terms used to refer to the components are used to distinguish them from one another and are not intended to limit the scope of the embodiments. Furthermore, in this specification, the singular expressions "a," "an," and "the" are interpreted as including the plural unless otherwise specified by the context.
[0016] In this specification, terms such as first, second, etc. are used to describe various components. However, these terms should not be used to limit the components. The terms are used to distinguish one element from another element.
[0017] As used herein, the term "comprising" is intended to specify certain features, regions, steps, processes, elements, and / or components, and does not exclude the presence or addition of any other features, regions, steps, processes, elements, and / or components, unless specifically stated to the contrary.
[0018] In the numerical ranges limiting the contents, physical properties, and the like of the components described in this specification, when a numerical range limited only by an upper limit value and a numerical range limited only by a lower limit value are separately exemplified, it should be understood that a numerical range combining these upper and lower limits is also included in the exemplary range of the present invention.
[0019] The molecular weights of the compounds or polymers described herein, for example number average molecular weight or weight average molecular weight, are relative masses based on carbon 12, as is well known. Although no units are given, they can be understood, if necessary, as molar masses (g / mole) of the same numerical value.
[0020] The polymerization raw material of the present invention containing recycled bis(2-hydroxyethyl) terephthalate is obtained by depolymerization of waste polyester, and when measured by high performance liquid chromatography (HPLC), the peak area of acetic acid ester compounds is 1.0% or less in total, and the peak area of diethylene glycol ester compounds is 2.0% or less in total.
[0021] The polymerization raw material according to one embodiment is obtained by depolymerization of waste polyester, and when measured by high performance liquid chromatography (HPLC), the peak area of bis(2-hydroxyethyl) terephthalate is 95% or more, the peak area of acetate ester compounds is 0.001% to 1.0% in total, and the peak area of diethylene glycol ester compounds is 0.001% to 2.0% in total.
[0022] The content of acetic acid ester compounds and diethylene glycol ester compounds in the polymerization raw materials is adjusted to a specific level, so that it is possible to prevent the deterioration of heat resistance properties caused by these compounds during the polymerization of recycled polyester resin.
[0023] The polymerization raw materials according to the present invention will now be described in detail.
[0024] Polymerization raw materials containing recycled bis(2-hydroxyethyl) terephthalate Bis(2-hydroxyethyl)terephthalate (BHET) is an ester of two ethylene glycols and one terephthalic acid. For example, BHET is a compound formed as an intermediate in the process of preparing polyesters such as polyethylene terephthalate (PET) by polymerization of ethylene glycol with terephthalic acid or its esters.
[0025] On the other hand, the polymerization raw material containing regenerated bis(2-hydroxyethyl) terephthalate (regenerated BHET) obtained by depolymerization of waste polyester may contain by-products formed by side reactions with reagents or solvents used in various chemical steps during depolymerization of waste polyester. Therefore, the polymerization raw material containing regenerated bis(2-hydroxyethyl) terephthalate obtained by depolymerization of the above-mentioned waste polyester can be seen as one type of composition containing two or more constituent components. Therefore, in the present invention, the polymerization raw material containing regenerated BHET may be referred to as a "regenerated BHET composition" or a "polymerization raw material composition".
[0026] The polymerization raw material containing BHET regenerated by a general depolymerization process contains organic and inorganic impurities in addition to BHET as the main component, and therefore has low purity. However, the polymerization raw material containing the regenerated bis(2-hydroxyethyl) terephthalate according to the present invention has excellent purity and quality, even though it is obtained by depolymerization of waste polyester.
[0027] The purity of the polymerization raw material containing the regenerated BHET can be measured using liquid chromatography, etc. In detail, the purity of the polymerization raw material containing the regenerated BHET can be calculated by measuring the portion (%) of the peak area of BHET in the total peak area in a spectrum obtained using high performance liquid chromatography (HPLC).
[0028] The polymerization raw material may have a peak area of bis(2-hydroxyethyl)terephthalate of 95% or more when measured by high performance liquid chromatography (HPLC). For example, the peak area of bis(2-hydroxyethyl)terephthalate may be 95% or more, 97% or more, 98% or more, 99% or more, or 99.5% or more, and may be 99.998% or less, 99.99% or less, 99.9% or less, or 99% or less, and more specifically, may be 95% to 99.998%, or 97% to 99.998%. According to one embodiment, the polymerization raw material may have a peak area of bis(2-hydroxyethyl) terephthalate of 95% to 99.998%, specifically, 97% to 99.998%, 98% to 99.998%, 99% to 99.998%, or 99.5% to 99.998%, when measured by high performance liquid chromatography (HPLC).
[0029] On the other hand, the polymerization raw materials may contain compounds other than BHET, specifically, BHET analogs, BHET oligomers (e.g., dimers, trimers), esters, and acetate-based compounds.
[0030] In particular, the polymerization raw material may have a peak area portion of dimers or higher oligomers of 2.0% or less in total when measured by high performance liquid chromatography (HPLC). More particularly, the peak area portion of dimers or higher oligomers may be 1.5% or less, 1.0% or less, or 0.5% or less in total. Meanwhile, the lower limit of the peak area portion of dimers or higher oligomers may be 0% or more, 0.001% or more, 0.01% or more, or 0.1% or more in total.
[0031] In general, polymerization raw materials regenerated by depolymerization of waste polyester resin contain oligomer substances such as dimers and trimers in addition to by-products derived from diethylene glycol (DEG) formed at high depolymerization temperatures, which are factors that impair the quality of the product.
[0032] In addition, acetates (e.g., zinc acetate), which are mainly used as catalysts in glycolysis reactions, react with ethylene glycol during the depolymerization reaction to convert it into hydroxyethyl acetate (HA). HA has a boiling point close to that of ethylene glycol, which is mainly used as a solvent, and therefore is not easy to filter as an impurity during the recovery and reuse of ethylene glycol. As a result, it accumulates and forms by-products as the process is repeated.
[0033] As shown in Reaction Scheme 1 below, acetic acid (AA), derived from metal acetates that are commonly used as catalysts, can react with ethylene glycol (EG) to produce acetate-based compounds such as 2-hydroxyethyl acetate (HA) and water (HO).
[0034] [ka]
[0035] Furthermore, as shown in Reaction Scheme 2 below, 2-hydroxyethyl acetate (HA) can be converted to ester compounds such as 2-hydroxyethyl(2-acetoxyethyl)terephthalate (HAET) and ethylene glycol (EG) by transesterification with bis(2-hydroxyethyl)terephthalate (BHET).
[0036] [ka]
[0037] The polymerization raw material according to the embodiment has a peak area portion of acetic acid ester compounds of 1.0% or less in total when measured by high performance liquid chromatography (HPLC). In particular, the polymerization raw material may have a peak area portion of acetic acid ester compounds of 0.7% or less, 0.5% or less, 0.3% or less, or 0.2% or less in total when measured by high performance liquid chromatography (HPLC). Meanwhile, the lower limit of the peak area portion of the acetic acid ester compounds may be 0.001% or more, 0.01% or more, or 0.1% or more in total. According to one embodiment, the polymerization raw material may have a peak area portion of acetic acid ester compounds of 0.001% to 1.0%, in particular, 0.001% to 0.7%, 0.001% to 0.5%, 0.001% to 0.3%, or 0.001% to 0.2% in total when measured by high performance liquid chromatography (HPLC). The acetic acid ester compound may be a 2-hydroxyethyl acetic acid ester compound. In particular, the acetic acid ester compound may include at least one selected from the group consisting of 2-hydroxyethyl(2-acetoxyethyl)terephthalate (HAET), 2-acetoxyethyl[2-(2-hydroxyethoxy)ethyl]terephthalate, and 2-hydroxyethyl[2-[2-(2-hydroxyethoxy)ethoxy]ethyl]terephthalate. As a more detailed example, the acetic acid ester compound may include 2-hydroxyethyl(2-acetoxyethyl)terephthalate.
[0038] Furthermore, the polymerization raw material has a peak area portion of diethylene glycol (DEG) ester compounds of 2.0% or less in total when measured by high performance liquid chromatography (HPLC). For example, the peak area portion of diethylene glycol (DEG) ester compounds may be 1.5% or less, 1% or less, or 0.5% or less in total. Meanwhile, the lower limit of the peak area portion of diethylene glycol (DEG) ester compounds may be 0.001% or more, 0.01% or more, or 0.1% or more in total. According to one embodiment, the polymerization raw material may have a peak area portion of diethylene glycol (DEG) ester compounds of 0.001% to 2.0%, specifically, 0.001% to 1.5%, 0.001% to 1%, or 0.001% to 0.5% in total when measured by high performance liquid chromatography (HPLC). The diethylene glycol ester compound may include 2-hydroxyethyl [2-(2-hydroxyethoxy)ethyl] terephthalate and bis [2-(2-hydroxyethoxy)ethyl] benzene-1,4-dicarboxylate, which are represented by Formula 1 and Formula 2 below, respectively.
[0039] [ka] [ka]
[0040] In the present invention, the contents of acetic acid ester compounds and diethylene glycol ester compounds in the polymerization raw materials are adjusted to specific levels, so that it is possible to prevent a decrease in heat resistance properties caused by these compounds during the polymerization of recycled polyester resin.
[0041] As the content of diethylene glycol ester compounds in the polymerization raw materials increases, the heat resistance properties of the final polymer resin, such as the melting point, decrease linearly. The acetate-based ester compounds act as polymerization terminators that inhibit the growth of the polymer chains. As their content increases, the heat resistance properties of the final polymer resin decrease exponentially. Using these relationships, equations can be derived to predict the heat resistance properties of the polymer resins prepared from the polymerization raw materials.
[0042] For example, the polymerization materials may have a thermal property drop index (TDI), defined as follows, of 6.0 or less, 5.0 or less, 4.0 or less, or 3.0 or less, as measured by high performance liquid chromatography (HPLC). TDI = [DEG-ester-1] + [DEG-ester-2] × 2 + exp^[HA-ester]
[0043] Here, DEG-ester-1 is the peak area portion (%) of 2-hydroxyethyl [2-(2-hydroxyethoxy)ethyl] terephthalate, DEG-ester-2 is the peak area portion (%) of bis [2-(2-hydroxyethoxy)ethyl] benzene-1,4-dicarboxylate, and HA-ester is the peak area portion (%) of 2-hydroxyethyl (2-acetoxyethyl) terephthalate. This formula is calculated only with the numerical values of these parameters without the units.
[0044] In particular, when the thermal property degradation index (TDI) defined by the above formula is 3.0 or less, it is possible to more effectively prevent the deterioration of heat resistance properties caused by these compounds during polymerization of the recycled polyester resin. More particularly, the thermal property degradation index (TDI) may be 2.5 or less or 2.0 or less. Alternatively, the thermal property degradation index (TDI) may be 0 to 3.0, 0 to 2.5, 0.5 to 3.0, 1.0 to 3.0, or 0.5 to 2.5.
[0045] Additionally, the polymerization feedstock may have a monohydroxyethyl terephthalate (MHET) peak area fraction of 2% or less, 1.5% or less, 1% or less, or 0.5% or less, as measured by high performance liquid chromatography (HPLC).
[0046] The polymerization raw material of the present invention has excellent crystallinity, which results in a high melting point and excellent qualities such as color.
[0047] For example, the polymerization raw material may have a melting point (mp) of 100° C. or more, 105° C. or more, or 110° C. or more, and 125° C. or less, 120° C. or less, or 115° C. or less. As a specific example, the polymerization raw material may have a melting point of 110° C. to 115° C.
[0048] The polymerization feedstock may have a Yellowness Index (YID) of 5.0 or less when measured on a 25% by weight solution in dimethylformamide. In particular, the Yellowness Index may be 5.0 or less, 4.5 or less, 4.0 or less, 3.5 or less, 3.0 or less, 2.5 or less, 2.0 or less, 1.5 or less, or 1.0 or less.
[0049] Furthermore, the total content of residual ethylene glycol in the polymerization raw material may be 1 wt% or less, 0.9 wt% or less, 0.5 wt% or less, or 0.3 wt% or less, based on the weight ratio detected by gas chromatography analysis. More specifically, the content of residual ethylene glycol in the polymerization raw material may be 0.5 wt% or less. More specifically, the content of residual ethylene glycol in the polymerization raw material may be 0.2 wt% or less, 0.15 wt% or less, or 0.1 wt% or less.
[0050] The method for preparing polymerization feedstock according to the present invention includes: (a) depolymerizing waste polyester by glycolysis to obtain a crude bis(2-hydroxyethyl) terephthalate solution; (b) cooling the crude bis(2-hydroxyethyl) terephthalate solution to crystallize it; and (c) separating the crystallized product into solid and liquid using a pressure filter.
[0051] During the purification process, low-weight organic matters including acetic acid can be removed by cooling crystallization and pressure filtration, which can effectively suppress the content of by-products such as acetic acid-based ester compounds or diethylene glycol ester compounds.
[0052] Each step of the method for preparing the polymerization raw material according to the present invention will now be described in detail.
[0053] Depolymerization of waste polyester First, waste polyester is depolymerized by glycolysis to obtain a crude bis(2-hydroxyethyl) terephthalate solution.
[0054] The waste polyester raw material can be obtained from polyester material products that are discarded after use. In particular, the waste polyester can be obtained by pre-processing various post-consumer wastes including polyester materials (e.g., polyethylene terephthalate (PET) materials), such as beverage bottles, fabrics, films, cases, boxes, partitions, shelves, protective panels, packaging materials, building materials, and interior and exterior materials.
[0055] The pretreatment can be carried out by removing other plastics, metals and foreign objects mixed in the waste, washing it, and then crushing it in a crusher. As a result of the pretreatment, the waste polyester raw material may have a flake shape. Furthermore, the waste polyester raw material may have a fine structure like fibers.
[0056] The waste polyester thus pretreated is then subjected to a depolymerization process. The depolymerization process may, for example, include a glycolysis reaction. As is well known, a glycolysis reaction refers to a chemical reaction in which polymer chains or the like are cut by a glycol, such as ethylene glycol. The total weight of glycol added may be 1, 2, 3 or more times the weight of the waste polyester resin, and may be 7, 5, 4 or less times the weight of the waste polyester resin. For example, the weight of glycol added may be 1 to 7 times, particularly 2 to 5 times, and more particularly 3 to 4 times the weight of the waste polyester resin.
[0057] A catalyst can be used in the glycolysis reaction. The catalyst may be a metal catalyst, for example, a metal salt catalyst or a metal organic catalyst. In particular, the catalyst may be a metal acetate, carbonate, oxide, or hydroxide, and the metal may be an alkali metal, an alkaline earth metal, or a transition metal. As a detailed example, the catalyst includes a metal acetate, or an anhydride or hydride thereof. More particularly, it may be at least one selected from the group consisting of zinc acetate, sodium acetate, cobalt acetate, and manganese acetate, or in the form of a hydrate or anhydride thereof. Furthermore, the weight of the catalyst to be added may be 0.01 parts by weight or more, 0.1 parts by weight or more, 0.2 parts by weight or more, or 0.3 parts by weight or more, and 5 parts by weight or less, 1 part by weight or less, 0.7 parts by weight or less, 0.5 parts by weight or less, or 0.4 parts by weight or less, based on 100 parts by weight of the waste polyester resin. For example, the weight of the catalyst to be added may be 0.1 to 1 part by weight, specifically 0.2 to 0.7 parts by weight, based on 100 parts by weight of the waste polyester resin. More specifically, the catalyst may be used in an amount of 0.2 to 0.4 parts by weight based on 100 parts by weight of the waste polyester.
[0058] As a detailed example, the glycolysis in step (a) may comprise reacting the waste polyester with ethylene glycol in the presence of an acetic acid based catalyst.
[0059] The depolymerization may, for example, include multi-step depolymerization reactions at low temperatures. According to one embodiment, the depolymerization includes subjecting the waste polyester to depolymerization by a first glycolytic reaction at high temperature; and subjecting the product thereof to depolymerization by a second glycolytic reaction at low temperature.
[0060] The temperature during the first glycolytic reaction may be 170° C. or more, 180° C. or more, or 190° C. or more, and may be 205° C. or less, 200° C. or less, 195° C. or less, or 190° C. or less. For example, the temperature during the first glycolytic reaction may be 180° C. to 200° C., specifically 180° C. to 195° C., and more specifically 180° C. to 190° C.
[0061] Furthermore, the temperature during the second glycolytic reaction may be 140° C. or higher, 150° C. or higher, or 160° C. or higher, and may be 170° C. or lower, or may be 160° C. or lower. For example, the temperature during the second glycolytic reaction may be 150° C. to 170° C., specifically 150° C. to 160° C., and more specifically 150° C. to 155° C.
[0062] As a detailed example, the depolymerization may include: (1) subjecting waste polyester to depolymerization by a first glycolysis reaction at a temperature of 180 to 200°C to obtain a first reactant; and (2) subjecting the first reactant to depolymerization by a second glycolysis reaction at a temperature of 150 to 170°C to obtain a second reactant.
[0063] The period required for the first and second glycolytic reactions may be 1 hour or more, or 2 hours or more, and 4 hours or less, or 3 hours or less, from the time when the optimum temperature is reached. For example, the period required for the first and second glycolytic reactions may be 1 hour to 4 hours, specifically 1 hour to 3 hours, and more specifically 1 hour to 2 hours, from the time when the optimum temperature is reached.
[0064] As a more detailed example, the first glycolytic reaction can be carried out for 1 to 3 hours at a temperature of 180° C. to 190° C. Furthermore, the second glycolytic reaction can be carried out for 1 to 3 hours at a temperature of 150° C. to 160° C.
[0065] As an example, the first glycolytic reaction can be carried out in the presence of anhydrous zinc acetate catalyst. As a detailed example, the first glycolytic reaction can be carried out in the presence of anhydrous zinc acetate catalyst at a temperature of 180°C to 200°C for 1 hour to 3 hours. Anhydrous zinc acetate may be used in an amount of 0.2 parts by weight to 0.4 parts by weight per 100 parts by weight of waste polyester. Furthermore, the second glycolytic reaction can be carried out without adding a catalyst, after further adding ethylene glycol, at a temperature of 140°C to 160°C for 1 hour to 3 hours.
[0066] Cooling and filtering The crude bis(2-hydroxyethyl) terephthalate solution obtained by depolymerization can then be cooled. The cooling temperature may be, for example, 150° C. or lower, 140° C. or lower, 130° C. or lower, 120° C. or lower, 110° C. or lower, or 100° C. or lower, and may be 50° C. or higher, 60° C. or higher, 70° C. or higher, 80° C. or higher, or 90° C. or higher.
[0067] As an example, the cooling can be performed by a vacuum flash process. In particular, the temperature of the crude bis(2-hydroxyethyl) terephthalate solution can be reduced by evaporating ethylene glycol by applying a vacuum in a vacuum flash process. For example, the crude bis(2-hydroxyethyl) terephthalate solution can be further subjected to a step of cooling to 120°C or less by a vacuum flash prior to the subsequent step. More particularly, the temperature of the crude bis(2-hydroxyethyl) terephthalate solution can be reduced to 110°C or less or 100°C or less by a vacuum flash process. The pressure condition of the vacuum flash process can be, for example, 200 Torr or less, 100 Torr or less, or 50 Torr or less, in particular, 10 Torr to 200 Torr, 10 Torr to 100 Torr, or 10 Torr to 50 Torr.
[0068] Then, insoluble foreign matter can be removed from the cooled crude bis(2-hydroxyethyl) terephthalate solution by filtration. As a detailed example, the crude bis(2-hydroxyethyl) terephthalate solution can be cooled to 120° C. or less, and a filter aid can be added and filtered. As a result, fine particles and insoluble organic matter present in the crude bis(2-hydroxyethyl) terephthalate solution can be filtered by solid-liquid separation.
[0069] As the filter aid, known components such as diatomaceous earth, perlite, and asbestos powder can be used. For example, 0.1 to 2.0 parts by weight of the filter aid may be added to 100 parts by weight of the crude bis(2-hydroxyethyl) terephthalate solution.
[0070] Since bis(2-hydroxyethyl) terephthalate (BHET) or oligomer obtained by the depolymerization reaction exists in a solid form at room temperature, it is difficult to separate the foreign matter at room temperature. Therefore, it is preferable to separate them at a temperature condition of 90°C to 150°C, more specifically, 110°C to 150°C. Furthermore, when the above temperature range is maintained, the fluidity becomes good, so that it may be easy to remove the insoluble foreign matter.
[0071] Various methods and devices can be used to remove insoluble foreign matter by solid-liquid separation. For example, devices such as a pressure filter, a centrifuge, a filter press, and a belt press can be used. However, the method is not limited to these as long as it can be used to separate foreign matter.
[0072] According to one embodiment, the crude bis(2-hydroxyethyl) terephthalate solution is subjected to a solid-liquid separation step by filtering off the low-weight organic substances contained therein, so that most of the acetic acid ester compounds and diethylene glycol ester compounds can be discharged in liquid form.
[0073] A process according to one embodiment includes cooling the crude bis(2-hydroxyethyl) terephthalate solution to crystallize it; and separating the crystallized product into solids and liquids using a pressure filter.
[0074] The temperature of the cooling crystallization may be, for example, 70° C. or less, 60° C. or less, 50° C. or less, 40° C. or less, 30° C. or less, or 25° C. or less, and may be 0° C. or more, 5° C. or more, 10° C. or more, 5° C. or more, or 20° C. or more. As a specific example, the temperature may be room temperature.
[0075] The acetic acid-based compounds and diethylene glycol-based compounds can be removed by cooling crystallization.
[0076] The operating pressure of the pressure filter may be from 0.1 bar to 21 bar, more particularly from 1 bar to 5 bar. Furthermore, the operating temperature of the pressure filter may be from 5°C to 35°C, more particularly from 15°C to 25°C.
[0077] The pressure filter may be a Nutsche filter or a filter press.
[0078] Before using the Nutsche filter, it is desirable to inert the inside of the container by purging with nitrogen or the like. First, the mixture is placed in the Nutsche filter, and an inert gas such as nitrogen is injected and pressurized to separate the solvent from the filter cake. Then, water is injected into the Nutsche filter to wash out the residual solvent remaining in the filter cake, and an inert gas is injected and pressurized to separate the filter cake from the water. The obtained filter cake may be dried and cooled.
[0079] A filter press is a device that separates solids and liquids by forcing the reactants between the filter cloth and the lid under high pressure, forming a filtration chamber with a filter plate having a filtering surface, a filter cloth, and a lid. Compared to a vacuum filter, a filter press can achieve more effective solid-liquid separation because the pressure difference between the front and rear of the filter material, which acts as a solid-liquid separation surface, is greater.
[0080] The acetic acid-based compounds and diethylene glycol-based compounds may be removed by a pressure filter.
[0081] Ion exchange Furthermore, the crude bis(2-hydroxyethyl) terephthalate solution can be further subjected to ion exchange with an ion exchange resin. By performing ion exchange, ionic impurities present in the crude bis(2-hydroxyethyl) terephthalate solution, specifically, catalysts and foreign matter, can be removed.
[0082] As is well known, ion exchange resin refers to a resin or polymer that acts as a medium for ion exchange. Ion exchange resins may include cation exchange resins, anion exchange resins, amphoteric ion exchange resins, chelating resins, and the like.
[0083] The cation exchange resin may include a strongly acidic cation exchange resin having a sulfonic acid group (SO3H) and a weakly acidic cation exchange resin having a carboxyl group (-COOH).The anion exchange resin may include a strongly basic anion exchange resin in the form of a quaternary ammonium salt and a weakly basic anion exchange resin having a primary to tertiary amino group.
[0084] As a specific example, the ion exchange resin may include at least one selected from the group consisting of a strong acid cation exchange resin, a weak acid cation exchange resin, and a chelating resin.
[0085] According to one embodiment, the ion exchange is carried out by adding an ion exchange resin to the crude bis(2-hydroxyethyl) terephthalate solution.
[0086] The weight of the ion exchange resin added may be 1, 3, or 5 times or more the weight of the catalyst added in the depolymerization reaction, and may be 20, 15, 10, 8 times or less. For example, the weight of the ion exchange resin added may be 1 to 20 times, specifically 3 to 15 times, and more specifically 5 to 8 times the weight of the catalyst added in the depolymerization reaction.
[0087] Furthermore, the weight of the ion exchange resin to be added may be 1 part by weight or more, 3 parts by weight or more, or 5 parts by weight or more, and may be 50 parts by weight or less, 20 parts by weight or less, 15 parts by weight or less, 10 parts by weight or less, or 7 parts by weight or less, based on 100 parts by weight of the waste polyester resin used in the depolymerization reaction.
[0088] As a specific example, the ion exchange resin can be used in an amount of 1 to 20 parts by weight based on 100 parts by weight of the waste polyester.
[0089] According to another embodiment, the ion exchange is carried out by using a column containing an ion exchange resin.
[0090] In particular, a column can be packed with particles of ion exchange resin, and ion exchange can be carried out while the crude bis(2-hydroxyethyl) terephthalate solution passes through the column.
[0091] The particle diameter of the ion exchange resin particles may be, for example, 0.3 mm to 1.5 mm, more specifically, 0.6 mm to 0.9 mm.
[0092] The ion exchange temperature may be, for example, 140°C or less, 130°C or less, 120°C or less, 110°C or less, or 100°C or less, and may be 50°C or more, 60°C or more, 70°C or more, 80°C or more, or 90°C or more.
[0093] Further purification steps The polymerization raw material containing the above-mentioned regenerated bis(2-hydroxyethyl) terephthalate can be further subjected to a purification step as necessary. According to one example, the polymerization raw material containing the regenerated bis(2-hydroxyethyl) terephthalate can be prepared by further performing a step of removing unreacted glycol by distillation.
[0094] Since unreacted glycol remains in the depolymerized product after filtration in the previous step, it is necessary to remove the glycol from the product before the next step.
[0095] Furthermore, in order to carry out an economical depolymerization process, it is necessary to carry out a step of recovering the unreacted glycols, i.e., the glycols such as ethylene glycol, propylene glycol, and diethylene glycol that were previously used in the depolymerization and that remain uninvolved in the glycolysis reaction can be recovered and reused.
[0096] The distillation to remove the unreacted glycol can be carried out, for example, by vacuum distillation. For this purpose, a glass distillation apparatus or a rotary evaporator may be used.
[0097] When the vacuum distillation for removing the unreacted glycol is carried out at a temperature of 150°C or less, the formation of diethylene glycol and impurities derived therefrom can be further reduced, and the purity of BHET can be improved. For example, the vacuum distillation for removing the unreacted glycol can be carried out at a temperature of 150°C or less, 130°C or less, or 120°C or less, and 80°C or more, 90°C or more, 100°C or more, or 110°C or more. In detail, the temperature during the distillation for removing the unreacted glycol may be 80°C to 190°C or 90°C to 150°C. As a more detailed example, the distillation for removing the unreacted glycol may be carried out at a temperature of 100°C to 130°C.
[0098] The pressure during the reduced pressure distillation to remove the unreacted glycol may be, for example, 0.1 Torr to 760 Torr, 0.1 Torr to 200 Torr, or 0.5 Torr to 30 Torr. More specifically, the reduced pressure distillation can be carried out under reduced pressure conditions stepwise from 760 Torr to 0.8 Torr.
[0099] According to another example, the polymerization raw material containing the regenerated bis(2-hydroxyethyl) terephthalate can be prepared by further performing at least one of the following: thin-film distillation under reduced pressure; and dissolution in water followed by adsorption crystallization.
[0100] Thin film distillation is a distillation method in which a mixture to be separated is made into a thin film in order to increase the surface area in contact with a heat source. In detail, the mixture supplied to the evaporator of the thin film evaporator forms a thin film on the inner wall of the thin film evaporator by the wiper rotor. Then, distillation is performed under appropriate temperature conditions by heating. Furthermore, a condenser for recovering the evaporated product may be provided inside the thin film evaporator.
[0101] Thin film evaporation can be performed by short path evaporation. Such short path and thin film evaporation has a short residence time and allows reduced pressure distillation using high vacuum, so it is possible to separate high boiling point materials or high molecular weight materials that are difficult to separate by other distillation methods while minimizing changes in reactants due to heat. In addition, when the pressure in the thin film evaporator is reduced, the vapor pressure of the material is reduced, which has the advantage that it can be evaporated at a temperature lower than its original boiling point.
[0102] As a detailed example, the depolymerization product is supplied to the short path and thin film evaporator, and the thin film forming wiper is rotated at 300 rpm or more. As a result, the vaporized material and the non-vaporized material can be separated from each other. The internal thin film temperature of the upper thin film evaporator during the thin film evaporation may be, for example, 150°C to 250°C, 190°C to 250°C, or 180°C to 220°C. Furthermore, the internal pressure of the upper thin film evaporator during the thin film evaporation may be, for example, 0.005 Torr to 5.0 Torr, 0.05 Torr to 5.0 Torr, 0.05 Torr to 1.5 Torr, or 0.05 Torr to 1 Torr.
[0103] Adsorption crystallization can be carried out, for example, by using water as a solvent, adding an adsorbent, filtering, and crystallizing.
[0104] Various solvents can be used for adsorption crystallization, but the solvent is preferably one that can dissolve bis(2-hydroxyethyl) terephthalate. As a detailed example, to obtain the final reaction product, water is added as a solvent to the polymerization raw material containing the regenerated bis(2-hydroxyethyl) terephthalate, and the mixture is dissolved by heating, and an adsorbent is added thereto, followed by crystallization of the solution obtained by filtration, and finally filtration. As a result, the polymerization raw material with high purity can be obtained.
[0105] Water may be added in an amount of 100 to 500 parts by weight, specifically 200 to 400 parts by weight, and more specifically 300 to 350 parts by weight, relative to 100 parts by weight of the polymerization raw material.
[0106] Furthermore, the dissolution temperature may be from 50°C to 95°C, specifically from 60°C to 85°C, and more specifically from 70°C to 75°C.
[0107] The adsorbent added can function to adsorb and remove other foreign matter. It may be added in an amount of 0.1 to 3 parts by weight per 100 parts by weight of the polymerization raw material. The type and form of the adsorbent are not particularly limited. For example, activated carbon may be used.
[0108] [Mode of invention] Hereinafter, preferred embodiments of the present invention will be described for the understanding of the present invention. However, the following examples are provided for the purpose of facilitating the understanding of the present invention, and the scope of the present invention is not limited thereto.
[0109] Example 1 1,000g of waste polyester resin, 2,000g of ethylene glycol, and 5.0g of zinc acetate anhydride were charged into a first reactor made of stainless steel (SUS). The temperature inside the reactor was raised to 180°C, and depolymerization (first glycolysis reaction) was carried out for 2 hours. The reaction product thus obtained (first reaction product) was transferred to a second reactor and cooled to 150°C. 2,000g of ethylene glycol was further added thereto, and depolymerization (second glycolysis reaction) was carried out for 2 hours while maintaining the reactor temperature at 150°C.
[0110] The reaction product thus obtained (second reaction product) was cooled to 120°C by vacuum flashing, 16 g of a filter aid (Celite (trademark) 545) was added thereto, and then pressure filtration was performed to perform solid-liquid separation. The separated liquid reaction product was passed through a column filled with an ion exchange resin (Bonlite's BC107 (H)) to remove ionic impurities, and a mixture containing bis(2-hydroxyethyl) terephthalate and ethylene glycol (third reaction product) was obtained.
[0111] This mixture (third reactant) was cooled to room temperature over 2 hours while stirring at 100 rpm in a 10 liter crystallizer equipped with a cooling water circulation jacket. The resulting crystallized product was filtered through a pressure Nutsche filter (jacket type, filtration area 0.2 m) under a pressure of 3 bar. 2 The solid and liquid were separated using a cyclohexane distillation column to obtain a BHET cake (fourth reactant).
[0112] The BHET cake was transferred to a 10-liter distillation apparatus and heated again to 130°C. Unreacted ethylene glycol was recovered by vacuum distillation under reduced pressure conditions stepwise from 760 Torr to 0.8 Torr. The reaction product from which ethylene glycol had been removed (the fifth reaction product) was subjected to thin-film evaporation at 220°C and 0.08 Torr in a thin-film evaporator (VTA's VKL70-4S) to obtain 1,040 g of a product from which dimers and higher oligomers had been removed. Then, for adsorption crystallization, 1,040 g of the above product and 3,120 g of distilled water were charged into a 10-liter glass reactor and dissolved at a temperature of 70°C, and then 5.2 g of activated carbon was added thereto, followed by stirring for 30 minutes and filtering. The filtrate was cooled to room temperature for crystallization, filtered, and dried in a vacuum oven. As a result, 1,980 g of polymerization raw material containing regenerated bis(2-hydroxyethyl) terephthalate was obtained.
[0113] Example 2 The same operations as in Example 1 were repeated except that the reaction time of the first glycolysis reaction was adjusted to 1 hour, to obtain a polymerization raw material containing regenerated bis(2-hydroxyethyl) terephthalate.
[0114] Example 3 Filtration was carried out using a filter press (filtration area 0.4 m) under a pressure of 18 bar instead of a pressure Nutsche filter. 2 The same operations as in Example 1 were repeated except that 4 ea of filter plates were used to obtain a polymerization raw material containing regenerated bis(2-hydroxyethyl) terephthalate.
[0115] Example 4 The same procedure as in Example 1 was repeated except that waste polyester fiber was used as the waste polyester resin, to obtain a polymerization raw material containing regenerated bis(2-hydroxyethyl) terephthalate.
[0116] Example 5 The same operations as in Example 1 were repeated except that the adsorption crystallization was not carried out after the thin-film distillation, to obtain a polymerization raw material containing regenerated bis(2-hydroxyethyl) terephthalate.
[0117] Comparative Example 1 The same operations as in Example 1 were repeated except that the temperature of the first glycolysis reaction was adjusted to 210°C and the temperature of the second glycolysis reaction was adjusted to 250°C, thereby obtaining a polymerization raw material containing regenerated bis(2-hydroxyethyl) terephthalate.
[0118] Comparative Example 2 The same procedure as in Example 1 was repeated, except that the cooling crystallization and pressure Nutsche filter steps were omitted, to obtain a polymerization raw material containing regenerated bis(2-hydroxyethyl) terephthalate.
[0119] Test Example The polymerization feedstocks containing the recycled bis(2-hydroxyethyl) terephthalate of the examples and comparative examples were each tested as follows.
[0120] (1) High-performance liquid chromatography (HPLC) About 0.01 g of each polymerization raw material containing regenerated bis(2-hydroxyethyl) terephthalate was diluted with about 20 ml of methanol and analyzed by high performance liquid chromatography (HPLC) (model: Waters e2695, column: C18 (4.6 x 250 mm), 5 μm, UV detector: 242 nm, injection volume: 10 μl, eluent (gradient) A: H2O + H3PO4, B: acetonitrile). Then, the peak area portion (%) of the following components out of the total peak area of HPLC was obtained. MHET: Monohydroxyethyl terephthalate BHET: Bis(2-hydroxyethyl) terephthalate DEG-Ester-1: 2-Hydroxyethyl [2-(2-hydroxyethoxy)ethyl] terephthalate DEG-Ester-2: Bis[2-(2-hydroxyethoxy)ethyl]benzene-1,4-dicarboxylate HA-ester: 2-hydroxyethyl (2-acetoxyethyl) terephthalate Dimer: BHET dimer Trimer: BHET trimer
[0121] (2) Gas chromatography (GC) 0.1 g of each of the polymerization raw materials containing the regenerated bis(2-hydroxyethyl) terephthalate was dissolved in 10 ml of CHCl, filtered through a 0.45 μm filter, and measured by GC. Model: Agilent 7890B Column: DB-624 (30m x 0.25mm x 1.4μm) Oven temperature: 60℃(2min)-10℃ / min-200℃(0min)-20℃ / min-260℃(5min) Injector temperature: 250℃ Detector temperature: 250℃ Flow rate: 1.5ml / min (N2), split ratio: 1 / 50
[0122] (3) TDI Each polymerization raw material containing the regenerated bis(2-hydroxyethyl) terephthalate was subjected to HPLC analysis in the same manner as in section (1) above. Then, the thermal degradation index (TDI) was calculated, which is defined as follows: TDI = [DEG-ester-1] + [DEG-ester-2] × 2 + exp^[HA-ester] Here, DEG-ester-1 is the peak area fraction (%) of 2-hydroxyethyl [2-(2-hydroxyethoxy)ethyl] terephthalate, DEG-ester-2 is the peak area fraction (%) of bis[2-(2-hydroxyethoxy)ethyl] benzene-1,4-dicarboxylate, and HA-ester is the peak area fraction (%) of 2-hydroxyethyl (2-acetoxyethyl) terephthalate. This index was calculated by removing the units of these parameters and taking only the numerical values.
[0123] (4) Differential scanning calorimetry (DSC) For each polymerization feedstock, including the regenerated bis(2-hydroxyethyl) terephthalate, the melting point (mp) was measured using a differential scanning calorimeter (DSC, TA Instruments Q20) while heating from 30° C. to 280° C. at a rate of 20° C. / min.
[0124] (5) Inductively Coupled Plasma Atomic Emission Spectroscopy (ICP-AES) 0.3 g of each polymerization raw material containing regenerated bis(2-hydroxyethyl) terephthalate was sonicated and diluted with ultrapure water. The inorganic content (ppm) was measured using ICP-AES (Agilent Model 5100) (detection limit 5 ppm).
[0125] (6)Yellowness index (YID) Each polymerization raw material, including the regenerated bis(2-hydroxyethyl) terephthalate, was dissolved in dimethylformamide at room temperature at a concentration of 25% by weight, and the yellowness index was measured after 30 minutes. Transmission data was obtained using a Hunterlab Color Flex EZ with a D65 light source at an observer angle of 2°. Yellowness index (YID) values were calculated using the software Color Analyzer.
[0126] The results of the test examples are shown in the table below.
[0127] [Table 1]
[0128] As can be seen from the above table, the polymerization raw materials containing recycled BHET obtained in Examples 1 to 5 had a total of 2.0% or less of HPLC peak area of diethylene glycol ester compounds (DEG-ester-1, DEG-ester-2) and 1.0% or less of HPLC peak area of acetic acid ester compounds (HA-ester), but were excellent in other impurities (MHET, dimer, trimer) or residual EG content, melting point (mp), inorganic matter content, and yellowness index (YID). In particular, the polymerization raw materials containing recycled BHET obtained in Examples 1 to 5 had a thermal property drop index (TDI) of 3.0 or less. Therefore, when recycled polyester resin is polymerized from this, it is expected to have excellent heat resistance properties.
[0129] In contrast, the polymerization raw materials containing recycled BHET obtained in Comparative Examples 1 and 2 had a total of more than 2.0% of diethylene glycol ester compounds (DEG-ester-1, DEG-ester-2) HPLC peak area, and a total of more than 1.0% of acetic acid ester compounds (HA-ester) HPLC peak area, but were inferior in other impurities (MHET, dimer, trimer) or residual EG content, melting point (mp), inorganic matter content, and yellowness index (YID). In particular, the polymerization raw materials containing recycled BHET obtained in Comparative Examples 1 and 2 had a maximum thermal property drop index (TDI) of 9.23. Therefore, when recycled polyester resin is polymerized from this, it is expected that the heat resistance properties will be inferior.
Claims
1. A polymerization raw material obtained by depolymerization of waste polyester, the polymerization raw material having a peak area of bis(2-hydroxyethyl) terephthalate of 95% or more, a peak area of acetate ester compounds of 0.001% to 1.0% in total, and a peak area of diethylene glycol ester compounds of 0.001% to 2.0% in total, when measured by high performance liquid chromatography (HPLC).
2. The polymerization raw material according to claim 1, wherein the acetic acid ester compound comprises 2-hydroxyethyl (2-acetoxyethyl) terephthalate.
3. 2. The polymerization material of claim 1, wherein the diethylene glycol ester compounds include 2-hydroxyethyl[2-(2-hydroxyethoxy)ethyl]terephthalate and bis[2-(2-hydroxyethoxy)ethyl]benzene-1,4-dicarboxylate.
4. When measured by high performance liquid chromatography (HPLC), the compound had the following formula: TDI = [DEG-ester-1] + [DEG-ester-2] x 2 + exp^[HA-ester] The thermal property drop index is 3.0 or less, The polymerization raw material according to claim 1, wherein DEG-ester-1 is the peak area portion (%) of 2-hydroxyethyl[2-(2-hydroxyethoxy)ethyl]terephthalate, DEG-ester-2 is the peak area portion (%) of bis[2-(2-hydroxyethoxy)ethyl]benzene-1,4-dicarboxylate, and HA-ester is the peak area portion (%) of 2-hydroxyethyl(2-acetoxyethyl)terephthalate, and the index is calculated by taking only the numerical values of these parameters excluding the units.
5. 2. The polymerization raw material according to claim 1, which has a peak area of dimers or higher oligomers of 2.0% or less in total when measured by high performance liquid chromatography (HPLC).
6. 2. The polymerization raw material according to claim 1, wherein the content of residual ethylene glycol in the polymerization raw material is 0.5% by weight or less.
7. 2. The polymerization material of claim 1 having a Yellowness Index (YID) of 5.0 or less when measured on a 25% by weight solution in dimethylformamide.
8. 2. The polymerization material of claim 1 having a melting point of 110°C to 115°C.
9. 2. A method for preparing the polymerization material of claim 1, comprising: (a) depolymerizing waste polyester by glycolysis to obtain a crude bis(2-hydroxyethyl) terephthalate solution; (b) cooling the crude bis(2-hydroxyethyl) terephthalate solution to crystallize it; (c) separating the crystallized product into a solid and a liquid using a pressure filter.
10. The depolymerization of step (a) (1) subjecting the waste polyester to depolymerization by a first glycolysis reaction at a temperature of 180° C. to 200° C. to obtain a first reactant; (2) subjecting the first reactant to depolymerization by a second glycolysis reaction at a temperature of 150 to 170° C. to obtain a second reactant; 10. The method of claim 9, comprising:
11. 10. The method of claim 9, wherein the pressure filter in step (c) is a Nutsche filter or a filter press.
12. 10. The method of claim 9, wherein acetic acid-based compounds and diethylene glycol-based compounds are removed by the pressure filter in step (c).
13. 10. The method of claim 9, wherein the polymerization feed is prepared by the further step of removing unreacted glycol by distillation.
14. 10. The method of claim 9, wherein the polymerization material is prepared by further performing at least one of: thin film distillation under reduced pressure; and dissolution in water followed by adsorptive crystallization.
Citation Information
Patent Citations
METHOD FOR PRODUCING BIS-beta-HYDROXYETHYL TEREPHTHALATE
JP2003055300A
Method for recovering ester monomer from polyester fibers
JP2005330444A
Method for recovering ester monomer from polyester fiber waste
JP2006232701A
Multipurpose shoe closet
KR1020220159669A
KR20210067555A
Cited By
Polyamide recovery method and polyamide recovery system
JP2026128674A