Process for recovering dialkyl terephthalates from polyester compositions - Patents.com

The method addresses the high resource and energy demands of conventional polyester recycling by using glycolysis and alcoholysis processes at reduced temperatures and pressures, achieving efficient and high-purity dialkyl terephthalate recovery.

JP2024539955AInactive Publication Date: 2024-10-31EASTMAN CHEM CO
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
JP2024524630
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2021-10-25
Filing Date
2022-10-25
Publication Date
2024-10-31
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Conventional glycolysis and methanolysis processes for recycling polyester compositions require substantial amounts of resources and energy.

Method used

A method involving glycolysis and alcoholysis processes is employed, where a polyester composition is exposed to a first glycol composition and glycolysis catalysts under depolymerization conditions, followed by alcoholysis to recover dialkyl terephthalates, utilizing reduced temperatures and pressures to minimize energy and resource consumption.

Benefits of technology

The method achieves high yields and high purity of dialkyl terephthalates with reduced energy and resource requirements, enabling efficient recycling of polyester compositions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024539955000011
    Figure 2024539955000011
  • Figure 2024539955000001
    Figure 2024539955000001
  • Figure 2024539955000002
    Figure 2024539955000002
Patent Text Reader

Abstract

A method for recovering dialkyl terephthalates. The method may include exposing a polyester composition to depolymerization conditions to one or more glycols, thereby providing one or more depolymerized products. The one or more glycols may include diethylene glycol (DEG), triethylene glycol (TEG), 1,4-cyclohexanedimethanol (CHDM), poly(ethylene glycol) (PEG), neopentyl glycol (NPG), propanediol (PDO), butanediol (BDO), 2-methyl-2,4-pentanediol (MP diol), poly(tetramethylene ether) glycol (PTMG), or combinations thereof. The one or more depolymerized products may be exposed to an alcoholysis process to recover dialkyl terephthalates. Optionally, ethylene glycol (EG) produced from the depolymerization process may be recovered and reused in subsequent dialkyl terephthalate recovery or other processes.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to methods for recycling polyester compositions. More particularly, the present disclosure relates to recovering dialkyl terephthalates from polyester compositions. [Background technology]

[0002] Certain conventional systems may utilize glycolysis and / or methanolysis processes in an attempt to recycle polyesters, however, certain conventional glycolysis and / or methanolysis processes may require substantial amounts of resources and energy to arrive at a product suitable for use in a subsequent production process, such as a production process to make recycled polyester or other compositions. Summary of the Invention

[0003] In one aspect, a method for recovering one or more dialkyl terephthalates from a polyester composition is provided. The method may include exposing the polyester composition to a first glycol composition and one or more glycolysis catalysts in a reaction vessel under depolymerization conditions to provide a first mixture, the first mixture comprising one or more depolymerization products; ethylene glycol (EG); and one or more insoluble components. The depolymerization conditions include a temperature in the range of about 120° C. to about 260° C., a pressure in the range of about 0.013 atm (0.2 psig) to about 10.2 atm (150 psig), and a time period in the range of about 0.5 hours to about 10 hours. The first glycol composition comprises diethylene glycol (DEG), triethylene glycol (TEG), 1,4-cyclohexanedimethanol (CHDM), poly(ethylene glycol) (PEG), neopentyl glycol (NPG), propanediol (PDO), butanediol (BDO), 2-methyl-2,4-pentanediol (MP diol), poly(tetramethylene ether) glycol (PTMG), or combinations thereof. The method further comprises removing at least a portion of the EG from the reaction vessel while exposing the polyester composition to the first glycol composition and one or more glycolysis catalysts in the reaction vessel. The method may also comprise exposing at least a portion of a first liquid component of the first mixture to one or more alcohols and an alcoholysis catalyst under alcoholysis conditions to provide a second mixture, the second mixture comprising a solid component comprising one or more dialkyl terephthalates and a second liquid component. The alcoholysis conditions include a temperature in the range of about 25° C. to about 90° C., a pressure in the range of about 1 atm (14.7 psig) to about 2 atm (30 psig), and a duration in the range of about 0.5 hours to about 5 hours. The method may also include separating at least a portion of the one or more dialkyl terephthalates from the second mixture by solid-liquid separation.

[0004] In another aspect, a method for recovering one or more dialkyl terephthalates from a polyester composition is provided. The method may include exposing the polyester composition to a first glycol composition and one or more glycolysis catalysts in a reaction vessel under depolymerization conditions to provide a first mixture, the first mixture comprising a first liquid component and one or more insoluble components. The first glycol composition comprises diethylene glycol (DEG), triethylene glycol (TEG), 1,4-cyclohexanedimethanol (CHDM), poly(ethylene glycol) (PEG), neopentyl glycol (NPG), propanediol (PDO), butanediol (BDO), 2-methyl-2,4-pentanediol (MP diol), poly(tetramethylene ether) glycol (PTMG), or a combination thereof. The first liquid component comprises one or more depolymerization products and ethylene glycol (EG), and the depolymerization conditions comprise a temperature in the range of about 120° C. to about 260° C., a pressure in the range of about 0.013 atm (0.2 psig) to about 10.2 atm (150 psig), and a time period in the range of about 0.5 hours to about 10 hours. The method may also comprise exposing at least a portion of the first liquid component to one or more alcohols and an alcoholysis catalyst under alcoholysis conditions in an alcoholysis reactor to provide a second mixture, the second mixture comprising a solid component comprising one or more dialkyl terephthalates and a second liquid component. The alcoholysis conditions comprise a temperature in the range of about 25° C. to about 90° C., a pressure in the range of about 1 atm (14.7 psig) to about 2 atm (30 psig), and a time period in the range of about 0.5 hours to about 5 hours. The method may also include separating at least a portion of the one or more dialkyl terephthalates from the second mixture; and exposing at least a portion of the second liquid component to distillation conditions to separate at least a portion of the EG and provide a recycled glycol composition, wherein the recycled glycol composition comprises at least a portion of the first glycol composition. [Brief description of the drawings]

[0005] [Figure 1]1 is an exemplary system for recovering one or more dialkyl terephthalates from a polyester composition according to an embodiment of the present disclosure. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0006] overview The present disclosure may be more readily understood by reference to the following detailed description of certain aspects and examples of the disclosure. In accordance with the purposes of this disclosure, certain aspects of the disclosure are described in the Summary of the Invention and further described herein below. Other aspects of the disclosure are also described herein.

[0007] Aspects herein relate to methods for recovering one or more dialkyl terephthalates from a polyester composition. As described herein, an exemplary method may include exposing a polyester composition to one or more glycols under depolymerization conditions to produce one or more depolymerization products, which are then exposed to an alcoholysis process to recover the dialkyl terephthalates.

[0008] As discussed above, certain conventional glycolysis and / or methanolysis processes may require substantial amounts of resources and energy to arrive at a product suitable for use in a downstream production process, such as a production process for making recycled polyester or other compositions.

[0009] The methods and systems disclosed herein can alleviate one or more of the above problems. For example, in certain embodiments, the methods disclosed herein can include exposing a polyester composition to depolymerization conditions with one or more glycols to provide one or more depolymerization products. In various embodiments, the one or more depolymerization products can include monomers, oligomers, or combinations thereof. In embodiments, the one or more depolymerization products can be exposed to alcoholysis conditions to obtain high yields and high purity dialkyl terephthalate products. As discussed herein, the alcoholysis conditions include reduced temperatures compared to certain conventional systems, which reduces the overall energy and resources required.

[0010] Polyester Composition As discussed above, the methods described herein relate to recovering one or more dialkyl terephthalates from a polyester composition. The term "polyester" may refer to a synthetic polymer prepared by the reaction of one or more difunctional carboxylic acids and / or polyfunctional carboxylic acids with one or more difunctional hydroxyl compounds and / or polyfunctional hydroxyl compounds. The difunctional carboxylic acids may be dicarboxylic acids and the difunctional hydroxyl compounds may be dihydric alcohols such as glycols. Additionally, as used herein, the term "diacid" or "dicarboxylic acid" includes polyfunctional acids such as branching agents. As used herein, the term "glycol" or "diol" includes, but is not limited to, diols, glycols, and / or polyfunctional hydroxyl compounds. The dicarboxylic acid residues may be derived from dicarboxylic acid monomers or their associated acid halides, esters, salts, anhydrides, or mixtures thereof. Thus, as used herein, the term dicarboxylic acid is intended to include dicarboxylic acids and any derivatives thereof, including their associated acid halides, esters, half esters, salts, half salts, anhydrides, mixed anhydrides, or mixtures thereof, that are useful in the reaction process with diols to make polyesters. As used herein, the term "polyester" should be understood to also refer to copolyesters.

[0011] As used herein, the term "residue" refers to a monomeric or repeating unit in a polymer, oligomer, or dimer. For example, a polymer may be made from the condensation of the following monomers: terephthalic acid ("TPA") and cyclohexyl-1,4-dimethanol ("CHDM"). The condensation reaction results in the loss of a water molecule. The residue in the resulting polymer comes from either terephthalic acid or cyclohexyl-1,4-dimethanol. Formula (I) below illustrates a non-limiting example of a polyester.

[0012] [ka]

[0013] In an embodiment, the polyester composition exhibits an intrinsic viscosity of from about 0.1 dL / g to about 1.2 dL / g, as determined in accordance with ASTM D2857-70, from about 0.2 dL / g to about 1.2 dL / g, as determined in accordance with ASTM D2857-70, from about 0.3 dL / g to about 1.2 dL / g, as determined in accordance with ASTM D2857-70, or from about 0.4 dL / g to about 1.2 dL / g, as determined in accordance with ASTM D2857-70.

[0014] In embodiments, the polyester composition may include one or more polyesters. In various embodiments, the one or more polyesters may include terephthalate polyesters. Terephthalate polyesters are polyesters that include residues of terephthalic acid or any derivative of terephthalic acid, including its associated acid halides, esters, half esters, salts, half salts, anhydrides, mixed anhydrides, and / or mixtures thereof or residues thereof, that are useful in the reaction process with diols to make copolyesters. In various embodiments, the polyester composition may include polyethylene terephthalate (PET). In one or more embodiments, the polyester composition may include glycol modified PET. In certain embodiments, the polyester composition may comprise polyethylene terephthalate (PET), 1,4-cyclohexanedimethanol (CHDM) modified PET, isophthalic acid (IPA) modified PET, diethylene glycol (DEG) modified PET, glycol modified PET, neopentyl glycol (NPG) modified PET, propanediol (PDO) modified PET, butanediol (BDO) modified PET, heaxanediol (HDO) modified PET, 2-methyl-2,4-pentanediol (MP diol) modified PET, isosorbide modified PET, polycyclohexylene dimethylene terephthalate (PCT), cyclohexanedimethanol (CHDM) containing copolyesters, isosorbide containing copolyesters, or combinations thereof.

[0015] In various embodiments, the polyester composition may include CHDM. In one embodiment, the polyester composition may include about 0 mol% to about 100 mol% CHDM, about 1 mol% to about 100 mol% CHDM, about 1 mol% to about 90 mol% CHDM, about 1 mol% to about 80 mol% CHDM, about 1 mol% to about 70% CHDM, about 1 mol% to about 60 mol% CHDM, about 1 mol% to about 50 mol% CHDM, about 1 mol% to about 40 mol% CHDM, about 1 mol% to about 35 mol% CHDM, about 1 mol% to about 30 mol% CHDM, about 1 mol% to about 25 mol% CHDM, about 1 mol% to about 20 mol% CHDM, about 1 mol% to about 10 mol% CHDM, or about 1 mol% to about 5 mol% CHDM. In an embodiment, the mol% of CHDM refers to the mol% of CHDM relative to all diol equivalents in the polyester composition. In various embodiments, the polyester composition may include DEG. In embodiments, the polyester composition may include about 0 mol% to about 100 mol% DEG, about 1 mol% to about 100 mol% DEG, about 1 mol% to about 90 mol% DEG, about 1 mol% to about 80 mol% DEG, about 1 mol% to about 70 mol% DEG, about 1 mol% to about 60 mol% DEG, about 1 mol% to about 50 mol% DEG, about 1 mol% to about 40 mol% DEG, about 1 mol% to about 35 mol% DEG, about 1 mol% to about 30 mol% DEG, about 1 mol% to about 20 mol% DEG, about 1 mol% to about 10 mol% DEG, about 1 mol% to about 5 mol% DEG, or about 1 mol% to about 3 mol% DEG. In embodiments, the mol% of DEG refers to the mol% of DEG relative to all diol equivalents in the polyester composition. In an embodiment, the polyester composition may include isophthalic acid.In an embodiment, the polyester composition may comprise from about 0 mol% to about 30 mol% isophthalic acid, from about 1 mol% to about 30 mol% isophthalic acid, from about 1 mol% to about 25 mol% isophthalic acid, from about 1 mol% to about 20 mol% isophthalic acid, from about 1 mol% to about 15 mol% isophthalic acid, from about 1 mol% to about 10 mol% isophthalic acid, from about 1 mol% to about 7.5 mol% isophthalic acid, from about 1 mol% to about 5 mol% isophthalic acid, from about 1 mol% to about 3 mol% isophthalic acid, up to about 10 mol% isophthalic acid, up to about 7.5 mol% isophthalic acid, up to about 5 mol% isophthalic acid, or up to about 3 mol% isophthalic acid. In an embodiment, the mol% of isophthalic acid refers to the mol% of isophthalic acid relative to the total diacid equivalents in the polyester composition. In certain embodiments, the polyester composition may comprise about 0 mol% to about 100 mol% CHDM, about 0 mol% to about 100 mol% DEG, about 0 mol% to about 30 mol% isophthalic acid, or a combination thereof. In certain embodiments, the polyester composition may comprise about 1 mol% to about 100 mol% CHDM, about 1 mol% to about 100 mol% DEG, about 1 mol% to about 30 mol% isophthalic acid, or a combination thereof. In various embodiments, the polyester composition may comprise other glycols, such as those other than those mentioned above. For example, in embodiments, the polyester composition may comprise, but is not limited to, neopentyl glycol (NPG), 2-methyl-2,4-pentanediol (MP diol), butanediol (BDO), propanediol (PDO), hexanediol (HDO), isosorbide, poly(tetramethylene ether) glycol (PTMG), poly(ethylene) glycol (PEG), or a combination thereof.In certain embodiments, each of NPG, MP diol, BDO, PDO, HDO, isosorbide, PTMG and PEG may be present in the polyester composition in an amount of 0 mol % to about 100 mol %, about 1 mol % to about 100 mol %, about 1 mol % to about 90 mol %, about 1 mol % to about 80 mol %, about 1 mol % to about 70 mol %, about 1 mol % to about 60 mol %, about 1 mol % to about 50 mol %, about 1 mol % to about 40 mol %, about 1 mol % to about 35 mol %, about 1 mol % to about 30 mol %, about 1 mol % to about 25 mol %, about 1 mol % to about 20 mol %, about 1 mol % to about 10 mol %, or about 1 mol % to about 5 mol %. In embodiments, the mole % of each of NPG, MP diol, BDO, PDO, HDO, isosorbide, PTMG, and PEG refers to the mole % of each of NPG, MP diol, BDO, PDO, HDO, isosorbide, PTMG, and PEG, respectively, relative to the total diol equivalents in the polyester composition. In various embodiments, the polyester composition may include CHDM, DEG, NPG, MP diol, BDO, PDO, HDO, isosorbide, PTMG, PEG, isophthalic acid, or combinations thereof, each component being present in any of the amounts for such components described in this paragraph.

[0016] In embodiments, the polyester composition or one or more polyesters present in the polyester composition may be recycled polyester. In various embodiments, recycled polyester may include materials recovered as manufacturing scrap, post-industrial waste, post-consumer waste, or combinations thereof. In embodiments, recycled polyester may be used and / or discarded post-consumer products. In embodiments, the polyester composition and / or recycled polyester may be obtained from various sources and / or in various forms, including, but not limited to, textiles, carpets, thermoforming materials, bottles, pellets, and films. In one or more embodiments, the polyester composition may include recycled polyester, e.g., polyester formed from DMT recovered from a prior DMT recovery process, such as the processes described herein.

[0017] In various embodiments, the polyester composition may include one or more foreign materials. In embodiments, the one or more foreign materials may include, but are not limited to, polyesters other than polyethylene terephthalate, polyvinyl chloride (PVC), polyvinyl acetal, polyvinyl butyral (PVB), polyvinyl alcohol (PVOH), ethylene vinyl alcohol (EVOH), cotton, polyolefins, polyethylene, polypropylene, polystyrene, polycarbonate, spandex, natural fibers, cellulose esters, polyacrylates, polymethacrylates, polyamides, nylons, poly(lactic acid), polydimethylsiloxanes, polysilanes, calcium carbonate, titanium dioxide, inorganic fillers, dyes, pigments, color toners, colorants, plasticizers, adhesives, flame retardants, metals, aluminum and iron, or combinations thereof. In various embodiments, the one or more foreign matter may be present in the polyester composition in an amount of from about 0.01 wt.% to about 50 wt.%, from about 0.01 wt.% to about 40 wt.%, from about 0.01 wt.% to about 30 wt.%, from about 0.01 wt.% to about 20 wt.%, from about 0.01 wt.% to about 15 wt.%, from about 0.01 wt.% to about 10 wt.%, from about 0.01 wt.% to about 7.5 wt.%, from about 0.01 wt.% to about 5 wt.%, from about 0.01 wt.% to about 2.5 wt.%, or from about 0.01 wt.% to about 1.0 wt.%, based on the weight of the one or more polyesters in the polyester composition.

[0018] In embodiments, the polyester composition may be in a solid form, liquid form, melt form, or solution. In certain embodiments, the solution may include the polyester composition pre-dissolved in a solvent, such as DMT, EG, DEG, TEG, or combinations thereof.

[0019] Optional Pretreatment of the Polyester Composition In certain embodiments, optional treatment of the polyester composition may be performed prior to glycolysis and / or methanolysis. In various embodiments, the optional pretreatment may include any type of treatment that aids in removing a portion of any contaminants from the polyester composition and / or aids in recovering one or more polyesters from a mixed feedstock, such as a feedstock containing the contaminants discussed above. For example, in one embodiment, the optional pretreatment may include exposing the polyester composition to one or more solvents to selectively dissolve the polyesters in the polyester composition (or at least a portion of the contaminants in the polyester composition) to allow separation between at least a portion of the contaminants and one or more polyesters in the polyester composition. In one example embodiment, the optional pretreatment may include exposing the polyester composition to one or more solvents, such as one or more solvents that can cause dissolution of the polyesters in the polyester composition. For example, the one or more solvents may include, but are not limited to, 4-methylcyclohexanemethanol (MCHM), ethylene glycol (EG), diethylene glycol (DEG), triethylene glycol (TEG), 1,4-cyclohexanedimethanol (CHDM), poly(ethylene glycol) (PEG), neopentyl glycol (NPG), propanediol (PDO), butanediol (BDO), 2-methyl-2,4-pentanediol (MP diol), poly(tetramethylene ether) glycol (PTMG), dibutyl terephthalate (DBT), dioctyl terephthalate (DOTP), ethylene carbonate (EC), dimethyl carbonate (DMC), dimethyl sulfoxide (DMSO), dimethylformamide (DMF), or combinations thereof. In the same or alternative embodiment, the polyester composition may be exposed to one or more solvents at a particular temperature to effect dissolution of one or more components. In various embodiments, the pretreatment process may include one or more dissolution and separation steps using various solvents and / or temperatures to achieve a desired level of contaminant removal and / or purity level of PET.For example, in one embodiment, dissolution and separation can be utilized using one solvent at a particular temperature, e.g., to remove one or more contaminants, followed by subsequent dissolution and separation of the polyester fraction using another solvent at a particular temperature, e.g., to remove one or more other contaminants. The dissolution and / or separation in this optional pretreatment step can utilize any suitable system, reactor, vessel, and / or separation technique to achieve the desired pretreated polyester composition.

[0020] Glycolysis of polyester compositions As discussed above, in various aspects, the methods disclosed herein may include exposing a polyester composition to depolymerization conditions to depolymerize at least a portion of the one or more polyesters into one or more depolymerized products. In various aspects, the one or more depolymerized products may include monomers, oligomers, or combinations thereof. In certain aspects, the oligomers may exhibit a degree of polymerization of 2-10, 2-8, 2-6, or 2-4. In aspects, the one or more polyesters may be depolymerized into one or more depolymerized products that may include monomers and terephthalate oligomers having a degree of polymerization of 2-10, 2-8, 2-6, or 2-4. In aspects, liquid chromatography may be performed to identify the degree of polymerization of the oligomers, and / or gel permeation chromatography may be utilized to identify the molecular weight of the oligomers.

[0021] In an embodiment, the term degree of polymerization (DP) may refer to the number of residues in an oligomer. As used herein, degree of polymerization (DP) refers to the number of difunctional carboxylic acid residues and / or polyfunctional carboxylic acid residues in an oligomer. For example, in one exemplary embodiment, a DP of 1 refers to a residue that contains one terephthalic acid residue or one isophthalic acid residue. In such an exemplary embodiment, a DP of 1 may also be referred to as a monomer. A non-limiting example of a DP of 1 is provided below in formula (II), where R may be a glycol, such as any of the glycols described herein in an embodiment.

[0022] [ka]

[0023]

[0028] The following formulas (III)-(V) show non-limiting examples of oligomers having DPs of 2, 3, and n, respectively, in embodiments. In formulas (III), (IV), and (V), R may be a glycol, such as any of the glycols described herein in embodiments.

[0024] [ka]

[0025] In an embodiment, this depolymerization may be carried out via a glycolysis process. In general, in an embodiment, the glycolysis process may include exposing the polyester composition to one or more glycols, which react with the polyester, optionally in the presence of a transesterification catalyst, to form a mixture of bis(hydroxyethyl) terephthalate (BHET) or other terephthalate residues (e.g., when DEG is utilized, bis(2-hydroxydiethylene terephthalate) (BHDET)) and low molecular weight terephthalate oligomers, depending on the glycol used. Some representative examples of glycolysis methods are disclosed in U.S. Patent Nos. 3,257,335; 3,907,868; 6,706,843; and 7,462,649, which are incorporated herein by reference.

[0026] In one embodiment of the glycolysis process, one or more polyesters, such as one or more recycled polyesters, and one or more glycols can be fed to a glycolysis reactor, where the one or more recycled polyesters are dissolved and depolymerized under depolymerization conditions.

[0027] In embodiments, any amount of one or more glycols suitable for use in a glycolysis process can be utilized. In various embodiments, the weight ratio of one or more glycols to the amount of polyester composition can be 9:1 to 1:9, 8:1 to 1:9, 7:1 to 1:9, 6:1 to 1:9, 5:1 to 1:9, 4:1 to 1:9, 3:1 to 1:9, 2:9 to 1:9, 9:1 to 1:8, 9:1 to 1:7, 9:1 to 1:6, 9:1 to 1:5, 9:1 to 1:4, 9:1 to 1:3, or 9:1 to 1:2.

[0028] In certain embodiments, the one or more glycols may include any glycol suitable for use in the glycolysis process. As used herein, the term "glycol" refers to aliphatic, cycloaliphatic, and aralkyl glycols. Exemplary glycols include ethylene glycol, 1,2-propanediol (also known as propylene glycol), 1,3-propanediol, 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol, 2,2-dimethyl-1,3-propanediol, 1,2-cyclohexanedimethanol, 1,3-cyclohexanedimethanol, 1,4-cyclohexanedimethanol, 2,2,4,4-tetramethyl-1,3-cyclobutanediol, isosorbide, p-xylylenediol, and the like. These glycols may also include ether linkages, such as in the case of diethylene glycol, triethylene glycol, and tetraethylene glycol. Additional glycol embodiments include the higher molecular weight homologs known as polyethylene glycols, such as those produced by Dow Chemical Company under the trade name Carbowax™. In one embodiment, the polyethylene glycol (PEG) has a molecular weight of greater than 200 to about 10,000 Daltons (M n ) These glycols also include higher alkyl analogs such as dipropylene glycol, dibutylene glycol, etc. Similarly, additional glycols have molecular weights of about 200 to about 10,000 Daltons (M n) (also referred to as g / mole) range, and higher polyalkylene ether diols such as polypropylene glycol and polytetramethylene glycol. In one aspect, the glycol can be selected from aliphatic, cycloaliphatic and aralkyl glycols. In various aspects, the glycol can be selected from polyalkylene ether diols selected from ethylene glycol; 1,2-propanediol; 1,3-propanediol; 1,4-butanediol; 1,5-pentanediol; 1,6-hexanediol; 2,2-dimethyl-1,3-propanediol; 1,2-cyclohexanedimethanol; 1,3-cyclohexanedimethanol; 1,4-cyclohexanedimethanol; 2,2,4,4-tetramethyl-1,3-cyclobutanediol; isosorbide; p-xylylenediol; diethylene glycol; triethylene glycol; tetraethylene glycol; polyethylene glycol; dipropylene glycol; dibutylene glycol; polypropylene glycol and polytetramethylene glycol.

[0029] In certain embodiments, the one or more glycols may include diethylene glycol (DEG), triethylene glycol (TEG), 1,4-cyclohexanedimethanol (CHDM), poly(ethylene glycol) (PEG), neopentyl glycol (NPG), propanediol (PDO), butanediol (BDO), 2-methyl-2,4-pentanediol (MP diol), poly(tetramethylene ether) glycol (PTMG), or combinations thereof; and optionally ii) ethylene glycol (EG). In such embodiments, the weight ratio of the glycols of group i) to EG may be 100:0 to 1:99. In certain embodiments, the one or more glycols may include about 0 wt.% to about 100 wt.% DEG, or about 1 wt.% to about 100 wt.% DEG, based on the total weight of the one or more glycols. In certain embodiments, the one or more glycols may comprise about 0 wt.% to about 100 wt.% TEG, or about 1 wt.% to about 100 wt.% TEG, based on the total weight of the one or more glycols. In embodiments, the one or more glycols may comprise about 0 wt.% to about 50 wt.% CHDM, or about 1 wt.% to about 100 wt.% CHDM, based on the total weight of the one or more glycols. In various embodiments, the one or more glycols may comprise 0 wt.% to about 100 wt.% PEG, or about 1 wt.% to about 100 wt.% PEG, based on the total weight of the one or more glycols. In various embodiments, the one or more glycols may comprise 0 wt.% to about 100 wt.% NPG, or about 1 wt.% to about 100 wt.% NPG, based on the total weight of the one or more glycols. In various embodiments, the one or more glycols may comprise 0 wt.% to about 100 wt.% PDO, or about 1 wt.% to about 100 wt.% PDO, based on the total weight of the one or more glycols. In various embodiments, the one or more glycols may comprise 0 wt.% to about 100 wt.% BDO, or about 1 wt.% to about 100 wt.% BDO, based on the total weight of the one or more glycols. In various embodiments, the one or more glycols may comprise 0 wt.% to about 100 wt.% MP diol, or about 1 wt.% to about 100 wt.% MP diol, based on the total weight of the one or more glycols.In various embodiments, the one or more glycols may comprise 0 wt.% to about 100 wt.% PTMG, or about 1 wt.% to about 100 wt.% PTMG, based on the total weight of the one or more glycols. In certain embodiments, the one or more glycols may comprise about 0 wt.% to about 100 wt.% EG, or about 1 wt.% to about 100 wt.% EG, based on the total weight of the one or more glycols. In one embodiment, the one or more glycols may include 0 wt.% to about 100 wt.% EG, 0 wt.% to about 100 wt.% DEG, 0 wt.% to about 100 wt.% TEG, 0 wt.% to about 100 wt.% PEG, 0 wt.% to about 100 wt.% NPG, 0 wt.% to about 100 wt.% PDO, 0 wt.% to about 100 wt.% BDO, 0 wt.% to about 100 wt.% MP diol, 0 wt.% to about 100 wt.% PTMG, and 0 wt.% to about 50 wt.% CHDM, based on the total weight of the one or more glycols. In certain embodiments, as discussed in detail below, the one or more glycols may be recycled glycols recovered from a prior glycolysis and / or methanolysis process to recover one or more dialkyl terephthalates, as disclosed herein.

[0030] In various embodiments, as discussed above, the glycolysis process may include one or more catalysts, such as a transesterification catalyst. In certain embodiments, the catalyst may be present in an amount of 0.1 wt.% to 10 wt.% based on the weight of the polyester composition. In embodiments, any suitable catalyst may be utilized. In one embodiment, the catalyst may include a carbonate catalyst, such as, but not limited to, Li2CO3, K2CO3, Na2CO3, Cs2CO3, ZrCO3, or combinations thereof. In one embodiment, the catalyst may include a hydroxide catalyst, such as, but not limited to, LiOH, NaOH, KOH, tetrabutylammonium hydroxide (TBAH), or combinations thereof. In one embodiment, the catalyst may include an alkoxide catalyst, such as, but not limited to, sodium methoxide (NaOMe), lithium methoxide (LiOMe), magnesium methoxide, potassium t-butoxide, ethylene glycol monosodium salt, ethylene glycol disodium salt, or combinations thereof. In one embodiment, the catalyst may include tetraisopropyl titanate (TIPT), butyltin tris-2-ethylhexanoate (FASCAT 4102), 1,8-diazabicyclo[5.4.0]undec-7-ene (DBU), zinc acetylacetonate hydrate (Zn(acac)2), zinc acetate (Zn(OAc)2), and manganese(II) acetate (Mn(OAc)2)), or combinations thereof. In certain embodiments, the catalyst may include LiOH, NaOH, KOH, tetraisopropyl titanate (TIPT), butyltin tris-2-ethylhexanoate (FASCAT 4102), ZrCO3, 1,8-diazabicyclo[5.4.0]undec-7-ene (DBU), sodium methoxide (NaOMe), lithium methoxide (LiOMe), and zinc acetylacetonate hydrate (Zn(acac)2), or combinations thereof. In one embodiment, the catalyst may include LiOH, NaOH, KOH, sodium methoxide (NaOMe), and lithium methoxide (LiOMe).In certain embodiments, the catalyst may include Li2CO3, K2CO3, CaCO3, Na2CO3, Cs2CO3, ZrCO3, LiOH, NaOH, KOH, tetrabutylammonium hydroxide (TBAH), sodium methoxide (NaOMe), lithium methoxide (LiOMe), magnesium methoxide (Mg(OMe)2, potassium t-butoxide, ethylene glycol monosodium salt, ethylene glycol disodium salt, tetraisopropyl titanate (TIPT), butyltin tris-2-ethylhexanoate (FASCAT 4102), 1,8-diazabicyclo[5.4.0]undec-7-ene (DBU), zinc acetylacetonate hydrate (Zn(acac)2), zinc acetate (Zn(OAc)2), manganese(II) acetate (Mn(OAc)2), hydrotalcite, zeolite, lithium chloride, or combinations thereof.

[0031] Depolymerization conditions may include temperatures of 120°C to 260°C for 0.5 hours to 10 hours in an agitated reactor, and absolute pressures of 0.013 atmospheres (atm) (0.2 psig) to 10.2 atm (150 psig). One or more reactors may be used to react the polyester with one or more glycols. For example, the reaction mixture may be continuously withdrawn from a first stage and introduced, along with additional glycol, into a second stage maintained under the aforementioned pressure range, with depolymerization continuing to the desired degree of completion. In various embodiments, any type of vessel, reactor, and / or reactor system may be utilized for the depolymerization or glycolysis of the polyester composition. In one embodiment, a continuous stirred tank reactor or vessel, a fixed bed reactor, or a melt extruder may be utilized. In the same or alternative embodiments, the depolymerization or glycolysis of the polyester composition may be a batch or continuous process.

[0032] In various embodiments, the depolymerization process may also result in the formation and / or accumulation of EG. In certain embodiments, it may be desirable to remove EG from the depolymerization reactor, which may facilitate further depolymerization of the polyester composition in certain circumstances. In one embodiment, to facilitate removal of EG from the depolymerization reactor, a solvent may be present during the depolymerization process to facilitate removal of EG. In one or more embodiments, the solvent may be any solvent that can facilitate separation and / or removal of EG from the depolymerization reactor under depolymerization conditions. In certain embodiments, C7-C16 hydrocarbons having a boiling point between 100° C. and 250° C. may be utilized. In certain embodiments, toluene, xylene, isopar C, isopar E, isopar G, isopar H, isopar L, isopar M, or combinations thereof may be utilized.

[0033] Without being bound to a particular theory, it is believed that such solvents can form an azeotrope with EG, thereby lowering the boiling point of EG and facilitating removal of EG from the depolymerization reactor, for example, as gaseous EG. In various embodiments, the solvent may be present in an amount of 30 wt.% to about 200 wt.% based on the weight of the polyester present in the depolymerization reactor. In the same or alternative embodiments, the solvent may be present in an amount of 30 wt.% to about 200 wt.% based on the weight of the one or more glycols present in the depolymerization reactor. In various embodiments, the polyester composition, solvent, EG and / or other components in the depolymerization reactor can be subjected to nitrogen sparging and / or reduced pressure, for example, 0.013 atm (0.2 psig) to about 1 atm (14.7 psig), to facilitate removal of gaseous EG. In one embodiment, the depolymerization conditions may include reduced pressure, for example, from 0.013 atm (0.2 psig) to about 1 atm (14.7 psig), and a temperature ranging from 150° C. to 260° C. to effect removal of EG.

[0034] In various embodiments, EG may be removed from the depolymerization reactor in a solventless process. For example, in certain embodiments, the polyester composition, catalyst, and one or more glycols in the depolymerization reactor may be subjected to nitrogen sparging and / or reduced pressure, e.g., 0.013 atm (0.2 psig) to about 1 atm (14.7 psig), to facilitate removal of gaseous EG. In one embodiment, the depolymerization conditions may include reduced pressure, e.g., 0.013 atm (0.2 psig) to about 1 atm (14.7 psig), and a temperature in the range of 150°C to 260°C.

[0035] After exposure to the depolymerization conditions detailed above, the resulting mixture can be optionally cooled to a temperature below about 150° C., or between about 50° C. and about 150° C. In embodiments, the resulting mixture can be cooled to a desired temperature in the glycolysis reactor or transferred to a different vessel to reduce the temperature. The resulting mixture can include a solid component and a liquid component. In embodiments, the liquid component can include one or more depolymerization products, such as monomers and / or oligomers having a degree of polymerization of 2 to 10, along with one or more glycols, and can further include any additional soluble components from the polyester composition, one or more glycols, catalyst, or combinations thereof. In various embodiments, the solid component can be residual foreign matter and any other insoluble components of the polyester composition and can be considered waste to be disposed of.

[0036] As further discussed below, the liquid component is further subjected to at least a methanolysis process and / or an alcoholysis process to recover one or more dialkyl terephthalates. In various embodiments, the liquid component can be separated from the solid component prior to the methanolysis process. In embodiments, the liquid component may be separated from the solid component using any system. In one embodiment, the liquid component can be separated from the solid component while the resulting mixture is at a temperature of about 50° C. to about 150° C. In such an embodiment, separating the liquid component from the solid component at a temperature of about 150° C. or less, e.g., about 50° C. to about 150° C., can provide a more efficient and / or less resource intensive process than current conventional methods. In the same or alternative embodiment, separating the liquid component from the solid component at a temperature of about 150° C. or less, e.g., about 50° C. to about 150° C., can be beneficial because some impurities may be unstable at higher temperatures, e.g., temperatures above 150° C., thereby adversely affecting the process described herein, product yield, and / or product purity.

[0037] In various embodiments, the separation of the liquid component from the solid component may include a filtration process. In such embodiments, any suitable filtration process capable of withstanding elevated filtration temperatures of about 50° C. to about 150° C. may be utilized. In certain embodiments, the solid components may be removed by centrifugation. In certain embodiments, the solids may be removed by settling or sedimentation. In certain embodiments, the solid components may settle to the bottom of the vessel, and the liquid components may be removed through vessel conduits or valves appropriately positioned within the vessel. In one embodiment, such conduits and / or valves may include filtration devices to minimize inclusion of the solid components in downstream processes.

[0038] Alcoholysis of one or more of the depolymerization products As discussed above, in embodiments, one or more of the depolymerized products produced in the glycolysis process described above may be subjected to an alcoholysis process.

[0039] Generally, in a typical alcoholysis process, a polyester is reacted with an alcohol, such as methanol, to produce a depolymerized mixture that includes oligomers, terephthalate monomers, such as dimethyl terephthalate (DMT), and one or more glycols. In other embodiments, depending on the composition of the polyester, other monomers may also be produced, such as, for example, CHDM, DEG, and dimethyl isophthalate (DMI). In one embodiment, during the alcoholysis process, terephthalate oligomers are reacted with methanol to produce a depolymerized polyester mixture that includes polyester oligomers, DMT, CHDM, and / or EG.

[0040] Some representative examples of the methanolysis of PET are described in U.S. Patent Nos. 3,321,510; 3,776,945; 5,051,528; 5,298,530; 5,414,022; 5,432,203; 5,576,456; and 6,262,294, which are incorporated herein by reference.

[0041] In an embodiment, the alcoholysis process may include exposing the liquid component and / or one or more depolymerized products obtained from the glycolysis process to an alcohol composition under conditions that result in one or more dialkyl terephthalates. As discussed above, in an embodiment, the one or more depolymerized products may be present in the liquid component obtained from the glycolysis process. In various embodiments, as discussed above, before subjecting the one or more depolymerized products and / or liquid component obtained from the glycolysis process to the alcoholysis process, the liquid component may be separated from the resulting mixture of the glycolysis process and / or from the resulting solid component. In certain embodiments, after separating the liquid component from the solid component of the glycolysis process, the liquid component may be directly utilized in the alcoholysis process. In the same or alternative embodiments, after separating the liquid component from the solid component of the glycolysis process, the liquid component is not subjected to further processing, such as distillation and / or other separation processes, before being utilized in the alcoholysis process. Without being bound to any particular theory, it is believed that because the glycolysis process is carried out using a smaller amount of glycol (or a weight ratio of glycol to amount of polyester composition of from 3:1 to 1:9) compared to certain conventional processes, the liquid components resulting from the glycolysis process can be utilized directly in the alcoholysis process without the need for further processing, for example, to concentrate the resulting depolymerization product(s) and / or remove a portion of the glycol.

[0042] The alcohol composition may comprise any suitable alcohol known in the art for use in an alcoholysis process to obtain a particular dialkyl terephthalate. In one embodiment, the alcohol composition may be and / or comprise methanol. In an embodiment, when methanol is utilized as the alcohol composition, it may be the methanolysis product that results in DMT.

[0043] In certain embodiments, the amount of the alcohol composition may be any amount that is in excess by weight relative to the amount or weight of the polyester composition. In certain embodiments, the weight ratio of the amount of the alcohol composition to the amount of the polyester composition may be from about 2:1 to about 10:1. In various embodiments, the weight ratio of the amount of the alcohol composition to the amount of the polyester composition may be from about 2:1 to about 9:1, from about 2:1 to about 8:1, from about 2:1 to about 7:1, from about 2:1 to about 6:1, or from about 2:1 to about 5:1. In embodiments, the amount of the polyester composition refers to the amount or weight of the polyester composition utilized in the glycolysis process described above.

[0044] In embodiments, the alcoholysis reaction may be carried out at a temperature of about 90° C. or less, about 80° C. or less, about 70° C. or less, about 60° C. or less, about 50° C. or less, about 40° C. or less, or about 30° C. or less. In the same or alternative embodiments, the alcoholysis reaction may be carried out at a temperature of about 20° C. to about 90° C., about 20° C. to about 80° C., about 20° C. to about 70° C., about 20° C. to about 60° C., about 20° C. to about 50° C., about 20° C. to about 40° C., or about 20° C. to about 30° C. In certain embodiments, the alcoholysis reaction may be carried out at a temperature of about 25° C. to about 90° C., about 25° C. to about 80° C., about 25° C. to about 70° C., about 25° C. to about 60° C., about 25° C. to about 50° C., about 25° C. to about 40° C., or about 25° C. to about 30° C. In various aspects, without being bound to any particular theory, it is believed that in the methods disclosed herein, the polyester in the polyester composition has already undergone at least a partial depolymerization process, e.g., in the glycolysis step discussed above, so that the methanolysis process can be carried out at the relatively reduced temperatures described above compared to certain other conventional processes. Additionally or alternatively, without being bound to any particular theory, it is believed that the alcoholysis process can be carried out at the reduced temperatures described above because one or more depolymerization products produced in the glycolysis process are separated from waste or insoluble materials prior to the alcoholysis process.

[0045] In embodiments, the alcoholysis process may be carried out in any suitable reactor and / or vessel. In embodiments, the alcoholysis reactor may be in fluid communication with the reactor utilized in the glycolysis process described above. In certain embodiments, the alcoholysis reactor is a different reactor than the vessel used for glycolysis. Alternatively, in various embodiments, the alcoholysis process may be carried out in the same vessel as the glycolysis process and / or filtration process described above. In certain embodiments, the alcoholysis process may be carried out at ambient pressure, e.g., at a pressure of about 1 atm, or from about 1 atm to about 5 atm, or from about 1 atm to about 3 atm, or from about 1 atm to about 2 atm. In various embodiments, the alcoholysis reaction may be carried out at pressures above ambient pressure, e.g., greater than 1 atm, or less than about 5 atm, less than about 3 atm, less than about 2 atm, when the alcoholysis reaction temperature is high relative to the process conditions disclosed herein, e.g., greater than about 50° C., greater than about 60° C., greater than about 70° C., greater than about 80° C., or greater than about 90° C.

[0046] In various embodiments, an alcoholysis catalyst can be utilized in the alcoholysis process. In embodiments, the alcoholysis catalyst may be present in an amount of about 0.1 wt.% to about 20 wt.% based on the weight of the polyester composition, or about 0.1 wt.% to about 10 wt.% based on the weight of the polyester composition, or about 0.1 wt.% to about 5 wt.% based on the weight of the polyester composition, or about 0.1 wt.% to about 2 wt.% based on the weight of the polyester composition, or about 0.1 wt.% to about 1 wt.% based on the weight of the polyester composition, or about 0.1 wt.% to about 0.5 wt.% based on the weight of the polyester composition. In such embodiments, the amount of polyester composition refers to the amount or weight of the polyester composition utilized in the above-mentioned alcoholysis process. In various embodiments, the amount of alcoholysis catalyst disclosed in this paragraph refers to the amount of alcoholysis catalyst present in the alcoholysis reaction. In various embodiments, the amount of alcoholysis catalyst disclosed in this paragraph refers to the amount of alcoholysis catalyst added to one or more depolymerization products and one or more alcohols to promote the alcoholysis reaction. In certain embodiments, a reduced or smaller amount of alcoholysis catalyst can be added to one or more depolymerization products and one or more alcohols to promote the alcoholysis reaction, for example, about 0.1 wt.% to about 10 wt.% by weight of the polyester composition, or about 0.1 wt.% to about 5 wt.% by weight of the polyester composition, or about 0.1 wt.% to about 2 wt.% by weight of the polyester composition, or about 0.1 wt.% to about 1 wt.% by weight of the polyester composition, or about 0.1 wt.% to about 0.5 wt.% by weight of the polyester composition. In embodiments, such a smaller amount of alcoholysis catalyst can be added, at least in part, because the alcoholysis catalyst is already present in one or more depolymerization products and / or one or more alcohols. In such embodiments, as discussed below, the alcohol and / or glycol may be recycled and reused in subsequent glycolysis and alcoholysis processes disclosed herein, which may include at least a portion of the alcoholysis catalyst from the preceding alcoholysis and / or glycolysis process.

[0047] In various embodiments, the alcoholysis catalyst may include carbonate catalysts, such as, but not limited to, K2CO3, Na2CO3, Li2CO3, Cs2CO3; hydroxide catalysts, such as, but not limited to, KOH, LiOH, NaOH; alkoxide catalysts, such as, but not limited to, NaOMe, Mg(OMe)2, KOMe, KOt-Bu, ethylene glycol monosodium salt, ethylene glycol disodium salt, or combinations thereof. In certain embodiments, the alcoholysis catalyst may include KOH, NaOH, LiOH, or combinations thereof. In certain embodiments, the alcoholysis catalyst may include NaOMe, KOMe, Mg(OMe)2, KOt-Bu, ethylene glycol monosodium salt, ethylene glycol disodium salt, or combinations thereof. In various embodiments, the alcoholysis catalyst may be in solid form, in solution form in water, methanol, or ethylene glycol, or combinations thereof. In certain embodiments, an alcoholysis catalyst may be added to the one or more depolymerization products and the alcohol composition once the alcohol composition and the one or more depolymerization products reach the desired reaction temperature or temperature range disclosed above.

[0048] The one or more depolymerization products may be exposed to the alcohol composition and optionally the alcoholysis catalyst under the above-mentioned temperature and pressure conditions for a time to achieve a desired yield of the resulting dialkyl terephthalate. In certain embodiments, the one or more depolymerization products may be exposed to the alcohol composition and optionally the alcoholysis catalyst under the above-mentioned temperature and pressure conditions for a time of about 5 minutes to about 5 hours, or about 5 minutes to about 2 hours, or about 5 minutes to about 1 hour, or about 5 minutes to about 30 minutes, or about 5 minutes to about 15 minutes, or about 5 minutes to about 10 minutes.

[0049] In an embodiment, the alcoholysis process results in a mixture comprising one or more dialkyl terephthalates. In various embodiments, the alcoholysis process results in a mixture in which the dialkyl terephthalates are insoluble and / or solid components. In an embodiment, the liquid component of the mixture may comprise one or more glycols, alcohol compositions, or combinations thereof. In an embodiment, the glycols may be glycols utilized in the glycolysis process that were present with the one or more depolymerization products at the start of the alcoholysis process. In various embodiments, the dialkyl terephthalates may be isolated from the mixture using any known separation technique, such as filtration, centrifugation, precipitation, sedimentation, or a combination of one or more separation techniques. In an embodiment, the filtration may include washing the solid components with additional alcohol compositions or other solvents. The resulting liquid components may include filtrates and washes. The resulting solid component may comprise about 90 wt.% or more of a dialkyl terephthalate, e.g., DMT, about 93 wt.% or more of a dialkyl terephthalate, e.g., DMT, or about 95 wt.% or more of a dialkyl terephthalate, e.g., DMT, based on the weight of the solid component. In the same or alternative embodiments, the dialkyl terephthalate, e.g., DMT, in the resulting solid component may be about 90% or more pure, about 93% or more pure, or about 95% or more pure. In various embodiments, the solid component may also comprise dimethyl isophthalate (DMI). In such embodiments, the DMI may be present in an amount of about 1000 ppm or less, or about 500 ppm or less, or about 1 ppm to about 1000 ppm, or about 1 ppm to about 500 ppm. In one or more embodiments, the solid component may also comprise bisphenol A (BPA). In such embodiments, BPA may be present in an amount of about 1000 ppm or less, or about 500 ppm or less, or from about 1 ppm to about 1000 ppm, or from about 1 ppm to about 500 ppm.

[0050] The processes described herein, e.g., glycolysis and / or alcoholysis processes, are substantially milder than certain conventional processes, e.g., high temperature one-step glycolysis or methanolysis processes. For example, certain conventional one-step processes may utilize a glycolysis process at a temperature of 240° C. or higher in the presence of a Lewis acid catalyst, e.g., Zn(OAc) 2 or KOAc. Such harsh conditions may result in reduced EG yield from depolymerization due to EG being converted in various side reactions to various impurity compounds, including, but not limited to, diethylene glycol (DEG), triethylene glycol (TEG), acetaldehyde, 1,1-dimethoxyethane, 1,2-dimethoxyethane, dioxane, 2-methoxyethanol, 1-methoxyethanol, and dimethyl ether. In an embodiment, the processes described herein are substantially milder than such conventional processes, and further result in less EG yield loss, e.g., due to fewer side reactions that convert EG to various impurities. In one embodiment, the process described herein results in a yield loss of about 5% or less of EG, a yield loss of about 2% or less of EG, or a yield loss of about 1% or less of EG, or a yield loss of about 0.5% or less of EG. In such an embodiment, the yield loss of EG is the percentage of EG formed into impurities, e.g., DEG, relative to the combined amount of EG from the polyester composition feed and EG added in the glycolysis process. In the same or alternative embodiment, the process described herein produces minimal glycol impurities. For example, in one aspect, the processes described herein can result in a net generation of about 5 wt.% or less DEG, about 2 wt.% or less DEG, or about 1 wt.% or less DEG, or about 0.5 wt.% or less DEG, or about 0.01 wt.% to about 5 wt.% DEG, about 0.01 wt.% to about 2 wt.% DEG, or about 0.01 wt.% to about 1 wt.% DEG, or about 0.01 wt.% to about 0.5 wt.% DEG, or about 0.01 wt.% to about 0.2 wt.% DEG when EG is used as one or more glycols in the glycolysis process.In an embodiment, the processes described herein can result in a net generation of about 5 wt.% or less DEG and / or other impurities, about 2 wt.% or less DEG and / or other impurities, or about 1 wt.% or less DEG and / or other impurities, or about 0.5 wt.% or less DEG and / or other impurities, or about 0.01 wt.% to about 5 wt.% DEG and / or other impurities, about 0.01 wt.% to about 2 wt.% DEG and / or other impurities, or about 0.01 wt.% to about 1 wt.% DEG and / or other impurities, or about 0.01 wt.% to about 0.5 wt.% DEG and / or other impurities, or about 0.01 wt.% to about 0.2 wt.% DEG and / or other impurities when EG is used as one or more glycols in the glycolysis process. In an embodiment, the net generation of DEG (or other impurities) is the weight percent of the amount of DEG or other impurities present relative to the amount of DEG or other impurities present in the polyester composition feed. In an embodiment, the DEG produced may be produced in a glycolysis process described herein and / or an alcoholysis process described herein. In certain embodiments, when EG is used as one or more glycols in the glycolysis process, EG such as DEG and / or any glycol impurities may be present in the liquid component resulting from the alcoholysis step. In certain embodiments, the utilization of a Lewis base catalyst, e.g., a hydroxide-based or carbonate-based catalyst, in the glycolysis process may also facilitate or contribute to the reduction of EG decomposition and / or the reduction of glycol impurities.

[0051] Recycling of glycol and alcohol compositions As discussed above, in various embodiments, the glycol utilized in the glycolysis process can be reused in a subsequent process sequence to recover one or more dialkyl terephthalates disclosed herein. In embodiments, at a high level, the liquid component obtained from the alcoholysis process can be processed for reuse, for example, for reuse in a subsequent glycolysis sequence of a subsequent polyester composition to recover one or more dialkyl terephthalates. In the same or alternative embodiments, methanol can be recovered from the liquid component obtained from the alcoholysis process, for example, reused in a subsequent alcoholysis process. In such embodiments, methanol can be recovered by exposing the liquid component to distillation conditions.

[0052] In embodiments, as discussed above, the liquid component resulting from the alcoholysis process may include glycols used in the glycolysis process, alcohol compositions, and glycols generated in the glycolysis process, e.g., EG, DEG, and / or CHDM. In various embodiments, the liquid component may be subjected to a separation process, e.g., to remove or separate at least a portion of the alcohol composition, e.g., methanol, or a mixture of methanol and ethylene glycol. In certain embodiments, the liquid component may be exposed to distillation or short path distillation to remove at least a portion of the alcohol composition. In exemplary non-limiting embodiments, the distillation conditions may include exposing the liquid component to a temperature of about 260° C. or less, about 220° C. or less, about 200° C. or less, about 180° C. or less, about 160° C. or less, about 150° C. or less, about 130° C. or less, about 60° C. or more, about 70° C. or more, about 60° C. to about 220° C., about 70° C. to about 220° C., about 60° C. to about 180° C., or about 60° C. to about 160° C. In the same or alternative embodiments, the distillation conditions may include a pressure of from about 1 Torr (133.3 Pa) to about 800 Torr (106,657 Pa), or from about 30 Torr (3999 Pa) to about 500 Torr (66,661 Pa). In embodiments, the liquid component may be exposed to the distillation conditions until all or a substantial portion of the alcohol composition is removed from the liquid component, e.g., vaporized. In certain embodiments, at least a portion of the alcohol composition, if present with the recycle glycol, may be removed during a subsequent glycolysis process, e.g., removed or vaporized by the glycolysis conditions. In certain embodiments, the alcohol, e.g., methanol, recovered from the liquid component may be returned to the alcoholysis reactor vessel for use in a subsequent alcoholysis process.

[0053] In embodiments, distillation of the liquid components may be carried out in any vessel or distillation system suitable for use in the methods and systems described herein. In one embodiment, the distillation vessel can be in fluid communication with the alcoholysis reaction vessel and / or any component of the filtration process utilized subsequent to alcoholysis, for example, to isolate the dialkyl terephthalate solid or insoluble components. In the same or alternative embodiments, the distillation vessel can be in fluid communication with the glycolysis vessel.

[0054] In various embodiments, distillation of the liquid component can vaporize the alcohol composition and leave a pot residue. In embodiments, the pot residue includes glycols and any other heavies present in the liquid component, such as non-vaporizable compounds. In embodiments, the glycols in the pot residue can be referred to as recycled glycols, and / or the glycols from the non-vaporizable portion of the continuous distillation process using the distillation conditions described herein can be referred to as recycled glycols. In an embodiment, the recycled glycols can include ethylene glycol (EG), diethylene glycol (DEG), triethylene glycol (TEG), 1,4-cyclohexanedimethanol (CHDM), poly(ethylene glycol) (PEG), neopentyl glycol (NPG), propanediol (PDO), butanediol (BDO), 2-methyl-2,4-pentanediol (MP diol), poly(tetramethylene ether) glycol (PTMG), or combinations thereof.

[0055] In an embodiment, as discussed above, the recycled glycol may be utilized in a subsequent process sequence described herein to recover one or more dialkyl terephthalates from the polyester composition. Furthermore, in an embodiment, the recycled glycol may be recycled again using the process described herein after this subsequent dialkyl terephthalate recovery sequence. In an embodiment, the recycled glycol may be recovered and reused at least two times, at least three times, at least four times, or at least five times. In certain embodiments, when the recycled glycol is used in a subsequent dialkyl terephthalate recovery sequence, the addition of a catalyst in the subsequent glycolysis step may be omitted since the recycled glycol may contain a used catalyst.

[0056] In embodiments, it has been unexpectedly discovered that when recycled glycol is recovered and reused, the resulting recovered dialkyl terephthalate exhibits a purity comparable to that of dialkyl terephthalate recovered using glycol that was not recovered and reused. In embodiments, this comparable purity of dialkyl terephthalate exists after reusing recycled glycol at least two, at least three, at least four, or at least five times, resulting in the recovery of dialkyl terephthalate having a purity of at least about 90%, at least about 93%, or at least about 95%.

[0057] Exemplary System FIG. 1 illustrates generally one exemplary system and / or method for recovering one or more dialkyl terephthalates from a polyester composition. System 100 includes a source 110 of a polyester composition, such as the polyester composition described above. In one exemplary embodiment, the polyester composition can undergo an optional pretreatment process, as discussed in detail above. In such an embodiment, this optional pretreatment can occur prior to exposing the polyester composition to depolymerization conditions in vessel 120. Vessel 120 represents a glycolysis vessel, in which the polyester composition is received and exposed to one or more glycols under depolymerization conditions, as discussed in detail above. In an embodiment, vessel 120 can be in fluid communication with source 110. In various embodiments, the polyester composition is converted to one or more depolymerization products after being exposed to depolymerization conditions in vessel 120, as discussed in detail above. In various embodiments, as discussed above, the one or more depolymerization products may include monomers and / or oligomers having a degree of polymerization of 2-10, 2-8, 2-6, or 2-4. In embodiments, the one or more depolymerization products are present in a mixture including a liquid component and a solid component, with the one or more depolymerization products in the liquid component. As discussed above, the depolymerization conditions can result in the production of EG. In certain embodiments, as discussed in detail above, EG generated in vessel 120 from the depolymerization process can be removed from vessel 120. In embodiments, as discussed above, the mixture is exposed to a solid-liquid separation device 130, e.g., a filtration system, where the liquid component including the one or more depolymerization products is separated from the solid component. In various embodiments, as discussed herein, the solid-liquid separation device 130 can be in fluid communication with vessel 120 and / or vessel 140. In the embodiment shown in FIG. 1, the one or more depolymerization products and / or the liquid component can be exposed to alcoholysis conditions in vessel 140. In an embodiment, one or more of the depolymerization products and / or liquid components may be utilized directly in the alcoholysis process.In such embodiments, the one or more depolymerization products and / or liquid components may not be subjected to any further processing, e.g., distillation and / or other separation processes, before being utilized in the alcoholysis process. Alcohololysis conditions are discussed in detail above. In embodiments, as discussed above, alcoholysis of one or more depolymerization products and / or liquid components may result in a mixture including an insoluble or solid component including dialkyl terephthalate, and a liquid component including alcohol compositions, glycols, and potentially other soluble components as described herein. As discussed above, the resulting alcoholysis reaction mixture may be exposed to a solid-liquid separation device 150, e.g., a filtration system, to separate the solid component including the recovered dialkyl terephthalate 160. In embodiments, the solid-liquid separation device 150 may be in fluid communication with the vessel 140. In various embodiments, the liquid component resulting from the solid-liquid separation in the solid-liquid separation device 150 may include one or more alcohols, one or more glycols, or both. In such embodiments, the liquid component may be subjected to one or more distillation or other separation processes in system 170. In system 170, one or more alcohols may be separated from the liquid component as discussed above and optionally returned to vessel 140 for use in a subsequent alcoholysis process. In the same or alternative embodiments, in system 170, one or more glycols may be recovered as discussed above and returned to vessel 120 for a subsequent depolymerization process. Additionally, in various embodiments, system 170 may selectively remove EG from the liquid component for purposes other than storage or return to vessel 120. System 170 may be any type of separation or distillation system suitable for selectively recovering one or more alcohols and / or one or more glycols from a liquid component. In certain embodiments, the methods described herein relating to system 100 may be implemented as continuous, batch, or semi-continuous methods. It is understood that system 100 is merely an example system and other configurations of system components are contemplated by the disclosure herein.For example, one or more components of system 100 may not be physically separate or distinct from one or more other components of system 100. It is further understood that system 100 is depicted only diagrammatically to highlight aspects of the methods disclosed herein.

[0058] Use of Recovered Dialkyl Terephthalates to Form Polyesters or Other Products As discussed above, the methods disclosed herein can result in high purity dialkyl terephthalates such as DMT. For example, in certain embodiments, the recovered DMT may be utilized to form one or more polyesters, including, but not limited to, PET and TMCD-containing polyesters. In certain embodiments, the polyesters formed using the recovered DMT may be referred to as recycled polyesters. In various embodiments, the products formed using the recovered DMT may be indistinguishable from similar products formed from virgin DMT. In such embodiments, any suitable process for forming PET and TMCD-containing polyesters may be utilized, since the DMT is of sufficient purity.

[0059] In the same or alternative embodiments, the recovered DMT may be utilized to form CHDM. In various embodiments, the CHDM formed using the recovered DMT may be indistinguishable from CHDM formed from virgin DMT due to the high purity of the recovered DMT. In such embodiments, the CHDM may be formed from the recovered DMT using any suitable process.

[0060] In various embodiments, the recovered DMT may be utilized to form one or more plasticizers. In certain embodiments, the plasticizers formed using the recovered DMT may include dibutyl terephthalate (DBT) and / or dioctyl terephthalate (DOTP). In various embodiments, the DBT and / or DOTP formed using the recovered DMT may be indistinguishable from the DBT and / or DOTP, respectively, formed from virgin DMT due to the high purity of the recovered DMT. In such embodiments, the DBT and / or DOTP may be formed from the recovered DMT using any suitable process.

[0061] The present disclosure can be further illustrated by the following examples of its aspects, although it will be understood that these examples are included for illustrative purposes only and are not intended to limit the scope of the disclosure unless specifically indicated otherwise. EXAMPLES

[0062] material FDST-5 contains 100 mol % TPA, 93.0 mol % EG, 4.1 mol % CHDM, and 2.9 mol % DEG and is available from Eastman. IV: 0.751 dL / g.

[0063] FDST-3 contains 97.7 mol % TPA, 2.3 mol % IPA, 96.7 mol % EG, and 3.3 mol % DEG and is available from PolyQuest. IV: 0.563 dL / g.

[0064] Ethylene glycol (EG), diethylene glycol (DEG), triethylene glycol (TEG), poly(ethylene glycol) (PEG200), 1,4-cyclohexanedimethanol (CHDM), methanol, potassium carbonate, 50% aqueous sodium hydroxide, toluene and xylene are available from Aldrich. Isoparaffinic hydrocarbons (isopar™), including Isopar C, Isopar E, Isopar G, Isopar H, Isopar L and Isopar M, are available from ExxonMobil. All chemicals and reagents were used as received unless otherwise noted.

[0065] Analytical procedures Combustion Ion Chromatography (CIC) Analysis. CIC analysis was performed using a 930 Metrohm Combustion Ion Chromatography system. Samples were first combusted at 1000 °C in a combustion module. The resulting gases evolved during combustion were dissolved in an absorption solution in a Metrohm 920 absorption module. The absorption solution was pre-concentrated and analyzed by ion chromatography.

[0066] Gas Chromatography (GC) Analysis. GC analysis was performed on an Agilent Model 7890B Gas Chromatograph equipped with a 7693A autosampler and two G4513A towers. The GC was equipped with two columns, a 60m x 0.32mm x 1.0 micron DB-1701™ (J&W123-0763) and a 60m x 0.32 x 1 micron DB-1™ (J&W123-1063), and samples were injected simultaneously onto both columns. A common oven temperature program was used and sample components were detected by flame ionization detection (FID). A five-point calibration was performed for components of interest. The gas chromatograph was interfaced to an EZChrom Elite Chromatography Data System.

[0067] Methanolysis product samples were prepared by adding a known volume of pyridine-based internal standard solution to a known mass of sample, followed by derivatization with N,O-bis(trimethylsilyl)trifluoroacetamide (BSTFA).

[0068] The % BHET GC yield was calculated as follows: (wt% BHET in crude by GC) / (theoretical wt% BHET based on PET / EG input) * 100% The % BHDET GC yield was calculated as follows: (wt% BHDET in crude by GC) / (theoretical wt% BHDET based on PET / DEG input). * 100% The % DMT GC yield was calculated as follows: (weight of final DMT) / (weight of theoretical DMT). * 100%.

[0069] DMT GC purity % was calculated as follows: (wt.% DMT in final product by GC) / (total wt.% by GC). * 100%. Major impurities as shown by GC include MeOH, water, and EG. DMT purity in almost all examples is greater than 99% excluding MeOH, water, and EG.

[0070] Gel Permeation Chromatography (GPC). Size Exclusion Chromatography GPC analysis was performed on an Agilent 1100 series GPC / SEC analytical system equipped with a UV-Vis detector. The column set used was a Polymer Laboratories 5 μm Plgel with guard, mixed C and oligopore. The eluent consisted of 95% methylene chloride and 5% hexafluoroisopropanol with tetraethylammonium nitrate (1 gram / 2 liters of solvent). The tests were performed at ambient temperature with a flow rate of 1.0 mL / min. The instrument was calibrated with linear PET oligomer standards.

[0071] Samples were prepared by dissolving 10 mg of sample in 10 mL of methylene chloride / hexafluoroisopropanol (70 / 30). 10 μL of toluene was added as a flow rate marker. The injection volume was 10 μL.

[0072] Liquid chromatography (LC). LC analysis of oligomers was performed on an HP 1100 series liquid chromatograph equipped with a diode array detector (DAD) with a range of 190-900 nm. The system was equipped with a Zorbax Poroshell 120 EC-C18 (4.6 × 50 mm, 2.7 μm) column at 40 °C. The flow rate was 1.0 mL / min. The mobile phase was water (25 nM ammonium acetate) (A) and acetonitrile (B). The elution gradient was as follows: 0 min, 95% A / 5% B; 2 min, 95% A / 5% B; 18 min, 0% A / 100% B; 28 min, 0% A / 100% B; 28.1 min, 95% A / 5% B; 33 min, 95% A / 5% B. Sample solutions were prepared by dissolving approximately 4 mg of sample in 1 mL of DMF / DMSO (50 / 50). The injection volume was 2 μL. Oligomer distributions were reported as area %.

[0073] Measurement of Intrinsic Viscosity. The intrinsic viscosity (IV) of certain polymeric materials useful herein is determined according to the ASTM D2857-70 procedure on a LabGlass Wagner Viscometer with a 1 / 2 mL capillary valve using a polymer concentration of about 0.5 wt % in 60 / 40 phenol / tetrachloroethane by weight. The procedure is performed by heating the polymer / solvent system at 120° C. for 15 minutes, cooling the solution to 25° C., and measuring the flow time at 25° C. The IV is calculated from the following formula:

[0074]

number

[0075] (wherein η is the intrinsic viscosity at 25° C. at a polymer concentration of 0.5 g / 100 mL of solvent, tS is the sample flow time, t0 is the solvent blank flow time, and C is the polymer concentration in grams per 100 mL of solvent). The unit of intrinsic viscosity in this application is deciliter / gram.

[0076] In the following examples, viscosity was measured in tetrachloroethane / phenol (50 / 50, by weight) at 30° C. and calculated according to the following formula:

[0077]

number

[0078] (In the formula, η sp is the specific viscosity and C is the concentration).

[0079] Example 1: Glycolysis catalyst In this Example 1, FDST-3 (3 g) and DEG (or EG or PEG200) (7 g) and catalyst were charged into a 20 mL vial equipped with a magnetic stir bar. The resulting mixture was heated in a heating block at a set temperature and stirred for 4 hours. The reaction aliquots were analyzed by GC analysis. Different catalysts were utilized at different temperatures for PET glycolysis (Table 1). Bis 2-(2-hydroxyethoxy)ethyl) terephthalate (BHDET) yield, e.g., BHDET wt.%, was determined using GC analysis. BHDET wt.% is relative to the total weight of PET in the glycolysis reaction. Bis 2-hydroxyethyl terephthalate (BHET) yield, e.g., BHET wt.%, was determined using GC analysis. BHET wt.% is relative to the total weight of PET in the glycolysis reaction. The results are shown in Table 1. As can be seen in Table 1, many catalysts provided high (e.g., 50% or higher) BHDET (or BHET) yields at a wide variety of glycolysis temperatures.

[0080] In this example, DEG performed slightly better than EG in terms of yield of monomer glycolysis product at both 150° C. and 170° C. PEG-200 also performed well at both 30% PET / glycol and 50% PET / glycol, however the crude products were not analyzed for monomer % due to lack of a test method.

[0081] [Table 1]

[0082] Examples 2A-2C: Examples of glycolysis / methanolysis reactions using various glycols. Example 2A - PEG-200 A three-neck 500 mL round bottom flask was equipped with a mechanical stirrer, reflux condenser and thermocouple. FDST-5 pellets (50.04 g), potassium carbonate (0.50 g) and poly(ethylene glycol) (100.0 g) were charged. The resulting mixture was heated to 200° C. under nitrogen atmosphere and held at 200° C. until the PET pellets were dissolved. The heating mantle was removed and the solution was cooled to ambient temperature. The mixture was charged with methanol (200.35 g). The resulting mixture was heated to 50° C. and then 50% NaOH solution (0.208 mL) was added dropwise. Stirring was continued for 15 min. The heating mantle was removed and the flask was cooled to room temperature for 2 h. The product was collected by filtration / washing and dried in air. The product was obtained as a white crystalline solid (46.03 g, 91% yield, 97% GC purity).

[0083] Example 2B - TEG / EG 1 / 1 (wt.) A three-necked, 1-liter round-bottom flask was equipped with a mechanical stirrer, reflux condenser, and thermocouple. FDST-5 pellets (75.11 g), potassium carbonate (0.78 g), ethylene glycol (38.06 g), and triethylene glycol (37.82 g) were charged. The resulting mixture was heated to 195° C. under nitrogen and held at 195° C. until the PET pellets were dissolved. The heating mantle was removed and the solution was cooled to ambient temperature. Methanol (300.40 g) was charged to the mixture. The resulting mixture was heated to reflux and then 50% NaOH solution (0.312 mL) was added dropwise. Stirring was continued for 15 minutes. The heating mantle was removed and the flask was allowed to cool to room temperature for 2 hours. The product was collected by filtration / washing and dried in air. The DMT product was obtained as a white crystalline solid (67.76 g, 89% yield, 98% GC purity).

[0084] Example 2C - CHDM / EG 1 / 1 (wt.) A three-necked, 1-liter round-bottom flask was equipped with a mechanical stirrer, reflux condenser, and thermocouple. FDST-5 pellets (75.93 g), potassium carbonate (0.74 g), ethylene glycol (37.65 g), and 1,4-cyclohexanedimethanol (37.53 g) were charged. The resulting mixture was heated to 195° C. under nitrogen and held at 195° C. until the PET pellets were dissolved. The heating mantle was removed and the solution was cooled to ambient temperature. Methanol (300.72 g) was charged to the mixture. The resulting mixture was heated to reflux and then 50% NaOH solution (0.312 mL) was added dropwise. Stirring was continued for 15 minutes. The heating mantle was removed and the flask was cooled to room temperature for 2 hours. The product was collected by filtration / washing and dried in air. The DMT product was obtained as a white crystalline solid (68.61 g, 91% yield, 98% GC purity).

[0085] Examples 3A-3D - DEG Glycolysis with EG Overhead Removal Standard reaction procedure. Place a 3-neck 1-liter RB flask in a heating mantle equipped with a mechanical stirrer, Dean-Stark trap or decanter, condenser, calorimeter, and nitrogen blanketing. Charge the RB with the PET sample, DEG, EG if required, and solvent. Fill the decanter with xylene if using xylene, or leave the trap empty if using only DEG. Turn on N2 flow and stirring. Heat to set temperature. Hold until PET dissolves (1-8 hours). EG solvent collects in the decanter and monitors its rate of formation over time and removes as needed. If using only DEG (no xylene), run the reaction under vacuum ~150 torr (range 0-400 torr) and sparge with subsurface N2 as needed. Once the reaction is complete, turn off the heat and cool to room temperature. Filter the product if required and analyze the liquid by GC, GPC, and viscosity (optional). The solid residue from the filtration is washed with methanol, dried and analyzed by uniquant and CHN analysis.

[0086] Standard Solvent Assisted Glycolysis Procedure. A 3-neck 1-liter RB flask was placed in a heating mantle equipped with a mechanical stirrer, decanter, condenser, thermocouple and nitrogen blanketing. The RB was charged with the PET sample, DEG and solvent. The decanter was filled with entrained solvent. Turn on N2 flow and agitation. Heat to set temperature. Hold until PET is dissolved (1-8 hours). EG solvent is collected as the bottom phase in the decanter. Monitor the rate of rEG collection over time and remove as needed. Turn off heat when reaction is complete and cool to <60°C. Filter the product and analyze the liquid by GC, GPC and viscosity (optional). The solid residue from the filtration is washed with methanol, dried and analyzed by uniquant and CHN analysis.

[0087] Standard Solvent-Free Glycolysis Procedure. A three-neck 1-liter RB flask was placed in a heating mantle equipped with a mechanical stirrer, Oldershaw column, reflux head or simple distillation head, condenser, thermocouple, vacuum controller, and nitrogen atmosphere generator. The RB was charged with the PET sample, DEG, and EG if desired. Turn on N2 flow and stirring. Heat to set temperature. Hold until PET is dissolved (1-8 hours). Set the vacuum controller to the desired pressure. If using a reflux head, set the reflux percentage using the magnet power timer and set the takeoff temperature. Once the desired vapor temperature is reached, rEG will begin to collect in the distillate collection flask. The reaction can be sparged with subsurface N2 if necessary to drive off EG overhead. Once the reaction is complete, turn off the heat and cool to room temperature. Filter the product if desired and analyze the liquid by GC, GPC, and viscosity (optional). Wash the solid residue from the filtration with methanol, dry, and analyze by uniquant and CHN analysis.

[0088] Example 3A - Solvent-free DEG Glycolysis with Overhead EG Removal In this example, PET was subjected to glycolysis conditions similar to the standard solvent-free glycolysis procedure described above. Specifically, a 3-neck 1-liter RB flask was placed in a heating mantle equipped with a mechanical stirrer, Oldershaw column, simple distillation head, condenser, thermocouple, vacuum controller, subsurface nitrogen line, and nitrogen blanket generator. The RB was charged with 114.2 g of PET, 145.7 g of DEG, and 1.14 g of K2CO3. Nitrogen flow and stirring were turned on. The flask was heated to a setpoint of 200° C., controlled by a thermocouple in the solution. The vacuum controller was set to 400 torr (0.53 atm). Nitrogen was sparged subsurface throughout the solution. The maximum temperature of the solution reached was 200.6° C., and the PET was all visibly dissolved in approximately 1 hour at temperature. 42.62 g of distillate was collected and GC analysis showed it to be about 57.6% EG with the remainder being DEG. The DEG oligomers were cooled and filtered through a Buchner funnel. A 15 g sample of the DEG oligomers was subjected to low temperature methanolysis at 65° C. using 40 mg of NaOH catalyst and 13.5 g of methanol, cooling to 25° C. The yield of DMT was 96.3%.

[0089] Example 3B - Solvent-free DEG Glycolysis with Overhead EG Removal In this example, PET was subjected to glycolysis conditions similar to the standard solvent-free glycolysis procedure described above. Specifically, a three-necked 1-liter RB flask was placed in a heating mantle equipped with a mechanical stirrer, Oldershaw column, reflux head, condenser, thermocouple, vacuum controller, and nitrogen atmosphere generator. The RB was charged with 75 g PET, 95.7 g DEG, 5 g EG (to increase reflux in the column), and 0.75 g K2CO3. The nitrogen flow and stirring were turned on. The flask was heated to a setpoint of 200°C controlled by a thermocouple in the solution. The vacuum controller was set to 150 torr (0.2 atm). The vapor takeoff head, controlled by an electromagnet, was set to 30-50% takeoff. The maximum temperature of the solution reached was 194.5°C, and the PET was all visibly dissolved in approximately 1 hour at temperature. 13.875 g of EG distillate was collected. The DEG oligomers were cooled and filtered through a Buchner funnel. A 15 g sample of the DEG oligomers was subjected to low temperature methanolysis at 65° C. using 40 mg of NaOH catalyst and 16.1 g of methanol, cooling to 25° C. The yield of DMT was 78%.

[0090] Example 3C - Solvent-free PET Glycolysis with DEG and EG Removal Nitrogen sparging and vacuum pressure were tested for EG removal in a glycolysis reaction with PET and DEG as listed in the table below. The glycolysis reaction utilized for the data in Table 2 was similar to that utilized in Example 2. The results are shown in Table 2. As shown in Table 2, the PET was completely reacted and dissolved within 1.5 hours. Up to 86% of the EG was recovered in the glycolysis process.

[0091] [Table 2]

[0092] Example 3D - Solvent-assisted PET glycolysis with DEG and EG removal PET glycolysis was carried out with DEG in the presence of various entrained solvents in a manner similar to that described above for the glycolysis step of the standard solvent-assisted glycolysis procedure. Additional information regarding the specific conditions can be found in Table 3 below. As can be seen in Table 3 below, two entrained solvents were tested in the removal of EG during PET glycolysis. The experiments were carried out at 150 and 175°C in the presence of K2CO3 and NaOMe. As shown in Table 3, EG was recovered in good yields. However, a significant amount of insoluble PET was recovered at the end of the reaction.

[0093] [Table 3]

[0094] Example 4 – Low temperature methanolysis of glycolysis intermediates In this example, some of the glycolysis intermediates produced in the above examples were subjected to a methanolysis reaction. In this example, the glycolysis intermediates (DEG oligomers) were subjected to methanolysis conditions, which included exposing the DEG oligomers to methanol and an alcoholysis catalyst at 65° C. for 15 minutes, cooling to 25° C. over 30 minutes, and holding at 25° C. for 30 minutes. The glycolysis intermediates utilized in this example were produced in the above examples, as referenced in Table 4 below.

[0095] [Table 4]

[0096] Example 4 – Two-Step Glycolysis and Methanolysis Process In this example, PET was subjected to a glycolysis and methanolysis process, which includes exposing PET to one or more glycols in the presence of a glycolysis catalyst (1 wt.% K2CO3) at 195°C and subjecting the glycolysis reaction product to methanolysis in the presence of 1.5 mol.% NaOH at 50°C (methanol is present in an amount of 4 parts methanol to 1 part PET). The specific reactions and processes are described in the examples above for the referenced reactions shown in Table 5. As can be seen in Table 5, excellent DMT yields and DMT quality were obtained in all experiments.

[0097] [Table 5]

[0098] The present disclosure may also be described according to the following numbered sections: Item 1. A method for recovering one or more dialkyl terephthalates from a polyester composition, comprising the steps of: exposing the polyester composition to a first glycol composition and one or more glycolysis catalysts in a reaction vessel under depolymerization conditions to provide a first mixture, the first mixture comprising one or more depolymerization products; ethylene glycol (EG); and one or more insoluble components, the depolymerization conditions comprising a temperature in the range of about 120° C. to about 260° C., a pressure in the range of about 0.013 atm (0.2 psig) to about 10.2 atm (150 psig), and a time period in the range of about 0.5 hours to about 10 hours, the first glycol composition being selected from the group consisting of diethylene glycol (DEG), triethylene glycol (TEG), 1,4-cyclohexanedimethanol (CHDM), poly(ethylene glycol) (PEG), neopentyl glycol (NPG), propanediol (PDO), butanediol (BDO), 2-methyl-2,4-pentanediol (DMSO), 2-methyl-2,4-pentanediol ( ... 1. A method for producing a polyester composition comprising the steps of: including a first glycol composition, a poly(tetramethylene ether) glycol (MP diol), a poly(tetramethylene ether) glycol (PTMG), or a combination thereof; removing at least a portion of the EG from the reaction vessel while exposing the polyester composition to a first glycol composition and one or more glycolysis catalysts in the reaction vessel; exposing at least a portion of a first liquid component of the first mixture to one or more alcohols and an alcoholysis catalyst under alcoholysis conditions to provide a second mixture, the second mixture including a solid component comprising one or more dialkyl terephthalates and a second liquid component, the alcoholysis conditions including a temperature in the range of about 25° C. to about 90° C., a pressure in the range of about 1 atm (14.7 psig) to about 2 atm (30 psig), and a time period in the range of about 0.5 hours to about 5 hours; and separating at least a portion of the one or more dialkyl terephthalates from the second mixture by solid-liquid separation.

[0099] Item 2. The method of item 1, wherein a solvent is present during exposure of the polyester composition to the first glycol composition and the one or more glycolysis catalysts in the reaction vessel. Item 3. The method according to Item 2, wherein the solvent is a C7 to C16 hydrocarbon having a boiling point of 100° C. to 250° C.

[0100] Item 4. The method according to any one of Items 1 to 3, wherein the depolymerization conditions include a pressure of 0.013 atm (0.2 psig) to about 1 atm (14.7 psig). Item 5. The method according to any one of items 1 to 4, wherein the weight ratio of the first glycol composition to the polyester composition is in the range of about 1:9 to about 9:1 during the exposure of the polyester composition to the first glycol composition and one or more glycolysis catalysts in a reaction vessel under depolymerization conditions.

[0101] Item 6. The method according to any one of items 1 to 5, wherein the first glycol composition further comprises EG, and the weight ratio of EG to diethylene glycol (DEG), triethylene glycol (TEG), 1,4-cyclohexanedimethanol (CHDM), poly(ethylene glycol) (PEG), neopentyl glycol (NPG), propanediol (PDO), butanediol (BDO), 2-methyl-2,4-pentanediol (MP diol), poly(tetramethylene ether) glycol (PTMG), or a combination thereof is in the range of about 99:1 to about 0:100.

[0102] Item 7. The method according to any one of items 1 to 6, wherein the weight ratio of the one or more alcohols to the polyester composition can be in the range of about 2:1 to about 10:1. Item 8. The polyester composition is polyethylene terephthalate (PET), 1,4-cyclohexanedimethanol (CHDM) modified PET, isophthalic acid (IPA) modified PET, diethylene glycol (DEG) modified PET, neopentyl glycol (NPG) modified PET, propanediol (PDO) modified PET, butanediol (BDO) modified PET, hexanediol (HDO) modified PET, 2-methyl-2,4-pentanediol (MP diol) modified PET, isosorbide modified PET, poly (tetramethylene ether) glycol (PTMG) modified PET, poly (ethylene glycol) (PEG) modified PET, polycyclohexylene dimethylene terephthalate (PCT), cyclohexanedimethanol (CHDM) containing copolyester, isosorbide containing copolyester, or a combination thereof. The method according to any one of items 1 to 7.

[0103] Item 9. The method according to any one of items 1 to 8, wherein the polyester composition comprises 0 mol% to 100 mol% CHDM, 0 mol% to 100 mol% DEG, 0 mol% to 100 mol% NPG, 0 mol% to 100 mol% PDO, 0 mol% to 100 mol% BDO, 0 mol% to 100 mol% HDO, 0 mol% to 100 mol% MP diol, 0 mol% to 100 mol% isosorbide, 0 mol% to 100 mol% PTMG, 0 mol% to 100 mol% PEG, and 0 mol% to 30 mol% isophthalic acid, wherein the total of the diol equivalents in the one or more polyesters is about 100 mol%, and the total of the diacid equivalents in the one or more polyesters is about 100 mol%.

[0104] Item 10. The method according to any one of items 1 to 9, wherein the polyester composition has an intrinsic viscosity of about 0.1 dL / g to about 1.2 dL / g as determined according to ASTM D2857-70. Item 11. The method according to any one of items 1 to 10, wherein one or more polyesters present in the polyester composition are recycled polyesters.

[0105] Item 12. The polyester composition contains one or more foreign substances, and the one or more foreign substances are polyesters other than polyethylene terephthalate, polyvinyl chloride (PVC), polyvinyl acetal, polyvinyl butyral (PVB), polyvinyl alcohol (PVOH), ethylene vinyl alcohol (EVOH), cotton, polyolefins, polyethylene, polypropylene, polystyrene, polycarbonate, spandex, natural fibers, cellulose esters, polyacrylates, polymethacrylates, polyamides, nylons, poly(lactic acid), polydimethylsiloxanes, polysilanes, calcium carbonate, titanium dioxide, inorganic fillers, dyes, pigments, color toners, colorants, plasticizers, adhesives, flame retardants, metals, aluminum, and iron. The method according to any one of items 1 to 11.

[0106] Item 13. The method according to item 12, wherein the one or more foreign substances are present in the polyester composition in an amount of 0.01 wt.% to 50 wt.% based on the weight of the one or more polyesters in the polyester composition.

[0107] Item 14. The method according to any one of Items 1 to 13, wherein the one or more dialkyl terephthalates in the solid component include dimethyl terephthalate (DMT), and the DMT has a purity of at least 90%. Item 15. The method according to any one of items 1 to 14, wherein the solid component further comprises dimethyl isophthalate (DMI) in an amount of 1000 ppm or less, or 500 ppm or less; bisphenol A (BPA) in an amount of 1000 ppm or less, or 500 ppm or less; or both.

[0108] Item 16. One or more glycolysis catalysts are selected from the group consisting of Li2CO3, K2CO3, CaCO3, Na2CO3, Cs2CO3, ZrCO3, LiOH, NaOH, KOH, tetrabutylammonium hydroxide (TBAH), sodium methoxide (NaOMe), lithium methoxide (LiOMe), magnesium methoxide (Mg(OMe)2, potassium t-butoxide, ethylene glycol monosodium salt, ethylene glycol disodium salt, tetraisopropyl titanate (TIPT), butyltin tris-2-ethylhexanoate (FASCAT 4102), 1,8-diazabicyclo[5.4.0]undec-7-ene (DBU), zinc acetylacetonate hydrate (Zn(acac)2), zinc acetate (Zn(OAc)2), manganese(II) acetate (Mn(OAc)2), hydrotalcite, zeolite and lithium chloride.

[0109] Clause 17. The method of clause 16, wherein the one or more glycolysis catalysts comprise a member selected from the group consisting of LiOH, NaOH, KOH, tetraisopropyl titanate (TIPT), butyltin tris-2-ethylhexanoate (FASCAT 4102), ZrCO3, 1,8-diazabicyclo[5.4.0]undec-7-ene (DBU), sodium methoxide (NaOMe), lithium methoxide (LiOMe), zinc acetylacetonate hydrate (Zn(acac)2), Cs2CO3, ethylene glycol sodium salt, and manganese(II) acetate (Mn(OAc)2).

[0110] Item 18. The method of item 16, wherein the one or more glycolysis catalysts comprise a member selected from the group consisting of LiOH, NaOH, KOH, sodium methoxide (NaOMe), Cs2CO3, ethylene glycol sodium salt, and lithium methoxide (LiOMe).

[0111] Item 19. The method according to items 12 to 13, further comprising a step of separating at least a portion of one or more insoluble components from the first liquid component of the first mixture before exposing at least a portion of the first liquid component of the first mixture to one or more alcohols and an alcoholysis catalyst, wherein at least a portion of the foreign matter is present in the one or more insoluble components.

[0112] Item 20. The method of item 19, wherein the separating comprises filtration, centrifugation, sedimentation, sedimentation, or a combination thereof. Item 21. The method according to items 1 to 20, wherein the one or more alcohols include methanol.

[0113] Item 22. The method according to any one of items 1 to 21, wherein the alcoholysis catalyst is present in an amount of 0.1 wt.% to 20 wt.% based on the weight of the polyester composition. Item 23. The method according to items 1 to 22, wherein the alcoholysis catalyst comprises K2CO3, Na2CO3, Li2CO3, Cs2CO3; KOH, LiOH, NaOH; NaOMe, Mg(OMe)2, KOMe, KOt-Bu, ethylene glycol monosodium salt, ethylene glycol disodium salt, or a combination thereof.

[0114] Item 24. The method of item 23, wherein the alcoholysis catalyst comprises KOH, NaOH, NaOMe, or a combination thereof. Item 25. The method according to any one of items 1 to 24, wherein the second liquid component comprises at least a portion of the first glycol composition, at least a portion of the alcohol composition, or a combination thereof.

[0115] Item 26. The method of item 25, further comprising separating at least a portion of the first glycol composition from the second liquid component to form a recycled glycol composition. Item 27. The method of item 26, further comprising depolymerizing one or more polyesters in the second polyester composition in the presence of the recycled glycol composition.

[0116] Item 28. The method of items 1 to 27, carried out as a batch process, a semi-continuous process, or a continuous process. Item 29. The method of any one of items 1 to 28, wherein the one or more depolymerization products include monomers, oligomers, or combinations thereof.

[0117] Item 30. The method according to item 29, wherein the one or more oligomers have a degree of polymerization of 2 to 10. Clause 31. The method of clause 26, wherein the step of separating the first glycol composition from the second liquid component to form a recycled glycol composition comprises exposing the second liquid component to a distillation process to recover at least a portion of the first glycol composition.

[0118] Item 32. A method for recovering one or more dialkyl terephthalates from a polyester composition, comprising exposing the polyester composition to a first glycol composition and one or more glycolysis catalysts in a reaction vessel under depolymerization conditions to prepare a first mixture, the first mixture comprising a first liquid component and one or more insoluble components, the first glycol composition comprising diethylene glycol (DEG), triethylene glycol (TEG), 1,4-cyclohexanedimethanol (CHDM), poly(ethylene glycol) (PEG), neopentyl glycol (NPG), propanediol (PDO), butanediol (BDO), 2-methyl-2,4-pentanediol (MP diol), poly(tetramethylene ether) glycol (PTMG), or a combination thereof, the first liquid component comprising one or more depolymerization products and ethylene glycol (EG), the depolymerization conditions comprising a temperature in the range of about 120° C. to about 260° C., a pressure of about 0.013 atm (0.2 psi), and a pressure of about 0.013 atm (0.2 psi). g) exposing at least a portion of the first liquid component to one or more alcohols and an alcoholysis catalyst in an alcoholysis reaction vessel under alcoholysis conditions to provide a second mixture, the second mixture comprising a solid component comprising one or more dialkyl terephthalates and a second liquid component, the alcoholysis conditions comprising a temperature in the range of about 25° C. to about 90° C., a pressure in the range of about 1 atm (14.7 psig) to about 2 atm (30 psig), and a time period in the range of about 0.5 hours to about 5 hours; separating at least a portion of the one or more dialkyl terephthalates from the second mixture; and exposing at least a portion of the second liquid component to distillation conditions to separate at least a portion of the EG and provide a recycled glycol composition, the recycled glycol composition comprising at least a portion of the first glycol composition.

[0119] Item 33. The method according to item 32, wherein the weight ratio of the first glycol composition to the polyester composition ranges from about 1:9 to about 9:1 during exposing the polyester composition to the first glycol composition and one or more glycolysis catalysts in a reaction vessel under depolymerization conditions to prepare a first mixture.

[0120] Item 34. The method according to any one of items 32 to 33, wherein the first glycol composition further comprises EG, and the weight ratio of EG to diethylene glycol (DEG), triethylene glycol (TEG), 1,4-cyclohexanedimethanol (CHDM), poly(ethylene glycol) (PEG), neopentyl glycol (NPG), propanediol (PDO), butanediol (BDO), 2-methyl-2,4-pentanediol (MP diol), poly(tetramethylene ether) glycol (PTMG), or a combination thereof is in the range of about 99:1 to about 0:100.

[0121] Item 35. The method according to any one of items 32 to 34, wherein the weight ratio of the one or more alcohols to the polyester composition can be in the range of about 2:1 to about 10:1. Item 36. The polyester composition is polyethylene terephthalate (PET), 1,4-cyclohexanedimethanol (CHDM) modified PET, isophthalic acid (IPA) modified PET, diethylene glycol (DEG) modified PET, neopentyl glycol (NPG) modified PET, propanediol (PDO) modified PET, butanediol (BDO) modified PET, hexanediol (HDO) modified PET, 2-methyl-2,4-pentanediol (MP diol) modified PET, isosorbide modified PET, polycyclohexylene dimethylene terephthalate (PCT), cyclohexanedimethanol (CHDM)-containing copolyester, isosorbide-containing copolyester, PTMG modified PET, or a combination thereof. The method according to any one of items 32 to 35.

[0122] Item 37. The polyester composition comprises 0 mol% to 100 mol% CHDM, 0 mol% to 100 mol% DEG, 0 mol% to 100 mol% NPG, 0 mol% to 100 mol% PDO, 0 mol% to 100 mol% BDO, 0 mol% to 100 mol% HDO, 0 mol% to 100 mol% MP diol, 0 mol% to 100 mol% isosorbide, 0 mol% to 100 mol% PTMG, 0 mol% to 100 mol% PEG, and 0 mol% to 30 mol% isophthalic acid, wherein the total of the diol equivalents in the one or more polyesters is about 100 mol%, and the total of the diacid equivalents in the one or more polyesters is about 100 mol%. The method of any one of items 32 to 36.

[0123] Item 38. The method according to any one of items 32 to 37, wherein the polyester composition has an intrinsic viscosity of about 0.1 dL / g to about 1.2 dL / g as determined according to ASTM D2857-70. Item 39. The method according to items 32 to 38, wherein one or more polyesters present in the polyester composition are recycled polyesters.

[0124] Item 40. The polyester composition contains one or more foreign substances, and the one or more foreign substances are polyesters other than polyethylene terephthalate, polyvinyl chloride (PVC), polyvinyl acetal, polyvinyl butyral (PVB), polyvinyl alcohol (PVOH), ethylene vinyl alcohol (EVOH), cotton, polyolefins, polyethylene, polypropylene, polystyrene, polycarbonate, spandex, natural fibers, cellulose esters, polyacrylates, polymethacrylates, polyamides, nylons, poly(lactic acid), polydimethylsiloxanes, polysilanes, calcium carbonate, titanium dioxide, inorganic fillers, dyes, pigments, color toners, colorants, plasticizers, adhesives, flame retardants, metals, aluminum, and iron. The method according to any one of items 32 to 39.

[0125] Item 41. The method according to item 40, wherein one or more foreign substances are present in the polyester composition in an amount of 0.01 wt.% to 50 wt.% based on the weight of one or more polyesters in the polyester composition.

[0126] Item 42. The method according to any one of Items 32 to 41, wherein the one or more dialkyl terephthalates in the solid component include dimethyl terephthalate (DMT), and the DMT has a purity of at least 90%.

[0127] Item 43. The method according to any one of items 32 to 42, wherein the solid component further comprises dimethyl isophthalate (DMI) in an amount of 1000 ppm or less, or 500 ppm or less; bisphenol A (BPA) in an amount of 1000 ppm or less, or 500 ppm or less; or both.

[0128] Item 44. One or more glycolysis catalysts are selected from the group consisting of Li2CO3, K2CO3, CaCO3, Na2CO3, Cs2CO3, ZrCO3, LiOH, NaOH, KOH, tetrabutylammonium hydroxide (TBAH), sodium methoxide (NaOMe), lithium methoxide (LiOMe), magnesium methoxide (Mg(OMe)2, potassium t-butoxide, ethylene glycol monosodium salt, ethylene glycol disodium salt, tetraisopropyl titanate (TIPT), butyltin tris-2-ethylhexanoate (FASCAT 4102), 1,8-diazabicyclo[5.4.0]undec-7-ene (DBU), zinc acetylacetonate hydrate (Zn(acac)2), zinc acetate (Zn(OAc)2), manganese(II) acetate (Mn(OAc)2), hydrotalcite, zeolite and lithium chloride.

[0129] Clause 45. The method of clause 44, wherein the one or more glycolysis catalysts comprise a member selected from the group consisting of LiOH, NaOH, KOH, tetraisopropyl titanate (TIPT), butyltin tris-2-ethylhexanoate (FASCAT 4102), ZrCO3, 1,8-diazabicyclo[5.4.0]undec-7-ene (DBU), sodium methoxide (NaOMe), lithium methoxide (LiOMe), zinc acetylacetonate hydrate (Zn(acac)2), Cs2CO3, ethylene glycol sodium salt, and manganese(II) acetate (Mn(OAc)2).

[0130] Clause 46. The method of clause 44, wherein the one or more glycolysis catalysts comprise a member selected from the group consisting of LiOH, NaOH, KOH, sodium methoxide (NaOMe), Cs2CO3, ethylene glycol sodium salt, lithium methoxide (LiOMe), hydrotalcite, and zeolite.

[0131] Item 47. The method according to items 40 to 41, further comprising a step of separating at least a portion of one or more insoluble components from the first liquid component of the first mixture before exposing at least a portion of the first liquid component to one or more alcohols and an alcoholysis catalyst, wherein at least a portion of the foreign matter is present in the one or more insoluble components.

[0132] Item 48. The method of item 47, wherein the separating comprises filtration, centrifugation, sedimentation, sedimentation or a combination thereof. Item 49. The method according to items 32 to 48, wherein the one or more alcohols include methanol.

[0133] Item 50. The method of any one of items 32 to 49, wherein exposing at least a portion of the second liquid component to distillation conditions to separate at least a portion of the EG further results in a recycled alcohol composition.

[0134] Item 51. The method of item 50, further comprising the step of supplying at least a portion of the recycled alcohol composition to an alcoholysis reaction vessel. Item 52. The method according to items 2 to 31, wherein the solvent is toluene, xylene, isopar C, isopar E, isopar G, isopar H, isopar L, isopar M, or a combination thereof.

[0135] The present disclosure has been described in detail with particular reference to certain embodiments thereof, but it will be understood that variations and modifications can be made within the spirit and scope of the disclosure.

Claims

1. 1. A method for recovering one or more dialkyl terephthalates from a polyester composition comprising the steps of exposing the polyester composition to a first glycol composition and one or more glycolysis catalysts in a reaction vessel under depolymerization conditions to provide a first mixture, the first mixture comprising one or more depolymerization products; ethylene glycol (EG); and one or more insoluble components, the depolymerization conditions comprising a temperature in the range of about 120° C. to about 260° C., a pressure in the range of about 0.013 atm (0.2 psig) to about 10.2 atm (150 psig), and a time period in the range of about 0.5 hours to about 10 hours, the first glycol composition being selected from the group consisting of diethylene glycol (DEG), triethylene glycol (TEG), 1,4-cyclohexanedimethanol (CHDM), poly(ethylene glycol) (PEG), neopentyl glycol (NPG), propanediol (PDO), butanediol (BDO), 2-methyl-2,4-pentanediol (DMSO), ethylene glycol (EG ...

16. A method for producing a polyester composition comprising the steps of: including a first glycol composition, a poly(tetramethylene ether) glycol (MP diol), a poly(tetramethylene ether) glycol (PTMG), or a combination thereof; removing at least a portion of the EG from the reaction vessel while exposing the polyester composition to a first glycol composition and one or more glycolysis catalysts in the reaction vessel; exposing at least a portion of a first liquid component of the first mixture to one or more alcohols and an alcoholysis catalyst under alcoholysis conditions to provide a second mixture, the second mixture comprising a solid component comprising one or more dialkyl terephthalates and a second liquid component, the alcoholysis conditions comprising a temperature in the range of about 25° C. to about 90° C., a pressure in the range of about 1 atm (14.7 psig) to about 2 atm (30 psig), and a time period in the range of about 0.5 hours to about 5 hours; and separating at least a portion of the one or more dialkyl terephthalates from the second mixture by solid-liquid separation.

2. 10. The process of claim 1, wherein a solvent is present during exposure of the polyester composition to the first glycol composition and the one or more glycolysis catalysts in the reaction vessel.

3. The method of claim 2, wherein the solvent is a C7 to C16 hydrocarbon having a boiling point of 100°C to 250°C.

4. 10. The process of claim 1 , wherein the depolymerization conditions comprise a pressure of from 0.013 atm (0.2 psig) to about 1 atm (14.7 psig).

5. 2. The method of claim 1, wherein during exposure of the polyester composition to the first glycol composition and the one or more glycolysis catalysts in a reaction vessel under depolymerization conditions, the weight ratio of the first glycol composition to the polyester composition ranges from about 1:9 to about 9:

1.

6. 2. The method of claim 1, wherein the first glycol composition further comprises EG, and a weight ratio of EG to diethylene glycol (DEG), triethylene glycol (TEG), 1,4-cyclohexanedimethanol (CHDM), poly(ethylene glycol) (PEG), neopentyl glycol (NPG), propanediol (PDO), butanediol (BDO), 2-methyl-2,4-pentanediol (MP diol), poly(tetramethylene ether) glycol (PTMG), or combinations thereof ranges from about 99:1 to about 0:

100.

7. 4. The method of claim 3, wherein the solvent is toluene, xylene, isopar C, isopar E, isopar G, isopar H, isopar L, isopar M, or a combination thereof.

8. 2. The method of claim 1, wherein the polyester composition comprises polyethylene terephthalate (PET), 1,4-cyclohexanedimethanol (CHDM) modified PET, isophthalic acid (IPA) modified PET, diethylene glycol (DEG) modified PET, neopentyl glycol (NPG) modified PET, propanediol (PDO) modified PET, butanediol (BDO) modified PET, hexanediol (HDO) modified PET, 2-methyl-2,4-pentanediol (MP diol) modified PET, isosorbide modified PET, poly(tetramethylene ether) glycol (PTMG) modified PET, poly(ethylene glycol) (PEG) modified PET, polycyclohexylene dimethylene terephthalate (PCT), cyclohexanedimethanol (CHDM)-containing copolyesters, isosorbide-containing copolyesters, or combinations thereof.

9. 10. The method of claim 1, wherein the polyester composition comprises one or more contaminants, the one or more contaminants being present in the polyester composition in an amount of 0.01 wt. % to 50 wt. %, based on the weight of the one or more polyesters in the polyester composition, and the one or more contaminants comprises at least one member selected from the group consisting of polyesters other than polyethylene terephthalate, polyvinyl chloride (PVC), polyvinyl acetal, polyvinyl butyral (PVB), polyvinyl alcohol (PVOH), ethylene vinyl alcohol (EVOH), cotton, polyolefins, polyethylene, polypropylene, polystyrene, polycarbonate, spandex, natural fibers, cellulose esters, polyacrylates, polymethacrylates, polyamides, nylons, poly(lactic acid), polydimethylsiloxanes, polysilanes, calcium carbonate, titanium dioxide, inorganic fillers, dyes, pigments, color toners, colorants, plasticizers, adhesives, flame retardants, metals, aluminum, and iron.

10. 2. The method of claim 1, wherein the one or more dialkyl terephthalates in the solid component comprises dimethyl terephthalate (DMT), the DMT being at least 90% pure.

11. The one or more glycolysis catalysts are Li 2 CO 3 , K 2 CO 3 , CaCO 3 , Na 2 CO 3 , Cs 2 CO 3 , ZrCO3, LiOH, NaOH, KOH, tetrabutylammonium hydroxide (TBAH), sodium methoxide (NaOMe), lithium methoxide (LiOMe), magnesium methoxide (Mg(OMe) 2 , potassium t-butoxide, ethylene glycol monosodium salt, ethylene glycol disodium salt, tetraisopropyl titanate (TIPT), butyltin tris-2-ethylhexanoate (FASCAT 4102), 1,8-diazabicyclo[5.4.0]undec-7-ene (DBU), zinc acetylacetonate hydrate (Zn(acac) 2 ), zinc acetate (Zn(OAc) 2 ), Manganese(II) acetate (Mn(OAc) 2 ), a member selected from the group consisting of hydrotalcite, zeolite and lithium chloride.

12. 10. The method of claim 9, further comprising the step of separating at least a portion of the one or more insoluble components from the first liquid component of the first mixture prior to exposing the at least a portion of the first liquid component of the first mixture to the one or more alcohols and the alcoholysis catalyst, wherein at least a portion of the foreign matter is present in the one or more insoluble components.

13. The one or more alcohols include methanol, and the alcoholysis catalyst is present in an amount of 0.1 wt. % to 20 wt. % based on the weight of the polyester composition, and the alcoholysis catalyst is selected from the group consisting of K 2 CO 3 , Na 2 CO 3 , Li 2 CO 3 , Cs 2 CO 3 ;KOH, LiOH, NaOH; NaOMe, Mg(OMe) 2 , KOMe, KOt-Bu, ethylene glycol monosodium salt, ethylene glycol disodium salt, or combinations thereof.

14. 10. The method of claim 1, further comprising the steps of separating at least a portion of the first glycol composition from the second liquid component to form a recycled glycol composition; and depolymerizing one or more polyesters in the second polyester composition in the presence of the recycled glycol composition.

15. 1. A method for recovering one or more dialkyl terephthalates from a polyester composition comprising the steps of exposing the polyester composition to a first glycol composition and one or more glycolysis catalysts in a reaction vessel under depolymerization conditions to provide a first mixture, the first mixture comprising a first liquid component and one or more insoluble components, the first glycol composition comprising diethylene glycol (DEG), triethylene glycol (TEG), 1,4-cyclohexanedimethanol (CHDM), poly(ethylene glycol) (PEG), neopentyl glycol (NPG), propanediol (PDO), butanediol (BDO), 2-methyl-2,4-pentanediol (MP diol), poly(tetramethylene ether) glycol (PTMG), or combinations thereof, the first liquid component comprising one or more depolymerization products and ethylene glycol (EG), and the depolymerization conditions comprising a temperature in the range of about 120° C. to about 260° C., a pressure of about 0.013 atm (0.2 psig) or ... to about 10.2 atm (150 psig) and for a time period ranging from about 0.5 hours to about 10 hours; exposing at least a portion of the first liquid component to one or more alcohols and an alcoholysis catalyst under alcoholysis conditions in an alcoholysis reaction vessel to provide a second mixture, the second mixture comprising a solid component comprising one or more dialkyl terephthalates and a second liquid component, the alcoholysis conditions comprising a temperature in the range of about 25° C. to about 90° C., a pressure in the range of about 1 atm (14.7 psig) to about 2 atm (30 psig), and a time period ranging from about 0.5 hours to about 5 hours; separating at least a portion of the one or more dialkyl terephthalates from the second mixture; and exposing at least a portion of the second liquid component to distillation conditions to separate at least a portion of the EG and provide a recycled glycol composition, the recycled glycol composition comprising at least a portion of the first glycol composition.

16. 16. The method of claim 15, wherein during exposing the polyester composition to the first glycol composition and one or more glycolysis catalysts in a reaction vessel under depolymerization conditions to provide a first mixture, a weight ratio of the first glycol composition to the polyester composition ranges from about 1:9 to about 9:

1.

17. 16. The method of claim 15, wherein the one or more dialkyl terephthalates in the solid component comprises dimethyl terephthalate (DMT), the DMT being at least 90% pure.

18. 16. The method of claim 15, wherein the polyester composition comprises one or more foreign matter in an amount of 0.01 wt. % to 50 wt. %, based on the weight of the one or more polyesters in the polyester composition, and the one or more foreign matter comprises at least one member selected from the group consisting of polyesters other than polyethylene terephthalate, polyvinyl chloride (PVC), polyvinyl acetal, polyvinyl butyral (PVB), polyvinyl alcohol (PVOH), ethylene vinyl alcohol (EVOH), cotton, polyolefins, polyethylene, polypropylene, polystyrene, polycarbonate, spandex, natural fibers, cellulose esters, polyacrylates, polymethacrylates, polyamides, nylons, poly(lactic acid), polydimethylsiloxanes, polysilanes, calcium carbonate, titanium dioxide, inorganic fillers, dyes, pigments, color toners, colorants, plasticizers, adhesives, flame retardants, metals, aluminum, and iron.

19. 20. The method of claim 18, further comprising the step of separating at least a portion of the one or more insoluble components from the first liquid component of the first mixture prior to exposing at least a portion of the first liquid component to the one or more alcohols and the alcoholysis catalyst, wherein at least a portion of the foreign matter is present in the one or more insoluble components.

20. 16. The method of claim 15, wherein exposing at least a portion of the second liquid component to distillation conditions to separate at least a portion of the EG further results in a recycled alcohol composition, and the method further comprises feeding at least a portion of the recycled alcohol composition to an alcoholysis reactor vessel.