Ion-exchangeable glass with high fracture toughness
Lithium aluminosilicate glasses with tailored compositions and ion-exchange processes address bending and sharp contact failures in portable devices, offering high fracture toughness and durability for thin cover glasses.
Patent Information
- Application Number
- JP2024525423
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2021-10-26
- Filing Date
- 2022-10-25
- Publication Date
- 2024-10-31
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Portable electronic devices such as smartphones and tablets are prone to damage from bending failure and sharp contact fractures due to their portable nature, with existing ion-exchanged glasses offering limited protection against dynamic sharp contacts.
Development of lithium aluminosilicate glasses with specific compositions and ion-exchange processes to enhance compressive stress, central tension, and fracture toughness, allowing for the formation of thin, damage-resistant cover glasses.
The glasses exhibit high fracture toughness and Young's modulus, providing improved resistance to bending and sharp contact damage while maintaining thinness and manufacturability, enhancing drop performance and durability.
Smart Images

Figure 2024540112000001_ABST
Abstract
Description
Priority
[0001] This application claims the benefit of priority to U.S. Provisional Patent Application No. 63 / 271,813, filed October 26, 2021, the contents of which are relied upon and incorporated herein by reference in their entirety. [Technical field]
[0002] This disclosure relates generally to glass compositions suitable for use in cover glass for electronic devices. More particularly, this disclosure relates to ion-exchangeable glasses that can be formed into cover glass for electronic devices. [Background technology]
[0003] The portable nature of portable devices such as smartphones, tablets, portable media players, personal computers, and cameras makes these devices particularly susceptible to situations where they are accidentally dropped onto a hard surface, such as the ground. These devices typically incorporate a cover glass that can be damaged upon impact with a hard surface. In many of these devices, the cover glass acts as a cover for the display and may provide touch functionality, and thus, use of the device is adversely affected when the cover glass is damaged.
[0004] There are two primary failure modes for cover glass when the associated portable device is dropped onto a hard surface. One of these modes is bending failure, which occurs due to bending of the glass when the device is subjected to dynamic loads from impact with the hard surface. The other mode is sharp contact failure, which occurs due to the introduction of damage into the glass surface. When glass impacts with rough hard surfaces such as asphalt, granite, etc., sharp indentations can be created on the glass surface. These indentations become breakage sites in the glass surface from which cracks can initiate and propagate.
[0005] Glass can be made more resistant to bending fracture by ion-exchange techniques, which involve inducing compressive stresses in the glass surface. However, ion-exchanged glass is still vulnerable to dynamic sharp contact due to high stress concentrations caused by localized indentation of the glass by the sharp contact.
[0006] Glass manufacturers and manufacturers of handheld devices have continually worked to improve the resistance of handheld devices to breakage due to sharp contact. Solutions range from coatings on the cover glass to bezels that prevent the cover glass from directly impacting a hard surface when the device is dropped onto it. However, due to constraints of aesthetic and functional requirements, it is very difficult to completely prevent the cover glass from impacting a hard surface.
[0007] It is also desirable for portable devices to be as thin as possible. Thus, in addition to strength, it is also desirable to make the glass to be used as a cover glass in a portable device as thin as possible. Therefore, in addition to enhancing the strength of the cover glass, it is also desirable for the glass to have mechanical properties that allow it to be formed by processes that allow the production of thin glass-based articles, such as thin glass sheets. Summary of the Invention [Problem to be solved by the invention]
[0008] Thus, there is a need for glasses that can be strengthened, such as by ion exchange, and that have mechanical properties that allow them to be formed into thin glass-based articles. [Means for solving the problem]
[0009] According to an aspect (1), there is provided a glass comprising 45 mol% to 70 mol% SiO2, 11.5 mol% to 25 mol% Al2O3, 2 mol% to 20 mol% Li2O, 0 mol% to 10 mol% Na2O, 9 mol% to 19 mol% MgO, 0 mol% to 4 mol% ZrO2, and 0 mol% to 0.5 mol% TiO2.
[0010] According to aspect (2), there is provided a glass comprising 45 mol% to 70 mol% SiO2, 4 mol% to 25 mol% Al2O3, 5 mol% to 20 mol% Li2O, 0.1 mol% to 10 mol% Na2O, 6 mol% to 25 mol% MgO, 0.1 mol% to 4 mol% ZrO2, 0.1 mol% to 5 mol% K2O, and 0.05 mol% to 0.5 mol% SnO2.
[0011] According to an embodiment (3), there is provided the glass of any of the previous embodiments, comprising 51 mol % or more and 65 mol % or less of SiO2.
[0012] According to an embodiment (4), there is provided the glass of any of the previous embodiments, comprising 12.0 mol % or more and 19 mol % or less of Al2O3.
[0013] According to an embodiment (5), there is provided the glass of any of the previous embodiments, comprising 3 mol % or more and 12 mol % or less of Li2O.
[0014] According to an embodiment (6), there is provided the glass of any of the previous embodiments, comprising 0.25 mol % or more and 6 mol % or less Na2O.
[0015] According to an embodiment (7), there is provided the glass of any of the previous embodiments, comprising 10 mol % or more and 19 mol % or less of MgO.
[0016] According to an embodiment (8), there is provided the glass of any of the previous embodiments, comprising 0.25 mol % or more and 2 mol % or less ZrO2.
[0017] According to an aspect (9), there is provided the glass of any of the previous aspects, wherein the glass is substantially free of TiO2.
[0018] According to an embodiment (10), there is provided the glass of any of the previous embodiments, comprising greater than or equal to 0 mol % and less than or equal to 10 mol % B2O3.
[0019] According to an embodiment (11), there is provided the glass of any of the previous embodiments, comprising greater than or equal to 0 mol % and less than or equal to 6 mol % B2O3.
[0020] According to an aspect (12), there is provided the glass of any of the previous aspects, wherein the glass is substantially free of B2O3.
[0021] According to an embodiment (13), there is provided the glass of any of the previous embodiments, comprising greater than or equal to 0 mol % and less than or equal to 4 mol % P2O5.
[0022] According to an embodiment (14), there is provided the glass of any of the previous embodiments, comprising greater than or equal to 0 mol % and less than or equal to 3 mol % P2O5.
[0023] According to an embodiment (15), there is provided the glass of any of the previous embodiments, wherein the glass is substantially free of P2O5.
[0024] According to an embodiment (16), there is provided the glass of any of the previous embodiments, comprising greater than or equal to 0 mol % and less than or equal to 3 mol % K2O.
[0025] According to an embodiment (17), there is provided the glass of any of the previous embodiments, wherein the glass is substantially free of KO.
[0026] According to an embodiment (18), there is provided the glass of any of the previous embodiments, comprising greater than or equal to 0 mol % and less than or equal to 3 mol % CaO.
[0027] According to an embodiment (19), there is provided the glass of any of the previous embodiments, wherein the glass is substantially free of CaO.
[0028] According to an embodiment (20), there is provided the glass of any of the previous embodiments, comprising from 0 mol % to 3 mol % SrO.
[0029] According to an embodiment (21), there is provided the glass of any of the previous embodiments, wherein the glass is substantially free of SrO.
[0030] According to an embodiment (22), there is provided the glass of any of the previous embodiments, comprising from 0 mol % to 5 mol % of ZnO.
[0031] According to an aspect (23), there is provided the glass of any of the previous aspects, wherein the glass is substantially free of ZnO.
[0032] According to aspect (24), the glass has a viscosity of 0.8 MPa m 0.5 Above 1.0MPa·M 0.5 Fracture toughness K IC The glass of any of the previous aspects is provided, having
[0033] According to an embodiment (25), there is provided the glass of any of the previous embodiments, wherein the glass has a Young's modulus of 80 GPa or more and 100 GPa or less.
[0034] According to aspect (26), there is provided a method comprising ion exchanging a glass-based substrate in a molten salt bath to form a glass-based article comprising a compressive stress layer extending from a surface of the glass-based article to a compression depth, the glass-based article comprising a central tension region, and the glass-based substrate made from the glass of any of the previous aspects.
[0035] According to an embodiment (27), there is provided the method of embodiment (26), wherein the molten salt bath comprises NaNO.
[0036] According to embodiment (28), there is provided the method of any of embodiments (26) through the immediately preceding embodiment, wherein the molten salt bath comprises KNO.
[0037] According to embodiment (29), there is provided the method of any of embodiments (26) through the immediately preceding embodiment, wherein the molten salt bath is at a temperature of from 400° C. or more to 550° C. or less.
[0038] According to embodiment (30), there is provided the method of any of embodiments (26) to the immediately preceding embodiment, wherein the ion exchange is for a period of from 0.5 hours or more to 48 hours or less.
[0039] According to embodiment (31), there is provided the method of any of embodiments (26) through the immediately preceding embodiment, further comprising ion exchanging the glass-based article in a second molten salt bath.
[0040] According to an embodiment (32), there is provided the method of the immediately preceding embodiment, wherein the second molten salt bath comprises KNO.
[0041] According to embodiment (33), there is provided a glass-based article having a compressive stress layer extending from the surface to a compression depth of the glass-based article, a central tension region, and a composition at the center of the glass-based article comprising: 45 mol% to 70 mol% SiO2, 11.5 mol% to 25 mol% Al2O3, 2 mol% to 20 mol% Li2O, 0 mol% to 10 mol% Na2O, 9 mol% to 19 mol% MgO, 0 mol% to 4 mol% ZrO2, and 0 mol% to 0.5 mol% TiO2.
[0042] According to embodiment (34), a glass-based article is provided having a compressive stress layer extending from the surface to a compression depth of the glass-based article, a central tension region, and a composition at the center of the glass-based article comprising: 45 mol% to 70 mol% SiO2, 4 mol% to 25 mol% Al2O3, 5 mol% to 20 mol% Li2O, 0.1 mol% to 10 mol% Na2O, 6 mol% to 25 mol% MgO, 0.1 mol% to 4 mol% ZrO2, 0.1 mol% to 5 mol% K2O, and 0.05 mol% to 0.5 mol% SnO2.
[0043] According to an embodiment (35), there is provided the glass-based article of any of the embodiments (33) to the immediately preceding embodiment, wherein the compressive stress layer has a compressive stress of 400 MPa or more and 2000 MPa or less.
[0044] According to embodiment (36), there is provided the glass-based article of any of embodiments (33) to the immediately preceding embodiment, wherein the central tension region has a maximum central tension of 30 MPa or more and 300 MPa or less.
[0045] According to embodiment (37), there is provided the glass-based article of any of embodiments (33) to the immediately preceding embodiment, wherein the compression depth is from 0.15t to 0.25t, inclusive, where t is the thickness of the glass-based article.
[0046] According to embodiment (38), there is provided the glass-based article of any of embodiments (33) through the immediately preceding embodiment, wherein the compressive stress layer has a compressive stress spike extending from a surface of the glass-based article to a compressive stress spike depth, the compressive stress spike depth being from 3 μm or more to 10 μm or less.
[0047] According to embodiment (39), there is provided the glass-based article of any of embodiments (33) to the immediately preceding embodiment, wherein the glass-based article has a thickness, t, of 0.2 mm or more and 2 mm or less.
[0048] According to an embodiment (40), there is provided the glass-based article of any of the embodiments (33) to the immediately preceding embodiment, wherein the composition at the center of the glass-based article comprises 51 mol% or more and 65 mol% or less of SiO2.
[0049] According to an embodiment (41), there is provided the glass-based article of any of the embodiments (33) to the immediately preceding embodiment, wherein the composition at the center of the glass-based article comprises from 12.0 mol% or more and 19 mol% or less Al2O3.
[0050] According to an embodiment (42), there is provided the glass-based article of any of the embodiments (33) to the immediately preceding embodiment, wherein the composition at the center of the glass-based article comprises 3 mol % or more and 12 mol % or less LiO.
[0051] According to an embodiment (43), there is provided the glass-based article of any of the embodiments (33) to the immediately preceding embodiment, wherein the composition at the center of the glass-based article comprises from 0.25 mol % or more and 6 mol % or less NaO.
[0052] According to an embodiment (44), there is provided the glass-based article of any of the embodiments (33) to the immediately preceding embodiment, wherein the composition at the center of the glass-based article comprises 10 mol% or more and 19 mol% or less MgO.
[0053] According to an embodiment (45), there is provided the glass-based article of any of the embodiments (33) to the immediately preceding embodiment, wherein the composition at the center of the glass-based article comprises 0.25 mol % or more and 2 mol % or less ZrO2.
[0054] According to embodiment (46), there is provided the glass-based article of any of embodiments (33) to the immediately preceding embodiment, wherein the composition at the center of the glass-based article is substantially free of TiO2.
[0055] According to an embodiment (47), there is provided the glass-based article of any of the embodiments (33) to the immediately preceding embodiment, wherein the composition at the center of the glass-based article comprises greater than or equal to 0 mol % and less than or equal to 10 mol % B2O3.
[0056] According to an embodiment (48), there is provided the glass-based article of any of the embodiments (33) to the immediately preceding embodiment, wherein the composition at the center of the glass-based article comprises greater than or equal to 0 mol % and less than or equal to 6 mol % B2O3.
[0057] According to embodiment (49), there is provided the glass-based article of any of embodiments (33) to the immediately preceding embodiment, wherein the composition at the center of the glass-based article is substantially free of B2O3.
[0058] According to an embodiment (50), there is provided the glass-based article of any of the embodiments (33) to the immediately preceding embodiment, wherein the composition at the center of the glass-based article comprises greater than or equal to 0 mol % and less than or equal to 4 mol % P2O5.
[0059] According to an embodiment (51), there is provided the glass-based article of any of the embodiments (33) to the immediately preceding embodiment, wherein the composition at the center of the glass-based article comprises greater than or equal to 0 mol % and less than or equal to 3 mol % P2O5.
[0060] According to an embodiment (52), there is provided the glass-based article of any of the embodiments (33) to the immediately preceding embodiment, wherein the composition at the center of the glass-based article is substantially free of P2O5.
[0061] According to embodiment (53), there is provided the glass-based article of any of embodiments (33) to the immediately preceding embodiment, wherein the composition at the center of the glass-based article comprises greater than or equal to 0 mol % and less than or equal to 3 mol % KO.
[0062] According to embodiment (54), there is provided the glass-based article of any of embodiments (33) to the immediately preceding embodiment, wherein the composition at the center of the glass-based article is substantially free of KO.
[0063] According to embodiment (55), there is provided the glass-based article of any of embodiments (33) to the immediately preceding embodiment, wherein the composition at the center of the glass-based article comprises greater than or equal to 0 mol % and less than or equal to 3 mol % CaO.
[0064] According to embodiment (56), there is provided the glass-based article of any of embodiments (33) to the immediately preceding embodiment, wherein the composition at the center of the glass-based article is substantially free of CaO.
[0065] According to embodiment (57), there is provided the glass-based article of any of embodiments (33) to the immediately preceding embodiment, wherein the composition at the center of the glass-based article comprises greater than or equal to 0 mol % and less than or equal to 3 mol % SrO.
[0066] According to embodiment (58), there is provided the glass-based article of any of embodiments (33) to the immediately preceding embodiment, wherein the composition at the center of the glass-based article is substantially free of SrO.
[0067] According to embodiment (59), there is provided the glass-based article of any of embodiments (33) to the immediately preceding embodiment, wherein the composition at the center of the glass-based article comprises greater than or equal to 0 mol % and less than or equal to 5 mol % ZnO.
[0068] According to embodiment (60), there is provided the glass-based article of any of embodiments (33) to the immediately preceding embodiment, wherein the composition at the center of the glass-based article is substantially free of ZnO.
[0069] According to embodiment (61), a glass having the same composition and microstructure as the composition at the center of the glass-based article is melt-melted at 0.8 MPa m 0.5 Above 1.0MPa·M 0.5 Fracture toughness K IC The glass-based article of any of embodiment (33) to the immediately preceding embodiment is provided, having
[0070] According to embodiment (62), there is provided the glass-based article of any of embodiments (33) to the immediately preceding embodiment, wherein the glass having the same composition and microstructure as the composition at the center of the glass-based article has a Young's modulus of 80 GPa or more and 100 GPa or less.
[0071] According to aspect (63), there is provided a consumer electronics product comprising: a housing having a front, a back, and a side; electrical components disposed at least partially within the housing, the electrical components including at least a controller, a memory, and a display disposed at or adjacent to the front of the housing; and a cover substrate disposed over the display, at least a portion of at least one of the housing and the cover substrate being made from the glass-based article of any of aspects (33) through the immediately preceding aspect.
[0072] Additional features and advantages are set forth in the following detailed description, and in part will be readily apparent to those skilled in the art from that description, or will be learned by practicing the embodiments described herein, including the following detailed description, the claims, and the accompanying drawings.
[0073] It should be understood that both the foregoing general description and the following detailed description describe various embodiments and are intended to provide an overview or framework for understanding the nature and character of the claimed subject matter. The accompanying drawings are included to provide a further understanding of the various embodiments, and are incorporated into and constitute a part of this specification. The drawings illustrate various embodiments described herein and, together with the description, serve to explain the principles and operation of the claimed subject matter. [Brief description of the drawings]
[0074] [Figure 1] 1 is a schematic diagram of a cross section of a glass-based article having a compressive stress region according to embodiments described and disclosed herein; [Figure 2A] FIG. 1 is a plan view of an example electronic device incorporating any of the glass-based articles disclosed herein. [Figure 2B] FIG. 2B is a perspective view of the example electronic device of FIG. [Diagram 3] Graph showing stress profiles for exemplary and comparative ion-exchanged glass articles. [Figure 4] Graph plotting residual strength of exemplary and comparative glass articles. [Diagram 5] Graph plotting residual strength of exemplary and comparative glass articles. [Figure 6] Schematic diagram of an apparatus for damaging glass articles by impact with an impact object. [Figure 7] Schematic diagram of the specimen and its cross section used in the double cantilever beam (DCB) procedure for determining the fracture toughness KIC DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0075] Reference will now be made in detail to lithium aluminosilicate glasses, according to various embodiments. Lithium aluminosilicate glasses have good ion exchangeability, and chemical strengthening processes have been used to achieve high strength and toughness properties in lithium aluminosilicate glasses. Lithium aluminosilicate glasses are highly ion-exchanged glasses with high glass quality. Substitution of Al2O3 in the silicate glass network increases the interdiffusivity of monovalent cations during ion exchange. Chemical strengthening in a molten salt bath (e.g., KNO3 or NaNO3) can result in glasses with high strength, high toughness, and high resistance to indentation crack formation. The stress profile achieved by chemical strengthening can have a variety of shapes that improve the drop performance, strength, toughness, and other attributes of glass-based articles.
[0076] Therefore, lithium aluminosilicate glasses with good physical properties, chemical durability, and ion exchangeability have been attracting attention for use as cover glasses. Specifically, lithium-containing aluminosilicate glasses with higher fracture toughness and higher Young's modulus are provided herein. By different ion exchange processes, larger central tension (CT), depth of compression (DOC), and high compressive stress (CS) can be achieved. However, the addition of lithium into aluminosilicate glasses can reduce the melting point, softening point, or liquidus viscosity of the glasses.
[0077] The term "residual strength" as used herein refers to the strength of a glass article after damage is introduced by an impact force when the article is bent to impart a tensile stress. The damage is introduced according to the method described in U.S. Patent Application Publication No. 2019 / 0072469 A1, which is incorporated herein by reference. For example, an apparatus for impact testing a glass article is shown in FIG. 6 at 1100. The apparatus 1100 comprises a pendulum 1102 including a bob 1104 attached to a pivot 1106. As used herein, the term "plumb" on a pendulum is a weight suspended from an arm and connected to the pivot at the arm. Thus, the illustrated plumb 1104 is connected to the pivot 1106 at an arm 1108. The plumb 1104 comprises a base 1110 for receiving a glass article, to which the glass article is secured. The apparatus 1100 further comprises an impacting object 1140 positioned such that when the plumb bob 1104 is released from a position at an angle greater than zero from the equilibrium position, a surface of the plumb bob 1104 contacts the impacting object 1140. The impacting object comprises an abrasive sheet having an abrasive surface to be placed in contact with the exterior surface of the glass article. The abrasive sheet may comprise abrasive paper, which may have a grit size ranging from 30 grit to 400 grit, or from 100 grit to 300 grit, for example 180 grit.
[0078] For the purposes of this disclosure, the impact object was in the form of a 6 mm diameter disk of 80 grit, 120 grit, or 180 grit abrasive paper that was fixed to the device. Glass articles having a thickness of about 600 μm were fixed to a plumb bob. A new abrasive paper disk was used for each impact. Damage to the glass articles was inflicted with an impact force of about 500 N, with the swing of the device's arm raised to an angle of about 90°. About 10 samples were impacted for each glass article.
[0079] At least 12 hours after damage introduction, the glass articles were broken in four-point bending (4PB). The damaged glass articles were placed on the support rods (support intervals) between the load paths (load intervals) with the damaged area facing down (i.e., tension side). For the purposes of this disclosure, the load interval was 18 mm and the support interval was 36 mm. The radius of curvature of the load rods and support rods was 3.2 mm. Loading was performed at a constant displacement rate of 5 mm / min using a screw-type testing device (Instron®, Norwood, Massachusetts, USA) until the glass broke. The 4PB test was performed at a temperature of 22° C.±2° C. and 50%±5% RH (relative humidity).
[0080] The applied fracture stress (or the applied stress to failure) in four-point bending (4PB) app is the expression:
[0081]
number
[0082] In the formula, P is the maximum fracture load, L (=36 mm) is the distance between the support rods (support interval), α (=18 mm) is the distance between the loading rods (load interval), b is the width of the glass plate, h is the thickness of the glass plate, and ν is the Poisson's ratio of the glass composition. The term (1 / (1-ν 2 )) takes into account the reinforcing effect of the plate. In four-point bending, the stress is constant under the loading interval, therefore the damage site is under uniaxial tensile stress loading of mode I. The stress rate for the four-point bending test of the specimens was estimated to be 15 MPa to 17 MPa per second. The residual strength of the glass composition is the highest applied fracture stress at which no fracture occurs.
[0083] As used herein, the term "softening point" refers to the point at which the viscosity of a glass composition is reduced to 1×10 7.6The softening point is referred to as the temperature at which the viscosity is in poise. This softening point was determined using the parallel plate viscosity method of ASTM C1351M-96(2012).
[0084] As used herein, the term "anneal point" refers to the point at which the viscosity of a glass composition is reduced to 1×10 13 The temperature at which the viscosity is in poise is called the temperature.
[0085] As used herein, the term "strain point" refers to the point at which the viscosity of a glass composition decreases to 1×10 14.68 The temperature at which the viscosity is in poise is called the temperature.
[0086] As used herein, unless otherwise specified, the term "CTE" refers to the average coefficient of thermal expansion of a glass composition over a temperature range from about 20° C. to about 300° C.
[0087] In the embodiments of the glass compositions described herein, concentrations of components (e.g., SiO2, Al2O3, Li2O, etc.) are given in mole percent (mol%) on an oxide basis unless otherwise specified. The components of the alkali aluminosilicate glass compositions according to the embodiments are described individually below. It should be understood that any of the various recited ranges of a component may be individually combined with any of the various recited ranges of any other component. As used herein, a trailing zero in a number is intended to represent a significant digit in that number. For example, "1.0" has two significant digits, and "1.00" has three significant digits.
[0088] As used herein, "glass substrate" refers to a piece of glass that has not been ion-exchanged. Similarly, "glass article" refers to a piece of glass that has been ion-exchanged and is formed by subjecting a glass substrate to an ion-exchange process. "Glass-based substrate" and "glass-based article" are defined accordingly and include glass substrates and glass articles, as well as substrates and articles made wholly or partially from glass, such as glass substrates and glass articles with surface coatings. Glass substrates and glass articles are sometimes referred to broadly and for convenience herein, although descriptions of glass substrates and glass articles should be understood to apply equally to glass-based substrates and glass-based articles.
[0089] High fracture toughness (K IC Disclosed herein is a lithium aluminosilicate glass composition containing MgO and ZrO2 that exhibits a high Young's modulus and a low melting point of at least 0.8 MPa m 0.5 K IC The glass composition is characterized by a fracture toughness value. In embodiments, the glass composition is characterized by a Young's modulus of at least 80 GPa. These properties are achieved, at least in part, by the inclusion of MgO, ZrO2, and Al2O3 in the glass.
[0090] While scratch performance is desirable, drop performance is a key attribute for glass-based articles incorporated into portable electronic devices. Fracture toughness and stress at depth are important for improving rough surface drop performance. For this reason, maximizing the amount of stress that can be provided to the glass before the frangibility limit is reached will increase stress at depth and rough surface drop performance. Fracture toughness is known to control the frangibility limit, and increasing fracture toughness increases the frangibility limit. The glass compositions disclosed herein have high fracture toughness and can achieve high compressive stress levels while remaining non-brittle. These features of the glass compositions allow for the development of improved stress profiles designed to address specific fracture modes. This capability allows ion-exchanged glass-based articles made from the glass compositions described herein to be customized with different stress profiles to address specific fracture modes of interest.
[0091] Glass compositions with high fracture toughness and Young's modulus are particularly suitable for forming chemically strengthened glass-based articles due to their ability to store large amounts of strain energy imparted by chemical strengthening without becoming brittle. The stored strain energy (Σ0) of commercial cover glasses and portable device housings is controlled to achieve the desired fracture resistance while avoiding the release of small particles upon fracture. The size (x) of the fragments that may form upon fracture is determined by the following formula:
[0092]
number
[0093] The fracture toughness (K IC) and the maximum central tension (CT) of the glass-based article, where t is the thickness of the glass-based article, v is the Poisson's ratio of the glass utilized to form the chemically strengthened glass-based article, and DOC is the compression depth of the glass-based article. The above equation indicates that glass compositions with higher fracture toughness will produce chemically strengthened glass-based articles with reduced size of small particles expelled.
[0094] The number of fragments that are generated when a glass-based article breaks is calculated using the following formula:
[0095]
number
[0096] where E is the Young's modulus of the glass utilized to form the glass-based article, σ is the stress as a function of depth, z=0.5t-DOC, such that -z to z defines the central tension zone of the glass-based article. As shown by the stored strain energy equation above, glass compositions having higher Young's modulus values have lower stored strain energy for any given stress profile, reducing the number of fragments produced when a glass-based article formed from that glass composition is fractured. Considering the fragment size equation and the stored strain energy equation together, it is apparent that glass compositions having high fracture toughness in combination with a high Young's modulus can produce glass-based articles with high maximum central tension while avoiding spallation.
[0097] The compositions described herein are selected to achieve high fracture toughness and Young's modulus values while maintaining a desired degree of manufacturability. The compositions include high amounts of Al2O3 and Li2O to produce the desired fracture toughness while maintaining compatibility with desired manufacturing limitations. The drop performance of ion-exchanged glass-based articles formed from the glass compositions described herein is improved by increasing the amount of compressive stress imparted to the glass article. The glass compositions described herein provide improved ion exchange performance as evidenced by increased center tensile capacity and increased ion exchange rates.
[0098] In the glass compositions described herein, SiO2 is the most abundant component, and thus SiO2 is the main component of the glass network formed from the glass composition. Pure SiO2 has a relatively low CTE. However, the melting point of pure SiO2 is high. Thus, if the concentration of SiO2 in the glass composition is too high, the formability of the glass composition will be reduced because the higher concentration of SiO2 increases the difficulty of melting the glass, which in turn adversely affects the formability of the glass. In addition, if the glass composition contains too much SiO2, the glass's ability to generate compressive stress through ion exchange will be reduced. If the concentration of SiO2 in the glass composition is too low, the chemical durability of the glass may be reduced, and the glass will be susceptible to surface damage during post-molding processing. In embodiments, the glass composition generally comprises SiO in an amount of from 45 mol% to 70 mol%, e.g., from 50 mol% to 65 mol%, from 51 mol% to 65 mol%, from 51 mol% to 64 mol%, from 52 mol% to 63 mol%, from 53 mol% to 62 mol%, from 54 mol% to 61 mol%, from 55 mol% to 60 mol%, from 56 mol% to 59 mol%, from 57 mol% to 58 mol%, and all ranges and subranges therebetween.
[0099] The glass composition includes Al2O3. Al2O3 may act as a glass network former, similar to SiO2. If the amount of Al2O3 is too high, Al2O3 may increase the liquidus viscosity of a glass melt formed from the glass composition and reduce the formability of the glass composition due to tetrahedral coordination. However, when the concentration of Al2O3 is balanced relative to the concentration of SiO2 and the concentration of alkali oxides in the glass composition, Al2O3 can reduce the liquidus temperature of the glass melt, thereby improving the liquidus viscosity and improving the compatibility of the glass composition with certain forming processes. Increasing the content of Al2O3 relative to the total content of alkali and alkaline earth oxides in the glass composition generally improves the durability of the glass. When the concentration of alkali oxides (R2O) approaches or exceeds the amount of Al2O3 in the glass composition, nearly all or all of the aluminum in the glass is present in a tetrahedral coordination state, and the alkali ions act as charge compensators. This charge balance increases the diffusivity of the alkali ions and increases the rate of ion exchange. The inclusion of Al2O3 in the glass composition can provide high fracture toughness values, as described herein. In an embodiment, the glass composition includes Al2O3 in a concentration of from 11.5 mol% to 25 mol%, e.g., from 12.0 mol% to 19 mol%, from 12 mol% to 24.5 mol%, from 12.5 mol% to 24 mol%, from 13 mol% to 23.5 mol%, from 13.5 mol% to 23 mol%, from 14 mol% to 22.5 mol%, from 14.5 mol% to 22 mol%, from 15 mol% to 21.5 mol%, from 15.5 mol% to 21 mol%, from 16 mol% to 20.5 mol%, from 16.5 mol% to 20 mol%, from 17 mol% to 19.5 mol%, from 17.5 mol% to 19 mol%, from 18 mol% to 18.5 mol%, and all ranges and sub-ranges therebetween.
[0100] In an embodiment, the glass composition includes Al2O3 in a concentration of from 4 mol% to 25 mol%, e.g., from 5 mol% to 24 mol%, from 6 mol% to 23 mol%, from 7 mol% to 22 mol%, from 8 mol% to 21 mol%, from 9 mol% to 20 mol%, from 10 mol% to 19 mol%, from 11 mol% to 18 mol%, from 12 mol% to 17 mol%, from 13 mol% to 16 mol%, from 14 mol% to 15 mol%, and all ranges and subranges therebetween.
[0101] The glass composition includes Li2O. The inclusion of Li2O in the glass composition allows for better control of the ion exchange process and further reduces the softening point, liquidus temperature, and melting temperature of the glass, thereby increasing the manufacturability of the glass. The presence of Li2O in the glass composition can also create a stress profile with a parabolic shape. Li2O in the glass composition also enables the high fracture toughness values described herein. If the glass composition contains too much Li2O, the thermal expansion coefficient of the glass increases and the chemical durability decreases. If the glass composition contains insufficient Li2O, the ability of the glass to be ion exchanged may be undesirably reduced and the desired stress profile may not be achieved. In embodiments, the glass composition includes LiO in an amount of from 2 mol% to 20 mol%, e.g., from 3 mol% to 12 mol%, from 4 mol% to 19 mol%, from 5 mol% to 18 mol%, from 6 mol% to 17 mol%, from 7 mol% to 16 mol%, from 8 mol% to 15 mol%, from 9 mol% to 14 mol%, from 10 mol% to 13 mol%, from 11 mol% to 12 mol%, and all ranges and subranges therebetween.
[0102] In embodiments, the glass composition includes LiO in an amount of from 5 mol% to 20 mol%, e.g., from 6 mol% to 19 mol%, from 7 mol% to 18 mol%, from 8 mol% to 17 mol%, from 9 mol% to 16 mol%, from 10 mol% to 15 mol%, from 11 mol% to 14 mol%, from 12 mol% to 13 mol%, and all ranges and subranges therebetween.
[0103] The glass compositions described herein include Na2O. Na2O aids in the ion-exchangeability of the glass composition, improving its formability, and therefore its manufacturability. However, adding too much Na2O to the glass composition may result in too low a CTE. Additionally, including too much Na2O in the glass relative to the amount of Li2O may reduce the glass's ability to achieve a large compression depth when ion-exchanged. In embodiments, the glass compositions include Na2O in an amount from greater than 0 mol% to less than or equal to 10 mol%, e.g., from greater than or equal to 0.25 mol% to less than or equal to 6 mol%, from greater than or equal to 0.5 mol% to less than or equal to 9 mol%, from greater than or equal to 1 mol% to less than or equal to 8 mol%, from greater than or equal to 2 mol% to less than or equal to 7 mol%, from greater than or equal to 3 mol% to less than or equal to 6 mol%, from greater than or equal to 4 mol% to less than or equal to 5 mol%, and all ranges and subranges therebetween.
[0104] In embodiments, the glass composition includes NaO in an amount from 0.1 mol% to 10 mol%, e.g., from 0.25 mol% to 6 mol%, from 0.5 mol% to 9 mol%, from 1 mol% to 8 mol%, from 2 mol% to 7 mol%, from 3 mol% to 6 mol%, from 4 mol% to 5 mol%, and all ranges and subranges therebetween.
[0105] The glass compositions described herein include MgO. MgO may reduce the liquidus viscosity of the glass and improve the melting behavior, which improves the formability and manufacturability of the glass. The inclusion of MgO in the glass composition may also improve the strain point and Young's modulus of the glass composition. However, if too much MgO is added to the glass composition, the liquidus viscosity may become too low to be compatible with desired forming techniques. Adding too much MgO may increase the density and CTE of the glass composition to undesirable levels and may also reduce the mobility of alkali ions in the glass, reducing the effectiveness of ion exchange processes. The inclusion of MgO in the glass composition helps achieve the high fracture toughness values described herein due to the strong electric field strength of MgO. In embodiments, the glass composition includes MgO in an amount from greater than or equal to 9 mol% to less than or equal to 19 mol%, e.g., from greater than or equal to 10 mol% to less than or equal to 19 mol%, e.g., from greater than or equal to 11 mol% to less than or equal to 18 mol%, from greater than or equal to 12 mol% to less than or equal to 17 mol%, from greater than or equal to 13 mol% to less than or equal to 16 mol%, from greater than or equal to 14 mol% to less than or equal to 15 mol%, and all ranges and subranges therebetween.
[0106] In embodiments, the glass composition includes MgO in an amount of from 6 mol% to 25 mol%, e.g., from 7 mol% to 24 mol%, from 8 mol% to 23 mol%, from 9 mol% to 22 mol%, from 10 mol% to 21 mol%, from 11 mol% to 20 mol%, from 12 mol% to 19 mol%, from 13 mol% to 18 mol%, from 14 mol% to 17 mol%, from 15 mol% to 16 mol%, and all ranges and subranges therebetween.
[0107] The glass compositions described herein include ZrO2. The inclusion of ZrO2 in the glass increases fracture toughness and allows the glass composition to achieve the high fracture toughness values described herein for high electric field strengths. The inclusion of ZrO2 in the glass composition also improves the chemical durability of the glass. If the glass composition contains too much ZrO2, undesirable zirconia inclusions may form in the glass due, at least in part, to the low solubility of ZrO2 in the glass. In addition, there are cost and supply constraints that make it undesirable to include too much ZrO2 in the glass composition. In embodiments, the glass compositions include ZrO2 in an amount from greater than 0 mol% to less than or equal to 4 mol%, e.g., from greater than or equal to 0.25 mol% to less than or equal to 2 mol%, from greater than or equal to 0.25 mol% to less than or equal to 3.5 mol%, from greater than or equal to 0.5 mol% to less than or equal to 3 mol%, from greater than or equal to 1 mol% to less than or equal to 2.5 mol%, from greater than or equal to 1.5 mol% to less than or equal to 2 mol%, and all ranges and subranges therebetween.
[0108] In embodiments, the glass composition includes ZrO in an amount from greater than or equal to 0.1 mol % to less than or equal to 4 mol %, e.g., from greater than or equal to 0.25 mol % to less than or equal to 2 mol %, from greater than or equal to 0.25 mol % to less than or equal to 3.5 mol %, from greater than or equal to 0.5 mol % to less than or equal to 3 mol %, from greater than or equal to 1 mol % to less than or equal to 2.5 mol %, from greater than or equal to 1.5 mol % to less than or equal to 2 mol %, and all ranges and subranges therebetween.
[0109] The glass compositions described herein may include TiO2. If the glass composition contains too much TiO2, the glass may be prone to devitrification and / or exhibit undesirable coloration, as well as undesirably alter the liquidus. The inclusion of some TiO2 in the glass composition may prevent undesirable discoloration of the glass when exposed to strong ultraviolet light, such as during post-fabrication processing. In embodiments, the glass composition includes an amount of TiO2 from 0 mol% to 0.5 mol%, e.g., from 0.1 mol% to 0.4 mol%, e.g., from 0.2 mol% to 0.3 mol%, and all ranges and subranges therebetween. In embodiments, the glass composition is substantially free or free of TiO2. As used herein, the term "substantially free" means that the component is not intentionally added as a component of the batch materials, even if the component is present in the final glass composition in very small amounts as a contaminant, such as less than 0.1 mol%.
[0110] The glass compositions described herein may include B2O3. The inclusion of B2O3 increases the fracture toughness of the glass, thereby increasing its damage resistance. Specifically, the glass compositions include boron in trigonal form, which increases the Knoop scratch threshold and fracture toughness of the glass. Including too much B2O3 in the composition reduces the amount of compressive stress imparted during the ion exchange process and may increase volatility at the free surface during fabrication to unacceptable levels. Including B2O3 in the glass composition also reduces the solution viscosity, which helps inhibit fracture of the zircon. In an embodiment, the glass composition includes B2O3 in an amount from greater than or equal to 0 mol% to less than or equal to 10 mol%, e.g., from greater than or equal to 0 mol% to less than or equal to 6 mol%, from greater than or equal to 0.5 mol% to less than or equal to 9 mol%, from greater than or equal to 1 mol% to less than or equal to 8 mol%, from greater than or equal to 2 mol% to less than or equal to 7 mol%, from greater than or equal to 3 mol% to less than or equal to 6 mol%, from greater than or equal to 4 mol% to less than or equal to 5 mol%, and all ranges and subranges therebetween. In embodiments, the glass composition is substantially free or free of B2O3.
[0111] The glass compositions described herein may include P2O5. The inclusion of P2O5 increases the diffusivity of ions in the glass and increases the rate of the ion exchange process. If the composition contains too much P2O5, the amount of compressive stress imparted during the ion exchange process may decrease and volatility at the free surface during fabrication may increase to unacceptable levels. In embodiments, the glass compositions include P2O5 in an amount of from 0 mol% to 4 mol%, e.g., from 0 mol% to 3 mol%, from 0.5 mol% to 3.5 mol%, from 1 mol% to 3 mol%, from 1.5 mol% to 2.5 mol%, from 0.5 mol% to 2 mol%, and all ranges and subranges therebetween. In embodiments, the glass compositions are substantially free or free of P2O5.
[0112] The glass compositions described herein may include K2O. The inclusion of K2O in the glass composition increases potassium diffusivity in the glass, resulting in a deeper compressive stress spike depth (DOL). SP ) can be achieved in shorter ion-exchange times. If the composition contains too much KO, the amount of compressive stress imparted during the ion-exchange process can be reduced. In embodiments, the glass composition contains KO in an amount from 0 mol % to 3 mol %, e.g., from 0.25 mol % to 2.5 mol %, e.g., from 0.5 mol % to 2 mol %, from 1 mol % to 1.5 mol %, and all ranges and subranges therebetween. In embodiments, the glass composition is substantially free or free of KO.
[0113] In embodiments, the glass composition includes KO in an amount from greater than or equal to 0.1 mol % to less than or equal to 5 mol %, e.g., from greater than or equal to 0.5 mol % to less than or equal to 4.5 mol %, from greater than or equal to 1 mol % to less than or equal to 4 mol %, from greater than or equal to 1.5 mol % to less than or equal to 3.5 mol %, from greater than or equal to 2 mol % to less than or equal to 3 mol %, and all ranges and subranges therebetween.
[0114] The glass compositions described herein may include CaO. CaO may reduce the liquidus viscosity of the glass, which may improve formability, strain point, and Young's modulus. However, if too much CaO is added to the glass composition, the density and CTE of the glass composition may increase to unacceptable levels, and the ion-exchangeability of the glass may be undesirably hindered due to reduced alkali ion mobility. In embodiments, the glass composition includes CaO in an amount of from 0 mol% to 3 mol%, e.g., from 0.25 mol% to 2.5 mol%, from 0.5 mol% to 2 mol%, from 1 mol% to 1.5 mol%, and all ranges and subranges therebetween. In embodiments, the glass composition is substantially free or free of CaO.
[0115] The glass compositions described herein may include SrO. SrO may reduce the viscosity of the glass, which may improve formability, strain point, and Young's modulus. However, adding too much SrO to the glass composition may increase the density and CTE of the glass composition to unacceptable levels and may undesirably hinder the ion-exchangeability of the glass. In embodiments, the glass compositions include SrO in an amount of from 0 mol% to 3 mol%, e.g., from 0.25 mol% to 2.5 mol%, from 0.5 mol% to 2 mol%, from 1 mol% to 1.5 mol%, and all ranges and subranges therebetween. In embodiments, the glass compositions are substantially free or free of SrO.
[0116] The glass compositions described herein may include ZnO. ZnO may reduce the liquidus viscosity of the glass, which may improve formability, strain point, and Young's modulus. However, adding too much ZnO to the glass composition may increase the density and CTE of the glass composition to unacceptable levels. The inclusion of ZnO in the glass composition also provides protection against UV-induced discoloration. In embodiments, the glass composition includes an amount of ZnO from 0 mol% to 5 mol%, e.g., from 0.5 mol% to 5 mol%, from 1 mol% to 4 mol%, from 2 mol% to 3 mol%, and all ranges and subranges therebetween. In embodiments, the glass composition is substantially free or free of ZnO.
[0117] The glass composition may include one or more fining agents. In embodiments, an example of a fining agent may include SnO2. In embodiments, SnO2 may be present in the glass composition in an amount of 0.2 mol% or less, such as from 0 mol% to 0.2 mol%, from 0 mol% to 0.1 mol%, from 0 mol% to 0.2 mol%, and all ranges and subranges therebetween. In some embodiments, the glass composition may be substantially free or free of SnO2. In embodiments, the glass composition may be substantially free of one or both of arsenic and antimony. In other embodiments, the glass composition may be free of one or both of arsenic and antimony.
[0118] In embodiments, the glass composition may include SnO2 in an amount from greater than or equal to 0.05 mol % to less than or equal to 0.5 mol %, e.g., from greater than or equal to 0.1 mol % to less than or equal to 0.45 mol %, from greater than or equal to 0.15 mol % to less than or equal to 0.40 mol %, from greater than or equal to 0.2 mol % to less than or equal to 0.35 mol %, from greater than or equal to 0.25 mol % to less than or equal to 0.3 mol %, and all ranges and subranges therebetween.
[0119] The glass compositions described herein may be formed primarily from SiO2, Al2O3, Li2O, Na2O, MgO, and ZrO2. In embodiments, the glass compositions are substantially free or free of components other than SiO2, Al2O3, Li2O, Na2O, MgO, ZrO2, P2O5, B2O3, and TiO2. In embodiments, the glass compositions are substantially free or free of components other than SiO2, Al2O3, Li2O, Na2O, MgO, ZrO2, P2O5, B2O3, TiO2, and fining agents.
[0120] In embodiments, the glass compositions may be substantially free or free of Fe2O3. Iron is often present in the raw materials utilized to form the glass compositions, and as a result, may be detectable in the glass compositions described herein even when not actively added to the glass batch.
[0121] In embodiments, the glass composition may be substantially free of, or free of, at least one of Ta2O5, HfO2, La2O3, and Y2O3. In embodiments, the glass composition may be substantially free of, or free of, Ta2O5, HfO2, La2O3, and Y2O3. These components, when included, may increase the fracture toughness of the glass, but there are cost and supply constraints that make these components undesirable for commercial purposes. Stated another way, the ability of the glass compositions described herein to achieve high fracture toughness values by including Ta2O5, HfO2, La2O3, and Y2O3 provides cost and manufacturability advantages.
[0122] The physical properties of the glass compositions disclosed above are now described.
[0123] Glass compositions according to embodiments have high fracture toughness. Without intending to be bound by any particular theory, high fracture toughness may provide glass compositions with improved drop performance. The high fracture toughness of the glass compositions described herein increases the damage resistance of the glass and allows the glass to be highly stressed by ion exchange without becoming brittle, as characterized by central tension. As used herein, fracture toughness is defined as the K value, as measured by the Chevron Notched Small Square Bar Method, unless otherwise specified. IC The value is called K IC The chevron notched small square bar (CNSB) method used to measure the Y * m is disclosed in Reddy, KPR et al., "Fracture Toughness Measurement of Glass and Ceramic Materials Using Chevron-Notched Specimens," J. Am. Ceram. Soc., 71 [6], C-310-C-313 (1988), except that it is calculated using Equation 5 in Bubsey, RT et al., "Closed-Form Expressions for Crack-Mouth Displacement and Stress Intensity Factors for Chevron-Notched Short Bar and Short Rod Specimens Based on Experimental Compliance Measurements," NASA Technical Memorandum 83796, pp. 1-30 (October 1992). IC The value is the K before the glass-based substrate is ion-exchanged to form the glass-based article. IC The K values mentioned here are measured on unstrengthened glass samples. IC Values are in MPa m unless otherwise stated 0.5 has been reported.
[0124] In an embodiment, the glass composition has a viscosity of 0.8 MPa m 0.5For example, 0.80 MPa m 0.5 More than 0.81MPa m 0.5 More than 0.82MPa m 0.5 More than 0.83MPa m 0.5 More than 0.84MPa m 0.5 More than 0.85MPa m 0.5 More than 0.86MPa m 0.5 More than 0.87MPa m 0.5 Above, 0.88MPa m 0.5 More than 0.89MPa m 0.5 More than 0.90MPa m 0.5 More than 0.91MPa m 0.5 More than 0.92MPa m 0.5 More than 0.93MPa m 0.5 More than 0.94MPa m 0.5 More than 0.95MPa m 0.5 Greater than or equal to K IC In one embodiment, the glass composition has a viscosity of 0.8 MPa m 0.5 Above 1.0MPa m 0.5 For example, 0.83 MPa m 0.5 Above 0.95MPa m 0.5 Below, 0.81MPa m 0.5 Above 0.99MPa m 0.5 Below, 0.82MPa m 0.5 Above 0.98MPa m 0.5 Below, 0.83MPa m 0.5 Above 0.97MPa m 0.5 Below, 0.84MPa m 0.5 Above 0.96MPa m 0.5 Below, 0.85MPa m 0.5 Above 0.95MPa m 0.5 Below, 0.86MPa m 0.5 Above 0.94MPa m 0.5 Below, 0.87MPa m 0.5 Above 0.93MPa m 0.5 Below, 0.88MPa m 0.5 Above 0.92MPa m 0.5 Below, 0.89MPa m 0.5Above 0.91MPa m 0.5 Below, 0.82MPa m 0.5 Above 0.90MPa m 0.5 All ranges and subranges between the following and preceding values of K IC Indicates the value.
[0125] Glass compositions according to embodiments have a high Young's modulus. High Young's modulus values reduce the stored strain energy present in the glass after ion exchange. As used herein, Young's modulus (E) refers to a value measured by a general type of resonant ultrasonic spectroscopy technique described in ASTM E2001-13, entitled "Standard Guide for Resonant Ultrasound Spectroscopy for Defect Detection in Both Metallic and Non-metallic Parts." In embodiments, the glass compositions have a Young's modulus of 80 GPa or more, e.g., 81 GPa or more, 82 GPa or more, 83 GPa or more, 84 GPa or more, 85 GPa or more, 86 GPa or more, 87 GPa or more, 88 GPa or more, 89 GPa or more, 90 GPa or more, 91 GPa or more, 92 GPa or more, 93 GPa or more, 94 GPa or more, 95 GPa or more, 96 GPa or more, 97 GPa or more, 98 GPa or more, or more. In embodiments, the glass composition has a Young's modulus of 80 GPa to 100 GPa, e.g., 83 GPa to 99 GPa, 81 GPa to 99 GPa, 82 GPa to 98 GPa, 83 GPa to 97 GPa, 84 GPa to 96 GPa, 85 GPa to 95 GPa, 86 GPa to 94 GPa, 87 GPa to 93 GPa, 88 GPa to 92 GPa, 89 GPa to 91 GPa, 90 GPa to 100 GPa, and all ranges and subranges therebetween.
[0126] The glass compositions described herein have liquidus viscosities compatible with manufacturing processes that are particularly suited for forming thin glass sheets. For example, the glass compositions are compatible with conventional forming methods such as float, rolling, or pressing. Glass-based substrate embodiments may be described as fusion formable (i.e., formable using a fusion draw process). The fusion process uses a draw vessel having a passageway for receiving molten raw glass material. The passageway has a weir on either side of the passageway that is open at the top along the length of the passageway. When the passageway is filled with molten material, the molten glass overflows the weir. The molten glass flows down the exterior surfaces of the draw vessel as two flowing glass films due to gravity. These exterior surfaces of the draw vessel extend downward and inward to meet at the lower edge of the draw vessel. The two flowing glass films meet at this edge and fuse to form a flowing glass-based article. The fusion of these glass films creates a fusion line in the glass-based substrate that can identify a fusion-formed glass-based substrate without the need for additional knowledge of its manufacturing history. The fusion draw process offers the advantage that, as the two glass films overflowing the passageway fuse together, none of the exterior surfaces of the resulting glass-based article come into contact with any part of the equipment. Thus, the surface properties of the glass-based article produced by the fusion draw process are not affected by such contact.
[0127] The glass compositions described herein may be selected to have a liquidus viscosity that is compatible with the fusion draw process. Thus, the glass compositions described herein are compatible with existing forming processes, increasing the manufacturability of glass-based articles formed from the glass compositions. As used herein, the term "liquidus viscosity" refers to the viscosity of molten glass at its liquidus temperature, where the liquidus temperature refers to the temperature at which crystals first appear as the molten glass cools from the melting temperature, or the temperature at which the last crystals melt away as the temperature is increased from room temperature. Unless otherwise specified, the liquidus viscosity values disclosed in this application are determined by the following method. First, the liquidus temperature of the glass is measured according to ASTM C829-81 (2015), entitled "Standard Practice for Measurement of Liquidus Temperature of Glass by the Gradient Furnace Method". The viscosity of the glass at its liquidus temperature is then measured according to ASTM C965-96 (2012), entitled "Standard Practice for Measuring Viscosity of Glass Above the Softening Point." Unless otherwise specified, the liquidus viscosity and temperature of a glass composition or article are measured before the composition or article is subjected to any ion exchange process or any other strengthening process. In particular, the liquidus viscosity and temperature of a glass composition or article are measured before the composition or article is exposed to, e.g., immersed in, an ion exchange solution.
[0128] In one or more embodiments, the glass compositions described herein may form glass-based articles that exhibit an amorphous microstructure and may be substantially free of crystals or crystallites. In other words, glass-based articles formed from the glass compositions described herein may exclude glass-ceramic materials.
[0129] As mentioned above, in embodiments, the glass compositions described herein can be strengthened, such as by ion exchange, to produce glass-based articles that are damage resistant for applications such as, but not limited to, display covers. Referring to FIG. 1, a glass-based article is shown having a first region under compressive stress (e.g., first and second compressive stress layers 120, 122 in FIG. 1) extending from the surface of the glass-based article to a depth of compression (DOC) and a second region under tensile stress or central tension (CT) (e.g., central region 130 in FIG. 1) extending from the DOC to a central or interior region of the glass-based article. As used herein, DOC refers to the depth at which stress within a glass-based article changes from compression to tension. At the DOC, the stress crosses from positive (compressive) stress to negative (tensile) stress, and therefore exhibits a stress value of zero.
[0130] According to common conventions in the art, compression or compressive stress is expressed as a negative (<0) stress, and tension or tensile stress is expressed as a positive (>0) stress. However, throughout this specification, CS is expressed as a positive or absolute value. That is, as set forth herein, CS=|CS|. Compressive stress (CS) has a maximum value at or near the surface of the glass-based article, and CS varies with distance d from the surface according to a function. Referring again to FIG. 1, a first section 120 extends from the first surface 110 to a depth d1, and a second section 122 extends from the second surface 112 to a depth d2. These sections together define the compression or CS of the glass-based article 100. Surface compressive stress (CS) may be measured using the Scattered Light Polariscope (SCALP) technique or the Refractive Near Field (RNF) technique known in the art. The CS values given herein are measured using the SCALP technique unless otherwise specified. As used herein, the term "CSk" refers to the compressive stress at the depth of the bend (ie, the transition point) as measured by RNF.
[0131] In embodiments, the CS of the glass-based article is from 400 MPa to 2000 MPa, e.g., from 500 MPa to 1900 MPa, from 600 MPa to 1800 MPa, from 700 MPa to 1700 MPa, from 800 MPa to 1300 MPa, from 900 MPa to 1200 MPa, from 1000 MPa to 1100 MPa, and all ranges and sub-ranges therebetween.
[0132] In an embodiment, Na + and K. + ions are exchanged into the glass-based article, + The ion is K + ions diffuse into glass-based articles to greater depths than K + The depth of penetration of ions ("potassium DOL") is distinct from the DOC because it represents the depth of potassium penetration as a result of the ion exchange process. The potassium DOL is typically smaller than the DOC for the glass articles described herein. The potassium DOL may be measured using a surface stress meter, such as the commercially available FSM-6000 surface stress meter manufactured by Orihara Seisakusho Co., Ltd. (Japan). This surface stress meter relies on precise measurements of the stress optical coefficient (SOC). The potassium DOL is calculated by measuring the depth of the compressive stress spike (DOL SP ), where the stress profile transitions from a steep spike region to a less steep deep region. The deep region extends from the base of the spike region to the compression depth. SP can be from 3 μm to 10 μm, for example, from 4 μm to 9 μm, from 5 μm to 8 μm, from 6 μm to 7 μm, and all ranges and subranges therebetween.
[0133] The compressive stresses on both major surfaces (110, 112 in FIG. 1) are balanced by a stored tension in the central region (130) of the glass-based article. The surface compressive stress (CS), maximum central tension (CT), and DOC may be measured using the scattered light polariscope (SCALP) technique, which is known in the art. The SCALP method may also be used to determine the stress profile of the glass-based article.
[0134] The measurement of maximum CT value is an indication of the total amount of stress stored in a reinforced article. For this reason, the ability to achieve higher CT values correlates to the ability to achieve higher degrees of reinforcement and improved performance. In embodiments, the glass-based article may have a maximum CT of 30 MPa or more to 300 MPa or less, e.g., 40 MPa or more to 290 MPa or less, 50 MPa or more to 280 MPa or less, 60 MPa or more to 270 MPa or less, 70 MPa or more to 260 MPa or less, 80 MPa or more to 250 MPa or less, 90 MPa or more to 240 MPa or less, 100 MPa or more to 230 MPa or less, 110 MPa or more to 220 MPa or less, 120 MPa or more to 210 MPa or less, 130 MPa or more to 200 MPa or less, 140 MPa or more to 190 MPa or less, 150 MPa or more to 180 MPa or less, 16 MPa or more to 170 MPa or less, and all ranges and sub-ranges therebetween.
[0135] The high fracture toughness values of the glass compositions described herein may also allow for improved performance. The brittleness limit of glass-based articles manufactured utilizing the glass compositions described herein depends at least in part on the fracture toughness. For this reason, the high fracture toughness of the glass compositions described herein allows the glass-based articles formed therefrom to have a large amount of stored strain energy without becoming brittle. The increased amount of stored strain energy that may be included in the glass-based article may then allow the glass-based article to exhibit increased fracture resistance, which may be observed through the drop performance of the glass-based article. The relationship between brittleness limit and fracture toughness is described in U.S. Patent Application Publication No. 2020 / 0079689A1, entitled "Glass-based Articles with Improved Fracture Resistance," published March 12, 2020, which is incorporated herein by reference in its entirety. The relationship between fracture toughness and drop performance is described in U.S. Patent Application Publication No. 2019 / 0369672 A1, entitled "Glass with Improved Drop Performance," published on December 5, 2019, which is incorporated herein by reference in its entirety.
[0136] As mentioned above, the DOC is measured using a scattered light polarimeter (SCALP) known in the art. The DOC is given herein as a fraction of the thickness (t) of the glass-based article in some embodiments. In embodiments, the glass-based article may have a depth of compression (DOC) of 0.15t or more to 0.25t or less, such as 0.16t or more to 0.24t or less, 0.17t or more to 0.23t or less, 0.18t or more to 0.22t or less, 0.19t or more to 0.20t or less, 0.15t or more to 0.21t or less, and all ranges and subranges therebetween. The high DOC values that result when the glass compositions described herein are ion-exchanged provide improved fracture resistance, especially for situations where deep scratches may be introduced. For example, a deep DOC improves fracture resistance when dropped onto a rough surface.
[0137] The thickness (t) of the glass-based article 100 is measured between the surface 110 and the surface 112. In embodiments, the thickness of the glass-based article 100 can be in the range of 0.1 mm to 4 mm, e.g., 0.2 mm to 2 mm, 0.2 mm to 3.5 mm, 0.3 mm to 3 mm, 0.4 mm to 2.5 mm, 0.5 mm to 2 mm, 0.6 mm to 1.5 mm, 0.7 mm to 1 mm, 0.2 mm to 2 mm, and all ranges and sub-ranges therebetween. The glass substrate utilized to form the glass-based article can have a thickness similar to that desired for the glass-based article.
[0138] The compressive stress layer may be formed in the glass by exposing the glass to an ion-exchange medium. In embodiments, the ion-exchange medium may be a molten salt bath, such as a bath containing molten nitrates. In embodiments, the ion-exchange medium may be a molten salt bath including KNO3, NaNO3, or combinations thereof. In embodiments, other sodium and potassium salts may be used in the ion-exchange medium, such as, for example, sodium or potassium nitrates, phosphates, or sulfates. In embodiments, the ion-exchange medium may include a lithium salt, such as LiNO3. The ion-exchange medium may additionally include additives commonly included when ion-exchanging glasses, such as silicic acid. The ion-exchange process is performed on the glass-based substrate to form a glass-based article that includes a compressive stress layer and a central tension region that extend from the surface to the compression depth of the glass-based article. The glass-based substrate utilized in the ion-exchange process may include any of the glass compositions described herein.
[0139] In an embodiment, the ion exchange medium includes NaNO3. The sodium in the ion exchange medium exchanges with lithium ions in the glass to create a compressive stress. In an embodiment, the ion exchange medium may include 95% or less by weight NaNO3, e.g., 90% or less, 80% or less, 70% or less, 60% or less, 50% or less, 40% or less, 30% or less, 20% or less, 10% or less, or less. In an embodiment, the ion exchange medium may include 5% or more by weight NaNO3, e.g., 10% or more, 20% or more, 30% or more, 40% or more, 50% or more, 60% or more, 70% or more, 80% or more, 90% or more, or more. In embodiments, the ion exchange medium may include NaNO3 in an amount of from 0 to 100% by weight, such as from 10 to 90%, from 20 to 80%, from 30 to 70%, from 40 to 60%, from 50 to 90%, and all ranges and subranges therebetween. In embodiments, the molten ion exchange bath includes 100% NaNO3 by weight.
[0140] In embodiments, the ion exchange medium comprises KNO3. In embodiments, the ion exchange medium may comprise 95% by weight or less, e.g., 90% by weight or less, 80% by weight or less, 70% by weight or less, 60% by weight or less, 50% by weight or less, 40% by weight or less, 30% by weight or less, 20% by weight or less, 10% by weight or less, or less than that. In embodiments, the ion exchange medium may comprise 5% by weight or more, e.g., 10% by weight or more, 20% by weight or more, 30% by weight or more, 40% by weight or more, 50% by weight or more, 60% by weight or more, 70% by weight or more, 80% by weight or more, 90% by weight or more, or more than that. In embodiments, the ion exchange medium may include KNO3 in an amount of from 0 to 100% by weight, such as from 10 to 90%, from 20 to 80%, from 30 to 70%, from 40 to 60%, from 50 to 90%, and all ranges and subranges therebetween. In embodiments, the molten ion exchange bath includes 100% KNO3 by weight.
[0141] The ion exchange medium may include a mixture of sodium and potassium. In embodiments, the ion exchange medium is a mixture of potassium and sodium, such as a molten salt bath containing both NaNO3 and KNO3. In embodiments, the ion exchange medium may include any combination of NaNO3 and KNO3 in the amounts described above, such as a molten salt bath containing 80% NaNO3 and 20% KNO3 by weight.
[0142] The glass composition may be exposed to an ion exchange medium by immersing a glass substrate made from the glass composition in a bath of the ion exchange medium, spraying the ion exchange medium onto a glass substrate made from the glass composition, or otherwise physically applying the ion exchange medium to a glass substrate made from the glass composition to form an ion exchanged glass-based article. The ion exchange medium may be at a temperature of from 400° C. to 550° C., e.g., from 410° C. to 540° C., from 420° C. to 530° C., from 430° C. to 520° C., from 440° C. to 510° C., from 450° C. to 500° C., from 460° C. to 490° C., from 470° C. to 480° C., and all ranges and subranges therebetween during exposure to the glass composition, according to embodiments. In embodiments, the glass composition may be exposed to the ion exchange solution for a period of from 0.5 hours to 48 hours, e.g., from 1 hour to 24 hours, from 2 hours to 12 hours, from 1 hour to 18 hours, from 2 hours to 16 hours, from 7 hours to 12 hours, and all ranges and subranges therebetween.
[0143] The ion exchange process may include a second ion exchange process. In embodiments, the second ion exchange process may include ion exchanging the glass-based article in a second molten salt bath. The second ion exchange process may utilize any of the ion exchange media described herein. In embodiments, the second ion exchange process utilizes a second molten salt bath including KNO3.
[0144] The ion exchange process may be carried out in an ion exchange medium under processing conditions that provide an improved compressive stress profile, such as those disclosed in U.S. Patent Application Publication No. 2016 / 0102011, which is incorporated herein by reference in its entirety. In some embodiments, the ion exchange process may be selected to produce a parabolic stress profile in the glass-based article, such as the stress profile described in U.S. Patent Application Publication No. 2016 / 0102014, which is incorporated herein by reference in its entirety.
[0145] It should be understood that after the ion-exchange process has been performed, the composition at the surface of the ion-exchanged glass-based article will differ from the composition of the as-formed glass substrate (i.e., the glass substrate before the ion-exchange process has been performed). + or K + Replaced by larger alkali metal ions such as Li + or Na + Such glass compositions may result from one type of alkali metal ion in the as-formed glass substrate, such as ion-exchanged glass, ion-exchanged glass, etc. However, the glass composition at or near the center of the depth of the glass-based article will, in embodiments, still have the composition of the as-formed, non-ion-exchanged glass substrate utilized to form the glass-based article. As used herein, the center of a glass-based article refers to any location in the glass-based article that is at least 0.5t away from all of its surfaces, where t is the thickness of the glass-based article.
[0146] The glass-based articles disclosed herein may be incorporated into another article, such as an article with a display (or display article) (e.g., consumer electronics including cell phones, tablets, computers, navigation systems, etc.), a building article, a transportation article (e.g., automobiles, trains, aircraft, ships, etc.), an appliance, or any article requiring some degree of transparency, scratch resistance, abrasion resistance, or a combination thereof. An exemplary article incorporating any of the glass-based articles disclosed herein is shown in Figures 2A and 2B. In particular, Figures 2A and 2B show a consumer electronics device 200 comprising a housing 202 having a front surface 204, a back surface 206, and a side surface 208; at least partially inside or completely within the housing, electrical components (not shown) including at least a controller, memory, and a display 210 at or adjacent to the front surface of the housing; and a cover 212 at or on the front surface of the housing to cover the display. In an embodiment, at least a portion of at least one of the cover 212 and the housing 202 may include any of the glass-based articles described herein. EXAMPLES
[0147] The embodiments will be further clarified by the following examples, which should be understood as not limiting the embodiments described above.
[0148] Glass compositions were prepared and analyzed. The analyzed glass compositions contained the components listed in Table I below and were prepared by conventional glass forming methods. In Table I, all components are expressed in mole percent and are K. ICFracture toughness was measured by the Chevron Notch (CNSB) method described herein. Liquidus temperature and liquidus viscosity were measured according to the methods described herein. Poisson's ratio (ν), Young's modulus (E), and shear modulus (G) of the glass compositions were measured by the general type of resonant ultrasonic spectroscopy technique described in ASTM E2001-13, entitled "Standard Guide for Resonant Ultrasound Spectroscopy for Defect Detection in Both Metallic and Non-metallic Parts". The refractive index and stress-optical coefficient (SOC) at 589.3 nm of the substrates are also reported in Table I. The refractive index was measured using a PerkinElmer 950 spectrometer. The SOC was measured according to procedure C (glass disk method) described in ASTM standard C770-16, entitled "Standard Test Method for Measurement of Glass Stress-Optical Coefficient". The density of the glass compositions was determined using the buoyancy method of ASTM C693-93 (2013).
[0149] Alternative fracture toughness K ICMeasurements of were performed on several specimens by the double cantilever beam (DCB) technique and are also reported in Table I. The geometry of the DCB specimens is shown in Figure 7, with the important parameters being the crack length a, the applied load P, the cross-sectional dimensions w and 2h, and the thickness b of the crack induction groove. The specimens were cut into rectangles with width 2h = 1.25 cm and thickness ranging from w = 0.3 mm to 1 mm, and the total length of the specimens varied from 5 cm to 10 cm, but this is not a critical dimension. Holes were drilled at both ends with a diamond drill to provide a means of attaching the specimen to a specimen holder and load. The crack "induction groove" was cut the length of the specimen on both flat sides using a wafer dicing saw equipped with a diamond blade, leaving a "web" of material approximately half the total thickness of the plate (dimension b in Figure 7) with a height of 180 μm, corresponding to the thickness of the blade. The high precision dimensional tolerances of the dicing saw allow for minimal variation between specimens. This dicing saw was also used to cut the initial crack with a = 15 mm. This final operation resulted in the formation of a very thin wedge of material near the crack tip (due to the curvature of the blade), making it easier for crack initiation within the sample. The sample was mounted in a metal sample holder with a steel wire in the hole at the bottom of the sample. The sample was supported at the opposite end to keep it horizontal under low load conditions. The top hole was hooked to a spring in series with a load cell (FUTEK, LSB200), which was then stretched and gradually loaded using a rope and precision slide. The crack was monitored using a microscope with a resolution of 5 μm attached to a digital camera and computer. The following equation:
[0150]
number
[0151] Using the applied stress intensity K PFor each specimen, a crack was first initiated at the leading edge of the web, and then the initiating crack was carefully grown subcritically until the dimension ratio a / h was greater than 1.5 in order to accurately calculate the stress intensity. At this point, the length of the crack, a, was measured and recorded using a moving microscope with a resolution of 5 μm. A drop of toluene was then placed in the crack groove and carried along the entire length of the groove by capillary forces, pinning the crack against movement until the fracture toughness was reached. The load was then increased until the specimen broke, and the critical stress intensity, K, was calculated from the fracture load and specimen dimensions. IC We calculated K P is the measurement method, K IC is equal to.
[0152] [Table 1-01]
[0153] [Table 1-02]
[0154] [Table 1-03]
[0155] [Table 1-04]
[0156] [Table 1-05]
[0157] [Table 1-06]
[0158] [Table 1-07]
[0159] [Table 1-08]
[0160] [Table 1-09]
[0161] [Table 1-10]
[0162] [Table 1-11]
[0163] [Table 1-12]
[0164] [Table 1-13]
[0165] [Table 1-14]
[0166] Substrates were formed from the compositions in Table I and subsequently ion-exchanged to form the exemplary articles. The ion-exchange involved immersing the substrate in a molten salt bath. The salt bath contained 100% NaNO3 by weight. In Table II, the length of the ion-exchange, the bath temperature, and the maximum central tension (CT) of the ion-exchanged articles are reported. The maximum central tension (CT) was measured according to the method described herein.
[0167] [Table 2]
[0168] Substrates were formed from the compositions in Table I and subsequently ion-exchanged to form the exemplary articles. The ion-exchange involved immersing the substrate in a molten salt bath. The salt bath contained 100% NaNO3 by weight and had a temperature of 450° C. In Table III, the length of the ion-exchange, the mass gain that occurred during the ion-exchange process, and the maximum central tension (CT), surface compressive stress (CS), and depth of compression (DOC) of the ion-exchanged articles are reported.
[0169] [Table 3]
[0170] Additional substrates were formed from the compositions of Table I and subsequently ion-exchanged to form exemplary articles. The ion-exchange involved immersing the substrate in a mixed molten salt bath. The salt bath included a mixture of NaNO3, KNO3, and LiNO3 at a temperature of 470° C. Table IV reports the length of the ion-exchange, the mass gain that occurred during the ion-exchange process, as well as the maximum central tension (CT), surface compressive stress (CS), and potassium depth of layer (DOL) of the ion-exchanged articles.
[0171] [Table 4-1]
[0172] [Table 4-2]
[0173] [Table 4-3]
[0174] [Table 4-4]
[0175] [Table 4-5]
[0176] Additional substrates were formed from exemplary glass composition 84 and comparative glass composition CA that underwent ion exchange under the conditions reported in Table V. Exemplary glass composition 84 was used to make three ion-exchanged glass articles BQ, BR, and BS, and comparative glass composition CA was used to make comparative ion-exchanged glass article CA, as reported in Table V. Comparative glass composition CA included 58.35 mol% SiO2, 17.81 mol% Al2O3, 6.07 mol% B2O3, 1.73 mol% Na2O, 0.20 mol% K2O, 10.74 mol% Li2O, 4.43 mol% MgO, 0.57 mol% CaO, and 0.08 mol% SnO2.
[0177] [Table 5]
[0178] Figure 3 shows the stress profiles of exemplary articles BQ, BR, and BS, and comparative article CA. Compressive stress was measured using the refractive near-field (RNF) technique.
[0179] Figures 4 and 5 show the residual strength of the articles. As shown in Figure 4, the exemplary BQ articles had failure loads ranging from 22.5 kgf (about 220 N) to 37.5 kgf (about 368 N), with an average failure load of 30 kgf (about 294 N), when the edge of the glass article was impacted with 60 grit abrasive paper at a force of 500 N. The exemplary BR articles had failure loads ranging from 25 kgf (about 245 N) to 32.5 kgf (about 319 N), with an average failure load of 30 kgf (about 294 N), when the edge of the glass article was impacted with 60 grit abrasive paper at a force of 500 N. The exemplary BS articles had failure loads ranging from 32.5 kgf (about 319 N) to 37.5 kgf (about 368 N), with an average failure load of 34 kgf (about 333 N), when the edge of the glass article was impacted with 60 grit abrasive paper at a force of 500 N. The comparative CA articles had failure loads ranging from 17.5 kgf (about 171 N) to 27.5 kgf (about 270 N), with an average failure load of 22 kgf (about 215 N), when the edge of the glass article was impacted with 60 grit abrasive paper at a force of 500 N.
[0180] As shown in Figure 5, the exemplary BQ article had a residual strength ranging from 275 MPa to 325 MPa, with an average residual strength of 300 MPa, when impacted with 180 grit abrasive paper at a force of 500 N, and a residual strength ranging from 125 MPa to 275 MPa, with an average residual strength of 227 MPa, when impacted with 80 grit abrasive paper at a force of 500 N. The exemplary BR article had a residual strength ranging from 275 MPa to 350 MPa, with an average residual strength of 322 MPa, when impacted with 180 grit abrasive paper at a force of 500 N, and a residual strength ranging from 200 MPa to 275 MPa, with an average residual strength of 256 MPa, when impacted with 80 grit abrasive paper at a force of 500 N. The exemplary BS articles had residual strengths ranging from 250 MPa to 350 MPa, with an average residual strength of 319 MPa, when impacted with 180 grit abrasive paper at a force of 500 N, and had residual strengths ranging from 200 MPa to 325 MPa, with an average residual strength of 262 MPa, when impacted with 80 grit abrasive paper at a force of 500 N. The comparative CA articles had residual strengths ranging from 250 MPa to 300 MPa, with an average residual strength of 274 MPa, when impacted with 180 grit abrasive paper at a force of 500 N, and had residual strengths ranging from 200 MPa to 250 MPa, with an average residual strength of 227 MPa, when impacted with 80 grit abrasive paper at a force of 500 N. As illustrated in Figures 4 and 5, ion-exchanged glass articles made from the glass compositions described herein have comparable or improved residual strengths compared to the comparative ion-exchanged glass articles.
[0181] All compositional components, relationships, and ratios described herein are given in mole percent unless otherwise specified. All ranges disclosed herein include any and all ranges and subranges encompassed by the broadly disclosed range, whether or not a range is expressly set forth before or after the disclosure.
[0182] It will be apparent to those skilled in the art that various modifications and variations can be made to the embodiments disclosed herein without departing from the spirit and scope of the claimed subject matter. Therefore, it is intended that this specification cover modifications and variations of the various embodiments described herein, provided such modifications and variations come within the scope of the appended claims and their equivalents.
[0183] Preferred embodiments of the present invention will be described below in detail.
[0184] EMBODIMENT 1 A glass, 45 mol% or more and 70 mol% or less of SiO2; 11.5 mol% or more and 25 mol% or less of Al2O3; 2 mol % or more and 20 mol % or less of Li2O, from greater than 0 mol % to 10 mol % or less of Na2O; 9 mol% or more and 19 mol% or less of MgO; greater than 0 mol% to 4 mol% or less ZrO2, and 0 mol% to 0.5 mol% TiO2, Including glass.
[0185] EMBODIMENT 2 A glass, 45 mol% or more and 70 mol% or less of SiO2; 4 mol% or more and 25 mol% or less of Al2O3, 5 mol % or more and 20 mol % or less of Li2O, 0.1 mol% or more and 10 mol% or less of Na2O, 6 mol % or more and 25 mol % or less of MgO; 0.1 mol% to 4 mol% ZrO2; 0.1 mol% or more and 5 mol% or less of K2O, and 0.05 mol % or more and 0.5 mol % or less of SnO2; Including glass.
[0186] EMBODIMENT 3 SiO2 from 51 mol% to 65 mol% 3. The glass of embodiment 1 or 2, comprising:
[0187] EMBODIMENT 4 12.0 mol% or more and 19 mol% or less of Al2O3; 4. The glass of any one of claims 1 to 3, comprising:
[0188] EMBODIMENT 5 3 mol % or more and 12 mol % or less of Li2O; 5. The glass of any one of the preceding claims, comprising:
[0189] EMBODIMENT 6 0.25 mol % or more and 6 mol % or less of Na2O, 6. The glass of any one of the preceding claims, comprising:
[0190] EMBODIMENT 7 10 mol % or more and 19 mol % or less of MgO; 7. The glass of any one of the preceding claims, comprising:
[0191] EMBODIMENT 8 0.25 mol% or more and 2 mol% or less of ZrO2; 8. The glass of any one of the preceding claims, comprising:
[0192] EMBODIMENT 9 9. The glass of any one of the preceding claims, wherein the glass is substantially free of TiO2.
[0193] EMBODIMENT 10 0 mol% to 10 mol% B2O3, 10. The glass of any one of the preceding claims, comprising:
[0194] EMBODIMENT 11 0 mol% to 6 mol% B2O3, 11. The glass of any one of the preceding claims, comprising:
[0195] EMBODIMENT 12 12. The glass of any one of the preceding claims, wherein the glass is substantially free of B2O3.
[0196] EMBODIMENT 13 0 mol% to 4 mol% P2O5, 13. The glass of any of the preceding claims, comprising:
[0197] EMBODIMENT 14 0 mol% to 3 mol% P2O5, 14. The glass of any one of the preceding claims, comprising:
[0198] EMBODIMENT 15 15. The glass of any one of the preceding claims, wherein the glass is substantially free of P2O5.
[0199] EMBODIMENT 16 0 mol% or more and 3 mol% or less of K2O, 15. The glass of any one of claims 1 or 3 to 14, comprising:
[0200] EMBODIMENT 17 The glass of any one of claims 1 or 3-15, wherein the glass is substantially free of KO.
[0201] EMBODIMENT 18 0 mol% or more and 3 mol% or less of CaO; 18. The glass of any of the preceding claims, comprising:
[0202] EMBODIMENT 19 19. The glass of any one of the preceding claims, wherein the glass is substantially free of CaO.
[0203] EMBODIMENT 20 0 mol % or more and 3 mol % or less of SrO; 20. The glass of any one of the preceding claims, comprising:
[0204] EMBODIMENT 21 21. The glass of any one of the preceding claims, wherein the glass is substantially free of SrO.
[0205] EMBODIMENT 22 0 mol % or more and 5 mol % or less of ZnO; 22. The glass of any of the preceding claims, comprising:
[0206] EMBODIMENT 23 23. The glass of any one of the preceding claims, wherein the glass is substantially free of ZnO.
[0207] EMBODIMENT 24 The glass has a viscosity of 0.8 MPa m 0.5 Above 1.0MPa·M 0.5 Fracture toughness K IC 24. The glass of any one of the preceding claims, having
[0208] EMBODIMENT 25 25. The glass of any one of the preceding claims, wherein the glass has a Young's modulus of 80 GPa or more and 100 GPa or less.
[0209] EMBODIMENT 26 In the method, ion exchanging the glass-based substrate in a molten salt bath to form a glass-based article; Including, 26. The method of claim 1, wherein the glass-based article comprises a compressive stress layer extending from a surface of the glass-based article to a compression depth, the glass-based article comprises a central tension region, and the glass-based substrate is made from the glass of any of claims 1 to 25.
[0210] EMBODIMENT 27 27. The method of embodiment 26, wherein the molten salt bath comprises NaNO.
[0211] EMBODIMENT 28 28. The method of embodiment 26 or 27, wherein the molten salt bath comprises KNO.
[0212] EMBODIMENT 29 29. The method of any of embodiments 26 to 28, wherein the molten salt bath is at a temperature of from 400° C. or more to 550° C. or less.
[0213] EMBODIMENT 30 30. The method of any of embodiments 26 to 29, wherein the ion exchange is for a period of from 0.5 hours to 48 hours.
[0214] EMBODIMENT 31 31. The method of any of claims 26 to 30, further comprising ion exchanging the glass-based article in a second molten salt bath.
[0215] EMBODIMENT 32 32. The method of embodiment 31, wherein the second molten salt bath comprises KNO.
[0216] EMBODIMENT 31 1. A glass-based article comprising: a compressive stress layer extending from the surface of the glass-based article to a compression depth; a central tension area, and 45 mol% or more and 70 mol% or less of SiO2; 11.5 mol% or more and 25 mol% or less of Al2O3; 2 mol % or more and 20 mol % or less of Li2O, from greater than 0 mol % to 10 mol % or less of Na2O; 9 mol% or more and 19 mol% or less of MgO; greater than 0 mol% to 4 mol% or less ZrO2, and 0 mol% to 0.5 mol% TiO2, A composition at the center of the glass-based article comprising: A glass-based article having the above structure.
[0217] EMBODIMENT 34 1. A glass-based article comprising: a compressive stress layer extending from the surface of the glass-based article to a compression depth; a central tension area, and 45 mol% or more and 70 mol% or less of SiO2; 4 mol% or more and 25 mol% or less of Al2O3, 5 mol % or more and 20 mol % or less of Li2O, 0.1 mol% or more and 10 mol% or less of Na2O, 6 mol % or more and 25 mol % or less of MgO; 0.1 mol% to 4 mol% ZrO2; 0.1 mol% or more and 5 mol% or less of K2O, and 0.05 mol % or more and 0.5 mol % or less of SnO2; A composition at the center of the glass-based article comprising: A glass-based article having the above structure.
[0218] EMBODIMENT 35 35. The glass-based article of claim 33 or 34, wherein the compressive stress layer has a compressive stress of from 400 MPa or more to 2000 MPa or less.
[0219] EMBODIMENT 36 36. The glass-based article of any of claims 33 to 35, wherein the central tension zone has a maximum central tension of 30 MPa or more and 300 MPa or less.
[0220] EMBODIMENT 37 37. The glass-based article of any of claims 33-36, wherein the compression depth is from 0.15t to 0.25t, inclusive, where t is a thickness of the glass-based article.
[0221] EMBODIMENT 38 38. The glass-based article of any of claims 33-37, wherein the compressive stress layer has a compressive stress spike extending from a surface of the glass-based article to a compressive stress spike depth, the compressive stress spike depth being from 3 μm or more to 10 μm or less.
[0222] EMBODIMENT 39 39. The glass-based article of any of claims 33 to 38, wherein the glass-based article has a thickness t of from 0.2 mm or more to 2 mm or less.
[0223] EMBODIMENT 40 The composition at the center of the glass-based article is SiO2 from 51 mol% to 65 mol% 40. The glass-based article of any of claims 33 to 39, comprising:
[0224] EMBODIMENT 41 The composition at the center of the glass-based article is 12.0 mol% or more and 19 mol% or less of Al2O3; 41. The glass-based article of any of claims 33 to 40, comprising:
[0225] EMBODIMENT 42 The composition at the center of the glass-based article is 3 mol % or more and 12 mol % or less of Li2O; 42. The glass-based article of any of claims 33 to 41, comprising:
[0226] EMBODIMENT 43 The composition at the center of the glass-based article is 0.25 mol % or more and 6 mol % or less of Na2O, 43. The glass-based article of any of claims 33 to 42, comprising:
[0227] EMBODIMENT 44 The composition at the center of the glass-based article is 10 mol % or more and 19 mol % or less of MgO; 44. The glass-based article of any of claims 33 to 43, comprising:
[0228] EMBODIMENT 45 The composition at the center of the glass-based article is 0.25 mol% or more and 2 mol% or less of ZrO2; 45. The glass-based article of any of claims 33 to 44, comprising:
[0229] EMBODIMENT 46 46. The glass-based article of any of claims 33 to 45, wherein the composition at the center of the glass-based article is substantially free of TiO2.
[0230] EMBODIMENT 47 The composition at the center of the glass-based article is 0 mol% to 10 mol% B2O3, 47. The glass-based article of any of claims 33 to 46, comprising:
[0231] EMBODIMENT 48 The composition at the center of the glass-based article is 0 mol% to 6 mol% B2O3, 48. The glass-based article of any of claims 33 to 47, comprising:
[0232] EMBODIMENT 49 49. The glass-based article of any of claims 33 to 48, wherein the composition at the center of the glass-based article is substantially free of B2O3.
[0233] EMBODIMENT 50 The composition at the center of the glass-based article is 0 mol% to 4 mol% P2O5, 50. The glass-based article of any of claims 33 to 49, comprising:
[0234] EMBODIMENT 51 The composition at the center of the glass-based article is 0 mol% to 3 mol% P2O5, 51. The glass-based article of any of claims 33 to 50, comprising:
[0235] EMBODIMENT 52 52. The glass-based article of any of claims 33 to 51, wherein the composition at the center of the glass-based article is substantially free of P2O5.
[0236] EMBODIMENT 53 The composition at the center of the glass-based article is 0 mol% or more and 3 mol% or less of K2O, 53. The glass-based article of any of claims 33 or 35 to 52, comprising:
[0237] EMBODIMENT 54 54. The glass-based article of any of claims 33 or 35-53, wherein the composition at the center of the glass-based article is substantially free of KO.
[0238] EMBODIMENT 55 The composition at the center of the glass-based article is 0 mol% or more and 3 mol% or less of CaO; 55. The glass-based article of any of claims 33 to 54, comprising:
[0239] EMBODIMENT 56 56. The glass-based article of any of claims 33 to 55, wherein the composition at the center of the glass-based article is substantially free of CaO.
[0240] EMBODIMENT 57 The composition at the center of the glass-based article is 0 mol % or more and 3 mol % or less of SrO; 57. The glass-based article of any of claims 33 to 56, comprising:
[0241] EMBODIMENT 58 58. The glass-based article of any of claims 33 to 57, wherein the composition at the center of the glass-based article is substantially free of SrO.
[0242] EMBODIMENT 59 The composition at the center of the glass-based article is 0 mol % or more and 5 mol % or less of ZnO; 59. The glass-based article of any of claims 33 to 58, comprising:
[0243] EMBODIMENT 60 60. The glass-based article of any of claims 33 to 59, wherein the composition at the center of the glass-based article is substantially free of ZnO.
[0244] EMBODIMENT 61 A glass having the same composition and microstructure as that at the center of the glass-based article is melted at 0.8 MPa m 0.5 Above 1.0MPa·M 0.5 Fracture toughness K IC 61. The glass-based article of any of claims 33 to 60, having
[0245] EMBODIMENT 62 62. The glass-based article of any of claims 33 to 61, wherein the glass having the same composition and microstructure as the composition at the center of the glass-based article has a Young's modulus of 80 GPa or more and 100 GPa or less.
[0246] EMBODIMENT 63 In consumer electronics, a housing having a front, a back, and sides; Electrical components disposed at least partially within said housing, the electrical components including at least a controller, a memory, and a display disposed on or adjacent a front surface of the housing; and a cover substrate disposed over the display; Equipped with 63. A consumer electronic product, wherein at least a portion of at least one of the housing and the cover substrate is made from the glass-based article of any of claims 33 to 62. [Explanation of symbols]
[0247] 100 Glass-based products 110 First Surface 112 Second Surface 120 First Section 122 Second Section 130 Central area 200 Household electronics 202 Case 204 Front 206 Back 208 Side 210 Display 212 Cover 1100 Apparatus for performing impact tests 1102 Pendulum 1104 Plumb 1106 Swivel shaft 1108 Arm 1110 Base 1140 Impact Object
Claims
1. A glass, 45 mol % to 70 mol % of SiO 2 , 4 mol % to 25 mol % Al 2 O 3 , 5 mol% to 20 mol% Li 2 O. 0.1 mol% to 10 mol% Na 2 O. 6 mol % or more and 25 mol % or less of MgO; 0.1 mol% to 4 mol% ZrO 2 , 0.1 mol % to 5 mol % K 2 O, and 0.05 mol % to 0.5 mol % SnO 2 , Including glass.
2. 51 mol % to 65 mol % of SiO 2 , The glass of claim 1 , comprising:
3. 12.0 mol% or more and 19 mol% or less of Al 2 O 3 , The glass of claim 1 or 2, comprising:
4. 3 mol% or more to 12 mol% or less of Li 2 O. The glass of claim 1 or 2, comprising:
5. 0.25 mol% to 6 mol% Na 2 O. The glass of claim 1 or 2, comprising:
6. 1. A glass-based article comprising: a compressive stress layer extending from the surface of the glass-based article to a compression depth; a central tension area, and 45 mol % to 70 mol % of SiO 2 , 4 mol % to 25 mol % Al 2 O 3 , 5 mol% to 20 mol% Li 2 O. 0.1 mol% to 10 mol% Na 2 O. 6 mol % or more and 25 mol % or less of MgO; 0.1 mol% to 4 mol% ZrO 2 , 0.1 mol % to 5 mol % K 2 O, and 0.05 mol % to 0.5 mol % SnO 2 , A composition at the center of the glass-based article comprising: A glass-based article having the following structure.
7. The glass-based article according to claim 6, wherein the compressive stress layer has a compressive stress of 400 MPa or more and 2000 MPa or less.
8. 8. The glass-based article of claim 6 or 7, wherein the central tension region has a maximum central tension of 30 MPa or more and 300 MPa or less.
9. 8. The glass-based article of claim 6 or 7, wherein the compression depth is from 0.15t to 0.25t, inclusive, where t is the thickness of the glass-based article.
10. 8. The glass-based article of claim 6 or 7, wherein the compressive stress layer has a compressive stress spike extending from a surface of the glass-based article to a compressive stress spike depth, the compressive stress spike depth being from 3 μm or more to 10 μm or less.