Stimuli-Responsive Block Copolymers

Stimuli-responsive block copolymers address the toxicity and administrative challenges of DMSO-based embolization systems by forming a gel in vivo, offering a biocompatible and easy-to-use solution for embolization and therapeutic applications.

JP2024540636AActive Publication Date: 2024-10-31BOSTON SCIENTIFIC SCIMED INC
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2024530459
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2021-11-23
Filing Date
2022-11-22
Publication Date
2024-10-31
Estimated Expiration
2042-11-22

AI Technical Summary

Technical Problem

Existing liquid embolization systems for neurological and peripheral diseases face limitations due to the toxicity of DMSO, which causes tissue necrosis and vasospasm, and require additional administrative procedures for informed consent due to a strong odor, while aqueous-based systems lack sufficient biocompatibility and ease of use.

Method used

Development of stimuli-responsive block copolymers comprising poly(N-isopropylaminoacrylamide) and poly(2-(di-(C1~5)alkylamino)(C1~5)alkyl methacrylate) blocks that form a gel in situ in response to pH and temperature changes, allowing for easy delivery and biocompatible embolization without DMSO.

Benefits of technology

The block copolymers provide a biocompatible and easy-to-use embolization solution that forms a gel in vivo, reducing toxicity and odor issues, and can be used for embolization, fiducial markers, tissue fillers, and therapeutic agent depots, with controlled release of therapeutic agents.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024540636000001_ABST
    Figure 2024540636000001_ABST
Patent Text Reader

Abstract

In various embodiments, the present disclosure relates to compositions for medical applications. In some embodiments, the compositions comprise one or more poly(N-isopropylaminoacrylamide) blocks and one or more poly(2-(di-(C 1~5 )Alkylamino)(C 1~5 In some embodiments, the composition is in liquid form at 25° C. Other embodiments relate to methods comprising delivering such a composition to a patient.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] This application claims the benefit of priority to U.S. Provisional Patent Application No. 63 / 282,349, filed November 23, 2021, the entire disclosure of which is incorporated herein by reference for all purposes.

[0002] The present disclosure relates to stimuli-responsive block copolymers, compositions containing such stimuli-responsive block copolymers, and methods of using such stimuli-responsive block copolymers. The stimuli-responsive block copolymers of the present disclosure are useful in a variety of biomedical applications, including, for example, embolization. [Background technology]

[0003] Liquid embolic systems are increasingly accepted as effective agents for embolization or filling of neurological and peripheral diseases such as hypervascular tumors, arteriovenous malformations, aneurysms, and endoleaks. DMSO solvent-based technologies used in commercial or developmental products such as Onyx® (Medtronic), Squidperi™ (Emboflu / Balt), PHIL™ (Terumo), and Easyx™ (Antia AG) are based on the change in solubility of the embolic polymer during the transition from the DMSO solvent to blood water. These have limitations due to the inherent toxicity of DMSO, which can cause tissue necrosis and vasospasm. The presence of DMSO in the formulation can also result in the patient noticing a strong odor similar to garlic after the procedure, which means that additional paperwork such as informed consent is required to make each patient aware of this potential side effect.

[0004] Aqueous-based systems have a lot of appeal to physicians and patients in this field because they eliminate DMSO. They also have the potential for greater biocompatibility and ease of use. This could also have potential for drug-loading applications, if desired, as well as benign embolization in a variety of indications.

[0005] Several notable aqueous-based products have undergone development and preclinical testing. For example, the polyelectrolyte GPX™ system (Fluidx Medical) uses electrostatically condensed, oppositely charged polyelectrolytes, polycationic salmine sulfate (Sal) and polyanion sodium inositol hexaphosphate (IP6), which are coacervates generated by charge interaction. A specific property of the polyelectrolyte complex is that the charge interactions between the polymer chains can be shielded by a high ionic strength NaCl solution (1200 mM), resulting in a clear, homogeneous, low viscosity fluid. Subsequent release of NaCl during in vivo delivery results in a sol-gel transition to a high viscosity coacervate. Tantalum powder is mixed with the formulation to provide the required radiopacity under a fluoroscope. Obsidio hydrogel is a novel bioengineered tantalum-loaded nanocomposite gel embolic material (Ta-GEM). The system is formulated by mixing gelatin (Type A, 18%), silicate nanoplatelets (Laponite XLG, 9%), ultrapure water and tantalum powder (2 μm, 20%, w / w). The disk-like Laponite nanoplatelets have negative charges on two faces, which can interact with the positively charged gelatin to form a composite gel structure. Other aqueous hydrogels that have been reported are PuraMatrix™, a polypeptide hydrogel, and SELP (Silk-elastin-like Protein Polymer, University of Utah), a temperature-sensitive system. Summary of the Invention

[0006] In various embodiments, the present disclosure relates to compositions for medical applications. The compositions include one or more poly(N-isopropylaminoacrylamide) blocks and one or more poly(2-(di-(C 1~5 )Alkylamino)(C 1~5 ) alkyl methacrylate) blocks, 1~5The alkyl groups are independently selected from methyl, ethyl, propyl, butyl, and pentyl groups. 1~5 Each of the alkyl groups is identical to the other.

[0007] In some embodiments, the composition comprises one or more poly(N-isopropylaminoacrylamide) blocks and one or more poly(2-(di-(C 1~5 ) alkylamino) ethyl methacrylate block, 1~5 The alkyl groups are independently selected from methyl, ethyl, propyl, butyl, and pentyl groups. 1~5 Each of the alkyl groups is identical to the other.

[0008] In various embodiments that may be used in conjunction with the above embodiments, one or more poly(2-(di-(C 1~5 )Alkylamino)(C 1~5 )alkyl methacrylate) block is poly(2-(di-(C 3~5 ) alkylamino) ethyl methacrylate) blocks, and more typically poly(2-(dibutylamino) ethyl methacrylate) blocks.

[0009] In various embodiments that can be used in conjunction with the above embodiments, the composition is in liquid form at 25°C. In various embodiments that can be used in conjunction with the above embodiments, the composition has a pH in the range of 1-7.4, typically in the range of 4.5-6.5, and more typically in the range of 5-6.

[0010] In various embodiments that can be used in conjunction with the above embodiments, the composition becomes a gel when injected into phosphate buffered saline having a pH of 7.4 and a temperature of 37° C. (e.g., at 20-25° C.).

[0011] In various embodiments that can be used in conjunction with the above embodiments, the composition becomes a gel when injected (e.g., at 20-25° C.) into the vascular system of a patient (e.g., a mammalian patient such as a human).

[0012] In various embodiments that can be used in conjunction with the above embodiments, the block copolymer comprises two poly(N-isopropylaminoacrylamide) blocks and one poly(2-(di-(C 1~5 )Alkylamino)(C 1~5 )alkyl methacrylate) blocks, more typically two poly(N-isopropylaminoacrylamide) blocks and one poly(2-(di-(C 3~5 It is a triblock copolymer having an alkylaminoethyl methacrylate block.

[0013] In various embodiments that can be used in conjunction with the above embodiments, the block copolymer comprises one poly(N-isopropylaminoacrylamide) block and two poly(2-(di-(C 1~5 )Alkylamino)(C 1~5 )alkyl methacrylate) block, more typically one poly(N-isopropylaminoacrylamide) block and two poly(2-(di-(C 3~5 It is a triblock copolymer having an alkylaminoethyl methacrylate block.

[0014] In various embodiments that can be used in conjunction with the above embodiments, each of the one or more poly(N-isopropylaminoacrylamide) blocks in the block copolymer ranges from 5 to 1000 monomer units in length, more typically from 100 to 600 monomer units in length.

[0015] In various embodiments that can be used in conjunction with the above embodiments, one or more poly(2-(di-(C 1~5 )Alkylamino)(C 1~5Each of the alkyl methacrylate blocks ranges from 10 to 500 units in length, more typically from 50 to 300 monomer units in length.

[0016] In various embodiments that can be used in conjunction with the above embodiments, the block copolymer has a number average molecular weight in the range of 2000 to 500,000 Da. In various embodiments that can be used in conjunction with the above embodiments, the block copolymer is present in the composition at a concentration ranging from 1 to 50% wt / wt, based on the weight of the composition.

[0017] In various embodiments that can be used in conjunction with the above embodiments, the composition has a viscosity in the range of 10 mPa·s to 5000 mPa·s when measured at a temperature of 25° C. and a shear rate of 50 1 / s.

[0018] In various embodiments that can be used in conjunction with the above embodiments, the block copolymer further comprises an additional polymer block ranging from 1 to 500 monomer units in length that comprises an amine group. For example, the amine group can be selected from aminoalkyl groups, alkylaminoalkyl groups, and dialkylaminoalkyl groups, among others.

[0019] In various embodiments that can be used in conjunction with the above embodiments, the composition, in addition to the block copolymer, further comprises an anionic polymer that includes negatively charged groups selected from sulfonate groups, sulfate groups, phosphate groups, phosphonate groups, and carboxylate groups, among others.

[0020] In various embodiments that can be used in conjunction with the above embodiments, the anionic polymer has a number average molecular weight in the range of 1000 to 5,000,000 Da. In various embodiments that can be used in conjunction with the above embodiments, the anionic polymer is present in an amount ranging from 0.1 to 50% wt / wt by weight of the composition.

[0021] In various embodiments that can be used in conjunction with the above embodiments, the anionic polymer is selected from sulfonate polymers, polyphosphates, poly(carboxylic acids), and negatively charged polysaccharides, among others.

[0022] In various embodiments that can be used in conjunction with the above embodiments, the composition further comprises an imaging agent. For example, the imaging agent can be a radiological contrast agent, which in some cases can include, for example, metallic particles.

[0023] In various embodiments that can be used in conjunction with the above embodiments, the composition further comprises an inorganic salt, such as sodium chloride or potassium chloride, among others. The inorganic salt may be present at a concentration ranging from 0.2M to 5.0M, more typically from 0.5M to 2.0M, among other possible values.

[0024] In various embodiments that can be used in conjunction with the above embodiments, the composition further comprises a therapeutic agent. In various embodiments that can be used in conjunction with the above embodiments, the composition is provided in a vial or syringe barrel.

[0025] In various embodiments, the present disclosure relates to a method comprising delivering to a patient a composition according to any of the above embodiments. In some embodiments, the method is a therapeutic method and the composition is delivered into the vascular system of a patient. For example, the therapeutic method can be selected from, among others, a method for treating a tumor, a method for treating an arteriovenous malformation, a method for treating an aneurysm, a method for treating an endoleak, a method for treating gastrointestinal bleeding, or a method for treating bleeding caused by disease or trauma.

[0026] In some embodiments, the methods include delivering the composition to the patient as a fiducial marker. In some embodiments, the method includes delivering a composition between a first tissue and a second tissue of the patient, thereby spacing the first tissue from the second tissue.

[0027] In various embodiments, the present disclosure relates to the use of the compositions of any of the above embodiments as, inter alia, an embolic agent, a fiducial marker, a tissue filler, a tissue spacer, or a therapeutic agent depot. [Brief description of the drawings]

[0028] [Figure 1] Schematic diagram of poly(N-isopropylaminoacrylamide)-poly(2-(dibutylamino)ethyl methacrylate)-poly(N-isopropylaminoacrylamide) triblock copolymer, also referred to herein as NIPAAM-DBA-NIPAAM triblock copolymer, pNIPAAM-pDBA-pNIPAAM triblock copolymer, or pNIPAAM-b-pDBA-b-pNIPAAM triblock copolymer. [Diagram 2] FIG. 1 is a schematic diagram of a NIPAAM-DBA-NIPAAM triblock copolymer with additional amino groups, according to one embodiment of the present disclosure. [Diagram 3] Schematic diagram of (a) phase changes during mixing of protonated triblock copolymer with poly(2-acrylamido-2-methylpropanesulfonate) (polyAMPS) to form a coacervate ( FIG. 3A ), (b) temperature increase to introduce NIPAAm aggregation ( FIG. 3B ), and (c) in vivo pH change causing partial deprotonation of DBA and enhanced gel hydrophobicity ( FIG. 3C ), according to one embodiment of the present disclosure. [Figure 4] Schematic diagram of the synthesis of pNIPAAM-b-pDBA-b-pNIPAAM triblock copolymer, according to one embodiment of the present disclosure. [Figure 5A] FIG. 1 shows proton NMR of a polymer after formation of the initial pNIPAAM block, according to one embodiment of the present disclosure. [Figure 5B] FIG. 1 shows proton NMR of the polymer after formation of the pNIPAAM-b-pDBA diblock copolymer, according to one embodiment of the present disclosure. [Figure 5C]FIG. 1 shows proton NMR of the polymer after formation of pNIPAAM-b-pDBA-b-pNIPAAMa triblock copolymer, according to one embodiment of the present disclosure. [Figure 5D] FIG. 1 shows proton NMR of pNIPAAM-b-pDBA-b-pNIPAAMa triblock copolymer after purification by dialysis against methanol (dialysis membrane MWCO 12000-14000 Da) according to one embodiment of the present disclosure. [Figure 6] An image of hydrogel formation after delivery into PBS (phosphate buffered saline) at 37° C., according to one embodiment of the present disclosure. [Figure 7] FIG. 14 shows storage and loss modulus versus temperature plots for several charge ratios between the pDBA block of pNIPAAM-b-pDBA-b-pNIPAAMa triblock copolymer and polyAMPS for the rheological properties of the polymer composites according to embodiments of the present disclosure. The solid symbols are the storage modulus (G') and the open symbols are the loss modulus (G''). [Figure 8] 1 is a plot of storage and loss modulus of various pNIPAAM-b-pDBA-b-pNIPAAMa triblock copolymer samples versus temperature gradient, according to embodiments of the present disclosure. Filled symbols are storage modulus (G') and open symbols are loss modulus (G''). [Figure 9] FIG. 13 shows the elastic modulus change induced by adding PBS and by increasing pH, according to one embodiment of the present disclosure. [Figure 10] 1 shows the elastic modulus change of NIPAAM-DEA-NIPAAM / polyAMPS composite gels (solid symbols) and NIPAAM-DBA-NIPAAM / polyAMPS composite gels (open symbols) according to embodiments of the present disclosure. Square symbols indicate storage modulus (G') and triangle symbols indicate loss modulus (G''). [Figure 11]FIG. 1 shows catheter delivery of NIPAAM-DBA-NIPAAM / PolyAMPS complex into a flow model (PBS medium, 37° C.) according to one embodiment of the present disclosure, in which a foam pad is held in place within a polymer tube by a spring that maintains the foam against the flow of PBS. [Figure 12] 12A-12C show embolization studies of NIPAAM-DBA-NIPAAM / polyAMPS complexes injected into a porcine kidney model. FIG. 12A corresponds to before embolization. FIG. 12B corresponds to after embolization. FIG. 12C corresponds to contrast injection after embolization. [Figure 13] 13A-13C show embolization studies of a reference composition injected into a porcine kidney model according to one embodiment of the present disclosure, where Fig. 13A corresponds to pre-embolization, Fig. 13B corresponds to post-embolization, and Fig. 13C corresponds to contrast injection after embolization. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0029] In various embodiments, the present disclosure provides a polymerizable composition comprising one or more poly(N-isopropylaminoacrylamide) blocks and one or more poly(2-(di-(C 1~5 )Alkylamino)(C 1~5 In a composition for medical use comprising a block copolymer comprising a) alkyl methacrylate) block, each C 1~5 The alkyl groups are independently selected from methyl, ethyl, propyl (where propyl includes n-propyl and isopropyl), butyl (where butyl includes n-butyl, isobutyl, sec-butyl and tert-butyl) and pentyl (where pentyl includes n-pentyl, tert-pentyl, neopentyl, isopentyl, sec-pentyl, 3-pentyl, sec-isopentyl, activated pentyl) groups. In various embodiments, the one or more poly(2-(di-(C 1~5 )Alkylamino)(C 1~5 )alkyl methacrylate) block is poly(2-(di-(C 1~5) alkylamino) ethyl methacrylate) blocks, and more typically poly(2-(dibutylamino) ethyl methacrylate) blocks.

[0030] Such compositions include liquid compositions suitable for injection into the body. The compositions of the present disclosure may be provided in a vial or syringe barrel. In some embodiments, the composition in the vial or syringe barrel may be a liquid composition, e.g., an aqueous liquid composition. In some embodiments, the composition in the vial or syringe barrel may be a dry composition to which a suitable fluid (e.g., water for injection, dextrose 5% in water (D5W), saline, buffer (e.g., phosphate buffered saline), etc.) may be added to form a liquid composition. In some embodiments, the vial or syringe may be stored under refrigerated conditions at a temperature ranging from 2 to 8°C. The compositions of the present disclosure may be provided in a sterile form.

[0031] In various embodiments, the compositions of the present disclosure are liquid compositions that form a gel material (also referred to herein as a hydrogel material or a solidified material) in situ upon injection into the body. Such liquid compositions include liquid compositions that can form a gel in response to in vivo conditions. In various embodiments, the liquid composition forms a gel in response to both a change in pH and a change in temperature.

[0032] In various embodiments, the compositions of the present disclosure are in liquid form at room temperature (e.g., below 25° C., or in some embodiments below 30° C.) and may have a pH below 7.0, typically in the range of 4.5 to 6.5, and more typically in the range of 5 to 6. After delivery to a patient's body (e.g., to in vivo conditions where the temperature is about 37° C. and the pH is about 7), the liquid composition spontaneously forms a gel.

[0033] Such liquid compositions can be used in a number of medical applications, including use as liquid embolic compositions, fiducial markers, tissue fillers, tissue spacers, and depots containing therapeutic agents from which the therapeutic agent elutes into the surrounding tissue.

[0034] In embodiments in which the liquid composition of the present disclosure is injected into the subject's body, the liquid composition can be adapted to pass through the particular delivery device used for injection, preferably with manual pressure. For example, a typical injection involves pushing the plunger with the thumb and stabilizing the side of the syringe barrel with the index and middle fingers of the same side, with an injection force of less than 50 N being preferred. The desired viscosity level will typically depend on the procedure and delivery method. For direct injection with a needle and syringe, the amount of pressure required will depend, for example, on the gauge of the needle. Similarly, for injection through a catheter, the amount of pressure required will depend, for example, on the inner diameter of the catheter.

[0035] In some embodiments, the liquid composition of the present disclosure has a viscosity in the range of 10 mPa·s or less to 5000 mPa·s or more when measured at a shear rate of 50 1 / s at a temperature of 25° C. For example, the composition may have a viscosity anywhere in the range of 10 mPa·s to 25 mPa·s to 50 mPa·s to 100 mPa·s to 250 mPa·s to 500 mPa·s to 1000 mPa·s to 2500 mPa·s to 5000 mPa·s at a shear rate of 50 1 / s and a temperature of 25° C.

[0036] As previously mentioned, the compositions of the present disclosure comprise one or more poly(N-isopropylaminoacrylamide) blocks and one or more poly(2-(di-(C 1~5 )Alkylamino)(C 1~5 )alkyl methacrylate) blocks, more typically one or more poly(N-isopropylaminoacrylamide) blocks and one or more poly(2-(di-(C 3~5 )alkylamino)ethyl methacrylate) blocks, for example, block copolymers comprising one or more poly(N-isopropylaminoacrylamide) blocks and one or more poly(2-(dibutylamino)ethyl methacrylate) blocks.

[0037] In some embodiments, each of the poly(N-isopropylaminoacrylamide) blocks is in the range of 5 monomer units or less to 1000 monomer units or more in length, such as 5 to 10 to 25 to 50 to 100 to 300 to 600 to 1000 monomer units in length (i.e., between any two of the above values). In certain beneficial embodiments, each of the poly(N-isopropylaminoacrylamide) blocks is greater than 100 monomer units in length and less than 600 monomer units in length.

[0038] In some embodiments, the one or more poly(2-(di-(C 1~5 )Alkylamino)(C 1~5 Each of the poly(2-(di-(C alkyl methacrylate)) blocks has a length ranging from 10 monomer units or less to 500 monomer units or more, for example, a length ranging from 10 to 25 to 50 to 75 to 100 to 200 to 250 to 300 to 500 monomer units. 1~5 )Alkylamino)(C 1~5 Each of the alkyl methacrylate blocks is greater than 50 monomer units in length and less than 300 monomer units in length.

[0039] In some embodiments, the number average molecular weight of the block copolymer is in the range of 2000 Da or less to 500,000 Da or more. For example, the number average molecular weight of the block copolymer may be in any range of 2000 Da to 5000 Da to 10,000 Da to 20,000 Da to 50,000 Da to 100,000 Da to 200,000 Da to 500,000 Da.

[0040] In some embodiments, the block copolymer is poly(2-(di-(C 1~5 )Alkylamino)(C 1~5 ) alkyl methacrylate) center block and two poly(N-isopropylaminoacrylamide) outer blocks.

[0041] In some embodiments, the block copolymer comprises a poly(N-isopropylaminoacrylamide) center block and two poly(2-(di-(C 1~5 )Alkylamino)(C 1~5 )alkyl methacrylate) outer blocks. Such triblock copolymers include poly(2-(di-(C 1~5 )Alkylamino)(C 1~5 The poly(2-(dibutylamino)ethyl methacrylate) block is a poly(2-(dibutylamino)ethyl methacrylate) block and is shown in FIG. 1, where l and n are integers. For example, l can be an integer in the range of 10 to 500, and n can be an integer in the range of 5 to 1000.

[0042] In some embodiments, the block copolymer further comprises an additional polymer block comprising an amine group, which may be formed from an amine-containing monomer. For example, the additional polymer block may comprise an aminoalkyl group (e.g., amino-C 1 ~C 4 -alkyl groups), alkylaminoalkyl groups (e.g., C 1 ~C 4 -Alkylamino-C 1 ~C 4 -alkyl groups), or dialkylaminoalkyl groups (e.g., di-C 1 ~C 4 -Alkyl-amino-(C 1 ~C 4-alkyl) groups), specific examples of which include aminomethyl, aminoethyl, aminopropyl, methylaminomethyl, dimethylaminomethyl, ethylaminomethyl, diethylaminomethyl, methylaminoethyl, dimethylaminoethyl, ethylaminoethyl, diethylaminoethyl, methylaminopropyl, dimethylaminopropyl, ethylaminopropyl, or diethylaminopropyl groups. In some embodiments, the additional polymer blocks range in length from 1 to 500 or more monomer units, for example, from 1 to 2 to 5 to 10 to 20 to 50 to 100 to 200 to 500 monomer units in length. An example of such a block copolymer is shown in FIG. 2, where the amine-containing monomer is 2-aminoethyl methacrylate. Such monomers may provide additional functional groups for subsequent linkage with molecules (e.g., thrombin peptides), among other purposes. During synthesis of the block copolymer by the RAFT technique illustrated in FIG. 2, the amino group in 2-aminoethyl methacrylate may be protected to avoid interference with chain transfer agents by using common protecting groups. Typical protecting groups include, among others, 9-fluorenylmethyl carbamate, t-butyl carbamate, benzyl carbamate, acetamide, and trifluoroacetamide. After polymerization, the protecting groups are deprotected accordingly.

[0043] In some embodiments, the block copolymer is present in a concentration ranging from 1% wt / wt or less to 50% wt / wt or more by weight of the composition, which may be a liquid composition, such as an aqueous liquid composition, for example. For example, the block copolymer may be present in the composition in a concentration ranging from 1% wt / wt to 2% wt / wt to 5% wt / wt to 10% wt / wt to 20% wt / wt to 30% wt / wt to 40% wt / wt to 50% wt / wt.

[0044] In some embodiments, the compositions of the present disclosure further comprise at least one anionic polymer comprising one or more groups selected from sulfonate, sulfate, phosphate, phosphonate, or carboxylate groups, which are negatively charged at pH 7, preferably negatively charged at a pH greater than 4 or 5, and in some cases negatively charged at a pH greater than 2. Such anionic polymers may be combined / mixed with the block copolymer to further tailor the properties of the gel compositions described herein, including gel strength, flexibility, cohesiveness, flowability, and / or gel stability, among other properties. Particular examples of anionic polymers include sulfonate polymers, such as poly(2-acrylamido-2-methylpropanesulfonate) (polyAMPS) or polystyrenesulfonate, polyphosphates, poly(carboxylic acids), such as poly(acrylic acid) or poly(methacrylic acid), negatively charged polysaccharides, including alginates, hyaluronates, pectins, carrageenans, gellan gum, gum arabic, guar gum or xanthan gum. The anionic polymers may be provided in salt form, such as, inter alia, sodium or potassium salt form. In some embodiments, the anionic polymer may have a number average molecular weight in the range of 1,000 Da to 5,000,000 Da, for example, any range of 1,000 Da to 2,000 Da to 5,000 Da to 10,000 Da to 20,000 Da to 50,000 Da to 100,000 Da to 200,000 Da to 500,000 Da to 1,000,000 Da to 2,000,000 Da to 5,000,000 Da.

[0045] In some embodiments, the at least one anionic polymer is present in an amount ranging from 0.1% wt / wt or less to 50% wt / wt or more by weight of the composition, which may be a liquid composition, such as an aqueous liquid composition, for example, the at least one anionic polymer may be present in an amount ranging from 0.1% wt / wt to 0.2% wt / wt to 0.5% wt / wt to 1% wt / wt to 2% wt / wt to 5% wt / wt to 10% wt / wt to 20% wt / wt to 30% wt / wt to 40% wt / wt to 50% wt / wt by weight of the composition.

[0046] In some embodiments, the molar ratio of positively charged amino groups in the DBA block (assuming 100% ionization) to negatively charged groups in the anionic polymer (assuming 100% ionization) ranges from 0.1:1 to 10:1, typically from 0.5:1 to 2:1, more typically from 1:1 to 1:1.5.

[0047] In some embodiments, the composition may further comprise at least one imaging agent.Examples of imaging agents include radio contrast agents, imageable radioisotopes, fluorescent dyes, magnetic resonance imaging (MRI) contrast agents, ultrasound contrast agents and near infrared (NIR) imaging contrast agents.Specific examples of radio contrast agents include metal particles, such as tantalum, tungsten, rhenium, niobium, molybdenum and their alloy particles, and the metal particles can be spherical or non-spherical. Specific examples of radiocontrast agents further include non-ionic radiocontrast agents (e.g., iohexol, iodixanol, ioversol, iopamidol, ioxilan, or iopromide), ionic radiocontrast agents (e.g., diatrizoate, iothalamate, metrizoate, or ioxaglate), and iodized oils, including ethiodized poppyseed oil (available as Lipiodol®). Further specific examples of imaging agents include (a) fluorescent dyes, such as fluorescein, indocyanine green, or fluorescent proteins (e.g., green, blue, cyan fluorescent proteins), (b) Gd (III) , Mn (II) , Fe (III)(c) contrast agents for use with ultrasound imaging, including organic and inorganic echogenic particles (i.e., particles that result in an increase in reflected ultrasound energy) or organic and inorganic echotransparent particles (i.e., particles that result in a decrease in reflected ultrasound energy); (d) contrast agents for use with magnetic resonance imaging (MRI), including contrast agents containing elements that form paramagnetic ions such as gadolinium ion chelated with diethylenetriaminepentaacetic acid; (e) contrast agents for use with ultrasound imaging, including organic and inorganic echogenic particles (i.e., particles that result in an increase in reflected ultrasound energy) or organic and inorganic echotransparent particles (i.e., particles that result in a decrease in reflected ultrasound energy); (f) contrast agents for use with deep tissue imaging and device imaging, including contrast agents containing elements that form paramagnetic ions such as gadolinium ion chelated with diethylenetriaminepentaacetic acid; Contrast agents for use with near infrared (NIR) imaging that enable isotopic marking, such as, inter alia, gold nanoshells, NIR-sensitive nanoparticles such as carbon nanotubes (e.g., nanotubes derivatized with hydroxyl or carboxyl groups, e.g., partially oxidized carbon nanotubes), dye-containing nanoparticles such as dye-doped nanofibers and dye-encapsulated nanoparticles, and semiconductor quantum dots, and NIR-sensitive dyes such as cyanine dyes, squaraines, phthalocyanines, porphyrin derivatives, and boron dipyrromethane (BODIPY) analogs, inter alia, and (e) inter alia, 99m Tc, 201 Th, 51 Cr, 67 Ga, 68 Ga, 111 In, 64 Cu, 89 Zr, 59 Fe, 42 K, 82 Rb, 24 Na, 45 Ti, 44 Sc, 51 Cr and 177 Imaging radioisotopes include Lu.

[0048] In some embodiments, the at least one imaging agent is present in an amount ranging from 1% wt / wt or less to 50% wt / wt or more by weight of the composition, which may be a liquid composition, such as an aqueous liquid composition, for example, the at least one imaging agent may be present in the composition at a concentration ranging from 1% wt / wt to 2% wt / wt to 5% wt / wt to 10% wt / wt to 20% wt / wt to 30% wt / wt to 40% wt / wt to 50% wt / wt.

[0049] In some embodiments, the composition may further comprise one or more therapeutic agents. Examples of therapeutic agents include small molecule therapeutic agents (defined herein as therapeutic agents having a molecular weight of less than 2000 g / mol, typically less than 1500 g / mol, more typically less than 1000 g / mol), biomolecules (e.g., polypeptides, including proteins and protein fragments, such as antibodies and antibody fragments and oligopeptides, and polynucleotides and oligonucleotides, including nucleic acids and nucleic acid analogs, such as deoxyribonucleic acid, ribonucleic acid, peptide nucleic acid, and fragments thereof), and radioisotopes.

[0050] In some embodiments, the one or more therapeutic agents are present in an amount ranging from 0.001% wt / wt (10 ppm) or less to 80% wt / wt or more by weight of the composition, which may be a liquid composition, such as an aqueous liquid composition. For example, the one or more therapeutic agents may be present in the composition at a concentration ranging from 0.001% wt / wt to 0.002% wt / wt to 0.005% wt / wt to 0.01% wt / wt to 0.02% wt / wt to 0.05% wt / wt to 0.1% wt / wt to 0.2% wt / wt to 0.5% wt / wt to 1% wt / wt to 2% wt / wt to 5% wt / wt to 10% wt / wt to 20% wt / wt to 50% wt / wt to 80% wt / wt.

[0051] Specific examples of therapeutic agents include, inter alia, anti-angiogenic agents, cytotoxic agents, chemotherapeutic agents, checkpoint inhibitors, immunomodulatory cytokines, T cell agonists, and STING (stimulator of interferon genes) agonists.

[0052] Examples of therapeutic agents include, among others, checkpoint inhibitors including inhibitors of PD-1 binding to PD-L1, inhibitors of CTLA-4 binding to CD80 and / or CD86, inhibitors of TIGIT binding to CD-112, and inhibitors of LAG-3 binding to MHC class II molecules; inhibitors of PD-1 (e.g., pembrolizumab, nivolumab dombanalimab, etc.), PD-L1 (e.g., atezolizumab, avelumab, durvalumab, etc.), LAG-3 (e.g., leratlimab, etc.), TIM- Antibodies or antigen-binding fragments thereof that bind to CD3, CD19, CD20, CD22, CD52, CD79B, CD30, CD33, CD38, CD52, CD79B, HER2, EGFR, VEGF, VEGFR2, EPCAM / CD3, GD2, IL-6, RANKL, Antibodies or antigen-binding fragments thereof that bind to SLAMF7, CCR4, PDGFRα, Nectin-4 or TROP2; immunomodulatory cytokines such as IL-2, IL-12, IL-15, IL-23, interferon gamma (IFN-γ) and gm-CSF (granulocyte colony-stimulating factor); TLR3 agonists (e.g., polyinosinic acid:polycytidylic acid, double-stranded RNA, etc.), TLR7 agonists (e.g., TMX-202, Guardiquimod, Imiquimod, etc.), TLR8 agonists (e.g., Examples of such agonists include T cell agonists such as VTX-2337, TLR7 / 8 agonists (e.g., MEDI9197, R848, resiquimod, etc.), TLR9 agonists (e.g., lefitolimod (MGN1703), tilsotolimod, CpG oligodeoxynucleotides (e.g., agatolimod), etc.); and STING agonists such as GSK532, cyclic dinucleotides (e.g., cyclic guanosine monophosphate adenosine monophosphate), CRD5500 (LB-061), E7766, ADU-S100, SB11285 MSA2, MK1454, TTI-10001.

[0053] Exemplary therapeutic agents also include camptothecins (e.g., irinotecan, topotecan, and exatecan) and anthracyclines (e.g., doxorubicin, daunorubicin, idarubicin, and epirubicin), antiangiogenic agents (e.g., vascular endothelial growth factor receptor (VEGFR) inhibitors (e.g., axitinib, bortezomib, bosutinib, canertinib, dovitinib, dasatinib, erlotinib, gefitinib, imatinib, lapatinib, lestaurine, serotoninib ... tinib, mastinib, muvitinib, pazopanib, pazopanib semaxanib, sorafenib, sunitinib, tandutinib, vandetanib, vatalanib, and vismodegib), microtubule assembly inhibitors (e.g., vinblastine, vinorelbine, and vincristine), aromatase inhibitors (e.g., anastrazole), platinum drugs (e.g., cisplatin, oxaliplatin, carboplatin, and miriplatin), nucleoside analogues (e.g., 5-F U, cytarabine, fludarabine and gemcitabine), paclitaxel, docetaxel, mitomycin C, mitoxantrone, bleomycin, pinyagumycin, abiraterone, amifostine, buserelin, degarelix, folinic acid, goserelin, lanreotide, lenalidomide, letrozole, leuprolide, octreotide, tamoxifen, triptorelin, bendamustine, chlorambucil, dacarbazine, melphalin, procarbazine temozolomide, rapamycin (and analogs such as zotarolimus, everonib, umirolimus, sirolimus, etc.), antimetabolites (e.g., 5-fluorouracil), multi-tyrosine kinase inhibitors (e.g., sorafenib, sunitinib, regorafenib, brivanib, dasatinib, bosutinib, erlotinib, gefitinib, imatinib, and vandetinib), methotrexate, pemetrexed, or raltitrexed.

[0054] Therapeutic radioisotopes include: 177 Lu, 90 Y, 131 I, 89 Sr, 153 Sm, 223 Ra, 224 Ra, 211 At,225 Ac, 227 Th, 212 Bi, 213 Bi, and / or 212 These include, but are not limited to, Pb.

[0055] In some embodiments, the compositions described herein may include therapeutic agents that are charged and / or uncharged at physiological pH. Charged therapeutic agents may be electrostatically held within a gel composition and subsequently released therefrom by ion exchange mechanisms (e.g., when the composition further comprises an anionic polymer that includes one or more negatively charged groups selected from sulfonate, sulfate, phosphate, phosphonate, or carboxylate groups). Charged therapeutic agents electrostatically held in the gel composition may elute from the gel composition in an electrolyte medium (e.g., saline (0.90% w / v NaCl)) or in vivo (e.g., in blood or tissue) to provide sustained release of the therapeutic agent over hours, days, or even weeks. Uncharged therapeutic agents in the gel composition may also elute from the gel composition in vivo. This may be particularly advantageous, for example, when rapid elution or a "burst effect" is desired, for example, for rapid delivery of the therapeutic agent to tissues, or when the low solubility of the therapeutic agent under physiological conditions determines the release profile rather than ionic interactions.

[0056] Embodiments of the present disclosure also relate to medical compositions corresponding to or formed from the liquid compositions of any of the preceding embodiments, For example, as previously described, such liquid compositions may be used for embolization, fiducial markers, tissue fillers, tissue spacers, and in vivo formation of therapeutic agent depots.

[0057] Some embodiments of the present disclosure further relate to medical treatment using the liquid composition described herein.For example, in some embodiments, the medical treatment is a method of tissue embolization, comprising delivering said liquid composition into one or more blood vessels that supply nutrients to tissue.Such treatment can be used to treat various conditions, including treating arteriovenous malformation, treating gastrointestinal bleeding, treating endoleaks, filling aneurysms, treating bleeding caused by disease or trauma, treating solid tumors (especially hypervascular tumors such as liver, prostate, kidney, brain, colon, bone and lung tumors), and treating benign hyperplasia conditions (e.g., treating prostatic hyperplasia or treating uterine fibroids).

[0058] In some embodiments, the medical procedure is a method of local or systemic therapeutic release that includes delivering (e.g., by injection, spraying, etc.) a liquid composition described herein to a patient (e.g., onto, within, between a patient's tissue, etc.).

[0059] In some embodiments, the medical procedure is a therapeutic method comprising delivering (e.g., by injection, spraying, etc.) a liquid composition described herein into or onto a tumor of a patient, where the therapeutic agent is released into the tumor.

[0060] In some embodiments, the medical procedure is a method of spacing a first tissue from a second tissue, comprising delivering (e.g., injecting, etc.) a liquid composition described herein between the first tissue and the second tissue (e.g., between a prostate tissue and a rectal tissue).

[0061] In some embodiments, the medical procedure is a therapeutic method comprising delivering (eg, by injection, spraying, etc.) a liquid composition described herein into a patient as a fiducial marker.

[0062] In still further embodiments, the present disclosure relates to the use of the liquid compositions described herein in the manufacture of medicaments for the treatment of various diseases and conditions, including the treatment of arteriovenous malformations, the treatment of gastrointestinal bleeding, the filling of aneurysms, the treatment of solid tumors (particularly hypervascular tumors such as tumors of the liver, prostate, kidney, brain, colon, bone, and lung), and the treatment of benign hyperplastic conditions such as prostatic hyperplasia or uterine fibroids.

[0063] The present disclosure also relates to the use of any of the therapeutic agents described herein in the manufacture of a medicament for the treatment of such diseases and conditions, where the therapeutic agent is incorporated into a liquid or gel composition described herein. The present disclosure also relates to the use of any of the therapeutic agents herein in the treatment of such diseases and conditions, where the therapeutic agent is incorporated into a liquid or gel composition described herein. The liquid compositions may be used, particularly when the liquid compositions are delivered by a transcatheter route, by injection, by implantation, by spraying, etc.

[0064] The foregoing embodiments may include one or more poly(N-isopropylaminoacrylamide) blocks and one or more poly(2-(di-(C 1~5 )Alkylamino)(C 1~5 However, in any of the embodiments described herein, the one or more poly(2-(di-(C 1~5 )Alkylamino)(C 1~5It should be understood that instead of the poly(N,N-dimethylaminoethyl methacrylate) block, any of the following blocks may be used: one or more poly(N,N-diethylaminoethyl methacrylate) blocks, one or more poly(2-(tetramethyleneimino)ethyl methacrylate) blocks, one or more poly(2-(pentamethyleneimino)ethyl methacrylate) blocks, one or more poly(2-(hex ... (2-(piperidino)ethyl methacrylate)) block, one or more poly(dioctylaminoethyl acrylate) blocks, one or more poly(piperidylethyl acrylate) blocks, one or more poly(N,N-dimethylaminoethyl acrylate) blocks, one or more poly(N,N-diethylaminoethyl methacrylate) blocks, one or more poly(N,N-diisopropylaminoethyl acrylate) blocks, one or more poly(N,N-di(n-butyl)-aminoethyl acrylate) blocks, one or more poly(2-(tetramethylene iodo)ethyl acrylate) blocks, one or more poly(2-(pentamethyleneimino)ethyl acrylate) blocks, one or more poly(2-(hexamethyleneimino)ethyl acrylate) blocks, one or more poly(N,N-dimethylaminoethyl methacrylamide) blocks, one or more poly(N,N-diethylaminoethyl methacrylamide) blocks, one or more poly(N,N-diisopropylaminoethyl methacrylamide) blocks, one or more poly(N,N-di(n-butyl)aminoethyl methacrylamide) blocks, one or more poly(N,N-dimethylaminoethyl methacrylamide) blocks, (2-(tetramethyleneimino)ethyl methacrylamide) blocks, one or more poly(2-(pentamethyleneimino)ethyl methacrylamide) blocks, one or more poly(2-(hexamethyleneimino)ethyl methacrylamide) blocks, one or more poly(2-(piperidino)ethyl methacrylamide) blocks, one or more poly(dioctylaminoethyl acrylamide) blocks, one or more poly(piperidylethyl acrylamide) blocks, one or more poly(N,N-dimethylaminoethyl acrylamide) blocks, one or more poly(N,N-diethylaminoethylacrylamide) blocks, one or more poly(N,N-diisopropylaminoethylacrylamide) blocks, one or more poly(N,N-di(n-butyl)-aminoethylacrylamide) blocks, one or more poly(2-(tetramethyleneimino)ethylacrylamide) blocks, one or more poly(2-(pentamethyleneimino)ethylacrylamide) blocks, or one or more poly(2-(hexamethyleneimino)ethylacrylamide) blocks.

[0065] experiment A specific example is presented here for an ABA triblock copolymer composition, where the ABA triblock copolymer comprises a pH-responsive central poly(2-(dibutylamino)ethyl methacrylate) block and two thermo-responsive poly(N-isopropylaminoacrylamide) end blocks (see Figure 1). The ABA triblock copolymer was synthesized by using RAFT (reversible addition-fragmentation chain transfer radical polymerization) technique starting with the polymerization of N-isopropylacrylamide (NIPAAM) initiated by 4,4'-azobis(4-cyanovaleric acid) (ACVA) and the chain transfer agent 4-((((2-carboxyethyl)thio)carbonothioyl)thio)-4-cyanopentanoic acid (CETCPA). After the first block was synthesized, the DBA block was polymerized using protonated 2-(dibutylamino)ethyl methacrylate monomer (DBA), followed by copolymerization of the third block of NIPAAM (see Figure 4). Methanol was used as the reaction solvent.

[0066] Without being bound by theory, it is believed that the resulting solution of NIPAAM-DBA-NIPAAM copolymer forms a hydrogel that is physically crosslinked by hydrophobic interactions at physiological conditions, pH 7 and 37 °C. In this regard, at ambient temperature (20-25 °C) and pH 5-6, the resulting aqueous solution of NIPAAM-DBA-NIPAAM copolymer is in a free-flowing liquid form since both the NIPAAM and DBA blocks are water soluble. When mixed with polyAMPS, the positively charged amine groups of the DBA block complex with the negatively charged sulfonate groups of polyAMPS to generate a coacervate viscous liquid phase (schematically shown in Figure 3A). This viscous liquid is relatively easily deliverable through a 2.7-2.8 Fr catheter using a 1 mL or 3 mL syringe. During catheter delivery, the temperature of the blood vessel in which the catheter is located is approximately 37 °C, and as a result, the temperature of the complex liquid increases to approximately 30-37 °C. A sol-gel transition of the NIPAAm block occurs due to the increased hydrophobicity of the NIPAAm at higher temperatures, and a physically crosslinked "flowable" hydrogel structure composed of mixed micelles and complexes is formed (schematically shown in Figure 3B). The micelle core is the NIPAAm, and the corona portion is balanced by the hydrophilic, protonated DBA block that interacts with polyAMPS. When this gel is then placed in a physiological solution at pH 7-7.4 (e.g., within the vasculature), partial DBA deprotonation occurs, as DBA has a pKa=5. The hydrogel structure is further enhanced by the increased hydrophobicity of the DBA block, and the hydrogel strength and viscosity are significantly increased (schematically shown in Figure 3C).

[0067] Example 1. pNIPAAM 300 Synthesis of CETCPA (0.0272 g, 0.09 mmol), NIPAAM (3 g, 26.51 mmol, NIPAAM / CPATTC molar ratio = 300), and ACVA (5 mg, 0.02 mmol, ACVA / CETCPA molar ratio = 0.2) were added to a round-bottom flask (RBF) and dissolved in 3 mL of methanol. The RBF was sealed with a rubber stopper and the reaction mixture was quenched with N 2 The degassing step was carried out by pumping N into the reaction mixture using a short needle (on the stopper, as an outlet) and a long needle (as an inlet) while keeping the RBF under constant stirring in an ice bath. 2 After degassing, the RBF was placed in a preheated oil bath at 70 °C and the reaction was allowed to proceed for 24 h under constant magnetic stirring. The reaction was stopped by opening the RBF to air and placing the RBF in an ice bath. An aliquot (50 μL) of the reaction mixture was 1 A sample was taken for H NMR analysis (see FIG. 5A). No purification was performed. Proton NMR analysis of the mixture indicated that >98% of the NIPAAM monomer had reacted.

[0068] Example 2. pNIPAAM 300 -pDBA 100 Synthesis of 2-(Dibutylamino)ethyl methacrylate (DBA) (2.13 g, 8.84 mmol, DBA / pNIPAAM 300 Molar ratio = 100) and deionized water (2 mL) were mixed in a RBF and stirred with a magnetic stirrer. The RBF was placed in an ice bath while HCl 25 wt% solution (1.151 mL, DBA / HCl molar ratio = 1) was added and maintained at room temperature under constant stirring until all DBA was dissolved. The pH of the mixture was adjusted to 6 with NaOH 1 M solution (0.673 mL). The protonated DBA solution was added to the pNIPAAM prepared in the previous step. 300 The mixture was then transferred to the RBF containing ACVA (5 mg, 0.02 mmol, ACVA / pNIPAAM). 300 (molar ratio = 0.2) was added to the reaction mixture. Similarly, the reaction mixture was cooled to 100°C. 2 After degassing at 40° C. for 30 min, the RBF was placed in a preheated oil bath at 70° C. for 24 h. An aliquot (50 μL) of the reaction mixture was 1It was removed for H NMR analysis (see FIG. 5B). No purification was performed.

[0069] Example 3. pNIPAAM 300 -pDBA 100 -pNIPAAM 300 Synthesis of pNIPAAM 300 -pDBA 100 RBF containing NIPAAM (3 g, 26.51 mmol, NIPAAM / pNIPAAM 300 -pDBA 100 Molar ratio = 300) to ACVA (5 mg, 0.02 mmol, ACVA / pNIPAAM 300 -pDBA 100 The reaction mixture was added with 10 mL of toluene (molar ratio = 0.2) and methanol (4 mL). 2 After degassing at 4°C for a minimum of 30 min, the RBF was placed in a preheated oil bath at 70°C for 24 h. An aliquot (50 μL) of the reaction mixture was 1 The purified sample was then taken for 1 H NMR analysis (see FIG. 5C). 1 The copolymers were analyzed by H NMR analysis (see FIG. 5D). The synthesis of the triblock copolymers is shown diagrammatically in FIG. 4. A list of copolymers synthesized using this technique is shown in Table 1.

[0070] [Table 1]

[0071] Example 4. Synthesis of NIPAAM-DEA-NIPAAM triblock copolymer The triblock copolymer was synthesized by the ATRP method. 0.11 g (1 eq.) diethyl meso-2,5-dibromoadipate initiator, 5.6 g (100 eq.) DEA (2-(diethylamino)ethyl methacrylate) monomer, 0.138 g (2 eq.) HMTETA (1,1,4,7,10,10-hexamethyltriethylenetetramine) catalyst, and 0.086 g (2 eq.) copper(I) bromide were placed in a 250 mL three-neck round-bottom flask with 6 mL of anhydrous methanol. The mixture in the flask was frozen by liquid nitrogen and degassed by three freeze-thaw processes, and then polymerized overnight in an oil bath at 70 °C. The resulting DEA polymer was purified by passing it through a silica gel column to remove the copper catalyst. PolyDEA was further dried in vacuum at 40 °C for 24 h.

[0072] 2.5 g of the resulting polyDEA macromer was mixed with 6.0 g of NIPAAm monomer in 15 mL of anhydrous methanol, followed by degassing with nitrogen for 50 min. Under a nitrogen atmosphere, 0.038 g (2 equivalents) of catalyst copper(I) bromide and Me 4 Cyclam (1,4,8,11-tetramethyl-1,4,8,11-tetraazacyclotetradecane), 0.068 g (2 eq.) was added at ambient temperature. The reaction was stirred overnight under nitrogen and after completion of the reaction, the solution was passed through a silica gel column to remove the catalyst using MeOH as eluent. The solvent was removed by rotary evaporation and the polymer was further dried under vacuum at 40° C. for 24 hours.

[0073] Example 5. Typical procedure for preparation of polymer emboli by mixing triblock copolymers with polyAMPS. As a typical procedure for the preparation of the composite hydrogel, to make a 20% wt / wt polymer solution, 2 g of triblock copolymer (Sample 4, Table 1) was dissolved in 8 g of deionized water by repeatedly placing the vial of solution in either an ice-water bath or a refrigerator (2-8 °C) for 1-2 h, followed by roller mixing for 1 h until most of the solid polymer was dissolved. The solution was then kept in the refrigerator overnight and roller mixed again for 2 h to obtain a homogenous solution.

[0074] This solution was mixed homogeneously with 0.9 g of tantalum powder (20% solids) in a 10 mL syringe. Air bubbles were removed by tapping the syringe. PolyAMPS sodium form was prepared by slowly adding NaOH powder to poly(2-acrylamido-2-methyl-1-propanesulfonic acid) solution (MW approx. 2 million Da, 15% concentration) while stirring to adjust the pH to approximately pH 4. 0.54 g of polyAMPS in a second 10 mL syringe was mixed with the tantalum polymer suspension through a three-way stopcock to form a homogeneous mixture to provide a charge ratio of approximately 1:1.5. The mixture was then pushed into one 10 mL syringe and capped for steam sterilization at 121 °C for 30 min. The suspension was mixed repeatedly by exchanging with another syringe through the three-way stopcock at room temperature. Finally, the suspension was dispensed into 1 mL syringes for catheter delivery. The final composition contained 11.1% wt / wt of triblock copolymer, 3.7% wt / wt of polyAMPS, and 20% wt / wt of tantalum. Figure 6 shows the hydrogel formed after injecting the composition through an 18G needle into PBS buffer at 37°C. The PBS buffer composition is 140 mM NaCl, 10 mM phosphate buffer, and 3 mM KCl, pH 7.4.

[0075] A similar process was used to prepare representative composite gels of NIPAAM-DEA-NIPAAM triblock copolymer and polyAMPS. Example 6. Rheological study of composite gels with different charge ratios between DBA blocks and polyAMPS NIPAAM-DBA-NIPAAM copolymer solutions were prepared under slightly acidic conditions to fully protonate the DBA block, and the pH of the resulting solutions was measured to be in the approximate pH range of 5-6. When polyAMPS solution was mixed with the copolymer solution via two-syringe mixing, a viscous coacervate solution was formed at room temperature. By controlling the ratio of charges of DBA and polyAMPS in the composition, the rheological properties of the solutions could be altered.

[0076] Figure 7 shows the rheological behavior of NIPAAM300-DBA100-NIPAAM300 composite gels with different charge ratios between DBA and polyAMPS, specifically 1:0, 1:1 and 1:1.5. No tantalum powder was used in this study. Figure 7 shows that without the addition of AMPS (1:0 ratio), there is no charge-charge interaction, resulting in the formation of soft gels. In low temperature (<30°C) solutions, the hydrogels of the copolymers with 1:1.5 ratio behaved more like soft solids (G'<100 Pa) compared to the gels with 1:1 ratio, which were relatively soft and slightly stiffer gels. This can be attributed to the contribution of the extra polyAMPS chains to reduce both the storage and loss moduli. At higher temperatures, around 37°C, all gels were more solid-like (G'>G'') and the gels with 1:1 ratio were stiffer compared to the gels with 1:1.5 ratio. For the sample containing NIPAAM400-DBA200-NIPAAM400, the 1:1 and 1:1.5 ratio gels showed nearly identical behavior, which may be explained by the high molecular weight and strong chain entanglements.

[0077] Example 7. Effect of DBA and NIPAAM chains on the rheological properties of temperature- and pH-responsive composite gels Figure 8 shows the storage and loss moduli of various pNIPAAM-b-pDBA-b-pNIPAAMa triblock copolymer samples versus temperature gradient. The results suggest that increasing the chain length of the NIPAAM block tends to increase the storage modulus of the hydrogel at elevated temperatures, approximately 37 °C. No tantalum powder was used in this study. As the temperature increased beyond 33-37 °C, the storage modulus of the DBA100 copolymer gel increased from 4 kPa to 7 kPa, and from NIPAAM200 to NIPAAM300, respectively. The storage modulus of the DBA200 copolymer gel increased from approximately 10 kPa to 11 kPa with the change from NIPAAM300 to NIPAAM400, respectively.

[0078] As can be seen from the graph in Figure 8, at temperatures below 30°C, the composite gels of the short chain copolymers exhibited more liquid-like behavior, with loss moduli greater than the storage modulus (10-50 Pa). With increasing molecular weight up to (sample 7, Table 1), the storage and loss moduli were nearly the same, at 200-300 Pa, suggesting a more solid-like composite gel. The measurements are consistent with the observation that samples 3 and 4 (Table 1) were relatively easy to deliver, while samples 6 and 7 (Table 1) were much stiffer gels requiring more force for catheter delivery.

[0079] Without wishing to be bound by any theory, the role played by the DBA block in the formation of the hydrogel appears to be a complex with the DBA component interacting with polyAMPS at pH below pH 7, while the hydrophobic portion enhances the gel strength with NIPAAM at 37° C. and pH 7. Figure 8 shows two copolymers, DBA100 and DBA200, with the same NIPAAM300 length. The DBA200 copolymer has an increased storage modulus compared to DBA100.

[0080] To study the effect of DBA length, copolymers with DBA300 and DBA400 were synthesized and related composite hydrogel samples were prepared. Table 2 lists the morphology and properties of the samples. Samples 4 and 6 (Table 2) both have NIPAAM300 blocks with either 100 or 200 units of DBA blocks, while samples 3, 8 and 9 have NIPAAM200 blocks with 100-400 units of DBA blocks. In general, gel samples with short DBA chains of 100-200 units are more homogenous and liquid-like. The gels are relatively easy to deliver through 2.7-2.8 Fr catheters.

[0081] [Table 2]

[0082] Samples with longer DBA units (i.e., 300-400 units) immediately formed a composite precipitate when mixed with polyAMPS. The composite gels were found to be difficult to mix, and this was true even at the sample preparation stage. The gels tended to break down into small particles and then aggregate, resulting in blockages in the syringe. Rheological studies were not performed with NIPAAM400-DBA300-NIPAAM400 mixed with polyAMPS, as a uniform gel could not be produced.

[0083] Example 8. Effect of pH change on composite gel properties The composite hydrogel in this example is composed of protonated NIPAAM-DBA-NIPAAM triblock copolymer and polyAMPS, with a pH range of 5-6 in pre-delivery and post-delivery states. After delivery to a physiological environment, the DBA block began to partially deprotonate and become hydrophobic, further enhancing the hydrophobicity of the composite gel together with NIPAAM at 37°C. A preliminary rheological study was performed by oscillatory method to measure the gel modulus. To understand the effect of pH change on the gel properties, the first study was performed on the gel at 37°C, followed by the addition of PBS buffer to the test cell. The cell was made from a 3D printed plastic cylinder with an O-ring sealed at the bottom connected to the test plate of the rheometer. To study the gel behavior at pH 5-6, first, the gel was placed under a 25 mm parallel plate geometry to perform oscillatory testing in air, mimicking the pre-delivery of the gel in a catheter. Then, PBS buffer at pH 7.4 was added to the cell to cause a gel pH change that mimics the gel after delivery to a physiological environment. Changes in storage and loss moduli were recorded to demonstrate gel behavior before and after delivery.

[0084] Figure 9 showed the test results of two composite gels, NIPAAM300-DBA100-NIPAAM300 (sample 4, Table 2) and NIPAAM400-DBA200-NIPAAM400 (sample 7, Table 2), copolymer samples with polyAMPS at a charge ratio of 1:1.5. The increase in elastic modulus shown in Figure 9 demonstrated that deprotonation of the DBA moiety could enhance the hydrophobic interactions of the hydrogel network formed at high temperature. After adding PBS buffer, the increase in elastic modulus observed in both samples was relatively small, probably because the contact between the gel and the PBS solution only occurred at the edge of the shape initially, and deprotonation of the internal gel may require a longer time. It may also be that the higher fraction of NIPAAM in the polymer formed a more hydrophobic barrier that slowed down the PBS diffusion into the sample disk under the plate. Thus, the observed increase in elastic modulus was much lower than the actual gel hardening in vivo, which could be attributed to the very small contact area of ​​the sample disk edge.

[0085] Rheological studies confirmed the thermoresponsiveness of the polymer by increasing the temperature from 15 °C to 40 °C, and the sol-gel transition of the polymer solution was observed at approximately 32-34 °C. These were measured at a fixed shear strain of 0.1% and an angular frequency of 10 rad / s. The effect of pH on the elastic modulus of the hydrogel was studied by adding PBS to the top of the polymer solution trapped under a 25 mm flat geometry at 37 °C. The same shear strain and angular frequency were applied.

[0086] Example 9. Comparison of NIPAAM-DEA-NIPAAM triblock copolymer with NIPAAM-DBA-NIPAAM triblock copolymer Compared to the triblock copolymer NIPAAM200-DBA100-NIPAAM200, the DEA block of NIPAAM200-DEA100-NIPAAM200 is less hydrophobic due to the difference of four carbons between the diethylamino group and the dibutylamino group. Figure 10 shows the effect of this difference on the rheology of the composite gel formed with polyAMPS. The composite gel of NIPAAM-DEA-NIPAAM was more solid-like, with G'>G''. Although it is temperature sensitive, its storage modulus (G' about 200 Pa) at a temperature of approximately 37°C did not increase significantly compared to the storage modulus at 25°C, which suggested a weak gel. Visual inspection of the gel also showed a homogeneous mixture and complexation between the DEA block and polyAMPS (Table 2). Sedimentation and flow model tests confirmed the rheological test data, i.e., gel fragment formation during stirring and passage through the pores of the flow model. Furthermore, the DEA block has a pKa of 7.4, suggesting that the NIPAAM-DEA-NIPAAM copolymer does not exhibit significant pH responsiveness under physiological conditions.

[0087] Example 11. Precipitation test of tantalum mixed composite gels with different compositions Samples of copolymer-polyAMPS composite gels mixed with 20% tantalum powder were first tested in PBS at 37°C by delivering the solution through a needle (18 gauge) into PBS and observing precipitation. Samples 3, 4, 6 and 7 were tested with two levels of polyAMPS at charge ratios of 1:1 or 1:1.5. The compositions contained 9.2-12.9% wt / wt of triblock copolymer, 2.4-4.0% wt / wt (1:1 ratio) or 3.2-5.1% wt / wt (1:1.5 ratio) of polyAMPS, and 20% wt / wt of tantalum. Test results are shown in Table 3. Samples 13, 14 and 15 were formulated with pAMPS at charge ratios of 1:1, 1:1.2, 1:1.5 and 1:2. Tantalum powder and 1.0-1.2 M NaCl solution were also added to the formulations. The compositions tested contained 5.0-7.3% wt / wt of triblock copolymer, 5.0-7.7% wt / wt of polyAMPS, and 20% wt / wt of tantalum powder. The addition of NaCl was to shield charge-charge interactions and allow for more distal delivery of the formulation. Upon diffusion of concentrated NaCl from the fluid, the coacervated gel solidified and embolized small blood vessels.

[0088] [Table 3-1]

[0089] [Table 3-2]

[0090] All eight samples were thread-like in gel morphology, suggesting that the gel had already started to form within the needle prior to delivery. Samples 3 and 4 showed less gel particles / fragments in PBS and higher cohesion. Sample 4 appeared to have improved cohesion compared to Sample 3. In addition, the gels with higher polyAMPS (1:1.5 ratio) were softer compared to the samples with 1:1 ratio, which is consistent with other rheology test results. The samples withstood vigorous vial shaking at a temperature of approximately 37°C and no broken fragments were observed. When the temperature of the PBS was reduced below 30°C, the gel began to disintegrate and the tantalum powder leached out of the gel. Meanwhile, the solution became translucent, which may be due to the dispersed micelle formation from the NIPAAM-DBA-NIPAAM block copolymer.

[0091] Samples 6 and 7, which have longer DBA and NIPAAM chains, appeared to be less cohesive when delivered in PBS buffer at 37° C., and large fragments of polymer and small amounts of tantalum powder were found in solution even at temperatures above 35° C. Similar to Samples 3 and 4, gels with longer DBA and NIPAAM chains result in the formation of smaller fragments and dispersed tantalum powder when the temperature of the PBS was reduced below 30° C.

[0092] Based on the test results, Sample 4 had higher gel strength and cohesiveness even after vigorously shaking the vial, but had a storage modulus of 6 kPa, suggesting a relatively stiff gel.

[0093] Example 12. Tantalum mixed composite gel delivered in a flow model Solutions of NIPAAM-DBA-NIPAAM triblock copolymers prepared at low temperatures and pH 5-6 could also be easily delivered through catheters as liquid embolic compositions (Figure 11). During catheter delivery in the PBS flow model system, the polymer solution tended to begin to gel within the catheter as the temperature increased from ambient to 37 °C. Nevertheless, the gel remained pushable without excessive force, which allows for rapid gelation with adequate gel strength (i.e., without being sheared into fragments) after entering the bloodstream. As saline began to exchange with water in the gel, the pH of the gel increased to pH 7, causing deprotonation of DBA, enhancing gel strength and resulting in favorable long-term gel stability.

[0094] Radiopaque contrast agents and tantalum powder may be added to the composition to facilitate fluoroscopically guided surgical procedures. For example, liquid contrast agents, such as iodized oils, such as iodized poppy oil, may also be used to confirm the quality of embolization. This can be easily accomplished, for example, by using a three-way stopcock attached to a syringe proximal to the catheter so that the contrast agent can be injected after embolization is complete.

[0095] Example 13. Preclinical testing of the composite gel in porcine kidney and liver models To evaluate the deliverability, handling, embolization performance, and visibility of the composite gel in a porcine model, Sample 4 (Table 3) and a reference sample (containing gelatin, laponite, and tantalum mixed with water) were delivered to the renal and hepatic arteries.

[0096] Gel samples at 18% concentration were first autoclaved in 3 mL syringes at 121 °C for 30 min. Testing showed that the treated gel samples maintained their thermo- and pH-responsive gelation properties and were not significantly different from the samples before autoclaving. Preliminary observations from the physician user experience were that delivery of the samples was easy and without difficulty. The gel exiting the catheter tip appeared as a coil-like string with a proximal distribution. Three blood vessels with diameters of approximately 1.8-2.5 mm were initially embolized, followed by contrast flow, demonstrating good embolization efficiency. Embolization of deep blood vessels was also successful (Figures 12A-12C). Testing showed better visibility of the gel under a fluoroscope compared to the reference sample (Figures 13A-13C).

[0097] Example 14. Addition of drugs to composite gel liquid embolic preparations and release of drugs from the composite gel liquid embolic preparations Doxorubicin solution (25 mg / mL) was thoroughly mixed with the aqueous solution of triblock copolymer (20%) by forcing it between the two syringes through a three-way stopcock. After delivery in PBS at 37°C, the drug-loaded and solidified embolic hydrogels began to gradually release doxorubicin. After 24 hours, the solution was red in color indicating drug release. The solution was then replaced with fresh PBS at 37°C, which was red again after 24 hours, indicating continued drug release.

Claims

1. One or more poly(N-isopropylaminoacrylamide) blocks and one or more poly(2-(di-(C 3~5 A medical composition comprising an aqueous solution of a block copolymer comprising a C) alkylamino) ethyl methacrylate) block, 3~5 A composition wherein the alkyl groups are independently selected from propyl, butyl and pentyl groups, and which is in liquid form at 25°C.

2. The one or more poly(2-(di-(C 3~5 2. The composition of claim 1, wherein the poly(2-(dibutylamino)ethyl methacrylate) block is a poly(2-(dibutylamino)ethyl methacrylate) block.

3. The composition of claim 1 or claim 2, wherein the composition has a pH in the range of 5 to 6.

4. The composition of any one of claims 1 to 3, wherein the composition becomes a gel when injected into phosphate buffered saline having a pH of 7.4 and a temperature of 37°C.

5. The block copolymer comprises two poly(N-isopropylaminoacrylamide) blocks and one poly(2-(di-(C 3~5 a triblock copolymer having one poly(N-isopropylaminoacrylamide) block and two poly(2-(di-(C 3~5 The composition of any one of claims 1 to 4, which is a triblock copolymer having a) alkylamino) ethyl methacrylate) block.

6. The composition of any one of claims 1 to 5, wherein each of the one or more poly(N-isopropylaminoacrylamide) blocks in the block copolymer ranges from 5 to 600 monomer units in length.

7. The one or more poly(2-(di-(C 3~5 The composition of any one of claims 1 to 6, wherein each of the (alkylamino)ethyl methacrylate) blocks ranges in length from 50 to 300 monomer units.

8. The composition according to any one of claims 1 to 7, wherein the number average molecular weight of the block copolymer is in the range of 2000 to 500,000 Da.

9. The composition according to any one of claims 1 to 8, wherein the composition has a viscosity in the range of 10 mPa·s to 5000 mPa·s when measured at a shear rate of 50 1 / s at a temperature of 25°C.

10. The composition of any one of claims 1 to 9, wherein the block copolymer further comprises an additional polymer block ranging from 1 to 500 monomer units in length comprising an amine group.

11. The composition of any one of claims 1 to 10, further comprising an anionic polymer containing negatively charged groups selected from sulfonate groups, sulfate groups, phosphate groups, phosphonate groups and carboxylate groups.

12. 12. The composition of claim 11, wherein the anionic polymer is selected from sulfonate polymers, polyphosphates, poly(carboxylic acids) and negatively charged polysaccharides, preferably the anionic polymer is poly(2-acrylamido-2-methylpropanesulfonate).

13. The composition of any one of claims 1 to 12, further comprising an imaging or therapeutic agent.

14. The composition of any one of claims 1 to 13, wherein the composition is provided in a vial or a syringe barrel.

15. 15. Use of the composition of any one of claims 1 to 14 as an embolic agent, a fiducial marker, a tissue filler, a tissue spacer, or a therapeutic depot.

Citation Information

Patent Citations

  • Liquid phase polymeric vascular occlusion material which gives rise to sol-gel phase transition and its application

    JP2002102331A

  • Multi-stimulation reversible hydrogel

    JP2004512389A

  • ABA triblock copolymer, thickener, and aqueous composition

    JP2013241567A

  • Stimulus-responsive protein-polymer conjugates for bioseparation

    JP2017534602A

  • Heat-sensitive hydrogel collagenase preparation

    JP2018528962A