Polyamide resins, compositions, and their use in engineering plastics
The development of polyamide resins with controlled water extractable and hypophosphite content addresses mold fouling and white spots in ultra-thin articles, enhancing production efficiency and mechanical properties for use in electrical and electronic devices, including acidic environments.
Patent Information
- Application Number
- JP2024529168
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2021-11-19
- Filing Date
- 2022-01-27
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2042-01-27
AI Technical Summary
Polyamide 5X resins used in ultra-thin articles like relays and capacitors face issues with mold fouling and white spots due to high heating and shearing during injection molding, which affect production efficiency and product appearance, primarily because of high water extractable content and hypophosphite levels.
Development of polyamide resins with a water extractable content of 0.7% by weight or less and hypophosphite content of 10-500 ppm, along with a controlled polymerization process to produce polyamide resins with improved mechanical properties, yellowing resistance, and acid corrosion resistance, using specific diamine and dicarboxylic acid structural units and additives.
The new polyamide resins exhibit reduced mold fouling, improved appearance quality, and enhanced mechanical properties, allowing for efficient production and use in electrical and electronic devices, with applications in acidic environments.
Smart Images

Figure 2024540752000001 
Figure 2024540752000002 
Figure 2024540752000003
Abstract
Description
Detailed Description of the Invention
[0001] [Technical field] The present disclosure is in the field of polymeric materials, and in particular, relates to polyamide resins and their preparation methods, compositions, and textile products.
[0002] [Background technology] Due to its excellent properties and ease of melt molding, polyamides have been widely used and attracted attention in materials for clothing, industrial materials, fibers, or general engineering plastics. Polyamide 5X is a linear long-chain polymer synthesized from bio-based pentanediamine and a series of dicarboxylic acids. Because amide bonds are easy to form hydrogen bonds, polyamide 5X fibers have high strength and excellent moisture absorption. During the polymerization of polyamide 5X, due to the occurrence of cyclization reaction, the polymer macromolecular chain is cut into two segments during the amide group exchange reaction within the chain, or the linear low molecular substance undergoes a direct dehydration reaction to produce a low molecular weight polymer. In general, water extractables are low molecular weight polymers ranging from monomers to decamers, such as dimers and trimers, and include linear and cyclic structures. The presence of these water extractables may affect the performance and applications of the resin.
[0003] For example, in the case of ultra-thin articles (thickness 0.3mm-0.4mm) such as relays and capacitors, because the articles are very thin, they require injection molding at high temperature and high speed, under which the heating and shearing of the material itself is significantly higher than other injection molding conditions, and the occurrence of mold contamination is particularly significant, which requires regular cleaning of the mold surface during continuous processing, resulting in reduced production efficiency. In addition, in severe cases, problems such as white spots may occur on the surface of the article, which may seriously affect the appearance of the product.
[0004] Summary of the Invention To address the shortcomings of the prior art techniques and products, it is an object of the present disclosure to provide a polyamide resin.
[0005] The polyamide resin contains a diamine structural unit and a dicarboxylic acid structural unit, and has a water extractable content of 0.7% by weight or less, and a hypophosphite content, calculated as P, of 10 ppm to 500 ppm.
[0006] According to some embodiments of the present disclosure, the water extractable content is 0.6 wt% or less, preferably 0.5 wt% or less. The water extractable is mainly oligomers produced from monomer feedstock during the polymerization process, such as linear or cyclic monomers to decamers.
[0007] In some preferred embodiments of the present disclosure, when the water extractable content is within the above defined range, the yellowing resistance of the polyamide resin and the resin composition containing the same described below is improved.
[0008] In some preferred embodiments of the present disclosure, when the water extractable content is within the above defined range, the mechanical properties of the polyamide resin and the resin composition containing the same described below are improved.
[0009] In some preferred embodiments of the present disclosure, when the water extractable content is within the above defined range, the polyamide resin and the resin composition containing it described below have good appearance quality and no obvious precipitation.
[0010] In some preferred embodiments of the present disclosure, when the water extractable content is within the above defined range, the acid corrosion resistance of the polyamide resin and the resin composition containing the same described below is improved.
[0011] In some preferred embodiments of the present disclosure, the polyamide resin has a water extractable content of 0.05 wt% or more, preferably 0.1 wt% or more, more preferably 0.2 wt% or more, and even more preferably 0.25 wt% or more. If the water extractable content is below the range defined above, the performance of the polyamide resin and the resin composition containing it described below will be reduced to a certain extent.
[0012] The water extractable content of the polyamide resin is the percentage of the mass of components that can be extracted into water after extraction treatment, relative to the mass of the polyamide resin before extraction treatment, when the polyamide resin is heated in deionized water and subjected to extraction treatment (for example, when the polyamide resin is extracted with water at 97°C to 100°C for 24 hours).
[0013] Water extractable content (%) = [(mass (m1) of polyamide resin before water extraction - mass (m2) of polyamide resin after water extraction) / mass (m1) of polyamide resin before water extraction)] x 100%.
[0014] The extraction conditions include, for example, extracting the polyamide resin with water at 97° C. to 100° C. for 24 hours, with a mass ratio of polyamide resin to water of 1:48 to 51, for example 1:50.
[0015] Furthermore, the method for measuring the water extractable content is as follows: a polyamide resin sample is dried in an air-drying oven at 130° C. for 7 hours, then sealed in an aluminum plastic bag and cooled in a dryer. Then, weigh about 2g of the polyamide resin sample and record the actual mass (m1);The polyamide resin sample is placed in a 250mL round-bottom flask, 100mL of deionized water is added, and the resulting mixture is heated under reflux at 97°C to 100°C for 24 hours to extract the polyamide resin sample with water, and then the polyamide resin sample is taken out of the water and washed with deionized water three times, and then the polyamide resin sample is dried in an air-drying oven at 130°C for 7 hours;The polyamide resin sample is then transferred to a pre-weighed aluminum plastic bag, sealed in the aluminum plastic bag, and cooled in a dryer, and the total weight of the aluminum plastic bag and the polyamide sample and the weight of the aluminum plastic bag are weighed, and the latter is subtracted from the former to obtain the weight of the polyamide sample after water extraction (m2).The water extract content is calculated from the difference between the weights of the polyamide sample before and after water extraction. Water extract content (%)=[(m1-m2) / m1]×100%.
[0016] Furthermore, when the water extractable content of a polyamide resin melt is measured, the melt is introduced into a sealed container, cooled, and then sampled and measured according to the above-mentioned method.
[0017] According to some embodiments of the present disclosure, the water extract has a number average molecular weight of 200 g / mol to 2,000 g / mol as determined by GPC method.
[0018] According to some embodiments of the present disclosure, the aqueous extract comprises one or two of the following structures: [ka] Here, n1 and n2 are independently selected from integers of 1 to 8, preferably, n1 and n2 are independently selected from integers of 1 to 6, more preferably, n1 and n2 are independently selected from integers of 1 to 5, and even more preferably, n1 is 2, 3 or 4, n2 is 2, 3, 4 or 5, m1 is 4, and m2 is 4.
[0019] In a preferred embodiment of the present disclosure, the hypophosphite is contained in an amount, calculated as P, of 10 ppm to 300 ppm, preferably 10 ppm to 200 ppm.
[0020] In a preferred embodiment of the present disclosure, the hypophosphite comprises an alkali metal hypophosphite and an alkaline earth metal hypophosphite, preferably any one of sodium hypophosphite, potassium hypophosphite, calcium hypophosphite, and magnesium hypophosphite, or a combination of two or more of the above.
[0021] According to some embodiments of the present disclosure, the pentanediamine structural units in the polyamide resin can be derived from chemically derived pentanediamine or biologically derived pentanediamine, preferably biologically derived 1,5-pentanediamine.
[0022] In a preferred embodiment of the present disclosure, 90 mol % or more of the dicarboxylic acid structural units are derived from adipic acid, and 90 mol % or more of the diamine structural units are derived from 1,5-pentanediamine.
[0023] In a preferred embodiment of the present disclosure, 95 mol % or more, preferably 97 mol % or more, of the diamine structural units in the polyamide resin are derived from 1,5-pentanediamine.
[0024] Furthermore, the diamine structural units in the polyamide resin can further include one or more structural units derived from butanediamine, hexanediamine, decanediamine, and dodecanediamine.
[0025] In a preferred embodiment of the present disclosure, 95 mol % or more, preferably 97 mol % or more, of the dicarboxylic acid structural units in the polyamide resin are derived from adipic acid.
[0026] According to some embodiments of the present disclosure, the dicarboxylic acid structural units in the polyamide resin may further include one or more structural units derived from succinic acid, glutaric acid, pimelic acid, suberic acid, azelaic acid, decanedioic acid, undecanedioic acid, dodecanedioic acid, tridecanedioic acid, tetradecanedioic acid, pentadecanedioic acid, hexadecanedioic acid, heptadecanedioic acid, octadecanedioic acid, terephthalic acid, isophthalic acid, and phthalic acid.
[0027] In a preferred embodiment of the present disclosure, the content of the polyamide (main polymer) composed of the diamine structural unit and the dicarboxylic acid structural unit in the polyamide resin is 90% by weight or more, preferably 95% by weight or more, more preferably 97% by weight or more, and even more preferably 99% by weight or more. The diamine structural unit and the dicarboxylic acid structural unit are defined as above.
[0028] According to some embodiments of the present disclosure, the polyamide resin includes an additive in addition to hypophosphite.
[0029] The additives include, but are not limited to, end-capping agents, nucleating agents, antioxidants, antifoaming agents, and flow improvers, or combinations of two or more thereof. End-capping agents include lauric acid, stearic acid, benzoic acid, and acetic acid.
[0030] In some preferred embodiments of the present disclosure, the additives in the polyamide resin are present in an amount of 10 wt % or less, preferably 5 wt % or less, more preferably 3 wt % or less, and even more preferably 1 wt % or less.
[0031] According to some embodiments of the present disclosure, the polyamide resin is a polyamide 56 resin having a polyamide 56 content of 90% by weight or more, further 95% by weight or more, further 97% by weight or more, and even 99% by weight or more.
[0032] In a preferred embodiment of the present disclosure, the polyamide resin has a relative viscosity of 1.8 to 4.0, preferably 2.2 to 3.5, and more preferably 2.4 to 3.3.
[0033] In a preferred embodiment of the present disclosure, the polyamide resin has a yellowness index of less than 7, preferably less than 5, and more preferably less than 4.2.
[0034] A second object of the present disclosure is to provide a method for preparing said polyamide resin.
[0035] According to some embodiments of the present disclosure, the method includes the steps of: S1, prepare nylon salt solution in an inert gas atmosphere; S2, heating the nylon salt solution to increase the pressure of the nylon salt solution reaction system to 0.5 to 2.5 MPa, maintaining the pressure by degassing for 0.5 to 4 hours, then reducing the pressure in the reaction system to 0 to 0.7 MPa (gauge pressure), and then evacuating the reaction system to a vacuum degree of -0.01 to -0.08 MPa to obtain a polyamide melt; and S3, the polyamide melt is discharged and strand pelletized to obtain polyamide chips.
[0036] Unless otherwise stated or clearly contradictory, pressures referred to in this disclosure refer to gauge pressure. In this disclosure, the nylon salts and polyamide salts can be used interchangeably.
[0037] Among these, in step S1, 1,5-pentanediamine and dicarboxylic acid are used in a molar ratio of (1-1.1:1) to prepare the nylon salt solution.
[0038] In step S2, the temperature of the reaction system is 232° C. to 260° C. at the end of maintaining the pressure.
[0039] In step S2, the temperature of the reaction system is 240° C. to 295° C., and further 243° C. to 288° C., at the end of the decompression.
[0040] In step S2, the temperature of the reaction system after evacuation is 250°C to 290°C, and further 252°C to 285°C.
[0041] In step S2, the vacuum level is maintained for a period of 11 to 75 minutes after evacuation.
[0042] In step S3, the strand pelletization is carried out in water at a water temperature of 15° C. to 50° C. to obtain polyamide chips or polyamide pellets.
[0043] According to some embodiments of the present disclosure, the method further comprises the steps of: S4, mixing the polyamide chips with water in a reactor to obtain a mixture, and then replacing the air in the reactor with an inert gas; and S5, heating and filtering the mixture in an inert gas atmosphere, and rinsing and / or drying the polyamide chips to obtain the polyamide resin.
[0044] In step S4, the reactor can be formed into a closed environment. In step S4, the reactor can be, for example, a continuous extraction column or a batch reactor.
[0045] Preferably, in step S4, the air in the reactor can be replaced by using a vacuum pump to evacuate the reactor, and then the reactor can be refilled with nitrogen gas or an inert gas. The above operation for replacing the air in the reactor can be repeated two or more times.
[0046] In step S4, the water is deionized water, and further deoxygenated water that has been subjected to a deoxygenation process, where the deoxygenation process can be one of thermal deoxygenation, ultrasonic deoxygenation, vacuum deoxygenation, chemical deoxygenation, decomposition deoxygenation, or any other deoxygenation method, or a combination of two or more thereof. In some preferred embodiments, after the deoxygenation process, the deionized water has a dissolved oxygen content of 0.5 mg / L or less, or even 0.1 mg / L or less.
[0047] In step S4, the water is used in an amount of at least 1 time, preferably at least 2 times, for example 1 to 12 times, 1 to 10 times, 2 to 10 times, 2 to 6 times, 1.5 times, 2.3 times, 2.5 times, 3 times, 5 times, or 8 times the mass of the polyamide chips.
[0048] In steps S1, S4 and S5, the inert gas includes one or two of argon gas and helium gas, and more preferably includes high-purity argon gas and high-purity helium gas.
[0049] According to some embodiments of the present disclosure, the air replacement in step S4 is performed as follows: the reactor is evacuated to a vacuum level of −0.1 MPa to −0.001 MPa (gauge pressure), maintained for 5 to 20 minutes, and then refilled with nitrogen gas or an inert gas, and more preferably, the air replacement operation is repeated 5 to 15 times, more preferably 8 to 10 times.
[0050] According to some embodiments of the present disclosure, in step S5, the mixture is heated for 4 to 50 hours, preferably 8 to 45 hours.
[0051] According to some embodiments of the present disclosure, in step S5, the mixture is heated at a temperature of 80°C to 140°C, preferably 85°C to 120°C.
[0052] According to some embodiments of the present disclosure, the rinsing in step S5 is performed with hot water at a temperature between 50°C and 100°C.
[0053] According to some embodiments of the present disclosure, the drying in step S5 is performed by one or more of vacuum drying, freeze drying, air flow drying, microwave drying, infrared drying and radio frequency drying.
[0054] A third object of the present disclosure is to provide a resin composition comprising the following components in parts by weight: 100 parts polyamide resin and 10-70 parts glass fiber.
[0055] In a preferred embodiment of the present disclosure, the glass fibers have a length to diameter ratio of (2-800):1, even (200-650):1.
[0056] In a preferred embodiment of the present disclosure, the glass fiber has a length of 3 mm to 12 mm, preferably 3 mm to 8 mm.
[0057] In some preferred embodiments of the present disclosure, when the glass fibers have parameters within the ranges defined above, the mechanical properties of the resin composition are improved.
[0058] Further, the composition may include any one of an antioxidant, a nucleating agent, a lubricant, a flame retardant, a coupling agent, a heat stabilizer, a light stabilizer, an antistatic agent, an ultraviolet absorber, and a colorant, or a combination of two or more of the above.
[0059] Further, the antioxidant is present in an amount of 0.02 to 2 parts by weight, and the antioxidant preferably includes any one of a hindered phenol-based antioxidant, a hindered amine-based antioxidant, and a phosphite-based antioxidant, such as any one of Antioxidant 168, Antioxidant 1098, Antioxidant 1010, and Antioxidant S9228, or a combination of two or more of the above.
[0060] In a preferred embodiment of the present disclosure, in an acid resistance test, no or only a small amount of precipitates (floating fibers) are present on the surface of the resin composition.
[0061] In a preferred embodiment of the present disclosure, after injection molding of the resin composition, there is no obvious mold fouling or only a small amount of mold fouling.
[0062] In a preferred embodiment of the present disclosure, the polyamide resin is as defined above.
[0063] A method for preparing a polyamide resin composition, comprising the steps of: The ingredients are added to a twin screw extruder and mixed, then extruded from the twin screw extruder, cooled, and pelletized to obtain a polyamide composition.
[0064] Additionally, during the mixing, the glass fibers are fed through a side feed port of the twin screw extruder.
[0065] The ingredients are then mixed and melted in the twin-screw extruder at a temperature of 210°C to 290°C.
[0066] In an embodiment of the present disclosure, during the mixing, the twin screw extruder adopts a 7-zone heating mode, and the temperature in zone 1 is 210°C-250°C, and / or the temperature in zone 2 is 210°C-250°C, and / or the temperature in zone 3 is 240°C-260°C, the temperature in zone 4 is 260°C-280°C, and / or the temperature in zone 5 is 270°C-290°C, and / or the temperature in zone 6 is 270°C-290°C, and / or the temperature in zone 7 is 255°C-285°C; where the direction from zone 1 to zone 7 is from the feed throat to the die.
[0067] The die temperature of the twin-screw extruder is 260°C to 275°C.
[0068] The screw speed of the twin-screw extruder is 350 r / min to 500 r / min.
[0069] The twin screw extruder has a D / L ratio (diameter to length ratio) of 1:(30-50), preferably 1:40.
[0070] A fourth object of the present disclosure is to provide a use of the aforementioned polyamide resin or composition in engineering plastics.
[0071] The present disclosure has at least the following advantages over the prior art: 1. The preparation method of polyamide resin according to the present disclosure is simple, the process parameters are easy to control, large-scale equipment is not required, and mass production is convenient.
[0072] 2. The polyamide resin composition has the advantages of a short molding cycle, a fast crystallization rate, little mold contamination during injection molding, and good appearance quality, and therefore can be applied to devices in the electrical and electronic fields.
[0073] 3. The polyamide resin composition has the advantage of being resistant to acid corrosion, and can be used in acidic environments, such as in packaging and containers for acidic foods.
[0074] Detailed Description In order to make the objectives, technical solutions and advantages of the present disclosure clearer, the technical solutions in the embodiments of the present disclosure are described below in conjunction with the embodiments of the present disclosure clearly and completely. Obviously, the described embodiments are only some of the embodiments of the present disclosure, not all of the embodiments. All other embodiments that can be achieved by those skilled in the art based on the embodiments of the present disclosure without creative work fall within the protection scope of the present disclosure.
[0075] 1. Measurement method for relative viscosity ηr Concentrated sulfuric acid method using an Ubbelohde viscometer: Accurately weigh out 0.5±0.0002 g of a dry polyamide resin sample, add 50 mL of concentrated sulfuric acid (98%) to dissolve, and measure and record the flow time (t0) of the concentrated sulfuric acid and the flow time (t) of the polyamide resin solution in a thermostatic water bath at 25°C. Formula for calculating relative viscosity: relative viscosity ηr=t / t0.
[0076] 2. Method for measuring water extractables content of polyamide resin Each polyamide resin sample is dried in an air-drying oven at 130°C for 7 hours, then sealed in an aluminum plastic bag, cooled in a dryer, and approximately 2 g of the polyamide resin sample is accurately weighed to obtain the actual mass (m1). The weighed polyamide resin sample is placed in a 250 mL round-bottom flask, 100 mL of deionized water is added, and the resulting mixture is heated under reflux at 97°C to 100°C for 24 hours to extract the polyamide resin sample with water, and then the polyamide resin sample is taken out and washed three times with deionized water, and then the polyamide resin sample is dried in an air-drying oven at 130°C for 7 hours. The polyamide resin sample is transferred to a pre-weighed aluminum plastic bag, sealed in the aluminum plastic bag, and then cooled in a dryer. The total weight of the aluminum plastic bag and the polyamide resin sample and the weight of the aluminum plastic bag are weighed, and the latter is subtracted from the former to obtain the weight of the polyamide resin sample after water extraction (m2). The amount of water extractables was calculated from the difference in weight of the polyamide sample before and after water extraction: Water extractables content (%) = [(m1-m2) / m1] x 100%.
[0077] When the water extractable content of a polyamide resin melt is measured, the melt is introduced into a sealed container, cooled, and then sampled and measured according to the above-mentioned method.
[0078] 3.Yellowness (YI) Yellowness is tested according to HG / T 3862.
[0079] 4.Crystallization test Each polyamide resin sample is subjected to crystallinity analysis using differential scanning calorimetry (DSC): each polyamide resin sample obtained from the examples and comparative examples is heated from room temperature to 280°C at a heating rate of 50°C / min, held at 280°C for 3 minutes, and then cooled to room temperature at a rate of 10°C / min to obtain the crystallization temperature and crystallization half time.
[0080] 5. Tensile strength The tensile strength is tested according to ISO 527-2 at a pulling speed of 50 mm / min.
[0081] 6. Bending strength The flexural strength is tested according to ISO 178 at a speed of 2 mm / min.
[0082] 7.Acid resistance test Each polyamide resin sample is immersed in a 10% by weight aqueous solution of acetic acid at 40°C for 180 days, and the precipitates on the surface of each sample are observed and graded from 1 to 5, where grade 1 is the worst since a large amount of precipitates are formed, and grade 5 is the best since there are no obvious precipitates.
[0083] Preparation Example 1 (1) Under nitrogen gas conditions, 1,5-pentanediamine, adipic acid and water were mixed uniformly in a molar ratio of 1,5-pentanediamine to adipic acid of 1.08:1 to prepare a 60% by weight nylon salt solution (where % is the mass % of the nylon salt solution); the nylon salt solution was sampled and diluted to a concentration of 10% by weight. The pH value at this time was 7.85.
[0084] (2) 1200g of nylon salt solution and 500ppm of sodium hypophosphite were added to a polymerization reactor, and the pressure in the reaction system was increased to 2.3MPa in 1.5 hours by heating, and then the pressure was maintained for 3 hours by degassing, and at the end of the pressure holding process, the temperature of the reaction system was 245°C, and then the pressure in the reaction system was reduced to 0.003MPa (gauge pressure) in 1 hour, and the temperature of the reaction system after the reduction in pressure was 273°C. The reaction system was evacuated for 32 minutes and maintained at a vacuum degree of -0.06MPa, and the temperature of the reaction system after the evacuation was 272°C, and a melt of polyamide 56 was obtained.
[0085] (3) The molten material obtained in step (2) was discharged and strand-pelletized under water cooling at a water temperature of 20° C. to obtain polyamide 56 chips.
[0086] Example 1 (a) The polyamide 56 chips prepared in Preparation Example 1 and deoxygenated deionized water were added to a reactor in a mass ratio of the chips to the deoxygenated deionized water of 1:6. The air in the reactor was replaced with nitrogen gas as follows: the reactor was evacuated to a vacuum of -0.09 MPa (gauge pressure) and held at this vacuum for 10 minutes, after which it was refilled with nitrogen gas, and the replacement with nitrogen gas was repeated 9 times.
[0087] (b) Under a nitrogen gas atmosphere, the resulting mixture was heated at 90°C for 32 hours, then filtered to separate the chips from the water, the resulting chips were rinsed with water at 95°C, and then vacuum dried at 105°C for 15 hours to obtain a polyamide 56 resin.
[0088] Example 2 (1) Under a nitrogen gas atmosphere, 1,5-pentanediamine, adipic acid and water were mixed uniformly in a molar ratio of 1,5-pentanediamine to adipic acid of 1:1 to prepare a 70% by weight nylon salt solution (where % is the mass % of the nylon salt solution); the nylon salt solution was sampled and diluted to a concentration of 10% by weight. The pH value at this time was 7.96.
[0089] (2) 1200g of nylon salt solution and 300ppm of sodium hypophosphite were added to a polymerization reactor, and the pressure in the reaction system was increased to 2.0M in 1.5 hours by heating, and then the pressure was maintained at 2.40MPa for 3 hours by degassing, and at the end of the pressure holding process, the temperature of the reaction system was 243°C, and then the pressure in the reaction system was reduced to 0.005MPa (gauge pressure) over 1 hour, and the temperature of the reaction system after the reduction was completed was 290°C. The reaction system was evacuated for 30 minutes and maintained at a vacuum degree of -0.08MPa, and the temperature of the reaction system after the evacuation was 290°C, and a melt of polyamide 56 was obtained.
[0090] (3) The molten material obtained in step (2) was discharged and strand-pelletized under water cooling at 20° C. to obtain polyamide 56 chips.
[0091] (4) Polyamide 56 chips and deoxygenated deionized water were added to a reactor in a mass ratio of the chips to the deoxygenated deionized water of 1:6. The air was replaced with nitrogen gas as follows: the reactor was evacuated to a vacuum of -0.07 MPa (gauge pressure) and held at this vacuum for 10 minutes, then refilled with nitrogen gas, and the nitrogen gas replacement was repeated 10 times.
[0092] (5) The reactor in step (4) was protected by introducing nitrogen gas, and the resulting mixture was heated at 96°C for 46 hours, then filtered to separate the chips from the water, and the resulting chips were rinsed with water at 95°C, and then vacuum dried at 105°C for 15 hours to obtain a polyamide 56 resin.
[0093] Example 3 (a) The polyamide 56 chips prepared in Preparation Example 1 and deoxygenated deionized water were added to a reactor in a mass ratio of the chips to the deoxygenated deionized water of 1:12. The air in the reactor was replaced with nitrogen gas as follows: the reactor was evacuated to a vacuum of -0.09 MPa (gauge pressure) and held at this vacuum for 10 minutes, after which it was refilled with nitrogen gas and the replacement with nitrogen gas was repeated 10 times.
[0094] (b) The reactor in step (a) was protected with nitrogen gas, and the resulting mixture was heated at 95°C for 55 hours, then filtered to separate the chips from the water, and the resulting chips were rinsed with hot water at 95°C, and then vacuum dried at 105°C for 15 hours to obtain a polyamide 56 resin.
[0095] Example 4 (1) Under a nitrogen gas atmosphere, 1,5-pentanediamine, adipic acid and water were uniformly mixed in a molar ratio of 1,5-pentanediamine to adipic acid of 1.05:1 to prepare a 60% by weight nylon salt solution (where % is the mass % of the nylon salt solution); the nylon salt solution was sampled and diluted to a concentration of 10% by weight. The pH value at this time was 7.98.
[0096] (2) 1200g of nylon salt solution and 1200ppm of sodium hypophosphite were added to a polymerization reactor, and the pressure in the reaction system was increased to 2.0MPa in 1.5 hours by heating, and then the pressure was maintained for 3 hours by degassing, and at the end of the pressure holding process, the temperature of the reaction system was 243°C, and then the pressure in the reaction system was reduced to 0.005MPa (gauge pressure) in 1 hour, and the temperature of the reaction system after the reduction in pressure was 290°C. The reaction system was evacuated for 30 minutes and maintained at a vacuum degree of -0.08MPa, and the temperature of the reaction system after the evacuation was 290°C, and a melt of polyamide 56 was obtained.
[0097] (3) The molten material obtained in step (2) was discharged and strand-pelletized under water cooling at 20° C. to obtain polyamide 56 chips.
[0098] (4) The chips were vacuum dried at 105°C for 15 hours to obtain a polyamide 56 resin.
[0099] Example 5 (1) Under a nitrogen gas atmosphere, 1,5-pentanediamine, adipic acid and water were uniformly mixed in a molar ratio of 1,5-pentanediamine to adipic acid of 1.05:1 to prepare a 60% by weight nylon salt solution (where % is the mass % of the nylon salt solution); the nylon salt solution was sampled and diluted to a concentration of 10% by weight. The pH value at this time was 7.98.
[0100] (2) 1200g of nylon salt solution and 2400ppm of sodium hypophosphite were added to a polymerization reactor, and the pressure in the reaction system was increased to 2.0MPa in 1.5 hours by heating, and then the pressure was maintained for 3 hours by degassing, and at the end of the pressure holding process, the temperature of the reaction system was 243°C, and then the pressure in the reaction system was reduced to 0.005MPa (gauge pressure) in 1 hour, and the temperature of the reaction system after the reduction in pressure was 290°C. The reaction system was evacuated for 30 minutes and maintained at a vacuum degree of -0.08MPa, and the temperature of the reaction system after the evacuation was 290°C, and a melt of polyamide 56 was obtained.
[0101] (3) The molten material obtained in step (2) was discharged and strand-pelletized under water cooling at a water temperature of 20° C. to obtain polyamide 56 chips.
[0102] (4) The chips were vacuum dried at 105°C for 15 hours to obtain a polyamide 56 resin.
[0103] Example 6 (1) Under a nitrogen gas atmosphere, 1,5-pentanediamine, adipic acid and water were uniformly mixed in a molar ratio of 1,5-pentanediamine to adipic acid of 1.05:1 to prepare a 60% by weight nylon salt solution (where % is the mass % of the nylon salt solution); the nylon salt solution was sampled and diluted to a concentration of 10% by weight. The pH value at this time was 7.98.
[0104] (2) 1200g of nylon salt solution and 85ppm of sodium hypophosphite were added to a polymerization reactor, and the pressure in the reaction system was increased to 2.0MPa in 1.5 hours by heating, and then the pressure was maintained for 3 hours by degassing, and at the end of the pressure holding process, the temperature of the reaction system was 243°C, and then the pressure in the reaction system was reduced to 0.005MPa (gauge pressure) in 1 hour, and the temperature of the reaction system after the reduction in pressure was 290°C. The reaction system was evacuated for 30 minutes and maintained at a vacuum degree of -0.08MPa, and the temperature of the reaction system after the evacuation was 290°C, and a melt of polyamide 56 was obtained.
[0105] (3) The molten material obtained in step (2) was discharged and strand-pelletized under water cooling at a water temperature of 20° C. to obtain polyamide 56 chips.
[0106] (4) The chips were vacuum dried at 105°C for 15 hours to obtain a polyamide 56 resin.
[0107] The polyamide resins obtained in Examples 1 to 6 were tested for relative viscosity, water extract content, hypophosphorous acid content (P conversion), crystallization temperature, half crystallization time, acid resistance and yellowness. The test results are shown in Table 1.
[0108] [Table 1]
[0109] Polyamide compositions were prepared using the polyamide resins, glass fibers, and antioxidants of Examples 1 to 6 as raw materials. The formulation of the compositions is shown in Table 2.
[0110] The composition was prepared as follows: Polyamide resin, glass fiber and antioxidant were used as raw materials and kneaded in a twin-screw extruder, and then the strand extruded from the twin-screw extruder was cooled in water as a cooling medium to a temperature below the melting point of polyamide, and pelletized to obtain a polyamide resin composition. The twin-screw extruder adopted a 7-zone heating mode, and the temperatures from zone 1 to zone 7 were 250°C, 260°C, 260°C, 280°C, 270°C, 270°C and 270°C consecutively. The die temperature was 260°C, the screw speed was 480r / min, and the D / L ratio of the twin-screw extruder was 1:40.
[0111] The resulting polyamide resin composition was dried at 110°C for 5 hours, and then injection molded with a sample thickness of 3 mm under the following conditions: barrel temperature 280°C and mold surface temperature 110°C. Fifty consecutive injection moldings were performed, and mold staining on the high gloss surface of the mold was observed and rated on a five-point scale. Here, the amount of mold staining decreased sequentially from grade 1 to grade 5, with grade 1 being the worst with a large amount of mold staining, and grade 5 being the best with no obvious mold staining. The test results of the injection molded samples are shown in Table 2.
[0112] [Table 2]
[0113] Finally, it should be noted that the above embodiments are only intended to illustrate the technical solutions of the present disclosure, and are not intended to limit it. Although the present disclosure has been described in detail with reference to the above embodiments, those skilled in the art should understand that the technical solutions described in the above embodiments may be modified, or equivalent replacements may be made to some or all of the technical features thereof, and these modifications or replacements will not cause the essence of the corresponding technical solutions to depart from the scope of the technical solutions in the embodiments of the present disclosure.
Claims
1. The polyamide resin contains a diamine structural unit and a dicarboxylic acid structural unit, has a water extractable content of 0.7% by weight or less, and has a hypophosphite content of 10 ppm to 500 ppm calculated as P.
2. 90 mol % or more of the dicarboxylic acid structural units are derived from adipic acid and 90 mol % or more of the diamine structural units are derived from 1,5-pentanediamine; and / or The hypophosphites include alkali metal hypophosphites and alkaline earth metal hypophosphites, preferably including any one of sodium hypophosphite, potassium hypophosphite, calcium hypophosphite, and magnesium hypophosphite or a combination of two or more thereof; and / or the polyamide resin has a water extractables content of 0.05 wt.% or more, preferably 0.1 wt.% or more, more preferably 0.2 wt.% or more, even more preferably 0.25 wt.% or more; and / or The polyamide resin has a hypophosphite content, calculated as P, of 10 ppm to 300 ppm, preferably 10 ppm to 200 ppm; and / or the polyamide resin has a relative viscosity of 1.8 to 4.0, preferably 2.2 to 3.5, more preferably 2.4 to 3.3; and / or The polyamide resin has a yellowness index of less than 7, preferably less than 5. The polyamide resin according to claim 1.
3. 3. A composition comprising the polyamide resin of claim 1 or 2, the composition comprising the following components in parts by weight: 100 parts polyamide resin and 10-70 parts glass fiber.
4. the glass fibers have a length to diameter ratio of (2-800):1, preferably (200-650):1; and / or the glass fibres have a length of between 3mm and 12mm, preferably between 3mm and 8mm; and / or 4. The composition of claim 3, wherein the composition contains any one of an antioxidant, a nucleating agent, a lubricant, a flame retardant, a coupling agent, a heat stabilizer, a light stabilizer, an antistatic agent, an ultraviolet light absorber, and a colorant, or a combination of two or more thereof.
5. A method for preparing a polyamide resin, comprising the steps of: The method includes the steps of: S1, preparing a nylon salt solution in an inert gas atmosphere; S2, heating the nylon salt solution to increase the pressure of the nylon salt solution reaction system to a pressure of 0.5 to 2.5 MPa, maintaining the pressure by degassing for 0.5 to 4 hours, then reducing the pressure in the reaction system to 0 to 0.7 MPa by depressurizing, and then evacuating the reaction system to a vacuum degree of -0.01 to -0.08 MPa to obtain a polyamide melt; and S3: Discharge the polyamide melt and pelletize it into strands to obtain polyamide chips.
6. In step S1, 1,5-pentanediamine and dicarboxylic acid are used in a molar ratio of (1-1.1):1 for the preparation of the nylon salt solution; and / or In step S2, the reaction system has a temperature of 232° C. to 260° C. at the end of the pressure maintenance; and / or In step S2, the reaction system has a temperature of 240° C. to 295° C. at the end of depressurization; and / or In step S2, the reaction system has a temperature of 250° C. to 290° C. after evacuation; and / or In step S2, the vacuum is maintained for 11 to 75 minutes after evacuation; and / or In step S3, the strand pelletization is carried out in water at a water temperature of 15°C to 50°C; The method according to claim 5.
7. The method of claim 5 further comprising the steps of: S4, mixing the polyamide chips with water in a reactor to obtain a mixture, and then replacing the air in the reactor with an inert gas; and S5, in an inert gas atmosphere, the mixture is heated and filtered, and the polyamide chips are rinsed and / or dried to obtain the polyamide resin.
8. In step S4, the reactor is selected from a continuous extraction column and a batch reactor; and / or In step S4, the air in the reactor is replaced by evacuating the reactor using a vacuum pump and then backfilling the reactor with nitrogen gas or an inert gas; and / or In step S4, the operation for replacing the air in the reactor is repeated two or more times; and / or In step S4, the water is deionized water, preferably deionized water that has been subjected to a deoxidization treatment; and / or In step S4, the water is used in an amount of at least 1 times the mass of the polyamide chips, preferably at least 2 times the mass of the polyamide chips, for example 1 to 12 times the mass of the polyamide chips, 2 to 10 times the mass of the polyamide chips, and 2 to 6 times the mass of the polyamide chips; and / or In steps S4 and S5, the inert gas contains one or two of argon gas and helium gas. The method of claim 7.
9. In step S5, the mixture is heated for 4 to 50 hours, preferably 8 to 45 hours; and / or In step S5, the mixture is heated to between 80°C and 140°C, preferably between 85°C and 120°C; and / or In step S5, the rinsing is carried out using hot water at a temperature between 50° C. and 100° C.; and / or 8. The method according to claim 7, wherein in step S5, the drying is carried out by one or more selected from vacuum drying, freeze drying, air flow drying, microwave drying, infrared drying and radio frequency drying.
10. 5. Use of the polyamide resin according to claim 1 or 2 or the composition according to claim 3 or 4 in engineering plastics.
Citation Information
Patent Citations
Bio-based PA56T and PA56 composite material and preparation method thereof
CN110903644A
Polyamide composite for improving laser weldability
CN111138852A
Yellowing-resistant polyamide resin and preparation method thereof
CN111269414A
High and low temperature aging resistant toughened polyamide 5X resin and preparation method thereof