Uranium-Based Phosphors and Compositions for Display and Lighting Applications - Patent application
Uranium-based phosphors with specific formulations and dopants address the limitations of current LED technologies by providing efficient energy transfer and tunable emissions, enhancing CRI and color gamut in displays and lighting, particularly for human-centered and horticultural uses.
Patent Information
- Application Number
- JP2024521064
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2022-04-13
- Filing Date
- 2022-10-10
- Publication Date
- 2024-11-06
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Current LED lighting and display technologies face challenges in achieving high color rendering index (CRI) and efficient energy transfer for next-generation micro-LEDs, particularly in creating wide color gamut displays and human-centered lighting, due to limitations in phosphor materials.
Development of uranium-based phosphor materials, such as uranyl (UO2) compounds with specific formulas, doped with activator ions like Pr3+, Sm3+, and Eu3+, and counterions like Li+, Na+, K+, Rb+, Cs+, which exhibit efficient energy transfer and tunable emission spectra, filling the dark blue-green gap and providing both green and red emissions from a single phosphor.
The uranium-based phosphors achieve high CRI values, efficient energy transfer, and tunable emission spectra, enabling high-intensity, human-centered lighting and wide color gamut displays, suitable for both general illumination and horticultural applications.
Smart Images

Figure 2024540849000001_ABST
Abstract
Description
CROSS-REFERENCE TO RELATED APPLICATIONS
[0001] This application claims the benefit of priority to U.S. Provisional Patent Application No. 63 / 254,021, filed October 8, 2021, and International Application No. PCT / US2022 / 024577, filed April 13, 2022, each of which is incorporated by reference in its entirety herein. [Background technology]
[0002] The field of the invention relates generally to phosphor materials and devices, and more particularly to uranium-based phosphor materials useful for display and lighting applications.
[0003] General lighting is based on the solar spectrum and the sensitivity of the human eye to visible radiation. The effect of eye sensitivity is related to the total lumen output, while the match with the full spectrum of solar radiation results in the color rendering index (CRI). Traditional general lighting includes incandescent and fluorescent lighting. LED lighting has improved efficiency, reduced electricity usage by 40%, and increased life expectancy compared to traditional general lighting. LED lighting can cover a nearly continuous range across the visible wavelengths from about 380 nm to about 750 nm and can be used for general lighting and display applications. The tunability of LED lighting can be used to create both full spectrum (high CRI) and high efficiency (lumens / watt) lighting based on the desired characteristics and phosphor combinations used. LED lighting also creates the ability to have human-centric lighting that changes color subtly throughout the day, and specialized lighting for applications such as plant growth.
[0004] White light can be produced by using near ultraviolet (UV) or blue emitting LEDs in combination with inorganic phosphors or blends of inorganic phosphors such as red emitting phosphors and green or yellow-green emitting phosphors. The total emission from the phosphors and LED chip provides a color point with corresponding color coordinates (x and y on the 1931 CIE chromaticity diagram) and correlated color temperature (CCT), whose spectral distribution provides color rendering capabilities measured by the Color Rendering Index (CRI) based on a scale of 100. Effectiveness is a measure of the amount of light emitted per unit of power used (lumens / watt) with higher amounts being preferred. Mn 4+ Narrow band red emitting phosphors based on complex fluoride materials activated by cerium are described in U.S. Patent Nos. 7,358,542, 7,497,973 and 7,648,649. These complex fluorides are cerium doped yttrium aluminum garnet Y 3 Al 5 O 12 :Ce 3+ In combination with yellow-green emitting phosphors such as (YAG) or other garnet compositions, blue LEDs can be used to achieve warm white light (CCT<5000K at the blackbody locus, color rendering index (CRI>80) with high efficiency. High efficiency with varying emission from the phosphor material is also desirable.
[0005] Current display device technology relies on liquid crystal displays (LCDs), which are one of the most widely used flat panel displays for industrial and residential applications. Next generation devices will have low energy consumption, small size, and high brightness, and will require wider color gamut coverage. Next generation devices will require smaller LEDs, such as mini-LEDs or micro-LEDs. Mini-LEDs are on the order of 100μm to 0.7mm in size. For micro-LEDs, the display may be self-emissive or may include a miniature backlight arrayed with individual LEDs smaller than 100μm. If these next generation micro-LED displays are self-emissive and require a color conversion layer, a very thin layer or film of phosphor material with a high absorption coefficient is required. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] U.S. Patent No. 7,358,542 [Patent Document 2] U.S. Patent No. 7,497,973 [Patent Document 3] U.S. Patent No. 7,648,649 Summary of the Invention
[0007] In one embodiment, the uranium based phosphor material is uranyl (UO 2 ) group and having formula I, II, III, IV or V, [Ba 1-a-b Sr a Ca b ] x [Mg,Zn] y (UO 2 ) z ([P,V]O 4 ) 2(x+y+z) / 3 (I), [Ba 1-a-b Sr a Ca b ] p (UO 2 ) q [P,V] r O (2p+2q+5r) / 2 (II), A 2 UO 2 [P,V] 2 O 7 (III), A 4 UO 2 ([P,V]O 4 ) 2 (IV), or AUO 2 ([P,V]O 3 ) 3 (V) wherein 0≦a≦1, 0≦b≦1, 0.75≦x≦1.25, 0.75≦y≦1.25, 0.75≦z≦1.25, 2.5≦p≦3.5, 1.75≦q≦2.25, 3.5≦r≦4.5, and A is Li, Na, K, Rb, Cs, or a combination thereof.
[0008] In some embodiments, the uranium-based phosphor is doped with an activator ion. In some embodiments, the activator ion is Pr 3+ , Sm 3+ In some embodiments, the activator ion is Eu 3+ ,Pr 3+ , Sm 3+ In some embodiments, the uranium-based phosphor is doped with a counterion. In some embodiments, the counterion is one or more alkali metal ions. In other embodiments, the counterion is Li + , K + , Na + , Rb + , Cs + and mixtures thereof.
[0009] In one aspect, a uranium-based phosphor is provided, the uranium-based phosphor comprising: (i) a phosphor having formula I or II, [Ba 1-a-b Sr a Ca b ] x [Mg,Zn] y (UO 2 ) z ([P,V]O 4 ) 2(x+y+z) / 3 (I) [Ba 1-a-b Sr a Ca b ] p (UO 2 ) q [P,V] r O (2p+2q+5r) / 2 (II), The phosphor having the formula I or II is 3+ , Sm 3+or mixtures thereof, wherein 0≦a≦1, 0≦b≦1, 0.75≦x≦1.25, 0.75≦y≦1.25, 0.75≦z≦1.25, 2.5≦p≦3.5, 1.75≦q≦2.25, and 3.5≦r≦4.5; (ii) a phosphor having the formula I or II, wherein the phosphor having the formula I or II is selected from the group consisting of Eu 3+ ,Pr 3+ , Sm 3+ and mixtures thereof, and a counterion comprising one or more alkali metal ions; and (iii) a phosphor having formula III, A 2 UO 2 [P,V] 2 O 7 (III) The phosphor having formula III is 3+ ,Pr 3+ , Sm 3+ and mixtures thereof, where A is selected from phosphors that are Li, Na, K, Rb, Cs, or combinations thereof.
[0010] In another aspect, a uranium-based phosphor is provided having the formula (III), (IV) or (V): A 2 UO 2 [P,V] 2 O 7 (III), A 4 UO 2 ([P,V]O 4 ) 2 (IV) or AUO 2 ([P,V]O 3 ) 3 (V), where A is a uranium-based phosphor that is Li, Na, K, Rb, Cs, or a combination thereof.
[0011] In another aspect, a phosphor composition is provided. The composition includes a uranium-based phosphor and at least one other luminescent material. The uranium-based phosphor is (i) a phosphor having formula I or II, [Ba 1-a-b Sr a Ca b ] x [Mg,Zn] y (UO 2 ) z ([P,V]O 4 ) 2(x+y+z) / 3 (I) [Ba 1-a-b Sr a Ca b ] p (UO 2 ) q [P,V] r O (2p+2q+5r) / 2 (II), The phosphor having the formula I or II is 3+ , Sm 3+ or mixtures thereof, wherein 0≦a≦1, 0≦b≦1, 0.75≦x≦1.25, 0.75≦y≦1.25, 0.75≦z≦1.25, 2.5≦p≦3.5, 1.75≦q≦2.25, and 3.5≦r≦4.5; (ii) a phosphor having the formula I or II, wherein the phosphor having the formula I or II is selected from the group consisting of Eu 3+ ,Pr 3+ , Sm 3+ and mixtures thereof, and a counterion comprising one or more alkali metal ions; and (iii) a phosphor having formula III, A 2 UO 2 [P,V] 2 O 7 (III) The phosphor having formula III is 3+ ,Pr 3+ , Sm 3+ and mixtures thereof, where A is selected from phosphors that are Li, Na, K, Rb, Cs, or combinations thereof.
[0012] In another aspect, a phosphor composition is provided, the composition comprising a uranium-based phosphor and at least one other luminescent material, the uranium-based phosphor having the formula (III), (IV) or (V): A 2 UO 2 [P,V] 2 O 7 (III), A 4 UO 2 ([P,V]O 4 ) 2 (IV), or AUO 2 ([P,V]O 3 ) 3 (V), where A is a uranium-based phosphor that is Li, Na, K, Rb, Cs, or a combination thereof.
[0013] In another aspect, a phosphor composition is provided. The composition includes a uranium-based phosphor and a red-emitting phosphor. The uranium-based phosphor is (i) a phosphor having formula I or II, [Ba 1-a-b Sr a Ca b ] x [Mg,Zn] y (UO 2 ) z ([P,V]O 4 ) 2(x+y+z) / 3 (I) [Ba 1-a-b Sr a Ca b ] p (UO 2 ) q [P,V] r O (2p+2q+5r) / 2 (II), The phosphor having the formula I or II is 3+ , Sm 3+or mixtures thereof, wherein 0≦a≦1, 0≦b≦1, 0.75≦x≦1.25, 0.75≦y≦1.25, 0.75≦z≦1.25, 2.5≦p≦3.5, 1.75≦q≦2.25, and 3.5≦r≦4.5; (ii) a phosphor having the formula I or II, wherein the phosphor having the formula I or II is selected from the group consisting of Eu 3+ ,Pr 3+ , Sm 3+ and mixtures thereof, and a counterion comprising one or more alkali metal ions; and (iii) a phosphor having formula III, A 2 UO 2 [P,V] 2 O 7 (III) The phosphor having formula III is 3+ ,Pr 3+ , Sm 3+ and mixtures thereof, where A is selected from phosphors that are Li, Na, K, Rb, Cs, or combinations thereof. The red-emitting phosphor has formula VI: A x MF y :Mn 4+ (VI) wherein A is Li, Na, K, Rb, Cs, or a combination thereof; M is Si, Ge, Sn, Ti, Zr, Al, Ga, In, Sc, Hf, Y, La, Nb, Ta, Bi, Gd, or a combination thereof; and x is MF y is the absolute value of the charge of the ion, and y is 5, 6, or 7.
[0014] In another aspect, a phosphor composition is provided. The composition includes a uranium-based phosphor and a red-emitting phosphor. The uranium-based phosphor has the formula (III), (IV), or (V), A 2 UO 2 [P,V] 2 O 7 (III), A 4 UO2 ([P,V]O 4 ) 2 (IV), or AUO 2 ([P,V]O 3 ) 3 (V), A uranium-based phosphor has the formula VI, where A is Li, Na, K, Rb, Cs, or a combination thereof. A red-emitting phosphor has the formula VI, A x MF y :Mn 4+ (VI) wherein A is Li, Na, K, Rb, Cs, or a combination thereof; M is Si, Ge, Sn, Ti, Zr, Al, Ga, In, Sc, Hf, Y, La, Nb, Ta, Bi, Gd, or a combination thereof; and x is MF y is the absolute value of the charge of the ion, and y is 5, 6, or 7.
[0015] In yet another aspect, a device is provided that includes an LED light source radiatively and / or optically coupled to a uranium-based phosphor. (i) a phosphor having formula I or II, [Ba 1-a-b Sr a Ca b ] x [Mg,Zn] y (UO 2 ) z ([P,V]O 4 ) 2(x+y+z) / 3 (I) [Ba 1-a-b Sr a Ca b ] p (UO 2 ) q [P,V] r O (2p+2q+5r) / 2 (II), The phosphor having the formula I or II is 3+ , Sm 3+or mixtures thereof, wherein 0≦a≦1, 0≦b≦1, 0.75≦x≦1.25, 0.75≦y≦1.25, 0.75≦z≦1.25, 2.5≦p≦3.5, 1.75≦q≦2.25, and 3.5≦r≦4.5; (ii) a phosphor having the formula I or II, wherein the phosphor having the formula I or II is selected from the group consisting of Eu 3+ ,Pr 3+ , Sm 3+ and mixtures thereof, and a counterion comprising one or more alkali metal ions; and (iii) a phosphor having formula III, A 2 UO 2 [P,V] 2 O 7 (III) The phosphor having formula III is 3+ ,Pr 3+ , Sm 3+ and mixtures thereof, where A is selected from phosphors that are Li, Na, K, Rb, Cs, or combinations thereof.
[0016] In yet another aspect, a device is provided that includes an LED light source radiatively and / or optically coupled to a uranium-based phosphor having the formula (III), (IV) or (V): A 2 UO 2 [P,V] 2 O 7 (III), A 4 UO 2 ([P,V]O 4 ) 2 (IV), or AUO 2 ([P,V]O 3 ) 3 (V), where A is a uranium-based phosphor that is Li, Na, K, Rb, Cs, or a combination thereof.
[0017] Another aspect is a lighting device comprising the device. Yet another aspect is a backlight device comprising the device. Another aspect is a device and a lighting device for horticultural lighting. Another aspect is a phosphor package for horticultural lighting. [Brief description of the drawings]
[0018] [Figure 1] FIG. 2 is a schematic cross-sectional view of a device according to one embodiment of the present disclosure. [Diagram 2] FIG. 1 is a schematic cross-sectional view of a lighting device according to one embodiment of the present disclosure. [Diagram 3] 1 is a schematic cross-sectional view of a lighting device according to another embodiment of the present disclosure. [Figure 4] FIG. 1 is a cutaway side perspective view of a lighting device according to one embodiment of the present disclosure. [Diagram 5] FIG. 1 is a schematic perspective view of a surface mounted device (SMD) according to one embodiment of the present disclosure. [Figure 6A] 1 is a spectral graph of emission wavelength (nm) versus emission intensity for Na2UO2P2O7. [Figure 6B] 1 is a spectral graph of emission wavelength (nm) versus emission intensity for Eu3+-doped Na2UO2P2O7. [Figure 6C] 1 is a spectral graph of emission wavelength (nm) versus emission intensity for Pr3+-doped Na2UO2P2O7. [Figure 6D] 1 is a spectral graph of emission wavelength (nm) versus emission intensity of Sm3+-doped Na2UO2P2O7. [Figure 6E] 1 is a spectral graph of emission wavelength (nm) versus emission intensity of Tb3+-doped Na2UO2P2O7. [Figure 6F] 1 is a spectral graph of emission wavelength (nm) versus emission intensity of Dy3+-doped Na2UO2P2O7. [Figure 6G] 1 is a spectral graph of emission wavelength (nm) versus emission intensity for Eu3+ and Pr3+ doped Na2UO2P2O7. [Figure 6H]1 is a spectral graph of emission wavelength (nm) versus emission intensity for Eu3+ and Sm3+ doped Na2UO2P2O7. [Figure 7A] 1 is a spectral graph of emission wavelength (nm) versus emission intensity for K2UO2P2O7. [Figure 7B] 1 is a spectral graph of emission wavelength (nm) versus emission intensity for Eu3+-doped K2UO2P2O7. [Figure 7C] 1 is a spectral graph of emission wavelength (nm) versus emission intensity for Sm3+-doped K2UO2P2O7. [Figure 7D] 1 is a spectral graph of emission wavelength (nm) versus emission intensity for Pr3+-doped K2UO2P2O7. [Figure 8A] 1 is a spectrum graph of emission wavelength (nm) versus emission intensity of NaUO2P3O9. [Figure 8B] 1 is a spectral graph of emission wavelength (nm) versus emission intensity of Eu3+-doped NaUO2P3O9. [Figure 9A] 1 is a spectral graph of emission wavelength (nm) versus emission intensity for K4UO2(PO4)2. [Figure 9B] 1 is a spectral graph of emission wavelength (nm) versus emission intensity for Eu3+-doped K4UO2(PO4)2. [Figure 10A] 1 is a spectral graph of emission wavelength (nm) versus emission intensity for Ba3(PO4)2(UO2)2P2O7. [Figure 10B] 1 is a spectral graph of emission wavelength (nm) versus emission intensity for Ba3(PO4)2(UO2)2P2O7 doped with Eu3+. [Figure 10C] 1 is a spectral graph of emission wavelength (nm) versus emission intensity for Eu3+ and K+ doped Ba3(PO4)2(UO2)2P2O7. [Figure 10D] 1 is a spectral graph of emission wavelength (nm) versus emission intensity for Sm3+ and K+ doped Ba3(PO4)2(UO2)2P2O7. [Figure 10E]1 is a spectral graph of emission wavelength (nm) versus emission intensity for Pr3+ and K+ doped Ba3(PO4)2(UO2)2P2O7. [Figure 10F] 1 is a spectral graph of emission wavelength (nm) versus emission intensity for Sm3+ and K+ doped Ba3(PO4)2(UO2)2P2O7. [Figure 10G] 1 is a spectral graph of emission wavelength (nm) versus emission intensity for Pr3+ and K+ doped Ba3(PO4)2(UO2)2P2O7. [Figure 10H] 1 is a spectral graph of emission wavelength (nm) versus emission intensity for Eu3+ and K+ doped Ba3(PO4)2(UO2)2P2O7. [Figure 11A] 1 is a spectrum graph of emission wavelength (nm) versus emission intensity of BaZnUO2(PO4)2. [Figure 11B] 1 is a spectral graph of emission wavelength (nm) versus emission intensity of Eu3+-doped BaZnUO2(PO4)2. [Figure 11C] 1 is a spectral graph of emission wavelength (nm) versus emission intensity of Eu3+ and K+ doped BaZnUO2(PO4)2. [Figure 11D] 1 is a spectral graph of emission wavelength (nm) versus emission intensity of Eu3+ and Li+ doped BaZnUO2(PO4)2. [Figure 11E] 1 is a spectral graph of emission wavelength (nm) versus emission intensity of Eu3+ and Na+ doped BaZnUO2(PO4)2. [Figure 11F] 1 is a spectral graph of emission wavelength (nm) versus emission intensity of Pr3+-doped BaZnUO2(PO4)2. [Figure 11G] 1 is a spectral graph of emission wavelength (nm) versus emission intensity for Pr3+ and K+ doped BaZnUO2(PO4)2. [Figure 11H] 1 is a spectral graph of emission wavelength (nm) versus emission intensity of Sm3+-doped BaZnUO2(PO4)2. [Figure 11I]1 is a spectral graph of emission wavelength (nm) versus emission intensity of BaZnUO2(PO4)2 doped with Sm3+ and K+. [Figure 11J] 1 is a spectral graph of emission wavelength (nm) versus emission intensity of Eu3+ and Li+ doped BaZnUO2(PO4)2. [Figure 12] 1 is a spectral graph of emission wavelength (nm) versus emission intensity of Eu3+-doped BaZnUO2(PO4)2. [Figure 13A] 1 is a spectral graph of emission wavelength (nm) versus emission intensity for γ-Ba2UO2(PO4)2. [Figure 13B] 1 is a spectral graph of emission wavelength (nm) versus emission intensity of Eu3+-doped γ-Ba2UO2(PO4)2. [Figure 13C] 1 is a spectral graph of emission wavelength (nm) versus emission intensity for Eu3+ and K+ doped γ-Ba2UO2(PO4)2. [Figure 13D] 1 is a spectral graph of emission wavelength (nm) versus emission intensity of Sm3+ and K+ doped γ-Ba2UO2(PO4)2. [Figure 13E] 1 is a spectral graph of emission wavelength (nm) versus emission intensity for Pr3+ and K+ doped γ-Ba2UO2(PO4)2. [Figure 13F] 1 is a spectral graph of emission wavelength (nm) versus emission intensity of Dy3+ and K+ doped γ-Ba2UO2(PO4)2. [Figure 13G] 1 is a spectral graph of emission wavelength (nm) versus emission intensity for Tb3+ and K+ doped γ-Ba2UO2(PO4)2. [Figure 13H] FIG. 1 shows the powder XRD pattern of γ-Ba2UO2(PO4)2. [Figure 14] 1 is a spectral graph of emission wavelength versus emission intensity for Na2UO2P2O7:Eu3+ (U-Eu red) and PFS phosphors of Example 11. [Figure 15] 1 is a spectral graph of emission wavelength (nm) versus emission intensity for Eu3+-doped Na2UO2P2O7. [Figure 16]1 is a spectral graph of emission wavelength (nm) versus emission intensity for Eu3+-doped Na2UO2P2O7. [Figure 17A] 1 is a spectral graph of emission wavelength (nm) versus emission intensity for Rb2UO2P2O7. [Figure 17B] 1 is a spectral graph of emission wavelength (nm) versus emission intensity for Sm3+-doped Rb2UO2P2O7. [Figure 17C] 1 is a spectral graph of emission wavelength (nm) versus emission intensity for Eu3+-doped Rb2UO2P2O7. [Figure 17D] 1 is a spectral graph of emission wavelength (nm) versus emission intensity for Pr3+-doped Rb2UO2P2O7. [Figure 18A] 1 is a spectral graph of emission wavelength (nm) versus emission intensity for Cs2UO2P2O7. [Figure 18B] 1 is a spectral graph of emission wavelength (nm) versus emission intensity for Eu3+-doped Cs2UO2P2O7. [Figure 18C] 1 is a spectral graph of emission wavelength (nm) versus emission intensity for Pr3+-doped Cs2UO2P2O7. [Figure 18D] 1 is a spectral graph of emission wavelength (nm) versus emission intensity for Sm3+-doped Cs2UO2P2O7. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0019] In the following specification and claims, reference will be made to a number of terms that shall be defined to have the following meanings.
[0020] The singular forms "a," "an," and "the" include plural references unless the context clearly dictates otherwise.
[0021] Approximate language used herein throughout the specification and claims may be applied to modify any quantitative expression that may vary within acceptable limits without causing a change in the basic function to which it pertains. Thus, values modified with terms such as "about," "substantially," and "approximately" are not limited to the exact values specified. In at least some instances, approximate language may correspond to the precision of an instrument for measuring the value. Here, and throughout the specification and claims, range limitations may be combined and / or substituted, and such ranges are identified and include all subranges contained therein, unless the context or language dictates otherwise. All references are incorporated herein by reference.
[0022] The brackets in a formula indicate that at least one of the elements in the brackets is present in the phosphor material, and any combination of two or more of them may be present, as limited by the stoichiometry of the composition. For example, the formula [Ca,Sr,Ba] 3 MgSi 2 O 8 :EU 2+ ,Mn 2+ includes at least one of Ca, Sr, or Ba, or any combination of two or more of Ca, Sr, or Ba. 3 MgSi 2 O 8 :EU 2+ ,Mn 2+ , Sr 3 MgSi 2 O 8 :EU 2+ ,Mn 2+ , or Ba 3 MgSi 2 O 8 :EU 2+ ,Mn 2+Formulas that include an activator after a colon ":" indicate that the phosphor composition is doped with the activator. Formulas that include two or more activators separated by a "," after a colon ":" indicate that the phosphor composition is doped with the activator or both activators. For example, the formula [Ca,Sr,Ba] 3 MgSi 2 O 8 :EU 2+ ,Mn 2+ is [Ca,Sr,Ba] 3 MgSi 2 O 8 :EU 2+ , [Ca,Sr,Ba] 3 MgSi 2 O 8 :Mn 2+ or [Ca,Sr,Ba] 3 MgSi 2 O 8 :EU 2+ and Mn 2+ Includes:
[0023] The disclosed uranium-based phosphor materials provide narrowband green emission and, in some cases, good energy transfer with good quantum efficiency. These phosphors can be used in a variety of LED-based lighting and display applications. The pure green emission itself can be used in displays to provide a wide color gamut and fill the dark blue-green gap in human-centric lighting. 3+ Pr 3+ and Sm 3+ The efficient energy transfer of these materials to ions such as uranium makes them suitable for providing spectrally superior efficacy lighting (lumens / watt) and their use in phosphor blends can produce lighting devices with high efficacy and CRI values. Uranium-based phosphors are spectrally blue-shifted compared to other commercially available phosphors. This color shift provides greater overlap with the sensitivity of the human eye and higher lumen / watt measurements.
[0024] EU 3+ Pr 3+ and Sm 3+The activators also provide emission spectra for specialized high CRI lighting and illumination for plant growth. In some embodiments, uranium-based phosphors sensitized with europium, praseodymium, and samarium activator ions provide narrow emission spectra in the red / far-red region (approximately 600 nm to 800 nm) that are desirable for horticultural lighting. In some embodiments, the horticultural lighting includes LED-based white lighting having a composition that includes the uranium-based phosphor, which can be used for indoor and outdoor lighting for plant growth. In other embodiments, the horticultural lighting includes a phosphor package that includes the uranium-based phosphor. In some embodiments, the horticultural lighting may be solar-based.
[0025] EU 3+ , Sm 3+ , and Pr 3+ The doped phosphors also have tunable emission spectra based on the amount of activator ion added to the host composition. This spectral tuning provides the ability to create phosphors for display applications that have both green and red emission peaks, allowing displays with a wide color gamut to be created, which is particularly useful for film-based displays where film mura is important in the end use. Instead of needing to ensure multiple phosphors are uniformly distributed within the film, only one phosphor needs to be uniformly distributed as it provides both green and red emission.
[0026] The inventors have discovered that the uranium-based phosphor materials of the present disclosure can produce energy transfer with good quantum efficiency when uranyl ions are used as sensitizers for the activator ions europium, praseodymium, or samarium. This is surprising because others have attempted for years to sensitize europium emission for use in LEDs, but all attempts to date have been unsuccessful due to too low energy transfer, poor absorption, and / or quantum efficiency to be useful for the end application.
[0027] The inventors have discovered that certain luminescent materials can be activated by uranium-based phosphors to provide efficient energy transfer. In another embodiment, the inventors have unexpectedly discovered that Eu 3+ ,Pr 3+ and Sm 3+ We have discovered that by co-doping certain activator ions, such as , with alkali counterions, the efficient energy transfer of uranium-based phosphor materials can be increased.
[0028] The emission of europium, praseodymium or samarium shows that the emission can be used in lighting applications to obtain general lighting with high efficacy (Lms / W) not obtainable with commercial phosphor solutions. The pure uranium emission spectrum of the phosphor material absorbs at 450nm and can fill the dark blue-green gap, resulting in a complete spectrum and higher CRI values in general lighting. The pure uranium spectrum can be used in display backlighting applications to provide a wide color gamut.
[0029] In some embodiments, the inventors have surprisingly discovered that the phosphor material exhibits complete energy transfer to europium, praseodymium and samarium activator ions. The phosphor material has very high absorption, and in some embodiments, the full conversion red-emitting phosphor material can be used to prepare the thin phosphor films required for smaller LEDs, such as micro-LEDs and mini-LEDs. The phosphor material produces a high color gamut and can be easily processed to make films for smaller LEDs, or can be deposited on micro-LEDs to achieve full red conversion.
[0030] In one embodiment, the uranium based phosphor material is uranyl (UO 2 ) group and having formula I, II, III, IV or V, [Ba 1-a-b Sr a Ca b ] x [Mg,Zn] y (UO 2) z ([P,V]O 4 ) 2(x+y+z) / 3 (I), [Ba 1-a-b Sr a Ca b ] p (UO 2 ) q [P,V] r O (2p+2q+5r) / 2 (II), A 2 UO 2 [P,V] 2 O 7 (III), A 4 UO 2 ([P,V]O 4 ) 2 (IV), or AUO 2 ([P,V]O 3 ) 3 (V) wherein 0≦a≦1, 0≦b≦1, 0.75≦x≦1.25, 0.75≦y≦1.25, 0.75≦z≦1.25, 2.5≦p≦3.5, 1.75≦q≦2.25, 3.5≦r≦4.5, and A is Li, Na, K, Rb, Cs, or a combination thereof.
[0031] In some embodiments, the uranium-based phosphor is doped with an activator ion. In some embodiments, the activator ion is Pr 3+ , Sm 3+ In some embodiments, the activator ion is Eu 3+ ,Pr 3+ , Sm 3+ In some embodiments, the uranium-based phosphor is doped with a counterion. In some embodiments, the counterion is one or more alkali metal ions. In other embodiments, the counterion is Li + , K + , Na + , Rb + , or Cs + and mixtures thereof.
[0032] In one aspect, an activated uranium-based phosphor is provided. The uranium-based phosphor material comprises: (i) a phosphor having formula I or II, [Ba 1-a-b Sr a Ca b ] x [Mg,Zn] y (UO 2 ) z ([P,V]O 4 ) 2(x+y+z) / 3 (I) [Ba 1-a-b Sr a Ca b ] p (UO 2 ) q [P,V] r O (2p+2q+5r) / 2 (II), The phosphor having the formula I or II is 3+ , Sm 3+ or mixtures thereof, wherein 0≦a≦1, 0≦b≦1, 0.75≦x≦1.25, 0.75≦y≦1.25, 0.75≦z≦1.25, 2.5≦p≦3.5, 1.75≦q≦2.25, and 3.5≦r≦4.5; (ii) a phosphor having the formula I or II, wherein the phosphor having the formula I or II is selected from the group consisting of Eu 3+ ,Pr 3+ , Sm 3+ and mixtures thereof, and a counterion comprising one or more alkali metal ions; and (iii) a phosphor having formula III, A 2 UO 2 [P,V] 2 O 7 (III) The phosphor having formula III is 3+ ,Pr 3+ , Sm 3+ and mixtures thereof, where A is selected from phosphors that are Li, Na, K, Rb, Cs, or combinations thereof.
[0033] Uranium-based phosphor materials may be co-doped with uranium ions and activator ions. Lanthanide activator ions, particularly Eu 3+ ,Pr 3+ Or Sm 3+ Mn has luminescent properties. 2+ , Mn 4+ , Ce 3+ , Sn 2+ , Bi 3+ , Sb 3+ , Cr 3+ , Tb 3+ , Ti 4+ , In + , Tl + , Dy 3+ and Pb 2+ Additional ions such as Eu may also be present. 3+ ,Pr 3+ Or Sm 3+ We have discovered that uranium-based phosphor materials co-doped with lanthanide activator ions such as lanthanide ions, exhibit efficient energy transfer from the green pure uranium emission spectrum. This was surprising because other ions in the lanthanide series did not exhibit energy transfer or good quantum efficiency.
[0034] The inventors have 3+ ,Pr 3+ Or Sm 3+ It has been found that uranium-based phosphor materials co-doped with activator ions such as are color tunable, i.e., the ratio of the green emission from uranium to the emission color of the activator ions can be adjusted depending on the ratio of activator ions. The color shift of the phosphor can be a large change in color coordinate values (ccx and ccy values) or a very small change in color coordinate values, as desired. In some embodiments, the emission of the phosphor can be spectrally shifted closer to the eye's sensitivity range centered at 555 nm. These activator ions can be used for lighting applications that provide higher intensity in human-centric lighting and high-efficiency (Lms / W) lighting that is not available in currently commercially available phosphor solutions.
[0035] In some embodiments, there is complete energy transfer to the activator ion that completely quenches the uranium emission. For example, europium emission is red, and the inventors have discovered that uranium-based phosphor materials co-doped with europium activator ions can be tuned from pure green emission to pure red emission depending on the doping amount of europium activator ion. In other embodiments, there is partial quenching of the uranium emission. For example, Pr 3+ Or Sm 3+ The uranium-based phosphor material co-doped with activator ions can tune the pure green emission to orange or orange-red emission depending on the doping amount of activator ions.
[0036] In some embodiments, uranium-based phosphor materials can be used for high efficiency general lighting. In other embodiments, uranium-based phosphor materials can be color tuned to reduce harmful blue emissions for use in eye-safe displays. In other embodiments, uranium-based phosphor materials can be color tuned to produce emissions suitable for plant growth. In other embodiments, uranium-based phosphors can be color tuned to produce wide color gamut displays with green and red emissions produced from a single phosphor.
[0037] The inventors have surprisingly discovered that by co-doping a uranium-based phosphor with an activator ion and a counter ion, it is possible to increase the energy transfer in the uranium-based phosphor, and by co-doping a uranium-based phosphor with an activator ion and a counter ion, it is possible to improve the quantum efficiency of the phosphor. + , K + , Na + , Rb + Or Cs + and mixtures thereof. This was unexpected because alkali metal ions do not enhance all lanthanide activator ions and uranium based phosphors, as shown in the examples.
[0038] The energy transfer from the uranium ions to the activator ions can be measured by the change in color coordinate values ccx and ccy (x and y on the 1931 CIE chromaticity diagram). Because the phosphors are color tunable, the change in color coordinate values can be very small or can range from very large differences if desired. In some embodiments, the change in color coordinate values (ccx and ccy values) can be less than 10%. In other embodiments, the change in color coordinate values can be less than 5%. In other embodiments, the change in color coordinate values is at least 10%. In some embodiments, the activated phosphor exhibits a change in ccx value of at least 15% and a change in ccy value of at least 10%. In some embodiments, the activated phosphor exhibits a change in ccx value of at least 25%. In other embodiments, the activated phosphor exhibits a change in ccx value of at least 50%. In some embodiments, the activated phosphor exhibits a change in ccx value of about 15% to about 200%. In other embodiments, the change in ccx value is about 25% to about 200%, and in other embodiments, the change in ccx value is about 50% to about 200%. In some embodiments, the activated phosphor exhibits a ccy value change of at least 10%. In other embodiments, the activated phosphor exhibits a ccy value change of about 10% to about 50%.
[0039] Without wishing to be bound by theory, it is believed that the alkali metals interact with the europium, praseodymium and samarium activator ions and help distribute the activator ions within the host lattice by reducing the need for charge compensating defects.
[0040] In some embodiments, the uranium-based phosphor has the formula I: [Ba 1-a-b Sr a Ca b ] x [Mg,Zn] y (UO 2 ) z ([P,V)]O 4 ) 2(x+y+z) / 3 wherein 0≦a≦1, 0≦b≦1, 0.75≦x≦1.25, 0.75≦y≦1.25, and 0.75≦z≦1.25. 3+ ,Pr3+ Or Sm 3+ In another embodiment, one or more counter ions may be present. The counter ions may be alkali metals. In some embodiments, the counter ions are Li + , Na + , K + , Rb + , Cs + , or a mixture thereof. Specifically, Ba[Mg,Zn]UO 2 (PO 4 ) 2 , more specifically, BaMgUO 2 (PO 4 ) 2 and BaZnUO 2 (PO 4 ) 2 Examples include:
[0041] In some embodiments, the uranium-based phosphor has the formula II: [Ba 1-a-b Sr a Ca b ] p (UO 2 ) q [P,V] r O (2p+2q+5r) / 2 In some embodiments, the uranium-based phosphor has the formula IIA: [Ba,Sr,Ca,] p (UO 2 ) q [P,V] r O (2p+2q+5r) / 2 In some embodiments, Eu 3+ ,Pr 3+ Or Sm 3+ There may be one or more activator ions for formula II or IIA, such as and mixtures thereof. In another embodiment, there may be one or more counter ions for formula II or IIA. The counter ion may be an alkali metal. In some embodiments, the counter ion is Li + , Na + , K + , Rb +Or Cs + Specifically, the compound may be one or more of Ba. 3 (PO 4 ) 2 (UO 2 ) 2 P 2 O 7 , B.A. 3 (PO 4 ) 2 (UO 2 ) 2 V 2 O 7 and In one embodiment, when the formula is [Ba], p is 3.5, q is 1.75, [P], and r is 3.5, the compound is Ba 2 UO 2 (PO 4 ) 2 and is in the gamma phase. In another embodiment, 2 UO 2 (PO 4 ) 2 If γ-Ba 2 UO 2 (PO 4 ) 2 The phosphor gamma-phase Ba is described in PCT Publication No. WO2021 / 211600, which is incorporated herein by reference. 2 UO 2 (PO 4 ) 2 The γ-phase Ba had a powder XRD pattern as shown in FIG. 2 UO 2 (PO 4 ) 2 or γ-Ba 2 UO 2 (PO 4 ) 2 .
[0042] In other embodiments, the uranium-based phosphor has Formula III:A 2 UO 2 [P,V] 2 O 7where A is Li, Na, K, Rb, Cs, or a combination thereof. In some embodiments, Eu 3+ ,Pr 3+ Or Sm 3+ In some embodiments, A is Li + , Na + , K + , Rb + Or Cs + Specifically, A 2 UO 2 P 2 O 7 More specifically, Na 2 UO 2 P 2 O 7 and K 2 UO 2 P 2 O 7 Examples include:
[0043] In one embodiment, the uranium-based phosphor is Ba 3 (PO 4 ) 2 (UO 2 ) 2 P 2 O 7 , BaZnUO 2 (PO 4 ) 2 , Na 2 UO 2 P 2 O 7 , K 2 UO 2 P 2 O 7 , BaMgUO 2 (PO 4 ) 2 or An example is JPEG2024540849000003.jpg662.
[0044] The phosphor of the present disclosure is U 6+ions are part of the luminescent species and can therefore be characterized as uranium-doped or U-doped. The term "U-doped" typically indicates that a relatively small number of uranium atoms are substituted into the host lattice. In many compounds, uranium is substituted with the uranyl ion (UO 2 ) 2+ Since the uranyl ion is characterized by linear OUO bonds, there is typically an upper limit to the substitution that can be achieved, on the order of a few mole percent relative to the substituted sites. M 2+ When ion is substituted, M 2+ and (UO 2 ) 2+ There may be size constraints between the centers, which may cause distortions in the host lattice and / or compensating defects in the host lattice. 6+ Concentration quenching of emission usually occurs before complete substitution is achieved. In contrast, the phosphors of the present disclosure do not contain UO as part of the host lattice. 2 M species present 2+ It contains a high concentration of uranyl ions, about 40 mol % based on the total number of moles of cations.
[0045] The phosphor material is Eu 3+ ,Pr 3+ Or Sm 3+ A small number of activator ions are incorporated into the compound's host lattice. In another embodiment, the phosphor material may be doped with both activator ions and counter ions. Eu 3+ ,Pr 3+ Or Sm 3+ A small number of activator ions, such as Li, and counter ions, such as alkali ions, are incorporated into the host lattice of the compound. + , Na + , K + , Rb + Or Cs + Examples include:
[0046] In some embodiments, the phosphor material may include activator ions in an amount of about 0.001 to about 10 mol %. In other embodiments, the activator ions may be present in an amount of about 0.01 mol % to about 10 mol %. In other embodiments, the activator ions may be present in an amount of about 0.1 mol % to about 10 mol %. In other embodiments, the activator ions may be present in an amount of about 0.5 to about 5 mol %. In other embodiments, the activator may be present in an amount of about 1 to about 3 mol %. In other embodiments, the activator ions may be present in an amount of about 0.01 mol % to about 1 mol %. In other embodiments, the activator ions may be present in an amount of about 0.05 mol % to about 1 mol %. In other embodiments, the activator ions may be present in an amount of about 0.1 mol % to about 1 mol %. In other embodiments, the activator ions may be present in an amount of about 0.5 mol % to about 1 mol %.
[0047] The uranium-based phosphor material may be co-doped with one or more counter ions. In one embodiment, the counter ions may be present in an amount of about 0.01 mol % to about 10 mol %. In one embodiment, the counter ions may be present in an amount of about 0.1 to about 10 mol %. In another embodiment, the counter ions may be present in an amount of about 0.5 to about 5 mol %. In another embodiment, the counter ions may be present in an amount of about 1 to about 3 mol %. In another embodiment, the counter ions may be present in an amount of about 0.01 mol % to about 1 mol %. In another embodiment, the counter ions may be present in an amount of about 0.05 mol % to about 1 mol %. In another embodiment, the counter ions may be present in an amount of about 0.1 mol % to about 1 mol %. In another embodiment, the counter ions may be present in an amount of about 0.5 mol % to about 1 mol %.
[0048] In another aspect, a uranium-based phosphor is provided having the formula (III), (IV) or (V): A 2 UO 2 [P,V] 2 O 7 (III), A 4 UO 2 ([P,V]O 4 ) 2 (IV) or AUO2 ([P,V]O 3 ) 3 (V), where A is a uranium-based phosphor that is Li, Na, K, Rb, Cs, or a combination thereof.
[0049] Uranium-based phosphors can absorb at 450 nm and emit in the green range. Phosphors with formulas III, IV, and V emit bright green, which can provide a high color gamut for displays. For general lighting, the phosphors fill the dark blue-green gap to provide a full spectrum for human-centric lighting with higher CRI values.
[0050] In some embodiments, the uranium-based phosphor has Formula III:A 2 UO 2 [P,V] 2 O 7 where A is Li, Na, K, Rb, Cs, or a combination thereof. 2 UO 2 P 2 O 7 , Na 2 UO 2 P 2 O 7 , Rb 2 UO 2 P 2 O 7 and Cs 2 UO 2 P 2 O 7 Examples include:
[0051] In some embodiments, the uranium-based phosphor has Formula IV:A 4 UO 2 ([P,V]O 4 ) 2 where A is Li, Na, K, Rb, Cs, or a combination thereof. 4 UO 2 (PO 4 ) 2 Or K 4 UO 2 (VO 4 ) 2Examples include:
[0052] In some embodiments, the uranium-based phosphor has the formula V:AUO 2 ([P,V]O 3 ) 3 where A is Li, Na, K, Rb, Cs, or a combination thereof. In one embodiment, the phosphor has the formula: NaUO 2 P 3 O 9 It's fine.
[0053] In one embodiment, the uranium-based phosphor is K 2 UO 2 P 2 O 7 , Na 2 UO 2 P 2 O 7 , Rb 2 UO 2 P 2 O 7 , Cs 2 UO 2 P 2 O 7 , K 4 UO 2 (PO 4 ) 2 or NaUO 2 P 3 O 9 The phosphor emits bright green light and can provide a wide color gamut for display applications.
[0054] The uranium-based phosphor materials of the present disclosure can be produced by firing a mixture of precursors under an oxidizing atmosphere. Non-limiting examples of suitable precursors include suitable metal oxides, hydroxides, alkoxides, carbonates, nitrates, aluminates, silicates, citrates, oxalates, carboxylates, tartrates, stearates, nitrites, peroxides, phosphates, pyrophosphates, alkali salts, and combinations thereof. Materials suitable for use as precursors include BaCO 3 , BaHPO 4 , B.A. 3 (PO 4 ) 2、Ba 2 Q 2 O 7 、Ba 2 Zn(PO 4 ) 2 、BaZnP 2 O 7 、Ba(OH) 2 、Ba(C 2 O 4 )、Ba(C 2 A 3 O 2 ) 2 、Ba 3 (C 6 A 5 O 7 ) 2 、Ba(NO 3 ) 2 、CaCO 3 、Cs 2 CO 3 、EGG 2 NIGHT 4 -4H 2 O、KH 2 NIGHT 4 、K 2 HPO 4 、K 2 CO 3 、Li 2 CO 3 、Li 2 HPO 4 、LiH 2 NIGHT 4 、Mg(C 2 O 4 )、Mg(C 2 A 3 O 2 ) 2 、Mg(C 6 A 6 O 7 ), MgCO 3 、MgO、Mg(OH) 2 、Mg 3 (NIGHT 4 ) 2 、Mg 2 Q 2 O 7 、Mg 2 Ba(PO 4 ) 2 、MgHPO 4 、Mg(NO 3 ) 2、NaH 2 NIGHT 4 、So 2 HPO 4 、So 2 CO 3 、NH 4 MgPO 4 、(NH 4 ) 2 HPO 4 、NH 4 VO 3 、Rb 2 CO 3 、SrCO 3 、Zn(C 2 O 4 )、Zn(C 2 A 3 O 2 ) 2 、Zn 3 (C 6 A 5 O 7 ) 2 、ZnCO 3 、ZnO、Zn(OH) 2 、Zn 3 (NIGHT 4 ) 2 、Zn 2 Q 2 O 7 、Zn 2 Ba(PO 4 ) 2 、ZnHPO 4 、Zn(NO 3 ) 2 、NH 4 ZnPO 4 、UO 2 、UO 2 (NO 3 ) 2 、(UO 2 ) 2 Q 2 O 7 、(UO 2 ) 3 (NIGHT 4 ) 2 、NH 4 (UO 2 )NIGHT 4 、UO 2 CO 3 、UO 2 (C 2 A 3 O2 ) 2 , U.O. 2 (C 2 O 4 ), H(UO 2 )PO 4 , U.O. 2 (OH) 2 , and ZnUO 2 (C 2 H 3 O 2 ) 4 , as well as various hydrates. For example, a suitable amount of BaCO 3 , ZnO, and UO 2 Add an appropriate amount of (NH 4 ) 2 HPO 4 and then firing the mixture under air atmosphere to obtain the exemplary phosphor BaZnUO 2 (PO 4 ) 2 can be produced. The precursors can be in solid form or in solution. Non-limiting examples of solvents include water, ethanol, acetone, and isopropanol, with suitability depending primarily on the solubility of the precursor in the solvent. After firing, the phosphor can be crushed to break up any agglomerates that may have formed during the firing procedure.
[0055] The mixture of starting materials for producing the phosphor is Eu 2 O 3 , Sm 2 O 3 , or Pr 6 O 11 Activator precursor oxide compounds such as EuPO, 4 , SmPO 4 , or PrPO 4 These include, but are not limited to, precursor phosphate compounds such as:
[0056] The mixture of starting materials for producing the phosphor can also include one or more low melting flux materials, such as boric acid, borate compounds such as lithium tetraborate, alkaline phosphates, and combinations thereof. Non-limiting examples include (NH 4 ) 2HPO 4 (DAP), Li 3 PO 4 , Na 3 PO 4 , NaBO 3 -H 2 O, Li 2 B 4 O 7 , K 4 P 2 O 7 , Na 4 P 2 O 7 , H 3 BO 3 , and B 2 O 3 Fluxes can reduce the firing temperature and / or firing time of the phosphor. When using a flux, it may be desirable to wash the final phosphor product with a suitable solvent to remove residual soluble impurities that may come from the flux.
[0057] The calcination of the samples is generally carried out in air, but uranium is calcined in its highest oxidation state (U 6+ ) containing oxygen partial pressures exceeding 1 atmosphere. 2 or other wet or dry oxidizing atmosphere at a temperature of about 300°C to about 1300°C, particularly about 500°C to about 1200°C, for a time sufficient to convert the mixture to the phosphor. The required firing time may range from about 1 to 20 hours, depending on the amount of mixture being fired, the degree of contact between the solids and the atmospheric gases, and the degree of mixing while the mixture is fired or heated. The mixture may be rapidly brought to the final temperature and held there, or the mixture may be heated to the final temperature at a slower rate, such as about 2°C / min to about 200°C / min.
[0058] The phosphor can be ground or milled by conventional methods to a smaller particle size, if desired. In some embodiments, the median particle size of the phosphor can be in the range of about 1 to about 50 microns. In other embodiments, the median particle size can be in the range of about 15 to about 35 microns. In other embodiments, the median particle size can be about 30 microns or less.
[0059] In another embodiment, the phosphor is in the form of particles having a particle size in the range of about 0.1 μm to about 15 μm. In another embodiment, the particle size is in the range of about 0.1 μm to about 10 μm. In another embodiment, the particle size distribution is D50 less than 15 μm, particularly D50 less than 10 μm, particularly D50 less than 5 μm, or D50 less than 3 μm, or D50 less than 2 μm, or D50 less than 1 μm. In another embodiment, the particle size distribution D50 may be in the range of about 0.1 μm to about 5 μm. In another embodiment, the D50 particle size is in the range of about 0.1 μm to about 3 μm. In another embodiment, the D50 particle size is in the range of about 0.1 μm to about 1 μm. In another embodiment, the D50 particle size is in the range of about 1 μm to about 5 μm. D50(D 50 D90 or D 90 D10 or D is the particle size of a volume distribution that is larger than the particle size of 90% of the particles in the distribution. 10 is the particle size of the volume distribution that is larger than the size of 10% of the particles in the distribution. The particle size of phosphors can be conveniently measured by laser diffraction or optical microscopy, and commercially available software can generate particle size distributions and spans. Span is a measure of the width of the particle size distribution curve of a granular material or powder and is defined according to the following equation:
number
[0060] In another aspect, a composition is provided. The composition includes an activated uranium-based phosphor and a red-emitting phosphor. The uranium-based phosphor is (i) a phosphor having formula I or II, [Ba 1-a-b Sr a Ca b ] x [Mg,Zn] y (UO 2) z ([P,V]O 4 ) 2(x+y+z) / 3 (I) [Ba 1-a-b Sr a Ca b ] p (UO 2 ) q [P,V] r O (2p+2q+5r) / 2 (II), The phosphor having the formula I or II is 3+ , Sm 3+ or mixtures thereof, wherein 0≦a≦1, 0≦b≦1, 0.75≦x≦1.25, 0.75≦y≦1.25, 0.75≦z≦1.25, 2.5≦p≦3.5, 1.75≦q≦2.25, and 3.5≦r≦4.5; (ii) a phosphor having the formula I or II, wherein the phosphor having the formula I or II is selected from the group consisting of Eu 3+ ,Pr 3+ , Sm 3+ and mixtures thereof, and a counterion comprising one or more alkali metal ions; and (iii) a phosphor having formula III, A 2 UO 2 [P,V] 2 O 7 (III) The phosphor having formula III is 3+ ,Pr 3+ , Sm 3+ and mixtures thereof, where A is selected from phosphors that are Li, Na, K, Rb, Cs, or combinations thereof.
[0061] In another aspect, a composition is provided. The composition includes a uranium-based phosphor and a red-emitting phosphor. The uranium-based phosphor has the formula (III), (IV), or (V), A 2 UO 2 [P,V] 2 O 7 (III), A4 UO 2 ([P,V]O 4 ) 2 (IV), or AUO 2 ([P,V]O 3 ) 3 (V), where A is a uranium-based phosphor that is Li, Na, K, Rb, Cs, or a combination thereof.
[0062] In one embodiment, the red-emitting phosphor has Formula VI: A x MF y :Mn 4+ (VI) wherein A is Li, Na, K, Rb, Cs, or a combination thereof; M is Si, Ge, Sn, Ti, Zr, Al, Ga, In, Sc, Hf, Y, La, Nb, Ta, Bi, Gd, or a combination thereof; and x is MF y is the absolute value of the charge of the ion, and y is 5, 6, or 7.
[0063] The red-emitting phosphor of formula VI is emissively and / or optically coupled to an LED light source. Phosphors of formula I are described in U.S. Patent Nos. 7,497,973 and 8,906,724, and related patents assigned to General Electric Company. Examples of red-emitting phosphors of formula VI include K 2 (TiF 6 ):Mn 4+ , K 2 (SnF 6 ):Mn 4+ , Cs 2 (TiF 6 ):Mn 4+ , Rb 2 (TiF 6 ):Mn 4+ , Cs 2 (SiF 6 ):Mn 4+ , Rb 2 (SiF 6 ):Mn 4+ , Na 2 (SiF 6 ):Mn 4+ , Na 2(TiF 6 ):Mn 4+ , Na 2 (ZrF 6 ):Mn 4+ , K 3 (ZrF 7 ):Mn 4+ , K 3 (BiF 7 ):Mn 4+ , K 3 (Y.F. 7 ):Mn 4+ , K 3 (LaF 7 ):Mn 4+ , K 3 (GdF 7 ):Mn 4+ , K 3 (NbF 7 ):Mn 4+ Or K 3 (TaF 7 ):Mn 4+ In certain embodiments, the phosphor of formula VI is 2 SiF 6 :Mn 4+ (PFS).
[0064] In one embodiment, the red-emitting phosphor has a Mn content or Mn % of at least 1 wt %. In another embodiment, the red-emitting phosphor has a Mn content of at least 1.5 wt %. In another embodiment, the red-emitting phosphor has a Mn content of at least 2 wt %. In another embodiment, the red-emitting phosphor has a Mn % of at least 3 wt %. In another embodiment, the Mn % is greater than 3.0 wt %. In another embodiment, the content of Mn in the red-emitting phosphor is from about 1 wt % to about 4 wt %.
[0065] In one embodiment, Mn 4+ Red-emitting phosphors based on phosphor-activated complex fluoride materials can be at least partially coated with a surface coating to increase the stability of the phosphor particles, to resist agglomeration by modifying the surface of the particles, and to increase the zeta potential of the particles. In one embodiment, the surface coating can be a metal fluoride, silica, or an organic coating. In one embodiment, Mn4+ Red-emitting phosphors based on phosphor-activated complex fluoride materials are at least partially coated with a metal fluoride to increase the positive zeta potential and reduce aggregation. In one embodiment, the metal fluoride coating is MgF 2 , CaF 2 , SrF 2 , BaF 2 , AgF, ZnF 2 , AlF 3 , or a combination thereof. In another embodiment, the metal fluoride coating is present in an amount of about 0.1% to about 10% by weight. In another embodiment, the metal fluoride coating is present in an amount of about 0.1% to about 5% by weight. In another embodiment, the metal fluoride coating is present in an amount of about 0.3% to about 3% by weight. Mn 4+ Metal fluoride coated red-emitting phosphors based on complex fluoride materials activated by are prepared as described in WO 2018 / 093832, U.S. Patent Application Publication No. 2018 / 0163126, and U.S. Patent Application Publication No. 2020 / 0369956, the entire contents of each of which are incorporated herein by reference.
[0066] The red-emitting phosphor having Formula VI can be used in any particle size desired. In some embodiments, the median particle size of the phosphor can range from about 1 to about 50 microns. In other embodiments, the median particle size can range from about 15 to about 35 microns. In other embodiments, the median particle size can be about 30 microns or less.
[0067] In one embodiment, the red-emitting phosphor is in the form of particles having a particle size in the range of about 0.1 μm to about 15 μm. In another embodiment, the particle size is in the range of about 0.1 μm to about 10 μm. In another embodiment, the particle size distribution is D50 less than 15 μm, particularly D50 less than 10 μm, particularly D50 less than 5 μm, or D50 less than 3 μm, or D50 less than 2 μm, or D50 less than 1 μm. In another embodiment, the particle size distribution D50 may be in the range of about 0.1 μm to about 5 μm. In another embodiment, the D50 particle size is in the range of about 0.1 μm to about 3 μm. In another embodiment, the D50 particle size is in the range of about 0.1 μm to about 1 μm. In another embodiment, the D50 particle size is in the range of about 1 μm to about 5 μm. D50(D 50 D90 or D 90 D10 or D is the particle size of a volume distribution that is larger than the particle size of 90% of the particles in the distribution. 10 is the particle size of the volume distribution that is larger than the size of 10% of the particles in the distribution. The particle size of phosphors can be conveniently measured by laser diffraction or optical microscopy, and commercially available software can generate particle size distributions and spans. Span is a measure of the width of the particle size distribution curve of a granular material or powder and is defined according to the following equation:
number
[0068] In another aspect, a composition is provided. The composition includes an activated uranium-based phosphor and at least one other luminescent material. The uranium-based phosphor is (i) a phosphor having formula I or II, [Ba 1-a-b Sr a Ca b ] x [Mg,Zn] y (UO 2 ) z([P,V]O 4 ) 2(x+y+z) / 3 (I) [Ba 1-a-b Sr a Ca b ] p (UO 2 ) q [P,V] r O (2p+2q+5r) / 2 (II), The phosphor having the formula I or II is 3+ , Sm 3+ or mixtures thereof, wherein 0≦a≦1, 0≦b≦1, 0.75≦x≦1.25, 0.75≦y≦1.25, 0.75≦z≦1.25, 2.5≦p≦3.5, 1.75≦q≦2.25, and 3.5≦r≦4.5; (ii) a phosphor having the formula I or II, wherein the phosphor having the formula I or II is selected from the group consisting of Eu 3+ ,Pr 3+ , Sm 3+ and mixtures thereof, and a counterion comprising one or more alkali metal ions; and (iii) a phosphor having formula III, A 2 UO 2 [P,V] 2 O 7 (III) The phosphor having formula III is 3+ ,Pr 3+ , Sm 3+ and mixtures thereof, where A is selected from phosphors that are Li, Na, K, Rb, Cs, or combinations thereof.
[0069] In another aspect, a composition is provided. The composition includes a uranium-based phosphor and at least one other luminescent material. The uranium-based phosphor has the formula (III), (IV), or (V):
[0070] A uranium-based phosphor having the formula (III), (IV) or (V): A 2 UO2 [P,V] 2 O 7 (III), A 4 UO 2 ([P,V]O 4 ) 2 (IV), or AUO 2 ([P,V]O 3 ) 3 (V), where A is a uranium-based phosphor that is Li, Na, K, Rb, Cs, or a combination thereof.
[0071] The phosphor compositions according to the present disclosure may include one or more other luminescent materials in addition to the uranium-based phosphor material. Additional luminescent materials, such as blue, yellow, red, orange, or other color phosphors, can be used in the phosphor composition to customize the white color of the resulting light and to produce specific spectral output distributions.
[0072] Suitable phosphors for use in the phosphor composition include ((Sr 1-z [Ca,Ba,Mg,Zn] z ) 1-(x+w) [Li,Na,K,Rb] w Cex) 3 (Al 1-y S y )O 4+y+3(x-w) F 1-y-3(x-w) , 0 <x≦0.10、0≦y≦0.5、0≦z≦0.5、0≦w≦x;[Ca,Ce] 3 Sc 2 S 3 O 12 (CaSiG);[Sr,Ca,Ba] 3 Al 1-x S x O 4+x F 1-x :Ce 3+ (SASOF));[Ba,Sr,Ca] 5 (PO 4 ) 3 [Cl,F,Br,OH]:Eu 2+ ,Mn 2+ ;[Ba,Sr,Ca]BPO 5 :EU 2+ ,Mn2+ ; [Sr, Ca] 10 (PO 4 ) 6 * vB 2 O 3 : Eu 2+ (where 0 < v ≤ 1); Sr 2 Si 3 O 8 * 2SrCl 2 : Eu 2+ ; [Ca, Sr, Ba] 3 MgSi 2 O 8 : Eu 2+ , Mn 2+ ; BaAl 8 O 13 : Eu 2+ ; 2SrO * 0.84P 2 O 5 *0.16B 2 O 3 : Eu 2+ ; [Ba, Sr, Ca]MgAl 10 O 17 : Eu 2+ , Mn 2+ ; [Ba, Sr, Ca]Al 2 O 4 : Eu 2+ ; [Y, Gd, Lu, Sc, La]BO 3 : Ce 3+ , Tb 3+ ; ZnS: Cu + , Cl - ; ZnS: Cu + , Al 3+ ; ZnS: Ag + , Cl - ; ZnS: Ag + , Al 3+ ; [Ba, Sr, Ca] 2 Si 1-n O 4-2n : Eu 2+ (where 0 ≤ n ≤ 0.2); [Ba, Sr, Ca] 2 [Mg, Zn]Si 2 O 7 : Eu 2+ ; [Sr, Ca, Ba][Al, Ga, In] 2 S 4 : Eu2+ ; [Y, Gd, Tb, La, Sm, Pr, Lu] 3 [Al, Ga] 5-a O 12-3 / 2a :Ce 3+ (where 0 ≦ a ≦ 0.5); [Ca, Sr] 8 [Mg, Zn](SiO 4 ) 4 Cl 2 :Eu 2+ ,Mn 2+ ;Na 2 Gd 2 B 2 O 7 :Ce 3+ ,Tb 3+ ; [Sr, Ca, Ba, Mg, Zn] 2 P 2 O 7 :Eu 2+ ,Mn 2+ ; [Gd, Y, Lu, La] 2 O 3 :Eu 3+ ,Bi 3+ ; [Gd, Y, Lu, La] 2 O 2 S:Eu 3+ ,Bi 3+ ; [Gd, Y, Lu, La]VO 4 :Eu 3+ ,Bi 3+ ; [Ca, Sr, Mg]S:Eu 2+ ,Ce 3+ ;SrY 2 S 4 :Eu 2+ ;CaLa 2 S 4 :Ce 3+ ; [Ba, Sr, Ca]MgP 2 O 7 :Eu 2+ ,Mn 2+ ; [Y, Lu] 2 WO 6 :Eu 3+ ,Mo 6+ ; [Ba, Sr, Ca] b Si g N m :Eu 2+ (where 2b + 4g = 3m); Ca 3 (SiO 4 )Cl2 : Eu 2+ ; [Lu, Sc, Y, Tb] 2-u-v Ce v Ca 1+u Li w Mg 2-w P w [Si, Ge] 3-w O 12-u / 2 (where 0.5 ≤ u ≤ 1, 0 < v ≤ 0.1, and 0 ≤ w ≤ 0.2); [Y, Lu, Gd] 2-m [Y, Lu, Gd]Ca m Si 4 N 6+m C 1-m : Ce 3+ (where 0 ≤ m ≤ 0.5); [Lu, Ca, Li, Mg, Y], Eu 2+ and / or Ce 3+ doped α-SiAlON; Sr(LiAl 3 N 4 ): Eu 2+ , [Ca, Sr, Ba]SiO 2 N 2 : Eu 2+ , Ce 3+ ; β-SiAlON: Eu 2+ ; 3.5MgO * 0.5MgF 2 * GeO 2 : Mn 4+ ; Ca 1-c-f Ce c Eu f Al 1+c Si 1-c N 3 (where 0 ≤ c ≤ 0.2, 0 ≤ f ≤ 0.2); Ca 1-h-r Ce h Eu r Al 1-h (Mg, Zn) h SiN 3 , (where 0 ≤ h ≤ 0.2, 0 ≤ r ≤ 0.2); Ca 1-2s-t Ce s [Li, Na] s Eu t AlSiN 3 , (where 0 ≤ s ≤ 0.2, 0 ≤ t ≤ 0.2, s + t > 0); [Sr, Ca]AlSiN 3 : and Eu 2+ , Ce3+ ,Li 2 CaSiO 4 :EU 2+ These include, but are not limited to:
[0073] In one embodiment, the additional emissive material may be a red-emitting phosphor of Formula VI above, A x MF y :Mn 4+ (VI) wherein A is Li, Na, K, Rb, Cs, or a combination thereof; M is Si, Ge, Sn, Ti, Zr, Al, Ga, In, Sc, Hf, Y, La, Nb, Ta, Bi, Gd, or a combination thereof; and x is MF y is the absolute value of the charge of the ion, and y is 5, 6, or 7.
[0074] In a particular embodiment, the additional phosphor is [Y,Gd,Lu,Tb] 3 [Al,Ga] 5 O 12 :Ce 3+ , β-SiAlON:Eu 2+ [Sr,Ca,Ba][Ga,Al] 2 S 4 :EU 2+ , [Li,Ca]α-SiAlON:Eu 2+ , [Ba,Sr,Ca] 2 S 5 N 8 :EU 2+ , [Ca,Sr]AlSiN 3 :EU 2+ , [Ba,Sr,Ca]LiAl 3 N 4 :EU 2+ , [Sr,Ca,Mg]S:Eu 2+ , [Ba,Sr,Ca] 2 S 2 O 4 :EU 2+ and K 2 SiF 6 :Mn 4+ Examples include:
[0075] Other additional emissive materials suitable for use in the phosphor composition may include electroluminescent polymers such as polyfluorenes, preferably poly(9,9-dioctylfluorene) and its copolymers, e.g., poly(9,9'-dioctylfluorene-co-bis-N,N'-(4-butylphenyl)diphenylamine) (F8-TFB); poly(vinylcarbazole) and polyphenylenevinylene and their derivatives. Additionally, the emissive layer may include blue, yellow, orange, green or red phosphorescent dyes or metal complexes, quantum dot materials, or combinations thereof. Materials suitable for use as phosphorescent dyes include, but are not limited to, tris(1-phenylisoquinoline)iridium(III) (red dye), tris(2-phenylpyridine)iridium (green dye), and iridium(III) bis(2-(4,6-difluorenephenyl)pyridinato-N,C2) (blue dye). Commercially available fluorescent and phosphorescent metal complexes from ADS (American Dyes Source) can also be used. ADS green dyes include ADS060GE, ADS061GE, ADS063GE, and ADS066GE, ADS078GE, and ADS090GE. ADS blue dyes include ADS064BE, ADS065BE, and ADS070BE. ADS red dyes include ADS067RE, ADS068RE, ADS069RE, ADS075RE, ADS076RE, ADS067RE, and ADS077RE.
[0076] Exemplary QD materials include II-IV compound semiconductors such as CdS, CdSe, CdS / ZnS, CdSe / ZnS, or CdSe / CdS / ZnS; CdTe, ZnSe, ZnTe, ZnS, HgTe, HgS, HgSe, CdSeTe, CdSTe, ZnSeS, ZnSeTe, ZnSTe, HgSeS, HgSeTe, HgSTe, CdZnS, CdZnSe, CdZnTe, CdHgS, CdHgSe, CdHgTe, HgZnS, HgZnSe, HgZnTe, CdZnSeS, CdZnSeTe, CdZnSTe, CdHgSeS, CdHgSeTe, CdHgSTe, HgZn Group II-VI compounds such as SeS, HgZnSeTe, and HgZnSTe; Group III-V or Group IV-VI compound semiconductors such as GaN, GaP, GaNP, GaNAs, GaPAs, GaAs, GaAlNP, GaAlNAs, GaAlPAs, GaInNP, GaInNAs, GaInPAs, AlN, AlNP, AlNAs, AlP, AlPAs, AlAs, InN, InNP, InP, InNAs, InPAs, InAS, InAlNP, InAlNAs, InAlPAs, PbS / ZnS, and PbSe / ZnS; Group IV compounds such as Si, Ge, SiC, and SiGe; and CuInS 2 , CuInSe 2 , CuGaS 2 , CuGaSe 2 , AgInS 2 , AgInSe 2 , AgGaS 2 , AgGaSe 2 Chalcopyrite-type compounds, or ABX, including, but not limited to, 3 Examples of perovskite QDs include, but are not limited to, perovskite QDs having the formula: where A is cesium, methylammonium, or formamidinium, B is lead or tin, and C is chloride, bromide, or iodide.
[0077] In one embodiment, the perovskite quantum dots may be CsPbX3, where X is Cl, Br, I, or a combination thereof. The average size of the QD material may range from about 2 nm to about 20 nm. The surface of the QD particles may be further modified with ligands such as amine ligands, phosphine ligands, phosphatides, and polyvinylpyridines. In one aspect, the red phosphor may be the quantum dot material.
[0078] All semiconductor quantum dots may have a suitable shell or coating for passivation and / or environmental protection. The QD material may be a core / shell QD comprising a core, at least one shell coated on the core, and an outer coating comprising one or more ligands, preferably organic polymeric ligands. Exemplary materials for making core-shell QDs include Si, Ge, Sn, Se, Te, B, C (including diamond), P, Co, Au, BN, BP, BAs, AlN, AlP, AlAs, AlSb, GaN, GaP, GaAs, GaSb, InN, InP, InAs, InSb, AlN, AlP, AlAs, AlSb, GaN, GaP, GaAs, GaSb, ZnO, ZnS, ZnSe, ZnTe, CdS, CdSe, CdSeZn, CdTe, HgS, HgSe, HgTe, BeS, BeSe, BeTe, MgS, MgSe, MnS, MnSe, GeS, GeSe, GeTe, SnS, SnSe, SnTe, PbO, PbS, PbSe, PbTe, CuF, CuCl, CuBr, CuI, Si 3 N 4 , Ge 3 N 4 , Al 2 O 3 , [Al, Ga, In] 2 [S, Se, Te] 3 , and suitable combinations of two or more such materials. Exemplary core-shell luminescent nanocrystals include, but are not limited to, CdSe / ZnS, CdSe / CdS, CdSe / CdS / ZnS, CdSeZn / CdS / ZnS, CdSeZn / ZnS, InP / ZnS, PbSe / PbS, PbSe / PbS, CdTe / CdS, and CdTe / ZnS.
[0079] In one embodiment, the phosphor composition may include scattering particles. In one embodiment, the scattering particles have a particle size of at least 1 μm. In another embodiment, the scattering particles have a particle size of about 1 μm to about 10 μm. In another embodiment, the scattering particles are titanium dioxide, aluminum oxide (Al 2 O 3 ), zirconium oxide, indium tin oxide, cerium oxide, tantalum oxide, zinc oxide, magnesium fluoride (MgF 2 ), calcium fluoride (CaF 2 ), strontium fluoride (SrF 2 ), barium fluoride (BaF 2 ), silver fluoride (AgF), aluminum fluoride (AlF 3 ), or a combination thereof.
[0080] The ratio of each of the individual phosphors and other luminescent materials in the phosphor composition can vary depending on the desired light output characteristics. The relative proportions of the individual phosphors and other luminescent materials in the various phosphor compositions can be adjusted so that when their emissions are mixed and used in a device, such as a lighting device, they produce visible light at predetermined x and y values on the CIE chromaticity diagram.
[0081] In one embodiment, the phosphor composition may include a uranium-based phosphor having formula III, IV, or V, and a red phosphor having formula VI. 4 UO 2 (PO 4 ) 2 , K 4 UO 2 (PO 4 ) 2 or NaUO 2 P 3 O 9 Uranium-based phosphors such as K 2 SiF 6 :Mn 4 Includes:
[0082] The phosphor composition may be in the form of an ink or slurry composition that can be applied to a substrate, such as an LED light source, or formed into a film. The ink composition may be blended with a binder or solvent.
[0083] Examples of binders include, but are not limited to, silicone polymers, polysiloxanes, ethyl cellulose, polystyrene, polyacrylates, polymethyl acrylate (PMA), polymethyl methacrylate (PMMA), polycarbonate, polyurethane, polyether ether ketone, polysulfone, polyphenylene sulfide, polyvinylpyrrolidone (PVP), polyethyleneimine (PEI), poly(1-naphthyl methacrylate), poly(vinyl phenyl sulfide) (PVPS), polyvinyl alcohol (PVA), polyvinyl butyral (PVB), poly(N-vinyl phthalimide), polyvinylidene fluoride (PDVF), poly(vinylidene fluoride-co-hexafluoropropylene) (PVDF-HFP), silicone materials, and UV-curable materials, such as epoxy resins, acrylic resins, acrylate resins, and urethane-based materials.
[0084] Examples of solvents include, but are not limited to, water, ethanol, acetone, and isopropanol.
[0085] In another aspect, a device is provided that includes an LED light source radiatively and / or optically coupled to an activated uranium-based phosphor material. (i) a phosphor having formula I or II, [Ba 1-a-b Sr a Ca b ] x [Mg,Zn] y (UO 2 ) z ([P,V]O 4 ) 2(x+y+z) / 3 (I) [Ba 1-a-b Sr a Ca b ] p (UO 2 )q [P,V] r O (2p+2q+5r) / 2 (II), The phosphor having the formula I or II is 3+ , Sm 3+ or mixtures thereof, wherein 0≦a≦1, 0≦b≦1, 0.75≦x≦1.25, 0.75≦y≦1.25, 0.75≦z≦1.25, 2.5≦p≦3.5, 1.75≦q≦2.25, and 3.5≦r≦4.5; (ii) a phosphor having the formula I or II, wherein the phosphor having the formula I or II is selected from the group consisting of Eu 3+ ,Pr 3+ , Sm 3+ and mixtures thereof, and a counterion comprising one or more alkali metal ions; and (iii) a phosphor having formula III, A 2 UO 2 [P,V] 2 O 7 (III) The phosphor having formula III is 3+ ,Pr 3+ , Sm 3+ and mixtures thereof, where A is selected from phosphors that are Li, Na, K, Rb, Cs, or combinations thereof.
[0086] In yet another aspect, a device is provided that includes an LED light source radiatively and / or optically coupled to a uranium-based phosphor having the formula (III), (IV) or (V): A 2 UO 2 [P,V] 2 O 7 (III), A 4 UO 2 ([P,V]O 4 ) 2 (IV) or AUO 2 ([P,V]O 3 )3 (V), where A is a uranium-based phosphor that is Li, Na, K, Rb, Cs, or a combination thereof.
[0087] In one embodiment, a lighting apparatus includes the device. In another embodiment, a backlight apparatus includes the device. In one embodiment, the device and lighting apparatus are for use in horticultural lighting. In one embodiment, the phosphor package is for use in horticultural lighting.
[0088] A device according to the present disclosure includes an LED light source radiatively coupled and / or optically coupled to one or more of the uranium-based phosphor materials, such as uranium-based phosphors having formula I, II, III, IV, or V. In some embodiments, the uranium-based phosphor may be an activated uranium-based phosphor having formula I, II, or III. FIG. 1 illustrates a device 10 according to one embodiment of the present disclosure. The device 10 includes an LED light source 12 and a phosphor composition 14 including the uranium-based phosphor material of the present disclosure. The LED light source 12 may be a UV or blue emitting LED. In some embodiments, the LED light source 12 produces blue light in the wavelength range of about 380 nm to about 460 nm. In the device 10, the phosphor composition 14 including the uranium-based phosphor material described herein is radiatively coupled and / or optically coupled to the LED light source 12. By radiatively coupled or coupled or optically coupled, it is meant that radiation from the LED light source 12 can excite the phosphor composition 14, and the phosphor composition 14 can emit light in response to excitation by the radiation. Phosphor composition 14 may be disposed on or in a portion of LED light source 12 or may be disposed remotely from LED light source 12. In some embodiments, the device may be a backlight unit for a display application.
[0089] The general description of the exemplary LED light sources described herein is directed to inorganic LED-based light sources. The most common white LEDs are based on blue or UV-emitting GaInN chips. In addition to inorganic LED light sources, the term LED light source is meant to encompass all LED light sources, such as semiconductor laser diodes (LDs), organic light-emitting diodes (OLEDs), or hybrids of LEDs and LDs. The LED light source may be a mini-LED or micro-LED that can be used for self-emissive displays. Furthermore, it should be understood that the LED light source may be replaced, supplemented, or augmented by another radiation source, unless otherwise stated, and references to semiconductors, semiconductor LEDs, or LED chips merely represent any suitable radiation source, including, but not limited to, LDs and OLEDs.
[0090] The phosphor composition 14 may be present in any form, such as a powder, glass, or composite, such as a phosphor-polymer composite or phosphor-glass composite. Furthermore, the phosphor composition 14 may be used as a layer, sheet, film, strip, dispersed particulate, or combinations thereof. In some embodiments, the phosphor composition 14 includes a uranium-based phosphor material in a glass form. In some of these embodiments, the device 10 may include the phosphor composition 14 in the form of a phosphor wheel (not shown). The phosphor wheel may include a uranium-based phosphor material embedded in glass. Phosphor wheels and related devices are described in WO 2017 / 196779.
[0091] The uranium-based phosphor material is optically coupled or radiatively connected to the LED light source. In one embodiment, a white light blend can be obtained by blending the uranium-based phosphor material with an additional luminescent material with an LED light source, such as a blue or UV LED. The pure uranium emission spectrum of the phosphor material has a narrow band emission in the green range near the center of the eye's sensitivity range. The phosphor material can absorb at 450 nm and fill the dark blue-green gap range of human-centric lighting, which results in a complete spectrum for general lighting and provides a high CRI value. The pure uranium spectrum can be used for display backlighting applications to provide a wide color gamut display.
[0092] In one embodiment, the uranium-based phosphor material is doped with activator ions that provide orange or red emission. In one embodiment, the uranium-based phosphor is doped with europium activator ions that have a red emission spectrally close to the eye's sensitivity range, which appears brighter to human vision. In one embodiment, the europium-doped uranium-based phosphor is combined with a yellow-green or green emitting phosphor, such as an yttrium-aluminum garnet (YAG) phosphor, and a blue-emitting or UV-emitting LED to prepare a white blend with high efficacy (lumens / watt) values. In another embodiment, the composition comprises an activated uranium-based phosphor and a red phosphor having formula VI.
[0093] In some embodiments, uranium-based phosphors may be used in horticulture lighting. In one embodiment, the horticulture lighting blend or composition includes Sm 3+ In another embodiment, the plant lighting composition includes a uranium-based phosphor doped with Pr and having a peak emission at about 650 nm. 3+ The phosphor includes a uranium-based phosphor doped with
[0094] 2 illustrates a lighting device or lamp 20 according to some embodiments. In one embodiment, the lighting device 20 may be a backlight device. The lighting device 20 includes an LED chip 22 and leads 24 electrically attached to the LED chip 22. The leads 24 may include thin wires supported by a thicker lead frame 26, or the leads 24 may include self-supporting electrodes and the lead frame may be omitted. The leads 24 provide current to the LED chip 22, thus causing it to emit light.
[0095] A layer 30 of phosphor composition including uranium-based phosphor material is disposed on the surface of the LED chip 22. The phosphor layer 30 can be disposed by any suitable method, for example, using a slurry or ink composition prepared by mixing the phosphor composition with a binder material or solvent (described above). In one such method, a silicone slurry in which the phosphor composition particles are randomly suspended or uniformly dispersed is disposed around the LED chip 22. This method is merely illustrative of possible locations of the phosphor layer 30 and the LED chip 22. The phosphor layer 30 can be coated on the light emitting surface of the LED chip 22 or directly by coating and drying the slurry on the LED chip 22. The light emitted by the LED chip 22 mixes with the light emitted by the phosphor composition to produce the desired light emission.
[0096] 2, the LED chip 22 may be encapsulated within an envelope 28. The envelope 28 may be formed of, for example, glass or plastic. The LED chip 22 may be surrounded by an encapsulant material 32. The encapsulant material 32 may be a low temperature glass, or a polymer or resin known in the art, such as an epoxy, silicone, epoxy-silicone, acrylate, or combinations thereof. In an alternative embodiment, the lighting device 20 may include only the encapsulant material 32 without the envelope 28. Both the envelope 28 and the encapsulant material 32 must be transparent to allow light to pass through those elements.
[0097] In some embodiments shown in Figure 3, the uranium-based phosphor material of phosphor composition 33 is interspersed within encapsulant material 32 instead of being formed directly on LED chip 22 as shown in Figure 2. Phosphor composition 33 can be interspersed within a portion of encapsulant material 32 or throughout the entire volume of encapsulant material 32. Blue or UV light emitted by LED chip 22 mixes with the light emitted by phosphor composition 33, and the mixed light is transmitted from lighting device 20.
[0098] In yet another embodiment, a layer 34 of phosphor composition including uranium-based phosphor material is coated on the surface of the envelope 28 instead of being formed on the LED chip 22 as shown in FIG. 4. As shown, the phosphor layer 34 is coated on the inner surface 29 of the envelope 28, but the phosphor layer 34 may be coated on the outer surface of the envelope 28 if desired. The phosphor layer 34 may be coated on the entire surface of the envelope 28 or only on the top of the inner surface 29 of the envelope 28. The UV / blue light emitted by the LED chip 22 mixes with the light emitted by the phosphor layer 34, and the mixed light is transmitted outward. Of course, the phosphor composition may be located in any two or all three locations (as shown in FIGS. 2-4), or in any other suitable location, such as a location separate from the envelope 28, away from the LED chip 22, or integrated into the LED chip 22. In one embodiment, the phosphor layer 34 may be a film and may be located away from the LED chip 22. In another embodiment, the phosphor layer 34 may be a film and disposed on the LED chip 22. In some embodiments, the phosphor layer 34 may be applied to the LED chip 22 as an ink composition. In some embodiments, the phosphor layer 34 may be applied to the LED chip 22 as an ink composition and dried to form a film on the LED chip 22. In some embodiments, the phosphor composition may be a single layer or multiple layers. In some embodiments, the film is a multi-layer structure, each layer of the multi-layer structure includes at least one phosphor or quantum dot material. In another embodiment, the device structure includes a layer of the phosphor composition on the LED chip and a remote layer including a quantum dot material. In another embodiment, the device structure includes a layer of the phosphor composition on the LED chip and a remote layer including a quantum dot material and a phosphor material. In another embodiment, the device structure includes a layer of the phosphor composition on the LED chip and a film including a quantum dot material disposed away from the LED chip. In another embodiment, the device structure includes a layer of the phosphor composition on the LED chip and a film including a quantum dot material and a phosphor material disposed away from the LED chip.
[0099] In any of the above structures, the lighting device 20 (FIGS. 2-4) may also include a plurality of scattering particles (not shown) embedded in the encapsulant material 32. The scattering particles may include, for example, alumina, silica, zirconia, or titania. The scattering particles effectively scatter the directional light emitted from the LED chip 22, preferably with a negligible amount of absorption.
[0100] In one embodiment, the lighting device 20 shown in FIG. 3 or FIG. 4 may be a backlight device. In another embodiment, the backlight device comprises a backlight unit 10. Some embodiments include a surface mounted device (SMD) type light emitting diode 50 for backlighting applications, for example as shown in FIG. 5. The SMD is "side-emitting" and has a light emitting window 52 at the protruding portion of the light guide member 54. The SMD package may include an LED chip as defined above and a phosphor composition including a green-emitting phosphor as described herein. In another embodiment, the device may be a direct-lit display.
[0101] The phosphor compositions described herein can be used to provide devices that generate white light for display applications, such as LCD backlight units, with a wide color gamut and high brightness, or devices that generate white light for general illumination purposes, with high brightness and high CRI values over a wide range of target color temperatures (2000K to 10,000K).
[0102] The devices of the present disclosure include lighting and display devices for general lighting and display applications. Examples of display devices include liquid crystal display (LCD) backlight units, televisions, computer monitors, vehicle displays, laptops, computer notebooks, mobile phones, smartphones, tablet computers, and other portable devices. When the display is a backlight unit, the uranium-based phosphor material may be incorporated into a film, sheet, or strip that is radiatively and / or optically coupled to an LED light source, as described in U.S. Patent Application Publication No. 2017 / 0254943. Examples of other devices include chromatic lamps, plasma screens, xenon-excited lamps, UV-excited marking systems, automotive headlamps, home and theater projectors, laser pump devices, and point sensors. This list of applications is meant to be merely illustrative and not exhaustive. In some embodiments, the display may be an eye-safe display with reduced harmful blue light emission.
[0103] In some embodiments, the device of the present disclosure includes a horticultural light. In one embodiment, the horticultural light can include a device including an LED light source radiatively and / or optically coupled to a uranium-based phosphor having formula (I), (II), (III), (IV) or (V). In another embodiment, the device can include a red phosphor having formula (VI). In another embodiment, the device includes a uranium-based phosphor having formula (I), (II), (III), (IV) or (V) and a red phosphor having formula (VI). In another embodiment, the horticultural light can include a device including an activated uranium-based phosphor having formula (I), (II) or (III) and a red phosphor having formula (VI), where the uranium-based phosphor is selected from the group consisting of Eu 3+ , Sm 3+ and / or Pr 3+In another embodiment, the horticultural lighting comprises a device including an activated uranium-based phosphor of (i), (ii) or (iii). In another embodiment, the horticultural lighting comprises a device having formula (I), (II) or (III) and a red phosphor having formula (VI), wherein the uranium-based phosphor is doped with an activator ion selected from the group consisting of Sm 3+ and / or Pr 3+ is doped.
[0104] In another embodiment, the horticultural lighting can include a phosphor package including the activated uranium-based phosphor of section (i), (ii) or (iii). In another embodiment, the horticultural lighting can include a composition including the uranium-based phosphor of section (i), (ii) or (iii) and a red phosphor having formula (VI). In some embodiments, the phosphor package is a film or sheet including the activated uranium-based phosphor dispersed therein. In other embodiments, the phosphor package includes the activated uranium-based phosphor dispersed in a medium or substrate. In some embodiments, the medium or substrate is transparent and can be used for solar plant lighting.
[0105] In some embodiments, a film containing a single phosphor material can be placed on a small LED, such as a micro-LED or mini-LED. In some embodiments, the film contains a red-emitting uranium-based phosphor material containing europium activator ions. The uranium-based phosphor material strongly absorbs UV / blue-emitting LED light and has a short decay time. The uranium-based phosphor material is stable in water and can be easily crushed or milled into small particle sizes for processing into films and can maintain good quantum efficiency. Because the phosphor material has high absorption, a minimal loading of phosphor material can be used in the film to make full conversion micro-LED displays or for use in applications where the thickness of the film layer is important. In some embodiments, the uranium-based phosphor can emit in both green and red, which is beneficial for preparing very thin single phosphor films with good mura measurements. In some embodiments, the uranium-based phosphor material can be prepared into films by inkjet printing, spin coating or slot die coating.
[0106] In another embodiment, the film comprises a phosphor particle size of about 0.1 to about 15 microns. In another embodiment, less than 5 microns. In another embodiment, the film comprises a phosphor particle size of about 0.1 microns to about 5 microns. In another embodiment, the film comprises a particle size of about 0.5 microns to about 5 microns. In another embodiment, the film comprises a particle size of about 0.1 microns to about 1 micron. In another embodiment, the film comprises a particle size of about 0.5 microns to about 1 micron. In another embodiment, the film comprises a particle size of about 1 micron to about 3 microns.
[0107] In some embodiments, the film may include scattering agents. In another embodiment, a brightness enhancement film, such as a dual brightness enhancement film (DBEF), can be used in the lighting device to increase brightness to the observer or to the plants when used in horticultural lighting.
[0108] Although specific features of various embodiments of the present disclosure may be shown in some drawings and not in others, this is for convenience only, and in accordance with the principles of the present disclosure, any feature of a drawing may be referenced and / or claimed in combination with any feature of any other drawing. EXAMPLES
[0109] Quantum efficiency measurements of example phosphors were performed on cured silicone tape. Phosphor particles were dispersed by mixing in a polyacrylate binder material or a two-part thermosetting polydimethylsiloxane elastomer (e.g., sold by Dow Corning as Sylgard® 184). Dispersed phosphor particles were prepared at a concentration of 0.5 g phosphor per 1.5 g silicone, from 0.12 g phosphor to 1.8 g silicone. The mixture was applied to silicone tape and cured. The quantum efficiency (QE) of the phosphor particles was measured for these films. QE measurements were reported for the QE of potassium fluoride sulfide phosphor (PFS) or β-SiAlON.
[0110] Example 1: Na 2 UO 2 P 2 O 7 Phosphor and 1% activator ion (Eu 3+ ,Pr 3+ , Sm 3+ , Tb 3+ and Dy 3+ ) doped Na 2 UO 2 P 2 O 7 Preparation of Na 2 CO 3 , H.U.O. 2 PO 4 -4H 2 O and NaH 2 PO 4were weighed out in a molar ratio of 0.5:1:1 and then placed in a Nalgene bottle containing zirconia media and ball milled for 2 hours. After the mixture was thoroughly blended, the powder was transferred to an alumina crucible and fired at 500°C for 5 hours, then the mixture was sieved through a 40 mesh sieve and blended again in the same Nalgene bottle for an additional 2 hours. The powder was transferred back to the alumina crucible and fired at 900°C for 5 hours. After the final firing, a yellow body colored powder was obtained. Na 2 UO 2 P 2 O 7 The emission spectrum of is shown in FIG. 6A.
[0111] 1% molar amount of Eu 3+ Doped Na 2 UO 2 P 2 O 7 To prepare 0.005 Eu 2 O 3 The Na in the blend was added. 2 CO 3 The same procedure as above was used, except that the amount of Eu was adjusted to 0.495. 3+ Doped Na 2 UO 2 P 2 O 7 The emission spectrum of is shown in FIG. 6B.
[0112] 1% molar amount of Pr 3+ Doped Na 2 UO 2 P 2 O 7 isEu 2 O 3 Instead of Pr 6 O 11 Except for the use of 1% molar amount of Eu 3+ Doped Na 2 UO 2 P 2 O 7 It was prepared in the same manner as Pr 3+ Doped Na 2 UO 2 P 2 O 7 The emission spectrum of is shown in FIG. 6C.
[0113] 1% molar amount of Sm 3+ Doped Na 2 UO 2 P 2 O 7 isEu 2 O 3 Instead of Sm 2 O 3 Except for the use of 1% molar amount of Eu 3+ Doped Na 2 UO 2 P 2 O 7 It was prepared in the same manner as Sm 3+ Doped Na 2 UO 2 P 2 O 7 The emission spectrum of is shown in FIG. 6D.
[0114] 1% molar amount of Tb 3+ Doped Na 2 UO 2 P 2 O 7 isEu 2 O 3 Instead of Tb 4 O 7 Except for the use of 1% molar amount of Eu 3+ Doped Na 2 UO 2 P 2 O 7 It was prepared in the same manner as Tb 3+ Doped Na 2 UO 2 P 2 O 7 The emission spectrum of is shown in FIG. 6E.
[0115] 1% molar amount of Dy 3+ Doped Na 2 UO 2 P 2 O 7 isEu 2 O 3 Instead of Dy 2 O 3 Except for the use of 1% molar amount of Eu 3+ Doped Na2 UO 2 P 2 O 7 It was prepared in the same manner as Dy 3+ Doped Na 2 UO 2 P 2 O 7 The emission spectrum of is shown in FIG. 6F.
[0116] 1%Eu 3+ and 1%Pr 3+ Doped Na 2 UO 2 P 2 O 7 To prepare Na 2 HPO 4 , H.U.O. 2 PO 4 -4H 2 O, Eu 2 O 3 , (NH 4 ) 2 HPO 4 and Pr 6 O 11 were weighed out in a molar ratio of 0.99:1:0.005:0.025:0.00167 and then placed in a Nalgene bottle containing zirconia media and ball milled for 2 hours. After the mixture was thoroughly blended, the powder was transferred to an alumina crucible and fired at 500°C for 5 hours, then the mixture was sieved through a 40 mesh sieve and blended again in the same Nalgene bottle for an additional 2 hours. The powder was transferred back to the alumina crucible and fired at 900°C for 5 hours. After the final firing, a yellow body colored powder was obtained. 2 UO 2 P 2 O 7 :EU 3+ :Pr 3+ The emission spectrum of is shown in FIG. 6G, and the results are shown in Table 1.
[0117] 1% molar amount of Eu 3+ and Sm 3+ Doped Na 2 UO 2 P 2 O 7 To prepare 0.00167 Pr 6 O11 to 0.005 Sm 2 O 3 The same procedure as above was used, except for replacing Na 2 UO 2 P 2 O 7 :EU 3+ ,Sm 3+ The emission spectrum of is shown in FIG. 6H, and the results are shown in Table 1.
[0118] The results are shown in Table 1. [Table 1]
[0119] The energy transfer is demonstrated by the difference in color coordinates ccx and ccy on the CIE chromaticity diagram. 3+ ,Pr 3+ and Sm 3+ Phosphor material doped with Na 2 UO 2 P 2 O 7 indicates the energy transfer from uranium ions to activator ions. For example, the phosphor Na 2 UO 2 P 2 O 7 has a ccx value of 0.2054 and a ccy value of 0.6689. 3+ Doped Na 2 UO 2 P 2 O 7 has a ccx value of 0.6448 and a ccy value of 0.3496, which indicates a significant difference in color change on the CIE chromaticity diagram, and the addition of the activator ion Eu 3+ This shows that there has been an energy transfer to the activator ion Tb. The energy transfer is also shown in FIG. 6B. The emission spectrum in FIG. 6B shows a significant shift in emission wavelength compared to the emission spectrum in FIG. 6A. 3+ and Dy 3+ Phosphor material doped with Na 2 UO 2 P 2 O 7does not show any energy transfer from the uranium ion to the activator ion. 2 UO 2 P 2 O 7 The difference in the ccx and ccy values compared to is minimal, and there is little change in the emission spectra of Figures 6E and 6F compared to that of Figure 6A, indicating that not all activator ions in the lanthanide group will work in uranium-based phosphors.
[0120] Activator ion Eu 3+ Doped Na 2 UO 2 P 2 O 7 shows a significant increase in quantum efficiency (QE). This is believed to be the first example of efficient energy transfer from uranium ions to europium activator ions. Figure 6B shows the Eu 3+ There is complete energy transfer to the ion, indicating that the uranium emission is completely quenched.
[0121] Activator ion Sm 3+ Doped Na 2 UO 2 P 2 O 7 indicates an increase in quantum efficiency. Activator ion Eu 3+ and Sm 3+ Co-doped Na 2 UO 2 P 2 O 7 The activator ion Eu also shows an increase in quantum efficiency. 3+ and Pr 3+ Co-doped Na 2 UO 2 P 2 O 7 Na 2 UO 2 P 2 O 7 Although the color shift was reduced compared to Example 1, the quantum efficiency was reduced. The following examples demonstrate how the quantum efficiency can be increased in phosphor samples.
[0122] Example 2: 2 UO 2 P 2 O 7 Phosphor and Co-doped K 2 UO 2 P 2 O 7 Preparation of K 2 CO 3 , H.U.O. 2 PO 4 -4H 2 O and KH 2 PO 4 were weighed out in a molar ratio of 0.5:1:1 and then placed in a Nalgene bottle containing zirconia media and ball milled for 2 hours. After the mixture was thoroughly blended, the powder was transferred to an alumina crucible and fired at 500°C for 5 hours, then the mixture was sieved through a 40 mesh sieve and blended again in the same Nalgene bottle for an additional 2 hours. The powder was transferred back to the alumina crucible and fired at 900°C for 5 hours. After firing, a yellow solid color powder was obtained. 2 UO 2 P 2 O 7 The emission spectrum of is shown in FIG. 7A.
[0123] 1% molar amount of Eu 3+ Doped K 2 UO 2 P 2 O 7 To prepare 0.005 Eu 2 O 3 Add K in the blend. 2 CO 3 The same procedure as above was used, except that the amount of Eu was adjusted to 0.495. 3+ Doped K 2 UO 2 P 2 O 7 The emission spectrum of is shown in FIG. 7B.
[0124] 1% molar amount of Sm 3+ Doped K 2 UO 2 P 2 O 7 isEu 2 O3 Instead of Sm 2 O 3 Except for the use of 1% molar amount of Eu 3+ Doped K 2 UO 2 P 2 O 7 It was prepared in the same manner as Sm 3+ Doped K 2 UO 2 P 2 O 7 The emission spectrum of is shown in FIG. 7C.
[0125] 1% molar amount of Pr 3+ Doped K 2 UO 2 P 2 O 7 isEu 2 O 3 Instead of Pr 6 O 11 Except for the use of 1% molar amount of Eu 3+ Doped K 2 UO 2 P 2 O 7 It was prepared in the same manner as Pr 3+ Doped K 2 UO 2 P 2 O 7 The emission spectrum of is shown in FIG. 7D.
[0126] The results are shown in Table 2. [Table 2]
[0127] The energy transfer is demonstrated by the difference in color coordinates ccx and ccy. 3+ , Sm 3+ and Pr 3+ Phosphor material K doped with 2 UO 2 P 2 O 7 indicates that there is energy transfer from the uranium ion to the activator ion. 3+ Doped K2 UO 2 P 2 O 7 The quantum efficiency (QE) of Sm is maintained, but 3+ and Pr 3+ Doped K 2 UO 2 P 2 O 7 The QE of the phosphor sample is decreased. The following examples demonstrate how the quantum efficiency can be increased in phosphor samples.
[0128] Example 3: NaUO 2 P 3 O 9 Phosphor and 1% Eu 3+ Doped NaUO 2 P 3 O 9 Preparation of (NH 4 ) 2 HPO 4 (DAP), HUO 2 PO 4 -4H 2 O and NaH 2 PO 4 were weighed out in a 1:1:1 molar ratio and then placed in a Nalgene bottle containing zirconia media and ball milled for 2 hours. After the mixture was thoroughly blended, the powder was transferred to an alumina crucible and fired at 300°C for 5 hours, then the mixture was sieved through a 40 mesh sieve and blended again in the same Nalgene bottle for an additional 2 hours. The powder was transferred back to the alumina crucible and fired at 500°C for 5 hours. After firing, a yellow solid color powder was obtained. NaUO 2 P 3 O 9 The emission spectrum of is shown in FIG. 8A.
[0129] 1%Eu 3+ Doped NaUO 2 P 3 O 9 To prepare 0.005 Eu 2 O 3 Add NaH in the blend. 2 PO 4The same procedure as above was used, except that the amount of NaUO was adjusted to 0.495. After calcination, a yellow solid color powder was obtained. 2 P 3 O 9 The emission spectrum of this compound is shown in FIG. 8B.
[0130] The results are shown in Table 3. [Table 3]
[0131] Phosphor NaUO 2 P 3 O 9 emits bright green light and can provide a wide color gamut for display applications. 2 P 3 O 9 isEu 3+ However, when doped with uranium, they did not demonstrate energy transfer from the uranium ions to the activator ions.
[0132] Example 4: K 4 UO 2 (PO 4 ) 2 Phosphor and 1% Eu 3+ Doped K 4 UO 2 (PO 4 ) 2 Preparation of K 2 CO 3 , H.U.O. 2 PO 4 -4H 2 O and KH 2 PO 4 were weighed out in a molar ratio of 1.5:1:1 and then placed in a Nalgene bottle containing zirconia media and ball milled for 2 hours. After the mixture was thoroughly blended, the powder was transferred to an alumina crucible and fired at 500°C for 5 hours, then the mixture was sieved through a 40 mesh sieve and blended again in the same Nalgene bottle for an additional 2 hours. The powder was transferred back to the alumina crucible and fired at 900°C for 5 hours. After firing, a yellow solid color powder was obtained. 4 UO 2 (PO4 ) 2 The emission spectrum of is shown in FIG. 9A.
[0133] 1% molar amount of Eu 3+ Doped K 4 UO 2 (PO 4 ) 2 To prepare 0.005 Eu 2 O 3 Add K in the blend. 2 CO 3 The same procedure as above was used, except that the amount of was adjusted to 1.495. After calcination, a yellow solid color powder was obtained. 4 UO 2 (PO 4 ) 2 The emission spectrum of is shown in FIG. 9B.
[0134] The results are shown in Table 4. [Table 4]
[0135] Phosphor K 4 UO 2 (PO 4 ) 2 emits bright green light and can provide a wide color gamut for display applications. 4 UO 2 (PO 4 ) 2 isEu 3+ did not demonstrate energy transfer from uranium ions to activator ions when doped with .
[0136] Example 5: Ba 3 (PO 4 ) 2 (UO 2 ) 2 P 2 O 7 Phosphor and co-doped Ba 3 (PO 4 ) 2 (UO 2 ) 2 P 2 O7 Preparation of phosphor materials BaHPO 4 , BaCO 3 , H.U.O. 2 PO 4 -4H 2 O and DAP were weighed in a molar ratio of 2:1:2:0.05 and then placed in a Nalgene bottle containing zirconia media and ball milled for 2 hours. After the mixture was thoroughly mixed, the powder was transferred to an alumina crucible and fired at 1100°C for 5 hours. After firing, a yellow solid color powder was obtained. 3 (PO 4 ) 2 (UO 2 ) 2 P 2 O 7 The emission spectrum of Ba is shown in Figure 10A. 3 (PO 4 ) 2 (UO 2 ) 2 P 2 O 7 The results are shown in Table 5 as Sample 1.
[0137] 1% molar amount of Eu 3+ Doped Ba 3 (PO 4 ) 2 (UO 2 ) 2 P 2 O 7 To prepare 0.005 Eu 2 O 3 Add BaCO 3 The same procedure as above was used, except that the amount of Eu was adjusted to 0.995. After calcination, a yellow solid color powder was obtained. 3+ Doped Ba 3 (PO 4 ) 2 (UO 2 ) 2 P 2 O 7 The emission spectrum of Eu is shown in Figure 10B. 3+ Doped Ba 3 (PO 4 ) 2 (UO 2 ) 2 P2 O 7 The results are shown in Table 5 as Sample 2.
[0138] 1% molar amount of Eu 3+ and K + Doped Ba 3 (PO 4 ) 2 (UO 2 ) 2 P 2 O 7 To prepare BaCO 3 Instead of 0.005 Eu 2 O 3 and K of 0.005 2 CO 3 The same procedure was used as above, except that Eu 3+ and K + Doped Ba 3 (PO 4 ) 2 (UO 2 ) 2 P 2 O 7 The emission spectrum of Eu is shown in Figure 10C. 3+ and K + Doped Ba 3 (PO 4 ) 2 (UO 2 ) 2 P 2 O 7 The results are shown in Table 5 as Sample 3.
[0139] 1% molar amount of Sm 3+ and K + Doped Ba 3 (PO 4 ) 2 (UO 2 ) 2 P 2 O 7 isEu 2 O 3 Instead of Sm 2 O 3 Except for the use of 1% molar amount of Eu 3+ and K + Doped Ba 3 (PO 4 )2 (UO 2 ) 2 P 2 O 7 It was prepared in the same manner as above. 1% molar amount of Sm 3+ and K + Doped Ba 3 (PO 4 ) 2 (UO 2 ) 2 P 2 O 7 The emission spectrum of 1% molar amount of Sm is shown in FIG. 3+ and K + Doped Ba 3 (PO 4 ) 2 (UO 2 ) 2 P 2 O 7 The results are shown in Table 5 as Sample 4.
[0140] 1% molar amount of Pr 3+ and K + Doped Ba 3 (PO 4 ) 2 (UO 2 ) 2 P 2 O 7 isEu 2 O 3 Instead of Pr 6 O 11 Except for the use of 1% molar amount of Eu 3+ and K + Doped Ba 3 (PO 4 ) 2 (UO 2 ) 2 P 2 O 7 It was prepared in the same manner as above. 1% molar amount of Eu 3+ and K + Doped Ba 3 (PO 4 ) 2 (UO 2 ) 2 P 2 O 7 The emission spectrum of 1% molar amount of Pr is shown in FIG. 3+and K + Doped Ba 3 (PO 4 ) 2 (UO 2 ) 2 P 2 O 7 The results are shown in Table 5 as Sample 5.
[0141] 1% molar amount of Sm 3+ and K + Doped Ba 3 (PO 4 ) 2 (UO 2 ) 2 P 2 O 7 isEu 2 O 3 Instead of SmPO 4 Using K 2 CO 3 Instead of KH 2 PO 4 Except for the use of 1% molar amount of Eu 3+ and K + Doped Ba 3 (PO 4 ) 2 (UO 2 ) 2 P 2 O 7 It was prepared in the same manner as above. 1% molar amount of Sm 3+ and K + Doped Ba 3 (PO 4 ) 2 (UO 2 ) 2 P 2 O 7 The emission spectrum of 1% molar amount of Sm is shown in FIG. 3+ and K + Doped Ba 3 (PO 4 ) 2 (UO 2 ) 2 P 2 O 7 The results are shown in Table 5 as Sample 6.
[0142] 1% molar amount of Pr 3+ and K+ Doped Ba 3 (PO 4 ) 2 (UO 2 ) 2 P 2 O 7 isEu 2 O 3 Instead of PrPO 4 Using K 2 CO 3 Instead of KH 2 PO 4 Except for the use of 1% molar amount of Eu 3+ and K + Doped Ba 3 (PO 4 ) 2 (UO 2 ) 2 P 2 O 7 It was prepared in the same manner as above. 1% molar amount of Pr 3+ and K + Doped Ba 3 (PO 4 ) 2 (UO 2 ) 2 P 2 O 7 The emission spectrum of 1% molar amount of Pr is shown in FIG. 3+ and K + Doped Ba 3 (PO 4 ) 2 (UO 2 ) 2 P 2 O 7 The results are shown in Table 5 as Sample 7.
[0143] 1% molar amount of Eu 3+ and K + Doped Ba 3 (PO 4 ) 2 (UO 2 ) 2 P 2 O 7 isEu 2 O 3 Instead of EuPO 4 Using K 2 CO 3Instead of KH 2 PO 4 Except for the use of 1% molar amount of Eu 3+ and K + Doped Ba 3 (PO 4 ) 2 (UO 2 ) 2 P 2 O 7 It was prepared in the same manner as above. 1% molar amount of Eu 3+ and K + Doped Ba 3 (PO 4 ) 2 (UO 2 ) 2 P 2 O 7 The emission spectrum of 1% molar amount of Eu is shown in FIG. 3+ and K + Doped Ba 3 (PO 4 ) 2 (UO 2 ) 2 P 2 O 7 The results are shown in Table 5 as Sample 8. [Table 5]
[0144] The energy transfer is demonstrated by the difference in color coordinates ccx and ccy. Each of samples 2 to 8 shows that there is an energy transfer from the uranium ion to the activator ion. The activator ion Eu 3+ Ba doped phosphor material 3 (PO 4 ) 2 (UO 2 ) 2 P 2 O 7 decreases the quantum efficiency, but the counter ion K + By adding Ba, the phosphor material 3 (PO 4 ) 2 (UO 2 ) 2 P 2 O 7The QE is increased over sample 1. Samples 4-8 have decreased quantum efficiency. Other examples demonstrate how quantum efficiency can be increased in phosphor samples.
[0145] Example 6: BaZnUO 2 (PO 4 ) 2 Phosphor and codoped BaZnUO 2 (PO 4 ) 2 Preparation of phosphor materials BaHPO 4 , H.U.O. 2 PO 4 -4H 2 O, ZnO and DAP were weighed in a molar ratio of 1:1:1:0.05 and then placed in a Nalgene bottle containing zirconia media and ball milled for 2 hours. After the mixture was thoroughly mixed, the powder was transferred to an alumina crucible and fired at 1050 °C for 5 hours under flowing moist air. After firing, a yellow solid color powder was obtained. 2 (PO 4 ) 2 The emission spectrum of BaZnUO is shown in Figure 11A. 2 (PO 4 ) 2 The results are shown in Table 6 as Sample A.
[0146] 1% molar amount of Eu 3+ Doped BaZnUO 2 (PO 4 ) 2 To prepare BaHPO 4 Instead of 0.005 Eu 2 O 3 The same procedure as above was used, except that Eu was used. After calcination, a yellow solid color powder was obtained. 3+ Doped BaZnUO 2 (PO 4 ) 2 The emission spectrum of Eu is shown in Figure 11B. 3+ Doped BaZnUO 2 (PO 4 ) 2 The results are shown in Table 6 as Sample B.
[0147] 1% molar amount of Eu 3+ and K + Doped BaZnUO 2 (PO 4 ) 2 To prepare BaHPO 4 Instead of 0.005 Eu 2 O 3 and K of 0.005 2 CO 3 The same procedure as above was used, except that Eu was used. After calcination, a yellow solid color powder was obtained. 3+ and K + Doped BaZnUO 2 (PO 4 ) 2 The emission spectrum of Eu is shown in FIG. 3+ and K + Doped BaZnUO 2 (PO 4 ) 2 The results are shown in Table 6 as sample B1.
[0148] 1% molar amount of Eu 3+ and K + Doped BaZnUO 2 (PO 4 ) 2 isEu 2 O 3 Instead of EuPO 4 Using K 2 CO 3 Instead of KH 2 PO 4 It was prepared in the same manner as sample B1, except that 1% molar amount of Eu was used. 3+ and K + Doped Ba 3 (PO 4 ) 2 (UO 2 ) 2 P 2 O 7 The results are shown in Table 6 as sample B2.
[0149] 1% molar amount of Eu 3+ and Li + Doped BaZnUO2 (PO 4 ) 2 is K 2 CO 3 Instead of Li 2 CO 3 It was prepared in the same manner as sample B1, except that 1% molar amount of Eu was used. 3+ and Li + Doped Ba 3 (PO 4 ) 2 (UO 2 ) 2 P 2 O 7 The emission spectrum of 1% molar amount of Eu is shown in FIG. 3+ and Li + Doped Ba 3 (PO 4 ) 2 (UO 2 ) 2 P 2 O 7 The results are shown in Table 6 as sample B3.
[0150] 1% molar amount of Eu 3+ and Na + Doped BaZnUO 2 (PO 4 ) 2 is K 2 CO 3 Instead of Na 2 CO 3 It was prepared in the same manner as sample B1, except that 1% molar amount of Eu was used. 3+ and Na + Doped BaZnUO 2 (PO 4 ) 2 The emission spectrum of 1% molar amount of Eu is shown in FIG. 3+ and Na + Doped BaZnUO 2 (PO 4 ) 2 The results are shown in Table 6 as sample B4.
[0151] 1% molar amount of Eu 3+ , Tb 3+ and K + Doped BaZnUO2 (PO 4 ) 2 is Tb 4 O 7 It was prepared similarly to sample B1, except that it also contained 1% molar Eu 3+ , Tb 3+ and K + Doped BaZnUO 2 (PO 4 ) 2 The results are shown in Table 6 as sample B5.
[0152] 1% molar amount of Eu 3+ , Dy 3+ and K + Doped BaZnUO 2 (PO 4 ) 2 Dy 2 O 3 It was prepared similarly to sample B1, except that it also contained 1% molar Eu 3+ , Dy 3+ and K + Doped BaZnUO 2 (PO 4 ) 2 The results are shown in Table 6 as sample B6.
[0153] 1% molar amount of Eu 3+ , Sm 3+ and K + Doped BaZnUO 2 (PO 4 ) 2 is Sm 2 O 3 It was prepared similarly to sample B1, except that it also contained 1% molar Eu 3+ , Sm 3+ and K + Doped BaZnUO 2 (PO 4 ) 2 The results are shown in Table 6 as sample B7.
[0154] 1% molar amount of Pr 3+ Doped BaZnUO 2 (PO 4 ) 2 isEu 2 O3 Instead of Pr 6 O 11 Except for the use of 1% molar amount of Eu 3+ Doped BaZnUO 2 (PO 4 ) 2 It was prepared in the same manner as Pr 3+ Doped BaZnUO 2 (PO 4 ) 2 The emission spectrum of Pr is shown in Figure 11F. 3+ Doped BaZnUO 2 (PO 4 ) 2 The results are shown in Table 6 as Sample C.
[0155] 1% molar amount of Pr 3+ and K + Doped BaZnUO 2 (PO 4 ) 2 isEu 2 O 3 Instead of Pr 6 O 11 It was prepared in the same manner as sample B1, except that Pr 3+ and K + Doped BaZnUO 2 (PO 4 ) 2 The emission spectrum of Pr is shown in Figure 11G. 3+ and K + Doped BaZnUO 2 (PO 4 ) 2 The results are shown in Table 6 as sample C1.
[0156] 1% molar amount of Pr 3+ and K + Doped BaZnUO 2 (PO 4 ) 2 isEu 2 O 3 Instead of PrPO 4 Using K 2 CO 3 Instead of KH 2 PO 4It was prepared in the same manner as sample B1, except that 1% molar amount of Pr was used. 3+ and K + Doped BaZnUO 2 (PO 4 ) 2 The results are shown in Table 6 as sample C2.
[0157] 1% molar amount of Sm 3+ Doped BaZnUO 2 (PO 4 ) 2 isEu 2 O 3 Instead of Sm 2 O 3 Except for the use of 1% molar amount of Eu 3+ Doped BaZnUO 2 (PO 4 ) 2 It was prepared in the same manner as Sm 3+ Doped BaZnUO 2 (PO 4 ) 2 The emission spectrum of Sm is shown in Figure 11H. 3+ Doped BaZnUO 2 (PO 4 ) 2 The results are shown in Table 6 as Sample D.
[0158] 1% molar amount of Sm 3+ and K + Doped BaZnUO 2 (PO 4 ) 2 isEu 2 O 3 Instead of Sm 2 O 3 It was prepared in the same manner as sample B1, except that Sm 3+ and K + Doped BaZnUO 2 (PO 4 ) 2 The emission spectrum of Sm is shown in Figure 11I. 3+ and K + Doped BaZnUO 2 (PO 4 ) 2 The results are shown in Table 6 as sample D1.
[0159] 1% molar amount of Sm 3+ and K + Doped BaZnUO 2 (PO 4 ) 2 isEu 2 O 3 Instead of PrPO 4 Using K 2 CO 3 Instead of KH 2 PO 4 The sample was prepared in the same manner as sample B1, except that 1% molar amount of Sm was used. 3+ and K + Doped BaZnUO 2 (PO 4 ) 2 The results are shown in Table 6 as sample D2.
[0160] 1% molar amount of Sm 3+ , Tb 3+ and K + Doped BaZnUO 2 (PO 4 ) 2 is Tb 4 O 7 It was prepared similarly to sample D2, except that Sm was also included. 3+ , Tb 3+ and K + Doped BaZnUO 2 (PO 4 ) 2 The results are shown in Table 6 as sample D3.
[0161] 1% molar amount of Sm 3+ , Dy 3+ and K + Doped BaZnUO 2 (PO 4 ) 2 Dy 2 O 3 It was prepared similarly to sample D2, except that Sm was also included. 3+ , Dy 3+ and K + Doped BaZnUO 2 (PO 4 ) 2The results are shown in Table 6 as sample D4.
[0162] 1% molar amount of Tb 3+ Doped BaZnUO 2 (PO 4 ) 2 isEu 2 O 3 Instead of Tb 4 O 7 Except for the use of 1% molar amount of Eu 3+ Doped BaZnUO 2 (PO 4 ) 2 It was prepared in the same manner as Tb 3+ Doped BaZnUO 2 (PO 4 ) 2 The results are shown in Table 6 as Sample E.
[0163] 1% molar amount of Dy 3+ Doped BaZnUO 2 (PO 4 ) 2 isEu 2 O 3 Instead of Dy 2 O 3 Except for the use of 1% molar amount of Eu 3+ Doped BaZnUO 2 (PO 4 ) 2 It was prepared in the same manner as Dy 3+ Doped BaZnUO 2 (PO 4 ) 2 The results are shown in Table 6 as Sample F.
[0164] 1% molar amount of Ce 3+ Doped BaZnUO 2 (PO 4 ) 2 isEu 2 O 3 Instead of CeO 2 Except for the use of 1% molar amount of Eu 3+ Doped BaZnUO 2 (PO 4 ) 2 It was prepared in the same manner as Ce3+ Doped BaZnUO 2 (PO 4 ) 2 The results are shown in Table 6 as Sample G.
[0165] 1% molar amount of Ce 3+ and K + Doped BaZnUO 2 (PO 4 ) 2 isEu 2 O 3 Instead of CeO 2 It was prepared in the same manner as sample B1, except that Ce was used. 3+ and K + Doped BaZnUO 2 (PO 4 ) 2 The results are shown in Table 6 as sample G1.
[0166] 1% molar amount of Sn 2+ Doped BaZnUO 2 (PO 4 ) 2 isEu 2 O 3 Except for using SnO instead of Eu at 1% molar amount 3+ Doped BaZnUO 2 (PO 4 ) 2 It was prepared in the same manner as Sn 2+ Doped BaZnUO 2 (PO 4 ) 2 The results are shown in Table 6 as Sample H.
[0167] 1% molar amount of Sb 3+ Doped BaZnUO 2 (PO 4 ) 2 isEu 2 O 3 Instead of Sb 2 O 3 Except for the use of 1% molar amount of Eu 3+ Doped BaZnUO 2 (PO 4 ) 2 It was prepared in the same manner as Sb3+ Doped BaZnUO 2 (PO 4 ) 2 The results are shown in Table 6 as Sample I.
[0168] 1% molar amount of Mn 2+ Doped BaZnUO 2 (PO 4 ) 2 isEu 2 O 3 Instead of MnCO 3 Except for the use of 1% molar amount of Eu 3+ Doped BaZnUO 2 (PO 4 ) 2 It was prepared in the same manner as Mn 2+ Doped BaZnUO 2 (PO 4 ) 2 The results are shown in Table 6 as Sample J.
[0169] 1% molar amount of Er 3+ Doped BaZnUO 2 (PO 4 ) 2 isEu 2 O 3 Instead of Er 2 O 3 It was prepared in the same manner as sample A, except that Er 3+ Doped BaZnUO 2 (PO 4 ) 2 The results are shown in Table 6 as sample K.
[0170] 1% molar amount of Tm 3+ Doped BaZnUO 2 (PO 4 ) 2 isEu 2 O 3 Instead of Tm 2 O 3 It was prepared in the same manner as sample A, except that Tm 3+ Doped BaZnUO 2 (PO 4 ) 2 The results are shown in Table 6 as Sample L.
[0171] 1% molar amount of Yb 3+ Doped BaZnUO 2 (PO 4 ) 2 isEu 2 O 3 Instead of Yb 2 O 3 It was prepared in the same manner as sample A, except that Yb was used. 3+ Doped BaZnUO 2 (PO 4 ) 2 The results are shown in Table 6 as Sample M.
[0172] 1% molar amount of Yb 3+ and K + Doped BaZnUO 2 (PO 4 ) 2 isEu 2 O 3 Instead of Yb 2 O 3 It was prepared in the same manner as sample B1, except that Yb was used. 3+ and K + Doped BaZnUO 2 (PO 4 ) 2 The results are shown in Table 6 as sample M1.
[0173] 1% molar amount of Nd 3+ Doped BaZnUO 2 (PO 4 ) 2 isEu 2 O 3 Instead of Nd 2 O 3 It was prepared in the same manner as sample A, except that Nd 3+ Doped BaZnUO 2 (PO 4 ) 2 The results are shown in Table 6 as Sample N.
[0174] 1% molar amount of Gd 3+ Doped BaZnUO 2 (PO 4 )2 isEu 2 O 3 Instead of Gd 2 O 3 It was prepared in the same manner as sample A, except that Gd 3+ Doped BaZnUO 2 (PO 4 ) 2 The results are shown in Table 6 as Sample O.
[0175] 1% molar amount of Bi 3+ Doped BaZnUO 2 (PO 4 ) 2 isEu 2 O 3 Instead of Bi 2 O 3 It was prepared in the same manner as sample A, except that Bi was used. 3+ Doped BaZnUO 2 (PO 4 ) 2 The results are shown in Table 6 as sample P.
[0176] 1% molar amount of Ho 3+ Doped BaZnUO 2 (PO 4 ) 2 isEu 2 O 3 Instead of Ho 2 O 3 It was prepared in the same manner as sample A, except that Ho was used. 3+ Doped BaZnUO 2 (PO 4 ) 2 The results are shown in Table 6 as sample Q.
[0177] 1%Eu 3+ -1%Li + BaZnUO 2 (PO 4 ) 2 To prepare BaHPO 4 , H.U.O. 2 PO 4 -4H 2 O, ZnO, DAP, Eu 2 O 3 and Li2 CO 3 were weighed out in a molar ratio of 0.98:1:1:0.05:0.005:0.005 and then placed in a Nalgene bottle containing zirconia media and ball milled for 2 hours. After the mixture was thoroughly mixed, the powder was transferred to an alumina crucible and fired at 1050 °C for 5 hours under flowing moist air. After firing, a yellow solid color powder was obtained. 2 (PO 4 ) 2 :EU 3+ ,Li + The emission spectrum of BaZnUO is shown as A in FIG. 2 (PO 4 ) 2 :EU 3+ ,Li + The results are shown in Table 6 as sample R.
[0178] 1% molar amount of Eu 3+ and 1% Li + Doped nonstoichiometric BaZnUO 2 (PO 4 ) 2 To prepare BaHPO 4 , H.U.O. 2 PO 4 -4H 2 O, ZnO, DAP, Eu 2 O 3 and Li 2 CO 3 were weighed out in a molar ratio of 0.97:0.96:1.05:0.05:0.005:0.005, and the same procedure as above was used, except that the blend ratio was deviated from the stoichiometric ratio above. After calcination, a yellow solid color powder was obtained. 3+ and Li + Doped nonstoichiometric BaZnUO 2 (PO 4 ) 2 The emission spectrum of Eu is shown in FIG. 3+ Doped BaZnUO 2 (PO 4 ) 2 (Ba 0.99 Zinc 1.05 (UO 2 )0.96 (PO 4 ) 2 The results are shown in Table 6 for sample S. [Table 6]
[0179] The energy transfer is demonstrated by the difference in color coordinates ccx and ccy. 3+ , Sm 3+ and Pr 3+ BaZnUO doped phosphor material 2 (PO 4 ) 2 indicates that there is energy transfer from the uranium ion to the activator ion. 3+ , Sn 2+ , Sb 3+ , Mn 2+ , Tb 3+ , Er 3+ , Tm 3+ , Yb 3+ , Nd 3+ , Gd 3+ , Bi 3+ , Ho 3+ and Dy 3+ BaZnUO doped phosphor material 2 (PO 4 ) 2 does not show energy transfer from the uranium ion to the activator ion, which represents an unexpected result since not all activator ions in the lanthanide group work in uranium-based phosphors.
[0180] The alkali counter ion is the activator ion Eu 3+ , Sm 3+ and Pr 3+ The energy transfer and quantum efficiency properties of phosphors doped with Eu can be improved or at least maintained. 3+ Doped BaZnUO 2 (PO 4 ) 2 is the alkali counterion (K + and Li +) is co-doped, the energy transfer and quantum efficiency are significantly improved, but Ce 3+ and Yb 3+ As shown for , if there is no energy transfer to the activator ion, the counter ion does not provide energy transfer.
[0181] Example 7 Co-doped BaZnUO 2 (PO 4 ) 2 Preparation of phosphor materials BaHPO 4 , H.U.O. 2 PO 4 -4H 2 O, ZnO, DAP, Eu 2 O 3 and K 2 CO 3 were weighed out in a molar ratio of 0.98:1:1:0.07:0.005:0.005, then placed in a Nalgene bottle containing zirconia media and ball milled for 2 hours to obtain a 1% molar amount of Eu. 3+ and K + Doped BaZnUO 2 (PO 4 ) 2 After the mixture was thoroughly mixed, the powder was transferred to an alumina crucible and fired at 1050 °C for 5 hours under a stream of moist air. After firing, a yellow solid color powder was obtained. 3+ and K + Doped BaZnUO 2 (PO 4 ) 2 The results are shown in Table 7 as sample B5-1%.
[0182] 2% molar amount of Eu 3+ and K + Doped BaZnUO 2 (PO 4 ) 2 2%Eu 2 O 3 and 2%K 2 CO 3 It was prepared similarly to sample B5-1%, except that 2% molar amount of Eu was added. 3+ and K+ Doped Ba 3 (PO 4 ) 2 (UO 2 ) 2 P 2 O 7 The results are shown in Table 7 as sample B5-2%.
[0183] 3% molar amount of Eu 3+ and K + Doped BaZnUO 2 (PO 4 ) 2 3%Eu 2 O 3 and 3%K 2 CO 3 It was prepared similarly to sample B5-1%, except that 3% molar amount of Eu was added. 3+ and K + Doped BaZnUO 2 (PO 4 ) 2 The results are shown in Table 7 as sample B5-3%. [Table 7]
[0184] The energy transfer is demonstrated by the difference in color coordinates ccx and ccy. + Co-doped phosphor material BaZnUO 2 (PO 4 ) 2 indicates increased QE. 3+ We show how phosphors can be color tuned by using
[0185] Example 8 BaZnUO 2 (PO 4 ) 2 and preparation of co-doped phosphor materials For sample A in Example 6, BaZnUO 2 (PO 4 ) 2 was prepared as described above.
[0186] 1% molar amount of Eu 3+ Doped BaZnUO 2 (PO 4 ) 2 To prepare BaHPO 4 , H.U.O. 2 PO 4 -4H 2 O, ZnO, DAP and Eu 2 O 3 were weighed out in a molar ratio of 0.99:1:1:0.06:0.005, then placed in a Nalgene bottle containing zirconia media and ball milled for 2 hours. After the mixture was thoroughly mixed, the powder was transferred to an alumina crucible and fired at 1050 °C for 5 hours under flowing moist air. After firing, a yellow solid color powder was obtained. 3+ Doped BaZnUO 2 (PO 4 ) 2 The emission spectrum is shown in FIG.
[0187] 1% molar amount of Eu 3+ and K + Doped BaZnUO 2 (PO 4 ) 2 To prepare BaHPO 4 , H.U.O. 2 PO 4 -4H 2 O, ZnO, DAP, Eu 2 O 3 and K 2 CO 3 were weighed out in a molar ratio of 0.98:1:1:0.07:0.005:0.005, then placed in a Nalgene bottle containing zirconia media and ball milled for 2 hours. After the mixture was thoroughly mixed, the powder was transferred to an alumina crucible and fired at 1050°C for 5 hours under flowing moist air. After firing, a yellow solid color powder was obtained.
[0188] 1% molar amount of Eu 3+ and Li + Doped BaZnUO 2 (PO 4 ) 2 is K 2 CO3 Instead of Li 2 CO 3 Except for the use of 1% molar amount of Eu 3+ and K + Doped BaZnUO 2 (PO 4 ) 2 It was prepared in the same manner as in the preparation of Example 1.
[0189] 1% molar amount of Eu 3+ and Na + Doped BaZnUO 2 (PO 4 ) 2 is K 2 CO 3 Instead of Na 2 CO 3 Except for the use of 1% molar amount of Eu 3+ and K + Doped BaZnUO 2 (PO 4 ) 2 It was prepared in the same manner as in the preparation of Example 1.
[0190] 1% molar amount of Eu 3+ and Rb + Doped BaZnUO 2 (PO 4 ) 2 is K 2 CO 3 Instead of Rb 2 CO 3 Except for the use of 1% molar amount of Eu 3+ and K + Doped BaZnUO 2 (PO 4 ) 2 It was prepared in the same manner as in the preparation of Example 1.
[0191] 1% molar amount of Eu 3+ and Cs + Doped BaZnUO 2 (PO 4 ) 2 is K 2 CO 3 Instead of Cs 2 CO 3 Except for the use of 1% molar amount of Eu3+ and K + Doped BaZnUO 2 (PO 4 ) 2 It was prepared in the same manner as in the preparation of Example 1.
[0192] The results are shown in Table 8. [Table 8]
[0193] The energy transfer is demonstrated by the difference in color coordinates ccx and ccy. 2 (PO 4 ) 2 indicates energy transfer. BaZnUO co-doped with activator ions and counter ions 2 (PO 4 ) 2 exhibits energy transfer and can increase or maintain the QE of the phosphor material without the counter ion.
[0194] Example 9 γ-Ba 2 UO 2 (PO 4 ) 2 and preparation of co-doped phosphor materials γ-Ba 2 UO 2 (PO 4 ) 2 To prepare BaHPO 4 , U.O. 2 γ-Ba and DAP were weighed in a molar ratio of 2:1:0.05, then placed in a Nalgene bottle containing zirconia media and ball milled for 2 hours. After the mixture was thoroughly mixed, the powder was transferred to an alumina crucible and calcined at 1100°C in air for 5 hours. After calcination, a yellow solid color powder was obtained. 2 UO 2 (PO 4 ) 2 The emission spectrum of γ-Ba is shown in FIG. 2 UO 2 (PO 4 ) 2 The powder XRD pattern of is shown in FIG. 13H.
[0195] 1 mol% Eu 3+ Doped γ-Ba 2 UO 2 (PO 4 ) 2 To prepare BaHPO 4 , U.O. 2 , DAP and Eu 2 O 3 were weighed out in a molar ratio of 1.99:1:0.05:0.005, then placed in a Nalgene bottle containing zirconia media and ball milled for 2 hours. After the mixture was thoroughly mixed, the powder was transferred to an alumina crucible and calcined at 1100°C in air for 5 hours. After calcination, a yellow solid color powder was obtained. 3+ Doped γ-Ba 2 UO 2 (PO 4 ) 2 The emission spectrum of is shown in FIG. 13B.
[0196] 1 mol% Eu 3+ and 1 mol% K + Doped γ-Ba 2 UO 2 (PO 4 ) 2 To prepare BaHPO 4 , U.O. 2 , DAP, Eu 2 O 3 and K 2 CO 3 were weighed out in a molar ratio of 1.98:1:0.05:0.005:0.005, then placed in a Nalgene bottle containing zirconia media and ball milled for 2 hours. After the mixture was thoroughly mixed, the powder was transferred to an alumina crucible and calcined at 1100°C in air for 5 hours. After calcination, a yellow solid color powder was obtained. 3+ and K + Doped γ-Ba 2 UO 2 (PO 4 ) 2 The emission spectrum of is shown in FIG. 13C.
[0197] 1 mol% Sm 3+and 1 mol% K + Doped γ-Ba 2 UO 2 (PO 4 ) 2 To prepare BaHPO 4 , U.O. 2 , DAP, Sm 2 O 3 and K 2 CO 3 were weighed out in a molar ratio of 1.98:1:0.05:0.005:0.005 and then placed in a Nalgene bottle containing zirconia media and ball milled for 2 hours. After the mixture was thoroughly mixed, the powder was transferred to an alumina crucible and fired at 1100°C in air for 5 hours. After firing, a yellow solid color powder was obtained. 3+ and K + Doped γ-Ba 2 UO 2 (PO 4 ) 2 The emission spectrum of is shown in FIG. 13D.
[0198] 1 mol% Pr 3+ and 1 mol% K + Doped γ-Ba 2 UO 2 (PO 4 ) 2 To prepare BaHPO 4 , U.O. 2 , DAP, Pr 6 O 11 and K 2 CO 3 were weighed out in a molar ratio of 1.98:1:0.05:0.00167:0.005, then placed in a Nalgene bottle containing zirconia media and ball milled for 2 hours. After the mixture was thoroughly mixed, the powder was transferred to an alumina crucible and calcined at 1100 °C in air for 5 hours. After calcination, a yellow solid color powder was obtained. 3+ and K + Doped γ-Ba 2 UO 2 (PO 4 ) 2 The emission spectrum of is shown in FIG. 13E.
[0199] 1 mol% Dy3+ and 1 mol% K + Doped γ-Ba 2 UO 2 (PO 4 ) 2 To prepare BaHPO 4 , U.O. 2 , DAP, Dy 2 O 3 and K 2 CO 3 were weighed out in a molar ratio of 1.98:1:0.05:0.005:0.005, then placed in a Nalgene bottle containing zirconia media and ball milled for 2 hours. After the mixture was thoroughly mixed, the powder was transferred to an alumina crucible and calcined at 1100°C in air for 5 hours. After calcination, a yellow solid color powder was obtained. 3+ and K + Doped γ-Ba 2 UO 2 (PO 4 ) 2 The emission spectrum of is shown in FIG. 13F.
[0200] 1 mol% Tb 3+ and 1 mol% K + Doped γ-Ba 2 UO 2 (PO 4 ) 2 To prepare BaHPO 4 , U.O. 2 , DAP, Tb 4 O 7 and K 2 CO 3 were weighed out in a molar ratio of 1.98:1:0.05:0.0025:0.005, then placed in a Nalgene bottle containing zirconia media and ball milled for 2 hours. After the mixture was thoroughly mixed, the powder was transferred to an alumina crucible and calcined at 1100°C in air for 5 hours. After calcination, a yellow solid color powder was obtained. 3+ and K + Doped γ-Ba 2 UO 2 (PO 4 ) 2 The emission spectrum of is shown in FIG. 13G.
[0201] The results are shown in Table 9. [Table 9]
[0202] The energy transfer is demonstrated by the difference in color coordinates ccx and ccy. 3+ ,Pr 3+ and Sm 3+ Co-doped phosphor material γ-Ba 2 UO 2 (PO 4 ) 2 There is energy transfer from the uranium ions to the activator ions; however, the peak is very broad, so the changes in ccx and ccy are not as strong as in the other compositions (see FIG. 13A). 3+ The addition of Sm can be seen at about 610 in FIG. 13B. The addition of both the activator ion and counter ion shows a more pronounced peak formation at 610 in FIG. 13C. The addition of the activator peak is also seen in FIG. 13D (Sm 3+ ) and FIG. 13E (Pr 3+ ), while Dy 3+ and Tb 3+ No additional peaks are observed in Figures 13F and 13G for uranium ions, indicating no energy transfer from the activator ions. 2 UO 2 (PO 4 ) 2 increases or maintains the QE of the phosphor material without the counter ion. Other examples herein demonstrate how quantum efficiency can be further increased in phosphor samples.
[0203] Example 10 γ-Ba 2 UO 2 (PO 4 ) 2 and preparation of co-doped phosphor materials 1 mol% Eu 3+ and 1 mol% K + Doped γ-Ba 2 UO 2 (PO 4 )2 To prepare BaHPO 4 , U.O. 2 , DAP, Eu 2 O 3 and K 2 CO 3 were weighed out in a molar ratio of 1.98:1:0.05:0.005:0.005, then placed in a Nalgene bottle containing zirconia media and ball milled for 2 hours. After the mixture was thoroughly mixed, the powder was transferred to an alumina crucible and fired at 1100°C in air for 5 hours. After firing, a yellow solid color powder was obtained.
[0204] 2 mol% Eu 3+ and 2 mol% K + Doped γ-Ba 2 UO 2 (PO 4 ) 2 To prepare BaHPO 4 , U.O. 2 , DAP, Eu 2 O 3 and K 2 CO 3 were weighed out in a molar ratio of 1.96:1:0.05:0.01:0.01, then placed in a Nalgene bottle containing zirconia media and ball milled for 2 hours. After the mixture was thoroughly mixed, the powder was transferred to an alumina crucible and calcined at 1100°C in air for 5 hours. After calcination, a yellow solid color powder was obtained.
[0205] 3 mol% Eu 3+ and 3 mol% K + Doped γ-Ba 2 UO 2 (PO 4 ) 2 To prepare BaHPO 4 , U.O. 2 , DAP, Eu 2 O 3 and K 2 CO 3were weighed out in a molar ratio of 1.94:1:0.05:0.015:0.015, then placed in a Nalgene bottle containing zirconia media and ball milled for 2 hours. After the mixture was thoroughly mixed, the powder was transferred to an alumina crucible and fired at 1100°C in air for 5 hours. After firing, a yellow solid color powder was obtained.
[0206] The results are shown in Table 10. [Table 10]
[0207] Coordinates ccx and ccy. Counterion K + Phosphor material Ba co-doped with 2 UO 2 (PO 4 ) 2 indicates increased QE. 3+ We show how phosphors can be color tuned by using
[0208] Example 11 1% molar amount of Eu 3+ Doped Na 2 UO 2 P 2 O 7 (U-Eu red phosphor) is Na 2 CO 3 , H.U.O. 2 PO 4 -4H 2 O, NaH 2 PO 4 and Eu 2 O 3 were weighed into a Nalgene bottle containing zirconia media in a molar ratio of 0.5:1:1:0.005 and ball milled for 2 hours. After the mixture was thoroughly mixed, the powder was transferred to an alumina crucible and fired at 500°C for 5 hours. The mixture was then sieved through a 40 mesh sieve and blended again in the same Nalgene bottle for an additional 2 hours. The powder was transferred back to the alumina crucible and fired at 900°C for 5 hours. After firing, a yellow solid color powder was obtained.
[0209] The U-Eu red phosphor was 2 SiF 6 :Mn 4+ FIG. 14 also shows the eye sensitivity range associated with human vision in daylight or other bright light conditions. The eye sensitivity range is centered at 555 nm. The U-Eu red phosphor has a red color and is spectrally shifted to the center of the eye sensitivity range more than the PFS, and the emitted light of the U-Eu red phosphor appears brighter. The U-Eu red phosphor has a spectral output of 317.42 lms / Wrad and the PFS has a spectral output of 200.82 Lms / Wrad. The U-Eu red phosphor exhibits 58% higher absorbance than the PFS.
[0210] The efficacy of white light blends using U-Eu red and PFS phosphors was modeled. Each red phosphor was blended with a YAG phosphor and modeled with a blue LED with a CCT of 4100K. Both blends were modeled in the device to determine efficacy (Lms / Watt) measurements. White light blends with PFS were also measured in the device. The efficacy measurements for the white light blends are shown in Table 11. [Table 11]
[0211] The modeled efficacy of the white blend with U-Eu red phosphor is a 15% increase in efficacy over the white blend with PFS. The high efficacy of the white blend with U-Eu red phosphor is not currently available in commercially available phosphor blends or white LEDs. The measured CRI for both the white blend with U-EU red and the white blend with PFS is greater than 80.
[0212] Example 12: Na 2 UO 2 P 2 O 7 Phosphor and 1% activator ion Eu 3+ and various amounts of (NH 4 ) 2 HPO 4 (DAP) doped Na 2 UO2 P 2 O 7 Preparation of Na 2 HPO 4 , H.U.O. 2 PO 4 -4H 2 O, Eu 2 O 3 and (NH 4 ) 2 HPO 4 were weighed out in a molar ratio of 0.995:1:0.005:0 and then placed in a Nalgene bottle containing zirconia media and ball milled for 2 hours. After the mixture was thoroughly blended, the powder was transferred to an alumina crucible and fired at 500°C for 5 hours, then the mixture was sieved through a 40 mesh sieve and blended again in the same Nalgene bottle for an additional 2 hours. The powder was transferred back to the alumina crucible and fired at 900°C for 5 hours. After the final firing, a yellow body colored powder was obtained. 2 UO 2 P 2 O 7 :EU 3+ The emission spectrum is shown in FIG. 15, and the results are shown in Table 12.
[0213] 1% molar amount of Eu 3+ and Na doped with 2.5% excess DAP. 2 UO 2 P 2 O 7 The same procedure as above was used to prepare Eu, except that 0.025 DAP was added. 3+ and Na doped with 2.5% excess (xs) DAP. 2 UO 2 P 2 O 7 The QE and results are shown in Table 12.
[0214] 1% molar amount of Eu 3+ and Na doped with 5% excess DAP. 2 UO 2 P 2 O 7 used the same procedure as above, except for the addition of 0.05 DAP. 3+and Na doped with 5% xs DAP 2 UO 2 P 2 O 7 The QEs are shown in Table 12.
[0215] 1% molar amount of Eu 3+ and Na doped with 7.5% excess DAP. 2 UO 2 P 2 O 7 used the same procedure as above, except that 0.075 DAP was added. 3+ and 7.5%xs DAP doped Na 2 UO 2 P 2 O 7 The QEs are shown in Table 12. [Table 12]
[0216] The color point of the phosphor remains the same for DAPs with excess (xs) of 0 to 7.5%, but the QE shows a maximum at a DAP of 2.5% xs. Only one spectrum is shown in Figure 15.
[0217] Example 13: Various Eu 3+ Na with concentration 2 UO 2 P 2 O 7 Preparation of phosphors 1%Eu 3+ Doped Na 2 UO 2 P 2 O 7 To prepare Na 2 HPO 4 , H.U.O. 2 PO 4 -4H 2 O, Eu 2 O 3 and (NH 4 ) 2 HPO 4were weighed out in a molar ratio of 0.995:1:0.005:0.25 and then placed in a Nalgene bottle containing zirconia media and ball milled for 2 hours. After the mixture was thoroughly blended, the powder was transferred to an alumina crucible and fired at 500°C for 5 hours, then the mixture was sieved through a 40 mesh sieve and blended again in the same Nalgene bottle for an additional 2 hours. The powder was transferred back to the alumina crucible and fired at 900°C for 5 hours. After the final firing, a yellow body colored powder was obtained. 2 UO 2 P 2 O 7 :EU 3+ The emission spectrum of is shown in FIG. 15 and is the same as the sample used in Example 12, and is shown as Sample A in the results in Table 13.
[0218] 0.1% molar amount of Eu 3+ Doped Na 2 UO 2 P 2 O 7 To prepare 0.9995 Na 2 HPO 4 and 0.0005 Eu 2 O 3 The same procedure as above was used, except for the addition of 0.1% Eu. 3+ Doped Na 2 UO 2 P 2 O 7 The emission spectrum of sample B is shown in FIG. 16, and the results are shown in Table 13.
[0219] 0.05% molar amount of Eu 3+ Doped Na 2 UO 2 P 2 O 7 To prepare 0.99975 Na 2 HPO 4 and 0.00025 Eu 2 O 3 The same procedure as above was used, except for the addition of Eu 3+ and 0.05% Eu 3+ Na 2 UO 2 P2 O 7 The emission spectrum of sample C is shown in FIG. 16, and the results are shown in Table 13.
[0220] 0.03% molar amount of Eu 3+ Doped Na 2 UO 2 P 2 O 7 To prepare 0.99985 Na 2 HPO 4 and 0.00015 Eu 2 O 3 The same procedure as above was used, except for the addition of 0.03% Eu. 3+ Doped Na 2 UO 2 P 2 O 7 The emission spectrum of sample D is shown in FIG. 16, and the results are shown in Table 13.
[0221] 0.02% molar amount of Eu 3+ Doped Na 2 UO 2 P 2 O 7 About 0.9999 Na 2 HPO 4 and 0.0001 Eu 2 O 3 The same procedure as above was used, except for the addition of Eu 3+ and 0.02% Eu 3+ Na 2 UO 2 P 2 O 7 The emission spectrum of sample E is shown in FIG. 16, and the results are shown in Table 13. [Table 13]
[0222] Example 16: Sm 3+ ,EU 3+ and Pr 3+ Rb doped with 1% activator ion 2 UO 2 P 2 O7 Preparation of phosphors. Rb 2 CO 3 , H.U.O. 2 PO 4 -4H 2 O and (NH 4 ) 2 HPO 4 were weighed out in a 1:1:1 molar ratio and then placed in a Nalgene bottle containing zirconia media and ball milled for 2 hours. After the mixture was thoroughly mixed, the powder was transferred to an alumina crucible and fired at 500°C for 5 hours. The mixture was then sieved through a 40 mesh sieve and blended again in the same Nalgene bottle for an additional 2 hours. The powder was transferred back to the alumina crucible and fired at 900°C for 5 hours. After the final firing, a yellow body colored powder was obtained. 2 UO 2 P 2 O 7 The emission spectrum of is shown in FIG. 17A and the results are shown in Table 16.
[0223] 1% molar amount of Sm 3+ Doped Rb 2 UO 2 P 2 O 7 To prepare 0.995% Rb 2 CO 3 and 0.005 Sm 2 O 3 The same procedure as above was used, except for the addition of Sm 3+ Doped Rb 2 UO 2 P 2 O 7 The results are shown in FIG. 17B and in Table 16.
[0224] 1% molar amount of Eu 3+ Doped Rb 2 UO 2 P 2 O 7 To prepare 0.995% Rb 2 CO 3 and 0.005 Eu 2 O 3 The same procedure as above was used, except for the addition of Eu3+ Doped Rb 2 UO 2 P 2 O 7 The results are shown in FIG. 17C and in Table 16.
[0225] 1% molar amount of Pr 3+ Doped Rb 2 UO 2 P 2 O 7 To prepare 0.995% Rb 2 CO 3 and Pr of 0.00167 6 O 11 The same procedure as above was used, except for the addition of Pr. 3+ Doped Rb 2 UO 2 P 2 O 7 The results are shown in FIG. 17D and in Table 16. [Table 16]
[0226] The change in color point indicates the energy transfer to Sm, Eu, and Pr ions. 3+ The addition of activator ion Sm 3+ and Pr 3 Other examples herein demonstrate how quantum efficiency can be increased in phosphor samples.
[0227] Example 17: Eu 3+ ,Pr 3+ and Sm 3+ Cs doped with 1% activator ions 2 UO 2 P 2 O 7 Preparation of phosphors. Cs 2 UO 2 P 2 O 7 To prepare Cs 2 CO 4 , H.U.O. 2 PO4 -4H 2 O and (NH 4 ) 2 HPO 4 were weighed out in a 1:1:1 molar ratio and then placed in a Nalgene bottle containing zirconia media and ball milled for 2 hours. After the mixture was thoroughly blended, the powder was transferred to an alumina crucible and fired at 500°C for 5 hours, then the mixture was sieved through a 40 mesh sieve and blended again in the same Nalgene bottle for an additional 2 hours. The powder was transferred back to the alumina crucible and fired at 900°C for 5 hours. After the final firing, a yellow body colored powder was obtained. Cs 2 UO 2 P 2 O 7 The emission spectrum of is shown in FIG. 18A and the results are shown in Table 17.
[0228] 1% molar amount of Eu 3+ Doped Cs 2 UO 2 P 2 O 7 To prepare 0.995% Cs 2 CO 3 and 0.005 Eu 2 O 3 The same procedure as above was used, except for the addition of 1% Eu 3+ Doped Cs 2 UO 2 P 2 O 7 The emission spectrum is shown in FIG. 18B and the results are shown in Table 17.
[0229] 1% molar amount of Eu 3+ Doped Cs 2 UO 2 P 2 O 7 Another sample of 1% molar Eu was prepared similarly and included a washing step. 3+ The Cs doped sample 2 UO 2 P 2 O 7 The results are shown in Table 17.
[0230] 1% molar amount of Pr3+ Doped Cs 2 UO 2 P 2 O 7 About 0.995 Cs 2 CO 3 and Pr of 0.00167 6 O 11 The same procedure as above was used, except for the addition of 1% Pr. 3+ Doped Cs 2 UO 2 P 2 O 7 The emission spectrum is shown in FIG. 18C and the results are shown in Table 17.
[0231] 1% molar amount of Sm 3+ Doped Cs 2 UO 2 P 2 O 7 To prepare 0.995% Cs 2 CO 3 and 0.005 Sm 2 O 3 The same procedure as above was used, except for the addition of 1% Sm 3+ Doped Cs 2 UO 2 P 2 O 7 The emission spectrum of is shown in FIG. 18D and the results are shown in Table 17. [Table 17]
[0232] The change in color point indicates that there is energy transfer to the Eu, Pr and Sm ions. The measured QE of the phosphor containing the activator ion Sm is slightly decreased. 3+ The QE measurements of phosphors containing 1,2-dichloro-1,3-trifluoroethylene (1,2,3-tetrafluoroethylene) were improved. The QE measurements were further improved by adding a washing step. The water washing step not only slightly increased the QE of the samples, but also demonstrated that the host lattice was not hygroscopic.
[0233] Example 18: Various amounts of Eu 3+ Doped Cs2 UO 2 P 2 O 7 Preparation of phosphors 1%Eu 3+ Doped Cs 2 UO 2 P 2 O 7 To prepare Cs 2 CO 3 , H.U.O. 2 PO 4 -4H 2 O, (NH 4 ) 2 HPO 4 and Eu 2 O 3 were weighed out in a molar ratio of 0.995:1:1:0.005 and then placed in a Nalgene bottle containing zirconia media and ball milled for 2 hours. After the mixture was thoroughly blended, the powder was transferred to an alumina crucible and fired at 500°C for 5 hours, then the mixture was sieved through a 40 mesh sieve and blended again in the same Nalgene bottle for an additional 2 hours. The powder was transferred back to the alumina crucible and fired at 900°C for 5 hours. After the final firing, a yellow body colored powder was obtained. 2 UO 2 P 2 O 7 :1%Eu 3+ The results are shown in Table 18.
[0234] 2% molar amount of Eu 3+ Doped Cs 2 UO 2 P 2 O 7 To prepare 0.99% Cs 2 CO 3 and 0.01 Eu 2 O 3 The same procedure as above was used, except for the addition of Cs. 2 UO 2 P 2 O 7 :2%Eu 3+ The results are shown in Table 18.
[0235] 3% molar amount of Eu 3+ Doped Cs2 UO 2 P 2 O 7 To prepare 0.985Cs 2 CO 3 and 0.015 Eu 2 O 3 The same procedure as above was used, except for the addition of Cs. 2 UO 2 P 2 O 7 :3%Eu 3+ The results are shown in Table 18. [Table 18]
[0236] This specification uses examples to disclose the invention, including the best mode, and to enable those skilled in the art to practice the invention, including making and using any device or system, and performing any incorporated methods. The patentable scope of the invention is defined by the claims, and may include other examples that occur to those skilled in the art. Such other examples are intended to be within the scope of the claims if they have structural elements that do not differ from the literal language of the claims, or if they include equivalent structural elements that do not differ insubstantially from the literal language of the claims.
Claims
1. (i) A phosphor having formula I or II, [Ba 1-a-b Sr a Ca b ] x [Mg,Zn] y (UO 2 ) z ([P,V]O 4 ) 2(x+y+z)/3 (I) [BL 1-a-b Sr a Ca b ] p (OO 2 ) q [P,V] r O (2p+2q+5r)/2 (II), The phosphor having the formula I or II is Pr 3+ , Sm 3+ or mixtures thereof, wherein 0≦a≦1, 0≦b≦1, 0.75≦x≦1.25, 0.75≦y≦1.25, 0.75≦z≦1.25, 2.5≦p≦3.5, 1.75≦q≦2.25, and 3.5≦r≦4.5; (ii) A phosphor having the formula I or II, wherein the phosphor having the formula I or II is Eu 3+ , P 3+ , Sm 3+ and mixtures thereof, and a counterion comprising one or more alkali metal ions; (iii) a phosphor having formula III, A 2 OO 2 [P,V] 2 O 7 (III) The phosphor having the formula III is Eu 3+ , P 3+ , Sm 3+ and mixtures thereof, wherein A is Li, Na, K, Rb, Cs, or a combination thereof. A uranium-based phosphor selected from the group consisting of:
2. The uranium-based phosphor is (i) a phosphor having the formula I or II, 3+ , Sm 3+ 10. The uranium-based phosphor of claim 1, which is an activator ion doped phosphor comprising:
3. The phosphor having the formula I or II is Ba 3 (P.O. 4 ) 2 (U.O. 2 ) 2 P 2 O 7 , BaZnUO 2 (P.O. 4 ) 2 , BaMgUO 2 (P.O. 4 ) 2 , and wherein the phosphor having the formula III is selected from the group consisting of Na 2 UO 2 P 2 O 7 , K 2 UO 2 P 2 O 7 , Rb 2 UO 2 P 2 O 7 , and Cs 2 UO 2 P 2 O 7 2. The uranium-based phosphor of claim 1 , wherein the uranium-based phosphor is selected from the group consisting of:
4. The uranium-based phosphor is (ii) a phosphor having formula I or II, 3+ , P 3+ , Sm 3+ 10. The uranium-based phosphor of claim 1, which is a phosphor doped with activator ions selected from the group consisting of: ##STR1## and mixtures thereof, and counterions comprising one or more alkali metal ions.
5. The one or more alkali metal ions are Li + , Na + , K + , Rb + and Cs + 5. The uranium-based phosphor of claim 4 selected from the group consisting of:
6. The uranium-based phosphor is a phosphor having the formula (iii) III, 3+ , P 3+ , Sm 3+ 10. The uranium-based phosphor of claim 1, which is a phosphor doped with an activator ion selected from the group consisting of:
7. 10. The uranium-based phosphor of claim 1, wherein the counterion is present in an amount from about 0.1 mol % to about 10 mol %.
8. A uranium-based phosphor having the formula (III), (IV) or (V): A 2 OO 2 [P,V] 2 O 7 (III), A 4 UO 2 ([P, V]O 4 ) 2 (IV), or AUO 2 ([P,V]O 3 ) 3 (V), A uranium-based phosphor, wherein A is Li, Na, K, Rb, Cs, or a combination thereof.
9. The uranium-based phosphor is K 2 UO 2 P 2 O 7 , Na 2 UO 2 P 2 O 7 , Rb 2 UO 2 P 2 O 7 , Cs 2 UO 2 P 2 O 7 , K 4 UO 2 (P.O. 4 ) 2 or NaUO 2 P 3 O 9 9. The uranium-based phosphor according to claim 8 ,
10. 9. The uranium-based phosphor of claim 1 or claim 8, wherein the uranium-based phosphor has a D50 particle size of about 0.1 μm to about 15 μm.
11. 9. The uranium-based phosphor of claim 1 or claim 8 and a red-emitting phosphor having formula VI, A x MF y :Mn 4+ (VI) wherein A is Li, Na, K, Rb, Cs, or a combination thereof; M is Si, Ge, Sn, Ti, Zr, Al, Ga, In, Sc, Hf, Y, La, Nb, Ta, Bi, Gd, or a combination thereof; and x is MF y a red-emitting phosphor, wherein y is the absolute value of the charge of the ion, and y is 5, 6, or 7.
12. The red light emitting phosphor is K 2 (TiF 6 ): Mn 4+ , K 2 (SnF 6 ): Mn 4+ , Cs 2 (TiF 6 ): Mn 4+ , Rb 2 (TiF 6 ): Mn 4+ , Cs 2 (SiF 6 ): Mn 4+ , Rb 2 (SiF 6 ): Mn 4+ , Na 2 (SiF 6 ): Mn 4+ , Na 2 (TiF 6 ): Mn 4+ , Na 2 (ZrF 6 ): Mn 4+ , K 3 (ZrF 7 ): Mn 4+ , K 3 (BiF 7 ): Mn 4+ , K 3 (Y.F. 7 ): Mn 4+ , K 3 (LaF 7 ): Mn 4+ , K 3 (GdF 7 ): Mn 4+ , K 3 (NbF 7 ): Mn 4+ Or K 3 (TaF 7 ): Mn 4+ The phosphor composition of claim 11 , comprising:
13. The red-emitting phosphor is K 2 SiF 6 : Mn 4+ The phosphor composition according to claim 11 ,
14. 12. The phosphor composition of claim 11, wherein the red-emitting phosphor is at least partially coated with a surface coating comprising a metal fluoride or silica.
15. The metal fluoride is MgF 2 , CaF 2 , SrF 2 , BaF 2 , AgF, ZnF 2 , AlF 3 15. The phosphor composition of claim 14, wherein the phosphor composition is selected from the group consisting of:
16. 12. The phosphor composition of claim 11, wherein the uranium-based phosphor and the red-emitting phosphor have a D50 particle size of about 0.1 μm to about 15 μm.
17. A phosphor composition comprising the uranium-based phosphor of claim 1 or claim 8 and at least one other luminescent material.
18. The at least one other luminescent phosphor material is [Ba, Sr, Ca] 2 SiO 4 :Eu 2+ , [Y, Gd, Lu, Tb] 3 [Al, Ga] 5 O 12 : Ce 3+ , β-SiAlON:Eu 2+ , [Sr, Ca, Ba] [Ga, Al] 2 S 4 :Eu 2+ , [Li,Ca]α-SiAlON:Eu 2+ , [Ba, Sr, Ca] 2 S 5 N 8 :Eu 2+ , [Ca,Sr]AlSiN 3 :Eu 2+ , [Ba,Sr,Ca]LiAl 3 N 4 :Eu 2+ , [Sr,Ca,Mg]S:Eu 2+ , K 2 SiF 6 : Mn 4+ 20. The phosphor composition of claim 17 comprising a phosphorescent dye, a color filter pigment, a scattering particle, a polyfluorene, or a quantum dot material.
19. 20. The phosphor composition of claim 18, wherein the quantum dot material comprises perovskite quantum dots.
20. 10. A device comprising an LED light source radiatively and / or optically coupled to the uranium-based phosphor of claim 1 or claim 8.
21. 1. A red-emitting phosphor having formula VI, A x MF y :Mn 4+ (VI) wherein A is Li, Na, K, Rb, Cs, or a combination thereof; M is Si, Ge, Sn, Ti, Zr, Al, Ga, In, Sc, Hf, Y, La, Nb, Ta, Bi, Gd, or a combination thereof; and x is MF y 21. The device of claim 20, further comprising a red-emitting phosphor, where y is the absolute value of the charge of the ion, and y is 5, 6, or 7.
22. [Ba, Sr, Ca] 2 SiO 4 :Eu 2+ , [Y, Gd, Lu, Tb] 3 [Al, Ga] 5 O 12 : Ce 3+ , β-SiAlON:Eu 2+ , [Sr, Ca, Ba] [Ga, Al] 2 S 4 :Eu 2+ , [Li,Ca]α-SiAlON:Eu 2+ , [Ba, Sr, Ca] 2 S 5 N 8 :Eu 2+ , [Ca,Sr]AlSiN 3 :Eu 2+ , [Ba,Sr,Ca]LiAl 3 N 4 :Eu 2+ , [Sr,Ca,Mg]S:Eu 2+ , K 2 SiF 6 : Mn 4+ 21. The device of claim 20, further comprising at least one other light emitting material comprising a polyfluorene, a polyfluorene, or a quantum dot material.
23. 23. The device of claim 22, wherein the uranium-based phosphor and the at least one other luminescent material are in the form of a film and are disposed remotely from the LED light source.
24. 24. The device of claim 23, wherein the at least one other luminescent material further comprises a quantum dot material, the film being a multi-layer structure, each layer of the multi-layer structure comprising at least one phosphor or quantum dot material.
25. 21. A lighting apparatus comprising a device according to claim 20.
26. A backlighting apparatus comprising the device according to claim 20.
27. A display apparatus comprising the device of claim 20.
28. 21. The device of claim 20, wherein the LED light source is a mini-LED or a micro-LED.
29. A television comprising the backlight device according to claim 26.
30. A mobile phone comprising the backlight device according to claim 26.
31. A computer monitor comprising a backlight device according to claim 26.
32. A laptop comprising a backlight device according to claim 26.
33. A tablet computer comprising the backlight device according to claim 26.
34. 27. An automotive display comprising the backlight device according to claim 26.
35. A horticultural lighting apparatus comprising a device according to claim 20.
36. 1. A red-emitting phosphor of formula VI, A x MF y :Mn 4+ (VI) wherein A is Li, Na, K, Rb, Cs, or a combination thereof; M is Si, Ge, Sn, Ti, Zr, Al, Ga, In, Sc, Hf, Y, La, Nb, Ta, Bi, Gd, or a combination thereof; and x is MF y 36. The horticultural lighting device of claim 35, further comprising a red-emitting phosphor, y being the absolute value of the charge of the ion, and y being 5, 6, or 7.
37. 10. A phosphor package for horticultural lighting, comprising a phosphor material comprising the uranium-based phosphor of claim 1 or 8.
38. 1. A red phosphor having formula VI: A x MF y :Mn 4+ (VI) wherein A is Li, Na, K, Rb, Cs, or a combination thereof; M is Si, Ge, Sn, Ti, Zr, Al, Ga, In, Sc, Hf, Y, La, Nb, Ta, Bi, Gd, or a combination thereof; and x is MF y 38. The horticultural lighting phosphor package of claim 37, further comprising a red phosphor, where y is the absolute value of the charge of the ion and is 5, 6, or 7.
39. 40. The phosphor package of claim 38, wherein the uranium based phosphor and the red phosphor have particle sizes between about 0.1 microns and about 5 microns and are dispersed in a film or sheet.
40. The activator ion is Sm 3+ Or P 3+ 38. The phosphor package of claim 37, wherein:
41. 38. The phosphor package of claim 37, wherein the uranium based phosphor has a particle size of about 0.1 microns to about 5 microns and is dispersed in a film or sheet.
Citation Information
Patent Citations
Red emitting phosphor materials for use in LED and LCD applications
US7358542B2
Red line emitting phosphor materials for use in LED applications
US7497973B2
Red line emitting phosphors for use in led applications
US7648649B2