Method for recycling polyolefin foam and compositions and articles obtained therefrom - Patents.com
A water-based adhesive system for polyolefin foam recycling addresses health and environmental issues by forming durable articles from recycled foam fragments, enhancing safety and sustainability.
Patent Information
- Application Number
- JP2024524680
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2021-11-18
- Filing Date
- 2022-10-13
- Publication Date
- 2024-11-08
AI Technical Summary
Existing methods for recycling polyolefin foam rely on organic solvent-based adhesives, which pose health and environmental risks, necessitating a safer, water-based adhesive solution for bonding polyolefin foam pieces.
A method involving a mixture of polyolefin foam fragments and an aqueous composition containing dispersed polyolefin particles, followed by water removal, to form new polyolefin foam articles.
Enables the creation of durable, reusable polyolefin foam articles using a water-based adhesive system, addressing health and environmental concerns associated with organic solvents.
Smart Images

Figure 2024541234000001 
Figure 2024541234000002 
Figure 2024541234000003
Abstract
Description
[Background technology]
[0001] Polyolefin foams are used in a variety of applications, including protective packaging (e.g., padding for electronic products during transport), building and construction applications (e.g., pipe insulation), recreational products (e.g., swim noodles and fitness mats), and automotive applications. There is an increasing need to recycle (regenerate) foam after use, or foam that has been produced for one purpose and then needs to be used for a different purpose. Post-consumer recycled (PCR) foam or post-industrial recycled (PIR) foam can be recycled by first mechanically reducing the foam into relatively small pieces (if the foam does not already exist as relatively small pieces) and then sintering the foam pieces using one or more adhesives to form a larger, useful article. Some adhesives that could be considered for use in this manner are organic solvent-based and suffer from various health and environmental drawbacks resulting from the use of organic solvents.
[0002] US Pat. No. 7,837,831 discloses tissue paper made from an aqueous dispersion containing an olefin polymer and natural or synthetic cellulose fibers.
[0003] It would be desirable to provide a method for recycling polyolefin foam that uses an effective water-based adhesive to bond pieces of polyolefin foam together to form new and useful polyolefin foam articles. Summary of the Invention
[0004] The following is a description of the present invention.
[0005] A first aspect of the present invention is a method for recycling polyolefin foam, comprising the steps of: a) providing a mixture, the mixture comprising: i) pieces of polyolefin foam; ii) an aqueous composition comprising dispersed polyolefin particles; b) removing water from the mixture.
[0006] A second aspect of the invention is a composition comprising: i) pieces of polyolefin foam; ii) an aqueous composition comprising dispersed polyolefin particles.
[0007] A third aspect of the invention is an article formed by a process comprising removing water from the composition of the second aspect. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0008] The following is a detailed description of the present invention.
[0009] As used herein, the following terms have the definitions specified, unless the context clearly indicates otherwise.
[0010] As used herein, a polymer is a relatively large molecule composed of the reaction product of smaller chemical repeating units. A polymer may have a structure that is linear, branched, star-shaped, looped, hyperbranched, crosslinked, or a combination thereof, and a polymer may have a single type of repeating unit ("homopolymer") or two or more types of repeating units ("copolymer"). A copolymer may have different types of repeating units arranged randomly, sequentially, in blocks, in other arrangements, or in any mixture or combination thereof. A polymer has a number average molecular weight of 1,000 or more.
[0011] As used herein, "weight of polymer" means the dry weight of the polymer.
[0012] As used herein, a "thermoplastic" polymer is one that meets the following criteria: A thermoplastic polymer is solid over the temperature range from absolute zero to Tsolid, where Tsolid is less than 200° C. At some temperature (Tflow) above Tsolid, the thermoplastic polymer becomes soft enough to change into a new shape under gravity or under mechanically applied forces. When the thermoplastic polymer is recooled to a temperature below Tsolid, it will generally retain the new shape. The softening of the polymer may be due to a glass transition, a melting transition, some other softening process, or a combination thereof.
[0013] Molecules that can react with each other to form repeat units of a polymer are referred to herein as "monomers." The repeat units so formed are referred to herein as "polymerized units" of the monomer.
[0014] An "olefin" is a hydrocarbon compound containing exactly one carbon-carbon double bond and no carbon-carbon triple bonds. Olefins may be linear, cyclic, branched, or combinations thereof. A "polyolefin" is a polymer in which 40 weight percent or more of the polymerized units are olefins, based on the weight of the polymer.
[0015] As used herein, a "vinyl ester" is a compound having the formula R3C-C(O)-O-CR=CR2, where each R group, independently of every other R group, is hydrogen or a substituted or unsubstituted organic group. As used herein, "(meth)acrylic acid" means acrylic acid, methacrylic acid, or a mixture thereof. As used herein, "(meth)acrylic acid ester" means an ester of (meth)acrylic acid, in which the ester group is a substituted or unsubstituted C1-C 20It means an ester of (meth)acrylic acid, which is an alkyl group. As used herein, a "diene" is a hydrocarbon compound that has exactly two carbon-carbon double bonds and no carbon-carbon triple bonds. The diene may be linear, branched, cyclic, or a combination thereof.
[0016] As used herein, a carboxylic acid compound is any of the following: a carboxylic acid in which the carboxyl group is in neutral, anionic, or a mixture thereof; a salt of a carboxylic acid; an ester of a carboxylic acid; or a mixture thereof. A sulfonate compound is a compound having a sulfonic acid group, which may be in neutral, anionic, salt, ester, or a mixture thereof.
[0017] As used herein, a "foam" is a solid article containing a plurality of cells. A cell is a gas-filled mass that is partially or completely surrounded by a solid material. If 50% or more of the cells are completely surrounded by a solid material by number, the foam is referred to as a "closed-cell" foam. Other foams are referred to as "open-cell" foams. Foams that are 50% or more by weight polyolefin are referred to as "polyolefin foams." When a polyolefin foam contains two or more polyolefins, the polyolefin in the foam that has the greatest weight percentage based on the weight of the foam is referred to herein as the "predominant" polyolefin in the foam. When a polyolefin foam contains exactly one polyolefin, that polyolefin is the predominant polyolefin.
[0018] A piece of polyolefin foam having no dimension greater than 20 cm is referred to herein as a "piece." The piece of polyolefin foam may be in the form in which it was found, or a larger piece of polyolefin foam may be reduced to the pieces, for example, by one or more mechanical processes, such as crushing, chopping, shearing, breaking, other mechanical processes, etc., or any combination thereof.
[0019] As used herein, a "particle" is a discrete article. A particle may be solid or liquid. As used herein, the "diameter" of a particle is considered to be the diameter of an imaginary sphere having the same volume as the actual particle. The "aspect" ratio of a particle is the ratio of its largest dimension to its smallest dimension. A particle is said to be "non-fibrous" herein if its aspect ratio is 2:1 or less. A "polyolefin particle" contains 50% or more by weight of polyolefin based on the weight of the particle.
[0020] As used herein, an "aqueous" composition is a composition that contains 30% or more by weight of water based on the weight of the composition. An aqueous medium is a continuous liquid medium that contains 50% or more by weight of water based on the weight of the medium. Particles are said to be "dispersed" in a liquid medium when they are distributed throughout the liquid medium. Particles dispersed in a liquid medium can form compositions that are commonly referred to as, for example, slurries, dispersions, emulsions, latexes, some other type of composition, or combinations thereof. A collection of particles dispersed in a liquid medium is characterized by a volume average diameter, which can be measured by light scattering, for example, by a Coulter LS230 device (Beckman Coulter Co., Indianapolis, IN, USA). Particle size distribution index is defined herein as the index obtained by dividing the volume average particle size Dv by the number average particle size Dn.
[0021] The melting temperature of a polymer is measured by Differential Scanning Calorimeter (DSC). An endothermic peak is observed at the melting temperature.
[0022] The crystallinity of a polymer is measured by observing the heat of fusion at the melting point generated in a DSC evaluation. "Crystallization" is determined by normalizing the observed heat of fusion to that of a 100% crystalline sample of the same polymer and is reported as a percentage.
[0023] The weight-average molecular weight (Mw) of a polymer sample is measured by light scattering in a dilute solution of the polymer using the intercept of a Zimm plot of scattering intensity versus polymer concentration and scattering angle. The polydispersity index is defined as the index obtained by dividing the weight-average molecular weight (Mw) by the number-average molecular weight (Mn).
[0024] The glass transition temperature (Tg) of a polymer sample is measured by DSC at 10° C. / min as the midpoint of a step change in the heat flow curve.
[0025] The melt index ("I2") of a polymer is measured according to ASTM D1238, condition 190°C / 2.16 kg. I2 is reported in grams dissolved per 10 minutes (g / 10 min).
[0026] The ratios presented herein are characterized as follows. For example, when a ratio is said to be 3:1 or more, it can be 3:1, or 5:1, or 100:1, but not 2:1. This characterization can be generally described as follows. When a ratio is said to be X:1 or more herein, it means that the ratio is Y:1, where Y is X or more. In another example, when a ratio is said to be 15:1 or less, it can be 15:1, or 10:1, or 0.1:1, but not 20:1. Generally, when a ratio is said to be W:1 or less herein, it means that the ratio is Z:1, where Z is W or less.
[0027] Preferably, the volume average particle size of the dispersed particles in the aqueous composition is 10 micrometers or less, more preferably 5 micrometers or less, more preferably 2.5 micrometers or less, more preferably 1.5 micrometers or less. Preferably, the volume average particle size of the dispersed particles in the aqueous composition is 0.05 micrometers or more, more preferably 0.1 micrometers or more, more preferably 0.2 micrometers or more. Preferably, the particle size distribution index of the dispersed particles in the aqueous composition is 2 or less, more preferably 1.9 or less, more preferably 1.7 or less, more preferably 1.5 or less.
[0028] Examples of suitable aqueous compositions containing dispersed polyolefin particles are disclosed, for example, in US Pat. No. 5,688,842, US Pat. No. 8,053,503, and US Pat. No. 8,163,837.
[0029] The polyolefin particles preferably contain polyolefin in an amount of 50% by weight or more, more preferably 60% by weight or more, more preferably 70% by weight or more, more preferably 80% by weight or more, more preferably 90% by weight or more, based on the total weight of the particle.
[0030] Preferably, the polyolefin particles contain one or more "first polyolefins." In the "first polyolefins," the polymerized units of the olefin are present in an amount of 70% by weight or more, more preferably 80% by weight or more, more preferably 90% by weight or more, based on the weight of the first polyolefin. Preferably, the first polyolefin contains polymerized units of one or more primary monomers, optionally one or more comonomers, and optionally one additional monomer. The primary monomers are ethylene, propylene, or mixtures thereof. The comonomers are one or more dienes, one or more vinyl esters, one or more olefins of the formula H2C=CHR, where R is C2-C 20 Linear, branched, or cyclic alkyl groups, or C6-C 20 aryl group), and mixtures thereof.
[0031] In the first polyolefin, the polymerized units of the main monomer are preferably either 90% by weight to 100% by weight of polymerized units of ethylene or 90% by weight to 100% by weight of polymerized units of propylene, more preferably 90% by weight to 100% by weight of polymerized units of ethylene, more preferably 100% by weight of polymerized units of ethylene, based on the weight of the polymerized units of the main monomer. In the first polyolefin, the amount of the polymerized units of the main monomer is preferably 65% by weight or more, more preferably 75% by weight or more, based on the weight of the first polyolefin. In the first polyolefin, the amount of the polymerized units of the main monomer is preferably 100% by weight or less, more preferably 99% by weight or less, more preferably 90% by weight or less, based on the weight of the first polyolefin.
[0032] With respect to the one or more comonomers, when one or more dienes are used in the first polyolefin, the comonomers are preferably C4 to C6 20 Linear, branched or cyclic dienes are preferred. When one or more vinyl esters are used in the first polyolefin, vinyl acetate is preferred. When one or more compounds having the formula H2C=CHR (as defined above) are used in the first polyolefin, 1-butene, 3-methyl-1-butene, 4-methyl-1-pentene, 3-methyl-1-pentene, 1-heptene, 1-hexene, 1-octene, 1-decene, 1-dodecene and mixtures thereof are preferred, and 1-heptene, 1-hexene, 1-octene, 1-decene, 1-dodecene and mixtures thereof are more preferred. In the first polyolefin, preferably, the comonomer comprises one or more compounds having the formula H2C=CHR. In the first polyolefin, the amount of the compound of formula H2CHR in the comonomer is preferably 50% by weight or more, more preferably 75% by weight or more, more preferably 90% by weight or more, more preferably 100% based on the weight of the comonomer. Preferably, the amount of polymerized units of the comonomer in the first polyolefin is 0-25% by weight, more preferably 1-25% by weight, based on the weight of the first polyolefin.
[0033] With regard to the additional monomer in the first polyolefin, preferably, any additional monomer used is different from any of the main monomers and different from any of the comonomers. Preferably, little or no polymerized units of the additional monomer are present in the first polyolefin. That is, preferably, the amount of polymerized units of the additional monomer present in the first polyolefin is 0-10 wt%, more preferably 0-1 wt%, more preferably 0 wt%, based on the weight of the first polyolefin.
[0034] Preferably, the first polyolefin is thermoplastic. Preferably, the first polyolefin has a crystallinity of less than 50%, preferably less than 25%. Preferably, the first polyolefin has a weight average molecular weight of 15,000 or more, more preferably 20,000 or more. Preferably, the first polyolefin has a weight average molecular weight of 5,000,000 or less, more preferably 1,000,000 or less. Preferably, the first polyolefin has a molecular weight polydispersity index of 1.01 or more, more preferably 1.5 or more, more preferably 1.8 or more. Preferably, the first polyolefin has a molecular weight polydispersity index of 40 or less, more preferably 20 or less, more preferably 10 or less.
[0035] Preferably, the first polyolefin has a glass transition temperature of 50° C. or less, more preferably 40° C. or less. Preferably, the first polyolefin has a glass transition temperature of 25° C. or more, more preferably 30° C. or more. Preferably, the first polyolefin has a melting temperature of 140° C. or less, more preferably 130° C. or less, more preferably 120° C. or less. Preferably, the first polyolefin has a melt index, in grams per 10 minutes, of 0.001 or more, more preferably 0.5 or more, more preferably 100 or more. Preferably, the first polyolefin has a melt index, in grams per 10 minutes, of 1,000 or less, more preferably 800 or less, more preferably 700 or less.
[0036] Examples of suitable first polyolefins include, for example, the following: heterogeneously branched polyolefins, including linear low density polyethylene (LLDPE) and copolymers; heterogeneously branched ultra low density linear polyethylene (ULDPE), homogeneously branched linear copolymers of ethylene and one or more α-olefins other than ethylene, and homogeneously branched substantially linear copolymers of ethylene and one or more α-olefins other than ethylene.
[0037] Preferably, the aqueous composition further contains one or more dispersants.The dispersant molecules may be dissolved in the continuous aqueous phase, or may be attached to one or more polyolefin particles, or may be partially present on the surface of the polyolefin particles and partially present in the continuous aqueous phase.Suitable dispersants include non-polymeric carboxylic acid compounds, non-polymeric sulfonate compounds, olefin / (meth)acrylic acid copolymers, sulfated or phosphated polyoxyethylenated alcohols, ethylene oxide / propylene oxide / ethyleneoxy block copolymers, primary and secondary alcohol ethoxylates, alkyl glycosides, alkyl glycerides, and mixtures thereof.
[0038] Among the non-polymeric carboxylic acid compounds, those in which the carboxylic acid portion of the molecule contains 8 or more carbon atoms, more preferably 12 or more carbon atoms, more preferably 15 or more carbon atoms are preferred. Among the non-polymeric carboxylic acid compounds, those in which the carboxylic acid portion of the molecule contains 60 or less carbon atoms, more preferably 30 or less carbon atoms are preferred. Among the non-polymeric carboxylic acid compounds, salts in which the cation is selected from an alkali metal cation, an alkaline earth cation, an ammonium cation, an alkylammonium cation, or mixtures thereof are preferred.
[0039] Preferably, the dispersant comprises one or more olefin / (meth)acrylic acid copolymers. Among the olefin / (meth)acrylic acid copolymers, copolymers comprising polymerized units of ethylene, propylene, or a mixture thereof are preferred. Among the olefin / (meth)acrylic acid copolymers, preferably, the polymerized units of the olefin monomer are either 90% by weight to 100% by weight of polymerized units of ethylene or 90% by weight to 100% by weight of polymerized units of propylene, more preferably 90% by weight to 100% by weight of polymerized units of ethylene, more preferably 100% by weight of polymerized units of ethylene, based on the weight of all polymerized units of the olefin monomer. Among the olefin / (meth)acrylic acid copolymers, preferably, the amount of polymerized units of the olefin monomer is preferably 40% by weight or more, more preferably 50% by weight or more, based on the weight of the olefin / (meth)acrylic acid copolymer. In the olefin / (meth)acrylic acid copolymer, preferably the amount of polymerized units of olefin monomer is preferably 98 wt % or less, more preferably 95 wt % or less, more preferably 90 wt % or less, more preferably 70 wt % or less, based on the weight of the olefin / (meth)acrylic acid copolymer.
[0040] Among the olefin / (meth)acrylic acid copolymers, preferably, the olefin / (meth)acrylic acid copolymer contains 2% by weight or more of polymerized units of (meth)acrylic acid based on the weight of the olefin / (meth)acrylic acid copolymer. More preferably, the amount of polymerized units of (meth)acrylic acid in the olefin / (meth)acrylic acid copolymer is 5% by weight or more, more preferably 10% by weight or more, more preferably 30% by weight or more based on the weight of the olefin / acrylic acid copolymer. Preferably, the amount of polymerized units of (meth)acrylic acid in the olefin / (meth)acrylic acid copolymer is 60% by weight or less, more preferably 50% by weight or less based on the weight of the olefin / (meth)acrylic acid copolymer.
[0041] The olefin / (meth)acrylic acid copolymer optionally contains polymerized units of one or more additional monomers, i.e., polymerized units of monomers other than an olefin monomer and (meth)acrylic acid. Preferably, little or no polymerized units of the additional monomer are present in the olefin / (meth)acrylic acid copolymer. That is, preferably, the amount of polymerized units of the additional monomer present in the olefin / (meth)acrylic acid copolymer is 0-10 wt%, more preferably 0-1 wt%, more preferably 0 wt%, based on the weight of the olefin / (meth)acrylic acid copolymer.
[0042] Preferably, the aqueous composition contains both one or more first polyolefins and one or more dispersants. Preferably, the weight ratio of the first polyolefin to the dispersant is less than or equal to 300:1. Preferably, the weight ratio of the first polyolefin to the dispersant is greater than or equal to 0.5:1.
[0043] When the dispersant contains one or more olefin / (meth)acrylic acid copolymers, preferably the weight ratio of the first polyolefin to the olefin / (meth)acrylic acid copolymer is not more than 20:1, more preferably not more than 10:1, more preferably not more than 6:1. When the dispersant contains one or more olefin / (meth)acrylic acid copolymers, preferably the weight ratio of the first polyolefin to the dispersant is not less than 0.5:1, more preferably not less than 0.75:1, more preferably not less than 1:1.
[0044] When the dispersant contains one or more non-polymeric carboxylic acid compounds, preferably the weight ratio of the first polyolefin to the non-polymeric carboxylic acid compounds is not greater than 300:1, more preferably not greater than 200:1, more preferably not greater than 120:1. When the dispersant contains one or more non-polymeric carboxylic acid compounds, preferably the weight ratio of the first polyolefin to the non-polymeric carboxylic acid compounds is not less than 5:1, more preferably not less than 10:1, more preferably not less than 16:1.
[0045] The aqueous composition contains a continuous liquid medium and also contains dispersed polyolefin particles. The amount of water in the continuous liquid medium is preferably 50% by weight or more, more preferably 75% by weight or more, more preferably 85% by weight or more, based on the weight of the continuous liquid medium.
[0046] Preferably, the amount of polyolefin in the aqueous composition is 25% by weight or more, more preferably 30% by weight or more, more preferably 35% by weight or more, more preferably 40% by weight or more, based on the weight of the aqueous composition. Preferably, the amount of polyolefin in the aqueous composition is 75% by weight or less, more preferably 70% by weight or less, more preferably 60% by weight or less, more preferably 50% by weight or less, based on the weight of the aqueous composition.
[0047] Preferably, the pH of the aqueous composition is greater than or equal to 5, more preferably greater than or equal to 7. Preferably, the pH of the aqueous composition is less than or equal to 11.5, more preferably less than or equal to 11. Optionally, the pH of the aqueous composition may be adjusted by including one or more acids or bases in the aqueous composition.
[0048] The present invention also involves the use of fragments of polyolefin foam. Preferably, the polyolefin foam is recycled. Preferably, the polyolefin is present in the foam in an amount of 60% by weight or more, more preferably 70% by weight or more, more preferably 80% by weight or more, based on the weight of the foam. In the polyolefin foam, the amount of the polymerization units of the main monomer is preferably either 90% by weight to 100% by weight of polymerization units of ethylene or 90% by weight to 100% by weight of polymerization units of propylene, more preferably 90% by weight to 100% by weight of polymerization units of ethylene, more preferably 100% by weight of polymerization units of ethylene. In the polyolefin foam, the amount of the polymerization units of the main monomer is preferably 75% by weight to 100% by weight, more preferably 90% by weight to 100% by weight, based on the weight of the total polymerization units in the polyolefin foam. In the polyolefin foam, the amount of the polymerized units of the comonomer is preferably 0% by weight to 25% by weight, more preferably 0% by weight to 10% by weight, based on the weight of all the polymerized units in the polyolefin foam. Preferably, the polyolefin in the polyolefin foam contains low density polyethylene (LDPE) in an amount of 80% by weight or more, or 90% by weight or more, based on the weight of the polyolefin foam.
[0049] Preferably, the primary polyolefin in the polyolefin foam is either crosslinked or has a melting temperature (Tmfoam) of 150° C. or less, more preferably, it is crosslinked or has a Tmfoam of 120° C. or less. Preferably, the primary polyolefin in the polyolefin foam is either crosslinked or has a melting temperature (Tmfoam) of 60° C. or more, more preferably, it is crosslinked or has a Tmfoam of 80° C. or more.
[0050] The polyolefin foam optionally contains one or more nucleating agents. Suitable nucleating agents include, for example, talc, citric acid, and sodium bicarbonate. The amount of nucleating agent in the polyolefin foam, if present, is preferably 15 wt% or less based on the weight of the polyolefin foam.
[0051] The polyolefin foam optionally contains one or more blowing agents. A suitable blowing agent is, for example, glycerol monostearate. The amount of blowing agent in the polyolefin foam, if present, is preferably 5 wt.% or less based on the weight of the polyolefin foam.
[0052] The polyolefin foam may be an open-cell foam, or a closed-cell foam, or a combination thereof. Suitable polyolefin foams may be, for example, high density foams or low density foams. High density foams typically have a volume average cell size of 50 to 200 micrometers. High density foams typically have a volume average cell size of 240 kg / m 3 (15lb / ft 3 ) higher. Low density foams typically have a volume average cell size of 100 to 3,000 micrometers. Low density foams typically have a volume average cell size of 8 kg / m 3 (0.5 lb / ft 3 )~240kg / m 3 (15lb / ft 3 )
[0053] The polyolefin in the polyolefin foam may be thermoplastic or crosslinked. Either type of foam is suitable for use in the present invention. Of particular interest in the practice of the present invention are crosslinked foams, because they typically cannot be recycled by melting and reforming. Thus, the present invention is advantageous because it provides a method for making new useful articles from already used crosslinked foams.
[0054] In the practice of the present invention, the polyolefin foam is present in the form of a plurality of pieces. Each piece may be characterized by its maximum dimension ("DMAX"). The collection of pieces may be characterized by a D90, which is a size such that 90% or more of the pieces by weight, based on the weight of all the pieces, have a DMAX of D90 or less. Preferably, the collection of pieces of polyolefin foam has a D90 of 20 cm or less, more preferably 12 cm or less, more preferably 7 mm or less. Preferably, 90% or more of the pieces by weight, based on the weight of all the pieces, are non-fibrous.
[0055] In some embodiments, the foam is produced as a relatively large article, such as a sheet, board, or plank, for example, by extrusion, and then mechanically reduced into smaller pieces. Other than the size reduction, it is contemplated that these foam pieces will retain the properties of the original foam article, such as cell size, foam density, and porosity.
[0056] The present invention includes the use of a mixture of polyolefin foam shreds and an aqueous composition. The mixture can be made by any method. Examples of suitable methods include, for example, blending (e.g., combining the aqueous composition and polyolefin foam shreds in a container and stirring the mixture); dip coating (e.g., placing the aqueous composition in a first container and immersing the polyolefin foam shreds in the aqueous composition until the polyolefin foam shreds are coated with the aqueous composition, then removing the coated polyolefin foam shreds to another container); spray coating (e.g., spraying the aqueous composition onto the polyolefin foam shreds); other methods; and combinations thereof.
[0057] In a preferred embodiment, one of the following conditions ("I" or "II") exists: I) the dispersed polyolefin particles contain 50% by weight or more of polymerized units of ethylene, based on the total weight of all polymerized units in all polymers in the dispersed polyolefin particles; the polyolefin foam fragments comprising 50 wt. % or more of polymerized units of ethylene, based on the total weight of all polymerized units in the polyolefin foam fragments; Or, II) the dispersed polyolefin particles contain 50% by weight or more of polymerized units of propylene, based on the total weight of all polymerized units in all polymers in the dispersed polyolefin particles; The polyolefin foam fragments contain 50% by weight or more of polymerized units of propylene, based on the total weight of all polymerized units in the polyolefin foam fragments.
[0058] Condition I is preferred. When Condition I is implemented, preferably the amount of polymerized units of ethylene in all polymers in the dispersed polyolefin particles is 60% by weight or more, more preferably 70% by weight or more, more preferably 80% by weight or more, based on the total weight of all polymerized polyolefin particles. When Condition I is implemented, preferably the amount of polymerized units of ethylene in the polyolefin foam is 60% by weight or more, more preferably 70% by weight or more, more preferably 80% by weight or more, based on the total weight of all polymerized units in the polyolefin foam fragments.
[0059] When condition II is implemented, preferably the amount of polymerized units of propylene in all polymers in the dispersed polyolefin particles is 60 wt% or more, more preferably 70 wt% or more, more preferably 80 wt% or more, based on the total weight of all polymerized polyolefin particles.When condition II is implemented, preferably the amount of polymerized units of propylene in the polyolefin foam is 60 wt% or more, more preferably 70 wt% or more, more preferably 80 wt% or more, based on the total weight of all polymerized units in the polyolefin foam fragments.
[0060] The mixture of the aqueous composition and the polyolefin foam fragments can be characterized by the ratio of the weight of the polyolefin in the aqueous composition to the weight of the polyolefin foam. Preferably, the ratio is 0.2:1 or more, more preferably 0.5:1 or more, more preferably 0.75:1 or more. Preferably, the ratio is 5:1 or less, more preferably 3:1 or less.
[0061] The practice of the present invention involves removing water from a mixture of an aqueous composition and polyolefin foam particles.Preferably, water is removed by a process involving water evaporation.To accelerate the removal of water, the mixture can be subjected to, for example, one or more of the following: a temperature above 30°C; moving air; and combinations thereof.
[0062] When a temperature above 30° C. is used, it is preferably 60° C. or higher, more preferably 70° C. or higher. When a temperature above 30° C. is used, it is preferably 150° C. or lower, more preferably 125° C. or lower. Temperatures above 30° C. can be achieved by any method. Some suitable methods include, for example, exposure to radiation (e.g., infrared radiation, etc.), exposure to heated gas (e.g., heated air, etc.), other heating methods, and combinations thereof.
[0063] If moving air is desired to be used, one suitable method is to place the mixture in an oven that mechanically moves air within the oven, such as, for example, a convection oven. If the mixture is placed in an oven that mechanically moves air within the oven, the mixture may be exposed to both moving air and temperatures above 30° C. simultaneously. Alternatively, the mixture may be exposed to moving air in a situation other than within an oven (with or without simultaneous exposure to temperatures above 30° C.). Alternatively, moving air may not be used.
[0064] When the mixture is exposed to a temperature above 30° C., it is preferred that the mixture reach a temperature equal to or greater than the Tflow of the first polyolefin. It is contemplated that when the mixture reaches a temperature equal to or greater than the Tflow of the first polyolefin, some or all of the particles containing the first polyolefin tend to fuse together, bonding the pieces of polyolefin foam into a single mass.
[0065] It is contemplated that exposure to temperatures above 30°C will aid in both the fusion of the particles of the first polyolefin and the removal of water from the mixture. These effects may be achieved in any order, or simultaneously, or any combination thereof. For example, the mixture may first be exposed to conditions that optimize water removal (e.g., relatively low temperature and relatively high air flow), and then to conditions that optimize particle fusion (e.g., relatively high temperature). In another example, the mixture may first be exposed to conditions that optimize particle fusion, and then to conditions that optimize water removal. In another example, conditions may be selected that allow particle fusion and water removal to occur simultaneously. It is contemplated that when conditions that optimize or favor one effect (e.g., water removal) are applied, other processes (e.g., particle fusion) will occur to some degree simultaneously.
[0066] When the mixture is exposed to a temperature above 30° C. and the predominant polyolefin in the polyolefin foam is thermoplastic, the maximum temperature Tmax attained by the mixture shall conform to Tmax<(T2-10° C.), where T2 is the Tsoft of the predominant polyolefin in the polyolefin foam. It is expected that maintaining Tmax at 10° C. below T2 will allow the polyolefin foam fragments to retain their foam structure without collapsing.
[0067] Optionally, mechanical pressure is applied to the mixture while it is at a temperature sufficient to soften some or all of the polyolefin in the particles from the aqueous composition.
[0068] After removing the water from the mixture, if it was heated, it is returned to an ambient temperature of about 25° C., and the remaining composition is considered herein to be the finished article. It is contemplated that some water may be retained in the finished article. Preferably, the amount of water in the finished article is 20% by weight or less, more preferably 10% by weight or less, more preferably 5% by weight or less, based on the weight of the finished article.
[0069] The polyolefin foam pieces may, for example, be placed in a container that acts as a mold to determine the final shape of the finished article. The polyolefin foam pieces may be placed in such a container either before or after the polyolefin foam pieces are contacted with the aqueous composition. EXAMPLES
[0070] The following are examples of the present invention. Unless otherwise stated, operations were carried out at room temperature (about 23° C.).
[0071] The following materials were used: "Binder" = HYPOD(TM) 8501 aqueous acid-modified ethylene copolymer-based polyolefin dispersion, approximately 45% solids by weight, manufactured by Dow Chemical Company · Reclaimed (recycled) foam: Previously manufactured polyolefin foam was reduced to pieces with a D90 of less than 5mm.
[0072] Example 1 97 grams of binder was mixed with the recycled foam in the bath until a uniform coverage of binder on the foam particles was achieved. The binder coated foam particles were placed into a heavy duty aluminum loaf pan measuring 21.6 cm x 11.7 cm x 7.0 cm (8.5 in x 4.6 in x 2.75 in). Using another pan as a lid, the sample was placed in a convection oven set at 90°C for 50 minutes and a 1.8 kg (4 lb) weight was placed on the lid. The lid was then removed and the sample was dried in the oven at 90°C for 2 hours.
[0073] Example 2 Same as Example 1 except that a hole was drilled in the lid.
[0074] Example 3 The binder was spray coated evenly onto 15 grams of recycled foam. The spray coated foam particles were placed in a 90° C. oven for 30 minutes. The coated foam was then weighed, resulting in 16.7 grams, demonstrating that 1.6 grams of polymer from the binder coated the 15 grams of recycled foam particles. The coated foam particles were placed in a pan and then covered with a lid. A 4 pound weight was placed on top of the lid. The pan was placed in a 90° C. oven for 10 minutes. An additional 4 pound weight was placed on the lid and the pan was placed in the 90° C. oven for an additional 10 minutes.
[0075] Example 4 15 grams of foam was immersed in a bath of binder and mixed until a uniform coating was achieved. The dip-coated foam particles were placed in a 90° C. oven for 50 minutes. At that point, the coated foam particles weighed 30 grams, demonstrating that 15 grams of polymer from the binder had coated 15 grams of recycled foam. The coated foam particles were then placed in a 4 pound lidded pan in a 90° C. oven for 5 minutes. An additional 4 pound weight was placed on the lid and the pan was placed in the 90° C. oven for an additional 10 minutes.
[0076] The result of each of Examples 1-4 was a solid block containing polyolefin foam that was robust when handled and that appeared to be useful in any of a wide variety of applications, such as, for example, protective packaging (e.g., padding for electronic products during transport), building and construction applications (e.g., pipe insulation), recreational products (e.g., swim noodles and fitness mats), and automotive applications.
Claims
1. 1. A method for recycling polyolefin foam, comprising the steps of: a) providing a mixture, said mixture comprising: i) pieces of polyolefin foam; ii) an aqueous composition comprising dispersed polyolefin particles; b) removing water from said mixture.
2. 10. The method of claim 1, further comprising the step of: c) fusing or allowing some or all of the dispersed polyolefin particles to fuse together.
3. The method of claim 1, wherein the dispersed polyolefin particles have a volume average particle size of from 0.05 micrometers to 10 micrometers.
4. The dispersed polyolefin particles are a first polyolefin, based on the weight of the first polyolefin, i) 65% to 99% by weight of ethylene or propylene or a mixture thereof; ii) 1% to 25% by weight of one or more dienes, one or more vinyl esters, of formula H 2 C=CHR (wherein R is C 2 ~C 20 A linear, branched, or cyclic alkyl group, or C 6 ~C 20 aryl group), and mixtures thereof; and 3. The method of claim 1, comprising: a first polyolefin comprising polymerized units of iii) from 0 to 10 weight percent of one or more monomers different from i) and ii).
5. The method of claim 1 , wherein the aqueous composition further comprises one or more olefin / (meth)acrylate copolymers.
6. 2. The method of claim 1, wherein the dispersed polyolefin particles comprise 50 wt% or more polymerized units of ethylene, based on the total weight of all polymerized units in all polymers in the dispersed polyolefin particles, and the polyolefin foam pieces comprise 50 wt% or more polymerized units of ethylene, based on the total weight of all polymerized units in the polyolefin foam pieces.
7. 2. The method of claim 1, wherein the dispersed polyolefin particles comprise 50 wt. % or more polymerized units of propylene, based on the total weight of all polymerized units in all polymers in the dispersed polyolefin particles, and the polyolefin foam pieces comprise 50 wt. % or more polymerized units of propylene, based on the total weight of all polymerized units in the polyolefin foam pieces.
8. 10. The method of claim 1, wherein the polyolefin foam shreds comprise 80% or more by weight of low density polyethylene, based on the total weight of the polyolefin foam shreds.
9. 1. A composition comprising: i) pieces of polyolefin foam; ii) an aqueous composition comprising dispersed polyolefin particles.
10. 10. An article formed by a process comprising removing water from the composition of claim 9.
Citation Information
Patent Citations
Dispersion of highly crystallinity olefins
JP2011501764A
Method for producing molded parts from particle foams
WO2021009720A2