Polypropylene microspheres and their manufacturing method, 3D printing raw materials and applications
By employing direct copolymerization with a tailored catalyst system, polypropylene microspheres with uniform crystalline distribution and spherical morphology are produced, addressing irregularity issues in existing methods, enhancing 3D printing performance and foamed material quality.
Patent Information
- Application Number
- JP2024525712
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2021-10-27
- Filing Date
- 2022-10-27
- Publication Date
- 2024-11-08
Smart Images

Figure 2024541265000001_ABST
Abstract
Description
Detailed Description of the Invention
[0001] CROSS-REFERENCE TO RELATED APPLICATIONS The present invention claims priority to a Chinese patent application entitled "Polymerized Synthetic Polypropylene Microspheres" filed on October 27, 2021, with application number CN202111258205.6, the entire contents of which are incorporated herein by reference.
[0002] [Technical field] The present invention relates to the technical field of polypropylene materials, in particular to polypropylene microspheres and their manufacturing method, 3D printing raw material and applications.
[0003] [Background technology] 3D printing, also known as "additive manufacturing," is a type of rapid molding technology that uses a 3D printer to print materials such as metal powder or plastic according to a digital design, layer by layer, and finally complete the manufacture of an item. This technology allows for on-demand production at any time and anywhere, and is applied to fields such as daily necessities such as footwear, construction, automotive, aerospace, medicine, and education. This emerging technology is gradually changing human life, and its future potential is widely seen in various industries. The weekly magazine Time ranked 3D printing as the "fastest growing industry in the United States." The British magazine The Economist believes that 3D printing will drive the third industrial revolution.
[0004] Selective Laser Sintering (SLS) technology is a rapid molding technology that is currently the most widely applied and most promising technology in additive manufacturing technology, and has a tendency to develop rapidly in recent years. SLS technology is a technology in which a computer first scans a three-dimensional object, then a high-intensity laser is used to irradiate the material powder that has been laid on the worktable or part in advance, selectively melting and sintering it layer by layer, and then molding it layer by layer. SLS technology has a high degree of design flexibility, can produce accurate models and prototypes, has a reliable structure, can mold parts that can be directly used, can shorten the production cycle, and can simplify the process, making it particularly suitable for the development of new products.
[0005] Theoretically, the types of molding materials that can be used in SLS technology are wide, such as polymers, paraffin, metals, ceramics, and their composites. However, the performance and properties of the molding material are important factors in the success of sintering in SLS technology, and directly affect the molding speed, accuracy, physical and chemical performance, and overall performance of the molded part. At present, there are few polymer powder raw materials on the market that can be directly applied to SLS technology and successfully produce molded products with small dimensional error, clean surface, and low porosity. Therefore, there is an urgent need to develop and improve the types of polymers suitable for SLS technology and the corresponding solid powder raw materials.
[0006] In the prior art, powder raw materials suitable for SLS are usually produced by grinding methods, such as cryogenic grinding. For example, CN104031319A discloses polypropylene powder obtained by cryogenic grinding. However, this method not only requires specific equipment, but also the surface of the produced powder raw material particles is rough, the particle size is not uniform, and the shape is irregular, which is unfavorable to the formation of sintered compacts and affects the performance of the compacts.
[0007] In addition, polymer powder raw materials, such as polyamide powder, can also be produced by precipitation. In this method, polyamide is usually dissolved in a suitable solvent, the material is uniformly distributed in the solvent by stirring, and then cooled to precipitate the powder. For example, CN103374223A discloses a precipitated polymer powder based on AABB type polyamide obtained by reprecipitating polyamide obtained by polycondensation of diamine and dicarboxylic acid. In the method described in the patent, an alcohol-based solvent is used in the reprecipitation process. However, such a method requires the use of a large amount of organic solvent, and the yield and efficiency are both low, and there is no environmental protection or economic advantage.
[0008] When the polymer is polypropylene, due to the manufacturing characteristics of polypropylene, it is not possible to use common methods for producing polymer microparticles, such as emulsion polymerization, soap-free emulsion polymerization, microemulsion polymerization, miniemulsion polymerization, suspension polymerization, dispersion polymerization, precipitation polymerization, seed polymerization, etc., under low-temperature conditions, by utilizing the low-temperature brittleness of the material, it can only be pulverized into micron-order powder under low-temperature conditions, but the pulverization of polyolefins often requires the adoption of a relatively expensive liquid nitrogen deep-freezing treatment method for pulverization, and the morphology of the powder obtained by pulverization is poor, irregular, and has poor fluidity, which is the most undesirable. When sintering with SLS technology, the polymer microparticles need to be laid one layer at a time and then sintered one layer at a time, but when such irregularly shaped and poorly fluidized microparticles are used, it is very difficult to lay the powder, and printing cannot be performed. The more uniform the crystal composition of the polymer, the higher the melt flow rate index of the polymer, which is favorable for uniform melting during printing and favorable for the structural stability of the printing member. Therefore, polypropylene microspheres with good fluidity and good shape are required to meet actual needs.
[0009] Polypropylene foam material has the advantages of low density, high specific strength, good thermal stability, excellent impact resistance, environmentally friendly production raw materials and processes, and easy recovery and recycling, and can be used as functional materials for cushioning, vibration control, sound insulation, heat insulation, etc. Currently, common polypropylene foam materials are mainly divided into four types according to the processing process: autoclave foaming, press foaming, extrusion foaming, and injection foaming. In addition to the advantages common to polypropylene foam materials, autoclave expanded polypropylene (EPP) beads and moldings have the most prominent advantage in free moldability, and by molding EPP beads, foam products with complex geometric shapes and high three-dimensional dimensional accuracy can be obtained. Polypropylene foamed bead molded products have good rigidity, better impact resistance than polystyrene, and are difficult to recover compared to polystyrene foam. Polypropylene foam is an environmentally friendly material, has a high heat distortion temperature, can be used in several high-temperature fields, has good energy absorption properties and excellent pressure energy absorption performance, has good dimensional shape recovery stability, the product can withstand multiple continuous collisions and deflections without permanent deformation, the density of the foamed product is low, easy to recover and reuse, the product is non-toxic, and does not produce toxic substances when burned. Due to these excellent properties, its application is very wide, and its application in packaging, automobiles, construction and other fields is expanding. It is especially suitable for high-end fields such as automobile interior and exterior, cold chain logistics and electronic product packaging.
[0010] For EPP beads, the in-mold secondary moldability is very important. For this reason, it is necessary to select polypropylene microparticles with a regular shape (preferably roughly spherical) and small particle size as the foaming raw material. Foamed beads produced with relatively regular spherical microparticles are also roughly spherical, and are easily piled up tightly during molding, and large voids are not easily formed. Similarly, the production of polypropylene foamed particles requires crushing by a relatively expensive deep-freezing treatment method using liquid nitrogen, which results in poor powder shape, irregular shape, poor fluidity, and easy bridges during particle transportation, making production unstable. In addition, such crushed particles are not uniformly foamed, have a relatively rough surface, and whitening occurs. At the same expansion ratio, the smaller the PP microparticles, the smaller the beads after foaming, which is favorable for transportation in the process pipe of the EPP bead molding device, reduces the blockage phenomenon, and can be densely piled up in the cavity. This results in a better binding effect between the beads during molding, a lower amount of steam is used, and the mechanical properties and heat retention properties of the product are better. Furthermore, small particle sizes are advantageous in producing products with thin walls and complex structures, and the surfaces of the products are smoother and flatter.
[0011] Conventional strand cutting and underwater cutting usually have difficulty in producing particles with a particle size of 0.5 mm or less, and the aspect ratio is high. In order to obtain fine particles with an average particle size of 0.5 mm or less, it is often necessary to crush them using a relatively expensive liquid nitrogen deep-freezing method, which results in poor powder morphology, irregular shapes, poor fluidity, and easy bridges during particle transportation, making production unstable. In addition, such crushed particles often have non-uniform foaming, a relatively rough surface, and whitening.
[0012] The crystal distribution of polypropylene produced using ZN catalysts usually has a large dispersity, which is reflected in the wide half-value width in DSC measurement results. The crystal distribution of polypropylene produced using metallocene catalysts is relatively uniform, but the latter has a narrow molecular weight distribution, which often results in poor processing performance of the product. The former has a wide molecular weight distribution, which is advantageous for improving the rigidity-toughness balance of the resin.
[0013] Therefore, developing a method for producing polypropylene microspheres that have good flowability, good morphology, and can be used in 3D printing and foaming materials is of great practical significance.
[0014] Summary of the Invention In order to solve the technical problem that the distribution uniformity of the crystal arrangement of polypropylene microspheres in the prior art is poor, and the melt uniformity of the product is poor when used in 3D printing, the present invention provides polypropylene microspheres and a method for producing the same.
[0015] According to a first aspect of the present invention, there is provided polypropylene microspheres comprising 0.2 wt % to 10 wt % of constituent units derived from ethylene and 90 wt % to 99.8 wt % of constituent units derived from propylene, the melting endothermic curve of which is measured by a differential scanning calorimeter (DSC) and has a half-width (Wm) of 4 to 10°C.
[0016] Optionally, the polypropylene microspheres have a half-width of melting endothermic curve of 5-8°C.
[0017] Optionally, the polypropylene microspheres have a molecular weight distribution (Mw / Mn) of 4-9.
[0018] Optionally, the polypropylene microspheres have a molecular weight distribution of 5, 6, 7, 8, or any value between any two of the above points.
[0019] Optionally, the polypropylene microspheres have a bulk density of 0.20 g / cm3 ~0.50g / cm 3 and preferably 0.32 g / cm 3 ~0.48g / cm 3 It is.
[0020] Optionally, the angle of repose of the polypropylene microspheres is between 10° and 23°, preferably between 13° and 20°.
[0021] Optionally, the isotacticity index of the polypropylene microspheres is between 60% and 94%, preferably between 64% and 90%.
[0022] Optionally, the ash content of the polypropylene microspheres is 0.005% to 0.04%.
[0023] Optionally, the ash content of the polypropylene microspheres is 0.01%, 0.015%, 0.02%, 0.025%, 0.03%, 0.035%, or any value between any two of the above points.
[0024] Optionally, the melt index of the polypropylene microspheres is 3-160 g / 10 min, preferably 15-100 g / 10 min.
[0025] Optionally, if DSC measurements are performed, the DSC results are expressed as λi = (dH / dt) i+1 -(dH / dt) i ,
[0026] [ka]
[0027] (i is T m <T i <T fm where the ordinate is the heat flow dH / dt and the abscissa is the temperature T.
[0028] In the melting endothermic curve obtained by DSC measurement, the endothermic effect is represented by a convex peak value (an increase in enthalpy).
[0029] DSC was performed using a Perkin-Elmer DSC-7 differential scanning calorimeter. The sample was heated to 200°C at 10°C / min, held for 5 min, then cooled to 50°C at 10°C / min, held at 50°C for 1 min, and then heated to 200°C at 10°C / min. The DSC diagram is shown in Figure 2. The ordinate of the DSC result is heat flow dH / dt, the abscissa is temperature (T), the endothermic effect is represented by the peak value of the convex curve (enthalpy increases), and the heating curve is the result of the second heating curve (usually, the second heating curve is used in both cases to eliminate the thermal history of the test sample). As generally shown, T m represents the melting point of the measured sample, and T fm represents the temperature at which the melting peak joins the baseline.
[0030] The polymer microspheres having a narrower half-width obtained by the present invention can significantly improve the expansion ratio and uniformity of EPP beads during autoclave expansion and molding, and can be molded at a lower temperature, reducing the energy consumption during EPP bead molding and accelerating the production cycle of EPP bead molding, thereby effectively reducing the production costs of EPP beads and molded products. In addition, the EPP bead molded products made from the beads have better appearance quality, which is particularly advantageous for manufacturing EPP molded products with thin walls or complex shapes.
[0031] Optionally, the polypropylene microspheres have an average particle size of 50 μm to 200 μm, preferably, the polypropylene microspheres have an average particle size of 60 μm to 160 μm, and most preferably, the polypropylene microspheres have an average particle size of 80 μm to 120 μm.
[0032] Optionally, the aspect ratio of said polypropylene microspheres is 0.9-1.1, preferably, the aspect ratio of said polypropylene microspheres is 0.95-1.05, and most preferably, the aspect ratio of said polypropylene microspheres is 1.
[0033] In a specific embodiment of the present invention, the polypropylene microspheres are prepared by direct copolymerization.
[0034] According to a second aspect of the present invention, there is provided a process for producing polypropylene microspheres comprising copolymerizing a propylene containing olefin in the presence of an olefin polymerization catalyst system to obtain polypropylene microspheres.
[0035] Optionally, the olefin polymerization catalyst system comprises a catalyst component, an alkylaluminum compound component and optionally an external electron donor compound component, with or without added, or a reaction product of those components.
[0036] The alkylaluminum compound may be any of the various alkylaluminum compounds that can be used as cocatalysts for Ziegler-Natta type catalysts commonly used in the field of olefin polymerization.
[0037] Optionally, the alkylaluminum compound may be at least one of, but is not limited to, trimethylaluminum, triethylaluminum, triisobutylaluminum, trioctylaluminum, diethylaluminum monohydride, diisobutylaluminum monohydride, diethylaluminum monochloride, diisobutylaluminum monochloride, ethylaluminum sesquichloride, and ethylaluminum dichloride.
[0038] The external electron donor compound may be any external electron donor compound that can be used as a cocatalyst for Ziegler-Natta type catalysts commonly used in the field of olefin polymerization.
[0039] Optionally, the external electron donor compound is selected from the group consisting of trimethylmethoxysilane, trimethylethoxysilane, trimethylphenoxytriethylmethoxysilane, triethylethoxysilane, dimethyldimethoxysilane, dimethyldiethoxysilane, ethylisopropyldimethoxysilane, propylisopropyldimethoxysilane, diisopropyldimethoxysilane, diisobutyldimethoxysilane, isopropylisobutyldimethoxysilane, di-t-butyldimethoxysilane, t-butylmethyldimethoxysilane, t-butylethyl ...methyldimethoxysilane, t-butylethyldimethoxysilane, t-butylmethyldimethoxysilane, t-butylmethyldimethoxysilane, t-butylethyldimethoxysilane, t-butylmethyldimethoxysilane, t-butylmethyl t-butylpropyldimethoxysilane, t-butylisopropyldimethoxysilane, t-butylbutyldimethoxysilane, t-butylisobutyldimethoxysilane, t-butyl(s-butyl)dimethoxysilane, t-butylpentyldimethoxysilane, t-butylnonyldimethoxysilane, t-butylhexyldimethoxysilane, t-butylheptyldimethoxysilane, t-butyloctyldimethoxysilane, t-butyldecyldimethoxysilane, methylt-butyldimethoxysilane, cyclohexylmethyldimethoxysilane, cyclohexylethyldimethoxysilane cyclohexylpropyldimethoxysilane, cyclohexylisobutyldimethoxysilane, dicyclohexyldimethoxysilane, cyclohexylt-butyldimethoxysilane, cyclopentylmethyldimethoxysilane, cyclopentylethyldimethoxysilane, cyclopentylpropyldimethoxysilane, cyclopentylt-butyldimethoxysilane, dicyclopentyldimethoxysilane, cyclopentylcyclohexyldimethoxysilane, bis(2-methylcyclopentyl)dimethoxysilane, diphenyldimethoxysilane, diphenyldiethoxy Sisilane, phenyltriethoxysilane, methyltrimethoxysilane, methyltriethoxysilane, ethyltrimethoxysilane, ethyltriethoxysilane, propyltrimethoxysilane, isopropyltrimethoxysilane, butyltrimethoxysilane, butyltriethoxysilane, isobutyltrimethoxysilane, t-butyltrimethoxysilane, s-butyltrimethoxysilane, pentyltrimethoxysilane, isopentyltrimethoxysilane, cyclopentyltrimethoxysilane, cyclohexyltrimethoxysilane, diphenyldimethoxysilane,The external electron donor compound may be, but is not limited to, at least one of diphenyldiethoxysilane, phenyltrimethoxysilane, phenyltriethoxysilane, n-propyltrimethoxysilane, vinyltrimethoxysilane, tetramethoxysilane, tetraethoxysilane, tetrabutoxysilane, 2-ethylpiperidinyl-2-t-butyldimethoxysilane, (1,1,1-trifluoro-2-propyl)-2-ethylpiperidinyldimethoxysilane and (1,1,1-trifluoro-2-propyl)-methyldimethoxysilane. More preferably, the external electron donor compound may be at least one of dicyclopentyldimethoxysilane, diisopropyldimethoxysilane, diisobutyldimethoxysilane, cyclohexylmethyldimethoxysilane, methylt-butyldimethoxysilane and tetramethoxysilane.
[0040] Optionally, the catalyst comprises a magnesium-containing compound support, a titanium compound, and an internal electron donor compound.
[0041] Alternatively, the molar ratio of the titanium compound, the magnesium-containing compound carrier, and the internal electron donor compound is (37-255):(2-15):1, preferably (67-235):(4-12):1.
[0042] Optionally, the structure of the magnesium-containing compound support is represented by formula (I):
[0043] [ka]
[0044] In formula (I), R1 is C1-C 10 is an alkyl group of the formula R2 and R3 are the same or different and each independently represents H, C1-C 10 or C1-C substituted with 1 to 10 halogen atoms. 10 is a halogenated alkyl group of the formula: R4 is a C1-C substituted with at least one halogen atom.10 is an alkyl halide group or a C6-C aryl halide group substituted with at least one halogen atom, 20 and R5 is a C1-C5 alkyl group, X is fluorine, chlorine, bromine or iodine, preferably, X is chlorine or bromine, m is 0.1 to 1.9, n is 0.1 to 1.9, and m + n = 2, preferably, m is 0.8 to 1.2 and n is 0.8 to 1.2, 0 < q < 0.2, 0 < a < 0.1, preferably, 0.005 ≤ q ≤ 0.2 and 0.001 < a < 0.05.
[0045] Optionally, the internal electron donor compound is at least one selected from carboxylic acid esters, alcohol esters, ethers, ketones, nitriles, amines and silanes, preferably, at least one selected from monovalent or polyvalent aliphatic carboxylic acid esters, monovalent or polyvalent aromatic carboxylic acid esters, divalent alcohol esters and divalent ethers.
[0046] Optionally, the divalent alcohol ester may be a glycol carboxylic acid ester.
[0047] Optionally, the internal electron donor compound is at least one of divalent ethers, and the structure of the divalent ether is represented by formula (III),
[0048]
Chemical formula
[0049] However, R 21 and R 22 are each independently hydrogen, a C1-C 20 alkyl group, a C3-C 20 cycloalkyl group, a C6-C 20 aryl group, a C7-C 20 aralkyl group or a C7-C 20R 21 and R 22 and may be optionally bonded to form a ring; 23 and R 24 are each independently, C1-C 10 is an alkyl group.
[0050] Specifically, the internal electron donor compound is 2-(2-ethylhexyl)-1,3-dimethoxypropane, 2-isopropyl-1,3-dimethoxypropane, 2-butyl-1,3-dimethoxypropane, 2-s-butyl-1,3-dimethoxypropane, 2-cyclohexyl-1,3-dimethoxypropane, 2-phenyl-1,3-dimethoxypropane, 2-(2-phenylethyl)-1,3-dimethoxypropane, 2-(2-cyclohexylethyl)-1,3-dimethoxypropane, 2-(p-chlorophenyl)-1,3-dimethoxypropane, 2-(diphenyl)-1,3-dimethoxypropane, 2,2-dicyclohexyl-1,3-dimethoxypropane, 2,2-dicyclopentyl-1,3-dimethoxypropane, 2,2-diethyl-1,3-dimethoxypropane, 2,2-dipropyl-1,3-dimethoxypropane, 2,2-diisopropyl-1,3-dimethoxypropane, 2,2-dibutyl-1,3-dimethoxypropane, 2-methyl-2-propyl-1,3-dimethoxypropane, 2-methyl-2-benzyl-1,3-dimethoxypropane, 2-methyl-2-ethyl-1,3-dimethoxypropane 2-methyl-2-isopropyl-1,3-dimethoxypropane, 2-methyl-2-phenyl-1,3-dimethoxypropane, 2-methyl-2-cyclohexyl-1,3-dimethoxypropane, 2,2-bis(2-cyclohexylethyl)-1,3-dimethoxypropane, 2-methyl-2-isobutyl-1,3-dimethoxypropane, 2-methyl-2-(2-ethylhexyl)-1,3-dimethoxypropane, 2,2-diisobutyl-1,3-dimethoxypropane, 2,2-diphenyl-1,3-dimethoxypropane, 2,2-dibenzyl-1,3-dimethoxypropane 2-isopropyl-2-isopropyl-1,3-dimethoxypropane, 2-phenyl-2-isopropyl-1,3-dimethoxypropane, 2-phenyl-2-s-butyl-1,3-dimethoxypropane, 2-benzyl-2-isopropyl-1,3-dimethoxypropane, 2-cyclopentyl-2-isopropyl-1,3-dimethoxypropane, 2-isopropyl-2-isopentyl-1,3-dimethoxypropane, 2-phenyl-2-isopropyl-1,3-dimethoxypropane, 2-phenyl-2-s-butyl-1,3-dimethoxypropane, 2-benzyl-2-isopropyl-1,3-dimethoxypropane, 2-cyclopentyl-2-isopropyl-1,At least one selected from 3-dimethoxypropane, 2-cyclopentyl-2-s-butyl-1,3-dimethoxypropane, 2-cyclohexyl-2-isopropyl-1,3-dimethoxypropane, 2-cyclohexyl-2-s-butyl-1,3-dimethoxypropane, 2-isopropyl-2-s-butyl-1,3-dimethoxypropane, 2-cyclohexyl-2-cyclohexylmethyl-1,3-dimethoxypropane, and 9,9-dimethoxymethylfluorene may be used.
[0051] Optionally, the titanium compound has the general formula Ti(OR6) 4-b X' b where R6 is C1-C 14 wherein X′ is F, Cl or Br, and b is an integer of 1 to 4.
[0052] The titanium compound is preferably at least one of titanium tetrachloride, titanium tetrabromide, titanium tetrafluoride, tributoxytitanium chloride, dibutoxytitanium dichloride, butoxytitanium chloride, triethoxytitanium chloride, diethoxytitanium dichloride, and ethoxytitanium chloride.
[0053] Optionally, the method for producing the magnesium-containing compound support includes: Step S1: a first contact and emulsification of a magnesium halide having a general formula of MgX″Y with a first alcohol-based compound having a general formula of R7OH to obtain a first product; Step S2 of contacting the first product with an ethylene oxide compound having a structure represented by formula (II) in a second step to obtain a second product; The general formula is R 10 OH, halogenated alcohols with the general formula R 11 a step S3 of carrying out a third contact of a second alcohol-based compound, which is OH, with the second product to obtain a third product; and step S4 of spray drying the third product to obtain a magnesium-containing compound support.
[0054] Optionally, as a specific embodiment of the present invention, in the S1, in the general formula MgX″Y, X″ is selected from fluorine, chlorine, bromine or iodine, and Y is fluorine, chlorine, bromine, iodine, C 1-6 Alkyl groups of C 1-6 Alkoxy groups, C 6-14 or an aryl group of C 6-14 The aryloxy group is selected from the group consisting of the following:
[0055] Preferably, X″ is selected from chlorine or bromine, and Y is chlorine, bromine, C 1-5 Alkyl groups of C 1-5 Alkoxy groups, C 6-10 or an aryl group of C 6-10 The aryloxy group Y is selected from the group consisting of C 1-6 Alkyl groups of C 1-6 When the alkyl group and the alkoxy group are selected from the alkoxy groups of C, the alkyl group and the alkoxy group are linear or branched alkyl group and alkoxy group, and the C 1-6 The alkyl group in the above formula refers to an alkyl group having 1 to 6 carbon atoms, and examples thereof include, but are not limited to, a methyl group, an ethyl group, an n-propyl group, an isopropyl group, an n-butyl group, an isobutyl group, a t-butyl group, an n-pentyl group, an isopentyl group, and the like. 1-6 The alkoxy group refers to an alkoxy group having 1 to 6 carbon atoms, and examples thereof include, but are not limited to, a methoxy group, an ethoxy group, an n-propoxy group, an isopropoxy group, an n-butoxy group, an s-butoxy group, an isobutoxy group, a t-butoxy group, an n-pentyloxy group, and an isopentyloxy group.
[0056] Said C 6-14 The aryl group refers to an aryl group having 6 to 14 carbon atoms, and examples thereof include, but are not limited to, a phenyl group, an o-tolyl group, a m-tolyl group, a p-tolyl group, an o-ethylphenyl group, a m-ethylphenyl group, a p-ethylphenyl group, and a naphthyl group.
[0057] Said C 6-14The aryloxy group refers to an aryloxy group having 6 to 14 carbon atoms, and examples thereof include, but are not limited to, a phenoxy group, a naphthyloxy group, an o-methylphenoxy group, an o-ethylphenoxy group, and an m-methylphenoxy group.
[0058] Optionally, the magnesium halide is at least one selected from magnesium chloride, magnesium bromide, phenoxymagnesium chloride, isopropoxymagnesium chloride and n-butoxymagnesium chloride, preferably magnesium chloride.
[0059] Optionally, in the formula R7OH, R7 is C 1-10 is an alkyl group.
[0060] Optionally, in S2, the structural formula of the ethylene oxide compound is represented by formula (II):
[0061] [ka]
[0062] R8 and R9 are each independently H, C 1-10 C alkyl group substituted with 1 to 10 halogen atoms 1-10 Preferably, R and R are each independently selected from H, C 1-5 C alkyl group substituted with 1 to 10 halogen atoms 1-5 The halogenated alkyl groups are selected from the group consisting of:
[0063] Optionally, the ethylene oxide-based compound is at least one selected from ethylene oxide, propylene oxide, butylene oxide, epoxy chloropropane, epoxy chlorobutane, epoxy bromopropane, and epoxy bromobutane.
[0064] Optionally, in S3, the formula R 10 In OH, R10 is C substituted with at least one halogen atom 1-10 or C substituted with at least one halogen atom 6-20 The halogenated aryl group is selected from the group consisting of:
[0065] The halogenated alcohol may be a monohalogenated alcohol or a polyhalogenated alcohol, and is preferably a chlorinated, brominated or iodized alcohol, such as 2,2,2-trichloroethanol, 2,2-dichloroethanol, 2-chloroethanol, 3-chloro-1-propanol, 6-chloro-1-hexanol, 3-bromo-1-propanol, 5-chloro-1-pentanol, 4-chloro-1-butanol, 2-chlorocyclohexanol, 1,2-dichloroethanol, 1,3-dichloropropanol, 1,4-dichlorobutanol or 2-iodoethanol.
[0066] However, in order to obtain a catalyst support with better performance, according to yet another preferred specific embodiment of the present invention, 10 In OH, R 10 is a C substituted with at least two halogen atoms 1-10 or a halogenated alkyl group substituted with at least two halogen atoms 6-20 and the halogen atom is at least one selected from a chlorine atom, a bromine atom and an iodine atom.
[0067] Preferably, the halogenated alcohol is at least one selected from 2,2,2-trichloroethanol, 2,2-dichloroethanol, 1,2-dichloroethanol, 1,3-dichloropropanol, and 1,4-dichlorobutanol.
[0068] Optionally, said formula R 11 In OH, R 11 is C 1-5 is an alkyl group.
[0069] In the present invention, the second alcohol compound is ethanol, methanol, n-propanol, isopropanol, n-butanol or isobutanol. However, in order to obtain a catalyst support with better performance, according to yet another preferred embodiment of the present invention, the second alcohol compound is represented by the formula R 11 In OH, R 11 is C 1-2 That is, the second alcohol compound is methanol and / or ethanol.
[0070] Alternatively, the amount of the halogenated alcohol used is 0.05 to 6.5 mol, and the amount of the second alcohol compound used is 5 to 100 mol, relative to 1 mol of the magnesium halide.
[0071] If the amount of the halogenated alcohol compound used is too large, the resulting catalyst support becomes sticky and blocks, making subsequent operations impossible.
[0072] Alternatively, the amount of the first alcohol compound used is 1 to 30 mol, and the amount of the ethylene oxide compound used is 1 to 10 mol, relative to 1 mol of the magnesium halide.
[0073] Preferably, the amount of the first alcohol-based compound used is 6 to 22 mol, the amount of the ethylene oxide-based compound used is 2 to 6 mol, the amount of the halogenated alcohol used is 1 to 5 mol, and the amount of the second alcohol-based compound used is 8 to 80 mol, more preferably 31 to 50 mol, relative to 1 mol of the magnesium halide.
[0074] In addition, since the trace amount of water contained in each of the above reactants is also involved in the reaction to form the spherical carriers, the produced spherical carriers may contain trace amounts of water derived from the reaction raw materials and reaction medium, and those skilled in the art should not understand this as limiting the present invention.
[0075] Optionally, in S1, the first contact is performed under stirring conditions, and the first contact conditions include a temperature of 80 to 120°C and a time of 0.5 to 5 hours, and preferably, in S1, the first contact conditions include a temperature of 80 to 100°C and a time of 0.5 to 3 hours.
[0076] In S1, the present invention is not particularly limited to the specific operation method of the emulsification, and can be performed by a method known to those skilled in the art. The emulsification is performed, for example, by low-speed shear or high-speed shear. When low-speed shear is adopted, the stirring speed of the low-speed shear is preferably 400 to 800 rpm. The high-speed shear method is known to those skilled in the art, and is performed, for example, at a high-speed stirring speed disclosed in CN1330086A. The emulsification operation can also be performed with reference to the method disclosed in the following patent application, and as disclosed in CN1580136A, a solution containing a liquid magnesium halide compound is rotated and dispersed (rotation speed is 100 to 3000 rpm) on a supergravity bed. Furthermore, as disclosed in CN1463990A, a solution containing a liquid magnesium halide adduct is outputted at a speed of 1500 to 8000 rpm by an emulsifier. Furthermore, as disclosed in US6020279A, a solution containing a liquid magnesium halide adduct is emulsified by a spray method.
[0077] Optionally, in S2, the second contact conditions include a temperature of 50 to 120°C and a time of 20 to 60 minutes, and preferably, the second contact conditions include a temperature of 80 to 100°C and a time of 20 to 50 minutes.
[0078] Optionally, in S3, after washing the second product with an inert solvent, a compound having the general formula R 10 OH, halogenated alcohols with the general formula R 11 and performing the third contact with a second alcoholic compound where the second alcoholic compound is OH, and preferably the inert solvent is at least one selected from pentane, hexane, heptane, petroleum ether, and gasoline.
[0079] In the present invention, the specific conditions of the third contact in S3 are not particularly limited, and the general formula is R 10 OH, halogenated alcohols with the general formula R 11 It is sufficient that the second alcohol compound, which is OH, and the second product are sufficiently contacted to form a fluid. However, in order to obtain a catalyst carrier with better performance, preferably, in S3, the third contacting conditions include being performed under stirring conditions, the temperature being 0 to 120°C, and the time being 0.5 to 6 hours.
[0080] The present invention is not particularly limited with respect to the specific manner of the third contact in S3. The halogenated alcohol and the second alcohol-based compound may be mixed and contacted with the second component simultaneously, or the halogenated alcohol and the second alcohol-based compound may be contacted with the second component in sequence.
[0081] As a specific embodiment of the present invention, in S4, the conditions of the spray drying can be the conditions that can form a conventional catalyst carrier for olefin polymerization, but in order to obtain a catalyst carrier with better performance, according to a preferred specific embodiment of the present invention, the spray drying is carried out in a sprayer having a spray nozzle, the spray nozzle includes a material conduit and a nozzle head, and the third product is introduced into the nozzle head through the material conduit and sprayed into a tower body containing an inert medium of the sprayer through the nozzle head to harden. Preferably, the temperature of the third product in the material conduit is 0°C to 80°C, the temperature of the third product in the nozzle head is 80 to 180°C, and more preferably, the temperature of the third product in the nozzle head is 120 to 180°C.
[0082] Optionally, in S4, the spray drying conditions include a temperature of 60 to 200° C., more preferably 90 to 150° C. In the present invention, the spray drying temperature refers to the temperature of the inert medium in the sprayer.
[0083] In a specific embodiment of the present invention, the inert medium may include a protective gas medium and / or an inert liquid medium, the type of the protective gas medium is not particularly limited, and may be, for example, nitrogen gas, an inert gas medium, for example, helium gas, or other suitable gas, for example, carbon dioxide, etc., and the inert liquid medium is a variety of liquid media that do not produce chemical reactions with the reactants and reaction products commonly used in this field, preferably, the inert liquid medium is silicone oil and / or an inert liquid hydrocarbon solvent, more preferably, the inert liquid medium is at least one selected from kerosene, paraffin oil, Vaseline oil, white oil, methyl silicone oil, ethyl silicone oil, methyl ethyl silicone oil, phenyl silicone oil and methyl phenyl silicone oil, more preferably, white oil.
[0084] As a specific embodiment of the present invention, the amount of the inert liquid medium used in the sprayer can be selected according to the amount of magnesium halide having a general formula of MgX″Y used, and is preferably 0.8-10 L, more preferably 2-8 L.
[0085] As a specific embodiment of the present invention, the manufacturing method described in the present invention further includes post-treatment means such as solid-liquid separation, washing, drying, etc., which are common in this field, and the present invention is not particularly limited thereto. The solid-liquid separation can employ various methods capable of realizing conventional separation of solid and liquid phases, such as suction filtration, pressure filtration, or centrifugation, and preferably, the method of solid-liquid separation is pressure filtration. In the present invention, the conditions of pressure filtration are not particularly limited, and the basis is to realize separation of solid and liquid phases as fully as possible. The washing can be performed by washing the obtained solid phase product by a method known to those skilled in the art, for example, the obtained solid phase product can be washed with an inert hydrocarbon solvent (e.g., pentane, hexane, heptane, petroleum ether, and gasoline). In the present invention, the specific conditions of the drying are not particularly limited, and for example, the drying temperature can be 20 to 70°C, the drying time can be 0.5 to 10 h, and the drying can be performed under normal pressure or reduced pressure conditions.
[0086] In a specific embodiment of the present invention, the composition of the catalyst is not particularly limited and may be the composition of a conventional catalyst for olefin polymerization in this field, but it is preferred that the catalyst comprises the support, a titanium halide compound and an electron donor compound, so as to obtain a catalyst suitable for olefin polymerization, particularly propylene polymerization. Preferably, the titanium halide compound is at least one selected from titanium tetrachloride, titanium tetrabromide, titanium tetraiodide, tetra n-butoxy titanium, tetraethoxy titanium, monochlorotri n-butoxy titanium, dichlorodi n-butoxy titanium, trichloromono n-butoxy titanium, monochlorotriethoxy titanium, dichlorodiethoxy titanium, trichloromonoethoxy titanium and titanium trichloride. Preferably, the electron donor compound is at least one selected from diisobutyl phthalate, carboxylic acid diol ester and phosphoric acid ester. In addition, the present invention is not particularly limited to the content of each component in the catalyst, and those skilled in the art can appropriately adjust and design according to actual needs.
[0087] Alternatively, the magnesium-containing compound carrier has an average particle size of 2-100 microns and a particle size distribution of less than 2, and preferably, the magnesium-containing compound carrier has an average particle size of 2-19 microns and a particle size distribution of 0.6-1.6.
[0088] When a catalyst containing a magnesium-containing compound support is used for olefin polymerization, in order to obtain an olefin polymer having a higher bulk density, it is more preferable that the magnesium-containing compound support has an average particle size of 2 to 10 microns and a particle size distribution of 0.6 to 1.
[0089] In the method for producing polypropylene microspheres of the present invention, the catalyst has the characteristic of "morphological duplication" in the process of catalyzing the polymerization of propylene, and spherical catalysts do not necessarily produce spherical polymers; spherical polymers can generally only be produced from spherical catalysts. The smaller the particle size of the catalyst, the smaller the particle size of the resulting polymer is generally, and the structure and shape of the catalyst itself play an important role in the shape of the polymer. Good catalyst structure and shape contribute to reducing the friction between polymers, reducing the angle of repose of the final polymer, and contributing to the production and transportation of the polymer.
[0090] According to a third aspect of the present invention, there is provided a 3D printing raw material comprising the above polypropylene microspheres and / or the polypropylene microspheres produced by the above production method.
[0091] According to a fourth aspect of the present invention there is provided a use of said polypropylene microspheres or polypropylene microspheres produced by said production method for 3D printing, in particular for laser sintering printing, most preferably for Selective Laser Sintering (SLS).
[0092] Compared with the prior art, the present invention includes the following beneficial effects:
[0093] 1. The half-width of the conventional polypropylene microspheres is wide, while the half-width of the polypropylene microspheres of the present invention is only 4-10°C, which is narrower than the conventional ones. This indicates that the crystal arrangement distribution of the obtained polypropylene microspheres is relatively uniform. When used in 3D printing, it can improve the uniformity of melting and fusing of polymer particles, improve the melt uniformity of 3D printing products, and improve the structural strength and surface performance of sintered samples. At the same time, the present invention has a wider molecular weight distribution than the polypropylene microspheres produced by metallocene catalysts, and the obtained sintered products have a better rigidity-toughness balance.
[0094] 2. The average particle size of the polypropylene microspheres of the present invention is less than 160 microns, and can be used directly in 3D printing without the need for secondary processing. The repose angle of the polypropylene microspheres of the present invention is less than 23°, and has better fluidity, and the powder is laid more uniformly during printing. The ethylene content of the polypropylene microspheres of the present invention is greater than 0.2wt%, and they do not warp during 3D printing. The polypropylene microspheres of the present invention have good spherical morphology, regular particles, good fluidity, and great potential for industrial application.
[0095] 3. The method for producing polypropylene microspheres of the present invention has a large specific surface area of the catalyst and good polymerization activity. Due to the properties of the catalyst, the amount of alkylaluminum used can be reduced. A smaller amount of triethylaluminum is mixed with cyclohexylmethyldimethoxysilane, catalyst, hydrogen gas and propylene monomer and reacted to obtain polypropylene microspheres. This further reduces the ash content of the resulting polymer microspheres and essentially eliminates irregular shapes.
[0096] 4. In the preparation method of polypropylene microspheres of the present invention, the catalyst has the property of "morphological replication" to directly polymerize and obtain spherical polymers. Due to the good structural and morphological properties of the catalyst, the friction between the resulting polymers is small and the angle of repose of the polymer is small, which is advantageous for the production and transportation of the polymer.
[0097] 5. The polypropylene microspheres provided by the present invention are directly polymerized in the reactor, which avoids the post-processing process and saves costs.
[0098] BRIEF DESCRIPTION OF THE DRAWINGS [Figure 1] Figure 1 is an electron microscope photograph of the polypropylene powder obtained in Example 1.
[0099] [Figure 2] Figure 2 is a schematic diagram of a DSC.
[0100] [Mode for carrying out the invention] The present invention will be further described below with reference to specific examples, but the present invention is not limited thereto.
[0101] In the present invention, the average particle size and particle size distribution of the magnesium-containing compound carrier are measured using a Masters Sizer 2000 particle sizer (manufactured by Malvern Instruments Ltd).
[0102] In the present invention, the external appearance of the polypropylene powder is observed using an XL-30 type field emission electron microscope manufactured by FEI Corporation, USA.
[0103] In the present invention, the structure and composition of the magnesium-containing compound carrier are obtained by performing 1H-NMR measurement on the carrier using an AVANCE 300 nuclear magnetic resonance spectrometer manufactured by Bruker, Switzerland, and performing measurements on the carrier using a PY-2020iD cracker manufactured by Fronteerlab, a TraceGC Ultra chromatograph manufactured by Thermo Fisher, and a DSD II mass spectrometer.
[0104] In the present invention, the DSC measurement is performed according to the method specified in "GBT 19466 Plastics Differential Scanning Calorimetry (DSC)." Here, the half-width in DSC measurement is the absolute value of the temperature difference between two points where a line parallel to the baseline passing through the midpoint of the peak height intersects with both sides of the peak.
[0105] In the present invention, the molecular weight distribution index Mw / Mn of the polypropylene powder is measured by the method specified in GB / T36214-2018.
[0106] In the present invention, the catalytic copolymerization activity is evaluated by the ratio of the weight of the product obtained after polymerization to the weight of the amount of the catalyst used.
[0107] In the present invention, the bulk density of the polypropylene powder is measured by the method specified in GB / T 1636-2008.
[0108] In the present invention, the ash content of the polypropylene powder is measured by the method specified in GB_T 9345.1-2008.
[0109] In the present invention, the specific surface area of the polypropylene powder is measured using a POREMASTER GT60 type mercury porosimeter.
[0110] In the present invention, the angle of repose of the polypropylene powder is measured by the method specified in GB / T 11986-1989.
[0111] In the present invention, the aspect ratio of the polypropylene powder refers to the ratio of the major axis of the particle projection to its average minor axis.
[0112] In the present invention, the ethylene content of the polypropylene powder is measured using a Fourier transform infrared spectrophotometer, and a sample is prepared by a film hot press method.
[0113] In the present invention, the tensile strength of the sample is measured by the method specified in GB / T 1040.2-2006.
[0114] In the present invention, the surface smoothness is measured by a comparative method, which involves comparing the surface to be measured with a standard product, and evaluating the roughness of the surface to be measured by visual, tactile or other methods. Five workers score the surface roughness, with the standard product being given 10 points, and the average score being taken.
[0115] [Table 1]
[0116] In the present invention, unless otherwise specified, all raw materials used are commercially available products.
[0117] 1,3-Dichloropropanol was purchased from J&K Scientific.
[0118] Epoxychloropropane was purchased from J&K Scientific.
[0119] Diisobutyl phthalate was purchased from J&K Scientific.
[0120] Titanium tetrachloride was purchased from J&K Scientific.
[0121] Triethylaluminum was purchased from J&K Scientific.
[0122] Cyclohexylmethyldimethoxysilane was purchased from J&K Scientific.
[0123] In each of the examples and comparative examples of the present invention, unless otherwise specified, emulsification was carried out under stirring at 600 rpm in the process of producing the catalyst carrier.
[0124] DSC was performed using a Perkin-Elmer DSC-7 type differential scanning calorimeter. The sample was heated to 200°C at 10°C / min, held for 5 min, then cooled to 50°C at 10°C / min, held at 50°C for 1 min, and then heated again to 200°C at 10°C / min. The results of the second heating test were calculated using the formula λi=(dH / dt) i+1 -(dH / dt) i Using
[0125] [ka]
[0126] (i is T m <T i <T fm If the result is less than 0,
[0127] [ka]
[0128] is No, and conversely, if none of the calculated values are less than 0,
[0129] [ka]
[0130] The answer is Yes. λi is T i+1 Temperature and T i It is the difference in heat flow at different temperatures.
[0131] <Example 1-1> 1) Production of magnesium-containing compound carriers S1: 0.08 mol of magnesium chloride and 1.7 mol of ethanol (first alcohol compound) were sequentially added to a 0.6 L reaction vessel, and the mixture was heated to 90°C with stirring. The mixture was reacted at a constant temperature for 1 hour to carry out a first contact, and then emulsified to obtain a first product.
[0132] S2: The first product is subjected to a second contact with 0.48 mol of epoxychloropropane to obtain a second product, and the second contact conditions include a temperature of 90° C. and a time of 30 min.
[0133] S3: The second product was pressure filtered, and then thoroughly mixed and stirred with 2.5 mol of ethanol (a second alcoholic compound) and 0.35 mol of 1,3-dichloropropanol (a halogenated alcohol) to form a third contact, thereby obtaining a third product.
[0134] S4: Using the sprayer B-290 including a nozzle head and a material pipe, the third product is sprayed into the circulating nitrogen gas at 100°C in the sprayer tower and spray-dried, the temperature of the third product in the material pipe is 15°C, and the temperature of the third product in the nozzle head is 120°C, and the catalyst spherical carrier Z1 is obtained.
[0135] Measurements revealed that the average particle size (D50) of the spherical catalyst carrier Z1 was 4 microns, and the particle size distribution ((D90-D10) / D50) was 0.9.
[0136] It was found that the particle morphology of the catalyst spherical carrier Z1 was relatively regular, the surface was smooth, the shape was almost spherical, the particle size distribution was relatively concentrated, and there were almost no irregular-shaped particles.
[0137] During the preparation of the catalyst spherical carrier Z1, no clogging occurred in the nozzle head of the sprayer, and a total of 11.8 g of catalyst spherical carrier Z1 was obtained.
[0138] 2) Production of olefin polymerization catalysts S1: 100 mL of titanium tetrachloride was added to a 300 mL reaction flask and cooled to minus 20° C., and 8 grams of the catalyst spherical carrier Z1 obtained in Example 1 was added, and the mixture was stirred at minus 20° C. for 30 minutes to obtain a first product.
[0139] S2: The first product obtained in S1 was gradually heated to 110°C. During the heating process, 1.5 mL of 2-isopropyl-2-isopentyl-1,3-dimethoxypropane was added, and the mixture was maintained at 110°C for 30 minutes. The liquid was then filtered to obtain the second product.
[0140] S3: The second product obtained in S2 was washed twice with titanium tetrachloride and three times with hexane, and then dried to obtain the olefin polymerization catalyst C1.
[0141] 3) Preparation of polypropylene copolymer microspheres In a 5L stainless steel autoclave, under a nitrogen gas protective atmosphere, 0.25mmol of triethylaluminum in hexane solution (concentration of triethylaluminum is 0.5mmol / mL), 10mL of anhydrous hexane, 10mg of catalyst C1, 1.5L (standard volume) of hydrogen gas and 2L of liquid propylene monomer were added, ethylene was introduced, the temperature was raised to 70℃, and the reaction was carried out at this temperature for 40min, after which the temperature was lowered, the pressure was released, the mixture was discharged and dried to obtain copolymerized polypropylene powder.
[0142] The copolymerized polypropylene powder obtained in Example 1-1 exhibited a good spherical morphology when viewed under an electron microscope (FIG. 1), with almost no irregularities present.
[0143] <Example 1-2> In this example, polypropylene was produced by the method provided in Example 1-1. The difference was that the volume of hydrogen gas used was different, but everything else was the same.
[0144] Specifically, 1.5 L (standard volume) of hydrogen gas was replaced with 6.5 L (standard volume) of hydrogen gas to obtain polypropylene powder.
[0145] The polypropylene powder exhibited good spherical morphology when viewed under an electron microscope, with very little out-of-shape material present.
[0146] <Example 2-1> (1) 0.08 mol of magnesium chloride and 1.4 mol of ethanol (first alcohol compound) were added to a 0.6 L reaction vessel, and the mixture was heated to 90°C with stirring. The mixture was reacted at a constant temperature for 1.5 hours to carry out a first contact, and then emulsified to obtain a first product.
[0147] (2) carrying out a second contact of the first product with 0.35 mol of epoxychloropropane to obtain a second product, and the second contact conditions include a temperature of 90° C. and a time of 30 min.
[0148] (3) The second product was subjected to pressure filtration, and then thoroughly mixed and stirred with 2.5 mol of ethanol (a second alcohol compound) and 0.25 mol of 1,3-dichloropropanol (a halogenated alcohol) to form a third contact to obtain a third product.
[0149] (4) Using a sprayer B-290 including a nozzle head and a material pipe, the third product was sprayed into the circulating nitrogen gas at 100°C in the sprayer tower and spray-dried, the temperature of the third product in the material pipe was 15°C, and the temperature of the third product in the nozzle head was 120°C, and the catalyst spherical carrier Z2 was obtained.
[0150] Measurements showed that the average particle size (D50) of the catalyst spherical carrier Z2 was 4 microns, and the particle size distribution ((D90-D10) / D50) was 0.8.
[0151] It was observed that the particle morphology of the spherical catalyst support Z2 for olefin polymerization was relatively regular, the surface was smooth, and the shape was almost spherical. The particle size distribution was relatively concentrated, and there were almost no irregular particles.
[0152] During the preparation of the catalyst spherical carrier Z2, no clogging occurred in the nozzle head of the sprayer, and a total of 11.9 g of the catalyst spherical carrier Z2 was obtained.
[0153] Polypropylene was produced by a method similar to that of Example 1-1. In step S1, the type of catalyst carrier used was different, but the rest was the same as that of Example 1-1.
[0154] Specifically, the same weight of the catalyst spherical carrier Z2 prepared in Example 2-1 was used in place of the catalyst spherical carrier Z1 to obtain an olefin polymerization catalyst C2.
[0155] Catalyst C2 was determined to be spherical when observed under an electron microscope. The average particle size (D50) of catalyst C2 was determined to be 4 microns, with a particle size distribution ((D90-D10) / D50) of 0.8.
[0156] The resulting polypropylene powder particles had good morphology and, when viewed under an electron microscope, showed a good spherical morphology with almost no irregularities present.
[0157] <Example 2-2> In this example, polypropylene was produced by the method provided in Example 2-1. The difference was that the volume of hydrogen gas used was different, but everything else was the same.
[0158] Specifically, 1.5 L (standard volume) of hydrogen gas was replaced with 6.5 L (standard volume) of hydrogen gas to obtain polypropylene powder.
[0159] The polypropylene powder exhibited good spherical morphology when viewed under an electron microscope, with very little out-of-shape material present.
[0160] <Example 3-1> (1) 0.08 mol of magnesium chloride and 1.4 mol of ethanol (first alcohol compound) were added to a 0.6 L reaction vessel, and the mixture was heated to 90°C with stirring. The mixture was reacted at a constant temperature for 1.5 hours to carry out a first contact, and then emulsified to obtain a first product.
[0161] (2) carrying out a second contact of the first product with 0.35 mol of epoxychloropropane to obtain a second product, and the second contact conditions include a temperature of 90° C. and a time of 30 min.
[0162] (3) The second product was pressure filtered, then mixed with 2.5 mol of ethanol (a second alcoholic compound) and 0.1 mol of 1,3-dichloropropanol (a halogenated alcohol), and stirred until a fluid was formed in a third contact to obtain a third product.
[0163] (4) Using a sprayer B-290 including a nozzle head and a material pipe, the third product was sprayed into the circulating nitrogen gas at 100°C in the sprayer tower, the temperature of the third product in the material pipe was 15°C, and the temperature of the third product in the nozzle head was 120°C, and the catalyst spherical carrier Z3 was obtained.
[0164] Measurements showed that the average particle size (D50) of the catalyst spherical carrier Z3 was 5 microns, and the particle size distribution ((D90-D10) / D50) was 0.8.
[0165] It was found that the particle morphology of the catalyst spherical carrier Z3 was relatively regular, the surface was smooth, the shape was almost spherical, the particle size distribution was relatively concentrated, and there were almost no irregular particles.
[0166] During the preparation of the catalyst spherical carrier Z3, no clogging occurred in the nozzle head of the sprayer, and a total of 12.0 g of the catalyst spherical carrier Z3 was obtained.
[0167] The catalytic polymerization was the same as in Example 2-1, except that Z3 was used instead of Z2.
[0168] The polypropylene powder exhibited good spherical morphology when viewed under an electron microscope, with very little out-of-shape material present.
[0169] <Example 3-2> In this example, polypropylene was produced by the method provided in Example 3-1. The difference was that the volume of hydrogen gas used was different, but everything else was the same.
[0170] Specifically, 1.5 L (standard volume) of hydrogen gas was replaced with 6.5 L (standard volume) of hydrogen gas to obtain polypropylene powder.
[0171] The polypropylene powder exhibited good spherical morphology when viewed under an electron microscope, with very little out-of-shape material present.
[0172] <Example 4> In this example, polypropylene was produced by the method provided by Example 1-1. The difference is that 0.25 mmol of triethylaluminum was added and 0.01 mmol of cyclohexylmethyldimethoxysilane was added, but otherwise the same procedure as in Example 1-1 was followed to obtain polypropylene powder.
[0173] The polypropylene powder exhibited good spherical morphology when viewed under an electron microscope, with very little out-of-shape material present.
[0174] <Comparative Manufacturing Example 3> (1) 0.08 mol of magnesium chloride and 1.7 mol of ethanol were added to a 0.6 L reaction vessel, and the temperature was raised to 90°C with stirring. After reacting at a constant temperature for 1 hour, 0.48 mol of epoxychloropropane was added and reacted at 90°C for 30 minutes to obtain the first product.
[0175] (2) The first product was pressure filtered, and then 2.5 mol of ethanol was added thereto and stirred until a fluid mixture was formed.
[0176] (3) The fluid mixture was sprayed into circulating nitrogen gas at 100°C using an atomizer including a nozzle head and a material conduit, and the temperature of the third product in the material conduit was 15°C and the temperature in the nozzle head was 120°C, thereby obtaining an olefin polymerization catalyst support DZ3.
[0177] The average particle size (D50) of the olefin polymerization catalyst support DZ3 was 3 microns, and the particle size distribution ((D90-D10) / D50) was 0.8.
[0178] <Comparative Example 1> Polypropylene was produced in a manner similar to that of Example 1-1. The difference was that diisobutyl phthalate was used instead of 2-isopropyl-2-isopentyl-1,3-dimethoxypropane in the preparation of the olefin polymerization catalyst, but all other steps were the same.
[0179] <Comparative Example 2> Polypropylene was produced in a manner similar to that of Comparative Example 1. In producing polypropylene copolymer microspheres, the volume of hydrogen gas used was 6.5 NL, but otherwise everything was the same as in Comparative Example 1.
[0180] <Comparative Example 3> Polypropylene was produced in a manner similar to that of Example 1-1, except that DZ3 was used instead of Z1, and everything else was the same.
[0181] <Comparative Example 4> Polypropylene was produced in a manner similar to that of Example 1-1, except that no ethylene was added during polymerization.
[0182] <Comparative Example 5> (1) The magnesium halide adduct MgXY·mR1OH was prepared according to the method disclosed in Example 1 of CN1718595, specifically as follows.
[0183] In a 150L reactor with stirring, 10 kg of anhydrous magnesium chloride and 12.6 kg of ethanol were added to 60 L of white oil with a viscosity of 30 centipoise (20°C) and reacted at 125°C for 2 hours. Next, the mixture of the obtained molten adduct and white oil was transferred to a methyl silicone oil medium preheated to 125°C, the viscosity of the methyl silicone oil was 300 centipoise (20°C), the amount of methyl silicone oil used was 120L, and the mixture was stirred at a rotation speed of 200 rpm for 10-30 minutes to obtain a mixture. The mixture was introduced into a supergravity rotating bed and dispersed, and under stirring conditions, the mixture after dispersion was introduced into a hexane medium previously cooled to -35°C, the amount of hexane used was 1200L, and the magnesium chloride / alcohol adduct melt dispersed in small droplets was cooled and solidified to become spherical solid particles. After quenching, solid particles were filtered from the suspension obtained, and the particles were washed with hexane at room temperature. The amount of hexane used was 100 L per wash, and the particles were washed five times in total. The solid was obtained by vacuuming at 60°C.
[0184] The magnesium halide adduct had an average particle size (D50) of 52 microns, and a particle size distribution ((D90-D10) / D50) of 1.1. Observation of the particle morphology with an electron microscope showed that the particle morphology of the magnesium halide adduct was relatively regular, the surface was relatively smooth, and the particle size distribution was relatively concentrated.
[0185] Gas chromatography-mass spectrometry, nuclear magnetic resonance and elemental analysis determined the structural formula of magnesium halide adduct D5 to be MgCl2·2.5C2H5OH.
[0186] The same as Example 1, except that D5 was used instead of Z1.
[0187] <Comparative Example 6> The volume of hydrogen gas used in the preparation of polypropylene copolymer microspheres was different at 6.5 NL, but everything else was the same as in Comparative Example 5.
[0188] <Comparative Example 7> Random copolymerized polypropylene pellets produced using the commercial DQC401 catalyst were cryogenically frozen in liquid nitrogen and then ground.
[0189] [Table 2]
[0190] [Table 3]
[0191] As can be seen from Table 2 above, the polypropylene microspheres of the present invention have a broader molecular weight distribution and a narrower half-width, and the crystal arrangement distribution of the obtained polypropylene microspheres is relatively uniform, and when used in 3D printing, the particles melt uniformly and the performance of the obtained product is good. In addition, the broader molecular weight distribution can also impart a better stiffness-toughness balance to the product.
[0192] <Test example 1: Laser sintering 3D printing> 5 mg of antioxidant 1010 was dissolved in 100 ml of hexane, and a certain amount of the polypropylene powder described in the above examples or comparative examples was added. After uniform mixing, the mixture was dried by suction, and a certain amount of the polypropylene powder was added in a selective laser sintering printer, and the operation temperature was 130 to 132°C, the laser power was 40 W, and the scanning speed was 1500 mm s -1 The parameters were adjusted so that the scanning interval was 0.1 mm, and after printing the sample, the mechanical performance of the sample was measured. The specific results are shown in Table 3.
[0193] [Table 4]
[0194] As described above, the copolymerized polypropylene powder produced by the catalyst provided by the present invention has good spherical morphology, good fluidity, small repose angle, good tensile performance of 3D printing parts, and good smoothness of the article. The smaller repose angle has a good powder laying effect, which is favorable for reducing spatial defects in the printing process, and also has a large specific surface area and good fusion effect with antioxidants, which greatly reduces local decomposition in the laser sintering process of polypropylene. The ethylene propylene copolymer product of the present invention has a narrower DSC half-width and a more uniform copolymer crystal composition, which improves the uniformity of melting and fusion of polymer particles, and improves the structural strength and surface performance of sintered samples.
[0195] <Test Example 2: Autoclave foamed beads> 1. The compressive strength of the foamed molding was measured according to the method of GB / T8813-2008 (Determination of Compressive Properties of Rigid Foamed Plastics), and the flexural strength of the foamed molding was measured according to the method of GB / T8812-2007 (Determination of Flexural Properties of Rigid Foamed Plastics).
[0196] 2. Measurement method of the expansion ratio of foamed beads: Using the density accessory YDK01 of the German Satorius CPA225D balance, obtain the density of the polypropylene composition foamed beads by the drainage method, and measure according to the method introduced in the national standard GB / T1033.1-2008 and ISO1183-1:2012. The expansion ratio of the obtained polypropylene composition foamed material is calculated by the formula: b=ρ1 / ρ2, where b is the expansion ratio, ρ1 is the density of the binary random copolymer polypropylene base resin, and ρ2 is the apparent density of the foamed material.
[0197] 200g of copolymerized polypropylene microspheres were placed in an autoclave, and 0.2g of antioxidant 1010, 1000g of dispersion medium (deionized water), 1g of surfactant (sodium dodecylbenzenesulfonate), 1g of dispersant (kaolin) and 0.02g of dispersion enhancer (aluminum sulfate) were added and mixed, and low-pressure carbon dioxide was further introduced to completely replace the air in the autoclave, and high-pressure carbon dioxide was further introduced, the autoclave temperature was raised to 138°C, the pressure was controlled to 6MPa, and swelling penetration was performed for 30 minutes. After that, the pressure was rapidly removed to make the gauge pressure 0, the pressure removal rate was controlled to 10MPa / s, and the material in the kettle was placed in cold water at 5°C and dried. The different expanded beads obtained by the above-mentioned expansion process were press-molded at a certain steam pressure for a certain time using a mold molding machine, and then the obtained molded body was aged for 24 hours under conditions of a temperature of 100°C and a pressure of standard atmospheric pressure to obtain an expanded bead molded body.
[0198] The expansion ratio of the foamed beads, the steam pressure for molding, and the molding time are shown in Table 4.
[0199] [Table 5]
[0200] As can be seen from the data in Table 4, when the polymer copolymer microspheres of the present invention are used for foaming, not only is the expansion ratio higher, but the steam pressure required is lower and the molding time is shorter. Lower steam pressure not only contributes to energy saving and cost reduction, but also contributes to reducing process risks. Shorter molding time means higher production efficiency, which is meaningful for improving profits and increasing production income.
[0201] It should be understood that the endpoints of the ranges and any values disclosed herein are not limited to the exact ranges or values, and that these ranges or values include values close to these ranges or values. Numerical ranges between the endpoints of each range, between the endpoints of each range and a single point value, and between the single point values can be combined with each other to obtain one or more new numerical ranges, and these numerical ranges should be considered to be specifically disclosed herein.
[0202] The above-described embodiments are for the purpose of illustrating the present invention, and are not intended to limit the present invention. Although the present invention has been described with reference to exemplary embodiments, it should be understood that the terms used are descriptive and interpretive terms, not limiting terms. The present invention can be modified within the scope of the claims of the present invention. Although the present invention relates to specific methods, materials, and embodiments, it is not meant to limit the present invention to the specific examples disclosed, but rather the present invention can be extended to all other methods and applications having the same functions. [Brief description of the drawings]
[0203] [Figure 1] FIG. 1 is an electron microscope photograph of the polypropylene powder obtained in Example 1. [Diagram 2] FIG. 2 is a schematic diagram of a DSC.
Claims
1. Polypropylene microspheres comprising 0.2 wt % to 10 wt % of constituent units derived from ethylene and 90 wt % to 99.8 wt % of constituent units derived from propylene, wherein a melting endothermic curve of the polypropylene microspheres is obtained by a differential scanning calorimeter and the half width of the melting endothermic curve of the polypropylene microspheres is 4 to 10°C.
2. 2. The polypropylene microspheres according to claim 1, characterized in that the half-width of the melting endothermic curve of the polypropylene microspheres is 5 to 8°C.
3. 3. The polypropylene microspheres according to claim 1, characterized in that the molecular weight distribution of the polypropylene microspheres is 4-9.
4. The polypropylene microspheres have a bulk density of 0.20 g / cm 3 ~0.50g / cm 3 and preferably 0.32 g / cm 3 ~0.48g / cm 3 and and / or the angle of repose is between 10° and 23°, preferably between 13° and 20°; and / or an isotacticity index of 60% to 94%, preferably 64% to 90%; and / or the ash content is 0.005% to 0.04%; And / or the polypropylene microspheres according to any one of claims 1 to 3, characterized in that the melt index is 3 to 160 g / 10 min, preferably 15 to 100 g / 10 min.
5. When DSC measurement is performed, the DSC result is λi=(dH / dt) i+1 -(dH / dt) i , 【Chemistry 1】 (i is T m <T i <T fm 5. Polypropylene microspheres according to any one of claims 1 to 4, characterized in that they satisfy the following characteristic:
6. The polypropylene microspheres according to any one of claims 1 to 5, characterized in that the average particle size of the polypropylene microspheres is 50 μm to 200 μm, preferably, the average particle size of the polypropylene microspheres is 60 μm to 160 μm, and more preferably, the average particle size of the polypropylene microspheres is 80 μm to 120 μm.
7. The polypropylene microspheres according to any one of claims 1 to 6, characterized in that the aspect ratio of the polypropylene microspheres is 0.9 to 1.1, preferably the aspect ratio of the polypropylene microspheres is 0.95 to 1.05, more preferably the aspect ratio of the polypropylene microspheres is 1.
8. The process for producing polypropylene microspheres according to any one of claims 1 to 7, characterized in that the process comprises copolymerizing a propylene-containing olefin in the presence of an olefin polymerization catalyst system to obtain polypropylene microspheres.
9. The olefin polymerization catalyst system comprises a catalyst component, an alkylaluminum compound component, and optionally an external electron donor compound component, with or without an added external electron donor compound component, or a reaction product of those components; and / or the catalyst comprises a magnesium-containing compound support, a titanium compound and an internal electron donor compound; And / or the molar ratio of the titanium compound, magnesium-containing compound carrier and internal electron donor compound is (37-255):(2-15):1, preferably (67-235):(4-12):
1.
10. The structure of the magnesium-containing compound support is represented by formula (I): 【Chemistry 2】 In formula (I), R 1 is C 1 -C 10 is an alkyl group of the formula R 2 and R 3 are the same or different and each independently represent H, C 1 -C 10 or C substituted with 1 to 10 halogen atoms 1 -C 10 is a halogenated alkyl group of the formula: R 4 is C substituted with at least one halogen atom 1 -C 10 or a halogenated alkyl group of the formula (I) or a C substituted with at least one halogen atom 6 -C 20 is a halogenated aryl group of the formula R 5 is C 1 -C 5 is an alkyl group of X is fluorine, chlorine, bromine or iodine; m is 0.1 to 1.9, n is 0.1 to 1.9, and m+n=2, preferably, m is 0.8 to 1.2, and n is 0.8 to 1.2; 0<q<0.2, 0<a<0.1, preferably 0.005≦q≦0.2, 0.001<a<0.05; and / or the internal electron donor compound is at least one selected from carboxylic acid esters, alcohol esters, ethers, ketones, nitriles, amines and silanes, and is preferably at least one selected from monohydric or polyhydric aliphatic carboxylic acid esters, monohydric or polyhydric aromatic carboxylic acid esters, dihydric alcohol esters and dihydric ethers; And / or the general formula of the titanium compound is Ti(OR 6 ) 4-b X' b and However, R 6 is C 1 -C 14 is an aliphatic hydrocarbon group of the formula X' is F, Cl or Br; b is an integer from 1 to 4; The method according to claim 9, wherein the titanium compound is at least one selected from the group consisting of titanium tetrachloride, titanium tetrabromide, titanium tetrafluoride, tributoxytitanium chloride, dibutoxytitanium dichloride, butoxytitanium chloride, triethoxytitanium chloride, diethoxytitanium dichloride and ethoxytitanium chloride.
11. The method for producing the magnesium-containing compound support includes the steps of: Magnesium halides having the general formula MgX″Y and magnesium halides having the general formula R 7 Step S1 of contacting and emulsifying a first alcohol-based compound, which is OH, for a first time to obtain a first product; In the general formula MgX″Y, X″ is any one selected from fluorine, chlorine, bromine, and iodine, and Y is fluorine, chlorine, bromine, iodine, C 1-6 Alkyl groups of C 1-6 an alkoxy group of C 6-14 an aryl group of C 6-14 is any one selected from the aryloxy groups Formula R 7 In OH, R 7 is C 1-10 is an alkyl group of the formula Step S2 of contacting the first product with an ethylene oxide-based compound having a structure represented by formula (II) in a second manner to obtain a second product; In S2, the structural formula of the ethylene oxide compound is represented by formula (II), 【Chemistry 3】 However, R 8 and R 9 are each independently H, C 1-10 an alkyl group of 1 to 10 halogen atoms; 1-10 and wherein the halogenated alkyl group is selected from the group consisting of The general formula is R 10 OH, halogenated alcohols having the general formula R 11 Step S3 of carrying out a third contact of a second alcohol-based compound, which is OH, with the second product to obtain a third product; Formula R 10 In OH, R 10 is C substituted with at least one halogen atom 1-10 or a halogenated alkyl group of the formula (I) or a C substituted with at least one halogen atom 6-20 and wherein the halogenated aryl group is selected from the group consisting of Formula R 11 In OH, R 11 is C 1-5 is an alkyl group of the formula and step S4 of spray-drying the third product to obtain a magnesium-containing compound support.
12. The method according to claim 11, wherein, relative to 1 mol of the magnesium halide, the amount of the first alcohol-based compound used is 1 to 30 mol, the amount of the ethylene oxide-based compound used is 1 to 10 mol, the amount of the halogenated alcohol used is 0.05 to 6.5 mol, and the amount of the second alcohol-based compound used is 5 to 100 mol, preferably, relative to 1 mol of the magnesium halide, the amount of the first alcohol-based compound used is 6 to 22 mol, the amount of the ethylene oxide-based compound used is 2 to 6 mol, the amount of the halogenated alcohol used is 1 to 5 mol, and the amount of the second alcohol-based compound used is 8 to 80 mol, and more preferably, relative to 1 mol of the magnesium halide, the amount of the second alcohol-based compound used is 31 to 50 mol.
13. The method according to any one of claims 9 to 12, characterized in that the magnesium-containing compound carrier has an average particle size of 2 to 100 microns and a particle size distribution of less than 2, preferably, the magnesium-containing compound carrier has an average particle size of 2 to 19 microns and a particle size distribution of 0.6 to 1.6, and more preferably, the magnesium-containing compound carrier has an average particle size of 2 to 10 microns and a particle size distribution of 0.6 to 1.
14. A 3D printing material comprising polypropylene microspheres according to any one of claims 1 to 7 and / or polypropylene microspheres produced by the method according to any one of claims 8 to 13.
15. Use of polypropylene microspheres according to any one of claims 1 to 7 or produced by the process according to any one of claims 8 to 13 for 3D printing, in particular for laser sintering printing, most preferably for selective laser sintering.
Citation Information
Patent Citations
Polypropylene powder for selective laser sintering and preparation thereof
CN107304270A
Propylene-based polymer and film using the same
JP2002128825A
Carrier for olefin polymerization catalyst and its application, catalyst for olefin polymerization and its application, and olefin polymerization method
JP2023540543A
OLEFIN-BASED PAINT CONTAINING PROPYLENE / α-OLEFIN COPOLYMER
WO2014196206A1
MODIFIED PROPYLENE-(α-OLEFIN) COPOLYMER, METHOD FOR PRODUCING SAME, COATING MATERIAL COMPRISING SAME, RESIN COMPOSITION FOR MOLDING USE, AND HOT-MELT COMPOSITION
WO2015068385A1