Biodegradable polymer
The polybutylene adipate terephthalate copolymer, with specific monomer combinations and ratios, addresses the challenge of maintaining mechanical properties and biodegradability in PBAT, achieving improved toughness and processability.
Patent Information
- Application Number
- JP2024528562
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2022-11-28
- Filing Date
- 2022-11-29
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2042-11-29
AI Technical Summary
Existing biodegradable polybutylene adipate terephthalate (PBAT) polymers face challenges in maintaining mechanical properties while ensuring high biodegradability, particularly when compounded with organic fillers, leading to issues like gelation and reduced processability.
A polybutylene adipate terephthalate copolymer is developed, incorporating specific repeating units derived from terephthalic, adipic, 3-methyladipic, and butanediol monomers, with controlled molar ratios to enhance mechanical properties and biodegradability, including a crystallinity value of 29.0% or less.
The copolymer achieves superior mechanical properties with enhanced biodegradability, demonstrated by elongation values of 500% to 700% and a weight average molecular weight of 50,000 to 100,000, while maintaining processability and biodegradability.
Smart Images

Figure 2024541374000001 
Figure 2024541374000002 
Figure 2024541374000003
Abstract
Description
[Technical field]
[0001] The present specification relates to a biodegradable polymer that has excellent mechanical properties and a high degree of biodegradability. [Background technology]
[0002] Polyester resins have excellent mechanical and chemical properties and have been used in a wide range of applications, such as drinking water containers, medical applications, food packaging paper, food containers, sheets, films, and automotive molded products.
[0003] Among them, polybutylene adipate terephthalate (PBAT) is a soft polyester that is biodegradable, and is therefore in the spotlight as a substitute for polyolefin polymers that are mainly used in packaging materials and agricultural films in response to recent environmental regulations.
[0004] However, when using soft PBAT alone for this purpose, it is necessary to process it into a thin film to ensure biodegradability. However, due to such a thin thickness, the physical properties of the film are often inferior to the actual resin properties. Therefore, a branching agent is added during polymerization to ensure film stability, or PBAT is blended with hard polylactic acid (PLA), or PBAT is used alone and compounded with an organic filler such as carbon black.
[0005] However, adding more than a certain amount of branching agent has the disadvantage of intensifying gelation, leading to defects in appearance and reduced physical properties, and when blended with PLA, the biodegradability is lower than that of PBAT alone, so a compatibilizer must be added. When PBAT is used alone through compounding with an organic filler, mixing through an extruder is used, but this type of physical mixing has limitations in dispersing the organic filler, and in many cases an excess amount is added compared to the actual amount required, which can reduce the biodegradability or mechanical properties of PBAT. Summary of the Invention [Problem to be solved by the invention]
[0006] The present specification aims to provide a biodegradable polymer that is excellent in mechanical properties and has a high degree of biodegradability. [Means for solving the problem]
[0007] In one embodiment of the present invention, a polybutylene adipate terephthalate copolymer is provided, which includes a first repeat unit derived from a terephthalic acid monomer, a second repeat unit derived from an adipic acid monomer, and a third repeat unit derived from a butanediol monomer, the second repeat unit including at least one of a 2-1 repeat unit derived from adipic acid and a 2-2 repeat unit derived from 3-methyladipic acid, and the third repeat unit including at least one of a 3-1 repeat unit derived from 1,4-butanediol and a 3-2 repeat unit derived from 1,2-butanediol.
[0008] The polybutylene adipate terephthalate copolymer may necessarily contain at least one of the 2-2 repeating unit and the 3-2 repeating unit.
[0009] In the polybutylene adipate terephthalate copolymer, the molar ratio of the second repeating unit to the first repeating unit may be about 0.5:1 to about 1.5:1. That is, the repeating unit derived from the adipic acid monomer may be contained in a ratio of about 50 mol to about 150 mol, about 80 mol to about 120 mol, or about 100 mol to about 120 mol, per 100 mol of the repeating unit derived from the terephthalic acid monomer.
[0010] The third repeat unit may be contained in the polybutylene adipate terephthalate copolymer at a ratio of about 50 to about 60 mol %.
[0011] In the polybutylene adipate terephthalate copolymer, the second repeating unit may include both a 2-1 repeating unit derived from adipic acid and a 2-2 repeating unit derived from 3-methyladipic acid.
[0012] In this case, the molar ratio of the 2-1 repeat unit: the 2-2 repeat unit in the polybutylene adipate terephthalate copolymer may be about 1000: 1 to about 100: 20. In other words, when the polybutylene adipate terephthalate copolymer contains both adipic acid-derived repeat units and 3-methyladipic acid-derived repeat units, the 3-methyladipic acid-derived repeat units may be contained in a ratio of about 0.1 to about 20 moles, about 0.5 to about 15 moles, or about 0.5 to about 10 moles per 100 moles of adipic acid-derived repeat units.
[0013] In the polybutylene adipate terephthalate copolymer, the third repeating unit may include both a 3-1 repeating unit derived from 1,4-butanediol and a 3-2 repeating unit derived from 1,2-butanediol.
[0014] In this case, the molar ratio of the 3-1 repeating unit: the 3-2 repeating unit in the polybutylene adipate terephthalate copolymer may be about 1000: 1 to about 100: 20. In other words, when the polybutylene adipate terephthalate copolymer contains both a repeating unit derived from 1,4-butanediol and a repeating unit derived from 1,2-butanediol, the repeating unit derived from 1,2-butanediol may be contained in a ratio of about 0.1 to about 5 mol, or about 0.2 to about 3 mol, per 100 mol of the repeating unit derived from 1,4-butanediol.
[0015] And, the polybutylene adipate terephthalate copolymer may have a crystallinity value of about 29.0% or less, or from about 20 to about 29%, or from about 25 to about 28%, as measured using a differential scanning calorimeter.
[0016] And, the polybutylene adipate terephthalate copolymer may have an MD elongation value, as measured by ASTM D 882, of about 500% or more, or about 500 to about 700%, or about 500 to about 650%, or about 550 to about 620%.
[0017] And, the polybutylene adipate terephthalate copolymer may have a TD elongation value, as measured by ASTM D 882, of about 500% or more, or about 500 to 700%, or about 550 to about 700%.
[0018] And, the polybutylene adipate terephthalate copolymer may have a weight average molecular weight value of about 50,000 to about 100,000, or 50,000 or more, or about 60,000 or more, or about 70,000 or more, and about 100,000 or less, or about 90,000 or less, or about 85,000 or less, or about 80,000 or less.
[0019] In the present invention, the terms "first", "second", etc. are used to describe various components, and the terms are used only for the purpose of distinguishing one component from another component.
[0020] Furthermore, the terms used in this specification are merely used to describe exemplary embodiments and are not intended to limit the present invention.
[0021] A singular expression includes a plural expression unless the context clearly indicates otherwise.
[0022] As used herein, terms such as "including," "comprising," or "having" are intended to describe implemented features, numbers, steps, components, or combinations thereof, and do not exclude the possibility of one or more other features, numbers, steps, components, combinations thereof, or additional features.
[0023] Also, in this specification, when a layer or element is referred to as being "on" or "on top of" another layer or element, this means that the layer or element is formed directly on the layer or element, or that other layers or elements may be additionally formed between layers, on the object, or on the substrate.
[0024] The present invention can be modified in various ways and can have various forms, and a specific embodiment will be exemplified and described in detail below. However, it should be understood that the present invention is not limited to the specific disclosed form, but includes all modifications, equivalents, and alternatives included in the spirit and technical scope of the present invention.
[0025] According to one aspect of the present invention, there is provided a polybutylene adipate terephthalate copolymer comprising a first repeat unit derived from a terephthalic acid based monomer, a second repeat unit derived from an adipic acid based monomer, and a third repeat unit derived from a butanediol based monomer, the second repeat unit comprising at least one of a 2-1 repeat unit derived from adipic acid and a 2-2 repeat unit derived from 3-methyladipic acid, and the third repeat unit comprising at least one of a 3-1 repeat unit derived from 1,4-butanediol and a 3-2 repeat unit derived from 1,2-butanediol.
[0026] As mentioned above, PBAT is highly biodegradable, and much research is being conducted to utilize this property. However, it has been difficult to improve the mechanical properties of PBAT while maintaining its excellent biodegradability.
[0027] The inventors of the present invention have found that when a polybutylene adipate terephthalate copolymer is produced by partially adding a monomer other than a monomer that has been commonly used in the past, the bond structure of the copolymer is changed, and the copolymer can maintain high biodegradability and effectively improve its mechanical properties, thereby completing the present invention.
[0028] A polybutylene adipate terephthalate copolymer according to one aspect of the present invention comprises a first repeating unit derived from a terephthalic acid monomer, a second repeating unit derived from an adipic acid monomer, and a third repeating unit derived from a butanediol monomer, the second repeating unit comprising at least one of a 2-1 repeating unit derived from adipic acid and a 2-2 repeating unit derived from 3-methyladipic acid, and the third repeating unit comprising at least one of a 3-1 repeating unit derived from 1,4-butanediol and a 3-2 repeating unit derived from 1,2-butanediol.
[0029] Each monomer used in the polybutylene adipate terephthalate copolymer of the present invention will be described below.
[0030] First, a polybutylene adipate terephthalate copolymer according to one aspect of the present invention contains a first repeating unit derived from a terephthalic acid monomer.
[0031] In this specification, the first repeat unit refers to a residue remaining in a polymer chain in a reaction in which a terephthalic acid monomer is condensed to form a polybutylene adipate terephthalate copolymer.
[0032] That is, when producing the polybutylene adipate terephthalate of the present invention, a terephthalic acid monomer is used, and the group derived from the terephthalic acid monomer is referred to as the first repeating unit.
[0033] Here, the terephthalic acid monomer means terephthalic acid and its derivatives.
[0034] The polybutylene adipate terephthalate copolymer according to one aspect of the present invention contains a second repeating unit derived from an adipic acid monomer.
[0035] In this specification, the second repeat unit refers to a group that remains in the polymer chain in the reaction in which an adipic acid-based monomer is condensed to form a polybutylene adipate terephthalate copolymer.
[0036] That is, when producing the polybutylene adipate terephthalate of the present invention, an adipic acid monomer is used, and the residue derived from the adipic acid monomer is referred to as the second repeating unit.
[0037] The second repeating unit further includes at least one of a 2-1 repeating unit derived from adipic acid and a 2-2 repeating unit derived from 3-methyladipic acid.
[0038] That is, when producing the polybutylene adipate terephthalate of the present invention, at least one of adipic acid and 3-methyladipic acid is necessarily used, and the polybutylene adipate terephthalate produced thereby necessarily contains at least one of the 2-1 repeat unit and the 2-2 repeat unit.
[0039] In particular, 3-methyladipic acid has a methyl group linked to the side chain of the adipic acid structure, which can increase the frequency of chain entanglement during the production of PBAT, thereby improving the toughness of the produced polymer and improving the mechanical properties of the polymer.
[0040] The polybutylene adipate terephthalate copolymer according to one aspect of the present invention contains a third repeating unit derived from a butanediol-based monomer.
[0041] In this specification, the third repeat unit refers to a residue remaining in a polymer chain in a reaction in which a butanediol-based monomer is condensed to form a polybutylene adipate terephthalate copolymer.
[0042] That is, when producing the polybutylene adipate terephthalate of the present invention, a butanediol-based monomer is used, and the group derived from the butanediol-based monomer is referred to as the third repeating unit.
[0043] The third repeating unit further includes at least one of a 3-1 repeating unit derived from 1,4-butanediol and a 3-2 repeating unit derived from 1,2-butanediol.
[0044] That is, when producing the polybutylene adipate terephthalate of the present invention, at least one of 1,4-butanediol and 1,2-butanediol is necessarily used, and the polybutylene adipate terephthalate produced thereby necessarily contains at least one of the 3-1 repeat unit and the 3-2 repeat unit.
[0045] In particular, 1,2-butanediol, unlike 1,4-butanediol, has a methyl group linked thereto that can act as a side chain in terms of structure, and this can increase the frequency of chain entanglement during the preparation of PBAT, thereby improving the toughness of the prepared polymer and the mechanical properties of the polymer.
[0046] The polybutylene adipate terephthalate copolymer may necessarily contain at least one of the 2-2 repeating unit and the 3-2 repeating unit.
[0047] More specifically, for example, the polybutylene adipate terephthalate copolymer of the present invention may comprise: i) a 1 repeat unit, a 2-1 repeat unit, and a 3-1 repeat unit; ii) a 1 repeat unit, a 2-1 repeat unit, and a 3-2 repeat unit; iii) a 1 repeat unit, a 2-2 repeat unit, and a 3-1 repeat unit; iv) a 1 repeat unit, a 2-2 repeat unit, and a 3-2 repeat unit; or v) comprising a 1st repeat unit, a 2-1st repeat unit, a 2-2nd repeat unit, and a 3-1st repeat unit; or vi) comprising a 1st repeat unit, a 2-1st repeat unit, a 3-1st repeat unit, and a 3-2nd repeat unit; or vii) It may have a form including a 1st repeating unit, a 2-1st repeating unit, a 2-2nd repeating unit, a 3-1st repeating unit, and a 3-2nd repeating unit.
[0048] In the polybutylene adipate terephthalate copolymer, the molar ratio of the second repeating unit to the first repeating unit may be about 0.5:1 to about 1.5:1. That is, the repeating unit derived from the adipic acid monomer may be contained in a ratio of about 50 mol to about 150 mol, about 80 mol to about 120 mol, or about 100 mol to about 120 mol, per 100 mol of the repeating unit derived from the terephthalic acid monomer.
[0049] If the content of terephthalic acid is too high, the biodegradability and processability of the produced polybutylene adipate terephthalate copolymer may be rapidly reduced.
[0050] The third repeat unit may be included in the polybutylene adipate terephthalate copolymer at a ratio of about 50 to 60 mol %.
[0051] In the polybutylene adipate terephthalate copolymer, the second repeating unit may include both a 2-1 repeating unit derived from adipic acid and a 2-2 repeating unit derived from 3-methyladipic acid.
[0052] In this case, the molar ratio of the 2-1 repeat unit: the 2-2 repeat unit in the polybutylene adipate terephthalate copolymer may be about 1000: 1 to about 100: 20. In other words, when the polybutylene adipate terephthalate copolymer contains both adipic acid-derived repeat units and 3-methyladipic acid-derived repeat units, the 3-methyladipic acid-derived repeat units may be contained in a ratio of about 0.1 to about 20 moles, about 0.5 to about 15 moles, or about 0.5 to about 10 moles per 100 moles of adipic acid-derived repeat units.
[0053] If the content of the repeating unit derived from 3-methyladipic acid, i.e., the 2-2 repeating unit, is too low, the effect of improving mechanical properties is minimal, and if the content of the repeating unit derived from 3-methyladipic acid, i.e., the 2-2 repeating unit, is too high, the degree of entanglement of polymer chains in the produced polybutylene adipate terephthalate copolymer increases, and the melt viscosity of the copolymer can increase rapidly, which can cause problems in the processing step, such as reduced processability and productivity.
[0054] In the polybutylene adipate terephthalate copolymer, the third repeating unit may include both a 3-1 repeating unit derived from 1,4-butanediol and a 3-2 repeating unit derived from 1,2-butanediol.
[0055] In this case, the molar ratio of the 3-1 repeating unit: the 3-2 repeating unit in the polybutylene adipate terephthalate copolymer may be about 1000: 1 to about 100: 20. In other words, when the polybutylene adipate terephthalate copolymer contains both a repeating unit derived from 1,4-butanediol and a repeating unit derived from 1,2-butanediol, the repeating unit derived from 1,2-butanediol may be contained in a ratio of about 0.1 to about 5 mol, or about 0.2 to about 3 mol, per 100 mol of the repeating unit derived from 1,4-butanediol.
[0056] If the content of the repeating unit derived from 1,2-butanediol, i.e., the 3-2 repeating unit, is too low, the effect of improving mechanical properties is minimal, and if the content of the repeating unit derived from 1,2-butanediol, i.e., the 3-2 repeating unit, is too high, the degree of entanglement of polymer chains in the produced polybutylene adipate terephthalate copolymer increases, and the melt viscosity of the copolymer can increase rapidly, which can cause problems in the processing step, such as reduced processability and productivity.
[0057] And, the polybutylene adipate terephthalate copolymer may have a crystallinity value of about 29.0% or less, or from about 20 to about 29%, or from about 25 to about 28%, as measured using a differential scanning calorimeter.
[0058] The degree of crystallinity can be calculated as the weight fraction of the crystalline portion relative to the entire resin. In the case of biodegradable polyester resins, it is known that the higher the degree of crystallinity, the lower the degree of biodegradation, and the degree of biodegradation can be roughly predicted based on the degree of crystallinity.
[0059] The polybutylene adipate terephthalate copolymer of the embodiment contains a monomer having a structure that has not been commonly used in the past, and has a lower chain symmetry than existing PBAT, which results in a lower crystallinity.
[0060] The polybutylene adipate terephthalate copolymer of the present invention has a crystallinity value within the above range, which allows it to maintain excellent biodegradability.
[0061] Here, the crystallinity can be measured using a differential scanning calorimeter. Specifically, a differential scanning calorimeter (DSC, device name: DSC 2500, manufacturer: TA Instrument) is used to sequentially perform primary heating, primary cooling, and secondary heating in a temperature range (-70 to 200 degrees, 10 degrees / min), and the crystallinity is calculated using the heat of fusion of the melting transition during the secondary heating (PBAT ΔH m 0 =114 J / g available).
[0062] And, the polybutylene adipate terephthalate copolymer may have an MD elongation value, as measured by ASTM D 882, of about 500% or more, or about 500 to about 700%, or about 500 to about 650%, or about 550 to about 620%.
[0063] And, the polybutylene adipate terephthalate copolymer may have a TD elongation value, as measured by ASTM D 882, of about 500% or more, or about 500 to 700%, or about 550 to about 700%.
[0064] In this way, the polybutylene adipate terephthalate copolymer according to one embodiment of the present invention can achieve superior mechanical properties compared to conventional copolymers.
[0065] And, the polybutylene adipate terephthalate copolymer may have a weight average molecular weight value of about 50,000 to about 150,000, or 50,000 or more, or about 60,000 or more, or about 70,000 or more, and about 150,000 or less, or about 100,000 or less, or about 90,000 or less, or about 85,000 or less, or about 80,000 or less.
[0066] The polybutylene adipate terephthalate copolymer can be produced by subjecting a monomer mixture containing the above-mentioned monomers to an esterification reaction in the presence of a polymerization catalyst.
[0067] The catalyst is not particularly limited as long as it is widely used as a polyester polymerization catalyst in the technical field to which the present invention pertains.
[0068] Specifically, the catalyst may be at least one selected from the group consisting of titanium methoxide, titanium ethoxide, titanium propoxide, titanium isopropoxide, titanium butoxide, and titanium isobutoxide.
[0069] For example, the catalyst may be titanium butoxide.
[0070] The polymerization reaction may be carried out on a total monomer mixture in which the above-mentioned monomers and catalyst are all mixed together, or each monomer and catalyst may be mixed separately and then individually charged into a reactor to carry out the polymerization reaction, or a prepolymer may be first produced and then the main polymerization reaction may be carried out.
[0071] In the case of separately preparing the catalyst mixture, a butanediol-based monomer and a catalyst may be mixed to prepare a catalyst mixture, and a terephthalic acid-based monomer and an adipic acid-based monomer may be prepared as a separate monomer mixture, and then the two may be mixed.
[0072] The catalyst in the catalyst mixture may be included in an amount of 0.001 to 10 parts by weight based on 100 parts by weight of adipic acid in the monomer mixture.
[0073] Within this range, the esterification reaction of the monomer mixture and the polymerization of the esterification reaction product (ie, prepolymer) can be adequately mediated.
[0074] However, if the amount of catalyst added during the preparation of the catalyst mixture is too small, the polymerization time will be long and the productivity will decrease.In contrast, if the amount of catalyst added is too large, the polymerization time will be short, but the possibility of discoloration of the final PBAT will increase, so the amount of heat stabilizer added must be increased in proportion to the amount of catalyst added, which will increase the production cost.
[0075] Considering such a tendency, the amount of catalyst in the catalyst mixture can be adjusted. For example, the catalyst in the catalyst mixture may be used in an amount of 0.001 parts by weight or more, 0.005 parts by weight or more, or 0.01 parts by weight or more, and 10 parts by weight or less, 5 parts by weight or less, or 0.1 parts by weight or less, based on 100 parts by weight of the adipic acid-based monomer in the monomer mixture.
[0076] On the other hand, a prepolymer refers to a polymer with a relatively low degree of polymerization, in which the polymerization reaction is stopped at the intermediate coating stage in order to facilitate molding.
[0077] When producing a prepolymer, a monomer mixture containing adipic acid and terephthalic acid is subjected to an esterification reaction in the presence of the catalyst mixture to carry out primary polymerization, thereby producing a low molecular weight copolymer having a low degree of polymerization.
[0078] When preparing the prepolymer, 0.1 to 1 part by weight of a crosslinking agent or branching agent may be added based on 100 parts by weight of adipic acid in the monomer mixture to carry out the esterification reaction.
[0079] When a crosslinking agent is added and an esterification reaction is carried out, an internally crosslinked prepolymer is produced, which can improve the mechanical properties of the final composite.
[0080] The crosslinking agent is a low molecular weight compound containing three or more hydroxy groups or three or more carboxy groups in the molecule, and may be, for example, an erythritol-based compound, a glycerol-based compound, a citric acid-based compound, etc. For example, the crosslinking agent may be pentaerythritol.
[0081] The step of preparing the prepolymer may be carried out at a temperature range of 150 to 350°C.
[0082] Within this temperature range, the prepolymer can be produced while maintaining uniform dispersion of each monomer.
[0083] For example, the step of producing the prepolymer may be carried out at a temperature range that is 150°C or more, 170°C or more, 190°C or more, or 210°C or more, and 350°C or less, 320°C or less, 290°C or less, or 250°C or less.
[0084] Nitrogen gas may be injected during the preparation of the prepolymer. Specifically, by quickly removing water generated as a by-product during the nitrogen gas injection, reverse reactions caused by water are suppressed, improving the monomer conversion rate and thereby increasing the molecular weight of the copolymer produced.
[0085] For example, nitrogen gas may be injected at a rate of at least (0.00)1 ml / min, at least (0.0)1 ml / min, at least (0.02) ml / min, or at least (0.05) ml / min, and at most (100) ml / min, at most (50) ml / min, at most (10) ml / min, or at most (5) ml / min.
[0086] In the main polymerization reaction for repolymerizing the prepolymer, 0.001 to 10 parts by weight of a catalyst may be additionally added based on 100 parts by weight of adipic acid in the monomer mixture.
[0087] The activity of the catalyst initially added is likely to decrease during the prepolymer production step. For example, titanium, the central metal component of the catalyst, may react with water, a by-product of the esterification reaction, to form titanium oxide, and the monomer component or prepolymer component may be substituted at the alkoxide site of titanium alkoxide.
[0088] Therefore, it is preferable to additionally add a catalyst immediately before the reaction.
[0089] For example, the additional catalyst may be used in an amount of 0.001 parts by weight or more, 0.005 parts by weight or more, or 0.01 parts by weight or more, and 10 parts by weight or less, 5 parts by weight or less, or 0.1 parts by weight or less, based on 100 parts by weight of the adipic acid-based monomer in the monomer mixture.
[0090] After the catalyst is added, a heat stabilizer may be added, which can suppress discoloration of the final PBAT.
[0091] Specifically, 0.001 to 1 part by weight of a heat stabilizer may be added based on 100 parts by weight of the adipic acid monomer in the monomer mixture.
[0092] For example, based on 100 parts by weight of adipic acid in the monomer mixture, the heat stabilizer may be added in an amount of 0.001 parts by weight or more, 0.005 parts by weight or more, 0.08 parts by weight or more, or 0.01 parts by weight or more, and 1 part by weight or less, 0.6 parts by weight or less, 0.3 parts by weight or less, or 0.1 parts by weight or less.
[0093] During polymerization of the prepolymer, the method may include the steps of: increasing the temperature of a reactor containing the prepolymer until the temperature reaches a range of 150 to 350° C.; reducing the pressure of the reactor after the temperature increase until the pressure reaches 0.1 to 0.00001 atm; and terminating the reaction after 2 to 8 hours while maintaining the reduced pressure and temperature.
[0094] For example, the temperature of the reactor containing the prepolymer may be increased until it reaches a temperature range that is 150°C or more, 170°C or more, 190°C or more, or 210°C or more, and 350°C or less, 320°C or less, 290°C or less, or 250°C or less.
[0095] After reaching the temperature range, 1 to 10 minutes later, the pressure in the reactor may be reduced to a pressure range of 0.00001 atm or more, 0.00005 atm or more, 0.0001 atm or more, or 0.0002 atm or more, and 0.1 atm or less, 0.05 atm or less, 0.03 atm or less, or 0.01 atm or less.
[0096] After the pressure reduction, the pressure and temperature are maintained to carry out the reaction, and the reaction may be terminated after 2 hours or more, 2.2 hours or more, 2.4 hours or more, or 3 hours or more and 8 hours or less, 7.5 hours or less, 7 hours or less, or 6 hours have elapsed since the start of the reaction. Effect of the Invention
[0097] The biodegradable polymer according to the example given in this specification has excellent mechanical properties and can have a high degree of biodegradability. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0098] The functions and effects of the present invention will be described in more detail below through specific examples of the present invention. However, these examples are presented only as examples of the present invention and do not define the scope of the invention.
[0099] <Example> The reaction was carried out in a batch system, and after preparing a prepolymer, the main polymerization reaction was carried out.
[0100] The monomer components summarized in Table 1 below, pentaerythritol, and titanium butoxide (primary, 0.5 mmol) were filled into a reactor, and the reactor was maintained at about 230° C. Nitrogen gas was introduced into the reactor for about 3 hours to remove by-products, and an esterification reaction (prepolymer reaction) was carried out.
[0101] When the prepolymer reaction was completed, titanium butoxide (2nd generation, 0.7 mmol) and triethyl phosphonoacetate (1.3 mmol) as a thermal stabilizer component were added thereto, and the mixture was stirred so that the catalyst component and the thermal stabilizer component were uniformly dispersed in the prepolymer.
[0102] Thereafter, the temperature of the reactor was raised to about 240°C, and 5 minutes after the temperature of the reactor reached about 240°C, the pressure inside the reactor was reduced, and the main polymerization reaction was carried out at a pressure of 3 mbar or less for about 4 hours to obtain a PBAT polymer.
[0103] The reaction conditions for each of the Examples and Comparative Examples are summarized in Table 1 below.
[0104] [Table 1] *Tp: terephthalic acid; Ad: adipic acid; 3Mad: 3-methyladipic acid; 1,4Bd: 1,4-butanediol; 1,2-Bd: 1,2-butanediol
[0105] Physical property evaluation Weight average molecular weight determination: The measurement target was dissolved in chloroform at a concentration of 1 mg / ml, and the solution was then loaded into a gel permeation chromatography (GPC, PL GPC220, Agilent Technologies) instrument to measure the molecular weight. At this time, polystyrene was used as the standard polymer.
[0106] Crystallinity measurement: For each of the biodegradable polymer composites of Examples 1 to 4 and the PBATs of Comparative Examples 1 to 3, a differential scanning calorimeter (DSC, device name: DSC 2500, manufacturer: TA Instrument) was used to sequentially carry out primary heating, primary cooling, and secondary heating in a temperature range (-70 to 200°C, 10°C / min). The crystallinity was calculated using the heat of fusion of the melting transition during the secondary heating (PBAT ΔH m 0 =114 J / g used).
[0107] Elongation: The PBAT copolymers of the examples and comparative examples were blown into blown films at an extrusion temperature of 130°C to 170°C using a short extruder (SHINWHA Industrial Single Screw Extruder, Blown Film M / C, 50mm, L / D=20) to a thickness of about 50μm. The die gap was 2.0mm and the blow-up ratio was 2.3.
[0108] Elongation: A tensile test was performed on each film specimen at a stretching speed of 10 mm / min using an Instron Universal Testing Machine (UTM) according to ASTM D 882 to measure the elongation value. The conditions of the tensile test were Load Cell 10KN, LE position 40 mm, and the elongation was measured in both the machine direction (MD) and transverse direction (TD).
[0109] The measurement results are summarized in Table 2 below. [Table 2] Referring to Table 2, it can be seen that the polybutylene adipate terephthalate copolymer according to one embodiment of the present invention has a similar degree of polymerization to the comparative example, even though it further contains a monomer having a specific structure during polymerization.
[0110] In addition, the crystallinity of the polybutylene adipate terephthalate copolymers according to the examples is generally lower than that of the comparative examples. This is believed to be due to the steric hindrance effect of the side chain alkyl groups of the separately added monomers, which inhibit the crystallization of the chains of the polybutylene adipate terephthalate copolymer.
[0111] In addition, it is generally known that as the crystallinity of polybutylene adipate terephthalate copolymer decreases, the mechanical properties also decrease. However, in the case of the polybutylene adipate terephthalate copolymer according to an embodiment of the present invention, it was confirmed that the mechanical properties were improved compared to the comparative example, despite the crystallinity being lower than that of the comparative example. This is believed to be because the chain entanglement was increased due to the side chain alkyl group in the polymer chain, which increased the toughness of the polymer.
Claims
1. comprising a first repeat unit derived from a terephthalic acid based monomer, a second repeat unit derived from an adipic acid based monomer, and a third repeat unit derived from a butanediol based monomer; The second repeating unit includes at least one of a 2-1 repeating unit derived from adipic acid and a 2-2 repeating unit derived from 3-methyladipic acid, The third repeating unit includes at least one of a 3-1 repeating unit derived from 1,4-butanediol and a 3-2 repeating unit derived from 1,2-butanediol. Polybutylene adipate terephthalate copolymer.
2. At least one of the 2-2 repeat unit and the 3-2 repeat unit is necessarily included; 2. The polybutylene adipate terephthalate copolymer of claim 1.
3. the molar ratio of the second repeat unit to the first repeat unit is from 0.5:1 to 1.5:1; 2. The polybutylene adipate terephthalate copolymer of claim 1.
4. The third repeat unit is contained in an amount of 50 to 60 mol %.
2. The polybutylene adipate terephthalate copolymer of claim 1.
5. The second repeating unit includes a 2-1 repeating unit derived from adipic acid and a 2-2 repeating unit derived from 3-methyladipic acid.
2. The polybutylene adipate terephthalate copolymer of claim 1.
6. the molar ratio of the 2-1 repeat unit: the 2-2 repeat unit is from 1000:1 to 100:20; The polybutylene adipate terephthalate copolymer of claim 5.
7. The third repeating unit includes a 3-1 repeating unit derived from 1,4-butanediol and a 3-2 repeating unit derived from 1,2-butanediol.
2. The polybutylene adipate terephthalate copolymer of claim 1.
8. the molar ratio of the 3-1 repeat unit: the 3-2 repeat unit is 1000:1 to 100:20; The polybutylene adipate terephthalate copolymer of claim 7.
9. The weight average molecular weight is 50,000 to 150,000.
2. The polybutylene adipate terephthalate copolymer of claim 1.
Citation Information
Patent Citations
Ring opening polymerization method of PBAT / PLA (poly(butylene adipate-co-terephthalate) / poly(lactic acid)) block copolymer
CN107163232A
Biodegradable copolyester and preparation method thereof
CN111116883A
Polyester of terephthalic acid, method for the production thereof, and use of the same
KR1020080042101A
Process for producing aqueous dispersions of thermoplastic polyesters
KR1020130039729A
Polymer composition for highly disintegratable film
WO2018158269A1