Separator and manufacturing method thereof

A hydrophilic polymer-coated separator for lithium secondary batteries optimizes electrolyte impregnation and process productivity, addressing air permeability and electrolyte distribution issues in conventional separators, thus improving battery performance and longevity.

JP2024541393AActive Publication Date: 2024-11-08W SCOPE KOREA CO LTD +1
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
JP2024529214
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2021-11-26
Filing Date
2022-07-25
Publication Date
2024-11-08
Estimated Expiration
2042-07-25

AI Technical Summary

Technical Problem

Conventional polyolefin-based separators for lithium secondary batteries face challenges with reduced air permeability and electrolyte impregnation due to ceramic particle coatings, leading to decreased ion movement and uneven electrolyte distribution, which affects battery performance and longevity.

Method used

A separator is developed with a hydrophilic polymer coating on a porous support, optimized by a specific formula (0.015≦(C×D)/(A×B)≦0.65) to balance thickness, air permeability, and porosity, enhancing electrolyte impregnation and process productivity.

Benefits of technology

The hydrophilic polymer coating improves electrolyte impregnability and process productivity, maintaining mechanical and electrochemical properties while ensuring uniform electrolyte distribution, thereby enhancing battery performance and lifespan.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024541393000001
    Figure 2024541393000001
  • Figure 2024541393000002
    Figure 2024541393000002
  • Figure 2024541393000003
    Figure 2024541393000003
Patent Text Reader

Abstract

One aspect of the present invention provides a separator that includes a porous support and a hydrophilic polymer applied to a surface of the porous support from a solution containing the hydrophilic polymer and a solvent, and that satisfies the following formula, and a method for producing the same. <expression> 0.015≦(C×D) / (A×B)≦0.65 In the above formula, A is the thickness (μm) of the porous support, B is the air permeability (Gurley, sec / 100 ml) of the porous support, C is the porosity (volume %) of the porous support, and D is the content (weight %) of the hydrophilic polymer in the solution.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a separator and a manufacturing method thereof, and more particularly to a separator for a lithium secondary battery having improved impregnation with an electrolyte and a manufacturing method thereof. [Background technology]

[0002] Lithium secondary batteries are widely used as power sources for various electrical products that require compactness and light weight, such as smartphones, laptops, and tablet PCs. As their application range expands to include smart grids and medium- to large-sized batteries for electric vehicles, there is a demand for the development of lithium secondary batteries with large capacity, long life, and high stability.

[0003] As a means to achieve the above objective, research and development is being actively conducted on separators that have micropores that separate the positive and negative electrodes to prevent internal shorts and facilitate the movement of lithium ions during charging and discharging. In particular, microporous separators that use polyolefins such as polyethylene, which are advantageous in forming pores through thermally induced phase separation, are economical, and tend to satisfy the physical properties required for a separator.

[0004] Conventionally, polyolefin-based separators have problems with poor heat resistance and mechanical strength. To address this problem, a technology has been proposed in which a heat-resistant layer containing ceramic particles is coated on the surface of the separator. However, the heat-resistant layer has significant technical issues related to air permeability and electrical conductivity (resistance), which are factors that have a very important effect on the performance of the separator. That is, when a heat-resistant layer containing ceramic particles is formed on the surface of a porous substrate, the heat resistance of the separator is improved, but the ceramic particles contained in the heat-resistant layer close the pores formed in the porous substrate, reducing the air permeability of the separator, thereby greatly reducing the ion transfer path between the positive and negative electrodes, resulting in a significant decrease in the charge and discharge performance of the secondary battery. In addition, when the heat-resistant layer is continuously exposed to the electrolyte inside the battery, the ceramic particles are partially and continuously detached from the porous substrate, and in this case, the heat resistance of the separator may also gradually decrease.

[0005] In addition, a lithium secondary battery has a structure in which an electrode assembly having a positive electrode and a negative electrode, each of which has an active material applied to an electrode collector, and a porous separator interposed between them, is impregnated with a non-aqueous electrolyte containing a lithium salt.

[0006] Lithium secondary batteries are manufactured by stacking positive and negative electrodes alternately and preparing an electrode assembly with a separator between the positive and negative electrodes, inserting the electrode assembly into a battery case made of a can or pouch of a certain size and shape, and finally injecting an electrolyte. In this case, the electrolyte penetrates between the positive and negative electrodes and the separator by capillary force. However, because the positive and negative electrodes and the separator are hydrophobic due to the characteristics of the materials, while the electrolyte is hydrophilic, it takes a considerable amount of time and strict process conditions to improve the impregnation and wettability of the electrolyte to the electrodes and the separator, and therefore there is a limit to achieving and improving the balance between the impregnation of the electrolyte and the productivity of the process.

[0007] In order to improve the impregnation of the electrolyte, methods such as injecting the electrolyte at a high temperature or injecting the electrolyte under a pressurized or reduced pressure have been used, but these methods have problems such as deformation of the conventional electrode assembly and electrolyte due to heat, which can cause internal short circuits, etc. In addition, since the above process is performed after the electrode assembly is housed in a battery case together with the electrolyte, the impregnation of the electrode assembly with the electrolyte can be non-uniform, and in particular, in the case of a jelly-roll type electrode assembly, non-uniform impregnation occurs between the center and outer parts of the winding, which can shorten the life of the battery. Summary of the Invention [Problem to be solved by the invention]

[0008] The present invention is intended to solve the above-mentioned problems of the prior art, and an object of the present invention is to provide a separator and a manufacturing method thereof that can achieve a balanced combination of electrolyte impregnation and process productivity. [Means for solving the problem]

[0009] One aspect of the present invention provides a separator that includes a porous support and a hydrophilic polymer applied to a surface of the porous support from a solution containing the hydrophilic polymer and a solvent, and satisfies the following formula: <expression> 0.015≦(C×D) / (A×B)≦0.65 In the above formula, A is the thickness (μm) of the porous support, B is the air permeability (Gurley, sec / 100 ml) of the porous support, C is the porosity (volume %) of the porous support, and D is the content (weight %) of the hydrophilic polymer in the solution.

[0010] In one embodiment, the porous support may have a thickness of 1 to 30 μm. In one embodiment, the porosity of the porous support may be 40 to 70% by volume. In one embodiment, the porous support may comprise one selected from the group consisting of polyethylene, polypropylene, polybutylene, polymethylpentene, ethylene vinyl acetate, ethylene butyl acrylate, ethylene ethyl acrylate, and combinations of two or more thereof.

[0011] In one embodiment, the hydrophilic polymer may be one selected from the group consisting of ethylene vinyl alcohol, polyvinyl alcohol, polyacrylic acid, polyoxyethylene-polyoxypropylene block copolymers, polyethylene glycol, polyethylene oxide, polyvinylpyrrolidone, polyvinyl acetal, polyvinyl butyral, cellulose derivatives, glycerol, and combinations of two or more thereof. In one embodiment, the content of the hydrophilic polymer in the solution may be 0.05 to 3% by weight.

[0012] In one embodiment, the solvent is water, NMP (N-Methyl-2-pyrrolidone), acetone, DMF (N,N-dimethylformamide), DMSO (Dimethyl sulfoxide), CHP (Cyclohexyl-pyrrolidinone), N12P (N-dodecyl-pyrrolidone), benzyl benzoate, N8P (N-Octyl-pyrrolidone), DMEU (dimethyl-imidazolidinone), cyclohexanone, DMA (dimethylacetamide), NMF (N-Methyl Formamide), bromobenzene, chloroform, chlorobenzene, benzonitrile, quinoline, benzyl ether, ethanol, isopropyl alcohol, methanol, butanol, 2-ethoxyethanol, 2-butoxyethanol, 2-methoxypropanol, THF (tetrahydrofuran), ethylene glycol, pyridine, N-vinylpyrrolidone, methyl ethyl ketone, alpha-terpineol, formic acid, ethyl acetate, acrylonitrile, and combinations of two or more thereof.

[0013] In one embodiment, the length change rate in the machine direction (MD) of the electrolyte applied dropwise to the surface of the separator from immediately after the application of the electrolyte drop to a point where 3 minutes have elapsed may be 80% or more. In one embodiment, the length change rate in the lateral direction (TD) of the electrolyte applied to the surface of the separator from immediately after the application of the electrolyte to a point where 3 minutes have elapsed may be 80% or more.

[0014] Another aspect of the present invention provides a method for producing a separator, the method including: (a) preparing a porous support; and (b) preparing a solution containing a hydrophilic polymer and a solvent, and applying the solution to a surface of the porous support. Effect of the Invention

[0015] In one embodiment of the present invention, a separator is provided by applying a hydrophilic polymer to a hydrophobic polyolefin-based separator to impart hydrophilicity, and the thickness, air permeability, porosity, and concentration of a solution containing the hydrophilic polymer of the porous support constituting the separator are derived as variables for optimizing and realizing a predetermined level of electrolyte impregnation, and are combined to achieve a balanced productivity of the process for applying the hydrophilic polymer, the hydrophilicity of the separator, and the resulting electrolyte impregnation.

[0016] It should be understood that the effects of the present invention are not limited to the effects described above, but include all effects that can be inferred from the configuration of the invention described in the detailed description of the present invention or the claims. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0017] The present invention may, however, be embodied in many different forms and should not be construed as limited to the embodiments set forth herein.

[0018] Throughout the specification, when any part is said to be "connected" to another part, this includes not only the case where it is "directly connected" to another part, but also the case where it is "indirectly connected" through another member in between. Furthermore, when any part is said to "include" a certain component, this does not mean that it excludes the other component, but that it may further include the other component, unless otherwise specified to the contrary.

[0019] The separator according to one embodiment of the present invention may include a porous support and a hydrophilic polymer applied to a surface of the porous support by a solution containing a hydrophilic polymer and a solvent, and may satisfy the following formula: <expression> 0.015≦(C×D) / (A×B)≦0.65 In the above formula, A is the thickness (μm) of the porous support, B is the air permeability (Gurley, sec / 100 ml) of the porous support, C is the porosity (volume %) of the porous support, and D is the content (weight %) of the hydrophilic polymer in the solution.

[0020] The porous support is hydrophobic, but can be made hydrophilic by applying a certain amount of the hydrophilic polymer to the porous support. In this case, the thickness (A), air permeability (B), and porosity (C) of the porous support, and the concentration of the solution containing the hydrophilic polymer, i.e., the content (D) of the hydrophilic polymer in the solution, are derived as variables for optimizing and realizing the required electrolyte impregnation, and are combined to achieve a balanced productivity of the process for applying the hydrophilic polymer, the hydrophilicity of the separator, and the resulting electrolyte impregnation.

[0021] The value of (C×D) / (A×B) according to the above formula is 0.015 to 0.65, preferably 0.02 to 0.6, and more preferably 0.02 to 0.4. If the value of (C×D) / (A×B) according to the above formula is less than 0.015, the required hydrophilicity and the resulting electrolyte impregnation property cannot be imparted to the porous support, and if it exceeds 0.65, a part of the hydrophilic polymer closes the pores of the porous support, increasing the resistance and causing a deterioration in the electrochemical properties of the battery.

[0022] The thickness of the porous support is 1 to 30 μm, preferably 3 to 25 μm, and more preferably 5 to 20 μm. If the thickness of the porous support is less than 1 μm, the mechanical properties and heat resistance of the separator may decrease, while if it exceeds 30 μm, the resistance increases, and not only the electrochemical properties of the battery decrease, but also the productivity of the process required for introducing the hydrophilic polymer into the porous support may decrease.

[0023] The air permeability (Gurley) of the porous support is 40 sec to 300 sec / 100 ml, preferably 50 sec to 200 sec / 100 ml. If the air permeability of the porous support is less than 40 sec / 100 ml, the mechanical properties and heat resistance of the separator may be reduced, whereas if the air permeability exceeds 300 sec / 100 ml, the resistance increases, and not only the electrochemical properties of the battery are reduced, but also the productivity of the process required for introducing the hydrophilic polymer into the porous support may be reduced.

[0024] The porosity of the porous support is 40 to 70 vol%, preferably 45 to 70 vol%, more preferably 50 to 60 vol%. Generally, the porosity of a polyolefin-based porous separator for a lithium secondary battery is about 30 to 50 vol%, preferably about 30 to 40 vol%, but by increasing the porosity of the porous support, the area of ​​the surface and / or internal pores to which the hydrophilic polymer can be applied can be increased, and the larger the area of ​​the portion to which the hydrophilic polymer is applied, the more the impregnation of the electrolyte can be improved. If the porosity of the porous support is less than 40 vol%, the resistance increases, and not only the electrochemical properties of the battery deteriorate, but also the productivity of the process required for introducing the hydrophilic polymer into the porous support may decrease, and if it exceeds 70 vol%, the mechanical properties and heat resistance of the separator may decrease.

[0025] The porous support may include one selected from the group consisting of polyethylene, polypropylene, polybutylene, polymethylpentene, ethylene vinyl acetate, ethylene butyl acrylate, ethylene ethyl acrylate, and combinations of two or more thereof, and may preferably include a polyolefin resin such as polyethylene or polypropylene, and more preferably may include polyethylene, but is not limited thereto.

[0026] The hydrophilic polymer is applied to the surface of the porous support and the surfaces of the pores formed inside and / or outside the porous support through the solution, thereby imparting hydrophilicity to the porous support. The content of the hydrophilic polymer in the solution is 0.05 to 3 wt%, preferably 0.1 to 2 wt%, and more preferably 0.5 to 2 wt%. If the content of the hydrophilic polymer in the solution is less than 0.05 wt%, the required hydrophilicity and the resulting electrolyte impregnation property cannot be imparted to the porous support, and if it exceeds 3 wt%, a part of the hydrophilic polymer may close the pores of the porous support, increasing the resistance and deteriorating the electrochemical properties of the battery.

[0027] The hydrophilic polymer may be one selected from the group consisting of ethylene vinyl alcohol, polyvinyl alcohol, polyacrylic acid, polyoxyethylene-polyoxypropylene block copolymer, polyethylene glycol, polyethylene oxide, polyvinylpyrrolidone, polyvinyl acetal, polyvinyl butyral, cellulose derivatives, glycerol, and combinations of two or more of these, preferably ethylene vinyl alcohol, polyvinyl alcohol and / or polyacrylic acid, and more preferably ethylene vinyl alcohol, but is not limited thereto. The content of ethylene units in the ethylene vinyl alcohol is 10 to 60 mol%, preferably 20 to 50 mol%, and more preferably 25 to 40 mol%.

[0028] The solution may further include a solvent for appropriately dissolving the hydrophilic polymer, such as water, N-Methyl-2-pyrrolidone (NMP), acetone, N,N-dimethylformamide (DMF), dimethyl sulfoxide (DMSO), cyclohexyl-pyrrolidinone (CHP), N-dodecyl-pyrrolidone (N12P), benzyl benzoate, N-octyl-pyrrolidone (N8P), dimethyl-imidazolidinone (DMEU), cyclohexanone, dimethylacetamide (DMA), N-Methyl-2-pyrrolidone (NMF), dimethylformamide (DMA), dimethylformamide (DMSO), dimethylsulfoxide (DMSO), dimethylformamide ... Formamide), bromobenzene, chloroform, chlorobenzene, benzonitrile, quinoline, benzyl ether, ethanol, isopropyl alcohol, methanol, butanol, 2-ethoxyethanol, 2-butoxyethanol, 2-methoxypropanol, THF (tetrahydrofuran), ethylene glycol, pyridine, N-vinylpyrrolidone, methyl ethyl ketone, alpha-terpineol, formic acid, ethyl acetate, acrylonitrile, phenol, and combinations of two or more of these may be selected from the group consisting of, preferably, DMSO and / or isopropyl alcohol, and more preferably, when the hydrophilic polymer is ethylene vinyl alcohol, DMSO, which has excellent selective and specific solubility therefor and excellent impregnation ability for the porous support, may be used. The concentration of DMSO in the solvent may be substantially about 100%, but is not limited thereto.

[0029] The length change rate in the machine direction (MD) from immediately after the addition of the electrolyte droplets on the surface of the separator until 3 minutes have elapsed is 80% or more, preferably 90% or more, and more preferably 95% or more. If the longest length in the machine direction (MD) immediately after the addition of the electrolyte droplets on the surface of the separator is MD1 and the longest length in the machine direction (MD) 3 minutes after that is MD2, the length change rate can be calculated by the following formula 1. <Expression 1> Length change rate in the machine direction (MD) (%) = (MD2-MD1) / (MD1) x 100

[0030] The length change rate in the lateral direction (TD) from immediately after the addition of the electrolyte droplets on the surface of the separator until 3 minutes have elapsed is 80% or more, preferably 90% or more, and more preferably 95% or more. If the longest length in the lateral direction (TD) immediately after the addition of the electrolyte droplets on the surface of the separator is TD1 and the longest length in the lateral direction (TD) 3 minutes after that is TD2, the length change rate can be calculated by the following formula 2. <Expression 2> Transverse (TD) length change rate (%) = (TD2-TD1) / (TD1) x 100

[0031] The electrolyte may be one selected from the group consisting of ethylene carbonate (EC), propylene carbonate (PC), diethyl carbonate (DEC), dimethyl carbonate (DMC), ethyl methyl carbonate (EMC) and a combination of two or more thereof, preferably propylene carbonate (PC), but is not limited thereto.

[0032] When the electrolyte is propylene carbonate (PC), if the length change rate in the machine direction (MD) and the transverse direction (TD) is less than 80%, it can be evaluated that the required electrolyte impregnation cannot be achieved.

[0033] The ratio of the length change rate of the droplet of the electrolyte in the longitudinal direction (MD) to the length change rate of the droplet of the electrolyte in the transverse direction (TD) may be greater than 1.0. That is, the length change rate of the droplet of the electrolyte in the longitudinal direction (MD) may be greater than the length change rate of the droplet of the electrolyte in the transverse direction (TD). The ratio of the length change rate of the droplet of the electrolyte in the longitudinal direction (MD) to the length change rate of the droplet of the electrolyte in the transverse direction (TD) is 1.1 or less, preferably 1.05 or less, and more preferably 1.03 or less. If the ratio of the length change rate of the droplet of the electrolyte in the longitudinal direction (MD) to the length change rate of the droplet of the electrolyte in the transverse direction (TD) exceeds 1.1, the impregnation of the separator with the electrolyte may be non-uniform depending on the direction, and the electrochemical characteristics of the battery may be deteriorated.

[0034] The separator can be manufactured by a method including the steps of: (a) preparing a porous support; and (b) preparing a solution containing a hydrophilic polymer and a solvent, and applying the solution to a surface of the porous support.

[0035] The properties, types, effects, etc. of the porous support, the hydrophilic polymer, and the solvent are as described above.

[0036] In the step (b), a solution containing the hydrophilic polymer and the solvent is prepared, and the solution is applied to the surface of the porous support. The application can be performed by dipping, spraying, rolling, bar, or a combination of two or more of these, and is preferably performed by dipping, i.e., impregnation or immersion, but is not limited thereto.

[0037] The time required for applying the solution can be adjusted within a range of about 0.5 minutes to 48 hours, preferably about 0.5 to 10 minutes, and more preferably about 1 to 5 minutes, depending on the thickness, air permeability, porosity, and concentration of the solution of the porous support. If the application time is less than 0.5 minutes, the required hydrophilicity cannot be imparted, and if it exceeds 48 hours, the productivity of the process for imparting hydrophilicity may be significantly reduced.

[0038] In addition, after the step (b), the method may further include a step (c) of treating and washing the porous support with a solvent such as ethanol, water, or methylene chloride, and then drying the porous support. The solvent used for the washing may be ethanol, taking into consideration the external physical properties of the separator and the time required for drying, but is not limited thereto. That is, when the solvent is ethanol, the time required for the subsequent drying can be shortened, defects generated on the surface of the dried separator can be minimized, and appropriate external physical properties can be secured.

[0039] Hereinafter, examples of the present invention will be described in detail. Example 1-1 A porous support with a thickness of 9 μm, an air permeability of 50 sec / 100 ml (Gurley), and a porosity of 60% by volume was prepared. Ethylene vinyl alcohol (EVOH, Kuraray, EVAL, PE-32 mol%) was added to a dimethyl sulfoxide (DMSO) solvent and stirred at 80° C. for 1 hour to produce a solution with an ethylene vinyl alcohol content of 0.5 wt%.

[0040] The porous support was immersed in the solution for 30 seconds, and then excess solution remaining on both sides of the porous support was removed using a silicon blade.The porous support was immersed in ethanol for 60 seconds for cleaning, and then placed in an oven preheated to 60° C. and dried for 1 minute to produce a separator.

[0041] Example 1-2 A separator was manufactured in the same manner as in Example 1-1, except that the content of ethylene vinyl alcohol in the solution was changed to 0.75 wt %.

[0042] Examples 1-3 A separator was manufactured in the same manner as in Example 1-1, except that the content of ethylene vinyl alcohol in the solution was changed to 1 wt %.

[0043] Examples 1-4 A separator was manufactured in the same manner as in Example 1-1, except that the content of ethylene vinyl alcohol in the solution was changed to 3 wt %.

[0044] Comparative Example 1-1 A separator was manufactured in the same manner as in Example 1-1, except that the content of ethylene vinyl alcohol in the solution was changed to 5 wt %. The manufacturing conditions of the separators according to the examples and comparative examples are shown in Table 1 below. - Thickness (μm): The thickness of the porous support was measured using a micro thickness measuring device. -Air permeability (Gurley, sec / 100 ml): The time it takes for 100 ml of air to pass through the porous support at a measurement pressure of 0.025 MPa was measured using Asahi Seiko Co., Ltd.'s Gurley Densometer EGO2-5 model. Porosity (%): The porosity of the porous support was measured using a capillary porometer manufactured by PMI Corporation based on ASTM F316-03.

[0045] [Table 1]

[0046] Experimental Example 1 The electrolyte impregnation of the separators prepared in the examples and comparative examples was measured as follows: A propylene carbonate (PC) solution was used as the electrolyte, and 2 μl of the propylene carbonate solution was dropped onto the surface of the separator. Immediately after the drop, the droplet size (MD1, TD1) and the droplet size (MD2, TD2) of the dispersed droplets after 3 minutes were measured along the machine direction (MD) and the transverse direction (TD). The results are shown in Table 2 below.

[0047] [Table 2]

[0048] Referring to Table 2, both the Examples and Comparative Examples were evaluated to have good electrolyte impregnation, but in the case of the separator according to Comparative Example 1-1, the excessive amount of EVOH impregnated and coated blocked the pores of the separator, resulting in reduced air permeability and ionic conductivity.

[0049] Example 2-1 A porous support with a thickness of 20 μm, an air permeability of 180 sec / 100 ml (Gurley), and a porosity of 50% by volume was prepared. Ethylene vinyl alcohol (EVOH, Kuraray, EVAL, PE-32 mol%) was added to a dimethyl sulfoxide (DMSO) solvent and stirred at 80° C. for 1 hour to produce a solution with an ethylene vinyl alcohol content of 1.5% by weight.

[0050] The porous support was immersed in the solution for 30 seconds, and then excess solution remaining on both sides of the porous support was removed using a silicon blade.The porous support was immersed in ethanol for 60 seconds for cleaning, and then placed in an oven preheated to 60° C. and dried for 1 minute to produce a separator.

[0051] Example 2-2 A separator was manufactured in the same manner as in Example 2-1, except that the content of ethylene vinyl alcohol in the solution was changed to 2 wt %.

[0052] Example 2-3 A separator was prepared in the same manner as in Example 2-1, except that the porous support was immersed in the solution for 1 minute.

[0053] Examples 2-4 A separator was prepared in the same manner as in Example 2-2, except that the porous support was immersed in the solution for 1 minute.

[0054] Comparative Example 2-1 A separator was manufactured in the same manner as in Example 2-1, except that the content of ethylene vinyl alcohol in the solution was changed to 1 wt %.

[0055] Comparative Example 2-2 A separator was prepared in the same manner as in Comparative Example 2-1, except that the porous support was immersed in the solution for 3 minutes.

[0056] Comparative Example 2-3 A separator was prepared in the same manner as in Comparative Example 2-1, except that the porous support was immersed in the solution for 5 minutes.

[0057] Comparative Example 2-4 A separator was prepared in the same manner as in Comparative Example 2-1, except that the porous support was immersed in the solution for 10 minutes. The manufacturing conditions of the separators according to the examples and comparative examples are shown in Table 3 below.

[0058] [Table 3]

[0059] Experimental Example 2 The electrolyte impregnation of the separators prepared in the examples and comparative examples was measured in the same manner as in Experimental Example 1, and the results are shown in Table 4 below.

[0060] [Table 4]

[0061] The above description of the present invention is for illustrative purposes only, and those skilled in the art will understand that the present invention can be easily modified in other specific forms without changing the technical idea or essential features of the present invention. Therefore, the above-described embodiments should be understood to be illustrative in all respects and not restrictive. For example, each component described as a single type may be implemented in a distributed form, and similarly, each component described as a distributed type may be implemented in a combined form.

[0062] The scope of the present invention is defined by the claims set forth below, and all modifications and variations that fall within the meaning and scope of the claims and their equivalent concepts should be understood to be included within the scope of the present invention.

Claims

1. A porous support; a hydrophilic polymer applied to the surface of the porous support by a solution containing a hydrophilic polymer and a solvent; A separator that satisfies the following formula: <Formula> 0.015≦(C×D) / (A×B)≦0.65 In the above formula, A is the thickness of the porous support (μm); B is the air permeability of the porous support (Gurley, sec / 100 ml); C is the porosity (volume %) of the porous support; D is the content (wt %) of the hydrophilic polymer in the solution.

2. The separator according to claim 1, wherein the porous support has a thickness of 1 to 30 μm.

3. The separator according to claim 1, wherein the porosity of the porous support is 40 to 70 volume %.

4. 2. The separator of claim 1, wherein the porous support comprises one selected from the group consisting of polyethylene, polypropylene, polybutylene, polymethylpentene, ethylene vinyl acetate, ethylene butyl acrylate, ethylene ethyl acrylate, and combinations of two or more thereof.

5. 2. The separator according to claim 1, wherein the hydrophilic polymer is one selected from the group consisting of ethylene vinyl alcohol, polyvinyl alcohol, polyacrylic acid, polyoxyethylene-polyoxypropylene block copolymers, polyethylene glycol, polyethylene oxide, polyvinylpyrrolidone, polyvinyl acetal, polyvinyl butyral, cellulose derivatives, glycerol, and combinations of two or more thereof.

6. 2. The separator according to claim 1, wherein the content of the hydrophilic polymer in the solution is 0.05 to 3% by weight.

7. The solvent may be water, NMP (N-methyl-2-pyrrolidone), acetone, DMF (N,N-dimethylformamide), DMSO (dimethyl sulfoxide), CHP (cyclohexyl-pyrrolidone), N12P (N-dodecyl-pyrrolidone), benzyl benzoate, N8P (N-octyl-pyrrolidone), DMEU (dimethyl-imidazolidinone), cyclohexanone, DMA (dimethylacetamide), NMF (N-methyl 2. The separator according to claim 1, wherein the solvent is one selected from the group consisting of benzene, benzenediamine, bromobenzene, chloroform, chlorobenzene, benzonitrile, quinoline, benzyl ether, ethanol, isopropyl alcohol, methanol, butanol, 2-ethoxyethanol, 2-butoxyethanol, 2-methoxypropanol, THF (tetrahydrofuran), ethylene glycol, pyridine, N-vinylpyrrolidone, methyl ethyl ketone, alpha-terpineol, formic acid, ethyl acetate, acrylonitrile, and combinations of two or more thereof.

8. 2. The separator according to claim 1, wherein a length change rate in a machine direction (MD) from immediately after the electrolytic solution is dropped onto a surface of the separator until 3 minutes have elapsed is 80% or more.

9. 2. The separator according to claim 1, wherein a length change rate in a transverse direction (TD) from immediately after the electrolytic solution is dropped onto a surface of the separator until 3 minutes have elapsed is 80% or more.

10. A method for producing the separator according to any one of claims 1 to 9, comprising the steps of: (a) providing a porous support; (b) preparing a solution containing a hydrophilic polymer and a solvent, and applying the solution to the surface of the porous support.

Citation Information

Patent Citations

  • Multilayer porous membrane and method for producing the same

    JP2008210794A

  • Separator for nonaqueous secondary battery, and nonaqueous secondary battery

    JP2018163872A

  • Microporous membrane