(Ultra)high molecular weight polyethylene block copolymer, its manufacturing method and secondary battery separator manufactured using the same
A multistage polymerization process using specific catalysts and co-catalysts addresses the compatibility issues between polyethylene and polypropylene, producing ultra-high molecular weight block copolymers that enhance the performance of secondary battery separation membranes.
Patent Information
- Application Number
- JP2024529835
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2021-11-18
- Filing Date
- 2022-11-15
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2042-11-15
AI Technical Summary
The low compatibility between polyethylene and polypropylene during mixing results in decreased uniformity and processing stability, limiting the production of high-performance secondary battery separation membranes due to heterogeneous systems and poor mechanical properties.
A multistage polymerization process using a trivalent titanium catalyst, alkyl aluminum compound, and silicon compound as co-catalysts to produce ultra-high molecular weight polyethylene block copolymers with controlled molecular weights and structures, enhancing compatibility and processing stability.
The process improves the compatibility and processing stability of polyethylene and polypropylene, resulting in secondary battery separation membranes with enhanced puncture strength, tensile strength, and kneadability.
Smart Images

Figure 2024541442000001 
Figure 2024541442000002 
Figure 2024541442000003
Abstract
Description
[Technical field]
[0001] The present invention relates to an (ultra)high molecular weight polyethylene-based block copolymer, a manufacturing method thereof, and a separator for a secondary battery manufactured using the same as a raw material. More specifically, in order to solve the problem of reduced compatibility between polyethylene and polypropylene during the mixing process of (ultra)high molecular weight polyethylene and ultra-high molecular weight polypropylene used in a separator for a secondary battery, the present invention relates to an (ultra)high molecular weight polyethylene-based block copolymer having (ultra)high molecular weight polyethylene as a one-stage polymer with a linear structure by multi-stage polymerization, thereby improving uniformity and processing stability, a manufacturing method thereof, and a separator for a secondary battery manufactured using the same as a raw material. [Background technology]
[0002] In general, polypropylene polymerization is carried out using magnesium chloride as a carrier, titanium chloride containing phthalate, diether, and succinate compounds as internal electron donors as the main catalyst, alkylaluminum as a cocatalyst, and a silicon compound containing an alkoxy group as an external electron donor cocatalyst, and polymerization is carried out in various reaction forms such as slurry polymerization, bulk polymerization, and gas phase polymerization. Polyethylene polymerization is carried out by slurry polymerization using a titanium catalyst supported by magnesium chloride as the main catalyst and alkylaluminum compounds as a cocatalyst.
[0003] The polyethylene and polypropylene produced in this manner have low compatibility and are generally not compounded. However, for certain applications such as ropes, they can be partially mixed and compounded by using a polyethylene-polypropylene block copolymer as a compatibilizer to increase the kneadability.
[0004] Despite this lack of compatibility, in recent years, separators have been produced by mixing (ultra) high molecular weight polyethylene with polypropylene to improve the performance of secondary battery separators. However, general-purpose polypropylene has poor processability and mechanical properties due to its low viscosity, and a heterogeneous system exists due to the content of (ultra) high molecular weight polyethylene and ultra-high molecular weight polypropylene, which limits the production of separators with uniform performance. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] European Patent EP3157966B1 [Patent Document 2] Registered US Patent US8008417 [Patent Document 3] Korean Patent KR10-1161752 Summary of the Invention [Problem to be solved by the invention]
[0006] In order to solve the above problems, the present invention aims to provide a method for selecting a main catalyst capable of polymerizing polyethylene and polypropylene, a combination ratio of a main catalyst, a cocatalyst, a promoter, etc., polymerization conditions for adjusting the molecular weight and basic properties of each polyethylene and polypropylene during multi-stage polymerization, and a (ultra) high molecular weight polyethylene-based block copolymer for improving the performance of a separator for a secondary battery, a manufacturing method thereof, and a separator for a secondary battery manufactured using the same as a raw material. [Means for solving the problem]
[0007] In order to achieve the above object, the present invention discloses a method for producing an (ultra)high molecular weight polyethylene block copolymer, comprising: (a) a step of mixing and charging a cocatalyst (x) which is an alkylaluminum compound, a main catalyst (y) which is a titanium compound, and a promoter (z) which is a silicon compound in the presence of a hydrocarbon solvent having 1 to 20 carbon atoms into a reactor; (b) a step of charging only ethylene monomer or ethylene monomer and a trace amount of hydrogen into the mixed solution obtained in the step (a) to perform a first-stage polymerization reaction; (c) a step of removing unreacted monomers in the reactor after the first-stage polymerization reaction; (d) a step of charging propylene monomer into the mixed solution obtained in the step (c) to perform a second-stage polymerization reaction; and (e) a step of filtering and drying a polyethylene-polypropylene block copolymer powder from the reaction solution obtained in the step (d).
[0008] Here, the cocatalyst (x) may be at least one compound selected from the group consisting of triethylaluminum, trimethylaluminum, triisobutylaluminum, trioctylaluminum, diethylaluminum chloride, diethylaluminum bromide, diethylaluminum iodide, diethylaluminum fluoride, ethylaluminum dichloride, dimethylaluminum chloride, methylaluminum dichloride, and ethylaluminum sesquichloride.
[0009] Here, the co-catalyst (z) is cyclohexylmethyldimethoxysilane (CMCD), cyclohexyl-n-propyldimethoxysilane (CPDM), cyclohexyl-i-propyldimethoxysilane (CIPDM), cyclohexyl-n-butyldimethoxysilane (CBDM), cyclohexyl-i-butyldimethoxysilane (CIBDM), cyclohexyl-n-hexyldimethoxysilane (CHDM), cyclohexyl-n-octyldimethoxysilane (CODM), cyclohexyl-n-decyldimethoxysilane (CDeDM), dimethyldimethoxysilane, dimethyldiethoxysilane, dicyclo The compound may be any one or more compounds selected from the group consisting of pentyldimethoxysilane, diisopropyldimethoxysilane, dicyclopentyldimethoxysilane, methylphenyldimethoxysilane, diphenyldiethoxysilane, methyltrimethoxysilane, ethyltrimethoxysilane, vinyltrimethoxysilane, phenyltrimethoxysilane, methyltriethoxysilane, ethyltriethoxysilane, vinyltriethoxysilane, phenyltriethoxysilane, butyltriethoxysilane, ethyltriisopropoxysilane, vinyltributoxysilane, and methyltriaryloxysilane.
[0010] Here, the co-catalyst (x) which is the alkylaluminum compound may contain 10 to 500 moles of Al per mole of Ti in the main catalyst (y) which is the titanium compound.
[0011] Here, the co-catalyst (z) which is a silicon compound may contain 1 to 40 moles of Si per mole of Ti in the main catalyst (y) which is a titanium compound.
[0012] Here, in the first and second polymerization reactions, the polymerization temperature may be within the range of 30 to 90°C.
[0013] Here, in the first and second stage polymerization reactions, the polymerization pressure may be within the range of 1 to 40 bar.
[0014] Here, in the first-stage polymerization reaction, the ethylene monomer can be fed in an amount of 3 to 95% by weight, and in the second-stage polymerization reaction, the propylene monomer can be fed in an amount of 6 to 98% by weight.
[0015] On the other hand, in order to achieve the above-mentioned object, the present invention further discloses a (ultra)high molecular weight polyethylene-based block copolymer, comprising, relative to 100 weight % of the block copolymer, 25 to 90 weight % of (ultra)high molecular weight polyethylene; and 10 to 75 weight % of ultra-high molecular weight polypropylene, wherein the (ultra)high molecular weight polyethylene has a viscosity average molecular weight of 400,000 to 5,000,000 g / mol, the ultra-high molecular weight polypropylene has a viscosity average molecular weight of 1,000,000 to 4,000,000 g / mol, and the block copolymer has a viscosity average molecular weight of 400,000 to 5,000,000 g / mol under conditions where no hydrogen is added or a very small amount of hydrogen is added.
[0016] Here, the block copolymer can have the (ultra) high molecular weight polyethylene as a one-stage polymer having a linear structure by carrying out a first-stage polymerization reaction in which only ethylene monomer is added to a mixed solution, or by carrying out a first-stage polymerization reaction in which ethylene monomer and a trace amount of hydrogen are added to the mixed solution, and then carrying out a second-stage polymerization reaction in which propylene monomer is added to the mixed solution.
[0017] The block copolymer has an apparent density of 0.30 to 0.50 g / cm 3 may be also possible.
[0018] Here, the block copolymer may have an inorganic content of 1 to 30 ppm, and the inorganic substance may be used as a catalyst in the polymerization process.
[0019] Here, the block copolymer may have a particle size of 10 to 400 μm.
[0020] On the other hand, in order to achieve the above object, the present invention further discloses a secondary battery separator produced from an (ultra) high molecular weight polyethylene-based block copolymer, the (ultra) high molecular weight polyethylene-based block copolymer being composed of 25 to 90% by weight of (ultra) high molecular weight polyethylene and 10 to 75% by weight of ultra-high molecular weight polypropylene, relative to 100% by weight of the block copolymer, the (ultra) high molecular weight polyethylene having a viscosity average molecular weight of 400,000 to 5,000,000 g / mol, the ultra-high molecular weight polypropylene having a viscosity average molecular weight of 1,000,000 to 4,000,000 g / mol, and the block copolymer having a viscosity average molecular weight of 400,000 to 5,000,000 g / mol under conditions where no hydrogen or a very small amount of hydrogen is added.
[0021] Here, the secondary battery separator may have a puncture strength of 300 to 600 gf.
[0022] Here, the secondary battery separator has a tensile strength of 800 to 2,000 kgf / cm 2 may be also possible. Effect of the Invention
[0023] According to the (ultra) high molecular weight polyethylene-based block copolymer of the present invention, it is possible to use it as a compatibilizer to increase the kneading property during mixing and processing of polyethylene and polypropylene, which have low compatibility, and it is also effective in improving the kneading property, film surface and other physical properties compared to a secondary battery separator made of a heterogeneous composite material of polyethylene and polypropylene, which is simply mixed and processed. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0024] The terms used in this application are merely used to describe specific examples. Thus, for example, singular expressions include plural expressions unless the context clearly requires that they be singular. It should be noted that the terms "include" or "comprise" used in this application are used to clearly indicate the presence of features, steps, functions, components, or combinations thereof described in the specification, and do not preliminarily exclude the presence of other features, steps, functions, components, or combinations thereof.
[0025] On the other hand, unless otherwise defined, all terms used herein should be considered to have the same meaning as that commonly understood by a person having ordinary skill in the art to which the present invention pertains. Therefore, unless expressly defined herein, a particular term should not be construed in an overly ideal or formal sense.
[0026] To improve the performance of secondary battery separators made by mixing (ultra) high molecular weight polyethylene with polypropylene, a catalyst capable of multi-stage polymerization of (ultra) high molecular weight polyethylene and ultra-high molecular weight polypropylene must be selected, and technology must be secured to adjust the molecular weight of polyethylene and polypropylene and the degree of polymerization of polyethylene and polypropylene in multi-stage polymerization. In addition, adjustments to the particle shape and size of the powder are required to facilitate the production, supply and processing of the powder.
[0027] The present inventors have confirmed that it is possible to prepare an (ultra) high molecular weight polyethylene-based block copolymer having improved performance as a separator for a secondary battery by controlling the molecular weight of polyethylene and polypropylene and performing multi-stage polymerization, and thus completed the present invention. Meanwhile, the term "(ultra) high molecular weight" as used herein means a viscosity average molecular weight of 1,000,000 g / mol or more.
[0028] In addition, the term "high molecular weight" as used herein means a molecular weight having a viscosity average molecular weight of more than 400,000 g / mol and less than 1,000,000 g / mol.
[0029] Selection of titanium catalysts for the polymerization of polyethylene and polypropylene. In order to achieve the above-mentioned objectives, the present invention requires the selection of a main catalyst that can polymerize polyethylene and polypropylene and ensure a stable powder form, as well as the combination ratio of the main catalyst, cocatalyst, and promoter, etc. The titanium chloride catalyst supported by Ziegler-Natta magnesium chloride causes the degree of polymerization of polyethylene and polypropylene to differ depending on the acid value of titanium, which has a great impact on the molecular weight and granularity.
[0030] In particular, in the case of a trivalent titanium catalyst, since it is possible to polymerize both polyethylene and polypropylene, the present invention selects a trivalent titanium catalyst as a catalyst capable of multi-stage polymerization of (ultra)high molecular weight polyethylene and ultra-high molecular weight polypropylene, and provides a method for adjusting the ratio of cocatalyst and promoter to ensure molecular weight control and stable particle shape during polyethylene polymerization.
[0031] More specifically, the present invention provides a multi-stage polymerization method for producing an (ultra)high molecular weight polyethylene block copolymer by using a trivalent titanium catalyst as the main catalyst, which is the magnesium titanium chloride compound, and varying the input ratio of a co-catalyst, which is an alkylaluminum compound, and a promoter, which is a silicon compound containing an alkoxy group.
[0032] Method for producing (ultra)high molecular weight polyethylene block copolymers The present invention provides a method for multi-stage polymerization of (ultra) high molecular weight polyethylene block copolymers using a trivalent titanium catalyst as the main catalyst, which is the magnesium chloride-supported titanium compound, and varying the input ratios of a co-catalyst, which is an alkylaluminum compound, and a promoter, which is a silicon compound containing an alkoxy group.
[0033] In the method for producing a (ultra) high molecular weight polyethylene block copolymer of the present invention, each step is as follows.
[0034] (a) mixing and charging a cocatalyst (x) which is an alkylaluminum compound, a main catalyst (y) which is a titanium compound, and a cocatalyst (z) which is a silicon compound into a reactor in the presence of a hydrocarbon solvent having 1 to 20 carbon atoms;
[0035] (b) adding only ethylene monomer or adding ethylene monomer and a trace amount of hydrogen to the mixed solution obtained in the step (a) to carry out a first-stage polymerization reaction;
[0036] (c) removing unreacted monomers from the reactor after the first-stage polymerization reaction;
[0037] (d) adding propylene monomer to the mixed solution obtained in the step (c) to carry out a second-stage polymerization reaction; and
[0038] (e) filtering and drying a powder of the polyethylene block copolymer from the reaction solution obtained in step (d).
[0039] In the present invention, an (ultra) high molecular weight polyethylene-based block copolymer having an (ultra) high molecular weight polyethylene as a first-stage polymer with a linear structure can be produced by sequentially adding ethylene monomer in step (b) and then propylene monomer in step (d). That is, in the (ultra) high molecular weight polyethylene-based block copolymer of the present invention, the (ultra) high molecular weight polyethylene produced by the first-stage polymerization reaction can form a starting polymer chain with a linear structure, and then the ultra-high molecular weight polypropylene produced by the second-stage polymerization reaction can form a subsequent polymer chain that is linearly linked to the starting polymer chain.
[0040] Specifically, the (ultra) high molecular weight polyethylene can be the main chain of the (ultra) high molecular weight polyethylene-based block copolymer of the present invention, and the ultra-high molecular weight polypropylene can be a continuous main chain of one main chain of the (ultra) high molecular weight polyethylene-based block copolymer of the present invention.
[0041] The term "main chain" used in this specification means a trunk molecular chain that forms the backbone of a polymer, and means that a starting polymer chain and a subsequent polymer chain form one main chain. The present invention explains that (ultra) high molecular weight polyethylene and ultra high molecular weight polypropylene, which are different polymers, form blocks in the same main chain.
[0042] Furthermore, after performing step (d), steps (b) to (d) are performed again to prepare the block copolymer according to the present invention through four-stage polymerization. In this case, a block copolymer having uniform mixing properties and improved physical properties compared to the two-stage polymerization according to the present invention and a separator for a secondary battery prepared using the block copolymer as a raw material can be obtained.
[0043] The multi-stage polymerization of the (ultra) high molecular weight polyethylene block copolymer according to the present invention can be repeated within a range of 1 to 5 times, but is not limited thereto.
[0044] Here, the step (a) is preferably carried out under a nitrogen atmosphere, i.e., the step (a) is preferably carried out in the presence of an inert gas, but is not limited thereto.
[0045] In the method for producing an (ultra) high molecular weight polyethylene block copolymer of the present invention, the hydrocarbon solvent having 1 to 20 carbon atoms in step (a) may include at least one solvent selected from the group consisting of aliphatic hydrocarbon solvents such as pentane, hexane, cyclohexane, methylcyclohexane, heptane, octane, decane, undecane, dodecane, tridecane, or tetradecane; aromatic hydrocarbon solvents such as benzene, toluene, xylene, or ethylbenzene; and halogenated hydrocarbon solvents such as dichloropropane, dichloroethylene, trichloroethylene, carbon tetrachloride, or chlorobenzene. Alternatively, gas phase polymerization or bulk polymerization may be performed under high pressure propylene without a hydrocarbon.
[0046] In addition, in step (a) of the method for producing the (ultra) high molecular weight polyethylene block copolymer of the present invention, representative examples of the cocatalyst (x) include any one or more compounds selected from the group consisting of triethylaluminum, trimethylaluminum, triisobutylaluminum, trioctylaluminum, diethylaluminum chloride, diethylaluminum bromide, diethylaluminum iodide, diethylaluminum fluoride, ethylaluminum dichloride, dimethylaluminum chloride, methylaluminum dichloride, and ethylaluminum sesquichloride.
[0047] In step (a), the cocatalyst (x) is preferably added in an amount of 3 to 1,000 moles per mole of the main catalyst (y), but is not limited thereto. More specifically, it is preferable that the cocatalyst (x) which is an alkylaluminum compound contains 3 to 1,000 moles of Al per mole of Ti in the main catalyst (y) which is a titanium compound, and it is even more preferable that the cocatalyst (x) which is an alkylaluminum compound contains 5 to 500 moles of Al per mole of Ti in the main catalyst (y) which is a titanium compound. Furthermore, it is even more preferable that the cocatalyst (x) which is an alkylaluminum compound contains 10 to 500 moles of Al per mole of Ti in the main catalyst (y) which is a titanium compound. If the amount of Al in the cocatalyst (x), which is an alkylaluminum compound, is less than 5 mol per mol of Ti in the main catalyst (y), which is a titanium compound, a problem may arise in that the polymerization reaction does not proceed sufficiently. Conversely, if the amount of Al in the cocatalyst (x), which is an alkylaluminum compound, is more than 500 mol per mol of Ti in the main catalyst (y), which is a titanium compound, the alkyl group of the cocatalyst may cause scission of the molecular main chain, making it impossible to obtain a high molecular weight polyethylene resin, and making it impossible to obtain a (ultra)high molecular weight polyethylene block copolymer having uniform kneadability and improved physical properties.
[0048] In step (a), the main catalyst (y) contains a silicon compound including phthalate, diether, and succinate as an internal electron donor, and titanium trichloride is preferable as a Ziegler-Natta titanium chloride catalyst supported by magnesium chloride, and a catalyst that provides high stereoregularity depending on the form of the internal electron donor is more preferable, and a generally commercially available catalyst can be used.
[0049] In step (a), the co-catalyst (z) may be at least one compound selected from the group consisting of a compound represented by the following formula (1), a compound represented by the following formula (2), and a compound represented by the following formula (3): [ka] [ka] [ka] In the above chemical formulas (1) to (3), R a , R 7 , R 8 and R 9 are each independently an alkyl group, a cycloalkyl group, an aryl group, an allyl group, or a vinyl group having 1 to 12 carbon atoms; R b is an alkyl group having 1 to 6 carbon atoms or an aryl group, and R is an alkyl group having 1 to 12 carbon atoms, a cycloalkyl group, an aryl group, an allyl group, or -OR c In this case, R c is an alkyl group or an aryl group having 1 to 6 carbon atoms, and n is an integer from 0 to 6.
[0050] Specifically, representative examples of the compound of the formula (1) include cyclohexylmethyldimethoxysilane (CMCD), cyclohexyl-n-propyldimethoxysilane (CPDM), cyclohexyl-i-propyldimethoxysilane (CIPDM), cyclohexyl-n-butyldimethoxysilane (CBDM), cyclohexyl-i-butyldimethoxysilane (CIBDM), cyclohexyl-n-hexyldimethoxysilane (CHDM), cyclohexyl-n-octyldimethoxysilane (CODM), cyclohexyl-n-decyldimethoxysilane (CDeDM), dimethyldimethoxysilane, dimethyldiethoxysilane, and the like. and any one or more compounds selected from the group consisting of silane, dicyclopentyldimethoxysilane, diisopropyldimethoxysilane, dicyclopentyldimethoxysilane, methylphenyldimethoxysilane, diphenyldiethoxysilane, methyltrimethoxysilane, ethyltrimethoxysilane, vinyltrimethoxysilane, phenyltrimethoxysilane, methyltriethoxysilane, ethyltriethoxysilane, vinyltriethoxysilane, phenyltriethoxysilane, butyltriethoxysilane, ethyltriisopropoxysilane, vinyltributoxysilane, and methyltriaryloxysilane. Representative examples of the compound of the above chemical formula (1) may include any one or more compounds selected from the group consisting of dimethyldimethoxysilane, dimethyldiethoxysilane, dicyclopentyldimethoxysilane, cyclohexylmethyldimethoxysilane, diisopropyldimethoxysilane, dicyclopentyldimethoxysilane, methylphenyldimethoxysilane, diphenyldiethoxysilane, methyltrimethoxysilane, ethyltrimethoxysilane, vinyltrimethoxysilane, phenyltrimethoxysilane, methyltriethoxysilane, ethyltriethoxysilane, vinyltriethoxysilane, phenyltriethoxysilane, butyltriethoxysilane, ethyltriisopropoxysilane, vinyltributoxysilane, and methyltriaryloxysilane.
[0051] Representative examples of the compound of the chemical formula (2) include 1,1,3,3-tetramethoxy-1,3-dimethyl-1,3-disilanepropane (TMDMDP), 1,1,3,3-tetramethoxy-1-methyl-3-hexyl-1,3-disilanepropane (TMMHDP), 1,1,3,3-tetramethoxy-1,3-di-n-hexyl-1,3-disilanepropane (TMDHDP), 1,1,3,3-tetramethoxy-1-methyl-3-cyclohexyl-1,3-disilanepropane (TMDHDP), Examples of the compound include one or more compounds selected from the group consisting of 1,1,3,3-tetramethoxy-1,3-dicyclohexyl-1,3-disilanepropane (TMMCDP), 1,1,3,3-tetramethoxy-1,3-dicyclohexyl-1,3-disilanepropane (TMDCDP), 1,1,8,8-tetramethoxy-1,8-dicyclohexyl-1,8-disilaneoctane (TMDCDO) and 1,1,3,3-tetramethoxy-1,3-dimethyldisiloxane (TMDMDS).
[0052] Representative examples of the compound of the chemical formula (3) include one or more compounds selected from the group consisting of methyl(trimethylsilylmethyl)dimethoxysilane (MTDM), n-propyl(trimethylsilylmethyl)dimethoxysilane (PTDM), i-propyl(trimethylsilylmethyl)dimethoxysilane (IPTDM), n-butyl(trimethylsilylmethyl)dimethoxysilane (BTDM), i-butyl(trimethylsilylmethyl)dimethoxysilane (IBTDM), n-pentyl(trimethylsilylmethyl)dimethoxysilane (PnTDM), n-hexyl-(trimethylsilylmethyl)dimethoxysilane (HTDM), cyclopentyl(trimethylsilylmethyl)dimethoxysilane (CpTDM) and cyclohexyl(trimethylsilylmethyl)dimethoxysilane (CTDM).
[0053] In step (a), the co-catalyst (z) is preferably added in an amount of 0.5 to 40 moles per mole of the main catalyst (y), but is not limited thereto. More specifically, it is preferable that the co-catalyst Si, which is a silicon compound, is contained in an amount of 0.5 to 40 moles per mole of Ti in the main catalyst, which is a titanium compound, and it is even more preferable that the co-catalyst Si, which is a silicon compound, is contained in an amount of 1 to 40 moles per mole of Ti in the main catalyst, which is a titanium compound. In addition, it is even more preferable that the co-catalyst Si, which is a silicon compound, is contained in an amount of 1 to 30 moles per mole of Ti in the main catalyst, which is a titanium compound. For example, if the amount of Si in the silicon compound co-catalyst (z) is less than 1 mole per mole of Ti in the titanium compound main catalyst (y), the rapid reaction rate of ethylene in the first polymerization reaction will cause rapid and non-uniform particle growth to block the catalytic active sites, and sufficient polypropylene reaction will not occur in the second polymerization reaction. Conversely, if the amount of Si in the silicon compound co-catalyst exceeds 40 moles per mole of Ti in the titanium compound main catalyst (y), the oxygen atoms contained in the co-catalyst structure will act as a catalyst poison, causing a rapid decrease in activity, and a low degree of polymerization will prevent the production of ultra-high molecular weight polypropylene resin. Even if a polymerization reaction does occur, problems may occur in which it is not possible to sufficiently obtain an (ultra)high molecular weight polyethylene block copolymer having uniform kneadability and improved physical properties.
[0054] In the first-stage polymerization reaction of step (b), the ethylene monomer is preferably introduced in an amount of 3 to 95% by weight, but is not limited thereto. For example, when the ethylene monomer is introduced in an amount of less than 3% by weight, the ethylene content is low during the production of the block copolymer, and sufficient polymerization degree is not ensured, and high molecular weight polyethylene is not polymerized. Conversely, when the ethylene monomer is introduced in an amount of more than 95% by weight, it becomes difficult to adjust the composition of the copolymer as a target during the production of the block copolymer, and activity sufficient for the polypropylene reaction to proceed in two stages cannot be ensured, and copolymer resin cannot be obtained.
[0055] On the other hand, in step (b), only ethylene monomer is added to the mixed solution, or ethylene monomer and a very small amount of hydrogen are added, and the polymerization temperature for the first-stage polymerization reaction is preferably within the range of 30 to 90° C., but is not limited thereto. If the polymerization temperature for the polymerization reaction is less than 30° C., a problem may occur that the polymerization reaction does not occur sufficiently. Conversely, if the polymerization temperature for the polymerization reaction is more than 90° C., even if the polymerization reaction occurs, the generated resin will suddenly block the catalytic active sites due to the rapid reaction rate, making it difficult to adjust the composition of the target copolymer, and sufficient activity for the second-stage polymerization cannot be ensured.
[0056] In step (b), the polymerization pressure for carrying out the first-stage polymerization reaction is preferably within the range of 1 to 40 bar, but is not limited thereto. If the polymerization pressure for carrying out the polymerization reaction is less than 1 bar, the polymerization reaction may not proceed sufficiently. Conversely, if the polymerization pressure for carrying out the polymerization reaction exceeds 40 bar, even if the polymerization reaction does proceed, the generated resin will suddenly block the catalytic active sites due to the rapid reaction rate, making it difficult to adjust the composition of the target copolymer, and sufficient activity for the second-stage polymerization cannot be ensured.
[0057] In addition, in the first-stage polymerization reaction of step (b), ethylene monomer is added to the mixed solution, and a molecular weight regulator, hydrogen (H2), is added in a very small amount or not at all, thereby controlling the molecular weight range of the target ultra-high molecular weight polyethylene polymer. In this case, the content of hydrogen added to the first-stage polymerization reaction may be within the range of 0.001 to 500 mL under the reactor condition of 1 atmosphere, or may be supplied at a pressure of 0.001 to 0.5 bar, or the hydrogen molar content range compared to the olefin monomer may be 0.1 to 50 vol%, but is not limited thereto.
[0058] Step (c) corresponds to a process of removing unreacted monomer remaining in the reactor after the first polymerization reaction. Here, the unreacted monomer is preferably ethylene monomer, and if propylene monomer is added first instead of ethylene monomer in step (b), the unreacted monomer may be propylene monomer. In order to effectively remove the unreacted monomer, a vacuum pump can be used, but since the hexane in the reactor may be vaporized and removed, the degree of vacuum is limited to 30 torr, or the internal temperature of the reactor is maintained at 60 degrees or more, and the reactor is filled with nitrogen up to 2 bar and completely discharged to the atmosphere, and this method is repeated three or more times.
[0059] In the second polymerization reaction of step (d), the propylene monomer is preferably added in an amount of 6 to 98% by weight of the total monomers added, but is not limited thereto. For example, if the propylene monomer is added in an amount of less than 6% by weight, the propylene content is low during the preparation of the block copolymer, and the melting point of the block copolymer cannot reach 160°C or more, which corresponds to polypropylene, when the melting point is confirmed. Conversely, if the propylene monomer is added in an amount of more than 98% by weight, it becomes difficult to adjust the composition of the copolymer as a target during the preparation of the block copolymer, and a problem of reduced performance of the separator may occur during the preparation of a separator for a secondary battery using the copolymer as a raw material.
[0060] Meanwhile, in step (d), the polymerization temperature for adding propylene monomer to the mixed solution and carrying out the second-stage polymerization reaction is preferably within the range of 30 to 90° C., but is not limited thereto. If the polymerization temperature for carrying out the polymerization reaction is less than 30° C., a problem may occur that the polymerization reaction does not proceed sufficiently. Conversely, if the polymerization temperature for carrying out the polymerization reaction exceeds 90° C., even if the polymerization reaction proceeds, polypropylene with low stereoregularity is polymerized and dissolved in hexane, or the polymerization activity is rapidly reduced, making it difficult to adjust the composition of the target copolymer, and a problem may occur that the performance of the separator is reduced when the copolymer is used as a raw material for manufacturing a secondary battery separator.
[0061] In step (d), the polymerization pressure for adding propylene monomer to the mixed solution and carrying out the second-stage polymerization reaction is preferably within the range of 1 to 40 bar, but is not limited thereto. If the polymerization pressure for carrying out the polymerization reaction is less than 1 bar, a problem may occur in which the polymerization reaction does not proceed sufficiently, and conversely, if the polymerization pressure for carrying out the polymerization reaction exceeds 40 bar, even if the polymerization reaction proceeds, it becomes difficult to adjust the composition of the target copolymer, and a problem may occur in which the performance of the separator is reduced during the production of a secondary battery separator using the copolymer as a raw material.
[0062] In addition, when propylene monomer is added to the mixed solution in the second polymerization reaction of step (d) and hydrogen (H2), which is a molecular weight regulator, is added, ultra-high molecular weight polypropylene cannot be polymerized. In this case, the ratio of the main catalyst, cocatalyst, and promoter to adjust the molecular weight range can be adjusted to adjust the molecular weight range of the target ultra-high molecular weight polypropylene polymer and the molecular weight range of the final ultra-high molecular weight polyethylene block copolymer.
[0063] Meanwhile, the polymerization reaction in steps (b) and (d) may be performed in liquid, slurry, bulk phase, or gas phase polymerization, but is not limited thereto. Preferably, steps (b) and (d) are performed in a suspension polymerization reactor (autoclave), and may be performed in two or more consecutive reactors. In this case, the operating conditions of each reactor may be the same or different to adjust the physical properties of the polymer.
[0064] Step (e) is a step of filtering and drying a powder of a polyethylene block copolymer from the reaction solution obtained in step (d). More specifically, the (ultra) high molecular weight polyethylene block copolymer produced is mixed with a polar organic solvent, and separated, purified and dried using distilled water (y) or filtered water (y').
[0065] In this case, the mixing ratio of the (ultra) high molecular weight polyethylene block copolymer and the polar organic solvent may be 0.1 to 10 times the weight of the block copolymer, and preferably 0.5 to 3 times the weight of the block copolymer.
[0066] That is, it is preferable to mix 10 to 1,000 parts by weight of a polar organic solvent with 100 parts by weight of the produced block copolymer, and it is more preferable to mix 50 to 300 parts by weight of a polar organic solvent with 100 parts by weight of the produced block copolymer.
[0067] In this case, the polar organic solvent may be a compound represented by the following formula (4): R-OH····Chemical formula (4) HO-R1-R2-OH·····Chemical formula (5)
[0068] In the chemical formula (4), R is a linear or branched alkyl group having 1 to 12 carbon atoms. Specifically, representative examples of the compound corresponding to the chemical formula (4) may include one or more compounds selected from the group consisting of linear alkalis such as methanol, ethanol, propanol, butanol, pentanol, hexanol, heptanol, octanol, nonanol, decanol, undecanol, and dodecanol, and branched alkyl groups such as isopropanol, isobutanol, and isopentanol.
[0069] In the chemical formula (5), R1 and R2 are linear alkyl groups having 0 to 6 carbon atoms. Specifically, representative examples of the compound corresponding to the chemical formula (5) may include one or more compounds selected from the group consisting of methanediol, ethanediol, propanediol, butanediol, pentanediol, hexanediol, heptanediol, octanediol, nonanediol, decanediol, undecanediol, and dodecanediol.
[0070] The water used to separate the polar organic solvent in which the catalyst residue has been dissolved from the produced block copolymer may be distilled water or filtered water, and may be used in an amount 1 to 30 times, preferably 5 to 20 times, the weight of the polar organic solvent used.
[0071] That is, it is preferable to use 100 to 3000 parts by weight of distilled water or filtered water per 100 parts by weight of the polar organic solvent, and more preferably to use 500 to 2000 parts by weight of distilled water or filtered water per 100 parts by weight of the polar organic solvent. The mixture of the produced block copolymer and the polar organic solvent is contacted with water and then separated into layers, where the molecular polar organic solvent is mixed in the water layer, and the produced block copolymer floats on the upper layer of the water. After separating this using filter paper or a filter, it is dried in a dryer at 90 to 105 ° C. to obtain a (ultra) high molecular weight polyethylene-based block copolymer from which inorganic substances such as magnesium, titanium, aluminum, and silicon used as catalysts in the polymerization process have been removed.
[0072] (Ultra)high molecular weight polyethylene block copolymers Meanwhile, the present specification further discloses a (ultra) high molecular weight polyethylene-based block copolymer produced by the method for producing a (ultra) high molecular weight polyethylene-based block copolymer of the present invention.
[0073] In the (ultra) high molecular weight polyethylene-based block copolymer of the present invention, the content of the (ultra) high molecular weight polyethylene is 5 to 95% by weight, and the content of the ultra-high molecular weight polyethylene is preferably 5 to 95% by weight, but is not limited thereto.
[0074] In the (ultra) high molecular weight polyethylene block copolymer of the present invention, the viscosity average molecular weight of the (ultra) high molecular weight polyethylene is preferably 400,000 to 5,000,000 g / mol, and more preferably 800,000 to 4,000,000 g / mol.
[0075] In the (ultra) high molecular weight polyethylene block copolymer of the present invention, the viscosity average molecular weight of the ultra high molecular weight polyethylene is preferably 1,000,000 to 4,000,000 g / mol, and more preferably 1,200,000 to 3,000,000 g / mol.
[0076] Furthermore, the (ultra)high molecular weight polyethylene block copolymer of the present invention may have a viscosity average molecular weight of 400,000 to 5,000,000 g / mol, more preferably a viscosity average molecular weight of 900,000 to 4,000,000 g / mol, under conditions in which no hydrogen is added or a very small amount is added, preferably under conditions in which no hydrogen is added.
[0077] In addition, the (ultra) high molecular weight polyethylene block copolymer of the present invention can be produced by carrying out a first-stage polymerization reaction in which only ethylene monomer is added to a mixed solution, or by carrying out a first-stage polymerization reaction in which ethylene monomer and a trace amount of hydrogen are added to the mixed solution, and then carrying out a second-stage polymerization reaction in which propylene monomer is added to the mixed solution, thereby making it possible for the (ultra) high molecular weight polyethylene to be a one-stage polymer with a linear structure.
[0078] In addition, the (ultra) high molecular weight polyethylene block copolymer of the present invention can maintain the inorganic matter content at a level of 30 ppm or less by undergoing the catalyst residue removal process as described above. More specifically, the inorganic matter content of the (ultra) high molecular weight polyethylene block copolymer of the present invention is preferably 1 to 30 ppm, and more preferably 5 to 20 ppm.
[0079] In addition, the (ultra) high molecular weight polyethylene block copolymer of the present invention can maintain a particle size of 400 μm or less by adjusting the catalyst particle size and polymerization degree as described above. More specifically, the particle size of the (ultra) high molecular weight polyethylene block copolymer of the present invention is preferably 10 to 400 μm, and more preferably 50 to 300 μm.
[0080] In addition, the (ultra)high molecular weight polyethylene block copolymer of the present invention has an apparent density of 0.30 to 0.50 g / cm 3 is preferred, but is not limited to this.
[0081] Secondary battery separators made from (ultra)high molecular weight polyethylene block copolymers In addition, the (ultra) high molecular weight polyethylene-based block copolymer according to the present invention has increased kneadability compared to conventional copolymers of polyethylene and polypropylene, and therefore a separator for a secondary battery having excellent performance can be produced using the block copolymer according to the present invention as a raw material.
[0082] The secondary battery separator produced from the (ultra) high molecular weight polyethylene block copolymer according to the present invention preferably has a puncture strength of 300 to 600 gf, but is not limited thereto.
[0083] In addition, the secondary battery separator manufactured using the (ultra) high molecular weight polyethylene block copolymer according to the present invention as a raw material has a tensile strength of 800 to 2,000 kgf / cm 2 is preferred, but is not limited to this.
[0084] In addition, the secondary battery separator manufactured using the (ultra) high molecular weight polyethylene-based block copolymer according to the present invention as a raw material preferably has a tensile elongation (Elong) of 25 to 90%, but is not limited thereto. EXAMPLES
[0085] The claims of this specification will be described in more detail with reference to the accompanying drawings and examples. However, the drawings and examples presented in this specification can be modified in various ways by ordinary skilled artisans to have various forms, and the description of this specification should not be construed as limiting the present invention to the specific disclosed form, but should be considered as including all equivalents or alternatives within the spirit and technical scope of the present invention. The accompanying drawings are presented to help ordinary skilled artisans to more accurately understand the present invention, and may be exaggerated or reduced in size.
[0086] {Examples and Evaluation} Example 1 A 2L stainless steel reactor equipped with a stirrer is evacuated at room temperature, and 900mL of hexane is poured in as an organic solvent, followed by stirring. 900mg of triethylaluminum as a cocatalyst and 90mg of dicyclopentyldimethoxysilane as a promoter are added at room temperature, and 30mg of titanium compound catalyst is added as a main catalyst. The reactor is then placed in a thermostatic bath maintained at 70℃ and heated to 60℃. a. First stage polymerization After feeding 200 mL of hydrogen as a molecular weight regulator, gaseous ethylene monomer is fed at a rate of 1,050 mL / min using a mass flow meter for 85 minutes to polymerize at 70°C. b. Removing unreacted ethylene monomer. c. After removing the unreacted ethylene monomer, gas-phase propylene monomer is introduced at a rate of 500 mL / min for 120 minutes using a mass flow meter without hydrogen input, and polymerized at 70°C. After the reaction is completed, the unreacted propylene monomer is removed, the reactor is opened, and the organic solvent and polymerized resin are filtered and separated, and then the resin is dried in a dryer to obtain an (ultra)high molecular weight polyethylene block copolymer resin.
[0087] Example 2 The same procedure was carried out as in Example 1, except that after 100 mL of hydrogen gas was fed during the first-stage polymerization (a), the feed rate of gas-phase ethylene was adjusted to 500 mL / min, and the feed rate of gas-phase propylene in the second-stage polymerization (c) was adjusted to 750 mL / min.
[0088] Example 3 The same procedures as in Example 1 were carried out, except that in the first-stage polymerization of a., 300 mL of hydrogen gas was introduced, and then, the amount of gas-phase ethylene introduced was 1,100 mL / min for 120 minutes, and in the second-stage polymerization of c., the amount of gas-phase propylene introduced was 500 mL / min for 60 minutes.
[0089] Example 4 The same procedure as in Example 1 was repeated, except that a. 20 mL of hydrogen gas was fed during the first-stage polymerization, and then gas-phase ethylene was fed at 300 mL / min for 30 minutes, and c. the gas-phase propylene was fed at 730 mL / min for 150 minutes in the second-stage polymerization.
[0090] Example 5 The same procedures as in Example 1 were carried out, except that in the first-stage polymerization of a., 380 mL of hydrogen gas was fed, and then the amount of gas-phase ethylene fed was 1,400 mL / min for 120 minutes, and in the second-stage polymerization of c., the amount of gas-phase propylene fed was 200 mL / min for 30 minutes.
[0091] Example 6 The same procedure as in Example 1 was repeated, except that no hydrogen was added during the first stage of polymerization.
[0092] Example 7 The same procedure as in Example 1 was repeated, except that a. hydrogen was not fed during the first-stage polymerization and the reaction temperature of the second-stage polymerization was adjusted to 55°C.
[0093] Example 8 The same procedure was carried out as in Example 1, except that after the preparation steps for polymerization, a. the gas-phase ethylene for the first-stage polymerization was fed at 700 mL / min for 60 minutes, and c. the gas-phase propylene for the second-stage polymerization was fed at 500 mL / min for 60 minutes, and then the first and second stages of polymerization were repeated again to perform four-stage polymerization.
[0094] Example 9 The same procedure was carried out as in Example 1, except that the amount of the cocatalyst was reduced from 900 mg to 300 mg and the amount of the promoter was reduced from 90 mg to 30 mg.
[0095] Example 10 The same procedure was carried out as in Example 1, except that the amount of cocatalyst was reduced from 900 mg to 300 mg.
[0096] Example 11 The same procedure as in Example 6 was repeated, except that the polymerization temperature in the first and second stages was lowered from 70°C to 30°C.
[0097] Comparative Example 1 VH035 (viscosity average molecular weight: 400,000) and UHMWPP (viscosity average molecular weight: 1.5 million) manufactured by Daehan Petrochemical Co., Ltd. were mixed at a ratio of 50:50.
[0098] Comparative Example 2 U015 (viscosity average molecular weight: 1.5 million) and UHMWPP (viscosity average molecular weight: 1.5 million) manufactured by Daehan Petrochemical Co., Ltd. were mixed at a ratio of 50:50.
[0099] Comparative Example 3 VH100U (viscosity average molecular weight 1,000,000) and UHMWPP (viscosity average molecular weight 1,500,000) manufactured by Daehan Petrochemical Co., Ltd. were mixed at a ratio of 45:55.
[0100] Comparative Example 4 VH100U (viscosity average molecular weight 1 million) and UHMWPP (viscosity average molecular weight 1.5 million) manufactured by Daehan Petrochemical Co., Ltd. were mixed at a ratio of 40:60.
[0101] Comparative Example 5 The same procedure was carried out as in Example 1, except that the amount of the cocatalyst was reduced from 900 mg to 10 mg, and the amount of the promoter was reduced from 90 mg to 30 mg.
[0102] Comparative Example 6 The same procedure was carried out as in Example 1, except that the amount of cocatalyst was increased from 900 mg to 1,730 mg.
[0103] Comparative Example 7 The same procedure as in Example 1 was repeated, except that the amount of the promoter was reduced from 90 mg to 3 mg.
[0104] Comparative Example 8 The same procedure as in Example 1 was repeated, except that the amount of the promoter was increased from 90 mg to 130 mg.
[0105] Measurement method for physical properties of (ultra)high molecular weight polyethylene block copolymers (1) Viscosity average molecular weight (Mv): The viscosity average molecular weight was measured by obtaining the intrinsic viscosity according to the intrinsic viscosity measurement method defined by ASTM D5020 and ISO 1628-3, and the value was calculated by the Margolies Equation. Mv = 5.37 × 10 4 ×[η] 1.49 η: Intrinsic viscosity
[0106] (2) Polyethylene / polypropylene content: NMRC 13 The values analyzed in were integrated and expressed.
[0107] (3) Apparent density (g / cm 3 ): After removing moisture from the block copolymer resin powder, the apparent density was measured using a dry automatic density meter (AccuPycII 1340TC-10CC; Shimadzu Corporation; carrier gas; helium). The measurement was repeated until the measured values were equal five or more times in a row.
[0108] Measurement method for the physical properties of secondary battery separators (1) Piercing strength (gf): A piercing test was performed using a Kato Tech KES-G5 handy compression tester with a needle tip curvature radius of 0.5 mm and a piercing speed of 2 mm / sec. The maximum piercing load was taken as the piercing strength. The sample was fixed in a metal frame (sample holder) with a hole of 11.3 mm in diameter, together with a rubber gasket made of ricone.
[0109] (2) Tensile strength (kgf / cm 2): The tensile strength of the secondary battery separator is measured according to ASTM D882 (1997). An Instron-type tensile tester is used under the following conditions. The average value of five measurements is taken as the tensile strength in the present invention. The test specimen for measuring the tensile strength was cut from the secondary battery separator into a rectangle measuring 10 mm in the length direction and 50 mm in the width direction. The tensile speed was 100 mm / min, and the measurement environment was a temperature of 23°C and a humidity of 65% RH.
[0110] (3) Tensile elongation (Elong.%): A 1 / 2 JIS K7113 No. 2 test piece stamped from a 1 mm thick press sheet was used as the evaluation sample, and the measurement was performed at a tensile speed of 30 mm / min in an atmosphere of 23°C. Shimadzu AGS-50G was used for the measurement.
[0111] Measurement results of physical properties of (ultra)high molecular weight polyethylene block copolymer The polyethylene and polypropylene contents in the block copolymers prepared in Examples 1 to 11 and Comparative Examples 1 to 8, the viscosity average molecular weights after the first to fourth polymerization stages, and the properties of the secondary battery separators were evaluated and are shown in Table 1 below.
[0112] [Table 1]
[0113] Referring to Table 1, the characteristics of the separator for secondary batteries according to the content and molecular weight of polyethylene and polypropylene in the ultra-high molecular weight polyethylene-based block copolymer according to one embodiment of the present invention can be seen, and the physical properties and surface improvement can be seen compared to the comparative example of a simply mixed heterogeneous composite resin.
[0114] The (ultra)high molecular weight polyethylene block copolymers of the present invention according to Examples 1 to 11 contain 10 to 500 moles of Al as a co-catalyst which is an alkylaluminum compound and 1 to 40 moles of Si as a promoter which is a silicon compound per mole of Ti as a main catalyst which is a titanium compound, and can be confirmed to have a viscosity average molecular weight of 400,000 to 5,000,000 g / mol under the conditions where a trace amount of hydrogen (H2) as a molecular weight regulator is added or not added.
[0115] Furthermore, from Examples 6 and 11, it can be confirmed that when the (ultra) high molecular weight polyethylene-based block copolymer of the present invention is produced, when the polymerization temperature is 30 to 90°C, it is possible to produce an (ultra) high molecular weight polyethylene-based block copolymer having a viscosity average molecular weight of 400,000 to 5,000,000 g / mol.
[0116] In addition, the (ultra)high molecular weight polyethylene block copolymers of the present invention according to Examples 1 to 11 have an apparent density of 0.30 to 0.50 g / cm 3 It can be confirmed that it is.
[0117] On the other hand, the polyethylene and polypropylene block copolymers of Comparative Examples 5 to 8 all had an apparent density of 0.30 g / cm 3 It can be confirmed that it is less than.
[0118] Furthermore, it can be confirmed that the secondary battery separators prepared using the (ultra)high molecular weight polyethylene-based block copolymers of the present invention according to Examples 1 to 11 have improved mechanical properties, with a puncture strength of 300 to 600 gf, compared to the secondary battery separators prepared using the block copolymers according to Comparative Examples 1 to 4.
[0119] Meanwhile, it can be seen that the secondary battery separators manufactured using the polyethylene and polypropylene block copolymers according to Comparative Examples 1 to 4 all had a puncture strength of less than 300 gf.
[0120] In addition, the secondary battery separators produced using the (ultra)high molecular weight polyethylene-based block copolymers of the present invention according to Examples 1 to 10 as raw materials have a tensile strength of 800 to 2,000 kgf / cm 2 The tensile elongation (Elong) is 25 to 90%, which indicates that the secondary battery separators prepared using the block copolymers of Comparative Examples 1 to 4 have uniform mixing properties and improved physical properties.
[0121] Meanwhile, the secondary battery separators manufactured using the polyethylene and polypropylene block copolymers according to Comparative Examples 1 to 4 had a tensile strength and tensile elongation (Elong) of 600 kgf / cm 2 It can be confirmed that the ratio is less than 100 and less than 60%.
[0122] In particular, the secondary battery separator manufactured using the (ultra) high molecular weight polyethylene-based block copolymer of the present invention according to Example 8 as a raw material has a puncture strength of 559 gf and a tensile strength of 1,811 kgf / cm 2 The tensile elongation (Elong) was 81%, and it was found to have the best kneadability and improved physical properties as a separator for secondary batteries.
[0123] From this, it can be seen that compared to a second-stage polymerization in which ethylene monomer and propylene monomer are each added once and polymerized, a fourth-stage polymerization in which ethylene monomer and propylene monomer are each added once and then polymerized again with additional ethylene monomer and propylene monomer is performed, which improves the kneadability and mechanical properties of the produced block copolymer and the secondary battery separator produced using such a block copolymer as a raw material.
[0124] The (ultra) high molecular weight polyethylene block copolymer of the present invention can be used as a compatibilizer to increase the kneading property during mixing and processing of polyethylene and polypropylene, which have low compatibility, and has the effect of improving the kneading property, film surface and other physical properties compared to secondary battery separators made of heterogeneous composite materials of polyethylene and polypropylene, which are simply mixed and processed.
[0125] The above description is merely an illustrative example of the technical concept of the present invention, and various modifications and variations can be made by those having ordinary knowledge in the technical field to which the present invention pertains without departing from the essential characteristics of the present invention.
[0126] Therefore, the embodiments disclosed in the present invention are for illustration purposes only and are not intended to limit the technical idea of the present invention, and the scope of the technical idea of the present invention is not limited by such embodiments. The scope of protection of the present invention should be interpreted according to the following claims, and any technical idea within the scope equivalent thereto should be interpreted as being included in the scope of the present invention. [Industrial Applicability]
[0127] According to the present invention, it is possible to provide a secondary battery separator having improved kneadability, film surface and other physical properties compared to a secondary battery separator made of heterogeneous composite materials of polyethylene and polypropylene, which are simply mixed and processed, as well as by using a compatibilizer to increase kneadability during mixing and processing of polyethylene and polypropylene, which have low compatibility.
Claims
1. (a) mixing and charging a co-catalyst (x) which is an alkylaluminum compound, a main catalyst (y) which is a titanium compound, and a co-catalyst (z) which is a silicon compound in a reactor in the presence of a hydrocarbon solvent having 1 to 20 carbon atoms; (b) adding only ethylene monomer or adding ethylene monomer and a trace amount of hydrogen to the mixed solution obtained in the step (a) to carry out a first-stage polymerization reaction; (c) removing unreacted monomers from the reactor after the first-stage polymerization reaction; (d) adding propylene monomer to the mixed solution obtained in the step (c) to carry out a second-stage polymerization reaction; and (e) filtering and drying a powder of a polyethylene-polypropylene block copolymer from the reaction solution obtained in step (d).
2. 2. The method for producing a (ultra) high molecular weight polyethylene block copolymer according to claim 1, wherein the cocatalyst (x) is at least one compound selected from the group consisting of triethylaluminum, trimethylaluminum, triisobutylaluminum, trioctylaluminum, diethylaluminum chloride, diethylaluminum bromide, diethylaluminum iodide, diethylaluminum fluoride, ethylaluminum dichloride, dimethylaluminum chloride, methylaluminum dichloride, and ethylaluminum sesquichloride.
3. The cocatalyst (z) is selected from the group consisting of cyclohexylmethyldimethoxysilane (CMCD), cyclohexyl-n-propyldimethoxysilane (CPDM), cyclohexyl-i-propyldimethoxysilane (CIPDM), cyclohexyl-n-butyldimethoxysilane (CBDM), cyclohexyl-i-butyldimethoxysilane (CIBDM), cyclohexyl-n-hexyldimethoxysilane (CHDM), cyclohexyl-n-octyldimethoxysilane (CODM), cyclohexyl-n-decyldimethoxysilane (CDeDM), dimethyldimethoxysilane, dimethyldiethoxysilane, dicyclopentyldimethoxysilane, diisopropyl ...
1. A method for producing an (ultra) high molecular weight polyethylene block copolymer, characterized in that the block copolymer is one or more compounds selected from the group consisting of phenyldimethoxysilane, dicyclopentyldimethoxysilane, methylphenyldimethoxysilane, diphenyldiethoxysilane, methyltrimethoxysilane, ethyltrimethoxysilane, vinyltrimethoxysilane, phenyltrimethoxysilane, methyltriethoxysilane, ethyltriethoxysilane, vinyltriethoxysilane, phenyltriethoxysilane, butyltriethoxysilane, ethyltriisopropoxysilane, vinyltributoxysilane, and methyltriaryloxysilane.
4. The method for producing an (ultra)high molecular weight polyethylene block copolymer according to claim 1, characterized in that the co-catalyst (x) which is an alkylaluminum compound contains 10 to 500 moles of Al per mole of Ti in the main catalyst (y) which is a titanium compound.
5. The method for producing a (ultra)high molecular weight polyethylene block copolymer according to claim 1, characterized in that the co-catalyst (z) which is a silicon compound contains 1 to 40 moles of Si per mole of Ti in the main catalyst (y) which is a titanium compound.
6. The method for producing a (ultra)high molecular weight polyethylene block copolymer according to claim 1, characterized in that in the first and second polymerization stages, the polymerization temperature is 30 to 90°C.
7. The method for producing a (ultra) high molecular weight polyethylene block copolymer according to claim 1, characterized in that in the first and second polymerization stages, the polymerization pressure is 1 to 40 bar.
8. 2. The method for producing a (ultra)high molecular weight polyethylene block copolymer according to claim 1, wherein the ethylene monomer is added in an amount of 3 to 95% by weight in the first polymerization stage, and the propylene monomer is added in an amount of 6 to 98% by weight in the second polymerization stage.
9. In (ultra)high molecular weight polyethylene block copolymers, Relative to 100% by weight of the block copolymer, the block copolymer is composed of 25 to 90% by weight of (ultra) high molecular weight polyethylene; and 10 to 75% by weight of ultra high molecular weight polypropylene. The (ultra)high molecular weight polyethylene has a viscosity average molecular weight of 400,000 to 5,000,000 g / mol, and the ultra-high molecular weight polypropylene has a viscosity average molecular weight of 1,000,000 to 4,000,000 g / mol; The block copolymer is a (ultra) high molecular weight polyethylene block copolymer having a viscosity average molecular weight of 400,000 to 5,000,000 g / mol under conditions where no hydrogen is added or a very small amount of hydrogen is added.
10. The (ultra)high molecular weight polyethylene-based block copolymer according to claim 9, wherein the block copolymer is produced by carrying out a first-stage polymerization reaction in which only ethylene monomer is added to a mixed solution, or by carrying out a first-stage polymerization reaction in which ethylene monomer and a trace amount of hydrogen are added to the mixed solution, and then carrying out a second-stage polymerization reaction in which propylene monomer is added to the mixed solution, thereby having the (ultra)high molecular weight polyethylene as a first-stage polymer having a linear structure.
11. The block copolymer has an apparent density of 0.30 to 0.50 g / cm 3 The high molecular weight polyethylene block copolymer according to claim 9,
12. The block copolymer of (ultra) high molecular weight polyethylene according to claim 9, wherein the block copolymer has an inorganic content of 1 to 30 ppm, and the inorganic substance is used as a catalyst in a polymerization process.
13. The block copolymer based on (ultra) high molecular weight polyethylene according to claim 9, wherein the block copolymer has a particle size of 10 to 400 μm.
14. A secondary battery separator manufactured from an (ultra)high molecular weight polyethylene-based block copolymer, the (ultra)high molecular weight polyethylene-based block copolymer being composed of 25 to 90% by weight of (ultra)high molecular weight polyethylene and 10 to 75% by weight of ultra-high molecular weight polypropylene, relative to 100% by weight of the block copolymer, the (ultra)high molecular weight polyethylene having a viscosity average molecular weight of 400,000 to 5,000,000 g / mol, the ultra-high molecular weight polypropylene having a viscosity average molecular weight of 1,000,000 to 4,000,000 g / mol, and the block copolymer having a viscosity average molecular weight of 400,000 to 5,000,000 g / mol under conditions where no hydrogen or a very small amount of hydrogen is added.
15. The secondary battery separator according to claim 14, wherein the secondary battery separator has a puncture strength of 300 to 600 gf.
16. The secondary battery separator has a tensile strength of 800 to 2,000 kgf / cm 2 15. The secondary battery separator of claim 14,
Citation Information
Patent Citations
Olefin polymer and method for producing the same
JP2012087307A
Polypropylene resin composition containing ultra-high-molecular-weight propylene (CO)polymer
WO2020255873A1
Process for the polymerization of propylene
EP3157966B1
JPS478207B1
Preparation method of ultra high molecular weight polyethylene
KR101161752B1