Long-lasting water-repellent wave-transmitting paint and its manufacturing method and application

A long-life, water-repellent, wave-transparent coating for radomes addresses the issues of water resistance and electrical deterioration by using a specialized resin and filler formulation, ensuring structural integrity and prolonged underwater operation.

JP2024541702AActive Publication Date: 2024-11-08MARINE CHEM RES INST CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2024553744
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2021-12-06
Filing Date
2022-08-10
Publication Date
2024-11-08
Estimated Expiration
2042-08-10

AI Technical Summary

Technical Problem

Conventional radome coating technologies for underwater equipment suffer from low water resistance, rapid electrical performance deterioration, and short service life, leading to issues such as water absorption, leakage, and structural damage due to prolonged underwater operation.

Method used

A long-life, water-repellent, wave-transparent coating is developed using a formulation of low surface energy modified fluorocarbon resin, low dielectric fillers, pigments, and isocyanate curing agents, with specific ratios and surface treatments to enhance water repellency and electrical stability.

Benefits of technology

The coating maintains excellent electrical performance and water repellency, preventing water absorption and leakage, ensuring the radome's structural integrity and prolonged operation underwater.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024541702000001
    Figure 2024541702000001
  • Figure 2024541702000002
    Figure 2024541702000002
  • Figure 2024541702000003
    Figure 2024541702000003
Patent Text Reader

Abstract

The present invention provides a long-life water-repellent wave-transmitting paint and its manufacturing method and application. The long-life water-repellent wave-transmitting paint is made of component A and component B, component A is made of raw materials including low surface energy modified fluorocarbon resin, low dielectric filler, low dielectric pigment, wetting dispersant, leveling agent and organic solvent, and component B is an isocyanate curing agent component, the paint has excellent water repellency and dielectric performance, is easy to apply and maintain, can meet the protection requirements of radomes operating underwater for a long time, and reduces the risks of water absorption, leakage and structural damage of the radome body.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to the field of coating technology, and more particularly to a long-life water-repellent wave-transmitting coating material and its manufacturing method and application. [Background technology]

[0002] The marine exploration equipment plays an important role in the protection of marine rights and interests, the development of marine resources, early warning of marine disasters, and the strengthening of national defense, and is also an important indicator of the overall national strength of a country. The radome is an important component of the exploration system, and is used to ensure the normal operation of the internal radar system in all weather conditions and all seasons. Many radomes for underwater equipment use resin matrix composite materials, which have low water resistance and are affected by water pressure during long-term underwater operation, which further intensifies the risk of corrosive media such as seawater penetrating and penetrating the base material, seriously affecting the structural strength and electrical performance, and even causing water leakage of the radome body and damaging the radar system. Therefore, the underwater radome must be protected in combination with a wave-transmitting paint during use. Unlike the surface or above-water operating environment, the underwater radome is affected by the change in water depth and the osmotic pressure for a long time, and the protective coating is prone to problems such as water absorption and leakage.

[0003] In view of this, conventional radome coating technologies have problems such as low water resistance, rapid deterioration of electrical performance, and short service life, and it is necessary to develop a long-life water-repellent wave-transmitting paint for underwater radomes that can meet the protective requirements for long-term underwater operation of the radome, and has excellent electrical performance, water repellency, and water repellency stability, thereby reducing the risks of water absorption, leakage, and structural destruction of the radome body. Summary of the Invention

[0004] In order to solve the problems existing in the prior art, the present invention provides a long-life water-repellent wave-transmitting paint and its manufacturing method and application, which can meet the special demand of radomes operating underwater for a long period of time.

[0005] The long-life water-repellent wave-transmitting paint for underwater radomes of the present invention can meet the operational requirements of covering the entire area and period of an underwater radar system based on its excellent electrical performance, water repellency and water repellency stability.

[0006] One object of the present invention is to provide a long-lasting water-repellent wave-transmitting coating.

[0007] The long-life water-repellent wave-transmitting paint is made of component A and component B, The component A is produced from raw materials including a low surface energy modified fluorocarbon resin, a low dielectric filler, a low dielectric pigment, a wetting and dispersing agent, a leveling agent, and an organic solvent; The low surface energy modified fluorocarbon resin is 100 parts by weight, and the amounts of each component are in parts by weight: 100 parts by weight of low surface energy modified fluorocarbon resin, Low dielectric filler: 16 to 25 parts by weight, preferably 18 to 22 parts by weight, 1 to 3 parts by weight, preferably 2 to 3 parts by weight, of a low dielectric pigment; Wetting and dispersing agent: 0.8 to 1.5 parts by weight, preferably 1.0 to 1.5 parts by weight, Leveling agent: 0.5 to 1.5 parts by weight, preferably 0.8 to 1.2 parts by weight, Organic solvent A is 20 to 35 parts by weight, preferably 25 to 30 parts by weight, The component B is an isocyanate curing agent component, The molar ratio of --OH of component A to --NCO of component B is 1:(1.0 to 1.2), and preferably 1:(1.0 to 1.1).

[0008] The -OH in component A originates from the low surface energy modified fluorocarbon resin, and the -OH content is 0.8 mol / kg.

[0009] The low surface energy modified fluorocarbon resin in component A is WN-50713 resin manufactured by Marine Chemical Research Institute Co., Ltd., and its performance is shown in Table 1.

[0010] [Table 1]

[0011] The performance of the low surface energy modified fluorocarbon resin is as shown in Table 1. The performance of the low surface energy modified fluorocarbon resin is to support the water repellency of the coating film, where the water repellency includes the water repellency angle, the sliding angle and 14 days of submersion in water (49±2°C). By adding a filler to the low surface energy modified fluorocarbon resin base, it is possible to provide support for the wave transmission performance, where the wave transmission performance includes the dielectric constant and the tangent value of the loss angle. The resin and the filler have a mutual influence and a synergistic effect to achieve the object of the invention.

[0012] In a preferred embodiment of the present invention, The powder in component A contains two types, namely, a low dielectric filler and a low dielectric pigment. A low dielectric material is generally a material with a dielectric constant of less than 10 and a tangent value of the loss angle of less than 0.01. The low dielectric property contributes to reducing the dielectric constant and tangent value of the loss angle of the material.

[0013] The low dielectric filler is a mixture of nano boron nitride and silicone resin microspheres; Among them, the nano boron nitride is preferably in a sheet shape, and the silicone resin microspheres are preferably in a spherical shape. The particle size of the nano boron nitride is 50 nm to 100 nm. The silicone resin microspheres have a particle size of 6 μm to 8 μm.

[0014] In a preferred embodiment of the present invention, The mass ratio of the nano boron nitride to the silicone resin microspheres is (2-4):1, and preferably (2.8-3.2):1.

[0015] Boron nitride has a lamellar structure and silicone resin microbeads have a spherical structure; the two are mixed and blended with each other; different mixing ratios form different mixing relationships which directly affect its physical barrier ability; other ratios are likely to cause a decrease in the physical barrier effect and a decrease in the anti-penetration ability; an increase in the mass ratio of nano-boron nitride to silicone resin microspheres can improve the shielding and barrier effect against water; repeated experiments have shown that when the mass ratio is (2~4):1, the synergistic effect of the nano-sheet-shaped nano-boron nitride and the spherical silicone resin microspheres can be well embodied, and when the mass ratio is (2.8~3.2):1, the performance is even better.

[0016] Nano boron nitride and silicone microspheres have different dielectric properties, and by mixing them in an appropriate ratio, the dielectric properties of the material can be balanced.

[0017] In a preferred embodiment of the present invention, The nano-boron nitride is surface-coated with a surface-coating agent produced by mixing a polyisocyanate containing a perfluoroalkyl segment with an organic solvent B; The mass ratio of the polyisocyanate containing a perfluoroalkyl segment in the surface coating treatment agent is 5% to 15%.

[0018] Regarding the surface coating treatment of nano boron nitride, A surface coating treatment agent is prepared by mixing a polyisocyanate containing a perfluoroalkyl segment with an organic solvent B, in which the ratio of the polyisocyanate containing a perfluoroalkyl segment is 5 to 15%, and the rest is organic solvent B; The polyisocyanate containing perfluoroalkyl segments of the present invention is the polyisocyanate containing perfluoroalkyl segments in the patent application (patent number CN101143840A, the invention title is "Preparation and Application of Polyisocyanate Containing Perfluoroalkyl Segments").

[0019] The process includes the following steps: (1) Heat the surface coating agent to 40-45°C, fill with nitrogen, and keep the temperature for 10-15 minutes. (2) 1 to 3‰ of a dispersing agent is added dropwise. (3) Add nano boron nitride to the stirring treatment agent in several portions; (4) Heat to 60-65°C, fill with nitrogen and keep at that temperature for 3-4 hours. (5) The temperature is lowered to room temperature. (6) After suction filtration, it is dried in an oven at 80-85°C for 45-48 hours and then prepared for use. The dispersing aid is a commonly used dispersing aid in the art, preferably BYK163, BYK104s, BYK170, etc.

[0020] The present invention adopts a surface coating treatment method of nano boron nitride, and after treatment, the surface of nano boron nitride is hydrophobic, which is helpful in increasing the service life of the coating film.

[0021] In a preferred embodiment of the present invention, The low dielectric pigment is an organic powder, which is prepared according to color requirements, and is preferably at least one of Paliogen Black, Phthalocyanine Blue, and Phthalocyanine Green; and / or The wetting and dispersing agent is at least one of BYK163, BYK104s, BYK180, and / or The leveling agent is a silicone polyether copolymer, preferably at least one of BYK378, BYK390, and BYK388.

[0022] In a preferred embodiment of the present invention, The organic solvent A and the organic solvent B may be organic solvents commonly used in this field in the prior art, and are each independently selected from at least one of aromatic solvents, ester solvents, and ether ester solvents, and are preferably at least one of xylene, aromatic hydrocarbon compounds, butyl acetate, ethyl acetate, ethylene glycol ethyl ether acetate, and propylene glycol methyl ether acetate.

[0023] In a preferred embodiment of the present invention, The second component is a trimer of an aliphatic isocyanate, and is preferably at least one of N3375 and N3390 manufactured by Bayer.

[0024] Another object of the present invention is to A step of mixing the raw materials including the low surface energy modified fluorocarbon resin, the low dielectric filler, the low dielectric pigment, the wetting dispersant, and the organic solvent, grinding the mixture until the fineness is 20 μm to 30 μm, adding a leveling agent, stirring uniformly, and filtering to obtain the A component; and uniformly mixing the obtained components A and B in the molar ratio to obtain the long-life water-repellent wave-transmitting paint.

[0025] Yet another object of the present invention is to provide an application of long-life water-repellent wave-transmitting paint in underwater radomes.

[0026] The present invention specifically can adopt the following technical solutions.

[0027] Weigh out the various raw materials according to the amounts used above. The pigment filler is dried and prepared for use. The low surface energy modified fluorocarbon resin, low dielectric filler, low dielectric filler, wetting dispersant, and organic solvent are mixed, then added to a basket mill and ground until the fineness is 20-30 μm, and the material is discharged. After the material is discharged, a leveling agent is added, and the mixture is stirred and dispersed for 30 minutes at 2000 rpm, filtered through a 120 mesh filter, and the viscosity of the paint (paint-4 cups) is tested, weighed, and packaged. After the substances of component A are uniformly mixed, the weighed components A and B are uniformly mixed in a molar ratio of -OH:-NCO=1:(1.0-1.2) and allowed to stand for 20 minutes.

[0028] The method used for painting is spray painting or brush painting. The thickness of the dried film after one coating is controlled to 40μm to 60μm. Effect of the Invention

[0029] Compared with the prior art, the beneficial effects of the present invention are as follows:

[0030] The paint of the present invention is a long-life, water-repellent, wave-transmitting paint that is easy to apply and maintain, and can meet the protection requirements for a radome operating underwater for long periods of time, reducing the risks of water absorption, leakage, and structural destruction of the radome body.

[0031] The paint of the present invention uses a low surface energy modified fluorocarbon resin as a film-forming material, is applied using an air spray coating method, and dries and hardens at room temperature, solving the durability problems of conventional radome coating technology, such as hydrophilicity (a water film is formed on the surface), rapid deterioration of electrical performance, and short service life.

[0032] The coating of the present invention is spray applied to a composite substrate, and the performance characteristics of the coating are as follows: 1) The water contact angle is ≧120° when tested with an OCA20 contact angle meter (sitting drop method); 2) The sliding angle is ≦10° when tested with an OCA20 contact angle meter (sitting drop method). 3) The dielectric constant is ≦3.2 according to the vector network method (10 GHz); 4) The tangent value of the loss angle is ≦0.04 according to the vector network method (10 GHz); 5) After immersion in water for 14 days (49±2°C), the water repellency angle is ≧10° and the sliding angle is ≦15°.

[0033] The electrical performance of a radome for underwater equipment is rapidly reduced under the influence of a continuous water film on the surface. The present invention has excellent water repellency and dielectric performance, and after being submerged in water for 14 days, the water contact angle is still ≧1110° and the rolling angle is still ≦15°, so that the water droplets can roll freely on the surface of the coating film and do not form a continuous water film, which does not deteriorate the dielectric performance of the radome. At the same time, it prevents corrosive media from being conducted into the coating film, so as to ensure the protection requirements for the radome to operate underwater for a long period of time, and reduces the risks of water absorption, leakage, and structural damage of the radome body. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0034] The present invention will be specifically described below with reference to specific examples. It should be noted here that the following examples are used to further describe the present invention, and cannot be understood as limiting the protection scope of the present invention. Any non-essential improvements and adjustments made to the present invention by those skilled in the art based on the content of the present invention still belong to the protection scope of the present invention.

[0035] The raw materials used in the examples and comparative examples are all ordinary commercially available raw materials.

[0036] In the examples and comparative examples, all parts are by weight.

[0037] [Table 2]

[0038] The test instrument is a water contact angle meter OCA20 manufactured by LAUDA Scientific, Germany.

[0039] Example 1 Regarding the surface coating treatment of nano boron nitride, 1. Heat the surface coating agent (the mass ratio of polyisocyanate containing perfluoroalkyl segments is 5%, and the rest is xylene solvent) to 42°C, fill with nitrogen, and keep warm for 15 minutes. 2. Add 1.5‰ of BYK163 dispersant dropwise. 3. Add nano boron nitride to the stirring surface coating agent in several batches. 4. Heat to 65℃, fill with nitrogen and keep at that temperature for 4 hours. 5. Cool to room temperature. 6. After suction filtration, it is dried in an oven at 80℃ for 45 hours and then prepared for use. The first component is 100 parts by weight of low surface energy modified fluorocarbon resin, 14 parts by weight of nano boron nitride, 4.5 parts by weight of silicone resin microspheres, 2 parts by weight of Paliogen Black, 0.5 parts by weight of Phthalocyanine Blue, 0.5 parts by weight of Phthalocyanine Green, 1 part by weight of BYK163, 1 part by weight of BYK378, and 27 parts by weight of butyl acetate. The pigment filler was dried and prepared for use. The low surface energy modified fluorocarbon resin, low dielectric filler, low dielectric filler, wetting dispersant, and organic solvent were mixed, then added to a basket mill and ground until the fineness was 20-30 μm, and the material was discharged. After the material was discharged, a leveling agent was added, and the mixture was dispersed by stirring for 30 minutes at 2000 rpm, filtered through a 120 mesh filter, and the paint viscosity (paint-4 cups) was tested, weighed, and packaged.

[0040] The second component, N3375, is 20 parts by weight. The molar ratio is -OH:-NCO=1:1. According to the above-mentioned composition, the first and second components were mixed uniformly, left to stand for 20 minutes, and then spray-coated once to control the thickness of the dried coating to 50 μm. After drying, the performance was tested.

[0041] Example 2 Regarding the surface coating treatment of nano boron nitride, 1. Heat the surface coating treatment agent (the mass ratio of polyisocyanate containing perfluoroalkyl segments is 15%, and the rest is xylene solvent) to 45°C, fill with nitrogen, and keep warm for 10 minutes. Add 2-3‰ of BYK163 dispersant dropwise. 3. Add nano boron nitride to the stirring surface coating agent in several batches. 4. Heat to 60℃, fill with nitrogen and keep warm for 3 hours. 5. Cool to room temperature. 6. After suction filtration, it is dried in an oven at 85℃ for 48 hours and then prepared for use. The first component is 100 parts by weight of low surface energy modified fluorocarbon resin, 15 parts by weight of nano boron nitride, 4.8 parts by weight of silicone resin microspheres, 0.5 parts by weight of Paliogen Black, 1 part by weight of Phthalocyanine Blue, 0.5 parts by weight of Phthalocyanine Green, 1.2 parts by weight of BYK163, 0.8 parts by weight of BYK378, 15 parts by weight of butyl acetate, and 10 parts by weight of xylene. The manufacturing method of the A component is the same as that of Example 1. The second component N3390 is 22 parts by weight, The molar ratio is -OH:-NCO=1:1. According to the above-mentioned composition, the first and second components were mixed uniformly, left to stand for 20 minutes, and then spray-coated once to control the thickness of the dried coating to 50 μm. After drying, the performance was tested.

[0042] Example 3 Regarding the surface coating treatment of nano boron nitride, 1. Heat the surface coating agent (the mass ratio of polyisocyanate containing perfluoroalkyl segments is 10%, and the rest is butyl acetate solvent) to 42°C, fill with nitrogen, and keep warm for 15 minutes. 2. Add 1‰ of BYK104s dispersant dropwise. 3. Add nano boron nitride to the stirring treatment agent in several batches; 4. Heat to 65℃, fill with nitrogen and keep warm for 4 hours. 5. Cool to room temperature. 6. After suction filtration, it is dried in an oven at 80℃ for 45 hours and then prepared for use. The first component is 100 parts by weight of low surface energy modified fluorocarbon resin, 16 parts by weight of nano boron nitride, 5.7 parts by weight of silicone resin microspheres, 1 part by weight of Paliogen Black, 1 part by weight of Phthalocyanine Blue, 1 part by weight of Phthalocyanine Green, 1.5 parts by weight of BYK163, 1.2 parts by weight of BYK378, 20 parts by weight of butyl acetate, and 10 parts by weight of xylene. The manufacturing method of the A component is the same as that of Example 1. The second component N3390 is 24 parts by weight, The molar ratio is -OH:-NCO=1:1. According to the above-mentioned composition, the first and second components were mixed uniformly, left to stand for 20 minutes, and then spray-coated once to control the thickness of the dried coating to 50 μm. After drying, the performance was tested.

[0043] Comparative Example 1 Comparative Example 1 was distinguished from Example 1 in that the mass ratio of nano boron nitride to silicone resin microspheres was 1:1 compared to Example 1.

[0044] The surface coating treatment of nano boron nitride was the same as in Example 1. The first component is 100 parts by weight of low surface energy modified fluorocarbon resin, 10 parts by weight of nano boron nitride, 10 parts by weight of silicone resin microspheres, 2 parts by weight of Paliogen Black, 0.5 parts by weight of Phthalocyanine Blue, 0.5 parts by weight of Phthalocyanine Green, 1 part by weight of BYK163, 1 part by weight of BYK378, and 27 parts by weight of butyl acetate. The manufacturing method of the A component is the same as that of Example 1. The second component N3390 is 20 parts by weight, The molar ratio is -OH:-NCO=1:1. According to the above-mentioned composition, the first and second components were mixed uniformly, left to stand for 20 minutes, and then spray-coated once to control the thickness of the dried coating to 50 μm. After drying, the performance was tested.

[0045] Comparative Example 2 Comparative Example 2 is compared with Example 2.

[0046] Comparative Example 2 was distinguished from Example 2 primarily in that the nano boron nitride used was not surface coated and the fluorocarbon resin was commercially available GK570 fluorocarbon resin.

[0047] The other raw materials and amounts used in Comparative Example 2 were the same as those in Example 2. The production method of the components A and B in Comparative Example 2 and the ratio of the amounts of the components A and B used were all the same as in Example 2.

[0048] The A and B components were mixed uniformly according to the amounts used, left to stand for 20 minutes, and then spray-coated once to control the thickness of the dried coating to 50 μm. The performance was tested after drying.

[0049] Components A and B of Examples 1 to 3 and Comparative Examples 1 and 2 were mixed uniformly, left to stand for 20 minutes, and then spray-coated to a coating thickness of 50 μm. The performance is shown in Table 3 below.

[0050] [Table 3]

[0051] Table 3 shows the coating performance test results of Examples 1-3 and Comparative Examples 1-2. The coatings obtained in Examples 1-3 all passed the tests of water repellency angle, sliding angle, dielectric constant, and tangent value of loss angle. The water repellency angle item index requirement of the water repellency wave-transmitting paint after 14 days of submersion is 110° or more, while the water repellency angle of Comparative Example 1 after 14 days of submersion is 102.3°, which does not meet the item index requirement. Compared with Example 1, Comparative Example 1 has a mass ratio of nano boron nitride and silicone resin microspheres of 1:1, and after submersion, the coating water repellency (water repellency angle and sliding angle) is significantly reduced. The mass ratio of nano boron nitride and silicone resin microspheres is too low, the compounding ratio of sheet-shaped and spherical fillers is inappropriate, and the synergistic effect is poor, which shows that the penetration prevention effect of the coating is reduced, causing poor physical barrier performance.

[0052] Compared with Example 2, the water repellency (water repellency angle and sliding angle) of the coating film of Comparative Example 2 was significantly reduced. After the water immersion test, the water repellency angle was significantly reduced to 80.1°, failing to meet the index requirements, and the sliding angle test showed that it did not roll. This shows that the selection of low surface energy resin and the surface coating treatment of nano boron nitride play an important role in chemically blocking water vapor, and that the selection of low surface energy fluorocarbon resin and the chemical modification of the surface of the nano boron nitride filler both significantly improve the water repellency stability and strengthen the penetration prevention ability of the coating film.

[0053] Compared with Examples 1 to 3, the sliding angle after immersion for 14 days in water in Comparative Examples 1 and 2 increased significantly because the water-repellent stability of the coating film (chemical shielding action due to surface chemical modification + physical barrier action due to filler size synergy) changes to a different extent, making the surface of the coating film hydrophilic and showing a dynamic decrease in hydrophobicity, and the surface of the coating film is prone to water droplets and form a water film, reducing the wave transmittance, resulting in a greater effect due to the chemical and physical synergistic action.

[0054] The long-life water-repellent wave-transmitting paints prepared in Examples 1 to 3 have excellent water repellency and dielectric properties, and after being submerged in water for 14 days, the water contact angle is still ≧110°, the rolling angle is still ≦15°, the water droplets can roll freely on the surface of the coating film, and do not form a continuous water film, so as to not deteriorate the dielectric performance of the radome, and at the same time avoid the corrosive medium from being conducted into the inside of the coating film, so as to ensure the protection requirements of the radome when it operates for a long time underwater, and reduce the risks of water absorption, leakage, structural damage, etc. of the radome body. ...

Claims

1. It is manufactured from component A and component B, The component A is produced from raw materials including a low surface energy modified fluorocarbon resin, a low dielectric filler, a low dielectric pigment, a wetting and dispersing agent, a leveling agent, and an organic solvent; The low surface energy modified fluorocarbon resin is 100 parts by weight, and the amounts of each component are in parts by weight: 100 parts by weight of low surface energy modified fluorocarbon resin, Low dielectric filler: 16 to 25 parts by weight, Low dielectric pigment 1 to 3 parts by weight, Wetting and dispersing agent: 0.8 to 1.5 parts by weight, Leveling agent: 0.5 to 1.5 parts by weight, Organic solvent A is 20 to 35 parts by weight, The component B is an isocyanate curing agent component, The molar ratio of —OH of component A to —NCO of component B is 1:(1.0 to 1.2); A long-lasting water-repellent wave-transmitting paint.

2. The component A is 100 parts by weight of a low surface energy modified fluorocarbon resin, and each component is, by weight, 100 parts by weight of low surface energy modified fluorocarbon resin, Low dielectric filler: 18 to 22 parts by weight, Low dielectric pigment 2 to 3 parts by weight, Wetting and dispersing agent 1.0 to 1.5 parts by weight, Leveling agent: 0.8 to 1.2 parts by weight, Organic solvent A is 25 to 30 parts by weight, The molar ratio of —OH of component A to —NCO of component B is 1:(1.0 to 1.1); 2. The long-life water-repellent wave-transmitting paint according to claim 1.

3. The low dielectric filler is a mixture of nano boron nitride and silicone resin microspheres; The particle size of the nano boron nitride is 50 nm to 100 nm. The particle size of the silicone resin microspheres is 6 μm to 8 μm.

2. The long-life water-repellent wave-transmitting paint according to claim 1.

4. The mass ratio of nano boron nitride to silicone resin microspheres is (2-4):1, preferably (2.8-3.2):1; 4. A long-life water-repellent wave-transmitting paint according to claim 3.

5. The nano-boron nitride is surface-coated with a surface-coating agent produced by mixing a polyisocyanate containing a perfluoroalkyl segment with an organic solvent B; The mass ratio of the polyisocyanate containing a perfluoroalkyl segment in the surface coating treatment agent is 5% to 15%.

4. A long-life water-repellent wave-transmitting paint according to claim 3.

6. The low dielectric pigment is at least one of Paliogen Black, Phthalocyanine Blue, and Phthalocyanine Green; and / or The leveling agent is a silicone polyether copolymer.

2. The long-life water-repellent wave-transmitting paint according to claim 1.

7. The organic solvent A and the organic solvent B are each independently selected from at least one of aromatic solvents, ester solvents, and ether ester solvents, and are preferably at least one of xylene, aromatic hydrocarbon compounds, butyl acetate, ethyl acetate, ethylene glycol ethyl ether acetate, and propylene glycol methyl ether acetate.

6. A long-life water-repellent wave-transmitting paint according to claim 5.

8. The component B is a trimer of an aliphatic isocyanate.

2. The long-life water-repellent wave-transmitting paint according to claim 1.

9. A method for producing a long-life water-repellent wave-transmitting paint according to any one of claims 1 to 8, comprising the steps of: A step of mixing the raw materials including the low surface energy modified fluorocarbon resin, the low dielectric filler, the low dielectric pigment, the wetting dispersant, and the organic solvent, grinding the mixture until the fineness is 20 μm to 30 μm, adding a leveling agent, stirring uniformly, and filtering to obtain component A; The step of uniformly mixing the obtained component A and component B in the molar ratio to obtain the long-life water-repellent wave-transmitting paint includes: A method for producing a long-life water-repellent wave-transmitting paint according to any one of claims 1 to 8.

10. 10. Application of the long-life water-repellent wave-transmitting paint according to any one of claims 1 to 8 or the long-life water-repellent wave-transmitting paint produced by the method according to claim 9 to an underwater radome.

Citation Information

Patent Citations

  • Method for performing anticorrosive hydrophobic modification on surface of aluminum alloy

    CN101885934A

  • Titanate coupling agent modified pollution-flashover-preventing fluorocarbon paint and preparation method thereof

    CN103242718A

  • High-power-density microwave radiation resistant coating for radome and preparation method of high-power-density microwave radiation resistant coating

    CN104789085A

  • Composition for coating

    JP1994016992A

  • Electronic telecommunications articles comprising crosslinked fluoropolmyers and methods

    WO2021091864A1