Method for producing iridium oxide
A method for producing iridium oxide with high pore volume and surface area addresses commercial production challenges, resulting in improved catalyst durability and performance for fuel cells and water electrolysis.
Patent Information
- Application Number
- JP2024551880
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2021-12-14
- Filing Date
- 2022-12-12
- Publication Date
- 2024-11-11
- Estimated Expiration
- 2042-12-12
AI Technical Summary
Existing methods struggle to commercially produce iridium oxide with high pore volume and specific surface area, which is crucial for catalysts in fuel cells and water electrolysis due to issues like sintering and low surface area, leading to decreased durability and efficiency.
A method involving the preparation of iridium chloride, mixing with a solvent and pore control agent, followed by ion exchange and heat treatment, to produce iridium oxide with controlled pore size and high surface area, including steps like alkali metal compound mixing, firing, hydrochloric acid washing, and controlled heat treatment.
The method enables the production of iridium oxide with average pore sizes of 2-5 nm, pore volumes of 0.21-0.25 cm³/g, and specific surface areas of 100-420 m²/g, enhancing catalyst durability and performance in oxygen evolution reactions.
Smart Images

Figure 2024541748000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for easily and commercially producing iridium oxide having a high pore volume and a high specific surface area as a catalyst for oxygen evolution reaction that can be used in fuel cells and water electrolysis reactions. [Background technology]
[0002] Fuel cells and water electrolysis technologies have attracted attention as methods for achieving carbon neutrality, but commercialization has been delayed due to difficulties in overcoming the problem of catalyst durability.
[0003] When the fuel cell and water electrolysis system are operating and electricity is generated, the water generated as a by-product covers the surface of the catalyst. This causes a reversal voltage phenomenon at the cathode due to a lack of hydrogen supply, and the carbon that supports the catalyst reacts with the water and becomes oxidized due to the high voltage, causing corrosion of the cathode catalyst.
[0004] This leads to a decrease in the efficiency of the catalyst and to problems with its stability and durability.
[0005] One method to solve the problem of reduced durability of electrodes in fuel cells and water electrolysis systems is to introduce an iridium (Ir)-based oxygen evolution reaction (OER) catalyst into the cathode.
[0006] This decomposes the by-product water before it corrodes the carbon that supports the electrode catalyst, stabilizing the electrode catalyst and improving durability against reverse voltage phenomena.
[0007] The operating principle of a fuel cell can be expressed by the following reaction equation 1.
[0008] The operating principle of the oxygen generation reaction catalyst, which decomposes the water (H2O) generated here to generate oxygen, can be expressed by reaction formula 2.
[0009] [Reaction Scheme 1]
[0010] Anode: H 2 →2H + +2e -
[0011] Cathode: 1 / 2O2+2H + +2e - →H2O
[0012] Overall: H2+1 / 2O2→H2O+Heat
[0013] [Reaction Scheme 2]
[0014] 2H2O → 2H2+O2
[0015] On the other hand, the iridium oxide (IrO2) catalyst used in the oxygen evolution reaction must have nano-sized particles and a high specific surface area to have high performance.
[0016] However, when iridium metal is subjected to simple thermal oxidation at 1300℃ or higher, it can be converted into oxide, but when sintered, huge particles of micron size are generated and the specific surface area is only 30m2. 2 / g or less, it is difficult to exhibit catalytic performance.
[0017] Thus, there is a need for a method by which iridium oxide having a high pore volume and a high specific surface area can be readily produced commercially. [Prior art documents] [Patent documents]
[0018] [Patent Document 1] Korean Patent Publication No. 10-2019-0018836 [Patent Document 2] U.S. Patent No. 8,263,290 [Non-patent literature]
[0019] [Non-Patent Document 1] international journal of hydrogen energy 43(2018), 19460-19467 Summary of the Invention [Problem to be solved by the invention]
[0020] One embodiment of the present invention provides a method for producing iridium oxide, which can easily and commercially produce iridium oxide having a high pore volume and a high specific surface area from iridium metal. [Means for solving the problem]
[0021] According to one embodiment of the present invention, there is provided a method for producing iridium oxide, the method including the steps of preparing iridium chloride, mixing iridium chloride with a solvent and a pore control agent to prepare a dispersion, mixing an ion exchange agent with the dispersion to perform ion exchange, removing the solvent from the dispersion to prepare a powder, and heat treating the powder.
[0022] The step of preparing iridium chloride may include a mixing step of preparing a mixture of iridium metal powder and an alkali metal compound, a calcination step of calcining the mixture to produce an alkali-containing iridium oxide, a hydrochloric acid aqueous solution washing step of washing the alkali-containing iridium oxide with a hydrochloric acid aqueous solution to obtain iridium oxide, and a hydrochloric acid dissolution reaction step of dissolving iridium oxide in hydrochloric acid under pressure and then reacting it.
[0023] The alkali metal compound can include an alkali metal hydroxide, an alkali metal peroxide, or a mixture thereof.
[0024] The alkali metal hydroxide may include sodium hydroxide, potassium hydroxide, lithium hydroxide, or mixtures thereof.
[0025] The alkali metal peroxide may include sodium peroxide, potassium peroxide, lithium peroxide, or mixtures thereof.
[0026] The alkali-containing iridium oxide may include a compound represented by the following Chemical Formula 1:
[0027] [Chemical formula 1]
[0028] Na x Ir y O z
[0029] In Chemical Formula 1, x is an integer from 2 to 4, y is an integer from 1 to 3, and z is an integer from 3 to 8.
[0030] In the hydrochloric acid aqueous solution washing step, the concentration of the hydrochloric acid aqueous solution is 5% to 10%.
[0031] The hydrochloric acid dissolution reaction step is carried out under pressure of 5 to 10 pressures at 130°C to 170°C for 2 to 6 hours.
[0032] In the step of preparing the dispersion, the solvent is an alcohol-based mixed solvent.
[0033] The alcohol-based mixed solvent may include ethanol and isopropanol.
[0034] The weight ratio of isopropanol to ethanol is 4:6 to 6:4.
[0035] In the step of preparing the dispersion, the solvent is mixed in an amount of 10 to 20 parts by weight per 1 part by weight of iridium chloride.
[0036] The pore control agent is a compound containing a benzene ring or a hydrocarbon compound having 6 to 10 carbon atoms.
[0037] The pore control agent may include 1,2,3-trimethylbenzene, 1,2,4-trimethylbenzene, 1,3,5-trimethylbenzene, triethylbenzene, hexanol, xylene, toluene, butyl acetate, octanol, or mixtures thereof.
[0038] The molar ratio of iridium chloride to the pore control agent is 1:1 to 1:3.
[0039] The ion exchange agent is an alkali metal nitrate.
[0040] The molar ratio of iridium chloride to the ion exchange agent is 1:5 to 1:10.
[0041] The ion exchange is carried out at 70°C to 90°C.
[0042] The powder preparation step is carried out by drying at 150°C to 180°C for 12 hours or more.
[0043] The heat treatment step is carried out at 300° C. to 600° C. for 1 hour to 1.5 hours.
[0044] The iridium oxide produced had an average pore size of 2 nm to 5 nm and an average pore volume of 0.21 cm. 3 / g~0.25cm 3 / g and the specific surface area is 100m 2 / g~420m 2 / g. Effect of the Invention
[0045] The method for producing iridium oxide according to one embodiment of the present invention makes it possible to easily commercially produce iridium oxide having a high pore volume and a high specific surface area from iridium metal. [Brief description of the drawings]
[0046] [Figure 1] 2 is a process flow diagram illustrating steps for manufacturing iridium oxide according to an embodiment of the present invention.
[0047] [Diagram 2] FIG. 1 is a process flow chart showing the iridium chloride preparation step.
[0048] [Diagram 3] 3 is a photograph showing the products at each stage of producing iridium oxide in Example 1.
[0049] [Figure 4] 1 is a graph showing the results of X-ray diffraction analysis (XRD) of the iridium oxides produced in Examples 1 to 4. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0050] The advantages and features of the techniques described below, and the manner in which they are achieved, will become apparent from the following detailed description of the embodiments taken in conjunction with the accompanying drawings. However, the embodied forms are not limited to the embodiments disclosed below. Unless otherwise defined, all terms (including technical and scientific terms) used herein are used with the same meaning as commonly understood by one of ordinary skill in the art. Additionally, terms defined in commonly used dictionaries are not to be interpreted ideally or excessively unless specifically and explicitly defined. Throughout the specification, when a part is said to "comprise" a certain element, this means that it can further include other elements, but not to the exclusion of other elements, unless specifically stated to the contrary.
[0051] Also, the singular includes the plural unless the phrase specifically states otherwise.
[0052] FIG. 1 is a process flow diagram illustrating steps for producing iridium oxide according to one embodiment of the present invention.
[0053] With reference to FIG. 1, the method for producing iridium oxide will be described in detail.
[0054] The method for producing iridium oxide includes an iridium chloride preparation step (S1), a dispersion preparation step (S2), an ion exchange step (S3), a powder preparation step (S4), and a heat treatment step (S5).
[0055] As an example, in the iridium chloride preparation step (S1), iridium chloride can be produced from iridium metal powder.
[0056] FIG. 2 is a process flow diagram showing steps for producing iridium chloride.
[0057] With reference to FIG. 2, the method for producing iridium chloride will be described in detail.
[0058] The method for producing iridium chloride includes an alkali metal compound mixing step (S1-1), a calcination step (S1-2), a hydrochloric acid aqueous solution washing step (S1-4), and a hydrochloric acid dissolution reaction step (S1-5).
[0059] In the alkali metal compound mixing step (S1-1), a mixture of iridium metal powder and an alkali metal compound is mixed.
[0060] The alkali metal compound can include an alkali metal hydroxide, an alkali metal peroxide, or a mixture thereof, for example, a solid mixture of an alkali metal hydroxide and an alkali metal peroxide.
[0061] The alkali metal hydroxide can include sodium hydroxide, potassium hydroxide, lithium hydroxide, or mixtures thereof, for example, the alkali metal hydroxide is sodium hydroxide (NaOH).
[0062] The alkali metal peroxide can include sodium peroxide, potassium peroxide, lithium peroxide, or mixtures thereof, for example, the alkali metal peroxide is sodium peroxide (Na2O2).
[0063] As an example, the alkali metal hydroxide may include a mixture of sodium hydroxide and sodium peroxide.
[0064] The mixture may contain 0.5 parts by weight to 1 part by weight, for example 0.6 parts by weight to 0.7 parts by weight, of the alkali metal compound per part by weight of the iridium metal powder. If the content of the alkali metal compound is less than 0.5 parts by weight per part by weight of iridium metal powder, the amount of alkali component adsorbed on the surface of the iridium metal may be insufficient, and oxidation may not occur uniformly during the firing process. If the content exceeds 1 part by weight, the excess alkali metal compound may cover the surface of the iridium metal, preventing the oxidizing agent from coming into contact with the iridium metal.
[0065] Alternatively, the mixture may contain from 1 part by weight to 3 parts by weight, for example 1.75 parts by weight to 2.25 parts by weight, of an alkali metal peroxide in an alkali metal compound per part by weight of the iridium metal powder. If the content of alkali metal peroxide is less than 1 part by weight per part by weight of iridium metal powder, iridium metal may still remain after calcination due to a lack of oxidizing agent, and if it exceeds 3 parts by weight, iridium metal may be peroxidized to form iridium nanoparticles, which may make it difficult to pass through the filter paper in the subsequent filtration process to obtain the product.
[0066] In this case, when the alkali metal compound contains a mixture of an alkali metal hydroxide and an alkali metal peroxide, the weight ratio of the alkali metal hydroxide to the alkali metal peroxide is 1:2 to 1:4, for example, 1:2.5 to 1:3.5. If the weight ratio of the alkali metal peroxide is less than 2, iridium metal may remain even after calcination due to a lack of oxidizing agent, and if it exceeds 4, iridium metal may be overoxidized to form iridium nanoparticles, which may make it difficult to pass through the filter paper in the subsequent filtration process to obtain the product.
[0067] In the calcination step (S1-2), the mixture is calcined to produce an alkali-containing iridium oxide.
[0068] The firing is carried out at 750°C or higher. If the calcination temperature is less than 750°C, unreacted iridium metal may remain, whereas at temperatures above 750°C, iridium metal is completely converted into alkali-containing iridium oxide. For example, the firing is carried out by increasing the temperature to 750° C. or higher over a period of 5 to 10 hours and maintaining the temperature at 750° C. or higher for 2 to 4 hours.
[0069] The alkali-containing iridium oxide produced by calcination may include a compound represented by the following Chemical Formula 1.
[0070] [Chemical formula 1]
[0071] Na x Ir y O z
[0072] In Chemical Formula 1, x is an integer from 2 to 4, y is an integer from 1 to 3, and z is an integer from 3 to 8.
[0073] For example, the alkali-containing iridium oxide represented by Chemical Formula 1 can include Na2IrO3, Na4IrO4, Na4Ir3O8, or a mixture thereof.
[0074] Optionally, the alkali-containing iridium oxide obtained in the calcination step may be washed with water prior to the hydrochloric acid aqueous solution washing step (S1-3).
[0075] The water may be deionized water, distilled water, or ultrapure water, and for example, deionized water may be used.
[0076] As an example, the water washing step is carried out by washing the iridium oxide with water containing an alkali at 60° C. to 70° C. for 2 to 4 hours. If the temperature of the water washing step is less than 60°C, the washing will not be complete and there may be residual alkaline ions after washing. If it exceeds 70°C, the washing water may evaporate and become concentrated. If the water washing step time is less than 2 hours, the washing may not be complete, and if it exceeds 4 hours, the working time may be unnecessarily long.
[0077] Optionally, after the water washing step, a further filtration step can be included. For example, filtration may be performed hot using a paper filter on the water-washed solution.
[0078] Optionally, after the filtration step, a water washing step may be further carried out. For example, after filtration, the mixture may be washed with pre-prepared high-temperature water at 60°C to 70°C.
[0079] Through the water washing step, the alkali metal ions in the alkali-containing iridium oxide can be partially removed, and thus, a portion of the iridium oxide can be obtained. However, even after the water washing step, about 400 ppm or more of alkali metal components may remain.
[0080] In the hydrochloric acid washing step (S1-4), the iridium oxide containing alkali is washed with a hydrochloric acid solution to reduce the content of the remaining alkali metal components to 10 ppm or less, thereby producing iridium oxide.
[0081] The concentration of the aqueous hydrochloric acid solution may be 5% to 10%. If the concentration of the hydrochloric acid solution is less than 5%, the cleaning effect will not be good and alkali metals may still remain; if it exceeds 10%, in addition to alkali metals, some iridium metals may also be dissolved.
[0082] Optionally, a further filtration step can be included after the aqueous hydrochloric acid washing step. For example, filtration is performed at high temperature using a paper filter after washing with an aqueous hydrochloric acid solution.
[0083] Optionally, the iridium oxide that has been washed with the aqueous hydrochloric acid solution can be dried to produce a cake.
[0084] Drying is carried out at 100° C. or higher for 12 to 24 hours. If the drying temperature is less than 100°C, not only will the drying time be longer, but moisture may remain even after drying.
[0085] The content of remaining alkali metal components can be reduced through the step of washing with an aqueous hydrochloric acid solution. As a result, the iridium oxide cake has an alkali metal content of 10 ppm or less, for example, 0 ppm to 5 ppm.
[0086] If the content of alkali metal exceeds 10 ppm, the purity of the final product iridium chloride decreases, which may have a negative effect on the catalytic reaction when producing a catalyst using the same.
[0087] In the hydrochloric acid dissolution reaction step (S1-5), iridium oxide is dissolved in hydrochloric acid under pressure and then reacted to produce iridium chloride hydrate.
[0088] The content of hydrochloric acid relative to 1 part by weight of iridium oxide is 5 parts by weight to 15 parts by weight, for example, 8 parts by weight to 10 parts by weight. If the content of hydrochloric acid per 1 part by weight of iridium oxide is less than 5 parts by weight, the content of chloride ions required for the reaction is insufficient, and therefore 100% conversion of iridium oxide to iridium chloride may not be achieved. If the content of hydrochloric acid exceeds 15 parts by weight, excessive energy costs may be required for evaporation of the hydrochloric acid aqueous solution in the subsequent concentration process.
[0089] The hydrochloric acid dissolution reaction step may be carried out under pressure, for example in a pressurized vessel. The pressure during pressurization is 5 to 10 pressures, for example, 6 to 8 pressures. Since the pressure increases in proportion to the reaction temperature, there is no need to separately adjust the pressure within the following temperature range.
[0090] The hydrochloric acid dissolution reaction step is carried out under pressure at 130° C. to 170° C. for 2 to 6 hours, for example, at 150° C. to 170° C. for 2 to 4 hours. If the temperature in the hydrochloric acid dissolution reaction step is less than 130°C, it may be difficult to convert iridium oxide to iridium chloride 100%. If it exceeds 170°C, the conversion to iridium chloride is easy, but the pressure vessel may corrode or deform, making commercial application difficult. If the time is less than 2 hours, the conversion reaction rate of iridium chloride may decrease, and if it exceeds 6 hours, excessive energy costs may be incurred.
[0091] Optionally, a filtration step may be further included after the hydrochloric acid dissolution reaction step.
[0092] Through the filtration step, the iridium chloride hydrate produced in the hydrochloric acid dissolution reaction step can be obtained. For example, filtration is performed by using a paper filter to filter the solution that has undergone the hydrochloric acid dissolution reaction at a high temperature. At this time, a minimum amount of rinsing solution, such as deionized water, is used to recover the remaining solution.
[0093] The iridium chloride hydrate produced is, for example, a compound represented by H2IrCl6·xH2O. The iridium chloride hydrate obtained in the hydrochloric acid dissolution reaction step is substantially completely dissolved, for example, 99.9% or more dissolved, and has an alkali metal content of 10 ppm or less.
[0094] In the method for producing iridium chloride hydrate, the calcination step (S1-2) induces complete oxidation of iridium metal, thereby increasing the production yield; in the hydrochloric acid aqueous solution washing step (S1-4), nitrogen oxides are not generated by using a single solvent of hydrochloric acid aqueous solution; before the pressurized reaction, the alkali metal components used as oxidants are removed using hydrochloric acid, so that the content of alkali metals in the obtained iridium chloride is 10 ppm or less; and in the hydrochloric acid dissolution reaction step (S1-5), the solubility is 99.9% or more through the pressurized reaction, and there is no unreacted iridium, so the purity of the product is very high.
[0095] Alternatively, the produced iridium chloride hydrate can be concentrated to produce iridium chloride (S1-6).
[0096] As an example, the concentration can be performed by vacuum distillation.
[0097] The iridium chloride produced is, for example, a compound represented by IrCl4·xH2O.
[0098] In the dispersion preparation step (S2), the prepared iridium chloride is mixed with a solvent and a pore control agent to prepare a dispersion.
[0099] The solvent may be an alcoholic solvent such as ethanol, isopropanol, or a mixture thereof, for example a mixed solvent of ethanol and isopropanol. When a mixture of ethanol and isopropanol is used as a solvent, the particle size of the final product, iridium oxide (IrO2), can be made smaller than when each solvent is used individually. At this time, the weight ratio of isopropanol to ethanol is 4:6 to 6:4, and the molar ratio of isopropanol to ethanol is 1:1 to 1:1.5, for example, 1:1.2 to 1:1.4.
[0100] The solvent is mixed in an amount of 10 to 20 parts by weight per 1 part by weight of iridium chloride. If the content of the solvent is less than 10 parts by weight, the solubility of iridium chloride (IrCl4) may decrease, and if it exceeds 20 parts by weight, it may take a long time to remove the solvent thereafter.
[0101] The pore control agent serves to increase the spacing between iridium particles during the process of removing the solvent from the mixture of iridium chloride and solvent, thereby increasing the specific surface area and pore volume of the iridium oxide produced after the final heat treatment.
[0102] The pore control agent may be a compound containing a benzene ring or a hydrocarbon compound having 6 to 10 carbon atoms, such as 1,2,3-trimethylbenzene, 1,2,4-trimethylbenzene, 1,3,5-trimethylbenzene, triethylbenzene, hexanol, xylene, toluene, butyl acetate, octanol, or mixtures thereof.
[0103] When the pore control agent is a hydrocarbon compound having 6 to 10 carbon atoms, if the carbon number exceeds 10, the viscosity of the dispersion increases and the pore control agent may not be completely removed during the heat treatment process, and if the carbon number of the pore control agent is less than 6, the effect of the pore control agent may not be clearly manifested.
[0104] The molar ratio of iridium chloride to pore control agent can be 1:1 to 1:3. If the molar ratio of the pore-controlling agent exceeds 3, the particle size of the iridium oxide may increase due to rapid heat generation during the subsequent heat treatment, resulting in a decrease in the specific surface area. If the molar ratio is less than 1, the effect may not be clearly observed.
[0105] The solvent and the pore control agent are mixed with the iridium chloride simultaneously or separately. For example, the iridium chloride and the solvent can be mixed and stirred, and then the pore control agent can be added and stirred. At this time, the stirring time is not particularly limited, but if each is maintained for 1 hour or more, the iridium chloride can be completely dispersed.
[0106] In the ion exchange step (S3), an ion exchange agent is mixed with the dispersion liquid to carry out ion exchange.
[0107] The ion exchange agent exchanges the chloride ions in iridium chloride with other ions in the solvent, widening the distance between iridium particles during the process of removing the solvent, thereby reducing the size of the iridium oxide produced after the final heat treatment, and increasing the specific surface area and pore volume.
[0108] The ion exchange agent can be any material capable of exchanging the chloride ions of the iridium chloride, and can include, for example, easily washed alkali metal nitrates such as KNO3, NaNO3, or mixtures thereof.
[0109] The molar ratio of iridium chloride to ion exchange agent may be from 1:5 to 1:10, for example, from 1:6 to 1:8. If the molar ratio of the ion exchange agent is more than 10, residual ion exchange agent remains during the ion exchange reaction, and even after the solvent is removed, the water generating reaction continues, and the ion exchange agent may be liquefied before the subsequent heat treatment process. If the molar ratio of the ion exchange agent is less than 5, the ion exchange of chloride may not be completed.
[0110] The ion exchange can be carried out at 70°C to 90°C. If the ion exchange temperature is less than 70°C, the ion exchange efficiency may decrease, and if it exceeds 90°C, the solvent may evaporate first, causing powderization before the ion exchange reaction, which may also decrease the ion exchange rate.
[0111] The ion exchange is carried out at the above temperature with stirring for 5 hours or more. The stirring time is not particularly limited, but if the stirring is continued for 5 hours or more, the iridium chloride can be completely ion-exchanged.
[0112] In the powder production step (S4), the solvent is removed to produce a powder.
[0113] The solvent must be removed by drying at 200°C or higher in an atmospheric pressure environment. However, at this time, the iridium nitrate compound may be reduced by the alcohol-based solvent and transformed back into iridium metal. Therefore, the solvent can be removed by vacuum drying at a relatively low temperature of 150°C to 180°C, for example 160°C to 170°C, for 12 hours or more. When the drying temperature is lower than 150° C., it may be difficult to completely remove the solvent. When the drying temperature exceeds 180° C., the solvent can be completely removed, but there is no clear advantage compared to increasing the temperature.
[0114] The drying time during solvent removal is not particularly limited, but the solvent can be completely removed when maintained for 12 hours or more.
[0115] In the heat treatment step (S5), the nitrate ions and the pore control agents of hydrocarbons present in the powder after the solvent removal are removed.
[0116] The heat treatment temperature can be appropriately adjusted depending on the pore volume and specific surface area of the iridium oxide to be produced. As an example, the heat treatment step is performed at 300° C. to 600° C., for example, 350° C. to 450° C., for 1 hour to 1.5 hours. If the heat treatment temperature is less than 300° C., it may be difficult to completely remove nitrate ions, and if it exceeds 600° C., aggregation of iridium oxide may occur, reducing the pore volume and the high specific surface area.
[0117] During the heat treatment, the temperature increase and maintenance time may vary depending on the condition of the heat treatment furnace. For example, the temperature may be increased at a rate of 2° C. to 3° C. per minute and maintained for 1 hour to 1.5 hours. If the temperature is raised and the holding time is long, crystallization of iridium oxide may occur, increasing the pore size and decreasing the specific surface area, whereas if the holding time is short, the conversion to iridium oxide may not be complete.
[0118] Optionally, after the heat treatment step, a washing and filtering step may be further carried out (S6).
[0119] The washing may be performed using deionized water, distilled water, or ultrapure water, for example, deionized water, and the filtration may be performed using a paper filter for the solution washed with water. The washing and filtering are repeated several times until the alkali ion content in the produced iridium oxide is reduced to 5 ppm or less.
[0120] Optionally, after washing and filtering, a drying step may be further carried out.
[0121] The drying temperature and drying time are not particularly limited, and as an example, drying is performed until the moisture content of the iridium oxide after drying is less than 1% by weight, for example, at 100° C. or higher for 12 to 24 hours. If the drying temperature is less than 100°C, not only will the drying time be longer, but moisture may remain even after drying.
[0122] The iridium oxide produced is in the hydroxide form of iridium oxide (IrO2·xH2O).
[0123] Iridium oxide is manufactured using a pore control agent and an ion exchange agent, resulting in an average pore size of 2 nm to 5 nm and an average pore volume of 0.21 cm. 3 / g~0.25cm 3 / g and the specific surface area is 100m 2 / g~420m 2 / g. [Example]
[0124] Specific examples of the invention are presented below. However, the following examples are merely intended to specifically illustrate and explain the invention, and should not be construed as limiting the scope of the invention.
[0125] [Production Example 1: Production of iridium chloride]
[0126] 13.5 g of NaOH powder and 40 g of Na2O2 powder are added to 20 g of Ir metal powder and physically mixed.
[0127] The mixed powder is placed in a crucible and fired at 750°C, then allowed to cool gradually. The firing is carried out in stages, with the temperature increased to 750°C for 6 hours and maintained at that temperature for 2.5 hours. During firing, the lid of the crucible is left open.
[0128] The calcined powder is washed in 500 ml of deionized water and then filtered to remove potassium and sodium.
[0129] Next, it is further washed with 200 g of HCl solution diluted to 5% in deionized water, and then transferred to a dryer and dried at 100° C. for 12 hours to obtain a powder.
[0130] The powder is placed in a pressure vessel and mixed with an additional 250 g of HCl.
[0131] The prepared pressure vessel is placed in a heat treatment furnace and subjected to a high-temperature pressurized reaction at 150°C for 4 hours, after which it is cooled. Thereafter, when the pressure vessel is opened, the powder is all dissolved and present in solution.
[0132] The solution is distilled under reduced pressure at 80° C. until it becomes a powder, and finally the iridium chloride precursor is produced.
[0133] [Production Example 2: Production of iridium oxide]
[0134] Example 1
[0135] FIG. 3 is a photograph showing the products at each stage of producing iridium oxide in Example 1. The process for producing the iridium oxide of Example 1 will be described with reference to FIG.
[0136] 10 g of the iridium chloride powder produced in Production Example 1 and 75 g each of ethanol and isopropanol as solvents were added, and then 7 g of trimethylbenzene, a pore control agent, was added to a water bath capable of stirring, and the mixture was then stirred for 1 hour to disperse.
[0137] After sufficient stirring, 20 g of potassium nitrate, an ion exchange agent, is added to the mixture, which is then heated to 80° C. and stirred for 5 hours to carry out the ion exchange process.
[0138] After the ion exchange is completed, the mixture is transferred to a vacuum dryer, heated to 170° C., and dried for 12 hours to produce a powder from which the solvent has been completely removed.
[0139] The powder is then transferred to a heat treatment furnace and maintained at 350° C. for 1 hour to remove any remaining organic compounds.
[0140] Finally, the heat-treated powder is repeatedly washed and filtered using deionized water to remove residual potassium ions, and then dried in a dryer at 100°C for 24 hours.
[0141] X-ray diffraction (XRD) analysis of the iridium oxide produced confirmed that it had a composition of IrO2·xH2O with an amorphous crystal structure, and BET analysis revealed a specific surface area of 412 m 2 / g, pore volume 0.24 cm 3 / g and the pore size was confirmed to be 2.5 nm.
[0142] (Examples 2 to 4 and Comparative Examples 1 to 4)
[0143] Iridium oxide was produced in the same manner as in Example 1, except that the reaction conditions were changed as shown in Table 1 below.
[0144] [Table 1]
[0145] For reference, Examples 2 to 4 are cases where the heat treatment temperature was changed, Comparative Example 1 is a case where no pore-controlling agent was added, Comparative Examples 2 and 3 are cases where a single solvent was used, and Comparative Example 4 is a case where the iridium chloride precursor was directly subjected to heat treatment without going through a process of forming pores therein.
[0146] [Experimental example: Characterization of iridium oxide]
[0147] The iridium oxides produced in the examples and comparative examples were subjected to X-ray diffraction analysis (XRD) and BET analysis, and the results are summarized in Table 2 and FIG.
[0148] [Table 2]
[0149] Referring to Table 2 and FIG. 4, the crystallinity analysis (XRD analysis) was performed on the products of Examples 1 to 4, and it was found that as the heat treatment temperature increases, the iridium oxide is gradually converted into a crystalline substance, and therefore the specific surface area and pore volume decrease, and the particle size increases due to the aggregation phenomenon of the iridium oxide.
[0150] Based on the above results, it can be seen that the intermediate product (powder before heat treatment), which has a larger pore volume due to the introduction of a pore control agent, loses its particle skeleton as the heat treatment temperature increases, and ultimately turns into a material with a low specific surface area and pore volume.
[0151] Moreover, Example 1 and Comparative Example 1 are results of comparing pore distributions with and without the use of a pore control agent. It can be seen that Comparative Example 1, which does not use a pore control agent, has a very low specific surface area and pore volume compared to Example 1. This indicates that the pore control agent provides a fine framework when forming an iridium oxide intermediate, thereby generating and maintaining a porous morphology.
[0152] Example 1 and Comparative Examples 2 and 3 show the results of comparing the method of using the solvent when mixing the solvent and iridium chloride powder. Unlike Example 1, when a single solvent of ethanol or isopropanol is used, the pore control agent cannot exert its effect and is disadvantageous to the formation of pores even though other manufacturing conditions such as ion exchange and heat treatment are the same. This is expected to be due to the difference in solubility or binding strength between the solvent and the pore control agent.
[0153] Example 1 and Comparative Example 4 are the results of comparing products obtained by carrying out a simple heat treatment without using a pore-controlling agent or an ion exchange agent. Unlike Example 1, when no pore-forming agent was added, it was confirmed that the film showed very low pore characteristics despite the low heat treatment temperature.
[0154] Therefore, in order to produce iridium oxide with a high pore volume and a high specific surface area, a step of forming micropores must be carried out in the first step, and an appropriate heat treatment temperature is required to maintain the pore shape.
[0155] Although the embodiments of the present invention have been described in detail above, the scope of the present invention is not limited thereto, and various modifications and improvements made by those skilled in the art using the basic concept of the present invention defined in the claims also fall within the scope of the present invention. [Industrial Applicability]
[0156] The present invention provides a method for easily and commercially producing iridium oxide having a high pore volume and a high specific surface area as an oxygen evolution reaction catalyst that can be used in fuel cells and water electrolysis reactions.
Claims
1. Providing iridium chloride; mixing the iridium chloride with a solvent and a pore control agent to prepare a dispersion; mixing an ion exchange agent with the dispersion to perform ion exchange; removing the solvent from the dispersion to produce a powder; and heat treating the powder. A method for producing iridium oxide, comprising:
2. The step of preparing iridium chloride comprises: a mixing step of preparing a mixture of iridium metal powder and an alkali metal compound; a calcination step of calcining the mixture to produce an alkali-containing iridium oxide; a hydrochloric acid washing step of washing the alkali-containing iridium oxide with a hydrochloric acid aqueous solution to obtain iridium oxide; and a hydrochloric acid dissolution reaction step of dissolving the iridium oxide in hydrochloric acid under pressure and then reacting the iridium oxide; The method for producing iridium oxide according to claim 1 , comprising:
3. The method of claim 2 , wherein the alkali metal compound comprises an alkali metal hydroxide, an alkali metal peroxide, or a mixture thereof.
4. the alkali metal hydroxide comprises sodium hydroxide, potassium hydroxide, lithium hydroxide, or a mixture thereof; 4. The method of claim 3, wherein the alkali metal peroxide comprises sodium peroxide, potassium peroxide, lithium peroxide, or a mixture thereof.
5. The method for producing iridium oxide according to claim 2 , wherein the alkali-containing iridium oxide comprises a compound represented by the following Chemical Formula 1: [Chemical formula 1] Na x Ir y O z (In the above Chemical Formula 1, x is an integer of 2 to 4, y is an integer of 1 to 3, and z is an integer of 3 to 8.)
6. 3. The method of claim 2, wherein the concentration of the hydrochloric acid solution in the hydrochloric acid washing step is 5% to 10%.
7. 3. The method for producing iridium oxide according to claim 2, wherein the hydrochloric acid dissolving reaction step is carried out under pressure of 5 to 10 pressures at 130 to 170° C. for 2 to 6 hours.
8. The method of claim 1 , wherein in the step of preparing the dispersion, the solvent is an alcohol-based mixed solvent.
9. The method for producing iridium oxide according to claim 8 , wherein the alcohol-based mixed solvent contains ethanol and isopropanol.
10. The method for producing iridium oxide according to claim 9, wherein the weight ratio of the isopropanol to the ethanol is 4:6 to 6:
4.
11. 2. The method of claim 1, wherein in the step of preparing the dispersion, the solvent is mixed in an amount of 10 to 20 parts by weight with respect to 1 part by weight of the iridium chloride.
12. 2. The method for producing iridium oxide according to claim 1, wherein the pore-controlling agent is a compound containing a benzene ring or a hydrocarbon compound having 6 to 10 carbon atoms.
13. 13. The method of claim 12, wherein the pore control agent comprises 1,2,3-trimethylbenzene, 1,2,4-trimethylbenzene, 1,3,5-trimethylbenzene, triethylbenzene, hexanol, xylene, toluene, butyl acetate, octanol, or a mixture thereof.
14. 2. The method for producing iridium oxide according to claim 1, wherein the molar ratio of the iridium chloride to the pore control agent is 1:1 to 1:
3.
15. 2. The method for producing iridium oxide according to claim 1, wherein the ion exchange agent is an alkali metal nitrate.
16. 2. The method for producing iridium oxide according to claim 1, wherein the molar ratio of the iridium chloride to the ion exchange agent is 1:5 to 1:
10.
17. The method for producing iridium oxide according to claim 1, wherein the ion exchange is carried out at 70°C to 90°C.
18. The method of claim 1, wherein the powder is dried at 150° C. to 180° C. for 12 hours or more.
19. 2. The method of claim 1, wherein the heat treatment is performed at 300° C. to 600° C. for 1 hour to 1.5 hours.
20. The iridium oxide produced is The average pore size is 2 nm to 5 nm; Average pore volume is 0.21 cm 3 / g ~ 0.25 cm 3 / g, Specific surface area is 100m 2 / g~420m 2 The method for producing iridium oxide according to claim 1, wherein the iridium oxide content is 1 / g.
Citation Information
Patent Citations
Porous IrO2 oxygen evolution catalyst with super-high specific surface area and preparation method of porous IrO2 oxygen evolution catalyst
CN106111130A
Method for directly preparing chloroiridic acid from iridium-containing waste
CN112357979A
Production method of iridium oxide and iridium oxide
JP2020132465A
Method for producing highly pure iridium(III) chloride hydrate
JP2020515487A
Iridium oxide NANO catalyst and preparation method thereof
KR1020190018836A