Method for enhancing wettability of contact lens compositions during molding - Patents.com
Polyether-modified polyolefin molds and silicone-containing monomer mixtures in contact lens manufacturing enhance surface wettability, eliminating the need for intermediate processing steps and ensuring stable, efficient lens production.
Patent Information
- Application Number
- JP2024529993
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2021-11-22
- Filing Date
- 2022-11-21
- Publication Date
- 2024-11-12
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Current contact lens manufacturing technologies face challenges in achieving sufficient surface wettability, which is crucial for user comfort and physiological behavior, often requiring additional processing steps like oxygen plasma treatment or surface coatings, and these methods lack stability and efficiency.
The use of polyether-modified polyolefin molds and specific silicone-containing monomer mixtures to form contact lenses with water contact angles less than 90°, eliminating the need for intermediate processing steps.
Contact lenses with improved surface wettability are produced directly after hydration without additional treatments, maintaining desired physical properties and reducing manufacturing inefficiencies.
Smart Images

Figure 2024541760000001 
Figure 2024541760000002 
Figure 2024541760000003
Abstract
Description
[Technical field]
[0001] CROSS-REFERENCE TO RELATED APPLICATIONS This application claims priority to U.S. Provisional Patent Application No. 63 / 281,927, filed November 22, 2021, the disclosure of which is incorporated by reference in its entirety herein. [Background technology]
[0002] In current popular bulk hydrogel and silicone modified hydrogel (SiHy) contact lens manufacturing techniques, a mixture of unsaturated monomers selected for their performance in providing mechanical properties, oxygen permeability, and user comfort is cast and polymerized into single-use polyolefin molds. These molds typically have multiple cavities (e.g., four or more cavities). In manufacturing, a liquid monomer mixture or composition is filled into the polyolefin mold and then polymerized to form the lens using UV light irradiation or thermal energy.
[0003] Following polymerization, the lens is removed from the mold (delensed) and the mold is discarded. After delensing and before use, the lens is usually removed and the residual monomers are removed, and the initiator by-products are then hydrated in saline or a buffered saline solution. Due to the inherent limitations of the surface properties of the as-molded lenses, the SiHy lenses must then be modified by one or more additional intermediate processing steps. The surface wettability of unmodified SiHy lenses, characterized by high water contact angles, is not sufficient. Surface wettability is not only an important parameter in short-term user comfort, but also plays an important role in protein adsorption and other factors affecting physiological behavior. Consequently, after delensing, surface wettability is introduced by oxygen plasma treatment or achieved by a surface coating process. In addition to the inefficiencies caused by the additional manufacturing steps, surface modifications often lack stability and their effectiveness decreases during storage or use. Another approach is to incorporate polymeric species such as polyvinylpyrrolidinone into the lens composition matrix, but this is of limited use due to both limited solubility in the lens monomer composition and reduced mechanical and optical properties of the final polymerized lens. Overviews of silicon hydrogels from a materials and processing technology perspective are provided by Musgrave ("Contact Lens Materials - A Materials Science Perspective Materials," Materials; 12, 261 (2019)), Goff ("Applications of Hybrid Polymers Generated by Living Anionic Ring Opening Polymerization Molecules," Macromolecules 26, 2755 (2021)), and N. Efron (Contact-Lens-Practice 3rd Edition, Chapter 5 Soft-Lens-Manufacture, Elsevier, pp. 61-67 (2018)). [Prior art documents] [Patent documents]
[0004] [Patent Document 1] U.S. Patent No. 10,669,294 [Patent Document 2] U.S. Patent No. 8,772,367 [Patent Document 3] U.S. Patent No. 9,102,110 [Patent Document 4] Patent Publication No. 2004-299222 [Non-patent literature]
[0005] [Non-Patent Document 1] Musgrave("Contact Lens Materials - A Materials Science Perspective Materials," Materials; 12, 261 (2019)) [Non-Patent Document 2] Goff("Applications of Hybrid Polymers Generated by Living Anionic Ring Opening Polymerization Molecules," Macromolecules 26, 2755 (2021)) [Non-Patent Document 3] N. Efron (Contact-Lens-Practice 3rd Edition, Chapter 5 Soft-Lens-Manufacture, Elsevier, pp. 61-67 (2018)) [Non-Patent Document 4] PBM Janssen, "Reactive Extrusion Systems" Marcel Dekker, pages 169-178 (2004) Summary of the Invention [Means for solving the problem]
[0006] In one aspect of the disclosure, there is provided a method for producing a contact lens having a water contact angle of less than about 90°, comprising the steps of: (a) preparing a mold molding resin containing polyether modified polyolefin; (b) forming the molding resin into a mold; (c) preparing a contact lens composition; (d) filling the contact lens composition into the mold; (e) polymerizing the contact lens composition to form a contact lens; A method is provided, comprising:
[0007] In another aspect of the present disclosure, there is provided a method for providing a water contact angle of less than 90° and improving surface wettability of a contact lens, the method comprising casting polymerizing a mixture of monomers in a mold formed from a molding resin containing a polyether-modified polyolefin to form a contact lens having a water contact angle of less than about 90°.
[0008] In a further aspect of the present disclosure, a single-use mold for making contact lenses is provided, the mold comprising a polyether-modified polyolefin composition.
[0009] In summary, the following embodiments are presented as particularly preferred within the scope of the present invention.
[0010] Embodiment 1: A method for producing a contact lens having a water contact angle of less than about 90°, comprising the steps of: (a) preparing a molding resin comprising a polyether-modified polyolefin; (b) forming the molding resin into a mold; (c) preparing a contact lens composition; (d) filling the contact lens composition into the mold; (e) polymerizing the contact lens composition to form a contact lens; A method comprising:
[0011] Embodiment 2: The method according to embodiment 1, wherein the polyolefin in the molding resin comprises at least one of polypropylene homopolymer, polypropylene copolymer, polyethylene homopolymer, and polymethylpentene.
[0012] Embodiment 3: The method according to embodiment 1 or 2, wherein step (a) comprises preparing a copolymer of a polyether and a polyolefin.
[0013] Embodiment 4: The method according to any one of embodiments 1 to 3, wherein step (a) comprises reacting a polyether with a maleated graft polymer of a polyolefin.
[0014] Embodiment 5: The method according to any one of embodiments 1 to 4, wherein the molding resin comprises a blend of polyether-modified polyolefin and unmodified polyolefin resin.
[0015]
[0023] Embodiment 6: The method according to embodiment 5, wherein the polyether-modified polyolefin is blended into the unmodified polyolefin resin in an amount of about 5 to 20 weight percent.
[0016] Embodiment 7: The method according to any one of embodiments 1 to 6, wherein the mold resin further comprises a hydrophilic additive selected from polyetheramines and methoxypolyethylene glycols.
[0017] Embodiment 8: The method according to any one of embodiments 1 to 7, wherein the polyether-modified polyolefin is a grafted polyolefin or copolymerized polyolefin containing anhydride or carboxylic acid groups, and the hydrophilic additive is present in an amount of about 0.25 to 1.00 molar equivalents relative to the anhydride or carboxylic acid content of the grafted polyolefin or copolymerized polyolefin.
[0018] Embodiment 9: The method according to any one of embodiments 1 to 8, wherein the contact lens composition comprises a base monomer, a silicone-containing macromer, and a crosslinker.
[0019] Embodiment 10: The method according to embodiment 9, wherein the silicone-containing macromer comprises at least two polyethyleneoxy groups (PEG).
[0020] Embodiment 11: The method according to any one of embodiments 1 to 10, wherein step (e) comprises applying UV radiation or heat to effect polymerization.
[0021] Embodiment 12: A method for making a contact lens have a water contact angle of less than 90° and improved surface wettability, comprising casting and polymerizing a mixture of monomers in a mold formed from a molding resin containing a polyether modified polyolefin to form a contact lens having a water contact angle of less than about 90°.
[0022] Embodiment 13: The method according to embodiment 12, wherein the polyolefin in the molding resin comprises at least one of polypropylene homopolymer, polypropylene copolymer, polyethylene homopolymer, and polymethylpentene.
[0023] Embodiment 14: The method according to embodiment 12 or 13, wherein the mold resin comprises a copolymer of polyether and polyolefin.
[0024] Embodiment 15: The method according to any one of embodiments 12 to 14, wherein the mold resin comprises a polyether reacted with a maleated graft polymer of a polyolefin.
[0025] Embodiment 16: The method according to any one of embodiments 12 to 15, wherein the molding resin comprises a blend of polyether-modified polyolefin and unmodified polyolefin resin.
[0026] Embodiment 17: The method according to embodiment 16, wherein the polyether-modified polyolefin is blended into the unmodified polyolefin resin in an amount of about 5 to 20 weight percent.
[0027] Embodiment 18: The method according to any one of embodiments 12 to 17, wherein the molding resin further comprises a hydrophilic additive selected from polyetheramines and methoxypolyethylene glycols.
[0028] Embodiment 19: The method according to any one of embodiments 12 to 18, wherein the polyether-modified polyolefin is a grafted polyolefin or copolymerized polyolefin containing anhydride or carboxylic acid groups, and the hydrophilic additive is present in an amount of about 0.25 to 1.00 molar equivalents relative to the anhydride or carboxylic acid content of the grafted polyolefin or copolymerized polyolefin.
[0029] Embodiment 20: The method according to any one of embodiments 12 to 19, wherein the mixture of monomers comprises a base monomer, a silicone-containing macromer, and a crosslinker.
[0030] Embodiment 21: The method according to embodiment 20, wherein the silicone-containing macromer comprises at least two polyethyleneoxy groups (PEG).
[0031] Embodiment 22: A single-use mold for making contact lenses, the single-use mold comprising a polyether-modified polyolefin composition.
[0032] Embodiment 23: The single-use mold according to embodiment 22, wherein the polyolefin in the composition comprises at least one of polypropylene homopolymer, polypropylene copolymer, polyethylene homopolymer, and polymethylpentene.
[0033] Embodiment 24: A single-use mold according to embodiment 22 or 23, wherein the composition comprises a copolymer of a polyolefin and a polyether.
[0034] Embodiment 25: A single-use mold according to any one of embodiments 22 to 24, wherein the composition comprises a polyether reacted with a maleated graft polymer of a polyolefin.
[0035] Embodiment 26: A single-use mold according to any one of embodiments 22 to 25, wherein the composition comprises a blend of polyether-modified polyolefin and unmodified polyolefin resin.
[0036] Embodiment 27: The single-use mold according to embodiment 26, wherein the polyether-modified polyolefin is blended into the unmodified polyolefin resin in an amount of about 5 to 20 weight percent.
[0037] Embodiment 28: A single-use mold according to any one of embodiments 22 to 27, wherein the composition further comprises a hydrophilic additive selected from polyetheramines and methoxypolyethylene glycols.
[0038] Embodiment 29: A single-use mold according to any one of embodiments 22 to 28, wherein the polyether-modified polyolefin is a grafted polyolefin or copolymerized polyolefin containing an acid anhydride group or a carboxylic acid group, and the hydrophilic additive is present in an amount of about 0.25 to 1.00 molar equivalents relative to the acid anhydride or carboxylic acid content of the grafted polyolefin or copolymerized polyolefin.
[0039] Embodiment 30: A single-use mold according to any one of embodiments 22 to 29, wherein a contact lens produced from the mold has a water contact angle of less than about 90°.
[0040] Embodiment 31: The single-use mold according to embodiment 30, wherein a contact lens is formed from a composition comprising a base monomer, a silicone-containing macromer, and a crosslinker.
[0041] Embodiment 32: A single-use mold according to embodiment 31, wherein the silicone-containing macromer comprises at least two polyethyleneoxy groups (PEG). DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0042] The present disclosure relates to a method for producing SiHy contact lenses with low water contact angles and surface wettability using modified polyolefin molds containing grafted polyethers or copolymerized polyethers. Surfaces with contact angles less than about 90° are generally considered wettable, and contact angles less than about 70° are preferred for contact lens applications. Thus, for the purposes of this disclosure, the term "low water contact angle" may be understood to refer to contact angles less than about 90°, preferably less than about 80°, more preferably less than about 70°, and even more preferably less than about 65°. By employing these modified polyolefin molds and specific mixtures of silicone-containing monomers, contact lenses with desired physical properties can be achieved after delensing and immediately after hydration without any intermediate processing steps such as oxygen plasma treatment or surface coating. Preferably, the mixture of monomers allows for the formation of polymers with polar pendant groups or bottle-brush structures. The most preferred polar groups are those that allow for the formation of hydrogen bonds and may be a substituent of any monomer in the monomer mixture used to mold the contact lenses. In a most preferred embodiment, the mixture includes a polar monomer that is also a silicon-containing monomer having pendant groups capable of forming hydrogen bonds after polymerization.
[0043] Single-use molds for manufacturing contact lenses The mold for making contact lenses according to the embodiment of the present disclosure is formed from a contact lens molding composition (molding resin) that includes polyether modified polyolefin. Suitable polyolefins according to the present disclosure include polypropylene, copolymers of propylene and ethylene or other olefins, polymethylpentene, and polyethylene, with polypropylene and polymethylpentene being preferred. These materials are desirable resins for high speed molding molds for contact lenses due to their release properties that allow contact lens stripping, sufficient high temperature properties to allow heat curing, suitable transparency to allow UV curing, hydrolysis resistance, and economy.
[0044] To produce polyether-modified polyolefins, these polyolefins are modified by the introduction of polyethers. The modification can be accomplished, for example, by introducing the polyether as a comonomer in a base resin, such as a copolymer of propylene and an allyl-terminated polyether. Alternatively, the modified base molding resin can be formed by reacting a polyether with a maleated graft polymer of polypropylene. In other embodiments, the modified polyolefins can be prepared by esterification, with a polyether, of a polyolefin-based copolymer modified with carboxylic acid groups, the carboxylic acid groups being introduced by copolymerization of acrylate monomers or by grafting acrylate monomers.
[0045] In a preferred embodiment, the polyether modified polyolefin is blended with an unmodified polyolefin resin. For example, the polyether modified polypropylene may be blended with standard polypropylene or other polyolefin resins (e.g., polypropylene copolymer, polyethylene, or polymethylpentene) at a level sufficient to provide a desirable water contact angle for the contact lens. In one embodiment, the maleated polyolefin reacted with the polyether can be blended into the base polymer by extrusion in an amount of about 5 to 20% by weight. Preferably, for compatibility, the base polymer used in the blend is the same as the polyolefin in the polyether modified polyolefin. However, it is believed that random copolymers may contribute to a slight reduction in the contact angle. In a preferred embodiment, the polyether modified polyolefin is blended with a polypropylene homopolymer or polypropylene copolymer. It is further within the scope of the present disclosure to form a mold using only the polyether modified polyolefin.
[0046] In one embodiment, the molding resins according to the present disclosure can be easily prepared by the reaction of maleated polyolefins, such as maleated polypropylene. As used herein, the term "maleated polypropylene" generally refers to the reaction product formed by grafting maleic anhydride, preferably covalently, onto the backbone of polypropylene, which may contain up to 10% of a comonomer such as ethylene. Melt grafting methods for maleating polyolefins are known and have been reviewed (see, for example, PBM Janssen, "Reactive Extrusion Systems" Marcel Dekker, pp. 169-178 (2004)). Maleated polyolefins are commercially available from, for example, Dow (Fusabond), SI Group (formerly Chemtura, Polybond), Westlake (Epolene), Eastman (G POLYMER), LyondellBasell (Plexar), and Mitsubishi Chemical (Modic), among others, and are most commonly used as adhesion promoters, adhesion layers, or compatibilizers.
[0047] It is further within the scope of the present disclosure to react / combine maleated polyolefins or other polyether modified polyolefins (optionally blended with unmodified polyolefin resins) with a hydrophilic additive, such as polyetheramines, methoxypolyethylene glycols, or other polyethylene glycols having a free hydroxyl group at one end and an alkyl group such as butyl at the other end, in an amount ranging from about 25% to about 100% molar equivalents relative to the amount of maleated polyolefin, preferably ranging from 50 to 75%. In other words, if the polyether modified polyolefin is a grafted polyolefin or copolymerized polyolefin containing anhydride or carboxylic acid groups, the hydrophilic additive may be present in an amount of about 0.25 to 1.00 molar equivalents relative to the anhydride or carboxylic acid content of the grafted polyolefin or copolymerized polyolefin. The currently preferred polyetheramines are amine terminated PEO-PPO copolymers. Other additives known in the art, such as, but not limited to, processing aids, antioxidants, and mold release agents, may additionally be incorporated.
[0048] Polyether modified polyolefins according to embodiments of the present disclosure may include, but are not limited to, conventional copolymers, graft copolymers, and blends of these materials with unmodified polyolefins. For example, a polyether reaction of a maleated graft copolymer of polypropylene with an alpha-amine terminated PEO-PPO copolymer having omega-methyl ends can be replaced with an alpha-hydroxy, omega-methyl terminated polyethylene oxide homopolymer. The degree of polymerization of the polyether modified materials described herein may range from about 2 to about 50, preferably from about 6 to about 20. The reaction product of an amine terminated polyether with maleated polypropylene can be referred to as maleamate or maleamic acid modified polypropylene. The reaction product of a hydroxyl terminated polyether with maleated polypropylene can be referred to as maleate ester modified polypropylene.
[0049] Once produced, the contact lens molding composition or resin containing the polyether modified polyolefin base polymer and optionally other ingredients is formed into a mold using known methods, typically by injection molding, and then used to produce a contact lens, as described in more detail below. As previously explained, the water contact angle of the resulting contact lens is less than about 90°, preferably less than about 85°, more preferably less than about 80°, even more preferably less than about 75°, even more preferably less than about 70°, and even more preferably less than about 65°. It is within the scope of the present invention for the mold to have multiple cavities, for example four or more cavities, in order to produce multiple contact lenses simultaneously.
[0050] As an example of a single-use contact lens mold according to the present disclosure, a polyether modified polyolefin may be employed, such as commercially available Polybond 7200, a polypropylene grafted with 1.5 to 1.9% by weight maleic anhydride. This material is a 25% molar equivalent amine terminated PEO-PPO copolymer (M W The grafted reactant can be reacted in the molten state (e.g., by using a co-rotating twin screw extruder) with a grafted polypropylene (approximately 1000 Daltons). The grafted reactant can be compounded with standard polypropylene (e.g., commercially available Pinnacle Polymers 1120H) at 20% by weight and then molded into plaques for analysis. It is noted that flat plaques are employed for testing and analysis purposes rather than contact lens molds. The water contact angle of the Pinnacle polypropylene base polymer was measured to be 96°, while the water contact angle of the Pinnacle polypropylene base polymer compounded with the modified grafted polymer was observed to be 79°.
[0051] Contact Lens Composition The composition of contact lenses is important to achieve optimal performance. The mixture of monomers used to form contact lenses usually contains at least three components: a base monomer (such as, but not limited to, dimethylacrylamide (DMA) or hydroxyethyl methacrylate (HEMA)), a silicone-containing macromer (such as, but not limited to, low molecular weight methacryloxypropyl terminated polydimethylsiloxane (MPDMS) DP about 10 (Gelest MCR-M11)), and a crosslinker (such as, but not limited to, ethylene glycol dimethacrylate (EGDMA)). Preferably, the silicone-containing macromer has at least three polyethyleneoxy groups (PEG). In a preferred embodiment, an additional monomer having a polyether segment bonded to the siloxane replaces some or all of the silicone-containing macromer. Examples of such macromers are described in U.S. Pat. No. 10,669,294, with a polyether comonomer content of 10 to 100%, and are also described in U.S. Pat. No. 8,772,367. These known macromers are not commercially used in the manufacture of contact lenses. Although their chemical structures differ, each of these compositions further contains two polyethyleneoxy groups (PEG).
[0052] Polyolefin surfaces are known to be extremely hydrophobic. The water contact angle of polypropylene has been observed to be between 105 and 110°, while commercial grades containing additives or comonomers are more typically between 96 and 103°, with a critical surface tension of 31 mN / m. Under the casting conditions employed in conventional contact lens manufacturing, these properties lead to the accumulation of hydrophobic groups at the interface with the mold, resulting in high contact angles and poor wettability of the contact lens. Without wishing to be bound by theory, it is believed that the surface of the modified polyolefin mold described herein is richer in polyether groups than in the bulk. As a result, the mixture of monomers in the contact lens composition is less prone to the accumulation of hydrophobic groups at the interface with the polypropylene mold. In a preferred embodiment, a mixture of monomers containing polar groups, and most preferably polyether groups, or other groups capable of forming hydrogen bonds, is included in the reactive monomer blend. The materials described herein are generally more hydrophilic. Preferred monomers are believed to adsorb in high concentrations at the interface, which is especially likely for polyethers containing monomers that allow for the formation of hydrogen bonds. The mechanism of enrichment of polar groups at the interface of the mold is not limited to reactive monomers. In the case of polymerized monomers containing pendant polyether groups, the polyether groups can be meandered or accommodated at the interface by orienting at the interface with the modified polyolefin mold.
[0053] For clarity, the molds formed from the compositions described herein are different from those obtained by applying a surfactant to the mold. Application of chemical species to the mold material would result in an extra manufacturing step in the application and would raise concerns regarding surfactant migration and contamination of the lens by the surfactant. In contrast, the contact lens mold molding compositions described herein are consistent with current contact lens casting technology, which relies on the optical, thermal, demolding, and mechanical properties, as well as economics, of polyolefins. While other resins with higher critical surface tensions may potentially have higher hydrophilicity, they tend to have poor demolding properties. Although lens surface wettability is not considered, U.S. Pat. No. 9,102,110 describes the involvement of polyvinyl alcohol molds in terms of mold opening and lens demolding. More typically, for example in JP 2004-299222 (2004) where glyceryl monostearate with polypropylene is employed, the mould materials are evaluated for their releasability or ability to form a smooth surface during the delensing process.
[0054] Method for forming contact lenses A further aspect of the present disclosure relates to a method for producing contact lenses that allow for surface wettability, as described above, with low water contact angles, more specifically less than about 90°, preferably less than about 80°, more preferably less than about 70°, and even more preferably less than 65°. The method includes first preparing a mold-molding composition (resin) comprising a polyether-modified polyolefin, as described above. The mold-molding resin may contain only polyether-modified polyolefin or may contain a blend comprising unmodified polyolefin in which the polyether-modified polyolefin is blended, and may further contain additives, as described above.
[0055] The molding resin is formed into a mold having a cavity by a conventional method, for example, injection molding.
[0056] In a subsequent step, the method includes preparing a contact lens composition, for example a composition containing a base monomer, a silicon-containing monomer, and a crosslinker, as described above. Methods for forming such compositions are well known in the art and do not require further description. Preferably, the silicon-containing monomer has at least two polyethyleneoxy groups (PEG). The contact lens composition containing the liquid monomer mixture is then filled into the cavity of the mold using conventional methods and polymerized to form the contact lens. Polymerization can be carried out thermally using heat or by UV irradiation, using a photoinitiator or a radical initiator, respectively, added to the contact lens composition. Finally, the contact lens is removed from the cavity (delensed) and the mold is discarded. Application of water, alone or in combination with an alcohol or a surfactant, may be utilized to aid in the release of the lens from the mold.
[0057] As already explained, in contrast to known methods, no surface treatment or coating process is performed on the contact lens after delensing. Rather, the observed superior properties of low water contact angle and enhanced surface wettability discussed above are the result of the composition used to form the mold in combination with the contact lens composition. As already explained, the resulting contact lens has a water contact angle of less than about 90°, preferably less than about 85°, more preferably less than about 80°, even more preferably less than about 75°, even more preferably less than about 70°, and even more preferably less than about 65°.
[0058] The use of the mold resins described herein has a dramatic effect on the water contact angle of the resulting contact lens. The extent of the effect varies depending on the material used to form the mold resin as well as the particular silicon-containing monomer used to form the contact lens. For example, the water contact angle of a macromer formed from a composition containing an α-methacryloxy, ω-butyl terminated polydimethylsiloxane homopolymer and polymerized onto a substrate containing polyether maleamate modified polypropylene was reduced to 99° compared to a water contact angle of 114° for a similar macromer polymerized onto an unmodified polypropylene substrate.
[0059] When the silicone-containing macromer in the contact lens composition had diethylene oxide (PEG) substitution, a more dramatic reduction in water contact angle was observed, suggesting enhanced wettability. For example, a macromer prepared from a composition containing an α-methacryloxy, ω-butyl terminated poly(methoxydiethylene-oxypropyl)-methylsiloxane) homopolymer exhibited a water contact angle of 116° when polymerized on unmodified polypropylene, but when polymerized on two different maleamate-modified polypropylene substrates, the water contact angles were 72° and 59°, respectively. Similarly, a macromer prepared from a composition containing an α-methacryloxy, ω-butyl terminated 50% (methoxydiethylene-oxypropyl)-methylsiloxane) 50% dimethylsiloxane copolymer exhibited a water contact angle of 109° when polymerized on unmodified polypropylene, but when polymerized on two different maleamate-modified polypropylene substrates, the water contact angles were 74° and 64°, respectively. Furthermore, a macromer prepared from a composition containing an α-methacryloxy, ω-butyl terminated 25% (methoxydiethylene-oxypropyl)-methylsiloxane) 75% dimethylsiloxane copolymer exhibited a water contact angle of 97° when polymerized on unmodified polypropylene, but water contact angles of 73° and 65°, respectively, when polymerized on two different maleamate-modified polypropylene substrates.
[0060] Similar results are observed with macromers polymerized on maleate-modified polypropylene substrates. Specifically, for example, the water contact angle of a macromer formed from a composition containing an α-methacryloxy, ω-butyl terminated polydimethylsiloxane homopolymer and polymerized on a substrate containing polyether maleate-modified polypropylene was reduced to 100° compared to 114° for a similar macromer polymerized on unmodified polypropylene.
[0061] When the silicone-containing macromer in the contact lens composition had diethylene oxide (PEG) substitution, a more dramatic reduction in water contact angle was observed, suggesting greater wettability. For example, a macromer prepared from a composition containing an α-methacryloxy, ω-butyl terminated 50% (methoxydiethylene-oxypropyl)-methylsiloxane) 50% dimethylsiloxane copolymer exhibited a water contact angle of 109° when polymerized on unmodified polypropylene, but a water contact angle of 95° when polymerized on a polyether maleate modified polypropylene substrate. Furthermore, a macromer prepared from a composition containing an α-methacryloxy, ω-butyl terminated 25% (methoxydiethylene-oxypropyl)-methylsiloxane) 75% dimethylsiloxane copolymer exhibited a water contact angle of 97° when polymerized on unmodified polypropylene, but a water contact angle of 94° when polymerized on a polyether maleate modified polypropylene substrate.
[0062] A further aspect of the present disclosure relates to a method for reducing the water contact angle and improving the surface wettability of a contact lens formed by polymerizing a monomer mixture by cast polymerization in a mold composed of polyether modified polyolefin, as previously described, wherein the water contact angle of the resulting contact lens is less than about 90°, preferably less than about 85°, more preferably less than about 80°, even more preferably less than about 75°, even more preferably less than about 70°, and even more preferably less than about 65°, as previously described.
[0063] In addition, the present disclosure provides a single-use mold for making contact lenses, the mold comprising the polyether modified polyolefin composition as described above.The mold may have multiple cavities, for example, four or more cavities, as known in the art.Contact lenses prepared using these molds, especially from the monomer mixtures described above, have low water contact angles as described above.
[0064] The invention will now be described with reference to the following non-limiting examples. EXAMPLES
[0065] Example 1: Preparation of a polyether maleate modified base molding composition Polybond 7200 (SI Group), a polypropylene grafted with 1.5 to 1.9 wt. % maleic anhydride, was selected as the base molding resin. The dried Polybond 7200 was reacted in the melt with an amine-terminated PEO-PPO copolymer (MW approx. 1000 Daltons, Jeffamine M1000 from Huntsman) at 25% molar equivalent using a 16 mm Haake (25 L / D) extruder. The graft reactant was compounded with standard polypropylene, Pinnacle Polymers 1120H, at 20 wt. %, and then molded into plaques. The water contact angle of the Pinnacle polypropylene base polymer was measured to be 96°, while the water contact angle of the Pinnacle polypropylene base polymer compounded with the modified graft polymer was 79°.
[0066] Example 2: Preparation of Contact Lenses A conventional base mixture of reactive monomers containing the following components: MCR-M11 silicone macromer, methacryloxypropyl tris(trimethylsiloxy)silane, dimethylacrylamide in about a 1:1:2 ratio with PEG200DMA as a crosslinker, and 2-hydroxy-2-methylpropiophenone (Darocur 1172) as a photoinitiator was used as a control. The mixture was polymerized on the plaques described in Example 1, and the water contact angle of the cured film was measured. The contact angle of the polymerized contact lens composition film was about 114° for the unmodified control (Pinnacle's propylene-based polymer) versus about 99° for the modified material prepared in Example 1. In this case, the reactive monomer blend with MCR-M11 shows the advantage of using the mold resin of Example 1. Note that the contact angle decreased from 114° to 99°, but 99° is still higher than 90° and is therefore not low enough to achieve acceptable wettability of the contact lenses. This blend containing MCR-M11 is a control for Example 3 in which MCR-M11 was essentially replaced with PEG-modified MCR-M11, demonstrating the ability of polyether-modified polyolefins to introduce greater surface wettability to contact lenses.
[0067] Example 3: Preparation of Contact Lenses Contact lenses were prepared as described in Example 2, except that MCR-M11 was replaced with a copolymer generally described in U.S. Pat. No. 10,669,294 having a DP of 10 and containing about 25 mole % of a comonomer unit having two pendant PEG units, as depicted in Structure 1.
[0068] [ka]
[0069] When polymerized on a polyether modified plaque as described in Example 1, the contact angle of the resulting mixture was about 65°, whereas when polymerized on an unmodified polypropylene control, it was about 97°. A similar, but slightly higher, contact angle of about 74° was observed in a similar example where 50% molar equivalent of maleated polypropylene was compounded at 10% loading, rather than 25% molar equivalent at 20% loading in Example 1.
[0070] Example 4: Preparation of maleamic acid modified polypropylene-polypropylene blend The blends were produced in a two-stage process. A mechanical pellet blend of 80% polypropylene homopolymer (PP) and 20% Pinnacle 1120H with 1.5 to 1.9 wt. % maleic anhydride grafted polypropylene (SI Group Polybond 7200) was melt compounded and pelletized at approximately 210°C using a 27 mm Leistritz (40 L / D) counter-rotating twin screw extruder. The dried pelletized alloy was fed back into a 16 mm Haake TSE (25 L / D) extruder. A room temperature liquid feed of 0.5 molar equivalents of α-amine, ω-methyl terminated polypropylene oxide-polyethylene oxide copolymer MW1000 (Huntsman Jeffamine M1000) was injected downstream of the extruder by a syringe pump. The pelletized extrudate was dried. Analysis showed the formation of reaction products, primarily maleamic acid derivatives of polypropylene. The material was then formed into plaques. The static water contact angle of the plaque was measured to be 62°±3°. The control polypropylene plaque exhibited a contact angle of 96°.
[0071] Example 5: Preparation of methyl-PEG ether modified maleic acid modified polypropylene-polypropylene blend The α-hydroxy, ω-methyl terminated polyethylene oxide was replaced with α-amine, ω-methyl terminated polypropylene oxide-polyethylene oxide under similar conditions as in Example 4. An alloy of PP homopolymer, Pinnacle 1120H with 1.5 to 1.9 wt% maleic anhydride grafted polypropylene (SI Group's Polybond 7200) was melt compounded and pelletized under conditions equivalent to Example 1. Methoxypolyethylene glycol (TCI America's MPEG 1000) was heated to 60°C and fed as a liquid at 0.25 molar equivalents downstream of the extrusion process. A melt temperature of 210 to 230° was maintained at a screw speed of 200 rpm. The modified polypropylene was compounded into Polybond 7200 at 10 wt% loading. The material was formed into a plaque and the sessile water contact angle was measured to be 77°.
[0072] Example 6: Inducing Surface Wettability of a Composition with Utility for Forming Contact Lenses Four compositions corresponding to compositions conventionally used to form contact lenses were cast onto modified polypropylene plaques and polymerized by UV irradiation. Each composition evaluated contained 21.5% silicone macromer; 21.5% (3-methacryloxy-2-hydroxypropoxypropyl)methylbis(trimethylsiloxy)silane; 54.0% dimethylacrylamide; 2.0% bismethacrylate ester of polyethylene oxide MW200, and 1.0% Darocur 1172 photoinitiator.
[0073] The four silicone macromers included α-methacryloxy, ω-butyl terminated polydimethylsiloxane; α-methacryloxy, ω-butyl terminated poly(methoxydiethylene-oxypropyl)-methylsiloxane) homopolymer; α-methacryloxy ω-butyl terminated 50% (methoxydiethylene-oxypropyl)-methylsiloxane) 50% dimethylsiloxane copolymer; and α-methacryloxy ω-butyl terminated 25% (methoxydiethylene-oxypropyl)-methylsiloxane) 75% dimethylsiloxane copolymer. Water contact angles of films prepared from these methacrylate-terminated macromers cast against unmodified polypropylene and two modified polypropylene substrates prepared in a manner similar to that described in Example 1, with the components shown below, were measured and are summarized in the table below. In all cases, the water contact angle was lower on the modified polypropylene than on the unmodified substrate. The macromer with diethylene oxide (PEG) substitution showed a more dramatic decrease in water contact angle, indicating greater wettability.
[0074] [Table 1]
[0075] Example 7: Preparation of modified maleamic acid modified polypropylene Polypropylene polymers containing 1.0 to 1.2 wt.% maleic acid from Mitsubishi Chemical were modified with 100% molar equivalent of α-amine, ω-methyl terminated polypropylene oxide-polyethylene oxide copolymer (MW1000) under the same general conditions as in Example 1. The modified graft copolymers were separately re-extruded at 50 wt.% with polypropylene homopolymer (Novatek MA3 from Mitsubishi Chemical) and random propylene-ethylene copolymer (Wintec WMG03 from Japan Polypropylene). Both the uncompounded homopolymer and random copolymers exhibited water contact angles of about 97°. The 50% homopolymer blend had a contact angle of 89°, while the 50% copolymer blend had a water contact angle of 82°. Infrared analysis showed that the reaction product was primarily polyethermaleamic acid, with observable but unquantified amounts of polyethermaleimide.
[0076] Example 8: Inducing Surface Wettability of a Composition with Utility for Forming Contact Lenses As in Example 6, three compositions corresponding to compositions conventionally used to form contact lenses were cast onto modified polypropylene plaques and polymerized by UV irradiation. Each composition evaluated contained 21.5% silicone macromer, 21.5% (3-methacryloxy-2-hydroxypropoxypropyl)methylbis(trimethylsiloxy)silane, 54.0% dimethylacrylamide, 2.0% bismethacrylate ester of polyethylene oxide MW200 (EGDMA200), and 1.0% Darocur 1172 photoinitiator.
[0077] The three silicone macromers included α-methacryloxy, ω-butyl terminated polydimethylsiloxane; α-methacryloxy ω-butyl terminated 50% (methoxydiethylene-oxypropyl)-methylsiloxane) 50% dimethylsiloxane copolymer; and α-methacryloxy ω-butyl terminated 25% (methoxydiethylene-oxypropyl)-methylsiloxane) 75% dimethylsiloxane copolymer. The water contact angles of films prepared from these methacrylate-terminated macromers cast on unmodified polypropylene and a 10% methyl-PEG ether modified maleic acid modified polypropylene-90% polypropylene blend were as described in Example 5. As shown in the table below, the contact angles of films of the polymerized contact lens composition exhibited a contact angle of about 114° on the unmodified control compared to about 100° for the modified material. When the concentration of methyl-PEG ether modified maleic acid modified polypropylene was increased to 20%, a further decrease in the water contact angle of the film of about 10° was typically observed compared to the other contact lens formulations.
[0078] [Table 2]
[0079] It will be appreciated by those skilled in the art that changes could be made to the embodiments described above without departing from the broad inventive concept. It is understood, therefore, that the invention is not limited to the particular embodiments disclosed, but it is intended to cover modifications within the spirit and scope of the invention as defined by the appended claims.
Claims
1. 1. A method for making a contact lens having a water contact angle of less than about 90°, comprising the steps of: (f) preparing a mold-molding resin containing a polyether-modified polyolefin; (g) forming the molding resin into a mold; (h) preparing a contact lens composition; (i) filling a contact lens composition into a mold; and (j) polymerizing the contact lens composition to form a contact lens. A manufacturing method comprising:
2. 10. The method of claim 1, wherein the polyolefin in the molding resin comprises at least one of polypropylene homopolymer, polypropylene copolymer, polyethylene homopolymer, and polymethylpentene.
3. 3. The method of claim 1 or 2, wherein step (a) comprises preparing a copolymer of a polyolefin and a polyether.
4. 4. The method of claim 1, wherein step (a) comprises reacting a polyether with a maleated graft polymer of a polyolefin.
5. 5. The method of any one of claims 1 to 4, wherein the molding resin comprises a blend of polyether modified polyolefin and unmodified polyolefin resin.
6. 6. The method of claim 5, wherein the polyether modified polyolefin is blended into the unmodified polyolefin resin in an amount of about 5 to 20 weight percent.
7. 7. The method of claim 1, wherein the molding resin further comprises a hydrophilic additive selected from polyetheramines and methoxypolyethylene glycols.
8. 8. The method of any one of claims 1 to 7, wherein the polyether modified polyolefin is a grafted polyolefin or copolymerized polyolefin containing anhydride or carboxylic acid groups, and the hydrophilic additive is present in an amount of about 0.25 to 1.00 molar equivalents relative to the anhydride or carboxylic acid content of the grafted polyolefin or copolymerized polyolefin.
9. The method of claim 1 , wherein the contact lens composition comprises a base monomer, a silicone-containing macromer, and a crosslinker.
10. The method of claim 9 , wherein the silicone-containing macromer comprises at least two polyethyleneoxy groups (PEG).
11. 11. The method of any one of claims 1 to 10, wherein step (e) comprises applying UV radiation or heat to effect polymerization.
12. A method for making a contact lens have a water contact angle of less than 90° and improving surface wettability, the method comprising the steps of casting and polymerizing a mixture of monomers in a mold formed from a molding resin comprising a polyether-modified polyolefin to form a contact lens having a water contact angle of less than about 90°.
13. 13. The method of claim 12, wherein the polyolefin in the molding resin comprises at least one of polypropylene homopolymer, polypropylene copolymer, polyethylene homopolymer, and polymethylpentene.
14. 14. The method of claim 12 or 13, wherein the molding resin comprises a copolymer of a polyether and a polyolefin.
15. 15. The method of any one of claims 12 to 14, wherein the molding resin comprises a polyether reacted with a maleated graft polymer of a polyolefin.
16. 16. The method of any one of claims 12 to 15, wherein the molding resin comprises a blend of polyether modified polyolefin and unmodified polyolefin resin.
17. 17. The method of claim 16, wherein the polyether modified polyolefin is blended into the unmodified polyolefin resin in an amount of about 5 to 20 weight percent.
18. 18. The method of any one of claims 12 to 17, wherein the molding resin further comprises a hydrophilic additive selected from polyetheramines and methoxypolyethylene glycols.
19. 19. The method of any one of claims 12 to 18, wherein the polyether modified polyolefin is a grafted polyolefin or copolymerized polyolefin containing anhydride or carboxylic acid groups, and the hydrophilic additive is present in an amount of about 0.25 to 1.00 molar equivalents relative to the anhydride or carboxylic acid content of the grafted polyolefin or copolymerized polyolefin.
20. 20. The method of any one of claims 12 to 19, wherein the mixture of monomers comprises a base monomer, a silicone-containing macromer, and a crosslinker.
21. The method of claim 20, wherein the silicone-containing macromer comprises at least two polyethyleneoxy groups (PEG).
22. A single-use mold for making contact lenses, the single-use mold comprising a polyether-modified polyolefin composition.
23. 23. The single-use mold of claim 22, wherein the polyolefin in the composition comprises at least one of a polypropylene homopolymer, a polypropylene copolymer, a polyethylene homopolymer, and a polymethylpentene.
24. 24. The single-use mold of claim 22 or 23, wherein the composition comprises a copolymer of a polyether and a polyolefin.
25. 25. The single-use mold of any one of claims 22 to 24, wherein the composition comprises a polyether reacted with a maleated graft polymer of a polyolefin.
26. 26. The single-use mold of any one of claims 22 to 25, wherein the composition comprises a blend of polyether-modified polyolefin and unmodified polyolefin resin.
27. 27. The single-use mold of claim 26, wherein the polyether-modified polyolefin is blended into the unmodified polyolefin resin in an amount of about 5 to 20 weight percent.
28. 28. The single-use mold of any one of claims 22 to 27, wherein the composition further comprises a hydrophilic additive selected from polyetheramines and methoxypolyethylene glycols.
29. 29. The single-use mold according to any one of claims 22 to 28, wherein the polyether modified polyolefin is a grafted polyolefin or a copolyolefin containing an anhydride or carboxylic acid group, and the hydrophilic additive is present in an amount of about 0.25 to 1.00 molar equivalents relative to the anhydride or carboxylic acid content of the grafted polyolefin or copolyolefin.
30. 30. The single-use mold of any one of claims 22 to 29, wherein a contact lens produced from the mold has a water contact angle of less than about 90°.
31. 31. The single-use mold of claim 30, wherein the contact lens is formed from a composition comprising a base monomer, a silicone-containing macromer, and a crosslinker.
32. 32. The single-use mold of claim 31, wherein the silicone-containing macromer comprises at least two polyethyleneoxy groups (PEG).
Citation Information
Patent Citations
Polyetheramine modification of polypropylene
JP2000515903A
Facilitating release of silicone hydrogel ophthalmic lens
JP2007279690A
Inorganic particle composite, and method for manufacturing the same
JP2011068122A
Molds for manufacturing ophthalmic instruments
JP2011502061A
Silicone hydrogel contact lens
JP2013008055A