Electrode wire and its manufacturing method
The electrode wire with a copper-zinc alloy coating and controlled manufacturing process addresses limitations in erosion yield and speed, achieving enhanced machining efficiency and reduced material loss.
Patent Information
- Application Number
- JP2024529878
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2021-11-16
- Filing Date
- 2022-09-29
- Publication Date
- 2024-11-13
AI Technical Summary
Existing electrode wires for electrolytic corrosion processing have limitations in erosion yield and processing speed, despite advancements in materials and topography.
The electrode wire features a central core made of conductive material, coated with a layer of copper-zinc alloy in beta phase, followed by a gamma phase with a high zinc concentration, and optionally a surface layer of even higher zinc concentration, achieved through controlled heating and rapid cooling or electroplating, resulting in a metastable state that enhances mechanical strength and conductivity.
The electrode wire exhibits improved erosion yield and processing speed, with reduced material loss and better surface topography preservation, allowing for faster and more efficient machining.
Smart Images

Figure 2024542236000001_ABST
Abstract
Description
[Technical field]
[0001] The present disclosure relates to an electrode wire that can be used as an electrode wire for electroerosion processing, and to a method for manufacturing the electrode wire. [Background technology]
[0002] Electrode wires are used in electroerosive machines to cut metals or conductive materials by electroerosion.
[0003] The well-known method of electrochemical machining, or spark erosion, can remove material from a conductive part by generating sparks in a machining region between the workpiece and a conductive electrode wire. The electrode wire is continuously unwound near the part along its length held by a guide and gradually translated laterally towards the part by lateral translation of the wire guide or translation of the part.
[0004] A generator connected to the electrode wire by an electrical contact remote from the machining area establishes a suitable potential difference between the electrode wire and the conductive part to be machined. The machining area between the electrode wire and the part is immersed in a suitable dielectric fluid. The potential difference generates a spark between the electrode wire and the workpiece, which gradually erodes the part and the electrode wire. The longitudinal unwinding of the electrode wire ensures that a sufficient wire diameter is always maintained to prevent cuts in the machining area. Relative lateral movement of the wire and the part allows the part to be cut or its surface to be treated, if required.
[0005] Particles detached from the electrode wire and component by the spark are dispersed in a dielectric fluid and discharged.
[0006] Precision machining, especially small radius corner cutting, requires the use of wires with small diameters and capable of withstanding large mechanical tensile strengths in order to provide tension in the machining area and limit the amplitude of vibrations.
[0007] Most of the recent electrolytic processing machines generally use a diameter of 0.25 mm and a tensile strength of 400 N / mm 2 to 1,000N / mm 2 It is designed to use a range of metal wires.
[0008] When a spark occurs between the electrode wire and the part, the surface of the electrode wire is suddenly heated to a very high temperature in a short time. As a result, at the location of the spark, the material of the surface layer of the electrode wire transitions from a solid state to a liquid or gas state and migrates to the surface of the electrode wire and / or is released into the dielectric fluid. The outer surface of the electrode wire where the spark reached is deformed, typically exhibiting a slightly concave crater shape, indicating an area where the material has melted and solidified again.
[0009] It has been observed that the efficiency of the spark for electroerosion depends mainly on the nature and topography of the surface layer of the electrode wire. To this end, significant advances in electroerosion efficiency have been achieved by using electrode wires that include: - a core made of one or more metals or alloys that ensure good conduction of electric current and good mechanical strength to maintain the mechanical tensile strength of the wire; and - Coatings made of one or more other metals or alloys and / or a particular topography (eg cracks) which ensures a better efficiency of electroerosion, eg a higher erosion rate.
[0010] For example, US Patent No. 5,945,010 describes an electrode wire having a brass core covered with a layer of a gamma phase of a copper-zinc alloy, which is optionally covered with a layer of an epsilon phase of a copper-zinc alloy. The application teaches that such a layer of a gamma phase of a copper-zinc alloy can improve the performance of the electrode wire. In particular, the application describes electrode wire sample No. 3, which includes a layer of a gamma phase of a copper-zinc alloy covered with a surface layer of an epsilon phase of a copper-zinc alloy. The thickness of the surface layer is 3 μm. The zinc concentration of the gamma phase of the copper-zinc alloy layer is 68 atomic %. The application also describes electrode wire sample No. 4, which includes a surface layer of a gamma phase of a copper-zinc alloy. In this case, the zinc concentration of the gamma phase of the copper-zinc alloy surface layer is 65 atomic %.
[0011] Prior art is also known from US Patent Application Publication No. 2017 / 259361, US Patent Application Publication No. 2008 / 179296 and US Patent Application Publication No. 2009 / 025959. [Prior art documents] [Patent documents]
[0012] [Patent Document 1] U.S. Patent No. 5,945,010 [Patent Document 2] US Patent Application Publication No. 2017 / 259361 [Patent Document 3] US Patent Application Publication No. 2008 / 179296 [Patent Document 4] US Patent Application Publication No. 2009 / 025959 [Patent Document 5] U.S. Pat. No. 5,762,726 [Patent Document 6] European Patent Application Publication No. 1949995 [Non-patent literature]
[0013] [Non-Patent Document 1] Liang et al.: “Thermodynamic assessment of the Al-Cu-Zn system, part I: Cu-Zn binary system”. CALPHAD, volume 51, 2015, pages 224 to 232 Summary of the Invention [Problem to be solved by the invention]
[0014] The electrode wire of US Patent No. 5,945,010 has high performance. However, an electrode wire having even better performance, particularly at least one of improved erosive yield and improved machining speed, is desired.
[0015] The present disclosure aims to meet this need by proposing an electrode wire as claimed in claim 1.
[0016] Yet another object of the disclosure is a method for manufacturing an electrode wire as claimed in claim 1. [Brief description of the drawings]
[0017] The present disclosure will be better understood from reading the following description, given only by way of non-limiting example, with reference to the drawings, in which: [Figure 1] FIG. 1 is a schematic diagram of a cross section of an electrode wire. [Diagram 2] FIG. 2 is a flow chart of a method for manufacturing the electrode wire of FIG. [Diagram 3] FIG. 3 is a black and white photograph of a portion of a cross section of a wire produced according to the method of FIG. 2 prior to the drawing step. [Figure 4] FIG. 4 is an image of a portion of a cross section of an electrode wire produced according to the method of FIG. 2 after a drawing step. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0018] Throughout these figures, the same reference numerals are used to denote the same elements.Throughout the remainder of this description, features and functions well known to those skilled in the art will not be described in detail.
[0019] Definitions of certain terms are provided below in Section I. Detailed examples of embodiments are described in Section II with reference to the figures. Next, other embodiments of these embodiments are introduced in Section III. Finally, advantages of various embodiments are introduced in Section IV.
[0020] Chapter I: Definitions and Terminology The phrase "an element made from material A" or "an element made of material A" denotes an element in which material A constitutes at least 90% of the weight of the element, preferably at least 95% or 98% of the weight of the element.
[0021] The expression "copper-zinc alloy" denotes an alloy formed exclusively from copper and zinc, excluding unavoidable impurities.
[0022] A "phase" in copper-zinc alloy refers to a solid phase of copper-zinc alloy that exhibits a specific crystal structure. More specifically, the phases of the copper-zinc system are distinguished from one another in terms of their composition and specific crystal structure. This specific crystal structure distinguishes the copper-zinc alloy phases from a simple mixture of copper and zinc particulates with the same overall composition. Representative phases of copper-zinc alloy are the alpha (α), beta (β), gamma (γ), delta (δ), epsilon (ε) and eta (η) phases. The specific crystal structure of a phase can be identified using various means. For example, optical or metallographic micrographs of polished specimens will show different shades of color for each phase, as long as the specimen has been properly chemically treated. Thus, to distinguish between the gamma and epsilon phases, an attack with "Nital", a 3% solution of nitric acid diluted in ethanol, is performed. The gamma phase will then appear gray in low zinc and gray with shades of brown in high zinc. The epsilon phase will appear darker brown. It is also possible to distinguish between the γ and ε phases by observing the sample in a scanning electron microscope using a backscattered electron detector. It is also possible to distinguish the phases of a sample by X-ray diffraction. In this case, a wire sample is placed under an X-ray beam of a precise wavelength. For example, the K α The intensity of the diffraction lines is evaluated at each diffraction angle. The gamma phase has a known x-ray diffraction spectrum that is different from that of other phases in the Cu-Zn system and from zinc oxide, ZnO, which is often located on the wire surface. If the Cu-Zn alloy is not crystallized in at least one of the α, β, γ, δ, ε, or η phases, it is amorphous and the x-ray diffraction spectrum shows flattened bumps rather than prominent peaks.
[0023] At a certain temperature, the various phases of a copper-zinc alloy each correspond to a specific zinc concentration range. The magnitude of each of these specific zinc concentration ranges varies as a function of temperature. The zinc concentration of each phase of a sample can be obtained by compositional microanalysis. Compositional microanalysis is performed using a scanning electron microscope equipped with a spectroscopic probe. An electron beam accelerated in an electric field of, for example, 20 kV strikes the surface of the sample and emits X-rays. These X-rays have an energy spectrum characteristic of the composition of the sample surface struck by the electron beam. The spectrum of the X-rays emitted from the sample surface is measured using an energy dispersive spectroscopy (EDS) or wavelength dispersive spectroscopy (WDS) analytical probe. An algorithm makes it possible to select the elements to be analyzed (thus eliminating the effects of impurities) and to calculate the composition of the sample affected by the electron beam based on the measured spectrum. It should be noted that due to the interaction of X-rays with materials, the volume analyzed by EDS (or WDS) is generally about one cubic micrometer. At the boundary between two phases, it is possible to measure average concentrations that are not actually present in either of the two phases. The concentrations indicated in this case relate to the pure phase of the analyzed volume. The area over which the concentration is measured is larger than a micrometer-sized cube.
[0024] The phrase "the zinc concentration in a region of a copper-zinc alloy is greater than X atomic %" means that the average zinc concentration in this region is greater than X atomic %. The average concentration is obtained, for example, by measuring the zinc concentration at different locations in this region and averaging these concentration measurements. The measurement locations are evenly spaced at locations where the concentration is likely to be lowest, where the concentration is likely to be close to the average, and where the concentration is likely to be highest. Thus, the measurement locations are typically located along an axis passing through the axis of the electrode wire.
[0025] "Conductivity" is defined as 10 6 S / m or more, preferably 10 7 This refers to materials that have a conductivity of S / m or higher.
[0026] The longitudinal axis of a wire is the axis along which the wire primarily extends.
[0027] The expression "cross section" refers to a cross section of an electrode wire perpendicular to its longitudinal axis.
[0028] The expression "layer of the electrode wire" refers to an annular layer of the electrode wire located between an inner circular boundary line and an outer circular boundary line in each cross section of the electrode wire. In reality, these boundaries are not necessarily perfect circles. However, as a first approximation, these boundaries are likened to circles in this specification. Both of these circular boundaries are centered on the longitudinal axis of the electrode wire. The inner circular boundary line is the boundary line of the layer closest to the longitudinal axis of the electrode wire. Conversely, the outer circular boundary line is the boundary line of the layer furthest from the longitudinal axis of the electrode wire. Between these inner and outer circular boundaries, the phase of the copper-zinc alloy is either homogeneous or is formed by a heterogeneous network of different phases of the copper-zinc alloy. Conversely, at the inner and outer circular boundaries, there is an abrupt change in chemical composition and / or crystal morphology.
[0029] A homogeneous layer refers to a layer consisting of a single phase of copper-zinc alloy.
[0030] The expression "homogeneous" layer refers to a layer formed by a material that extends continuously or substantially continuously inside the layer around the axis of the wire in the cross section of the wire. A homogeneous layer therefore does not contain multiple fractures that are divided into multiple regions separated from each other by these multiple radial fractures (fractures, breaks, ruptures) in the cross section of the wire. "Multiple radial fractures" refers to about 10 or more radial fractures that divide the layer into about 10 regions mechanically separated from each other by these radial fractures in the cross section of the wire.
[0031] Conversely, the term "fractured layer" refers to a layer that contains multiple discontinuities that divides the wire in its cross-section into multiple regions separated from one another by multiple radial discontinuities.
[0032] The expression "metallic surface layer" or simply "surface layer" refers to the copper-zinc alloy or zinc layer of the electrode wire, which is the outermost layer of the electrode wire. This metallic surface layer may contain a thin oxide film on its surface. Typically, this oxide film is mainly composed of zinc oxide, zinc hydroxide, zinc carbonate and possible residues such as wire drawing lubricant residues. Thus, the outer surface of this metallic surface layer either coincides with the outer surface of the electrode wire in the absence of the thin oxide film, or is separated from the outer surface of the electrode wire only by this thin oxide film.
[0033] "Radial fracture" refers to fractures that extend primarily radially within the cross-section of the electrode wire.
[0034] The expression "normal temperature" means a temperature ranging from 15°C to 30°C, typically equal to 25°C.
[0035] The "erosion yield" of an electrode wire is equal to the ratio of the surface area cut in one minute to the average intensity of the current passing through the electrode wire in cutting this surface area. For example, if the feed rate of the wire in the cutting material is 2 mm / min in a steel part 50 mm high, the cutting speed is 100 mm / min. 2 When the average machining current is 10A, the erosion yield of the wire under these conditions is 10mm 2 / min / A.
[0036] Chapter II: Example embodiments FIG. 1 shows an electrode wire 2 for electro-erosion processing as described in the introduction of this specification.
[0037] For this purpose, the electrode wire 2 has a resistance of 400 N / mm 2 to 1,000N / mm 2 The electrode wire 2 extends along a longitudinal axis 4, which in this case is perpendicular to the plane of the sheet. The length of the electrode wire 2 is greater than 1 m, typically greater than 10 m or 50 m.
[0038] The electrode wire 2 has an outer surface 6 that is directly exposed to sparks when electroerosion machining is performed with the wire. The outer surface 6 is a cylindrical surface extending along the longitudinal axis 4. The directrix (quadratic curve) of the outer surface 6 is mainly a circle centered on the longitudinal axis 4. The cross section of the electrode wire 2 is therefore circular. The diameter D2 (outer diameter D2) of the electrode wire 2 typically ranges from 50 μm to 1 mm, most often from 70 μm to 400 μm. In this case, the diameter of the electrode wire 2 is equal to 250 μm.
[0039] In this embodiment, the electrode wire 2 includes a central core 10 of a conductive material and a coating 12 deposited directly on the central core 10 .
[0040] The function of the central core 10 is to provide the majority of the tensile strength of the electrode wire 2. A further function of the central core 10 is to provide electrical conductivity for the electrode wire 2. For this purpose, the central core 10 is made of an electrically conductive material. Typically, the central core 10 is made of a metal or metal alloy. For example, in this embodiment, the central core 10 is made of copper.
[0041] Diameter D of central core 10 10 D2 is in the range of 0.75D2 to 0.98D2, typically 0.85D2 to 0.95D2, where D2 is the outer diameter of the electrode wire 2. For example, in this case, the diameter D 10 is equal to 230 μm.
[0042] The coating 12 is designed to increase the machining speed and therefore the erosion yield of the electrode wire 2 and / or the surface quality of the part obtained after electroerosion machining. The quality of the surface cut by electroerosion machining is even better when it exhibits a low roughness.
[0043] The thickness of the coating 12 is low compared to the diameter D2 of the electrode wire 2, i.e. less than 10% of the diameter D2, preferably less than 8% of the diameter D2. The thickness of the coating 12 corresponds in cross section to the shortest distance between the outer surface 6 and the circular boundary line separating the central core 10 from the coating 12.
[0044] In this embodiment, the coating 12 consists of two layers 14 , 16 stacked directly from the central core 10 towards the outer surface 6 , and a possible surface layer 18 deposited directly on layer 16 .
[0045] In the following, the structure of the electrode wire 2 will be described in the presence of the surface layer 18. All the descriptions provided in this particular case also apply in the absence of the surface layer 18. In this case, the surface layer of the electrode wire 2 is directly layer 16.
[0046] Layer 14 is a homogeneous, uniform layer of the beta phase of a copper-zinc alloy. Thus, the zinc concentration in layer 14 is typically between 45 and 50 atomic percent, with the remainder being copper and unavoidable impurities. The thickness of layer 14 is, for example, less than 5 μm.
[0047] Layer 16 is a homogeneous layer of the gamma phase of a copper-zinc alloy. The zinc concentration in layer 16 is high, in this case above the threshold value S 16 This threshold S 16 % or more, preferably 66.4 atomic % or more, 68.4 atomic % or more, or even 70 atomic % or more, the balance being copper and unavoidable impurities. The zinc concentration in layer 16 is typically less than 84 atomic % or less than 75 atomic %.
[0048] According to a recently updated equilibrium diagram for the Cu-Zn system, in a stable state, the gamma phase of a Cu-Zn alloy has a zinc concentration in the range of 60 atomic % to 62 atomic % at room temperature, with the remainder being copper. A recently updated equilibrium diagram for the Cu-Zn system is given, for example, in Liang et al., “Thermodynamic assessment of the Al-Cu-Zn system, part I: Cu-Zn binary system”. CALPHAD, volume 51, 2015, pages 224 to 232.
[0049] Therefore, the threshold S 16 At these zinc concentrations, the gamma phase of the copper-zinc alloy of layer 16 is not in a stable state at room temperature. In this case, it is in a metastable state. In the metastable state, the transformation of the gamma phase of the copper-zinc alloy to a stable state, i.e., the decrease in the zinc concentration, is very slow at room temperature. In other words, this transformation from the gamma phase to a stable state at room temperature is barely perceptible to humans. Therefore, the composition of this metastable gamma phase hardly changes from the time of manufacture until it arrives at the processing area of the electrochemical processing machine, if this electrode wire 2 is stored and transported under normal conditions and maintained at room temperature. A method for producing such a copper-zinc alloy metastable layer is described below.
[0050] The thickness of layer 16 is greater than the thickness of surface layer 18. In FIG. 1, by way of example, the thickness of layer 16 is also greater than the thickness of layer 14. Advantageously, the thickness of layer 16 is greater than 10%, 20% or 30% of the total thickness of coating 12. To this end, the thickness of layer 16 is typically greater than 1% or 2% of diameter D2. For example, the thickness of layer 16 is greater than 2.5 μm, 5 μm or 10 μm. Also, the thickness of layer 16 is very low so that it may be destroyed when drawing the electrode wire. For example, the thickness of layer 16 is less than 25 μm or 20 μm to this end.
[0051] Layer 16 is located less than 1 μm, preferably less than 0.5 μm, from outer surface 6. In this case, layer 16 is separated from outer surface 6 only by surface layer 18. For this purpose, surface layer 18, if present, therefore has a thickness of less than 1 μm, preferably less than 0.5 μm.
[0052] Surface layer 18 is a metallic surface layer that is more zinc-rich than layer 16. For example, surface layer 18 is comprised of a copper-zinc alloy, with the zinc concentration of surface layer 18 being higher than the zinc concentration of layer 16. Typically, the difference in zinc concentration between layers 16 and 18 is greater than 2 atomic %, 5 atomic %, or 10 atomic %. Typically, surface layer 18 is a layer of the ε, δ, or η phase of a copper-zinc alloy, or is comprised of zinc.
[0053] In this embodiment, the layer 16 and the surface layer 18 are broken. Thus, the layer 16 and the surface layer 18 contain fissures (fractures, breaks, fractures) that divide each of these layers into a number of regions that are mechanically separated from one another in cross section by radial breaks. As will be explained below, these fissures are obtained by drawing (drawing, drawing, drawing) a wire in which the layer 16 and the surface layer 18 are homogeneous or substantially homogeneous. After drawing, the same material no longer extends completely continuously around the longitudinal axis 4, but is divided into several regions of material that are mechanically separated from one another in cross section by radial breaks. These fissures extend mainly radially and completely through the layer 16 and the surface layer 18.
[0054] For example, a crack may begin at the circular boundary between layers 14 and 16 and appear at outer surface 6 .
[0055] 1 shows diagrammatically three fractures (fractures, breaks, ruptures) 22-24 that divide the surface layer 18 into three distinct regions 26-28 and the layer 16 into three distinct regions 30-32.
[0056] These cracks correspond to empty recesses or hollows in the solid or liquid material. The width of the cracks in the direction perpendicular to the radial direction in which they extend is generally less than 2 μm. In this case, it should be emphasized that if the thickness of the surface layer 18 is very low, the copper-zinc alloy of the surface layer 18 does not penetrate into the cracks and does not cover these cracks.
[0057] Each region of layer 16 is typically longer than the thickness of layer 16. In this case, each region of layer 16 is longer than 5 μm or 10 μm. The length and width of a region in cross section are defined herein as equal to the length and width, respectively, of a rectangle with the smallest surface area that completely contains this region.
[0058] Chapter II-1 Manufacturing Example Using Rapid Copper Diffusion: Example 1: Rapid diffusion in a tunnel furnace A first example of a method for manufacturing the electrode wire 2 will be described with reference to the flow chart of FIG. 16 % and the surface layer 18 is omitted.
[0059] First, a metal rough wire is provided in step 80. In this example, the metal rough wire is a copper wire with a diameter of 1.25 mm.
[0060] Then, in step 82, a coating is produced on the rough metal wire. This coating covers the entire outer surface of the rough metal wire continuously. It consists of one or several materials capable of forming a layer 16 covered by a more zinc-rich layer in a temperature range between 500° C. and 700° C. In this example, at this stage, the coating is formed only by a zinc layer deposited directly on the outer surface of the rough metal wire. To this end, a zinc layer is deposited on the rough metal wire by an electrolytic galvanizing method, obtaining an electrogalvanized wire with a diameter of 1.25 mm or more.
[0061] In this case, at the end of step 82, the electrogalvanized wire is stretched to a diameter of 420 μm, where in the present embodiment the thickness of the zinc coating is 25 μm in order to obtain a thick layer 16 in which the zinc concentration is easy to measure.
[0062] In step 84, the electrogalvanized and drawn wire is CHeat to a temperature equal to T C is in the range of 500° C. to 700° C. In this embodiment, the temperature T C is in the range of 500° C. to 600° C., and more advantageously in the range of 559° C. to 600° C. The temperature T C By selecting the temperature T C is equal to 600°C.
[0063] For example, in step 84, the electrogalvanized drawn wire is heated to an internal temperature of T C The heat treatment is preferably carried out in air at atmospheric pressure in order to oxidize the outer surface of the electrode wire.
[0064] In this case, the electrogalvanized wire is considered to be very short successive sections of electrogalvanized wire arranged in succession along the longitudinal axis 4. For example, in the present discussion, a short section is a section of length 0.1 mm. Successive sections of the electrogalvanized wire enter the heating zone in succession, and these successive sections are successively heated to a temperature T C More specifically, the heated region is heated to a temperature T C The temperature before the inlet and after the outlet is equal to temperature T C In this case, this heating area is the tunnel of a tunnel furnace.
[0065] Each piece of electrogalvanized wire enters the heated zone at an inlet and moves through the heated zone at a constant speed. Finally, the piece leaves the heated zone at an outlet after remaining in the heated zone for a period d0. The period d0 is equal to the time interval separating: - the moment when a part of the electrogalvanized wire enters the heating zone t ini And, - the instant t0 at which this same portion of electrogalvanized wire leaves the heated area.
[0066] The period d0 is adjusted by setting the travel speed of the electrogalvanized wire in the heating zone. Upon completion of step 84, the entire zinc coating is heated to a temperature T C The entire electrogalvanized wire is passed through the heating zone so that it is heated to a constant temperature.
[0067] As taught in U.S. Pat. No. 5,762,726, the temperature T C In this way, copper gradually diffuses into the zinc coating. Thus, in a portion of the coating that was originally made up of zinc, the copper concentration gradually increases over time.
[0068] Also, because copper diffuses from the rough copper wire outward into the coating, there is a copper concentration gradient in the thickness of the coating. The copper concentration in the coating gradually decreases from the rough copper wire outward. Conversely, the zinc concentration increases as one approaches the outer surface of the rough copper wire. This copper concentration gradient results in an overlay of different phase copper-zinc alloy layers at step 84, with each layer being arranged such that the zinc concentration increases as one approaches the outer surface. Thus, the surface layer of copper-zinc alloy is always the layer with the highest zinc concentration.
[0069] In this case, the purpose of step 84 is to form a layer 16 of the gamma phase of the copper-zinc alloy located less than 1 μm from the outer surface 6 of the electrode wire 2 and having a high zinc concentration.
[0070] When the method described in U.S. Pat. No. 5,762,726 is carried out, the zinc concentration in the γ phase layer of the copper-zinc alloy increases at the moment t optIt is known that the zinc concentration in the gamma phase approaches a maximum value around the moment t when the ε phase is present. This is explained by the fact that, in fact, as long as this ε phase exists, the zinc concentration in the gamma phase approaches that of the ε phase. However, when the ε phase disappears, the zinc concentration in the gamma phase tends to balance with the zinc concentration in the β phase layer of the Cu-Zn alloy that appeared below the γ phase layer of the Cu-Zn alloy. Therefore, when the ε phase layer of the Cu-Zn alloy disappears, the zinc concentration in the γ phase layer of the Cu-Zn alloy drops rapidly. Therefore, the zinc concentration in the γ phase layer of the Cu-Zn alloy decreases at the moment t when the ε phase layer of the Cu-Zn alloy disappears. opt It should be noted that this teaching is not found in U.S. Pat. No. 5,762,726. In fact, this teaching is based on the idea that the optimum opt or moment t opt The '726 patent does not teach that it is advantageous to interrupt the heating of the electrogalvanized wire at a moment very close to the moment t opt On the other hand, to obtain a surface layer of the gamma phase of the Cu-Zn alloy, it is recommended to interrupt the heating well before the moment t opt After a significant amount of time, heating is discontinued.
[0071] Therefore, to take advantage of this observation, in this case, for each piece of electrogalvanized wire, at the moment t 0min From 0max Step 84 is interrupted at a moment t0 between the moment t 0min is the moment when the thickness of the surface layer of the ε phase of the Cu-Zn alloy covering the layer of the γ phase of the Cu-Zn alloy is equal to 1 μm. In fact, when the thickness of the layer of the ε phase of the Cu-Zn alloy is less than 1 μm, the zinc concentration in the layer of the γ phase of the Cu-Zn alloy is maximum or very close to maximum. Also, in order to suppress the deformation of the topography (surface shape) of the outer surface during electrolytic corrosion, it is important that the layer of the ε phase of the Cu-Zn alloy has a low thickness. Moreover, it is known that the erosion yield of the ε phase of the Cu-Zn alloy is lower than the erosion yield of the γ phase of the Cu-Zn alloy.
[0072] Moment 0max is the moment when the surface layer of the ε phase of the Cu-Zn alloy disappears. opt occurs after the moment t optAfter the moment t opt After this, the zinc concentration in the gamma phase layer of the Cu-Zn alloy decreases rapidly, and at the instant t 0max Then, the threshold S 16 Typically, at a moment t 0max is the period d 0max Interval [t ini ;t 0max ] is 1.2*d opt or 1.1*d opt is less than the period d opt is the interval [t ini ;t opt ] duration.
[0073] Therefore, for each piece of electrogalvanized wire, the spacing [t 0min ;t 0max ], step 84 determines whether the zinc concentration in the gamma phase layer of the copper-zinc alloy is S 16 while forming a surface layer of the electrode wire or being covered with a very thin surface layer that is more zinc-rich, i.e. in this case a very thin layer of the ε-phase of the Cu-Zn alloy.
[0074] Typically, the period d0, and therefore the instant t0, is determined by successive experiments. Indeed, as shown in Chapter I, methods exist that allow: 1) the thickness of the layers of the γ and ε phases of the Cu-Zn alloy measured on the cross section of the electrode wire, and 2) The zinc concentration in the gamma phase layer of the Cu-Zn alloy being measured. The period d0 is therefore determined by successively trying several possible values for this period d0.
[0075] Next, the moment t0 is in the interval [t opt ;t 0max ], surface layer 18 is omitted.
[0076] By way of example, it is noted that under these conditions, a duration d0 equal to 10 seconds results in a surface layer of the gamma phase of a copper-zinc alloy having a zinc concentration of 67 atomic %.
[0077] At the end of the period d0, the coating deposited on the copper wire consists of a layer 14 of the β phase of the copper-zinc alloy covered by a surface layer 16 of the γ phase of the copper-zinc alloy.
[0078] At this stage, such rapid heating of the electrogalvanized wire can, for example, heat a coil of electrogalvanized wire, which may contain several thousand turns, to a temperature T C It should be noted that this cannot be obtained by placing the wire in a conventional static furnace heated to a temperature T C The heating rate of a turn of the electrode wire that is mechanically isolated from the heated air by an overlay of another turn is much slower than that of a turn that is in direct contact with the heated air. Thus, the temperature T C By placing the coil in air heated to 100° C. for 10 seconds, only a portion of the electro-galvanized wire is heated rapidly and other portions are heated much more slowly. Thus, only a portion of the electro-galvanized wire contains a layer of the gamma phase of the copper-zinc alloy characteristic of layer 16, while the majority of the electro-galvanized wire, which has been subjected to the slower heating, does not contain a layer of the gamma phase of the copper-zinc alloy with a high zinc concentration. That is, the period d0 of each portion of the electro-galvanized wire cannot be precisely controlled in a conventional static furnace.
[0079] For each section of electrogalvanized wire, as soon as the moment t0 is reached, i.e. in this case from the end of the period d0, a rapid cooling step 90 is carried out. The purpose of the rapid cooling step 90 is to freeze the composition of the layer 16 obtained at the moment t0, so that it is in a metastable state at room temperature. For this purpose, immediately after the moment t0, in step 90, each section of wire is rapidly cooled for a period d1, so that the temperature of the layer 16 of this section drops sharply to 30° C. in less than 10 seconds.
[0080] This cooling is called rapid cooling because the period d1 is less than 10 seconds. Preferably, the period d1 is less than 1 second or 0.5 seconds. To obtain such a short period d1, the cooling rate in step 90 is fast. In this first embodiment, the period d1 is less than 1 second. Therefore, the average cooling rate in the period d1 is (T c −30)° / s or more. Therefore, in this first embodiment, the average cooling rate is 570° C. / s or more.
[0081] In this case, step 90 is applied successively to each of the wire portions leaving the heated zone, so that each portion of the wire undergoes this rapid cooling, thus freezing the zinc concentration of layer 16 over the entire length of electrode wire 2.
[0082] For this purpose, the wire section is immersed in a fluid at room temperature as soon as it leaves the heated zone. For example, in this case, a liquid bath at 25 ° C is installed at the outlet of the heated zone. The liquid is, for example, water. In this case, each section of wire passes through a first section of a trajectory between the outlet of the heated zone and the inlet of the liquid bath, during which this first section is first immersed in air at room temperature. This section of wire then enters the liquid bath at room temperature and passes through a second section of this liquid bath, during which it is in direct contact with the liquid at room temperature. At the end of this second section, the wire section leaves the liquid bath. The length of the first and second sections is adapted such that the temperature of each section of wire falls below 30 ° C within 10 seconds from the moment t0. In this case, each section of wire passes through the first section in less than 1 second. The average cooling rate of the wire section in water at room temperature is about 20,000 ° C / s. Under these conditions, in the manufacture of this first embodiment, the period d1 is less than 1 second.
[0083] At this stage, such rapid cooling, for example, to temperature T CIt should be noted that this cannot be achieved by immersing a coil of electrode wire with several thousand turns, heated to a temperature of 1000° C., in a bath at room temperature, even in a liquid bath. Indeed, in such a case, for reasons similar to those in the case of rapid heating, the cooling rate of a winding of the electrode wire that is mechanically isolated from the liquid by overlapping other windings will be much slower than that of a winding that is in direct contact with the liquid. This means that immersion of the coil of windings in a liquid bath does not allow for precise control of the period d1 during which each part of the electrode wire is cooled.
[0084] At the end of step 90, layer 16 is in a metastable state, and the zinc concentration at room temperature remains below threshold S 16 Greater than.
[0085] Then, in a drawing step 94, the wire obtained at the end of step 90 is drawn (drawn, drawn, drawn) to obtain the electrode wire 2. In this drawing step 94, the diameter of the electrode wire is brought to the desired diameter, in this case a diameter of 250 μm. In the drawing step 94, the layer 16 and the surface layer 18 are broken. Thus, most of the breaks (cracks) located in the layer 16 and the surface layer 18 occur in this drawing step 94.
[0086] 3 is an image of a portion of the cross section of electrode wire 2 obtained at the end of step 90 and before the drawing step 94. The image was obtained using an optical microscope. The composition of layer 16 was measured using an Energy Dispersive Spectroscopy (EDS) spectroscopic probe. The zinc concentration in layer 16 is 67 atomic %.
[0087] FIG. 4 is an image of a portion of the electrode wire 2 obtained upon completion of the drawing step 94. This image was also obtained using an optical microscope. The layer 16 is broken; therefore, it is divided into a number of regions separated from each other by the breaks. This image shows that some of the regions of the Cu-Zn alloy gamma phase may be separated from the outer surface 6 by another region of the Cu-Zn alloy gamma phase. In this case, this region is located more than 1 μm from the outer surface 6. However, the majority of the regions of the Cu-Zn alloy gamma phase, typically more than 70% or 80%, are less than 1 μm from the outer surface 6, in this case less than 0.5 μm. In this document, a "majority" of the regions of the Cu-Zn alloy gamma phase corresponds to more than 50% of the regions of the Cu-Zn alloy gamma phase present in the electrode wire.
[0088] The image also shows that some of these areas may be covered by remnants 100 of the surface layer 18 .
[0089] Example 2: Joule effect heating The fabrication of the second embodiment is the same as that of the first embodiment, with the following exceptions. - The thickness of the zinc is 18μm. - Heating is achieved by the Joule effect; and - The period d0 is the time from moment t0 to t 0min and 0opt , so that the surface layer 18 is present on the manufactured electrode wire.
[0090] In the case of Joule effect heating, the heating area is a segment of electrogalvanized wire located between first and second conductive pulleys polarized by a DC generator. The potential difference between these two conductive pulleys creates a DC current flowing through the segment of electrogalvanized wire located between these two conductive pulleys. The segment of electrogalvanized wire located between these two conductive pulleys is heated by the Joule effect. Typically, the intensity of the DC current is greater than 10 A.
[0091] The various parameters of the Joule effect heating are determined so that the instant t0 of each piece of electrogalvanized wire leaving this heating zone occurs within a predefined interval [t 0min ;t 0max ]. Adjustable parameters of the Joule effect heating are the intensity of the direct current, the potential difference between the two conductive pulleys, the unwinding speed of the electrogalvanized wire and the length of the heating zone of the electrogalvanized wire between the two conductive pulleys. For example, in this case, the length of the heating zone before the electrogalvanized wire enters directly into the water bath at 25° C. is considered to be 1,530 mm. The unwinding speed of the electrogalvanized wire in the heating zone is 4.59 m / min. The intensity of the current flowing in the electrogalvanized wire between the two conductive pulleys is 17.9 A. Under this condition, the period d0 is equal to 20 seconds. In this embodiment, each part of the electrogalvanized wire can enter the water bath before reaching the second conductive pulley and is not immersed in air before being immersed in the water bath.
[0092] The wire obtained after step 90 was analyzed. At some places around the wire, layer 16 is covered with a further zinc-rich copper-zinc alloy layer, while at other places, on the contrary, layer 16 is the only metal alloy present at the surface of the wire. In both cases, zinc oxide is also present at the surface of the wire.
[0093] In areas covered by the zinc-rich layer, layer 16 has a zinc concentration essentially in the range of 65.4 to 69.4 atomic %. In areas not covered by the zinc-rich layer, layer 16 has a zinc concentration essentially in the range of 65.4 to 66.3 atomic %.
[0094] Furthermore, the portion where the zinc-rich layer exists is considered to be the δ phase of the copper-zinc alloy.
[0095] Example 3: Diffusion temperature 700°C The following experiment was performed, and it was found that when the temperature TC was 400°C or higher, the interval [t 0min ;t 0maXThis indicates that a copper-zinc alloy layer having a high zinc concentration cannot be produced by only practicing the teachings of U.S. Pat. No. 5,762,726.
[0096] A copper wire with a diameter of 420 μm and a length of 100 mm coated with 18 μm of zinc was placed in a static furnace at 700°C for a certain period of time, then rapidly removed within 1 second and immersed in water at room temperature.
[0097] When the residence time d0 in the static furnace is set to 6 seconds, a layer of the gamma phase of a copper-zinc alloy with a zinc concentration of 68 atomic % is obtained, and a surface layer 18 of the epsilon phase of a copper-zinc alloy with a thickness of 0.5 μm or less is superimposed on the gamma phase layer. Under the same conditions with a residence time in the static furnace of 7 seconds, the obtained electrode wire does not include the surface layer 18 of the epsilon phase of a copper-zinc alloy, and the zinc concentration of the gamma phase layer of the copper-zinc alloy is only 63 atomic %.
[0098] This was confirmed by carrying out the method of Example 1, - The rough metal wire is a brass wire with a zinc concentration of 37 atomic %. - In step 82, the metal wire is drawn to a diameter of 460 μm, and the zinc coating after drawing is only 5 μm thick. And - Duration d0 is equal to 9 seconds. In this condition, the zinc concentration of the obtained surface layer 16 is 63 atomic %, which is much smaller than 65.4 atomic %. In fact, the thickness of the zinc coating is reduced so that the moment t opt Therefore, if step 84 is interrupted after 9 seconds, the rapid cooling step 90 is triggered too late, and the instant t 0max It will be later.
[0099] Chapter II 2. Examples of manufacturing by slow diffusion of copper Example 4 The manufacturing method is the same as that of the first embodiment, but in step 84, - The thickness of the zinc is 18μm. - Use a static furnace. - Temperature T Cis equal to 250°C. - Duration d0 is equal to 65 minutes. During step 90, the cooling is not rapid.
[0100] In this embodiment, the temperature T C Assuming that is low, i.e. typically below 300°C, the period d0 is sufficiently long so that the heat treatment applied to the electro-galvanized wire is substantially the same in all parts of this electro-galvanized wire, even if the heated electro-galvanized wire is present in the form of a coil having several thousand turns.
[0101] During the rapid cooling step 90, at the exit of the heating zone, the wire is immersed only in ambient air at 25° C., without the need for rapid cooling. In fact, the test is carried out at a temperature T C A low Zn concentration indicates that such rapid cooling of the wire after it leaves the static furnace is not necessary, in other words, the zinc concentration in layer 16 with rapid cooling is the same as the zinc concentration in layer 16 without such rapid cooling.
[0102] Upon completion of the drawing step 94, the resulting wire comprises a surface layer 18 less than 0.5 μm thick. This surface layer 18 is the ε phase of a copper-zinc alloy. The zinc concentration in layer 16 is in the range of 65.3 to 68.3 atomic %. This layer 16 in the γ phase of a copper-zinc alloy appears to be less ductile than a layer of similar composition obtained at 600° C.
[0103] Chapter II 3: Manufacturing with Electroplating Example 5 Fabrication using electroplating involves directly depositing layer 16 by aqueous electroplating without a copper diffusion step.
[0104] For this purpose, the rough metal wire forms the cathode and the anode consists of a mixture of copper and zinc, the zinc concentration of the anode being greater than 65.4 or 77 atomic %. For example, in the tests described herein, the anode is formed from a mixture of copper balls and zinc plates. An electrolytic bath is applied to deposit a layer of the gamma phase of a copper-zinc alloy on the rough metal wire with a high zinc concentration.
[0105] In this example, the bath is an “Oplinger” type bath of 200 liter capacity containing: - water as a solvent, - 12 kg of sodium hydroxide (beads) NaOH, i.e. 60 g / l, - 12 kg of sodium cyanide NaCN, i.e. 60 g / l, - 3.4 kg of copper cyanide, CuCN, i.e. 17 g / l; - 212 kg of zinc cyanide Zn(CN), i.e. 60 g / l, and - 80 g of sodium sulfite Na2SO3, i.e. 0.4 g / l.
[0106] The bath temperature was 45°C and the current density was 20 amperes per square decimeter (20A / dm 2 ) The faradaic yield is about 56%. In this way, a brass wire with a diameter of 0.51 mm was coated with a layer 16 with a thickness of 7 μm.
[0107] EDS analysis of this layer 16 determined that the zinc concentration was 66.4 atomic %.
[0108] The electroplated gamma coated wire was then drawn to a diameter of 0.25 mm.
[0109] The advantage of electroplating a copper-zinc alloy is that its composition is constant through the thickness of the coating, unlike diffusing zinc onto a copper or brass substrate, which has a composition gradient. Thus, the electrode wire produced according to this Example 5 does not include layer 14 and surface layer 18, but only layer 16.
[0110] Example 6 The manufacturing method of Example 6 is similar to that of Example 5, except that the bath was changed to increase the zinc concentration in layer 16. To this end, the bath of Example 5 was replaced by a bath having the following characteristics: - The solvent is water. - The concentration of sodium hydroxide (NaOH) is 90g / l. - The concentration of sodium cyanide (NaCN) is 60 g / l. - The concentration of copper cyanide (CuCn) is 17 g / l. - The concentration of zinc cyanide (Zn(CN)2) is 90 g / l. - The concentration of sodium sulfite (Na2SO3) is 0.6 g / l.
[0111] The zinc concentration in layer 16, determined by EDS analysis, is 82.3 atomic % under the same electroplating conditions.
[0112] When the wire was drawn to a diameter of 0.25 mm, fracture of the coating was observed, which is characteristic of the γ phase of Cu-Zn alloys, not the ε phase of Cu-Zn alloys.
[0113] However, if the coating obtained with the bath shows residues of the ε-phase of the Cu-Zn alloy, these can be reduced or eliminated by lowering the concentrations of NaOH and Zn(CN)2, for example in the range of 60 g / l to 90 g / l.
[0114] Chapter II 4: Performance The erosion yields of different 0.25 mm diameter wires were compared. Each test was carried out under the following conditions. - The electrolytic etching equipment used was manufactured by GFMS (GF Machining Solutions) (reference: "CUT 200 MS"). - The cutting part is a steel block 50 mm high. - The top and bottom nozzles are spaced approximately 5mm apart. - Processing parameters: diameter 0.25mm, tensile strength 900N / mm 2 Standard bare brass wire, plating spray nozzle conditions.
[0115] To avoid wire breakage (to effectively separate the nozzle) and to clearly demonstrate the effect of layer 16, the spark interval was reduced to 25 μs (corresponding to an average intensity of about 6.5 A) to measure the erosion yield. By decreasing the spark interval and increasing the frequency, the maximum cutting speed before breakage of the test wire was measured.
[0116] The electrode wires compared were as follows: Wire A: a wire sold under the trademark "Thermo SA" by Thermocompact® and described in EP 1 949 995 A1, having a brass core (64% copper and 36% zinc by mass) and including a surface layer of gamma phase of a copper-zinc alloy divided into blocks. The zinc concentration of these blocks in the gamma phase is 61.3 atomic %. Wire B: Electrode wire manufactured according to Example 5 above, the zinc concentration in the surface layer 16 being 66.4 atomic %. Wire C: Electrode wire manufactured according to Example 6 above, the zinc concentration in layer 16 being 82.3 atomic %. [Table 1]
[0117] Wire B has a better erosion yield than Wire A. Wire C can withstand a greater machining intensity before breaking, which results in a higher maximum machining speed than the other wires.
[0118] It should be noted that the thickness of the oxide layer of Wire A is about 50 nm, which is favorable for the erosion yield. The oxide layers of Wire B and Wire C are much thinner than this. It is estimated that if the manufacturing conditions of Wire B are modified to obtain an oxide layer with a thickness of about 50 nm, the erosion yield will be even higher.
[0119] Chapter III: Alternative Embodiments Other embodiments of the electrode wire: The central core 10 of the electrode wire 2 does not necessarily have to be made of copper or an alloy containing copper, such as brass. For example, the central core 10 can also be made of steel or another conductive metal. If the central core 10 does not contain copper, the layer 16 is obtained by electroplating.
[0120] The central core 10 does not necessarily have to be made of one metal or one metal alloy. In another embodiment, the central core 10 includes several layers, each of which is made of a metal or metal alloy. For example, the central core 10 includes a central body made of copper or steel coated with a brass layer. The brass layer can be a layer of the beta phase of a copper-zinc alloy.
[0121] Layer 14 may be omitted. This is especially true if layer 16 is produced by electroplating. In other embodiments, layer 16 is uniform and does not break. Thus, layer 16 is formed by a single region that extends continuously around the entire circumference of central core 10. For example, to manufacture this alternative embodiment, during step 82, the electrogalvanized wire is drawn to directly obtain the desired final diameter, and drawing step 94 is omitted. The other steps of the method of FIG. 2, for example, remain unchanged.
[0122] In other embodiments, the surface layer 18 is the δ or η phase of a copper-zinc alloy, or is made of zinc.
[0123] In another embodiment, surface layer 18 is not present and layer 16 forms the surface layer of the electrode wire.
[0124] Another embodiment of the manufacturing method: Numerous other methods for manufacturing the electrode wire 2 are possible. For example, the manufacturing methods involving fast or slow copper diffusion described in chapter II can be carried out with a rough metal wire that is not necessarily made entirely of copper. For example, in another embodiment, the rough metal wire comprises only a surface layer, the copper concentration of which is greater than 50 or 60 atomic % and less than 95 or 90 atomic %. Similarly, it can be carried out with a coating having a zinc concentration less than 100 atomic %. However, preferably, the zinc concentration of the coating is high, i.e. greater than 95 atomic % or 98 atomic %.
[0125] Temperature T for carrying out the manufacturing method with slow copper diffusion C can be selected between 150° C. and 500° C., and the period d0 is the period of time until the selected temperature T C However, it is preferable that the temperature T C is selected to be less than 300° C. or 250° C. or 200° C., so that a static furnace can be used and there is no need to perform rapid cooling. C If T exceeds 300 or 400 °C, a tunnel furnace is used instead of a stationary furnace to better control the durations d0 and d1. In this case, the manufacturing method by slow copper diffusion is performed at a temperature T C The method is the same as that of Example 1, except that the temperature is in the range of 150°C to 500°C, not in the range of 500°C to 700°C.
[0126] The stretching step 94 may be omitted.
[0127] Section IV: Advantages of the Described Embodiments: An electrode wire having a high zinc concentration, but with a region of gamma phase of the copper-zinc alloy less than 1 μm from the outer surface of the electrode wire, has at least one of the following advantages over the electrode wire of US Pat. No. 5,945,010: - improved erosion yield and / or - Maximum erosion speed is increased.
[0128] Here, the performance improvement of the electrode wire of the present disclosure will be described. The layer 16 of the gamma phase has a high zinc concentration, which results in a high melting point and a low sublimation temperature. These two are recognized as the performance improvement of the electrode wire. In addition, the thickness of the zinc-rich surface layer is also less than 0 or 1 μm. In fact, the melting point of the surface layer 18 is lower than that of the layer 16. Therefore, during electrolytic corrosion, this surface layer 18 melts before the gamma phase of the copper-zinc alloy. By reducing the thickness or removing this surface layer 18, the amount of liquid that appears on the surface of the electrode wire during the electrolytic processing method is significantly reduced. As a result, for example, craters resulting from electrolytic sparks have less resolidification area. The electrode wire also loses less material during sparks. In addition, there are fewer breaks or pores hidden by the flow of molten metal. Thus, the surface topography of the electrode wire is better preserved. - Reducing electrode wire consumption by reducing the electrode wire unwinding speed while maintaining good machining speed. - Improve processing speed while maintaining the same rewinding speed.
[0129] Here, in US Patent No. 5,945,010, the layer of the gamma phase of the Cu-Zn alloy of Sample No. 4 has a lower zinc concentration than the layer of the gamma phase of the Cu-Zn alloy of Sample No. 3. However, US Patent No. 5,945,010 teaches that Sample No. 4 has the best performance. Furthermore, the application of US Patent No. 5,945,010 does not teach how to further increase the zinc concentration of the surface layer of Sample No. 4. In particular, the application teaches that the heating of the electrode wire is instantaneous t opt There is no instruction to interrupt it quickly nearby.
[0130] The gamma phase regions of the Cu-Zn alloy are directly flush with the outer surface, further reducing the amount of liquid that appears during galvanic corrosion, further improving the performance of the electrode wire.
[0131] Further increasing the zinc concentration in each region of the gamma phase of the Cu-Zn alloy, especially above 68.4 atomic %, further improves the performance of the electrode wire.
[0132] The copper-zinc alloy layer is destroyed, thereby improving the erosion yield of the electrode wire.
[0133] Advantageously, a diffusion heat treatment at or above 500° C. results in an electrode wire further comprising layer 14 below layer 16 .
[0134] Conversely, if the electrode wire is fabricated with slow copper diffusion, it is not possible to obtain a thicker layer 14 below layer 16. However, the slower diffusion allows a more uniform thickness of layer 16 to be obtained.
[0135] By rapidly cooling layer 16, the decrease in zinc concentration in step 90 can be limited or prevented.
[0136] By depositing layer 16 by electroplating, it is possible to obtain a layer 16 having a zinc concentration of more than 66 or 70 atomic %. Furthermore, the thickness of layer 16 is more uniform.
Claims
1. An electrode wire that can be used as an electrode wire for electroerosion processing, A metal core (10) extending along a longitudinal axis; a coating on a metal core; the coating comprises one or more regions (30-32) of a gamma phase of a copper-zinc alloy; Each region is formed only of the gamma phase of the Cu-Zn alloy. At room temperature (25°C), the zinc concentration in the gamma phase of the Cu-Zn alloy in each region is greater than 65.4 atomic percent. More than 50% of one or more regions (30-32) of the gamma phase of the copper-zinc alloy are located less than 1 μm from the outer surface of the electrode wire; Electrode wire.
2. At room temperature, more than 50% of one or more regions (30-32) of the gamma phase of the copper-zinc alloy are directly flush with the outer surface of the electrode wire; The electrode wire of claim 1 .
3. At room temperature, the zinc concentration in each region (30-32) of the gamma phase of the Cu-Zn alloy is 68.4 atomic % or more; 3. The electrode wire according to claim 1 or 2.
4. At room temperature, the coating is formed in the following order from the outside towards the metal core of the electrode wire: a first surface layer (18) having a zinc concentration of greater than 72 atomic %; a second layer (16) including regions (30-32) of a gamma phase of a copper-zinc alloy; the thickness of the first surface layer is less than 1 μm or 0.5 μm; the second layer is directly beneath the first surface layer; 4. The electrode wire according to claim 1 or 3.
5. The first surface layer (18) is made of an ε phase of a copper-zinc alloy.
5. The electrode wire of claim 4.
6. the coating comprises a third homogenous layer (14) of a copper-zinc alloy consisting exclusively of the β phase of the copper-zinc alloy; The third homogeneous layer (14) is directly beneath the second layer (16); 6. An electrode wire according to claim 4 or 5.
7. the electrode wire has fractures (22-24) that mechanically separate regions of gamma phase of the Cu-Zn alloy in a cross-section of the electrode wire; The electrode wire according to any one of claims 1 to 6.
8. At least one region (30-32) of the gamma phase of the copper-zinc alloy has a thickness perpendicular to the longitudinal axis that is greater than 1% of the outer diameter of the electrode wire; The electrode wire according to any one of claims 1 to 7.
9. More than 50% of the one or more gamma phase regions (30-32) of the copper-zinc alloy have a cross section perpendicular to the longitudinal axis, the cross section having a length greater than 5 μm and a width greater than 4 μm; The length and width of a cross section of one region of the gamma phase of the copper-zinc alloy are equal to the width and length, respectively, of a rectangle of the smallest surface area that completely encompasses the cross section; The electrode wire according to any one of claims 1 to 8.
10. The method includes the step of producing a layer of a gamma phase of a copper-zinc alloy on the metal core, At room temperature (25°C), the layer of gamma phase of the copper-zinc alloy is located less than 1 μm from the outer surface of the electrode wire; Zinc concentration is threshold S 16 is greater than the threshold value S 16 is 65.4 atomic % or more, The method for manufacturing an electrode wire according to any one of claims 1 to 9.
11. The method of claim 10, wherein the step of producing a layer of the gamma phase of the copper-zinc alloy comprises the steps of: a) producing a coating on a rough metal wire comprising a surface layer with a copper concentration of more than 50 atomic % or 60 atomic % that, when heated to a temperature of more than 150°C, is capable of diffusing copper from the surface layer of the rough metal wire into the coating to form a layer of the gamma phase of the copper-zinc alloy (82); b) Then, each successive portion of the metal wire from which the coating is to be produced is subjected to a temperature T C and sequentially heating (84) the This causes a part of the coating of the heated part to be transformed into a layer of the gamma phase of a copper-zinc alloy covered by a further zinc-rich surface layer, and for this purpose each part of the metal wire is heated at a moment t ini At the moment t 0 At the moment t 0 is determined to correspond to the instant when The thickness of the zinc-rich surface layer in the portion of the rough metal wire exiting the heated region is less than 1 μm, or the surface layer disappears; a step (84) in which the zinc concentration in the gamma phase layer of the Cu-Zn alloy in the portion of the rough metal wire exiting the heating zone is still greater than 65.4 atomic %; c) Then, at the said moment t 0 From the moment t 0 and cooling (90) the portion of the rough metal wire exiting the heated zone so as to reduce the temperature of the gamma phase layer of the copper-zinc alloy of the portion of the rough metal wire exiting the heated zone to 30° C. in less than 10 seconds, the cooling step being applied to each portion of the rough metal wire exiting the heated zone.
12. During step b), each portion of the coating is subjected to a temperature T in the range of 500° C. to 700° C. C is heated to The method of claim 11.
13. The step of producing the coating comprises producing a layer with a zinc concentration of more than 98 atomic % directly on a surface layer of a rough metal wire with a copper concentration of more than 50 or 60 atomic %; The method according to any one of claims 10 to 12.
14. 11. The method of claim 10, wherein the step of producing a layer of the gamma phase of the copper-zinc alloy comprises the steps of: a) producing a coating on a rough metal wire having a surface layer with a copper concentration of more than 50 atomic % or 60 atomic % by heating the rough metal wire to a temperature of more than 150° C., thereby diffusing copper from the surface layer of the rough metal wire into the coating, thereby forming a layer of a gamma phase of a copper-zinc alloy; b) The metal wire on which the coating was produced is then heated in a stationary furnace at a temperature T in the range of 150° C. to 300° C. C heating at 0° C. for 10 min at 200° C., whereby a portion of said coating is transformed into a layer of a gamma phase of a Cu-Zn alloy, which layer of the gamma phase of the Cu-Zn alloy is further covered by a zinc-rich surface layer, the thickness of which gradually decreases as heating continues; c) Then, at moment t 0 Step b) is interrupted at a time t 0 is the step corresponding to the next instant, The thickness of the further zinc-rich surface layer on the metal rough wire is less than 1 μm, or the surface layer disappears, and The zinc concentration in the gamma phase layer of the copper-zinc alloy on the metal rough wire is still greater than 65.4 atomic %.
15. The step of producing the layer of gamma phase of the copper-zinc alloy includes electroplating the layer of gamma phase of the copper-zinc alloy on the metal core, the zinc concentration of the layer being 65.4 atomic % or more.
11. The method of claim 10.
Citation Information
Patent Citations
Electrode wire for wire-discharge machining
WO2018211772A1
Electrode wire for electric discharge machining
EP1949995A1
Electrode wire for spark erosion
US20080179296A1
EDM wire
US20090025959A1
Electrode wire for electrical discharge machining and manufacturing method for same
US20170259361A1