Anti-glare anti-reflective coating for displays

A multi-layer coating structure with AG, HR, and AR layers using specific particles enhances durability and optical performance, addressing the limitations of single-layer coatings by improving hardness and abrasion resistance while reducing glare and enhancing visibility.

JP2024542339AActive Publication Date: 2024-11-15シュ ヤオ
View PDF 11 Cites 0 Cited by

Patent Information

Application Number
JP2023572754
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2022-10-20
Filing Date
2023-02-28
Publication Date
2024-11-15
Estimated Expiration
2043-02-28

AI Technical Summary

Technical Problem

Current anti-reflection coatings for displays suffer from high haze, low wear resistance, and limited durability, which affect visibility and wider application due to the use of single-layer wet coatings with low refractive index layers.

Method used

A multi-layer coating structure comprising an anti-glare (AG) coating, a high-refractive (HR) coating, and an anti-reflection (AR) coating, utilizing specific combinations of silica, organic, and inorganic particles, along with nanozirconia and hollow silica, to enhance durability and optical performance.

Benefits of technology

The multi-layer coating integrates anti-glare and anti-reflection functions, improving hardness, abrasion resistance, and optical clarity, reducing glare and enhancing visibility.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024542339000001_ABST
    Figure 2024542339000001_ABST
Patent Text Reader

Abstract

An anti-glare anti-reflective film for displays includes, from bottom to top, a substrate (10), an AG coating (20), an HR coating (30), and an AR coating (40). The anti-glare AG coating (20), a high refractive HR coating (30), and a low refractive AR coating (40) are combined in a manner that defines a hierarchical structure. The components and morphology of the inorganic wear-resistant particles in the AG coating (20) are defined, and these are dispersed in a binder resin to achieve functions such as improving anti-glare and wear resistance. The particle size and morphology of the silica are defined, and the aggregated morphology partially forms an uneven shape on the coating surface after curing, and partially exists inside the coating, thereby improving the anti-glare effect.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to the technical field of films, specifically to anti-glare anti-reflective films for displays. [Background technology]

[0002] For example, display devices such as cathode ray tube displays (CRT), plasma displays (PDP), electroluminescent displays (ELD) and liquid crystal displays (LCD) are usually provided with an anti-reflection film on the outer surface of the display device to prevent a decrease in contrast due to reflection of external light and to prevent external light from being reflected and entering an image.

[0003] Anti-reflection coating, also called AR coating, is based on the wave nature of light and the phenomenon of interference, and its main function is to reduce or eliminate the reflected light on the surface of optical elements, thereby increasing the light transmittance of these elements and reducing or eliminating the stray light of the system. Anti-reflection coating occupies a very important position in the optical thin film industry.

[0004] In general, anti-reflection films are formed by using a chemical vapor deposition (CVD) method or a physical vapor deposition (PVD) method on a transparent thin film substrate, as in the conventional Patent Document 1, to form a multi-layered anti-reflection layer. A combination of a high refractive index layer and a low refractive index layer can realize wideband anti-reflection. This technology has been realized in dry coating, but dry coating has the disadvantages of having to form a film in a vacuum, which requires a complex structure for production equipment, high capital investment, and low productivity. For this reason, in recent years, wet coating technology, which allows low-cost coating over a large area and continuous production, has been attracting attention. However, in the current conventional technology, as in Patent Documents 2-3, for example, single-layer anti-reflection films are the mainstream in wet coating.

[0005] In the field of wet coating, there is a problem that the film layer has high haze and cannot be used.

[0006] The light emitted by the liquid crystal display device itself and the reflected light from the display screen of the light source in the environment overlap each other to form glare, which not only affects the human eye for a long time, causing visual discomfort, but also may cause visual impairment if the glare is strong. Therefore, an anti-glare film (AG film) is attached to the surface of each liquid crystal display device on the market, and such a cured film must also have high abrasion resistance. For example, the anti-glare cured film for electronic whiteboards must also have a good flash point and writing effect.

[0007] Therefore, current displays are required to have not only an optical film with anti-reflection function on the surface, but also an optical film with anti-glare function, which can provide better visibility. In addition, the coating applied to the display cover plate needs to have high hardness and good wear resistance, but currently, the low refractive index layer produced by wet coating technology has low hardness, only reaching a maximum of 500g / 1H, and also has low wear resistance, only reaching 100g / 10 times. This also limits the wider application of anti-reflection films. [Prior art documents] [Patent documents]

[0008] [Patent Document 1] China Patent Application Publication No. 104614787 [Patent Document 2] Chinese Patent No. 1322338 [Patent Document 3] Taiwan Patent No. I515271 Summary of the Invention

[0009] In order to solve at least one of the above technical deficiencies, the present invention provides the following technical solution:

[0010] The anti-glare anti-reflection coating for a display of the present application includes a substrate, an AG coating, an HR coating, and an AR coating, which are arranged in this order from bottom to top, The AG coating comprises a binder resin, silica particles, organic particles, and inorganic wear-resistant particles, the silica particles being aggregate particles of 100 nm-3000 nm, the organic particles being one or more of polymethyl methacrylate microparticles, polystyrene microparticles, polymethyl methacrylate-polystyrene copolymer microparticles, and polysilsesquioxane microparticles, the inorganic wear-resistant particles being formed of one or more of nano alumina, nano zirconia, nano diamond, and hexagonal boron nitride nanosheets, the inorganic wear-resistant particles being aggregate particles of 50-200 nm, The refractive index of HR coating is 1.53-1.74, The refractive index of the AR coating is 1.2-1.48.

[0011] In this proposal, anti-glare AG coating, high refractive index HR coating, and low refractive index AR coating are combined in a hierarchical structure to integrate anti-glare and anti-reflection functions.

[0012] In AG coating, the composition and shape of inorganic wear-resistant particles are limited and dispersed in binder resin to play a role of improving anti-glare and wear resistance. Silica with limited particle size and shape is preferred, and aggregated silica forms unevenness on the coating surface after partial curing, and some of it exists inside the coating, thereby improving the anti-glare effect. Preferably, organic particles exist inside the coating, improve the internal haze, reduce the re-aggregation of silica particle aggregates, reduce the filling resin, and adjust the refractive index difference between the particles and the resin, achieving a balance between the internal and external haze, and the film produced by the coating has improved performance such as hardness and wear resistance, and the film layer has advantages such as high resolution, low flash point, and good whitening suppression.

[0013] Further, the coating includes a binder resin and inorganic metal oxide particles having a refractive index of 2.0-2.8, the inorganic metal oxide particles being aggregated in the coating to have a particle diameter of 10-80 nm, the inorganic metal oxide particles being nano-zirconia or titanium oxide; The AR coating contains a binder resin and hollow silica particles with a refractive index of 1.15-1.40.

[0014] The addition of morphologically defined inorganic metal oxides to HR coatings reduces haze and contributes to improving the resolution and mechanical performance of the film layer. Hollow silica is added to AR coatings to adjust the refractive index, and the film layers made of the above hierarchical and component layers are stably bonded, resulting in new advances in hardness, abrasion resistance, and other performance.

[0015] Further, the AG coating contains, by weight, 22-45 parts of binder resin, 3-7 parts of silica particles, 1-3 parts of organic particles, and 1-3 parts of inorganic wear-resistant particles; The HR coating contains, by weight, 40-200 parts binder resin, 20-75 parts nano-zirconia particles, The AR coating contains, by weight, 9-25 parts binder resin and 30-80 parts hollow silica particles.

[0016] The ratio of the amounts of the binder resin and the functional particles is the basic component constituting the coating, and auxiliary agents such as lubricants, antifoaming agents, and leveling agents, and hardeners for hardening and molding can be freely added as necessary.

[0017] Furthermore, the binder resins in the coating liquid components of the curable molding AG coating, the coating liquid components of the curable molding HR coating, and the coating liquid components of the curable molding AR coating all contain a photocurable oligomer resin having six or more functional groups, and a photocurable diluent monomer resin having three or more functional groups, The photocurable oligomer resin is one or more of polyurethane acrylate oligomer, epoxy acrylate oligomer, polyester acrylate and polyether acrylate, polyacrylic resin oligomer, epoxy resin polymer, oxygen-containing acrylate, uric acid acrylate; The light curable diluted monomer resin is one or more of ethyl methacrylate, ethylhexyl methacrylate, styrene, methylstyrene, N-vinylpyrrolidone monofunctional monomer, polymethylolpropane trimethacrylate, diethylene glycol dimethacrylate, tripropylene glycol dimethacrylate, 1,6-hexanediol dimethacrylate, hexanediol methacrylate, pentaerythritol trimethacrylate, dipentaerythritol hexamethacrylate, neopentyl glycol dimethacrylate.

[0018] The resin component preferably has a limited structure, is convenient for photocuring and molding, and contributes to improving the hardness, flexibility, etc. of the coating.

[0019] Further, the AR coating comprises 2-8 parts of fluorine-containing polymer, 5-30 parts of inorganic particles, and 5-23 parts of POSS. The inorganic particles are one or more of magnesium fluoride, boron nitride, silica, and alumina, the fluorine-containing polymer is one or more of partially fluorinated acrylate silicone copolymer, partially or fully fluorinated acrylic compound, and partially or fully fluorinated vinyl ether, and the POSS is one or more of phenyl POSS, amino POSS, vinyl POSS, and acrylic POSS. The fluorine-containing polymer mainly plays a role of increasing the water contact angle and improving the abrasion resistance of the coating film, the POSS plays a role of improving the hardness of the AR coating, and the inorganic particles play a role of improving the abrasion resistance of the AR coating.

[0020] In addition, the AG coating preferably contains, by mass percentage, 18%-38% photocurable oligomer resin with 6 or more functional groups, 4%-7% photocurable dilution monomer resin with 3 or more functional groups, 3%-7% silica particles, 1%-3% organic particles, 1%-3% inorganic wear-resistant particles, 1%-5% auxiliary agent, and 1%-3% photoinitiator, and the solid content in the AG coating is 42%-55%; The HR coating contains, by mass percentage, 1%-2% photocurable oligomer resin with 6 or more functional groups, 0.3%-1% photocurable dilute monomer resin with 3 or more functional groups, 1%-3% nano zirconia particles, 0.05%-0.2% auxiliary agent, and 0.1%-0.5% photoinitiator, and the solid content in the HR coating is preferably 3%-6%.

[0021] The AR coating contains, by weight, 0.25%-0.5% 6+ functional photocurable oligomer resin, 0.05%-0.1% 3+ functional photocurable diluent monomer resin, 0.3%-1.5% hollow silica particles, 0.1%-1% solid silica particles, 0.1%-1% POSS, and 0.1%-0.5% photoinitiator. The solid content in the AR coating is preferably 2.0%-5.0%.

[0022] The coating material with the above-mentioned component ratio is preferably photocured and molded, and when used, each coating material is coated by known coating techniques such as slit coating, microgravure coating, blade coating, roll coating, etc., and then cured by one or a combination of two of ultraviolet curing, electron radiation curing, and heat curing. The ultraviolet curing method is preferred because it has the advantage of having more selectable raw materials.

[0023] Examples of the auxiliary include a wetting leveling agent, an antifoaming agent, a polymerization inhibitor, and a surface control agent. Examples of the photoinitiator include acetophenones, benzophenones, thioxanthones, benzoin, and benzoin methyl ether. When an aromatic diazonium salt, an aromatic sulfonium salt, an aromatic iodonium salt, a metallocene compound, or a benzoin sulfonate ester is used, an active organic amine such as triethylamine or n-butylamine may be blended as a co-initiator.

[0024] Each of the above coatings is prepared by mixing the corresponding components using a solvent. The solvent used includes, for example, polar solvents and non-polar solvents, specifically selected from acetone, methyl ethyl ketone, methyl isobutyl ketone, cyclohexanone, methyl acetate, ethyl acetate, propyl acetate, butyl acetate, methyl formate, ethyl formate, propyl formate, butyl formate, methanol, ethanol, propanol, isopropanol, isobutanol, propylene glycol methyl ether, and n-butanol, and preferably selected from methyl isobutyl ketone, propylene glycol methyl ether, isobutanol, ethyl acetate, and butyl acetate. The solvent may be a single solvent, or a mixed solvent of three or more kinds.

[0025] Furthermore, in AG coating, the silica particles are added as a dispersion liquid, and mixed with a solvent to obtain a silica particle dispersion liquid with a secondary particle diameter of 100nm to 2000nm, with a primary particle diameter of 10nm to 50nm.

[0026] The inorganic wear-resistant particles are added as a dispersion, with a primary particle size of 10-50 nm, and mixed with a solvent to obtain a dispersion with secondary particle sizes of 50-200 nm.

[0027] The particle size of the organic particles is 1 μm to 10 μm.

[0028] By limiting the particle morphology and the type of addition, it was found through testing that this contributes to further improving the membrane layer performance.

[0029] In addition, the average particle size of nano-zirconia particles is 5%-80% of the thickness of the HR coating, the average particle size of hollow silica is 50-80nm, and the average particle size of solid silica is 30%-100% of the thickness of the AR coating, which contributes to improving the membrane layer performance.

[0030] Furthermore, the inorganic wear-resistant particles are formed by pre-treating a hexagonal boron nitride nanosheet, and in the pre-treatment step, a hexagonal boron nitride nanosheet having a primary particle size is stirred and mixed with a solvent and subjected to ultrasonic dispersion treatment to obtain a colloidal liquid, and the colloidal liquid is centrifuged to obtain a primary bottom solid; Repeat the above pretreatment process on the primary bottom solid to obtain a secondary bottom solid; The above pretreatment process is repeated on the secondary bottom solid, and the resulting centrifugal liquid, the dispersion of inorganic wear-resistant particles, is collected. Designing the preparation process of the dispersion according to the purpose can contribute to uniform distribution and further improve the performance of the membrane layer.

[0031] Hexagonal boron nitride nanosheets can be obtained by known production methods, such as the arc discharge method, the solvothermal method, the vapor deposition method, and the liquid phase method. Nanoparticles have high surface energy and tend to aggregate, so their surfaces must be treated with, for example, a polymer dispersant or a coupling agent. The surface treatment agent is preferably a silane coupling agent having a reactive functional group that can contribute to the reaction of the resin.

[0032] Furthermore, the nano-zirconia particles are one or a mixture of two or more of a tetragonal crystal type and a cubic crystal type. The crystal type is limited, which contributes to improving the performance of the film layer.

[0033] Furthermore, the nano-zirconia particles are added as a dispersion to the coating solution used to form the HR coating, and the dispersion of nano-zirconia particles is prepared as follows.

[0034] First, a zirconium-containing compound is mixed with a solvent and an organic acid mixture in a predetermined ratio, heated to 250-320°C, and reacted at a constant temperature for 3-18 hours. Then, the filtrate obtained from the reaction is washed multiple times to obtain tetragonal or cubic nano-zirconia particles; The nano-zirconia particles and dispersion aid obtained are then added to a solvent and processed to obtain a transparent nano-zirconia dispersion liquid, in which the nano-zirconia particles form an aggregated state with a secondary dispersion particle diameter of 10-50 nm.

[0035] The nano-zirconia is a crystalline nano-zirconia produced by a solvothermal one-step synthesis method. The raw material is a zirconium-containing compound and an organic solvent, or a mixture of an organic solvent and an organic acid. The zirconium-containing compound may be an organic zirconium compound including zirconium n-propoxide, zirconium n-butoxide, zirconium tetra tert-butoxide, etc., or an inorganic zirconium compound including zirconium nitrate, zirconium chloride, basic zirconium carbonate, etc., preferably an organic zirconium compound, more preferably zirconium n-propoxide. The organic solvent includes methanol, ethanol, butyl ether, benzyl alcohol, etc., preferably methanol, ethanol, benzyl alcohol, and the organic acid includes formic acid, decyl acid, stearic acid, oleic acid, etc., preferably formic acid, oleic acid.

[0036] The solvent used in the nanozirconia dispersion may be a polar solvent or a nonpolar solvent, such as n-hexane, toluene, ethanol, butyl acetate, ethyl acetate, isopropanol, isobutanol, acetone, butanone, methyl isobutyl ketone, propylene glycol methyl ether, etc., and preferably toluene, butyl acetate, isopropanol, isobutanol, methyl isobutyl ketone, propylene glycol, methyl ether, etc.

[0037] When preparing this nano-zirconia dispersion, it is necessary to add an appropriate amount of a dispersing aid. The dispersing aid may be a silane coupling agent, a titanate coupling agent, a high molecular weight polymer having surface affinity, an acrylate monomer, or an acrylate oligomer. It is preferable to disperse the zirconia powder with a high molecular weight polymer having surface affinity and an acrylate monomer.

[0038] In this process, the process flow and reaction temperature are limited, which contributes to obtaining nano-zirconia with the desired morphology.

[0039] Furthermore, the thickness of the AG coating is 2-50 μm, and the water contact angle of the surface of the AG coating is less than 80°, and the optical thickness of the HR coating is 1 / 2λ 0 and the optical thickness of the AR coating is 1 / 4λ 0 It is.

[0040] By defining the optical thickness relationship of the coating, a broadband anti-reflection coating with a W-shaped reflectance curve is obtained.

[0041] The substrate may be one of triacetyl cellulose film (TAC), polyethylene terephthalate film (PET), polynorbornene film (COP), polymethyl methacrylate film (PMMA), polycarbonate film (PC), transparent polyimide film (CPI), etc., but triacetyl cellulose film (TAC) is preferred from the viewpoints of transparency and optical retardation. The thickness of the substrate is preferably 25 μm-300 μm, and when used as a polarizing plate surface protection film, it is preferably 25 μm-80 μm from the viewpoint of thinning.

[0042] Compared with the prior art, the beneficial effects of the present invention are as follows:

[0043] The film layer of the present invention integrates anti-glare and anti-reflection functions, and the film layer has the advantages of high resolution, low flash point, good whitening inhibition, high hardness, abrasion resistance and so on. [Brief description of the drawings]

[0044] In order to more clearly describe the technical solutions in the embodiments of the present invention, the drawings used in the description of the embodiments will be briefly described below. Obviously, the drawings in the following description are only some embodiments of the present invention, and those skilled in the art can obtain other drawings based on these drawings without creative labor. [Figure 1] An explanatory diagram of the layer structure of the AG-HR-AR film. [Diagram 2] 4 shows the transmittance and reflectance spectra of the AG1-HR1-AR1 film of Example 1. [Diagram 3] Transmittance and reflectance spectra of the AG2-HR1-AR1 film of Example 2. [Figure 4] Transmittance and reflectance spectra of the AG1-HR1-AR2 film of Comparative Example 1. [Diagram 5] Transmittance and reflectance spectra of the AG1-AR1 film of Comparative Example 2. [Figure 6] Cross-sectional view of the AG layer of the AG1-HR1-AR1 film of Example 1 taken by a scanning electron microscope. [Figure 7] FIG. 2 is an enlarged cross-sectional view of the AG layer of the AG1-HR1-AR1 film of Example 1 taken by a scanning electron microscope. [Figure 8] FIG. 2 is a cross-sectional view of the AR layer of the AG1-HR1-AR1 film of Example 1 taken by a scanning electron microscope. [Figure 9] Electron microscope photograph of crystalline nano-zirconia of Example 7. [Figure 10] XRD pattern of crystalline nano-zirconia of Example 7. [Figure 11] FIG. 13 is a particle size distribution diagram of the zirconia dispersion of Example 7.

[0045] The symbols are as follows:

[0046] 10 Substrate, 20 AG coating, 21 Organic fine particles, 22 Silica particle aggregates, 23 Inorganic wear-resistant particle aggregates, 30 HR coating, 31 Nano-zirconia particle aggregates, 40 AR coating, 41 Hollow silica particles, 42 Solid silica particles DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0047] The present invention will now be further described with reference to the drawings and specific examples.

[0048] 1. Preparation of Crystalline Nano-zirconia Dispersion Example 1. Preparation method of crystalline nano-zirconia dispersion: Zirconium n-propoxide and benzyl alcohol are added to the kettle in a mass ratio of 0.6:1 (the total volume of the reactants does not exceed 60% of the volume of the kettle), the rotation speed is set to 450 rpm, and the maximum temperature of the kettle is set to 275°C. After the reaction is completed, the obtained powder is washed with ethanol and propylene glycol methyl ether multiple times (three times each), and then propylene glycol methyl ether is used as the solvent and a high molecular weight polymer (pigment affinity group-containing copolymer DISPERBYK2014, purchased from BYK) is used as a dispersion aid to ultrasonically disperse the zirconia powder to obtain a nano-zirconia dispersion with a solid content of 20%. The dispersed particle diameter of the nano-zirconia is 57 nm, the primary particle diameter of the nano-zirconia is 5-10 nm, and the XRD measurement shows that the crystal type of the nano-zirconia is a mixture of tetragonal and cubic.

[0049] Example 2. Preparation method of crystalline nano-zirconia dispersion: Zirconium n-butoxide and diacetone alcohol are added to the kettle in a mass ratio of 0.56:1 (the total volume of the reactants does not exceed 60% of the volume of the kettle), the rotation speed is set to 450 rpm, and the maximum temperature of the kettle is set to 275°C. After the reaction is completed, the obtained powder is washed with ethanol and MIBK (methyl isobutyl ketone) multiple times (three times each), and then the zirconia powder is ultrasonically dispersed using MIBK as the solvent and a high molecular weight polymer (pigment affinity group-containing structured copolymer DISPERBYK-2013, purchased from BYK) as a dispersion aid to obtain a nano-zirconia dispersion with a solid content of 20%. The dispersed particle size of nano-zirconia is 42 nm, the primary particle size of nano-zirconia is 8-12 nm, and the XRD measurement shows that the crystal type of nano-zirconia is a mixture of tetragonal and cubic.

[0050] Example 3. Preparation method of crystalline nano-zirconia dispersion: Basic zirconium carbonate and n-hexanol are added to the kettle in a mass ratio of 0.62:1 (the total volume of the reactants does not exceed 60% of the kettle volume), the rotation speed is set to 450 rpm, and the maximum temperature of the kettle body is set to 275°C. After the reaction is completed, the obtained powder is washed with ethanol and MIBK (methyl isobutyl ketone) multiple times (three times each), and then, using MIBK as the solvent and a high molecular weight polymer (pigment affinity group-containing structured copolymer DISPERBYK-2013, purchased from BYK) as a dispersion aid, the zirconia powder is ultrasonically dispersed to obtain a nano-zirconia dispersion with a solid content of 20%. The dispersed particle size of nano-zirconia is 45 nm, the primary particle size of nano-zirconia is 8-12 nm, and the XRD measurement shows that the crystal type of nano-zirconia is a mixture of tetragonal and cubic.

[0051] Example 4. Preparation method of crystalline nano-zirconia dispersion: Zirconium n-butoxide and benzyl alcohol are added to the kettle in a mass ratio of 0.48:1 (the total volume of the reactants does not exceed 60% of the volume of the kettle), the rotation speed is set to 450 rpm, and the maximum temperature of the kettle is set to 275°C. After the reaction is completed, the obtained powder is washed several times with ethanol and MIBK (methyl isobutyl ketone) in sequence (three times each), and then the zirconia powder is ultrasonically dispersed using MIBK as the solvent and a high molecular weight polymer (pigment affinity group-containing structured copolymer DISPERBYK-2013, purchased from BYK) as the dispersion aid to obtain a nano-zirconia dispersion with a solid content of 20%. The dispersed particle size of the nano-zirconia is 45 nm, the primary particle size of the nano-zirconia is 8-12 nm, and the XRD measurement shows that the crystal type of the nano-zirconia is a mixture of tetragonal and cubic.

[0052] Example 5. Preparation method of crystalline nano-zirconia dispersion: A mixture of zirconium nitrate, urea and water is added to a kettle in a mass ratio of 0.48:1 (the total volume of the reactants does not exceed 60% of the volume of the kettle), the rotation speed is set to 450 rpm, and the maximum temperature of the kettle is set to 270°C. After the reaction is completed, the obtained powder is washed several times with ethanol and MIBK (methyl isobutyl ketone) (three times each), and then, using MIBK as a solvent and a high molecular weight polymer (pigment affinity group-containing copolymer DISPERSANT-2008, purchased from BYK) as a dispersion aid, the zirconia powder is ultrasonically dispersed to obtain a nano-zirconia dispersion with a solid content of 20%. The primary particle size of the nano-zirconia is 20-25 nm, and XRD measurement shows that the crystal form of the nano-zirconia is a mixture of monoclinic and tetragonal. Because the reaction takes place in an aqueous solution, it is difficult to completely remove the water in post-treatment, and the resulting dispersion has large secondary particle sizes exceeding 100 nm, and is somewhat cloudy and not transparent.

[0053] Example 6. Preparation method of crystalline nano-zirconia dispersion: Zirconium tetra tert-butoxide and benzyl alcohol are added to the kettle in a mass ratio of 0.6:1 (the total volume of the reactants does not exceed 60% of the volume of the kettle), the rotation speed is set to 450 rpm, and the maximum temperature of the kettle is set to 300 ° C. After the reaction is completed, the obtained powder is washed with ethanol and propylene glycol methyl ether multiple times (three times each), and then propylene glycol methyl ether is used as the solvent and a high molecular weight polymer (pigment affinity group-containing copolymer UNIQ-SPERSE670U, purchased from AllnexGroup, Germany) is used as a dispersion aid to ultrasonically disperse the zirconia powder to obtain a nano-zirconia dispersion with a solid content of 20%. The primary particle size of the nano-zirconia is 15-25 nm, and XRD measurement shows that the crystal type of the nano-zirconia is mainly cubic. Nano-zirconia prepared at too high a reaction temperature has a large primary particle size and is more difficult to disperse; the nano-zirconia dispersion prepared under these conditions has a secondary particle size of more than 100 nm and is slightly cloudy and not transparent.

[0054] The results of the above examples and comparative examples show that the selection of different raw materials and solvents affects the primary particle size and crystal type of nano-zirconia, and the dispersed particle size of the obtained nano-zirconia is larger. If this nano-zirconia dispersion is selected and added to the HR coating, the transmittance of the coating will be lower, the haze will be higher, and the refractive index of the coating will be affected (see Comparative Example 3 below). 2. Preparation of Dispersion Silica particle dispersion: The dispersion is prepared by crushing commercially available solid silica particles (without surface treatment) with a primary particle diameter of 10-50 nm in an ethanol solvent using a ball mill method to obtain a silica particle dispersion with a secondary dispersed particle diameter within a specified range. The secondary dispersed particle diameter can be adjusted by adjusting the solvent ratio, crushing parameters, etc., but this will not be explained here.

[0055] Inorganic wear-resistant particle dispersion: First, in the pretreatment process, deionized water and ethanol are mixed in a volume ratio of 1:1, and a commercially available hexagonal boron nitride nanosheet (without surface treatment) with a primary particle size of 10-50 nm is added while stirring, stirred for 6-24 hours, and ultrasonically dispersed for about 10 minutes. Furthermore, the centrifuge speed is set to 6000-10000 rpm, and the dispersion is centrifuged for 5-10 minutes, the supernatant liquid is discarded, and the lower layer precipitate (primary bottom solid) is left.

[0056] Next, the above pretreatment steps (mixing with solvent, stirring, ultrasonication, centrifugation) are repeated with the primary bottom solid to obtain a secondary bottom solid for use.

[0057] Finally, the above pretreatment process is carried out on the solvent (propylene glycol methyl ether) and the above secondary bottom solid to obtain a nano hexagonal boron nitride dispersion, which is a centrifugal colloidal liquid.

[0058] The above pretreatment process is continued on the obtained bottom sediment, the centrifugal colloid liquid is recovered, and the above pretreatment process is performed on the centrifuged bottom solid sediment until the bottom sediment disappears, and the recovered centrifugal colloid liquid is a nano hexagonal boron nitride dispersion liquid.

[0059] 3. Preparation of coating solution used for coating Preparation of coating solution AG1 used for coating: 10 kg of coating solution is prepared. Here, in terms of mass percentage, 10-functional polyurethane acrylate oligomer (JD8098 purchased from Shanghai Yangshi Industrial Co., Ltd.) accounts for 28%, 6-functional polyurethane acrylate oligomer (EB1290 purchased from Allnex Group, Germany) accounts for 3%, 3-functional acrylate monomer (pentaerythritol triacrylate) accounts for 3%, 6-functional acrylate monomer (dipentaerythritol hexaacrylate) accounts for 3%, thiol-based polymerization inhibitor (butylthiopentaerythritol) accounts for 2%, silica with a dispersed particle diameter of 240 nm accounts for 8%, and polysilsesquioxane microparticles (DF20A purchased from Changxing Special Materials (Suzhou) Co., Ltd. 0) accounts for 0.5%, hexagonal boron nitride nanosheets with a dispersed particle size of 80 nm account for 2%, a photoinitiator (photoinitiator 184, purchased from Shanghai Yinchang New Materials Co., Ltd.) accounts for 2%, and a mixed solvent of butyl acetate and isobutanol (butyl acetate accounts for 75% and isobutanol accounts for 25% by volume) accounts for the other proportions. Each component is added to the mixed solvent of butyl acetate and isobutanol and stirred until each component is completely dissolved, thereby obtaining coating solution AG1 with a solid content of 51.5%.

[0060] Preparation of coating solution AG2: 10 kg of coating solution is prepared. Here, in terms of mass percentage, 9-functional polyurethane acrylate oligomer (JR9929 purchased from Changzhou Qiaorun New Materials Technology Co., Ltd.) accounts for 21.5%, 30-functional hyperbranched acrylate oligomer (BDT-4330 purchased from Shanghai Hesheng Industry Group Co., Ltd.) accounts for 2.8%, 3-functional acrylate monomer (pentaerythritol triacrylate) accounts for 1.0%, 6-functional acrylate monomer (dipentaerythritol hexaacrylate) accounts for 2.4%, thiol-based polymerization inhibitor (butylthiopentaerythritol) accounts for 2%, and polyethylene glycol (600% purchased from Wuhan Huaxiang Kejie Biological Technology Co., Ltd.) accounts for 2.5%. DA) accounts for 1.9%, silica with a dispersed particle size of 350 nm accounts for 8%, cross-linked polystyrene microparticles (purchased from Sigma-Aldrich (Shanghai) Trading Co., Ltd.) accounts for 1%, nanodiamond particles with a dispersed particle size of 100 nm accounts for 2%, photoinitiator 184 accounts for 2.1%, and a mixed solvent of butyl acetate and propylene glycol methyl ether (butyl acetate accounts for 75% and propylene glycol methyl ether accounts for 25% by volume) accounts for the other proportions. Each component is added to the mixed solvent of butyl acetate and propylene glycol methyl ether and stirred until each component is completely dissolved, thereby obtaining coating solution AG2 with a solid content of 44.7%.

[0061] Preparation of coating solution AG3: 10 kg of coating solution is prepared. Here, in terms of mass percentage, 9-functional polyurethane acrylate oligomer (SU5039 purchased from Kashan Trading (Shanghai) Co., Ltd.) accounts for 21.7%, 30-functional hyperbranched acrylate oligomer (BDT-4330 purchased from Shanghai Hesheng Industry Group Co., Ltd.) accounts for 3.1%, 3-functional acrylate monomer (pentaerythritol triacrylate) accounts for 1.2%, 6-functional acrylate monomer (dipentaerythritol hexaacrylate) accounts for 2.4%, thiol-based polymerization inhibitor (butylthiopentaerythritol) accounts for 1.9%, and polyethylene glycol 60 The dispersion liquid contains 2% 0DA, 10% silica having a secondary particle diameter of 600 nm, 1.5% polymethyl methacrylate microparticles, 2% nano alumina particles having a dispersed particle diameter of 80 nm, 2.1% photoinitiator 184, and a mixed solvent of butyl acetate and propylene glycol methyl ether (by volume ratio, butyl acetate is 75% and propylene glycol methyl ether is 25%). Each component is added to the mixed solvent of butyl acetate and propylene glycol methyl ether and stirred until the above components are completely dissolved, thereby obtaining coating liquid AG3 with a solid content of 47.9%.

[0062] Preparation of Coating Solution AG4: The difference in the preparation method of Coating Solution 3 is that no polymethyl methacrylate fine particles are added.

[0063] Preparation of Coating Solution AG5: The preparation method of Coating Solution 3 is different in that nano alumina particles are not added.

[0064] Preparation of coating solution HR1: 10 kg of coating solution is prepared. Here, the weight percentage is: aliphatic hexaacrylate (EBECRYL purchased from Zhanxin Resin (China) Co., Ltd.) 1290N) accounts for 1.24%, 15-functional polyurethane acrylate prepolymer (W991 purchased from Guangzhou Wuxing Materials Technology Co., Ltd.) accounts for 0.165%, 4-functional acrylate monomer (ditrimethylolpropane tetraacrylate) accounts for 0.245%, 3-functional acrylate monomer (trimethylolpropane trimethacrylate) accounts for 0.31%, dispersed particle size 20 nm nano zirconia (crystal nano zirconia prepared in Example 1) accounts for 1.4%, leveling agent (polyether modified dimethyl polysiloxane BYK-378 purchased from BYK) accounts for 0.11%, photoinitiator (1-hydroxycyclohexyl phenyl ketone) accounts for 0.27%, propylene glycol methyl ether is the other proportion, each component is added to the propylene glycol methyl ether solvent and stirred until each component is completely dissolved to obtain coating solution HR1 with a solid content of 3.7%.

[0065] Preparation of Coating Liquid HR2: In the preparation method of Coating Liquid HR1, the zirconia dispersion liquid prepared in Example 5 having a dispersed particle diameter of more than 100 nm is selected.

[0066] Preparation of coating solution AR1: Prepare a coating solution. Here, in terms of mass percentage, 9-functional aliphatic polyurethane acrylate (JR9929 purchased from Changzhou Qiaorun New Materials Technology Co., Ltd.) accounts for 0.314%, 2-functional epoxy acrylate (G5100 purchased from Guangzhou Wuxing Materials Technology Co., Ltd.) accounts for 0.078%, hollow silica with a particle size of 70 nm accounts for 1.26%, solid silica accounts for 0.27%, POSS accounts for 0.5%, photoinitiator accounts for 0.24%, and solvent is the other proportion. Each component is added to a mixed solvent of methyl isobutyl ketone, propylene glycol methyl ether, isobutanol, ethyl acetate, and butyl acetate (volume ratio of each component is 1:4:3:4:8), and stirred until each component is completely dissolved to obtain coating solution AR1 with a solid content of 2.7%.

[0067] Preparation of Coating Solution AR2: In the preparation method of Coating Solution AR1, the difference is that hollow silica of 20 nm is selected.

[0068] Preparation of Coating Solution AR3: The difference in the preparation method of Coating Solution AR1 is that solid silica is not added.

[0069] Preparation of coating solution AR4: The same procedure as in preparing coating solution AR1 was repeated except that no POSS was added.

[0070] 4. Preparation of Coatings The membrane layer structure in each of the following examples is shown in Table 1.

[0071] Example 1 First, the coating solution AG1 was applied to a triacetyl cellulose film having a thickness of 80 μm using a microgravure roll coater, and then dried at 80° C. Then, in a nitrogen atmosphere, a high-pressure mercury lamp was used to apply 600 mJ / cm 2 The coating was cured with a curing energy of 0.05 to obtain a film AG1 with a coating thickness of 4 μm. The water contact angle of the surface of the corresponding AG coating is less than 80°.

[0072] Thereafter, the coating solution HR1 was applied to the AG1 film using a slit coater and dried at 80° C. Then, in a nitrogen atmosphere, a high-pressure mercury lamp was used to apply 600 mJ / cm 2 The coating was cured with a curing energy of 0.05 to obtain a film AG1-HR1 with a HR coating thickness of (1 / 2)λ0.

[0073] Finally, the coating solution AR1 was applied to the AG1-HR1 film using a slit coater and dried at 80° C. Then, the coating solution was irradiated with 600 mJ / cm 2 using a high-pressure mercury lamp under a nitrogen atmosphere. 2 The coating was cured with a curing energy of 0.05 to obtain a film AG1-HR1-AR1 with a coating thickness of AR of (1 / 4)λ0.

[0074] Example 2 In the method of Example 1, the coating thickness of HR was halved to 1 / 4λ0 to obtain a film AG1-HR1(1 / 4λ0)-AR1.

[0075] Example 3 In the method of Example 1, the coating solution AG1 was changed to AG2 (surface water contact angle of less than 80°) to obtain a film AG2-HR1-AR1.

[0076] Example 4 In the method of Example 1, the coating solution AG1 was changed to AG3 (surface water contact angle of less than 80°) to obtain a film AG3-HR1-AR1.

[0077] Example 5 In the method of Example 1, the coating solution AG1 was changed to AG4 (surface water contact angle of less than 80°) to obtain a film AG4-HR1-AR1.

[0078] Example 6 In the method of Example 1, the coating solution AG1 was changed to AG5 (surface water contact angle of less than 80°) to obtain a film AG5-HR1-AR1.

[0079] Comparative Example 1 In the method of Example 1, the coating solution AR1 was replaced with AR2 to obtain a film AG1-HR1-AR2.

[0080] Comparative Example 2 In the same manner as in Example 1, the membranes AG1-AR1 were obtained without coating the HR layer.

[0081] Comparative Example 3 In the method of Example 1, the coating solution HR1 was replaced with HR2 to obtain a film AG1-HR2-AR1.

[0082] Comparative Example 4 In the method of Example 1, the coating solution AG1 was replaced with AG2, and the coating solution AR1 was replaced with AR3 to obtain a film AG2-HR1-AR3.

[0083] Comparative Example 5 In the method of Example 1, the coating solution AG1 was replaced with AG3, and the coating solution AR1 was replaced with AR4 to obtain a film AG3-HR1-AR4.

[0084] 5. Testing The film layer structure of the present invention, as shown in Fig. 1, is a transparent substrate 10 at the bottom, on which an AG coating 20, an HR coating 30, and an AR coating 40 are sequentially arranged. The AG coating 20 contains organic microparticles 21, silica particle aggregates 22, and inorganic wear-resistant particle aggregates 23, and the silica particle aggregates 22 are located on the surface. The HR coating 30 contains nano-zirconia particle aggregates 31, and the AR coating 40 contains hollow silica particles 41 and solid silica particles 42.

[0085] Explanation of test evaluation methodology: (1) Optical performance of anti-reflection coating Measuring equipment: Ultraviolet spectrophotometer Measurement method: After coating, the flexible film is subjected to optical performance tests to measure the transmittance and reflectance of the film. The test range is 300-1100 nm.

[0086] (2) Hydrophobic function of anti-reflective coating Measuring equipment: Contact angle tester Measurement method: After coating, the flexible film is subjected to a water contact angle test. The volume of the water droplet is 2 μL.

[0087] (3) Abrasion resistance of anti-reflective coating Measuring equipment: Abrasion resistance tester Testing method: The coating flexible film is subjected to the friction resistance test, and the weight is placed according to different requirements, and the number of times and speed of sliding are changed.

[0088] (4) Hardness of anti-reflective coating Measuring equipment: electric pencil hardness meter Measurement method: A hardness test is performed on the flexible film after coating. The test conditions are 500g and speed 40.

[0089] (5) Coating refractive index measurement: Measurement equipment: Ellipsometer Semilab SE-2000 Measurement method: The coating liquid is applied to a silicon sheet by the pull-up coating method, and the silicon sheet is placed in an ellipsometer for measurement.

[0090] (6) Coating thickness: Measuring equipment: Thickness gauge Measurement method: Place the coated flexible film on a thickness gauge and measure.

[0091] (7) Coating Haze: Measuring equipment: Photoelectric haze meter WGW Measurement method: After coating, the flexible film is placed on a haze meter and measured.

[0092] (8) Anti-glare film resolution and whitening suppression test Resolution: The outline of a fluorescent lamp is observed through the anti-glare film to evaluate the film's transmittance and diffusion.

[0093] ◎: The lamp is clearly visible, the outline is clear, and there is no diffusion effect.

[0094] ○: The lamp is visible and the outline is slightly blurred.

[0095] ×: The lamp is not clearly visible and the diffusion effect is obvious.

[0096] Whitening prevention: The anti-glare film is attached to a black acrylic plate, and the degree of whitening of the coating is observed.

[0097] ⊚: The whitening suppression property is extremely good.

[0098] ◯: The whitening suppression property is good.

[0099] ×: Poor whitening suppression properties.

[0100] The test results are shown in Table 1 and Figures 2 to 11.

[0101] [Table 1]

[0102] As can be seen from the results of Example 1 and Comparative Example 1, when the AR coating selects hollow silica particles of 20 nm, the abrasion resistance is improved, but it affects the optical performance, so it is necessary to select hollow silica particles with an appropriate particle size.

[0103] As can be seen from the results of Example 1 and Comparative Example 2, the addition of an HR layer improves both the hardness and abrasion resistance of the coating, increases the transmittance, and decreases the reflectance, so it is necessary to select hollow silica particles with an appropriate particle size.

[0104] As can be seen from the results of Example 1 and Comparative Example 3, adding nano-zirconia particles with a dispersed particle size of more than 100 nm to the HR coating affects the optical transmission performance of the coating film, so nano-zirconia particles with a dispersed particle size of less than 100 nm are preferred.

[0105] As can be seen from the results of Example 3 and Comparative Example 4, the absence of solid silica particles in the AR coating reduces the abrasion resistance of the coating.

[0106] As can be seen from the results of Example 4 and Comparative Example 5, if POSS is not added to the AR coating, both the hardness and abrasion resistance of the coating film decrease.

[0107] As can be seen from the results of Example 5, if organic particles are not added to the AG layer, internal scattering increases and internal haze cannot be obtained, so the total haze of the coating film is significantly reduced.

[0108] As can be seen from the results of Example 6, the steel wool abrasion resistance of the coating is significantly reduced if inorganic abrasion resistant particles are not added to the AG layer.

[0109] The above is merely a preferred embodiment of the present invention, and the scope of protection of the present invention is not limited to the above embodiment, and any technical solutions that belong to the concept of the present invention are within the scope of protection of the present invention. In addition, those skilled in the art may make various modifications or improvements without departing from the principle of the present invention, and these modifications or improvements should also be considered as within the scope of protection of the present invention.

Claims

1. The coating includes a substrate, an AG coating, an HR coating, and an AR coating, which are arranged in this order from bottom to top, the AG coating comprises a binder resin, silica particles, organic particles, and inorganic wear-resistant particles, the silica particles being aggregate particles of 100 nm to 3000 nm, the organic particles being one or more of polymethyl methacrylate fine particles, polystyrene fine particles, polymethyl methacrylate-polystyrene copolymer fine particles, and polysilsesquioxane fine particles, the inorganic wear-resistant particles being one or more of nano alumina, nano zirconia, nano diamond, and hexagonal boron nitride nanosheets, the inorganic wear-resistant particles being aggregate particles of 50 to 200 nm, The refractive index of the HR coating is 1.53-1.74, The refractive index of the AR coating is 1.2-1.

48. An anti-glare anti-reflection film for a display.

2. The HR coating comprises a binder resin and inorganic metal oxide particles having a refractive index of 2.0-2.8, the inorganic metal oxide particles being aggregated in the coating to have a particle diameter of 10-80 nm, the inorganic metal oxide particles being nano-zirconia or titanium oxide; The AR coating comprises a binder resin and hollow silica particles having a refractive index of 1.15-1.

40. Characterized in that The anti-glare anti-reflection film for a display according to claim 1.

3. The AG coating comprises, by weight, 22-45 parts binder resin, 3-7 parts silica particles, 1-3 parts organic particles, and 1-3 parts inorganic wear-resistant particles; The HR coating comprises, by weight, 40-200 parts binder resin, 20-75 parts nano-zirconia particles, The AR coating comprises, by weight, 9-25 parts binder resin and 30-80 parts hollow silica particles; Characterized in that The anti-glare anti-reflection film for a display according to claim 1.

4. The binder resin in the AG coating, the HR coating, and the AR coating all contains a photocurable oligomer resin having 6 or more functional groups, and a photocurable diluent monomer resin having 3 or more functional groups, The photocurable oligomer resin is one or more of polyurethane acrylate oligomer, epoxy acrylate oligomer, polyester acrylate and polyether acrylate, polyacrylic acid resin oligomer, epoxy resin polymer, oxygen-containing acrylate, uric acid acrylate; The photocurable diluted monomer resin is one or more of ethyl methacrylate, ethylhexyl methacrylate, styrene, methylstyrene, N-vinylpyrrolidone monofunctional monomer, polymethylolpropane trimethacrylate, diethylene glycol dimethacrylate, tripropylene glycol dimethacrylate, 1,6-hexanediol dimethacrylate, hexanediol methacrylate, pentaerythritol trimethacrylate, dipentaerythritol hexamethacrylate, and neopentyl glycol dimethacrylate; Characterized in that The anti-glare anti-reflection film for a display according to claim 3.

5. The AR coating comprises 2-8 parts of a fluorine-containing polymer, 5-30 parts of inorganic particles, and 5-23 parts of POSS, the inorganic particles being one or more of magnesium fluoride, boron nitride, silica, and alumina, the fluorine-containing polymer being one or more of a partially fluorinated acrylate silicone copolymer, a partially or fully fluorinated acrylic compound, and a partially or fully fluorinated vinyl ether, and the POSS being one or more of a phenyl POSS, an amino POSS, a vinyl POSS, and an acrylic POSS. Characterized in that The anti-glare anti-reflection film for a display according to claim 3.

6. The coating solution used to form the AG coating contains, by mass percentage, 18%-38% of a photocurable oligomer resin having 6 or more functional groups, 4%-7% of a photocurable diluent monomer resin having 3 or more functional groups, 8%-12% of silica particles, 1%-3% of organic particles, 1%-3% of inorganic wear-resistant particles, 1%-5% of an auxiliary agent, and 1%-3% of a photoinitiator. Characterized in that The anti-glare anti-reflection film for a display according to claim 3.

7. The coating solution used to form the HR coating contains, by mass percentage, 1%-3% of a photocurable oligomer resin having 6 or more functional groups, 0.3%-1% of a photocurable diluent monomer resin having 3 or more functional groups, 1%-3% of nano-zirconia particles, 0.05%-0.2% of an auxiliary agent, and 0.1%-0.5% of a photoinitiator. Characterized in that The anti-glare anti-reflection film for a display according to claim 3.

8. The coating solution used to form the AR coating contains, by mass percentage, 0.25%-0.5% of a photocurable oligomer resin having 6 or more functional groups, 0.05%-0.1% of a photocurable diluent monomer resin having 3 or more functional groups, 0.3%-1.5% of hollow silica particles, 0.1%-1% of solid silica particles, 0.1%-1% of POSS, and 0.1%-0.5% of a photoinitiator. Characterized in that The anti-glare anti-reflection film for a display according to claim 3.

9. In a coating liquid used to form an AG coating, the silica particles are added as a dispersion liquid, and are mixed with a solvent to obtain a silica particle dispersion liquid having a primary particle diameter of 10 nm to 50 nm and a secondary particle diameter of 100 nm to 2000 nm; The inorganic wear-resistant particles are added as a dispersion, with a primary particle size of 10-50 nm, and mixed with a solvent to obtain a dispersion with secondary particles having a size of 50-200 nm; The particle size of the organic particles is 1 μm to 10 μm. Characterized in that The anti-glare anti-reflection film for a display according to claim 6.

10. The average particle size of the nano-zirconia particles is 5%-80% of the thickness of the HR coating, the particle size of the hollow silica is 50-80 nm, and the average particle size of the solid silica is 30%-100% of the thickness of the AR coating. Characterized in that The anti-glare anti-reflection film for a display according to claim 8.

11. The inorganic wear-resistant particles are formed by pretreating a hexagonal boron nitride nanosheet. In the pretreatment step, a hexagonal boron nitride nanosheet having a primary particle size is stirred and mixed with a solvent, and ultrasonically dispersed to obtain a colloidal liquid, and the colloidal liquid is centrifuged to obtain a primary bottom solid; Repeat the above pretreatment process on the primary bottom solid to obtain a secondary bottom solid; repeating the above pretreatment steps on the secondary bottom solids and collecting the resulting centrate, a dispersion of inorganic wear-resistant particles; Characterized in that The anti-glare anti-reflection film for a display according to claim 9.

12. The nano-zirconia particles are one or a mixture of two or more of tetragonal and cubic crystal types. Characterized in that The anti-glare anti-reflection film for a display according to claim 2.

13. The nano-zirconia particles are added as a dispersion to a coating solution used to form the HR coating; The dispersion of nano-zirconia particles is First, a zirconium-containing compound is mixed with a mixture of a solvent and an organic acid in a predetermined ratio, heated to 250-320° C., and reacted at a constant temperature for 3-18 hours. Next, the filtrate obtained by the reaction is washed several times to obtain tetragonal or cubic nano-zirconia particles, The nano-zirconia particles thus obtained and the dispersion aid are added to a solvent and processed to obtain a transparent nano-zirconia dispersion liquid, and the nano-zirconia particles in the dispersion liquid form an aggregated state with a secondary dispersion particle diameter of 10-50 nm. It is prepared as follows: Characterized in that The anti-glare anti-reflection film for a display according to claim 12.

14. The thickness of the AG coating is 2-50 μm, and the water contact angle of the surface of the AG coating is less than 80°, and the optical thickness of the HR coating is 1 / 2λ. 0 and the optical thickness of the AR coating is 1 / 4λ 0 That is, Characterized in that The anti-glare anti-reflection film for a display according to any one of claims 1 to 13.

Citation Information

Patent Citations

  • Non-glare coating and non-glare membrane

    CN105566963A

  • Antireflection film

    JP2005181543A

  • Antireflection membrane and antireflection film

    JP2006349830A

  • Optical film, antireflection film, polarizing plate and image display device

    JP2007233185A

  • Functional film and display apparatus

    JP2009244382A