How to recycle lithium-ion batteries
Chloroaluminate ionic liquids effectively extract lithium and cobalt from lithium-ion battery cathodes, addressing inefficiencies and environmental concerns in existing recycling methods by achieving high recovery rates with low energy and emissions.
Patent Information
- Application Number
- JP2024529513
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2021-11-19
- Filing Date
- 2022-10-28
- Publication Date
- 2024-11-15
AI Technical Summary
The recycling of lithium-ion batteries is challenging due to the inefficiency in recovering lithium and cobalt, which are critical components, and existing methods are environmentally harmful or energy-intensive, posing risks to groundwater and requiring scarce resources.
The use of chloroaluminate ionic liquids, such as tetrachloroaluminate anion (AlCl4-) in organic solvents, to extract lithium and cobalt from lithium-ion battery cathodes by reducing Co(III) to Co(II) and forming soluble anions, allowing for efficient separation and recovery.
This method achieves 100% extraction efficiency of lithium and 99.7% recovery of cobalt with low energy consumption and minimal environmental impact, avoiding hazardous chemicals and emissions.
Smart Images

Figure 2024542471000001_ABST
Abstract
Description
[Background technology]
[0001] Lithium-ion batteries (LIBs) are popular as portable power sources due to their high specific capacity, high energy density, and long cycling capability. With the rapid development of technology, the use of LIBs has increased dramatically, and their recycling has become an urgent need both economically and environmentally.
[0002] The transition to net-zero is a vital endeavor for the future of the planet. This ambitious plan has several sub-branches including air pollution and solid waste management, as well as reducing energy usage. The emergence and improvement of electric vehicles (EVs) foresees an effective route to address the aforementioned issues. The International Energy Agency (IEA) recently released a report that provides a detailed global outlook for the growth of EV demand, predicting that global sales will increase from 120,000 in 2012 to 2 million in the first quarter of 2022. The total number of EVs is also projected to reach 21 million by the end of 2030.
[0003] However, battery cell components play a critical role in these rechargeable power sources, and the limited global resources of these components are a bottleneck. In particular, cobalt (Co), used in high-energy cathode materials for EVs, is predicted to be a constraint in the LIB supply chain. According to the United States Geological Survey (USGS), the world's proven reserves of cobalt are estimated at 7.6 million tonnes. In addition to the uneven distribution of these reserves, the electrification of the automotive industry is continuously increasing the demand for this transition metal, which is estimated to reach 117,000 tonnes by 2025. Summary of the Invention
[0004] The present disclosure relates to the tetrachloroaluminate anion (AlCl4 -) or chloroaluminate ionic liquids with aluminum chloride (AlCl3) solutions on organic solvents to synthesize lithium cobalt oxide (LiCoO2), lithium nickel manganese cobalt oxide (LiNi x Mn y Co 1-x-y The present invention provides a strategy for recycling lithium-ion battery cathode materials, such as lithium-ion lithium-ion battery cathode materials (e.g., lithium-ion lithium-ion battery cathodes), lithium-ion lithium-ion battery cathode materials, and any related materials, including lithium transition metal oxides.
[0005] In case of improper recycling of LIBs, the electrolyte reaction with water can produce dangerous gases, while heavy metals in the cathode such as Co, nickel (Ni), or manganese (Mn) can cause serious contamination in soil or groundwater. It is therefore important to recycle these battery materials before we face significant shortages or environmental problems in the near future. Some industrial recycling methods start with a pretreatment step to increase efficiency and separate several portions of the battery waste with different physical properties. After pretreatment (chemical, mechanical, thermal, or other), the battery waste stream is amenable to various processing routes. Many sites utilize pyrometallurgy methods. Although this method has high recycling efficiencies for valuable metals such as Co, Ni, or Cu, it is unable to recycle lithium as it either flows out in oxide and gas form or remains unrecoverable as slag. Furthermore, the nature of this process requires high energy consumption due to its high heat usage. Another commercialized recycling route is hydrometallurgy, which uses organic or inorganic acid solutions to leach out the valuable cathode materials as ions, providing high recycling efficiencies with relatively low energy. However, the problem lies in the fact that corrosive reagents are harmful to both the environment and workers.
[0006] In comparison, chloroaluminate ionic liquids or solutions of AlCl3 in organic solvents acting as the reaction medium provide a greener and much safer alternative to acids.
[0007] In one example, the tetrachloroaluminate anion (AlCl4) present in a room temperature ionic liquid composed of 1-ethyl-3-methylimidazolium chloride (EMIMCl) and aluminum chloride (AlCl3) in a 1:1 molar ratio. - ) can effectively extract lithium (Li) and cobalt (Co) from lithium cobalt oxide (LiCoO2) cathodes in used lithium-ion batteries. Experimental analysis has shown that AlCl4 - It was shown that the strong affinity between LiCoO2 and LiCoO3 allows lithium to be extracted from LiCoO2 to form lithium chloride (LiCl). As a result, Co(III) in LiCoO2 is reduced to Co(II) by the oxide, and oxygen gas is generated. UV-Vis and X-ray photoelectron spectroscopy (XPS) analysis showed that Co(II) is converted to cobalt tetrachloride (CoCl4 2- ) anion. - The extraction efficiency of both lithium and cobalt reaches 100%, and the Al content (AlCl4 - The cobalt can then be recovered as cobalt hydroxide (Co(OH)2) with a recovery rate of 99.7%.
[0008] In another example, a solution of aluminum chloride (AlCl3) in an organic solvent, typically ethanol, can dissolve lithium cobalt oxide (LiCoO2) and LiNi in used Li-ion batteries. 0.6 Mn 0.2 Co 0.2 Lithium (Li), cobalt (Co), nickel (Ni), and manganese (Mn) can be effectively extracted from O2 cathodes. Specifically, a solution of AlCl3 in ethanol can extract LiCoO2 and LiNi under mild heating conditions. 0.6 Mn 0.2 Co 0.2The O2 cathode can be rapidly dissolved. UV-vis spectroscopy showed that transition metal (Co, Ni, and Mn) tetrachloride anions were formed in the solution, and evaporation of the ethanol yielded a solid product containing lithium chloride, transition metal chlorides, and amorphous compounds containing Al. The Al-containing compounds can be converted to aluminum oxide, which is insoluble in water, by mild heat treatment at 150 °C and can then be removed by rinsing with water. The resulting aqueous solution can contain 99.5% of the transition metals extracted from the cathode material.
[0009] These various exemplary methods of recycling lithium-ion batteries using chloroaluminate ionic liquids and AlCl3 solutions in organic solvents can have many advantages and benefits by avoiding other techniques. These methods can enable clean extraction of transition metals, such as cobalt, from lithium-ion battery cathode materials with low emissions and low energy consumption.
[0010] In one example, a method for recycling a lithium ion battery cathode material can include reducing the lithium ion battery cathode material with an ionic liquid including a chloroaluminate anion and separating the material from the lithium ion battery cathode.
[0011] In another example, a method for recycling a lithium ion battery cathode material can include reducing the lithium ion battery cathode material with an organic solution of AlCl3 and separating the material from the lithium ion battery cathode. [Brief description of the drawings]
[0012] The patent or application file contains at least one drawing executed in color. Copies of this patent or patent application publication containing color drawing(s) will be provided by the Office upon request and payment of the necessary fee. The drawings are not necessarily drawn to scale, and like numerals represent substantially similar components throughout the several views. Like numerals with different subscripts represent different instances of substantially similar components. The drawings are generally intended to illustrate, by way of example, and not by way of limitation, various embodiments discussed herein. [Figure 1] FIG. 1 shows XRD data for a lithium ion battery cathode recycling in one example. [Diagram 2] FIG. 2 shows UV-Vis data for lithium ion battery cathode recycling in one example. [Diagram 3] FIG. 3 shows NMR data for lithium ion battery cathode recycling in one example. [Figure 4] FIG. 4 shows XRD data for a lithium ion battery cathode recycling in one example. [Diagram 5] FIG. 5 shows XPS data for lithium ion battery cathode recycling in one example. [Figure 6] FIG. 6 shows NMR data for lithium ion battery cathode recycling in one example. [Figure 7] FIG. 7 shows UV-Vis data for lithium ion battery cathode recycling in one example. [Figure 8] FIG. 8 shows UV-Vis data for lithium ion battery cathode recycling in one example. [Figure 9] FIG. 9 shows XRD data for a lithium ion battery cathode recycling in one example. [Figure 10] FIG. 10 shows XRD data for a lithium ion battery cathode recycling in one example. [Figure 11] FIG. 11 shows NMR data for lithium ion battery cathode recycling in one example. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0013] Reference will now be made in detail to certain examples of the disclosed subject matter, examples of which are illustrated in part in the accompanying drawings. While the disclosed subject matter will be described in conjunction with the enumerated claims, it will be understood that the illustrated subject matter is not intended to limit the claims to the disclosed subject matter.
[0014] definition Throughout this specification, values expressed in range format should be interpreted flexibly to include not only the numerical values explicitly recited as the limits of the range, but also all individual numerical values or subranges subsumed within the range as if each numerical value and subrange were explicitly recited. For example, the range "about 0.1% to about 5%" or "about 0.1% to 5%" should be interpreted to include not only about 0.1% to about 5%, but also the individual values (e.g., 1%, 2%, 3%, and 4%) and subranges (e.g., 0.1% to 0.5%, 1.1% to 2.2%, 3.3% to 4.4%) within the indicated range. The statement "about X to Y" has the same meaning as "about X to about Y" unless otherwise indicated. Similarly, the statement "about X, Y, or about Z" has the same meaning as "about X, about Y, or about Z" unless otherwise indicated.
[0015] In this specification, the terms "a", "an", or "the" are used to include one or more than one, unless the context clearly indicates otherwise. The term "or" is used to refer to a non-exclusive "or" unless otherwise indicated. The statement "at least one of A and B" has the same meaning as "A, B, or A and B". Furthermore, it should be understood that expressions or terms used herein and not otherwise defined are for descriptive purposes only and not for limiting purposes. Section headings are used to aid in the reading of this specification and should not be construed as limiting, and information associated with a section heading may be present within or outside that particular section.
[0016] In the methods described herein, unless a temporal or operational order is explicitly recited, acts may be performed in any order without departing from the principles of the present disclosure. Moreover, some specified acts may be performed simultaneously unless the claim language explicitly recites that they be performed separately. For example, a claimed act of performing X and a claimed act of performing Y may be performed simultaneously in a single operation, and the resulting process would fall within the literal scope of the claimed process.
[0017] As used herein, the term "about" allows for some variability in a value or range, such as, for example, within 10%, within 5%, or within 1% of a stated value or the limits of a stated range, and includes the exact value or range as stated.
[0018] As used herein, the term "substantially" refers to a majority or majority, such as at least about 50%, 60%, 70%, 80%, 90%, 95%, 96%, 97%, 98%, 99%, 99.5%, 99.9%, 99.99%, or at least about 99.999% or more, or 100%.
[0019] The term "organic group" as used herein refers to any functional group that contains carbon. Examples can include oxygen-containing groups such as alkoxy groups, aryloxy groups, aralkyloxy groups, and oxo (carbonyl) groups; carboxyl groups, including carboxylic acids, carboxylates, and esters; sulfur-containing groups such as alkyl and aryl sulfide groups; and other heteroatom-containing groups. Non-limiting examples of organic groups include OR, OOR, OC(O)N(R), CN, CF, OCF, R, C(O), methylenedioxy, ethylenedioxy, N(R), SR, SOR, SO, SO, N(R), SO, C(O)R, C(O)C(O)R, C(O)CHC(O)R, C(S)R, C(O)OR, OC(O)R, C(O)N(R), OC(O)N(R), C(S)N(R), (CH) 0-2 N(R)C(O)R, (CH2) 0-2 N(R)N(R)2, N(R)N(R)C(O)R, N(R)N(R)C(O)OR, N(R)N(R)CON(R)2, N(R)SO2R, N(R)SO2N(R)2, N(R)C(O)OR, N(R)C(O)R, N( R)C(S)R, N(R)C(O)N(R)2, N(R)C(S)N(R)2, N(COR)COR, N(OR)R, C(=NH)N(R)2, C(O)N(OR)R, C(=NOR)R, and substituted or unsubstituted (C1~C 100 ) hydrocarbyl, where R can be hydrogen (in instances containing other carbon atoms) or a carbon-based moiety, which can be substituted or unsubstituted.
[0020] The term "substituted" as used herein in relation to a molecule or organic group defined herein refers to a state in which one or more hydrogen atoms contained therein are replaced by one or more non-hydrogen atoms. The term "functional group" or "substituent" as used herein refers to a group that can be substituted or is substituted on a molecule or organic group. Examples of substituents or functional groups include, but are not limited to, halogens (e.g., F, Cl, Br, and I); oxygen atoms in groups such as hydroxyl groups, alkoxy groups, aryloxy groups, aralkyloxy groups, oxo(carbonyl) groups, carboxylic acids, carboxylates, and carboxylate esters; sulfur atoms in groups such as thiol groups, alkyl and aryl sulfide groups, sulfoxide groups, sulfone groups, sulfonyl groups, and sulfonamide groups; nitrogen atoms in groups such as amines, hydroxylamine, nitriles, nitro groups, N-oxides, hydrazides, azides, and enamines; and other heteroatoms in various other groups. Non-limiting examples of substituents which may be attached to a substituted carbon (or other) atom include F, Cl, Br, I, OR, OC(O)N(R), CN, NO, NO, ONO, azido, CF, OCF, R, O(oxo), S(thiono), C(O), S(O), methylenedioxy, ethylenedioxy, N(R), SR, SOR, SO, SO, N(R), SO, R, C(O)R, C(O)C(O)R, C(O)CHC(O)R, C(S)R, C(O)OR, OC(O)R, C(O)N(R), OC(O)N(R), C(S)N(R), (CH) 0-2 N(R)C(O)R, (CH2) 0-2 N(R)N(R), N(R)N(R)C(O)R, N(R)N(R)C(O)OR, N(R)N(R)CON(R), N(R)SOR, N(R)SON(R), N(R)C(O)OR, N(R)C(O)R, N(R)C(S)R, N(R)C(O)N(R), N(R)C(S)N(R), N(COR)COR, N(OR)R, C(=NH)N(R), C(O)N(OR)R, and C(=NOR)R, where R can be hydrogen or a carbon-based moiety, e.g., R can be hydrogen, (C1-C 100) hydrocarbyl, alkyl, acyl, cycloalkyl, aryl, aralkyl, heterocyclyl, heteroaryl, or heteroarylalkyl, or two R groups attached to the nitrogen atom or adjacent nitrogen atoms can be taken together with one or more nitrogen atoms to form a heterocyclyl.
[0021] The term "deplete" as used herein refers to a reduction in the amount or concentration of a liquid, gas, or solute, etc. For example, a mixture of gases A and B can be depleted of gas B when the concentration or amount of gas B is reduced, e.g., by selectively permeating gas B through a membrane to remove gas B from the mixture, or by selectively permeating gas A through a membrane to add gas A to the mixture.
[0022] The term "solvent" as used herein refers to a liquid capable of dissolving a solid, liquid, or gas. Non-limiting examples of solvents are silicones, organic compounds, water, alcohols, ionic liquids, and supercritical fluids.
[0023] As used herein, the term "room temperature" refers to a temperature between about 15°C and 28°C. As used herein, the term "standard temperature and pressure" refers to 20° C. and 101 kPa.
[0024] In various examples, the salt having a positively charged counterion can include any suitable positively charged counterion. For example, the counterion can be ammonium (NH + ), or sodium (Na + ), potassium (K + ), or lithium (Li + In some instances, the counterion can have a positive charge greater than +1, which in some instances is an alkali metal such as Zn 2+ , Al 3+ , or Ca 2+ Or Mg 2+It can form complexes with multiple ionizable groups such as alkaline earth metals.
[0025] In various examples, the salt with a negatively charged counterion can include any suitable negatively charged counterion. For example, the counterion can be a halide, such as fluoride, chloride, iodide, or bromide. In other examples, the counterion can be a nitrate, hydrogen sulfate, dihydrogen phosphate, bicarbonate, nitrite, perchlorate, iodate, chlorate, bromate, chlorite, hypochlorite, hypobromite, cyanide, amide, cyanate, hydroxide, or permanganate. The counterion can be a conjugate base of any carboxylic acid, such as acetate or formate. In some examples, the counterion can have a negative charge greater than -1, which can be complexed with multiple ionized groups, such as oxide, sulfide, nitride, arsenate, phosphate, arsenite, hydrogen phosphate, sulfate, thiosulfate, sulfite, carbonate, chromate, dichromate, peroxide, or oxalate.
[0026] Reaction mechanism In an exemplary method, LiCoO2, LiNi x Mn y Co 1-x-y Lithium metal oxide cathodes, such as O2, and any other transition metal containing, are not limited to the presented EMIMAlCl4 ionic liquid, but may be used with AlCl4 - It can be recycled by deep eutectic systems containing the anions AlCl4 - Any deep eutectic system or ionic liquid may work, including: EMIMAlCl4 ionic liquid is a 1:1 molar mixture of aluminum chloride (AlCl3) and 1-ethyl-3-methylimidazolium aluminum chloride (EMIMCl), which reacts with EMIMAlCl4 according to the following reaction: + Cation and tetrachloroaluminate anion (AlCl4 - )
[0027] EMIMCl+AlCl3 → EMIM + +AlCl4 - Experimental elemental ratios and LiCl, CoCl4 2- Based on the identification of the product containing O2, lithium is AlCl4 - Cl in anion - The oxygen vacancies in LiCoO2 can be extracted from the crystal lattice of LiCoO2 by the strong affinity between Al cations and oxides. Alternatively, oxygen vacancies in LiCoO2 can be generated by the strong affinity between Al cations and oxides. As a result, Co(III) can be reduced to Co(II) by oxides in LiCoO2, and oxygen gas can be released. LiCoO2 and AlCl4 - An exemplary reaction mechanism between may be as follows:
[0028] [ka]
[0029] Low LiCoO2 / AlCl4 - The proposed compound Al4Cl6O3 from the reaction ratio is amorphous and has a high LiCoO2 / AlCl4 - It is a stoichiometric combination of the more well-defined compounds AlCl3 and aluminum oxychloride (AlOCl) that result from the reaction of the ratio
[0030] This shows a method to extract lithium and cobalt from LiCoO2, which can be used to recycle used lithium-ion batteries. The method is carried out by extracting tetrachloroaluminate AlCl4 - Based on the reaction between the anion and LiCoO2. AlCl4 - Reagents containing anions include LiCoO2, LiNi x Mn y Co 1-x-y It can be used to extract lithium and transition metals from lithium-ion batteries that use lithium transition metal oxide cathodes, including O2, and related materials.
[0031] In another example, a solution of AlCl3 in an organic solvent can be used as the recycling medium. If an organic solvent such as ethanol is used to prepare the solution, the following reaction mechanism can occur:
[0032] [ka]
[0033] Here, AlCl2 + and AlCl 2+ is an aluminum-chloride complex cation and is a representative active species in an AlCl3 solution in ethanol (EtOH-AlCl3) that can react with LiCoO2. These reaction mechanisms are supported and discussed with reference to the Examples section below.
[0034] method In one example, a method for recycling a lithium ion battery cathode material includes reducing the lithium ion battery cathode material with a liquid including a chloroaluminate ionic liquid or an AlCl3 solution in an organic solvent and separating the material from the lithium ion battery cathode.
[0035] Chloroaluminate ionic liquids are Lewis neutral chloroaluminate anions (AlCl4 - ) or Lewis acidic chloroaluminate anion (Al2Cl7 - ).
[0036] The AlCl3 solution in an organic solvent can contain chloroaluminate anions, chloride anions, and aluminum-chloride complex cations. The lithium ion battery cathode material can include any lithium ion battery cathode material that includes lithium and a transition metal. The lithium ion battery cathode material can include, for example, lithium cobalt oxide (LCO), lithium nickel cobalt aluminum oxide (NCA), lithium manganese oxide (LMO), lithium iron phosphate (LFP), lithium nickel manganese cobalt oxide-LiNi(1-yz)Mn(y)Co(z)O2 (NMC), or combinations thereof.
[0037] Reducing the lithium ion battery cathode material can include, for example, adding 1-ethyl-3-methylimidazolium tetrachloroaluminate ionic liquid to the lithium ion battery cathode material or adding tetrachloroaluminate ionic liquid to the lithium ion battery cathode material.
[0038] The addition of tetrachloroaluminate ionic liquid to cobalt (or other transition metal) in lithium ion battery cathode materials can be done in a 1:20 molar ratio, a 1:10 molar ratio, a 1:5 molar ratio, or a 1:2 molar ratio.
[0039] In some cases, reducing the lithium ion battery cathode material includes adding an EtOH-AlCl3 solution to the lithium ion battery cathode material. Separating the material from the lithium ion battery cathode can include separating and removing cobalt from the lithium ion battery cathode or separating and removing lithium from the lithium ion battery cathode. In some cases, separating the material from the lithium ion battery cathode can include centrifugation. In some cases, separating the material from the lithium ion battery cathode can include extracting cobalt and other transition metals as cations.
[0040] Separating the material from the lithium ion battery cathode can include extracting the cathode active material, for example at room temperature, for example without discharge. Preparing the ionic liquid can include a chloroaluminate anion prior to reducing the lithium ion battery cathode material. Preparing the ionic liquid can include mixing EMIMCl with AlCl3 in a 1:1 molar ratio. In some cases, preparing the ionic liquid can include gradually adding anhydrous AlCl3 powder to EMIMCl.
[0041] Preparing the AlCl3 solution inorganic solvent can include adding anhydrous AlCl3 to ethanol. EXAMPLES
[0042] Various embodiments of the present disclosure may be better understood by reference to the following examples, which are provided by way of illustration and are not intended to limit the present disclosure to the examples set forth herein.
[0043] Example 1: Tetrachloroaluminate anion (AlCl - Extraction of lithium and cobalt from LiCoO2 cathode by ionic liquids containing In Example 1, lithium-ion battery cathode materials were recycled by extracting lithium and cobalt using an ionic liquid containing tetrachloroaluminate anions. In Example 1, the reactivity of LiCoO2 with EMIMAlCl4 ionic liquid was tested.
[0044] First, the reaction of LiCoO2 with EMIMAlCl4 was carried out. 1-Ethyl-3-methylimidazolium tetrachloroaluminate (EMIMAlCl4) ionic liquid was prepared by slowly mixing 1-Ethyl-3-methylimidazolium chloride (EMIMCl) (>98%, HPLC, TCI Chemicals) with AlCl3 (AlCl3, anhydrous, 99.99%, Sigma-Aldrich) in a 1:1 molar ratio (EMIMCl:AlCl3), followed by stirring at room temperature for 12 hours before use. 1-Ethyl-3-methylimidazolium chloride (EMIMCl) (>98%, HPLC, TCI Chemicals) was dried at 60 °C under vacuum in a glove box for 12 hours before use.
[0045] After preparing the EMIMAlCl4 ionic liquid, lithium cobalt oxide (LiCoO2, 99.8% trace metals basis, Sigma-Aldrich) powder was added in different LiCoO2:EMIMAlCl4 molar ratios (1:20, 1:10, 1:5, and 1:2) and then stirred at 150 °C for 12 h. The reaction flask was equipped with a condenser on top to circulate water at 10 °C. LiCoO2 appears to dissolve in EMIMAlCl4, producing a blue solution and a white solid precipitate upon reaction. Oxygen evolution was detected by a dissolved oxygen kit (Atlas Scientific).
[0046] LiCoO2 / AlCl4 - For reactions with molar ratios of 1:20, 1:10, and 1:5, the supernatants and precipitates after the reactions were separated by centrifugation at 20,000 g for 5 min and further analyzed.
[0047] Powder X-ray diffraction measurements (XRD) were performed using a Panalytical Empyrean Series 2 to analyze the precipitate. The precipitate was washed with benzene three times and then dried at room temperature for 24 hours in an argon gas-filled glove box. The dried powder was then pressed to form a pallet on a zero-diffraction silicon plate, and the surface was then covered with a Kapton tape film to prevent the sample from reacting with air and to avoid moisture absorption. XRD measurements were then performed. The XRD pattern in Figure 1 shows that the precipitate contains lithium chloride (LiCl).
[0048] The Co species in the supernatant were analyzed using an Agilent Cary 60 UV-Vis spectrophotometer. 3 ml of the supernatant diluted with EMIMAlCl4 ionic liquid was placed in a 10 × 10 mm quartz cuvette and sealed with a cap. A baseline measurement was taken in the range of 550–750 nm for EMIMAlCl4 ionic liquid alone in the same cuvette. Figure 2 shows the UV-Vis spectrum of the supernatant after the reaction. The distinguishable peaks at 630 nm, 667 nm, and 696 nm are the cobalt tetrachloride anion (CoCl4 2- )
[0049] Liquid-phase nuclear magnetic resonance (NMR) was also performed on the supernatant. 27 Al and 1 H) was acquired on a Bruker Avance 600 spectrometer equipped with a 14.1 T narrow-bore superconducting magnet operating at 104.26 MHz and 600.13 MHz for 27Al and 1H nuclei, respectively. To avoid mixing of the sample with the standard solution, a double-tube assembly was used, where the sample was sealed inside a 5 mm NMR tube and a standard chloroform-d was placed in a 3 mm NMR tube and inserted inside the larger tube (sample:standard volume ratio of 2:3). All liquid phase 27 Al and 1 The H experiments were performed at radio frequency field strengths of 20.8 kHz and 26 kHz, respectively, with a recycle delay of 12.0 s for all spins to return to thermal equilibrium. 27 Al and 1H NMR was performed at 110 °C and 25 °C, respectively.
[0050] Compared to the original EMIMAlCl4, the different LiCoO2 / AlCl4 - of the supernatant after the reaction in molar ratio 1 H nuclear magnetic resonance (NMR) spectrum (Figure 3) was analyzed by EMIM + This indicates that the cations remain intact. LiCoO2 / AlCl4 - The downfield chemical shift and peak broadening with increasing molar ratio are due to the Co 2+ This is due to the paramagnetic effect of the pure EMIMAlCl4. 27 The NMR spectrum of Al shows a single peak at 104.1 ppm, which is the same as that of AlCl4 - Represents anion. 1:20 and 1:10 LiCoO2 / AlCl4 - Room temperature of the supernatant after the reaction at molar ratio 27 The NMR spectrum of Al was also - peak, suggesting that no soluble Al-containing species were produced during the reaction. However, at 1:5 LiCoO2 / AlCl4 - of the supernatant after the reaction in molar ratio 27 The NMR spectrum of Al shows broader peaks shifted further downfield compared to those from the 1:20 and 1:10 ratios. - of the supernatant from the molar ratio 27 The NMR spectrum of Al was obtained at 150 °C. As shown in the inset of Figure 3, the spectrum corresponds to the AlCl4 - and AlCl4 according to the following reaction: - A new anion species, Al2Cl7, formed from the reaction between AlCl3 and - Two peaks corresponding to and are shown.
[0051] AlCl4 - +AlCl3→Al2Cl7 - Therefore, this result is consistent with the high LiCoO2 / AlCl4 - This shows that AlCl3 can be produced from the reaction in a molar ratio.
[0052] The reaction of LiCoO2 with EMIMCl4 ionic liquid in a 1:2 molar ratio resulted in a paste-like product with high precipitate content. This paste-like product was characterized by X-ray diffraction (XRD). The XRD pattern of the project in Figure 4 shows the pattern of LiCl when the sample was sealed using Kapton tape to prevent contact from the surrounding environment. When the tape was removed, the XRD pattern shows the inclusion of AlCl3·6H2O, water of crystallization likely absorbed from the environment. The XRD also shows EMIMCl and CoCl2.
[0053] Oxygen gas was observed in the reaction with a 1:2 molar ratio of LiCoO2:EMIMAlCl4. The reaction was carried out sealed in a glove box with O2<0.01 ppm. When the reaction was complete, the valve connected to the reaction flask was opened while the exhaust re-ignited a half-smelted match proving the presence of oxygen. This suggests that oxygen gas was being evolved by the reaction.
[0054] LiCl, CoCl4 2- Based on the knowledge that AlCl4 - Anion Cl - It is believed that lithium is extracted from the crystal lattice of LiCoO2 by its strong affinity with O. 2- and Al 3+ Due to its strong affinity with Co, oxygen vacancies are formed, so that Co(III) can be reduced to Co(II) by the oxide in LiCoO2 and oxygen gas can be released.
[0055] Based on the above spectroscopic analysis, LiCoO2 and AlCl4 - The reaction mechanism between is as follows:
[0056] [ka]
[0057] Low LiCoO2 / AlCl4 - The compound Al4Cl6O3 from the reaction is amorphous and has a high LiCoO2 / AlCl4 - It is a stoichiometric combination of the more well-defined compounds AlCl3 and aluminum oxychloride (AlOCl) that result from the reaction of the ratio
[0058] X-ray photoelectron spectroscopy (XPS) analysis was performed on 1:2 LiCoO2 / AlCl4 - The analysis was performed on the products from the reaction in molar ratios. XPS data were collected at UC Irvine Materials Research Institute (IMRI) using a Kratos AXIS Supra (Al Kα=1486.7 eV). Samples were transported to the XPS facility in stainless steel tubes with KF flange seals filled with argon. Samples were loaded into the sample chamber in a glove box integrated with the Kratos AXIS Supra for XPS analysis. All peaks in the XPS data were analyzed by a Casa XPS52 and calibrated with the reference peak of C 1s at 284.6 eV (exotic carbon).
[0059] Figure 5 shows the cobalt 2p X-ray photoelectron spectroscopy (XPS) spectra of pure LiCoO2 and the product. The cobalt 2p spectrum of pure LiCoO2 shows that the binding energy difference between the satellites 2p 1 / 2 (790.4 eV) and 2p 1 / 2 (780 eV) is about 10 eV, indicating that the valence of the cobalt ion is 3+. In the cobalt 2p XPS spectrum of the product, there is a significant change in the binding energy difference between the satellites 2p 1 / 2 (785.8 eV) and 2p 1 / 2 (780.8 eV) of 5 eV, indicating that the valence of the cobalt ion in the product is 2+. Comparison of the XPS spectra clearly shows that Co(III) in LiCoO2 is converted to Co(II) during the reaction.
[0060] Further evidence of cobalt and lithium extraction from the battery materials was shown by visual inspection.- The product from the reaction in molar ratio dissolved completely in water, resulting in a clear solution with the characteristic pink color indicative of hydrated Co(II). The aqueous solution was stirred overnight at 70 °C in an ambient environment, producing a white precipitate. Inductively Coupled Plasma Optical Emission Spectroscopy (ICP-OES) analysis showed that the only metal contained in the precipitate was Al, and XRD demonstrated its amorphous nature. This is likely aluminum oxide (Al2O3) produced from the oxidation of AlOCl and Al4O3Cl6. After filtering the precipitate, the water is evaporated from the solution. The resulting blue powder was further heated at 150 °C overnight. The heated powder was added to water, producing a pink solution with a white precipitate. The precipitate, which is Al2O3 converted from AlCl3 by heating, is filtered.
[0061] Inductively Coupled Plasma Optical Emission Spectroscopy (ICP-OES) was performed on the samples including the final pink supernatant and total precipitate. The amounts of aluminum (Al), cobalt (Co), and lithium (Li) were measured by a Perkin-Elmer Optima 7300 DV ICP-OES instrument. The percentages of metals in the supernatant and precipitate are shown in Table 1.
[0062] [Table 1]
[0063] Elemental analysis revealed that (AlCl4 - 99.61% of the Al (from the anion) is removed as a precipitate (Al2O3) and 99.86% of the cobalt is removed as Co 2+ It was found that lithium was extracted as a cation into the aqueous solution, which contained 36.16% of the total Li, with the remaining 63.82% being present in the precipitate.
[0064] This shows a method to extract lithium and cobalt from LiCoO2, which can be used to recycle used lithium-ion batteries. The method is carried out by extracting tetrachloroaluminate AlCl4 -Based on the reaction between the anion and LiCoO2. Based on these results, AlCl4 - Any reagent containing an anion, such as LiCoO2, LiNi x Mn y Co 1-x-y It is likely that they could be used to extract lithium and transition metals from lithium-ion batteries that use lithium transition metal oxide cathodes containing O2, and related materials.
[0065] Example 2: Lithium-ion battery recycling technology using organic solution of aluminum chloride In Example 2, an AlCl3 solution in ethanol (EtOH-AlCl3) is used to recycle lithium-ion battery cathode materials. Here, in an argon-filled glove box (H2O and O2 < 0.1 ppm), 10 wt% AlCl3 (98.5%, anhydrous powder, Thermo Fisher Scientific) was slowly added to 10 ml of ethanol (> 99.5%, 200 proof, anhydrous, Sigma-Aldrich) while cooling the solution. LiCoO2 or LiNi in a molar ratio of 2:1 (Al:LiCoO2 or NMC622) was then added to the AlCl3 solution. 0.6 Mn 0.2 Co 0.2 O2 (NMC622) was added to the EtOH-AlCl3 solution. The samples were heated at 75 °C for 12 h with a condenser (10 °C) on top. LiCoO2 or NMC622 completely dissolved during the reaction.
[0066] The EtOH-AlCl3 solutions and the solutions after reaction with LiCoO2 or NMC622 were characterized in several ways. 27 Al and 1H NMR spectra were acquired on a Bruker Avance 600 spectrometer. The spectrometer was run at 104.26 MHz and 600.13 MHz for 27Al and 1H nuclei, respectively, with a 14.1 T narrow-bore superconducting magnet at radio frequency field strengths of 20.8 kHz and 26 kHz, respectively, and all spines were allowed to relax back to thermal equilibrium with a recycle delay of 12.0 seconds. No standard solutions were used in the experiments, and all signals were detected at room temperature.
[0067] For EtOH-AlCl3 (10 wt% AlCl3) solution at room temperature 27 The Al nuclear magnetic resonance (NMR) spectrum (Figure 6) shows [AlCl(EtOH)5] at 9.8 ppm and 12.8 ppm, respectively. 2+ and [AlCl2(EtOH)4] + Two distinct signals assigned to the cations are clearly shown. When LiCoO2 (Co / Al molar ratio is 1:2) was completely dissolved in solution after 12 h at 75 °C, [AlCl(EtOH)5] 2+ and [AlCl2(EtOH)4] + The new peaks are shifted downfield due to magnetic effects from the dissolved Co(II) cations. 27 No Al NMR peaks are observed (Figure 6).
[0068] For UV-visible spectroscopy, an Agilent Cary 60 UV-Vis spectrophotometer was used. The spectrum of pure EtOH-AlCl3 solution in the range of 350-750 nm was used as the baseline measurement. The solutions after reaction with NMC622 or LiCoO2 were diluted with EtOH-AlCl3 solution for UV-Vis measurements. Samples were placed in 10x10mm quart cuvettes sealed with plastic caps.
[0069] The presence of Co(II) cations is evidenced by the UV-Vis spectrum of the solution after reaction with LiCoO2, as shown in Figure 7. The spectrum shows that the cobalt tetrachloride anion (CoCl4 2-) and the inset in Figure 7 shows a photograph of the solution colored in cobalt blue. The same dissolution behavior of NMC622 in EtOH-AlCl3 under identical reaction conditions is also observed. Figure 8 shows the UV-Vis spectrum of the solution after NMC622 has dissolved, and CoCl4 2- and NiCl4 2- Shows characteristic peaks of anions. MnCl4 2- The anion does not absorb in the UV-Vis range. The inset in Figure 8 is a photograph of a solution of NMC622 in EtOH-AlCl3, showing the characteristic green color of Ni(II). After the reaction was completed, the ethanol was evaporated and collected by rotary evaporation to obtain blue (from LiCoO2) and green (NMC622) powders. The rotary evaporation of ethanol was performed under vacuum at a rotation speed of 120 rpm and a temperature of 80 °C.
[0070] The crystal structure of the powders was identified using X-ray powder diffractometry (XRD) utilizing a Panalytical Empyrean Series 2. All samples were dried in a vacuum at 80 °C for 12 h in an argon-filled glove box. The dried powders were then pressed onto a zero-diffraction silicon plate to form a flat pallet. The surface was sealed with Kapton tape to avoid contact with air and moisture. The scanning range was 10-90°, the step size was 0.013°, and the time per step was 148.92 s.
[0071] The X-ray diffraction (XRD) pattern of the blue powder (from LiCoO2) in Figure 9 clearly shows the content of lithium chloride (LiCl) and cobalt(II) chloride (CoCl2). Figure 10 shows the XRD pattern of the green powder (from NMC622), showing the content of LiCl, CoCl2, nickel(II) chloride (NiCl2), and manganese(II) chloride (MnCl2). The above analysis indicates that the transition metal in the cathode material is reduced from M(III) to M(II).
[0072] An oxygen gas test was performed on the sample, where oxygen gas was identified using a 100g EtOH-AlCl3 batch with LiCoO2 molar ratio of 2:1 = Al:Co, sealed in a glove box with O2 < 0.01 ppm. The gas test did not detect the evolution of oxygen gas, therefore, the oxide in the cathode is unlikely to be the reducing agent.
[0073] A possible reducing agent is ethanol, which is known to be capable of reducing to acetaldehyde. To follow up on this, further characterization by NMR was performed. Figure 11 shows the NMR spectra of EtOH-AlCl3 after complete dissolution of LiCoO2. 1 H NMR is shown (dotted line). To identify acetaldehyde as the reaction product, 10% by volume of anhydrous acetaldehyde was also added to the same solution. 1 A H NMR spectrum was obtained (solid line in FIG. 11), and the comparison demonstrated the formation of acetaldehyde after the reaction, as indicated by the doublet at 4 ppm.
[0074] Based on the above analysis, the representative active species was AlCl2 + and AlCl 2+ Using the formula, the following reaction mechanism between EtOH-AlCl3 and LiCoO2 is proposed:
[0075] [ka]
[0076] NMC622 follows the same reaction mechanism. The efficiency of the leaching and purification steps was measured by inductively coupled plasma optical emission spectroscopy (ICP-OES) by measuring the amount of aluminum (Al), cobalt (Co), and lithium (Li) utilizing a Perkin-Elmer Optima 7300 DV ICP-OES instrument. A known amount (mg) of sample was dissolved in a strong acidic solution and then the volume was made up to 100 ml.
[0077] ICP-OES measurements showed that the Al content in the blue powder from LiCoO2 could be easily removed by water washing and filtration after heat treatment at 150°C. The heated powder was mixed with deionized water, and then a pink transparent supernatant and a white precipitate could be separated. The elemental analysis by ICP-OES of the supernatant and precipitate are shown in Table 2.
[0078] [Table 2]
[0079] These results demonstrate that EtOH-AlCl3 can extract cathode active materials with high efficiency, low temperature, and without emissions. When compared to hydrometallurgical processes, an extremely acidic solution (pH below zero) was utilized to enhance leaching efficiency, along with the addition of a reducing agent such as H2O2. The low acidity of the solution proposed here demonstrates the importance of aluminum complexes in the extraction of transition metals, as ethanol acts as a reducing agent, eliminating the need to introduce H2O2 into the system. The method can be used with any type of AlCl3, including primary aliphatic alcohols, to dissolve AlCl3. n (3-n) (where n = 4, 3, 2, and 1) is universal for all other solvents that form ions. For example, AlCl3 in diglyme and tetraglyme is AlCl4 - Anions and AlCl2 + cation, or in tetrahydrofuran (THF), AlCl4 - [AlCl2(THF)4] + and [AlCl(THF)5] 2+ With AlCl3(THF)2, aluminum complexes such as AlCl3 are formed. All these AlCl3 solutions show high leaching efficiency for the cathode material. This new type of extraction reagent consisting of AlCl3 in an organic solvent can be used to recycle used lithium-ion batteries with any type of lithium transition metal oxide cathode.
[0080] The terms and expressions employed are used for purposes of description and not limitation, and there is no intention in the use of such terms and expressions to exclude any equivalents of the features shown and described or portions thereof, but it is recognized that various modifications are possible within the scope of the embodiments of the present disclosure. Thus, although the present disclosure has been specifically disclosed by specific embodiments and optional features, it is to be understood that modifications and variations of the concepts disclosed herein may be made by those skilled in the art, and that such modifications and variations are considered to be within the scope of the embodiments of the present disclosure.
[0081] Further examples Illustrative examples are provided below, the numbering of which should not be construed as designating a level of importance.
[0082] Example 1 is a method for recycling a lithium ion battery cathode material, comprising reducing the lithium ion battery cathode material with an ionic liquid comprising a chloroaluminate anion, and separating the material from the lithium ion battery cathode.
[0083] In Example 2, the subject matter of Example 1 optionally includes that the ionic liquid comprises a Lewis-neutral chloroaluminate anion. In Example 3, the subject matter of any one or more of Examples 1-2 optionally includes that the ionic liquid includes a tetrachloroaluminate anion.
[0084] In Example 4, the subject matter of any one or more of Examples 1-3 optionally includes that the ionic liquid comprises an organic solution of aluminum chloride. In Example 5, the subject matter of any one or more of Examples 1-4 optionally includes a -methylimidazolium tetrachloroaluminate ionic liquid for a lithium ion battery cathode material.
[0085] In Example 6, the subject matter of any one or more of Examples 1-5 optionally includes, wherein reducing the lithium ion battery cathode material includes adding a tetrachloroaluminate ionic liquid to the lithium ion battery cathode material.
[0086] In Example 7, the subject matter of any one or more of Examples 1-6 optionally includes a molar ratio of 1:2. In Example 8, the subject matter of any one or more of Examples 1-7 optionally includes a molar ratio of 1:10.
[0087] In Example 9, the subject matter of any one or more of Examples 1-8 optionally includes a molar ratio of 1:50. In Example 10, the subject matter of any one or more of Examples 1-9 optionally includes a solution for a lithium ion battery cathode material.
[0088] In Example 11, the subject matter of any one or more of Examples 1-10 optionally includes where separating material from the lithium ion battery cathode includes separating and removing cobalt from the lithium ion battery cathode.
[0089] In Example 12, the subject matter of any one or more of Examples 1-11 optionally includes where separating material from the lithium ion battery cathode includes separating and removing lithium from the lithium ion battery cathode.
[0090] In Example 13, the subject matter of any one or more of Examples 1-12 optionally includes where separating the material from the lithium ion battery cathode includes centrifugation.
[0091] In Example 14, the subject matter of any one or more of Examples 1-13 optionally includes where separating the material from the lithium ion battery cathode includes extracting cobalt as a cation.
[0092] In Example 15, the subject matter of any one or more of Examples 1-14 optionally includes where separating material from the lithium ion battery cathode includes extracting cathode active material.
[0093] In Example 16, the subject matter of any one or more of Examples 1-15 optionally includes where separating the material from the lithium ion battery cathode includes extracting the cathode active material without emissions.
[0094] In Example 17, the subject matter of any one or more of Examples 1-16 optionally includes where separating the material from the lithium ion battery cathode includes extracting the cathode active material at room temperature.
[0095] In Example 18, the subject matter of any one or more of Examples 1-17 optionally includes preparing an ionic liquid including a chloroaluminate anion prior to reducing the lithium ion battery cathode material.
[0096] In Example 19, the subject matter of Example 18 optionally includes mixing EMIMCl with AlCl3 in a 1:1 molar ratio. In Example 20, the subject matter of any one or more of Examples 18-19 optionally includes a powder for EMIMCl.
[0097] In Example 21, the subject matter of any one or more of Examples 18-20 optionally includes ethanol.
Claims
1. 1. A method for recycling a battery cathode material, comprising: reducing the battery cathode material with a liquid comprising chloroaluminate ions; and separating a material from the battery cathode material.
2. 2. The method of claim 1, wherein the liquid containing chloroaluminate ions comprises an ionic liquid having a Lewis-neutral chloroaluminate anion.
3. 2. The method of claim 1, wherein the liquid containing chloroaluminate ions comprises an ionic liquid having tetrachloroaluminate anions.
4. The method of claim 1 , wherein the liquid containing the chloroaluminate ions comprises an organic solution of aluminum chloride.
5. 10. The method of claim 1, wherein reducing the battery cathode material comprises adding 1-ethyl-3-methylimidazolium tetrachloroaluminate ionic liquid to the battery cathode material.
6. 10. The method of claim 1, wherein reducing the battery cathode material comprises adding a tetrachloroaluminate ionic liquid to the battery cathode material.
7. 10. The method of claim 1, wherein reducing the cathodic material comprises adding tetrachloroaluminate ionic liquid to the cathodic material in a 1:2 molar ratio.
8. 10. The method of claim 1, wherein reducing the cathodic material comprises adding tetrachloroaluminate ionic liquid to the cathodic material in a molar ratio of 1:
10.
9. 10. The method of claim 1, wherein reducing the cathodic material comprises adding tetrachloroaluminate ionic liquid to the cathodic material in a molar ratio of 1:
50.
10. Reducing the cathodic material comprises reducing the cathodic material by 3 The method of claim 1 comprising adding a solution to the battery cathode material.
11. 10. The method of claim 1, wherein separating materials from the battery cathode material comprises separating and removing cobalt from the battery cathode material.
12. 10. The method of claim 1, wherein separating material from the battery cathode material comprises separating and removing lithium from the battery cathode material.
13. The method of claim 1 , wherein separating the material from the battery cathode material further comprises centrifuging.
14. 10. The method of claim 1, wherein separating materials from the battery cathode material comprises extracting cobalt as a cation.
15. The method of claim 1 , wherein separating materials from the battery cathode material comprises extracting cathode active material.
16. 10. The method of claim 1, wherein separating materials from the battery cathode material comprises extracting the cathode active material without emissions.
17. 10. The method of claim 1, wherein separating the material from the battery cathode material comprises extracting the cathode active material at room temperature.
18. 10. The method of claim 1, further comprising preparing the liquid containing chloroaluminate ions prior to reducing a lithium ion battery cathode material.
19. The step of preparing the liquid containing chloroaluminate ions comprises adding AlCl to EMIMCl. 3 20. The method of claim 18, comprising mixing in a 1:1 molar ratio.
20. Preparing the liquid containing chloroaluminate ions comprises anhydrous AlCl 320. The method of claim 18, comprising gradually adding the powder to the EMIMCl.
21. Preparing the liquid containing chloroaluminate ions comprises anhydrous AlCl 3 to ethanol.
Citation Information
Patent Citations
Recycle method for cathode material of nickel-cobalt-manganese acid lithium battery
CN111206153A
Method and apparatus for recycling lithium-ion batteries
KR1020180080992A
Processes for recovering rare earth elements
US20170306514A1