Method for preparing lithium hexafluorophosphate

A novel LiPF6 production process using ultra-high purity AHF and lithium fluoride, along with a specialized crystallization apparatus, addresses impurity issues in high-strength batteries, achieving enhanced purity and safety for electric vehicle batteries.

JP2024542511APending Publication Date: 2024-11-15GUJARAT FLUOROCHEMICALS LTD

Patent Information

Application Number
JP2024530420
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2021-11-24
Filing Date
2022-11-22
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

Current high-purity lithium hexafluorophosphate (LiPF6) manufacturing processes fail to meet the stringent requirements of modern high-strength batteries for electric vehicles due to high impurity levels, particularly hydrogen fluoride (HF), metal impurities, and water content, which affect battery performance and safety.

Method used

A novel process involving the use of ultra-high purity anhydrous hydrogen fluoride (AHF) and lithium fluoride, combined with a specialized crystallization apparatus, minimizes impurities by controlling reaction conditions and employing a triple-in-one apparatus for crystallization, filtration, and drying, resulting in LiPF6 with purity greater than 99.97% and reduced HF, metal, and water content.

Benefits of technology

The process achieves ultra-high purity LiPF6 with minimal HF (below 70 ppm), metal impurities (1 ppm or less), and water content (10 ppm or less), enhancing battery performance and safety by reducing corrosion and dendrite growth, thereby improving cycle life and capacity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024542511000007
    Figure 2024542511000007
  • Figure 2024542511000001
    Figure 2024542511000001
  • Figure 2024542511000002
    Figure 2024542511000002
Patent Text Reader

Abstract

The present invention discloses a process for preparing high purity lithium hexafluorophosphate (LiPF6), which includes the following steps: The method includes the steps of (a) reacting highly purified anhydrous hydrogen fluoride (AHF) gas with solid phosphorus pentachloride to produce a mixture of pure phosphorus pentafluoride and hydrogen chloride gas; (b) reacting highly purified lithium fluoride dissolved in AHF solution with the mixture of phosphorus pentafluoride and hydrogen chloride gas obtained in step (a) to obtain LiPF6 mother liquor, which is LiPF6 dissolved in AHF; crystallizing LiPF6 from the mother liquor in a static crystallizer, separating the mother liquor and drying the product to remove HF; and then drying and grinding the LiPF6 crystals to obtain LiPF6 powder.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to a method for preparing lithium hexafluorophosphate (LiPF6), more particularly, the present invention relates to a method for preparing high purity LiPF6 useful as an electrolyte in electric vehicle batteries. [Background technology]

[0002] Lithium-ion batteries are now widely found in consumer electronic devices such as mobile phones, laptops, watches, earphones, music systems, etc., due to their high energy density compared to other means of electrical energy storage. Lithium-ion batteries perform well over a wide temperature range, do not self-discharge, can be charged quickly, and are lightweight.

[0003] Apart from consumer electronics, the changing preference from fossil fuel-powered vehicles to electric vehicles is driving renewed interest in batteries. According to a July 23, 2021 report published by Statista Research Department, global battery demand is expected to grow from 185 GWh in 2020 to over 2,000 GWh by 2030. The report predicts that this significant increase will be primarily driven by the electrification of transportation systems, which will account for a large portion of battery demand in 2030 in terms of total energy storage capacity.

[0004] Lithium hexafluorophosphate (LiPF6) is a widely used electrolyte salt in lithium-ion batteries. Other electrolyte salts of Li include LiAsF6, LiBF4, LiClO4, etc. However, LiPF6 is superior to other electrolyte salts in that it exhibits excellent solubility and high conductivity in various solvents, is electrically stable, environmentally friendly, can form a suitable solid electrolyte interface (SEI) film at the electrode, and can induce passivation on the anode current collector to prevent its dissolution.

[0005] Despite being a widely used electrolyte salt in lithium-ion batteries, current manufacturing processes for high-purity LiPF6 are unable to meet the requirements of modern high-strength batteries for use in electric vehicles.

[0006] High-strength batteries are required to satisfy certain conditions, such as the number of cycles must exceed 3,000, the battery decay rate within seven years must not be less than 75%, the charge / discharge temperature, battery safety in extreme climates, and the electrolyte acidity (HF concentration) must be lower, the better.

[0007] In the conventional production of LiPF6, PF5 gas is passed through a solution of LiF in HF to produce LiPF6. Then, the HF is removed and the LiPF6 is crystallized. However, one of the drawbacks of the conventional method is that a large amount of impurities are adsorbed on the surface of the LiPF6 crystals in the form of HF, etc. Furthermore, it is very difficult to reduce the amount of such impurities in LiPF6, such as HF, without resorting to complicated reactions, procedures, and additional purification steps.

[0008] Impurities in the form of HF etc. cause corrosion of the electrodes, which directly affects the capacity and performance of the battery.

[0009] Furthermore, the presence of various metallic impurities, such as transition metal impurities, is detrimental to battery performance. For example, transition metal ions dissolved in the electrolyte can deposit on the anode surface, which can cause decomposition of LiPF6 and the growth of lithium dendrites, resulting in an internal short circuit.

[0010] Water is another problematic impurity in lithium-ion batteries. Its presence has a detrimental effect on battery performance. Water can react with LiPF6, thereby reducing the capacity of the battery. Its presence is also associated with reduced cycling performance and loss of active material. Water can destroy the protective solid electrolyte interfacial layer and be reduced at the anode to produce H2 gas. The presence of H2 gas can increase the internal pressure of the battery, posing a risk of explosion. Summary of the Invention [Problem to be solved by the invention]

[0011] Therefore, there is a need to develop a process for the preparation of LiPF6 that addresses one or more of the above-mentioned shortcomings. [Means for solving the problem]

[0012] In one aspect, the present invention provides a process for preparing ultra-high purity LiPF6, which is useful as an electrolyte in batteries, preferably as an electrolyte in electric vehicle batteries.

[0013] In yet another aspect, the present invention provides ultra-high purity LiPF6 with minimal concentration of hydrogen fluoride (HF), preferably 70 ppm or less.

[0014] Reference may be made to embodiments of the present invention, examples of which are illustrated in the accompanying drawings, which are intended to be illustrative and not limiting, and while the invention will generally be described in relation to these embodiments, it will be understood that it is not intended to limit the scope of the invention to these particular embodiments. [Brief description of the drawings]

[0015] [Figure 1] A process flow diagram is shown. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0016] It should be noted that as used herein, the singular forms "a," "a," and "the" include plural references unless the context clearly dictates otherwise. Thus, for example, reference to a composition containing "a compound" includes a mixture of two or more compounds. It should also be noted that the term "or" is typically used in the sense of including "and / or" unless the context clearly dictates otherwise.

[0017] The various quantity expressions relating to "%" or "% w / w" mean percentage by weight of the total solution or composition, unless otherwise specified.

[0018] The present invention relates to a process for preparing ultra-high purity LiPF6, which is useful as an electrolyte in high strength batteries, preferably as an electrolyte in electric vehicle batteries.

[0019] In one embodiment, the process for preparing ultra-high purity LiPF6 comprises: (a) reacting anhydrous hydrogen fluoride (AHF) gas with solid phosphorus pentachloride to produce high purity phosphorus pentafluoride and hydrogen chloride gas; PCl5 + 5AHF → PF5 + 5HCl; (b) reacting the lithium fluoride dissolved in AHF with the mixture of phosphorus pentafluoride and hydrogen chloride gas obtained in step (a) to obtain a lithium hexafluorophosphate mother liquor, which is LiPF6 dissolved in AHF; PF5+LiF → LiPF6; and (c) crystallizing LiPF6 from the mother liquor and separating the crystallized LiPF6 from the mother liquor; (d) drying the crystallized LiPF6 to evaporate HF from the crystal surface, optionally followed by solvent-assisted drying; (e) grinding and optionally sieving the dried LiPF6 crystals to obtain LiPF6 powder; Including, Here, anhydrous hydrogen fluoride (AHF) gas is purified prior to use in the process, and the lithium fluoride used in the method is obtained from lithium bicarbonate and hydrogen fluoride.

[0020] In one embodiment of the present invention, the purified anhydrous hydrogen fluoride (AHF) gas contains less than 0.1 ppm cationic (metallic) impurities, or less than 1 ppm anionic impurities, or less than 0.1 ppm water, or a combination thereof.

[0021] In yet another embodiment, purified anhydrous hydrogen fluoride (AHF) gas is reacted with a PCl5 solid bed reactor under stirring.

[0022] In yet another embodiment, anhydrous hydrogen fluoride (AHF) gas is purified by treatment with fluorine (F2) gas as an oxidizing agent.

[0023] In a preferred embodiment, step (b) is carried out in a reactor and the off-gas from the dissolver or reactor containing PF5, HCl, and HF is redirected to the dissolver for second stage reabsorption.

[0024] In yet another embodiment, step (b) is carried out at a temperature in the range of -5 to 5°C, preferably 0°C.

[0025] In yet another embodiment, step (b) is carried out in a dissolver and the off-gas from the dissolver containing PF5, HCl, and HF is redirected to the dissolver for resorption of PF5.

[0026] In a preferred embodiment, the crystallization of LiPF6 in step (c) is carried out under vacuum or reduced pressure and cooling at -45 to -5°C, preferably -35°C, for an extended period of time.

[0027] In yet another embodiment, the crystallization of LiPF in step (c) is carried out in a static crystallizer.

[0028] One aspect of the present invention provides a special crystallizer structure, which simplifies the traditional three chemical processes into one device by using a three-in-one device for crystallization, filtration, and primary drying, which greatly reduces the risk of multiple movements of HF-reactive materials and the associated risks faced by operators performing this operation.

[0029] In a preferred embodiment, the static crystallizer rotates once every 48 hours, allowing the crystals to grow slowly to large size and minimizing surface area for HF adsorption.

[0030] In another preferred embodiment, the mother liquor of step (c) is recycled by adding LiF at -5 to 5°C, preferably at 0°C.

[0031] In a preferred embodiment, drying of the crystallized LiPF6 in step (d) is carried out by hot water circulation in the dryer jacket, preferably at 60-70°C, under vacuum for about 6 hours.

[0032] In yet another embodiment, drying of the crystallized LiPF6 in step (d) is followed by solvent assisted drying, preferably using a solvent such as methanol, ether, dichloromethane, etc.

[0033] Another aspect of the method is to use a mesh size that screens out the larger crystals with less adsorbed HF as the final product, while the smaller crystals with more adsorbed HF are recycled through the mother liquor, thus reducing the total concentration of HF in the final product and reducing the production cost by recovering the LiPF6 crystals.

[0034] In a preferred embodiment, sieving of the dried LiPF6 crystals is carried out through a mesh size of 90 or less.

[0035] In another embodiment, the lithium fluoride used in the present process is obtained from the following steps: (1) treating lithium carbonate with carbon dioxide to obtain lithium bicarbonate; Li2CO3+H2O+CO2→2LiHCO3; (2) reacting lithium bicarbonate with ultrapure hydrogen fluoride to obtain lithium fluoride; LiHCO3+HF → LiF+CO2+H2O; and (3) drying and grinding the lithium fluoride.

[0036] In a preferred embodiment, the CO2 is recycled and reused.

[0037] In another embodiment, the reactor effluent containing PF5, HCl, oxides of phosphorus and HF is redirected to the mother liquor for a second stage reabsorption process, improving the overall efficiency of the process.

[0038] In another embodiment, the gaseous effluent from the mother liquor tank containing HCl and HF is redirected to a recovery system, improving the efficiency of the overall process.

[0039] Another aspect of the present invention relates to ultra-high purity lithium hexafluorophosphate (LiPF6) having a purity of at least 99.97%.

[0040] In a preferred embodiment of the present invention, the ultra-high purity lithium hexafluorophosphate (LiPF6) is - Insoluble materials in an amount not exceeding 200 ppm; or - Metallic impurities, each present in an amount not exceeding 1 ppm, or Hydrogen fluoride in an amount not exceeding -70 ppm; or -10 ppm or less of sulfate ion (SO4 2- ), or -5ppm or less of nitrate ion (NO3 - ), or -5 ppm or less of chloride ions (Cl - ), or - Water / moisture or a combination thereof in amounts less than 10ppm Includes.

[0041] In a preferred embodiment of the present invention, the ultra-high purity lithium hexafluorophosphate (LiPF6) contains the following metal impurities:

[0042] [Table 1]

[0043] According to the method of the present invention, battery grade high purity PCl5 is obtained from a commercial source. In step (a), gaseous high purity anhydrous hydrogen fluoride (AHF) reacts with solid phosphorus pentachloride (PCl5) to produce phosphorus pentafluoride (PF5) and hydrogen chloride.

[0044] The impurities in LiPF6 are a direct result of impurities present in the primary raw materials, i.e., AHF and LiF. Therefore, as described below, the AHF and LiF used in the present invention are purified to minimize moisture, insoluble impurities, and metallic impurities. In other words, only high purity AHF and LiF are used in the present invention.

[0045] Usually, PF5 is prepared by dissolving PCl5 in AHF. This results in impurities such as AsF5, BF4, etc. However, in the present invention, gaseous AHF is reacted with solid PCl5 in a packed bed reactor. The resulting PF5 is then passed through a filter to remove any PCl5 particles that may be floating in the gas stream, resulting in high purity PF5 gas. Thus, the process can be carried out in a packed bed reactor with high purity gaseous AHF to remove or minimize impurities and water in the PF5 gas.

[0046] In step (b), the PF5 produced in step (a) enters reactor 2 where it reacts with LiF dissolved in AHF. This results in the formation of LiPF6 dissolved in AHF, also called mother liquor. Preferably, step (b) is carried out at a temperature in the range of -5 to 5°C, more preferably at 0°C.

[0047] The reactor effluent, containing PF5, HCl, oxides of phosphorus and HF, is redirected to the mother liquor for the second stage reabsorption process, which improves the overall efficiency of the reaction, particularly by improving the recovery efficiency of PF5.

[0048] Crystallization is carried out from the mother liquor in a crystallization vessel where the mother liquor is cooled. The mother liquor is cooled for an extended period of time.

[0049] The static crystallizer used in the present invention rotates once every 48 hours. The LiPF6 crystals slowly grow to a large size. The larger the size of the LiPF6 crystals, the smaller the surface area on which HF can adsorb, resulting in LiPF6 with the lowest HF content. The crystals are separated by passing through a mesh sieve. The relatively large crystals of the separated LiPF6 are crushed and dried under vacuum at a temperature of 60-70°C for about 6 hours to remove as much HF as possible, in order to obtain high-purity powder LiPF6.

[0050] The relatively small crystals of LiPF6 can be recycled by adding a certain amount of lithium fluoride to the mother liquor at -5 to 5 °C, preferably at 0 °C, and repeating the process to obtain larger sized crystals.

[0051] Using a conventional rotary crystallizer instead of a static crystallizer results in smaller crystals with HF contents in the range of 150-250 ppm. Using higher temperatures for drying leads to decomposition and production of HF from the LiPF6 crystals. EXAMPLES

[0052] Several representative embodiments of the present invention are discussed below. The present invention, in its broader aspects, is not limited to the specific details and representative methods. Illustrative examples are described in this section in connection with the embodiments and methods provided.

[0053] The following examples are illustrative of the invention but are not intended to limit its scope.

[0054] FIG. 1 shows a process flow diagram for preparing LiPF6 according to an embodiment of the present disclosure. According to this process, HF solution (101) is passed through an evaporator (V1) to convert HF into gaseous state (102). The gaseous state HF (102) obtained from the evaporator (V1) is reacted with PCl5 powder (103) in a first reactor (R1) to obtain intermediate product PF5, HCl (g), and unreacted HF (105). The intermediate product (105) is passed through a filter (F1) and sent to a second reactor (R2) to obtain a product solution (106) containing LiPF6 and HF solution, which is transferred to a residence tank (V2). The product solution (106) from the residence tank (V2) is transferred to a crystallizer (V3) where the product LiPF6 (107) is recovered and the mother liquor (108) is separated. The product (107) is passed through a sieve (S1) to obtain the product LiPF6 of the desired size, and the remainder is recycled to the mother liquor tank (V4). The mother liquor (108) containing LiF and HF solution is sent to the mother liquor tank (V4), where HF solution and LiF (104) are further added, and the treated mother liquor (109) is recycled to the second reactor (R2) to obtain the product solution (106) containing LiPF6 and HF solution. The tail gas (111) from the mother liquor tank (V4) is sent to a recovery system (S2) to reuse and recycle the HF gas (102), and the unrecovered tail gas (110) is sent to a three-stage scrubber (S3) for disposal.

[0055] The impurities in LiPF6 are a direct result of impurities present in the primary raw materials, i.e., AHF and LiF. Therefore, as described below, the AHF and LiF used in the present invention are purified to minimize moisture, insoluble impurities, and metallic impurities. In other words, only high purity AHF and LiF are used in the present invention.

[0056] In commercial HF, metals such as Fe, Ca, and Mg react with active PF5 in the synthesis reaction vessel to produce FeF3, CaF2, and MgF2, which increases impurities in the LiPF6 crystals. Therefore, the AHF used in the present invention is purified before being used in the method of the present invention.

[0057] Commercially available AHF is purified by treatment with fluorine (F2) as an oxidizing agent to fluorinate AHF impurities and remove most metals such as arsenic. If AHF is not purified by reacting with F2, gaseous impurities such as metal fluorides, AsF5, and BF4 can contaminate the mother liquor. The use of purified AHF in the present invention further minimizes impurities in the LiPF6 crystals of the present invention.

[0058] <Example 1> Example 1: Preparation of high purity AHF: Pure fluorine gas was added at 0.2 kg / cm 2 The commercial AHF in the reactor is purged at 25° C. for 3 minutes at a pressure of 1000 psi and a temperature of 25° C. After the impurities are precipitated as fluorides, the pure AHF is transferred from the reactor to a distillation column. The impurity levels in the commercial and purified AHF are shown below.

[0059] [Table 2]

[0060] Insoluble impurities such as silicates, fluorosilicates, and sulfates of metals such as Fe, Ca, K, Na, Ni, Pb, Zn, Cr, Mg, Cu, and Al are present in LiF. Some metals do not dissolve in AHF and remain as solid particles. Others react with AHF to produce fluoride materials such as FeF3, NaF, CaF2, and MgF2. In this case, the fluoride materials precipitate as solids at the bottom of the crystallizer and stay with the LiPF6 crystals. This is the main source of impurities in LiPF6. These insoluble impurities reach LiPF6, thereby increasing the total levels of Ca, Mg, Na, K, etc. to more than 100 ppm. Therefore, to produce high purity LiPF6, it is necessary that the LiF used in the process is free of the above metal impurities.

[0061] <Example 2> Example-2: Preparation of high purity LiF: In a 100 L reactor, 3.9 kg of commercial Li2CO3 is mixed with 78 liters of pure deionized water to prepare a slurry. Pure carbon dioxide gas (99% purity) is added at 3 kg / cm 2 The slurry is passed through a reactor at a pressure of 100000000000000000 for 6 hours to produce soluble LiHCO3. The LiHCO3 solution is passed through two sets of cartridge filters to filter out insoluble impurities. The LiHCO3 solution is then passed through a cation exchange resin column to remove soluble impurities. 84 kg of the purified LiHCO3 solution is then reacted with 425 liters of 50% HF to obtain LiF. The LiF thus produced is filtered and dried by evaporating water at 130° C. The impurity levels of the purified LiF are as follows:

[0062] [Table 3]

[0063] Therefore, to improve the purity of LiF, lithium carbonate is treated with CO2 gas to produce soluble lithium bicarbonate (LiHCO3). This process removes heavy metal ions and insoluble impurities with water. The insoluble impurities are filtered through two sets of fine filters. The ions dissolved in the water are removed by cation exchange. The resulting LiHCO3 is substantially free of any insoluble heavy metal impurities. To further improve the efficiency of the process, the CO2 released during the reaction is recycled.

[0064] <Example 3> Example-3: Preparation of LiPF6 - 930g of high purity AHF produced as above is added to 1500g of solid PCl5 maintained at a temperature of 40-80°C. The mixture of PF5+HCl+HF produced from this reaction is fed to a solution of LiF+AHF (171g+7800g of AHF) at -5-5°C to produce 1kg of LiPF6 in AHF solvent. LiPF6 is crystallized from this solution, filtered and dried to obtain the pure product. The impurity levels of ultra-high purity LiPF6 by the process of the present invention are shown below:

[0065] [Table 4]

[0066] The LiPF6 obtained by the above process contains insoluble materials in an amount of 200 ppm or less, and / or contains metal impurities each present in an amount of 1 ppm or less, and / or contains HF in an amount of 70 ppm or less, and / or contains SO4 in an amount of 10 ppm or less. 2- and / or NO3 in amounts less than 5 ppm - and / or Cl in an amount not exceeding 5 ppm - and / or contains water in an amount of 10 ppm or less, or a combination thereof.

[0067] The purity of LiPF6 obtained by the process of the present invention is at least 99.97%.

[0068] In the absence of the AHF purification process, preparation of high purity LiF, and the crystallization and drying steps, metallic impurities will carry over and become part of the final product, i.e., LiPF6. In that case, the LiPF6 impurity profile will be 30-80 ppm total metallic impurities instead of 1 ppm or less.

[0069] Furthermore, it can be seen that the metal impurities of the ultra-high purity LiPF6 according to the present invention are significantly lower than those of the battery grade LiPF6 commercially available from SIGMA-ALDRICH-MERCK or NANOSHEL as shown in the table below. It can be concluded that the ultra-high purity LiPF6 produced by the process disclosed in the present invention is superior.

[0070] [Table 5]

[0071] The above description of the present invention is merely illustrative of the present invention and is not intended to be limiting. Since modifications of the disclosed embodiments incorporating the essence and substance of the present invention may occur to those skilled in the art, the present invention should be construed as including all within the scope of the present disclosure.

Claims

1. Ultra-high purity lithium hexafluorophosphate (LiPF 6 ), comprising the steps of: (a) reacting anhydrous hydrogen fluoride (AHF) gas with solid phosphorus pentachloride to produce high purity phosphorus pentafluoride and hydrogen chloride gas; PCl 5 +5AHF→PF 5 +5HCl; (b) reacting lithium fluoride dissolved in AHF with the mixture of phosphorus pentafluoride and hydrogen chloride gas obtained in step (a) to produce LiPF dissolved in AHF; 6 obtaining a lithium hexafluorophosphate mother liquor which is P.F. 5 + LiF → LiPF 6 and (c) The LiPF 6 is crystallized from the mother liquor, and the crystallized LiPF 6 from said mother liquor; (d) The crystallized LiPF 6 to evaporate HF from the crystal surface, followed by solvent-assisted drying; and (e) The dried LiPF 6 The crystals are crushed and optionally sieved to obtain LiPF 6 Obtaining a powder, The anhydrous hydrogen fluoride (AHF) gas is purified prior to use in the process, and the lithium fluoride used in the process is obtained from lithium bicarbonate and hydrogen fluoride. method.

2. 2. The method of claim 1, wherein the purified anhydrous hydrogen fluoride (AHF) gas contains 0.1 ppm or less of cationic (metallic) impurities, or 1 ppm or less of anionic impurities, or 0.1 ppm or less of moisture, or a combination thereof.

3. The purified anhydrous hydrogen fluoride (AHF) gas is 5 The method of claim 1 , further comprising reacting with a solid layer.

4. The anhydrous hydrogen fluoride (AHF) gas contains pure fluorine (F 2 ) or fluorine (F 2 ) and nitrogen (N 2 2. The method of claim 1 , wherein the ester is purified by treatment with a mixture of 1,2-dichlorophenyl ether.

5. The step (b) is carried out in a dissolver or reactor, 5 2. The method of claim 1, wherein tail gas from the dissolver or reactor containing HCl and HF is redirected back to the dissolver for second stage reabsorption.

6. The method of claim 1, wherein said step (b) is carried out at a temperature in the range of -5 to 5°C, preferably at 0°C.

7. LiPF in step (c) 6 is carried out under vacuum or reduced pressure and cooling at -45 to -5°C, preferably -35°C, for a long period of time, preferably 24 to 36 hours.

8. LiPF in step (c) 6 The method of claim 1 , wherein the crystallization of is carried out in a static crystallizer.

9. 9. The method of claim 8, wherein the static crystallizer rotates once every 48 hours, allowing the crystals to grow slowly to large size and minimizing the surface area for HF adsorption.

10. The process according to claim 1, wherein the mother liquor in step (c) is recycled by adding LiF at -5 to 5°C, preferably at 0°C.

11. The crystallized LiPF in step (d) 6 The method according to claim 1, wherein drying of is carried out by hot water circulation in the dryer jacket, preferably at 60-70° C., under vacuum, for about 6 hours.

12. Crystallized LiPF in step (d) 6 2. The method according to claim 1, wherein said drying of is followed by solvent assisted drying, preferably using solvents such as methanol, ether and dichloromethane.

13. Dried LiPF 6 2. The method of claim 1, wherein the sieving of the crystals is performed through a mesh size of 90 or less.

14. The lithium fluoride used in the process is (1) treating lithium carbonate with carbon dioxide to obtain lithium bicarbonate; Li 2 CO 3 +H 2 O+CO 2 →2LiHG 3 ; (2) reacting the lithium bicarbonate with ultra-pure hydrogen fluoride to obtain lithium fluoride; LiHCO 3 +HF→LiF+CO 2 +H 2 O; and (3) drying and pulverizing the lithium fluoride; The method of claim 1 , wherein the compound is obtained from

15. The CO 2 The method of claim 14, wherein is recycled and reused.

16. P.F. 5 2. The method of claim 1, wherein the effluent from the reactor, comprising HCl, oxides of phosphorus and HF, is redirected to the mother liquor for a second stage reabsorption process.

17. 10. The method of claim 1, wherein a gaseous effluent from the mother liquor tank comprising HCl and HF is redirected to a recovery system.

18. Ultra-high purity lithium hexafluorophosphate (LiPF) having a purity of at least 99.97% 6 ).

19. - Insoluble material in an amount not exceeding 200 ppm; or - metallic impurities, each present in an amount not exceeding 1 ppm, or Hydrogen fluoride in an amount not exceeding -70 ppm; or -10 ppm or less of sulfate ion (SO 4 2- ), or Nitrate ions (NO 3 - ), or -5 ppm or less of chloride ions (Cl - ), or - Water / moisture in an amount less than or equal to 10 ppm, or a combination thereof The ultra-high purity lithium hexafluorophosphate (LiPF) according to claim 18, 6 ).

20. The ultra-high purity lithium hexafluorophosphate (LiPF) according to claim 18 or 19, which contains the following metal impurities: 6 ). 【Table 1】

Citation Information

Patent Citations

  • A method for preparing crystalline lithium hexafluorophosphate

    CN105036100B

  • Preparation method of high-end lithium hexafluorophosphate

    CN108439362A

Cited By

  • Preparation method of phosphorus pentafluoride and lithium hexafluorophosphate

    CN119976757A