Low dielectric polyamic acid and polyimide films
Optimized polyamic acid and polyimide films with specific compositions address the insulation and adhesion issues in flexible thin circuit boards, ensuring low dielectric loss and high adhesion for reliable high-frequency signal transmission.
Patent Information
- Application Number
- JP2024530578
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2021-11-25
- Filing Date
- 2022-11-23
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2042-11-23
AI Technical Summary
Existing polyimide films do not possess sufficient low dielectric properties and adhesion to maintain insulation at high frequencies, leading to increased stray capacitance and dielectric loss, which affects communication speed and reliability in flexible thin circuit boards.
The development of polyamic acid and polyimide films using specific compositions of biphenyltetracarboxylic dianhydride, pyromellitic dianhydride, and p-phenylenebis(trimellitate anhydride) with diamines like oxydianiline, m-tolidine, and paraphenylenediamine, optimized for low dielectric loss and high adhesion, forming flexible metal foil laminates and electronic components.
The films achieve low dielectric loss factors of 0.0025 or less, high adhesion strength of 0.8 gf/cm or more, and maintain insulation stability at high frequencies, enabling efficient signal transmission up to 10 GHz.
Smart Images

Figure 2024542527000001 
Figure 2024542527000002 
Figure 2024542527000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a polyamic acid and a polyimide film having excellent low dielectric properties, adhesiveness and heat resistance. [Background technology]
[0002] Polyimide (PI) is a polymeric material based on imide rings, which have excellent chemical stability along with a rigid aromatic main chain, and has the highest levels of heat resistance, chemical resistance, electrical insulation, chemical resistance, and weather resistance among organic materials. In particular, due to its excellent electrical properties such as excellent insulating properties, i.e., low dielectric constant, it has been attracting attention as a highly functional polymer material in the electrical, electronic and optical fields.
[0003] 2. Description of the Related Art Recently, with the trend towards lighter and smaller electronic products, flexible thin circuit boards with high integration density have been actively developed. Such thin circuit boards tend to have a structure in which a circuit containing metal foil is formed on a polyimide film that has excellent heat resistance, low temperature resistance and insulating properties, but is also easily flexible. Flexible metal clad laminates are mainly used for such thin circuit boards, and an example is Flexible Copper Clad Laminate (FCCL), which uses a thin copper plate as a metal foil. Polyimide is also used as a protective film and insulating film for thin circuit boards.
[0004] Meanwhile, as electronic devices are increasingly equipped with a variety of functions, they are required to have high operation and communication speeds. To meet this demand, thin circuit boards capable of high-speed communication at high frequencies have been developed. To realize high-frequency and high-speed communication, insulators with high impedance that can maintain electrical insulation even at high frequencies are required. Since impedance is inversely proportional to the frequency and dielectric constant (Dk) formed in the insulator, the dielectric constant must be as low as possible to maintain insulation even at high frequencies. However, in the case of ordinary polyimide, the dielectric properties are not currently at a level excellent enough to maintain sufficient insulation for high-frequency communications.
[0005] In addition, the lower the dielectric properties of the insulator, the less stray capacitance (stray capacitance) that is undesirable in thin circuit boards. It is known that it is possible to reduce the capacitance and noise generation, thereby eliminating a significant portion of the causes of communication delays.
[0006] Therefore, the low dielectric properties of polyimide are currently recognized as the most important factor in the performance of thin circuit boards. In particular, in the case of high-frequency communication, the dielectric loss caused by polyimide is inevitable. The dielectric dissipation factor (Df) indicates the degree of electrical energy wasted in a thin circuit board and is closely related to the signal transmission delay that determines the communication speed. Therefore, keeping the dielectric dissipation factor of polyimide as low as possible is recognized as an important factor in the performance of thin circuit boards.
[0007] In addition, the more moisture the polyimide film contains, the higher the dielectric constant becomes and the higher the dielectric loss factor becomes. Polyimide film has excellent inherent properties, making it ideal for use in thin circuit boards. However, due to the imide group exhibiting polarity, it is relatively vulnerable to moisture, which can cause a decrease in its insulating properties. Therefore, there is a need to develop a polyimide film having dielectric properties, particularly a low dielectric loss factor, while maintaining a certain level of the mechanical properties, thermal properties and highly adhesive surface properties inherent to polyimides. [Prior art documents] [Patent documents]
[0008] [Patent Document 1] Republic of Korea Patent Publication No. 10-2021-0055230 Summary of the Invention [Problem to be solved by the invention]
[0009] In order to solve the above problems, an object of the present invention is to provide a polyamic acid and polyimide film having excellent low dielectric properties, high adhesion and heat resistance. Therefore, a substantial object of the present invention is to provide specific examples thereof. [Means for solving the problem]
[0010] In order to achieve the above object, one embodiment of the present invention relates to a dianhydride acid component including two or more selected from the group consisting of biphenyltetracarboxylic dianhydride (BPDA), pyromellitic dianhydride (PMDA), and p-phenylenebis(trimellitate anhydride) (TAHQ); and a diamine component including at least one selected from the group consisting of oxydianiline (ODA), m-tolidine, and paraphenylenediamine (PPD), A polyamic acid is provided. (However, the polyamic acid necessarily contains m-tolidine as the diamine component.)
[0011] Other embodiments of the present invention include biphenyltetracarboxylic dianhydride (BPDA), pyromellitic dianhydride (PMDA) and p-phenylenebis(trimellitate anhydride). anhydride, TAHQ, and / or 2-hydroxybutanol; and a diamine component including at least one selected from the group consisting of oxydianiline (ODA), m-tolidine, and paraphenylenediamine (PPD), A polyimide film is provided. (However, the polyimide film necessarily contains m-tolidine as the diamine component.) Yet another embodiment of the present invention is a laminate comprising the polyimide film and a thermoplastic resin layer, A multilayer film is provided.
[0012] Yet another embodiment of the present invention is a method for manufacturing a laminate comprising the polyimide film and an electrically conductive metal foil, A flexible metal foil laminate is provided. Yet another embodiment of the present invention includes the flexible metal foil laminate, Provide electronic components. Effect of the Invention
[0013] As described above, the polyamic acid and polyimide film of the present invention, which are composed of specific components and in a specific composition ratio, provide low dielectric properties, high adhesive properties and high heat resistance, and are useful in various fields where such properties are required, particularly in electronic components such as flexible metal foil laminates. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0014] Hereinafter, embodiments of the present invention will be described in more detail. Prior to this, the terms and words used in this specification and claims should not be interpreted limited to their ordinary or dictionary meanings, but should be interpreted with meanings and concepts that correspond to the technical ideas of the present invention, in accordance with the principle that an inventor can appropriately define the concepts of terms in order to explain his / her invention in the best possible way. Therefore, it should be understood that the configuration of the embodiment described in this specification is merely one of the most preferred embodiments of the present invention and does not fully represent the technical ideas of the present invention, and that there may be various equivalents and modifications that can replace them at the time of this application.
[0015] In this specification, the singular expression includes the plural expression unless the context clearly indicates otherwise. It should be understood that in this specification, the terms "comprise", "comprise", "have" and the like are intended to specify the presence of embodied features, numbers, steps, components, or combinations thereof, and do not preclude the possibility of the presence or addition of one or more other features, numbers, steps, components, or combinations thereof.
[0016] Whenever an amount, concentration, or other value or parameter is given herein as a range, a preferred range or a list of an upper preferred value and a lower preferred value, it should be understood to specifically disclose all ranges formed by any pair of any upper range limit or preferred value, and any lower range limit or preferred value, regardless of whether a range is otherwise disclosed. Where a range of numerical values is recited herein, unless otherwise stated, the range is intended to include the endpoints thereof, and all integers and fractions within the range. It is not intended that the scope of the invention be limited to the specific values recited when defining a range.
[0017] As used herein, "dianhydride acid" is intended to include precursors or derivatives thereof which may not technically be dianhydrides but which nevertheless must react with a diamine to form a polyamic acid which is then converted back to a polyimide.
[0018] As used herein, "diamine" is intended to include precursors or derivatives thereof, which may not technically be diamines, but which nevertheless must react with a dianhydride to form a polyamic acid, which is then converted back to a polyimide.
[0019] The polyamic acid according to the present invention is copolymerized with a dianhydride component including two or more selected from the group consisting of biphenyltetracarboxylic dianhydride (BPDA), pyromellitic dianhydride (PMDA), and p-phenylenebis(trimellitate anhydride, TAHQ), and a diamine component including one or more selected from the group consisting of oxydianiline (ODA), m-tolidine, and paraphenylenediamine (PPD). However, the polyamic acid must contain m-tolidine as the diamine component. can be done.
[0020] Preferably, the dianhydride acid component can include p-phenylene bis(trimellitate anhydride). For example, the dianhydride acid component may be p-phenylene bis(trimellitate anhydride) alone, a combination of p-phenylene bis(trimellitate anhydride) and biphenyltetracarboxylic dianhydride, or a combination of p-phenylene bis(trimellitate anhydride) and pyromellitic dianhydride.
[0021] The diamine component may also be m-tolidine alone, a combination of m-tolidine and paraphenylenediamine, or a combination of m-tolidine and oxydianiline.
[0022] In one embodiment, based on a total content of the dianhydride acid components of 100 mol%, the content of the biphenyltetracarboxylic dianhydride may be 30 mol% or more and 75 mol% or less, the content of the pyromellitic dianhydride may be 60 mol% or less, and the content of the p-phenylene bis(trimellitate anhydride) may be 30 mol% or more and 70 mol% or less.
[0023] In one embodiment, based on 100 mol% of the total content of the diamine components, the content of the m-tolidine may be 40 mol% or more and 100 mol% or less, the content of the paraphenylenediamine may be 60 mol% or less, and the content of the oxydianiline may be 60 mol% or less.
[0024] In one embodiment, the ratio of the mole % of the m-tolidine to the mole % of the p-phenylene bis(trimellitate anhydride) (mol % of m-tolidine / p-phenylene bis(trimellitate anhydride)) may be 1.1 or more and 3.5 or less. Preferably, the ratio of the molar percentage of the m-tolidine to the molar percentage of the p-phenylene bis(trimellitate anhydride) (mole percentage of m-tolidine / p-phenylene bis(trimellitate anhydride)) may be 1.5 or more and 2.9 or less.
[0025] The polyimide film according to the present invention is obtained by subjecting a polyamic acid solution containing a dianhydride acid component including two or more selected from the group consisting of biphenyltetracarboxylic dianhydride (BPDA), pyromellitic dianhydride (PMDA), and p-phenylenebis(trimellitate anhydride) (TAHQ), and a diamine component including one or more selected from the group consisting of oxydianiline (ODA), m-tolidine, and paraphenylenediamine (PPD) to an imidization reaction.
[0026] The polyimide film may necessarily contain m-tolidine as the diamine component. Preferably, the dianhydride acid component can include p-phenylene bis(trimellitate anhydride). For example, the dianhydride acid component may be p-phenylene bis(trimellitate anhydride) alone, a combination of p-phenylene bis(trimellitate anhydride) and biphenyltetracarboxylic dianhydride, or a combination of p-phenylene bis(trimellitate anhydride) and pyromellitic dianhydride.
[0027] The diamine component may be m-tolidine alone, a combination of m-tolidine and paraphenylenediamine, or a combination of m-tolidine and oxydianiline. stomach.
[0028] In one embodiment, based on a total content of the dianhydride acid components of 100 mol%, the content of the biphenyltetracarboxylic dianhydride may be 30 mol% or more and 75 mol% or less, the content of the pyromellitic dianhydride may be 60 mol% or less, and the content of the p-phenylene bis(trimellitate anhydride) may be 30 mol% or more and 70 mol% or less.
[0029] If the content of the p-phenylene bis(trimellitate anhydride) exceeds 70 mol %, the heat resistance of the polyimide film may decrease, making it difficult to form the film.
[0030] Furthermore, if the content of the biphenyltetracarboxylic dianhydride exceeds 75 mol %, the dielectric loss factor of the polyimide film increases, and the low dielectric properties may be deteriorated.
[0031] In one embodiment, based on 100 mol% of the total content of the diamine components, the content of the m-tolidine may be 40 mol% or more and 100 mol% or less, the content of the paraphenylenediamine may be 60 mol% or less, and the content of the oxydianiline may be 60 mol% or less.
[0032] In one embodiment, the ratio of the mole % of the m-tolidine to the mole % of the p-phenylene bis(trimellitate anhydride) (mol % of m-tolidine / p-phenylene bis(trimellitate anhydride)) may be 1.1 or more and 3.5 or less. Preferably, the ratio of the mole % of m-tolidine to the mole % of p-phenylene bis(trimellitate anhydride) may be ≧1.5 and ≦2.9. If the ratio of the mol% of the m-tolidine to the mol% of the p-phenylene bis(trimellitate anhydride) (mol% of m-tolidine / p-phenylene bis(trimellitate anhydride)) is less than 1.1 or exceeds 3.5, the dielectric loss factor of the polyimide film may increase, resulting in reduced low dielectric properties.
[0033] In one embodiment, the polyimide film may have a dielectric loss factor (Df) of 0.0025 or less and an adhesive strength of 0.8 gf / cm or more. Preferably, the polyimide film may have a dielectric loss factor of 0.0026 or less.
[0034] The polyimide film may have a glass transition temperature of 270° C. or lower. Preferably, the polyimide film may have a glass transition temperature of 205° C. or higher.
[0035] Meanwhile, the polyimide film can be formed even at a process temperature of 400° C. or more.
[0036] As described above, the polyimide film according to the present invention satisfies all of the above-mentioned requirements and can be used as an insulating film for flexible metal foil laminates. In addition, the polyimide film can ensure insulation stability even at high frequencies and minimize signal transmission delay.
[0037] The present invention provides a multilayer film comprising the above-mentioned polyimide film and a thermoplastic resin layer, and a flexible metal foil laminate comprising the above-mentioned polyimide film and an electrically conductive metal foil.
[0038] As the thermoplastic resin layer, for example, a thermoplastic polyimide resin layer can be used. do.
[0039] The metal foil used is not particularly limited, but when the flexible metal foil laminate of the present invention is used for electronic or electrical equipment, the metal foil may be, for example, copper or a copper alloy, stainless steel or an alloy thereof, nickel or a nickel alloy (including alloy 42), aluminum or an aluminum alloy.
[0040] In general flexible metal foil laminates, copper foils such as rolled copper foils and electrolytic copper foils are often used, and are also preferably usable in the present invention. In addition, the surface of these metal foils may be coated with an anti-rust layer, a heat-resistant layer, or an adhesive layer.
[0041] In the present invention, the thickness of the metal foil is not particularly limited, and may be any thickness that allows the metal foil to exhibit sufficient function depending on the application.
[0042] The flexible metal foil laminate according to the present invention may have a structure in which a metal foil is laminated on one side of the polyimide film, or an adhesive layer containing a thermoplastic polyimide is added to one side of the polyimide film, and the metal foil is laminated in a state of being attached to the adhesive layer.
[0043] The present invention further provides an electronic component including the flexible metal foil laminate as an electrical signal transmission circuit, the electrical signal transmission circuit being an electronic component that transmits signals at a high frequency of at least 2 GHz, particularly at least 5 GHz, and more particularly at least 10 GHz.
[0044] The electronic component may be, for example, but is not limited to, a communication circuit for a mobile terminal, a communication circuit for a computer, or a communication circuit for an aerospace application.
[0045] In the present invention, the polyamic acid can be produced, for example, by (1) A method in which the entire amount of the diamine component is placed in a solvent, and then the dianhydride component is added in an amount substantially equimolar to the diamine component to polymerize it; (2) A method in which the entire amount of the dianhydride component is placed in a solvent, and then a diamine component is added in an amount substantially equimolar to the dianhydride component to polymerize it; (3) A method in which a part of the diamine component is placed in a solvent, a part of the dianhydride component is mixed with the reaction components in a ratio of about 95 to 105 mol %, the remaining diamine component is added, and the remaining dianhydride component is added successively thereto, so that the diamine component and the dianhydride component are polymerized in substantially equimolar amounts; (4) A method in which a dianhydride component is placed in a solvent, a part of the components in the diamine compound is mixed in a ratio of 95 to 105 mol % relative to the reactive components, and then another dianhydride component is added, followed by the remaining diamine component, so that the diamine component and the dianhydride component are substantially equimolar, thereby polymerizing the mixture; (5) A method of forming a first composition by reacting some diamine components and some dianhydride acid components in a solvent so that one of them is in excess, and forming a second composition by reacting some diamine components and some dianhydride acid components in another solvent so that one of them is in excess, and then mixing the first and second compositions to complete polymerization, in which if the diamine component is in excess when the first composition is formed, the dianhydride acid component is in excess in the second composition, and if the dianhydride acid component is in excess in the first composition, the diamine component is in excess in the second composition, and the first and second compositions are mixed to polymerize so that the total diamine components and dianhydride acid components used in these reactions are substantially equimolar. However, the polymerization method is not limited to the above example, and any known method can be used to produce polyamic acid.
[0046] In one embodiment, a method for producing a polyimide film according to the present invention includes the steps of: preparing a polyamic acid by polymerizing a dianhydride component including two or more selected from the group consisting of biphenyltetracarboxylic dianhydride (BPDA), pyromellitic dianhydride (PMDA), and p-phenylenebis(trimellitate anhydride, TAHQ), and a diamine component including one or more selected from the group consisting of m-tolidine and paraphenylenediamine (PPD); The method may further include a step of forming a film of the precursor composition containing the polyamic acid on a support and then imidizing the film.
[0047] In the present invention, the polymerization method of the polyamic acid as described above can be defined as a random polymerization method, and the polyimide film prepared from the polyamic acid of the present invention prepared by the above process can be preferably applied in terms of maximizing the effect of the present invention, which is to reduce the dielectric loss factor (Df), moisture absorption rate and air permeability. However, in the above polymerization method, the length of the repeating unit in the polymer chain is relatively short as described above, so that there may be a limit to the excellent properties of the polyimide chain derived from the dianhydride acid component. Therefore, the polymerization method of polyamic acid that can be particularly preferably used in the present invention is the block polymerization method.
[0048] On the other hand, the solvent for synthesizing the polyamic acid is not particularly limited, and any solvent that dissolves the polyamic acid can be used, but an amide-based solvent is preferable. Specifically, the solvent may be an organic polar solvent, more specifically, an aprotic polar solvent, for example, one or more selected from the group consisting of N,N-dimethylformamide (DMF), N,N-dimethylacetamide, N-methyl-pyrrolidone (NMP), gamma-butyrolactone (GBL), and diglyme, but is not limited thereto, and may be used alone or in combination of two or more kinds as needed. In one example, the solvent is preferably N,N-dimethylformamide or N,N-dimethylacetamide.
[0049] In addition, in the process for producing the polyamic acid, a filler may be added for the purpose of improving various properties of the film such as sliding properties, thermal conductivity, corona resistance, loop hardness, etc. The filler to be added is not particularly limited, but preferred examples include silica, titanium oxide, alumina, silicon nitride, boron nitride, calcium hydrogen phosphate, calcium phosphate, mica, etc.
[0050] The particle size of the filler is not particularly limited and may be determined depending on the film properties to be modified and the type of filler to be added. In general, the average particle size is 0.05 to 100 μm, preferably 0.1 to 75 μm, more preferably 0.1 to 50 μm, and particularly preferably 0.1 to 25 μm. If the particle size is below this range, the modifying effect is unlikely to be achieved, whereas if it exceeds this range, the surface properties may be significantly damaged or the mechanical properties may be significantly reduced.
[0051] The amount of the filler to be added is not particularly limited, and may be determined depending on the film properties to be modified, the particle size of the filler, etc. In general, the amount of the filler to be added is 0.01 to 100 parts by weight, preferably 0.01 to 90 parts by weight, and more preferably 0.02 to 80 parts by weight, relative to 100 parts by weight of polyimide. If the amount of filler added is below this range, the modifying effect of the filler is difficult to manifest. If the temperature exceeds this range, the mechanical properties of the film may be significantly damaged. The method of adding the filler is not particularly limited, and any known method may be used.
[0052] In the production method of the present invention, the polyimide film is produced by a thermal imidization method and a chemical imidization method. Alternatively, the imidation layer may be produced by a hybrid imidation method in which a thermal imidization method and a chemical imidization method are performed in parallel.
[0053] The thermal imidization method is a method in which a chemical catalyst is excluded and the imidization reaction is induced by a heat source such as hot air or an infrared dryer. The thermal imidization method can imidize the amic acid groups present in the gel film by heat-treating the gel film at a variable temperature in the range of 100 to 600°C, specifically, 200 to 500°C, more specifically, 300 to 500°C. However, even during the process of forming the gel film, a portion of the amic acid (approximately 0.1 mol % to 10 mol %) is imidized, and therefore the polyamic acid composition can be dried at a variable temperature in the range of 50°C to 200°C, which also falls within the category of the thermal imidization method.
[0054] In the case of the chemical imidization method, a polyimide film can be produced using a dehydrating agent and an imidization agent by methods known in the art. As an example of the composite imidization method, a dehydrating agent and an imidization agent are added to a polyamic acid solution, which is then heated at 80 to 200°C, preferably 100 to 180°C, partially cured and dried, and then heated at 200 to 400°C for 5 to 400 seconds to produce a polyimide film. EXAMPLES
[0055] The functions and effects of the present invention will be described in more detail below through specific examples of the present invention, however, these examples are merely presented as examples of the present invention and do not define the scope of the invention.
[0056] Manufacturing example: Manufacturing of polyimide film The polyimide film of the present invention can be prepared by the following conventional method known in the art: First, the dianhydride and diamine components are reacted in an organic solvent to obtain a polyamic acid solution. In this case, the solvent may be an aprotic polar solvent such as an amide solvent, for example, N,N'-dimethylformamide, N,N'-dimethylacetamide, N-methyl-pyrrolidone, or a combination thereof. The dianhydride and diamine components may be added in the form of powder, lump, or solution. It is preferable to add them in the form of powder at the beginning of the reaction to proceed with the reaction, and then add them in the form of a solution to adjust the polymerization viscosity. The resulting polyamic acid solution is mixed with an imidization catalyst and a dehydrating agent and applied to a support. Examples of the catalyst used include tertiary amines (e.g., isoquinoline, β-picoline, pyridine, etc.), and examples of the dehydrating agent include, but are not limited to, anhydrous acids. In addition, examples of the support used include, but are not limited to, glass plates, aluminum foils, circular stainless steel belts, stainless steel drums, etc.
[0057] The film coated on the support is gelled on the support by dry air and heat treatment. The gelled film is separated from the support and heat treated to complete drying and imidization. After the heat treatment, the film is heat treated under a certain tension to remove residual stress inside the film generated during the film formation process.
[0058] Specifically, 500ml of DMF was added to a reactor equipped with a stirrer and nitrogen inlet / outlet pipes while injecting nitrogen, and the temperature of the reactor was set to 30°C. Then, biphenyltetracarboxylic dianhydride (BPDA), pyromellitic dianhydride (PMDA), p-phenylenebis(trimellitate anhydride, TAHQ), m-tolidine (MTD), paraphenylenediamine (PPD) and oxydianiline (ODA) were added in a controlled composition ratio and in a designated order and completely dissolved. Thereafter, the temperature of the reactor was raised to 40°C under a nitrogen atmosphere and the mixture was stirred for 120 minutes to produce a polyamic acid with a primary reaction viscosity of 1,500cP. The polyamic acid thus produced was stirred so as to have a final viscosity of 100,000 to 120,000 cP. The catalyst and dehydrating agent were added to the prepared final polyamic acid in an adjusted content, and then a polyimide film was produced using an applicator.
[0059] Examples and Comparative Examples As shown in Table 1 below, the contents of the dianhydride acid component and the diamine component in Examples 1 to 6 and Comparative Examples 1 to 3 were adjusted to produce polyimide films according to the Production Examples.
[0060] In the polyimide films of Examples 1 to 6, the ratio of the molar percentage of m-tolidine to the molar percentage of p-phenylene bis(trimellitate anhydride) (mole percentage of m-tolidine / p-phenylene bis(trimellitate anhydride)) was adjusted to 1.1 or more and 3.5 or less.
[0061] [Table 1]
[0062] The dielectric loss factor (Df), adhesive strength and glass transition temperature (Tg) of the prepared polyimide film were measured, and the film formability at a process temperature of 400° C. was observed. The results are shown in Table 2 below.
[0063] [Table 2]
[0064] In the film formability in Table 2, "O" indicates that the film was formed at a process temperature of 400°C, and "X" indicates that the film was not formed at a process temperature of 400°C.
[0065] The dielectric loss factor (Df), adhesive strength and glass transition temperature of the prepared polyimide film were measured as follows.
[0066] (1) Measurement of dielectric loss factor The dielectric loss factor (Df) is measured using Keysight's ENA (Vector Network The film was left in an environment of 23°C / 50% RH for 24 hours and measured using a cavity resonance method (SPDR) using a 3-phase diffractive optical analyzer.
[0067] (2) Measurement of adhesive strength The adhesive strength was measured by placing a bonding sheet (1 mil, epoxy type) on both sides of the polyimide film, placing 1 / 2 oz copper foil on both sides, placing protective PI on them, and then heating to 160°C and thermocompressing for 30 minutes at a pressure of 5 MPa. The film was cut into 10 mm width pieces and then subjected to a 180° peel test.
[0068] (3) Measurement of glass transition temperature The glass transition temperature (Tg) was measured by determining the loss modulus and storage modulus of each film using DMA, and the inflection point in the tangent graph of these was taken as the glass transition temperature.
[0069] As shown in Table 2, it was confirmed that the polyimide film prepared according to the embodiment of the present invention not only exhibited a low dielectric loss factor of 0.0025 or less, but also had an adhesive strength of 0.8 gf / cm or more. In addition, the glass transition temperature was equivalent to 270°C or less, and no problems occurred during film formation even at a process temperature of 400°C.
[0070] In contrast, in Comparative Example 1, which had the same components and composition ratio of the dianhydride acid as in Example 1 but used only oxydianiline as the diamine component, the heat resistance was significantly reduced and no film was formed. Furthermore, in comparison with Examples 1 to 3, the content of p-phenylene bis(trimellitate anhydride) was increased to more than 70 mol % in Comparative Example 3, and the heat resistance was significantly reduced and no film was formed.
[0071] On the other hand, in comparison with Examples 1 to 3, in Comparative Example 2 in which the ratio of the molar percentage of m-tolidine to the molar percentage of p-phenylene bis(trimellitate anhydride) (mole % of m-tolidine / p-phenylene bis(trimellitate anhydride)) was adjusted to exceed 3.5, there was no problem in film formation, but the dielectric loss factor exceeded 0.0025 and the glass transition temperature exceeded 270°C. Therefore, it can be seen that the low dielectric properties and heat resistance of the polyimide film of the present application are achieved by the components and composition ratios specified in the present application.
[0072] In contrast, in the case of Comparative Examples 1 to 3, in which components and composition ratios different from those in the Examples were used, problems arose in film formability due to a higher dielectric loss factor and lower heat resistance compared to the Examples. Therefore, it can be expected that the Comparative Examples are difficult to use in electronic components in which signal transmission is performed at high frequencies in the gigahertz range.
[0073] The present invention has been described above with reference to an embodiment thereof. However, a person having ordinary knowledge in the field to which the present invention pertains will be able to make various applications and modifications within the scope of the present invention based on the above content. [Industrial Applicability]
[0074] The polyamic acid and polyimide film of the present invention, which are composed of specific components and in a specific composition ratio, provide low dielectric properties, high adhesive properties, and high heat resistance, and are therefore useful in various fields where such properties are required, particularly in electronic components such as flexible metal foil laminates.
Claims
1. a dianhydride acid component including two or more selected from the group consisting of biphenyltetracarboxylic dianhydride (BPDA), pyromelitic dianhydride (PMDA), and p-phenylenebis(trimellitate anhydride) (TAHQ); and a diamine component including at least one selected from the group consisting of oxydianiline (ODA), m-tolidine, and paraphenylenediamine (PPD), Polyamic acid. (However, the polyamic acid necessarily contains m-tolidine as the diamine component.)
2. the content of the biphenyltetracarboxylic dianhydride is 30 mol % or more and 75 mol % or less, the content of the pyromellitic dianhydride is 60 mol % or less, and the content of the p-phenylene bis(trimellitate anhydride) is 30 mol % or more and 70 mol % or less, based on 100 mol % of the total content of the dianhydride acid components; The polyamic acid according to claim 1 .
3. the content of the m-tolidine is 40 mol % or more and 100 mol % or less, based on 100 mol % of the total content of the diamine components; The content of the paraphenylenediamine is 60 mol% or less, The content of the oxydianiline is 60 mol% or less. The polyamic acid according to claim 1 .
4. the ratio of the mole percent of m-tolidine to the mole percent of p-phenylene bis(trimellitate anhydride) (mole percent of m-tolidine / p-phenylene bis(trimellitate anhydride)) is 1.1 or more and 3.5 or less; The polyamic acid according to claim 1 .
5. a dianhydride acid component including two or more selected from the group consisting of biphenyltetracarboxylic dianhydride (BPDA), pyromelitic dianhydride (PMDA), and p-phenylenebis(trimellitate anhydride) (TAHQ); and a diamine component including at least one selected from the group consisting of oxydianiline (ODA), m-tolidine, and paraphenylenediamine (PPD), Polyimide film. (However, the polyimide film necessarily contains m-tolidine as the diamine component.)
6. the content of the biphenyltetracarboxylic dianhydride is 30 mol % or more and 75 mol % or less, the content of the pyromellitic dianhydride is 60 mol % or less, and the content of the p-phenylene bis(trimellitate anhydride) is 30 mol % or more and 70 mol % or less, based on 100 mol % of the total content of the dianhydride acid components; The polyimide film according to claim 5 .
7. the content of the m-tolidine is 40 mol % or more and 100 mol % or less, based on 100 mol % of the total content of the diamine components; The content of the paraphenylenediamine is 60 mol% or less, The content of the oxydianiline is 60 mol% or less. The polyimide film according to claim 5 .
8. The dielectric loss factor (Df) is 0.0025 or less, The adhesive strength is 0.8 gf / cm or more. The polyimide film according to claim 5 .
9. the ratio of the mole percent of m-tolidine to the mole percent of p-phenylene bis(trimellitate anhydride) (mole percent of m-tolidine / p-phenylene bis(trimellitate anhydride)) is 1.1 or more and 3.5 or less; The polyimide film according to claim 5 .
10. A polyimide film according to any one of claims 5 to 9, and a thermoplastic resin layer. Multilayer film.
11. A laminate comprising the polyimide film according to any one of claims 5 to 9 and an electrically conductive metal foil. Flexible metal foil laminate.
12. Comprising the flexible metal foil laminate of claim 11. Electronic components.
Citation Information
Patent Citations
Polyimide precursor resin composition, polyimide resin film, flexible printed wiring board, circuit-fitted suspension, and hard disc drive
JP2014208793A
Flexible metal-clad laminate and method for manufacturing the same
JP2015507563A
Polyimide resin precursor
JP2017132898A
Metal-clad laminate and patterned metal-clad laminate
JP2020044690A
Amino compound, polyamic acid and polyimide that are based on that amino compound, and method for producing them