Thin Wall Heat Shrink Tubing

PTFE heat shrink tubing with high recovery ratios and minimal length change addresses the limitations of existing materials, enabling efficient encapsulation and improved heat transfer in complex applications.

JP2024542559AActive Publication Date: 2024-11-15ZEUS CO LLC
View PDF 14 Cites 0 Cited by

Patent Information

Application Number
JP2024531190
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2022-04-15
Filing Date
2023-03-03
Publication Date
2024-11-15
Estimated Expiration
2043-03-03

AI Technical Summary

Technical Problem

Existing heat shrink tubing materials have limited recovery ratios of up to 4:1 and exhibit significant longitudinal length changes, which hinder efficient encapsulation and heat transfer in applications requiring high precision and complex geometries.

Method used

Development of PTFE heat shrink tubing with recovery ratios exceeding 5:1 and thin walls, achieving minimal longitudinal length change during recovery, facilitated by controlled expansion and cooling processes.

Benefits of technology

The new PTFE heat shrink tubing provides enhanced encapsulation capabilities for complex geometries and improved heat transfer, allowing for efficient processing and reduced material decomposition at lower temperatures.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024542559000001_ABST
    Figure 2024542559000001_ABST
Patent Text Reader

Abstract

Heat shrink tubing is provided that generally comprises at least one fluoropolymer resin and exhibits a variety of desirable properties. The tubing may exhibit desirable physical properties such as heat shrinkability, high expansion / recovery ratios, low longitudinal shrinkage, low temperature recovery, and average wall thickness of less than about 0.003 inches.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present application relates to heat-shrinkable polymeric tubing, which finds application in a variety of fields, and to methods for making such heat-shrinkable polymeric tubing. [Background technology]

[0002] Heat shrink tubing generally comprises a plastic material extruded and expanded into a tubular shape. The extruded and expanded tube is designed to shrink (i.e., reduce in diameter) when heated to a predetermined temperature. Because of this, heat shrink tubing can provide a variety of functions. Heat shrink tubing can provide a tightly fitting protective jacket that closely covers and insulates various elements (e.g., protects the elements from abrasion and provides thermal, chemical, moisture and / or electrical insulation). Heat shrink tubing can be useful for holding certain elements together (i.e., within the same heat shrink tube). Additionally, heat shrink tubing can act to seal / isolate certain elements from other elements and can be used to join / fuse two elements, e.g., two tubes. Heat shrink tubing can also be useful for modifying the properties of an underlying material (e.g., by surrounding another material and shrinking that material as well). These properties make the tubing useful for a variety of purposes, and heat shrink tubing is utilized across a variety of industries, such as medical, chemical, electrical, optical, electronic, aerospace, automotive, and telecommunications.

[0003] In medical applications, heat shrink tubing is particularly useful in designing smaller and more complex devices (e.g., catheters, endoscopes, etc.) that are inserted into the body. One representative medical application of heat shrink tubing is in the manufacture of guide catheters that comprise a tubular structure having an inner layer of polymer, a middle layer of wire braid, and an outer layer of another polymer. To assemble such catheters, an expanded heat shrink tubing is typically applied to a shaft assembled around a mandrel, and the assembly is exposed to a high temperature sufficient to shrink the heat shrink tubing. Under these conditions, the outer polymeric layer within the catheter shaft melts and flows out, the heat shrink tubing shrinks, and a compressive force is applied such that the inner and outer polymeric layers of the catheter shaft bond together, encapsulating the wire braid within. The heat shrink tubing is then removed and disposed of, and the catheter assembly is removed from the mandrel. See, for example, U.S. Pat. No. 5,399,433 to Ross and U.S. Pat. No. 5,499,433 to Lunn, both of which are incorporated herein by reference.

[0004] It should be noted that heat shrink tubing has been commercially manufactured for decades using a variety of processes, such as, for example, vacuum expansion, gas pressure forming, sequential heating / stretching, etc. Known methods of expanding heat shrink tubing are shown, for example, in the disclosures of Edward et al., U.S. Pat. No. 6,399,433, Sullivan, U.S. Pat. No. 6,399,452, Yoshida et al., U.S. Pat. No. 6,399,623, Henson, U.S. Pat. No. 6,399,711, Henson, U.S. Pat. No. 6,399,723, and Roof et al., U.S. Pat. No. 6,399,623, each of which is incorporated herein by reference. However, heat shrink tubing is typically only commercially available in grades having a maximum recovery ratio of 4:1. For example, typical polytetrafluoroethylene ("PTFE") heat shrink tubing is currently commercially available with a maximum recovery ratio of 4:1, and typical fluorinated ethylene propylene ("FEP") heat shrink tubing is currently commercially available with a maximum recovery ratio of 2:1. Furthermore, these products typically have a longitudinal length change of up to 15% upon recovery.

[0005] Thus, there is a need for tubing that can be applied to device components to encapsulate and compress them as needed, providing high recovery without a corresponding increase in longitudinal deformation. Additionally, there is a need for tubing with thin walls that can enhance heat transfer during stacking and increase overall efficiency. [Prior art documents] [Patent documents]

[0006] [Patent Document 1] U.S. Patent No. 7,306,585 [Patent Document 2] U.S. Patent No. 5,755,704 [Patent Document 3] U.S. Patent No. 2,987,767 [Patent Document 4] U.S. Patent No. 3,412,189 [Patent Document 5] U.S. Patent No. 7,625,194 [Patent Document 6] U.S. Patent No. 9,296,165 [Patent Document 7] U.S. Patent No. 9,327,444 [Patent Document 8] U.S. Patent No. 9,440,044 Summary of the Invention

[0007] The present disclosure relates to fluoropolymer heat shrink tubing in an expanded form that exhibits higher recovery rates than conventional heat shrink tubing without a corresponding significant longitudinal increase (as typically seen in conventional heat shrink tubing). Additionally, certain heat shrink tubing of the present disclosure has thin walls previously unattainable in commercially available fluoropolymer heat shrink tubing and / or is recoverable at lower temperatures than are used in conventional heat shrink processes.

[0008] One aspect of the present disclosure provides PTFE heat shrink tubing having a recovery ratio (RR) of greater than about 5:1. In some embodiments, the PTFE heat shrink tubing of the present disclosure may have a recovery ratio of greater than about 5.5:1, greater than about 6:1, greater than about 7:1, greater than about 8:1, or greater than about 9:1. In some embodiments, the PTFE heat shrink tubing of the present disclosure may have an average wall thickness of 0.003 inches or less after expansion. In certain embodiments, the PTFE heat shrink tubing may have an average wall thickness of about 0.0005 inches or less after expansion.

[0009] Another aspect of the present disclosure provides a PTFE heat shrink tubing, wherein a linear regression performed on a plot of diameter change versus recovery temperature between 310°C and 330°C produces a slope value of greater than about 1.3% / °C. In some embodiments, the PTFE heat shrink tubing has a RR of greater than about 5:1. In certain embodiments, the PTFE heat shrink tubing may have a RR of greater than about 5.5:1, greater than about 6:1, greater than about 7:1, greater than about 8:1, or greater than about 9:1. In some embodiments, the PTFE heat shrink tubing according to the present disclosure may have an average wall thickness of 0.003 inches or less after expansion. In certain embodiments, the PTFE heat shrink tubing may have an average wall thickness of about 0.0005 inches or less after expansion.

[0010] Another aspect of the present disclosure provides a PTFE heat shrink tubing having a difference between the temperature corresponding to the peak temperature of the melting endotherm obtained from a DSC temperature ramp using a heating rate of 10° C. per minute and the temperature corresponding to the relative minimum in an E′-T curve obtained in a DMA temperature ramp of a circumferentially oriented heat shrink tubing specimen in a tensile grip that is greater than about 7.5° C. In some embodiments, the PTFE heat shrink tubing may have a RR of greater than about 5:1. In certain embodiments, the PTFE heat shrink tubing may have a RR of greater than about 5.5:1, greater than about 6:1, greater than about 7:1, greater than about 8:1, or greater than about 9:1. In some embodiments, the PTFE heat shrink tubing according to the present disclosure may have an average wall thickness of 0.003 inches or less after expansion. In certain embodiments, the PTFE heat shrink tubing may have an average wall thickness of about 0.0005 inches or less after expansion. In some embodiments, a linear regression performed on a plot of diameter change versus recovery temperature between 310° C. and 330° C. produces a slope value of greater than about 1.3% / ° C. for the heat shrink tubing of the present disclosure.

[0011] A further aspect of the present disclosure provides a heat shrink tubing comprising tubing with a wall comprising PTFE having an inner diameter (ID) of about 0.3 inches or less after expansion, and the ID is shrinkable by at least about 78% when heated to 350°C for 10 minutes. In some embodiments, the ID of the heat shrink tubing is shrinkable by at least about 80% when heated to 350°C for 10 minutes. In some embodiments, the heat shrink tubing wall has an average wall thickness of about 0.003 inches or less after expansion. In certain embodiments, the heat shrink tubing wall has an average wall thickness of about 0.0005 inches or less after expansion. In certain embodiments, the difference between the temperature corresponding to the peak temperature of the melting endotherm obtained from a DSC temperature ramp using a heating rate of 10°C per minute and the temperature corresponding to the relative minimum in the E'-T curve obtained in a DMA temperature ramp of a circumferentially oriented heat shrink tubing specimen in a tensile grip is greater than about 7.5°C. In some embodiments, a linear regression performed on a plot of diameter change versus recovery temperature between 310° C. and 330° C. produces a slope value of greater than about 1.3% / ° C. for the heat shrink tubing of the present disclosure.

[0012] These and other features, aspects, and advantages of the present disclosure will become apparent from a reading of the following detailed description in conjunction with the accompanying drawings, which are briefly described below. The present disclosure includes any combination of two, three, four, or more features or elements shown in the disclosure or recited in any one or more of the claims, regardless of whether such features or elements are explicitly combined or otherwise recited in the description of a specific embodiment or in the claims herein. The present disclosure is intended to be read in its entirety such that it should be considered that it is intended that any separable features or elements of the present disclosure can be combined, in any of its aspects and embodiments, unless otherwise clearly indicated by the context of the disclosure.

[0013] For an understanding of embodiments of the present invention, reference is made to the accompanying drawings, which are not necessarily drawn to scale and in which reference characters represent components of exemplary embodiments of the present invention. The drawings are merely illustrative and are not to be construed as limiting the present invention. [Brief description of the drawings]

[0014] [Figure 1] 1 is a graph showing storage modulus as a function of temperature for PTFE heat shrink tubing made according to exemplary embodiments of the present disclosure compared to several commercially available PTFE heat shrink tubing; [Diagram 2] FIG. 1 illustrates an overlay of DSC and DMA curves obtained from a PTFE heat shrink tubing made according to an exemplary embodiment of the present disclosure. [Diagram 3] 1 is a graph showing the percent inner diameter change and its linear regression measured in the range of 310° C. to 330° C. for PTFE heat shrink tubing made according to exemplary embodiments of the present disclosure compared to several commercially available PTFE heat shrink tubings when recovered for 10 minutes at various temperatures. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0015] DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS Some, but not all, embodiments of the present invention are described in more detail below with reference to the accompanying drawings. Indeed, these inventions may be embodied in many different forms and are not to be construed as limited to the embodiments set forth herein. Rather, these embodiments are presented so that this disclosure will satisfy applicable legal requirements. Like numbers refer to like elements throughout.

[0016] The terminology used herein is for the purpose of describing particular embodiments only and is not intended to be limiting of the invention. As used herein, the singular forms "a", "an" and "the" are intended to include the plural forms as well, unless the context clearly dictates otherwise. It will be further understood that as used herein, the terms "comprises" and / or "comprising" specify the presence of stated features, integers, steps, operations, elements, and / or components, but do not exclude the presence or addition of one or more other features, integers, steps, operations, elements, components, and / or groups thereof.

[0017] The present disclosure provides heat shrink tubing with unique properties and combinations of unique properties, as further outlined herein. In general, "heat shrink tubing" is shrinkable tubing made by expanding polymeric ("input") tubing (e.g., extruded tubing) to obtain heat shrink tubing (also referred to herein as the "expanded" form). Upon heating and / or sintering, the heat shrink tubing "shrinks" to a size equivalent (or close to) its original / input size (commonly referred to as its "recovered" size). The composition and overall size of the heat shrink tubing according to the present disclosure can range widely and is not particularly limited. The heat shrink tubing can be measured, for example, by its inner diameter ("ID") after expansion (referred to herein as the "expanded inner diameter" (ID e ) or its inner diameter ("ID") after recovery (referred to herein as the "recovered inner diameter (ID) r )), its length, its average wall thickness, its expansion rate (ER), and its recovery rate (RR).

[0018] In some embodiments, the disclosed heat shrink tubing comprises, consists essentially of, or consists of one or more fluorinated polymers. Exemplary fluorinated polymers according to the present disclosure include, but are not limited to, fluorinated ethylene propylene (FEP), polyvinylidene fluoride (PVDF), perfluoroalkoxyalkanes (PFA), perfluoro(alkyl vinyl ethers) (PAVEs) (e.g., perfluoro(methyl vinyl) ether, PMVE, or perfluoro(propyl vinyl) ether (PPVE)), polytetrafluoroethylene (PTFE), terpolymers of tetrafluoroethylene, hexafluoropropylene, and vinylidene fluoride (THV), poly(ethylene-co-tetrafluoroethylene) (ETFE), ethylene chlorotrifluoroethylene (ECTFE), polychlorotrifluoroethylene (PCTFE), copolymers of tetrafluoroethylene and perfluoromethyl vinyl ether (MFA), or copolymers, blends, or derivatives of any two or more of the foregoing. In certain embodiments, the disclosed heat shrink tubing comprises, consists essentially of, or consists of PTFE, and such heat shrink tubing may be referred to herein as "PTFE heat shrink tubing." In some other embodiments, the disclosed heat shrink tubing may comprise, consist essentially of, or consist of one or more non-fluorinated polymers, such as polyaryletherketones. Exemplary polyaryletherketones according to the present disclosure include, but are not limited to, polyetherketone (PEK), polyetheretherketone (PEEK), polyetheretherketoneketone (PEKK), polyetheretherketoneketone (PEEKK), and polyetherketoneetherketoneketone (PEKEKK).

[0019] In some embodiments, one or more additives can be incorporated into the tubing wall. In some such embodiments, one or more additives can be distributed (e.g., substantially uniformly) throughout the wall thickness and length of the tubing. In some embodiments, the one or more additives can include a lubricant, such as, for example, an aliphatic hydrocarbon-based lubricant. In certain embodiments, the lubricant can be, for example, naphthalene. It should be noted that one or more additives mentioned herein may or may not be present in the final product (i.e., the final heat shrink tubing) according to various embodiments of the present disclosure. For example, in certain embodiments, a lubricant can be applied to a polymer resin (e.g., PTFE resin, etc.) before extruding the input tubing, followed by evaporating the lubricant after the input tubing exits the extrusion die and before sintering the input tubing. The amount of lubricant or other additives that can be included is not particularly limited. In some embodiments, for example, the additive (e.g., lubricant) may be included in an amount ranging from about 1% to about 30%, about 16% to about 25%, or about 10% to about 20% by weight based on the total weight of the tubing, hi other embodiments, the tubing may not include any additives therein.

[0020] The size (e.g., length, diameter (i.e., expanded inner diameter, ID), and average wall thickness) of the heat shrink tubing within the scope of the present disclosure is not particularly limited. For example, the length of the tubing described herein can vary from discrete size units (e.g., in some embodiments, 0.25 inches to 120 inches for catheter manufacturing) to lengths that can be easily transported and further cut into discrete size units to large scale production lengths (e.g., hundreds of feet, etc.). The diameter of the tubing described herein can vary, among other things, depending on the intended use of the tubing. Certain expanded IDs of the tubing described herein, particularly for medical applications, can range from about 0.01 inches to about 1.5 inches (e.g., about 0.025 inches to about 0.75 inches, or about 0.05 inches to about 0.5 inches), although tubing having expanded IDs outside this range are also encompassed by the present disclosure, particularly in the context of applications in different fields. In some embodiments, for example, the expanded ID of the tubing can range from about 0.034 inches to about 4 inches.

[0021] With respect to tubing wall thickness, it is noted that the higher expansion / recovery ratios exhibited by the PTFE heat shrink tubing of the present disclosure may, in some embodiments, result in thinner expanded and recovered walls than commercially available PTFE heat shrink tubing and / or FEP heat shrink tubing, for example, as shown in the examples provided herein below. In certain exemplary embodiments, the heat shrink tubing of the present disclosure may have an average wall thickness ranging from about 0.0001 inches to about 0.005 inches, from about 0.0001 inches to about 0.0025 inches, or from about 0.0001 inches to about 0.0005 inches. In some embodiments, the heat shrink tubing of the present disclosure may have an average wall thickness of about 0.005 inches or less, about 0.003 inches or less, about 0.001 inches or less, about 0.00075 inches or less, or about 0.0005 inches or less. Such values ​​are after expansion and before recovery.

[0022] These significantly thinner wall thicknesses may provide significant advantages over commercially available PTFE and FEP heat shrink tubing currently used in the market. For example, the thin wall PTFE heat shrink products of the present disclosure may enhance heat transfer during reflow and increase the overall efficiency of the reflow process. With respect to FEP heat shrink tubing, it is noted that the thermal conductivity of FEP (0.180 W / m·K at reflow temperatures of 200° C. or higher) is much lower than that of PTFE (0.280 W / m·K at reflow temperatures of 200° C. or higher), thus demonstrating improved heat transfer for PTFE heat shrink tubing compared to FEP heat shrink tubing. See, for example, DM Price, M. Jarratt, Thermochimica Acta, 392, 231, 2002, and LK Olifirov, AA Stepashkin, G. Sherif, VV Tcherdyntsev, Polymers, 13, 781, 2021, which are incorporated herein by reference.

[0023] The heat shrink tubing described herein may exhibit advantageous combinations of the following properties, such as two or more thereof: high expansion rate, high recovery rate, recovery at lower temperatures, small length change upon recovery, and / or thin walls after expansion and / or recovery. In some embodiments, heat shrink tubing is provided that exhibits two of these properties (e.g., high expansion rate and high recovery rate, high expansion rate and recovery at lower temperatures, high recovery rate and recovery at lower temperatures, high expansion rate and small length change during recovery, high recovery rate and small length change during recovery, low temperature recovery and small length change during recovery, high recovery rate and thin wall, high expansion rate and thin wall, low temperature recovery and thin wall, small length change and thin wall), three or more of these properties (e.g., high recovery rate, high expansion rate and thin wall, high recovery rate, high expansion rate and recovery at lower temperatures, high recovery rate, high expansion rate and small length change during recovery, etc.), four or more of these properties (e.g., high recovery rate, high expansion rate, thin wall and recovery at lower temperatures, high recovery rate, high expansion rate, thin wall and small length change after recovery, etc.), or all five of these properties are provided.

[0024] Such a property may be defined using the following equation: Expansion rate = ER = ID e / ID o Recovery rate=RR=ID e / ID r Change in length = ΔL = ((L r -L e ) / L e )(100) Diameter change = ΔD = (ID e -ID r ) / ID e )(100)

[0025] In these equations, L e and L r are the length of heat-shrink tubing (in the expanded form) and the length of "recovered" (i.e., heat-shrunk) tubing, respectively. o refers to the original inside diameter (ID) of the delivery tube (i.e., the tube before expansion and subsequent "deflation"), and ID e refers to the inside diameter (ID) of the expanded heat shrink tubing, and ID r refers to the inside diameter (ID) of the recovered (heat-shrunk) tubing. ER, RR, ΔL, and ΔD can be evaluated at any recovery temperature. As used herein, the above parameters were calculated as follows:

[0026] The length change (ΔL) is determined as follows: Cut the expanded tubing to a length of 4 inches before placing the heat shrink tubing in an oven to allow it to recover indefinitely. Carefully cut a 4 inch long specimen from the heat shrink tubing to ensure that the specimen is free of burrs or other deformations and perpendicular to the longitudinal axis of the tubing. After the indefinite recovery process at the specified temperature, re-measure the length of the tubing to the nearest 1 / 64 inch using a verified ruler to determine the amount of shrinkage or elongation that occurred during the process. For example, subtract the expanded length from the recovered length, divide by the expanded length, and then multiply this amount by 100 to obtain the overall length change percentage (ΔL). Typically, the longitudinal change is measured to be within about ±20% (i.e., the length change is allowed to elongate or shrink by about 20% or less during recovery). In some embodiments, the longitudinal change is measured to be within about ±15%, about ±10%, or about ±5%. In certain embodiments, longitudinal changes averaged 5% or less. Standard time and recovery temperature for PTFE heat shrink is 350°C for 10 minutes. Standard time and recovery temperature for FEP is 210°C-221°C for 10 minutes. For catheter manufacturing, PTFE heat shrink is recovered at 260°C to reflow the outer jacket.

[0027] The expansion ratio (ER) is calculated by dividing the measured expanded ID by the measured input ID. The recovery ratio (RR) is determined as follows: Five 4-inch long specimens are cut from the expanded tubing and the expanded ID of each is measured. The specimens are then individually placed in an oven set at a specified temperature for approximately 10 minutes (e.g., the first specimen is heated at 310°C, the second at 320°C, the third at 330°C, the fourth at 340°C, and the fifth at 350°C, respectively). After exposing each heat shrink tubing specimen to the specified recovery temperature for 10 minutes, it is removed from the oven and allowed to cool to ambient temperature. This allows the expanded heat shrink tubing to undergo an unlimited recovery process. After cooling to ambient temperature, the recovered tubing is cut into four pieces of equal length with a sharp razor blade. This provides five different measurement locations along the length of the recovered heat shrink tubing. The ID is then measured at each different location using a validated measuring device and the average is taken as the recovered ID. The ID of the expanded tubing is divided by the ID of the recovered tubing measured after the unlimited recovery process to obtain the recovery ratio (RR) of the heat shrink product at a specified temperature. The diameter change of the heat shrink tubing is subsequently calculated by subtracting the ID of the recovered tubing from the ID of the expanded tubing, dividing by the ID of the expanded tubing, and then multiplying this amount by 100 to obtain the overall diameter change percentage (ΔD).

[0028] With regard to heat shrinking capabilities, in certain embodiments, the tubing disclosed herein is capable of shrinking (reducing in diameter) when exposed to heat (e.g., due to being in an expanded state). Heat shrink material is generally applied to an underlying material (e.g., catheter structure, medical device member, etc.) and heated. When subjected to a thermal cycle, the inner and outer diameters of the tubing are reduced (resulting in a smaller inner diameter (ID) and smaller outer diameter (OD) than those exhibited by the expanded tubing, referred to as the "recovered" ID and OD). Preferably, only the diameter of the tubing is substantially contracted, and not the length (i.e., the tubing is only contracted in one plane). As stated above, the ratio between the expanded ID and the original input ID is referred to as the expansion ratio. The expansion ratio is the expanded ID divided by the original input ID. It has been found that by using a die temperature higher than that typically used, expansion ratios much greater than 4:1 can be obtained. For example, typical expansion ratios for the types of tubing described herein can be at least about 4:1, at least about 5:1, at least about 6:1, at least about 7:1, at least about 8:1, at least about 9:1, or at least about 10:1.

[0029] It is noted that while high expansion ratios can be achieved using commercially available heat shrink methods, the heat shrink tubing of the present disclosure can surprisingly exhibit higher recovery ratios compared to conventional heat shrink tubing known in the art (e.g., conventional heat shrink tubing known in the art typically has a recovery ratio of 4:1 or less). As noted above, for example, the ratio between the expanded ID and the recovered ID is referred to as the recovery ratio. The recovery ratio is the expanded ID divided by the recovered ID. Without intending to be bound by theory, it has been found that rapid cooling of the expanded tubing is effective to lock the tubing into an entropically unfavorable expanded state before it begins to appreciably recover, thereby producing a final product with a recovery ratio that exceeds the commercially available maximum of 4:1 recovery ratio. In some embodiments, this rapid cooling can be achieved by a water-cooled annular fixture attached to the end of the heated die. For example, in some embodiments, the PTFE heat shrink tubing of the present disclosure may exhibit a recovery ratio of at least about 4:1, at least about 5:1, at least about 6:1, at least about 7:1, at least about 8:1, at least about 9:1, or at least about 10:1.

[0030] The recovery rates of the heat shrink tubings of the present disclosure can also be characterized in terms of their inner diameter (ID) shrinkability (e.g., their overall percent diameter change (ΔD) calculated using the equation above). For example, a recovery rate of 4.55:1 equates to an ID that is shrinkable by about 78%, and a recovery rate of 5:1 equates to an ID that is shrinkable by about 80%. As shown in FIG. 3, both Example 1 and Example 2, made according to the method of the present disclosure, exhibited a percent diameter change of about 80% or more after recovery, while each of the comparative examples exhibited a significantly lower percent diameter change after recovery.

[0031] In some embodiments, when the percent recovery is within the ranges described herein above, the heat shrink tubing exhibits a small change in the longitudinal direction when shrunk, such as, for example, less than about 20%. In certain embodiments, such heat shrink tubing may exhibit even smaller changes in the longitudinal direction, such as, for example, less than about 20%, less than about 15%, less than about 10%, less than about 9%, less than about 8%, less than about 7%, less than about 6%, less than about 5%, less than about 4%, less than about 3%, less than about 2%, less than about 1%, less than about 0.5%, or less than about 0.1%.

[0032] It should be noted that the higher recovery rate of the heat shrink tubing described herein provides certain distinct advantages over commercially available heat shrink tubing. In particular, such higher recovery rate may enable encapsulation of complex mandrel shapes (e.g., including, but not limited to, tapered mandrels or mandrels with abrupt transitions). Furthermore, providing such high recovery rate at low temperatures as described herein advantageously increases the variety of polymeric materials that can be encapsulated without decomposition. For example, in some embodiments, a dual heat shrink structure with an outer layer (e.g., a PTFE heat shrink outer layer) having a higher recovery rate may enable complete encapsulation of the melting inner layer around complex parts and shapes. Examples of dual heat shrink structures and applications are shown, for example, in the disclosure of Hunter et al., U.S. Patent Application Publication No. 2021 / 0370581, which is incorporated herein by reference in its entirety. Furthermore, as described herein, such high recovery rates can result in heat shrink tubing with the ability to recover over complex mandrel contours, such as those with variations in diameter or taper angle and taper length, resulting in thin-walled catheter liners not currently available on the market.

[0033] In certain embodiments, the heat shrink tubing described herein can be described as "peelable" and can be easily peeled or torn longitudinally (e.g., to remove the heat shrink tubing from the underlying material). This peelability can advantageously allow the tubing to be provided, used, and in some embodiments, removed without any cuts, break lines, indentations, or perforations along the length of the tubing. It is noted that PTFE is inherently peelable in the flow direction (e.g., longitudinally), which can result in easy removal of the heat shrink tubing after reflowing the inner polymeric material (e.g., catheter jacket, medical device, or dual heat shrink structure). Examples of peelable heat shrink tubing are shown, for example, in U.S. Patent No. 5,399,323 to Roof et al., which is incorporated herein by reference in its entirety.

[0034] Certain properties of the tubing disclosed herein can be evaluated by differential scanning calorimetry (DSC). DSC is an analytical technique that provides information about the thermal properties of a material and is well known to those skilled in the art. A typical DSC experiment (commonly referred to as a single heat temperature ramp) can be performed to determine the peak temperature of the endothermic melting transition for a semi-crystalline polymeric material (e.g., PTFE). The peak temperature of the melting endotherm can vary depending on the specific configuration of the tubing (i.e., type of fluoropolymer resin) and the previous thermal history of the tubing (i.e., the thermo-mechanical history imparted to the material during processing). The peak temperature of the melting endotherm observed in the DSC thermogram is generally referred to as T m The thermo-mechanical history imparted to the heat shrink tubing of the present disclosure using the methods described herein results in a T m changes.

[0035] PTFE is known to have a high melting temperature and melt viscosity, with virgin PTFE resin having a melting temperature of approximately 342°C to 345°C and a melt viscosity in the range of about 1 GPa·s to 10 GPa·s. This high melt viscosity reduces flow, thereby allowing other thermoplastics to be processed by conventional melt extrusion techniques (e.g., using a screw extruder). Due to the high melt viscosity of PTFE, it is typically extruded as a paste through a ram extruder and sintered using equipment and procedures well known in the art. For example, PTFE tubes can be sintered at temperatures above the melting point of virgin PTFE resin (i.e., 342°C to 345°C), for example, at temperatures in the range of about 360°C to about 380°C. Typically, the PTFE tube is sintered for a period of time sufficient to proceed with fusion, coalescence, and void removal to maximize certain properties of the PTFE tube.

[0036] Certain properties of the tubing disclosed herein can be evaluated by dynamic mechanical analysis (DMA). DMA is an analytical technique used to study and characterize the viscoelastic behavior of polymers as a function of time, temperature, and frequency. The storage modulus (E') is a measure of the elastic behavior of a material (i.e., the ability of a material to store energy elastically). A typical DMA temperature ramp experiment involves increasing the temperature at a constant (i.e., linear) rate while simultaneously applying a sinusoidal deformation at a specified frequency and monitoring the material's response (i.e., stress).

[0037] As noted above in DMA, the storage modulus of a specimen obtained from heat shrink tubing in the circumferential direction undergoing a temperature ramp decreases with temperature until the expansion temperature is approached. At this point, a significant minimum is reached in the E'-T (storage modulus vs. temperature) curve, after which E' increases as the heat shrink tubing recovers in the direction of dynamic mechanical testing. The minimum in the E'-T curve is then referred to as E' min Let's call it E'. minThe presence of is believed to be independent of the crystallization process and is due to entropic elasticity as seen in the recovery of pre-stretched specimens, see e.g., L. Andena el al., Polym. Eng. Sci, 44, 2004, 1368-1378, which is incorporated herein by reference.

[0038] E' min It should be noted that T has been found to be an important parameter in describing the heat shrink tubing of the present invention. Typically, a combination of processing parameters and material properties determine the crystalline / amorphous morphology of the expanded heat shrink tubing that is locked in an entropically unfavorable state after the expansion process. This morphology determines not only the entropic resilience available for the tube to recover from its expanded shape, but also the extent to which the tube recovers when exposed to various recovery temperatures. Without intending to be bound by theory, it is believed that the T of the heat shrink tubing m At the lowest possible temperature relative to E' min It has been found that it is important to adjust the processing parameters to yield a heat shrinkable tubing that recovers to a greater extent at lower temperatures. For example, heat shrinkable tubing that recovers to a greater extent at lower temperatures will perform better in many applications. It is therefore desirable to produce PTFE heat shrinkable tubing that exhibits a large temperature difference between the melting endothermic peak obtained from the DSC temperature ramp and the minimum in the E'-T curve obtained from the DMA temperature ramp.

[0039] The heat shrink tubings provided herein can be used in a variety of applications. In certain applications, these heat shrink tubings can be applied to an underlying material (e.g., a device, device member, joint, fitting, wire, etc.) and heated to form a coating on the underlying material. Thus, the present disclosure encompasses materials or objects to which the tubings disclosed herein are applied. For example, in some embodiments, coated devices (e.g., medical devices) are provided that include the tubings disclosed herein. Exemplary coated devices include, but are not limited to, medical devices (e.g., catheters) to which any of the tubings disclosed herein are applied.

[0040] In various embodiments, the heat shrink tubing disclosed herein is made from one or more fluorinated polymer resins. As used herein, "resin" refers to a material consisting essentially of a given type of polymer (e.g., copolymer) or two or more polymers / copolymers. Resins are typically provided in solid form (e.g., as solid pellets), but are not limited thereto (having other forms including, but not limited to, powders, pastes, granules, dispersions, solutions, gels, etc.). In some embodiments, the heat shrink tubing disclosed herein may comprise, consist of, or consist essentially of one or more forms of fluorinated polymer resins described herein. In some cases, "resin" as used herein may include one or more additional components and / or one or more additives (such as, for example, lubricants, colorants, etc.) may be added thereto. In other embodiments, one or more additives (in granular, powder, or pellet form, or in gel or liquid form) may be included with and extruded together with the fluorinated polymer resin.

[0041] Any fluorinated polymer resin can be used according to the present disclosure. Of particular relevance to the present disclosure are fluoropolymer resins. Fluoropolymer resins are often used as heat shrink tubing for many applications that require lubricity, chemical inertness, or high temperature stability. FEP, PFA, and PTFE are among the more common fluoropolymer heat shrink tubings commercially available today, but the present disclosure is not limited thereto. Exemplary fluorinated polymer resins useful according to the present disclosure include, but are not limited to, resins where the polymer comprises, consists of, or consists essentially of fluorinated ethylene propylene (FEP), polyvinylidene fluoride (PVDF), perfluoroalkoxyalkanes (PFA), perfluoro(alkyl vinyl ethers) (PAVE) (e.g., perfluoro(methyl vinyl) ether, PMVE, or perfluoro(propyl vinyl) ether (PPVE)), terpolymers of tetrafluoroethylene, hexafluoropropylene, and vinylidene fluoride (THV), poly(ethylene-co-tetrafluoroethylene) (ETFE), ethylene chlorotrifluoroethylene (ECTFE), polychlorotrifluoroethylene (PCTFE), polytetrafluoroethylene (PTFE), copolymers of tetrafluoroethylene and perfluoromethyl vinyl ether (MFA), or copolymers, blends, or derivatives of any two or more thereof.

[0042] In certain embodiments, the heat shrink tubing of the present disclosure is made using PTFE resin, and therefore, in some embodiments, may consist of, consist essentially of, or include PTFE. Typically, PTFE resin can be provided in a variety of different forms, such as, for example, in the form of a solid, powder, granules, dispersion, solution, gel, and the like. In certain embodiments, the PTFE heat shrink tubing can be made using, among other things, PTFE powder. The type of PTFE powder incorporated in such embodiments can vary and can include not only conventional PTFE extrusion grade powder, but also PTFE granules, particles, and the like of various particle sizes. Extrusion grade PTFE resin is commercially available as POLYFLON™ PTFE F-205 from Daikin Industries, Ltd., and DYNEON™ PTFE TF 2053Z from 3M™. However, it should be understood that the heat shrink tubing provided herein is not limited to PTFE resin, and can be made using one or more fluorinated polymer resins described herein in addition to or instead of PTFE.

[0043] Generally, the methods of making such heat shrink tubing can vary. In general, the desired resin(s) (e.g., PTFE resin, etc.) are formed into a tubular form, for example, via extrusion, and then mechanically expanded. The means of carrying out these steps can vary as described herein.

[0044] For example, resins (such as PTFE resins) can be shaped into tubes by subjecting the resin to extrusion. Extrusion generally involves placing the desired resin(s) into an extruder (e.g., a ram extruder). In the extruder, the resin(s) is heated, compressed, and forced through an annular die set to produce a tube. Tubes of various diameters and lengths can be produced. The dimensions of the tube can be determined by the tooling size on the extrusion line, and other parameters of the extrusion process can also be adjusted and optimized to produce the desired tubing. In some embodiments, tubing with a relatively uniform wall thickness is provided. The tube forming tool is attached to the end of the extrusion cylinder and generally includes a rod, a mandrel, a master die, a tube die, and end cap heaters.

[0045] The size of the finished product required and the reduction ratio determine the appropriate tooling to be used. The reduction ratio controls the extrusion pressure, fibrillation, and mechanical properties of the PTFE resin or PTFE powder. The reduction ratio is an absolute number calculated from the ratio of the cross-sectional area of ​​the extrusion cylinder minus the cross-sectional area of ​​the mandrel rod to the cross-sectional area of ​​the extrusion die minus the cross-sectional area of ​​the mandrel tip.

[0046] During the extrusion process, as the resin particles enter the zone of the tube die, they are highly pressurized. Due to the reduced cross-sectional area in the flow direction, the particles deform and rub against each other under the application of high pressure. The PTFE starts to shear the secondary particles, and the crystallites begin to mechanically entangle, resulting in the interconnection of adjacent particles. As the particles flow towards the exit of the die, they accelerate and elongate, during which the mechanically entangled crystallites loosen and fibrils are generated. Typically, the more fibrils are generated, the more elastic the elongation properties the paste acquires, which induces higher extrusion pressures.

[0047] In some embodiments, upon exiting the extruder, the newly formed extruded tube can be transferred to an evaporation oven having a temperature in the range of about 232°C to about 260°C to remove any lubricants used during the preforming and extrusion processes. In certain embodiments, the extruded tube can then be sintered at a desired temperature for a period of time to obtain the desired final properties of the PTFE tube. In some embodiments, the extruded tube is sintered at a temperature above the melting point of virgin PTFE resin (i.e., 342°C to 345°C), for example, at a temperature in the range of about 360°C to about 380°C. Typically, the extruded tube is sintered for a period of time sufficient to proceed with fusion, coalescence, and void removal to maximize certain properties of the PTFE tube.

[0048] In certain embodiments, the extruded tube can be air-cooled following a sintering process to achieve a desired level of crystallinity in the final tubing. The level of crystallinity in the final tubing can vary as known in the art. For example, in some embodiments, the degree of crystallinity in the final PTFE tube can range from about 32% to about 48%.

[0049] The extruded tubular form is then typically radially expanded (e.g., by mechanical means) to obtain expanded tubing material, i.e., heat-shrunk tubing (i.e., tubing that decreases in diameter when heated). The expansion of the input tubing (i.e., the initial extruded tubular form) can be performed in-line with the extrusion or can be performed offline (i.e., independent of and / or subsequent to the extrusion process). All means of radially expanding the tubing are intended to be encompassed by the present invention. Generally, the tubing is radially expanded during the expansion process by pressurizing the inside of the tubing and applying stress to the tube walls. This pressurization can be achieved by any means capable of providing a pressure differential between the inside and outside of the tubing. Such a pressure differential can be created by applying a pressure above atmospheric pressure to the center of the tube, a pressure below atmospheric pressure to the outside of the tube, or a combination of the two. The stress induced in the tube walls causes the tube to radially expand, i.e., increase in diameter. The rate of expansion can be controlled so that the tube remains in the expanded state and does not recover until it is subjected to further thermal cycling. The extent to which the tube is expanded depends on the intended use of the tubing, in some embodiments, the tubing is expanded to an inner diameter of about 1.05 times its original (unexpanded) diameter to about 10 times its original (unexpanded) diameter.

[0050] In certain embodiments, the PTFE heat shrink tubing made according to the present disclosure can be radially expanded using, for example, the process described in U.S. Patent No. 6,399,323 to Henson, which is incorporated herein by reference in its entirety. For example, the U.S. Patent No. 6,399,323 patent describes a process for producing fluoropolymer heat shrink tubing using a first fluid inside the tube to expand the tube and a second fluid outside the tube to inhibit expansion in an expansion chamber. In other embodiments, the tubing can be expanded by, for example, adjusting the air flow rate outside the tube, the chamber temperature, the air pressure inside the tube, and the speed at which the tube passes through the expansion chamber. In certain embodiments, the heat shrink tubing of the present disclosure is expanded at high temperature through a die using any number of methods known in the art and subsequently cooled at the exit of the die. Cooling can be accomplished using a fluid such as water, oil, or air. Processing parameters that can be adjusted include die type, die diameter and length, die temperature, fluid pressure inside the tube, fluid pressure outside the tube, cooling method, coolant type and temperature, expansion rate, tube material, tube ID, tube OD, and tube wall thickness.

[0051] The heat shrink tubing provided herein can be used in a variety of applications. In certain applications, the heat shrink tubing provided herein can be applied to an underlying material (e.g., a device, device member, joint, fitting, wire, etc.) and heated / cured to form a coating on the underlying material. Thus, the present disclosure encompasses materials or objects to which the tubing disclosed herein is applied. For example, in some embodiments, a coated device (e.g., a medical device) is provided that includes the heat shrink tubing disclosed herein (e.g., in a cured form). Exemplary coated devices include, but are not limited to, medical devices (e.g., catheters) to which any of the tubing disclosed herein is applied.

[0052] Additionally, while this application focuses on tubing, it is noted that other products may be produced that exhibit the surprising and advantageous properties described herein. For example, a wide range of PTFE heat shrink products may be formed in accordance with the present disclosure and, in some embodiments, may exhibit the heat shrink capabilities, higher expansion / recovery, lower longitudinal shrinkage, lower temperature recovery, and / or thin wall construction disclosed herein.

[0053] experiment Aspects of the present invention will be more fully described by the following examples, which are provided to illustrate certain aspects of the invention and should not be construed as limiting the invention. Although the examples given relate specifically to PTFE heat shrink tubing, it will be understood that fluoropolymer heat shrink tubing in general will benefit from the invention.

[0054] Comparative Example 1 First, unexpanded control PTFE tube samples were made with a nominal recovery ratio of 1:1 according to the method set forth herein below. First, PTFE fine powder was mixed with 16%-25% aliphatic hydrocarbon lubricant, rolled for 10 minutes, and then aged for a period of 24 hours in a temperature controlled environment at 26°C. The lubricant was allowed to penetrate and coat the agglomerated PTFE particles for 24 hours. After aging, the PTFE powder / lubricant mixture was molded into a preform or billet by pressing in a preform press, where the PTFE powder / lubricant mixture was consolidated into a cylindrical preform or billet. The preform press has a rod in the center that allows the PTFE to flow around a mandrel to form a tube shape.

[0055] The cylindrical / tubular preform or billet was then loaded into the barrel or cylinder of a ram extruder with a rod that matched the inner diameter of the cylindrical preform. During the extrusion process, the PTFE preform is highly pressurized and extruded to form a pressurized PTFE tube. Upon exiting the extruder, the newly formed PTFE tube was transported to an evaporation oven having a temperature ranging from about 232°C to about 260°C. The evaporation oven is used to remove the lubricant used during the preforming and extrusion processes.

[0056] The PTFE tube was then sintered at a desired temperature for a period of time to obtain the final properties of the PTFE tube. The PTFE tube was sintered at a temperature above the melting point of virgin PTFE resin (342°C to 345°C), for example, in the range of 360°C to 380°C. The PTFE tube was sintered for a period of time to allow melting, coalescence, and void removal to proceed and maximize the properties of the PTFE tube. The PTFE tube was then air-cooled to achieve a specified crystallinity level in the final product. Typically, PTFE has a degree of crystallinity ranging from about 32% to about 48%. The final product (e.g., PTFE tube) of Comparative Example 1 was produced as described above to have an inner diameter of 0.359 inches and an average wall thickness of about 0.033 inches.

[0057] Comparative Example 2 A PTFE tube was made using the same method and conditions as set forth in Comparative Example 1. The resulting PTFE tube had an inside diameter of 0.487 inches and an average wall thickness of about 0.025 inches.

[0058] After preparation, the PTFE tube was expanded by pressurizing it with air as it entered a heated die to increase the inside diameter to the required expansion ratio. The expanded PTFE tube was subsequently cooled and fixed at the expanded diameter such that the RR value was approximately 2 when the tube was reheated to 350° C. The inside diameter and average wall thickness of the expanded PTFE tube were measured and are summarized in Table 1.

[0059] Comparative Example 3 A PTFE tube was prepared using the same method and conditions as set forth in Comparative Example 1. The resulting PTFE tube had an inside diameter of 0.159 inches and an average wall thickness of about 0.015 inches.

[0060] After preparation, the PTFE tube was expanded by pressurizing it with air as it entered a heated die to increase the inside diameter to the required expansion ratio. The expanded PTFE tube was subsequently cooled and fixed at the expanded diameter such that the RR value was approximately 4 when the tube was reheated to 350° C. The inside diameter and average wall thickness of the expanded PTFE tube were measured and are summarized in Table 1.

[0061] Comparative Example 4 PTFE tubes were fabricated using the same method and conditions as shown in Comparative Example 1. The inside diameter and average wall thickness of the PTFE tubes were measured and are summarized in Table 1.

[0062] The PTFE tube was then expanded by heating it and inflating it with compressed air as it entered the die. The die had an opening along its ID that allowed compressed air to circulate between the OD of the PTFE tube and the ID of the die to maintain the desired expanded diameter. The thus expanded PTFE tube was subsequently cooled as it exited the die and fixed at the expanded diameter such that the RR value was approximately 4 when the tube was reheated to 350°C. The inside diameter and average wall thickness of the expanded PTFE tube were measured and are summarized in Table 1.

[0063] Comparative Example 5 Commercially available PTFE heat shrink tubing was purchased from the market. The inner diameter and average wall thickness of the PTFE tube were measured and are summarized in Table 1. After preparation, the PTFE tube was then heated in an oven to 350°C for 10 minutes. The RR was calculated to be approximately 4.

[0064] Example 1 A PTFE tube was fabricated using the same method and conditions as set forth in Comparative Example 1. The resulting PTFE tube had an inside diameter of 0.042 inches and an average wall thickness of about 0.013 inches.

[0065] After preparation, the PTFE tube was then expanded using the process of Comparative Example 4. However, in this example, the processing parameters of expansion air pressure, expansion air temperature, die air pressure, die air temperature, die air flow rate, tube throughput, cooling air temperature, and flow rate were all adjusted to obtain a PTFE heat shrink tube according to the present disclosure. In particular, the PTFE tube was expanded using an expansion temperature of 443°C, an internal air pressure of 40 psi, and a die air flow rate of 2 cubic feet per minute (cfm). The inside diameter and average wall thickness of the expanded PTFE tube were measured. These are summarized in Table 1.

[0066] Example 2 A PTFE tube was fabricated using the same method and conditions as set forth in Comparative Example 1. The resulting PTFE tube had an inside diameter of 0.042 inches and an average wall thickness of about 0.013 inches.

[0067] The PTFE tube was then expanded using the process of Comparative Example 4. However, in this example, the processing parameters of expansion air pressure, expansion air temperature, die air pressure, die air temperature, die air flow rate, tube throughput, cooling air temperature, and cooling air flow rate were all adjusted to obtain a PTFE heat shrink tube according to the present disclosure. In particular, the PTFE tube was expanded using an expansion temperature of 443°C, an internal air pressure of 45 psi, and a die air flow rate of 2 cubic feet per minute (cfm). The inside diameter and average wall thickness of the expanded PTFE tube were measured. These are summarized in Table 1.

[0068] Cumulative results Table 1 below shows the nominal tube dimensions of the final PTFE tubes made in Comparative Examples 1-5 and Examples 1-2. Dimensions measured include inside diameter after expansion, average wall thickness after expansion, and nominal recovery rate. Both inside diameter and wall thickness were measured in inches. As shown in Table 1 below, the PTFE tubes made according to Examples 1 and 2 showed significantly smaller inside diameters compared to most of the Comparative Examples, significantly smaller wall thicknesses compared to Comparative Examples 1 and 2, and the highest recovery rates.

[0069] [Table 1]

[0070] Table 2 below summarizes the DMA and DSC temperature ramp data for the final PTFE tubes made in Comparative Examples 1-5 and Examples 1-2. The DMA and DSC data for an exemplary embodiment of the invention is shown in FIG. 2. Specific parameters recorded in Table 2 include the temperature at which the minimum storage modulus occurs (E' min ), the melting endothermic peak temperature (T m ), and the difference between the temperature at which the minimum storage modulus occurs and the peak temperature of the melting endotherm (ΔT(T m -E' min DSC thermograms were obtained by cutting approximately 10 mg specimens from the PTFE tubes, crimping them in non-hermetically sealed aluminum pans, and heating them in a TA Instruments DSC2500 (New Castle, Del.) from ambient temperature to 400 °C at a heating rate of 10 °C / min using a single temperature ramp to obtain the T mwas determined. To obtain the DMA temperature ramp data, specimens were prepared by cutting 5 mm lengths from shrink tubing and slicing the annulus longitudinally to obtain circumferentially oriented rectangular specimens. Temperature scans of E' were collected on a TA Instruments Q800 DMA (New Castle, Del.) in tensile mode at a heating rate of 3°C per minute and a deformation amplitude of 15 μm at 1 Hz from ambient temperature to approximately 340°C. It is noted that, as shown in FIG. 1, some of the collected temperature scans were automatically stopped by the instrument before reaching the final temperature of 340°C. Without intending to be bound by theory, this is because some specimens recovered to some degree before 340°C and the tensile grips made physical contact, forcing the instrument to terminate the experiment.

[0071] [Table 2]

[0072] Figure 1 shows the separation in temperature of the E' minima for Comparative Example 1-Comparative Example 5 and Examples 1-2. As shown in Figure 1, the control sample (Comparative Example 1) does not exhibit a clearly defined relative minimum in the E'-T curve as exhibited by Comparative Example 2-Comparative Example 5 and Examples 1-2. This allows for a clear separation of the E' minima as defined and disclosed herein. min It is demonstrated that the entropic elasticity of the PTFE heat shrink tubing is driven by the entropically unfavorable state fixed within the PTFE heat shrink tubing during expansion and is directly influenced by the amount of entropic elasticity available when recovery is initiated by heating the PTFE heat shrink tubing.

[0073] 2 shows the separation in temperature of the E' minimum and the peak of the melting endotherm for Example 1, which is representative of an exemplary embodiment of the present disclosure. As shown in FIG. 2, the heat shrink tubing of Example 1 shows a large temperature difference between the melting endotherm peak observed in the DSC thermogram and the minimum in the E'-T curve obtained during the DMA temperature ramp.

[0074] Table 3 below summarizes the percent recovery (RR) and length change (ΔL) for PTFE heat shrink tubing samples of Comparative Examples 2-5 and Examples 1-2 when recovered for 10 minutes at various temperatures as described above herein. As shown in Table 3, Examples 1 and 2 exhibited significantly higher percent recovery compared to the Comparative Examples, without any significant adverse effect on the length change of the final product upon recovery.

[0075] [Table 3]

[0076] Table 4 below summarizes the diameter change for PTFE heat shrink tubing samples of Comparative Examples 2-5 and Examples 1-2 upon recovery for 10 minutes at various temperatures. As shown in Table 4, Examples 1 and 2 exhibited a significantly higher percentage in diameter change compared to the Comparative Examples across the entire temperature range.

[0077] [Table 4]

[0078] Table 5 below shows the linear regression data obtained from a linear regression of the diameter change for each example in the range of 310°C to 330°C. The diameter change was calculated at various recovery temperatures to which the PTFE tubing was exposed for 10 minutes. This data was imported into OriginLab's OriginPro 2019 v.9.6 data analysis and graphing software, and the diameter change was plotted against the recovery temperature. A linear regression was performed on the plot of diameter change versus recovery temperature for each example in the range of 310°C to 330°C (well below 350°C, where the maximum achievable RR for PTFE heat shrink occurs) to evaluate the tendency of the example heat shrink tubing to recover more at lower temperatures. The plot of diameter change versus recovery temperature for each example, including the respective regression lines, is shown in Figure 3.

[0079] [Table 5]

[0080] Table 6 below summarizes the average diameter change for each example over the range of 310°C to 330°C. The average diameter change values ​​correspond to the slope values ​​obtained from the linear regression data in Table 5. From this analysis, it can be concluded that a larger slope value / diameter change explains a greater degree of recovery of the heat shrink tubing at lower temperatures, whereas a smaller slope value / diameter change explains a lesser degree of recovery of the heat shrink tubing at lower temperatures. As shown in Table 6, Examples 1 and 2 exhibited significantly greater diameter change over the measured temperature range compared to the Comparative Example, demonstrating a greater degree of recovery of the heat shrink tubing at lower temperatures.

[0081] [Table 6]

[0082] Many variations and other embodiments of the present disclosure will come to mind to one skilled in the art to which this disclosure pertains having the benefit of the teachings presented in the foregoing description. It is to be understood, therefore, that the present disclosure is not limited to the specific embodiments disclosed, but that variations and other embodiments are intended to be included within the scope of the appended claims. Although specific terms have been employed herein, they are used in a generic and descriptive sense only and not for purposes of limitation.

Claims

1. PTFE heat shrink tubing having a recovery ratio (RR) of greater than about 5:

1.

2. 2. The PTFE heat shrink tubing of claim 1, wherein the RR is greater than about 5.5:

1.

3. 2. The PTFE heat shrink tubing of claim 1, wherein the RR is greater than about 6:

1.

4. 10. The PTFE heat shrink tubing of claim 1, wherein the PTFE heat shrink tubing has an average wall thickness of 0.003 inches or less after expansion.

5. PTFE heat shrink tubing, where a linear regression performed on a plot of diameter change versus recovery temperature between 310°C and 330°C produces a slope value of greater than about 1.3% / °C.

6. 6. The PTFE heat shrink tubing of claim 5, wherein the PTFE heat shrink tubing has a RR of greater than about 5:

1.

7. 6. The PTFE heat shrink tubing of claim 5, wherein the PTFE heat shrink tubing has a RR of greater than about 5.5:

1.

8. 6. The PTFE heat shrink tubing of claim 5, wherein the PTFE heat shrink tubing has a RR of greater than about 6:

1.

9. 6. The PTFE heat shrink tubing of claim 5, wherein the PTFE heat shrink tubing has an average wall thickness of 0.003 inches or less after expansion.

10. PTFE heat shrink tubing, wherein the difference between the temperature corresponding to the peak temperature of the melting endotherm obtained from a DSC temperature ramp using a heating rate of 10°C per minute and the temperature corresponding to the relative minimum in the E'-T curve obtained in a DMA temperature ramp of a circumferentially oriented heat shrink tubing specimen in tensile grips is greater than about 7.5°C.

11. 11. The PTFE heat shrink tubing of claim 10, wherein the PTFE heat shrink tubing has a RR of greater than about 5:

1.

12. 11. The PTFE heat shrink tubing of claim 10, wherein the PTFE heat shrink tubing has a RR of greater than about 5.5:

1.

13. 11. The PTFE heat shrink tubing of claim 10, wherein the PTFE heat shrink tubing has a RR of greater than about 6:

1.

14. 11. The PTFE heat shrink tubing of claim 10, wherein the PTFE heat shrink tubing has an average wall thickness of 0.003 inches or less after expansion.

15. 11. The PTFE heat shrink tubing of claim 10, wherein a linear regression performed on a plot of diameter change versus recovery temperature between 310°C and 330°C produces a slope value of greater than about 1.3% / °C.

16. 1. A heat shrink tubing comprising: tubing with a wall comprising PTFE having an inner diameter (ID), said ID being about 0.3 inches or less after expansion, and said ID being shrinkable by at least about 78% when heated at 350° C. for 10 minutes.

17. 17. The heat shrink tubing of claim 16, wherein the ID is shrinkable by at least about 80% when heated at 350°C for 10 minutes.

18. 17. The heat shrink tubing of claim 16, wherein the walls of the heat shrink tubing have an average wall thickness of about 0.003 inches or less after expansion.

19. 17. The heat shrink tubing of claim 16, wherein the difference between the temperature corresponding to the peak temperature of the melting endotherm obtained from a DSC temperature ramp using a heating rate of 10° C. per minute and the temperature corresponding to the relative minimum in the E′-T curve obtained in a DMA temperature ramp of a circumferentially oriented heat shrink tubing specimen in tensile grips is greater than about 7.5° C.

20. 17. The heat shrink tubing of claim 16, wherein a linear regression performed on a plot of diameter change versus recovery temperature between 310°C and 330°C produces a slope value of greater than about 1.3% / °C.

Citation Information

Patent Citations

  • Moldable polytetrafluoroethylene resin, application product, and process for producing same

    CN102227453A

  • Quickly recovering polytetrafluoroethylene and preparation thereof

    JP1990000645A

  • Multiple wall dimensionally recoverable tubing for forming reinforced medical devices

    JP2015134174A

  • Method for producing fluororesin coating body

    JP2017205961A

  • Collection Devices and Related Methods of Use

    JP2018501033A