ISOCYANATE COMPOSITION AND METHOD FOR PRODUCING SAME
The isocyanate composition with controlled oligomer content and Hazen color number addresses discoloration issues, enhancing transparency in optical products by adhering to the formula 0<A/50+B/3<1, specifically benefiting optical lenses.
Patent Information
- Application Number
- JP2024532301
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2021-11-30
- Filing Date
- 2022-11-30
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2042-11-30
AI Technical Summary
Isocyanate compounds are prone to oxidation and self-polymerization, leading to discoloration and reduced transparency in optical products, and existing methods to suppress discoloration are insufficient.
The composition effectively suppresses discoloration and clouding, ensuring excellent transparency in optical articles, particularly optical lenses, by maintaining controlled oligomer content and Hazen color number.
Smart Images

Figure 2024542656000001 
Figure 2024542656000002 
Figure 2024542656000003
Abstract
Description
[Technical field]
[0001] CROSS-REFERENCE TO RELATED APPLICATIONS This application claims the benefit of priority based on Korean Patent Application No. 10-2021-0169322 dated November 30, 2021, and all contents disclosed in the documents of that Korean patent application are incorporated herein by reference. The present invention relates to an isocyanate composition which is suppressed from discoloring and becoming cloudy, and which can improve transparency when applied to a product, and a method for producing the same. [Background technology]
[0002] Isocyanate is a raw material for polyurethane and is used in a variety of applications such as coatings, adhesives, paints, foams, and optical materials, and is required to have minimal discoloration for polyurethanes used in fields that require excellent appearance, especially in the optical field where transparency is required. For this reason, it is important that not only does the polyurethane reaction not cause discoloration, but also that the raw material isocyanate, especially polyfunctional isocyanates with two or more functionalities, do not discolor.
[0003] However, since isocyanates are highly reactive, they are prone to oxidation due to oxygen in the air during storage, or to self-polymerization, causing deterioration or discoloration, and optical products using them, such as urethane lenses, also suffer from discoloration or cloudiness.In addition, when polyisocyanates are produced by polymerization of diisocyanates, specifically polyurethanes produced by the urethane reaction of diisocyanates with polyhydric alcohols, the polymers are prone to discoloration due to the catalysts or solvents used in the polymerization reaction.
[0004] In response to this, various methods have been researched and proposed as methods for preventing discoloration in isocyanates, polyisocyanates, and products manufactured using them, such as a method of manufacturing and storing the products by sealing them with nitrogen gas to isolate them from air, or a method of storing the products by adding additives such as ultraviolet absorbers.
[0005] Japanese Patent Application Laid-Open No. 2-228317 discloses a method of treating isocyanate with a peroxide after modifying the isocyanate during the production of a polyisocyanate for a light-colored polyurethane lacquer. Japanese Patent Application Laid-Open No. 8-291129 discloses a method of producing an isocyanate with reduced discoloration by contacting a discolored isocyanate with an ozone-containing gas. Further, Japanese Patent Application Publication No. 2012-506465 discloses a method of producing an isocyanate with reduced discoloration by irradiating a discolored isocyanate with light having a wavelength of 200 to 600 nm.
[0006] However, the above methods could not achieve a sufficiently reduced discoloration effect. As another method, a method of storing a compound that does not participate in the polymerization reaction by mixing it with isocyanate has been proposed, but there is a problem that the added compound causes discoloration during subsequent product production.
[0007] Therefore, research on polyisocyanate compositions that are not prone to discoloration or denaturation during the synthesis process, storage process, and further product processing process of isocyanate is necessary.
Summary of the Invention
Problems to be Solved by the Invention
[0008] The present invention provides an isocyanate composition and a method for producing the same, which suppress the occurrence of discoloration and cloudiness and can improve transparency when applied to a product.
Means for Solving the Problems
[0009] According to one embodiment of the present invention, an isocyanate-based mixture containing one or more compounds selected from the group consisting of monomers, dimers, trimers, and oligomers having a repeating unit of 4 to 200 of an isocyanate compound; phenol; and p-toluenesulfonyl isocyanate; is provided, and an isocyanate composition that satisfies the following formula 1 is provided: 0 < A / 50 + B / 3 < 1 ··· Formula 1
[0010] A is the Hazen color number (APHA) measured by ASTM D1003; B is the oligomer content relative to the total weight of the isocyanate mixture. According to another embodiment of the present invention, the method comprises the steps of reacting an amine compound with phosgene in a solvent to obtain an isocyanate-based mixture; and adding phenol and paratoluenesulfonyl isocyanate to the mixture; the mixture contains one or more compounds selected from the group consisting of monomers, dimers, trimers, and oligomers having 4 to 200 repeating units of an isocyanate compound; The present invention provides a method for producing an isocyanate composition that satisfies the following formula 1:
[0011] 0 A is the Hazen color number (APHA) measured by ASTM D1003; B is the oligomer content relative to the total weight of the isocyanate mixture. According to one embodiment of the present invention, there is provided a polyisocyanate composition comprising a polyisocyanate formed by a polymerization reaction between the above-described isocyanate composition and a polyhydric alcohol.
[0012] Further, according to one embodiment of the present invention, there is provided an optical article comprising the polyisocyanate composition described above. Effect of the Invention
[0013] The isocyanate composition according to the present invention can improve the transparency of a product by suppressing discoloration and cloudiness during the synthesis process, storage process, and further product processing process of the isocyanate composition, by controlling new parameters taking into account the content of oligomer in the composition and the Hazen color number of the composition.
[0014] As a result, the polyisocyanate composition obtained by polymerizing the isocyanate composition of the present invention exhibits excellent transparency when applied to optical articles, and in particular, exhibits excellent quality when applied to optical lenses. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0015] The terms used in this specification are merely used to describe exemplary embodiments and are not intended to limit the present invention. A singular expression includes a plural expression unless the context clearly indicates otherwise. In this specification, the terms "include", "comprise", "have" or "have" are intended to specify the presence of an embodied feature, number, step, component, or combination thereof, and should be understood not to preclude the possibility of the presence or addition of one or more other features, numbers, steps, components, or combinations thereof.
[0016] Although the present invention can be modified in various ways and has various forms, specific embodiments are exemplified and described in detail below. However, it is not intended to limit the present invention to the specific disclosed embodiments, and it should be understood that the present invention includes all modifications, equivalents, and alternatives falling within the spirit and technical scope of the present invention.
[0017] Due to their high reactivity, isocyanate compounds are prone to oxidation due to oxygen in the air during storage, or to self-polymerization, resulting in deterioration or discoloration, which has led to a problem of reduced transparency in optical articles to which they are applied.
[0018] In order to solve these problems, the present inventors have been conducting research into the composition of isocyanate compositions, and have confirmed that even when lenses are manufactured using isocyanate compositions that have yellowing, some products do not suffer from defects. The inventors have discovered that the transparency of a product is affected not only by the yellowing phenomenon of the composition but also by the clouding phenomenon, and that when the content of the oligomer of the isocyanate compound contained in the composition and the Hazen color number of the composition are controlled within a specific range, the yellowing and clouding can be controlled within an appropriate range, thereby improving the transparency of the final product, thereby completing the present invention.
[0019] Specifically, it has been confirmed that the isocyanate composition can be applied to optical articles, particularly optical lenses, to achieve excellent quality by controlling new parameters, which are variables of the content of the oligomer of the isocyanate compound contained in the composition and the Hazen color number of the composition. In particular, the new parameters can be realized by appropriately adding phenol and paratoluenesulfonyl isocyanate to the isocyanate-based mixture.
[0020] <Isocyanate composition> According to one embodiment of the invention, the isocyanate composition comprises: an isocyanate-based mixture containing one or more compounds selected from the group consisting of monomers, dimers, trimers, and oligomers having 4 to 200 repeating units of an isocyanate compound; phenol; and paratoluenesulfonyl isocyanate.
[0021] Here, the isocyanate-based mixture may contain, in addition to a monomer of the isocyanate compound itself, a dimer in which two isocyanate compounds are bonded, a trimer in which three isocyanate compounds are bonded, and an oligomer having a repeating unit of 4 to 200. The oligomer means a compound in which 4 to 200 isocyanate compounds are bonded.
[0022] The dimer, trimer and oligomer of the isocyanate compound may be a by-product generated by a side reaction during the synthesis of the isocyanate compound from the amine compound, or may be a by-product formed by the self-polymerization of the isocyanate compound due to high reactivity after synthesis. The by-product may cause not only the transparency and color of the isocyanate composition itself but also discoloration and cloudiness of the polyisocyanate composition in which the isocyanate composition is used, so that the content of such by-products must be reduced in the case of an isocyanate composition used in the optical field. However, in a commercial process, it is difficult to control the content of the by-products excessively in terms of process efficiency and cost. Therefore, in the present invention, the content of the oligomer in the isocyanate composition is controlled at an appropriate level, thereby improving the transparency and color properties of the product while maintaining the efficiency of the process.
[0023] In particular, the isocyanate composition contains phenol and paratoluenesulfonyl isocyanate, so that the content of oligomers in the isocyanate mixture and the Hazen color number of the composition can be controlled within appropriate ranges, and thus the parameter represented by the new mathematical formula 1 can be adjusted to a desired range. Here, the paratoluenesulfonyl isocyanate is a component different from the isocyanate compound.
[0024] The phenol is contained in an amount of 50 to 1,500 ppm, preferably 100 to 1,000 ppm, based on the total weight of the isocyanate mixture. By containing the phenol in this range, the content of oligomer in the mixture and the Hazen color number of the composition can be controlled within an appropriate range, thereby improving the transparency and color properties of the product while maintaining the process efficiency.
[0025] The paratoluenesulfonyl isocyanate is contained in an amount of 10 to 3,000 ppm, preferably 50 to 2,000 ppm, based on the total weight of the isocyanate mixture. By containing the paratoluenesulfonyl isocyanate in the above range, the content of oligomer in the mixture and the Hazen color number of the composition can be controlled within an appropriate range, thereby improving the transparency and color properties of the product while maintaining the efficiency of the process.
[0026] Examples of the isocyanate compound include 1,4-tetramethylene diisocyanate, 1,5-pentamethylene diisocyanate, 1,6-hexamethylene diisocyanate, 1,3-cyclohexylene diisocyanate, 1,4-cyclohexylene diisocyanate, isophorone diisocyanate, norbornene diisocyanate, methylene diphenyl diisocyanate, methylene dicyclohexyl isocyanate, toluene diisocyanate, m-xylylene diisocyanate, p-xylylene diisocyanate, and o-xylylene diisocyanate.
[0027] In addition, the isocyanate composition according to one embodiment of the present invention satisfies the parameters of the following formula 1. Formula 1 is an index for controlling the yellowing and clouding of the composition, and by satisfying formula 1, discoloration and clouding can be suppressed during the synthesis process, storage process, and further, during the product processing process, thereby improving the transparency of the product. More specifically, formula 1 is as follows:
[0028] 0 A is the Hazen color number (APHA) measured by ASTM D1003; B is the oligomer content relative to the total weight of the isocyanate mixture. Specifically, the content of the oligomer is less than 1.6 wt % based on the total weight of the isocyanate mixture. By containing the oligomer at less than 1.6 wt %, the occurrence of yellowing of the composition can be reduced, and at the same time, by satisfying the above formula 1, the occurrence of yellowing and cloudiness during the manufacturing of the product can be effectively controlled.
[0029] On the other hand, if the composition does not satisfy the range of the mathematical formula 1 and shows a value of 1 or more, when applied to an optical lens, the transparency is significantly decreased, green light is exhibited, and the quality of the product is significantly decreased. Preferably, within the range satisfying Formula 1, the Hazen color number (APHA) of variable A of Formula 1 is more than 0 and less than 50, and the value of the oligomer content of variable B of Formula 1 is more than 0 and less than 1.6. By satisfying the above ranges, the transparency and other physical properties can be significantly improved when applied to optical lenses.
[0030] The Hazen color number (APHA) of the variable A in the above Equation 1 is measured at room temperature of 25±1° C. according to ASTM D1003, and a specific measurement method will be described in more detail in the contents of the Experimental Examples. The value of the oligomer content of the variable B in the above Equation 1 means only the value excluding the unit in weight % of the oligomer. The oligomer content is measured by gel permeation chromatography (GPC) analysis, and the specific measurement method will be described in more detail in the experimental examples.
[0031] <Method for producing isocyanate composition> A method for producing an isocyanate composition according to an embodiment of the present invention includes the steps of reacting an amine compound with phosgene in a solvent to obtain an isocyanate-based mixture; and adding phenol and paratoluenesulfonyl isocyanate to the mixture, thereby satisfying the following mathematical formula 1:
[0032] 0 A is the Hazen color number (APHA) measured by ASTM D1003; B is the oligomer content relative to the total weight of the isocyanate mixture.
[0033] In particular, by further adding phenol and paratoluenesulfonyl isocyanate to the reaction mixture during the preparation of the isocyanate composition, the content of oligomers in the mixture and the Hazen color number of the composition can be controlled within an appropriate range, and thus the parameter represented by the new formula 1 can be adjusted to a desired range. The contents described above regarding Equation 1 are all equally applicable.
[0034] Hereinafter, the method for producing the isocyanate composition will be described step by step. First, the method includes a step of reacting an amine compound with phosgene in a solvent to obtain a reaction mixture containing an isocyanate compound.
[0035] Examples of the solvent used in the phosgenation reaction include aromatic hydrocarbon solvents such as benzene, toluene, xylene, and ethylbenzene; chlorinated aromatic hydrocarbon solvents such as monochlorobenzene, 1,2-dichlorobenzene, and 1,4-dichlorobenzene; and chlorinated hydrocarbon solvents such as dichloromethane, chloroform, and carbon tetrachloride. Two or more of these solvents may be mixed together.
[0036] The amine compound used in the phosgenation reaction may be, for example, an amine compound obtained by hydrogenating a nitro compound or a chloride thereof. Specifically, the amine compound may be one or more selected from the group consisting of 1,4-tetramethylenediamine, 1,5-pentamethylenediamine, 1,6-hexamethylenediamine, 1,3-cyclohexylenediamine, 1,4-cyclohexylenediamine, isophoronediamine, diamine, methylenediphenyldiamine, methylenedicyclohexyldiamine, toluenediamine, m-xylylenediamine, p-xylylenediamine, and o-xylylenediamine, and salts thereof, and preferably m-xylylenediamine, p-xylylenediamine, o-xylylenediamine, or salts thereof.
[0037] The amine compound is contained in an amount of 1 to 20 parts by weight based on 100 parts by weight of the solvent. If the content of the amine compound exceeds 20 parts by weight, a large amount of the amine compound may precipitate. Preferably, the content is 1 to 15 parts by weight or 3 to 10 parts by weight.
[0038] Specifically, the phosgenation reaction is carried out by a direct phosgenation method (Method 1) in which an amine compound is directly reacted with phosgene; a method in which an amine compound is reacted with anhydrous hydrochloric acid to form an amine-hydrochloride compound, and then the formed salt is reacted with phosgene (Method 2); or a method in which an amine compound is reacted with carbonic acid to form an aliphatic amine-carbonate compound, and then the formed salt is reacted with phosgene (Method 3).
[0039] The direct phosgenation method of the above-mentioned method 1 is carried out by reacting an amine compound with phosgene in the above-mentioned organic solvent. At this time, phosgene may be added all at once at the beginning of the reaction, or a portion of the phosgene may be added at the beginning of the reaction and the remainder may be added in portions during the reaction.
[0040] Meanwhile, the method 1 includes a first step of dissolving a part of phosgene in the solvent and then adding the amine compound, and a second step of adding the remaining phosgene after the addition of the amine compound to react with the amine compound. The first step is preferably carried out at a temperature of -15°C to -10°C to prevent the outflow of highly toxic phosgene and to prevent rapid heat generation when the amine compound is added, and the phosgenation reaction in the second step is adjusted to 120°C to 140°C so that the reaction occurs at an appropriate reaction rate without the risk of decomposition of the amine compound.
[0041] In the case of the method 2, the amine compound is reacted with hydrochloric acid in an organic solvent to form an amine-hydrochloride compound, and then phosgene is added to carry out the reaction. The formation of the amine-hydrochloride compound is carried out at a temperature of 30° C. or less, preferably at a temperature of about 23±5° C., and the reaction after the addition of phosgene is controlled to 120° C. to 140° C. When carried out under such temperature conditions, the solubility of the amine-hydrochloride compound is increased and thermal decomposition of the isocyanate is prevented, thereby producing a high-purity isocyanate compound in a high yield.
[0042] In the case of the method 3, the amine compound is reacted with carbonic acid in a solvent to form an amine-carbonate compound, and then phosgene is added to react. At this time, the formation of the amine-carbonate compound is performed at a temperature of 30° C. or less, preferably about 23±5° C., and the reaction after the addition of phosgene is controlled to 80° C. to 180° C. The reaction temperature may be preferably in the range of 100° C. or more, or 120° C. or more, and 150° C. or less, or 140° C. or less. When the reaction is performed under such temperature conditions, the solubility of the amine-carbonate compound is increased and the thermal decomposition of the isocyanate is prevented, thereby producing a high-purity isocyanate compound in a high yield.
[0043] It is preferable to carry out the production reaction of an isocyanate compound by the method 2, since the formation of by-products such as dimers, trimers, and oligomers of the isocyanate compound produced by the phosgenation reaction can be controlled within an appropriate range, and the chromaticity of the composition can also be controlled within an appropriate range, thereby allowing the composition to satisfy the mathematical formula 1.
[0044] After the reaction with phosgene is completed by each of the methods, a step of removing unreacted phosgene and hydrogen chloride gas by nitrogen bubbling or the like and a step of removing the solvent by distillation or the like may be selectively further carried out, or these steps may be carried out by conventional methods.
[0045] Next, the method includes adding phenol and paratoluenesulfonyl isocyanate to the reaction mixture. When the additives are added, it is easy to control the content range of oligomers among the components contained in the phosgenation reaction mixture, and at the same time, it is possible to adjust the color of the composition. This makes it possible to prepare an isocyanate composition that satisfies the parameters of the above-mentioned Equation 1.
[0046] The phenol is added in an amount of 50 to 1,500 ppm, preferably 100 to 1,000 ppm, based on the total weight of the isocyanate mixture. By adding the phenol in this range, the content of oligomer in the mixture and the Hazen color number of the composition can be controlled within an appropriate range, thereby improving the transparency and color properties of the product while maintaining the process efficiency.
[0047] The paratoluenesulfonyl isocyanate is a compound different from the isocyanate compound synthesized in the step of obtaining the isocyanate-based mixture described above. Here, the paratoluenesulfonyl isocyanate is added in an amount of 10 to 3,000 ppm, preferably 50 to 2,000 ppm, based on the total weight of the isocyanate-based mixture. By adding the paratoluenesulfonyl isocyanate in the above range, the content of oligomers in the mixture and the Hazen color number of the composition can be controlled within an appropriate range, thereby improving the transparency and color properties of the product while maintaining the efficiency of the process.
[0048] The phenol and paratoluenesulfonyl isocyanate addition steps can proceed under a nitrogen pad.
[0049] <Polyisocyanate composition> According to another embodiment of the invention, there is provided a polyisocyanate composition comprising a polyisocyanate formed by the polymerization reaction of the isocyanate composition with a polyhydric thiol.
[0050] The polyvalent thiol is a compound containing two or more thiol groups (-SH) in one molecule, and specifically may be a compound having two or more, or three or more, and eight or fewer, or five or fewer thiol groups in one molecule.
[0051] Examples of the polyvalent thiol compound include 1,9-dimercapto-3,7-dithianonane, 1,13-dimercapto-3,7,11-trithiatridecane, glycol di(3-mercaptopropionate), and glycol di(3-mercaptopropionate). di(3-mercaptopropionate), 1,4-Dithiane-2,5-diyldimethanethiol, 4-mercaptomethyl-1,8-dimercapto-3,6-dithiaoctane, 2-mercaptomethyl-1,5-dimercapto-3-thiapentane, trimethylolpropane tri(3-mercaptopropionate) tri(3-mercaptopropionate), 4,8-di(mercaptomethyl)-1,11-dimercapto-3,6,9-trithiaundecane, 5,9-di(mercaptoethyl)-1,12-dimercapto-3,7,10-trithiadodecane, pentaerythritol tetra(3-mercaptopropionate), pentaerythritol tetra(mercaptoacetate) tetra(mercaptoacetate), 3,6,9,12-Tetrathiatetradecane-1,14-dithiol, 3,6,10,13-Tetrathiapentadecane-1,8,15-trithiol15-trithiol).
[0052] The polymerization reaction is carried out by a thiourethanization reaction between an isocyanate compound in the isocyanate composition and a thiol group in the polyvalent thiol.
[0053] Specifically, the polythiol is added in an amount such that the molar ratio of the thiol group in the polythiol to 1 mole of the isocyanate group of the isocyanate compound is 0.8 or more, or 0.9 or more, and 1.1 or less, or 1.0. If the molar ratio of the thiol group to the isocyanate group is less than 0.8 beyond the above molar ratio range, the viscosity of the polymer produced by the excess isocyanate group may decrease, which may decrease the processability. In addition, if the molar ratio of the thiol group to the isocyanate group exceeds 1.1, the excess thiol group may decrease the discoloration prevention effect.
[0054] The polymerization reaction is carried out under normal pressure conditions in an inert gas atmosphere such as nitrogen or argon. The polymerization reaction is preferably carried out at a temperature range of -15°C or higher, or 0°C or higher, and 20°C or lower, or 15°C or lower, since this makes it possible to easily control the reaction rate without the risk of discoloration and to increase the reaction efficiency.
[0055] The polymerization reaction may be carried out without a catalyst, or in the presence of a catalyst that generally promotes a urethane reaction, such as a tin or amine-based catalyst. When the polymerization reaction is carried out in the presence of a catalyst, the catalyst is added together with the polythiol in the step of adding the polythiol to the isocyanate-based mixture.
[0056] The polymerization reaction can be performed until the concentration of the isocyanate group in the polymerization reactant reaches the calculated value of the remaining isocyanate group after the reaction with the polythiol. The degree of progress of the polymerization reaction can be predicted by measuring the concentration of the isocyanate group in the polymerization reactant by the n-dibutylamine method using a potentiometric titration apparatus or by measuring the refractive index. In the present invention, the polymerization reaction can be performed until the concentration of the isocyanate group in the polymerization reactant reaches the calculated value of the remaining isocyanate group after the reaction with the polythiol.
[0057] As a result of such polymerization reactions, polyisocyanates, specifically polythiourethanes, are produced.
[0058] The polyisocyanate composition may further contain additives such as an internal mold releasing agent, an ultraviolet absorber, a polymerization initiator, a heat stabilizer, a color correcting agent, a chain extender, a crosslinking agent, a light stabilizer, a filler, and a photosensitizer, as necessary, and the content thereof may be appropriately determined within a range that does not inhibit the discoloration and discoloration inhibition properties of the composition.
[0059] The polyisocyanate composition can be used in a wide range of fields due to its excellent physical properties, and may be used as an optical material that requires excellent appearance properties, particularly transparency, such as eyeglass lenses, camera lenses, plastic lenses, and prisms.
[0060] According to yet another embodiment of the invention, there is provided an article comprising or made with the polymer composition.
[0061] In this case, the article may be an optical article such as a spectacle lens, a camera lens, a plastic lens, or a prism.
[0062] The functions and effects of the present invention will be described in more detail below through specific examples of the present invention, however, these examples are merely presented as examples of the present invention and do not define the scope of the invention.
[0063] [Examples and Comparative Examples] Example 1-1 In a flask, 471g of 1,2-dichlorobenzene, 32.5g of m-XDA with a purity of 99.4%, and 0.24g of 4-hydroxy TEMPO were added, and anhydrous hydrochloric acid was added at a rate of 20g / hr at room temperature (23±5°C) and stirred. The temperature rose to 50°C after the anhydrous hydrochloric acid was added. After 4 hours of injection, the salt formed was cooled to room temperature, and 43g of phosgene was added to the reactor, and the reactor was heated to a temperature of 130°C. From the time of adding phosgene to the time of the end of the reaction, a dry ice-acetone cooler was used to prevent phosgene from leaking out. After the temperature of the reactor reached 130°C, the temperature of the reactor was maintained at 125-135°C for 2 hours so that the reaction solution became transparent. After the solution became transparent, the inside of the reactor was cooled to 80°C and cooled by blowing in nitrogen. The reaction solution from which phosgene had been removed was subjected to vacuum distillation to remove the solvent, and the product was purified under reduced pressure at a high temperature of 160° C. to obtain an isocyanate-based mixture containing m-XDI. Under nitrogen-filled conditions, 100 ppm of phenol and 50 ppm of paratoluenesulfonyl isocyanate were added to the mixture to prepare an isocyanate composition. After preparation, the mixture was stored at 5°C for 180 days.
[0064] Example 1-2 An isocyanate composition was produced and stored in the same manner as in Example 1-1, except that the phenol content was changed to 500 ppm.
[0065] Examples 1-3 An isocyanate composition was produced and stored in the same manner as in Example 1-1, except that the phenol content was changed to 1,000 ppm.
[0066] Examples 1-4 An isocyanate composition was produced and stored in the same manner as in Example 1-1, except that the content of paratoluenesulfonyl isocyanate was changed to 1,000 ppm.
[0067] Examples 1-5 An isocyanate composition was produced and stored in the same manner as in Example 1-1, except that the content of paratoluenesulfonyl isocyanate was changed to 2,000 ppm.
[0068] Examples 1-6 An isocyanate composition was produced and stored in the same manner as in Example 1-2, except that the content of paratoluenesulfonyl isocyanate was changed to 1,000 ppm.
[0069] Examples 1-7 An isocyanate composition was produced and stored in the same manner as in Example 1-2, except that the content of paratoluenesulfonyl isocyanate was changed to 2,000 ppm.
[0070] Examples 1-8 An isocyanate composition was produced and stored in the same manner as in Example 1-3, except that the content of paratoluenesulfonyl isocyanate was changed to 1,000 ppm.
[0071] Examples 1-9 An isocyanate composition was produced and stored in the same manner as in Example 1-3, except that the content of paratoluenesulfonyl isocyanate was changed to 2,000 ppm.
[0072] Comparative Example 1-1 An isocyanate composition was produced and stored in the same manner as in Example 1-1, except that phenol and paratoluenesulfonyl isocyanate were not added.
[0073] Comparative Example 1-2 An isocyanate composition was produced and stored in the same manner as in Example 1-1, except that paratoluenesulfonyl isocyanate was not added.
[0074] [Experimental Example 1: Analysis of Isocyanate Composition] (1) Measurement of Hazen color number (APHA) For the isocyanate compositions produced in the above Examples and Comparative Examples, the Hazen color number (APHA) measured by ASTM D1003 was measured, and the results are shown in Table 1. Specifically, the Hazen color number was measured using the xenon lamp light source of Hunterlab's Ultrascane device by a method of color difference analysis of the composition under normal temperature conditions.
[0075] (2) Gel Permeation Chromatography (GPC) Analysis For the isocyanate compositions produced in the above Examples and Comparative Examples, gel permeation chromatography (GPC) analysis was performed, and the oligomer contents derived therefrom are shown in Table 1.
[0076] <GPC Analysis Conditions> Equipment Used: Waters2988 Column: Shodex KF-801, KF-802, KF-803 300mm Sample Concentration: Prepare by dissolving 0.1 mg of a 1 wt / vol% sample in 9.9 ml of tetrahydrofuran) Carrier: THF Detection Method: UV Flow Rate: 1.0 ml / min Column Temperature: 40 °C Polystyrene with a molecular weight of 1000 - 20,000 g / mol was used when preparing the calibration curve.
[0077] (3) Derivation of the Value of Formula 1 For the isocyanate compositions produced in the above Examples and Comparative Examples, the value of the following Formula 1 was calculated, and the results are shown in Table 1. 0 < A / 50 + B / 3 < 1 ··· Formula 1 A is the Hazen color number (APHA) measured by ASTM D1003, B is the numerical value of the oligomer content with respect to the total weight of the isocyanate-based mixture.
[0078]
Table 1
[0079] [Example 2 and Comparative Example 2] Example 2-1: Manufacturing of optical lenses 20.8g of the isocyanate composition prepared in Example 1-1, 0.04g of zelec UN (Stepan), and 0.04g of biosorb583 (Sakai Chemical Industry Co., Ltd.) were stirred in a flask at room temperature for about 20 minutes. Next, 0.002g of dibutyltin chloride was added and stirred for 10 minutes, and 19.2g of 2,3-bis(2-sulfanyl ethyl sulfanyl)propane-1-thiol was added to the mixture, which was degassed at 5mbar and stirred for 1 hour to prepare a mixed liquid.
[0080] The mixture was filtered through a 1 μm PTFE filter and then poured into a mold consisting of a glass mold and tape. The mold was placed in an oven, and the temperature was gradually increased from 10° C. to 120° C., and a polymerization reaction was carried out for 20 hours. After the polymerization was completed, the mold was removed from the oven and demolded to obtain a plastic lens. The obtained plastic lens was annealed at 120° C. for 6 hours to produce a final optical lens sample.
[0081] Examples 2-2 to 2-9 and Comparative Examples 2-1 to 2-2 Optical lenses were produced in the same manner as in Example 2-1, except that the isocyanate composition of Example 1-1 was replaced with the isocyanate composition of Examples 1-2 to 1-9 and Comparative Examples 1-1 and 1-2.
[0082] [Experimental Example 2: Optical lens evaluation] (1) Color evaluation The optical lenses manufactured in the above examples and comparative examples were evaluated for color by the naked eye, and the results are shown in Table 2.
[0083] (2) Transparency evaluation The optical lenses manufactured in the above examples and comparative examples were evaluated for the degree of clouding observed with the naked eye under various light source conditions according to the following evaluation criteria. The results are shown in Table 2.
[0084] <Evaluation criteria> C (Clear): All transparent under fluorescent and zirconium lamps SH (Slightly lamp Haze): Transparent under fluorescent lamps, but partially cloudy under zirconium lamps. LH (Lamp Haze): Transparent under fluorescent lamps, but appears cloudy under zirconium lamps. VH (Visual Haze): All are observed to be cloudy under fluorescent and zirconium lamps
[0085] [Table 2]
[0086] As can be seen from Table 2, the optical lens manufactured using the composition satisfying the parameters of Formula 1 defined by the present invention was found to have superior chromaticity and transparency compared to the comparative example.
Claims
1. An isocyanate-based mixture containing one or more compounds selected from the group consisting of monomers, dimers, trimers and oligomers having 4 to 200 repeating units of an isocyanate compound; phenol; and paratoluenesulfonyl isocyanate; An isocyanate composition that satisfies the following formula 1: 0<A / 50+B / 3<1 ... Formula 1 A is the Hazen color number (APHA) measured by ASTM D1003; B is the oligomer content relative to the total weight of the isocyanate mixture.
2. The A is 0 or more and less than 50, The B is greater than 0 and less than 1.6; The isocyanate composition of claim 1.
3. The paratoluenesulfonyl isocyanate is different from the isocyanate compound. The isocyanate composition of claim 1.
4. The phenol is contained in an amount of 50 to 1,500 ppm based on the total weight of the isocyanate-based mixture, The paratoluenesulfonyl isocyanate is contained in an amount of 10 to 3,000 ppm based on the total weight of the isocyanate mixture. The isocyanate composition of claim 1.
5. The oligomer is present in an amount of less than 1.6% by weight based on the total weight of the isocyanate-based mixture. The isocyanate composition of claim 1.
6. The isocyanate compound is at least one selected from the group consisting of 1,4-tetramethylene diisocyanate, 1,5-pentamethylene diisocyanate, 1,6-hexamethylene diisocyanate, 1,3-cyclohexylene diisocyanate, 1,4-cyclohexylene diisocyanate, isophorone diisocyanate, norbornene diisocyanate, methylene diphenyl diisocyanate, methylene dicyclohexyl isocyanate, toluene diisocyanate, m-xylylene diisocyanate, p-xylylene diisocyanate, and o-xylylene diisocyanate. The isocyanate composition of claim 1.
7. reacting an amine compound with phosgene in a solvent to obtain an isocyanate-based mixture; and adding phenol and paratoluenesulfonyl isocyanate to the mixture; The mixture contains one or more compounds selected from the group consisting of monomers, dimers, trimers, and oligomers having 4 to 200 repeating units of an isocyanate compound; A method for producing an isocyanate composition that satisfies the following mathematical formula 1: 0<A / 50+B / 3<1 ... Formula 1 A is the Hazen color number (APHA) measured by ASTM D1003; B is the oligomer content relative to the total weight of the isocyanate mixture.
8. The A is 0 or more and less than 50, The B is more than 0 and less than 1.6; A method for producing the isocyanate composition according to claim 7.
9. The paratoluenesulfonyl isocyanate is different from the isocyanate compound. A method for producing the isocyanate composition according to claim 7.
10. The phenol is contained in an amount of 50 to 1,500 ppm based on the total weight of the isocyanate-based mixture, The paratoluenesulfonyl isocyanate is contained in an amount of 10 to 3,000 ppm based on the total weight of the isocyanate mixture. A method for producing the isocyanate composition according to claim 7.
11. The oligomer is present in an amount of less than 1.6% by weight based on the total weight of the isocyanate-based mixture. A method for producing the isocyanate composition according to claim 7.
12. A polyisocyanate composition comprising a polyisocyanate formed by the polymerization reaction of the isocyanate composition of claim 1 with a polyhydric thiol.
13. 13. An optical article comprising the polyisocyanate composition of claim 12.
Citation Information
Patent Citations
Reactive polyurethane composition with low residual monomer content
JP2005505664A
Xylylene diisocyanate composition, polymerizable composition, resin, molded body, optical element, and lens
JP2023159107A
Xylylene diisocyanate composition, xylylene diisocyanate modification composition, two-component resin starting material, and resin