Polyolefin porous membrane, its manufacturing method, battery separator, and electrochemical device
The controlled wet stretching process for polyolefin porous membranes addresses the issue of anisotropy in conventional separators, resulting in a membrane with uniform fiber orientation and balanced mechanical properties for enhanced battery safety and stability.
Patent Information
- Application Number
- JP2023544439
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2022-10-28
- Filing Date
- 2023-04-25
- Publication Date
- 2024-11-19
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Conventional polyolefin porous separators for lithium-ion batteries lack uniformity in microstructure and mechanical properties in different directions, leading to potential anisotropy and reduced safety and stability during impact or stress.
A polyolefin porous membrane is produced through a controlled wet stretching process, ensuring uniform fiber orientation and balanced mechanical properties by maintaining a specific ratio of stretching strengths and elongations in both machine and transverse directions, with controlled temperature and stretching conditions.
The membrane achieves improved safety and stability in batteries by uniformly distributing mechanical stress, reducing the likelihood of cracks and short circuits, and enhancing impact resistance.
Smart Images

Figure 2024542897000001_ABST
Abstract
Description
[Technical field]
[0001] [CROSS REFERENCE TO RELATED APPLICATIONS] This disclosure claims priority to a PCT patent application bearing application number PCT / CN2022 / 128427 and entitled "Polyolefin porous membrane, its manufacturing method, battery separator, and electrochemical device," filed with the China Patent Office as the receiving office on October 28, 2022, the entire contents of which are incorporated herein by reference.
[0002] [Technical field] The present disclosure relates to the technical field of separators for electrochemical devices, and in particular to a polyolefin porous membrane, a manufacturing method thereof, a battery separator, and an electrochemical device. [Background technology]
[0003] The separator is an important material in lithium-ion batteries, and its main functions are to separate the positive and negative electrodes, prevent short circuits, ensure the required electrolyte wettability and electrolyte retention, and provide a path for lithium ion transport. The properties of the separator directly determine the interface properties and internal resistance of the battery, and further affect the charge / discharge and cycle characteristics of the battery.
[0004] The conventional lithium-ion battery separator is mainly made of polyolefin porous separator, which contains many fine through-holes and has a three-dimensional structure with polyolefin as a skeleton to support many fine pores. Its manufacturing method is mainly divided into dry stretching method and wet stretching method. Among them, the dry method is a method in which a polyolefin film is formed and then stretched at a low temperature to form fine pores, and the stretching causes microcracks between the sheets, which are the crystallized parts of the polyolefin. The wet method is a method in which a polyolefin resin and a diluent are kneaded at a high temperature at which the polyolefin resin melts and becomes a single phase, and then the polyolefin and the diluent are phase-separated during cooling, and the diluent is removed to form pores.
[0005] In the wet method, after phase separation, mechanical strength and transparency are imparted through a stretching / extraction process, and the polyethylene blank sheet formed into a sheet is stretched. By adjusting the stretching conditions such as speed, magnification, and temperature, the amorphous part in the crystal structure is stretched to a long length, forming fine fibers and forming fine pores between the sheet layers. Compared to the dry method, the wet method has a thinner film thickness, more uniform pore size, and better physical properties.
[0006] The document with publication number JP2005056851A proposes a microporous film of a laminated film, and in order to reduce the thermal shrinkage rate of the separator in the TD direction (direction perpendicular to the machine, width direction), the manufacturing method does not involve stretching in the TD direction, so it can be said that there is no shrinkage in the TD direction. However, by drilling holes only in one axis in the MD direction (machine direction, length direction), a microporous film with extreme anisotropy and insufficient strength in the TD direction is formed, which may make it more likely to crack in one direction, for example, in a crush test or impact test of a battery.
[0007] Publication No. JP2014141644A describes a biaxially oriented porous polypropylene membrane with a ratio of MD / TD stretch strength of 0.9 or more and less than 1.5. However, this polypropylene membrane is produced by a dry method, so it has low gas resistance and needs further improvement in breaking elongation and toughness.
[0008] A Chinese patent with publication number CN107250234B discloses a polyolefin microporous membrane that is mainly composed of polypropylene, has a ratio of MD / TD stretch strength of 0.4 or more and 2.0 or less, and a ratio of MD / TD breaking elongation of 0.6 or more and 1.7 or less. By adding additives that promote or inhibit the crystallization of polyolefin resin, nucleating agents and crystallization inhibitors, the pore structure of the polyolefin porous membrane can be made uniform and fine, and the impact resistance can be further improved.
[0009] Therefore, in order to improve the safety of the battery, it is important to improve the properties of the separator. Conventional polyolefin porous separators have been maturely applied in lithium-ion batteries, but the conventional technology mainly focuses on the basic properties and physical and chemical properties of the separator, and little attention is paid to the consistency of the microstructure. In order to improve the properties of wet separators for lithium-ion batteries, it is necessary to optimize the microstructure to improve the properties and optimize the uniformity of the mechanical properties in each direction. [Prior art documents] [Patent documents]
[0010] [Patent Document 1] Patent Publication No. 2005-056851 (Japan / A) [Patent Document 2] JP2014-141644 (Japan / A) [Patent Document 3] Chinese Patent No. 107250234 (China / B) Summary of the Invention [Problem to be solved by the invention]
[0011] An object of the present disclosure is to provide a polyolefin porous membrane which, when used as a battery separator, can provide a battery with excellent battery safety and improve the production stability of the battery. Another object of the present disclosure is to provide a method for producing the above-mentioned polyolefin porous membrane, which can obtain a polyolefin porous membrane having a uniform orientation of the microfiber structure and a small difference in mechanical properties between two macroscopic directions by controlling the difference in orientation during the stretching of the separator to a small extent and controlling the molding temperature. [Means for solving the problem]
[0012] The polyolefin porous membrane according to the present disclosure is produced by wet stretching and has a mesh fiber structure, When observed in a 20,000x SEM image, it has the following characteristics: (1) Within a circle with a radius of 1000 nm, the fiber orientation R_MD in the MD direction of fibers with a fiber diameter > 15 nm is (R_MD) 2 <0.8 and R_MD is given by the following formula 1.
number
number
[0013] Optionally, the polyolefin porous membrane is produced by wet stretching and has a mesh fiber structure; When observed in a 20,000-fold SEM image, the polyolefin porous membrane has the following properties: (1) Within a circle with a radius of 1000 nm, the fiber orientation R_MD in the MD direction of fibers with a fiber diameter > 15 nm is (R_MD) 2 <0.5 and R_MD is given by the following formula 1.
number
number
[0014] The polyolefin microporous membrane further has the following properties:
[0015] Optionally, the ratio of the stretching strength in the MD direction to the stretching strength in the TD direction is an MD / TD stretching strength ratio, where 0.8≦MD / TD stretching strength ratio≦1.2.
[0016] Optionally, a ratio of the elongation at break in the MD direction to the elongation at break in the TD direction, MD / TD elongation at break ratio, is 0.4≦MD / TD elongation at break≦1.2.
[0017] Optionally, the polyolefin porous membrane has a thickness of 1 to 30 μm.
[0018] The present disclosure further relates to Step 1: kneading and extruding polyolefin, pore former, and additives so that the mass ratio of polyolefin in the kneaded mixture is ≧15%, and the mass ratio of antioxidant in the kneaded mixture is 0-0.5%, and dispersing and mixing at high temperature by twin screws, plasticizing, and extruding through a die to produce a cast sheet; Step 2: stretching the casting sheet, during the stretching process, the temperature of the casting sheet itself is below 140°C, the temperature difference between different points in the temperature field of the stretching area is less than 0.5°C, and the ratio of the stretching ratio in MD to the stretching ratio in TD is 0.9≦MD / TD stretching ratio≦1.1 to obtain an oily film; Step 3, after the oily film is extracted, is subjected to hot-set treatment, and the original relationship between the stretch ratios in MD and TD is maintained during the hot-set treatment process, and the ratio between the stretch ratio in MD and the stretch ratio in TD in step 2 is maintained by the width-widening stretching process during the hot-set treatment process; The present invention also provides a method for producing the polyolefin porous membrane, comprising the steps of:
[0019] Optionally, in step 2, the stretching ratio in the MD direction and the stretching ratio in the TD direction are both 5 times or more.
[0020] Optionally, the viscosity average molecular weight of the polyolefin is between 200,000 and 5,000,000.
[0021] Optionally, the pore former is one or more of white oil, paraffin oil, polyethylene glycol.
[0022] Optionally, in step 1, the additive comprises an antioxidant, and the antioxidant is one or more of amines, sulfur-containing compounds, nitrogen-containing compounds, phosphorus-containing compounds, and organometallic salts.
[0023] The present disclosure further provides a battery separator comprising the porous polyolefin membrane. The present disclosure further provides an electrochemical device comprising said porous polyolefin membrane or said battery separator as an element separating a positive electrode and a negative electrode. Effect of the Invention
[0024] The present disclosure has the following beneficial effects: The polyolefin porous membrane of the present disclosure has the same mechanical properties as a separator in a battery, improving the stability of the separator in battery production and the safety when used in a battery. [Brief description of the drawings]
[0025] In order to more clearly explain the technical solutions of the embodiments of the present disclosure, the following briefly describes the drawings used in the embodiments, but it should be understood that the following drawings only illustrate some embodiments of the present disclosure, and should not be regarded as limiting the scope, and those skilled in the art can also obtain other drawings based on these drawings without requiring creative efforts.
[0026] [Figure 1] 1 shows a scanning electron microscope image of the polyolefin porous membrane of Example 1. [Diagram 2] 1 shows a scanning electron microscope image of the polyolefin porous membrane of Example 2. [Diagram 3] 1 shows a scanning electron microscope image of the polyolefin porous membrane of Example 3. [Figure 4]1 shows a scanning electron microscope image of the polyolefin porous membrane of Example 4. [Diagram 5] 1 shows a scanning electron microscope image of the polyolefin porous membrane of Example 5. [Figure 6] 1 shows a scanning electron microscope image of the polyolefin porous membrane of Example 6. [Figure 7] 1 shows a scanning electron microscope image of the polyolefin porous membrane of Example 9. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0027] In order to make the objectives, technical solutions and advantages of the embodiments of the present disclosure clearer, the technical solutions in the embodiments of the present disclosure are described below clearly and completely. Unless conditions are specified in the embodiments, they are carried out according to normal conditions or conditions suggested by the manufacturer. Unless the manufacturers of the reagents or instruments used are specified, they are all normal products available on the market.
[0028] The inventors have found that the uniformity of the fiber structure in a polyolefin porous membrane is an important factor for ensuring the performance of the separator, that the characteristics of the microfiber structure determine each macro-performance of the polyolefin porous membrane as a battery separator, and that the uniformity of the fiber distribution and orientation determines the shrinkage uniformity of the separator's mechanical properties, and that when a polyolefin porous membrane has the following characteristics, it can achieve excellent uniformity of mechanical properties in each direction and also has higher safety when used in a battery. When observed in a 20,000-fold SEM image, the polyolefin porous membrane has the following properties: (1) Within a circle with a radius of 1000 nm, the fiber orientation R_MD in the MD direction of fibers with a fiber diameter > 15 nm is (R_MD) 2 <0.8 and R_MD is given by the following formula 1.
number
number
[0029] In one embodiment, the polyolefin porous membrane is produced by wet stretching and has a mesh fiber structure. When observed in a 20,000x SEM image, it has the following characteristics: (1) Within a circle with a radius of 1000 nm, the fiber orientation R_MD in the MD direction of fibers with a fiber diameter > 15 nm is (R_MD) 2 <0.5 and R_MD is given by the following formula 1.
number
number
[0030] [Polyolefin resin] Examples of the polyolefin resin that can be used as the raw material include polyethylene, polypropylene, etc. The polyethylene is not particularly limited, but various types of polyethylene, such as ultra-high molecular weight polyethylene (UHMwPE), high density polyethylene (HDPE), medium density polyethylene, branched low density polyethylene, linear low density polyethylene, etc., can be used. The polyethylene may be a homopolymer of ethylene or a copolymer of ethylene and another α-olefin, such as propylene, 1-butene, 1-hexene, 1-pentene, 4-methyl-1-pentene, octene, vinyl acetate, methyl methacrylate, or styrene. In this specification, the polyolefin porous membrane refers to the microporous membrane that is mainly composed of polyolefin resin, for example, the microporous membrane that the polyolefin resin is 90 mass% or more of the total amount of the microporous membrane.The physical properties of the polyolefin porous membrane according to this embodiment will be described below.
[0031] [MD / TD stretching strength ratio] In the polyolefin porous membrane of the present disclosure, the MD / TD stretching strength ratio, which is the ratio of the stretching strength in MD direction to that in TD direction, may be 0.8 or more and 1.2 or less.When the stretching strength ratio is in the above range, it can more uniformly bear the force against the impact in all directions, so that when it is applied to a battery as a separator, it has improved impact resistance, is more stable, and can suppress the breakage and short circuit of the membrane. From the viewpoint of safety and stability when applied to a battery, the MD / TD stretching strength ratio is optionally made close to 1. In this case, since the strength of the polyolefin porous membrane is not directional-dependent, when stress is applied to the membrane, the membrane has excellent toughness, cracks do not occur in a specific direction, and even if a foreign object penetrates the microporous membrane, the expansion of the through-hole can be avoided. Otherwise, if the stretching strength in the MD direction is too large, tearing in the MD direction may occur. If the stretching strength in the TD direction is too large, tearing in the TD direction or adhesive failure of the adhesive part of the electrode tab may occur, making it easier for a short circuit to occur.
[0032] [MD / TD breaking elongation ratio] In the polyolefin porous membrane of the present disclosure, the MD / TD breaking elongation ratio, which is the breaking elongation ratio between MD and TD, may be 0.8 or more and 1.2 or less. When the breaking elongation ratio is in the above range, it can more uniformly bear the force of impact in all directions, so that when it is applied to a battery as a separator, the impact resistance is improved, and it is more stable and can suppress the breakage and short circuit of the membrane. From the viewpoint of safety and stability when applied to a battery, the MD / TD breaking elongation ratio is optionally made close to 1. In this case, since the strength of the polyolefin microporous membrane is not directional-dependent, when stress is applied to the membrane, the membrane has excellent toughness and does not develop cracks in a specific direction, and even if a foreign object penetrates the microporous membrane, the expansion of the through hole can be prevented.
[0033] [Film thickness] The thickness of polyolefin porous membrane is not particularly limited.From the viewpoint of membrane strength, the thickness of the polyolefin porous membrane of the present disclosure is 2 μm or more, preferably 5 μm or more.In addition, from the viewpoint of permeability, the thickness of microporous membrane is 50 μm or less, preferably 30 μm or less.
[0034] [Stretching strength] In the polyolefin porous membrane of the present disclosure, the stretching strength is 150MPa or more, preferably 200MPa or more in both MD and TD. If the stretching strength is weak, the winding property of the battery is poor, and short circuit is easily caused by external battery impact test, foreign matter in the battery, etc. In addition, the upper limit of the stretching strength in the MD and TD directions is not particularly limited, and from actual production experience, the upper limit of the stretching strength in the MD and TD directions is preferably 700MPa or less, preferably 600MPa or less, and preferably 550MPa or less.
[0035] [Elongation at break] In the polyolefin porous membrane of the present disclosure, the breaking elongation in the MD direction and the TD direction may be 90% or more. When the breaking elongation is within the above range, the separator film can be prevented from breaking or short-circuiting when it is subjected to an impact in the battery by utilizing its flexibility. In addition, the upper limit of the breaking elongation in the MD direction and the TD direction is not particularly limited, and is, for example, 400% or less, preferably 300% or less, and preferably 200% or less. When the breaking elongation is within the above range, the separator does not stretch and deform when the electrode is wound, and the winding property is good. The breaking elongation in the MD and TD is 10 to 200%, preferably 10 to 150%, and preferably 10 to 120%, respectively. A microporous membrane having MD and TD breaking elongations in the above ranges not only has good winding properties for a battery, but also is less likely to deform in a battery crash test or the like.
[0036] [Heat shrinkage rate] The polyolefin porous film is required to have excellent heat shrinkage properties at high temperatures when used as a separator, and must show excellent results in high-temperature storage tests, high-temperature cycle tests, bake tests, and the like when used in a battery. From the viewpoint of dimensional stability of the separator during charging and discharging, the heat shrinkage rate in the MD direction is less than 5% and the heat shrinkage rate in the TD direction is less than 6.5%, preferably the heat shrinkage rate in the MD is 4% or less and the heat shrinkage rate in the TD is 4% or less, preferably the heat shrinkage rate in the MD is 3% or less and the heat shrinkage rate in the TD is 2.5% or less, preferably the heat shrinkage rate in the MD is 1% or less and the heat shrinkage rate in the TD is 1% or less. If the heat shrinkage rate is larger than the above range, the microporous membrane is likely to shrink in the width direction during the battery drying process, the battery high temperature cycle test, the battery high temperature storage test, etc., which is not preferable.
[0037] [Method of manufacturing polyolefin porous membrane] The polyolefin porous membrane of the present disclosure is produced by a wet stretching method, and the production method includes the steps of: kneading one or more polyolefin resin materials as main raw materials with a pore-forming agent and an antioxidant, and extruding the kneaded mixture through a die to form a cast sheet (1); biaxially stretching the cast sheet to produce an oily membrane (2); and extracting the oily membrane and then performing a hot-setting process (3).
[0038] The temperature of casting sheet during stretching and the stretching ratio control are one of the important factors for obtaining the polyolefin porous membrane with above-mentioned characteristics.In biaxial stretching, it is necessary to control the temperature field and the stretching field, the temperature of casting sheet itself must not exceed 140 ℃, the temperature difference between different points in the temperature field of stretching area must be less than 0.5 ℃, and the ratio of the stretching ratio of MD and the stretching ratio of TD must be 0.9 or more and 1.1 or less, and when the ratio of actual stretching ratio is within the above-mentioned range, the stretching strength or breaking elongation of the obtained polyolefin porous membrane is well balanced in MD and TD, which can further improve the strength of membrane and improve impact resistance.
[0039] Next, in the hot set treatment, it is necessary to maintain the original relationship between the MD and TD stretch ratios. Another important factor is to maintain the ratio of the MD stretch ratio to the TD stretch ratio at 0.9 or more and 1.1 or less, which is the ratio of the biaxial stretching in step (2).
[0040] Here, the stretch ratio in the MD direction and the stretch ratio in the TD direction are the actual stretch ratios in the MD direction and the TD direction of the actual separator.
[0041] In the case of simultaneous stretching, the stretch ratio in MD and the stretch ratio in TD can be obtained directly from the actual setting of the equipment, and can be obtained as follows: The simultaneous stretch ratio in MD is equal to the ratio of the MD speed of the oiled film obtained after simultaneous stretching to the running speed of the sheet before stretching; the simultaneous stretch ratio in TD is equal to the ratio of the TD width of the oiled film obtained after simultaneous stretching to the width of the TD stretched area of the sheet before stretching, and it should be noted that the length of the width of the clip gripping part should be subtracted.
[0042] In the case of non-simultaneous stretching, the non-simultaneous stretching ratio in the MD direction can be obtained directly from the actual setting of the equipment, and can be obtained from the ratio of the sheet speed after stretching in the MD direction and before TD stretching to the speed before stretching. The non-simultaneous stretching ratio in the TD direction is the ratio of the actual width of the oiled film after the end of TD stretching to the actual width of the gel-like sheet before MD stretching.
[0043] The method for producing the above-mentioned polyolefin porous membrane is not particularly limited in terms of the types and blending ratios of polyolefin, pore-forming agent and antioxidant, the kneading / extrusion method, the type of extractant and whether or not it is used, the process for mitigating hot set, etc., as long as a polyolefin porous membrane having the above-mentioned properties can be obtained.
[0044] Examples of the polyolefin resin that can be used as the raw material include polyethylene and polypropylene. The polyethylene is not particularly limited, and various types of polyethylene, such as ultra-high molecular weight polyethylene (UHMWPE), high density polyethylene (HDPE), medium density polyethylene, branched low density polyethylene, and linear low density polyethylene, can be used. The polyethylene may be a homopolymer of ethylene or a copolymer of ethylene and another α-olefin. Examples of the α-olefin include propylene, 1-butene, 1-hexene, 1-pentene, 4-methyl-1-pentene, octene, vinyl acetate, methyl methacrylate, and styrene.
[0045] The viscosity average molecular weight of the polyolefin resin is from 200,000 to 5,000,000 so that the polymer melt can be easily processed and the film does not break. When the viscosity average molecular weight of the polyolefin resin is in the above range, the film formability is good.
[0046] Furthermore, the film-forming material may contain a polymer of a resin component other than the polyolefin material as necessary, and for example, a heat-resistant resin such as polypropylene, polyimide, polyamide, fluororesin, etc. can be used. Here, the mass ratio of the polyolefin in the kneaded material is 15% or more, and the mass ratio of the heat-resistant resin in the kneaded material is less than 10%.
[0047] The pore former may be a liquid hydrocarbon mixture such as white oil, an organic acid ester such as dioctyl phthalate (DOP), an inorganic acid ester such as trioctyl phosphate (TOP), an organic material capable of forming a homogeneous solution with the polyolefin resin, or a mixture of the above pore formers.
[0048] The antioxidant may be one main antioxidant or a mixture of multiple antioxidants. The antioxidant can delay the deterioration of the polymer and the pore-forming agent over time during shear processing, and effectively improve the color, flatness, and strength of the film surface.
[0049] Optionally, the stretching temperature is in the range of not less than the softening point (Tcd) at which the mixture of the polyolefin resin and the pore-forming agent is sufficiently melted, and not more than the melting point of the polyolefin resin. Here, the melting point of the polyolefin resin is the melting point of the polyolefin resin in the gel-like sheet. When the stretching temperature is not more than the melting point of the polyolefin resin, the melting of the polyolefin resin in the gel-like sheet is suppressed, and the molecular chains can be efficiently oriented by stretching. In addition, when the stretching temperature is not less than the softening point (Tcd), the polyolefin resin in the gel-like sheet can be sufficiently softened to reduce the stretching force, so that the film formability is good, the film breakage during stretching can be suppressed, and high-magnification stretching is possible. The stretching temperature can be, for example, 50°C or more and 140°C or less, preferably 60°C or more and 130°C or less. Here, the stretching temperature is the temperature of the gel-like sheet.
[0050] By controlling the difference in orientation during the stretching of the separator to a small extent and controlling the molding temperature, a polyolefin porous membrane can be obtained in which the orientation of the microfiber structure is uniform and the difference in mechanical properties between the two macroscopic directions is small. When this polyolefin porous membrane is used as a battery separator, the stability of the separator in battery production and the safety of its use in the battery can be improved. EXAMPLES
[0051] The present disclosure will be described in detail below with reference to examples, but the present disclosure is not limited to these examples.
[0052] [Example 1] 25 parts by weight of polyethylene powder (GUR4116, Ticona CELANESE), 5 parts by weight of polypropylene (T30S, manufactured by Zhenhai Renka Co., Ltd.), and 70 parts by weight of paraffin oil (60#, manufactured by Zhejiang Zhengxin Co., Ltd.) were used, and 0.3 parts by weight of antioxidant (Irg1010 (Ciba Specialty Chemicals BASF)) and 0.1 parts by weight of antioxidant (P168 (manufactured by Ciba Specialty Chemicals Co., Ltd.)) were added to the total of 100 parts by weight of the polyolefin composition and paraffin oil, and these were mixed in order. After mixing the auxiliary, the ultra-high molecular weight polyethylene material and the paraffin oil were put together into a twin-screw extruder and kneaded, and finally a mixed melt gel was produced. The gel was extruded using a T-die, and the temperature of the extruded melt was controlled to 220°C or less. After that, the gel was quickly cooled with two thermostatic metal rolls with a surface temperature of 15°C, and then rolled into a sheet with a thickness of 1.5 mm. The sheet, i.e., the cast sheet, was stretched by pulling. High-speed stretching was performed at 120°C and a speed of 40m / min, where 6.5 times stretching was performed in both MD and TD. During stretching, the uniformity of the temperature field was controlled, and the temperature difference between different points in the temperature field of the stretching area was less than 0.3°C, and an oily film was obtained after stretching. The oily film was pulled into dichloromethane for extraction, and the paraffin oil in the oily film was removed by extraction. After that, the dichloromethane remaining in the separator was removed with constant-temperature hot air at 40°C, and during extraction and drying, a small amount of shrinkage of 15% occurred in the TD direction due to the action of MD pulling, so the original ratio of the stretching ratio in the MD direction and the stretching ratio in the TD direction was realized by hot setting and widening at 131°C, and finally, a polyolefin porous film with uniform fiber structure orientation was obtained.
[0053] [Example 2] 23 parts by weight of ultra-high molecular weight polyethylene powder (GUR4012, Ticona CELANESE) and 77 parts by weight of paraffin oil (60#, Zhejiang Zhengxin Co., Ltd.) were used, and 0.3 parts by weight of antioxidant (Irg1010 (Ciba Specialty Chemicals BASF)) and 0.1 parts by weight of antioxidant (P168 (Ciba Specialty Chemicals Co., Ltd.)) were added to the total of 100 parts by weight of the high molecular weight polyethylene and paraffin oil, and these were mixed in order. After mixing the auxiliary, the ultra-high molecular weight polyethylene material and the paraffin oil were fed together into a twin-screw extruder and kneaded, and finally a mixed melt gel was produced. The gel was extruded using a T-die, and the temperature of the extruded melt was controlled to 220°C or less. After that, it was quickly cooled with two thermostatic metal rolls with a surface temperature of 15°C, and rolled into a sheet with a thickness of 1.5 mm. The sheet, i.e., the cast sheet, was drawn and stretched. High-speed stretching was performed at 117°C and a speed of 40m / min, where stretching was performed by 7.5 times in the MD direction and 7.2 times in the TD direction. The uniformity of the temperature field was controlled during stretching, and the temperature difference between different points in the temperature field of the stretching area was less than 0.3°C, and an oily film was obtained after stretching. The oily film was drawn and extracted in dichloromethane, and the paraffin oil in the oily film was removed by extraction. After that, the dichloromethane remaining in the separator was removed with constant-temperature hot air at 40°C. During extraction and drying, a small amount of shrinkage of 18% occurred in the TD direction due to the action of MD traction. Next, the original ratio of the MD and TD stretching ratios was restored by hot setting and widening at 131°C, and finally a polyolefin porous membrane with uniform fiber structure orientation was obtained.
[0054] [Example 3] 15 parts by weight of ultra-high molecular weight polyethylene powder (GUR2122, Ticona CELANESE), 5 parts by weight of high density polyethylene powder (GUR4116, Ticona CELANESE), 80 parts by weight of paraffin oil (60#, Zhejiang Zhengxin Co., Ltd.), 0.3 parts by weight of antioxidant (Irg1010 (Ciba Specialty Chemicals BASF)) and 0.1 parts by weight of antioxidant (P168 (Ciba Specialty Chemicals Co., Ltd.)) were added to the high molecular weight polyethylene and paraffin oil in a total of 100 parts by weight, and these were mixed in order. After mixing the auxiliary, the ultra-high molecular weight polyethylene material and the paraffin oil were put together into a twin-screw extruder and kneaded, and finally a mixed melt gel was produced. The gel was extruded using a T-die, and the temperature of the extruded melt was controlled to 220°C or less. After that, it was quickly cooled with two thermostatic metal rolls with a surface temperature of 15°C, and rolled into a sheet with a thickness of 1.5 mm. The sheet, i.e., the cast sheet, was stretched by pulling. High-speed stretching was performed at 122°C and a speed of 40m / min, where stretching was performed at 7.2 times in the MD direction and 7.1 times in the TD direction. When stretching, the uniformity of the temperature field was controlled, and the temperature difference between different points in the temperature field of the stretching area was less than 0.3°C, and an oily film was obtained after stretching. The oily film was pulled into dichloromethane for extraction, and the paraffin oil in the oily film was removed by extraction. Then, the dichloromethane remaining in the separator was removed with constant-temperature hot air at 40°C, and during extraction and drying, a small amount of shrinkage of 20% occurred in the TD direction due to the action of MD pulling, so the original ratio of the stretching ratio in the MD direction and the stretching ratio in the TD direction was realized by hot setting and widening at 131°C, and finally, a polyolefin porous film with uniform fiber structure orientation was obtained.
[0055] [Example 4] Using 5 parts by weight of ultra-high molecular weight polyethylene powder (GUR2122, Ticona CELANESE), 10 parts by weight of high density polyethylene powder (VH200U, KPIC), 5 parts by weight of polyethylene powder (VH035, KPIC), and 80 parts by weight of paraffin oil (60#, Zhejiang Zhengxin Co., Ltd.), 0.3 parts by weight of antioxidant (Irg1010 (Ciba Specialty Chemicals BASF)) and 0.1 parts by weight of antioxidant (P168 (Ciba Specialty Chemicals Co., Ltd.)) were added to the total of 100 parts by weight of the high molecular weight polyethylene and paraffin oil, and these were mixed in order. After mixing the auxiliary, the ultra-high molecular weight polyethylene material and the paraffin oil were fed together into a twin-screw extruder and kneaded, and finally a mixed melt gel was produced. The gel was extruded using a T-die, and the temperature of the extruded melt was controlled to 220°C or less. After that, it was quickly cooled with two thermostatic metal rolls with a surface temperature of 15°C, and rolled into a sheet with a thickness of 1.5 mm. The sheet, i.e., the cast sheet, was stretched by pulling. High-speed stretching was performed at 117°C and a speed of 40m / min, where 6.8 times stretching was performed in the MD direction and 6.8 times stretching in the TD direction. When stretching, the uniformity of the temperature field was controlled, and the temperature difference between different points in the temperature field of the stretching area was less than 0.3°C, and an oily film was obtained after stretching. The oily film was pulled into dichloromethane for extraction, and the paraffin oil in the oily film was removed by extraction. Then, the dichloromethane remaining in the separator was removed with constant-temperature hot air at 40°C, and during extraction and drying, a small amount of shrinkage of 21% occurred in the TD direction due to the action of pulling in the MD direction. Next, the original ratio of the stretching ratio in the MD direction and the stretching ratio in the TD direction was realized by hot setting and widening at 131°C, and finally, a polyolefin porous film with uniform fiber structure orientation was obtained.
[0056] [Example 5] Using 5 parts by weight of ultra-high molecular weight polyethylene powder (GUR2122, Ticona CELANESE), 10 parts by weight of high density polyethylene powder (VH200U, KPIC), 5 parts by weight of polyethylene powder (VH035, KPIC), and 80 parts by weight of paraffin oil (60#, Zhejiang Zhengxin Co., Ltd.), 0.3 parts by weight of antioxidant (Irg1010 (Ciba Specialty Chemicals BASF)) and 0.1 parts by weight of antioxidant (P168 (Ciba Specialty Chemicals Co., Ltd.)) were added to the total of 100 parts by weight of the high molecular weight polyethylene and paraffin oil, and these were mixed in order. After mixing the auxiliary, the ultra-high molecular weight polyethylene material and the paraffin oil were fed together into a twin-screw extruder and kneaded, and finally a mixed melt gel was produced. The gel was extruded using a T-die, and the temperature of the extruded melt was controlled to 220°C or less. After that, it was quickly cooled with two thermostatic metal rolls with a surface temperature of 15°C, and rolled into a sheet with a thickness of 1.5 mm. The sheet, i.e., the cast sheet, was stretched by drawing. High-speed drawing was performed at 116°C and a speed of 40m / min, where 8 times drawing was performed in the MD direction and 8 times drawing in the TD direction. During drawing, the uniformity of the temperature field was controlled, and the temperature difference between different points in the temperature field of the drawing area was less than 0.3°C, and an oily film was obtained after drawing. The oily film was drawn into dichloromethane for extraction, and the paraffin oil in the oily film was removed by extraction. Then, the dichloromethane remaining in the separator was removed with constant-temperature hot air at 40°C, and during extraction and drying, a small amount of shrinkage of 21% occurred in the TD direction due to the action of drawing in the MD direction. Then, the original ratio of the drawing ratio in the MD direction and the drawing ratio in the TD direction was realized by hot setting and widening at 131°C, and finally, a polyolefin porous film with uniform fiber structure orientation was obtained.
[0057] [Example 6] Using 5 parts by weight of ultra-high molecular weight polyethylene powder (GUR2122, Ticona CELANESE), 10 parts by weight of high density polyethylene powder (VH200U, KPIC), 5 parts by weight of polyethylene powder (VH035, KPIC), and 80 parts by weight of paraffin oil (60#, Zhejiang Zhengxin Co., Ltd.), 0.3 parts by weight of antioxidant (Irg1010 (Ciba Specialty Chemicals BASF)) and 0.1 parts by weight of antioxidant (P168 (Ciba Specialty Chemicals Co., Ltd.)) were added to the total of 100 parts by weight of the high molecular weight polyethylene and paraffin oil, and these were mixed in order. After mixing the auxiliary, the ultra-high molecular weight polyethylene material and the paraffin oil were fed together into a twin-screw extruder and kneaded, and finally a mixed melt gel was produced. The gel was extruded using a T-die, and the temperature of the extruded melt was controlled to 220°C or less. After that, it was quickly cooled with two thermostatic metal rolls with a surface temperature of 15°C, and rolled into a sheet with a thickness of 1.5 mm. The sheet, i.e., the cast sheet, was stretched by pulling. High-speed stretching was performed at 115°C and a speed of 40m / min, where 10 times stretching was performed in the MD direction and 10 times stretching in the TD direction. During stretching, the uniformity of the temperature field was controlled, and the temperature difference between different points in the temperature field of the stretching area was less than 0.3°C, and an oily film was obtained after stretching. The oily film was pulled into dichloromethane for extraction, and the paraffin oil in the oily film was removed by extraction. Then, the dichloromethane remaining in the separator was removed with constant-temperature hot air at 40°C, and during extraction and drying, a small amount of shrinkage of 21% occurred in the TD direction due to the action of pulling in the MD direction. Next, the original ratio of the stretching ratio in the MD direction and the stretching ratio in the TD direction was realized by hot setting and widening at 131°C, and finally, a polyolefin porous film with uniform fiber structure orientation was obtained.
[0058] [Example 7] Using 5 parts by weight of ultra-high molecular weight polyethylene powder (GUR2122, Ticona CELANESE), 10 parts by weight of high density polyethylene powder (VH200U, KPIC), 5 parts by weight of polyethylene powder (VH035, KPIC), and 80 parts by weight of paraffin oil (60#, Zhejiang Zhengxin Co., Ltd.), 0.3 parts by weight of antioxidant (Irg1010 (Ciba Specialty Chemicals BASF)) and 0.1 parts by weight of antioxidant (P168 (Ciba Specialty Chemicals Co., Ltd.)) were added to the total of 100 parts by weight of the high molecular weight polyethylene and paraffin oil, and these were mixed in order. After mixing the auxiliary, the ultra-high molecular weight polyethylene material and the paraffin oil were fed together into a twin-screw extruder and kneaded, and finally a mixed melt gel was produced. The gel was extruded using a T-die, and the temperature of the extruded melt was controlled to 220°C or less. After that, it was quickly cooled with two thermostatic metal rolls with a surface temperature of 15°C, and rolled into a sheet with a thickness of 1.5 mm. The sheet, i.e., the cast sheet, was stretched by pulling. High-speed stretching was performed at 115°C and a speed of 40m / min, where 10 times stretching was performed in the MD direction and 11 times stretching in the TD direction. During stretching, the uniformity of the temperature field was controlled, and the temperature difference between different points in the temperature field of the stretching area was less than 0.3°C, and an oily film was obtained after stretching. The oily film was pulled into dichloromethane for extraction, and the paraffin oil in the oily film was removed by extraction. Then, the dichloromethane remaining in the separator was removed with constant-temperature hot air at 40°C, and during extraction and drying, a small amount of shrinkage of 21% occurred in the TD direction due to the action of pulling in the MD direction. Next, the original ratio of the stretching ratio in the MD direction and the stretching ratio in the TD direction was realized by hot setting and widening at 131°C, and finally, a polyolefin porous film with uniform fiber structure orientation was obtained.
[0059] [Example 8] Using 5 parts by weight of ultra-high molecular weight polyethylene powder (GUR2122, Ticona CELANESE), 10 parts by weight of high density polyethylene powder (VH200U, KPIC), 5 parts by weight of polyethylene powder (VH035, KPIC), and 80 parts by weight of paraffin oil (60#, Zhejiang Zhengxin Co., Ltd.), 0.3 parts by weight of antioxidant (Irg1010 (Ciba Specialty Chemicals BASF)) and 0.1 parts by weight of antioxidant (P168 (Ciba Specialty Chemicals Co., Ltd.)) were added to the total of 100 parts by weight of the high molecular weight polyethylene and paraffin oil, and these were mixed in order. After mixing the auxiliary, the ultra-high molecular weight polyethylene material and the paraffin oil were fed together into a twin-screw extruder and kneaded, and finally a mixed melt gel was produced. The gel was extruded using a T-die, and the temperature of the extruded melt was controlled to 220°C or less. After that, it was quickly cooled with two thermostatic metal rolls with a surface temperature of 15°C, and rolled into a sheet with a thickness of 1.5 mm. The sheet, i.e., the cast sheet, was stretched by pulling. High-speed stretching was performed at 115°C and a speed of 40m / min, where 10 times stretching was performed in the MD direction and 9.1 times stretching was performed in the TD direction. During stretching, the uniformity of the temperature field was controlled, and the temperature difference between different points in the temperature field of the stretching area was less than 0.3°C, and an oily film was obtained after stretching. The oily film was pulled into dichloromethane for extraction, and the paraffin oil in the oily film was removed by extraction. Then, the dichloromethane remaining in the separator was removed with constant-temperature hot air at 40°C, and during extraction and drying, a small amount of shrinkage of 21% occurred in the TD direction due to the action of pulling in the MD direction. Next, the original ratio of the stretching ratio in the MD direction and the stretching ratio in the TD direction was realized by hot setting and widening at 131°C, and finally, a polyolefin porous film with uniform fiber structure orientation was obtained.
[0060] [Example 9] Using 15 parts by weight of ultra-high molecular weight polyethylene powder (VH200U, LPIC), 5 parts by weight of high density polyethylene powder (VH035, KPIC), and 80 parts by weight of paraffin oil (60#, Zhejiang Zhengxin Co., Ltd.), 0.3 parts by weight of antioxidant (Irg1010 (Ciba Specialty Chemicals BASF)) and 0.1 parts by weight of antioxidant (P168 (Ciba Specialty Chemicals Co., Ltd.)) were added to the total of 100 parts by weight of the high molecular weight polyethylene and paraffin oil, and these were mixed in order. After mixing the auxiliary, the ultra-high molecular weight polyethylene material and the paraffin oil were put together into a twin-screw extruder and kneaded, and finally a mixed melt gel was produced. The gel was extruded using a T-die, and the temperature of the extruded melt was controlled to 220°C or less. After that, it was quickly cooled with two thermostatic metal rolls with a surface temperature of 15°C, and rolled into a sheet with a thickness of 1.5 mm. The sheet, i.e., the cast sheet, was drawn and stretched stepwise. Under the condition of 90°C, the cast sheet was drawn in the MD direction, where the stretch ratio in the MD direction was 9 times. Then, high-speed drawing in the TD direction was performed at 119°C and a speed of 60m / min, where the stretch ratio in the TD direction was 8.3 times (the ratio of the width at the outlet to the width of the original cast piece was 8.2 times). During drawing, the uniformity of the temperature field was controlled, and the temperature difference between different points of the temperature field in the drawing area was less than 0.3°C. After the drawing was completed, an oily film was obtained. The oily film was drawn into dichloromethane for extraction, and the paraffin oil in the oily film was removed by extraction. After that, the dichloromethane remaining in the separator was removed with constant-temperature hot air at 40°C. During extraction and drying, a small amount of shrinkage of 22% occurred in the TD direction due to the pulling force in the MD direction. Next, the film was hot-set at 131°C and widened to restore the original ratio of the stretch ratio in the MD direction to the stretch ratio in the TD direction. Finally, a polyolefin porous membrane with a uniform fiber structure orientation was obtained.
[0061] [Comparative Example 1] 25 parts by weight of ultra-high molecular weight polyethylene powder (GUR4116, Ticona CELANESE) and 77 parts by weight of paraffin oil (60#, Zhejiang Zhengxin Co., Ltd.) were used, and 0.3 parts by weight of antioxidant (Irg1010 (Ciba Specialty Chemicals BASF)) and 0.1 parts by weight of antioxidant (P168 (Ciba Specialty Chemicals Co., Ltd.)) were added to the total of 100 parts by weight of the high molecular weight polyethylene and paraffin oil, and these were mixed in order. After mixing the auxiliary, the ultra-high molecular weight polyethylene material and the paraffin oil were put together into a twin-screw extruder and kneaded, and finally a mixed melt gel was produced. The gel was extruded using a T-die, and the temperature of the extruded melt was controlled to 220°C or less. After that, it was quickly cooled with two thermostatic metal rolls with a surface temperature of 15°C, and rolled into a sheet with a thickness of 1.5 mm. The sheet, i.e., the cast sheet, was stretched by pulling. High-speed stretching was performed at 117°C and a speed of 40m / min, where MD and TD were stretched by 7.9 times and 6.5 times, respectively. During stretching, the uniformity of the temperature field was controlled, and the temperature difference between different points in the temperature field of the stretching area was less than 0.3°C, and an oily film was obtained after stretching. The oily film was pulled into dichloromethane for extraction, and the paraffin oil in the oily film was removed by extraction. After that, the dichloromethane remaining in the separator was removed with constant-temperature hot air at 40°C, and during extraction and drying, a small amount of shrinkage of 18% occurred in the TD direction due to the action of MD pulling, so the original ratio of the stretching ratio in the MD direction and the stretching ratio in the TD direction was realized by hot setting and widening at 131°C, and finally, a polyolefin porous membrane was obtained.
[0062] [Comparative Example 2] Using 5 parts by weight of ultra-high molecular weight polyethylene powder (GUR2122, Ticona CELANESE), 10 parts by weight of high density polyethylene powder (VH200U, KPIC), 5 parts by weight of polyethylene powder (VH035, KPIC), and 80 parts by weight of paraffin oil (60#, Zhejiang Zhengxin Co., Ltd.), 0.3 parts by weight of antioxidant (Irg1010 (Ciba Specialty Chemicals BASF)) and 0.1 parts by weight of antioxidant (P168 (Ciba Specialty Chemicals Co., Ltd.)) were added to the total of 100 parts by weight of the high molecular weight polyethylene and paraffin oil, and these were mixed in order. After mixing the auxiliary, the ultra-high molecular weight polyethylene material and the paraffin oil were fed together into a twin-screw extruder and kneaded, and finally a mixed melt gel was produced. The gel was extruded using a T-die, and the temperature of the extruded melt was controlled to 220°C or less. After that, it was quickly cooled with two thermostatic metal rolls with a surface temperature of 15°C, and rolled into a sheet with a thickness of 1.5 mm. The sheet, i.e., the cast sheet, was stretched by pulling. High-speed stretching was performed at 116°C and a speed of 40m / min, where 7.1 times stretching was performed in the MD direction and 5.4 times stretching in the TD direction. When stretching, the uniformity of the temperature field was controlled, and the temperature difference between different points in the temperature field of the stretching area was less than 0.3°C, and an oily film was obtained after stretching. The oily film was pulled into dichloromethane for extraction, and the paraffin oil in the oily film was removed by extraction. Then, the dichloromethane remaining in the separator was removed with constant-temperature hot air at 40°C, and during extraction and drying, a small amount of shrinkage of 21% occurred in the TD direction due to the action of pulling in the MD direction, so next, the original ratio of the stretching ratio in the MD direction and the stretching ratio in the TD direction was realized by hot setting and widening at 131°C, and finally, a polyolefin porous membrane was obtained.
[0063] <Evaluation method> (1) Film thickness test The thickness of the polyolefin porous membrane obtained in each example was measured with a high-precision micrometer. (2) Fiber orientation test Using a Nova Nano SEM 450 type field emission scanning electron microscope manufactured by FEI Corporation, USA, a SEM image of the polyolefin porous membrane was obtained at a magnification of 20,000 times, and a circle with a radius of 1000 nm was observed as the observation area. According to the above formulas 1 and 2, the fiber orientation result in the MD direction of the polyolefin porous membrane, R_MD, and the fiber orientation result in the TD direction, R_TD, were obtained. In addition, when calculating R_MD and R_TD, the fibers on the outermost surface of the polyolefin porous membrane are selected, N is the number of fibers on the outermost surface in the observation area, and each fiber is represented by n (n is a natural number), and the selected fiber length is the length of a segment of the same thickness having the same stretching direction on the same fiber, and when the thickness of the same fiber changes, it is not one length, but the difference needs to be corrected as necessary. The segment of the same thickness means that the increase rate of the width of the thickest part in the segment from the width of the thinnest part is within 5%, and the fiber diameter is the average value of the width of the thickest part and the width of the thinnest part on the segment of the same thickness, and the angle between the fiber and the MD direction or TD direction is the angle between the stretching direction of the segment of the same thickness and the MD direction or TD direction. (3) Stretching strength test The test was conducted in accordance with GB 1040.3-2006, the test specimens were prepared using the cutting method, and the type of test specimen was type 2. The test specimen was a long bar with a length of 200 mm and a width of 25 mm, the jig distance was (100±5) mm, and the test speed was (250±10) mm / min. (4) Breaking elongation test The test was conducted in accordance with GB 1040.3-2006, the test specimens were prepared using the cutting method, and the type of test specimen was type 2. The test specimen was a long bar with a length of 200 mm and a width of 25 mm, the jig distance was (100±5) mm, and the test speed was (250±10) mm / min. (5) Heat shrinkage test The test was conducted in accordance with GB / T12027-2004. A 100mm x 100mm sample was removed from the polyolefin microporous separator and placed in a ventilation oven and left to stand at 105°C for 1 hour. The thermal shrinkage rate was calculated using the following formula. MD heat shrinkage rate (%) = |(MD length before heating - MD length after heating) ÷ MD length before heating| × 100 TD heat shrinkage rate (%) = |(TD length before heating - TD length after heating) ÷ TD length before heating| × 100 Referring to Tables 1 and 2, the characteristic test results of the above examples and comparative examples are as follows.
[0064] Table 1: Parameter index of relevant properties of polyolefin porous membranes of Examples 1 to 9 [Table 1]
[0065] Table 2: Parameter index of related properties of polyolefin porous membranes of Comparative Examples 1 to 2 [Table 2]
[0066] Tables 1 and 2 show the relevant characteristic indexes of the polyolefin porous membranes of Examples 1 to 9 and Comparative Examples 1 and 2, respectively. The fiber orientation result R_MD in the MD direction in the polyolefin porous membrane is (R_MD) 2 <0.8 and the fiber orientation result in the TD direction R_TD is (R_TD) 2 When the ratio satisfies <0.8, the separator can be endowed with excellent mechanical properties with uniformity in each direction, and the safety can be increased when applied to a battery.
[0067] The above is merely a preferred embodiment of the present disclosure, and does not limit the present disclosure, and the present disclosure can be modified and changed by those skilled in the art. Any amendments, equivalent replacements and improvements made within the spirit and principle of the present disclosure shall be included within the scope of protection of the present disclosure.
Claims
1. It has a mesh fiber structure, A polyolefin porous membrane characterized by having the following properties when observed in a 20,000x SEM image: (1) Within a circle with a radius of 1000 nm, the fiber orientation R_MD in the MD direction of a fiber with a fiber diameter > 15 nm is (R_MD) 2 < 0.8, and R_MD is given by the following formula 1. [0010] Formula 1 (where θ n is the angle between the fiber and the MD direction, and θ n is obtained counterclockwise starting from the left in the MD direction, and the fiber length value L in μm n and cosθ n The product of this is L n cosθ n and φ n is the fiber diameter in nm.) (2) Within a circle with a radius of 1000 nm, the fiber orientation R_TD in the TD direction of fibers with a fiber diameter > 15 nm is (R_TD) 2 < 0.8, and R_TD is given by the following formula 2 [0025] Formula 2 (where β n is the angle between the fiber and the TD direction, and β n is obtained counterclockwise starting from the upward direction in the TD direction, and the fiber length value L in μm n and cosβ n The product of this is L n cosβ n and φ n is the fiber diameter in nm.)
2. It has a mesh fiber structure, The polyolefin porous membrane according to claim 1, characterized in that, when observed in a 20,000-times magnification SEM image, it has the following characteristics: (1) Within a circle with a radius of 1000 nm, the fiber orientation R_MD in the MD direction of a fiber with a fiber diameter > 15 nm is (R_MD) 2 < 0.5, and R_MD is obtained by the following formula 1. [0030] Formula 1 (where θ n is the angle between the fiber and the MD direction, and θ n is obtained counterclockwise starting from the left in the MD direction, and the fiber length value L in μm n and cosθ n The product of this is L n cosθ n and φ n is the fiber diameter in nm.) (2) Within a circle with a radius of 1000 nm, the fiber orientation R_TD in the TD direction of fibers with a fiber diameter > 15 nm is (R_TD) 2 < 0.5, and R_TD is given by the following formula 2. [0045] Formula 2 (where β n is the angle between the fiber and the TD direction, and β n is obtained counterclockwise starting from the upward direction in the TD direction, and the fiber length value L in μm n and cosβ n The product of this is L n cosβ n and φ n is the fiber diameter in nm.)
3. The MD / TD stretch strength ratio, which is the ratio of the stretch strength in the MD direction to the stretch strength in the TD direction, is The polyolefin porous membrane according to any one of claims 1 to 2, characterized in that the MD / TD stretching strength ratio is 0.8≦1.
2.
4. The MD / TD breaking elongation ratio, which is the ratio of the breaking elongation in the MD direction to the breaking elongation in the TD direction, is The polyolefin porous membrane according to any one of claims 1 to 2, characterized in that the MD / TD breaking elongation ratio is 0.75≦1.
34.
5. The polyolefin porous membrane according to any one of claims 1 to 2, characterized in that the membrane thickness is 1 to 30 µm.
6. The polyolefin porous membrane is It has a mesh fiber structure, When the SEM image was observed at 20,000 times magnification, it had the following characteristics: Step 1: mixing and extruding a polyolefin, a pore former and additives to produce a cast sheet; Step 2: stretching the casting sheet, during the stretching process, the temperature of the casting sheet itself is below 140°C, the temperature difference between different points in the temperature field of the stretching area is less than 0.5°C, and the ratio of the stretching ratio in the MD direction to the stretching ratio in the TD direction, that is, the MD / TD stretching ratio ratio is 0.9≦MD / TD stretching ratio≦1.1 to obtain an oily film; Step 3, after the oily film is extracted, is subjected to hot-setting treatment, and during the hot-setting treatment, the ratio of the stretching ratio in the MD direction to the stretching ratio in the TD direction in step 2 is maintained by a width-widening stretching treatment; A method for producing a polyolefin porous membrane, comprising: (1) Within a circle with a radius of 1000 nm, the fiber orientation R_MD in the MD direction of a fiber with a fiber diameter > 15 nm is (R_MD) 2 < 0.8, and R_MD is obtained by the following formula 1. [0050] Formula 1 (where θ n is the angle between the fiber and the MD direction, and θ n is obtained counterclockwise starting from the left in the MD direction, and the fiber length value L in μm n and cosθ n The product of this is L n cosθ n and φ n is the fiber diameter in nm.) (2) Within a circle with a radius of 1000 nm, the fiber orientation R_TD in the TD direction of fibers with a fiber diameter > 15 nm is (R_TD) 2 < 0.8, and R_TD is given by the following formula 2. [006] Formula 2 (where β n is the angle between the fiber and the TD direction, and β n is obtained counterclockwise starting from the upward direction in the TD direction, and the fiber length value L in μm n and cosβ n The product of this is L n cosβ n and φ n is the fiber diameter in nm.)
7. The polyolefin porous membrane has a mesh fiber structure, and when observed in a 20,000-times magnification SEM image, it has the following characteristics: Step 1: mixing and extruding a polyolefin, a pore former and additives to produce a cast sheet; Step 2: stretching the casting sheet, during the stretching process, the temperature of the casting sheet itself is below 140°C, the temperature difference between different points in the temperature field of the stretching area is less than 0.5°C, and the ratio of the stretching ratio in the MD direction to the stretching ratio in the TD direction, that is, the MD / TD stretching ratio ratio is 0.9≦MD / TD stretching ratio≦1.1, to obtain an oily film; Step 3, after the oily film is extracted, is subjected to hot-setting treatment, and during the hot-setting treatment, the ratio of the stretching ratio in the MD direction to the stretching ratio in the TD direction in step 2 is maintained by a width-widening stretching treatment; The method for producing the polyolefin porous membrane according to claim 6, comprising: (1) Within a circle with a radius of 1000 nm, the fiber orientation R_MD in the MD direction of a fiber with a fiber diameter > 15 nm is (R_MD) 2 < 0.5, and R_MD is obtained by the following formula 1. [0070] Formula 1 (where θ n is the angle between the fiber and the MD direction, and θ n is obtained counterclockwise starting from the left in the MD direction, and the fiber length value L in μm n and cosθ n The product of this is L n cosθ n and φ n is the fiber diameter in nm.) (2) Within a circle with a radius of 1000 nm, the fiber orientation R_TD in the TD direction of fibers with a fiber diameter > 15 nm is (R_TD) 2 < 0.5, and R_TD is given by the following formula 2. [0080] Formula 2 (where β n is the angle between the fiber and the TD direction, and β n is obtained counterclockwise starting from the upward direction in the TD direction, and the fiber length value L in μm n and cosβ n The product of this is L n cosβ n and φ n is the fiber diameter in nm.)
8. The method for producing a polyolefin porous membrane according to claim 6 or 7, characterized in that in step 2, the stretching ratio in the MD direction and the stretching ratio in the TD direction are both 5 times or more.
9. The method for producing a polyolefin porous membrane according to any one of claims 6 or 7, characterized in that in step 1, the mass ratio of the polyolefin in the kneaded product is 15% or more, and the viscosity average molecular weight of the polyolefin is between 200,000 and 5,000,000.
10. The method for producing a polyolefin porous membrane according to any one of claims 6 and 7, characterized in that the additives include an antioxidant, the mass ratio of the antioxidant in the kneaded mixture is 0 to 0.5%, and in step 1, the antioxidant is one or more of amines, sulfur-containing compounds, nitrogen-containing compounds, phosphorus-containing compounds, and organic metal salts.
11. The method for producing a polyolefin porous membrane according to any one of claims 6 and 7, characterized in that the pore-forming agent is one or more of white oil, paraffin oil, and polyethylene glycol.
12. A battery separator comprising the polyolefin porous membrane according to any one of claims 1 to 5.
13. An electrochemical device comprising the polyolefin porous membrane according to any one of claims 1 to 5 or the battery separator according to claim 12 as an element separating a positive electrode and a negative electrode.
Citation Information
Patent Citations
Polyolefin porous membrane and preparation method thereof, battery diaphragm and electrochemical device
CN115312973A
Microporous membranes, battery separators, and batteries
JP2010502472A
Polyolefin microporous membrane, production method therefor, and battery separator
CN107250234A
Battery separator and manufacturing method of the same
JP2005056851A
Biaxially oriented porous polypropylene film, separator film for electricity storage device and electricity storage device
JP2014141644A