Steel plate having a two-layer crystallization structure and a method for manufacturing such a steel plate

A two-layer crystallized steel sheet structure with a nitrogen-impermeable barrier layer addresses the challenge of maintaining high strength and formability, preventing surface roughening during deep drawing by ensuring a non-recrystallized region acts as a barrier to coarse grains, thus enhancing mechanical stability and corrosion resistance.

JP2024542905AInactive Publication Date: 2024-11-19THYSSENKRUPP RASSELSTEIN
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
JP2023574784
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2021-11-10
Filing Date
2022-11-03
Publication Date
2024-11-19
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing steel sheets used for packaging face challenges in maintaining high strength and formability, especially during deep drawing processes with small bending radii, leading to surface roughening and mechanical instability due to coarse grain structure.

Method used

A method involving a two-layer crystallized structure is created by applying a nitrogen-impermeable barrier layer on one side of the steel sheet, allowing nitrogen to diffuse only on the other side, resulting in a gradient of nitrogen concentration and increased recrystallization temperature, forming a completely recrystallized first region and a non- or partially recrystallized second region.

Benefits of technology

The method produces a steel sheet with high strength (>500 MPa) and good formability, preventing surface roughening and mechanical instability during severe forming, while maintaining rolling hardness and corrosion resistance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024542905000001_ABST
    Figure 2024542905000001_ABST
Patent Text Reader

Abstract

The present invention relates to a method for producing a packaging steel sheet containing a dual-phase recrystallized structure, the method comprising the steps of: Carbon content (C) of 10 to 1000 ppm by weight and a specific recrystallization temperature (T R (c) preparing a cold rolled steel sheet made from a steel having a first surface (a) and a second surface (b); applying an at least partially nitrogen impermeable barrier layer (3) onto a first side (a) of the steel sheet; Heating the steel sheet to a heating temperature (TE); Including, the heating step is carried out at least temporarily in a nitriding gas atmosphere until at least a recrystallization temperature (TR) is reached, whereby, during heating of the steel sheet, nitrogen from the gas atmosphere is diffused into and stored in at least a near-surface region (2) of the second side (b) of the steel sheet, whereby the recrystallization temperature of the steel is increased by a value ΔT in the near-surface region (2); The heating temperature (TE) is equal to or higher than the recrystallization temperature (TR) and is lower than the recrystallization temperature (TR+ΔT) increased by ΔT in the region (2) near the surface. (Figure 2)
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for producing a steel sheet having a dual crystallization structure, a steel sheet having a dual crystallization structure that can be used in particular for the production of packaging by deep drawing, and containers made from said steel sheet. [Background technology]

[0002] For the production of packaging from steel sheets such as tinplate or electrolytic chrome coated steel (ECCS), increasingly thinner steel sheets with thicknesses in the range of 0.1-0.25 mm are being used for reasons of resource efficiency. In order to ensure that sufficiently stable packaging can be produced from thinner steel sheets, it is necessary to improve the strength of the packaging steel. Furthermore, it is necessary to ensure that the steel sheets are still easily formable, unaffected by the reduction in thickness and the increase in strength, so that the steel sheets can be subjected to severe deformations that occur during the production of packaging in deep drawing and stretch forming processes.

[0003] It is widely known in the prior art to increase the strength of steel by introducing dissolved, unbound nitrogen into the steel, which is called sticking, nitriding or nitrifying and is a well-known process for solid solution strengthening of steel and steel products.

[0004] In the case of steel sheets intended for the manufacture of packaging (also known as packaging steel), it is also known to increase the strength by nitriding the steel. For example, according to German Patent Specification No. 102014116929, a method is known for producing nitrided packaging steel from a hot-rolled steel product having a carbon content of 400-1200 ppm, in which the hot-rolled strip is cold-rolled to form a plate-shaped steel product, and the plate-shaped cold-rolled steel product is then annealed and recrystallized in an annealing furnace (in particular a continuous annealing furnace), in which a nitrogen-containing gas is introduced into the annealing furnace and sprayed onto the plate-shaped steel product, in order to introduce into the plate-shaped steel product an amount of unbound nitrogen corresponding to a concentration of more than 100 ppm or to increase the amount of unbound nitrogen in the plate-shaped steel product to a concentration of more than 100 ppm. Finally, the annealed and nitrided plate-shaped steel product is cooled immediately after the recrystallization annealing at a cooling rate of more than 100 K / s. Using this method, it is possible to produce plate-shaped cold-rolled steel products for packaging purposes having tensile strengths of more than 650 MPa, in particular between 700 MPa and 850 MPa.

[0005] According to WO 2005 / 056841 a method is known for producing a steel sheet having a nitrogen gradient through the thickness of the sheet with a high nitrogen concentration at the surface and a low nitrogen concentration in the core region, in which nitrogen is introduced during or after annealing of the steel sheet in an annealing furnace in an ammonia gas atmosphere at temperatures between 550° C. and 800° C. after the steel sheet has been fully recrystallized.

[0006] A method for producing high strength steel strip for producing tin steel sheets and other packaging steels by nitriding the steel strip is known from US Pat. No. 3,219,494, in which the coiled steel strip is first nitrided in a bell-type annealing furnace to obtain a nitrogen-rich shell in the steel strip, the nitriding in the bell-type annealing furnace being carried out by an ammonia gas atmosphere, and when the steel strip is heated in an inert gas atmosphere to a temperature above the recrystallization temperature, a uniform distribution of nitrogen introduced near the surface through the thickness of the steel strip is obtained by nitrogen diffusion, so that nitrogen can diffuse from the nitrogen-rich shell through the steel strip towards its core region, resulting in a complete recrystallization of the structure of the steel. Strengths in the range of 439 MPa to 527 MPa have been achieved for steel strips with a thickness of 0.25 mm.

[0007] During the forming of steel sheets in deep drawing for the production of packaging, due to the grain structure of the steel, roughening occurs outside the forming zone, especially in areas with small bending radii, in particular in areas with bending radii smaller than 14 mm. The degree of roughening depends on the grain size of the steel structure. The smaller the average grain size of the steel structure, the lower the degree of roughening. Packaging steels with a low carbon content in the range of 100-1000 ppm (0.01-0.1% by weight) usually have a grain size (average grain size) in the range of 10-30 μm. Due to the (relatively coarse-grained) grain structure of the steel, roughening occurs outside the forming zone during forming, since the grains of the steel structure are extruded radially outwards during forming and can then penetrate the surface of the steel sheet. This is particularly noticeable in cold-rolled steel sheets that are fully recrystallized after cold rolling. Cold-rolled steel for manufacturing packaging is usually fully recrystallized after cold rolling in order to restore the original structure and formability of the steel. However, fully recrystallized steel has a coarse steel structure with a relatively large average grain size and is softer than rolled and quenched steel. The coarsening grain size and reduced strength of the recrystallized steel make it prone to severe roughening during forming, since the coarsening grains of the steel microstructure can be visibly extruded to the surface during forming. Such roughening often causes problems with the stability and corrosion resistance of the packaging (e.g. cans). This is because the roughened area is located on the outside of the packaging (e.g. the edge of the can bottom), which is subject to high mechanical stresses. Summary of the Invention

[0008] The object of the present invention is to disclose a steel sheet for packaging production with high strength and good formability, which does not develop roughening outside the forming area, even in the case of severe forming with small bending radii, especially with bending radii of less than 14 mm. In particular, the steel sheet must have a strength of 500 MPa or more with a breaking elongation of 5% or more in order to meet the mechanical requirements during forming, even for thin steel sheets of less than 0.3 mm. At the same time, the steel sheet must have sufficient formability, for example in deep drawing or stretch forming processes, for the intended use as packaging steel, so that packaging such as tin cans or beverage cans can be produced as intended from the plate-shaped steel products. A further object of the present invention is to provide a method for producing such a steel sheet for packaging.

[0009] These problems are solved by a method having the features of claim 1 and a steel sheet having the features of claim 12. Preferred embodiments of the method and the steel sheet according to the invention are set out in the dependent claims.

[0010] Reference to steel sheet means a flat steel product in the form of plate or strip. Values ​​in % or ppm relating to the content or concentration of alloying elements in the steel or cold rolled steel sheet refer in each case to the weight of the steel or steel sheet. Features of the invention disclosed below with respect to the manufacturing process also relate accordingly to the product of this process (i.e. the steel sheet) and vice versa.

[0011] In the method according to the invention for producing steel sheets for packaging, the carbon content (C) is 10 to 1000 ppm by weight and the recrystallization temperature (T R) (essentially predetermined by the steel composition), a cold-rolled steel sheet having a first side and a second side is provided on its first side with a barrier layer at least substantially impermeable to nitrogen and then preferably heated in a continuous annealing furnace to a heating temperature at least as high as the recrystallization temperature (maximum), the heating being carried out in a nitriding gas atmosphere until at least said recrystallization temperature is reached at least temporarily, whereby during the heating of the steel sheet nitrogen diffuses from the nitriding gas atmosphere into at least a near-surface region of the second side of the steel sheet and precipitates in this region, whereby the recrystallization temperature of the steel in the near-surface region of the second side of the steel sheet is increased by a value ΔT and the heating temperature T E is equal to or higher than the recrystallization temperature on the one hand and the recrystallization temperature (T R +ΔT).

[0012] Heating temperature T E is the maximum temperature in the heat treatment of the cold-rolled steel sheet, i.e., the cold-rolled steel sheet is heated to a (maximum) temperature T E When the cold-rolled steel sheet is heated, nitrogen from the nitriding gas atmosphere is incorporated only in the near-surface region of the second side of the steel sheet due to the diffusion of (atomic) nitrogen from the nitriding gas atmosphere to the near-surface region of the second side of the steel sheet. The opposite, first side of the steel sheet is covered by a barrier layer, which prevents the penetration of nitrogen through the barrier layer. As a result, the recrystallization temperature of the steel increases by a value ΔT only in the near-surface region of the second side of the steel sheet, while the recrystallization temperature of the steel in the region of the first side of the steel sheet remains at least substantially unchanged, i.e. corresponds to the original recrystallization temperature of the steel, which is determined by the steel composition of the cold-rolled steel sheet before heating. Thus, the heating temperature (T E ) is T R ≦T E <T R +ΔT, where T R is the initial recrystallization temperature of the steel.

[0013] As a result, a bilayer crystallization structure is formed in the steel sheet, which comprises a first region on the first side that is at least substantially completely recrystallized and a second region on the second side that is not recrystallized or at most only partially recrystallized. This bilayer structure of the crystallization structure results in the method according to the invention, because the second region (near the surface) of the second side of the steel sheet has a higher recrystallization temperature due to nitriding during heating than the adjacent first region of the first side, which is not nitrided during heating or at most is only slightly nitrided than the second region due to the barrier layer. Because the heating temperature is intermediate between the recrystallization temperature (raised by ΔT) of the second region (near the surface) and the adjacent first region (which is not nitrided and therefore has a recrystallization temperature at least substantially equal to the initial recrystallization temperature of the steel), only the non-nitrided first region recrystallizes during heating, while the nitrided second region (near the surface) does not recrystallize or only incompletely recrystallizes and, as a result, remains roll-hard (from cold rolling).

[0014] The barrier layer on the first side of the steel sheet prevents atomic nitrogen from diffusing through the surface of the steel sheet into the interior. To ensure this, the material forming the barrier layer is suitably heat-resistant, in particular to temperatures above 300° C. and preferably at least up to 600° C., because at these temperatures the steel sheet is nitrided in an annealing furnace and nitrogen atoms from the gas atmosphere of the annealing furnace are precipitated on the hot surface of the steel sheet by catalytic reaction and diffuse into the steel sheet.

[0015] The barrier layer can be formed, for example, by a heat-resistant paint, such as a furnace paint or a silicone resin-based engine paint. To apply the barrier layer, a heat-resistant paint material is applied, for example by spraying, to one side of the first side of the steel sheet before the steel sheet is placed in the annealing furnace. The barrier layer can also be formed by electrolytically depositing a coating on one side of the steel sheet, for example, in particular 80 to 140 mg / m 2 Alternatively, the coating may be formed by a chromium / chromium oxide layer having a chromium coating weight in the range of

[0016] The barrier layer is designed to largely prevent the passage of nitrogen from the nitrogen-containing gas atmosphere of the annealing furnace into the steel sheet, i.e. the ingress of nitrogen through the barrier layer on the first side of the steel sheet is suppressed, apart from unavoidable nitrogen residues which may diffuse into the steel sheet due to, for example, incomplete coverage of the surface of the first side of the steel sheet by the barrier layer or defects of the barrier layer on the first side. Preferably, the barrier layer is formed in such a way that the amount of nitrogen which can penetrate into the first side of the steel sheet is at most 10% of the amount of nitrogen which diffuses to the second side of the steel sheet. Thus, in the method according to the invention, nitrogen diffuses essentially only on the second side of the steel sheet and a gradient of the nitrogen concentration is formed over the entire cross section of the steel sheet, sloping from the second side towards the first side, which means that the steel sheet is heated to a heating temperature (T E ), the increased recrystallization temperature with increasing nitrogen content results in the formation of a bi-layer crystallized structure having an at least substantially recrystallized first region on a first surface and a non-recrystallized or at least not completely recrystallized second region on a second surface.

[0017] The barrier layer is preferably a sol-gel layer, in particular SiO 2 , TiO 2 and / or ZrO 2 Such a sol-gel layer can be produced by the sol-gel method and can be efficiently applied to the steel sheet surface by applying the sol (present as a colloidal dispersion) used as a coating solution to the surface of the first side of the steel sheet, followed by gelling and drying of the wet-chemically formed layer. SiO 2 To prepare the sol-gel layers, in particular silicon alcoholates can be used as precursors. Tetramethyl orthosilicate (TMOS), Tetraethyl orthosilicate (TEOS), or Tetraisopropyl orthosilicate (TPOS) The aqueous solution of ZrO 2 - or TiO 2To produce a sol-gel layer, an aqueous solution of zirconium propylate or titanium(2-propylate) can be applied.

[0018] The sol-gel layer is preferably wet-chemically applied to the surface of the steel strip on the first side in a strip coating process. In this way, the sol-gel method for applying the sol-gel layer to the steel strip surface can be integrated into a continuous strip coating process to achieve efficient process control, in which the steel strip is in strip form and the subsequent nitriding and annealing of the steel strip is performed in a continuous annealing furnace through which the strip passes at a predetermined strip speed. The sol-gel layer is applied in a separate step upstream of the continuous annealing furnace. The gelling and drying of the sol can take place at least partially during the heating of the steel strip in the continuous annealing furnace, thus achieving a highly efficient process and reducing the length of the strip line. The sol-gel method, in particular SiO 2 It has been shown that a dense and uniform barrier layer can be applied to one side of a steel sheet using the sol-gel method for producing the layer, which is why this method is preferred for applying the barrier layer.

[0019] In a particularly preferred embodiment, the silicate-containing barrier layer is electrolytically applied to one of the two surfaces of the steel sheet from a basic aqueous electrolyte containing silica and a sodium salt, and the silicate layer acting as a barrier layer is applied to one of the two surfaces of the steel sheet in an amount of 1 to 10 mg / m 2 Within the range of 3 to 6 mg / m 2 During the electrolytic application of the barrier layer, the strip surface is simultaneously degreased. The electrolytic application of the barrier layer makes it possible to produce a barrier layer that is uniformly distributed over the entire surface of the strip, has a homogeneous and sufficient coating weight, and prevents nitrogen penetration over the entire first side of the strip during the nitriding process in the annealing furnace.

[0020] In order to achieve at least substantially complete recrystallization of the first region by the nitriding process in the annealing furnace, the temperature of the steel sheet is preferably maintained for a predetermined annealing time (t G) throughout the heating temperature (T E ) The annealing time is preferably more than 1 second, in particular in the range of 1 to 80 seconds, preferably in the range of 1 to 10 seconds. Longer annealing times, for example more than 10 seconds, in addition to the complete recrystallization of the first region, result in an equalization of the distribution of nitrogen introduced during heating throughout the thickness of the steel sheet, resulting in a wide transition zone in the core region of the steel sheet between the recrystallized first region and the non- or barely recrystallized second region.

[0021] It is therefore also an object of the present invention to provide a steel sheet, which can in particular be used for the manufacture of packaging, made from a steel with a carbon content (C) of 10-1000 ppm by weight and a thickness of less than 0.5 mm, which has a bilayer crystallization structure with a first region on a first side and a second region on a second side, the first region being at least substantially recrystallized and the second region not recrystallized or at least not completely recrystallized, and in which an at least substantially nitrogen-impermeable barrier layer is arranged on the surface of the first side. Due to the barrier effect of the barrier layer, in the method according to the invention, nitrogen diffuses essentially only on the second side of the steel sheet, and a gradient of nitrogen concentration is formed which slopes from the second side towards the first side over the entire cross section of the steel sheet, which is due to the fact that the steel sheet is heated to a heating temperature (T E ), resulting in the formation of a duplex crystallization structure due to the increase in recrystallization temperature with increasing nitrogen content when the steel sheet is heated to 300° C. The duplex crystallization structure of the steel sheet according to the invention is hereinafter also referred to as duplex microstructure.

[0022] The steel sheet according to the invention has a very high strength of more than 500 MPa, in particular more than 600 MPa, preferably more than 700 MPa, and an elongation (elongation at break) of 5% or more, which is acceptable for deep drawing applications. At the same time, the steel sheet has good formability (especially in deep drawing). The steel sheet is particularly characterized by the fact that even in the case of severe forming with a very small bending radius, no roughening occurs outside the bending radius when the second zone, which maintains its rolling hardness and is not recrystallized, is located outside the bending radius. This is achieved by the fact that, due to the high strength of the second zone of rolling hardness, the coarse grains of the recrystallized first zone cannot be extruded to the surface outside the bending radius. The second zone, which remains rolling hard, therefore forms a barrier against the coarse grains of the recrystallized steel structure of the first zone. The second zone of rolling hardness prevents the coarse grains from the recrystallized first zone from being extruded to the surface of the steel sheet during forming. This prevents undesirable optical effects and mechanical instabilities during forming, and also prevents porosity and cracks in the coating applied to the surface of the second side of the steel sheet.

[0023] Particularly good formability of the steel sheet is obtained if the second zone of rolling hardness is as thin as possible, in particular thinner than the first zone of recrystallization. Preferably, the first zone has a thickness in the range of 50 μm to 450 μm, particularly preferably in the range of 90 μm to 400 μm, in particular in the range of 150 μm to 300 μm, and the thickness of the second zone is preferably in the range of 1 μm to 50 μm, particularly preferably in the range of 2 μm to 10 μm. Preferably, the thickness of the second zone is 1% to 10% of the thickness of the first zone. With such a small thickness of the second zone, which is not or barely recrystallized, the formability of the steel sheet is hardly affected by the high strength of the second zone of rolling hardness. Nevertheless, during forming of the steel sheet, the second zone forms a sufficient barrier against the coarse grains of the steel structure extruding through the surface of the steel sheet, thus preventing roughening of the surface.

[0024] The value ΔT of the increase in the recrystallization temperature of the second region due to the incorporation of nitrogen during heating of the steel sheet can be controlled by the nitrogen content introduced by the nitriding treatment in the second region of the steel sheet after the end of heating, and in particular a linear relationship can be observed which can be described by the following equation: ΔT = a · ΔN (ppm), where a is the proportionality constant and ΔN (ppm) is the nitrogen content in ppm (based on the weight of the steel) introduced in the second zone by the nitriding treatment during heating of the steel sheet. Tests on samples with different nitrogen contents and other same alloy compositions have given values ​​of a ≈ 1.2 K / ppm as an example. Thus, an increase in the recrystallization temperature in the near-surface zone in the range of ΔT ≈ 10 K to 24 K can be achieved already with small additions of ΔN in the range of 10 ppm to 20 ppm (corresponding to 0.001 to 0.002 wt%). At higher nitrogen loadings, for example ΔN = 100 ppm (corresponding to 0.01 wt%), the (theoretically achievable) increase in the recrystallization temperature in the near-surface zone is already about ΔT ≈ 120 K. Preferably, the value ΔT by which the recrystallization temperature of the second region increases due to the introduction of nitrogen during heating of the steel sheet is greater than K, particularly preferably greater than 100K, and particularly within the range of 100K to 250K.

[0025] In the method according to the invention, the steel sheet can be heated either in a single-stage heating process or in a two-stage heat treatment. In the single-stage heating process, the heating time (t E ) from room temperature to heating temperature (T E ) and heat the steel plate to the heating temperature (T E After reaching the specified annealing time (t G ) throughout the heating temperature (T E ) is held for heating time (t E ) is preferably in the range of 1.0 to 300 seconds, and / or the annealing time (t G ) is preferably in the range of 1.0 seconds to 80 seconds, particularly preferably in the range of 1 to 10 seconds. During heating, the steel sheet is at least temporarily exposed to a nitriding gas atmosphere, particularly an ammonia-containing gas atmosphere having an ammonia volume fraction in the range of 0.1 to 6%.

[0026] In the two-stage heating process, the nitriding treatment is performed at an intermediate temperature in the first stage, and the annealing is performed at a heating temperature higher than the intermediate temperature in the second stage (for this reason, the heating temperature below is also called the annealing temperature). The intermediate temperature is the original recrystallization temperature T R In the two-stage process, the steel sheet is heated from room temperature to an intermediate temperature T Z <T R is heated to t H The intermediate temperature T Z is preferably in the range of 300°C to 600°C, particularly preferably in the range of 400°C to 550°C. The reason for this is that, if ammonia gas is used as the nitriding component of the gas atmosphere of the annealing furnace, dissociation into atomic nitrogen on the metal surface begins at a temperature of about 300°C. In any case, at temperatures below about 550°C, (complete) recrystallization does not yet occur in the majority of the alloy composition according to the invention. Therefore, the preferred intermediate temperature T Z In this case, the diffusion of dissociated nitrogen from the nitriding gas atmosphere into the second region of the steel sheet occurs, but recrystallization does not yet occur. Recrystallization of the first region occurs at the original recrystallization temperature T R That's all, but R +ΔT is less than the heating temperature (annealing temperature) T E For example, the plate is heated to a temperature T E is the initial recrystallization temperature T of the steel used R Depending on the value of , it is in the range of 650°C to 800°C, in particular about 750°C.

[0027] As in the case of the single-stage heating of the steel sheet in the first embodiment, the two-stage process at least substantially results in only a (partial) recrystallization of the first region of the steel sheet, but not of the second region. The recrystallization of the second region, which was nitrided in the first stage, occurs at a recrystallization temperature T R Heating temperature (annealing temperature) T below +ΔT E This is prevented by selecting

[0028] In the two-stage heat treatment, the steel sheet is first heated in a continuous annealing furnace to the (initial) recrystallization temperature T R A relatively low intermediate temperature T Z In the first stage, the second region near the surface of the second side of the steel sheet is appropriately annealed for a holding time preferably in the range of 10 to 150 seconds, and in the second stage, the annealing time t is preferably in the range of 1 to 300 seconds, particularly preferably in the range of 1 to 10 seconds. G During this time, the temperature must be higher than the intermediate temperature and above the (initial) recrystallization temperature (T R ) above the heating temperature (annealing temperature T E ) is at least partially recrystallized only in the first region.

[0029] The first heating time (t E 1 The holding time (t) for holding the steel sheet at the intermediate temperature is preferably in the range of 1.0 to 120 seconds, particularly preferably in the range of 10 to 90 seconds, and can be adapted according to the desired material properties of the steel sheet according to the present invention, as in the first embodiment. H ) is also preferably in the range of 1.0 to 90 seconds, particularly preferably in the range of 10 to 60 seconds, and is likewise selected depending on the desired material properties of the steel sheet according to the invention. After the holding time has elapsed, the second heating time (t E 2 ), the steel plate is heated to a temperature T E (annealing temperature) and anneal for annealing time (t G ) at least approximately at this heating temperature T E Optionally, the annealing furnace can also be supplied with a nitriding gas atmosphere during the annealing period, so that dissociated (atomic) nitrogen is available and the (further) nitriding of the sheet occurs in the deeper second zone during the annealing period t G This leads to an increase in the dimension of the second region of the steel plate in the direction of the first surface, thus increasing the thickness of the second region. E (annealing temperature) is also the original recrystallization temperature T R The nitriding treatment of the steel sheet surface area results in TR +ΔT. Therefore, in the two-stage process, the heating temperature T E :T≦T RE <T R +ΔT also holds, and the intermediate temperature (T Z ) is the initial recrystallization temperature T R Lower than.

[0030] In both the single-stage and two-stage processes, the steel sheet is at least briefly exposed during heating and before reaching the recrystallization temperature to a nitriding gas atmosphere that supplies dissociated (atomic) nitrogen into the annealing furnace, the dissociated (atomic) nitrogen initially diffusing into the steel sheet near the surface only in a second region of the second side of the steel sheet, whereby the recrystallization temperature is increased, while the ingress of nitrogen through the barrier layer is prevented on the first side of the steel sheet.

[0031] The steel of the cold-rolled steel sheet preferably has the following composition by weight: Carbon, C: more than 0.001% and less than 0.1%, preferably less than 0.06%; Manganese, Mn: more than 0.01% and less than 0.6%; Phosphorus, P: less than 0.04%; Sulfur, S: less than 0.04% and preferably more than 0.001%; Aluminum, Al: less than 0.08%; Silicon, Si: less than 0.1%; · Optional Copper, Cu: less than 0.1%; Optional Chromium, Cr: less than 0.1%; Optional Nickel, Ni: less than 0.1%; · optional titanium, Ti: less than 0.1% and preferably more than 0.02%; optional niobium, Nb: less than 0.08% and preferably more than 0.01%; Optional Molybdenum, Mo: less than 0.08%; Optional Tin, Sn: less than 0.05%; optional boron, B: less than 0.01%, preferably less than 0.005% and preferably more than 0.0005%; Optional Nitrogen, N 0 : less than 0.02%, in particular less than 0.016% and preferably more than 0.001%; -Remaining iron and unavoidable impurities, Here, the average nitrogen weight content (N) averaged over the entire thickness of the cold-rolled steel sheet after heating in a nitriding gas atmosphere is 0.01% or more, and preferably 0.015% or more.

[0032] When referring to the average nitrogen content (N) or average nitrogen content, it means the nitrogen concentration averaged over the entire thickness of the respective sheet. Thus, when referring to the average nitrogen content (N) of a steel sheet, it means the nitrogen concentration averaged over the entire thickness of the steel sheet.

[0033] The steel of the cold-rolled steel sheet preferably has an initial nitrogen content N of more than 0.001% by weight and less than 0.02% by weight, particularly preferably less than 0.016% by weight. 0 However, steels containing no nitrogen (apart from unavoidable nitrogen impurities) may be used. Limiting the initial nitrogen content to a value below 0.02% by weight makes it possible to reasonably cold roll the hot strip produced from the steel by hot rolling using conventional cold rolling equipment (rolling mills for cold rolling steel sheets into ultrafine grained steel sheets). Furthermore, if the initial nitrogen content in the steel is N 0 A low content of <0.02% by weight prevents the formation of defects when casting the slabs. However, in order to achieve the highest possible (average) nitrogen content in the cold-rolled steel and thus a high solid-solution strengthening, it is advantageous if the steel used for producing the hot strip already has an (initial) nitrogen content which is preferably in the range of 0.001% to 0.02% by weight, particularly preferably 0.005% to 0.016% by weight.

[0034] The initial nitrogen content of the cold-rolled steel sheet (N 0 ), when the cold-rolled steel sheet is heated in a second region of the second surface of the steel sheet, the nitrogen content is increased to the initial nitrogen content (N 0), whereby the nitrogen content by weight in the second region, averaged over the thickness of this region, is preferably increased to a value greater than the initial nitrogen content of the steel (N 0 If the nitrogen content is increased to values ​​of more than 50 ppm, particularly preferably 400-800 ppm higher than the first zone, then, depending on the thickness of the second zone, a (sometimes considerable) increase in the strength of the steel sheet is observed. Steel sheets with strengths of more than 700 MPa with elongations at break of 5% or more can be achieved. The (average) nitrogen content of the nitrogen precipitated in the second zone by the nitriding process can reach the solubility limit of nitrogen in iron of about 1000 ppm.

[0035] Depending on the process parameters during annealing of the steel sheet at the heating temperature (annealing temperature), in particular the setting of the holding time and annealing time, as well as the (optional) concentration of the nitriding gas (in particular ammonia) in the gas atmosphere of the annealing furnace, the first region of the steel sheet is also nitrided to some extent. However, it is preferred to (significantly) reduce the nitriding of the first region in order to obtain the greatest possible difference in the degree of recrystallization between the first and second regions after annealing or at the end of heating. The degree of recrystallization of the second region is preferably less than 30%, more preferably less than 20%, and the degree of recrystallization of the first region is more than 70%, more preferably more than 80%. It is particularly preferred that the first region is fully recrystallized.

[0036] In a preferred embodiment, the steel from which the steel sheet according to the invention is produced in a preliminary stage by hot rolling followed by cold rolling contains, by weight, C >0.001% and <0.1%, Mn >0.01% and <0.6%, P <0.04%, S <0.04%, Al <0.08%, Si <0.1% and optionally an initial nitrogen content (N 0 ) at most 0.020%, and preferably at most 0.016%, the balance being iron and unavoidable impurities. After nitriding, the steel sheet preferably has an average nitrogen content N>N 0The steel sheet contains 0.020% or more, particularly preferably 0.025% or more, and particularly preferably 0.040 to 0.080% N. The tensile strength of a steel sheet having an average nitrogen content of N>0.040% is 800 MPa or more, and at the same time, the breaking elongation of this steel sheet is in the range of 2% to 10%, so that the steel sheet exhibits sufficient formability for deep drawing.

[0037] The nitrogen introduced into the second region during heating of the cold-rolled steel sheet can be present in dissolved form and / or in bound form as nitrides (below the solubility limit). If strong nitride formers are present in the steel, the inserted nitrogen is present at least partially as bound nitrogen in nitrides, in particular as TiN and / or NbN and / or AlN. Since the interstitial penetration of nitrogen introduced into the second region during the nitriding treatment is favorable for increasing strength, it is advantageous for the steel to contain as few nitride formers as possible, such as Ti, Nb, Mo or Al, when obtaining high strength steel sheets. The following upper limits for the weight percentage of nitride formers are therefore preferred: Al: Less than 0.08% Si: · Ti: less than 0.1% and preferably more than 0.02%; Nb: less than 0.08% and preferably more than 0.01%; · Mo: less than 0.08%; · B: less than 0.01%, preferably less than 0.005%;

[0038] On the other hand, the formation of nitrides during the nitriding of the second region promotes a clear boundary between the recrystallized first region of the steel sheet and the second region that is not recrystallized or at least not completely recrystallized. Therefore, if the greatest possible difference in the degree of recrystallization between the first and second regions is desired, strong nitride formers such as Ti, Nb, Mo and / or Al are added to the steel in sufficient amounts. In this connection, the steel of the cold-rolled steel sheet preferably contains, by weight, more than 200 ppm titanium and / or more than 100 ppm niobium and / or more than 0.0005% boron and / or more than 50 ppm aluminum. Particularly preferably, the sum of the strong nitride formers in this case by weight fraction is more than 300 ppm, preferably more than 500 ppm. Strong nitride formers such as titanium, niobium and / or aluminum bind the nitrogen precipitated in the first region and thus prevent the nitrogen initially precipitated only near the surface from diffusing further into the interior of the steel sheet towards the first face. Thus, a first zone is created at the surface of the steel sheet, which has a high nitrogen content and is very thin compared to the thickness of the steel sheet, leading to a significant increase in the recrystallization temperature of this zone. According to the method according to the invention, if the cold-rolled steel sheet is now heated to a temperature on the one hand higher than the (initial) recrystallization temperature of the steel in the (undoped or slightly doped) second zone of the steel sheet and on the other hand lower than the (increased) recrystallization temperature of the nitrided zone, only the first zone recrystallizes (fully) and the second zone retains its rolling hardness due to the increased recrystallization temperature. This leads to a biphasic crystallization of the microstructure of the steel sheet according to the invention, with a clear boundary between the first zone and the second zone.

[0039] Depending on the concentration of nitrogen in the nitrogen donor, a surface nitride layer, especially an iron nitride layer, can also be formed on the free surface of the second zone. This surface nitride layer is brittle and may peel off during forming, which is disadvantageous from the point of view of roughening during forming of the steel sheet. The formation of the surface nitride layer essentially depends on the concentration of nitrogen in the nitriding gas atmosphere of the annealing furnace. For example, when using a gas atmosphere containing ammonia as the nitrogen donor, the formation of a nitride layer on the surface of the first zone can be observed on a laboratory scale from an ammonia content of about 2-3% by volume. The nitride layer is very thin, its thickness being in the range of about 10 μm or less. In order to avoid a nitride layer on the surface of the second zone, the ammonia concentration in the gas atmosphere is preferably 3% by volume or less. The volume fraction of ammonia in the gas atmosphere refers to the state in a laboratory test where the steel sheet was heated by an induction heater, and the volume fraction of ammonia in the gas atmosphere of the experimental furnace was determined at room temperature.

[0040] The formation of a duplex microstructure associated with the crystallinity of the first and second regions of the steel sheet can be influenced in particular by the heating time and the annealing time. Preferably, the cold-rolled steel sheet is heated from room temperature to a heating temperature (T E ) (if necessary, stepwise with intervening holding periods during which the temperature is kept constant) for an annealing time (t G ) is held at the heating temperature throughout the entire time. The short heating time and the short annealing time contribute to a stronger formation of a nitrogen gradient from the second side to the first side of the steel sheet. The reason for this is that with the short heating time and the short annealing time, the nitrogen that is initially precipitated only on the surface of the second region of the steel sheet cannot diffuse to the core region. With the extended annealing time, the diffusion of nitrogen from the second region near the surface to the core region can be observed, so that the core region of the steel sheet is also at least slightly nitrided.

[0041] Thus, the thickness of the non-recrystallized second region can be controlled by the heating time, whereby a linear correlation can be observed between the thickness of the second region and the heating time. Thus, an adjustable process parameter of the method according to the invention is available via the heating time, whereby the thickness of the non-recrystallized and thus the rolling hardness second region can be specifically adjusted. Depending on the selected heating time, the thickness of the second region can be set to 0.1 μm to 150 μm, whereby the thickness of the second region should be as thin as possible, preferably 1 μm to 10 μm, in particular 1 μm to 2 μm. The barrier layer on the surface of the first region has a thin thickness, preferably less than 1 μm, in particular less than 0.1 μm, or less than 10 mg / m 2 The barrier layer has a weight support of less than 100° C., particularly preferably less than the second region. The thickness of the barrier layer is sufficiently thick to at least substantially completely prevent diffusion of nitrogen onto the first side of the steel sheet, particularly at temperatures above 300° C., in particular at temperatures between 300° C. and 600° C. At the same time, the barrier layer does not affect, or at least does not affect significantly, the mechanical properties of the steel sheet due to its low density.

[0042] When the cold-rolled steel sheet is heated in the nitriding gas atmosphere, a nitrogen content gradient is formed in the second region, where the nitrogen content gradually decreases from the second side to the first side of the cold-rolled steel sheet. The amount of nitrogen incorporated in the second region can be controlled by the nitrogen concentration of the nitriding gas atmosphere, in particular by the volume fraction of ammonia in the gas atmosphere of the annealing furnace.

[0043] Preferably, the steel sheet is heated in a continuous annealing furnace with a nitrogen-containing gas atmosphere through which the steel sheet passes. Conveniently, the steel sheet is in the form of a strip. The nitrogen-containing gas atmosphere can be provided by introducing, in particular, ammonia gas into the annealing furnace, so that during heating, ammonia molecules are thermally dissociated into atomic nitrogen by catalytic reaction on the heated surface of the second region of the steel sheet and diffuse through the surface of the second region into the steel sheet. At the first side of the steel sheet, this diffusion process is at least inhibited or preferably completely suppressed by a barrier layer, so that during heating, no or only little nitrogen can diffuse into the steel sheet there. The volume concentration of ammonia in the nitrogen-containing gas atmosphere is preferably more than 0.1%, in particular 0.1% to 10%, more preferably 0.1% to 5%, in particular 0.5% to 3%. Particularly preferably, the cold-rolled steel sheet is heated in an inert protective gas atmosphere, in particular containing HNx, the volume concentration of HNx in the nitrogen-containing gas atmosphere being preferably 90% to 99.5%.

[0044] Thus, with the method according to the invention, a steel sheet can be produced from a steel with a carbon content (C) of 10-1000 ppm by weight and a thickness of less than 0.5 mm, the steel sheet having a bilayer crystallization structure with a first region on a first side of the steel sheet and a second region on a second side of the steel sheet, the first region being at least substantially recrystallized and the second region not recrystallized or at least not completely recrystallized, and an at least substantially nitrogen-impermeable barrier layer (as a result of the production method) present on the surface of the first side. A gradient of nitrogen content is present at least in the second region of the steel sheet, the nitrogen content decreasing from the surface of the second side towards the first side.

[0045] Thus, the hardness of the second region of the steel plate is significantly greater than that of the first region. Preferably, the Vickers hardness of the second region is greater than 220 HV 0.025 More than 300HV, especially preferred 0.025 Preferably, the first region has a Vickers hardness of 100 HV or more. 0.025 Above 280HV 0.025Preferably, the ratio of the hardness of the second region to the hardness of the first region is greater than 1.2, particularly preferably greater than 1.4.

[0046] When the weight-average nitrogen content in the second region of the steel plate after nitriding is 400 to 800 ppm, particularly high strength and hardness values ​​can be obtained.

[0047] The two regions of the bilayer microstructure differ from each other not only in terms of their hardness or strength, but also in terms of their texture. For example, a first region, which is at least substantially recrystallized, and a second region, which is little or not recrystallized, can be distinguished by the ratio of {001} to {111} orientations in the ε fibers. The ratio of {001} to {111} orientations in the ε fibers can be defined as a "deformation index" that characterizes the forming behavior of the steel sheet. The {111} orientation allows good formability and has a good Lankford value (r-value), while the {001} orientation is poor. Here, the ε fibers are characterized by the presence of tensile strains parallel to the transverse direction (perpendicular to the rolling direction of the strip and the normal direction to the strip surface). <110> In the steel sheet according to the invention, in each case the recrystallized first zone has a deformation index of less than 0.8 and the second zone has a deformation index of more than 2.0, in particular between 2.0 and 5.0. The corresponding characterization of the texture of the first and second zones is similar to that of other fibers of the microstructure, e.g. in the rolling direction. <110> We can also define alpha fibers that are defined by vectors.

[0048] An advantageously clear boundary between the first and second regions is obtained if the (re)crystallinity of the steel sheet in the second region is less than 30%, preferably less than 20%, and / or if the (re)crystallinity of the first region is more than 70%, preferably more than 80%. E ) to T E =T R If +ΔT / 2 is applied, a particularly sharp boundary between the two regions can be obtained. E is T R +ΔT / 3~TR Within the range of +2ΔT / 3.

[0049] The steel sheets produced by the method according to the invention can be advantageously used for the production of packaging, by which the steel sheets can be formed, for example, into the body of a can, in a forming process. In some cases, the steel sheets are subjected to intensive forming with very small bending radii of less than 14 mm. The steel sheets according to the invention are characterized by the fact that hardly any roughening of the surface occurs outside the bending radius during forming, in particular when the second zone, which remains at rolling hardness, is outside the bending radius. The roughening occurring during forming can be detected, for example, by a four-radius cup test, in which a steel sheet test piece is deep-drawn to form a rectangular parallelepiped container with different bending radii at the four corners of the rectangular parallelepiped, and then the roughness outside the bending radius of the container is measured. In the steel sheets according to the invention, the roughness (Ra) of the outer surface of the second zone after forming the steel sheet with bending radii in the range of 8 mm to 14 mm is preferably less than 1.0 μm, particularly preferably less than 0.8 μm, and / or has a roughness factor of less than 3, preferably less than 2.5. The roughness factor is defined as the ratio of the surface roughness of the second area outside the 90° angle to the roughness of the steel plate in the non-deformed part of the container formed from the steel plate.

[0050] Thus, in addition to the manufacturing method and the steel sheet manufactured thereby, the subject of the invention is also a container having at least one convexly formed part manufactured from the steel sheet, whereby the second area of ​​the steel sheet according to the invention is located outside the convexity of the formed part. In particular, the container may be a can having a can base and a body formed thereon, the transition between the can base and the body forming a formed part.

[0051] These and other advantages of the packaging steel and manufacturing method according to the present invention are the result of the embodiments described in more detail below with reference to the accompanying drawings. [Brief description of the drawings]

[0052] [Figure 1]FIG. 2 is a schematic representation in the form of a temperature-time diagram of one embodiment of the heating step of the method according to the invention. [Diagram 2] 1 is a schematic diagram of a cross section of a steel sheet having a dual phase microstructure according to the present invention. [Diagram 3] 1 is a micrograph (metallographic cross-section) of a cross section of a steel sheet having a dual-layer microstructure according to the present invention. [Figure 4] 1 is a plot of the variation of Vickers hardness (HV0.025) versus thickness in the cross section of the steel plate, measured on different samples of the steel plate according to the invention, heated and nitrided for different heating times (tE) in the method according to the invention. [Diagram 5] FIG. 1 is a diagram showing a comparison of stress-strain curves [σ(ε)] of steel sheets according to the present invention heated and nitrided for different heating times (tE). [Figure 6] FIG. 1 is a schematic diagram of the four-radius cup test. [Figure 6a] 1 shows a top view of the bottom of the container manufactured in this test from a steel plate according to the invention, with different bending radii at the corners of the container. [Figure 6b] FIG. 2 is a cross-sectional view of a side view of a container. [Figure 7] FIG. 7 represents the results of the four-radius cup test of FIG. 6 carried out on test specimens of steel plate according to the invention; [Figure 7a] FIG. 6b shows the outer roughness (Ra in μm) of the bending radii (R1-R4) at different positions (P0-P4) from FIG. 6b. [Figure 7b] FIG. 1 shows the roughness coefficients (Ra coefficient=Ra / R0, where R0 is the roughness of the steel plate in the non-deformed portion of the vessel) at these positions (P0 to P4).

[0053] Steel sheets having a carbon content of 10-1000 ppm by weight and cold rolled after hot rolling are used as starting products for the production of steel sheets according to the invention. The alloy composition of the steel expediently complies with the limits specified by the standards for packaged steels (for example as defined in ASTM A623-11 "Standard Specification for Tin-Drawn Products" or "European Standard EN10202"), but may deviate from these, especially with regard to the initial nitrogen content, in particular when highly nitrided steel sheets with a high nitrogen content of more than 0.02% by weight are produced. The components of the steels from which the steel sheets according to the invention can be produced are described in detail below.

[0054] Steel composition: Carbon, C: more than 0.001% and less than 0.1%, preferably less than 0.06%; Carbon has the effect of increasing hardness and strength. The steel therefore preferably contains more than 0.001% by weight of carbon. In order to ensure the rollability of the steel sheet during the first cold rolling step and, if necessary, during the second cold rolling step (skin pass rolling), without reducing the elongation at break, the carbon content should not exceed 0.1% by weight.

[0055] Manganese, Mn: more than 0.01% and less than 0.6%; Manganese also has the effect of increasing hardness and strength. Manganese also improves the forgeability, weldability and wear resistance of the steel. In addition, the addition of manganese reduces the tendency of red fracture during hot rolling, and manganese also leads to grain refinement. Therefore, a manganese content of 0.01% by weight or more is preferred. To obtain high strength, a manganese content of more than 0.1% by weight, in particular 0.20% by weight or more, is preferred. However, if the manganese content becomes too high, the corrosion resistance of the steel is impaired. Furthermore, if the manganese content becomes too high, the strength becomes too great and the steel can no longer be cold rolled or formed. Therefore, an upper limit of 0.6% by weight of the manganese content is preferred.

[0056] Phosphorus, P: less than 0.04%. Phosphorus is an undesirable by-product in steel. High phosphorus contents, in particular, lead to embrittlement of the steel and therefore to reduced formability of the steel sheet. For this reason, the upper limit for phosphorus content is 0.04% by weight.

[0057] Sulfur, S: less than 0.04% and preferably more than 0.001%. Sulfur is an undesirable accessory element that reduces ductility and corrosion resistance. Therefore, the sulfur present in the steel should not exceed 0.04% by weight. On the other hand, sulfur contents below 0.001% by weight are no longer justified from an economic point of view, since complex and expensive measures must be taken to desulfurize the steel. Therefore, a sulfur content in the range of 0.001% to 0.04% by weight is preferred, particularly preferably in the range of 0.005% to 0.01% by weight.

[0058] Aluminum, Al: Less than 0.08% In the production of steel, aluminum acts as a deoxidizer in the casting process and sediments the steel. Aluminum also enhances the resistance to scaling and formability. Furthermore, aluminum forms nitrides together with nitrogen, which is advantageous in the steel sheets according to the invention. Aluminum is therefore preferably used in concentrations of 0.005% by weight or more. On the other hand, aluminum concentrations above 0.08% by weight can lead to surface defects in the form of aluminum clusters, and therefore the aluminum content is preferably not above this upper limit.

[0059] Silicon, Si: less than 0.1%; Silicon in steel increases the resistance to scaling. Silicon is also a solid solution hardener. In steelmaking, silicon has the positive effect of diluting the melt and acts as a deoxidizer. Another positive effect of silicon on steel is to increase the tensile strength, yield strength and resistance to scaling. Therefore, a silicon content of 0.003 wt.% or more is preferred. However, if the silicon content becomes too high, especially if it exceeds 0.1 wt.%, the corrosion resistance of the steel may decrease and surface treatment, especially by electrolytic coating, may become more difficult.

[0060] Optional Nitrogen, N 0 : less than 0.02%, in particular less than 0.016% and preferably more than 0.001%. Nitrogen is an optional component in the molten steel from which the steel for the steel sheet according to the invention is produced. It certainly acts as a solid solution strengthener, increasing hardness and strength. However, a nitrogen content in the molten steel of more than 0.02% by weight means that the hot strip produced from the molten steel can no longer be cold rolled. Furthermore, a high nitrogen content in the molten steel increases the risk of defects in the hot rolled strip. The reason for this is that at nitrogen concentrations of 0.016% by weight and above, the hot formability is reduced. According to the invention, it is envisaged to subsequently increase the nitrogen content of the steel sheet by subjecting the cold rolled steel sheet to a nitriding treatment in an annealing furnace. The introduction of nitrogen into the molten steel can thus be completely dispensed with. However, in order to achieve a strong solid solution strengthening, it is preferred that the molten steel already contains an initial nitrogen content of more than 0.001% by weight, particularly preferably 0.010% by weight or more.

[0061] Optional: nitride formers, especially niobium, titanium, zirconium, vanadium: Nitride-forming elements such as aluminum, titanium, niobium, zirconium or vanadium are optionally advantageous in the steel of the steel plate according to the invention, at least in part, in binding the nitrogen initially contained in the steel and the nitrogen introduced in the form of nitrides by the subsequent nitriding process in the annealing furnace. This improves the forming behavior and makes it possible to produce IF (Interstitial Free) steel plates that are substantially free of aging. Aluminum, titanium and / or niobium are particularly preferred as steel components, because, in addition to their properties as strong nitride-forming agents, they also act as trace elements, increasing the strength by grain refinement without reducing the toughness.

[0062] Thus, the steel may optionally comprise, by weight: Titanium, Ti: preferably more than 0.02%, particularly preferably more than 0.02% and less than 0.1%, and / or Niobium, Nb: preferably more than 0.01% and less than 0.08%, and / or Aluminum, Al: preferably more than 0.005% by weight and less than 0.08% by weight, and / or Molybdenum, Mo: less than 0.08%; It is preferred that the compound contains

[0063] Other optional ingredients: In order to (if necessary) give the steel further advantageous properties which can be obtained by the following additional elements, the steel contains, in addition to the balance iron (Fe) and unavoidable impurities: · Optional Copper, Cu: less than 0.1%; Optional Chromium, Cr: less than 0.1%; Optional Nickel, Ni: less than 0.1%; Optional Tin, Sn: less than 0.05%; optional boron, B: less than 0.01%, preferably less than 0.005% and preferably more than 0.0005%; It may also contain other optional ingredients such as:

[0064] Table 1 shows embodiments of steel compositions A, B and C from which steel sheets can be produced by hot rolling and cold rolling. These steel compositions can be processed in the method according to the invention to produce a duplex crystallization structure in cold rolled steel sheets.

[0065] Steel plate manufacturing method: The steel composition described is used to produce a molten steel, whereby in an example of a preferred embodiment, in order to achieve a high (average) nitrogen content in the steel sheet, the steel is preliminarily adjusted to an initial nitrogen content N by adding nitrogen to the molten steel, for example by blowing in nitrogen gas and / or by adding solid nitrogen compounds such as calcium cyanamide or manganese nitride. 0In order to prevent the strength of the steel plate produced from the molten steel from becoming too high due to nitrogen solid solution strengthening, and to maintain the hot formability of the steel, as well as to avoid defects caused by nitrides in the slabs produced from the molten steel, the initial nitrogen content of the steel (N 0 ) advantageously does not exceed 0.02% by weight and preferably does not exceed 0.016% by weight.

[0066] First, a slab is cast from molten steel, then hot rolled and cooled to room temperature. The hot strip thus produced has a thickness in the range of 1-4 mm and is wound into a coil at a predetermined coiling temperature in the range of 500-750°C, preferably 650°C-750°C. The hot strip is then wound into a coil at the predetermined coiling temperature. To produce packaged steel in the form of thin steel sheets with a normal thickness of less than 0.5 mm, preferably less than 0.3 mm, the hot strip is cold rolled, with a thickness reduction in the range of 50% to more than 90%.

[0067] Then, a silicate or sol-gel layer, in particular SiO 2 , which is at least substantially impermeable to (atomic) nitrogen, is applied. 2 , TiO 2 and / or ZrO 2 is applied to the surface of one of the two sides of a cold-rolled steel strip to a thickness of less than 0.5 mm. In the coil coating process, for example, a dispersion of silicon alcoholate is applied to the surface of the first side (a) of the steel strip. For this purpose, the dispersion is sprayed as a sol on the first side of the steel strip in a wet-chemical coating process using a spray nozzle or applied with a doctor blade and then dried. In this process, molecular chains are first formed and, after a longer time, microparticles are formed. In a further process, the particles form a network in the sol. In the wet-chemically applied sol layer, a gel state then occurs due to hydrolysis and condensation reactions. The gelling can be accelerated by applying heat.

[0068] For gelation and drying, the sol-coated steel strip is placed in a furnace. Drying of the sol can advantageously be carried out at least partially in a continuous annealing furnace, in which the steel strip is subsequently heat-treated for nitriding and partial recrystallization thereof. For this purpose, the cold-rolled steel strip provided on the first side with a barrier layer is passed through a continuous annealing furnace, in which the steel is heated to the (initial) recrystallization temperature T R The steel strip is heated to a temperature exceeding

[0069] In a particularly preferred embodiment, the silicate-containing barrier layer is electrolytically coated onto one of the two sides of the steel sheet from an aqueous electrolyte. For this purpose, a basic aqueous electrolyte solution containing silica and a sodium salt is added to an electrolyte tank and the steel sheet is passed through the electrolyte tank as the cathode at a given stripping speed. Table 2 shows the preferred composition of the electrolyte solution and Table 3 shows the preferred parameters of the electrolytic coating process. The silicate layer acting as a barrier layer is applied to one of the two sides of the steel sheet at a concentration of 1-10 mg / m2. 2 Within the range of 3 to 6 mg / m 2 Apply electrolyte to one side of steel sheet within the range of

[0070] In the method according to the invention, after the barrier layer has been applied, the cold-rolled steel sheet is nitrided by heating it in a nitriding gas atmosphere in a continuous annealing furnace before or, preferably, simultaneously with the recrystallization annealing. The nitriding is preferably carried out so that the steel sheet is heated to the (initial) recrystallization temperature T R While being heated to a higher temperature, a nitrogen-containing gas, preferably ammonia (NH 3 ) into the annealing furnace, simultaneously with the recrystallization annealing in the annealing furnace. When ammonia is used as the nitrogen-containing gas, preferably at temperatures in the annealing furnace above 300° C., atomic nitrogen is formed by dissociation of nitrogen from the nitrogen-containing gas by a catalytic reaction, which atomic nitrogen can diffuse (interstitially) into the steel sheet on the second side of the steel sheet at the surface of the steel sheet. On the first side of the steel sheet, the diffusion of nitrogen is prevented by a barrier layer.

[0071] In order to prevent oxidation of the second side of the steel sheet surface during heating, it is advantageous to use an inert gas atmosphere in the annealing furnace. Preferably, the atmosphere in the annealing furnace consists of a mixture of a nitrogen-containing gas acting as a nitrogen donor and an inert gas such as HNx, the volume fraction of the inert gas being preferably 90% to 99.5%, and the remaining volume fraction of the gas atmosphere being a nitrogen-containing gas, in particular ammonia gas (NH 3 It is formed by the reaction of gas.

[0072] FIG. 1 shows a schematic temperature-time profile of the heat treatment for nitriding and annealing a steel sheet in an annealing furnace in a preferred embodiment example of the method according to the invention. In this first embodiment example, the single-stage heat treatment of the steel sheet is carried out in a continuous annealing furnace, and during the single-stage heating, the steel sheet is simultaneously subjected to a recrystallization annealing and a nitriding treatment. As shown in FIG. 1, in this embodiment, the steel sheet is heated at a preferred (average) heating rate of 10-15° C. / s for a heating time (t E ) from room temperature to heating temperature T E ≧T R The annealing time (t G The heating temperature T E corresponds to the annealing temperature at which the steel sheet is annealed and recrystallized (in a particular region), and the initial recrystallization temperature T R and T due to nitriding in the near-surface area of ​​the steel plate. R +ΔT. Here, the heating temperature T E :T≦T RE <T R +ΔT holds true.

[0073] Heating time (t E ) is preferably in the range of 1.0 to 300 seconds, particularly preferably in the range of 10 to 120 seconds, and can be adjusted according to the desired material properties of the steel sheet according to the invention, as will be further explained below. To adjust the heating time, the heating rate at which the steel sheet is heated in the annealing furnace or the speed at which it is passed through the continuous annealing furnace can be adjusted according to the desired heating time. The preferred heating time (t EIn order to set the annealing time (t) in the range of 1.0 to 300 seconds, for example, a heating rate of 10 K / s to 80 K / s can be selected. During the heating time, the steel sheet in the continuous annealing furnace is exposed to a nitriding gas atmosphere, particularly an ammonia gas atmosphere. G The annealing time (t) is preferably in the range of 1.0 to 90 seconds, particularly preferably in the range of 10 to 60 seconds, and is selected according to the desired material properties of the steel sheet according to the present invention. G After this time, the steel sheet is removed from the annealing furnace and cooled either passively in the environment or actively, for example by water or gas flow cooling, to room temperature. Suitable cooling rates are in the range of 3 K / s to 20 K / s for gas flow cooling and above 1000 K / s for water cooling.

[0074] (initial) recrystallization temperature T of steel R Depends on the composition of the steel and is generally in the range of 550 to 720°C.

[0075] When the cold-rolled steel sheet is heated in an annealing furnace, nitrogen from the nitrogen-containing gas is initially precipitated only in the near-surface region of the second side of the steel sheet as atomic nitrogen diffuses through the steel sheet surface. Nitrogen that diffuses into the near-surface region is either incorporated interstitially between the iron lattices of the steel or is bonded as nitrides, especially if strong nitride formers such as Al, Nb, Ti or B are present in the steel. The incorporation of nitrogen increases the recrystallization temperature (T R ) increases by a value ΔT. The recrystallization temperature (T R This increase in is shown in Figure 1 as ΔT.

[0076] According to the present invention, the heating temperature (T E ) or the annealing temperature is T≦T RE <T R +ΔT is selected to be applied. Therefore, the heating temperature (T E ) or the annealing temperature is determined in the process according to the invention based on the (initial) recrystallization temperature (T R) and the recrystallization temperature (T R +ΔT) is set to be halfway between the heating temperature (T E By setting the heating temperature (T) (or annealing temperature) in this way, recrystallization occurs only in a first region on the first side of the steel sheet, adjacent to the inside of the second region near the surface, and in which no nitrogen is (yet) incorporated, at least initially, during the annealing and simultaneous nitriding treatment of the steel sheet. The reason for this is that only in this first region of the steel sheet, the heating temperature (T E ) is the recrystallization temperature (T R ) higher than the heating temperature (T E ) is T R +ΔT below the increased recrystallization temperature. Thus, a biphasic microstructure is formed across the cross section of the steel sheet, having at least essentially, preferably nearly completely recrystallized first regions 1 and second regions 2, which are not recrystallized or at least not completely recrystallized.

[0077] The microstructure resulting from heating the steel sheet in a nitrogen-containing gas atmosphere thus comprises at least essentially fully recrystallized first regions 1 and non-recrystallized second regions 2, as shown in the schematic cross-section of a steel sheet according to the invention in FIG. 2. The second regions 2, located on the second side b of the steel sheet, are not recrystallized, or at least not fully recrystallized, and thus retain the as-rolled state of the cold-rolled steel sheet. In contrast, the first regions 1, located on the first side a of the steel sheet, are (in particular fully) recrystallized. The barrier layer 3 shown in FIG. 2 is located on the first side a of the steel sheet.

[0078] The degree of recrystallization of the second region 2 and the first region 1 varies with the heating temperature (T E ) and annealing time (t G For example, the annealing time (t G ) for more than 10 seconds, and the heating temperature (T E ) is T R +ΔT / 3~TR +2ΔT / 3, a clear boundary between the core region 2 and the peripheral region 1 can be obtained. Similarly, the thickness of the peripheral region 1 changes with the heating temperature (T E ) and heating time (t E ) can be adjusted by the process parameters.

[0079] Thus, the method according to the invention can be used to produce a biphasic microstructure having a first region 1 that is at least largely recrystallized and a second region 2 that is rolled hard.

[0080] After production of the steel sheets according to the invention, they can be coated on one or both sides with a conversion or protective layer in the usual manner, in particular by electrolytic tin or chromium plating.

[0081] example: Examples of embodiments of the steel plate according to the invention, its use in the manufacture of containers and methods are described below.

[0082] Steel sheets with a thickness of 0.23 ± 0.01 mm were produced by hot rolling and subsequent cold rolling from molten steel A having the alloy composition listed in Table 1 (ppm values ​​refer to the weight fraction of the alloying elements in the steel from which the cold-rolled steel sheets were produced). The cold-rolled steel sheets were subjected to various heating times t in an ammonia-containing inert gas atmosphere with an ammonia volume fraction of 5%. E heating temperature T E Heat treatment at 750°C for 45 seconds t G The heating temperature T E was held.

[0083] The microstructure of the heat-treated steel sheet was examined under a microscope (cold embedded, ground, polished, etched with 3% nitric acid after nital). Figure 3 shows an example of a cross-sectional micrograph of a metallographic cross-section of a steel sheet according to the invention, from which two regions 1, 2 with different crystallinity and a barrier layer 3 on the first side of the steel sheet (not visible in the cross-section of Figure 3) can be seen. From Figure 3 it is clear that the steel sheet according to the invention has a biphasic microstructure with a first region 1 that is recrystallized and a second region 2 that is not recrystallized, the first region 1 being significantly thicker than the second region 2.

[0084] For the steel plate samples according to the invention, hardness was recorded at various positions across the cross section. Figure 4 shows the Vickers hardness HV at various positions (positions 1 to 7, where position 1 is the surface of the first side a of the steel plate and position 7 is the surface of the second side b of the steel plate) across the thickness of the steel plate specimen. 0.025 It can be seen from FIG. 4 that the hardness gradually (linearly) increases across the thickness of the steel plate specimen from the first surface a to the second surface b.

[0085] This variation in hardness through the thickness of the sheet is due to the nitriding treatment in the second region 2 of the sheet with a decrease in the nitrogen content from the outside towards the core of the sheet and the (complete) recrystallization of the first region 1 during the heat treatment in the annealing furnace. The second region 2 retains its rolling hardness and is therefore harder, with the hardness maximum being reached at the sheet surface at the second side b.

[0086] As can be seen from Fig. 4, the absolute value of the Vickers hardness increases with heating time t E It can be seen that it depends on short heating times (e.g., t E The sample heat-treated for t = 60 seconds has a low Vickers hardness of about 100 on the first surface a, but the hardness is low when heated for a long time (e.g., t E The specimens treated for heating time t = 300 seconds have a Vickers hardness of more than 150 on the same surface. Therefore, the hardness or strength of the steel plate according to the present invention increases with the heating time t EIt can also be seen from FIG. 4 that for longer heating times, above 120 seconds, at least partial hardening of the first region 1 also occurs during heating, with nitrogen diffusing into this zone and increasing the hardness or strength of the steel there.

[0087] This can also be confirmed by measurements of the strength and elongation of the steel plate according to the invention. Figure 5 shows examples of stress-strain diagrams of two specimens of the steel plate according to the invention, made from the steels of Table 1. These specimens were subjected to different heating times t E = 60 seconds and t E The specimen was heated for 300 seconds and subjected to nitriding treatment during the heating period.

[0088] From FIG. 5 it can be seen that the mechanical parameters of the steel sheet according to the invention, in particular the tensile strength and the elongation at break, can be adjusted via the heating time, with tensile strengths of more than 600 MPa and elongations at break of more than 7% being achievable.

[0089] The method according to the invention can therefore be used to produce (nitrided) steel sheets which are characterised by a very high strength of more than 600 MPa in combination with a good elongation at break of more than 5%, preferably more than 7%. Such steel sheets can be well processed in forming processes for the production of stable packaging such as food or drink cans as well as parts thereof, such as (tear-off) lids.

[0090] The exact composition of the microstructure (in particular the thickness and crystallinity of the first and second regions) as well as the nitrogen content of the first and second regions and the gradient of the nitrogen content through the thickness of the steel sheet produced by the nitriding process in the continuous annealing furnace can be influenced by changing the process parameters, and thus the properties of the steel sheet produced by the method according to the invention can be tailored to different applications.

[0091] The behaviour of the steel plate according to the invention during forming was investigated in a four-radius cup test by forming steel plate specimens into rectangular containers with different bending radii (R1, R2, R3 and R4) at each of the four corners of the container.

[0092] Figure 6 shows a schematic diagram of a vessel formed from a steel plate during a four-radius cup test, where Fig. 6a shows a top view of the vessel base and Fig. 6b shows a cross-sectional side view in the region of the vessel wall. Fig. 6a shows different bending radii (R1, R2, R3, R4) with the following sizes: R1=8mm, R2=10mm, R3=12mm, R4=14mm.

[0093] Roughness measurements were carried out at positions P0, P1, P2, P3 and P4 shown in Fig. 6b to determine the central roughness Ra values.

[0094] In the four-radius cup test, steel sheets with a bilayer crystallization structure were used in each case, where the recrystallized first region 1 and the non-recrystallized (and therefore still mill hard) second region 2 were located both outside and inside the bending radius. In this connection, steel sheets with different thicknesses of the second region 2 were also tested in the four-radius cup test. The different thicknesses of the second region 2 were determined by the different heating times of the stitching process (sample A: t E =1 second, sample B:t E = 300 seconds).

[0095] The results of the four-radius cup test are shown in Figures 7A and 7B. Figure 7A shows the central roughness (Ra values) measured at various bending radii R1, R2, R3, R4 for both deformations of the steel plate specimen after the test at positions P1-P4 (see Figure 6b) and in the area of ​​the non-deformed bottom of the vessel (position P0 in Figure 6b).

[0096] From Fig. 7A it can be seen that the roughness Ra at all bending radii R1-R4 is greater than the roughness at the non-deformed bottom of the container. Moreover, from Fig. 7A it can be seen that for containers with non-recrystallized second regions 2 (of rolling hardness) located outside the bending radii, the roughness at the bending radii R1-R4 is smaller. In contrast, for containers with recrystallized first regions 1 located outside the bending radii, the roughness Ra is greater. For containers with second regions 2 located outside the bending radii R1-R4, the central roughness (Ra) is less than 1.0 μm, in particular less than 0.8 μm.

[0097] Figure 7B shows the Ra coefficient, defined as the ratio of the Ra value at the bending radii R1-R4 to the Ra value in the non-deformed bottom region of the container. As can be seen from Figure 7B, the Ra coefficient is about three times smaller for containers in which the non-recrystallized second region 2 is located outside the bending radii R1-R4. For containers in which the second region 2 is located outside the bending radii R1-R4, the roughness coefficient (Ra coefficient) is less than 3, in particular less than 2.5.

[0098] It follows from this that when forming the steel sheet according to the invention, when the second side b of the steel sheet with the non-recrystallized second region 2 is on the outside, much less roughening occurs outside the bending radius. The results of the four-radius cup test therefore show that the steel sheet according to the invention is very suitable for the production of containers with low Ra values ​​and low roughening in the region of the bending radius of the container. When forming the steel sheet into a container, it is preferable to arrange the second side b of the steel sheet with the non-recrystallized second region 2 in such a way that this side is outside the bending radius of the container after forming. In this case, the non-recrystallized second region 2 of the steel sheet represents a barrier to the coarser grains of the steel structure, preventing them from being visibly extruded to the surface of the second side b and resulting in undesirable roughening outside the bending radius. The thickness of the second region 2 of the rolling hardness is preferably selected to be as thin as possible, in particular to be less than 50 μm. This ensures that the mechanical properties of the steel sheet, in particular its formability, are only slightly influenced by the roll-hardened second region 2. In particular, this ensures that, despite the high hardness and strength of the roll-hardened second region 2, the formability of the steel sheet is not significantly reduced. Indeed, inside the bending radii R1-R4, it is the softer, more easily formable first side a of the steel sheet, which has the recrystallized softer first region 1. When the steel sheet is formed into the bending radius, the first region 1 of the steel sheet is compressed inside the bending radius, and the recrystallized softer first region 1 only offers a small resistance to this forming. Thus, despite the high hardness and strength in the second side b, the steel sheet according to the invention can be easily formed into a container by conventional forming processes, in particular deep drawing, without harmful roughening occurring on the surface of the steel sheet outside the forming zone. Comparing the roughness values ​​of test piece A and test piece B shown in Fig. 7A, it can be seen that the thickness of the second region 2 only slightly affects the roughness. Therefore, from the viewpoint of avoiding surface roughening during steel sheet forming, the thickness of the second region can be made thin. [Table 1] [Table 2]

Table 3

Claims

1. A method for manufacturing a steel sheet for packaging, comprising the steps of: Carbon content (C) of 10 to 1000 ppm by weight and a given recrystallization temperature (T R providing a cold rolled sheet of steel having a first surface (a) and a second surface (b); applying an at least substantially nitrogen-impermeable barrier layer (3) to a first side (a) of said steel sheet; The steel plate is heated to a temperature (T E ) and Including, The heating is performed in a nitriding gas atmosphere until the recrystallization temperature (T R ), so that, during heating of the steel sheet, nitrogen diffuses from the gas atmosphere into at least the near-surface region (2) of the second side (b) of the steel sheet and is incorporated in this region (2), so that the recrystallization temperature of the steel in the near-surface region (2) is increased by a value ΔT; The heating temperature (T E ) is the recrystallization temperature (T R ) or higher, and the recrystallization temperature (T R +ΔT).

2. The cold-rolled steel sheet has the following composition by weight: C: more than 0.001% and less than 0.1%, preferably less than 0.06%; Mn: more than 0.01% and less than 0.6%; P: less than 0.04%; S: less than 0.04% and preferably more than 0.001%; Al: less than 0.08% and preferably more than 0.005%; Si: less than 0.1%; Optional Cu: less than 0.1%; Optional Cr: less than 0.1%; Optional Ni: less than 0.1%; Optional Ti: less than 0.1% and preferably more than 0.02%, particularly preferably more than 0.05%; Optional Nb: less than 0.08% and preferably more than 0.01%; Optional Mo: less than 0.08%; Optional Sn: less than 0.05%; Optional B: less than 0.01%, preferably less than 0.005%, and preferably more than 0.0005%; Optional N: less than 0.02%, particularly less than 0.016%, and preferably more than 0.001%; The balance is iron and unavoidable impurities, having 2. The method according to claim 1, wherein the cold rolled steel sheet has an average nitrogen content by weight of 0.005% or more, preferably 0.015% or more after heating in the nitriding gas atmosphere.

3. 3. The method according to claim 1 or 2, wherein the steel of the cold rolled steel sheet contains, by weight, more than 200 ppm, preferably more than 500 ppm titanium, and / or more than 100 ppm niobium, and / or more than 50 ppm aluminium.

4. The cold rolled steel sheet is heated for a heating time (t E ) from room temperature to the heating temperature (T E ) and the heating temperature (T E After reaching a predetermined annealing time (t G ) throughout the heating temperature (T E ) and the heating time (t E ) is preferably in the range of 1.0 to 300 seconds, and / or the annealing time (t G 4. The method according to claim 1, wherein the time t1 is preferably in the range of 1.0 seconds to 80 seconds.

5. The steel of the cold-rolled steel sheet has an initial nitrogen content (N 0 During heating of the cold rolled steel sheet, the average nitrogen content of the surface near region (2) is determined as the initial nitrogen content of the steel (N 0 5. The method according to claim 1 , wherein the nitrogen content is increased to a value of 50-1000 ppm above the surface area (100 ppm) of the cold rolled steel sheet, and wherein the nitrogen content gradient is in particular formed over the entire cross section of the cold rolled steel sheet, decreasing from the near-surface region (2) of the second side (b) of the steel sheet towards the first side (a) of the steel sheet provided with the barrier layer (3).

6. During the heating, in particular the holding time (t H ), the nitriding treatment of the near-surface region (2) on the second surface (b) of the cold-rolled steel sheet is at least temporarily performed during the annealing time (t G 6. The method according to claim 1, wherein during the heating step, a recrystallization annealing of the cold rolled steel sheet outside the near-surface region (2) is at least partially performed, in particular in a first region (1) on the first side (a) of the steel sheet, while the near-surface region (2) on the second side (b) of the steel sheet is not recrystallized.

7. 7. The method according to any one of claims 1 to 6, wherein the value ΔT, by which the recrystallization temperature in the near-surface region (2) increases due to the uptake of nitrogen when the steel sheet is heated, is greater than 30°C, preferably greater than 50°C, in particular in the range of 100°C to 250°C.

8. The barrier layer (3) is formed on the first side (a) of the steel sheet by a sol-gel layer, in particular a SiO 2 , TiO 2 and / or ZrO 2 8. The method according to claim 1 , characterized in that the coating is formed by applying a layer of

9. 9. The method according to claim 8, characterized in that the steel sheet is a steel strip and the sol-gel layer is applied onto the first side (a) of the surface of the steel strip in a strip coating process, in particular wet-chemically.

10. 8. The method according to any one of the preceding claims, characterized in that the barrier layer (3) is applied electrolytically to the surface of the first side (a) of the steel sheet from an aqueous electrolyte containing silica.

11. The coating weight of the barrier layer (3) is 1 to 10 mg / m 2 in the range of 3 to 6 mg / m 2 The method according to any one of claims 1 to 10, wherein the range is

12. A steel sheet, in particular a steel sheet for packaging, made from a steel having a carbon content (C) of 10 to 1000 ppm by weight, having a first side (a) and a second side (b) and a thickness of less than 0.5 mm, in which an at least substantially nitrogen-impermeable barrier layer (3) is present on the surface of said first side (a), said steel sheet having a bilayer crystallized structure comprising a first region (1) on said first side (a) and a second region (2) on said second side (b), said first region (1) being at least substantially recrystallized and said second region (2) not being recrystallized or at least not being completely recrystallized.

13. The steel sheet according to claim 12, C: more than 0.001% and less than 0.1%, preferably less than 0.06%; Mn: more than 0.01% and less than 0.6%; P: less than 0.04%; S: less than 0.04% and preferably more than 0.001%; Al: less than 0.08% and preferably more than 0.005%; Si: less than 0.1%; Optional Cu: less than 0.1%; Optional Cr: less than 0.1%; Optional Ni: less than 0.1%; Optional Ti: less than 0.1% and preferably more than 0.02%, particularly preferably more than 0.02%; Optional Nb: less than 0.08% and preferably more than 0.01%; Optional Mo: less than 0.08%; Optional Sn: less than 0.05%; Optional B: less than 0.01%, preferably less than 0.005%, and preferably more than 0.0005%; a nitrogen content averaged over the thickness of the steel sheet of 0.005% or more, preferably more than 0.015%, particularly preferably more than 0.02%; The balance is iron and unavoidable impurities. A steel plate having a weight composition of

14. 14. Steel sheet according to claim 12 or 13, characterized in that the thickness of the first region (1) is in the range of 50 μm to 450 μm, preferably in the range of 90 μm to 400 μm, in particular in the range of 150 μm to 300 μm, and / or the thickness of the second region (2) is in the range of 1 μm to 50 μm, preferably in the range of 2 μm to 10.0 μm.

15. 15. Steel sheet according to any one of claims 12 to 14, characterized in that it has a tensile strength of more than 500 MPa, preferably more than 700 MPa and / or an elongation at break of more than 5%, preferably more than 7%.

16. The steel plate according to any one of claims 12 to 15, characterized in that the average nitrogen content in the second region (2) of the steel plate is between 50 and 1000 ppm by weight.

17. 17. The steel sheet according to any one of claims 12 to 16, characterized in that a gradient in the nitrogen content exists at least in the second region (2) and / or throughout the thickness of the steel sheet, the nitrogen content decreasing from the second side (b) towards the first side (a) of the steel sheet.

18. The hardness and / or tensile strength of the second region (2) is greater than that of the first region (1), the ratio of the hardness of the second region (2) to the hardness of the first region (1) is preferably greater than 1.2, particularly preferably greater than 1.4, and the Vickers hardness of the second region (2) of the steel sheet is preferably 250 HV 0.025 More than 300HV, particularly preferably 300HV 0.025 The steel sheet according to any one of claims 12 to 17, characterized in that

19. 19. The steel sheet according to any one of claims 12 to 18, characterized in that the degree of recrystallization in the second regions (2) is less than 30%, preferably less than 20%, and / or the degree of recrystallization in the first regions (1) is more than 70%, preferably more than 80%.

20. 20. Steel sheet according to any one of claims 12 to 19, characterised in that a nitride layer, in particular an iron nitride layer, is present on the surface of the second region (2).

21. The barrier layer (3) is a sol-gel layer, in particular a SiO 2 , TiO 2 and / or ZrO 2 21. Steel sheet according to any one of claims 12 to 20, characterized in that it is a layer of

22. The barrier layer (3) on the surface of the first region (1) has a thickness of less than 1 μm, in particular less than 0.1 μm, or a thickness of less than 10 mg / m 2 less than 3 mg / m 2 ~6mg / m 2 22. Steel sheet according to any one of claims 12 to 21, characterized in that it has a coating weight of

23. 23. The steel sheet according to any one of claims 12 to 22, characterized in that the bending radius of the surface of the second region (2) after forming of the steel sheet is in the range of 8 mm to 14 mm, and the second region (2) outside the bending radius has a roughness (Ra) which is less than 1.0 μm, preferably less than 0.8 μm, and / or a roughness factor which is less than 3, preferably less than 2.5, said roughness factor being defined by the ratio of the roughness of the surface of the second region (2) outside the bending radius to the roughness of the steel sheet in a non-deformed part.

24. 24. A container, in particular a can, made from a steel plate according to any one of claims 12 to 23, wherein the container has at least one convex deformation, the second region (2) of the steel plate being located outside the convexity of the deformation.