Polymer Additive Manufacturing and Ophthalmic Lenses Formed Therefrom - Patent application
By employing controlled atmosphere and energy intensity mapping with grayscale images, the method addresses surface smoothness and consistency issues in additive manufacturing, reducing costs and waste while improving optical element quality.
Patent Information
- Application Number
- JP2023580352
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2022-11-09
- Filing Date
- 2022-12-02
- Publication Date
- 2024-11-19
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Conventional additive manufacturing methods lack surface smoothness and consistency in forming optical elements like contact lenses, leading to variations in patient experience and high environmental impact due to complex, costly equipment and waste generation.
A method involving controlled atmosphere and energy intensity mapping using grayscale images to deposit polymerizable droplets, followed by intermittent pinning and curing, ensuring precise oxygen concentration to achieve smooth and consistent optical elements.
This approach enhances surface quality, reduces manufacturing costs, minimizes waste, and improves design flexibility for optical elements, particularly contact lenses, by controlling oxygen exposure during polymerization.
Smart Images

Figure 2024542913000001_ABST
Abstract
Description
[Technical field]
[0001] CROSS-REFERENCE TO RELATED APPLICATIONS This application claims priority to U.S. Non-provisional Application No. 17 / 984,103, filed November 9, 2022, which claims the benefit of U.S. Provisional Application No. 63 / 306,472, filed February 3, 2022, and U.S. Provisional Application No. 63 / 356,583, filed June 29, 2022, the entire disclosures of which are incorporated herein by reference.
[0002] FIELD OF THEINVENTION The present invention relates to the field of improved additive manufacturing, and in particular to methods and apparatus for forming ophthalmic devices by repeated application of droplets of polymerizable material representative of energy transmittance mapping, and the resulting lenses. [Background technology]
[0003] 2. Background of the Invention Conventional additive manufacturing is known which involves the application of materials deposited based on a computer-aided design (CAD) model or other three-dimensional (3D) model. In such a process, the 3D model is sliced into layers, where each layer is a cross-section of the 3D design. Each cross-section is deposited sequentially to form the molded article. Sacrificial layers and / or portions of layers may be applied in the form of additives that are subsequently removed.
[0004] The material is typically applied by a sintering process, whereby small amounts of material are melted and placed in locations corresponding to specific cross-sections, resulting in a fusion deposition process. Such techniques include stereolithography and selective laser sintering. Summary of the Invention [Problem to be solved by the invention]
[0005] Additive manufacturing can be low cost and offers more flexibility in the design of manufactured articles and production runs, however, articles formed by additive manufacturing often lack the finish quality obtained by other manufacturing techniques, in particular lacking sufficient surface smoothness.
[0006] Contact lens manufacturing has evolved over the past few decades from lathe cutting to spin casting to cast molding, which remains the most cost-effective process. Lathing contact lenses typically involves machining one button of lens material at a time until the desired shape is reached. Such processes require complex lathe equipment and specialized operator expertise. Also, they are not efficient for mass production of contact lenses.
[0007] Although cast molds are effective for mass production of contact lenses, because each lens is formed to an approximate size and shape, variations of up to 1 / 8 or 1 / 4 diopter can occur within the same production run, resulting in variability in patient experience, sometimes referred to as "good contact lens days" and "bad contact lens days."
[0008] Cast molding of ophthalmic lenses is a complex process involving many variables that are difficult to maintain within acceptable parameters, which results in variable results in the final product. The variables can result from one or more of the following: depositing a hardenable mixture of polymerizable monomers into a mold cavity, forming the mold cavity through two mold sections, curing the monomer mixture within the cavity, and disassembling the mold assembly to remove the lens. One mold section forms the anterior lens surface and the other mold section forms the posterior lens surface.
[0009] The cost of cast molding equipment is very high due to the large size of the manufacturing lines involved. Furthermore, the manufacture of the optical quality metal inserts used to cast the lenses and the subsequent injection molding of the plastic molds requires a large up-front investment, and the associated designs are limited by the symmetry constraints of cast molding technology. Cast molding also results in large amounts of plastic waste with harmful associated environmental impacts and added costs.
[0010] Furthermore, cast molding requires the management of a vast inventory of SKUs and the associated warehousing, order picking and shipping logistics issues, all of which add significant environmental disadvantages and costs to the resulting contact lens products. Furthermore, the types of contact lenses produced in a lens molding process can only have a limited number of variations in optical power, base curve, and diameter.
[0011] Summary of the Invention Thus, the present invention provides an improved method and apparatus for the production of molded articles having a surface quality conducive to use as optical elements, such as for example use as contact lenses. The improvements presented here are directed to a process involving repeated application of monomer according to an energy intensity map, such as a grayscale image mapping the intensity of the energy spectrum associated with visible light. The improved method includes intermittent pinning and final curing of the applied monomer, resulting in increased design flexibility and reduced manufacturing costs for hydrogel-based ophthalmic devices, including ophthalmic devices that are not rotationally symmetric. In accordance with the present invention, the print head may be positioned during deposition at a position that is not perpendicular to the apex of the receiving surface, and the droplets may be non-spherical when they contact the receiving surface. The improvements also include reduced waste, reduced environmental impact, reduced warehousing overhead, and reduced labor required to manufacture and store ophthalmic lenses.
[0012] The present invention provides that a lens may be produced through two or more components, including an optic zone (sometimes referred to herein as "OZ"), and a peripheral zone, or edge portion. One or both of the optic zone and peripheral zone may be formed based on an energy intensity pattern that describes a water-free axial thickness profile.
[0013] In some embodiments, the additive manufacturing equipment may be controlled to make multiple passes of a print head that adds polymerizable material to a receiving surface to form a lens (or other molded article) according to an axial thickness profile that includes a lens power in air (P), a lens refractive index (n), a center thickness (CT), and a back surface radius of curvature (RB).
[0014] Some embodiments of the present disclosure may include a method of forming an ophthalmic lens by additive manufacturing, the method comprising positioning a substrate at a first position relative to an additive manufacturing print head and ejecting a pattern of deposited droplets of a polymerizable mixture from the print head, the pattern of deposited droplets of the polymerizable mixture corresponding to a portion of an energy transmittance map of the ophthalmic lens to be formed.
[0015] Some variations include receiving deposited droplets of the polymerizable mixture on a receiving surface, the receiving surface including one or both of a substrate and a previously ejected polymerizable mixture. Embodiments may include repositioning the substrate from a first position to a next position (current position plus N) relative to the print head. The repositioning may be accomplished by movement of one or both of the substrate and the print head.
[0016] Further, a variation of this embodiment includes ejecting a next pattern of deposited droplets of the polymerizable mixture (first position plus N) corresponding to a next portion of the energy transmittance map of the ophthalmic lens being formed. The multiple ejections may occur during a pass of the print head against a receiving surface, which may include a substrate.
[0017] Some variations may include coalescing material from the deposited droplets of the polymerizable mixture on the receiving surface and exposing the coalesced material to a pinning process that causes partial polymerization of the deposited droplets of the polymerizable mixture. Following the passage of the print head, one or more of gravity, surface tension, and microforces may act on at least a portion of the deposited droplets to allow the receiving surface to be smoothed, such as to uniform the interstitial spaces between the deposited droplets.
[0018] In some embodiments, at least a portion of the droplets of the polymerizable mixture deposited during the current pass may merge with previously deposited polymerizable mixture on the receiving surface to form the same volume, which may include a single volume of polymerizable mixture on the substrate. Embodiments may also include pinning the deposited droplets on the receiving surface via partial polymerization of the deposited droplets and hardening the deposited droplets of the polymerizable mixture. The merger of the deposited droplets alleviates the disclosed process from the requirement that the droplets maintain a particular shape during deposition, impact, or after impact.
[0019] In some embodiments, the pinning process may include exposing the deposited droplets of the polymerizable mixture to actinic radiation at a first wavelength for a limited time sufficient to cause gelation of the deposited droplets of the polymerizable mixture but not to cause hardening of the deposited droplets.
[0020] Further, in some embodiments, the curing process may include exposing the deposited droplets of the polymerizable mixture to actinic radiation of a second wavelength for a sufficient time and with sufficient intensity to cause polymerization of the deposited droplets of the polymerizable mixture in one or more cycles of droplet deposition.
[0021] The present invention further provides a method of manufacture that includes a periphery of the formed object and a central portion of the object contained with the peripheral portion. For example, in some embodiments of the present invention, an ocular contact lens having a generally spherical shape may have an edge portion including an essentially ring shape formed via additive manufacturing (or other manufacturing methods such as machining and / or custom molding) and an optical zone of the contact lens formed within the peripheral portion via an additive manufacturing process. The edge portion is preferably of greater mass than the central portion including the optical zone. During formation, the peripheral ring portion may be partially or fully cured and internal stresses may be borne more in the heavier portion of mass. Forming the edge portion while it is not acted upon by the central portion allows the edge portion to be formed with reduced stress while the deposited monomer cures into a polymer. The examples provided herein are generally described with reference to spherical contact lenses, but other embodiments are within the scope of the present invention, such as other molded articles such as oval or crescent-shaped contact lenses or complex shaped intraocular lenses.
[0022] In some aspects, the present invention provides for the application of a pattern of multiple defined regions contained within a single lens, with each region representing an amount of light that can transmit through its associated region. Each region may have a light transmittance value based on a scale, such as an 8-bit, 16-bit, 32-bit, or 64-bit scale (other scales are within the scope of the present invention). In some embodiments, each region may refer to the smallest single component of a digital image. Further, in some embodiments, the smallest single component of a digital image may be referred to herein as a "pixel." In some embodiments, a pixel may be associated with a distance measurement, such as, for example, a quantity of nanometers.
[0023] The invention provides for the subsequent application of polymerizable material in a plurality of successive patterns, each successive pattern corresponding to a grayscale image. Following application of each pattern of the grayscale image, the polymerizable material is pinned but not fully polymerized.
[0024] After a final application of monomer in the pattern of the grayscale image, the aggregated monomer from each application of the grayscale image is polymerized to form a polymeric lens, such as, for example, a hydrogel contact lens formed from etafilcon.
[0025] The application of multiple successive grayscale image patterns, which may be deposited one on top of another but positioned side-by-side, is preferably performed in a controlled atmosphere. The atmosphere may be controlled to limit certain amounts of variables, such as, by way of non-limiting example, suspended particulate matter and / or gases present in the atmosphere during certain process steps involved in the manufacturing process. As a specific example, a preferred embodiment includes an atmosphere that limits the amount of oxygen to which the monomer is exposed prior to polymerization, and also limits the size and amount of particulates that may interact with the monomer prior to polymerization.
[0026] In some embodiments, in some monomer or other polymerizable mixtures, oxygen may be controlled as a critical variable involved in the free radical polymerization of monomeric materials and prepolymers involved in the manufacturing process. This may be particularly relevant for ophthalmic devices formed from hydrogels that contain relatively low levels of crosslinkers that must be hydrated after polymerization and are easily susceptible to shape distortion from variations in the resulting polymer network.
[0027] According to another aspect of the invention, exposure of the monomer or other polymerizable mixture to a gas (such as oxygen) that may affect polymerization characteristics is carefully controlled in one or more of the amount of exposure, the consistency of exposure across the monomer, and the exposure time. It has been discovered that during polymerization, if the oxygen concentration is high on one side (side 1) or other portion of the monomer forming the optical device compared to the second side (side 2) or other region, side 1 may expand relatively more than side 2, which may result in distortion of the inherent optical properties of the optical device formed. Similarly, portions of the polymerizable mixture with high and low oxygen concentrations may expand by different amounts than other portions with different oxygen concentrations. By limiting the supply of oxygen to the polymerizable mixture prior to polymerization, a relatively consistent oxygen concentration may be maintained within the polymerizable mixture, thereby achieving a consistent expansion coefficient caused by oxygen concentration.
[0028] In some embodiments, relatively high concentrations of initiators, high intensity UV light energy, oxygen scavengers, waxes, or coatings may be used to manage the effects of oxygen prior to polymerization of the polymerizable mixture, however, to date, none of these have been shown to consistently produce high quality optical devices.
[0029] The present invention takes a novel approach to fabricating optical elements, such as ophthalmic devices, by controlling the presence and concentration of oxygen to low levels and / or simultaneously at regulated concentrations in the use of a 3D printing apparatus. In some embodiments, it is beneficial to control the level of oxygen in the polymerizable mixture relative to the oxygen level in the ambient atmosphere of the polymerizable mixture during the manufacture of the optical device in order to obtain the desired dimensions and resulting optical properties of the optical device contained in the optical element. This principle may be extended to include the substrate on which the deposition printing occurs. Thus, embodiments include oxygen levels that are maintained at a predetermined level before and during the polymerization process. [Means for solving the problem]
[0030] In a first aspect, the present invention relates to a method for three-dimensional deposition printing of optical elements, in which a plurality of droplets of a polymerizable mixture are deposited on a surface of a substrate under a controlled atmosphere, thereby forming a pattern of energy intensity transmission through the deposited polymerizable mixture, such as a grayscale by the polymerizable mixture, and the controlled atmosphere containing the pattern of the polymerizable mixture is maintained at an oxygen concentration of at most about 5.0% by volume (preferably at most about 1.0% by volume), and the oxygen equilibrium concentration of the polymerizable mixture is at most about 8.0% by volume (preferably at most about 2.0% by volume). In this context, due to the constraints of measuring the volume percentage of oxygen in the polymerizable mixture and the surrounding environment, "about" may be considered to be within 10% of the stated amount. [Brief description of the drawings]
[0031] [Figure 1] FIG. 1 illustrates an exemplary additive manufacturing apparatus that may be used in some embodiments of the present invention. [Diagram 2] FIG. 2 is a schematic diagram of an alternative 3D printing apparatus according to some embodiments of the present invention. [Diagram 3] FIG. 3 shows an exemplary energy intensity pattern, represented as a grayscale image, that may be used to generate a control protocol for a 3D printing device according to some embodiments of the present invention. [Figure 4] FIG. 4 is a schematic diagram of a spherical lens having a specified peripheral portion, according to some embodiments of the present invention. [Diagram 5] FIG. 5 is a schematic diagram of a profile cutaway of a lens having a peripheral portion and a carrier portion supporting an optical zone, according to some embodiments of the present invention. [Figure 6] FIG. 6 shows a graphical curve representing an exemplary water-containing surface of an ophthalmic lens that can be formed in accordance with the present invention. [Figure 7] FIG. 7 shows a graphical curve representing an exemplary water-free axial thickness of an ophthalmic lens moldable in accordance with the present invention. [Figure 8] FIG. 8 is a schematic diagram of a false color image of the peripheral region. [Figure 9] FIG. 9 is a schematic diagram of a false color image of a foil lens thickness profile having a transition region zone. [Figure 10] FIG. 10 shows a false color image of the thickness profile of the peripheral region zone of an astigmatic lens. [Figure 11] FIG. 11 shows a false color image of the thickness profile of an astigmatic lens. [Figure 12] FIG. 12 illustrates method steps that may be performed while implementing some embodiments of the present invention. [Figure 13] FIG. 13 is a schematic illustration of a deposited droplet of polymerizable mixture merging with a volume of polymerizable mixture previously deposited on a substrate. [Figure 13A] FIG. 13A is a schematic illustration of a deposited droplet of polymerizable mixture merging with a volume of polymerizable mixture previously deposited on a substrate. [Figure 14] FIG. 14 is a schematic diagram illustrating an exemplary change in shape of a droplet of a polymerizable mixture after ejection from a print head. [Figure 15] FIG. 15 shows a flowchart of method steps that may be performed in some embodiments of the present invention. [Figure 15A] FIG. 15A shows a flowchart of method steps that may be performed in some embodiments of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0032] Detailed Description of the Invention The present invention provides an apparatus and method for applying small droplets of a polymerizable mixture to a surface based on a pattern or map of energy transmittance. A grayscale image may be used as the map of transmittance of visible light energy. The surface may be a flat surface, an arcuate surface, or a complex variable surface. The droplets of polymerizable mixture applied to the surface accumulate into a pattern of polymerizable mixture that replicates the map of energy transmittance. Following application of the polymerizable mixture to the surface, the applied polymerizable mixture may be exposed to a limited amount of actinic conditions, such as radiation (limited in intensity and / or duration) and / or thermal energy. The exposure to the limited amount of actinic radiation is adequate to pin the applied polymerizable mixture in place.
[0033] The pinned polymerizable mixture may act as a subsequent receiving surface to receive additional polymerizable mixture applied in a pattern of energy transmittance. After the final application of polymerizable mixture, the polymerizable mixture accumulated on the substrate surface may be exposed to actinic conditions (e.g., radiation and thermal energy) sufficient to cure the accumulated polymerizable mixture into a polymer.
[0034] The atmosphere containing the droplets of the polymerizable mixture during application onto the receiving surface and during their residence on the receiving surface before curing may be carefully controlled to achieve consistent optical quality of the devices formed by the cured polymerizable mixture.
[0035] In the disclosure herein, ophthalmic lenses (and / or contact lenses) are used for purposes of illustration and discussion, however, the principles are applicable to forming molded articles generally, and the teachings presented may be used broadly for any optical element (or other molded article) where precise dimensions, optical properties, and / or similar uniform polymer properties are desirable, such as, for example, intraocular lenses.
[0036] According to the invention, in some embodiments, the polymerizable mixture is delivered in the form of very small droplets, typically 1-15 picoliters in volume, at high velocity in a gas atmosphere with a relatively high surface-to-volume ratio. A large number of droplets (estimated to be 1.5-9 million) are required to form a 25 milligram lens. Several factors may be considered to deliver each droplet to the correct location during production. These factors include, but are not limited to, one or more of the following: exposure of the droplet to ambient process conditions, thickness of the layer of material that results when the droplet impacts the surface of the substrate and / or the previously deposited polymerizable mixture, interaction with the receiving surface of the substrate and / or the previously deposited polymerizable mixture, such as wetting of the receiving substrate surface and coalescence with the previously deposited polymerizable mixture, effect of the impacting droplet, pinning between subsequent layers of droplets of polymerizable mixture via exposure time to actinic radiation and / or atmospheric gases, and curing / polymerization of the deposited polymerizable mixture.
[0037] During the additive manufacturing process, there is significant opportunity for the polymerizable mixture to be exposed to (and pick up) ambient gases, such as oxygen, from one or more of the ambient process atmosphere (sometimes referred to as a controlled atmosphere), the receiving substrate surface, and previously deposited droplets of the polymerizable mixture; if such factors are not precisely controlled, the surface and bulk properties (including the optical properties) of the resulting ophthalmic lens will be adversely affected.
[0038] The effect of oxygen is particularly pronounced in lenses made using hydrogel materials such as 2-hydroxyethyl methacrylate (HEMA) or other monomers used in soft contact lenses and soft intraocular lenses. In such materials, the variations caused by exposure to oxygen are more pronounced in the final cured lens after the lens has absorbed water. Thus, in preferred embodiments, exposure to oxygen may be considered to be detrimental.
[0039] Typically, the surface or skin portion of a lens formed in higher oxygen conditions contains more polymer network defects than the bulk portion, allowing more water to be absorbed in the regions formed in higher oxygen conditions. The distortions that occur in such skin regions usually have a detrimental effect on the overall mechanical properties (elastic modulus, tensile strength, elongation), optical properties (optical transmission, refractive index, etc.), shape, and part-to-part repeatability.
[0040] The present invention teaches controlling and adjusting the oxygen content of the polymerizable mixture in relation to the oxygen content of the controlled atmosphere (described herein) with the goal that the effect of oxygen is controlled to such an extent that the properties of the optical element formed are not significantly affected.
[0041] In these embodiments, including the formation of ophthalmic devices (e.g., contact lenses, intraocular lenses, and spectacle lenses), the ability to create an optical prescription is highly dependent on the precise shape of the curved surface. Creating these necessary surfaces on these and other non-ophthalmic optical elements can be accomplished by using the principles claimed in the present invention, thus enabling the advantages of using 3D deposition printing, such as simplicity, efficiency, more freedom in design, lower time requirements, and cost.
[0042] In some embodiments, the effect of oxygen in the polymerization process and the resulting effect on the properties of the formed article is eliminated or substantially reduced. This allows for improved control of the post-deposition movement of the polymerization mixture when forming the polymer matrix into layers. This is important in the creation of curved, arbitrary or irregular surfaces or shapes, especially when creating complex optical devices that require precise curved surfaces, including surfaces that incorporate multiple arcuate portions. Thus, the combined effect of overcoming oxygen inhibition and controlling the movement of the polymerizable mixture in optical product applications is likely to reduce or even eliminate optical artifacts and distortions.
[0043] In some embodiments, the present invention provides an apparatus and method of operating the apparatus for three-dimensional depositional fabrication of ophthalmic devices in which multiple droplets of a polymerizable mixture are deposited under a controlled atmosphere onto a surface of a substrate (and / or a previously deposited polymerizable mixture), thereby forming a layer of the polymerizable mixture into a pattern that replicates an energy transmittance map (e.g., a grayscale image).
[0044] In some embodiments of the invention, the oxygen concentration in the polymerizable mixture may be adjusted relative to one or more of the oxygen concentration of a controlled atmosphere to which the polymerizable mixture is exposed, the oxygen concentration in other parts of the environment (such as a substrate receiving droplets of the polymerizable mixture), such that migration of oxygen from one source to another is avoided or at least reduced to an extent that is insignificant to polymerization of the polymerizable mixture.
[0045] Glossary
[0046] In this specification and the claims directed to the invention presented, various terms may be used where the following definitions apply.
[0047] As used herein, "actinic radiation" refers to the emission of energy capable of initiating a chemical reaction in an associated polymerizable mixture. In some embodiments, actinic radiation includes radiation having a wavelength in the range of 280-450 nm. In some more specific exemplary embodiments, actinic radiation corresponding to UVA and blue light includes energy having a wavelength in the range of 315-450 nm, and in some preferred embodiments includes energy in the range of 365 nm-400 nm.
[0048] "Additive-based manufacturing" (sometimes referred to herein as "additive manufacturing") refers to a process in which units of material are added to a structure that is formed into a shape through the aggregation of the units of material into that shape.
[0049] As used herein, "arcuate" refers to a geometric shape that includes curved surfaces.
[0050] As used herein, "curing" refers to exposing a polymerizable mixture to actinic radiation conditions, which may include fixed radiation and / or thermal energy of sufficient intensity to crosslink a majority of the polymerizable mixture.
[0051] "Fixing radiation" as used herein refers to actinic radiation of the appropriate wavelength and of sufficient intensity and duration to crosslink a substantial portion of a polymerizable mixture exposed to the fixing radiation.
[0052] "Gel" or "gelling" refers to a degree of polymerization sufficient to stop or substantially slow the movement of the polymerizable mixture deposited on the receiving surface, allowing subsequent droplets to merge with previously deposited polymerizable mixture and form a structure having a single, distortion-free mass of polymerizable mixture. A gelled polymerizable mixture transitions to a higher viscosity state, but does not achieve full cure. Pinning or gelling (or gelling) enhances flow and shape control, providing a high quality surface.
[0053] As used herein, "gel point" refers to the point in the polymerization process where a gel or insoluble portion forms. The gel point may be considered as the degree of conversion at which the liquid polymerization mixture becomes a highly viscous material that is immobile on a stationary surface. The gel point may be determined, for example, using a Soxhlet experiment: the polymer reaction is stopped at different time points and the resulting polymer is analyzed to determine the weight fraction of the remaining insoluble polymer. The data may be extrapolated to the point where no gel is present. The gel point may be determined by analyzing the viscosity of the polymerizable mixture during the reaction. The viscosity may be measured using a parallel plate rheometer, with the polymerizable mixture sandwiched between parallel plates. At least one of the plates should be transparent to radiation at the wavelength used for polymerization. The point at which the viscosity approaches infinity is the gel point. The gel point occurs at the same degree of conversion for a given polymer system and given reaction conditions.
[0054] As used herein, an "inhibitor" refers to a chemical reactant or process that slows or stops a chemical reaction.
[0055] As used herein, "initiator" refers to a substance that starts a chain reaction or polymerization.
[0056] As used herein, "intensity" refers to the amount of power transmitted per unit area, where the area is measured on a plane perpendicular to the direction of energy propagation (e.g., watts per square meter (W / m 2 )).
[0057] As used herein, "lens" refers to any ophthalmic device that resides in or on the eye. These devices can provide optical correction or can be cosmetic. For example, the term lens can refer to contact lenses, intraocular lenses, overlay lenses, ocular inserts, optical inserts, or other similar devices that correct or modify vision or cosmetically enhance eye physiology without interfering with vision (e.g., iris color).
[0058] "Pinning," as used herein, refers to the application of actinic conditions, such as exposure to limited actinic radiation, to a sufficient amount of the polymerizable mixture to effect the gelation process or gelation but not hardening of the polymerizable mixture.
[0059] As used herein, a "polymerizable mixture" (sometimes referred to as a "PM") refers to a liquid mixture of components (reactive and sometimes non-reactive components) that can undergo polymerization to form a polymer or polymer network upon exposure to external energy (e.g., actinic radiation in the range of 280-450 nm (e.g., UV light or blue light or heat). The polymerizable mixture may include monomer or prepolymer materials that may form an ophthalmic lens that may be cured and / or crosslinked, or modify an existing lens or lens blank. Various embodiments may include a polymerizable mixture that includes one or more additives, such as: UV blockers, adhesives, colorants, photoinitiators or catalysts, and other additives desired in an ophthalmic lens, such as a contact lens or intraocular lens. In some embodiments, the polymerizable mixture may also be a hydrogel precursor.
[0060] As used herein, the expression oxygen equilibrium concentration of a polymerizable mixture of X is intended to mean the oxygen concentration in the polymerizable mixture that would result if the mixture were allowed to equilibrate with an atmosphere having an oxygen concentration of X% at 1.0 atmosphere (1013 mbar).
[0061] As used herein, the term optical element is intended to include, but is not limited to, ophthalmic devices, lenses used in industrial applications, lenses for endoscopes, inspection devices, fiber optic devices, camera lenses, telescope lenses, etc. An embodiment of particular present interest is an ophthalmic device.
[0062] In some embodiments, the optical element has one or more objects embedded therein, for example, a solid object selected from an insert, an electronic device, and a functional additive release reservoir or depot.
[0063] In other embodiments, the optical element includes one or more functionally active substances, including biologically active substances.
[0064] As used herein, an ophthalmic device is a device that is in front of the eye or in or on the eye or part of the eye, including the cornea, eyelids, and glands. These devices can provide optical correction, cosmetic enhancement (e.g., iris color), vision enhancement, therapeutic benefits (e.g., as bandage lenses), or devices that deliver therapeutic agents such as lubricants, humectants, anti-inflammatory, anti-allergic, anti-bacterial, anti-infective, anti-hypertensive, or nutritional supplements, vitamins, antioxidants for eye health, or any combination of the above. Illustrative examples of ophthalmic devices include those selected from spectacle lenses, contact lenses (e.g., soft or hard contact lenses), intraocular lenses, overlay lenses, corneal implants such as corneal inlay implants, and ophthalmic / ocular inserts.
[0065] In some embodiments, the ophthalmic device is a contact lens, particularly a soft contact lens such as a contact lens of a hydrogel material, while other embodiments may include an intraocular lens of a hydrogel material.
[0066] The term hydrogel refers to a crosslinked polymer that has absorbed water (swollen) to a water content of at least 10% by weight. Preferably, such hydrogel materials have a water content of at least 20% by weight, such as at least 25% by weight, and up to 70-90% by weight.
[0067] As used herein, the term polymerizable mixture refers to a liquid mixture of components (reactive and possibly non-reactive) that can undergo polymerization to form a polymer or polymer network upon exposure to external energy (e.g., 280-450 nm actinic radiation (such as UV light or blue light) or heat). Typically, the mixture includes reactive components such as monomers, macromers, prepolymers, crosslinkers, and initiators. In addition, the polymerizable mixture may further include other components such as additives such as wetting agents, release agents, dyes, light absorbing compounds such as UV absorbers and photochromic compounds, which may be reactive or non-reactive, any component capable of being retained in the resulting ophthalmic device, as well as pharmaceuticals, vitamins, antioxidants, and dietary supplement compounds. It will be appreciated that a wide range of additives may be added based on the ophthalmic device being manufactured and its intended use.
[0068] The fact that a mixture is polymerizable typically implies that one or more of the components of the mixture (e.g., monomers, macromers, prepolymers, crosslinkers, etc.) contains at least one polymerizable functional group, such as an ethylenically unsaturated group, such as (meth)acrylate, (meth)acrylamide, vinyl, N-vinyl lactam, N-vinyl amide, and styryl functionality.
[0069] In some embodiments, the polymerizable mixture contains at least one hydrophilic component, which in some embodiments can be selected from hydrophilic monomers, such as those known to be useful in preparing hydrogels.
[0070] In some embodiments, hydrophilic means that at least 5 grams of the compound(s) are soluble in 100 mL of deionized water at 25° C. under weakly acidic (pH 5-7) or basic (pH 7-9) conditions, and in some embodiments, 10 grams of the compound(s) are soluble in 100 mL of deionized water at 25° C. under weakly acidic or basic conditions.
[0071] In contrast to hydrophilicity, hydrophobicity means that 5 grams of a hydrophobic compound will not dissolve completely in 100 mL of deionized water at 25° C. under mildly acidic or basic conditions. The solubility of a compound may be confirmed by visual observation, where a visible precipitate or turbidity indicates that the compound is hydrophobic. Solubility may be determined after about 8 hours of mixing or stirring.
[0072] One class of suitable hydrophilic monomers includes acrylic or vinyl containing monomers. Such hydrophilic monomers may be used as crosslinkers themselves, but when hydrophilic monomers having one or more polymerizable functional groups are used, their concentration should be limited as described above to provide contact lenses with the desired elastic modulus.
[0073] The term vinyl-type or vinyl-containing monomer refers to a monomer that contains a vinyl group (-CH=CH2) and can be polymerized. Examples of hydrophilic vinyl-containing monomers include, but are not limited to, N-vinylamide, N-vinyllactam (e.g., N-vinylpyrrolidone (NVP)), N-vinyl-N-methylacetamide, N-vinyl-N-ethylacetamide, and N-vinyl-N-ethylformamide, N-vinylformamide, and other monomers. Alternative vinyl-containing monomers include, but are not limited to, 1-methyl-3-methylene-2-pyrrolidone, 1-methyl-5-methylene-2-pyrrolidone, and 5-methyl-3-methylene-2-pyrrolidone.
[0074] Acrylic monomers or acrylic-containing monomers are monomers that contain an acrylic group; (CH2=CRCOX), where R is H or CH3, and X is O or N, which are also known to polymerize readily, such as N,N-dimethylacrylamide (DMA), 2-hydroxyethyl methacrylate (HEMA), glycerol methacrylate, 2-hydroxyethyl methacrylamide, polyethylene glycol monomethacrylate, methacrylic acid, and mixtures thereof.
[0075] Other hydrophilic monomers that can be employed in the present invention include, but are not limited to, polyoxyethylene polyols in which one or more of the terminal hydroxyl groups are replaced with a functional group containing a polymerizable double bond.For example, polyethylene glycol, ethoxylated C1-20 alkyl glucoside, and ethoxylated bisphenol A may be reacted with one or more molar equivalents of end capping groups such as isocyanatoethyl methacrylate, methacrylic anhydride, methacryloyl chloride, vinylbenzoyl chloride, etc., to produce polyethylene polyols with one or more terminal polymerizable olefin groups attached to the polyethylene polyols via linking sites such as carbamate groups or ester groups.Other suitable hydrophilic monomers will be apparent to those skilled in the art.
[0076] In some embodiments, the hydrophilic component comprises at least one hydrophilic monomer, such as DMA, HEMA, glycerol methacrylate, 2-hydroxyethyl methacrylamide, NVP, N-vinyl-N-methylacrylamide, polyethylene glycol monomethacrylate, and combinations thereof. In another embodiment, the hydrophilic monomer comprises at least one of DMA, HEMA, NVP, and N-vinyl-N-methylacrylamide, and mixtures thereof. In another embodiment, the hydrophilic monomer comprises DMA and / or HEMA.
[0077] The hydrophilic component(s) (e.g., hydrophilic monomer(s)) may be present in a wide range of amounts depending on the particular balance of properties desired. In some embodiments, the amount of hydrophilic component is from 5 to 60% by weight, such as 40% by weight, based on the total reactive components.
[0078] A hydrophobic silicone-containing component (or silicone component) is one that contains at least one [-Si-O-Si] group in a monomer, macromer, or prepolymer. In some embodiments, the Si and attached O are present in the silicone-containing component in an amount greater than 20% by weight, such as greater than 30% by weight, based on the total molecular weight of the silicone-containing component. Useful silicone-containing components include polymerizable functional groups such as acrylate, methacrylate, acrylamide, methacrylamide, N-vinyl lactam, N-vinyl amide, and styryl functional groups.
[0079] Also, in some embodiments, crosslinking monomers may be employed alone or in combination and may include ethylene glycol dimethacrylate, trimethylolpropane trimethacrylate, glycerol trimethacrylate, polyethylene glycol dimethacrylate (wherein the polyethylene glycol has a molecular weight of, for example, up to 400), and other polyacrylate and polymethacrylate esters. The crosslinking monomers may be used in conventional amounts, for example, 0.1 to 5, preferably 0.2 to 3, based on 100 parts by weight of the polymerizable mixture.
[0080] Another monomer that may be used is methacrylic acid, which is used to affect the amount of water the hydrogel will absorb at equilibrium. Methacrylic acid is usually used in amounts of 0.2 to 8 parts by weight per 100 parts by weight of a hydrophilic monomer such as HEMA. Other monomers that may be present in the polymerization mixture include methoxyethyl methacrylate, acrylic acid, etc.
[0081] In an embodiment, the polymerizable mixture includes hydroxyethyl methacrylate (HEMA) or hydroxyethyl acrylate (HEA) monomers, preferably hydroxyethyl methacrylate (HEMA) monomers.
[0082] In embodiments, the polymerizable mixture includes a methacrylate or acrylate monomer that is not a hydroxyethyl methacrylate or hydroxyethyl acrylate monomer.
[0083] In embodiments, the polymerizable mixture includes a reactive silicone monomer or oligomer.
[0084] In a further embodiment, the polymerizable mixture after polymerization provides a polymer that is non-swellable in water, for example, a polymer that cannot take up more than 2% water by weight.
[0085] One or more polymerization initiators may be included in the polymerizable mixture. Examples of polymerization initiators include, but are not limited to, compounds that generate free radicals at moderately elevated temperatures, such as lauryl peroxide, benzoyl peroxide, isopropyl percarbonate, azobisisobutyronitrile, and the like, and photoinitiator systems, such as aromatic alpha-hydroxyketones, alkoxyoxybenzoins, acetophenones, acylphosphine oxides, bisacylphosphine oxides, and tertiary amines + diketones, mixtures thereof, and the like. Exemplary photoinitiators are 1-hydroxycyclohexyl phenyl ketone, 2-hydroxy-2-methyl-1-phenyl-propan-1-one, bis(2,6-dimethoxybenzoyl)-2,4-4-trimethyl)ylpentylphosphine oxide (DMBAPO), bis(2,4,6-trimethylbenzoyl)-phenylphosphine oxide (Irgacure 819), 2,4,6-trimethylbenzyldiphenylphosphine oxide and 2,4,6-trimethylbenzoyldiphenylphosphine oxide, benzoin methyl ester and camphorquinone in combination with ethyl 4-(N,N-dimethylamino)benzoate. Commercially available UV and visible light initiator systems include, but are not limited to, Irgacure 819® and Irgacure 1700® (from Ciba Specialty Chemicals), Lucirin TPO initiator (available from BASF). Commercially available UV photoinitiators include Irgacure 651, Darocur 1173, and Darocur 2959 (Ciba Specialty Chemicals). These and other photoinitiators may be used and are disclosed in "Photoinitiators for Free Radical Cationic and Anionic Photopolymerization, 2nd Edition," by JV Crivello & K. Dietliker, edited by G. Bradley, John Wiley and Sons, New York, 1998, Vol. 3.
[0086] In some embodiments, a polymerization initiator is included in the polymerizable mixture in an amount that may initiate polymerization of the polymerizable mixture, such as 0.1-2 wt.%. Polymerization of the polymerizable mixture may be initiated using an appropriate selection of heat or visible or ultraviolet light, or other energy, depending on the polymerization initiator used. Alternatively, in some embodiments, initiation may be performed without a photoinitiator, for example, using an e-beam. However, if a photoinitiator is used, the preferred initiator is a bisacylphosphine oxide, such as bis(2,4,6-trimethylbenzoyl)-phenylphosphine oxide (Irgacure 819®) or a combination of 1-hydroxycyclohexyl phenyl ketone and DMBAPO, and in another embodiment, the method of polymerization initiation is via visible light activation.
[0087] In some embodiments, the polymerizable mixture may include one or more internal wetting agents. Internal wetting agents include, but are not limited to, high molecular weight hydrophilic polymers. Examples of internal wetting agents include, but are not limited to, polyamides such as poly(N-vinylpyrrolidone) and poly(N-vinyl-N-methylacetamide).
[0088] The internal wetting agent(s) may be present in a wide range of amounts depending on the particular parameters desired, in some embodiments, the amount of wetting agent(s) is up to 50% by weight, such as 5-40% by weight, such as 6-30% by weight, based on the total reactive components.
[0089] Additionally, the polymerizable mixture may contain one or more auxiliary components selected from, but not limited to, chelating agents, polymerization inhibitors, viscosity modifiers, surface tension modifiers, glass transition modifiers, compatibilizing components, ultraviolet absorbing compounds, ophthalmic pharmaceutical agents, pharmaceutical agents such as ophthalmic anti-inflammatory agents, excipients, antimicrobial compounds, copolymerizable and non-polymerizable dyes, release agents, reactive tints, pigments, and chelating agents, and combinations thereof. In some embodiments, the total of such auxiliary components may be up to 20% by weight. Preferred embodiments may include a photoinitiator that generates reactive species when exposed to one or more of visible light, ultraviolet light, red light, and infrared light, and may include one or more of visible light, ultraviolet light, red light, and infrared light absorbing moieties.
[0090] The polymerizable mixture may be prepared, for example, by simply mixing the components of the mixture. In some embodiments, the reactive components (e.g., hydrophilic monomers, wetting agents, and / or other ingredients) are mixed together with an inert diluent to form the polymerizable mixture. Such diluents may have the effect of controlling the expansion of the formed ophthalmic device when hydrated, aiding in the solubility of the ingredients, and adjusting the glass transition temperature. Other embodiments may exclude the inert diluent.
[0091] Suitable classes of diluents include, but are not limited to, alcohols having 3-20 carbons, amides having 10-20 carbons derived from primary amines, ethers, polyethers, ketones having 3-10 carbons, and carboxylic acids having 8-20 carbons. As the carbon number increases, the number of polar moieties may also be increased to provide a desired level of water miscibility. In some embodiments, primary and tertiary alcohols are preferred. Preferred classes include alcohols having 4-20 carbons and carboxylic acids having 10-20 carbon atoms.
[0092] In some embodiments, the diluent is selected from 1,2-octanediol, t-amyl alcohol, 3-methyl-3-pentanol, decanoic acid, 3,7-dimethyl-3-octanol, 2-methyl-2-pentanol, 2-ethyl-1-butanol, 3,3-dimethyl-2-butanol, tripropylene methyl ether (TPMEX), butoxyethyl acetate, mixtures thereof, and the like.
[0093] In some embodiments, the diluent is selected to have some solubility in water, hi some embodiments, at least about 3% of the diluent is miscible with water. Examples of water soluble diluents include, but are not limited to, 1-octanol, 1-pentanol, 1-hexanol, 2-hexanol, 2-octanol, 3-methyl-3-pentanol, 2-pentanol, t-amyl alcohol, tert-butanol, 2-butanol, 1-butanol, ethanol, decanoic acid, octanoic acid, dodecanoic acid, 1-ethoxy-2-propanol, 1-tert-butoxy-2-propanol, EH-5 (available from Ethox Chemicals), 2,3,6,7-tetrahydroxy-2,3,6,7-tetramethyloctane, 9-(1-methylethyl)-2,5,8,10,13,16-hexaoxaheptadecane, 3,5,7,9,11,13-hexametrioxy-1-tetradecanol, mixtures thereof, and the like. Esters of alcohols, such as boric acid esters of alcohols, are other embodiments of diluents.
[0094] In some embodiments, the preferred amount of diluent is typically up to 60% by weight, such as 10-60% by weight, such as 20-50% by weight, based on the complete polymerizable mixture.
[0095] In another aspect, in some embodiments, the polymerizable mixture comprises one or more crosslinkers in an amount of 0.5-5.0 wt.%, one or more non-reactive diluents (e.g., polyhydric alcohols, esters of polyhydric alcohols, or ethers of polyhydric alcohols, such as, for example, glycerol and glycerol esters), and one or more polymerization inhibitors in an amount of less than 100.0 ppm, and preferably less than 50.0 ppm, based on the weight of the polymerizable mixture (e.g., glycerol and glycerol esters). The viscosity of the polymerizable mixture may also play an important role, typically 1-25 cP, e.g., 2-15 cP, especially 3-10 cP, although other viscosities are within the scope of the invention.
[0096] As mentioned above, the oxygen equilibrium concentration of the polymerizable mixture is preferably in the range of 0.05 to 8.0% by volume, for example 0.2 to 6.0% by volume, for example 0.5 to 6% by volume. The lower limits (0.05%, 0.1%, 0.2%, etc.) are stated for practical reasons, and it is quite possible to achieve even lower concentrations.
[0097] The oxygen content of the polymerizable mixture may be adjusted to a desired level (X) by exposing the polymerizable mixture (previously mixed under ambient atmosphere (1013 mbar, 21 vol% O2)) to a reduced pressure P, where P=X*1013 / 21 mbar. The reduced pressure (sometimes called "vacuum") may then be released and the oxygen-adjusted polymerizable mixture may be stored under an atmosphere having an oxygen concentration that corresponds to a suitable atmosphere having an oxygen concentration of X.
[0098] In some preferred embodiments, the oxygen concentration in the controlled ambient atmosphere surrounding the deposited polymerizable mixture, and the substrate in contact with the polymerizable mixture, is less than the equilibrium concentration of oxygen in the polymerizable mixture.
[0099] 3D printing device Deposition of multiple droplets is typically accomplished using an additive manufacturing print head. Such print heads are capable of simultaneous deposition of multiple droplets of liquid in either one-dimensional patterns (in the form of lines) or two-dimensional patterns. In some embodiments, the droplets are preferably in the picoliter range, such as about 3 picoliters to 20 picoliters per droplet, and preferably in the smaller range for additive manufacturing, such as 10 to 30 passes of the print head over the substrate.
[0100] In some embodiments, the desired speed and precision of deposition of multiple droplets may be achieved with an additive manufacturing print head capable of simultaneous deposition of two-dimensional patterns of polymerizable mixture, such that a pattern (or multiple successive patterns) of droplets of the polymerizable mixture may be printed that represents an integer map (e.g., a grayscale image) of the energy transmittance of an ophthalmic device.
[0101] In some preferred embodiments, such as those used to form the examples disclosed herein, a two-dimensional pattern representing an integer map of energy transmittance in the form of a grayscale image can be achieved in a single pass of a print head depositing droplets over an area at least the size of an ophthalmic device. Commercially available print heads suitable for this purpose include Fujifilm's Samba™ print heads, e.g., the Samba™ G3L print head, which has 2048 nozzles per module and is capable of depositing liquids with native drop sizes on the order of 2.4 picoliters to a maximum drop size of 13.2 picoliters with an accuracy of 1200 native dpi.
[0102] The pattern of each path of droplets deposited by the 3D printing device may be determined in relation to a desired transmittance pattern of the optical lens to be formed and a shape of the optical lens to be formed that correlates to the transmittance pattern. For example (in the case of an ophthalmic device), data collected from measuring a patient's eye may be used to generate the input. The data may include, for example, optical properties, surface properties, size and shape dimensions, observations of the state of eye disease, etc.
[0103] A three-dimensional (3D) printable model may be created based on a computer-aided design (CAD) pad cage or a scan of a patient's eye. A scan of a patient's eye may include collecting and analyzing digital data representative of the shape and appearance of the patient's eye. Based on the collected data, a three-dimensional model of a target ophthalmic device may be created. The three-dimensional model may be processed by software to convert the model into a grayscale image (or other energy intensity mapping) and generate a file containing instructions tailored to a particular type of 3D printer to repeatedly apply the polymerizable mixture according to the grayscale image or other energy transmittance pattern.
[0104] substrate The present invention provides for depositing a plurality of droplets of a polymerizable mixture onto a surface of a substrate. Suitable materials for the substrate include one or more of glass, polyolefins such as polypropylene, polystyrene, and other smooth materials.
[0105] In some preferred embodiments, the shape of the substrate represents the shape of one side of the resulting (non-hydrous) ophthalmic device, and may include at least a portion that is arcuate or otherwise curved for a contact lens and relatively flat for an intraocular lens. The size of the substrate is preferably adjusted to fit the required dimensions of the finished hydrous ophthalmic device. Substrates with an axis of rotation may be formed by one or more of lathing, grinding, and injection molding. Substrates that are not constrained to a shape with an axis of rotation may be made by other processes, such as 3D printing. The substrate may thus include a non-spherical optical surface shape, such as a substrate surface shape based on a portion of a patient's eye exposed to air.
[0106] In some embodiments, to tailor the wettability of the surface of the substrate receiving the polymerizable mixture, the surface of the substrate may be pretreated with one or more of a surfactant, UV exposure, ozone exposure, and plasma treatment, or a combination of these treatments. In some preferred embodiments, the receiving surface of a glass or polymer substrate may be pretreated with Tween 80, or a silicone surfactant such as Dow Corning Additive 67, Additive 14, Additive 57, Xiameter OFX-0193, etc. In some embodiments of the present invention, a surfactant may be included in the polymerizable mixture.
[0107] In some embodiments, the method of manufacturing an ophthalmic lens includes equilibrating the oxygen concentration in the substrate with the oxygen concentration in the controlled atmosphere. Similarly, in some preferred embodiments, the oxygen concentration in the substrate is equal to or less than the oxygen content of the polymerizable mixture deposited on the substrate.
[0108] The substrate may be allowed to be exposed to the controlled atmosphere (or a corresponding atmosphere) prior to deposition of the droplets for a period of, for example, at least 8 hours, in order to obtain an oxygen concentration in the substrate that is in equilibrium with the oxygen concentration in the controlled atmosphere.
[0109] In some embodiments, the substrate may have only a limited amount of oxygen available within it, and therefore special precautions may not need to be taken with regard to the oxygen concentration within the substrate.
[0110] In alternative embodiments, the substrate may itself be an ophthalmic device (e.g., a conventional commercial contact lens, etc.) that is modified by the methods described herein to form a final ophthalmic device (e.g., an ophthalmic device having one or more different optical properties, an ophthalmic device with an altered color pattern, an ophthalmic device having different physical properties, etc.).
[0111] Controlled atmosphere In some embodiments, the ambient atmosphere in which the deposition printing described herein occurs may be controlled. The controlled ambient atmosphere may include, by way of non-limiting example, a defined range of specific gases, a defined range of particulates, and / or a controlled wavelength of light or other energy. In some preferred embodiments, a suitably low concentration of oxygen is achieved in the atmosphere containing the polymerizable mixture such that the oxygen content of the polymerizable mixture is appropriately controlled. In some embodiments, the receiving surface of the substrate may be contained within a controlled ambient atmosphere.
[0112] As a specific, non-limiting example, in some embodiments, the controlled atmosphere has an oxygen concentration of at most 5.0% by volume. In some embodiments, the oxygen concentration in the controlled atmosphere is at most 2.0% by volume, such as 0.01-2.0% by volume, such as 0.03-1.5% by volume, such as 0.05-1.2% by volume, such as 0.1-1.1% by volume, more preferably at most 1.0% by volume. The lower limits (e.g., 0.01%, 0.03%, 0.05%, etc.) are stated for practical reasons, and even lower concentrations are fully achievable.
[0113] In another aspect, in some embodiments, the controlled atmosphere in which the deposition of the polymerizable mixture takes place is most conveniently 1.0 atm. (1013 mbar), which corresponds to an oxygen concentration of 21% by volume. Oxygen concentrations lower than the 21% by volume found in normal atmosphere may be suitably obtained by mixing atmospheric air with other gases, such as inert gases, such as one or more of nitrogen, helium, argon, or other inert gases, in some preferred embodiments.
[0114] In some embodiments, the controlled atmosphere may include an inert gas, such as nitrogen, mixed with a specific amount of pure oxygen. One preferred approach for a controlled atmosphere uses nitrogen as the inert gas to displace oxygen in the atmosphere, thereby achieving a desired level of oxygen concentration.
[0115] The oxygen concentration is monitored by an oximeter and adjusted one or more of before the additive manufacturing process, at the start of the additive manufacturing procedure, and during the manufacturing process, and may preferably also be intermittently or continuously controlled during the process of preparing one or both of the optical element and the substrate.
[0116] Droplet adhesion and hardening The method of the present invention involves successive deposition passes of multiple droplets of a polymerizable mixture under a controlled atmosphere onto one or both surfaces of a substrate and previously deposited droplets. The droplets of the polymerizable mixture are preferably ejected from a print head and deposited based on a two-dimensional pattern representative of an energy transmittance pattern, such as a grayscale image (or other light map representing light intensity). Following deposition of the droplets of the polymerizable mixture, the droplets may be exposed to a controlled amount of actinic radiation to induce a gelation process that pins the droplets of the polymerizable mixture in place relative to the substrate.
[0117] The polymerizable mixture is typically deposited using a 3D printing device, such as the printing devices described herein. In embodiments, the individual droplets have a volume of 0.5-50 pL, e.g., 1.5-30 pL, such as 1-40 pL, or 2.0-15 pL.
[0118] In some embodiments, each of the plurality of droplets of the polymerizable mixture is deposited on a surface relative to a substrate. The surface relative to the substrate may include droplets in contact with one or more of the top surface of the substrate, previously deposited droplets, and a molded article placed on one or both of the substrate and the previously deposited droplets of the polymerizable mixture. The polymerizable mixture deposited on the previously deposited polymerizable mixture may merge with the previously deposited polymerizable mixture such that a single mass of the polymerizable mixture forms on the substrate without a discernable layer. After contacting the surface, the polymerizable mixture may be exposed to limited actinic radiation or heat after deposition of the final layer of successive layers of droplets to form an ophthalmic device. The droplets of the polymerizable mixture deposited on the molded article may adhere to the molded article. The molded article may have a surface treated with a wetting agent.
[0119] In variations of the invention where successive layers of deposited polymerizable mixture are exposed to actinic radiation (e.g., UV light), the polymerizable mixture may include a photoinitiator. In variations of the invention where successive passes of polymerizable material are exposed to heat, the polymerizable mixture may include a thermal initiator.
[0120] In some variations of the invention, the continuous pattern is exposed to intermittent radiation (e.g., UV light) after each deposition of a layer of droplets. The degree of polymerization obtained by such intermittent exposure to actinic radiation is typically that required for the purpose of pinning or otherwise obtaining gelation of the polymerizable mixture so as to control the migration of the deposited droplets from a first location to another. In preferred embodiments, such control of migration allows a limited flow of the deposited polymerizable mixture, but prevents unlimited rearrangement of the deposited polymerizable mixture. For example, in some embodiments, the controlled migration allows gravity to merge the deposited droplets with the previously deposited polymerizable mixture, and then to fuse to the smoothed surface of the polymerizable mixture that is pinned in place by the gelation step.
[0121] In some embodiments of the present invention, multiple droplets of the polymerizable mixture are deposited onto a surface including one or both of a substrate and previously deposited polymerizable mixture, thereby forming a pattern of the polymerizable mixture having energy transmittance characteristics based on an integer map representing the energy transmittance, such as a two-dimensional grayscale image that is referenced to control a print head.
[0122] The deposited polymerizable mixture is preferably exposed to pinning actinic radiation after each pass (or several passes) of the print head that deposits the polymerizable mixture, and finally exposed to curing actinic radiation after deposition of the final pass of the print head that deposits droplets of the polymerizable mixture to form the optical element.
[0123] A pass of the print head may include one or both of the print head moving relative to the substrate on which the polymerizable mixture is received, the substrate and previously deposited polymerizable mixture moving relative to the print head, and / or the print head and substrate moving relative to each other as the polymerizable mixture is deposited. In some preferred embodiments, at least a portion of the pattern of polymerizable mixture deposited via subsequent passes of the print head after the first pass is combined with and integrated into the previously deposited polymerizable mixture, thereby forming a single volume of polymerizable mixture. Gravity induces limited movement of the deposited polymerizable mixture resulting in a smooth surface of the deposited polymerizable mixture, and gravity-based movement may be limited by surface tension and microforces. Preferably, the single volume of polymerizable mixture is pinned and / or gelled by exposure to a limited amount of actinic radiation, thereby limiting additional movement following the smoothing effect of gravity-induced movement.
[0124] In some versions of the invention, a series of successive passes, e.g., 2-20 passes, of a print head are deposited prior to exposure to intermittent actinic radiation effective to pin and / or gel the deposited polymerizable mixture. Prior to exposure to intermittent actinic radiation, the deposited polymerizable mixture may undergo migration confined to a single volumetric portion of the polymerizable mixture.
[0125] In some embodiments, the amount of polymerizable mixture deposited in one pass of the print head on any particular portion of the receiving surface may be up to 50 μm, but is preferably up to 25 μm.
[0126] In some variations of the invention, the polymerizable mixture includes multiple photoinitiators, with two or more photoinitiators responsive to different wavelengths of actinic radiation. This is particularly interesting when it is desirable to utilize one wavelength of UV light for intermittent exposure (for pinning or gelling) and another wavelength of UV light for the final curing of the deposited polymerizable mixture to form an optical element. Thus, in some variations of the invention, a first polymerization initiator is used (in conjunction with exposure to an appropriate first actinic radiation) to create a partially polymerized polymerizable mixture construct, and a second polymerization initiator is used (in conjunction with exposure to an appropriate second actinic radiation) to complete the curing step.
[0127] In addition to controlling the level of oxygen in the polymerizable mixture within a desired oxygen content range, some embodiments of the present invention include controlling the polymerization of the deposited polymerizable mixture to fabricate optical elements using the processes described in this disclosure, where the degree of polymerization of the deposited polymerizable mixture within a specified time frame after deposition is limited to a degree of gelation that stops or substantially slows the movement of the polymerizable mixture while allowing droplets from subsequent passes to merge with the previously deposited polymerizable mixture to form the structure of the optical element with limited strain.
[0128] The process for intermittent gelation is often referred to as pinning or gelling the deposited polymerizable mixture. In some versions of the invention, the pinning process may include applying a dose of actinic radiation at an intensity, wavelength and length of time suitable to cause gelation, such as, for example, application of ultraviolet (UV) light to a UV-curable polymerizable mixture and / or ink (UV ink). The wavelength of the actinic radiation may be matched to the photochemical properties of the polymerizable mixture and / or UV ink used in the manufacturing process.
[0129] As a result of the intermittent gelling, the deposited polymerizable mixture and / or ink droplets move to a higher viscosity state but do not fully cure. Variations of the present invention that include pinning or gelling (or gelling) improve the ability to control the flow and morphology of the deposited polymerizable mixture, thereby providing high optical quality in the formed optical element through final curing of the deposited polymerizable mixture. For example, sufficient flow is preferred to allow gravity to smooth the surface of the gelled polymerizable mixture but not significantly change the shape of the optical element. In some variations, other forces, such as centrifugal force, may be used to shape the surface.
[0130] The gelling and curing process may be modified based on the selection and / or concentration of one or more of the photoinitiator, crosslinker, source of actinic radiation (e.g., UV light source), intensity of actinic radiation, and exposure time. Examples of sources of actinic radiation may include light emitting diodes (LEDs) or light bulbs, lasers, etc.
[0131] In some specific embodiments, two photoinitiators absorbing at two different wavelengths are used with corresponding UV LED light sources (e.g., 365 nm and 400 nm). One initiator may be present at a concentration that can initiate gelation of the polymerizable mixture but is insufficient to complete polymerization. This allows the individual layers to reach the same relative degree of conversion before final curing. Final polymerization of the entire optical element may be performed as a separate step using another photoinitiator / UV LED light combination (e.g., actinic radiation energy of a second photoinitiator, or actinic radiation energy of a third photoinitiator, etc.), where the actinic radiation energy results in a uniform polymer network required for optical functionality.
[0132] Alternatively here, a thermal initiator active above Tg may be used in place of or in addition to a second (or other) photoinitiator to complete the curing of the deposited polymerizable mixture. The present invention also provides that without control of the oxygen content of the deposited polymerizable mixture throughout the deposition process steps and during the final curing step, oxygen inhibition effects can adversely affect the uniformity of the polymer network, leading to the production of incompletely cured polymers and therefore devices with sticky surfaces.
[0133] In some embodiments, when the polymerizable mixture is deposited on a curved surface, an initial deposit, or multiple deposits, according to the methods described herein, may be deposited on the curved surface as a pattern of droplets of the polymerizable mixture, the pattern of droplets including a volume and distribution that allows surface tension forces to maintain the pattern of droplets of the polymerizable mixture in a confined flow or other movement until partially cured in a gelation step that pins the deposited polymerizable mixture in place.
[0134] Subsequent depositions of additional droplets from the print head may fill in the spaces left by the initial deposition or subsequent layers until the surface of the receiving substrate is completely covered and established as a base for building optical elements thereon. Alternatives to dot patterns include depositing droplets to form very thin layers (e.g., 1 micron to 8 microns) and building optical elements on such very thin layers with the processes disclosed herein.
[0135] In some embodiments, it is useful to isolate the print head containing the monomer from receiving exposure to actinic radiation, such as UV radiation, to prevent premature gelation or polymerization of the monomer in the print head, which could render the print head inoperable or operable at a reduced performance level. Isolation from actinic radiation is particularly important when using reactive monomers that contain low levels of inhibitors and / or when using the print head in environments with low oxygen levels.
[0136] For purposes of achieving simultaneous printing and pinning of materials to stop or slow the movement of the ink or polymerizable mixture once deposited, some embodiments of the present invention include an apparatus operable to isolate the actinic radiation source (e.g., a UV light source) from the print head to essentially eliminate or substantially reduce the possibility of gelling / polymerization of the polymerizable mixture within the print head. Isolating the print head from the actinic radiation source and controlling both the oxygen levels and the movement of the polymerizable mixture allows precise geometries and optical devices to be produced without artifacts within the matrix that adversely affect the optical performance of the final lens produced.
[0137] In some embodiments, after the multiple deposition and gelling steps of the polymerizable mixture(s) are completed but before the final curing step is performed, it is preferred to wash the gelled and deposited polymerizable mixture with a solvent or water, e.g., to remove excess monomer.
[0138] Referring now to FIG. 1, a schematic diagram illustrates an example of an additive manufacturing system 100 comprising an apparatus and underlying software that, when executed, enables the apparatus to operate. As shown, the additive manufacturing system 100 includes one or more additive manufacturing printing devices 101-102 operable to deposit droplets 110 of a polymerizable mixture 103 in a pattern of energy intensity and / or energy transmittance (e.g., a grayscale pattern) onto a receiving surface 103A supported by a substrate 104. The receiving portion 104A of the substrate 104 may be smooth or arcuate, suitable as the back curve of a contact lens. The receiving surface 103A may include one or both of a given receiving portion 104A of the substrate 104 and a previously deposited polymerizable mixture 103.
[0139] One or more actinic radiation sources 105 and 106 (which may include LEDs that emit energy at the same wavelength or different wavelengths).
[0140] Some variations of the invention include a housing 114 having one or more ports 107 and 108 for providing a controlled atmosphere 109 within the housing 114. The housing 114 may contain an atmosphere surrounding and containing one or more of the substrate 104, the printing devices 101-102, the droplets 110, the polymerizable mixture from the deposited polymerizable mixture 103 accumulated on the substrate (positioned to form an ophthalmic lens, such as a contact lens), and the source of actinic radiation 105-106.
[0141] In some embodiments, the substrate 104 is positioned proximate to, for example below, at least one 3D printing device 101-1-2. The relationship of below or below is derived from the direction of gravity. The printing devices 101-102 are operative to eject droplets of the polymerizable mixture 110 onto a receiving surface 103A. The receiving surface 103A may include one or more of the surface of the receiving portion 104A of the substrate 104, the surface of a previously deposited polymerizable mixture 103, and the receiving portion of an insert such as a rigid lens or electronic device. The droplets are deposited in a pattern that reproduces an energy transmittance pattern such as a grayscale image. Successive depositions of the pattern are assembled to form a volume of the polymerizable mixture in the desired shape of the target optical element (see, for example, FIGS. 4,-5).
[0142] After applying a droplet 110 of the polymerizable mixture to a receiving surface 103A to form a volume of polymerizable mixture 103, the polymerizable mixture may be exposed to a first dose of actinic radiation, which is in a first wavelength range, for a first duration, and at a first intensity (such as, for example, ultraviolet light or blue light). In some embodiments, the first range of doses of actinic radiation may be delivered to the deposited polymerizable mixture via a first source of actinic radiation 105. Final curing may be achieved by exposing the aggregated polymerizable mixture to a second dose of actinic radiation, which includes a second range of wavelengths, a second duration, and a second intensity, which may be delivered from the same actinic radiation source 105 or a different actinic radiation source 106. The final curing will enable a molded article, such as an ophthalmic lens 111, to be removed from the substrate.
[0143] In some variations of the invention, a final curing process step may additionally be carried out in an environment having a controlled temperature, for example at an elevated temperature above ambient room temperature.
[0144] According to some embodiments, a first print head 101 of the system 100 may provide a first polymerizable mixture and a second print head 102 may provide a second polymerizable mixture, which may be compositionally the same or different from the first polymerizable mixture, which may include a functional additive or a non-polymerizable mixture (e.g., a functional additive or a solvent containing a functional additive).
[0145] The ambient conditions within the system 100 may be controlled, for example, particularly with respect to the oxygen content of the controlled atmosphere 109, and in some embodiments, the temperature, ambient light, amount of particulates, size of particulates, circulation or other movement of the ambient atmosphere, and virtually any variable that may affect one or more of the movement of the unpinned, unpolymerized deposited polymerizable mixture, the polymerization of the deposited polymerizable mixture, and the shape of the device formed by the polymerization of the deposited polymerizable mixture.
[0146] Provided that the substrate 104 is transmissive or transparent to actinic radiation, the sources of radiation 105 and / or 106 may be positioned individually or in alternating combinations below the substrate 104 or at an angle to the substrate 104, similar to that shown in Figure 1. In addition, shutters or other actinic radiation shields may be positioned above or laterally to the receiving surface, positioned and operative to shield the print head from actinic radiation or other actinic radiation conditions.
[0147] The nature of the surrounding gaseous environment may be controlled, for example, by the use of nitrogen gas purging through inlets 107, 108. Purging may be performed to increase or decrease the oxygen partial pressure to a predetermined level.
[0148] Referring now to Figure 2, a schematic diagram illustrates several alternative aspects that may be incorporated into a 3D additive manufacturing system 200. Some of the same reference numbers as in Figure 1 are used (e.g., 3D print heads 101-102, actinic radiation sources 105 and 106, substrate 104, housing 114 with one or more ports 107 and 108, and a controlled atmosphere for the deposited polymerizable mixture 110). Additionally, the embodiment illustrated in Figure 2 includes an oxygen sensor 204, a gate 205 for moving components in and out of housing 114, a UV blocking screen 112, and an actuation structure 203 (e.g., a belt drive or a stepper motor linear drive) configured to provide relative movement between substrate 104 and one or more 3D print heads 101-102 and / or one or more actinic radiation sources 105-106.
[0149] The illustrated 3D printing system 200, as shown in FIG. 2, is similar to that of FIG. 1 and also includes one or more actuators 201-203 configured (and operable) to provide relative movement between the substrate 104 and one or more of the 3D print heads 101-102, the actinic radiation sources 105-106, and, in some embodiments, the shielding screen 112 and / or the housing. In some embodiments, the print head actuator 201 is configured (and operable) to move one or more of the print heads 101-102 relative to the substrate 104. Similarly, the radiation source actuator 203 is configured (and / or operable) to move one or more of the actinic radiation sources 105-106 relative to the substrate 104. The substrate actuator 203 is configured (and / or operable) to move the substrate 104 relative to one or both of the print heads 101-102 and the actinic radiation sources 105-106. Although a belt drive 203A is shown as the actuating structure 203 and stepper motor tracks are shown as the actuating structures 201-202, other devices and apparatus are within the scope of the invention. The actuating structures 201-203 may be synchronized such that relative movement between the substrate 104, the print heads 101-102, and one or more of the actinic radiation sources 105-106 may be coordinated with the deposition of the polymerizable material 110 from the print head(s) 101-102.
[0150] The processes presented herein may be implemented in the described systems 100, 200 to form an optical element 211. The processes may include operation of one or more print heads 101-102 having a first print head 101 that ejects droplets 110 of a first polymerizable mixture, and one or more additional print head(s) 102 that eject droplets 110A of a composition that may include the first polymerizable mixture, a second polymerizable mixture that is compositionally different from the first polymerizable mixture, and a non-polymerizable substance or mixture.
[0151] In some embodiments, one or more of the first polymerizable mixture, the second polymerizable mixture, and the non-polymerizable mixture include one or more functionally active substances, e.g., substances in dissolved form.
[0152] Release of Ophthalmic Device from Substrate and Post-Processing After sufficient deposition of the polymerizable mixture 103 to form the optical element 211 (e.g., an ophthalmic device) and performing a curing step, the optical element 211 is typically released from the substrate. The polymerizable mixture 103 deposited in a particular pattern to form the optical element 211 is preferably sufficiently physically bonded to the substrate 104 during preparation of the optical element 211 to prevent unwanted movement relative to the substrate 104, but the polymerizable mixture 103 should not be bonded so securely that removal of the optical element 211 from the substrate 104 would damage the optical element 211. For example, in some embodiments, care should be taken to avoid the formation of covalent bonds between the polymerizable mixture 103 and the substrate 104 during preparation of the optical element 211, including curing of the polymerizable mixture 103.
[0153] The optical device 211 may be released (or otherwise removed) from the substrate 104 by physical means to allow the optical element 211 to be manipulated in various ways. For example, the optical element may be manipulated via one or more of washing the optical element 211 to remove by-products, soaking the optical element 211 in a buffered saline solution, staining, marking, and packaging the optical element 211. For example, in some variations of the invention, the optical element 211 may be soaked in one or both of water and a solution, such as a buffered saline solution, sufficiently so that the optical element 211 swells. The swelling facilitates the release of the optical element 211 from the substrate 104. The solution may also include one or more release agents. The release agent may include a compound, or a mixture of compounds, that when combined with water, reduces the time required to release the optical element 211 from the substrate 104 compared to the time required to release such an optical element 211 using an aqueous solution that does not include a release agent.
[0154] Although typically preferred, it is not strictly necessary that curing of optical element 211 be completed before release from substrate 104 .
[0155] In some embodiments, after curing, the optical element 211 is subjected to one or more extraction process steps to remove unreacted components from the optical element 211. The extraction process steps may be performed using one or more of a conventional extraction fluid, an organic solvent, an alcohol, water (or an aqueous solution such as buffered saline). In various embodiments, the extraction may be accomplished, for example, by immersion of the lens in an aqueous solution or exposure of the lens to a stream of an aqueous solution. In various embodiments, the extraction may also include, for example, one or more of the following: heating the aqueous solution, agitating the aqueous solution, increasing the level of a release aid in the aqueous solution to a level sufficient to cause release of the lens, mechanically or ultrasonically agitating the lens, and incorporating at least one elution aid in the aqueous solution to a level sufficient to sufficiently remove unreacted components from the lens. The above may be performed in a batch or continuous process, with or without the addition of heat, agitation, or both. The ophthalmic device may also be sterilized by known means, such as, but not limited to, autoclaving and radiation sterilization. Sterilization may occur before or after packaging the optical element 211 in a suitable storage container, and is preferably performed after packaging. In some preferred embodiments, the optical element 211 is packaged in an aqueous solution.
[0156] For optical elements 211 formed of hydrogel, packaging may include packaging in a saline solution having about 0.9% sodium chloride and a suitable buffer, such as a phosphate or borate buffer system. Additionally, the packaging solution may include one or more functionally active agents, including biologically active agents.
[0157] The aqueous solution may also contain additional water-soluble ingredients such as release agents, wetting agents, lubricants, active pharmaceutical ingredients (APIs), vitamins, antioxidants, and nutraceutical ingredients, combinations thereof, and the like. In some embodiments, the aqueous solution contains less than 10% by weight, in other embodiments less than 5% by weight, of an organic solvent such as isopropyl alcohol, and in other embodiments no organic solvent. Depending on the composition of the aqueous solution. The aqueous solution may or may not require special handling, such as purification, recycling, or special disposal procedures.
[0158] In some embodiments, the aqueous content of the hydrogel optical element 211 comprises at least 30% water by weight, in some embodiments at least 50% water by weight, in some embodiments at least 70% water by weight, and in other embodiments at least 90% water by weight.
[0159] In a variant of the invention, the polymerizable mixture 110 comprises a hydroxyethyl methacrylate (HEMA) monomer and the method comprises the next step of swelling the optical element, preferably an ophthalmic device, in water, whereby the optical element obtains a water content of 10-80% by weight, preferably 35-70% by weight.
[0160] In an embodiment, the polymerizable mixture 110 includes acrylate monomers that are free of HEMA monomers, and the method includes a subsequent step of swelling the optical element, preferably an ophthalmic device, in water, whereby the optical element achieves a water content of 10-80% by weight, preferably 35-70% by weight.
[0161] In an embodiment, the polymerizable mixture 110 comprises a reactive silicone precursor and the method comprises the next step of swelling the optical element, preferably an ophthalmic device, in water, whereby the optical element obtains a water content of 5-70% by weight, preferably 10-50% by weight.
[0162] Novel Ophthalmic Devices The methods and apparatus of the present invention allow for the creation of optical elements 211 with previously unobtainable designs, such as one or more of the following, as non-limiting examples: contact lenses or intraocular lenses with non-rotationally symmetric surfaces with corresponding optical corrections, including very steep radii of curvature and very high spherical and cylindrical correction components; contact lenses or intraocular lenses that include multiple spherical and cylindrical corrections in the same lens, as opposed to a single spherical correction power, and that include a spherical correction power that reflects the power distribution map of the eye, not just the average correction power of the refractive power from a phoropter or refractometer; contact lenses or intraocular lenses that can correct (due to non-rotational symmetry) optical aberrations resulting from poor surgical results of PRK or LASIK or LASER surgery or aberrations resulting from abnormal comal surfaces.
[0163] Additive manufacturing based on iterative grayscale images Referring now to FIG. 3 , an exemplary energy transmittance pattern, such as grayscale image 300, may be used to create additive manufacturing control commands that control the emission of droplets of a polymerizable mixture in a pattern that replicates grayscale image 300.
[0164] For example, in some embodiments, a map of data is used that represents, either directly or by titration conversion, the amount of polymerizable mixture deposited at a given location that corresponds to a data value associated with a pixel included in the grayscale image 300, such as an integer map. In other embodiments, the value associated with the pixel may be a floating point or other representation of a real integer. The data value may correspond to an amount of energy transmittance at the pixel location, and the data value may be accessed electronically, and a processor executing software commands may convert the data value into additive manufacturing print head control commands. The print head control commands are executable to control, on a pixel-by-pixel basis, the deposition of the polymerizable mixture at a location that corresponds to a pattern that replicates the grayscale image 300. For example, a data value having a relatively large digital number value may correspond to a darker region of the grayscale image 300 and may correspond to the emission of a larger amount of polymerizable mixture from the print head than the emission corresponding to a lighter region of the grayscale image. A larger amount of polymerizable mixture may be assigned to a thicker deposit 301, and the control command value may be assigned by conversion of the grayscale value at the location of the thicker deposit 301 to a print head control command value for the thicker deposit 301. Similarly, smaller values included in the grayscale may correspond to thinner deposits 301A, and appropriate print head control command values may be assigned by conversion of the smaller grayscale values to appropriate control command values for the thinner deposits 301A.
[0165] In some examples, the thicker deposit 301 may be formed by printing a relatively larger amount of polymerizable mixture at a particular location of the receiving surface during a pass of the 3D print head over the printed receiving surface, and the thinner deposit 301A may correspond to printing a relatively smaller amount of polymerizable mixture at the location of the thinner deposit 301A. The thicker amount 301 may correspond to a relatively darker portion of the grayscale image 300, and the thinner amount 301A may correspond to a relatively lighter portion of the grayscale image 300.
[0166] In accordance with the present invention, following each pass of the print head and associated deposition of the polymerizable mixture, the deposited polymerizable mixture may be allowed to "sit" for a short period of time to allow the material to be acted upon by physical forces such as gravity, surface tension, and microforces to modify the surface characteristics. Modifying the surface characteristics may include, by way of non-limiting example, one or more of leveling high and low areas formed during the deposition process, smoothing the surface of the deposited polymerizable mixture, allowing the deposited polymerizable mixture to flow into intervening areas, and forming uniform edges of the deposited polymerizable mixture.
[0167] In essence, the present invention is also capable of a top surface 302 that is formed by physical forces present in nature, as opposed to a manufactured surface, such as a mold surface and / or a turned surface. Gravity will smooth the top surface of the deposited polymerizable mixture before it undergoes a gelation process, such as being pinned by exposure to a controlled amount of actinic radiation.
[0168] In some variations of the invention, control commands may be used to determine how many passes of the 3D print head over the receiving surface. The number of passes of the 3D print head may correlate with the thickness of the deposited polymerizable mixture and may also correlate with the amount of energy transmittance at a particular location of the pattern of the deposited polymerizable mixture. In this manner, the deposited polymerizable mixture may be deposited, pinned, and finally cured in a shape and volume suitable for forming an ophthalmic lens having the desired ophthalmic quality. The deposited polymerizable mixture achieves sufficient thickness and appropriate shape through repeated application of the corresponding grayscale image.
[0169] In some variations of the invention, each pass of the 3D print head may print a pattern of the polymerizable mixture corresponding to the same grayscale image, while in other embodiments, different passes of the 3D print head may correspond to different grayscale images than the previous pass. As previously mentioned, in some variations of the invention, each pass of the 3D print head depositing the polymerizable mixture may be followed by exposure of the polymerizable mixture to a gelling process, such as actinic radiation, thermal activation, or the like, in an amount sufficient to partially polymerize the deposited polymerizable mixture. A curing process may be completed after the final pass of the polymerizable mixture is completed. In various embodiments, the final layer may be exposed to a pinning step and / or may move directly to a full curing process.
[0170] Curing and / or pinning may be facilitated by the inclusion of one or more photoinitiators in the deposited monomer. Photoinitiators may include, by way of non-limiting example, initiators activated by energies of about 392 nM and 400 nM.
[0171] In some examples, an energy transmittance pattern (e.g., a grayscale image) may be derived from the physical form of the molded article which may be processed, such as via optical scanning, image capture, or photography, to capture the energy transmittance data in electronic form, such as digital data values, which may be converted into control commands.
[0172] Some variations of the invention involve grayscale images having a generally spherical shape, with smaller values associated with thicker deposits, and therefore different transformation protocols may be assigned to different grayscale images depending on which values correspond to thick and thin deposits, respectively.
[0173] In some examples, a single grayscale image may be used to represent a desired product lens and associated control commands, which may be repeatedly deposited with successive passes of a 3D print head until the desired optical qualities are embodied in the deposited polymerizable mixture, which then hardens to form a molded article that also meets suitable physical parameters for placement in a patient's eye.
[0174] In another example, a series of grayscale images may be assembled to create a set of control commands. The control commands may result in the deposition of different shape designs to physically create an additive composite of the images. In another example, the grayscale images may be combined and processed before any processing occurs. In some examples, the combination of the images may be normalized to accommodate upper and lower thickness factors.
[0175] In some embodiments, different features such as edge profile 303, alignment features, etc. may be programmed into the optical element command protocol by adding a grayscale image to the lens profile.
[0176] In some examples, the refractive elements may be designed at a surface plane location as an array of grayscale values, where the values correspond to a thickness or range of thicknesses added in the printing process. In similar examples, a certain grayscale value may correspond to a plano lens element that adds no refractive power to any underlying structure.
[0177] In some examples, the grayscale image may be referenced from multiple file types, such as one or more of, by way of non-limiting example, jpeg, tiff, bmp, png, etc., and may be used to create a control command protocol for printing a desired part, such as an ophthalmic lens part, by varying the amount of polymerizable mixture deposited at discrete locations, resulting in greater deposition of polymerizable mixture in areas targeted for thicker deposition. Printing the entire pattern may result in a part without intervening areas.
[0178] In some variations of the invention, the gray scale of the image or the additive combination of images may correspond to the processing of multiple disjoint passes of the 3D printing head, where the amount of polymerizable mixture deposited at a particular location is subjected to a pinning step before the next deposition pass is completed. The polymerizable mixture deposited between the passes of the printing step may be a monomer mixture with various contained photoinitiators. One of the photoinitiators may be associated with the wavelength of actinic radiation during the associated pinning step. After the multiple printing passes have been processed, the entire volume of the polymerizable mixture deposited on the receiving substrate may be subjected to a curing step. In some examples, the curing step may be exposure to actinic radiation of different wavelengths and exposure times, intensities, etc.
[0179] In another aspect, in some embodiments, the grayscale or energy transmittance pattern may be dithered via a dithering process or algorithm prior to generation of printhead control commands based on the grayscale or energy transmittance pattern in order to generate a smoother image deposited via droplet ejection from the printhead and accumulation prior to curing. Dithering may include, by way of non-limiting example, processes consistent with Floyd-Steinberg, Burkes, Sierra, Two Row Sierra, Jarvis, Stevenson, Arce, or other processes.
[0180] 4, an optical element 400 is shown in accordance with some embodiments of the present invention. The optical element 400 includes a peripheral portion 401, which may be printed or otherwise formed prior to the optical zone portion 402 of the optical element 400. A lens carrier portion 403 may transition between the optical zone portion 402 and the peripheral portion 401. The carrier portion 403 is preferably of a size and shape suitable for comfortably maintaining the finished lens in place on the wearer's eye. During additive manufacturing of the optical element 400, the polymerizable mixture included in the peripheral portion 401 may be deposited and pinned, but not fully polymerized, before the polymerizable mixture included in the optical zone portion 402 is printed and pinned. In some preferred embodiments, the peripheral portion 401 may include a greater mass such that as the polymerizable mixture hardens into a polymer, stresses resulting from the polymerization process do not deform the optical zone portion 402 due to the stabilizing influence of the greater mass of the peripheral portion 401.
[0181] In some embodiments, the peripheral portion 401 may remain with the optical element 400 to form a pleasing edge feature. In other embodiments, some or all of the peripheral portion 401 may be removed, for example, by laser trimming.
[0182] An embodiment including a more massive peripheral zone portion 401 may be formed via the following steps: a) printing or otherwise depositing a polymerizable mixture in the peripheral zone portion (which may have a generally annular shape for spherical lenses, or a corresponding peripheral shape such as an oval or almond shape for other lenses); b) pinning the polymerizable mixture in the peripheral zone portion 401, preferably after each pass of the print head depositing the monomer; c) printing or depositing the polymerizable mixture in the optical zone; pinning the polymerizable mixture in the optical zone; and curing the deposited polymerizable mixture. Some embodiments may further include placing a cap on the optical zone to provide optical quality.
[0183] 5, a side cutaway view is shown having a peripheral portion 501 and a carrier portion 502 that supports an optical insert or cap 504 and an optical zone 503. In some embodiments of the invention, the peripheral portion 501 may include a greater mass than the carrier portion 502 and / or the optical zone 503 portions of the lens 500.
[0184] Generation of axial thickness profile Hydrated contact lens front curvature radius (R F ) is the lens power in air (P), the lens refractive index (n), the center thickness (CT), and the posterior surface radius of curvature (R B ) is generated from the thick lens formula:
[0185] Formulas for thick lenses may include, by way of non-limiting example, the following: The effective focal length for a principal plane of a thick lens is given by:
[0186]
number
[0187] The distance from the apex of the lens to the principal plane is
[0188]
number
[0189] For ophthalmic lenses, example variables may include:
[0190]
number
[0191] The anterior and posterior optical zone surfaces may be generated from the anterior and posterior radii of curvature of the spectacle lens and the central thicknesses of the other optical elements.
[0192] An exemplary surface is shown in FIG. 6 for a −3.0D design with a center thickness of 0.1008 mm, a rear radius of curvature of 9.1 mm, and a refractive index of 1.4055.
[0193] In some embodiments, the axial thickness profile may be generated by subtracting the aft surface position from the leading surface position for multiple radial positions.
[0194] The ratio of hydrated to non-hydrated lenses may vary based on lens material, with hydrated lenses being 1.4 times larger in each direction than non-hydrated lenses. Thus, the axial thickness profile of a non-hydrated lens may be about 1.4 times smaller (as used herein, the term about may be within 10% of the stated amount) than the axial thickness profile generated from the hydrated lens anterior and posterior surfaces. Also, the radial position may be about 1.4 times smaller for the non-hydrated lens.
[0195] Referring now to FIG. 6, there is shown a graphical representation 600 of the optical zone anterior curved surface 603 and posterior curved surface 604 of a wet ophthalmic lens.
[0196] The graphical representation 600 includes a first axis having a scale of water-containing surface position 601 and a second axis having a scale of water-containing radial position 602. The first curve maps values of an anterior curve 603 and the second curve maps values of a posterior curve 604 of the ophthalmic lens optical zone.
[0197] 7, a graphical representation 700 of the axial thickness profile 703 of a non-hydrated ophthalmic lens optical zone is shown. In a preferred embodiment, the axial thickness profile may be suitably described by an even fourth order polynomial. Coefficients from this model may be referenced to generate the optical zone portion of a grayscale print pattern, or other energy transmittance or energy intensity map pattern.
[0198] The graphical representation 700 includes a first axis having a scale of water-free axial thickness 701 and a second axis having a scale of water-free radial position 702. A curve maps values of axial thickness 703 of the ophthalmic lens optical zone, with a numerical value correlating to thickness 704 displayed in the center of the graphical representation 700.
[0199] In astigmatism lenses, the optical power is different for different directions (meridians) in the optical zone. For example, -2.75D / -4.5DX90 has a power of -2.75D vertically and -7.5D horizontally. The resulting axial thickness profile varies meridian-wise within the optical zone, being "flattest" vertically and "steepest" horizontally.
[0200] Referring now to FIG. 8, a false color image of thickness profile 800 is shown for the optical zone, with a "first intensity 801 representing a small thickness and a fourth intensity 804 representing an area having a relatively large thickness. One or more intermediate thicknesses 802-803 may also be included, such as a first intermediate thickness 802 and a second intermediate thickness 803. Each thickness may be achieved by depositing an appropriate amount of polymerizable mixture at a respective location indicated by thickness profile 800, allowing the polymerizable mixture to settle, pinning the settled polymerizable mixture in place via a gelling process, and finally curing the deposited and pinned polymerizable mixture.
[0201] The horizontal (most negative power) and vertical (most positive power) axial thickness profiles may be modeled by an even fourth order polynomial, the coefficients of which are used to generate the optical zone grayscale print pattern represented by thickness profile 800.
[0202] Energy transmittance printing pattern generation In some embodiments, the energy transmittance print pattern (which may be a grayscale print pattern or other representation of energy intensity) may include two (2) or more regions: optical zones 801-804 (exemplarily defined by an axial thickness profile): and a periphery 805. Other regions may also be included, such as regions containing pharmaceuticals or other elutable substances. Each region may be defined in various ways. For example, as a non-limiting example, the pixel size of the print pattern may be defined as approximately 0.021 mm. The diameter of a non-hydrated lens may be, for example, 10.0 mm. The number of pixels in the X & Y directions is defined by the following relationship:
[0203]
number
[0204] This definition is pixels is an odd number, ensuring that the center of the lens is at the center of the printed pattern.
[0205] Many grayscale levels may be specified, for example an 8-bit (255 gray levels) print pattern. It is within the scope of the present invention to vary both of these values, which may affect the quality of the printed lens.
[0206] spherical surface A spherical lens includes an optical zone that is generally rotationally symmetric (within 10% of symmetry) and may be defined, for example, by using the central thickness of a non-hydrated lens and coefficients from an even fourth order model:
[0207]
number
[0208] Here, (x0, y x ) is the focus of the printed pattern. Other variations are within the scope of the invention.
[0209] The center thickness (CT) used to generate the thickness profile may be based on the wet thickness for the layer thickness times the number of layers printed. Thus, if the wet lens CT is 0.120 mm, the number of layers to print is 6, and the layer thickness is 0.012 mm, then the CT used to generate the printed pattern is 0.120 mm-0.72 mm=0.048 mm.
[0210] In some preferred embodiments, this may be done to ensure that the ratio of the "lightest" to the "darkest" pixels in the pattern remains within an acceptable range for printing. In other embodiments, the image may be converted to a binary image by the print head controller software. If the grayscale range is too large, the "light" areas may not have enough "dark" pixels to form a smooth lens surface.
[0211] The thickness is defined as r = semidiameter of the water-free optical zone (r max ), typically may be calculated for pixels smaller than 4.0mm / 1.4 (~2.857mm).
[0212] The periphery 805 is the area where r (mm) is outside the optical zones 801-804 but within the lens diameter. Many different methods may be used to define the peripheral thickness profile. For example, in some preferred embodiments, the pattern uses the thickness at the edge of the optical zone for every pixel of the periphery. Alternative methods may include one or more of the following: linearly tapering the thickness from a value at the edge of the optic to a value defined at the "edge" of the lens; and tapering the thickness using a higher order polynomial or conic section from a value at the edge of the optic to a value defined at the "edge" of the lens; adding a "stiffening" ring to the periphery to improve handling of the lens; tapering using different methods in different zones of the periphery; and a combination of tapering and "stiffening" rings.
[0213] Toric (Astigmatism Lenses) The optical zone may not be rotationally symmetric and may be defined using the thickness of the non-hydrated lens center, two sets of coefficients from an even quartic model of the most positive and most negative power meridians, and the desired angle in the print pattern of the most positive power meridian.
[0214] For example, in some embodiments, the print pattern is generated by calculating the "effective" quadratic coefficients for each principal meridian:
[0215]
number
[0216] The "equivalent" r2 coefficient is defined as the average of the two effective coefficients. The astigmatism coefficient is defined as:
[0217]
number
[0218] Here, C 2,effective,plus is the effective second coefficient of the most positive meridian, and C 2,effective,minus is the effective second coefficient of the most negative meridian. For each pixel of the lens print pattern, its distance from the lens center (r(x,y)) and its angle in standard Cartesian coordinates (θ(x,y)) are calculated.
[0219] The optical zone thickness may be defined as:
[0220]
number
[0221] where φ is the angle of the most positive meridian.
[0222] The thickness at the edge of the optical zone varies with angle. For toric print patterns, a transition zone may be created to provide a single thickness value for all angles. The transition zone may be a 0.5 mm wide annular shape for hydrated lenses (0.5 mm / 1.4 for non-hydrated lenses). The target thickness for the transition may be equal to the minimum thickness at the boundary of the optical zone, or may be essentially equal to:
[0223]
number
[0224] The thickness of each pixel in the transition region is defined as a linear function of its radial position. The thickness at the optical zone edge is defined for each pixel in the transition region as:
[0225]
number
[0226] The slope of each point is defined as:
[0227]
number
[0228] The intercepts for each point are defined as follows:
[0229]
number
[0230] The thickness of each point in the transition region is defined as follows;
[0231]
number
[0232] 9, an exemplary graphical image of a transition region is shown. The peripheral axial thickness profile 900 is defined by a linear change from the end of the transition zone 904 to the minimum axial thickness of the optical zone 901. The slope and intercept of the peripheral points 902-903 are defined in the same manner as used to define the transition zone, only using the transition zone edge and minimum thickness for the end of the optical zone thickness and the end of the transition zone thickness, respectively. All pixels outside the lens diameter may be set to 0. FIG. 10 illustrates a thickness profile of a peripheral region 1000 of an ophthalmic lens having a number of different thicknesses 1002-1004 in the peripheral region of an optical zone 1001. 11 illustrates a thickness profile of a complete ophthalmic lens 1100. The illustrated thickness profile includes lens portions 1101-1105, which include optic zones 1101-1104 and a peripheral region 1105. Each of the lens portions 1101-1105 includes one or more pixels 1106 (shown in an expanded view). Each pixel 1106 may be associated with a thickness.
[0233] Printing Pattern
[0234] In some embodiments of an energy transmittance pattern (e.g., and energy intensity pattern or grayscale pattern) corresponding to a printed pattern, "light" pixels may represent unprinted areas and "dark" pixels may represent areas that receive deposited polymerizable mixture. The "intensity" of the "dark" pixels corresponds to the desired thickness of the resulting ophthalmic lens at that location.
[0235] In some exemplary embodiments, the print pattern “intensity” of a lens may be defined as follows:
[0236]
number
[0237] Here, floor( ) converts the value to the smallest integer.
[0238] All pixels outside the lens may be set to 255, with smaller intensity values indicating greater thickness, and the smallest value corresponding to the smallest thickness.
[0239] A value of 255 corresponds to an 8-bit image. If more than 255 gray levels are used, the value of 255 is replaced by the number of gray levels. For example, for a 10-bit image, the value would be 1023.
[0240] Referring now to FIG. 12, method steps for forming an ophthalmic lens according to some embodiments of the present disclosure are illustrated in flow chart form.
[0241] In step 1202, the method includes positioning a substrate at a first position relative to an additive manufacturing print head. The substrate may include a receiving portion, which may be planar or arcuate. The receiving portion may act as a receiving surface for a first pass of the print head to deposit the polymerizable mixture. After the first pass, the receiving surface will typically include at least some areas having previously deposited polymerizable mixture.
[0242] In step 1204, the method may include emitting a first pattern of deposited droplets of the polymerizable mixture from a print head, the pattern of deposited droplets of the polymerizable mixture corresponding to a first portion of an energy transmittance map of the ophthalmic lens to be formed. Preferably, the pattern is a two-dimensional image representing light intensity through a desired optical system. The droplets are emitted at a time designation, such as T1, which may be relative to other time designations. In a preferred embodiment, the two-dimensional representation will have a numerical value associated with an X,Y location (or other coordinate designation). The numerical value will represent the amount of light passing through the optical element at the location designated by the X,Y axis designation. The printed pattern may in some embodiments be based on a numerical value, such that the amount of polymerizable mixture deposited at a location on the receiving surface corresponding to the X,Y pattern correlates with the numerical value (e.g., lighter areas will have lower X,Y numerical values and will receive less polymerizable mixture, and darker areas will have higher X,Y numerical values and will receive more polymerizable mixture).
[0243] The design of the optical element may be accomplished by analysis of the ray tracing pattern of how light passes through the optical element. In some embodiments, the X,Y values may be derived from a mathematical model of the three-dimensional shape of the desired optical element.
[0244] In step 1206, the method may include receiving the deposited droplets of the polymerizable mixture on a receiving surface, which may include one or more of a substrate, a polymerizable mixture aggregate formed from previously released droplets of the polymerizable mixture, and an insert, which may include, for example, an optical insert, a passive electronic device, an active electronic device, and / or a power source, such as a battery, a harvesting device, or an antenna.
[0245] In step 1208, at a second time (T2), the deposited droplet of the polymerizable mixture on the receiving surface may be exposed to a pinning process. The pinning process will cause partial polymerization of the deposited droplet of the polymerizable mixture. Preferably, the partial polymerization results in a viscous aggregate of the partially polymerized mixture that is resistant to flow but may integrate with subsequently deposited polymerizable mixture.
[0246] In step 1210, the method may include repositioning the substrate (and the deposited polymerizable mixture) to a next position (position plus N) relative to the print head.
[0247] In step 1212, the method may include emitting a next pattern of deposited droplets of the polymerizable mixture that corresponds to a next portion of the energy transmittance map of the article being formed, for example, an ophthalmic lens being formed.
[0248] In various embodiments of the invention, the method may include repeating the steps multiple times. For example, there may be multiple passes of the print head over the substrate and multiple residence times during which gravity acts on at least a portion of the deposited droplets of polymerizable mixture to smooth the surface of the deposited polymerizable mixture, fill the interstitial spaces between the deposited droplets, and allow coalescence of the deposited material with previously deposited and pinned material. Thus, in step 1214, a next pattern of droplets of polymerizable material may be released. The pattern may be the same pattern as the previous pattern or a different pattern.
[0249] In step 1218, the polymerizable material deposited in the current pass of the print head may be combined with material on the receiving surface, such as previously deposited material, in some embodiments, the combined material may form a single volume of polymerizable mixture on the substrate.
[0250] In step 1220, gravity may act on at least a portion of the deposited droplets of polymerizable mixture to smooth the surface of the deposited polymerizable mixture, fill interstitial spaces between the deposited droplets, and cause the deposited material to coalesce with previously deposited and pinned material.
[0251] In step 1222, the method may include curing the deposited droplets of the polymerizable mixture.
[0252] In some embodiments, the pinning step may include exposing the deposited droplets of the polymerizable mixture to a first wavelength of actinic radiation for a limited time sufficient to cause the deposited droplets of the polymerizable mixture to gel and not cause hardening of the deposited droplets of the polymerizable mixture. Similarly, in some embodiments, the hardening step may include exposing the deposited polymerizable mixture to actinic radiation of a second wavelength for a sufficient time and with sufficient intensity to cause polymerization of the deposited droplets of the polymerizable mixture. Some embodiments may also include accelerating the hardening step by increasing the ambient temperature.
[0253] 13, a schematic diagram illustrates the deposition of one or more polymerizable mixtures 1302 from one or more print heads 1301 to form an ophthalmic lens 1307. The print heads 1301 deposit the polymerizable mixture 1302 until a volume of the polymerizable mixture 1303 is formed on a receiving area 1306 of the substrate 1305 in a pattern that replicates a 2D pattern used to generate control commands for each pass of the print head 1301 relative to the position of the substrate 1305. At least a portion of the receiving area 1306 of the substrate 1305 will act as a receiving surface for the deposited polymerizable mixture 1302 until the volume of the deposited polymerizable mixture 1303 covers the footprint area for the design of the ophthalmic lens 1307.
[0254] As described herein, in some preferred embodiments of optical elements, the amount of polymerizable mixture 1302 deposited from a print head 1301 to form an ophthalmic lens 1307 varies according to a two-dimensional pattern representing an integer map of energy intensity (which may represent the transmittance of energy through the ophthalmic lens).
[0255] The pattern is preferably a two-dimensional image representing the light intensity passing through the desired Ophthalmic Lens 1307. In a preferred embodiment, the two-dimensional representation will have respective numerical values associated with a number of X,Y locations. The numerical values may represent the amount of light passing through the Ophthalmic Lens 1307 at a given location identified by the X,Y axis designation.
[0256] Control commands to the print head cause the print head 1301 to deposit the polymerizable mixture 1302 based on a two-dimensional print pattern that specifies the amount of polymerizable mixture 1302 to be deposited at a given X,Y location. After multiple successive passes of depositing the polymerizable mixture 1302, the volume of polymerizable mixture 1303 on the substrate 1305 has a three-dimensional shape representative of a mathematical model of a desired ophthalmic lens.
[0257] The two-dimensional printed pattern of the amount of polymerizable mixture, representing the amount of light passing through the ophthalmic lens 1307 at a given location identified by the X,Y axis designation, may also correlate to the amount of polymerizable mixture 1302 deposited at the location on the receiving surface 1304 (e.g., lighter areas of the two-dimensional printed pattern have lower X,Y numerical values and will receive less polymerizable mixture, and darker areas have higher X,Y numerical values and will receive more polymerizable mixture).
[0258] In some embodiments, the design of an ophthalmic lens may be accomplished by analysis of ray tracing patterns of how light passes through an ophthalmic lens. Preferably, the values of X and Y may instead be derived from a mathematical model of the three-dimensional shape of the desired ophthalmic lens.
[0259] According to the invention, a two-dimensional printed pattern specifying the amount of polymerizable mixture deposited at a given X,Y location is printed multiple times in successive passes of the print head over the substrate 1305. The deposited polymerizable mixture 1302 is received on a receiving surface 1304. The receiving surface 1304 may include one or both of a previously deposited volume of polymerizable mixture 1303 and a receiving area 1306 of the substrate 1305.
[0260] The deposited polymerizable mixture 1303 undergoes a pinning and / or gelling process to form a volume of gelled polymerizable mixture 1303. The volume of gelled polymerizable mixture 1303 is sufficiently polymerized to prevent (or at least substantially slow) movement of the polymerizable mixture received on the receiving surface while allowing the subsequently deposited polymerizable mixture 1302 to fuse with the previously deposited (and pinned) volume of polymerizable mixture 1303 to form a structure having a single mass of polymerizable mixture. In a preferred embodiment, the fuse may include intermingling or becoming intermingled with the previously deposited and pinned volume of polymerizable mixture 1303 such that, once the volume of polymerizable mixture 1303 is hardened, individual layers or streaks of the deposited polymerizable mixture 1302 are no longer discernible in the volume of polymerizable mixture 1303 formed on the receiving area 1306 of the substrate 1305. Such an embodiment may be preferred as unwanted diffraction may be an optical quality resulting from successive steps or other interlayer artifacts associated with the presence of discrete layers of polymerized material in an ophthalmic lens.
[0261] Prior to pinning, gravity may act on the surface 1304 of the volume of polymerizable mixture 1303 to smooth the surface 1304 and fill in any interstitial aberrations in the surface, thereby improving the optical quality of the resulting ophthalmic device (compared to machined lens surfaces and / or lenses formed from machined mold parts).
[0262] Curing of the volume of polymerizable mixture 1303 follows placement of the droplets of polymerizable mixture 1302 during a final pass between the print head 1301 and the substrate 1305. Curing may be accomplished by exposure of the volume of polymerizable mixture 1303 to actinic radiation and / or heat sufficient to cause substantially complete polymerization of the volume of polymerizable mixture 1303.
[0263] 13 shows the print head 1301 being substantially perpendicular to the apex 1308 of the deposited polymerizable mixture 1303. In various embodiments, the droplets of polymerizable mixture 1302 may (or may not) follow a trajectory that is perpendicular to the apex 1308 of the receiving surface, which may include one or more of the substrate 1305, the receiving area 1306, and the surface of previously deposited polymerizable mixture 1303.
[0264] Referring now to FIG. 13A, a print head 1301 is shown moving in a print path direction 1309. The droplets of polymerizable mixture 1302A will follow a drop trajectory 1309 that is influenced by the speed and direction of the print head 1301 at the time of the ejection of the droplets of polymerizable mixture 1302A. The drop trajectory 1309 will have its own speed and direction. According to the present invention, in some embodiments, the print head 1301 and the drop trajectory 1309 may be at an angle other than perpendicular to the surface of the apex of the receiving surface 1304, because a portion (e.g., a majority) of the droplets of polymerizable mixture 1302A will be integrated, pinned, and ultimately cured with the previously deposited polymerizable mixture 1303A. In this way, the process differs from previously known processes that require small portions of additive manufacturing material to be incrementally placed on a surface and not integrated with the previously deposited material before being cured.
[0265] Referring now to FIG. 14, an exemplary dynamic shape of a droplet 1401 of a polymerizable mixture is shown at various times 1402 after ejection from a print head. According to the present invention, the shape of the droplet 1401 may change based on the speed of movement of the droplet 1401 through the surrounding atmosphere. In some preferred embodiments, the molded article formed by the process disclosed herein is generally not affected by the shape of the droplet 1401 of polymerizable material. The relatively small mass of each droplet 1401 and the integration of the droplets into other polymerizable material on the receiving surface makes the shape of the manufactured molded article essentially unaffected by the shape of the individual droplets 1401 or the changing shape of the droplets 1401 at various times 1402 after ejection by the print head (not shown in FIG. 14).
[0266] Referring now to FIG. 15, a flowchart 1500 illustrates exemplary method steps that may be performed in some embodiments of the present invention.
[0267] In step 1501, the process may include positioning a substrate at a first position relative to an additive manufacturing print head.
[0268] In step 1502, the process may include emitting a first pattern of deposited droplets of the polymerizable mixture from a print head, the first pattern of deposited droplets of the polymerizable mixture corresponding to a first portion of the grayscale image.
[0269] In step 1503, the process may include receiving the deposited droplet of the polymerizable mixture on a receiving surface, which may include one or more of a substrate, a previously released droplet of the polymerizable mixture, and an inserted molded article, which may include, by way of non-limiting example, one or more of an optical element, such as a rigid transmissive lens, an electronic device, and a power source.
[0270] In step 1504, the process may include repositioning the substrate to a next position relative to the print head. Repositioning may include moving one or both of the substrate and the print head relative to the other.
[0271] In step 1505, the process may include emitting a next pattern of deposited droplets of the polymerizable mixture from the print head corresponding to a next portion of the grayscale image.
[0272] In step 1506, the process may include allowing a physical force, such as gravity, to act on the deposited droplet of the polymerizable mixture.
[0273] In step 1507, the process may include combining at least some of the droplets to form a combined volume of the polymerizable mixture on the substrate.
[0274] In step 1508, the process may include exposing the deposited droplet of the polymerizable mixture on the receiving surface to a pinning process that causes partial polymerization of the deposited droplet of the polymerizable mixture.
[0275] In step 1509, the process may include repeating the positioning and deposition steps for multiple passes of the print head relative to the substrate.
[0276] In step 1510, the process may include curing the combined volumes of the polymerizable mixture to form an ophthalmic lens.
[0277] The process may include, following each pass of the print head over the substrate, combining at least some of the droplets of the polymerizable mixture deposited during a current pass with previously deposited polymerizable mixture on a receiving surface to form a combined volume of the polymerizable mixture on the substrate.
[0278] In step 1511, the process may include releasing the formed ophthalmic lens from the substrate.
[0279] Experimental details Method for determining the water content of a hydrogel device
[0280] The water content of a hydrogel device (e.g., a contact lens) may be determined as described in Section 4.6 of ISO / DIS 18369-4:2016 (gravimetric methods shown in 4.6.2).
[0281] Keratometry Measurements The goniometer measures the central radius of the cornea, in this case the anterior surface of a non-hydrated hydrogel part formed on a PMMA dome (see the experimental section on 3-D printing on PMMA domes). The equipment used was an automated keratometer from Nidek model ARK900S. The support was set up on a horizontal table and a wedge was added to align the center and axis of the PMMA dome with the hydrogel surface with the center and axis of the keratometer. In the first set of measurements, where the astigmatism was large, the wedge was not used and the measured astigmatism was an artifact of the measurements being taken off-axis.
[0282] Curvature radius measurement The power of a contact lens depends on the combination of the powers of the front and back surfaces of the contact lens modulated by the refractive index of the material and the thickness of the contact lens, which in turn depends on the radii of these surfaces.
[0283] The relationship between power and radius in air is Power = (contact lens refractive index - 1) / Radius, where power is in diopters and radius is in meters.
[0284] For the anterior surface, radius is defined in ISO 18369-1:2006(E)(2.1.2.2.5) as the radius of curvature of the anterior optical zone of a surface having a single refractive element.
[0285] The radius of curvature of the front surface of the PMMA dome was measured with an automated keratometer, also known as an ophthalmometer, which is one of the methods specified in ISO DIS 18369-3:2016 (Annex C). Ophthalmoscopy measures the size of the reflected image of a target placed at a known distance in front of a hard or soft lens surface, and the relationship between the curvature of the reflected image and the magnification is then used to determine the posterior optical zone radius. Nevertheless, this method was used to measure the front surface radius of the PMMA dome.
[0286] light transmittance Light transmittance is defined in ISO 18369-1:2006(E). The light transmittance values shown in the table below are average values from 380nm to 780nm. The measurement method is detailed in ISO DIS18369-3:2106(4,8.2).
[0287] Apparatus and materials A series of experiments were performed to demonstrate the principles of the present invention. The experiments were performed using:
[0288] raw materials 2-Hydroxyethyl methacrylate (HEMA); 99.9% HEMA with 16 ppm MEHQ; Ethylene glycol dimethacrylate (EGDMA); Assay: 98.0% Methacrylic acid (MAA); Assay 99.0% Trimethylolpropane trimethacrylate (TMPTMA), technical grade Irgacure 651 photoinitiator, from BASF Corp, Southfield, Mi Irgacure 819 photoinitiator, from BASF Corp, Southfield, Mi; Glass microscope slides, from EMS, Hatfield, Pa, and from Am Scope Tween 80 (Polysorbate 80) Surfactant Reagent grade isopropanol Deionized or distilled water Sterile saline, from Walgreens or B&L Nitrogen gas cylinder (<0.1% oxygen) and / or liquid nitrogen tank Rotovap, glove bag, desiccator, brown bottle, syringe, 5pm filter, lint-free towel, standard beaker, weighing scale (0.001g accuracy), vacuum pump LED Source and Meter OMNI lamps with 365nm and 400nm output. Omnicure LM 2011 Light Meter for Intensity Measurement Honeywell Toxi Pro 544590VD Simple Gas Oxygen Monitor Gauge that reads oxygen below 33 millibars (3.3 kilopascals)
[0289] 3D Printing Station It was custom built using a) a Fujifilm Samba print head, b) a conveyor belt that moves the material under the print head, and then two different sources of actinic radiation in the form of UV lamps. The entire print station is housed in an atmospheric pressure enclosure with gas ports.
[0290] Example Series A - Preparation of Model Samples In this series, square samples (10 mm × 10 mm) of uniform thickness of polymerized HEMA were prepared and evaluated.
[0291] 1. Preparation of Substrate Three drops of Tween 80 were added to 20 ml of reagent grade isopropanol and filtered through a 3.1 μm filter. A glass slide was dipped into this solution three times and air dried.
[0292] Preparation of aqueous solution Five drops of Tween 80 were mixed into 100 mL of deionized water and heated to 80-90°C.
[0293] PM-1A, PM-1B and PM-1C: HEMA:97. EGDMA: 1.6% Irgacure 819:0.2% Irgacure 651:0.5%
[0294] PM-2: HEMA: 98.1% EGDMA: 1.2% Irgacure 819; 0.2% Irgacure 651; 0.5%
[0295] PM-3A, PM-3B and PM-3C
[0296] Uncatalyzed polymerization mixture samples (PM-1A, PM-1B, PM-1C, PM-2, PM-3A, PM-3B, and PM-3C; see above) were prepared by mixing the monomers and crosslinker in an amber bottle and left in the refrigerator overnight. The final polymerization mixture samples, along with the photoinitiator, were run on a rotovap using alternating degassing and nitrogen blanketing. The samples were approximately 120 grams for each of PM-1A, PM-1B, PM-1C, and PM-2. The same amount was approximately 34.5 grams for each of PM-3A, PM-3B, and PM3C.
[0297] The partial pressures corresponding to the oxygen concentrations in the polymer mixture are: PM-1A: <0.5% O2 PM-1B: 2.0% O2 PM-1C: 5.0% O2 PM-2: <0.5% O2 PM-3A:<0.5% 02 PM-3B:2.0% 02 PM-3C: 8.5% 02
[0298] O2 concentration of <0.5% O2 120 g samples were processed using a Rotovap according to the following protocol by alternating 3-4 cycles of degassing to 11.0-12.0 torr (approximately 14.0 mbar) and blanketing with nitrogen at 760 torr (1013 mbar). One degassing cycle ranged from 5 to 20 minutes, and one blanketing cycle did not exceed 5 minutes.
[0299] O2 concentration of 2.0% O2 A 120 g sample was processed to 2.0% O2 by degassing to 72 torr (95 mbar) and blanketing with nitrogen to 760 torr (1013 mbar) according to the following protocol: degassing cycles took 49 minutes, blanketing cycles did not exceed 15 minutes.
[0300] O2 concentration of 5.0% O2 120 g samples were processed to 5.0% O2 with the following protocol on a Rotovap by degassing to 179 torr (235 mbar), holding for 45 minutes with mixing, and then blanketing with 760 torr (1013 mbar) nitrogen for no more than 5 minutes.
[0301] O2 concentration of 8.0% O2 120 g samples were processed with the following protocol on a Rotovap by degassing to 300 torr (400 mbar) to 8.5% O2, holding for 45 minutes with mixing, and then blanketing with 760 torr (1013 mbar) nitrogen for no longer than 15 minutes.
[0302] LED source and printing station setup The 400 nm omni lamp was set at 22.0 mm from the substrate and the intensity was set to 4.5 W / cm2 as measured by a photometer at the substrate position.
[0303] The 365 nm omni lamp was set 123 mm from the substrate and the intensity was set to 0.63 W / cm2 as measured with a photometer. The belt speed moving the substrate from the print station to the UV station was set to 40 ft / min (12 m / min).
[0304] A 10mm x 10mm square design of the polymerizable mixture was printed. UV pinning or gelling (streaky / tacky to the touch) occurred after 30 seconds (3 cycles of 10 seconds) of exposure to the 400 nm lamp. The measured layer thickness was about 24 μm. Several experiments were performed with different intensity settings and exposure times to select conditions.
[0305] 3D printing conditions: For UV pinning, a layer was printed and exposed to a 400 nm lamp for 30 seconds six times at 2400 dpi, after which the pinned or gelled samples were exposed under a 365 nm lamp for 120 seconds to cure the samples.
[0306] Oxygen concentration was measured by two oxygen probes, one mounted near the print station and one located near the UV station. Oxygen control was achieved by controlling separate flows of air and nitrogen that were mixed before entering the processing enclosure.
[0307] result Cross sections were made from hydrated samples printed on glass microscope slides by cutting down the middle of the sample with two stacked No. 23 surgical blades. The 400-micron-wide cut section was then placed laterally in a petri dish of 0.9% saline and allowed to equilibrate for 1 hour before the shape was observed under a microscope.
[0308] The non-uniformity or stress can be seen as a deviation from the intended shape, which in this case is flat.
[0309] Any inhomogeneity or stress will adversely affect the optical properties of the material.
[0310] The appearance and tack of the non-water-containing samples (after curing at 365 nm) were evaluated by visual inspection and touch, respectively.
[0311] The light transmittance values of the aqueous hydrogel samples (10 mm x 10 mm) prepared as above, and the commercially available ACUVUE 2 contact lens as a reference (transmittance 96.83%), were calculated as the average from 380 nm to 780 nm, see the table below.
[0312] The central thickness of the hydrated samples was measured optically under a cross-sectional microscope.
[0313] Evaluation of water-containing hydrogel samples
[0314] [Table 1]
[0315] [Table 2]
[0316] [Table 3]
[0317] [Table 4]
[0318] The oxygen level in the processing atmosphere affects the molded parts formed. The light transmittance of the hydrated samples, which is important for optical function, is quite high at low oxygen levels in the processing atmosphere (0.1%, 0.5%, 1.0%) and is comparable to commercial contact lenses. At 2.0% oxygen in the processing atmosphere, the light transmittance decreases, and at 5.0%, there is a significant decrease in light transmittance. Similarly, cross-sections of the hydrated samples show that the lowest levels of deformation are obtained at low oxygen levels in the processing atmosphere.
[0319] The oxygen level in the polymerizable mixture has some effect on light transmission, but up to 5.0% oxygen is acceptable if the oxygen in the processing atmosphere is low. Cross sections of the hydrous samples show the lowest levels of deformation at 2.0% and 5.0% oxygen in the polymerizable mixture, coupled with low levels of oxygen in the processing atmosphere.
[0320] The low level of deformation, as seen in the cross-sectional samples, suggests that the product is uniform and suitable for optical applications.
[0321] Observations were made on samples made with polymerization mixtures PM-3A, PM-3B, and PM-3C based on touch after six layers were printed and pinned without curing.
[0322] The oxygen concentration in the atmosphere was maintained at <0.5% by volume and was measured by oxygen probes mounted in close proximity to both the printing and pinning stations. Control of the oxygen concentration was achieved by a flow meter connected to a nitrogen tank.
[0323] result PM-3A with <0.5% oxygen: slightly tacky but not stringy.
[0324] PM-3B with 2.0% oxygen: slightly sticky but not stringy.
[0325] PM-3C with 8.5% oxygen: slightly sticky but not stringy
[0326] Example Series B - Preparation of Hydrogel Surfaces on PMMA Domes In this series, dome-shaped samples of polymerized HEMA with varying thicknesses were prepared and evaluated. Preparation of the polymerizable mixture HEMA: 97.9~98.1% EGDMA: 1.2-1.4% Irgacure 651:0.5% Irgacure 819:0.2%
[0327] Polymerizable mixtures were prepared as described in previous experiments corresponding to oxygen equilibrium concentrations of <0.5% by volume as in the preparation of PM-1A and PM-2.
[0328] 3D printing conditions: PMMA (poly(methyl methacrylate)) domes after Tween 80 treatment were degassed overnight, labeled D and E, and then used as substrates. After printing each layer, UV pinning was performed at 400 nm for 15 s, and six layers were deposited ranging from 4 mm to 11 mm in diameter, with a final cure at 365 nm for 120 s.
[0329] result Measurements of the two PMMA domes with printed hydrogel surfaces were taken in triplicate and measurements included three values: the flattest radius of curvature, the steepest radius of curvature, and the major axis. PMMA dome tilted up and down: 1. 8.09 / 8.06@180 2. 8.10 / 7.94@120 3. 8.12 / 7.95@112 Average: 8.10 / 7.99 PMMA dome E is pointing upwards and tilted very slightly to the left: 1. 8.16 / 7.97@82 2. 8.16 / 7.97@97 3. 16 / 7.96@94 Average: 8.16 / 7.97
[0330] The results demonstrate that: i. The presence of a regular optical surface (this is the surface characteristic required for measurement by an automated keratometer) ii. Repeatable measurements of both the flattest and steepest radii: Dome D: flat range 0.03mm, steep range 0.12mm; Dome E: flat range 0.00mm, steep range 0.01mm. The axes indicate the main directions and are varied due to the placement of the dome in front of the device without any special markings, therefore this variation is not relevant. iii. Both domes exhibited a small amount of astigmatism, which was calculated based on two assumed indices of refraction using the power equation described in the radius of curvature measurements.
[0331] PMMA dome with hydrogel surface D (n=1.49) Diopter 1=60.49D; Diopter 2=61.32D; Astigmatism=0.83D; (n=1.42) Diopter 1=51.85D; Diopter 2=52.57D; Astigmatism=0.72D.
[0332] PMMA dome with hydrogel surface F (n=1.49) Power 1=60.05D; Power 2=61.48D; Astigmatism=1.43D; (n=1.42) Power 1=51.47D; Power 2=52.69D; Astigmatism=1.22D.
[0333] The anterior surfaces of the PMMA domes printed with the hydrogel surfaces described above correspond to the anterior surfaces of equivalent anterior toric contact lenses, with dome D corresponding to a 0.75D toric contact lens and dome E corresponding to a 1.25D toric contact lens.
[0334] Example Series C - Preparation of embedded inserts Preparation of the polymerizable mixture: Same as in Example Series B. Polymerizable mixtures were prepared as described in previous experiments corresponding to an oxygen equilibrium concentration of <0.5% by volume as in the preparation of PM-1A and PM-2.
[0335] 3D printing conditions; The oxygen concentration in the atmosphere was maintained at <0.5% by volume and was measured by two oxygen probes, one mounted near the printing station and the other near the UV station. Control of the oxygen concentration was achieved by a flow meter connected to a nitrogen tank.
[0336] Degassed polypropylene spheres treated with Tween 80 were used as substrates. Six layers were deposited ranging from 4 mm to 11 mm in diameter, with UV pinning at 400 nm for 15 seconds after printing each layer. A blue-tinted PMMA insert (6 mm diameter, 50 microns thick) after Tween 80 treatment was degassed overnight and placed on top of the pinned layer, and two additional layers were deposited at 11 mm in diameter, with UV pinning at 400 nm for 15 seconds after pinning each layer. A final cure was done at 365 nm for 120 seconds.
[0337] result: The blue-tinted PMMA insert could be clearly observed and was found to be completely embedded within the hydrogel device. Furthermore, this method can be used to fabricate soft contact lenses with rigid inserts to mask astigmatism.
[0338] Example Series D - Preparation of Implanted Reservoirs or Depots Preparation of the polymerizable mixture: The same as the preparation of PM-2. The polymerizable mixture was prepared as described in the previous experiment corresponding to an oxygen equilibrium concentration of <0.5% by volume as in the preparation of PM-1A and PM-2.
[0339] 3D printing conditions: The oxygen concentration in the atmosphere was maintained at <0.5% by volume and was measured by two oxygen probes, one mounted near the printing station and the other near the UV station. Control of the oxygen concentration was achieved by a flow meter connected to a nitrogen tank.
[0340] A 13 mm diameter glass hemisphere treated with Tween 80 was used as the substrate. After printing each layer, UV pinning was performed at 400 nm for 15 seconds and 15 layers were deposited with a diameter of 9.5 mm. A small piece of a plastic micropipette packed with food dye crystals was then placed on top of the pinned 15 layers. After printing each layer, UV pinning was performed at 400 nm for 15 seconds and three more layers were deposited with a diameter of 9.5 mm. A few more drops of polymerizable mixture were deposited to ensure complete encapsulation of the micropipette pieces and the assembly was cured at 365 nm for 120 seconds.
[0341] result The plastic micropipette containing the food coloring crystals could be clearly observed and was completely embedded within the hydrogel device. This method demonstrates the embedding of a functional additive release reservoir or depot within an ophthalmic device such as a contact lens. Subsequent hydration of the assembly in water showed that the hydrated water was colored and that there were no food coloring crystals within the micropipette piece.
[0342] Example Series E - Preparation of Ophthalmic Devices with Asymmetric Design Preparation of the polymerizable mixture The same as the preparation of PM-2. The polymerizable mixture was prepared as described in the previous experiment corresponding to an oxygen equilibrium concentration of <0.5% by volume as in the preparation of PM-1A and PM-2.
[0343] 3D printing conditions; The oxygen concentration in the atmosphere was maintained at <0.5% by volume and was measured by two oxygen probes, one mounted near the printing station and the other near the UV station. Control of the oxygen concentration was achieved by a flow meter connected to a nitrogen tank.
[0344] A 13 mm diameter glass hemisphere treated with Tween 80 was used as the substrate. Ten layers with an asymmetric design (Atheneum Optical Sciences Logo) measuring approximately 6 mm x 4 mm were deposited on the substrate with UV pinning at 400 nm for 15 seconds after printing each layer. Then 17 layers were deposited with UV pinning at 400 nm for 15 seconds after printing each layer. The assembly was then cured at 365 nm for 120 seconds.
[0345] result The asymmetric design of the logo can be clearly observed in the hydrogel device before and after hydration with saline. This method demonstrates the feasibility of incorporating asymmetric structures to correct asymmetric refractive errors in ophthalmic devices such as contact lenses. Example Series F - Preparation of Samples with Image Quality Optical Systems and Refractive Correction Preparation of the polymerizable mixture: HEMA: 95.4% MAA: 2.5% EGDMA: 1.2% TMPMA: 0.1% Irgacure 819:0.3% Irgacure 651:0.5%
[0346] Polymerization mixtures were prepared as described in the previous experiments corresponding to an oxygen equilibrium concentration of <0.5% by volume, similar to the preparation of PM-1A and PM-2.
[0347] 3D printing conditions; The oxygen concentration in the atmosphere was maintained at <0.5% by volume and was measured by oxygen probes mounted near the printing and pinning stations. Control of the oxygen concentration was achieved by a flow meter connected to a nitrogen tank. The resolution of the Samba printhead was set at 1200 dpi.
[0348] Circular designs of 10.0 mm diameter were printed to produce samples. The belt speed was set at 10.0 feet per minute (3.05 meters per minute). UV pinning or gelling occurred after 10 seconds of exposure to a 400 nm UV lamp. Curing was done with 120 seconds of exposure to a 365 nm UV lamp. For the printed prescriptions, the base layer was printed, pinned, and cured first. Each prescription was then pinned and then cured for 120 seconds, after which the topcoat or final coat was printed, pinned, and cured. The substrates used to prepare the samples were glass microscope slides treated with Tween 80 as described in Example Series A. Degree of Drying (D) was measured with a Topcon CL-200. Dry samples were measured on the printed samples including the glass slide substrate, and the wettability was measured after releasing the samples from the aqueous solution (heated distilled water with Tween 80 as described above) and then equilibrating in saline for over 20 hours. The diameter of the aqueous sample was measured to be 13.9 ± 0.1 mm.
[0349] The results are shown in the table below:
[0350]
number
[0351] result The dry and wet diopter results shown in the table above suggest that 3D deposition printing can produce optical devices with image-quality optics, such as ophthalmic lenses for correcting refractive error.
[0352] Common findings Although the specification and claims may refer to mixtures (such as polymerizable mixtures), initiators, and other additives, it is within the scope of the present invention that the materials and compositions defined herein may be composed of one, two, or more types of individual components. In such embodiments, the total amount of each component should correspond to the amounts defined above for the individual components.
[0353] The (s) in expressions such as mixture(s), initiator(s), etc. indicates that one, two or more types of individual components may be present, whereas when the expression one is used, only one (1) of the respective component is present.
[0354] The expression % should be understood to mean % by weight of the respective component, unless otherwise specified.
[0355] conclusion
[0356] Numerous embodiments of the present disclosure have been described. Although the specification contains details of many specific embodiments, these should not be construed as limitations on the scope of any disclosure or what may be claimed, but rather as descriptions of features specific to particular embodiments of the present disclosure.
[0357] Certain features that are described in this specification in the context of separate embodiments may also be implemented in combination in a single embodiment. Conversely, various features that are described in the context of a single embodiment may also be implemented in multiple embodiments separately or in combination in any suitable subcombination. Moreover, although features may be described above as acting in a particular combination, and may even be initially claimed as such, one or more features from a claimed combination may in some cases be excised from the combination, and the claimed combination may be directed to a subcombination or a variation of the subcombination.
[0358] Similarly, although operations are depicted in the figures in a particular order, this should not be understood as requiring that such operations be performed in the particular order shown, or sequentially, or that all of the operations depicted be performed, to achieve desirable results. In certain situations, multitasking and parallel processing may be advantageous.
[0359] Furthermore, the separation of various system components in the embodiments described above should not be understood as requiring such separation in all embodiments, and it should be understood that the program components and systems described may generally be integrated together in a single hardware and / or software product or packaged in multiple products.
[0360] Thus, particular embodiments of the subject matter have been described. Other embodiments are within the scope of the following claims. In some cases, the actions recited in the claims can be performed in a different order to achieve desirable results. Moreover, the steps depicted in the accompanying figures do not necessarily require the particular order shown, or sequential order, to achieve desirable results. In certain embodiments, multitasking and parallel processing may be advantageous. It will be understood, however, that various modifications may be made without departing from the spirit and scope of the claimed disclosure.
Claims
1. 1. A method of forming an ophthalmic lens by additive manufacturing, the method comprising: a. positioning a substrate at a first position relative to an additive manufacturing print head; b. ejecting a first pattern of deposited droplets of a polymerizable mixture from a print head, said first pattern of deposited droplets of a polymerizable mixture corresponding to a first portion of a grayscale image; c. receiving the deposited droplet of the polymerizable mixture on a receiving surface, the receiving surface including one or both of the substrate and the previously discharged droplet of the polymerizable mixture; d. repositioning the substrate to a next position relative to the print head; e. ejecting a next pattern of deposited droplets of polymerizable mixture from said print head, said pattern corresponding to a next portion of said grayscale image; f. repeating steps a. through e. multiple times during a pass of the print head over the substrate; g. exposing the deposited droplets of the polymerizable mixture on the receiving surface to a pinning process that causes partial polymerization of the deposited droplets of the polymerizable mixture; h. repeating step f. for a next pass of the print head over the substrate; i. following each pass comprised in step h., applying gravity to at least a portion of the deposited droplet of polymerizable mixture to allow a surface of the polymerizable mixture to be smoothed; j) following each pass comprised in step h., combining at least a portion of the deposited droplet of the polymerizable mixture deposited during a current pass with a previously deposited polymerizable mixture on the receiving surface to form a combined volume of polymerizable mixture on the substrate; k. following each step j., pinning the deposited droplet of polymerizable mixture on the receiving surface via the partial polymerization of the deposited droplet of polymerizable mixture; l. curing the combined volume of the polymerizable mixture on the substrate; A method comprising:
2. 10. The method of claim 1, further comprising the step of housing the substrate and the deposited droplet of polymerizable mixture in a controlled atmosphere with an oxygen concentration of up to 5.0% by volume.
3. 3. The method of claim 2, comprising providing an oxygen equilibrium concentration of up to 8.0% by volume of the combined volume of the polymerizable mixture on the substrate.
4. The method of claim 3 further comprising the step of equilibrating an oxygen concentration in the substrate with an oxygen concentration in the controlled atmosphere.
5. 5. The method of claim 4, wherein at least one of the steps of ejecting a first pattern of deposited drops of polymerizable mixture from the print head and ejecting a next pattern of deposited drops of polymerizable mixture from the print head includes ejecting an amount of deposited polymerizable mixture in a given arrangement that corresponds to a data value associated with a pixel included in the grayscale image.
6. The method of claim 5 , wherein relatively larger digital values correspond to darker areas of the grayscale image than relatively smaller digital values which correspond to lighter areas of the grayscale image.
7. 2. The method of claim 1 , wherein the pinning step comprises exposing the deposited droplets of the polymerizable mixture to actinic radiation at a first wavelength for a limited time sufficient to cause gelation of the deposited droplets of the polymerizable mixture but not hardening of the deposited droplets of the polymerizable mixture.
8. 2. The method of claim 1 , wherein curing the combined volume of the polymerizable mixture comprises exposing the combined volume of the polymerizable mixture on the substrate to actinic radiation of a second wavelength for a sufficient time and of sufficient intensity to cause polymerization of deposited droplets of the polymerizable mixture.
9. 2. The method of claim 1 , wherein allowing gravity to act on at least a portion of the deposited droplets of the polymerizable mixture to smooth the surface of the polymerizable mixture comprises at least partially filling interstitial spaces between the deposited droplets of the polymerizable mixture.
10. 10. The method of claim 9, further comprising the step of equilibrating the oxygen concentration in the substrate with the oxygen concentration in a controlled atmosphere containing the substrate and the deposited droplets of the polymerizable mixture.
11. 1. A method of forming an ophthalmic lens by additive manufacturing, the method comprising: a. positioning a substrate at a first position relative to an additive manufacturing print head; b. ejecting a first pattern of deposited droplets of a polymerizable mixture from the additive manufacturing print head, the first pattern of deposited droplets of a polymerizable mixture corresponding to a first portion of an energy transmittance pattern; c. receiving the deposited droplet of the polymerizable mixture on a receiving surface; d. positioning the substrate at a next position (current position plus N) relative to the additive manufacturing print head; e. emitting a next pattern of deposited droplets of the polymerizable mixture corresponding to a next portion of said energy transmittance pattern; f. Allowing a physical force to smooth the surface of the droplet of polymerizable mixture deposited during the current pass; g. combining at least some of the deposited droplets of the polymerizable mixture deposited during a current pass with previously deposited polymerizable mixture on the receiving surface to form a combined volume of polymerizable mixture on the substrate; h. exposing the deposited droplets of the polymerizable mixture on the receiving surface to a pinning process that causes partial polymerization of the deposited droplets of the polymerizable mixture; i. repeating steps d through h. for multiple passes of the additive manufacturing print head over the substrate; and j. curing the combined volume of said polymerizable mixture on said substrate to produce said formed ophthalmic lens; A method comprising:
12. 12. The method of claim 11 , wherein receiving the deposited droplet of the polymerizable mixture on the receiving surface comprises receiving the deposited droplet on one or more of the substrate, a previously ejected droplet of polymerizable mixture, and an insert.
13. 13. The method of claim 12, further comprising repeating steps d. through g. multiple times during a pass of the additive manufacturing print head over the substrate.
14. The method of claim 12 , further comprising releasing the formed ophthalmic lens from the substrate.
15. 13. The method of claim 12, further comprising allowing gravity to act on at least a portion of the piled droplets of the polymerizable mixture to at least partially fill interstitial spaces between the piled droplets of the polymerizable mixture.
16. 12. The method of claim 11 , wherein the pinning step comprises exposing the deposited droplets of the polymerizable mixture to actinic radiation at a first wavelength for a limited time sufficient to cause gelling of the deposited droplets of the polymerizable mixture but not hardening of the deposited droplets of the polymerizable mixture.
17. 17. The method of claim 16, wherein curing the combined volume of the polymerizable mixture on the substrate comprises exposing the combined volume of the polymerizable mixture on the substrate to actinic radiation of a second wavelength for a sufficient time and with sufficient intensity to cause polymerization of the combined volume of the polymerizable mixture on the substrate.
18. 12. The method of claim 11, further comprising housing the substrate and the polymerizable mixture in a controlled atmosphere having an oxygen concentration comprising up to 2.0% by volume.
19. 20. The method of claim 18, further comprising the step of equilibrating an oxygen concentration in the substrate with an oxygen concentration in the controlled atmosphere.
20. The method of claim 11 , further comprising the step of dithering the energy transmittance pattern prior to generating control commands.
Citation Information
Patent Citations
3D printing of optical devices
JP2020501953A