Electrode wire and its manufacturing method

The electrode wire with a copper core and copper-zinc alloy coating, featuring a textured gamma and epsilon phase structure, addresses the limitations of existing wires by enhancing mechanical strength and discharge efficiency, leading to improved machining speed and reduced material loss.

JP2024543089APending Publication Date: 2024-11-19THERMOCOMPACT
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2024529463
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2021-11-16
Filing Date
2022-09-29
Publication Date
2024-11-19

AI Technical Summary

Technical Problem

Existing electrode wires for electrical discharge machining are limited by low machining speed and efficiency due to the nature and topography of their surface layers, particularly when subjected to high mechanical loads and rapid temperature changes during spark erosion.

Method used

The electrode wire features a central core made of copper surrounded by a coating comprising multiple layers of copper-zinc alloys with specific phase structures, including a textured surface layer of intertwined gamma and epsilon phases, which enhances mechanical strength and discharge efficiency.

Benefits of technology

The electrode wire maintains high tensile strength and improved erosion efficiency by minimizing material loss and preserving the surface topography, allowing for increased machining speed and reduced wire consumption.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024543089000001_ABST
    Figure 2024543089000001_ABST
Patent Text Reader

Abstract

The electrode wire for electrical discharge machining includes a metal core (10) and a coating (12) thereon that includes one or more textured regions (26-28) of Cu-Zn alloy formed solely by interlocking of Cu-Zn alloy gamma phase and Cu-Zn alloy epsilon phase. Within each Cu-Zn alloy textured region (26-28), the majority of the Cu-Zn alloy gamma phase has a lamellar texture, and the interstices between the Cu-Zn alloy gamma phase lamellae are filled with the Cu-Zn alloy epsilon phase.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to an electrode wire for electrical discharge machining and a method for making the same. [Background technology]

[0002] Electrode wires are used in electrical discharge machines to cut metals or conductive materials by electrical discharge.

[0003] A well-known method of electrical discharge machining, also known as spark erosion machining, allows for the removal of material from a conductive part by generating sparks in the machining region between the part to be machined and a conductive electrode wire. The electrode wire is continuously fed adjacent the part along its length, held by a guide, and gradually translated laterally towards the part, either by lateral translation of the wire guide or by translation of the part.

[0004] A generator connected to the electrode wire by electrical contacts outside the machining area establishes a suitable potential difference between the electrode wire and the conductive part to be machined. The machining area between the electrode wire and the part is immersed in a suitable insulating fluid. The potential difference generates a spark between the electrode wire and the part to be machined, gradually eroding the part and the electrode wire. The longitudinal movement of the electrode wire allows a continuous wire diameter sufficient to prevent wire breakage within the machining area. The relative lateral movement of the wire and the part allows the part to be cut or the surface to be treated as required.

[0005] Particles detached from the electrode wires and components by the spark are dispersed in the insulating fluid and are exhausted therefrom.

[0006] To obtain machining precision, especially for making angle cuts with small radii, it is necessary to use wires with small diameters, to withstand high mechanical loads at break, to provide tension in the machining area and to limit the amplitude of vibrations.

[0007] Most current EDM machines generally use a diameter of 0.25 mm and a maximum tensile strength of 400 N / mm 2 from 1000N / mm 2 It is designed to use metal wire.

[0008] When a spark occurs between the electrode wire and the part, the surface of the electrode wire heats up rapidly, reaching a very high temperature in a short time. As a result, the material on the surface of the electrode wire at the location of the spark goes from a solid state to a liquid or gaseous state and moves over the surface of the electrode wire and / or is exhausted into the insulating liquid. The outer surface of the electrode wire where the spark hits is deformed, typically appearing as a slightly concave crater shape, indicating an area where the material has melted and resolidified.

[0009] It has been found that the efficiency of the discharge spark is highly dependent on the nature and topography of the surface of the electrode wire. Significant advances in discharge efficiency have been achieved by using electrode wires that include: - a core made of one or more metals or alloys that ensure good conductivity of electric current and good mechanical strength to withstand mechanical tensile loads on the wire, and Coating with one or more other metals or alloys and / or specific surface geometries (e.g. cracks) to ensure better discharge efficiency, e.g. faster erosion rates.

[0010] For example, U.S. Patent No. 8,067,689 describes an electrode wire having a brass core coated with a copper-zinc alloy layer, in which the copper-zinc alloy layer comprises a mixture of gamma (γ) and epsilon (ε) phase copper-zinc alloys.

[0011] This particular coating structure is generally intended for faster electrical discharge machining of parts.

[0012] Furthermore, the following Patent Document 2 and Non-Patent Document 1 are known as prior art documents. [Prior art documents] [Patent documents]

[0013] [Patent Document 1] U.S. Pat. No. 8,067,689 [Patent Document 2] Patent No. 3090009 [Patent Document 3] U.S. Pat. No. 5,762,726 [Non-patent literature]

[0014] [Non-Patent Document 1] MA D et al.: "Unidirectional solidification of Zn-rich Zn-Cu peritectic alloys-I. Microstructure selection", ACTA MATERIALIA, Elsevier, Oxford, vol. 48, No. 2, 24 / 01 / 2000, pp. 419-431. [Non-Patent Document 2] Liang et al.: "Thermodynamic assessment of the Al-Cu-Zn system, part I: Cu-Zn binary system". CALPHAD, volume 51, 2015, pages 224 to 232. Summary of the Invention [Problem to be solved by the invention]

[0015] However, there remains a need to improve the speed of electrical discharge machining for a given electrical spark strength.

[0016] The present disclosure aims to meet this need by proposing an electrode wire complying with claim 1.

[0017] The present disclosure is also directed to a method for manufacturing an electrode wire conforming to claim 1. [Brief description of the drawings]

[0018] The present disclosure will be better understood on reading the following description, given by way of non-limiting example only, with reference to the drawings in which: [Figure 1] FIG. 1 is a schematic diagram of a cross section of an electrode wire. [Diagram 2] FIG. 2 is a larger scale schematic diagram of a cross section of a portion of the lamellar texture of the layer of the electrode wire of FIG. [Diagram 3] FIG. 3 is a larger scale schematic diagram of a portion of the lamellar texture of FIG. [Figure 4] FIG. 4 is a black and white photograph of the lamellar texture of FIG. [Diagram 5] FIG. 5 is a flow chart of a method for manufacturing the electrode wire of FIG. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0019] In these figures, the same reference numerals are used to denote the same elements. In the remainder of this description, features and functions well known to those skilled in the art are not described in detail.

[0020] Below, in Section I, definitions of certain terms are provided. In Section II, detailed exemplary embodiments are described with reference to the figures. Then, in Section III, variations on these embodiments are described. Finally, in Section IV, advantages of various embodiments are described.

[0021] Chapter I: Definitions and Terminology The expression "an element consisting of material A" refers to an element in which material A constitutes at least 90% by weight of the element, preferably at least 95% or 98% by weight.

[0022] The expression "copper-zinc alloy" denotes an alloy formed exclusively from copper and zinc, excluding unavoidable impurities.

[0023] A "phase" of a copper-zinc alloy refers to a solid phase of the copper-zinc alloy that has a specific crystal structure. More precisely, the phases of the copper-zinc system differ from each other by their composition and specific crystal structure. This specific crystal structure allows the copper-zinc alloy phases to be distinguished from a simple mixture of fine particles of copper and zinc with the same overall composition. The known phases of copper-zinc alloys are usually the alpha (α), beta (β), gamma (γ), delta (δ), epsilon (ε) and eta (η) phases. The specific crystal structure of a phase can be identified by various means. For example, optical or metallographic micrographs of a polished specimen will show different shades of color for each phase if the specimen has been properly chemically treated. Thus, to distinguish between the gamma and epsilon phases, a chemical treatment with "nital", a 3% solution of nitric acid diluted in ethanol, is used. This makes the gamma phase appear gray and the epsilon phase appear brown. It is also possible to distinguish between the gamma and epsilon phases by observing the specimen in a scanning electron microscope using a backscattered electron detector. It is also possible to identify the phase of a sample by X-ray diffraction. In this case, a wire sample is placed under the incidence of an X-ray beam of a precise wavelength; for example, copper Kα radiation with a wavelength of 0.1541 nm. The intensity of the diffracted line is evaluated at each diffraction angle. The gamma phase has a known X-ray diffraction spectrum that is distinct from other phases in the copper-zinc system and from zinc oxide, ZnO, which is commonly found on the surface of wires. If a copper-zinc alloy is not crystallized in at least one of the alpha, beta, gamma, delta, epsilon or eta phases, it is amorphous and the X-ray diffraction spectrum shows a flat hump rather than a prominent peak.

[0024] At a given temperature, the various phases of a copper-zinc alloy each correspond to a specific range of zinc concentrations. The size of each of these specific zinc concentration ranges varies as a function of temperature. The zinc concentrations of the phases of a sample are obtained by compositional microanalysis. Compositional microanalysis is performed using a scanning electron microscope equipped with a spectroscopic probe. An electron beam accelerated in an electric field of, for example, 20 kV strikes the surface of the sample and emits X-rays. These X-rays have an energy spectrum characteristic of the composition of the sample surface struck by the electron beam. The spectrum of the X-rays emitted from the sample surface is measured using an energy dispersive spectroscopy (EDS) or wavelength selective (WDS) analytical probe. An algorithm allows the selection of the elements to be analyzed (and the elimination of the effects of impurities) and the calculation of the composition of the sample struck by the electron beam based on the measured spectrum. It should be noted that due to the interaction of the X-rays with the material, the volume analyzed in an EDS (or WDS) analysis is generally about one cubic micrometer. At the boundary between two phases, an average concentration can be measured that is not actually present in either of the two phases. The concentrations given here are for the pure phase in the analyzed volume, except in the case of structured regions, where the regions over which the concentrations are measured are larger than a cube with sides of one micrometer.

[0025] The δ phase of copper-zinc alloys is characterized by being stable only between 559℃ and 700℃, and not existing in a stable state at room temperature. The crystal structure of the δ phase of the copper-zinc system, which is stable at a temperature of 600℃, was published in Zeitschrift fur Metallkunde, vol. 62, pp. 810-816, by J. Lenz and K. Schubert in 1971.

[0026] The expression "electrical conductor" means a material having a conductivity of 10 at 20°C. 6 S / m, preferably 10 7 Refers to materials with a value greater than S / m.

[0027] The longitudinal axis of a wire is the axis along which the wire primarily extends.

[0028] The expression "cross-section" refers to a cross-section of an electrode wire perpendicular to its longitudinal axis.

[0029] The expression "layer of the electrode wire" refers to an annular layer of the electrode wire located between an inner circular boundary line and an outer circular boundary line in each cross section of the electrode wire. In reality, these boundaries are not perfect circles. However, as a first approximation, in the present text, these boundaries are treated as circles. Both of these circular boundaries are in the center of the axis of the electrode wire. The inner circular boundary line is the limit of the layer closest to the axis of the electrode wire. Conversely, the outer circular boundary line is the limit of the layer furthest from the axis of the electrode wire. Between these inner and outer circular boundaries, the copper-zinc alloy phase is either homogeneous or is formed of an irregular entanglement of various phases of the copper-zinc alloy. Conversely, at the level of the inner and outer circular boundaries, the chemical composition and / or the crystal morphology change abruptly.

[0030] The expression "intertwining of different phases" in copper-zinc alloys refers to a mixture of different phases in the copper-zinc alloy, where the different phases are not arranged in homogeneous layers of each other, i.e., when moving along a circle around the longitudinal axis of the wire across this intertwining of phases, one phase alternates with another, and this is repeated several times.

[0031] A "homogeneous" layer is one formed by a single phase of copper-zinc alloy.

[0032] The expression "homogeneous layer" refers to a layer formed by a material that extends continuously or substantially continuously inside the layer in the cross section of the wire about the axis of the wire. Thus, a homogeneous layer does not include a multiplicity of fractures that is divided into a multiplicity of regions separated from each other by a multiplicity of radial fractures in the cross section of the wire. A multiplicity of radial fractures refers to about 10 or more radial fractures that divide the layer into about 10 regions mechanically separated from each other by the radial fractures in the cross section of the wire.

[0033] Conversely, the expression "fractured layer" refers to a layer that contains numerous discontinuities that divide the wire in its cross section into numerous regions separated from one another by a large number of radial breaks.

[0034] The expression "metallic surface layer" or simply "surface layer" refers to a layer of copper-zinc alloy or zinc of the electrode wire that is the outermost layer of the electrode wire. Said metallic surface layer may have a thin oxide film on its surface. This oxide film typically consists mainly of zinc oxide, zinc hydroxide, zinc carbonate and possible residues such as wire drawing lubricant residues. The outer surface of this metallic surface layer therefore coincides with the outer surface of the electrode wire in the absence of a fine oxide film or is separated from it only by a fine oxide film.

[0035] A "radial break" is a break that extends primarily radially in the cross-section of the electrode wire.

[0036] The expression "normal temperature" refers to a temperature greater than or equal to 15°C and less than or equal to 30°C, typically equal to 25°C.

[0037] A "central orbit of an elongate element" is the orbit along which the elongate element primarily extends. This central orbit is located in the middle of the thickness of the elongate element in a cross-section of the electrode wire. That is, the cross-section of the elongate element is centered on this central orbit. Thus, the area of ​​the elongate element on one side of the central orbit in the cross-section is equal to the area of ​​the elongate element on the other side of said central orbit.

[0038] The average thickness of an elongate element along its central trajectory is equal to the average of the thicknesses of said elongate element measured at each point of said central trajectory, where the thickness is measured in a direction perpendicular to said central trajectory and contained in the plane of the cross section.

[0039] Chapter II: Exemplary Embodiments FIG. 1 shows an electrode wire 2 for electrical discharge machining as described in the introduction of this specification.

[0040] For this purpose, the electrode wire 2 has a resistance of 400 N / mm 2More than 1000N / mm 2 It has an ultimate tensile strength of: The electrode wire 2 extends along a longitudinal axis 4, where the longitudinal axis 4 is perpendicular to the plane of the drawing. The length of the electrode wire 2 is greater than 1 m, typically greater than 10 m or 50 m.

[0041] The electrode wire 2 has an outer surface 6 that is directly exposed to sparks when the wire is used to machine a part by electrical discharge machining. The outer surface 6 is a cylindrical surface extending along the longitudinal axis 4. The quadratic curve of the outer surface 6 is mainly a circle centered on the longitudinal axis 4. Thus, the cross section of the electrode wire 2 is circular. The outer diameter D of the electrode wire 2 is 2 is typically between 50 μm and 1 mm, most often between 70 μm and 400 μm, where the outer diameter of the electrode wire 2 is equal to 250 μm.

[0042] In this embodiment, the electrode wire 2 includes a central core 10 of a conductive material and a coating 12 deposited directly on the central core 10 .

[0043] The function of the central core 10 is to ensure by itself a large part of the maximum tensile strength of the electrode wire 2. It also has the function of ensuring the electrical conductivity of the electrode wire 2. For this purpose, it is made of an electrically conductive material. It is typically made of a metal or a metal alloy. For example, in this embodiment, the central core 10 is made of copper.

[0044] Diameter D of central core 10 10 D 2 is the outer diameter of electrode wire 2, then 0.75D 2 and 0.98D 2 Typically 0.85D 2 and 0.95D 2 For example, here, the diameter D 10 is equal to 230 μm.

[0045] The coating 12 is designed to increase the machining speed and therefore the erosion yield of the electrode wire and / or the surface quality of the part obtained after EDM. The quality of the EDM cut surface improves as its roughness decreases.

[0046] The thickness of the coating 12 is determined by the outer diameter D of the electrode wire 2. 2 That is, the outer diameter D 2 less than 10% of the outer diameter D 2 The thickness of the coating 12 corresponds to the shortest distance in cross section between the outer surface 6 and the circular boundary line that separates the central core 10 and the coating 12.

[0047] In this embodiment, the coating 12 is made up of three layers 14, 16 and 18 stacked in direct succession from the longitudinal axis 4 towards the outer surface 6. The thickness of the layer 18 is typically 1 / 2 mm thick, approximately 1 / 2 mm thick, and approximately 1 / 2 mm thick. 2 For example, the thickness of layer 18 is at least 2 μm, 5 μm or 10 μm. The thicknesses of the other layers 14 and 16 are preferably less than the thickness of layer 18. For example, here, the thicknesses of layers 14 and 16 are less than 5 μm and less than 10 μm, respectively.

[0048] Layer 14 is a homogeneous, uniform layer of the beta phase of a copper-zinc alloy. Thus, the zinc concentration is typically between 45 atomic % and 50 atomic %, with the remainder being copper and unavoidable impurities.

[0049] Layer 16 is a homogeneous layer of the gamma phase of a copper-zinc alloy. The zinc concentration is typically between 62 and 71 atomic %, with the remainder being copper and unavoidable impurities. For example, here the zinc concentration is 64 atomic %.

[0050] A recently updated phase diagram for the Cu-Zn system shows that, at steady state, the gamma phase of Cu-Zn alloys has a zinc concentration between 60 and 62 atomic % at room temperature, with the remainder being copper. A recently updated phase diagram for the Cu-Zn system is published, for example, in Liang et al., "Thermodynamic assessment of the Al-Cu-Zn system, part I: Cu-Zn binary system". CALPHAD, volume 51, 2015, pages 224 to 232.

[0051] Therefore, the gamma phase of the copper-zinc alloy of the layer 16 is not in a stable state at room temperature when the zinc concentration is 64%. Here, it is in a metastable state. In the metastable state, the transformation of the copper-zinc alloy from the gamma phase to the stable state, i.e. the decrease in its zinc concentration, is very slow at room temperature. In other words, the transformation from the gamma phase to the stable state at room temperature is practically imperceptible to humans. Therefore, the composition of the metastable gamma phase hardly changes from its manufacture to its arrival at the machining area of ​​the electric discharge machine, if this electrode wire 2 is stored and transported under normal conditions and maintained at room temperature. Hereinafter, a method for manufacturing such a metastable copper-zinc alloy layer will be described.

[0052] Layer 18 is a textured surface layer of Cu-Zn alloy. More precisely, in each cross section, layer 18 is mainly formed by a plurality of texture regions, each of which is formed exclusively by the interlocking of the γ-phase of the Cu-Zn alloy and the ε-phase of the Cu-Zn alloy, said interlocking being explained in more detail below with reference to Figures 2 and 3.

[0053] In layer 18, the zinc concentration in each of the textured regions is greater than 72 atomic % or 73 atomic % and less than 80 atomic %, where the zinc concentration in the textured regions of layer 18 is equal to 74 atomic %, the remainder being copper and impurities. The thickness of layer 18 is preferably greater than 10%, 20%, or 30% of the total thickness of coating 12.

[0054] In this embodiment, layers 16 and 18 are broken. Thus, layers 16 and 18 contain fissures that divide each of these layers into a number of regions that are mechanically separated from one another in cross section by fractures. As explained below, these fissures are obtained by drawing (drawing, wire drawing) a wire in which layers 16 and 18 are homogeneous or substantially homogeneous. After drawing, the same material no longer extends continuously around the longitudinal axis 4 but is divided into a number of regions of material that are mechanically separated from one another in cross section by fractures or cracks. These fissures extend mainly in the radial direction and completely traverse layers 16 and / or 18.

[0055] More precisely, it has been observed that there are mainly two types of cracks in the electrode wire 2. The first type of crack is a crack that extends only inside the layer 16. This first type of crack does not cross the layer 18, i.e. does not cross the layer 18 completely. In Fig. 1, the reference number 20 refers to a schematic diagram of a first type of crack. The crack 20 extends from the circular border separating the layers 14 and 16 to the circular border separating the layers 16 and 18. The crack 20 does not extend inside the layers 14 and 18.

[0056] The second type of crack is a crack that extends across both ply 16 and ply 18. The second type of crack typically initiates at the level of the circular boundary between ply 14 and ply 16 and extends to outer surface 6. It is only this second type of crack that divides ply 18 into multiple distinct regions.

[0057] Three cracks of the second type are shown diagrammatically in Figure 1, namely, cracks 22-24. These three cracks 22-24 divide layer 18 into three distinct regions 26-28. Together with the first type of cracks, the second type of cracks contribute to dividing layer 16 into a number of distinct regions. In Figure 1, cracks 20 and 22-24 divide layer 16 into four distinct regions 30-33.

[0058] Whether they are the first or second type of fractures, said fractures correspond to recesses or hollows that do not contain solid or liquid matter. The width of the fractures in the direction perpendicular to the radial direction in which they extend is generally less than 2 μm.

[0059] The maximum width of each texture region in cross section is typically greater than the thickness of layer 18. Here, this maximum width is greater than 5 μm or 10 μm. The width of a texture region in cross section is defined herein as equal to the side length of a smallest area rectangle that completely contains the texture region, at least one of its sides passing through the texture region and perpendicular to a radial line contained within the cross section. The radial line passes through the longitudinal axis 4. The radial line bisects the smallest angular sector that completely contains the texture region in the cross section and has its apex on the longitudinal axis 4. The side of the rectangle along which the length is measured is perpendicular to the radial line.

[0060] Figure 2 shows an enlarged cross-section of the bottom of the textured regions of layer 18. Figure 3 shows a larger scale portion of one of these textured regions. In each textured region, the γ phase of the Cu-Zn alloy has a predominantly lamellar texture 40 (Figure 2) and the ε phase of the Cu-Zn alloy fills the interstices between the lamellae of the lamellar texture 40. The lamellar texture 40 is shown in white in Figures 2 and 3, while the ε phase of the Cu-Zn alloy is hatched in the figures.

[0061] The weight of the lamellar texture 40 is typically greater than 80% of the weight of the gamma phase of the copper-zinc alloy contained in layer 18, and generally greater than 90% or 95%.

[0062] As will be explained below, the lamellar texture 40 is obtained here by interrupting, before full completion, the transformation of a layer of Cu-Zn alloy δ-phase into a homogeneous sublayer of Cu-Zn alloy γ-phase possibly covered by a homogeneous sublayer of Cu-Zn alloy ε-phase.

[0063] The lamellar texture 40 is formed from a number of elongated lamellae that, in cross section, each extend primarily along a respective central trajectory. For example, Figure 3 shows two lamellae 44, 46 of the lamellar texture 40. The lamellae 44, 46 extend along central trajectories 48, 50, respectively.

[0064] In many cases, the lamellae extend for several micrometers and therefore their central trajectory is several micrometers long. The central trajectory along which the lamellae extend is often curved or tortuous.

[0065] In most cases, in each cross section, one of the ends of the lamella is directly mechanically connected to another lamella. Thus, the lamellar texture 40 forms a tree structure in each cross section, including a large number of paths that extend continuously from the layer 16 to the outer surface 6. The other end of the lamella is either free, i.e., not directly mechanically connected to another lamella, or is directly mechanically connected to another lamella.

[0066] For the majority of the lamellae of the lamellar texture 40, and typically 80% or more, 90% or more, or 95% or more of the lamellae, the average thickness of the lamellae along their central trajectory is less than 1 μm or 0.5 μm, and typically the average thickness of the lamellae along their central trajectory is greater than 0.1 μm.

[0067] Assuming that the lamellae are elongated, most of the gaps between the lamellae, typically more than 80%, are also elongated. More precisely, the gaps located between each lamella also extend mainly along the respective central track. Figure 3 shows one such gap 54 located between two lamellae 44 and 46 and extending along a central track 56.

[0068] The average thickness of the elongated gaps along each central track is less than 1 μm or 0.5 μm in more than 50% of cases, and in the most common cases is more than 80%. This average thickness is also generally greater than 0.1 μm.

[0069] In Figure 3, to make the central tracks of the elongated elements more visible, the central tracks are extended beyond the elongated elements on each side, but in reality each central track starts at one end of the elongated element and ends at the opposite end thereof.

[0070] FIG. 4 shows part of the textured region obtained by observing a cross section of the electrode wire 2 using an optical microscope. In this photograph, in layer 18, the Cu-Zn alloy γ-phase lamellae forming the lamellar texture 40 are colored white, while the Cu-Zn alloy ε-phase filling the gaps between the lamellae is colored black. The cross section observed in this photograph is that of the electrode wire just before it is subjected to a wire drawing operation, and therefore before the majority of the first and second types of cracks are generated. However, even before carrying out this wire drawing operation, layer 16 may contain the first type of cracks, as can be seen, for example, in the portion of layer 16 located at the top left.

[0071] Next, a method for producing the electrode wire 2 will be described with reference to FIG.

[0072] A metal wire blank is first obtained in step 80. In this example, the wire blank is a copper wire with a diameter of 1 mm.

[0073] Next, in step 82, a coating is produced on the wire blank. This coating covers the entire outer surface of the metal wire blank continuously. This coating consists of one or more materials capable of forming a surface layer of the δ phase of the copper-zinc alloy at a temperature between 559°C and 700°C. This temperature range corresponds to the temperature range in which the δ phase of the copper-zinc alloy is stable. Outside this temperature range, the δ phase is not stable. In particular, when the temperature drops below 559°C, the δ phase spontaneously decomposes on the one hand into the γ phase of the copper-zinc alloy and on the other hand into the ε phase of the copper-zinc alloy. Thus, if no special heat treatment is performed, for example if the layer of the δ phase of the copper-zinc alloy is simply cooled in air at room temperature, the layer of the δ phase of the copper-zinc alloy decomposes into a homogeneous sublayer of the γ phase of the copper-zinc alloy covered by a homogeneous sublayer of the ε phase of the copper-zinc alloy. At this stage in this example, the coating is formed only by a layer of zinc deposited directly on the outer surface of the metal wire blank. For this purpose, a layer of zinc is deposited on a metal wire blank by an electrolytic galvanizing process to obtain a wire having a diameter of more than 1 mm and electroplated with zinc.

[0074] Now, at the end of step 82, the wire electroplated with zinc is drawn until its diameter is 420 μm. At this stage, the thickness of the zinc coating is equal to 25 μm.

[0075] Then, during step 84, the temperature of the zinc coating is increased to a temperature T ini The temperature T below 600°C ini By selecting the temperature T, it is possible to limit the formation of droplets of molten zinc during heating. ini is equal to 600°C.

[0076] For example, in step 84, the drawn electrogalvanized wire is introduced into a furnace whose internal temperature is equal to 600° C. This heat treatment is carried out in air.

[0077] In step 84, the drawn electrogalvanized wire is subjected to a period of time d sufficient to form a surface layer of the δ phase of the Cu-Zn alloy having a thickness of at least 4 μm. ini During this time, the temperature T ini where, for period d ini is selected to be sufficiently short to prevent the formation of a layer of the ε phase of the Cu-Zn alloy on the layer of the δ phase of the Cu-Zn alloy. In fact, as suggested in U.S. Pat. No. 5,762,726, this temperature T ini At 0° C., copper diffuses gradually into the zinc coating, so that at a given location in the initial zinc coating, the copper concentration increases gradually with time.

[0078] Furthermore, assuming that copper diffuses into the coating by migrating from the copper wire blank to the exterior of the wire, a copper concentration gradient exists within the thickness of the coating. The copper concentration within the coating gradually decreases from the wire blank to the exterior. Conversely, the zinc concentration increases in the direction toward the exterior surface of the wire. Due to this copper concentration gradient, at step 84, multiple laminated copper-zinc alloy layers with various phases are revealed. In these laminated copper-zinc alloy layers, the layers are arranged such that the zinc concentration increases as one approaches the exterior surface. Thus, the surface layer of the copper-zinc alloy is always the layer with the highest zinc concentration.

[0079] Here, the purpose of step 84 is to form a surface layer of the δ phase of the Cu-Zn alloy. ini In the copper-zinc alloy, the delta phase appears when the zinc concentration is between 72 atomic % and 77 atomic % and the remainder is copper.

[0080] Therefore, period d ini is selected to be long enough to allow sufficient time for a sufficient amount of copper to diffuse to the surface layer so that the zinc concentration in the surface layer falls to between 72 atomic % and 77 atomic %. ini In the present invention, as long as the zinc concentration in the surface layer is between 72 and 77 atomic % inclusive, the copper-zinc alloy in this layer is in the δ phase.

[0081] Selected period dini If the period d is too short, the zinc concentration is not reduced sufficiently to allow the formation of the δ phase of the alloy, and the surface layer will be a layer of the ε phase of the Cu-Zn alloy. ini If the heating is too long, the zinc concentration in the surface layer will drop below 72 atomic %. For example, a surface layer of the gamma phase of a copper-zinc alloy or the beta phase of a copper-zinc alloy will be obtained.

[0082] Based on these explanations, period d ini is determined by successive experiments. For example, in the case described here, the period d ini is equal to 6 seconds.

[0083] Period D ini Finally, the coating deposited on the copper wire blank has a layer of Cu-Zn alloy β phase on top of a layer of Cu-Zn alloy γ phase on top of which is a surface layer comprising Cu-Zn alloy δ phase.

[0084] As soon as the surface layer is obtained, i.e., here, during the period d ini Immediately at the end of the cooling, the wire is successively subjected to a first step 90 of slow cooling, immediately followed by a second step 92 of rapid cooling.

[0085] During step 90, the wire is cooled slowly enough that 1min From d 1max Period until 1 During this time, the temperature of the surface layer is kept below 559°C and T 90min Maintain above temperature T 90min is 350°C or higher, preferably 400°C or higher or 500°C or lower.

[0086] Period D 1min is the minimum period for which the temperature of the δ phase of the Cu-Zn alloy must be maintained below 559°C. A part of the δ phase of the Cu-Zn alloy is transformed into the γ phase of the Cu-Zn alloy, forming a Cu-Zn alloy γ phase lamellar texture containing most of the γ phase of the Cu-Zn alloy. In parallel with the above, the remainder of the Cu-Zn alloy δ phase is transformed into the Cu-Zn alloy ε phase which fills the interlamellar spaces of the Cu-Zn alloy γ phase lamellar texture.

[0087] Period D 1max is the shortest period of time until the CuZn alloy lamellar texture disappears and transforms into a sub-phase with 90% by weight formed by the CuZn alloy γ phase.

[0088] Period D 1 It has been observed that the cooling time is generally between 0.1 and 1.5 seconds. Therefore, to maintain the surface layer temperature between 559°C and 350°C, a cooling rate of less than 2100°C / s during step 90 is required. The cooling rate during step 90 is preferably less than 1000°C / s or less than 400°C / s. Here, during step 90, the wire is quickly removed from the furnace and cooled for a period d 1 The wire is cooled by placing it entirely in room temperature air, where the cooling rate is typically between 50°C / s and 200°C / s, often close to or equal to 100°C / s.

[0089] Here, period d 1 was chosen to be equal to 0.6 seconds. For this purpose, the wire is removed from the furnace and then kept in air at room temperature for 1 second. In fact, under these conditions, it takes about 0.4 seconds for the temperature of the wire to go from 600 ° C to 559 ° C. The wire is therefore maintained at a temperature between 559 ° C and 350 ° C for 0.6 seconds. In this case, the period d 1 At the end of the process, the temperature of the surface layer is about 500°C, thus much higher than 350°C.

[0090] At the end of step 90, lamellar texture 40 is formed within layer 18. However, as mentioned above, at this stage this lamellar texture is not stable.

[0091] The purpose of step 92 is to fix the lamellar texture 40 obtained after step 90, thus making it metastable at room temperature. For this purpose, immediately after step 90 and during step 92, the wire is subjected to a period d 2 3. The lamellar texture 40 is then rapidly cooled between the first and second temperatures to suddenly reduce the temperature of the lamellar texture 40 to below 30°C.

[0092] This second cooling is called rapid. Period d 2 is period d 1 1 / 2, i.e., half, of the period d 1 Because it is 1 / 10 or 1 / 50 of the period d 2 is less than 0.05 seconds, and in most cases less than 0.03 seconds.

[0093] During this short period 2 In order to obtain a temperature of 100° C., the cooling rate during step 92 is much faster than during step 90. This cooling rate is typically greater than 10,000° C. / sec during step 92. For example, here, the period d 1 At the end of step 92, the wire is quenched in water at room temperature. In this case, the cooling rate during step 92 is of the order of 20,000° C. / s, and the period d 2 is approximately 0.02 seconds.

[0094] After step 92, the lamellar texture 40 is in a metastable state and therefore does not appreciably change any further as long as the wire is maintained at room temperature.

[0095] Then, in step 94, the wire obtained at the end of step 92 is drawn to obtain electrode wire 2. This wire drawing step 94 allows the diameter of the electrode wire to be set to the desired diameter, here 250 μm. In step 94, layers 16 and 18 are broken. Thus, the majority of the breaks located in layers 16 and 18 occur in this step 94.

[0096] Chapter III: Variations Modifications of the manufacturing method There are many other ways in which the electrode wire 2 can be manufactured. For example, the manufacturing method described in chapter II can be carried out using a wire blank that is not necessarily made entirely of copper. For example, the wire blank only comprises a surface layer that is more than 50 atomic % or 60 atomic % and less than 95 atomic % or 90 atomic %. Similarly, it can be carried out with a coating in which the concentration of zinc is less than 100 atomic %. However, it is preferred that the zinc concentration of the coating is greater than or equal to 95 atomic %, greater than or equal to 98 atomic %.

[0097] There are various ways to obtain a Cu-Zn alloy layer in the δ phase, with a first cooling in step 90 and a second cooling in step 92. For example, according to a first variant, the procedure for obtaining this Cu-Zn alloy layer in the δ phase is as follows: - Depositing a nickel layer approximately 5 μm thick on the surface of the wire blank. - immersing the nickel-coated wire blank in a bath of molten copper and zinc, the zinc concentration being between 72 atomic % and 77 atomic % and the remainder being copper; The diffusion takes place at a temperature between 559°C and 700°C, preferably between 559°C and 600°C, more preferably equal to 600°C, producing a Cu-Zn alloy surface layer in the δ phase which is stable as long as the temperature is maintained between 559°C and 700°C.

[0098] According to the second variant, the procedure is as follows. - Depositing a nickel layer approximately 5 μm thick on the surface of the wire blank. - co-extrusion of this wire blank coated with nickel with an alloy of copper and zinc, the zinc concentration of which is between 72 and 77 atomic %, and maintained at a temperature between 559 and 700°C, preferably equal to 600°C. This method produces a copper-zinc alloy surface layer in the δ phase, which is stable on this wire blank coated with nickel, as long as the temperature is equal to 600°C.

[0099] According to the third variant, the procedure is as follows. - Depositing a nickel layer approximately 5 μm thick on the surface of a metal wire blank. -Depositing a layer of copper on top of the nickel layer, then a layer of zinc in which the copper to zinc ratio is between 72 atomic % and 77 atomic % of the zinc, the excess of zinc being chosen to compensate for the inevitable evaporation of zinc during the subsequent diffusion step. the latter is diffused at a temperature between 559°C and 700°C, preferably between 559°C and 600°C or preferably equal to 600°C, to form a Cu-Zn alloy surface layer in the δ phase.

[0100] According to the fourth variant, the procedure is as follows. - A coating of copper and zinc in the δ phase composition is deposited on a wire blank by aqueous phase electrodeposition. The wire is heated to a temperature between 559°C and 700°C, preferably between 559°C and 600°C, more preferably between 595°C and 600°C, so as to form a Cu-Zn alloy surface layer in the -δ phase.

[0101] In practice for the aqueous phase electrodeposition of copper and zinc coatings of δ-phase composition, a wire blank constitutes the cathode and an anode is used, for example made of a copper-zinc alloy with a zinc concentration between 72 and 77 atomic %, i.e. a suitable mixture of γ and ε phases at room temperature. The electrolytic bath is adapted to deposit coatings of δ-phase composition, preferably containing 76% zinc in the deposit. For example, such a bath may include: - Water as a solvent - Copper cyanide CuCN: 9g / L - Zinc cyanide Zn(CN) 2 : 70g / L - Sodium cyanide NaCN: 125g / L - Potassium hydroxide KOH: 81 g / L - Temperature: 20℃~80℃ - Current density: 1 A / dm 2 ~10 A / dm 2 .

[0102] The advantage of electrodeposition of copper-zinc alloys is that the composition is constant within the thickness of the coating, in contrast to the diffusion of zinc on a copper or brass substrate, which has a composition gradient in the absence of a barrier layer.

[0103] The wire drawing step 94 can be omitted: in this case there are no discontinuities between the different textured regions, but rather the lamellar texture extends continuously around the entire circumference of the electrode wire.

[0104] Or, period d ini selects a period of time long enough for an ε-phase Cu-Zn alloy surface layer to form on a layer of δ-phase Cu-Zn alloy. In this case, after steps 90 and 92, layer 18 having lamellar texture is covered with a thin layer of ε-phase Cu-Zn alloy. Thus, in this case, layer 18 is not a surface layer of the electrode wire.

[0105] Electrode wire variations: The core of the electrode wire does not have to be made of copper or a copper-containing alloy, such as brass. The core may be made of, for example, steel or another conductive metal. If the core does not contain copper, the δ-phase copper-zinc alloy surface layer can be obtained in a different way. For example, it can be produced according to any of the production methods of the first to fourth variants described above.

[0106] Layers 14 and 16 can be omitted, particularly when the copper-zinc alloy surface layer in the δ phase is not obtained using a method in which the copper of the central core diffuses into the zinc coating. The manufacturing methods of the first to fourth variations are examples of manufacturing methods in which the copper of the central core diffuses into the zinc coating is not used.

[0107] The core need not be made of a single metal or single metal alloy, or it may comprise multiple layers of the respective metal or metal alloy, for example the core may comprise a central body of copper or steel coated with a layer of brass.

[0108] Alternatively, layer 18 is uniform and thus formed with a single textured region that extends continuously around the entire circumference of central core 10. For example, to manufacture this variant, during step 82, a wire electroplated with zinc is drawn directly to the required final diameter, and wire drawing step 94 is omitted. The other steps of the method from FIG. 5, for example, remain unchanged.

[0109] Section IV: Advantages of the Described Embodiments It has been observed that during its passage through the machining area of ​​the electric discharge machine in which the electric discharge machining process is used, the outer surface of the electrode wire is generally subjected to several successive sparks. This results in that, after a first spark that affects the outer surface of the electrode wire, subsequent sparks are generated on the outer surface modified by the first spark and other intermediate sparks. In other words, the sparks gradually modify the outer surface of the electrode wire, which may affect the efficacy of subsequent sparks, especially when the speed of the discharge is concerned. In particular, the sparks locally modify the topography of the coating of the electrode wire by melting the material that may flow. For example, in the case of the electrode wire described in US Pat. No. 8,067,689, it is in particular the melting of the copper-zinc alloy in the ε phase that modifies the topography of the coating, since the ε phase has a lower melting point than the γ phase.

[0110] In order to maintain a surface layer of the electrode wire with good erosion efficiency over the entire passage in the machining zone during electrical discharge machining, it is now proposed to reduce as much as possible the decrease in erosion efficiency due to successive machining sparks. In this way, the outer surface of the coating of the electrode wire can maintain good erosion efficiency during long parts of the movement in the machining zone where electrical discharge sparks are generated.

[0111] Compared to the electrode wire described in US Pat. No. 8,067,689, whose surface layer comprises islands of gamma-phase Cu-Zn alloy embedded in an epsilon-phase Cu-Zn alloy, the textured regions of the electrode wire described here produce less liquid when exposed to strong and short machining sparks. Craters resulting from discharge sparks are therefore characterized, for example, by fewer resolidification regions. When less liquid is produced, the electrode wire loses less material during the spark. Thus, the travel speed of the electrode wire can be reduced while maintaining a good machining speed, and thus the consumption of the electrode wire can be reduced.

[0112] On the other hand, when a smaller amount of liquid is produced, there are fewer breaks or pores to be blocked by the liquid flow, resulting in a better preservation of the surface shape of the electrode wire, thus increasing the processing speed.

[0113] The improved performance of the electrode wire described herein is presently explained by the fact that the ε-phase CuZn alloy present in layer 18 is sandwiched between lamellae of lamellar texture 40. Since the melting point of the CuZn alloy γ-phase lamellae is higher than the melting point of the CuZn alloy ε-phase, as the CuZn alloy ε-phase melts, it is held within the interstices by the lamellae of lamellar texture 40.

[0114] The fact that layer 18 is the surface layer of the electrode wire makes it possible to take advantage of the properties of the lamellar texture 40 from the very beginning of the EDM process.

Claims

1. An electrode wire for electric discharge machining, The electrode wire is A metal core (10); a coating (12) on said metallic core comprising one or more textured regions (26-28) of a copper-zinc alloy; The textured regions are formed only by the intertwining of the γ phase of the Cu-Zn alloy and the ε phase of the Cu-Zn alloy, respectively. a majority of the gamma phase of the copper-zinc alloy in each texture region (26-28) is in the form of a lamellar texture (40) in which gaps (54) between lamellae (44, 46) consisting of the gamma phase of the copper-zinc alloy are filled with the epsilon phase of the copper-zinc alloy; Electrode wire comprising:

2. The coating includes a first layer (18) of a copper-zinc alloy extending around the entire circumference of the metallic core; Each textured region of the copper-zinc alloy is located inside the first layer. The electrode wire of claim 1 .

3. the first layer (18) forms a surface layer of the electrode wire such that each textured region of copper-zinc alloy is flush with the outer surface of the electrode wire; 3. The electrode wire of claim 2.

4. the first layer (18) includes fissures (22-24) that mechanically separate respective textured regions (26-28) of Cu-Zn alloy in a cross-section of the electrode wire; 4. The electrode wire according to claim 2 or 3.

5. The coating (12) extends continuously from the metal core (10) to the outside of the electrode wire, a homogeneous second layer (16) of copper-zinc alloy formed only of the gamma phase of the copper-zinc alloy; the first layer (18) formed directly on the second layer; The electrode wire according to any one of claims 1 to 4.

6. the thickness of said first layer (18) of copper-zinc alloy is greater than 2 μm and the maximum width of each textured region (26-28) of copper-zinc alloy in the cross section of the electrode wire is greater than 5 μm; The electrode wire according to any one of claims 1 to 5.

7. each lamella (44, 46) of the lamellar texture extends primarily along a respective central trajectory (48, 50) in the cross-section of the electrode wire; For the majority of the lamellae of the lamellar texture, the average thickness of the lamellae along the central track is less than 1 μm or 0.5 μm. The electrode wire according to any one of claims 1 to 6.

8. The maximum width of the gap (54) between the two lamellae is less than 1 μm or less than 0.5 μm; 8. The electrode wire according to claim 7.

9. A method for manufacturing an electrode wire according to any one of claims 1 to 8, comprising the steps of: a) producing (82) a coating on a metal wire blank, the coating being capable of forming a layer of a Cu-Zn alloy δ-phase at a temperature between 559°C and 700°C; b) heating the coating to a temperature of at least 559°C and at most 700°C and maintaining it there until a layer of the CuZn alloy δ phase is obtained (84). c) then, as soon as the layer of δ phase of the Cu-Zn alloy is obtained, a first cooling is carried out for a period d, in which the temperature of the layer of δ phase of the Cu-Zn alloy is kept above 350°C and below 559°C; 1min From period d 1max Period d between 1 A step (90) performed during The period d 1min is the minimum period during which the temperature of the δ phase of the copper-zinc alloy must be maintained between 350°C and 559°C; a part of the δ phase of the copper-zinc alloy is transformed into a γ phase of the copper-zinc alloy to form a lamellar texture of the γ phase of the copper-zinc alloy containing a majority of the γ phase of the copper-zinc alloy; In parallel with this, the remainder of the Cu-Zn alloy δ phase is transformed into Cu-Zn alloy ε phase which fills the interstices between the lamellae of the Cu-Zn alloy γ phase lamellar texture; The period d 1max is the period of time until the lamellar texture CuZn alloy disappears and transforms into a sub-layer formed by the gamma phase of the CuZn alloy at 90% by weight (90). d) The said period d 1 Immediately after this time, a second cooling step (92) is performed to reduce the temperature of the lamellar texture to 30° C. in less than 0.05 seconds.

10. The period d 1min is 0.1 seconds or more, and the period d 1max is less than 1.5 seconds, The method for manufacturing an electrode wire according to claim 9 .

11. The copper concentration on the surface layer of the metal wire blank is greater than 50 atomic % or 60 atomic %; and Producing the coating includes producing a layer having a zinc concentration of greater than 98 atomic percent directly on a surface layer of the metal wire blank. The method for manufacturing an electrode wire according to claim 9 or 10.

12. In step b), placing the metal wire blank on which the coating is formed in a furnace at 600° C. for 6 seconds; The method for manufacturing an electrode wire according to claim 11 .

Citation Information

Patent Citations

  • Manufacture of wire electrode, and wire electrode

    JP1996318434A

  • EDM wire

    US20090025959A1

  • Electrode wire for use in electric discharge machining and process for preparing same

    US5945010A

  • Delta-phase brass electrode wire for electroerosion machining, and method for manufacturing same

    WO2020128953A1

  • Electrode wire for electrical discharge machining

    JP3090009B2