Process for producing microcrystalline cellulose having reduced nitrite content
Heat treatment of microcrystalline cellulose addresses the challenge of high nitrite content in MCC powder by achieving substantial nitrite reduction, ensuring safety in food and pharmaceutical applications.
Patent Information
- Application Number
- JP2024530458
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2022-01-11
- Filing Date
- 2022-09-22
- Publication Date
- 2024-11-19
AI Technical Summary
Existing methods are ineffective in reducing nitrite content in microcrystalline cellulose (MCC) when it is in powder form, posing a risk due to the potential formation of nitrosamines, which are considered human carcinogens.
A process involving heat treatment of microcrystalline cellulose, either in powder form or as a wet cake, to significantly reduce nitrite content without the use of chemical adjuvants.
The heat treatment method effectively reduces nitrite content in MCC by at least 50% and up to nearly complete removal, even when the MCC is in powder form, thereby minimizing health risks associated with nitrosamine formation.
Smart Images

Figure 2024543120000001 
Figure 2024543120000002 
Figure 2024543120000003
Abstract
Description
[Technical field]
[0001] The present specification relates to a process for producing microcrystalline cellulose having reduced nitrite content. [Background technology]
[0002] Microcrystalline cellulose, commonly referred to as "MCC", is widely used in the food and pharmaceutical industries to improve properties or attributes of final products. Applications of MCC include, for example, as a binder or stabilizer in beverages, as a binder or disintegrant in pharmaceutical tablets, as a suspending agent in liquid pharmaceutical formulations, in industrial applications, in household products such as detergents or bleaches, in agricultural formulations, or as a binder, disintegrant or processing aid in personal care products such as dentifrices or cosmetics.
[0003] Microcrystalline cellulose is typically produced by hydrolysis of cellulosic material, preferably high alpha content cellulosic material, obtained from fibrous plant material, with a mineral acid, preferably hydrochloric acid (acid hydrolysis). The mineral acid preferentially attacks the amorphous regions of the cellulosic material, thereby exposing, liberating and leaving behind the paracrystalline regions that form the crystalline aggregates that make up microcrystalline cellulose. The aggregated crystalline mass is then separated from the reaction mixture and washed to remove degraded by-products. The resulting wet mass, which typically contains 40%-60% moisture, is commonly referred to by those skilled in the art as "hydrolyzed cellulose wet cake" or "microcrystalline cellulose / MCC wet cake."
[0004] Processes for producing microcrystalline cellulose by acid hydrolysis are disclosed in U.S. Patents 2,978,446, 3,023,104, and 3,146,168. Alternative methods have been proposed to reduce the cost while maintaining the quality of microcrystalline cellulose. These include steam explosion (U.S. Patent 5,769,934), one-step hydrolysis and bleaching, reactive extrusion of the reaction solution of semicrystalline cellulose and water in a pressurized reactor at high temperatures (100-200°C) and partial hydrolysis (U.S. Patent 5,543,511).
[0005] It is well known that impurities in microcrystalline cellulose are glucose, formaldehyde, nitrates and nitrites (Ajit S. Narang et al., "Impact of Excipient Interactions of Solid Dosage Form Stability", Pharmaceutical Research volume 29, pages 2660-2683 (2012)). The formation of nitrosamines is possible in the presence of secondary, tertiary or quaternary amines and nitrites under acidic reaction conditions. Nitrosamines are considered to be probable human carcinogens, which creates a great need to minimize the concentration of nitrosamines in food and pharmaceutical applications. There is also an urgent need to reduce the concentration of nitrites present in MCC, since MCC is widely used in food and pharmaceutical applications. Summary of the Invention [Problem to be solved by the invention]
[0006] There are several known methods for reducing the concentration of nitrite in an aqueous solution, such as ozonation, catalysis, passing the aqueous solution through activated carbon, passing the aqueous solution through an ion exchange resin, using microalgae, or subjecting a water / glycol mixture to high pressure and temperatures above 120°C. Obviously, these methods are not useful for reducing the concentration of nitrite in MCC when the MCC is in the form of a powder. Therefore, there is still an urgent need to find a method for reducing the concentration of nitrite present in MCC. [Means for solving the problem]
[0007] One aspect of the invention is a process for reducing the nitrite content of microcrystalline cellulose comprising subjecting the microcrystalline cellulose to a heat treatment.
[0008] Another aspect of the present invention is a process for producing microcrystalline cellulose comprising the steps of: i) acid hydrolysis of cellulosic material to produce crude microcrystalline cellulose (MCC); ii) washing and at least partially neutralizing the crude MCC obtained in step i) to obtain an MCC wet cake; and iii) spray drying the MCC wet cake, wherein after step ii) or step iii), or after both steps ii) and iii), the MCC is subjected to a heat treatment.
[0009] Surprisingly, it has been found that simple heat treatment of MCC significantly reduces the concentration of nitrite in MCC, even when MCC is present in its powder form. Surprisingly, no chemical adjuvants such as charcoal or glycol are required for nitrite reduction. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] In some embodiments, MCC undergoes heat treatment in the process of the present invention when MCC is in its powder form. When MCC is in its powder form, MCC generally has a moisture content of up to 30%, up to 20%, up to 10%, or up to 5% based on the weight of dry MCC. The moisture content is generally 0% or more, typically 1% or more, more typically 2% or more, based on the weight of dry MCC. In the most preferred embodiment of the present invention, the moisture content is 3% or more, based on the weight of dry MCC. Alternatively, MCC wet cake can undergo heat treatment. MCC wet cake typically contains 30% to 90%, more typically 40% to 80% moisture, based on the weight of wet MCC. Surprisingly, it has been found that the moisture content of MCC before heat treatment affects the concentration of nitrite in MCC after heat treatment. When the moisture content of the MCC before heat treatment is 3-30%, more preferably 5-30%, and most preferably 9-25%, based on the weight of the dry MCC, the nitrite in the MCC can be reduced by heat treatment to a lower concentration in a shorter period of time than when the moisture content is less than 3%, based on the weight of the dry MCC. The moisture content is typically the moisture content in the MCC.
[0011] In some embodiments, the temperature of the heat treatment depends on the duration of the heat treatment. The shorter the duration of the heat treatment, the higher the temperature generally applied, and vice versa. Generally, the MCC is subjected to a heat treatment at a temperature of at least 35° C. The maximum temperature of the heat treatment is not critical, except that it does not cause significant degradation of the MCC. Generally, the heat treatment is performed at a temperature of up to 400° C., typically up to 350° C. In some embodiments, the heat treatment is performed in the absence of chemical adjuvants.
[0012] In some embodiments, the duration of heat treatment depends on the temperature during heat treatment. Generally, the higher the temperature, the shorter the duration of heat treatment, and vice versa. Generally, MCC undergoes heat treatment for at least 1 minute, typically at least 5 minutes. In some embodiments, MCC undergoes heat treatment for at least 30 minutes.
[0013] In one embodiment of the present invention, the MCC is subjected to heat treatment at a temperature of 35-50° C. (or 40-45° C.) for a period of 2 weeks to 12 months, 1-10 months, or 2-8 months.
[0014] In another embodiment, the MCC undergoes heat treatment at a temperature of 50-150° C., 60-120° C., or 70-100° C. for a period of 1-300 hours, 1-200 hours, or 2-100 hours.
[0015] In yet another embodiment, the MCC undergoes heat treatment at a temperature of 150-350° C. (or 200-300° C.) for a period of 1 minute to 1 hour (or 5 minutes to 30 minutes).
[0016] Typical nitrites reduced by the process of the present invention are ammonium and / or alkali metal nitrites, such as ammonium nitrite and / or sodium nitrite, preferably ammonium nitrite. By the process of the present invention, the nitrite content of the MCC is typically reduced by at least 50% by heat treatment, based on the weight of nitrite in the MCC before heat treatment. In some embodiments, the nitrite content of the MCC is reduced by at least 80%, at least 90%, or at least 95%.
[0017] Generally, microcrystalline cellulose (MCC) from any source can be used in the process of the present invention.Typically, suitable sources of MCC include, for example, wood pulp (such as bleached sulfite pulp and sulfate pulp), straw, cotton, flax, cotton linters, hemp, ramie, corn husk, bagasse, seaweed cellulose and fermented cellulose.Other sources include bleached softwood kraft pulp, bleached hardwood kraft pulp, bleached eucalyptus kraft pulp, paper pulp, fluff pulp, dissolving pulp and bleached non-wood cellulose pulp.In one embodiment, the MCC used is approved for human consumption by the US Food and Drug Administration.
[0018] If desired, low-cost pulp or a mixture of low-cost and specialty pulps can be used as the source of MCC. If so, for example, about 30-80% of the total MCC can be comprised of low-cost pulp. In some embodiments, the colloidal content of the resulting MCC product is at least 60%. Examples of low-cost pulp include fluff pulps such as paper pulp, southern bleached softwood kraft pulp, northern bleached softwood pulp, bleached eucalyptus kraft pulp, bleached sulfite pulp, bleached hardwood kraft pulp, bleached soda pulp, and bleached non-wood pulp.
[0019] The process for producing MCC comprises step i) of subjecting cellulosic material to acid hydrolysis to produce crude MCC. The term "acid hydrolysis" as used herein does not imply a limitation to complete hydrolysis, but encompasses partial hydrolysis as commonly applied in known processes for producing MCC. Crude MCC is typically produced by partially hydrolyzing the above-mentioned cellulosic feedstock with acid, in some embodiments with mineral acid, or in some embodiments with hydrochloric acid (acid hydrolysis). Processes for producing microcrystalline cellulose by acid hydrolysis are disclosed in US Pat. Nos. 2,978,446, 3,023,104, and 3,146,168. Mineral acid preferentially attacks the amorphous regions of the cellulosic feedstock, thereby exposing, liberating, and leaving behind the paracrystalline regions that form the crystalline aggregates that constitute microcrystalline cellulose. During partial hydrolysis of the cellulosic feedstock, the average degree of polymerization (=DP) is reduced to a plateau value that reflects the destruction of the original fibrous structure of the cellulosic feedstock. The plateau value that can be obtained by partial hydrolysis depends mainly on the choice of the feedstock. MCC with an average plateau DP in the range of 15 to 60 can be produced, for example, from regenerated forms of cellulose. MCC with an average plateau DP in the range of 60 to 125 can be obtained from alkali-swollen natural forms of cellulose, such as cotton linters and refined wood pulp. With sulfite pulp as raw material, MCC with an average plateau DP in the range of 200 to 400 is typically produced. The average plateau degree of polymerization (=DP) is determined according to DIN 54 270, parts 1 and 2.
[0020] MCC can be made more suitable for any of the wear processes described further below by chemical or mechanical treatment. For example, during or after the acid hydrolysis of MCC, MCC can be treated with carboxymethylcellulose (CMC), peroxide, peracetic acid, persulfate, performic acid, or ozone at acidic pH. Other additives such as iron salts can be added to promote hydrolysis of MCC. Promotion of hydrolysis can also be achieved by cooking MCC for an extended period of time or by modifying reaction conditions such as cooking temperature, acid concentration, etc.
[0021] The process for producing MCC further comprises step ii), in which after partial hydrolysis, the agglomerated crystalline mass, i.e., crude MCC, is washed and at least partially neutralized with an aqueous liquid to remove decomposed by-products and at least partially neutralize excess acid used in acid hydrolysis. Typically, the washing step includes filtration, followed by dilution to produce an MCC wet cake suitable for spray drying. A neutralizing agent can be added to the washing liquid. In some embodiments, it is added to the liquid used for dilution. Examples of neutralizing agents are, for example, ammonium bicarbonate or ammonium carbonate. In some embodiments, the neutralizing agent comprises ammonia or ammonium hydroxide.
[0022] In some embodiments, the washing liquid is water, brine, or an organic solvent mixed with water, such as an aqueous mixture of isopropanol, ethanol, or methanol. In some embodiments, the washing liquid is water or brine. The resulting wet mass typically contains 30% to 80%, more typically 40% to 70% moisture, based on the total weight of the wet MCC. Optionally, the MCC is modified for specific uses in food, pharmaceutical, or cosmetic applications, such as use as a gelling agent, thickener, fat replacer, non-caloric filler, suspending agent, texturizer, or stabilizer in emulsions. In some embodiments, the MCC is modified for such uses by subjecting the hydrolyzed wet MCC to high shear mixing, referred to as "attrition." The process of attrition typically breaks down the microcrystalline crystallites into fine particles (in some embodiments, in the colloidal range). Colloidal microcrystalline cellulose, such as that modified with CMC, is described in U.S. Pat. No. 3,539,365. Typically, the optionally attrited MCC is then diluted prior to spray drying. In some embodiments, the diluent is water, and in some embodiments includes a neutralizing agent as described above. Diluted MCC suitable for spray drying is generally in the form of an aqueous slurry of MCC, and typically contains about 10%-20% MCC and about 80%-90% water, based on the total weight of the dry MCC and water. Both wet MCC, containing 30%-80% water, based on the total weight of the wet MCC, and diluted MCC, containing about 10%-20% MCC and about 80%-90% water, based on the total weight of the dry MCC and water, are referred to herein as "MCC wet cake."
[0023] In step iii) of the process, the MCC wet cake is spray dried. The desired commercial grade of MCC is obtained by modifying and controlling the spray drying conditions to manipulate the agglomeration (particle size distribution) and moisture content of the MCC product. [G. Thorens, Int. J. Pharm. (2015), 490, 47-54; G. Thorens, Int. J. Pharm. (2014), 473, 64-72)]. Suitable spray drying equipment and conditions are known in the art.
[0024] Thus, the process for producing MCC comprises the steps of: i) acid hydrolysis of cellulosic material to produce crude microcrystalline cellulose (MCC); ii) washing and at least partially neutralizing the crude MCC obtained in step i) to obtain an MCC wet cake; and iii) spray drying the MCC wet cake. The embodiments of steps i)-iii) of this process are as described above. After step ii) or step iii), or both steps ii) and iii), the MCC is subjected to a heat treatment as further described above to reduce the nitrite content of the MCC.
[0025] In one embodiment, the MCC is subjected to a heat treatment as further described above after step ii) and before step iii), which can reduce the concentration of nitrite potentially originating from the starting materials used to produce the MCC and / or from step ii) involving partial or complete neutralization of the crude MCC obtained in step i).
[0026] In another embodiment, the MCC is subjected to a heat treatment as further described above after the spray-drying step iii), which not only reduces the concentration of nitrite potentially originating from the starting material used to produce the MCC, but also reduces the concentration of nitrite potentially originating from partial or complete neutralization of the crude MCC obtained in step i) and reduces the concentration of nitrite potentially originating from the spray-drying step, e.g. the concentration of nitrite potentially originating from the drying gas utilized in the spray-drying step.
[0027] Other features and advantages of the present invention will become apparent from the following examples. The disclosed embodiments are for illustrative purposes and are merely exemplary and should not be considered as limiting the invention. All parts, percentages and ratios are by weight unless otherwise stated. EXAMPLES
[0028] Determination of nitrite content of MCC Nitrite measurements were performed on an ion exchange chromatography system (Dionex ICS-6000 system consisting of an AS-AP autosampler, quaternary pump, KOH eluent generator, anion suppressor, conductivity detector, and Chromeleon 7.2.9 chromatography data system) equipped with a microbore analytical column and guard columns (Dionex IonPac AS 19, 2 × 250 mm, catalog no. 062886 and Dionex IonPac AG19, 2 × 50 mm, catalog no. 062888). A KOH gradient was generated simultaneously by a KOH eluent generator: - 10 min at 1 mmol for equilibration (meaning a 10 min pre-equilibration time to equilibrate the IC column before starting the IC method run), 0-15 min from 1 mmol to 20 mmol, 15.1 min to 50 mmol, and hold at 50 mmol until 28 min, 50 mmol to 1 mmol from 28-29 min, and the run stopped at 30 min. The flow rate was 0.5 mL / min. Anion suppression with an ADRS 2 mm suppressor was applied in dynamic mode with a starting voltage of 3.8 V. The column temperature was 30 °C and the compartment temperature was 15 °C. Injections were performed with a 25 μL sample loop.
[0029] For nitrite analysis, microcrystalline cellulose (MCC) samples were prepared by extracting 1 g of MCC with 15 g of high purity water (electrical resistivity >18 MΩ-cm at 25°C, prepared by filtering deionized water with any reliable laboratory water purification system such as Millipore Sigma's Milli-Q IQ7003 / 7005 / 7010 / 7015 system) in a 50 mL centrifuge tube for 30 minutes on a shaker at slow shaking speed. The tube was then centrifuged at 10000 rpm for 10 minutes to precipitate the MCC (Sorvall Legend XT / XF Centrifuge Series, Cat. 75004541). The clear extraction solution was filtered through a 0.45 μm PTFE filter and placed in an IC autosampler vial for analysis by ion exchange chromatography (IC). Samples were prepared using IC analytical standards (1000 μg / g nitrite (NO2 - ), part numbers ICNO31-125ML and ICNO21-125ML) were used to calibrate the reagent using external calibration standards prepared at 0.5 μg / g, 0.05 μg / g, and 0.005 μg / g.
[0030] Moisture analysis Moisture analysis was performed using a Mettler-Toledo HB 43-S halogen moisture meter and moisture was calculated as % loss on drying (LOD) at 110°C.
[0031] MCC Generation Process The MCC used as the starting material in the thermal treatment was produced by acid hydrolysis of commercial high purity wood pulp with alpha content above 90%. The acid hydrolysis was carried out using aqueous hydrochloric acid. The resulting MCC was separated from the reaction by-products and washed using water during a filtration process to produce an MCC wet cake with a solid content of about 35%-40% having an average degree of polymerization (DP) of about 240. The MCC wet cake was diluted with water to a solid content of about 20% and anhydrous ammonia was added along with the water to neutralize the residual acid to obtain a pH of 5.5-7.0 in the final powder. Finally, the diluted MCC was spray dried to produce a powder.
[0032] Example 1 The MCC samples were produced according to the MCC production process described above, except that an additional filtration was performed after ammonia neutralization and before spray drying.
[0033] 10 g of MCC sample was weighed into each of 2 oz HDPE bottles. These samples were heated in a non-humidity controlled commercial oven at 50°C, 70°C, and 90°C for 1, 2, or 3 hours, respectively. At each designed experimental time point, such as after 1 hour of heating at 90°C, the specific bottle used only for this test condition was removed from the oven, cooled, and the nitrite content was determined as above. The results in Table 1 below show the nitrite content in ppm after various times and various temperatures of heat treatment.
[0034] [Table 1]
[0035] Example 2 The MCC samples were produced according to the MCC production process described above, except that hydrogen peroxide was added after ammonia neutralization and before spray drying at a concentration of 3 wt. % based on the weight of the dried MCC. Additional filtration was applied after the addition of hydrogen peroxide and before spray drying.
[0036] The results in Table 2 below show the nitrite content in ppm after heat treatment for various times and temperatures.
[0037] [Table 2]
[0038] Example 3 The MCC samples were produced according to the MCC production process described above. No hydrogen peroxide addition and no additional filtration was applied.
[0039] The results in Table 3 below show the nitrite content in ppm after heat treatment for various times and temperatures.
[0040] [Table 3]
[0041] Example 4 A commercially available MCC material produced according to the MCC production process described above was evaluated.
[0042] The results in Table 4 below show the nitrite content in ppm after heat treatment for various times and various temperatures.
[0043] [Table 4]
[0044] The results in Tables 1-4 above show the surprising discovery that a simple heat treatment can almost completely remove the nitrite content of bulk MCC powder, even though only trace amounts of nitrite are present in the MCC powder before heat treatment. Surprisingly, the promise that nitrite would be stabilized in the MCC matrix, preventing a significant reduction in nitrite levels, was not fulfilled.
[0045] Example 5 MCC powder commercially available under the trademark AVICEL PH-102 was used for the heat treatment experiments. AVICEL PH-102 microcrystalline cellulose has a nominal particle size of 100 μm, a moisture content of 3.0-5.0% LOD (loss on drying), and a bulk density of 0.28-0.33 g / ml.
[0046] MCC sample 5-I was obtained by drying AVICEL PH-102 MCC in a vacuum oven at ambient temperature for several days to a desired final LOD of 0.4% based on the weight of the completely dried MCC.
[0047] MCC Sample 5-II was AVICEL PH-102 MCC with a moisture content, or LOD (loss on drying), of 4.2% based on the weight of the completely dried MCC.
[0048] MCC samples 5-III, 5-IV, and 5-V were obtained by humidifying AVICEL PH-102 MCC in a Lodige ploughshare reactor unit at room temperature. The desired amount of deionized (DI) water was sprayed (60 psig air pressure through a hollow cone nozzle with a 30° spray angle) onto the stirred MCC powder for 1-2 minutes. Stirring was continued for an additional hour for mixing / homogenization. The humidified MCC was then removed from the reactor. Humidification was performed three times by adding three different amounts of DI water. The LOD of each humidified MCC was measured to determine the new moisture level. The LOD of MCC sample 5-III was 9.3%, the LOD of MCC sample 5-IV was 12.4%, and the LOD of MCC sample 5-V was 24.9%. The samples were then subjected to heat treatment. The heat treatment experiments were carried out in a stirred Lodige VT10 ploughshare blender. The jacket system was heated using a self-contained heater / chiller system using a glycol / water mixture. The jacket system was set at 99°C to achieve an internal temperature of approximately 90°C. The unit was preheated before the MCC powder was added to the unit. Each of the MCC samples 5-I through 5-V were added individually to the preheated Lodige reactor and stirred at temperature over the first day and twice on the second day. All samples were measured for LOD and nitrite content immediately after removal from the reactor. Nitrite content is based on the weight of dry MCC. The results are shown in Table 5 below.
[0049] [Table 5]
[0050] [Table 6]
[0051] The results in Table 5 above confirm the surprising discovery that the nitrite content can be almost completely removed in bulk MCC powder by simple heat treatment, even though only trace amounts of nitrite are present in the MCC powder before heat treatment. The results in Table 5 above also show the surprising discovery that the rate and extent of reduction in nitrite content is dependent on the humidity of the MCC sample before heat treatment.
[0052] Example 6 MCC samples commercially available under the trademarks AVICEL PH-102, AVICEL PH-112 and AVICEL SMCC90 were used in the heat treatment experiments. AVICEL PH-102 microcrystalline cellulose has a nominal particle size of 100 μm, a moisture content of 3.0%-5.0%, and a bulk density of 0.28-0.33 g / ml. AVICEL PH-102 was from a different batch than Example 5, so the starting nitrite content was slightly different than Example 5. AVICEL PH-112 microcrystalline cellulose has a nominal particle size of 100 μm, a moisture content of 1.5% or less, and a bulk density of 0.28-0.34 g / ml. AVICEL SMCC90 has an average particle size (d50) of 90-150 μm and a bulk density of 0.25-0.37 g / ml as determined by laser diffraction. AVICEL SMCC90 is a co-processed spray dried excipient containing 98% MCC and 2% colloidal silicon dioxide.
[0053] 10g of MCC sample was weighed and placed into each of 2 oz (approximately 60ml) HDPE bottles. The bottles were placed in an oven and maintained at a temperature of 40°C and humidity of 75%. Designated bottles were removed from the oven for each specific experimental time point, such as 1 month treatment at 40°C and 75% humidity. Nitrite content was analyzed as above. The results in Table 6 below show the nitrite content in ppm after various periods of heat treatment.
[0054] [Table 7]
[0055] The results in Table 6 above show that even very gentle heating at only 40°C can achieve a significant reduction in nitrite content when the MCC is kept at this temperature for extended periods. For example, reduction in nitrite content can be achieved very simply by storing the MCC in a temperature controlled store.
[0056] Example 7 MCC commercially available under the trademark AVICEL PH-101 was used for the heat treatment experiments. AVICEL PH-101 microcrystalline cellulose has a nominal particle size of 50 μm, a moisture content of 3.0%-5.0%, and a bulk density of 0.26-0.31 g / ml. For heat treatment, 10 g of Avicel PH101 microcrystalline cellulose was stored at high temperature in a cabinet oven for a very short period of time. The results in Table 7 below show the nitrite content in ppm after heat treatment for various periods and at various temperatures.
[0057] [Table 8]
[0058] The results in Table 7 above show that at elevated temperatures a significant reduction in nitrite content can be achieved within a very short period of time.
[0059] Examples 8 and 9 The experiments of Examples 8 and 9 were conducted to evaluate whether the nitrite content of MCC could be reduced by simple heat treatment of MCC in bulk. In Example 8, a drum containing about 50 kg of MCC commercially available under the trademark AVICEL PH-112 was placed in a storage cabinet at a temperature of 40° C. The MCC was from a different batch than in Example 6, so the starting nitrite content was slightly different than in Example 6. The drum was simply left in the storage cabinet without agitation. At weekly intervals, MCC samples were taken from the drum and analyzed for nitrate content as further described above. The results are shown in Table 8 below.
[0060] [Table 9]
[0061] In Example 9, a box containing about 20 kg of MCC commercially available under the trademark AVICEL PH-102 was placed in a warehouse at a temperature of 40° C. The MCC was from a different batch than in Examples 5 and 6, so the starting nitrite content was slightly different than in Examples 5 and 6. The box was simply placed in the warehouse without shaking or other agitation. At weekly intervals, MCC samples were taken from the box and analyzed for nitrate content as further described above. The results are shown in Table 9 below.
[0062] [Table 10]
[0063] Results Tables 8 and 9 show the surprising discovery that the nitrite content of MCC can be reduced by about 50% or even more by simple heat treatment, even in large amounts, and even when the MCC is simply left to sit.
Claims
1. 1. A process for reducing the nitrite content of microcrystalline cellulose, comprising subjecting the microcrystalline cellulose to a heat treatment.
2. 2. The process of claim 1, wherein the microcrystalline cellulose in powder form is subjected to a heat treatment.
3. 3. The process of claim 1 or 2, wherein the microcrystalline cellulose is subjected to a heat treatment at a temperature of at least 35°C.
4. The process according to any one of claims 1 to 3, wherein the microcrystalline cellulose is subjected to a heat treatment for at least 30 minutes.
5. 5. The process according to any one of claims 1 to 4, wherein the microcrystalline cellulose is subjected to a heat treatment at a temperature of from 35 to 50°C for a period of from 2 weeks to 12 months.
6. 5. The process according to any one of claims 1 to 4, wherein the microcrystalline cellulose is subjected to a heat treatment at a temperature of from 50 to 150°C for a period of from 1 to 300 hours.
7. 4. The process according to any one of claims 1 to 3, wherein the microcrystalline cellulose is subjected to a heat treatment at a temperature of from 150 to 350°C for a period of from 1 minute to 1 hour.
8. 8. The process according to any one of claims 1 to 7, wherein the moisture content of the microcrystalline cellulose before heat treatment is from 3 to 30% based on the weight of the dry microcrystalline cellulose.
9. i) acid hydrolysis of a cellulosic material to produce crude microcrystalline cellulose (MCC); ii) washing and at least partially neutralizing the crude MCC obtained in step i) to obtain MCC wet cake; iii) spray drying the MCC wet cake; wherein after step ii) or step iii), or after both steps ii) and iii), the MCC is subjected to a heat treatment.
10. 10. The process of claim 9, wherein the microcrystalline cellulose is subjected to a heat treatment at a temperature of at least 35°C.
11. 11. The process of claim 9 or 10, wherein the microcrystalline cellulose is subjected to a heat treatment for at least 30 minutes.
12. 12. The process according to any one of claims 9 to 11, wherein the microcrystalline cellulose is subjected to a heat treatment at a temperature of from 35 to 50°C for a period of from 2 weeks to 12 months.
13. 12. The process according to any one of claims 9 to 11, wherein the microcrystalline cellulose is subjected to a heat treatment at a temperature of from 50 to 150°C for a period of from 1 to 300 hours.
14. 11. The process according to claim 9 or 10, wherein the microcrystalline cellulose is subjected to a heat treatment at a temperature of from 150 to 350°C for a period of from 1 minute to 1 hour.
15. The process according to any one of claims 9 to 14, wherein in step ii) ammonium bicarbonate, ammonium carbonate, ammonia or ammonium hydroxide is used as neutralizing agent.
Citation Information
Patent Citations
Microcrystalline cellulose and preparation method thereof
CN113336863A
Forms of ivabradine iydrochloride
EP2902384A1
Method and apparatus for producing nanocrystalline cellulose
JP2014167047A
Production method of cellulose
JP2018070665A