Epoxidation catalyst and method for preparing same
By employing a multi-step SiO2 addition process with controlled heating and pressure, the method enhances the catalytic performance of zeolite materials for propylene oxide production.
Patent Information
- Application Number
- JP2024530495
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2021-11-22
- Filing Date
- 2022-11-21
- Publication Date
- 2024-11-19
AI Technical Summary
Existing methods for preparing zeolite materials with skeletal structures containing Si and tetravalent elements like Ti, Sn, or Ge do not effectively utilize multiple SiO2 sources in a controlled manner, leading to suboptimal catalytic performance in reactions such as propylene oxide production.
A method involving the addition of one or more SiO2 sources in multiple steps, with controlled heating and pressure conditions, to produce zeolite materials with improved catalytic activity, particularly for propylene oxide synthesis.
The method results in zeolite materials with enhanced catalytic activity, achieving higher yields and conversion rates of propylene to propylene oxide.
Smart Images

Figure 2024543122000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a particular process for the preparation of a zeolitic material, wherein the framework structure of the zeolitic material comprises Si, O and a tetravalent element M other than Si, where M is selected from the group consisting of Ti, Sn, Zr, Ge and mixtures of two or more thereof. Furthermore, the present invention relates to a zeolitic material obtainable or obtainable by said process, the zeolitic material itself and methods of use thereof. Furthermore, the present invention relates to a moulded article comprising said zeolitic material. [Background technology]
[0002] Zeolitic materials containing another tetravalent element other than Si are known to be efficient catalysts in many applications, including, for example, epoxidation reactions. When carried out in industrial scale processes, such reactions are usually carried out in a continuous mode. Optionally, these zeolitic materials are used in the form of shaped articles that contain a suitable binder in addition to the catalytically active zeolitic material.
[0003] WO 2011 / 064191 A1 relates to a method for preparing a titanium zeolite catalyst. WO 2021 / 123227 A1 relates to a continuous synthesis of titanosilicate zeolite materials. WO 2020 / 221683 A1 relates to a molding comprising a MFI type zeolite titanosilicate and a silica binder, a method for its preparation and use as a catalyst. WO 2020 / 074586 A1 relates to a molding comprising a zeolite material with framework type MFI.
[0004] Xiujuan Deng et al. ("Low-cost synthesis of titanium silicalite-1 (TS-1) with high catalytic oxidation performance by a controlled hydrolysis process", INDUSTRIAL & ENGINEERING CHEMISTRY RESEARCH, Vol. 52, no. 3, January 23, 2013 (2013-01-23), pp. 1190-1196) disclose the synthesis of titanium silicate-1 (TS-1) at low molar ratio of TPAOH / SiO2 by two-step and multi-step hydrolysis processes.
[0005] Zhang Jian Hui et al. ("Synthesis of nano-sized TS-1 zeolite by solid-state conversion method with unprecedentedly low usage of tetrapropylammonium hydroxide", MICROPOROUS AND MESOPOROUS MATERIALS, Vol. 27, pp. 96-101) disclose the synthesis of nano-sized TS-1 zeolite at low molar ratio of TPAOH / SiO2 by solid-state conversion process. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] WO 2011 / 064191 A1 [Patent Document 2] WO 2021 / 123227 A1 [Patent Document 3] WO 2020 / 221683 A1 [Patent Document 4] WO 2020 / 074586 A1 [Non-patent literature]
[0007] [Non-Patent Document 1] Xiujuan Deng et al., "Low-cost synthesis of titanium silicalite-1 (TS-1) with high catalytic oxidation performance via a controlled hydrolysis process", INDUSTRIAL & ENGINEERING CHEMISTRY RESEARCH, Vol. 52, no. 3, January 23, 2013 (2013-01-23), pp. 1190-1196 [Non-Patent Document 2] Zhang Jian Hui et al., "Synthesis of nano-sized TS-1 zeolite by solid-state conversion method with unprecedentedly low usage of tetrapropylammonium hydroxide," MICROPOROUS AND MESOPOROUS MATERIALS, Vol. 217, pp. 96-101 Summary of the Invention [Problem to be solved by the invention]
[0008] The object of the present invention is to provide a novel process for the preparation of a zeolitic material, the framework of which comprises Si, O and a tetravalent element M other than Si, where M is selected from the group consisting of Ti, Sn, Zr, Ge and mixtures of two or more thereof. Furthermore, the object of the present invention is to provide a novel zeolitic material, which has advantageous properties when used as a catalyst or catalyst component, in particular in the epoxidation reaction of propene to propylene oxide, the framework of which comprises Si, O and a tetravalent element M other than Si, where M is selected from the group consisting of Ti, Sn, Zr, Ge and mixtures of two or more thereof. Furthermore, the object of the present invention was to provide a molded article comprising said zeolitic material. Furthermore, the object of the present invention was to provide an improved process for the preparation of propylene oxide. [Means for solving the problem]
[0009] Surprisingly, it has been found that an improved method for preparing zeolitic materials can be provided, in which one or more SiO2 sources are added to the reaction mixture, in particular in two or more steps. It has further been found that improved zeolitic materials can be prepared by said method, in which said zeolitic materials comprise Si, O, and a tetravalent element M other than Si, where M is selected from the group consisting of Ti, Sn, Zr, Ge, and mixtures of two or more thereof. In particular, it has been found that the zeolitic materials prepared according to the method of the present invention exhibit certain properties that make them powerful materials for use in catalytic reactions. In particular, it has been found that zeolitic materials can be produced that exhibit unique physical and chemical properties, and that said zeolitic materials exhibit improved catalytic activity, in particular in the conversion of propylene to propylene oxide. [Brief description of the drawings]
[0010] [Figure 1]1 shows XRD of the zeolite materials of Example 1 and Comparative Example 1. The horizontal axis shows 2θ angle (°), and the vertical axis shows intensity in arbitrary units. [Diagram 2] 2A and 2B show SEM images of the zeolite materials of Comparative Example 1 and Example 1, respectively. [Diagram 3] 3 shows the UV-vis spectra of the zeolite materials of Example 1 and Comparative Example 1. The horizontal axis shows wavelength (nm) and the vertical axis shows absorbance in arbitrary units. [Figure 4] 4 shows the FT-IR spectra of the zeolite materials of Example 1 and Comparative Example 1. The horizontal axis shows wavenumber (cm-1), and the vertical axis shows absorbance in arbitrary units. The absorption band with a maximum wavenumber in the range of 3740-3725 cm-1 is believed to be due to the "external" and "internal" Si-OH groups, while the absorption band with a maximum wavenumber at about 3500 cm-1 is believed to be due to the Si-OH "pores". DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0011] The present invention therefore relates to a method for producing a zeolitic material, preferably a zeolitic material according to any one of the particular and preferred embodiments of the present invention, wherein the framework structure of the zeolitic material comprises Si, O and a tetravalent element M other than Si, M being selected from the group consisting of Ti, Sn, Zr, Ge and mixtures of two or more thereof, said method comprising the steps of: (1) preparing a mixture comprising one or more MO sources, one or more organic templates, a first portion of one or more SiO sources, and a protic solvent system comprising water; (2) heating the mixture obtained in step (1) at a temperature in the range of from 30° C. to the boiling point of the mixture, preferably in the range of 50° C. to 95° C., more preferably in the range of 65° C. to 90° C., more preferably in the range of 75° C. to 85° C.; (3) heating the mixture obtained in step (2) under autogenous pressure at a temperature in the range of 100 to 250°C, preferably 140 to 200°C, more preferably 155 to 185°C, more preferably 165 to 175°C; Including, During step (2), a second portion of the one or more SiO2 sources is added to the mixture.
[0012] Preferably, the heating in step (2) is carried out at atmospheric pressure.
[0013] Preferably, the heating in step (3) is carried out for a duration in the range of 0.25 to 10 days, preferably in the range of 0.5 to 5 days, more preferably in the range of 1.5 to 2.5 days, more preferably in the range of 1.75 to 2.25 days.
[0014] Preferably, the one or more SiO2 sources comprise one or more alkoxysilanes, preferably one or more tetraalkoxysilanes, more preferably one or more tetraalkoxysilanes selected from the group consisting of (C1-C6) tetraalkoxysilanes and mixtures of two or more thereof, more preferably one or more tetraalkoxysilanes selected from the group consisting of (C1-C5) tetraalkoxysilanes and mixtures of two or more thereof, more preferably one or more tetraalkoxysilanes selected from the group consisting of (C1-C4) tetraalkoxysilanes and mixtures of two or more thereof, more preferably one or more tetraalkoxysilanes selected from the group consisting of (C1-C3) tetraalkoxysilanes and mixtures of two or more thereof, more preferably one or more tetraalkoxysilanes selected from the group consisting of tetramethoxysilane and tetraethoxysilane, where more preferably the one or more Si sources comprise tetraethoxysilane, and heating the mixture in step (2) comprises hydrolysis of at least a portion of the one or more alkoxysilanes and distillation of the resulting one or more alcohols from the mixture.
[0015] Preferably, M is selected from the group consisting of Ti, Sn, and mixtures thereof, preferably M comprises Ti, more preferably M is Ti.
[0016] Preferably, in step (1), the one or more organic templates are tetraalkylammonium cations R 1 R 2 R 3 R 4 N + R 1 , R 2 , R 3 and R 4 are each independently an alkyl group.
[0017] In step (1), one or more organic templates are provided that are substituted with a tetraalkylammonium cation R 1 R 2 R 3 R 4 N + Preferably, one or more tetraalkylammonium cations R 1 R 2 R 3 R 4 N + R of the containing compound 1 , R 2 , R 3 and R 4 are each independently an optionally branched (C1-C6) alkyl, preferably a (C1-C5) alkyl, more preferably a (C2-C4) alkyl, more preferably an optionally branched (C2-C3) alkyl, and more preferably R 1 , R 2 , R 3 and R 4 are each independently ethyl or propyl, more preferably one or more tetraalkylammonium cations R 1 R 2 R 3 R 4 N + R of the containing compound 1 , R 2 , R3 and R 4 are each independently propyl, preferably n-propyl. Furthermore, each independently one or more tetraalkylammonium cations R 1 R 2 R 3 R 4 N + The containing compound is preferably one or more salts selected from the group consisting of salts, preferably halides, preferably chlorides and / or bromides, more preferably chlorides, hydroxides, sulfates, nitrates, phosphates, acetates, and mixtures of two or more thereof, more preferably chlorides, hydroxides, sulfates, and mixtures of two or more thereof, and more preferably one or more tetraalkylammonium cations R 1 R 2 R 3 R 4 N + The containing compound is a tetraalkylammonium hydroxide and / or chloride, more preferably a tetraalkylammonium hydroxide.
[0018] It is preferred that M comprises Ti, preferably is Ti, and the one or more TiO2 sources are selected from the group consisting of oxides and salts of Ti, and mixtures thereof, and the one or more TiO2 sources are preferably one or more compounds selected from the group consisting of titanium oxides, titanium salts, titanyl compounds, titanic acids, titanic acid esters, and mixtures of two or more thereof, more preferably tetrabutyl orthotitanate, tetraisopropyl orthotitanate, tetraethyl orthotitanate, titanium dioxide, titanium tetrachloride, titanium tert-butoxide, TiOSO4, and and / or KTiOPO4, and mixtures of two or more thereof, more preferably one or more compounds selected from the group consisting of tetrabutyl orthotitanate, tetraisopropyl orthotitanate, tetraethyl orthotitanate, tetramethyl orthotitanate, titanium dioxide, titanium tetrachloride, titanium tert-butoxide, and mixtures of two or more thereof, more preferably the one or more TiO2 sources comprise titanium tert-butoxide, more preferably titanium tert-butoxide is used as the one or more TiO2 sources.
[0019] Preferably, the mixture obtained in step (2) comprises one or more SiO2 sources, calculated as SiO2, and one or more tetraalkylammonium cations R in a ratio of 1:0.20 to 1:0.05, preferably in a ratio of 1:0.15 to 1:0.09, more preferably in a ratio of 1:0.13 to 1:0.11. 1 R 2 R 3 R 4 N + It has a molar ratio with the contained compound.
[0020] Preferably, the mixture obtained in step (2) has a molar ratio of the one or more SiO2 sources, calculated as SiO2, to water in the range of 1:30 to 1:5, preferably in the range of 1:20 to 1:12, more preferably in the range of 1:17 to 1:15.
[0021] Preferably, the mixture obtained in step (2) has a molar ratio of the one or more SiO2 sources, calculated as SiO2, to the one or more MO2 sources, calculated as MO2, in the range of 1:0.0100 to 1:0.0010, preferably in the range of 1:0.0040 to 1:0.0020, more preferably in the range of 1:0.0035 to 1:0.0031.
[0022] It is preferred to add a second portion of the one or more SiO2 sources continuously or incrementally, preferably incrementally, during the course of step (2).
[0023] If the second portion of the one or more SiO2 sources is added continuously or incrementally during the course of step (2), preferably, the second portion of the one or more SiO2 sources is added incrementally in 1-20 steps, preferably 1-10 steps, more preferably 1-5 steps, more preferably 1 step during the course of step (2).
[0024] Preferably, the heating in step (2) is carried out continuously or intermittently, preferably intermittently.
[0025] When the heating in step (2) is performed intermittently, preferably the heating consists of two or more heating stages, in which the second portion of the one or more SiO2 sources is added during one or more intervals between the two or more heating stages, preferably the heating in step (2) consists of two heating stages, in which the second portion of the one or more SiO2 sources is added during the interval between the two heating stages.
[0026] When the heating in step (2) is performed intermittently, it is particularly preferred that the heating in step (2) consists of three or more heating stages, and one or more second portions of the SiO2 source are added in equal portions during respective intervals between the three or more heating stages, each portion corresponding to a proportion of 1 / n of the total amount of the second portions, n representing the number of intervals during which each portion is added respectively, n+1 corresponding to the number of heating stages, n being an integer comprised in the range of 2 to 5, and n being preferably 2 or 3, more preferably 2.
[0027] If the heating in step (2) is carried out intermittently, during each interval during which a second portion or portions of the one or more SiO2 sources are added, the mixture preferably has a temperature comprised in the range of 15 to 65° C., preferably in the range of 20 to 60° C., more preferably in the range of 35 to 55° C., more preferably in the range of 48 to 52° C. Furthermore, independently therefrom, preferably each heating stage independent of one another is carried out for a duration comprised in the range of 0.1 to 5 hours, preferably in the range of 0.5 to 3.5 hours, more preferably in the range of 1.75 to 2.25 hours.
[0028] When the heating in step (2) is carried out intermittently, the heating preferably consists of 2 to 6 heating stages, preferably 2 to 4 heating stages, more preferably 2 or 3 heating stages, and more preferably the heating consists of 2 heating stages.
[0029] Preferably, the first portion of the one or more SiO2 sources comprises an amount, calculated as SiO2, in the range of 45 to 90 mol %, preferably in the range of 60 to 75 mol %, more preferably in the range of 65 to 68 mol %, of the total amount (100 mol %) of the one or more SiO2 sources added to the mixture during steps (1) and (2), calculated as SiO2.
[0030] Preferably, the second portion of the one or more SiO2 sources comprises an amount, calculated as SiO2, in the range of 10 to 55 mol %, preferably in the range of 25 to 40 mol %, more preferably in the range of 32 to 35 mol %, of the total amount (100 mol %) of the one or more SiO2 sources added to the mixture during steps (1) and (2), calculated as SiO2.
[0031] Preferably, the mixture obtained in step (2) is heated in step (3) under a pressure in the range of 0.5 to 15 MPa, preferably in the range of 1 to 10 MPa, more preferably in the range of 2 to 6 MPa, more preferably in the range of 3 to 5 MPa.
[0032] Preferably, the method of the invention comprises the steps of: (4) isolating the zeolitic material obtained in step (3); (5) optionally washing the zeolite material obtained in step (3) or (4); (6) drying the zeolitic material obtained in step (3), (4) or (5); (7) Calcining the zeolite material obtained in step (3), (4), (5) or (6). The present invention further includes one or more of the following:
[0033] In step (4), separation of the zeolitic material obtained in step (3) is preferably carried out by one or more of centrifugation and filtration.
[0034] In step (5), it is preferred that the zeolitic material obtained in step (3) or (4) is washed with a polar protic solvent system, preferably water, more preferably deionized water.
[0035] Preferably, the drying in step (6) is carried out at a temperature in the range of 50 to 150°C, more preferably 70 to 130°C, more preferably 80 to 120°C, more preferably 90 to 110°C.
[0036] Preferably, the calcination in step (7) is carried out at a temperature in the range of 300 to 700°C, preferably 400 to 625°C, more preferably 500 to 600°C, more preferably 525 to 575°C, more preferably 540 to 560°C.
[0037] Preferably, the zeolitic material has a framework structure type selected from the group consisting of MFI, MEL, IMF, SVY, FER, SVR, and inter-growth structures of two or more thereof, preferably selected from the group consisting of MFI, MEL, and inter-growth structures thereof, more preferably the zeolitic material has an MFI framework structure type.
[0038] The present invention also relates to a zeolitic material obtainable and / or obtained by a method according to any one of the particular and preferred embodiments of the present invention.
[0039] The present invention also relates to a zeolitic material, preferably obtained or obtainable by a method according to any one of the specific and preferred embodiments of the present invention, wherein the framework structure of the zeolitic material comprises Si, O and a tetravalent element M other than Si, where M is selected from the group consisting of Ti, Sn, Zr, Ge and mixtures of two or more thereof, and wherein the UV-vis spectrum of the zeolitic material exhibits a first absorption band A1 having a maximum in the range of 180-230 nm, preferably in the range of 200-210 nm, and a second absorption band A2 having a maximum in the range of 290-370 nm, preferably in the range of 310-350 nm, and wherein the UV-vis spectrum is preferably determined according to Reference Example 1.8.
[0040] Preferably, the UV-vis spectrum does not exhibit any further maximum between the maximum of the first absorption band and the maximum of the second absorption band.
[0041] Preferably, the FTIR spectrum of the zeolite material has a wavelength of 3,450 to 3,550 cm -1 in the range of 3,475 to 3,525 cm -1 The first absorption band B1 has a maximum in the range of 3,700 to 3,775 cm -1 , preferably 3,725 to 3,740 cm -1 the intensity ratio B1:B2 of the first absorption band to the second absorption band is in the range of 0.70:1 to 0.90:1, preferably in the range of 0.73:1 to 0.88:1, and the FTIR spectrum is preferably determined according to Reference Example 1.7.
[0042] More preferably, the zeolitic material of the present invention has a molar ratio of Si to M in the range of 10-75, preferably in the range of 30-60, more preferably in the range of 35-55, more preferably in the range of 40-50, more preferably in the range of 43-45.
[0043] Also, preferably, the zeolite material of the present invention has a molecular weight of 350 to 510 m. 2 / g, preferably 400 to 460 m2 / g, preferably 411 to 448 m 2 / g, more preferably 419 to 440 m 2 / g, where the BET specific surface area is preferably determined according to ISO 9277:2010.
[0044] In addition, preferably, the zeolite material of the present invention has a pore size of 0.160 to 0.210 cm 3 / g, preferably 0.173 to 0.193 cm 3 / g, more preferably 0.179 to 0.187 cm 3 / g, more preferably 0.181 to 0.185 cm 3 / g, where the micropore volume is preferably determined according to ISO 15901-1:2016.
[0045] Also preferably, the zeolitic material of the present invention exhibits a total amount of acidic sites in the range of 0.020-0.070 mmol / g, preferably in the range of 0.032-0.056 mmol / g, more preferably in the range of 0.038-0.050 mmol / g, more preferably in the range of 0.042-0.046 mmol / g in a temperature programmed desorption (NH3-TPD) profile of ammonia, wherein the temperature programmed desorption (NH3-TPD) profile of ammonia is preferably determined according to Reference Example 1.5.
[0046] Also preferably, the zeolitic material of the present invention exhibits a band having a maximum in the range of 130-190°C, preferably in the range of 140-180°C, in the temperature programmed desorption (NH3-TPD) profile of ammonia.
[0047] More preferably, the zeolitic material of the present invention has a water adsorption amount in the range of 5 to 20 mass %, preferably in the range of 10 to 19 mass %, more preferably in the range of 12 to 17 mass %, more preferably in the range of 14.0 to 15.0 mass %, more preferably in the range of 14.1 to 14.5 mass %, when exposed to a relative humidity of 91%, wherein the water adsorption amount is preferably determined according to Reference Example 1.4.
[0048] More preferably, the zeolitic material of the present invention has a framework structure type selected from the group consisting of MFI, MEL, IMF, SVY, FER, SVR, and inter-growth structures of two or more thereof, preferably selected from the group consisting of MFI, MEL, and inter-growth structures thereof, more preferably the zeolitic material has an MFI framework structure type.
[0049] Preferably, M is selected from the group consisting of Ti, Sn, and mixtures of two or more thereof, preferably, M is Ti or Sn, more preferably, M is Ti.
[0050] Preferably, M is Ti and the zeolitic material has framework type MFI, more preferably the zeolitic material is a TS-1 zeolite.
[0051] The present invention also relates to a method for producing a method for manufacturing a semiconductor device comprising the steps of: (A) providing a zeolitic material according to any one of the specific and preferred embodiments of the present invention; (B) mixing the zeolitic material provided in step (A) with one or more binders; (C) optionally, kneading the mixture obtained in step (B); (D) shaping the mixture obtained in step (B) or (C) to obtain one or more shaped articles; (E) drying one or more molded articles obtained in step (D); (F) firing the dried molded product obtained in step (E); The present invention relates to a method for preparing a molded article, comprising:
[0052] Preferably, the one or more binders in step (B) are selected from the group consisting of inorganic binders, wherein the one or more binders are preferably selected from the group consisting of one or more sources of metal oxides and / or metalloid oxides, more preferably from the group consisting of silica, alumina, titania, zirconia, lanthana, magnesia, and mixtures and / or mixed oxides of two or more thereof, more preferably silica, alumina, titania, zirconia, magnesia, silica-alumina mixed oxides, silica-titania mixed oxides, silica-zirconia mixed oxides, silica-lanthana mixed oxides, silica-zirconia-lanthana mixed oxides, alumina-titania mixed oxides, alumina-zirconia mixed oxides, alumina-lanthana mixed oxides, alumina-zirconia-lanthana mixed oxides, titania-zirconia mixed oxides, and mixtures and / or mixed oxides of two or more thereof. More preferably, the one or more binders in step (B) comprise one or more sources of metal oxides and / or metalloid oxides selected from the group consisting of: silica, alumina, silica-alumina mixed oxides, and mixtures of two or more thereof; more preferably, the one or more binders in step (B) comprise one or more sources of silica; more preferably, the one or more binders in step (B) consist of one or more sources of silica, which preferably comprise one or more compounds selected from the group consisting of fumed silica, colloidal silica, silica-alumina, colloidal silica-alumina, and mixtures of two or more thereof, more preferably, one or more compounds selected from the group consisting of fumed silica, colloidal silica, and mixtures thereof; more preferably, the one or more binders in step (B) consist of colloidal silica.
[0053] Preferably, step (B) further comprises mixing the zeolitic material and one or more binders with a solvent system, wherein the solvent system comprises one or more solvents, preferably the solvent system comprises one or more hydrophilic solvents, the hydrophilic solvents being preferably selected from the group consisting of polar solvents, more preferably from the group consisting of polar protic solvents, more preferably the solvent system being selected from the group consisting of water, alcohols, carboxylic acids, and mixtures of two or more thereof, more preferably water, C1-C5 alcohols, C1-C5 carboxylic acids, and mixtures of two or more thereof, more preferably water, C1-C4 alcohols, C1-C5 carboxylic acids, and mixtures of two or more thereof. more preferably from the group consisting of water, C1-C3 alcohols, C1-C3 carboxylic acids and mixtures of two or more thereof, more preferably from the group consisting of water, methanol, ethanol, propanol, formic acid, acetic acid and mixtures of two or more thereof, more preferably from the group consisting of water, ethanol, acetic acid and mixtures of two or more thereof, more preferably the solvent system comprises water and / or ethanol, more preferably the solvent system comprises water, more preferably the solvent system consists of water.
[0054] Preferably, step (B) further comprises mixing the zeolitic material and one or more binders with one or more pore formers and / or lubricants and / or plasticizers, wherein the one or more pore formers and / or lubricants and / or plasticizers are preferably selected from the group consisting of polymers, carbohydrates, graphite, botanical additives, and mixtures of two or more thereof, more preferably selected from the group consisting of polymeric vinyl compounds, polyalkylene oxides, polyacrylates, polyolefins, polyamides, polyesters, cellulose and cellulose derivatives, sugars, Sesbania cannabina, and mixtures of two or more thereof, more preferably selected from the group consisting of polystyrene, C2-C3 polyalkylene oxides, cellulose derivatives, sugars, and mixtures of two or more thereof. More preferably, the one or more pore-forming agents and / or lubricants and / or plasticizers are selected from the group consisting of polystyrene, polyethylene oxide, C1-C2 hydroxyalkylated and / or C1-C2 alkylated cellulose derivatives, sugars, and mixtures of two or more thereof, more preferably, the one or more pore-forming agents and / or lubricants and / or plasticizers are one or more selected from the group consisting of polystyrene, polyethylene oxide, hydroxyethyl methylcellulose, and mixtures of two or more thereof, more preferably, the one or more pore-forming agents and / or lubricants and / or plasticizers are a mixture of polystyrene, polyethylene oxide, and hydroxyethyl methylcellulose.
[0055] The dried molded body obtained in step (E) is preferably fired at a temperature in the range of 350 to 850°C, preferably 400 to 700°C, more preferably 450 to 650°C, more preferably 475 to 600°C.
[0056] The present invention also relates to a moulded article obtainable or obtained by the method according to any one of the particular and preferred embodiments of the present invention.
[0057] The present invention also relates to the use of a zeolitic material according to any one of the specific and preferred embodiments of the present invention, or a shaped article according to any one of the specific and preferred embodiments of the present invention, as a catalyst, catalyst component, absorbent, adsorbent, or preferably as a catalyst and / or catalyst component for ion exchange, more preferably as a catalyst and / or catalyst component in reactions involving the formation and / or conversion of C-C bonds, preferably in isomerization reactions, ammoxidation reactions, amination reactions, hydrocracking reactions, alkylation reactions, acylation reactions, conversion of alkanes to olefins or conversion of one or more oxyacid salts to olefins. and / or as a catalyst and / or catalyst component in aromatic conversion reactions, hydrogen peroxide synthesis reactions, aldol condensation reactions, epoxide isomerization reactions, transesterification reactions or epoxidation reactions, preferably as a catalyst and / or catalyst component in olefin epoxidation reactions, more preferably epoxidation reactions of C2 to C5 alkenes, more preferably epoxidation reactions of C2 to C4 alkenes, epoxidation reactions of C2 or C3 alkenes, more preferably epoxidation reactions of C3 alkenes, more preferably as a catalyst or catalyst component for the conversion of propylene to propylene oxide.
[0058] The present invention is further described by the following series of embodiments and combinations of embodiments resulting from the indicated dependencies and back references. In particular, in each instance where a range of embodiments is mentioned, such as in the context of a term such as "the method according to any one of embodiments 1 to 4", it is to be noted that all embodiments within this range are meant to be explicitly disclosed to those skilled in the art, i.e., the wording of this term should be understood by those skilled in the art to be synonymous with "the method according to any one of embodiments 1, 2, 3, and 4". Furthermore, it is to be expressly noted that the following series of embodiments is not a set of claims determining the scope of protection, but represents a suitably constructed part of the description directed to the general and preferred aspects of the present invention.
[0059] 1. A method for producing a zeolitic material, preferably a zeolitic material according to any one of embodiments 32 to 44, wherein the framework structure of the zeolitic material comprises Si, O and a tetravalent element M other than Si, where M is selected from the group consisting of Ti, Sn, Zr, Ge and mixtures of two or more thereof, the method comprising the steps of: (1) preparing a mixture comprising one or more MO sources, one or more organic templates, a first portion of one or more SiO sources, and a protic solvent system comprising water; (2) heating the mixture obtained in step (1) at a temperature in the range of from 30° C. to the boiling point of the mixture, preferably in the range of 50° C. to 95° C., more preferably in the range of 65° C. to 90° C., more preferably in the range of 75° C. to 85° C.; (3) heating the mixture obtained in step (2) under autogenous pressure at a temperature in the range of 100 to 250°C, preferably 140 to 200°C, more preferably 155 to 185°C, more preferably 165 to 175°C; Including, The method wherein during step (2), a second portion of the one or more SiO2 sources is added to the mixture.
[0060] 2. The method of embodiment 1, wherein the heating in step (2) is carried out at atmospheric pressure.
[0061] 3. The method according to embodiment 1 or 2, wherein the heating in step (3) is carried out for a duration in the range of 0.25 to 10 days, preferably in the range of 0.5 to 5 days, more preferably in the range of 1.5 to 2.5 days, more preferably in the range of 1.75 to 2.25 days.
[0062] 4. The method according to any one of the preceding claims, wherein the one or more SiO2 sources comprise one or more alkoxysilanes, preferably one or more tetraalkoxysilanes, more preferably one or more tetraalkoxysilanes selected from the group consisting of (C1-C6) tetraalkoxysilanes and mixtures of two or more thereof, more preferably one or more tetraalkoxysilanes selected from the group consisting of (C1-C5) tetraalkoxysilanes and mixtures of two or more thereof, more preferably one or more tetraalkoxysilanes selected from the group consisting of (C1-C4) tetraalkoxysilanes and mixtures of two or more thereof, more preferably one or more tetraalkoxysilanes selected from the group consisting of (C1-C3) tetraalkoxysilanes and mixtures of two or more thereof, more preferably one or more of tetramethoxysilane and tetraethoxysilane, more preferably the one or more Si sources comprise tetraethoxysilane, and the heating of the mixture in step (2) comprises hydrolysis of at least a portion of the one or more alkoxysilanes and distillation of the resulting one or more alcohols from the mixture.
[0063] 5. The method of any one of the preceding claims, wherein M is selected from the group consisting of Ti, Sn, and mixtures thereof, preferably M comprises Ti, and more preferably M is Ti.
[0064] 6. In step (1), the one or more organic templates are each a tetraalkylammonium cation R 1 R 2 R 3 R 4 N + R 1 , R 2 , R 3 and R 4 The method of any one of the preceding embodiments, wherein, independently of each other, represent alkyl.
[0065] 7. The one or more tetraalkylammonium cations R 1 R 2 R3 R 4 N + R of the containing compound 1 , R 2 , R 3 and R 4 are each independently an optionally branched (C1-C6) alkyl, preferably a (C1-C5) alkyl, more preferably a (C2-C4) alkyl, more preferably an optionally branched (C2-C3) alkyl, and more preferably R 1 , R 2 , R 3 and R 4 are each independently ethyl or propyl, more preferably said one or more tetraalkylammonium cations R 1 R 2 R 3 R 4 N + R of the containing compound 1 , R 2 , R 3 and R 4 The method according to embodiment 6, wherein, independently of each other, represent propyl, preferably n-propyl.
[0066] 8. Independently of each other, said one or more tetraalkylammonium cations R 1 R 2 R 3 R 4 N + The containing compound is preferably one or more salts selected from the group consisting of salts, preferably halides, preferably chlorides and / or bromides, more preferably chlorides, hydroxides, sulfates, nitrates, phosphates, acetates, and mixtures of two or more thereof, more preferably chlorides, hydroxides, sulfates, and mixtures of two or more thereof, and more preferably one or more tetraalkylammonium cations R 1 R 2 R 3 R 4 N + The method of any one of embodiments 5 to 6, wherein the containing compound is a tetraalkylammonium hydroxide and / or chloride, more preferably a tetraalkylammonium hydroxide.
[0067] 9. M comprises Ti, preferably Ti, and one or more TiO2 sources are selected from the group consisting of oxides and salts of Ti, and mixtures thereof, said one or more TiO2 sources are preferably one or more compounds selected from the group consisting of titanium oxides, titanium salts, titanyl compounds, titanic acids, titanic acid esters, and mixtures of two or more thereof, more preferably tetrabutyl orthotitanate, tetraisopropyl orthotitanate, tetraethyl orthotitanate, titanium dioxide, titanium tetrachloride, titanium tert-butoxide, TiOSO4 and / or KTiOPO4, and mixtures thereof. The method of any one of the preceding claims, wherein the one or more TiO2 sources comprise one or more compounds selected from the group consisting of mixtures of two or more thereof, more preferably from the group consisting of tetrabutyl orthotitanate, tetraisopropyl orthotitanate, tetraethyl orthotitanate, tetramethyl orthotitanate, titanium dioxide, titanium tetrachloride, titanium tert-butoxide, and mixtures of two or more thereof, more preferably the one or more TiO2 sources comprise titanium tert-butoxide, and more preferably titanium tert-butoxide is used as the one or more TiO2 sources.
[0068] 10. The mixture obtained in step (2) is a mixture of the one or more SiO2 sources, calculated as SiO2, and the one or more tetraalkylammonium cations R 1 R 2 R 3 R 4 N + 10. The method of any one of the preceding claims, having a molar ratio with the containing compound.
[0069] 11. The method according to any one of the preceding claims, wherein the mixture obtained in step (2) has a molar ratio of the one or more SiO2 sources, calculated as SiO2, to water in the range of 1:30 to 1:5, preferably in the range of 1:20 to 1:12, more preferably in the range of 1:17 to 1:15.
[0070] 12. The method according to any one of the preceding claims, wherein the mixture obtained in step (2) has a molar ratio of the one or more SiO2 sources, calculated as SiO2, to the one or more MO2 sources, calculated as MO2, in the range of 1:0.0100 to 1:0.0010, preferably in the range of 1:0.0040 to 1:0.0020, and more preferably in the range of 1:0.0035 to 1:0.0031.
[0071] 13. The method of any one of the preceding claims, wherein during step (2), the second portion of the one or more SiO2 sources is added continuously or incrementally, preferably incrementally.
[0072] 14. The method of embodiment 13, wherein during the course of step (2), the second portion of the one or more SiO2 sources is added incrementally in 1 to 20 steps, preferably 1 to 10 steps, more preferably 1 to 5 steps, more preferably 1 step.
[0073] 15. The method according to any one of the preceding embodiments, wherein the heating in step (2) is carried out continuously or intermittently, preferably intermittently.
[0074] 16. The method of embodiment 15, wherein the heating in step (2) is performed intermittently, the heating consisting of two or more heating stages, and the second portion of the one or more SiO2 sources is added during one or more intervals between two or more heating stages, preferably, the heating in step (2) consisting of two heating stages, and the second portion of the one or more SiO2 sources is added during an interval between two heating stages.
[0075] 17. The method of embodiment 16, wherein the heating in step (2) consists of three or more heating stages, and the second portion of the one or more SiO2 sources is added in equal portions during respective intervals between three or more heating stages, each portion corresponding to a proportion of 1 / n of the total amount of the second portion, n representing the number of intervals during which each portion is added respectively, n+1 corresponding to the number of heating stages, n being an integer comprised between 2 and 5, and n being preferably 2 or 3, more preferably 2.
[0076] 18. The method according to embodiment 16 or 17, wherein during each interval during which the second portion or portions of the second portion of the one or more SiO2 sources are added, the mixture has a temperature comprised between 15 and 65 °C, preferably between 20 and 60 °C, more preferably between 35 and 55 °C, more preferably between 48 and 52 °C.
[0077] 19. The method according to any one of embodiments 16 to 18, wherein each heating stage independent of one another is carried out for a duration comprised in the range of 0.1 to 5 hours, preferably in the range of 0.5 to 3.5 hours, more preferably in the range of 1.75 to 2.25 hours.
[0078] 20. The method according to any one of embodiments 16 to 19, wherein the heating consists of 2 to 6 heating stages, preferably 2 to 4 heating stages, more preferably 2 or 3 heating stages, more preferably the heating consists of 2 heating stages.
[0079] 21. The method of any one of the preceding claims, wherein the first portion of the one or more SiO2 sources comprises an amount, calculated as SiO2, in the range of 45 to 90 mol %, preferably in the range of 60 to 75 mol %, and more preferably in the range of 65 to 68 mol %, of the total amount (100 mol %) of the one or more SiO2 sources added to the mixture during steps (1) and (2).
[0080] 22. The method of any one of the preceding claims, wherein the second portion of the one or more SiO2 sources comprises an amount, calculated as SiO2, in the range of 10 to 55 mol %, preferably in the range of 25 to 40 mol %, more preferably in the range of 32 to 35 mol %, of the total amount (100 mol %) of the one or more SiO2 sources added to the mixture during steps (1) and (2).
[0081] 23. The method according to any one of the preceding embodiments, wherein the mixture obtained in step (2) is heated in step (3) under a pressure in the range of 0.5 to 15 MPa, preferably in the range of 1 to 10 MPa, more preferably in the range of 2 to 6 MPa, more preferably in the range of 3 to 5 MPa.
[0082] 24. (4) isolating the zeolite material obtained in step (3); (5) optionally washing the zeolite material obtained in step (3) or (4); (6) drying the zeolitic material obtained in step (3), (4) or (5); (7) Calcining the zeolite material obtained in step (3), (4), (5) or (6). 24. The method of any one of the preceding claims, further comprising one or more of:
[0083] 25. The method of embodiment 24, wherein in step (4), the separation of the zeolitic material obtained in step (3) is carried out by one or more of centrifugation and filtration.
[0084] 26. The method of embodiment 24 or 25, wherein in step (5), the zeolitic material obtained in step (3) or (4) is washed with a polar protic solvent system, preferably water, more preferably deionized water.
[0085] 27. The method according to any one of embodiments 24 to 26, wherein the drying in step (6) is carried out at a temperature in the range of 50 to 150°C, more preferably 70 to 130°C, more preferably 80 to 120°C, more preferably 90 to 110°C.
[0086] 28. The method according to any one of embodiments 24 to 27, wherein the calcination in step (7) is carried out at a temperature in the range of 300 to 700°C, preferably 400 to 625°C, more preferably 500 to 600°C, more preferably 525 to 575°C, more preferably 540 to 560°C.
[0087] 29. The method according to any one of the preceding claims, wherein the zeolitic material has a framework structure type selected from the group consisting of MFI, MEL, IMF, SVY, FER, SVR, and inter-growth structures of two or more thereof, preferably selected from the group consisting of MFI, MEL, and inter-growth structures thereof, more preferably the zeolitic material has an MFI framework structure type.
[0088] 30. A zeolitic material obtainable and / or obtained by the method according to any one of embodiments 1 to 29.
[0089] 31. A zeolitic material preferably obtainable and / or obtainable by the method according to any one of embodiments 1 to 29, wherein the framework structure of the zeolitic material comprises Si, O and a tetravalent element M other than Si, where M is selected from the group consisting of Ti, Sn, Zr, Ge and mixtures of two or more thereof, and the UV-vis spectrum of the zeolitic material exhibits a first absorption band A1 having a maximum in the range of 180 to 230 nm, preferably in the range of 200 to 210 nm, and a second absorption band A2 having a maximum in the range of 290 to 370 nm, preferably in the range of 310 to 350 nm, and wherein the UV-vis spectrum is preferably determined according to Reference Example 1.8.
[0090] 32. The zeolitic material of embodiment 31, wherein the UV-vis spectrum does not exhibit any further maximum between the maximum of the first absorption band and the maximum of the second absorption band.
[0091] 33. The FTIR spectrum of the zeolite material is 3,450 to 3,550 cm -1in the range of 3,475 to 3,525 cm -1 The first absorption band B1 has a maximum in the range of 3,700 to 3,775 cm -1 , preferably 3,725 to 3,740 cm -1 and the intensity ratio B1:B2 of the first absorption band to the second absorption band is comprised in the range of 0.70:1 to 0.90:1, preferably in the range of 0.73:1 to 0.88:1, and the FTIR spectrum is preferably determined according to Reference Example 1.7.
[0092] 34. The zeolitic material according to any one of embodiments 31 to 33, having a molar ratio of Si to M in the range of 10 to 75, preferably in the range of 30 to 60, more preferably in the range of 35 to 55, more preferably in the range of 40 to 50, more preferably in the range of 43 to 45.
[0093] 35.350~510m 2 / g, preferably 400 to 460 m 2 / g, preferably 411 to 448 m 2 / g, more preferably 419 to 440 m 2 35. The zeolitic material according to any one of embodiments 31 to 34, having a BET specific surface area in the range of 0.1 g / g, the BET specific surface area preferably being determined according to ISO 9277:2010.
[0094] 36.0.160~0.210cm 3 / g, preferably 0.173 to 0.193 cm 3 / g, more preferably 0.179 to 0.187 cm 3 / g, more preferably 0.181 to 0.185 cm 3 36. The zeolitic material according to any one of embodiments 31 to 35, having a micropore volume in the range of 0.1 to 0.1 g / g, the micropore volume preferably being determined according to ISO 15901-1:2016.
[0095] 37. The zeolitic material according to any one of embodiments 31 to 36, wherein the ammonia temperature programmed desorption (NH3-TPD) profile exhibits a total amount of acidic sites in the range of 0.020 to 0.070 mmol / g, preferably in the range of 0.032 to 0.056 mmol / g, more preferably in the range of 0.038 to 0.050 mmol / g, more preferably in the range of 0.042 to 0.046 mmol / g, and wherein the ammonia temperature programmed desorption (NH3-TPD) profile is preferably determined according to Reference Example 1.5.
[0096] 38. The zeolitic material according to any one of embodiments 31 to 37, which exhibits a band in the ammonia temperature programmed desorption (NH3-TPD) profile with a maximum in the range of 130 to 190 °C, preferably in the range of 140 to 180 °C.
[0097] 39. The zeolitic material according to any one of embodiments 31 to 38, having a water adsorption amount in the range of 5 to 20% by mass, preferably in the range of 10 to 19% by mass, more preferably in the range of 12 to 17% by mass, more preferably in the range of 14.0 to 15.0% by mass, more preferably in the range of 14.1 to 14.5% by mass, when exposed to a relative humidity of 39.91%, wherein the water adsorption amount is preferably determined according to Reference Example 1.4.
[0098] 40. The zeolitic material according to any one of embodiments 31 to 39, having a framework structure type selected from the group consisting of MFI, MEL, IMF, SVY, FER, SVR, and intergrowth structures of two or more thereof, preferably selected from the group consisting of MFI, MEL, and intergrowth structures thereof, more preferably the zeolitic material has an MFI framework structure type.
[0099] 41. The zeolitic material according to any one of embodiments 31 to 40, wherein M is selected from the group consisting of Ti, Sn, and mixtures of two or more thereof, preferably M is Ti or Sn, more preferably M is Ti.
[0100] 42. The zeolitic material according to any one of embodiments 31 to 41, wherein M is Ti and the zeolitic material has framework structure type MFI, more preferably the zeolitic material is a TS-1 zeolite.
[0101] 43. (A) providing a zeolitic material according to any one of embodiments 30 to 42; (B) mixing the zeolitic material provided in step (A) with one or more binders; (C) optionally, kneading the mixture obtained in step (B); (D) shaping the mixture obtained in step (B) or (C) to obtain one or more shaped articles; (E) drying one or more molded articles obtained in step (D); (F) firing the dried molded product obtained in step (E); A method for preparing a molded article comprising:
[0102] 44. The one or more binders in step (B) are selected from the group consisting of inorganic binders, and the one or more binders are preferably one or more sources of metal oxides and / or metalloid oxides, more preferably from the group consisting of silica, alumina, titania, zirconia, lanthana, magnesia, and mixtures and / or mixed oxides of two or more thereof, more preferably from the group consisting of silica, alumina, titania, zirconia, magnesia, silica-alumina mixed oxide, silica-titania mixed oxide, silica-zirconia mixed oxide, silica-lanthana mixed oxide, silica-zirconia-lanthana mixed oxide, alumina-titania mixed oxide, alumina-zirconia mixed oxide, alumina-lanthana mixed oxide, alumina-zirconia-lanthana mixed oxide, titania-zirconia mixed oxide, and mixtures and / or mixed oxides of two or more thereof, The method according to embodiment 43, wherein the binder in step (B) comprises one or more sources of metal oxides and / or metalloid oxides, preferably selected from the group consisting of silica, alumina, silica-alumina mixed oxides, and mixtures of two or more thereof, more preferably the one or more binders in step (B) comprise one or more sources of silica, more preferably the one or more binders in step (B) consist of one or more sources of silica, the one or more sources of silica preferably comprise one or more compounds selected from the group consisting of fumed silica, colloidal silica, silica-alumina, colloidal silica-alumina, and mixtures of two or more thereof, more preferably the one or more compounds selected from the group consisting of fumed silica, colloidal silica, and mixtures thereof, more preferably the one or more binders in step (B) consist of colloidal silica.
[0103] 45. Step (B) further comprises mixing the zeolite material and the one or more binders with a solvent system, wherein the solvent system comprises one or more solvents, preferably the solvent system comprises one or more hydrophilic solvents, wherein the hydrophilic solvent is preferably selected from the group consisting of polar solvents, more preferably from the group consisting of polar protic solvents, more preferably from the group consisting of water, alcohols, carboxylic acids, and mixtures of two or more thereof, more preferably from the group consisting of water, C1-C5 alcohols, C1-C5 carboxylic acids, and mixtures of two or more thereof, more preferably water, C1-C4 alcohols, C1-C4 carboxylic acids, more preferably from the group consisting of ... The method according to embodiment 43 or 44, wherein the solvent system comprises one or more polar protic solvents selected from the group consisting of carboxylic acids and mixtures of two or more thereof, more preferably from the group consisting of water, C1-C3 alcohols, C1-C3 carboxylic acids and mixtures of two or more thereof, more preferably from the group consisting of water, methanol, ethanol, propanol, formic acid, acetic acid, and mixtures of two or more thereof, more preferably from the group consisting of water, ethanol, acetic acid, and mixtures of two or more thereof, more preferably said solvent system comprises water and / or ethanol, more preferably said solvent system comprises water, more preferably said solvent system consists of water.
[0104] 46. Step (B) further comprises mixing the zeolite material and the one or more binders with one or more pore formers and / or lubricants and / or plasticizers, the one or more pore formers and / or lubricants and / or plasticizers being preferably selected from the group consisting of polymers, carbohydrates, graphite, botanical additives, and mixtures of two or more thereof, more preferably selected from the group consisting of polymeric vinyl compounds, polyalkylene oxides, polyacrylates, polyolefins, polyamides, polyesters, cellulose and cellulose derivatives, sugars, sesbania cannabina, and mixtures of two or more thereof, more preferably selected from the group consisting of polystyrene, C2-C3 polyalkylene oxides, cellulose derivatives, sugars, and mixtures of two or more thereof, more preferably polystyrene, polyethylene 46. The method according to any one of embodiments 43 to 45, wherein the one or more pore formers and / or lubricants and / or plasticizers are selected from the group consisting of polystyrene, polyethylene oxide, hydroxyethyl methylcellulose, and mixtures of two or more thereof, more preferably from the group consisting of polystyrene, polyethylene oxide, hydroxyethyl methylcellulose, and mixtures of two or more thereof, more preferably the one or more pore formers and / or lubricants and / or plasticizers consist of one or more selected from the group consisting of polystyrene, polyethylene oxide, hydroxyethyl methylcellulose, and mixtures of two or more thereof, more preferably the one or more pore formers and / or lubricants and / or plasticizers consist of a mixture of polystyrene, polyethylene oxide, and hydroxyethyl methylcellulose.
[0105] 47. The method according to any one of embodiments 43 to 46, wherein the dried molded body obtained in step (E) is fired at a temperature in the range of 350 to 850°C, preferably 400 to 700°C, more preferably 450 to 650°C, more preferably 475 to 600°C.
[0106] 48. A shaped article obtainable or obtained by the method according to any one of embodiments 43 to 47.
[0107] 49. The zeolitic material according to any one of embodiments 30 to 42 or the shaped article according to embodiment 48 is used as a catalyst, catalyst component, absorbent, adsorbent or as a catalyst and / or catalyst component for ion exchange, more preferably as a catalyst and / or catalyst component in reactions involving the formation and / or conversion of C-C bonds, preferably in isomerization reactions, ammoxidation reactions, amination reactions, hydrocracking reactions, alkylation reactions, acylation reactions, conversion of alkanes to olefins or conversion of one or more oxyacid salts to olefins and / or aromatics. , as a catalyst and / or catalyst component in a hydrogen peroxide synthesis reaction, an aldol condensation reaction, an epoxide isomerization reaction, a transesterification reaction or an epoxidation reaction, preferably as a catalyst and / or catalyst component in an epoxidation reaction of an olefin, more preferably an epoxidation reaction of a C2 to C5 alkene, more preferably an epoxidation reaction of a C2 to C4 alkene, an epoxidation reaction of a C2 or C3 alkene, more preferably an epoxidation reaction of a C3 alkene, more preferably as a catalyst or catalyst component for the conversion of propylene to propylene oxide.
[0108] The present invention will be further illustrated by the following examples, comparative examples and reference examples. EXAMPLES
[0109] Reference example 1: Measurement method Reference Example 1.1: Determination of XRD diffraction spectrum Powder X-ray diffraction (XRD) was performed on a Rint-Ultima III (Rigaku) instrument using Cu Kalpha radiation (Lambda = 1.5406 Å, 40 kV, 40 mA).
[0110] Reference Example 1.2: Inductively Coupled Plasma Mass Spectroscopy (ICP-MS) Determination Elemental analysis was performed using an inductively coupled plasma atomic emission spectrometer (ICP-AES, Shimadzu ICPE-9000). Samples were dissolved in dilute HF solution.
[0111] Reference Example 1.3: Determination of N2 adsorption / desorption measurements Nitrogen adsorption and desorption measurements were performed using a BEL-mini analyzer (BEL Japan). Prior to the measurements, all samples were degassed at 350°C for 2 h.
[0112] Reference Example 1.4: Determination of water adsorption The determination of water absorption properties of the examples in the experimental section was carried out at 25° C. using a BEL-mini analyzer (BEL Japan). Before the start of the measurements, the samples were degassed at 350° C. for 2 h to remove residual moisture. The water adsorption of the samples was measured after exposing them to a relative humidity of 91%.
[0113] Reference Example 1.5: Measurement of temperature programmed desorption of ammonia (NH3-TPD) Temperature programmed desorption (NH3-TPD) profiles of ammonia were recorded using approximately 30 mg of sample on a Multitrack TPD instrument (Japan BEL).
[0114] Reference Example 1.6: Determination of NMR spectrum High resolution with JEOL ECA-600 spectrometer 29 Si MAS NMR spectra were obtained.
[0115] Reference Example 1.7: Determination of IR spectrum FTIR spectra were collected on a JASCO FT-IR 4100 spectrometer. Typically, samples in H-form were pressed into free-standing wafers (20 mm diameter, 30 ± 2 mg), placed in an IR cell, and preconditioned by evacuating at 723 K for 1 h. The temperature was then reduced to 423 K and the spectra were recorded.
[0116] Reference Example 1.8: Determination of UV-vis spectrum UV-visible diffuse reflectance spectra were recorded on a V-650DS spectrometer (JASCO) using BaSO4 as a reference.
[0117] Reference Example 1.9: Scanning Electron Microscope (SEM) Field emission scanning electron microscopy (FE-SEM) was performed on a Hitachi S-5200 microscope.
[0118] Example 1: Preparation of the zeolitic material according to the present invention Tetraethyl orthosilicate (TEOS, Wako, 97%) and titanium tetra-n-butoxide (TBOT, Wako, at least 95.0%) were used as the Si and Ti sources, respectively. Tetrapropylammonium hydroxide (TPAOH, TCI, 40% in water) was used as the organic structure directing agent (OSDA), and deionized water (Wako, 20 L) was used.
[0119] In a typical synthesis, 0.119 g of TBOT was mixed with 1.43 g of TEOS (2 / 3 of the total amount), and the mixture was added to 0.61 g of an aqueous solution containing 40 wt% TPAOH and 2.87 g of H2O. The resulting gel mixture had the following molar ratio of 1 Si: 0.0033 Ti: 0.12 TPAOH: 16 H2O. The gel mixture was then placed in an oven and stirred at 50°C for 30 minutes, and then stirred at 80°C for 2 hours to hydrolyze TEOS and TBOT and remove the generated alcohol. After this hydrolysis process, 0.72 g of TEOS (1 / 3 of the total amount) was added to the gel mixture, and the above hydrolysis process was repeated again. That is, the gel mixture was placed in an oven and stirred at 50°C for 30 minutes, and then stirred at 80°C for 2 hours. The resulting product was collected, washed with distilled water, and dried at 100°C overnight. The sample thus prepared was calcined in air at 550°C for 6 hours to remove the OSDA. The water adsorption amount of the obtained zeolite material was 14.3% by mass. Further, the properties of the obtained zeolite material are shown in Table 1 of Reference Example 2 below.
[0120] Comparative Example 1: Preparation of Zeolitic Material Not According to the Invention For the gel preparation, 500 g of tetraethyl orthosilicate (TEOS) and 15 g of tetraethyl orthotitanate (TEOTi; Merck) were charged into a beaker. Then, 300 g of deionized water and 220 g of an aqueous solution of tetrapropylammonium hydroxide (TPAOH; 40% by weight in water) were added under stirring (200 rpm). The resulting mixture had a pH of 13.5. The mixture was hydrolyzed at room temperature for 60 minutes, during which the temperature was increased to 60° C. The mixture had a pH of 12.6. Then, the ethanol was distilled off until the sample was at 95° C. The distillation yielded 540 g of distillate.
[0121] The synthesis gel was then cooled to 40° C. under stirring, and 542 g of deionized water was added to it. The pH of the resulting mixture was 11.9.
[0122] The synthesis gel was then transferred to an autoclave. The synthesis gel was heated in the autoclave with stirring to a temperature of 175 ° C and stirred at said temperature under autogenous pressure for 16 hours. The pressure ranged from 8.4 to 10.9 bar (abs). The suspension obtained was then worked up. For this purpose, the suspension obtained was diluted with deionized water, where the mass ratio of suspension to deionized water was 1:1. Then, about 164 g of nitric acid (10% by mass in water) was added and the pH of the mixture obtained was 7.35. The solid obtained was filtered off and washed four times with deionized water (1000 ml of deionized water was used each time). The solid was then dried in an oven in air at 120 ° C for 16 hours and calcined in air at 490 ° C for 5 hours.
[0123] The TS-1 material thus obtained had a Si content of 43 wt%, a Ti content of 2 wt%, and a total carbon loss of less than 0.1 wt%. The water adsorption was 15.3 wt%. The crystallinity by X-ray diffraction was 88%.
[0124] Reference Example 2: Characteristics of the zeolite materials according to Example 1 and Comparative Example 1
[0125] [Table 1]
[0126] Example 3: Catalytic testing - propylene epoxidation The epoxidation of propylene was carried out in an autoclave reactor with a 100 mL Teflon inner liner. The autoclave reactor was equipped with a water cooling system, a stirring blade, and a 0.5-3 MPa pressure gauge. Typically, 100 mg of catalyst, 8.1 mL of methanol, and 30 mmol of H2O2 (35 wt%, containing 1.9 mL of H2O) were added to the reactor. The autoclave was then filled with propylene at 0.2 MPa three times to replace the air inside. During the reaction, the propylene pressure in the autoclave was maintained at 0.4 MPa. The reaction mixture was stirred at 120 rpm and heated to 333 K at 8 °C / min. After 1 h at 333 K, the stirring and heating of the autoclave were stopped, the Teflon inner liner was removed, and it was rapidly cooled to room temperature in an ice bath.
[0127] The resulting liquid product was then separated from the solids by injection filtration and determined by a gas chromatograph (Shimadzu GC-14B) equipped with a DB-WAX column (60 m, 0.25 mm diameter, 0.25 μm film) and an FID detector using DMF as an internal standard. The amount of unconverted H2O2 was determined by standard titration with 0.1 M Ce(SO4)2 solution.
[0128] The results of the catalytic tests on the zeolitic materials of Example 1 and Comparative Example 1 are shown in Table 2 below.
[0129] [Table 2]
[0130] The following formula was used to calculate each data:
[0131]
number
[0132] (In the formula,
number
number
[0133] As can be seen from the results, the zeolite material according to Example 1 achieved a relatively high yield of propylene oxide (PO) and also achieved a high conversion rate of H2O2. In particular, the zeolite material of Example 1 showed an excellent yield of propylene oxide.
[0134] Cited prior art: - WO 2011 / 064191 A1 - WO 2021 / 123227 A1 - WO 2020 / 221683 A1 - WO 2020 / 074586 A1 - Xiujuan Deng et al., "Low-cost synthesis of titanium silicalite-1 (TS-1) with high catalytic oxidation performance via a controlled hydrolysis process", INDUSTRIAL & ENGINEERING CHEMISTRY RESEARCH, Vol. 52, no. 3, January 23, 2013 (2013-01-23), pp. 1190-1196 - Zhang Jian Hui et al., "Synthesis of nano-sized TS-1 zeolite by solid-state conversion method with unprecedentedly low usage of tetrapropylammonium hydroxide," MICROPOROUS AND MESOPOROUS MATERIALS, Vol. 217, pp. 96-101
Claims
1. A method for producing a zeolitic material, the framework structure of the zeolitic material comprising Si, O, and a tetravalent element M other than Si, where M is selected from the group consisting of Ti, Sn, Zr, Ge, and mixtures of two or more thereof, the method comprising the steps of: (1) One or more MOs 2 A source, one or more organic templates, one or more SiO 2 preparing a mixture comprising a first portion of the source and a protic solvent system comprising water; (2) heating the mixture obtained in step (1) at a temperature ranging from 30° C. to the boiling point of the mixture; (3) heating the mixture obtained in step (2) at a temperature comprised between 100 and 250° C. under autogenous pressure; Including, During the process of step (2), one or more SiO 2 A method wherein a second portion of the source is added to the mixture.
2. The method of claim 1 , wherein M is selected from the group consisting of Ti, Sn, and mixtures thereof.
3. The method according to claim 1 or 2, wherein the heating in step (2) is carried out continuously or intermittently.
4. The heating in step (2) is performed intermittently, the heating comprises two or more heating stages, and the one or more SiO 2 The method of claim 3 , wherein the second portion of the source is added during one or more intervals between two or more heating stages.
5. The method of claim 3, wherein the heating comprises 2 to 6 heating stages.
6. The one or more SiO 2 The first portion of the source is made of SiO 2 The one or more SiO 2 The method according to claim 1 or 2, wherein the amount of the source is in the range of 45 to 90 mol % of the total amount of sources (100 mol %).
7. The one or more SiO 2 The second portion of the source is SiO 2 The one or more SiO 2 The method according to claim 1 or 2, wherein the amount of the source is in the range of 10 to 55 mol % of the total amount of sources (100 mol %).
8. (4) isolating the zeolitic material obtained in step (3); (5) optionally washing the zeolite material obtained in step (3) or (4); (6) drying the zeolitic material obtained in step (3), (4) or (5); (7) Calcining the zeolite material obtained in step (3), (4), (5) or (6). The method of claim 1 or 2, further comprising one or more of:
9. 2. A zeolitic material obtainable and / or obtained by the method of claim 1.
10. A zeolite material, wherein a framework structure of the zeolite material comprises Si, O, and a tetravalent element M other than Si, where M is selected from the group consisting of Ti, Sn, Zr, Ge, and mixtures of two or more thereof, and a UV-vis spectrum of the zeolite material exhibits a first absorption band A1 having a maximum in the range of 180 to 230 nm, and a second absorption band A2 having a maximum in the range of 290 to 370 nm.
11. 11. The zeolitic material according to claim 10, wherein said UV-vis spectrum does not exhibit any further maximum between the maximum of said first absorption band and the maximum of said second absorption band.
12. The FTIR spectrum of the zeolite material is 3,450 to 3,550 cm -1 A first absorption band B1 having a maximum in the range of 3,700 to 3,775 cm -1 and wherein the intensity ratio B1:B2 of the first absorption band to the second absorption band is in the range of 0.70:1 to 0.90:
1.
13. (A) providing a zeolitic material according to claim 9; (B) mixing the zeolitic material provided in step (A) with one or more binders; (C) optionally, kneading the mixture obtained in step (B); (D) molding the mixture obtained in step (B) or (C) to obtain one or more molded articles; (E) drying the one or more molded articles obtained in step (D); (F) firing the dried molded product obtained in step (E); A method for preparing a molded article comprising:
14. A moulded article obtainable or obtained by the method according to claim 13.
15. 16. Use of the zeolitic material according to claim 9 or 10 or the shaped article according to claim 14 as a catalyst, catalyst component, absorbent, adsorbent or for ion exchange.
Citation Information
Patent Citations
Process for the preparation of a titanium zeolite catalyst
WO2011064191A1
A molding comprising a zeolitic material having framework type mfi
WO2020074586A1
Molding comprising a type MFI zeolitic titanosilicate and a silica binder, its preparation process and use as catalyst
WO2020221683A1
Continuous synthesis of a titanosilicate zeolitic material, said zeolitic material, molding prepared thereof, and their use