Vinyl chloride copolymers and copolymer compositions, and articles containing same - Patents.com
A copolymer composition of vinyl chloride, maleic acid, and acrylic acid units with additives addresses PVC's limitations, enhancing properties for diverse applications by improving elasticity, heat resistance, and reducing plasticizer migration.
Patent Information
- Application Number
- JP2024555271
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2021-11-16
- Filing Date
- 2022-11-09
- Publication Date
- 2024-11-19
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Polyvinyl chloride (PVC) exhibits limitations such as low heat resistance, brittleness, and low elasticity, making it difficult to shape into specific articles without additives, which can lead to issues like fish eyes and reduced properties when plasticizers are used, and complicates high-temperature applications.
A copolymer composition comprising 90-99% vinyl chloride polymer units, 0.5-10% maleic acid polymer units, and optionally 0-5% acrylic acid polymer units, with additives like stabilizers, impact modifiers, and plasticizers, to enhance properties like elasticity, heat resistance, and moldability.
The copolymer composition achieves improved hardness, elasticity, and low temperature adhesion, reduces plasticizer migration, and allows for easier molding with lower energy consumption, while maintaining appearance and performance in various applications.
Smart Images

Figure 2024543241000001 
Figure 2024543241000002 
Figure 2024543241000003
Abstract
Description
[Technical field]
[0001] Chemistry relating to copolymers and copolymer compositions, and articles containing same. [Background technology]
[0002] Vinyl chloride polymer, also known as polyvinyl chloride or PVC, is a thermoplastic material with favorable properties such as excellent chemical resistance, water resistance, and good electrical insulation. It is therefore commonly used in the manufacture of articles in various industries, such as water pipes, cling films, food packaging films, stickers, wire insulation, cables, etc. However, PVC has certain disadvantages such as low heat resistance, brittleness, and low elasticity. Therefore, it cannot be molded as needed to become a specific type of article. Therefore, in order to mold PVC into an article with some specific properties, it is necessary to mix PVC with other ingredients, such as additives or other types of polymers, as necessary to suit the application of the final product, to improve the properties of the polymer or polymer composition to be molded, such as heat resistance, low temperature resistance, flexibility, strength, elasticity, etc.
[0003] A common problem when PVC is mixed with other components is the incompatibility of the PVC with other components, namely plasticizers and additives. This can cause migration or transfer of additives from the contents of the article, or cause an uneven surface of the article with fish eyes. For example, if it is necessary to improve the flexibility of a polymer and give the article a smooth surface, this can be achieved by adding plasticizers and additives. It takes time for the plasticizer to be absorbed into the pores of the PVC, and therefore it consumes a lot of energy to absorb the plasticizer. As a result, the heat resistance of the article after molding is reduced. Furthermore, if the particle size of the PVC is larger than 500 μm, there is a high possibility of fish eyes being found on the surface of the article, and if the article is used for a long time, the plasticizer absorbed in such pores will migrate from the surface of the article, reducing the flexibility of the article. Furthermore, in certain applications where specific properties such as good oil resistance are required, adding a large amount of plasticizer to achieve the required flexibility will reduce the oil resistance of the article, and the properties of the article will not meet the requirements or specified standards. On the other hand, reducing the amount of plasticizer may adversely affect certain physical properties of the article or may damage the embedded chip due to the high heat during manufacturing in applications where the product's melting properties need to be improved, such as molding into credit cards with high temperature lamination above 120° C. Therefore, for this type of application, the polymer properties are usually improved by blending PVC with another polymer, such as vinyl chloride-vinyl acetate copolymer, to allow lamination at temperatures below 120° C., which complicates the preparation procedure.
[0004] Therefore, in addition to attempts to invent and develop methods to solve the above problems, there are also attempts to improve the properties of PVC resin to make it suitable for use. Examples of patent documents that disclose methods to improve the properties of PVC copolymer resins are as follows:
[0005] WO 2019 / 066496 discloses a vinyl chloride-based resin composition comprising a copolymer of monomers that are vinyl chloride monomer in the range of 10 to 90 parts by weight, ethylenically unsaturated monomer in the range of 0.1 to 50 parts by weight, (meth)acrylic acid ester monomer having a linear, branched, or cyclic alkyl group having 10 to 20 carbon atoms in the range of 1.0 part by weight or more, and hydroxyl monomer in the range of 1 to 30 parts by weight.
[0006] EP 2067795 discloses a method for preparing a copolymerized or grafted polyvinyl halide resin, which comprises (A) 90.0% to 99.9% by weight of a composite composition consisting of a vinyl halide monomer or a mixture of polymerizable monomers based on a vinyl halide monomer, and (B) 10.0% to 0.1% by weight of an alkyl acrylate monomer or latex or an alkyl acrylate / acrylic acid-based polymer powder.
[0007] China Patent No. 104250334 discloses a method for preparing vinyl chloride-acrylic acid copolymers, comprising reacting vinyl chloride monomer in an amount ranging from 90 to 99.5% by weight with acrylic acid monomer in an amount ranging from 0.5 to 10% by weight.
[0008] However, despite the research and development of various approaches to improving the properties of polyvinyl chloride, specifically, to improve the properties of polymers using copolymerization of vinyl chloride monomer with other comonomers, as disclosed in the prior art examples above, there remains a need to develop or improve the properties of polyvinyl chloride, as well as its copolymers, to meet the needs for using such polymers in various applications. Summary of the Invention [Problem to be solved by the invention]
[0009] The object of the present invention is to provide copolymers of polyvinyl chloride (PVC) whose specific properties, in particular elasticity, heat resistance, low temperature resistance, strength, oil resistance, ability to be molded at high and low temperatures as required, are improved to make them suitable for various applications as required.
[0010] Another object of the present invention is to provide copolymer compositions and articles made from or consisting of the copolymers according to the present invention having properties suitable for various applications, including rigid applications such as drinking water pipes, doors, windows, moldings, panel moldings, electrical conduits, hallway floors, cable trays, and rigid foam boards, semi-rigid applications such as films, sheets, blister packs, stickers, credit cards, semi-rigid plastic sheets, shrink sleeves, and cling films, flexible applications such as flexible plastic sheets, cables, indoor electrical wires, outdoor electrical wires, automotive electrical wires, rubber tiles, refrigerator seals, mirror edge seals, electrical tapes, artificial leather, and flexible plastic sheets, or adhesive applications such as PVC pipe adhesives.
[0011] The first aspect of the present invention is a. 90 to 99% by weight, preferably 93 to 99% by weight, of vinyl chloride polymer units; b. 0.5 to 10% by weight, preferably 0.5 to 7% by weight, of maleic acid polymer units; and c. 0 to 5% by weight, preferably 0.5 to 5% by weight, of acrylic acid polymer units. In another embodiment, the copolymer according to the present invention comprises a. 90 to 98% by weight of vinyl chloride polymer units; b. in the range of 2 to 10 weight percent maleic acid polymer units.
[0012] A second aspect of the present invention relates to a copolymer composition comprising the copolymer according to the present invention, which may also comprise other polymers, additives, or combinations thereof. That is, the copolymer composition may comprise the copolymer according to the present invention and one or more other polymers, or the copolymer according to the present invention and additives, or the copolymer according to the present invention together with one or more other polymers and additives. The additives may be of any type used to improve the properties of the copolymer composition to suit the application, such as, for example, stabilizers, impact modifiers, plasticizers, fillers, lubricants, flame retardants, blowing agents, pigments, or combinations thereof.
[0013] A third aspect of the invention relates to an article made from or comprising a copolymer or copolymer composition according to the invention.
[0014] The copolymers according to the present invention, copolymer compositions containing such copolymers, and articles made from or containing the copolymers or copolymer compositions have excellent physical properties such as hardness and elasticity, excellent adhesion at low temperatures, reduce the use of additives, and can solve or reduce problems such as migration of plasticizers from the surface of the article. Moreover, they not only provide good appearance to the article, but also have low power consumption for molding and are easy to mold into articles. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0015] Any embodiment shown herein is intended to encompass applications to other embodiments according to the present invention unless expressly stated otherwise.
[0016] Technical and scientific terms used herein have the meanings understood by those of ordinary skill in the art unless otherwise defined.
[0017] Throughout the present invention, the term "about" is used to indicate that any value appearing or indicated herein may vary or deviate. Such variations or deviations may be caused by errors in the equipment or method used to determine the value.
[0018] The terms "consist(s) of", "comprise(s)", "contain(s)", and "include(s)" are open-ended verbs. For example, any method that "consist(s) of", "comprise(s)", "contain(s)", or "include(s)" a component or components or a step or steps is not limited to only one component or step or steps or components, but also encompasses unspecified components or steps.
[0019] Any tools, devices, methods, materials, or chemicals referred to herein refer to tools, devices, methods, materials, or chemicals commonly used or practiced by those of skill in the art, unless otherwise specified.
[0020] All components and / or methods disclosed and claimed in the present invention are intended to cover aspects of the present invention resulting from the operation, practice, modification, or alteration of any element, which imparts characteristics and usefulness without the need for substantially different experiments from the present invention, and which, although not specifically stated in the claims, according to the judgment of a person skilled in the art, produces the same effect as the embodiment according to the present invention. Therefore, substitutes or similar to the embodiment according to the present invention, and slight modifications or changes obvious to a person skilled in the art, are also considered to be within the spirit, scope, and concept of the present invention.
[0021] definition The term "polymer unit" according to the present invention is intended to refer to any portion of a polymer or copolymer chain that is composed or formed by two or more monomeric or repeating units. As used herein, the term "polymeric unit" is also intended to include oligomers of such monomeric or repeating units.
[0022] The term "vinyl chloride polymer unit" according to the present invention is intended to refer to any portion of a copolymer chain that is constituted or formed by two or more vinyl chloride repeat units or vinyl chloride oligomers.
[0023] The term "maleic acid polymer unit" according to the present invention is intended to refer to any portion of a copolymer chain that is composed or formed by two or more maleic acid repeat units or maleic acid oligomers.
[0024] The term "acrylic acid polymer unit" according to the present invention is intended to refer to any portion of a copolymer chain that is composed or formed by two or more acrylic acid repeat units or acrylic acid oligomers.
[0025] The present invention will be described in more detail below with reference to experimental examples and characteristic test results, but they are not intended to limit the scope of the present invention.
[0026] The first aspect of the present invention is a. 90 to 99% by weight of vinyl chloride polymer units; b. in the range of 0.5 to 10 weight percent maleic acid polymer units; and c. 0 to 5 weight percent of acrylic acid polymer units. According to a preferred embodiment of the present invention, the copolymer comprises a. 93 to 99 weight percent vinyl chloride polymer units; b. in the range of 0.5 to 7 weight percent maleic acid polymer units; and c. acrylic acid polymer units in the range of 0.5 to 5 weight percent. According to another preferred embodiment of the invention, the copolymer comprises a. 90 to 98% by weight of vinyl chloride polymer units; b. in the range of 2 to 10 weight percent maleic acid polymer units.
[0027] The maleic acid according to the present invention may be a dialkyl maleate, preferably a dialkyl maleate having carbon atoms ranging from 6 to 36. Exemplary dialkyl maleates may be selected from the group consisting of di-2-ethylhexyl maleate, dimethyl maleate, dicetyl maleate, and combinations thereof.
[0028] The acrylic acid according to the present invention may be an alkyl acrylate, preferably an alkyl acrylate having carbon atoms ranging from 4 to 21. Exemplary alkyl acrylates may be selected from the group consisting of 2-ethylhexyl acrylate, methyl acrylate, stearyl acrylate, and combinations thereof.
[0029] According to the present invention, the copolymer has a K value in the range of 50 to 84. Preferably, in the above specified ranges, when the copolymer comprises vinyl chloride polymer units, maleic acid polymer units and acrylic acid polymer units, the copolymer has a K value in the range of 50 to 75. Also, when the copolymer comprises vinyl chloride polymer units and maleic acid polymer units, i.e., no acrylic acid polymer units, the copolymer has a K value in the range of 61 to 84.
[0030] Copolymers having the specified K values are selected to suit the application or properties of the final product, for example, for rigid applications, preferred copolymers will have low to medium K values, and for semi-rigid or flexible applications, preferred copolymers will have medium to high K values.
[0031] The copolymers according to the invention are suitable for various applications, for example: - rigid applications which may be selected from the group consisting of drinking water pipes, doors, windows, mouldings, panel mouldings, electrical conduits, corridor floors, cable trays, and rigid foam boards, etc.; Semi-rigid applications, which may be selected from the group consisting of films, sheets, blister packs, stickers, credit cards, semi-rigid plastic sheets, shrink sleeves, and cling films, etc. - flexible applications, which may be selected from the group consisting of flexible plastic sheets, cables, indoor wires, outdoor wires, automotive wires, rubber tiles, refrigerator seals, mirror edge seals, electrical tapes, artificial leather, and flexible plastic sheets, etc.; -Adhesive applications include PVC pipe adhesives.
[0032] A second aspect of the present invention relates to a copolymer composition comprising a copolymer according to the present invention having the above specified aspects and properties.
[0033] The copolymer composition according to the invention may also comprise other polymers, additives, or combinations thereof, i.e., the copolymer composition may comprise a copolymer according to the invention and one or more other polymers, or may comprise a copolymer according to the invention and additives, or may comprise a copolymer according to the invention together with one or more other polymers and additives.
[0034] Any additive may be used that can improve the properties of the copolymer composition to suit the application, for example, the additive may be selected from the group consisting of stabilizers, impact modifiers, plasticizers, fillers, lubricants, flame retardants, blowing agents, pigments, and combinations thereof.
[0035] Examples of stabilizers that can be used according to the present invention include agents that can be selected from the group consisting of tin stabilizers, methyltin stabilizers, octyltin stabilizers, organotin stabilizers, non-lead stabilizers such as calcium zinc stabilizers, lead stabilizers such as tribasic lead sulfate (TBLS), dibasic lead phosphite, dibasic lead stearate (DBL), and the like.
[0036] Examples of impact modifiers that may be used in accordance with the present invention include agents that may be selected from the group consisting of methylbutadienestyrene (MBS), acrylic impact modifiers (AIM), and chlorinated polyethylene modifiers (CPE).
[0037] Examples of plasticizers that can be used according to the present invention can be selected from the group consisting of phthalates such as diisodecyl phthalate (DIDP), diisononyl phthalate (DINP), benzyl butyl phthalate (BBP), non-phthalates such as dioctyl adipate (DOA), trioctyl trimellitate (TOTM), adipic polyesters, dioctyl phthalate (DOP), epoxidized soybean oil (EPO).
[0038] Examples of fillers that can be used according to the present invention include agents that can be selected from the group consisting of calcium carbonate (CaCO3), kaolin, and the like.
[0039] Examples of lubricants that can be used in accordance with the present invention include waxes, preferably polyethylene waxes.
[0040] A third aspect of the invention relates to an article comprising a copolymer or copolymer composition according to the invention.
[0041] The articles according to the invention are suitable for a variety of applications, for example: - rigid applications which may be selected from the group consisting of drinking water pipes, doors, windows, mouldings, panel mouldings, electrical conduits, corridor floors, cable trays, and rigid foam boards, etc.; Semi-rigid applications, which may be selected from the group consisting of films, sheets, blister packs, stickers, credit cards, semi-rigid plastic sheets, shrink sleeves, and cling films, etc. - flexible applications, which may be selected from the group consisting of flexible plastic sheets, cables, indoor wires, outdoor wires, automotive wires, rubber tiles, refrigerator seals, mirror edge seals, electrical tapes, artificial leather, flexible plastic sheets, and the like; or -Adhesive applications include PVC pipe adhesives.
[0042] The process for preparing the copolymers according to the present invention can be carried out using any suitable method known in the art.
[0043] Experimental Example To study the properties of the copolymers according to the present invention, as well as copolymer compositions and articles made from or including the copolymers according to the present invention, polymer examples were prepared, such as, for example, Examples 1-8 which are copolymers according to the present invention, Comparative Examples 1 and 2 which are polyvinyl chloride homopolymers, and Comparative Examples 3 and 4 which are copolymers, with each example differing in the amount and type of each polymer unit, as shown in Table 1.
[0044] [Table 1]
[0045] The example polymers were tested for properties, namely, average particle size of the polymer, plasticizer absorption time (PAT), and glass transition temperature (Tg), as detailed below.
[0046] 1) Measurement of average particle size To measure the average particle size of the polymer, the dry polymer powder was passed through sieves with different opening sizes, stacked with larger openings on top and smaller openings on the bottom. The sieves were shaken for 10 minutes using a sieve shaker. The particle size of the dry polymer powder was then calculated using the following formula: Polymer powder size = [(P1 x D1) + (P2 x D2) + ..... + (Pn x Dn)] / 100 where P1, P2, ..., Pn are the amounts (percentages) of polymer powder retained on the sieves of different opening sizes, and D1, D2, ..., Dn are the average opening sizes of the sieves, e.g., μm (microns). For example, P1 is the fraction of dry polymer powder that is retained on a sieve with average aperture size D1.
[0047] 2) Measurement of plasticizer absorption time (PAT) The plasticizer absorption time can be measured by a method according to the ASTM D2396-88 standard. The plasticizer absorption time is the time from when the plasticizer is added to the composition until the kneading torque of the planetary mixer reaches a minimum.
[0048] 3) Measurement of glass transition temperature (Tg) Glass transition temperature can be measured using a differential scanning calorimeter (DSC) to analyze the thermal changes of polymers by placing the test sample (polymer) in one tray and heating them, using another tray as a reference tray. The DSC will read the temperature that causes a chemical change in the polymer.
[0049] The results of the above tests, namely average particle size, plasticizer absorption time (PAT), and glass transition temperature (Tg) of the example polymers are shown in Table 2.
[0050] [Table 2]
[0051] From the above test results, it was found that the plasticizer absorption time (PAT) of the copolymer examples (Examples 1 to 8) according to the present invention was significantly shorter than that of the comparative examples (Comparative Examples 1 and 2) which were polyvinyl chloride homopolymers. The shortening of the PAT had the positive effect of reducing the time and energy used for mixing the drugs, thereby reducing production costs. Furthermore, the shortening of the PAT also helped to delay the degradation of the polymer.
[0052] Furthermore, when comparing only the copolymers containing vinyl chloride polymer units and di-2-ethylhexyl maleate polymer units, i.e., Examples 1, 6, 7, and 8 of the present invention, with Comparative Examples 3 and 4, it was found that the copolymers containing di-2-ethylhexyl maleate polymer units in the range of 0.5 to 10% by weight according to the present invention (Examples 1, 6, 7, and 8) had significantly lower glass transition temperatures (Tg) than the copolymers containing di-2-ethylhexyl maleate polymer units in the range of less than 0.5% by weight (Comparative Example 3), and even the copolymers containing di-2-ethylhexyl maleate polymer units in the range of more than 10% by weight (Comparative Example 4) had lower glass transition temperatures than the copolymers according to the present invention (Examples 1, 6, 7, and 8). However, when comparing the particle sizes of the copolymers, it was found that the copolymers according to Comparative Example 4 had much larger particle sizes than the copolymer examples according to Examples 1, 6, 7, and 8. Furthermore, it was also found that the copolymer according to Comparative Example 4 had a maximum of 10% of particles larger than 500 μm, and thus there was a high possibility that fish eyes would be found during article fabrication.
[0053] Test results The copolymer examples were then used to prepare copolymer compositions and articles depending on the application, ie, molding into credit cards, cable sheathing, cling film, etc., as detailed below.
[0054] 1. Credit Card Example compositions were prepared using the Example Copolymers and the Comparative Polymers with different amounts and types of additives, and the Example Compositions and articles molded therefrom were then tested for properties, namely impact strength, lamination, and thermal stability, as detailed below.
[0055] 1) Izod impact strength The Izod impact strength was measured according to the ASTM D-256 (2018) standard. The composition examples tested were 3 mm thick, had a V-shaped notch, and were struck with a 5.5 J pendulum.
[0056] 2) Laminate property test Laminate forming testing of the example compositions was carried out by preparing 0.5 mm thick laminate samples from each example composition at a temperature of 140° C. The resulting laminates were formed into workpieces by splicing two sample laminates together in a 1 mm thick frame using a hot press at temperatures of 100° C., 110° C., and 120° C. for 5 minutes under 50 bar pressure. Upon completion, the workpiece laminates were inspected for adhesion and evaluated by rating from 0 to 5, with 0 meaning not bonded and 5 meaning tightly bonded.
[0057] 3) Thermal stability test The thermal stability of the example compositions was measured using a metrastat machine at a temperature of 200° C. for 100 minutes using 0.5 mm thick example compositions. Thermal stability was inspected by visual inspection for discoloration and other signs of deterioration. The initial discoloration time of the test samples and the burnt discoloration time of the example compositions were also recorded.
[0058] Composition Examples 1 to 5 were prepared from Copolymer Examples 1 to 5 (Table 1), respectively, and Comparative Composition Example 1 was prepared from Comparative Polymer Example 1 (Table 1). These composition examples differ in the amount and type of additives, and the results of the aforementioned property tests are shown in Table 3.
[0059] [Table 3]
[0060] The test results in Table 3 show that the example compositions containing the copolymers according to the present invention (Examples 3, 4, and 5) have significantly improved impact strength compared to Comparative Example 1, which contains a vinyl chloride homopolymer.
[0061] When the lamination test results at various temperatures were examined, it was found that composition examples 1 to 5 according to the present invention could be laminated at a temperature of 120°C. At this temperature, composition examples 3 to 5 had the highest lamination evaluation scores (5 points), indicating that the copolymer composition according to the present invention has properties suitable for lamination. It was also found that only composition example 5 could be laminated at a temperature of 110°C.
[0062] The lamination ability at low temperature or high evaluation score of the composition according to the present invention is due to the lower glass transition temperature (Tg) of the polymer compared to the comparative example (see Table 2), which allows melting at low temperature. This lamination ability at low temperature is a very necessary property for some applications, specifically for the manufacture of credit cards or other products that contain heat-sensitive devices such as chips.
[0063] 2. Cable sheath Copolymer Examples 6 and 7 (Table 1) and Comparative Polymer Example 2 (Table 1) were used to prepare composition examples with different amounts and types of additives. The composition examples and articles molded therefrom, as well as Comparative Composition Example 2, were then tested for properties, namely melt time, melt flow index (MFI), volume resistivity (VR), hardness, and migration. The details are as follows:
[0064] 1) Melting time The melting time was tested according to the ASTM D2396:2020 standard by mixing the example compositions using a batch mixer at a temperature of 180° C. and a screw speed of 40 rpm until the torque decreased to a constant value and recording the time to reach the constant torque.
[0065] 2) Melt Flow Index (MFI) The melt flow index was tested according to the ASTM D1238:2020 standard by melting the example composition in a cylinder at a determined temperature and weight of force, weighing the example composition flowing out of the cylinder, and calculating the melt flow index using the following formula: MFI=10W / T where W is the average weight of the extruded example composition in grams. T is the extrusion time (min) of the extruded example composition.
[0066] 3) Volume resistivity (VR) Volume resistivity was measured according to ASTM D257 by placing a 2 mm thick example composition between two electrodes and applying a voltage for 60 seconds. Surface or volume resistivity was then measured. Apparent values (at 60 seconds of current flow) were calculated and reported.
[0067] 4)Hardness Hardness was measured according to the D2240-68:2021 standard by preparing 6 mm thick workpieces of the example compositions and testing them with a durometer using a Shore A indenter. Tests were performed at five points to determine an average value.
[0068] 5) Migration Plasticizer migration was determined by heating 1 mm thick example compositions after preparation in an oven for 10 days at a temperature of 70° C. The percentage of plasticizer migration to the surface of such examples was then calculated using the following formula: Transfer rate = (weight before insulation - weight after insulation) x 100 / weight before insulation
[0069] Composition Examples 6 and 7, prepared from Copolymer Examples 6 and 7 (Table 1), and Comparative Composition Example 2, prepared from Comparative Polymer Example 2 (Table 1), differ in the amount and type of additives, and the results of the above-mentioned property tests are shown in Table 4.
[0070] [Table 4]
[0071] The test results in Table 4 show that the copolymer compositions according to the present invention (Composition Examples 6 and 7) exhibit shorter melting times and higher polymer melt flow indexes than Comparative Composition Example 2. With such excellent results, the copolymer compositions according to the present invention can reduce the power consumption in wire manufacturing by up to 4.16%. In addition to saving power during manufacturing, the exterior surface of the exemplary molded workpiece of the copolymer composition according to the present invention also shows no fisheyes compared to Comparative Composition Example 2. This is an advantage of the present invention, since the exterior surface of the workpiece is one of the important properties to be considered for practical use.
[0072] To use a polymer for the manufacture of insulating products, such as cable sheath products, it is necessary to meet certain hardness values according to industry standards (IS) and to measure resistivity. Good insulating materials naturally have high volume resistivity and low electrical conductivity. Test results show that the copolymer composition according to the invention shows a higher resistance to electrical current in the material compared to Comparative Composition Example 2 as a result of the addition of plasticizer additive. At lower amounts (see Table 4), the flow of electrons in the material is less, but the hardness values are comparable to Comparative Composition Example 2, i.e. the hardness values of the articles molded from the copolymer composition according to the invention did not increase despite the addition of a lower amount of oil.
[0073] For semi-rigid or flexible applications, plasticizer additives need to be added to the formulation to soften the material. Excessive addition of plasticizer can cause the plasticizer to migrate to the surface, resulting in reduced flexibility, deterioration of certain properties, and sticky surface of the workpiece, which is not only undesirable for the application but also increases brittleness. From the above test, it was found that the copolymer composition according to the present invention has less migration of plasticizer (dioctyl phthalate) compared to the comparative composition example 2 with the same hardness value of the workpiece.
[0074] Furthermore, it was found that the copolymer composition example according to the present invention has a shorter plasticizer absorption time than the comparative composition example 2. The above value indicates the time it takes for the polymer to absorb oil. A shorter plasticizer absorption time means less energy and less mixing time, which saves energy, reduces processing time, reduces degradation of the polymer or the article molded from the polymer, and can result in a smoother surface or less fisheyes on the article.
[0075] 3. Cling film Copolymer Example 8 (Table 1) was used to prepare Example Composition 8, an example copolymer composition according to the present invention, and Comparative Polymer Example 2 (Table 1) was used to prepare Comparative Example Composition 3, which used different amounts and types of additives. Comparative Example Composition 3 as well as the example compositions and articles molded therefrom were then tested for properties, namely, plasticizer absorption time, hardness, melt flow index, overall migration (OM), and migration of plasticizer to the surface. Details of the measurements of plasticizer absorption time, hardness value, melt flow index (MFI), and migration of plasticizer to the surface are as described above.
[0076] Total migration (OM) testing was carried out by testing the prepared composition examples according to BS EN 1186-15:2002 standard. This was done by preparing 14x14cm test workpieces, weighing the workpieces from each composition example, and immersing them in isooctane solution at a temperature of 20°C for 2 days. After completion, the isooctane solution was removed and the workpieces immersed in the isooctane solution were weighed. The isooctane was then evaporated and the residual additives in the workpieces after evaporation were weighed. All weights measured were recorded and calculations were made using the following formula to measure total migration: M=(A-B) / S where M is the total migration amount (mg / dm 2 ).
[0077] A is the combined weight (mg) of the example work piece after evaporation and the vessel used for evaporation.
[0078] B is the weight (mg) of the container used for evaporation measured before the test.
[0079] S is the contact area (dm) between the example workpiece and the solution.
[0080] The example compositions contained different amounts and types of additives and the results of the aforementioned property tests are shown in Table 5.
[0081] [Table 5]
[0082] The test results in Table 5 show that the plasticizer absorption time of the test workpieces of the copolymer example compositions according to the present invention is significantly reduced compared to the comparative composition examples. A shorter plasticizer absorption time means less energy and shorter mixing time, which can save energy and also reduce degradation of the polymer or article.
[0083] The melt flow index of the test workpieces of the copolymer example compositions according to the invention is higher than that of the comparative example compositions.
[0084] Considering the total migration amount (OM) to test the resistance to extraction with a solution such as alcohol, the test workpiece of the copolymer example composition of the present invention was found to have a significantly smaller total migration amount than that of the comparative composition example, which indicates that the copolymer example composition of the present invention can be more resistant to extraction with a solution than the comparative composition example.
[0085] Generally, semi-rigid articles require the addition of plasticizers to ensure that the article has a hardness suitable for its application, and over time the plasticizers will migrate to the surface of the article, making the surface of the article sticky, undesirable for its application, and increasing its brittleness. From Table 5, it can be seen that the migration of plasticizers to the surface of the test workpieces made from the copolymer composition examples according to the present invention is significantly lower than that of the test workpieces made from the comparative composition examples.
[0086] From all the above test results, it can be concluded that the copolymer of polyvinyl chloride, as well as the copolymer composition containing such copolymer according to the present invention, has improved properties. That is, the copolymer of polyvinyl chloride can be molded at a lower temperature and melted more easily, so that the energy in the production of the workpiece can be saved. It can also have sufficient resistance to the solvent. In other words, the migration of plasticizer to the surface is reduced. Furthermore, it has been found that the copolymer of polyvinyl chloride according to the present invention can solve the fish eye problem on the surface of the workpiece or article, make the appearance of the article more beautiful and attractive, and extend the service life.
[0087] Best Mode for Carrying Out the Invention The best mode of the present invention is as described in the detailed description of the present invention.
Claims
1. A copolymer comprising: a. in the range of 90 to 99 weight percent vinyl chloride polymer units; b. in the range of 0.5 to 10 weight percent maleic acid polymeric units; c. acrylic acid polymeric units in the range of 0-5 weight percent.
2. a. in the range of 93 to 99 weight percent of said vinyl chloride polymer units; b. in the range of 0.5 to 7 weight percent of said maleic acid polymer units; and c. in the range of 0.5 to 5 weight percent of said acrylic acid polymeric units.
3. a. in the range of 90 to 98 weight percent of said vinyl chloride polymer units; b. in the range of 2 to 10 weight percent of said maleic acid polymeric units.
4. The copolymer of any one of claims 1 to 3, wherein the maleic acid is a dialkyl maleate.
5. The copolymer of claim 4, wherein the dialkyl maleate has in the range of 6 to 36 carbon atoms.
6. The copolymer of claim 4 or 5, wherein the dialkyl maleate is selected from the group consisting of di-2-ethylhexyl maleate, dimethyl maleate, dicetyl maleate, and combinations thereof.
7. 3. The copolymer of claim 1 or 2, wherein the acrylic acid is an alkyl acrylate.
8. The copolymer of claim 7, wherein the alkyl acrylate has in the range of 4 to 21 carbon atoms.
9. The copolymer of claims 7 or 8, wherein the alkyl acrylate is selected from the group consisting of 2-ethylhexyl acrylate, methyl acrylate, stearyl acrylate, and combinations thereof.
10. A copolymer according to any one of claims 1 to 3 having a K value in the range of 50 to 84.
11. 11. The copolymer of claim 2 or 10 having a K value in the range of 50 to 75.
12. 11. The copolymer of claim 3 or 10 having a K value in the range of 61 to 84.
13. Rigid applications, preferably drinking water pipes, doors, windows, mouldings, panel mouldings, conduits, corridor floors, cable trays and rigid foam boards; Semi-rigid applications, preferably films, sheets, blister packs, stickers, credit cards, semi-rigid plastic sheets, shrink sleeves, and cling films; Flexible applications, preferably flexible plastic sheets, cables, indoor electrical wires, outdoor electrical wires, automotive electrical wires, rubber tiles, refrigerator seals, mirror edge seals, electrical tapes, artificial leather, and flexible plastic sheets, or The copolymer according to any one of claims 1 to 12 for adhesive applications, preferably as a PVC pipe adhesive.
14. A copolymer composition comprising the copolymer of any one of claims 1 to 12.
15. 15. The copolymer composition of claim 14, further comprising other polymers, additives, or combinations thereof.
16. 16. The copolymer composition of claim 15, wherein the additive is selected from the group consisting of stabilizers, impact modifiers, plasticizers, fillers, lubricants, flame retardants, blowing agents, pigments, and combinations thereof.
17. A copolymer according to any one of claims 1 to 12, or An article comprising the copolymer composition of any one of claims 14 to 16.
18. Rigid applications, preferably drinking water pipes, doors, windows, mouldings, panel mouldings, conduits, corridor floors, cable trays and rigid foam boards; Semi-rigid applications, preferably films, sheets, blister packs, stickers, credit cards, semi-rigid plastic sheets, shrink sleeves, and cling films; Flexible applications, preferably flexible plastic sheets, cables, indoor electrical wires, outdoor electrical wires, automotive electrical wires, rubber tiles, refrigerator seals, mirror edge seals, electrical tapes, artificial leather, and flexible plastic sheets, or 18. The article of claim 17 for adhesive applications, preferably PVC pipe adhesive.