Selective Etching of Semimetals or Metals Using Fluorocarbon-Based Depositions
The method of using a fluorocarbon and metalloid/metal halide gas plasma for selective silicon oxide etching in semiconductor devices addresses the issue of spacer material etching, ensuring precise etching and reducing electrical leakage by employing a thin, etch-resistant hard mask.
Patent Information
- Application Number
- JP2024531437
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2021-12-01
- Filing Date
- 2022-11-28
- Publication Date
- 2024-11-26
AI Technical Summary
Current selective etching processes for silicon oxide in semiconductor devices are not selective enough, leading to the etching of extra portions of spacer materials and increased electrical leakage due to exposure of spacer corners, which can result in device failure.
A method involving the use of an etching gas that includes a fluorocarbon gas and a metalloid or metal halide gas, converted into plasma, to selectively etch silicon oxide regions while forming a metalloid or metal-containing hard mask over low oxygen content regions, thereby preventing spacer material etching.
This approach achieves highly selective etching of silicon oxide regions with minimal etching of low oxygen content areas, reducing electrical leakage and device failure by using a thin, etch-resistant metalloid or metal-containing hard mask that prevents spacer corner loss and clogging.
Smart Images

Figure 2024543922000001_ABST
Abstract
Description
[Technical field]
[0001] <CROSS REFERENCE TO RELATED APPLICATIONS> This application claims the benefit of priority to U.S. Application No. 63 / 284,877, filed December 1, 2021, and is incorporated by reference herein for all purposes. [Background technology]
[0002] The background discussion provided herein is intended to generally present the context of the present disclosure. The information set forth in this background section, as well as aspects of the description that may not otherwise qualify as prior art at the time of filing, are not admitted, either explicitly or implicitly, as prior art to the present disclosure.
[0003] The present disclosure relates to a method for forming semiconductor devices on a semiconductor wafer. More particularly, the present disclosure relates to selective etching of silicon oxide (SiO2) relative to other materials. In this specification and claims, etching of SiO2 includes etching of SiO2-based materials such as borophosphosilicate glass (BPSG, a silicon oxide glass doped with boron and phosphorus), or carbon-doped silicon oxide such as SiCOH, or other low-k silicon oxide-based materials. Such SiO2-based materials may also be other types of doped SiO2.
[0004] The minimum feature dimensions of semiconductor devices continue to shrink according to Moore's Law. One of these features is the contact between the first metal layer and the silicon layer with the gate and source / drain (S / D). Such features are typically fabricated by a process called self-aligned contact (SAC). In SAC etching, the SiO2 is etched to form holes or trenches. The holes or trenches are then filled with contact metal. Selective SiO2 etching is used to etch the SiO2 selectively to the spacer material. The spacer material is typically a silicon material with a low oxygen content, such as silicon nitride, silicon oxynitride, or silicon oxycarbonitride. Many selective etching processes are not selective enough. As a result, excess spacer material or corners of the spacer material are etched, which can increase electrical leakage and device failure rates. Summary of the Invention
[0005] To achieve the above and in accordance with the objectives of the present disclosure, a method is provided for selectively etching at least one feature in a silicon oxide region relative to an oxygen-poor region. An etching gas is provided that includes a fluorocarbon gas and at least one of a metalloid halide gas or a metal halide gas. The etching gas is turned into a plasma. At least one feature in the silicon oxide region is selectively etched relative to the oxygen-poor region while simultaneously forming a metalloid or metal-containing hard mask over the oxygen-poor region.
[0006] These and other features of the present disclosure are described in more detail in the following detailed description taken in conjunction with the following figures. [Brief description of the drawings]
[0007] The present disclosure is illustrated by way of example, and not by way of limitation, in the figures of the accompanying drawings, in which like reference numerals refer to similar elements and in which:
[0008] [Figure 1] FIG. 1 is a high level flow chart of one embodiment.
[0009] [Figure 2A] FIG. 2A is a schematic cross-sectional view of a structure processed according to one embodiment. [Figure 2B] FIG. 2B is a schematic cross-sectional view of a structure processed according to one embodiment. [Figure 2C] FIG. 2C is a schematic cross-sectional view of a structure processed according to one embodiment. [Figure 2D] FIG. 2D is a schematic cross-sectional view of a structure processed according to one embodiment. [Figure 2E] FIG. 2E is a schematic cross-sectional view of a structure processed according to one embodiment.
[0010] [Diagram 3] FIG. 3 is a more detailed flow chart of selectively etching silicon oxide regions while depositing a semi-metal or metal-containing hardmask.
[0011] [Figure 4] FIG. 4 is a high level flow chart of another embodiment.
[0012] [Diagram 5] FIG. 5 is a schematic diagram of an etching chamber that can be used in one embodiment.
[0013] [Figure 6] FIG. 6 is a schematic diagram of a computer system that can be used to implement one embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0014] The present disclosure will now be described in detail with reference to several exemplary embodiments illustrated in the accompanying drawings. In the following description, numerous specific details are set forth in order to provide a thorough understanding of the present disclosure. However, it will be apparent to one of ordinary skill in the art that the present disclosure may be practiced without some or all of these specific details. In other instances, well-known process steps and / or structures have not been described in detail in order not to unnecessarily obscure the present disclosure.
[0015] The contact holes or trenches must be placed very precisely with respect to the underlying gate and S / D. Current photolithography tools can only partially meet the contact placement requirements. As a result, the contact etch may expose the spacer around the gate. Such exposure often leads to corner loss of the spacer material, resulting in electrical leakage.
[0016] Selective SiO2 etching can be achieved by selectively depositing a carbon-based polymer on the spacer material to protect the spacer from etching. However, holes and trenches below the 5 nanometer (nm) node may have lateral dimensions less than 10 nm. More typically, such features may be in the range of 5-15 nm. The aspect ratio may be greater than 6:1. In some embodiments, the aspect ratio may be in the range of 6:1-12:1. Additionally, the use of carbon-based polymer masks has limited etch resistance. Due to the limited etch resistance, the mask must be deposited thick to protect the spacer during the SiO2 etch. Placing a thick polymer material on the spacer may clog and / or pinch off the contacts, preventing further etching. This etch inhibition may result in electrically open contacts, causing device failure. Additionally, thick polymer materials tend to deposit in different amounts in different parts of the pattern layout due to local shadowing of the features. This effect is sometimes called pattern loading and causes undesirable variations in the final etch result, including the critical dimension (CD) of the trench or hole.
[0017] The disclosed process and apparatus allows for selective deposition of a semi-metallic or metal-containing mask, such as a metal carbide, on the spacer material during the etching process. The mask is formed in situ during the etching process, rather than by initial photolithography. Compared to traditional carbon-based polymer masks, the semi-metallic or metal-containing mask has higher etch selectivity, so a thinner, less than 5 nm hard mask is sufficient. The semi-metallic or metal-containing hard mask prevents loss of spacer corners while avoiding the pinch-off issues of traditional polymer materials. The thin semi-metallic or metal-containing hard mask also allows for low variation due to pattern loading.
[0018] FIG. 1 is a high level flow chart of one embodiment for ease of understanding. A structure having a silicon oxide region is provided (step 104). FIG. 2A is a schematic cross-sectional view of a portion of a structure 200 having a silicon oxide region 204. In this example, the structure 200 also has a silicon oxycarbonitride (SiOCN) region 208, and a silicon (Si) region 212. The silicon region 212 may be crystalline or polycrystalline silicon, or amorphous silicon. SiOCN materials include silicon oxynitride (SiON), silicon oxycarbide (SiOC), silicon carbonitride (SiCN), organosilicon oxide (SiOCH x ) (back end of line (BEOL) low-k), silicon nitride (SiN), or silicon carbide (SiC). SiOCN region 208 and Si region 212 are referred to as oxygen-poor regions because they have a lower oxygen concentration than silicon oxide region 204. In this embodiment, a native silicon oxide layer 216 naturally forms over SiOCN region 208 and silicon region 212 when SiOCN region 208 and silicon region 212 are exposed to air. In an alternative embodiment, layer 216 is a deposited silicon oxide layer that covers SiOCN region 208 and silicon region 212 after silicon oxide region 204 is filled. As shown, a photolithography mask 220 of patterned photoresist is formed over structure 200. In an alternative embodiment, mask 220 can be a hard mask created by a prior lithography and etching process. Mask 220 can be a spin-on carbon material, silicon, silicon nitride, or other material that can be selectively etched over silicon oxide.
[0019] After the structure is provided, a selective pre-etch (step 108) is provided to selectively etch the silicon oxide regions 204 and the native silicon oxide layer 216 that are not covered by the photolithography mask 220. In this embodiment, the silicon oxide regions 204 are selectively etched using atomic layer etching (ALE). In this embodiment, the ALE provides hexafluoro-1,3-butadiene (C4F6) as a reactive gas. The C4F6 forms a polymer deposition layer on the silicon oxide regions 204 and the native silicon oxide layer 216. The reactive gas is purged and argon (Ar) is provided as an activation gas. The Ar activates the deposition layer, and the deposited fluorine selectively etches the silicon oxide regions 204 and the native silicon oxide layer 216. The ALE process of selective deposition and selective etching steps can be repeated for multiple cycles. FIG. 2B is a cross-sectional view of the structure 200 after the selective pre-etch (step 108) is completed. In this example, the silicon oxide regions 204 that are not covered by the photolithography mask 220 are partially etched, and the native silicon oxide layer 216 that is not covered by the photolithography mask 220 is etched away. The selective deposition of polymer and the selective etching of the silicon oxide regions 204 can be repeated until the silicon oxide regions 204 are sufficiently etched and the native silicon oxide layer 216 is removed. Such an etching process selectively etches the silicon oxide regions 204. However, the selectivity is not high enough. The SiOCN regions 208 and parts of the Si regions 212 are also etched away. Therefore, in this embodiment, this etching is only used for the pre-etching process. In some embodiments, the pre-etching process is not used.
[0020] After the selective pre-etch (step 108) is completed, the silicon oxide region 204 is selectively etched while depositing a metalloid or metal-containing hard mask (step 112). FIG. 3 is a more detailed flow chart of selectively etching the silicon oxide region 204 while depositing a metalloid or metal-containing hard mask (step 112). In such an embodiment, an etching gas is provided (step 304) including a fluorocarbon gas and at least one of a metalloid halide gas or a metal halide gas. In this embodiment, the etching gas includes hexafluorobutadiene (C4F6), tungsten hexafluoride (WF6), oxygen (O2), and argon (Ar). In this embodiment, the etching gas does not include hydrogen. The etching gas is provided by flowing the etching gas into a plasma processing chamber (step 304). While the etching gas is flowing into the plasma processing chamber, radio frequency power is provided to convert the etching gas into a plasma (step 308). In one example, a chamber pressure of 1-500 mTorr is provided. The etching gas includes 0.5-60 sccm CF6, 0.5-60 sccm WF6, 0.5-60 sccm oxygen, and 50-2000 sccm Ar. In one embodiment, a substrate or chuck temperature is provided in the range of 30° C.-150° C. In another embodiment, a substrate or chuck temperature is provided in the range of 30° C.-210° C. In another embodiment, the substrate or chuck is maintained at a temperature of about 210° C. or less. In another embodiment, the substrate or chuck is maintained at a temperature of about 300° C. or less. To plasmatize the etching gas and provide a bias, a radio frequency of 20-1000 W (capacitively coupled plasma (CCP) and bias), such as one or more of 13.56 megahertz (MHz), 60 MHz, 27 MHz, 2 MHz, 1 MHz, 400 kilohertz (kHz), or a combination thereof, is provided. The plasma selectively etches the silicon oxide regions 204 relative to the oxygen-poor regions while simultaneously forming a semi-metallic or metal-containing hardmask over the oxygen-poor regions (step 312).The selective etch is highly selective to the silicon oxide regions 204 relative to the photolithography mask 220. In this embodiment, the selective etch is a hydrogen-free selective etch.
[0021] 2C is a cross-sectional view of structure 200 after selective etching of silicon oxide region 204 (step 112) while depositing a metalloid or metal-containing hard mask partially etches feature 228 in silicon oxide region 204. Fluorine and carbon in the plasma etch silicon oxide region 204. Carbon and metal in the plasma selectively deposit metalloid or metal-containing hard mask 224 on SiOCN region 208 and Si region 212. Plasma conditions can reduce metalloid or metal-containing precursors or plasma fragments thereof to selectively deposit metalloid or metal-containing hard mask 224 on SiOCN region 208 and Si region 212. Alternatively, carbon in the plasma reacts with metalloid or metal-containing precursors or fragments thereof to form metalloid or metal-containing hard mask 224 on SiOCN region 208 and Si region 212. The oxygen-containing components of the silicon oxide regions 204 maintain the etching of the silicon oxide regions 204 by preventing or minimizing the deposition of a carbon-containing layer and / or a metalloid or metal-containing hard mask 224 on the silicon oxide regions 204. In this embodiment, the metalloid or metal-containing hard mask 224 is a tungsten carbide hard mask. The metalloid or metal-containing hard mask 224 prevents or minimizes the etching of low oxygen content regions while the silicon oxide regions 204 are being etched. As a result, the etch selectivity can approach infinity.
[0022] 2D is a cross-sectional view of structure 200 after the selective etching of silicon oxide regions 204 has been fully etched. Because the semi-metal or metal-containing hard mask 224 continues to deposit during the etching of silicon oxide regions 204, and because the semi-metal or metal-containing hard mask 224 is resistant to etching, the low oxygen content regions are not etched or are etched only a small and tolerable amount. In this embodiment, when the etching of silicon oxide regions 204 is completed, the semi-metal or metal-containing hard mask 224 remains.
[0023] After etching of the silicon oxide regions 204 is completed, the metalloid or metal-containing hardmask 224 is removed. In this embodiment, a wet clean is used to remove the metalloid or metal-containing hardmask 224. In this embodiment, an aqueous solution of ammonia (NH3) and hydrogen peroxide (H2O2) is used to remove the metalloid or metal-containing hardmask 224 selectively to the silicon oxide regions 204. Figure 2E is a cross-sectional view of the structure 200 after the metalloid or metal-containing hardmask 224 has been removed.
[0024] This embodiment provides a highly selective etch of silicon oxide relative to regions with low oxygen content. In various embodiments, the depth-to-width aspect ratio of features 228 etched into silicon oxide regions 204 is at least 6:1. For example, features 228 have a depth-to-width aspect ratio of 6:1 to 12:1. In this example, features 228 have a width of less than 10 nm. In various embodiments, features 228 have a width of 6 to 15 nm. The use of semi-metallic or metal-containing hard mask 224 prevents or reduces etching of SiOCN regions 208, thereby preventing or reducing corner loss of SiOCN regions 208. Additionally, semi-metallic or metal-containing hard mask 224 is kept thin, thereby preventing clogging and pinch-off of features 228. In some embodiments, the partial etch of the pre-etch step (step 108) provides a concave topography in silicon oxide regions 204. In some embodiments, the recessed initial topography of the silicon oxide regions 204 allows for more selective deposition of the semi-metal or metal-containing hard mask 224 and selective etching of the silicon oxide regions 204.
[0025] The melting and boiling points of metalloid or metal-containing materials, such as metal carbides, are very high, making the metalloid or metal-containing hard mask 224 highly resistant to etching. In other embodiments, other metalloid or metal-containing hard masks made of metal nitrides, metal borides, or metal silicides can be used in place of or in conjunction with metal carbides, provided that the metalloid or metal-containing hard mask is highly resistant to etching. In this embodiment, a metalloid or metal-containing hard mask 224 is provided that is highly resistant to etching, allowing the mask to be less than 5 nm thick. This thin hard mask avoids the risk of clogging and allows etching of very narrow features, less than 15 nm.
[0026] In an alternative embodiment, the flow of the metalloid or metal-containing precursor is reduced or stopped near the end of the etching of the silicon oxide regions 204, thereby reducing or stopping the deposition of the metalloid or metal-containing hardmask 224. In one embodiment, at the end of the etching of the silicon oxide regions 204, the metalloid or metal-containing hardmask 224 has been etched away, so that removal of the metalloid or metal-containing hardmask (step 116) is not necessary. In another embodiment, a dry etch is used to remove the metalloid or metal-containing hardmask selectively to the silicon oxide regions 204 (step 116).
[0027] In another embodiment, the metalloid or metal-containing precursor and halogen-containing component is molybdenum hexafluoride (MoF6). In other embodiments, the metalloid or metal-containing precursor may be other metalloid or metal halides. In such embodiments, metalloids such as boron (B), silicon (Si), germanium (Ge), antimony (Sb), or metals such as tin (Sn), titanium (Ti), zirconium (Zr), hafnium (Hf), vanadium (V), niobium (Nb), tantalum (Ta), aluminum (Al), gallium (Ga), indium (In), iron (Fe), ruthenium (Ru), rhenium (Re), tungsten (W), molybdenum (Mo), and bismuth (Bi) can be used (when metalloid or metal halides are present to allow the metalloid or metal halides to flow as gas or vapor). In some embodiments, liquid metal halides can be heated to generate metal halide vapor. In some embodiments, a solid metal halide can be heated to sublimate and produce a metal halide vapor. In other embodiments, a metalloid or metal bromide can be used. In other embodiments, the precursor can be a metalloid or metal oxyhalide.
[0028] In other embodiments, other low-oxygen regions can be used instead of the low-oxygen silicon-containing regions, for example silicon germanium (SiGe), germanium (Ge), elemental metals, or metal nitrides can form low-oxygen regions and can be protected so that SiO2 can be selectively etched relative to these materials.
[0029] In some embodiments, the etching gas further comprises an oxygen-containing component. In some embodiments, the oxygen-containing component comprises at least one of oxygen (O2), ozone (O3), carbon dioxide (CO2), carbon monoxide (CO), nitric oxide (NO), nitrogen dioxide (NO2), nitrous oxide (N2O), sulfur dioxide (SO2), sulfur trioxide (SO3), and carbonyl sulfide (COS). In various embodiments, the etching gas further comprises an inert gas. In some embodiments, the inert gas is selected from the group consisting of nitrogen, helium, argon, krypton, xenon, and neon. In various embodiments, the plasma is formed at a pressure of 1-500 millitorr, a power of 20-1000 watts, and a radio frequency such as one or more of 13.56 megahertz (MHz), 60 MHz, 27 MHz, 2 MHz, 1 MHz, 400 kilohertz (kHz), or a combination thereof.
[0030] In various embodiments, a selective pre-etch (step 108) can remove any native silicon oxide layer 216. If the low oxygen content areas do not form a native oxygen layer, the selective pre-etch (step 108) may not be necessary. A hard mask can be selectively deposited without the selective pre-etch (step 108).
[0031] Another embodiment is illustrated in the flow chart shown in Figure 4. In such an embodiment, a structure is provided with silicon oxide regions (step 404). The silicon oxide regions are selectively etched while a semi-metal or metal-containing hard mask is deposited (step 412).
[0032] In this embodiment, after the silicon oxide region is partially etched and the semi-metallic or metal-containing hard mask is left behind, the silicon oxide region is further or additionally etched by an atomic layer etching (ALE) process (step 416) utilizing the semi-metallic or metal-containing hard mask. In this embodiment, the ALE provides C4F6 as a reactive gas. The C4F6 forms a polymer deposition layer on the silicon oxide region and the semi-metallic or metal-containing hard mask. The reactive gas is purged and Ar is provided as an activation gas. The Ar activates the deposition layer such that the deposited fluorine selectively etches the silicon oxide region relative to the semi-metallic or metal-containing hard mask. The ALE process of selective deposition and selective etching steps can be repeated for multiple cycles.
[0033] Because the ALE process does not deposit a semi-metallic or metal-containing hardmask, the semi-metallic or metal-containing hardmask may be consumed during the ALE process. If the semi-metallic or metal-containing hardmask is consumed sufficiently before the etching of the silicon oxide region is completed, the ALE process (step 416) can be stopped to replenish the semi-metallic or metal-containing hardmask, and the step of selectively etching the silicon oxide region while depositing the semi-metallic or metal-containing hardmask (step 412) can be repeated (step 420). After the semi-metallic or metal hardmask is replenished, the step of selectively etching the silicon oxide region while depositing the semi-metallic or metal-containing hardmask (step 412) is stopped. The ALE process can be used to further etch the silicon oxide region (step 416). Both the steps of selectively etching the silicon oxide while depositing the semi-metallic or metal-containing hardmask (step 412) and the step of performing ALE using the semi-metallic or metal-containing hardmask (step 416) can be repeated cyclically until the features in the silicon oxide region are sufficiently etched. Once the features in the silicon oxide regions have been sufficiently etched, the cyclical process can be stopped. In this embodiment, the ALE process (step 416) consumes the semi-metallic or metallic hardmask, so a separate step of removing the metallic or semi-metallic hardmask is not required.
[0034] In some embodiments, the deposition and etching of the hardmask can be performed in separate sequential steps, however, performing the deposition and etching of the hardmask simultaneously in a single continuous step can provide a more rapid process.
[0035] It has been unexpectedly found that selective etching of silicon oxide regions without hydrogen while depositing a semi-metallic or metal-containing hard mask reduces pattern loading while still adequately protecting corners of low oxygen concentration regions. Preventing pattern loading allows for similar final top CDs to be achieved for features of various shapes within a single die. In practice, more exposed features typically have smaller CDs and features that are locally shaded by cut masks or the like have larger CDs. Providing a selective etch without hydrogen provides a CD that is less shadow dependent. Features with larger aspect ratios generally have more shadows. Thus, providing a process in which the CD is less shadow dependent improves the process for larger aspect ratio features. Without wishing to be bound by theory, it is proposed that process gases that include hydrogen elements in one or more gases tend to produce carbon-containing polymer precursors with higher sticking coefficients. Neutral deposition from these precursors tends to have more feature-dependent and aspect-ratio-dependent effects. Conversely, hydrogen-free processes tend to have carbon-containing precursors with lower sticking coefficients and result in less loading effects. The use of fluorocarbons instead of hydrofluorocarbons or hydrocarbons helps provide a hydrogen-free process. In other embodiments, other fluorocarbons (C4F6), such as perfluorocyclobutane (c-C4F8), octafluorocyclopentane (c-C5F8), tetrafluoroethylene (C2F4), carbon tetrafluoride (CF4), octafluoropropane (C3F8), and hexafluoroethane (C2F6), are used. x F y ) can be used. Some embodiments allow for thinner passivation layers that help reduce breadloafing issues in more exposed features. In some embodiments, etching 59 nm of SiO can result in less than 3 nm of SiN being etched.
[0036] 5 is a schematic diagram of an etch reactor system 500 that can be used in one embodiment. In one or more embodiments, the etch reactor system 500 includes a gas distribution plate 506 providing a gas inlet and an electrostatic chuck (ESC) 508 in an etch chamber 509 surrounded by a chamber wall 552. The structure 200 is disposed above the ESC 508 in the etch chamber 509. The ESC 508 can be biased by an ESC source 548. An etch gas source 510 is connected to the etch chamber 509 through the gas distribution plate 506. An ESC temperature controller 550 is connected to the ESC 508. A radio frequency (RF) source 530 provides RF power to the bottom electrode and / or top electrode, which in this embodiment are the ESC 508 and the gas distribution plate 506, respectively. In an exemplary embodiment, a 60 megahertz (MHz) and optionally a 2 MHz, 27 MHz power supply constitutes the RF source 530 and the ESC source 548. In this embodiment, the top electrode is grounded. In this embodiment, one generator is provided for each frequency. In other embodiments, the generators may be in separate RF sources or separate RF generators may be connected to different electrodes. For example, a top electrode may have an inner electrode and an outer electrode connected to different RF sources. In other embodiments, other arrangements of RF sources and electrodes may be used. A controller 535 is controllably connected to the RF source 530, the ESC source 548, the exhaust pump 520, and the etching gas source 510. One example of such an etching chamber is the Flex™ Etch System manufactured by Lam Research Corporation (Fremont, Calif.). In various embodiments, the process chamber may be a CCP (capacitively coupled plasma) reactor or an ICP (inductively coupled plasma) reactor.
[0037] To illustrate an example of the controller 535 in one embodiment, FIG. 6 is a high-level block diagram illustrating a computer system 600 suitable for implementing the controller 535 used in the embodiment. Computer systems can have a variety of physical forms, from integrated circuits, printed circuit boards, and small handheld devices to huge supercomputers. The computer system 600 includes one or more processors 602 and can further include an electronic display device 604 (displaying graphics, text, and other data), a main memory 606 (e.g., random access memory (RAM)), a storage device 608 (e.g., a hard disk drive), a removable storage device 610 (e.g., an optical disk drive), a user interface device 612 (e.g., a keyboard, touch screen, keypad, mouse or other pointing device, etc.), and a communication interface 614 (e.g., a wireless network interface). The communication interface 614 allows software and data to be transferred between the computer system 600 and external devices over a link. The system can also include a communication infrastructure 616 (e.g., a communication bus, crossover bar, or network) connected to the aforementioned devices / modules.
[0038] Information transferred through communications interface 614 may be in the form of signals, such as electronic, electromagnetic, optical, or other signals, that may be received by communications interface 614 over a signal-carrying communications link, which may be implemented using wire or cable, optical fiber, telephone line, cellular phone link, radio frequency link, and / or other communications channel. It is contemplated that such communications interfaces may enable one or more processors 602 to receive information from a network or output information to a network in the course of performing steps of the methods described above. Additionally, method embodiments may be performed solely on a processor or may be performed over a network, such as the Internet, in cooperation with a remote processor that shares a portion of the processing.
[0039] The term "non-transitory computer-readable medium" is generally used to refer to media such as primary storage, secondary storage, removable storage, and storage devices, e.g., hard disks, flash memory, disk drive memory, CD-ROMs, and other forms of persistent memory, and should not be construed to include transitory objects such as carrier waves or signals. Examples of computer code include machine code, such as code produced by a compiler, and files containing high-level language code that are executed by a computer using an interpreter. The computer-readable medium may also be computer code, conveyed by a computer data signal embodied in a carrier wave and representing a sequence of instructions executable by a processor.
[0040] Although the present disclosure has been described with reference to some exemplary embodiments, there are alternatives, modifications, permutations, and various equivalents that fall within the scope of the present disclosure. It should also be noted that there are many other ways to implement the method and apparatus of the present disclosure. Therefore, the appended claims are intended to be interpreted as including all such alternatives, modifications, permutations, and various equivalents that fall within the true spirit and scope of the present disclosure. As used herein, the phrase "A, B, or C" should be interpreted as meaning a logic using a non-exclusive disjunction "OR" ("A OR B OR C"), and not as meaning "only one of A or B or C". Each step in a process may be an optional step and is not required. In different embodiments, one or more steps may be deleted or steps may be provided in a different order. Furthermore, in various embodiments, different steps may be provided simultaneously rather than sequentially.
Claims
1. 1. A method for selectively etching at least one feature in a silicon oxide region relative to a low oxygen content region, comprising: providing an etching gas comprising a fluorocarbon gas and at least one of a metalloid halide gas or a metal halide gas; generating plasma from the etching gas; selectively etching the at least one feature in the silicon oxide region relative to the oxygen-lowered region and simultaneously forming a semi-metal or metal-containing hard mask over the oxygen-lowered region; A method comprising:
2. 10. The method of claim 1, wherein the etching gas does not include hydrogen.
3. 2. The method of claim 1, wherein the fluorocarbon gas is C x F y A method comprising:
4. 2. The method of claim 1, wherein the fluorocarbon gas is C 4 F 6 , c-C 4 F 8 , c-C 5 F 8 , C 2 F 4 , C.F. 4 , C 4 F 8 , C 3 F 8 , and C 2 F 6 The method includes at least one of the following:
5. 2. The method of claim 1, wherein the etching gas is O 2 , O 3 , CO 2 , CO, NO, NO 2 , N 2 O, S.O. 2 , S.O. 3and COS.
6. 2. The method of claim 1, wherein the etching gas further comprises an inert gas from the group consisting of nitrogen, helium, argon, krypton, xenon, and neon.
7. 10. The method of claim 1, further comprising providing a selective pre-etch prior to providing the etching gas, wherein the selective pre-etch selectively and partially etches the at least one feature in the silicon oxide region relative to the low oxygen content region without forming a semi-metal or metal-containing hard mask.
8. 2. The method of claim 1, wherein the metalloid halide gas or metal halide gas is WF 6 and MoF 6 The method includes at least one of the following gases:
9. 2. The method of claim 1, wherein the metalloid halide gas or metal halide gas comprises at least one of silicon (Si), germanium (Ge), tin (Sn), titanium (Ti), zirconium (Zr), hafnium (Hf), vanadium (V), niobium (Nb), tantalum (Ta), boron (B), aluminum (Al), gallium (Ga), indium (In), iron (Fe), ruthenium (Ru), rhenium (Re), antimony (Sb), tungsten (W), molybdenum (Mo), or bismuth (Bi).
10. 10. The method of claim 1, wherein the plasma is formed at a pressure between 1 and 500 millitorr and a power between 20 and 1000 watts.
11. 2. The method of claim 1, further comprising providing an atomic layer etch of the at least one feature in the silicon oxide region after selectively etching the at least one feature in the silicon oxide region relative to the low oxygen content region, the atomic layer etch using the semi-metal or metal containing hard mask to reduce etching of the low oxygen content region.
12. 10. The method of claim 1, wherein the at least one feature has a width less than 15 nm and a depth-to-width aspect ratio of at least 6:
1.
13. 10. The method of claim 1, further comprising providing an additional etch of the at least one feature in the silicon oxide region after selectively etching the at least one feature in the silicon oxide region relative to the low oxygen content region, the additional etch using a semi-metal or metal-containing hardmask as a mask and without further depositing the semi-metal or metal-containing hardmask.
14. 14. The method of claim 13, further comprising removing the semi-metal or metal-containing hardmask after the additional etching of the at least one feature.
15. 15. The method of claim 14, wherein removing the metalloid or metal-containing hardmask comprises a wet clean.
16. 10. The method of claim 1, further comprising providing a temperature of less than or equal to 300°C.
Citation Information
Patent Citations
Method of manufacturing semiconductor device
JP2010098101A
Plasma etch chemistries for high aspect ratio features in dielectrics
JP2021515988A
Selective ETCH using deposition of a metalloid or metal containing hardmask
WO2021207286A1