Granular epoxy resin composition
The granular epoxy resin composition with an anionic polymer addresses issues of fluidity and swelling in compression molding, enhancing filling performance and reliability of semiconductor devices.
Patent Information
- Application Number
- JP2024529220
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2021-12-29
- Filing Date
- 2022-11-07
- Publication Date
- 2024-11-27
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Conventional epoxy resin compositions face challenges in ensuring fluidity, fine gap filling properties, and swelling/leakage prevention suitable for compression molding, which affect the reliability and productivity of semiconductor devices.
A granular epoxy resin composition comprising an epoxy resin, a curing agent, a filler, and an anionic polymer with a carboxylic acid functional group, which enhances fluidity, moldability, and swelling prevention during compression molding.
The composition improves filling performance, minimizes equipment errors, and enhances the reliability of semiconductor devices by preventing swelling and leakage, while maintaining excellent fine gap filling characteristics.
Smart Images

Figure 2024544046000001 
Figure 2024544046000002 
Figure 2024544046000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a granular epoxy resin composition and a semiconductor device encapsulated with the same. [Background technology]
[0002] Epoxy molding compounds (EMC) are used as materials for protecting and encapsulating various types of semiconductor elements, such as integrated circuits (ICs), large scale integrated circuits (LSIs), transistors, and diodes, to improve the characteristics and reliability of semiconductor devices.
[0003] Recently, with the trend toward smaller, lighter, and more powerful electronic devices, the integration of semiconductors has accelerated, and research into improving the performance of materials used to encapsulate semiconductor elements has been ongoing in many ways. In particular, as the size of wafer chips in semiconductor elements increases and the thickness of semiconductor elements decreases, the thickness of the encapsulant on the semiconductor elements and the amount of encapsulant used per element are gradually decreasing. The thickness of the encapsulant on a semiconductor element refers to the thickness of the encapsulant encapsulating the surface of the semiconductor element opposite to the lead frame or circuit board mounting surface, and in the case of mounting one or more semiconductor elements on a lead frame or circuit board, it refers to the thickness of the encapsulant encapsulating the surface of the topmost semiconductor element opposite to the lead frame or circuit board mounting surface.
[0004] The encapsulation method for semiconductor devices has mainly been transfer molding, which uses tablets made by compressing a solid epoxy resin composition into a cylindrical shape. However, due to the recent technological development of semiconductor miniaturization and integration, and the increasing market demand for cost reduction, compression molding has been widely adopted.
[0005] However, conventional epoxy resin compositions have problems in that they are difficult to secure the fluidity, fine gap filling properties, and swelling / leakage prevention properties suitable for compression molding. Therefore, there is a need to develop a granular resin composition for encapsulating semiconductor devices that has workability and moldability suitable for compression molding. Summary of the Invention [Problem to be solved by the invention]
[0006] The present invention provides a granular epoxy resin composition having excellent flowability and filling properties when encapsulating a semiconductor device, excellent moldability of EMC, and improved swelling prevention properties during molding.
[0007] The present invention also provides a semiconductor device encapsulated with the granular epoxy resin composition. [Means for solving the problem]
[0008] The present invention provides a granular epoxy resin composition comprising an epoxy resin, a curing agent, a filler and an anionic polymer. Effect of the Invention
[0009] The granular epoxy resin composition of the present invention contains an anionic polymer having a carboxylic acid functional group, and prevents swelling during compression molding performed at high temperatures. As a result, it is possible to improve filling properties while minimizing the occurrence of equipment errors caused by leakage of the molten epoxy resin composition to the outside of the substrate and mold.
[0010] In addition, the granular epoxy resin composition of the present invention can provide high reliability when applied to thin film semiconductor devices, integrated semiconductor devices, etc. by improving fine gap filling properties.
[0011] [Best Mode for Carrying Out the Invention] The present invention will be described in detail below. However, the present invention is not limited to the following content, and each component may be modified or mixed in various ways as necessary. Therefore, it should be understood that the present invention includes all modifications, equivalents, and alternatives within the spirit and technical scope of the present invention.
[0012] [Granular epoxy resin composition] The granular epoxy resin composition according to the present invention contains an epoxy resin, a curing agent, a filler and an anionic polymer, and may further contain one or more additives that are commonly used in the art, such as a curing catalyst, a coupling agent, a colorant, a release agent, a modifier, a flame retardant, a stress reducing agent, an antifoaming agent, etc., in order to add functions to the composition as required within the range that does not impair the physical properties of the composition.
[0013] When compression molding is performed using an epoxy resin composition during the semiconductor device manufacturing process, swelling of the epoxy molding compound (EMC) formed by curing at high temperatures may occur, causing the molten epoxy molding compound to leak out of the mold, resulting in breakdown of the compression molding machine. In addition, a process of removing the leaked epoxy molding compound is required, which may reduce productivity. However, the epoxy resin composition of the present invention contains an anionic polymer and exhibits excellent fluidity, moldability, filling properties, and swelling prevention properties, and as a result, when applied to compression molding, the occurrence of the above-mentioned problems can be suppressed and reduced, improving reliability.
[0014] [Epoxy resin] The granular epoxy resin composition of the present invention may contain an epoxy resin as a main resin, which, after reacting with a curing agent and curing, forms a three-dimensional network structure, thereby imparting strong and firm adhesion to an adherend and heat resistance.
[0015] The epoxy resin can be any epoxy resin commonly used in the art without any particular limitations. Non-limiting examples of epoxy resins that can be used include bisphenol A type epoxy resins, alicyclic epoxy resins, cresol novolac type epoxy resins, bisphenol F type epoxy resins, bisphenol S type epoxy resins, naphthalene type epoxy resins, anthracene epoxy resins, tetramethylbiphenyl type epoxy resins, phenol novolac type epoxy resins, bisphenol A novolac type epoxy resins, bisphenol S novolac type epoxy resins, biphenyl novolac type epoxy resins, naphthol novolac type epoxy resins, naphthol phenol co-condensed novolac type epoxy resins, naphthol cresol co-condensed novolac type epoxy resins, aromatic hydrocarbon formaldehyde resin modified phenol resin type epoxy resins, triphenylmethane type epoxy resins, tetraphenylethane type epoxy resins, dicyclopentadiene type epoxy resins, dicyclopentadiene phenol addition reaction type epoxy resins, biphenyl type epoxy resins, phenol aralkyl type epoxy resins, polyfunctional phenol resins, naphthol aralkyl type epoxy resins, and the like, and one or more of these may be included.
[0016] In addition, the epoxy resin may have a softening point of 40 to 75° C., for example, 50 to 65° C. In addition, the epoxy resin may have an epoxy equivalent weight (EEW) of 100 to 400 g / eq, for example, 180 to 350 g / eq, or another example, 250 to 300 g / eq, and a viscosity (based on 150° C.) of 0.01 to 50 poise, for example, 0.01 to 10 poise, or another example, 0.01 to 2 poise. The epoxy resin composition described above can ensure fluidity and flowability even when it contains a high content of filler, and can be easily kneaded and have improved dispersibility, thereby providing excellent moldability.
[0017] Based on the total weight of the granular epoxy resin composition of the present invention, the content of the epoxy resin may be 2 to 20% by weight, for example, 5 to 15% by weight. If the content of the epoxy resin is less than the above range, the viscosity of the composition increases, and the flowability and moldability decrease, which may cause a problem of the epoxy resin composition not being filled in the semiconductor device, resulting in a decrease in workability. On the other hand, if the content of the epoxy resin exceeds the above range, the reliability of the semiconductor may be deteriorated due to an increase in moisture absorption, and the strength of the epoxy molding compound prepared using the epoxy resin composition may be decreased due to a relative decrease in the filler content.
[0018] [Hardening agent] The granular epoxy resin composition of the present invention contains a curing agent, which reacts with the epoxy resin to promote curing of the composition.
[0019] The curing agent undergoes a curing reaction with the epoxy resin and may be a curing agent generally known in the art, and may be, for example, a phenolic compound having two or more phenolic hydroxyl groups in one molecule. Non-limiting examples of usable curing agents include phenol novolac resins, cresol novolac resins, phenol aralkyl resins, polyfunctional phenolic compounds, and the like, and the curing agent may include one or more of these.
[0020] The curing agent may have a softening point of 50 to 85° C., for example, 60 to 79° C., or another example, 64 to 75° C. The curing agent may have a hydroxyl equivalent of 150 to 300 g / eq, for example, 190 to 230 g / eq, and a viscosity (based on 150° C.) of 0.01 to 10 poise, for example, 0.01 to 2 poise.
[0021] The content of the curing agent may be 2 to 20% by weight, for example, 2 to 15% by weight, based on the total weight of the granular epoxy resin composition of the present invention. If the content of the curing agent is less than the above range, the curability and moldability may be reduced, and if it exceeds the above range, the reliability of the semiconductor may be deteriorated and the strength may be reduced due to an increase in moisture absorption.
[0022] [Filling material] The granular epoxy resin composition of the present invention contains a filler, which serves to improve the mechanical properties (e.g., strength) of the epoxy resin composition and to reduce the moisture absorption.
[0023] As the filler, inorganic fillers generally used in the field of electronic materials can be used without any particular limitation. For example, inorganic fillers such as silica, silica nitride, alumina, aluminum nitride, boron nitride, etc. can be used, and these can be used alone or in combination of two or more. The shape of the filler is not particularly limited, and both angular and spherical shapes can be used. Non-limiting examples of fillers that can be used in the present invention include natural silica, synthetic silica, fused silica, etc., and for example, spherical silica particles can be used.
[0024] The filler may include two or more fillers with different particle sizes. In this case, the moldability and workability of the epoxy resin composition can be further improved. For example, the filler may be a mixture of two fillers with different average particle sizes (D50). For example, a first filler with an average particle size (D50) of 3.0 to 20 μm, e.g., 3.0 to 15 μm, and a second filler with an average particle size (D50) of 0.1 to 3 μm, e.g., 0.1 to 2 μm, may be mixed in an appropriate ratio and used.
[0025] The content of the filler may be 50 to 95% by weight, for example, 70 to 90% by weight, based on the total weight of the granular epoxy resin composition of the present invention. If the content of the filler is less than the above range, the moisture absorption amount of the cured product increases, which may reduce the reliability of the semiconductor device, and if it exceeds the above range, the flowability decreases and the moldability becomes poor.
[0026] [Anionic polymer] The granular epoxy resin composition of the present invention may contain an anionic polymer, which imparts excellent fluidity, filling property and swelling / leakage prevention properties during compression molding of the epoxy resin composition, thereby imparting workability suitable for compression molding, and thereby improving excellent moldability and reliability as a semiconductor element encapsulant.
[0027] The anionic polymer is a polymer having a functional group or moiety exhibiting a negative charge, and the functional group or moiety may be present in the main backbone or at the end or middle of a side chain. The functional group may be one or more of a carboxyl group (-COO-), a sulfonic acid group (-SO3-), or an acetoxy group (-CH2COO-). Preferably, the functional group may include a carboxyl group.
[0028] The anionic polymer may be linear or branched with a plurality of side chains bonded to a linear main chain. As an example, the anionic polymer may have a polycarboxylic acid main chain with a carboxyl group bonded to the end or side chain of the main chain as a functional group, may include a hydrocarbon chain or an ether bond (-O-) with oxygen intervening in the hydrocarbon chain, and may be a compound containing an unsaturated C=C double bond.
[0029] The negatively charged carboxyl group contained in the anionic polymer can participate in cross-linking with the epoxy resin, and the non-polar hydrocarbon of the main skeleton in the anionic polymer can increase the compatibility with the epoxy / phenol resin. In addition, the negatively charged carboxyl group of the anionic polymer improves the dispersibility of the filler in the epoxy resin composition and prevents precipitation, resulting in excellent storage stability, which can improve the moldability, storage stability (pot life), and bleeding resistance of the epoxy resin composition.
[0030] By including the anionic polymer, the granular epoxy resin composition of the present invention can exhibit fluidity suitable for compression molding, excellent filling properties, and swelling / leakage prevention properties. In particular, the anionic polymer exhibits excellent gap filling properties, for example, excellent filling properties even at a gap pitch of 30 microns or less. As a result, a relatively thin encapsulation layer can be formed, and filling properties can be significantly improved.
[0031] In addition, the anionic polymer uniformly disperses fillers with a size of 10 microns or less and stabilizes them within the resin matrix, significantly improving workability and EMC moldability during compression molding.
[0032] As an example, the anionic polymer may include a carboxylic acid group and an ether group in the main skeleton. As another example, the anionic polymer may be represented by the following Chemical Formula 1:
[0033] [ka]
[0034] In the above formula, R 1 is a substituted or unsubstituted alkyl group having 1 to 10 carbon atoms, R2 is a hydrogen atom, a carboxylic acid, a hydroxyl group, or a substituted or unsubstituted alkyl group having 1 to 10 carbon atoms, X is oxygen or a C=C double bond; p is 1 to 20.
[0035] The anionic polymer may have an acid value of 10 to 350 mgKOH / g, for example, 25 to 320 mgKOH / g. If the acid value is outside the above range, the storage stability may be poor.
[0036] The weight average molecular weight of the anionic polymer may be 500 to 10,000 g / mol, for example, 4,000 to 6,000 g / mol. If the weight average molecular weight of the anionic polymer is less than the above range, the swelling property and spreading property are not controlled, and if it exceeds the above range, the curing property of the epoxy resin cured material is deteriorated, which may cause a deterioration in the long-term reliability of the molded product.
[0037] The content of the anionic polymer may be 0.3 to 0.8 wt%, for example, 0.4 to 0.7 wt%, based on the total weight of the granular epoxy resin composition of the present invention. If the content of the anionic polymer is less than the above range, the swelling property and spreading property may not be sufficiently controlled, and if it exceeds the above range, the storage stability and workability may be poor.
[0038] [Additives] The epoxy resin composition of the present invention may further contain additives that are generally used in such compositions. Non-limiting examples of additives that can be used include curing catalysts, coupling agents, colorants, mold release agents, etc.
[0039] The curing catalyst accelerates the curing reaction, and may be an imidazole-based compound, a naphthalene-based latent catalyst, an amine-based compound, an organometallic compound, an organophosphorus compound, a boron compound, or the like. The coupling agent is added for stable dispersion of the organic and inorganic substances, and may be an epoxy silane, an amino silane, a mercapto silane, an acrylic silane, a vinyl silane, or the like. The colorant is added to impart color to the resin composition, and may be carbon black, red iron oxide, or the like. The release agent is added to ensure releasability between the EMC and the mold, and may be paraffin wax, carnauba wax, polyethylene wax, ester wax, or the like. In addition, an anion scavenger, a defoamer, or the like may be further included.
[0040] The additives may be added within the range of the content generally known in the art. For example, each of the additives may be included in an amount of 0.01 to 5% by weight based on the total weight of the granular epoxy resin composition, but is not limited thereto.
[0041] [Semiconductor element] The present invention provides a semiconductor device encapsulated with the above-mentioned granular epoxy resin composition. The semiconductor device may be a transistor, a diode, a microprocessor, a semiconductor memory, a power semiconductor, etc. In particular, the epoxy resin composition according to the present invention is applicable to a package-stacked type POP (Package On Package) and a semiconductor chip-stacked type COC (Chip On Chip).
[0042] The method for encapsulating a semiconductor element using the granular epoxy resin composition of the present invention can be carried out by a molding method commonly used in the art, such as transfer molding, compression molding, injection molding, etc. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0043] The present invention will be described in more detail below with reference to examples. However, the following examples are provided to aid in understanding the present invention, and are not intended to limit the scope of the present invention in any way.
[0044] [Experimental Example 1-14] Each component was mixed according to the composition shown in Tables 1 and 2 below, and then the mixture was melt-mixed at a temperature of 70 to 130°C using a melt kneader. The mixture was then passed through a granulator to produce a granular epoxy resin composition for each experimental example.
[0045] [Table 1]
[0046] [Table 2]
[0047] Epoxy resin: Aralkyl type epoxy resin (softening point 57°C, EEW 280g / eq, viscosity (150°C) 0.9 Pa s) Hardener: Aralkyl phenolic resin (softening point 66°C, hydroxyl equivalent 205g / eq, viscosity (150°C) 0.8Pa·s) Filler 1: Silica 1 (D50 4.8 μm, D90 9.95 μm) Filler 2: Silica 2 (D50 2.0 μm, D90 4.0 μm) Ionic polymer 1: Anionic polymer containing carboxyl groups (Hydroxystearic acid oligomers, Mw 5,500 g / mol, acid value 32 mg KOH / g) Ionic polymer 2: Anionic polymer containing carboxyl groups (Hydroxystearic acid oligomers, Mw 2,200 g / mol, acid value 73 mg KOH / g) Ionic polymer 3: Anionic polymer containing carboxyl groups (Octadecenyl succinic acid, Mw 600 g / mol, acid value 300 mg KOH / g) Ionic polymer 4: Anionic polymer without carboxyl group (Alkylaryl sulphonate, Mw 386g / mol) Ionic polymer 5: Anionic polymer without carboxyl group (Phosphate ester, Mw 1,200g / mol, acid value 85mgKOH / g) Ionic polymer 6: Anionic polymer that does not contain carboxyl groups (fatty acid ethylene ester, acid value 17 mg KOH / g) Ionic polymer 7: Cationic polymer (Alkylamide polyol, Mw 53,000 g / mol) Ionic polymer 8: Cationic polymer (Polyoxyalkylene amine derivative, Mw 2,600 g / mol) Ionic polymer 9: Cationic polymer (Croda, Hypermer KD11, Mw 1,000-10,000 g / mol)
[0048] [Physical property evaluation] The physical properties of the epoxy resin compositions prepared in each experimental example were measured as follows, and the results are shown in Tables 3 and 4 below.
[0049] [Spiral flow] The epoxy resin compositions produced in each experimental example were molded in a spiral flow mold using a heated transfer molding machine (pressure 70 kg / cm 2 After molding at 155°C for 200 seconds, the flowability of the product was measured.
[0050] [Gelation time] A small amount of the epoxy resin composition prepared according to each experimental example was spread widely and uniformly on a gel timer, and the time required for the composition to gel was measured.
[0051] [Hardness (155℃×200sec, Shore D)] The epoxy resin compositions produced in each experimental example were molded in a heated transfer molding machine (pressure 70 kg / cm2 After molding at 155°C for 200 seconds, the hardness of the product was measured.
[0052] Swelling 2g of the epoxy resin composition prepared in each experimental example was placed in a 20ml transparent vial measuring 28mm x 61mm, and the degree of swelling was measured under reduced pressure and heating (640torr or less, 150℃, 5 minutes). The swelling change rate was determined by the following formula as the ratio of the height under reduced pressure and heating to the initial height, and the lower the change rate, the better the swelling prevention properties.
[0053] Swelling rate (%) = (H / H0-1) x 100 (H0: initial height, H: swelling height)
[0054] [Spreading] 6.05g of the epoxy resin composition prepared according to each experimental example was dispensed in the center of a 240mm x 78mm board with an area (120mm x 39mm) corresponding to 1 / 4 of the total area, and then compression molded using a compression molding machine (temperature 155℃, curing time 30 seconds) to measure the spreading area. The spreading area ratio was determined by the following formula based on the area ratio of the cured product applied to the board after compression molding, and the closer the spreading area ratio is to 100%, the better the spreading.
[0055] Spread area ratio (%) = (A / substrate area) x 100 (Board area: 240mm×78mm=18,720mm 2 A: Area of the cured material applied to the substrate after compression molding)
[0056] [Fine gap filling ability] A test substrate was manufactured by attaching semiconductor chips (chips with a gap pitch of 30 μm) to the center and each corner (7 mm away from the edge of the substrate) of a substrate measuring 240 mm x 78 mm, for a total of five portions.
[0057] 24.2g of the epoxy resin composition prepared according to each experimental example was dropped onto the prepared test board, and then it was cured for 30 seconds under a pressure of 30 tons, a temperature of 155℃, and a vacuum of 70 torr, and compression molded (molded thickness: 700um), and then five semiconductor chips were observed with a SEM (scanning electron microscopy, 200x magnification) to see if the EMC was filled correctly. If all five semiconductor chips were filled, it was judged as "good", and if even one was not filled, it was judged as "no good".
[0058] [Table 3]
[0059] [Table 4]
[0060] As can be seen from the results of Tables 3 and 4, the epoxy resin compositions of Experimental Examples 2 to 4 according to the present invention showed generally excellent physical properties in all the measured items. On the other hand, the epoxy resin compositions outside the composition of the present invention showed generally inferior physical properties. Specifically, the epoxy resin composition of Experimental Example 1, which did not contain an ionic polymer, showed poor swelling and spreading properties, the epoxy resin compositions of Experimental Examples 5 to 7, which used an anionic polymer without a carboxyl group, showed poor overall measured physical properties, and the epoxy resin compositions of Experimental Examples 8 to 10, which used a cationic polymer instead of an anionic polymer, showed poor physical properties in at least one of swelling, spreading and filling properties. On the other hand, the epoxy resin compositions of Experimental Examples 11 to 14, which used an anionic polymer according to the present invention and in a content outside the range of the present invention, also showed poor overall measured physical properties. [Industrial Applicability]
[0061] The granular epoxy resin composition of the present invention contains an anionic polymer having a carboxylic acid functional group, and prevents swelling during compression molding performed at high temperatures, thereby minimizing equipment errors caused by leakage of the molten epoxy resin composition to the outside of the substrate and mold, and improving filling properties. In addition, the granular epoxy resin composition of the present invention improves fine gap filling properties, providing high reliability when applied to thin-film semiconductor devices, integrated semiconductor devices, etc.
Claims
1. Contains an epoxy resin, a hardener, a filler and an anionic polymer, A granular epoxy resin composition, wherein the anionic polymer contains a carboxylic acid group, A granular epoxy resin composition comprising 0.3 to 0.8% by weight of the anionic polymer based on the total weight of the granular epoxy resin composition.
2. The granular epoxy resin composition according to claim 1, wherein the anionic polymer is represented by the following chemical formula 1: 【Chemistry 1】 In the above formula, R 1 is a substituted or unsubstituted alkyl group having 1 to 10 carbon atoms, R 2 is hydrogen, a hydroxy group, a carboxylic acid, or a substituted or unsubstituted alkyl group having 1 to 10 carbon atoms, X is oxygen or a C═C double bond; p is 1 to 20.
3. 2. The granular epoxy resin composition according to claim 1, wherein the anionic polymer has an acid value of 10 to 350 mg KOH / g and a weight average molecular weight of 500 to 10,000 g / mol.
4. 2. The granular epoxy resin composition according to claim 1, comprising 2 to 20% by weight of the epoxy resin, 2 to 20% by weight of the curing agent, 50 to 95% by weight of the filler, and 0.3 to 0.8% by weight of the anionic polymer, based on the total weight of the granular epoxy resin composition.
5. A semiconductor element encapsulated with the granular epoxy resin composition according to any one of claims 1 to 4.
Citation Information
Patent Citations
Epoxy resin composition and semiconductor device
JP2006274184A
Epoxy resin composition for sealing semiconductor
JP2011153196A
Epoxy resin composition for sealing semiconductor and semiconductor device using the same
JP2013107960A
Granular semiconductor-sealing resin composition and semiconductor device
JP2021024945A
Resin molding material, molded article, and method for manufacturing said molded article