Fiber-reinforced plastic composites with improved UV and gloss properties, their preparation and use
The fiber-reinforced multilayer plastic composite with a UV-protective acrylate top layer addresses the deterioration of fiber-reinforced panels by ensuring minimal yellowing and maintaining gloss and mechanical properties under prolonged exposure to UV radiation and weather.
Patent Information
- Application Number
- JP2024531418
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2021-11-24
- Filing Date
- 2022-11-24
- Publication Date
- 2024-11-28
AI Technical Summary
Fiber-reinforced plastic panels deteriorate due to UV radiation and weather conditions, leading to significant mechanical property loss, yellowing, and reduced gloss over time, making them unsuitable for long-term outdoor use.
A fiber-reinforced multilayer plastic composite with a matrix layer and a UV-protective upper layer composed of unsaturated polyester or epoxy resins, topped by an acrylate resin that cures upon UV irradiation, providing enhanced UV resistance and gloss stability.
The composite exhibits minimal yellowing and maintains high gloss and mechanical properties for decades, offering improved durability and aesthetic appeal in outdoor applications.
Smart Images

Figure 2024544174000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a fibre-reinforced multilayer plastic composite, to a process for its production and to its use.
[0002] A fiber reinforced plastic panel is a panel constructed from a composite material, which may be constructed, for example, from a reinforced polymer resin matrix with embedded fibers. Due to the fibers reinforcing the polymer matrix, fiber reinforced plastic products generally have a high specific stiffness and high mechanical strength compared to non-reinforced polymer materials.
[0003] Advantageously, the term "panel" is understood to be a planar, flat structure of reinforced polymer matrix.
[0004] Fiber-reinforced panels, especially in outdoor areas, often prove to be disadvantageous due to their unprotected exposure to environmental influences, especially UV radiation and various weather conditions. Such environmental influences gradually degrade and / or destroy the reinforced polymer matrix. As a result, both the aesthetic appearance and the mechanical properties of the fiber-reinforced panels are impaired and deteriorate significantly over time and with increasing environmental influences.
[0005] In the worst case, environmental influences can render the fiber-reinforced product completely unusable: for example, increased brittleness of the polymer matrix, a significant reduction in gloss and / or obvious yellowing are due to environmental influences, UV action and the associated aging processes of the fiber-reinforced plastic panels.
[0006] assignment It is therefore an object of the present invention to provide a plastic composite which has a higher gloss stability compared to the known fibre-reinforced plastic products according to the prior art.
[0007] Furthermore, it is an object of the present invention to provide a plastic composite which is configured to be virtually non-yellowing, i.e. which barely yellows even after prolonged use under environmental influences, and moreover advantageously does not produce any yellowing visible to the observer.
[0008] It is a further object of the present invention to provide a plastic composite which meets high quality requirements and / or has reduced defects.
[0009] It is a further object of the present invention to provide a plastic composite which is lighter than known fiber-reinforced plastic panels.
[0010] Furthermore, it is an object of the present invention to provide an optimized plastic composite which has constant mechanical properties during aging.
[0011] It is a further object of the present invention to provide a plastic composite which has improved erosion resistance compared to known fiber-reinforced plastic panels.
[0012] solution This is achieved by the fibre-reinforced multilayer plastic composite according to claim 1.
[0013] The core of the invention is a fibre-reinforced multi-layer planar plastic composite with improved UV resistance, which comprises at least one matrix layer forming a support matrix body and at least one top layer arranged on the matrix layer, the top layer being configured as a surface sealant for the matrix layer and / or as a UV protection layer for the matrix layer, the matrix layer having at least one resin from the group of unsaturated polyester resins, vinyl ester resins, epoxy resins, polyurethane resins and / or combinations thereof, the top layer having at least one acrylate-based resin, the top layer being configured to cure in depth upon UV irradiation, at least the matrix layer being configured to be fibre-reinforced, the top layer having a layer thickness in the range of 40 to 150 μm in the cured state, the plastic composite having a delta E value of <1.0 in the colour system L / a / b in the test method for 1000 h according to DIN EN ISO 4892-2-A1 and a delta E value of <1.0 in the colour system L / a / b in the test method for 1000 h according to DIN EN ISO The objective of the present invention is to provide a composite material having a Delta E value of <1.7 in the L / a / b color system in a 3000 hour test method in accordance with 4892-2-A1.
[0014] Surprisingly, it has been found that such plastic composites offer many improvements over the prior art.
[0015] For example, a top layer with at least one unsaturated aliphatic resin based on acrylates protects the matrix layer located below it from UV damage and weathering. It has also been found to be advantageous that such resins can be crosslinked in a short time by UV irradiation, which prevents unevenness of the top layer.
[0016] Furthermore, it has surprisingly been found that the layer thickness of the top layer having the acrylate-based material composition described herein can have a significantly reduced thickness while still providing adequate protection for the underlying matrix material.
[0017] Furthermore, the plastic composites described herein achieve a significant reduction in overall weight compared to fiber-reinforced panels known from the prior art. For example, the plastic composites described herein can be used to fabricate panels of 1 m2 in area. 2 Weight reductions of up to 100 g can advantageously be achieved. As a result, the plastic composites described herein are advantageously particularly suitable for use in the architectural sector for lightweight construction, building facades, transport equipment for lorry superstructures or leisure vehicles in the caravan sector.
[0018] By aliphatic resin, it is preferably understood that the resin does not have an aromatic backbone.This is advantageous because the resin can be crosslinked by UV irradiation, without destroying the backbone.It has surprisingly been found that this works particularly well with unsaturated aliphatic resins based on acrylates.
[0019] Advantageously, "acrylate-based resin" can be understood to mean any type of acrylic and / or acrylate resin.
[0020] Advantageously, it has been found that the top layer of the finished end product has a particularly high color stability and also a particularly high gloss stability, which means that the entire plastic composite, as a fiber-reinforced plastic composite, has a significantly improved UV resistance, especially in the visible aspect, and also weather resistance. Advantageously, the material of the matrix layer selected from the group of unsaturated polyester resins, vinyl ester resins, epoxy resins, polyurethane resins and / or combinations thereof is understood to be the base layer material of the matrix layer.
[0021] The matrix material is preferably selected so that it has sufficient flexibility in the cured state. In this case, resins with a breaking elongation in the range of 1.0-3.0% (DIN EN ISO 527-4 / 2 / 2), more preferably 1.0%, 1.1%, 1.2%, 1.3%, 1.4%, 1.5%, 1.6%, 1.7%, 1.8%, 1.9%, 2.0%, 2.1%, 2.2%, 2.3%, 2.4%, 2.5%, 2.6%, 2.7%, 2.8%, 2.9% or 3.0%, have proven suitable. Values in between are also considered to be disclosed. The breaking elongations disclosed herein have proven to be advantageous in that they provide a material that is particularly easy to process. A low breaking elongation increases the risk of damage due to crack formation. A high breaking elongation leads to an overall less rigid material, which has proven to be clearly disadvantageous for the processing of the resulting plastic composite. The resulting plastic composite is then usually further processed by various pressing methods to obtain the sandwich element. Materials with low stiffness tend to lead to internal sandwich structure traces, and often also to unevenness and wavy surfaces.
[0022] In addition to the elongation at break of the resin, the deflection temperature under load provided is equally important. If this deflection temperature is selected too low, it may lead to thermal deformation of the plastic composite when using dark materials which require a relatively high thermal load. In particular, resins with a deflection temperature under load according to ISO 75 method A of at least 60°C have therefore proven to be suitable. Resins with a deflection temperature under load according to ISO 75 method A of 70 to 90°C, more advantageously 70°C, 71°C, 72°C, 73°C, 74°C, 75°C, 76°C, 77°C, 78°C, 79°C, 80°C, 81°C, 82°C, 83°C, 84°C, 85°C, 86°C, 87°C, 88°C, 89°C or 90°C have proven to be particularly suitable. All such ranges are considered to be disclosed as well. In particular, this deflection temperature value determined according to ISO 75 method A is advantageous for forming plastic composites which are easy to process and have a stable shape. Particularly advantageously, the matrix material is selected from the group of polyester resins, vinyl ester resins, epoxy resins, polyurethane resins and / or combinations thereof.
[0023] The present invention has created for the first time a comprehensive system of plastic composites made of fiber-reinforced plastics in virtually any color choice and with maximum UV stability that significantly minimizes or completely prevents yellowing even over the years.
[0024] The UV resistance of the top layer and / or the plastic composite and / or the matrix layer can be evaluated by the characteristics of the color change in the Delta E value in the color system L / a / b and / or by the gloss reduction.
[0025] Furthermore, it has been found to be advantageous for the plastic composites described herein to have a delta E value in the 1000-h Xeno test according to DIN EN ISO 4892-2-A1, also called accelerated weathering according to DIN EN ISO 4892-2-A1, of <1.0 in the color system L / a / b, and a delta E value in the 3000-h Xeno test according to DIN EN ISO 4892-2-A1, also called accelerated weathering according to DIN EN ISO 4892-2-A1, of <1.7 in the color system L / a / b. It should be noted that in this test, a delta E value of ≧3 results in a discoloration that is subjectively perceived by the observer. Thus, yellowing that is perceived as unpleasant by the observer can be eliminated even after decades. It should be noted here that yellowing is understood to be a significant difference in color that the user finds unpleasant and unattractive. Advantageously, delta E is understood to be a discoloration that is also called color difference.
[0026] These data were determined using a Konica Minolta spectrophotometer CM-2600d (light type D65, SCE, 10°) and the color values were determined to be L=44, a=-1.35, b=-2.35, with advantageous tolerances of L=±1.5, a=±0.7, b=±1.0.
[0027] It has further proved to be advantageous if the top layer has a layer thickness in the cured state in the range of 40-150 μm. At the same time, it has been found that the top layer described herein can be produced without defects, despite the above-mentioned small layer thickness. In particular, the resulting cured top layer is free of oil spots, thick spots, wrinkles, under-curing, dulling effects, etc.
[0028] It is now possible for the first time to produce such an upper layer in the layer thicknesses mentioned here in a continuous process over a length of 180 m without defects.
[0029] Due to the extremely low layer thickness, the plastic composite products produced can have a higher glass content at the same thickness and therefore also have better mechanical properties than previously possible from the prior art. It is also conceivable that the reduced layer thickness will result in a reduction in weight.
[0030] Further advantageous embodiments are set forth in the following dependent claims.
[0031] In a further advantageous embodiment, it has been found to be advantageous for the top layer to have at least one deep-curing UV initiator. This has been found to be advantageous because, upon exposure to UV radiation, the crosslinking process is not initiated at the very surface of the material, but in the volume present below. As a result, it is now feasible for the first time to avoid complete curing, particularly at the exposed surfaces directly irradiated by UV radiation. It has also been found to be advantageous if the UV initiator is susceptible to oxygen inhibition, since this slows down the reaction. In particular, the radicals formed are combined by the radical nature of atmospheric oxygen before they can initiate polymerization. The slow reaction at the boundary layer allows chemical crosslinking between the top layer and the matrix layer, advantageously resulting in a permanent bond between the matrix layer and the top layer. The plastic composites described herein have very good bonding properties between the top layer and the matrix layer. No loss of adhesion, for example in the form of peeling or cracking, is observed.
[0032] The UV initiator is necessary to start the radical polymerization upon exposure to UV radiation. It should be noted here that no crosslinking occurs without UV exposure. This has proven to be particularly advantageous when storing and providing the top material, since it can be used for long periods of time despite being mixed. As a result, a particularly long pot life is obtained, from several days to several months, advantageously up to 12 months, under UV exclusion. "Pot life" is generally understood to be the period during which two or more reactive components, such as a resin and a hardener, remain usable after mixing. The top layer is configured for deep curing.
[0033] In a further advantageous embodiment, it has proven to be advantageous for the deep-curing UV initiator to have at least one phosphine oxide group. In this case, in particular, phosphine oxides, such as diphenyl(2,4,6-trimethylbenzoyl)phosphine oxide (Omnirad TPO), ethyl(2,4,6-trimethylbenzoyl)phenylphosphinate (Omnirad TPO-L) or phenylbis(2,4,6-trimethylbenzoyl)phosphine oxide (Omnirad 819), have proven to be advantageous. The phosphine oxide groups can be cured and crosslinked by irradiation with long-wave UV radiation. At the free top surface, where the UV radiation is introduced, the formed radicals are combined with atmospheric oxygen. The progress of crosslinking is inhibited. Away from the free top surface, i.e. in the upper layer volume below it, crosslinking can proceed significantly better. Thus, the phosphine oxide groups introduced here in the upper layer can achieve deep curing.
[0034] Furthermore, it has been found that deep-curing UV initiators, advantageously selected from the abovementioned phosphine oxide groups, are advantageous when the top layer has at least one further additive, such as a color pigment. Due to the long-wave excitation of the UV initiators disclosed herein, the UV radiation introduced into the top layer is not absorbed by the color pigment exactly and is therefore fully available for the polymerization of the top layer. This makes it possible for the first time to crosslink and cure the colored top layer with high quality.
[0035] TPO-L has proven to be a particularly advantageous UV initiator since the composition can already be supplied in liquid aggregate form. The other two compositions, Omnirad 819 and Omnirad TPO, exist in solid aggregate form and must first be converted to a liquid aggregate form before use.
[0036] The applied top layer is then irradiated with at least one UV radiation source, resulting in the formation of a curing gradient: at the top layer surface, where the UV radiation hits directly, the crosslinking conversion is low, whereas the crosslinking conversion increases in the direction of the layer thickness, i.e. the deeper regions of the top layer experience a significantly higher conversion during crosslinking.
[0037] In addition, deep curing has the advantage that the top layer remains flat during the manufacturing process. For example, if deep curing is not sufficient, the top layer will rise during the manufacturing process, but the wavy or ridged top layer cannot be used, so production must be stopped. For example, when the initiator is methyl benzoyl formate or 1-hydroxycyclohexyl phenyl ketone, or when acetophenone or benzophenone is used, insufficient deep curing is observed, resulting in an unusable top layer.
[0038] In a further advantageous embodiment, the acrylate-based resin of the top layer can be a urethane acrylate resin. This can be referred to as the base layer material of the top layer. This base layer material has an aliphatic backbone with a large number of carbamate groups. This backbone further has at least one methacrylate group and / or one acrylate group as free end groups. Crosslinking is carried out by this group. As a result of crosslinking, a urethane acrylate network is formed, in which the individual oligomers interact with the aliphatic backbone, the carbamate group and at least one crosslinking group located on this backbone. The stability of this network is maintained by the crosslinkable acrylate and / or methacrylate groups of the oligomers. The carbamate groups of one oligomer can be reversibly bonded with other carbamate groups of other oligomers by hydrogen bridge bonds. This combination ensures that the top layer still has sufficient flexibility after crosslinking to prevent cracking and breaking.
[0039] More preferably, the at least one acrylate resin is configured to be photoinitiated, so that crosslinking occurs by radical polymerization upon UV irradiation. This has the further advantage that crosslinking can proceed in very short time intervals, while at the same time achieving a homogeneous surface and overall structure of the top layer. The top layer, which is deep-cured by UV irradiation, is irradiated with UV radiation in the wavelength range of 250-500 nm in a time interval of 3-30 seconds, more preferably 5-15 seconds, even more preferably 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15 seconds. Advantageously, for this purpose, a UV radiation of 400 mJ / cm 2 , for example, is used. 2 Metal-doped radiation sources such as gallium-doped or iron-doped mercury lamps that emit a dose of ±10% can be used. This very short time interval is sufficient to form a deep-cured crosslink of the top layer. This allows for particularly fast crosslinking, which means a particularly high degree of time savings for the entire production process. The time savings translate into reduced costs and a higher market success rate.
[0040] In a further advantageous embodiment, the material of the top layer may be mixed with further reactive monomers. Such monomers may be 1,6-hexanediol diacrylate (HDDA) and / or trimethylolpropane triacrylate (TMPTA). By adding reactive monomers to the acrylate-based resin, the properties of the top layer can be targeted to change, in particular those related to its flexibility. For example, the flexibility of the top layer in the cured state can be increased by adding 1,6-hexanediol diacrylate (HDDA) and / or trimethylolpropane triacrylate (TMPTA). This makes the top layer less susceptible to deep scratches and damage. 1,6-hexanediol diacrylate (HDDA) and / or trimethylolpropane triacrylate (TMPTA) can be understood as reactive solvents.
[0041] In a further advantageous embodiment, the matrix layer can have at least one type of fiber as reinforcement. The selected reinforcement, and therefore the type of fiber, advantageously depends on the intended use of the plastic composite to be produced. For example, carbon fibers, glass fibers, polymer fibers, basalt fibers and / or combinations thereof are possible. In addition, natural fibers, such as flax fibers, can also be used. The fibers introduced into the matrix layer serve to strengthen the matrix layer against external forces, for example, due to the operation of leisure or commercial vehicles, due to shock loads at campsites or road traffic, or even due to torsional forces due to weather phenomena such as hail or strong winds.
[0042] The fibers may be embedded in the matrix layer, for example, as chopped glass fibers, chopped glass mats, glass roving cloth, multiaxial woven fabrics and / or combinations thereof. Due to their ease of processing and high reinforcing properties, glass fibers in particular have proven to be particularly advantageous as reinforcing materials.
[0043] It is particularly advantageous if the reinforcement introduced is a textile semi-finished product, which may be, for example, chopped glass mat, glass roving cloth, multiaxial woven fabric and / or a combination thereof.
[0044] In the production of the plastic composites described herein, for example, chopped glass mat is used as a reinforcing material, which can be continuously unwound during the production process and initially placed from above on the liquid matrix layer material. Capillary forces allow the still liquid matrix layer to fully wet the chopped glass mat and / or the still liquid matrix layer to soak into the chopped glass mat. Optionally, an additional soaking aid can be provided to facilitate and improve the impregnation. The chopped glass mat is incorporated into the still liquid matrix layer.
[0045] Depending on the intended use of the finished plastic composite, it is also conceivable that several identical and / or several different fiber reinforcements are embedded in the matrix layer, for example several chopped glass mats, several multiaxial woven fabrics and / or several glass roving cloths, so that the reinforcing effect of each reinforcement can be tailored.
[0046] Of course, it is also conceivable to introduce several chopped glass mats into the matrix layer that has not yet hardened. The chopped glass mats are preferably applied one after the other from above with a time lag. The time lag application of several chopped glass mats has the advantage that the still liquid resin remains in layers and can be impregnated one after the other by capillary forces.
[0047] The random arrangement of the glass fibers in the length and width of the chopped glass mat results in an open structure, which is advantageous in order to allow the chopped glass mat to be soaked in the still liquid matrix layer material. If the structure were too dense, air would be trapped in the layer structure. The very open structure of the chopped glass mat used here supports the soaking and avoids the formation of pores due to trapped air. The chopped glass mat is applied from above to the already applied matrix layer material, which is still liquid, so that the chopped glass mat can be soaked in the liquid matrix material.
[0048] On the other hand, if a chopped glass mat four times thicker than a normal chopped glass mat is applied from above onto a matrix layer that is still liquid, the still liquid resin of the matrix layer will be displaced, destroying the layer and rendering it completely unusable.
[0049] It has proved to be particularly advantageous if the chopped glass mat used here is provided as a continuous mat. In that case, the mat has long, preferably continuous, fibers that are randomly deposited lengthwise and crosswise across the mat. As a result, an open structure results. This structure is advantageous in order to enable the chopped glass mat to be immersed in the still liquid matrix layer material. If the structure were too dense, air would be entrapped in the layer structure. The very open structure of the chopped glass mat used here supports the impregnation and avoids the formation of pores due to entrapment of air.
[0050] Advantageously, the finished plastic composite contains between 15 and 70% by weight of the cured plastic composite, i.e. 15%, 16%, 17%, 18%, 19%, 20%, 21%, 22%, 23%, 24%, 25%, 26%, 27%, 28%, 29%, 30%, 31%, 32%, 33%, 34%, 35%, 36%, 37%, 38%, 39%, 40%, 41%, 42%, 43%, 44%, 45%, 46%, 47%, 48%, 49%, 50%, 51%, 52%, 53%, 54%, 55%, 56%, 57%, 58%, 59%, 60%, 61%, 62%, 63%, 64%, 65%, 66%, 67%, 68%, 69%, 70%, 71%, 72%, 73%, 74%, 75%, 76%, 77%, 78%, 79%, 80%, 81%, 82%, 83%, 84%, 85%, 86%, 87%, 88%, 89%, 90%, 91%, 92%, 93%, 94%, 95%, 96%, 97%, 98%, 99%, 100%, 101%, 102%, 103%, 104%, 105%, 106%, 107%, 108%, 109%, 109%. The glass percentages are 1%, 42%, 43%, 44%, 45%, 46%, 47%, 48%, 49%, 50%, 51%, 52%, 53%, 54%, 55%, 56%, 57%, 58%, 59%, 60%, 61%, 62%, 63%, 64%, 65%, 66%, 67%, 68%, 69% and 70% by weight, all values being based on the total weight of the cured plastic composite. The amounts are based on the amount of the cured plastic composite, with values therebetween being disclosed, and even more advantageously, the cured plastic composite may be present in an amount of from 15 to 65% by weight based on the total weight of the cured plastic composite, thus 15%, 16%, 17%, 18%, 19%, 20%, 21%, 22%, 23%, 24%, 25%, 26%, 27%, 28%, 29%, 30%, 31%, 32%, 33%, 34%, 35%, 36%, 37%, The glass percentages are 38%, 39%, 40%, 41%, 42%, 43%, 44%, 45%, 46%, 47%, 48%, 49%, 50%, 51%, 52%, 53%, 54%, 55%, 56%, 57%, 58%, 59%, 60%, 61%, 62%, 63%, 64%, and 65% by weight, all values based on the total weight of the cured plastic composite. Values in between are also disclosed. This ensures sufficient reinforcement of the matrix layer while retaining adequate flexibility. This is necessary especially during finishing, because otherwise the cut ends would crack when cutting the continuous plastic composite.
[0051] When the matrix material hardens, the fibers arranged therein are accordingly fixed. This fixes the entire structure of the matrix material. Deformation processing is no longer possible. In particular, by fixing the fibers in the matrix layer, fiber reinforcement is achieved in such a way that mechanical stresses are transferred to the fibers, so that a high specific stiffness and a high mechanical strength (which can also be understood as high mechanical strength) of the resulting plastic composite can be achieved.
[0052] A chopped glass mat with fibres having a fineness of 12 to 30 tex has proven to be particularly advantageous, as with this fibre fineness a high surface flatness of the matrix layer can be achieved.
[0053] In a further advantageous embodiment, at least one separating layer may be arranged between the top layer and the matrix layer. This at least one separating layer may be configured, for example, as a glass nonwoven. This separating layer serves to create a separation between the top layer and the fibers of the matrix layer. On the one hand, this prevents the fibers from damaging the top layer, which is only hardened in depth, during the manufacturing process and causing serious defects.
[0054] Furthermore, the fibres embedded in the matrix layer form structures at the interface with the upper layer, known as fibre marks. These fibre marks are visible through the upper layer in the finished plastic composite. These fibre marks are highly undesirable, particularly when the plastic composite is used in the caravan sector. Due to the high quality demands imposed on the wall elements of caravans and / or campervans, visible fibre marks represent a quality reduction or defect. If the glass nonwoven has a thickness preferably in the range of 150-250 μm, the fibre marks visible through the upper layer are covered and their optical visibility is significantly reduced. The glass nonwoven has a thickness preferably in the range of 15-35 gr / m 2 It should be understood that the above glass percentages in the finished plastic composite are the total glass percentages, which include the glass percentages of one or more glass nonwovens.
[0055] Therefore, at least one separation layer is used to create optical isolation between the fibers in the upper layer and the matrix layer. At the same time, the fiber trace is covered, so that the fiber trace is reduced. Therefore, the plastic composite described herein has at least one separation layer that reduces the fiber trace when used as a mobile home wall element and / or a camper wall element.
[0056] In a further advantageous embodiment, the matrix layer is composed of unsaturated polyester resin and / or vinyl ester resin, both of which have unsaturated groups. To initiate the radical polymerization of the unsaturated groups, the matrix material advantageously has at least one organic peroxide that decomposes when exposed to temperature. Furthermore, a crosslinking agent that causes crosslinking of the respective resin can also be contained in the matrix material. As an example of such a crosslinking agent, styrene can be used.
[0057] In addition to functioning as a crosslinker, styrene also acts as a solvent for the respective resins, and can form covalent bonds with the overlying unsaturated aliphatic resins, for example when unsaturated polyester and / or vinyl ester resins are used.
[0058] In further exemplary embodiments of the present invention, the matrix material may be an epoxy resin and / or a polyurethane resin. Neither resin has unsaturated groups. When using this type of resin, a polyaddition must be initiated as a polymerization reaction. In this case, any type of molecule with a reactive oxygen can be used to crosslink the resin. This includes, for example, amines, acids, acid anhydrides, alcohols and / or thiols, and combinations thereof. When an epoxy resin and / or a polyurethane resin is used as the matrix material, the matrix material forms a non-covalent bond with the top layer. This occurs because both resin materials of the two layers are at least partially dissolved at the interface, resulting in a non-covalent interaction between the top layer and the matrix layer.
[0059] In a further advantageous embodiment, the top layer and / or the matrix layer may comprise at least one further additive, which may advantageously be selected from the group of color additives, effect pigments, UV initiators, UV stabilizers, radical scavengers and / or combinations thereof.
[0060] In one embodiment example, it has been found to be advantageous if both the matrix layer and the top layer each have at least one coloring additive. For example, it is conceivable that the top layer and the matrix layer each have at least one coloring pigment or pigment mixture. Advantageously, the top layer and the matrix layer have the same coloring pigment. Of course, this should not be understood as limiting, so it is also conceivable that a pigment mixture can be used. In this example, the same pigment mixture can be added to the top layer and the matrix layer. This overall coloring of the plastic composite makes possible external damage to the top layer, such as scratches, substantially less noticeable.
[0061] As a result, minor damages to the plastic composite can be compensated for in an optically superior manner by at least one color pigment in the top layer and in the matrix layer or at least one pigment mixture in the top layer and in the matrix layer. Advantageously, the finished plastic composite, i.e. its two layers, are colored throughout with the same color pigment or pigment mixture.
[0062] Depending on the application of the plastic composite, titanium dioxide, for example, exhibits a particularly good white coloring effect, which allows the layers containing titanium dioxide to be colored white. In addition to titanium dioxide, barium sulfate and zinc sulfide, for example, can also be mentioned as color pigments, which also allow the respective layers to be colored white.
[0063] Of course, this should not be understood as limiting, as it is also conceivable that one and / or both layers are colored black, for example by the addition of carbon.
[0064] It is furthermore conceivable for the matrix layer and / or the top layer to be coloured in a targeted manner by the addition of further colour pigments and / or dyes depending on the envisaged application.
[0065] In this case, it has proved to be advantageous, for example, that a blue dye can already be provided in the matrix material and / or the upper layer material provided. Mixtures of dyes and color pigments and / or of color pigments with each other are also possible. For example, by mixing titanium dioxide with carbon, a gray matrix layer and / or upper layer can be produced. The mixing ratio depends accordingly on the desired degree of gray. Another possible combination is the use of a pigment mixture which comprises at least titanium dioxide and phthalocyanine blue. Furthermore, it is also conceivable to use yellow and / or red iron oxides as pigments, either alone or in mixtures with each other or with titanium dioxide.
[0066] The coloring of both layers is understood here as exemplary, but is particularly advantageous. Depending on the application, it is also conceivable to apply different color additives to the top layer and to the matrix layer.
[0067] When color pigments are used, the color pigments are added in the range of 1 to 15 phr for each layer in the liquid state, i.e., 1 phr, 1.1 phr, 1.2 phr, 1.3 phr, 1.4 phr, 1.5 phr, 1.6 phr, 1.7 phr, 1.8 phr, 1.9 phr, 2.0 phr, 2.1 phr, 2.2 phr, 2.3 phr, 2.4 phr, 2.5 phr, 2.6 phr, 2.7 phr, 2.8 phr, 2.9 phr, 3.0 phr, 3.1 phr, 3.2 phr, 3.3 phr, 3.4 phr, 3.5 phr, 3.6 phr, 3.7 phr, 3.8 phr, 3.9phr, 4.0phr, 4.1phr, 4.2phr, 4.3phr, 4.4phr, 4.5phr, 4.6phr, 4.7phr, 4.8phr, 4.9phr, 5.0phr, 5.1phr, 5.2phr, 5.3phr, 5.4phr, 5.5phr, 5.6phr , 5.7phr, 5.8phr, 5.9phr, 6.0phr, 6.1phr, 6.2phr, 6.3phr, 6.4phr, 6.5phr, 6.6phr, 6.7phr, 6.8phr, 6.9phr, 7.0phr, 7.1phr, 7.2phr, 7.3phr, 7.4ph r, 7.5phr, 7.6phr, 7.7phr, 7.8phr, 7.9phr, 8.0phr, 8.1phr, 8.2phr, 8.3phr, 8.4phr, 8.5phr, 8.6phr, 8.7phr, 8.8phr, 8.9phr, 9.0phr, 9.1phr, 9.2p hr, 9.3phr, 9.4phr, 9.5phr, 9.6phr, 9.7phr, 9.8phr, 9.9phr, 10.0phr, 10.1phr, 10.2phr, 10.3phr, 10.4phr, 10.5phr, 10.6phr, 10.7phr, 10.8phr, 1 0.9phr, 11.0phr, 11.1phr, 11.2phr, 11.3phr, 11.4phr, 11.5phr, 11.6phr, 11.7phr, 11.8phr, 11.9phr, 12.0phr, 12.1phr, 12.2phr, 12.3phr, 12.4phr r, 12.5phr, 12.6phr, 12.7phr, 12.8phr, 12.9phr, 13.0phr, 13.1phr, 13.2phr, 13.3phr, 13.4phr, 13.5phr, 13.6phr, 13.7phr, 13.8phr, 13.9phr, 14.It has been found to be advantageous to introduce 0 phr, 14.1 phr, 14.2 phr, 14.3 phr, 14.4 phr, 14.5 phr, 14.6 phr, 14.7 phr, 14.8 phr, 14.9 phr, 15 phr, all values given above are for the respective layers in the liquid state. Values in between are also disclosed. The color pigments added to the top layer in this range provide sufficient protection against yellowing of the matrix layer. In addition, the top layer is configured to be further deep curable.
[0068] The addition of titanium dioxide to the top layer has been found to be particularly advantageous where white coloration of the plastic composite is desired. In order to ensure sufficient curing of the upper layer and to avoid wrinkling during curing, the range of 1.5 to 8 phr, more preferably 1.5 phr, 1.6 phr, 1.7 phr, 1.8 phr, 1.9 phr, 2.0 phr, 2.1 phr, 2.2 phr, 2.3 phr, 2.4 phr, 2.5 phr, 2.6 phr, 2.7 phr, 2.8 phr, 2.9 phr, 3.0 phr, 3.1 phr, 3.2 phr, 3.3 phr, 3.4 phr, 3.5 phr, 3.6 phr, 3.7 phr, 3.8 phr, 3.9 phr, 4.0 phr, 4.1 phr, 4.2 phr, 4.3 phr, 4.4 phr, 4.5 phr, 4.6 phr, 4.7 phr, 4.8 phr, 4.9 phr, 5.0 phr, 5.1 phr, 5.2 phr, 5.3 phr, 5.4 phr, 5.5 phr, 5.6 phr, 5.7 phr, 5.8 phr, 5.9 ... It has been found to be advantageous to select a titanium dioxide pigment content of 4.7phr, 4.8phr, 4.9phr, 5.0phr, 5.1phr, 5.2phr, 5.3phr, 5.4phr, 5.5phr, 5.6phr, 5.7phr, 5.8phr, 5.9phr, 6.0phr, 6.1phr, 6.2phr, 6.3phr, 6.4phr, 6.5phr, 6.6phr, 6.7phr, 6.8phr, 6.9phr, 7.0phr, 7.1phr, 7.2phr, 7.3phr, 7.4phr, 7.5phr, 7.6phr, 7.7phr, 7.8phr, 7.9phr, 8.0phr. Values in between are also disclosed. For example, if a titanium dioxide content of more than 8 phr is used, the curing of the top layer is adversely affected. A pre-curing of the top layer occurs, which leads to wrinkling of the surface, while the underlying substrate remains liquid. Titanium dioxide contents of more than 8 phr should therefore be avoided. Titanium dioxide contents below 1.5 phr are too low to produce sufficient coloration. The advantage of titanium dioxide and other color additives is that the pigments themselves and / or their absorption properties protect the underlying matrix layer and prevent its yellowing. Thus, color additives, such as color pigments, effect pigments and / or dyes, are configured as UV reflectors and / or UV filters for the underlying non-UV-resistant matrix layer.
[0069] In particularly advantageous embodiments, the plastic composites disclosed herein comprise a liquid top layer of 3 to 8 phr, more advantageously 3.0 phr, 3.1 phr, 3.2 phr, 3.3 phr, 3.4 phr, 3.5 phr, 3.6 phr, 3.7 phr, 3.8 phr, 3.9 phr, 4.0 phr, 4.1 phr, 4.2 phr, 4.3 phr, 4.4 phr, 4.5 phr, 4.6 phr, 4.7 phr, 4.8 phr, 4.9 phr, 5.0 phr, 5.1 phr, 5.2 phr, 5.3 phr, 5.4 phr, 5.5 phr, 5.6 phr, 5.7 phr, 5.8 phr, 5.9 phr, 6.0 phr It has been found that the color pigment content can be 6.1phr, 6.2phr, 6.3phr, 6.4phr, 6.5phr, 6.6phr, 6.7phr, 6.8phr, 6.9phr, 7.0phr, 7.1phr, 7.2phr, 7.3phr, 7.4phr, 7.5phr, 7.6phr, 7.7phr, 7.8phr, 7.9phr, 8.0phr, and the values in between are also disclosed, and by providing at least one deep-curing UV initiator in the upper layer as well, it has become possible for the first time to cure and crosslink the upper layer pigmented with the color pigment as desired. If a normal UV initiator, i.e. a UV initiator that is not a deep-curing UV initiator, is used, the acting UV rays are almost completely reflected by the color pigment, and no crosslinking occurs. Thus, in combination with at least one deep-cure UV initiator, high-quality curing of the pigmented top layer has been achieved for the first time.
[0070] For example, the upper layer is 3-8phr, i.e. 3.0phr, 3.1phr, 3.2phr, 3.3phr, 3.4phr, 3.5phr, 3.6phr, 3.7phr, 3.8phr, 3.9phr, 4.0phr, 4.1phr, 4.2phr, 4.3phr, 4.4phr, 4.5phr, 4.6phr, 4.7phr, 4.8phr, 4.9phr, 5.0phr, 5.1phr, 5.2phr, 5.3phr, 5.4phr, 5.5phr, 5.6phr, 5.7phr, 5.8phr, 5.9phr, 6.0phr , 6.1 phr, 6.2 phr, 6.3 phr, 6.4 phr, 6.5 phr, 6.6 phr, 6.7 phr, 6.8 phr, 6.9 phr, 7.0 phr, 7.1 phr, 7.2 phr, 7.3 phr, 7.4 phr, 7.5 phr, 7.6 phr, 7.7 phr, 7.8 phr, 7.9 phr, 8.0 phr (wherein the values in between are also deemed to be disclosed), it has further been found to be advantageous to add at least one, advantageously the same, coloring pigment to the matrix layer. The upper layer has a slight thickness and ranges from 3 to 8 phr, i.e. 3.0phr, 3.1phr, 3.2phr, 3.3phr, 3.4phr, 3.5phr, 3.6phr, 3.7phr, 3.8phr, 3.9phr, 4.0phr, 4.1phr, 4.2phr, 4.3phr, 4.4phr, 4.5phr, 4.6phr, 4.7phr, 4.8phr, 4.9phr, 5.0phr, 5.1phr, 5.2phr, 5.3phr, 5.4phr, 5.5phr. , 5.6phr, 5.7phr, 5.8phr, 5.9phr, 6.0phr, 6.1phr, 6.2phr, 6.3phr, 6.4phr, 6.5phr, 6.6phr, 6.7phr, 6.8phr, 6.9phr, 7.0phr, 7.1phr, 7.2phr, 7.3phr, 7.4phr, 7.5phr, 7.6phr, 7.7phr, 7.8phr, 7.9phr, 8.0phr in combination with a titanium dioxide content of 5.6phr, 5.7phr, 5.8phr, 5.9phr, 6.0phr, 6.1phr, 6.2phr, 6.3phr, 6.4phr, 6.5phr, 6.6phr, 6.7phr, 6.8phr, 6.9phr, 7.0phr, 7.1phr, 7.2phr, 7.3phr, 7.4phr, 7.5phr, 7.6phr, 7.7phr, 7.8phr, 7.9phr, 8.0phr, the top layer exhibits transparency, i.e. 100% hiding power is not achieved. It has therefore proved to be advantageous to correspondingly color the matrix layer as well. As a result, a plastic composite completely colored in white is obtained.This has the advantage, as already mentioned, that scratches are generally less visible, and even deep scratches are less visually noticeable.
[0071] This is also particularly important in the caravan sector, since the plastic composites used up until now yellow significantly over time, which clearly reduces and deteriorates the resale value and, naturally, the appearance.
[0072] At the same time, it has been found that a low proportion of the at least one color pigment in the top layer does not significantly affect the curing or subsequent optical effect of the top layer.
[0073] Furthermore, at least one effect pigment may also be used in the top layer and / or in the matrix layer. For example, it is conceivable to provide at least one effect pigment in the top layer, which can, for example, significantly increase its reflection, resulting in brilliant optical effects.
[0074] Examples of such effect pigments which have proven advantageous include, for example, glass particles, mica and / or layered silicate particles, which may optionally be coated with at least one or more of the following oxides: titanium dioxide, iron oxide, silicon dioxide and / or tin oxide.
[0075] It is also conceivable to select the effect pigments from aluminum, copper, brass or bronze particles and / or combinations thereof. This allows special metallic effects to be produced. Furthermore, it has also proven advantageous to use particles in the upper layer, since their scattering effect can be exploited, so that the incident UV radiation is reflected by the upper layer, more precisely by the particles introduced therein. This provides additional UV protection to the underlying matrix layer, thereby preventing it from yellowing.
[0076] Particularly advantageously, the effect pigments have an average particle size in the range of 10 to 100 μm. The particle size of the effect pigments is determined by laser granulometry d 50 The value is defined as d 50 The value indicates the average particle size of the effect pigment, where 50% of the effect pigment particles in the analyzed sample are smaller than this specified value.
[0077] Thus, advantageously, all kinds of color additives, effect pigments and dyes can be grouped together as color additives, which can be contained in the top layer and / or in the matrix layer.
[0078] Of course, the examples here should not be understood as limiting. It is also advantageous to combine effect pigments, such as mica, with color pigments, such as titanium dioxide, in a mixing ratio of 1:1, 1:2 or even 1:3, whereby an upper layer with optical effects and additional UV protection can be provided.
[0079] It is further contemplated that the top layer may have one or more UV stabilizers, UV initiators and / or one or more radical scavengers as further additives. Depending on the selection and proportion, this may further improve the UV and weather resistance of the entire plastic composite.
[0080] In further advantageous embodiments, the top layer can have a layer thickness in the cured state in the range of 50 μm, 55 μm, 60 μm, 65 μm, 70 μm, 75 μm, 80 μm, 85 μm, 90 μm, 95 μm, 100 μm, 105 μm and 110 μm, as well as all regions therebetween. A reduced layer thickness allows for less material consumption and generally faster curing. At the same time, it has been found that the top layer described herein can be produced without defects, despite the small layer thicknesses as mentioned above. In particular, the resulting cured top layer is free of oil spots, thick spots, wrinkles, undercuring, dulling effects, etc. It is now possible for the first time to produce such top layers without defects in a continuous process over a length of 180 m with the layer thicknesses mentioned herein. Due to the extremely small layer thicknesses, the plastic composite products produced can have a higher glass content at the same thickness and therefore also have better mechanical properties than previously possible from the prior art. It is also conceivable that a reduction in layer thickness will result in a reduction in weight.
[0081] It is further contemplated that the plastic composite may have a high glass content of up to 70% by weight based on the total weight of the cured plastic composite, and more preferably at least 65% by weight based on the total weight of the cured plastic composite. For example, a plastic composite having a high glass percentage of up to 70% by weight based on the total weight of the cured plastic composite produced in this manner may have a strength of about 400 N / mm 2 (DIN EN ISO 527-4 / 2 / 2) and tensile strength of approx. 23,000 N / mm 2 (DIN EN ISO 527-4 / 2 / 2).
[0082] In a further preferred embodiment, the upper layer, which is preferably constructed as a urethane acrylate, can have a maximum weight loss of 2% in the cured state compared to the liquid state. This loss is caused by reaction solvents, such as HDDA. The reaction solvents are released during curing. It is particularly advantageous that the upper layer has a very low shrinkage, because this allows material to be saved, which results in a reduction in production costs.
[0083] In a further advantageous embodiment, the top layer has a gloss retention of at least 80% after 3000 hours of Xeno test according to DIN EN ISO 4892-2-A1. This value of at least 80% is based on the original gloss value before the start of the test being taken as 100%. This test method is also called accelerated weathering test according to DIN EN ISO 4892-2-A1. Here, the gloss value is measured with a glossmeter (BYK micro-TRI-gloss) using a measuring angle of 20°. It has been found to be advantageous that the urethane acrylate used as the top layer of the plastic composite can be colored to a certain extent with colored particles, while maintaining its curability by UV radiation.
[0084] Furthermore, it has been found that these colour additives advantageously block a large portion of the UV radiation in outdoor applications, advantageously >95% of the incident radiation, to the extent that it does not reach the fibre reinforced matrix layer underneath. See Table 1, where a gallium doped mercury lamp was used as the UV radiation source. The top layers with different pigment content were placed on a Power Puck 2 radiometer and passed under the UV lamp at 120 W / cm and 10 m / min.
[0085] [Table 1]
[0086] As can be seen from Table 1, the addition of 1.5% by weight or more of a pigment, for example titanium dioxide, to the top layer relative to the complete formulation of the top layer in the cured state provides UV protection against yellowing of the underlying matrix layer. When radiation is passed through the top layer, UV radiation is no longer detectable below the top layer. The addition of only 0.75% by weight of a pigment relative to the complete formulation of the top layer in the cured state clearly reduces the UV radiation transmitted through the top layer. In the long term, this will also lead to yellowing of the underlying non-UV resistant matrix layer.
[0087] The matrix layer of the plastic composite described herein, which is constructed without UV radiation stabilizers, undergoes a visibly yellow coloration upon UV irradiation within a short time. It has been found that even UV-stabilized matrix systems tend to visibly yellow. This effect is due to the high proportion of aromatic groups in the matrix resin. This discoloration is perceived as unpleasant by the observer. The original white color turns yellow and is perceived as yellow by the observer. The so-called yellowing occurs.
[0088] The present invention has created for the first time a comprehensive system of plastic composites made of fiber-reinforced plastics with almost any color choice and maximum UV stability preventing yellowing over many years. The plastic composites are exposed to a defined dose of UV radiation for a defined period of time in the Xeno test according to DIN EN ISO 4892-2-A1, also called accelerated weathering test according to DIN EN ISO 4892-2-A1. After 3000 hours of this test according to DIN EN ISO 4892-2-A1, the top layer of the plastic composite disclosed herein has a gloss retention of at least 80%, where 80% is taken as the original gloss value of 100%.
[0089] Furthermore, it has been found that the top layer of the plastic composite described herein exhibits a gloss reduction of <10% relative to 100% original gloss in a 1000-hour Xeno test, also called accelerated weathering test according to DIN EN ISO 4892-2-A1. When the test method according to DIN EN ISO 4892-2-A1, also called accelerated weathering test according to DIN EN ISO 4892-2-A1, is carried out for 7000 hours, which corresponds to 15-20 years of outdoor exposure in a Central European climate, the top layer of the plastic composite described herein exhibits a gloss reduction of <30% relative to 100% original gloss. This means that the plastic composite described herein is configured to be particularly high quality and durable in outdoor areas. Even after 15-20 years, the gloss of the top layer is substantially retained, so that the plastic composite can continue to be used and does not have to be replaced or replaced due to cloudiness or dullness.
[0090] These data were obtained using a Konica Minolta spectrophotometer CM-2600d (illuminant type D65, measurement method SCE, observer 10°) and the measured color values can be determined as follows: L=44, a=-1.35, b=-2.35, with the tolerances advantageously being L=±1.5, a=±0.7, b=±1.0.
[0091] Particularly advantageously, the plastic composites described herein can be produced in a continuous process in widths of 1.5 m to 4 m, more advantageously 1.5 m, 1.6 m, 1.7 m, 1.8 m, 1.9 m, 2.0 m, 2.1 m, 2.2 m, 2.3 m, 2.4 m, 2.5 m, 2.6 m, 2.7 m, 2.8 m, 2.9 m, 3.0 m, 3.1 m, 3.2 m, 3.3 m, 3.4 m, 3.5 m, 3.6 m, 3.7 m, 3.8 m, 3.9 m, 4.0 m, and in lengths of up to 250 m, which length is required by the finishing treatment of the wound finished plastic composite. The production process itself is configured as a continuous process.
[0092] In a further advantageous embodiment and an advantageous alternative for the determination of the heat deflection temperature, the glass transition temperature (T g It has been found that resins having a T of at least 90°C are advantageous as matrix materials. g Resins with a glass transition temperature between 90 and 120°C, i.e. 90°C, 91°C, 92°C, 93°C, 94°C, 95°C, 96°C, 97°C, 98°C, 99°C, 100°C, 101°C, 102°C, 103°C, 104°C, 105°C, 106°C, 107°C, 108°C, 109°C, 110°C, 111°C, 112°C, 113°C, 114°C, 115°C, 116°C, 117°C, 118°C, 119°C, 120°C, have proven to be particularly suitable, all intermediate values being intended to be disclosed here. Advantageous examples of such resins are orthophthalic, isophthalic and / or terephthalic UP resins, epoxy and / or polyurethane resins, as well as mixtures thereof. In particular, these glass transition temperatures are advantageous, since this makes it possible to avoid thermal deformation due to heating in daylight. At the same time, good flatness of the plastic composite can be achieved at these temperatures.
[0093] The glass transition temperature is determined by dynamic mechanical analysis (DMA). The measurements are performed using a TA Instruments AR2000 rheometer and processed using the "Rheology Advantage" program. The measurement parameters are: free fixation length 40-44 mm, temperature gradient 0-120 °C, strain 0.1%, oscillation frequency 1 Hz, temperature gradient 3 K / min. The glass transition temperature T g is located at the maximum of the tan δ curve.
[0094] In a further advantageous embodiment, color pigments of different colors can also be used. These produce, for example, a color tone of L=90.09; a=-2.02, b=3.30, where the standard tolerances of L=±1.5, a=±0.7, b=±1.0 apply. Advantageously, this can be achieved with a pigment mixture that may have at least titanium dioxide and phthalocyanine blue. When carrying out accelerated weathering tests according to DIN EN ISO 4892-2-A1, the gloss retention after 3000 hours is determined to be at least 80% of the original gloss of 100%. Furthermore, the discoloration delta E under these conditions is determined to be <1.2.
[0095] These data were obtained using a Konica Minolta spectrophotometer CM-2600d (light type D65, measurement method SCE, observer 10°). Gloss is determined by measuring the ratio of the incident light to the light reflected from a surface using a reflectometer, taking into account the angle of specular reflection. Here, the measuring device used was a BYK-Gardner "tri-gloss" reflectometer, with a measuring angle of 20°.
[0096] The invention further relates to a method for producing a plastic composite according to claim 9.
[0097] The method comprises at least the following steps: a. applying an overlayer material to a substrate surface; b. forming the top layer material to obtain a layer on the substrate surface; c. irradiating the resulting top layer with UV radiation to deep cure the top layer; d. applying a matrix material to form a matrix layer; e. applying the fiber material to the matrix layer, whereby the fiber material is submerged in the still liquid matrix layer and / or surrounded by the still liquid matrix layer by capillary forces; f. curing the matrix layer; g. Removing the support material to obtain the final fiber-reinforced multi-layer plastic composite. has.
[0098] In the first step a), the liquid upper layer material to be cured is applied to the substrate surface. In a preferred embodiment, it has proven advantageous if the substrate surface itself is configured as a film. In particular, it has proven advantageous to use a polyethylene terephthalate (PET) film as substrate surface, onto which the upper layer material to be cured is applied. Polyethylene terephthalate is advantageous in this respect, since the upper layer material does not form a permanent adhesive bond with this film, and therefore this film can be easily removed again in a subsequent manufacturing step without destroying the upper layer.
[0099] Furthermore, it has proven advantageous if the PET film has a thickness in the range of 10-350 μm. The applied upper layer material is advantageously configured as an acrylate-based unsaturated aliphatic resin. Furthermore, additives such as, for example, color additives, UV stabilizers, UV initiators, reactivity accelerators and radical scavengers and / or combinations thereof can be added. These additives are advantageously already added to the upper layer material before application to the support surface.
[0100] Of course, the construction of the support surface as a PET film should not be understood as limiting, and other support surfaces can also be used, for example, any possible geometrical form can be considered as a support surface, and a tape-like transport surface can also be used.
[0101] In order to eliminate wrinkles in the PET film that may result from the manufacturing process or from winding the PET film, it has proven advantageous in one embodiment to subject the PET film to a pre-heat treatment before the application of the top layer material. Here, a temperature in the range of 40-80° C. has proven advantageous. This temperature is sufficient to smooth out wrinkles that may occur during the unwinding of the PET film, i.e. during the provision of the support surface. This can be done, for example, by applying uniaxial and / or biaxial tensile forces.
[0102] In the next method step b), the surface material to be cured is adjusted to the desired layer thickness. The layer structure of the plastic composite starting from the top layer makes it possible to adjust and control its properties particularly easily and targeted. The layer thickness of the top layer material to be cured is adjusted by means of a doctor blade. The layer thickness adjusted here corresponds to the layer thickness of the top layer that is to be deep cured in the next step.
[0103] It should be noted that the layer thicknesses adjusted here are selected so that the layer thickness in the deep hardened state in step c) taking into account the volumetric shrinkage is in the range of 40 to 150 μm, preferably in the range of 90 to 110 μm. Advantageously, the top layer applied here exhibits a volumetric shrinkage of only 0.5 to 4% with respect to the original volume.
[0104] In method step c), this upper layer material is now irradiated with UV radiation. For this purpose, for example, a gallium-doped UV radiation source can be used. In order to achieve a particularly effective and uniform deep curing, the UV radiation is emitted from above and hits the free surface of the upper layer. The upper layer is thus irradiated with UV radiation from the rear side with respect to the layer structure of the subsequent plastic composite. Deep crosslinking is initiated. A deeply cured upper layer is formed. This has the further advantage that the surface of the upper layer facing away from the radiation forms a continuous common interface with the support surface, which remains smooth and flat. The structure of this common interface is determined by the structure of the support surface. In the subsequent final plastic composite product, this common interface is the visible surface and is also directly exposed to weathering and UV radiation.
[0105] By irradiation of the back surface of the top layer, the curing process can be further controlled. This is realized, for example, by combination with deep-curing UV initiators consisting of phosphine oxide groups. This makes it possible for the first time to provide control of deep curing in the manufacturing process of thin layers. The free surface of the top layer, which is directly exposed to UV radiation, is only converted by 80-50%. As the layer thickness moves towards the support surface, the percentage of conversion increases. Advantageously, at the interface between the support surface and the top layer, a crosslink conversion of more than 90% can be achieved. This causes the later visible surface to harden and is stabilized by this hardening. Wrinkling in the manufacturing process can therefore be eliminated. However, the free surface remains only partially cured. This has the advantage that the top layer remains chemically reactive on the free surface.
[0106] Optionally, the temperature of the support material applied with the top layer can be controlled before and / or during and / or after the UV irradiation range. For this purpose, a temperature-controllable plate-shaped element can be arranged under the support material to manipulate the support material. The plate-shaped element is understood to be a support surface by which the support material with the top layer is manipulated. The plate-shaped element can dissipate heat from the temperature increase that may occur during UV irradiation in a fast and controlled manner. This prevents the support material from melting.
[0107] Furthermore, it is also conceivable that the support material with the liquid top layer can be subjected to a pre-heat treatment already before UV irradiation, which can have a positive effect on the flatness of the support film, so that the top layer arranged above it is prevented from wrinkling during the subsequent curing process.
[0108] This has proven to be particularly advantageous when applying the matrix layer material in the following step d). The outer surface of the top layer, on which the matrix material is applied at least partially, preferably completely, is still chemically reactive and can thus chemically interact with it. For example, it is conceivable that the top layer and the matrix layer interact with each other covalently or non-covalently. This can significantly improve the adhesion of the two layers to each other. It is also conceivable that the two layers are subsequently covalently bonded to each other by a radical polymerization reaction.
[0109] In the next method step d), a matrix material is applied to form a matrix layer. The matrix material is applied to the top layer. The layer can be adjusted, for example, in the same way as the surface layer. For example, in one embodiment, it is conceivable that the thickness of the matrix layer can be predetermined by a doctor blade.
[0110] This is followed in the next method step e) by the introduction of a reinforcing material into the matrix layer. As fiber reinforcement, woven or nonwoven fabrics, laid web nets, mats, short fibers or other fibers can be introduced. For this purpose, various types of fibers can be used, such as, for example, glass fibers, carbon fibers, basalt fibers and / or polymer fibers, such as aramid fibers, as well as combinations thereof.
[0111] In a particularly advantageous embodiment, the glass fibers have been found to be particularly advantageous, since they can be used not only as chopped fibers, but also as already textile semi-finished products, preferably as chopped glass mats, which have already been subjected to a finishing treatment. The chopped glass mats have been found to be particularly advantageous in that they provide a constant distribution of the glass fibers within one square meter. This prevents the fibers from shifting during impregnation, since they are fixed with a binder. In the case of chopped glass, shifting is inevitable. Furthermore, the existing cutting techniques provide a significantly lower precision in the distribution of the glass, which leads to a less flat surface and a less stable and reliable reinforcement. For this reason, in the plastic composites described herein, textile semi-finished products, preferably chopped glass mats, are advantageously used. Furthermore, the chopped glass mats have been found to be advantageous in that they can be introduced planarly throughout the matrix layer and are therefore distributed uniformly. This is precisely what is difficult with a random distribution of chopped fibers, since often an uneven accumulation of the chopped fibers occurs. This then has a negative effect on the quality of the matrix layer. This often leads to a high rejection rate for the product.
[0112] Advantageously, the glass fiber used is E-glass, which is used for electrical applications or for plastic reinforcement. By E-glass, advantageously, one can understand aluminium borosilicate glass that is substantially free of alkali metal oxides. Of course, this should not be understood as limiting, so that any other type of glass can be used here as reinforcement.
[0113] Thus, in a particularly advantageous embodiment of the method described herein, chopped glass mat is used for fiber reinforcement of the plastic composite. The chopped glass mat is introduced into the matrix layer that is not yet hardened. Due to capillary forces and the planar formation of the chopped glass mat, the chopped glass mat sinks into the matrix layer in a slow and controlled manner, preferably over the entire production width of the matrix layer. The chopped glass mat is, so to speak, immersed and soaked into the matrix material. This simultaneously impregnates the chopped glass mat.
[0114] This controlled feeding of the chopped glass mat into the matrix layer to be hardened and its rough formation completely avoids the inclusion of air, whereby possible entrapped air is carried upwards and out of the matrix layer by capillary forces and the rough structure of the chopped glass mat, resulting in a high-quality matrix layer which is hardened in the next step f).
[0115] Of course, the use of chopped glass fibers and / or chopped glass mat should not be understood as limiting, as for example carbon fiber mats or polymer fiber mats could be used in place of the chopped glass mat.
[0116] The curing in method step f) is preferably carried out thermally. Depending on the choice of the matrix material, in particular whether it still has unsaturated groups or not, the top layer and the matrix layer can interact with each other covalently or non-covalently, so that a composite interconnected layer structure is formed.
[0117] If the matrix material is selected from the group of unsaturated polyester resins, vinyl ester resins, epoxy resins and / or polyurethane resins and / or a combination of at least one of these, the layered composite is thermally cured. Naturally, this should not be understood as limiting, so other curing methods are also given. Depending on the subsequent use, the matrix layer in which the reinforcement is already located can have a layer thickness in the cured state ranging from 0.3 to 5 mm.
[0118] In the final step g), the support surface is removed: if it is configured, for example, as a film, this can simply be removed downwards from the plastic composite and, for example, rolled up again.
[0119] The final product can then be subjected to a finishing treatment, which is preferably designed in the form of panels.
[0120] If the plastic composite is intended for a special purpose, it is conceivable to further treat, for example, the side with the outer matrix layer. This can be, for example, to improve adhesion or to corona- and / or flame-treat to adjust the wettability and polarity of the surface. Meanwhile, the top layer remains as produced. Finally, optionally, the side of the plastic composite can be polished further. This can achieve improved installability when used as a facade construction element.
[0121] In a further advantageous embodiment, it has proven advantageous to configure the method described herein as a continuous process, which allows the production of plastic composites up to 4 m wide and which may have lengths of up to 250 m in short production times.
[0122] In a further advantageous embodiment, it has been found to be advantageous to insert at least between steps c) and d) a further step of applying at least one separating layer to the deep-cured top layer. The separating layer serves in particular to reduce fiber marks that may be formed later by fiber reinforcement of the matrix layer. The separating layer can advantageously be implemented as a glass nonwoven, which prevents significant glass fiber marks at the interface between the top layer and the matrix layer.
[0123] In a further advantageous embodiment, it has been found that at least between step e) and step f), a further carrier material is applied to cover the matrix layer. In the simplest case, this carrier material can be configured as a film, more preferably as a PET film. It is therefore conceivable that the carrier material for covering the matrix layer is the same as the carrier material for applying the top layer. This additional coating serves to improve curing and reduce defects in the entire manufacturing process.
[0124] In a further advantageous embodiment, an additional method step can be carried out between steps f) and g). This step can be carried out as a UV post-curing step of the top layer from the free back side of the support material. In this inserted method step, the top layer is post-cured. As already explained above, the top layer has only been deep-cured so far. The subsequent post-curing here, which is carried out by UV radiation, can completely cure the top layer. In particular, the common contact surface between the top layer and the matrix layer is still reactive and has not been completely cured and crosslinked. This post-curing also has the advantage that a significant reduction in the crack resistance can be achieved thereby.
[0125] It has therefore proved to be advantageous to carry out a post-curing step. It has proved to be particularly advantageous and effective if the UV radiation is applied from below. This means that the UV radiation source is arranged below the layer structure described herein. The UV radiation is thereby applied directly through the support surface to the upper layer. This has proved to be particularly advantageous, since it is not necessary to apply the UV radiation to the entire matrix layer material in which the fiber reinforcement is embedded. By applying the UV radiation in a direction from below, advantageously complete deep crosslinking and hardening of the upper layer at the interface with the matrix layer can be achieved in a particularly short time. With the abovementioned layer thicknesses, the upper layer hardens after only 3-15 seconds. This results in a time- and cost-saving production method.
[0126] The method described herein may also be understood as a method for producing a plastic composite as described above.
[0127] Furthermore, the invention relates to the use of the plastic composites according to the invention as surface elements for the interior and / or exterior of vehicles, aircraft, trains, ships, caravans, campervans, as surface elements for logistics and transport, for example for lorry superstructures, and / or as facade elements in the building industry.
[0128] This results in value retention as there is virtually no optical impairment due to yellowing of the plastic composite.
[0129] Furthermore, the present invention also relates to a plastic composite produced by the above-mentioned production method.
[0130] For the first time, it is possible to produce the plastic composites described herein over large areas in square meters. For example, it is possible for the plastic composites to form areas of at least 1 m x at least 1 m, at least 1 m x at least 1.5 m, at least 1.5 m x at least 1.5 m, at least 1 m x at least 2 m, at least 2 m x at least 2 m, at least 2 m x at least 4 m. Advantageously, the plastic composites have a planar shape. Depending on the application, the plastic composites may be configured as panel goods or even as roll goods. Thus, large areas can be covered with the plastic composites described herein without the need to cut them into pieces. This creates a particularly aesthetic appearance in use.
[0131] Moreover, it turns out that the top layer based on urethane acrylate resins does not itself initially cause an increase in the surface hardness of the plastic composite. However, the high hardness of the matrix material is more effective if the top layer has a small layer thickness. At the same time, this improves the quality. If, for example, a contaminant particle is pressed into the top layer, this particle cannot be removed to any great extent due to the small layer thickness. This means that the impression is significantly weaker. This is particularly advantageous, since the plastic composites described herein are often subsequently further processed in a pressing step. In this case, contaminant particles between the pressing surface and the plastic composite can occur more frequently. As a result, the small layer thickness allows a significant reduction in the impression of contaminants due to the applied pressing pressure. Often, a pressing pressure of 1.5 to 4 tons per square meter is used. As a result, the waste generated by pressed contaminants is significantly less.
[0132] The invention described herein advantageously exhibits high UV resistance with little to no discoloration while retaining gloss, which can be achieved in particular by the color additive in the top layer.
[0133] It has further been found to be advantageous that color additives, preferably color pigments, protect the underlying matrix layer, which is not UV stabilized and which comprises, for example, unsaturated polyester and / or epoxy resins, from UV radiation and thus prevent yellowing.
[0134] Furthermore, it has been found that the mechanical properties of the plastic composites described herein can be tuned by a factor of 15-20 by using different fiber reinforcements, resulting in a range of properties according to DIN EN ISO 527-4 / 2 / 2: - Short fiber mat: Strength approx. 60N / mm 2 |Elastic modulus approx. 6,000N / mm 2 - Textile reinforcement: strength approximately 150N / mm 2 |Elastic modulus approx. 10,000N / mm 2 - Biaxial laid web reinforcement: strength approx. 400N / mm 2 |Elastic modulus approx. 23,000N / mm 2 - Uniaxial laid web reinforcement: Strength approx. 1,000N / mm 2 |Elastic modulus approx. 45,000N / mm 2 - Uniaxial carbon fibre laid web reinforcement: strength approx. 1,300N / mm 2 |Elastic modulus approx. 110,000N / mm 2 .
[0135] Further advantages, features and configuration options are presented in the exemplary embodiments, which should be understood as being non-limiting. The term "substantially" is understood in all instances used herein where this term is used within the scope of the present invention to mean a deviation from the definition that would be given without the use of this term in the range of 1% to 20%, more preferably 1% to 10%, and even more preferably 1% to 5%.
[0136] DETAILED DESCRIPTION OF EXEMPLARY EMBODIMENTS The term "phr" is understood to be the parts by weight of the respective upper or matrix layer in a liquid state relative to 100 parts of base layer material.
[0137] 1.External side wall of caravan In the example embodiment described herein of a caravan exterior wall, the final product produced has a total thickness of 1.5mm±0.1mm and a total width of 2.8m. As the manufacturing process is arranged as a continuous process, the length of the product is variable and can be finished according to customer requirements.
[0138] First, the liquid surface material is applied to a biaxially stretched film, preferably a PET film. The layer thickness is then immediately adjusted to 110 μm ± 15 μm with a doctor blade. The PET film serves as the support material and has a thickness of 10 to 400 μm, although a thickness of 100 μm has proven to be particularly advantageous for the PET film. The PET film is stable enough to be used as a support film and is thin enough to allow passage of the UV radiation required for UV crosslinking. Advantageously, the surface material may be configured to contain at least one urethane acrylate.
[0139] The surface material applied in this example embodiment may have the following composition: 100 phr of urethane acrylate (Laromer UA9089) 0.5phr Hostaphin 3058 LIQ 0.5phr Tinuvin 1130 as UV absorber 4phr Titanium Dioxide 1.5phr TPO-L as deep curing UV initiator or 100phr Urethane Acrylate (Ebercryl IRR 1032) 0.5phr Hostaphin 3058 LIQ Tinuvin 1130 as a 0.5hr UV absorber 4phr Titanium Dioxide 1.5phr TPO-L as deep-cure UV initiator.
[0140] After the layer thickness has been adjusted, the liquid surface material applied to the support material is irradiated from above with at least one UV radiation source. In this way, UV is introduced directly through the exposed surface of the surface material layer. For this purpose, a gallium-doped mercury lamp is preferably used as the UV radiation source. This is preferably 400 mJ / cm2. 2 It has a UV exposure of ±10%.
[0141] Advantageously, the irradiation time is in the range of 3 to 30 seconds, more advantageously 5 to 15 seconds, and even more advantageously 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15 seconds.
[0142] The PET film configured as support material also serves the purpose of preventing oxygen inhibition at the interface between the film and the surface material. This allows a high crosslinking conversion of >90% to be achieved in the region of this interface. In contrast, the free surface is in contact with air and is oxygen inhibited. This results in a degree of crosslinking of 50-80%.
[0143] In the deeper layers, which are not affected by oxygen inhibition of the curing agent radicals, a degree of crosslinking of >90% is usually achieved (measured by IR-ATR; calculated by the peak area of the C-C double bond). It is worth noting in this regard that in the IR-ATR, the -1 ) is irradiated onto the sample. The radiation is absorbed at the surface depending on the covalent bonds present and then the remainder is reflected back into the instrument. Crosslinking measurements involve the absorption of double bonds. Double bonds have a wavelength of approximately 809 cm -1 This produces a unique peak where the Beer-Lambert law applies, which means that the peak area is directly proportional to the bond density.
[0144] Therefore, first the liquid sample is measured and the area under the measured peak is integrated. This area corresponds to a degree of crosslinking of 0% or 100% non-crosslinked bonds. After curing, the integration is carried out again, the area again indicating the amount of uncrosslinked bonds. The difference between the two corresponds to the degree of crosslinking achieved. In the next step, a matrix material is applied to the at least partially UV-cured exposed surface of the surface material. The layer thickness of the matrix material can be adapted to the subsequent application. In this embodiment example, a layer thickness of 1100 μm±100 μm was selected. The layer thickness is adjusted with a further doctor blade.
[0145] In the examples described herein, the matrix material has the following composition: 100phr unsaturated resin, advantageously the medium-reactive orthophthalic matrix resin Palatal P4 L21 5phr Titanium Dioxide 0.15phr 1% cobalt accelerator 1.7phr hardener, advantageously Curox I300.
[0146] As cobalt promoters, solvents with a corresponding cobalt proportion can be used, such as, for example, styrene, xylene, TXIB, 2-ethylhexan-1-ol.
[0147] In this embodiment, the reinforcing material is introduced into the matrix material to be removed. As the matrix material is still in a liquid agglomerate state, the reinforcing material is able to sink into the matrix material layer and is substantially completely, advantageously completely, surrounded by the matrix material layer, thereby simultaneously impregnating the reinforcing material. In the application given in this embodiment, chopped glass mat is typically chosen as the reinforcing material. The chopped glass mat has a density of 375 gr / m 2 As an alternative to chopped glass mat, chopped glass fibers can also be incorporated for reinforcement.
[0148] In order to reduce the fiber marks of the chopped glass fibers and / or chopped glass mat, preferably before or after the application of the matrix layer, at least one separating layer is arranged between the upper layer and the chopped glass fibers and / or chopped glass mat. The separating layer is preferably configured as a glass nonwoven. Furthermore, preferably, the glass nonwoven used here has a fiber thickness of preferably 20 g / m 2 This improves stability and prevents the individual chopped glass fibres and / or glass fibres of the mat from being pressed against the upper layer and, in the worst case scenario, protruding through the upper layer and out of the plastic composite. In addition, the interface between the upper layer and the fibres is more uniform, and the visual appearance of the fibre structure is masked and minimised.
[0149] In the example embodiments described herein, the following structure of the individual layers occurs: - upper layer - a separating layer, advantageously a glass nonwoven - Matrix layer with chopped glass mat introduced or - upper layer a matrix layer in which the separating layer is advantageously implemented as a glass nonwoven and in which a chopped glass mat is implemented.
[0150] Finally, a further support film, preferably a PET film, is preferably applied to the matrix layer. This prevents oxygen inhibition during the curing of the matrix material. The entire layer system is calendered to remove trapped air between the PET film and the resin. The matrix material is then thermally cured by heating to 100° C. for 20 minutes. The plastic composite is then cooled back down to room temperature. The plastic composite is again irradiated with UV radiation to crosslink the top layer containing urethane acrylate. This can be done, for example, at 400 mJ / cm 2 . 2This can be done with a further, preferably deep-curing UV radiation source configured as a gallium or iron-doped mercury lamp emitting a dose of ±10%. In the production process, this radiation source is arranged below the layer system, so that it first irradiates the support surface and then the upper layer. Irradiation is therefore performed from below. The irradiation time is preferably in the range of 3 to 30 seconds, more preferably 5 to 15 seconds, even more preferably 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15 seconds.
[0151] In the final step, the two carrier films that have limited the area of the plastic composite up to this point are removed. The plastic composite is then finished. The plastic composite produced in this way has a tensile strength of 70 N / mm according to DIN EN ISO 527-4 / 2 / 2. 2 and a tensile modulus according to DIN EN ISO 527-4 / 2 / 2 of 6,000 N / mm 2 It turned out to be.
[0152] In the present example embodiment described herein, the resulting plastic composite has a glass content of 20-30% by weight based on the total weight of the cured plastic composite.
[0153] The plastic composites with the two possible top layer options described herein show a significant improvement in gloss stability, are virtually free of yellowing in the test method according to DIN EN ISO 4892-2-A1 and have a coating strength of about 100 g / m2 compared to known fiber-reinforced plastic panels. 2 with a simultaneous improvement in mechanical properties. In particular, the significantly reduced yellowing and retention of gloss over decades, as determined by the Xeno test, also known as accelerated weathering test according to DIN EN ISO 4892-2-A1 (see above), is of great importance for value retention in the caravan sector: if, for example, a caravan looks as good as new after 15 years, shiny white without any dull yellowing, this significantly increases its resale value.
[0154] 2. Exterior walls of commercial vehicles In the second example embodiment described herein, the final product produced, i.e., a plastic composite, is used for the exterior sidewalls of a commercial vehicle. The plastic composite produced according to this second example embodiment has a total thickness of 1.4 mm ± 0.1 mm and a total width of 2.4 m. As the manufacturing process is configured as a continuous process, the length of the product is variable and can be finish processed according to customer requirements.
[0155] First, the liquid surface material is applied to a biaxially stretched film, preferably a PET film. The layer thickness is then immediately adjusted to 110 μm ± 15 μm with a doctor blade. The PET film serves as the support material and has a thickness of 10 to 400 μm, although a thickness of 100 μm has proven to be particularly advantageous for the PET film. The PET film is stable enough to be used as a support film and is thin enough to allow passage of the UV radiation required for UV crosslinking. Advantageously, the surface material may be configured to contain at least one urethane acrylate.
[0156] The surface material applied in this example embodiment may have the following composition: 100 phr of urethane acrylate (Laromer UA9089) 0.5phr Hostaphin 3058 LIQ 0.5phr Tinuvin 1130 (UV absorber) 4 phr Titanium Dioxide (more pigments can be added for whites or colors of shade color) 1.5phr TPO-L or 100phr Urethane Acrylate (Ebercryl IRR 1032) 0.5phr Hostaphin 3058 LIQ 0.5phr Tinuvin 1130 (UV absorber) 4 phr Titanium Dioxide (more pigments can be added for whites or colors of shade color) 1.5phr TPO-L.
[0157] After the layer thickness has been adjusted, the liquid surface material applied to the support material is irradiated from above with at least one UV radiation source. In this way, UV is introduced directly through the exposed surface of the surface material layer. For this purpose, a gallium-doped mercury lamp is preferably used as the UV radiation source. This is preferably 400 mJ / cm2. 2 The UV exposure is preferably for 3 to 30 seconds, more preferably for 5 to 15 seconds, and even more preferably for 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15 seconds.
[0158] The PET film configured as the support material is further responsible for preventing oxygen inhibition at the interface between the film and the surface material. This allows a high crosslinking conversion of >90% to be achieved in the region of this interface. In contrast, the free surface is in contact with air and is oxygen inhibited. This results in a degree of crosslinking of 50-80% at the free surface. In the deeper layers, which are not affected by oxygen inhibition of the hardener radicals, a degree of crosslinking of >90% is usually achieved (measured by IR-ATR; calculated from the peak area of the CC double bond - for measurement and evaluation see Example 1 - Caravan outer wall).
[0159] In a next step, a matrix material is applied to the exposed surface of the applied and at least partially cured top layer material. The layer thickness of the matrix material can be adapted to the subsequent application. In the example embodiments disclosed herein, the matrix layer advantageously has a layer thickness in the range of 700 μm±50 μm.
[0160] Advantageously, the matrix layer is configured to include at least one epoxy resin and has the following composition: 100phr Biresin LXR 121 26phr Biresin LXH 121-3.
[0161] The applied epoxy resin is applied to the rear side of the upper layer, which in this case is designed to be partially cured, and is removed with a doctor blade to a layer thickness of 700 μm±50 μm.
[0162] In this example embodiment, the reinforcing material is introduced into the matrix material being removed, and since the matrix material is still in a liquid aggregate state, the reinforcing material is able to sink into the matrix material layer and is substantially completely, advantageously completely, surrounded by the matrix material layer, thereby simultaneously impregnating the reinforcing material.
[0163] In the example embodiments described herein, the following structure of the individual layers occurs: - upper layer a matrix layer having - 812gr / m 2 A first biaxial glass laid web having a basis weight of - 812gr / m 2 a second biaxial glass laid web having a basis weight of
[0164] The biaxial glass laid web used is a textile semi-finished product having biaxially arranged glass roving strands.
[0165] The advantage of such biaxial glass laid webs is that a higher percentage of glass can be achieved in the resulting plastic composite while maintaining the same thickness, which allows for even further improved mechanical properties to be achieved at a lower weight. A low coefficient of thermal expansion is also achieved with the use of such biaxial glass laid webs.
[0166] Finally, a further support film, preferably a PET film, is applied to the matrix layer. This must be suitable for demolding from the matrix layer, i.e. from the epoxy resin that constitutes it in this embodiment. The entire layer system is calendered in order to remove any trapped air between the PET film and the resin. The matrix material is then thermally cured by heating to 100° C. for 30 minutes. The plastic composite is then cooled back down to room temperature. The plastic composite is again irradiated with UV radiation in order to crosslink the top layer containing urethane acrylate. This can be done, for example, at 400 mJ / cm 2 . 2 This can be achieved by means of a further, advantageously deep-curing UV radiation source configured as a gallium or iron-doped mercury lamp emitting a dose of ±10%. In the production process, this radiation source is arranged below the layer system, so that it directly irradiates the upper layers. Irradiation is therefore carried out from below. Advantageously, irradiation is carried out for 3 to 30 seconds, more advantageously for 5 to 15 seconds, even more advantageously for 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15 seconds.
[0167] In the final step, the two carrier films that have limited the area of the plastic composite up to this point are removed. The plastic composite is then finished. The plastic composite produced in this way has a tensile strength of 400 N / mm according to DIN EN ISO 527-4 / 2 / 2. 2 and a tensile modulus according to DIN EN ISO 527-4 / 2 / 2 of 23,000 N / mm 2 It has been found that the plastic composites described herein exhibit significantly improved gloss stability, virtually no yellowing, and improved mechanical properties while providing a 100 g / m2 composite panel compared to known fiber-reinforced plastic panels. 2In particular, the significantly reduced yellowing and gloss retention over decades, as determined by the test method according to DIN EN ISO 4892-2-A1, also known as the accelerated weathering test method according to DIN EN ISO 4892-2-A1 (also known as the Xeno test method), is of great importance for the preservation of the value of lorry superstructures. If, for example, a lorry superstructure still looks like new after 15 years, shiny white without any dull yellowing, this significantly increases its resale value. It also has a high resistance to erosion.
[0168] 3.Curtain wall facade panels for architectural industry In a third example embodiment described herein, the plastic composite manufactured according to this example embodiment is used, for example, as a curtain wall facade panel in the building industry. The manufactured plastic composite, i.e. the final product, has a total thickness of 5.0 mm ± 0.15 mm and a total width of about 2.4 m. The manufacturing method is further configured as a continuous method, so that the length of the product is variable and can be finished according to customer requirements.
[0169] First, the liquid surface material is applied to a biaxially stretched film, preferably a PET film. The layer thickness is then immediately adjusted to 110 μm ± 0.15 μm with a doctor blade. The PET film serves as the support material and has a thickness of 10 to 400 μm, although a thickness of 100 μm has proven to be particularly advantageous for the PET film. The PET film is stable enough to be used as a support film and is thin enough to allow passage of the UV radiation required for UV crosslinking. Advantageously, the surface material may be configured to contain at least one urethane acrylate.
[0170] The surface material applied in this example embodiment may have the following composition: 100 phr of urethane acrylate (Laromer UA9089) 0.5phr Hostaphin 3058 LIQ 0.5phr Tinuvin 1130 (UV absorber) 4 phr Titanium Dioxide (for whites or colors of shade color, further pigments can be added) 1.5phr TPO-L or 100phr Urethane Acrylate (Ebercryl IRR 1032) 0.5phr Hostaphin 3058 LIQ 0.5phr Tinuvin 1130 (UV absorber) 4 phr Titanium Dioxide (for whites or colors of shade color, further pigments can be added) 1.5phr TPO-L.
[0171] After the layer thickness has been adjusted, the liquid surface material applied to the support material is irradiated from above with at least one UV radiation source. In this way, UV is introduced directly through the exposed surface of the surface material layer. For this purpose, a gallium-doped mercury lamp is preferably used as the UV radiation source. This is preferably 400 mJ / cm2. 2 The UV exposure is preferably for 3 to 30 seconds, more preferably for 5 to 15 seconds, and even more preferably for 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15 seconds.
[0172] The PET film configured as the support material is further responsible for preventing oxygen inhibition at the interface between the film and the surface material. This allows a high crosslinking conversion of >90% to be achieved in the region of this interface. In contrast, the free surface is in contact with air and is oxygen inhibited. This results in a degree of crosslinking of 50-80% at the free surface. In the deeper layers, which are not affected by oxygen inhibition of the hardener radicals, a degree of crosslinking of >90% is usually achieved (measured by IR-ATR; calculated by the peak area of the CC double bond - for measurement and evaluation see embodiment example 1 - caravan outer wall). In the next step, a matrix material is applied to the at least partially UV-cured exposed surface of the surface material. The layer thickness of the matrix material can be adapted to the subsequent application. In this embodiment example, a layer thickness of 3700±100 μm of liquid matrix material is selected. The adjustment of the layer thickness is carried out with a further doctor blade.
[0173] In the examples described herein, the matrix material has the following composition: 100 phr of unsaturated resin, advantageously the medium-reactive orthophthalic matrix resin Palatal P4 L21 5 phr Titanium Dioxide (for whites or colors of shade color, further pigments can be added) 0.15phr 1% cobalt accelerator 1.7phr hardener (e.g. Curox I300).
[0174] In this embodiment, the reinforcement is introduced into the matrix material to be removed. The introduction of the reinforcement is performed from above. As the matrix material is still in a liquid aggregate state, the reinforcement can sink into the matrix material layer and is substantially completely, preferably completely, surrounded by the matrix material layer. This allows the reinforcement to be simultaneously impregnated. In the application given in this embodiment, chopped glass mat is usually selected as the reinforcement. As an alternative to chopped glass mat, chopped fibers can also be introduced for reinforcement.
[0175] In order to reduce the fiber marks of the chopped fibers and / or chopped glass mat, advantageously, before or after the application of the matrix layer, at least one separating layer is arranged between the upper layer and the chopped fibers and / or chopped glass mat. The separating layer is advantageously configured as a glass nonwoven. Furthermore advantageously, the glass nonwoven used here has a fiber density of advantageously 20 g / m 2 This improves stability and prevents the individual chopped glass fibres and / or glass fibres of the mat from being pressed against the upper layer and, in the worst case scenario, protruding through the upper layer and out of the plastic composite. In addition, the interface between the upper layer and the fibres is more uniform and the fibre structure is visually masked.
[0176] In the example embodiments described herein, the following structure of the individual layers occurs: - upper layer - 20g / m 2 A glass nonwoven fabric having a basis weight of - a matrix layer having: - Weight 375gr / m 2 The first chopped glass mat - Weight 375gr / m 2 The second chopped glass mat - Weight 375gr / m 2 The third chopped glass mat - Weight 375gr / m 2 The fourth chopped glass mat - Weight 450gr / m 2 Continuous matte or - upper layer - a matrix layer having: - an introduced separating layer, advantageously 20 g / m 2 The nonwoven glass fabric has a basis weight of - Weight 375gr / m 2 The first chopped glass mat - Weight 375gr / m 2 The second chopped glass mat - Weight 375gr / m 2 The third chopped glass mat - Weight 375gr / m 2 The fourth chopped glass mat - Weight 450gr / m 2 Continuous matte.
[0177] The four chopped glass mats used here are introduced one after the other from above into the matrix layer to be cured. By capillary action, the chopped glass mats are impregnated one after the other and surrounded by the matrix layer. Advantageously, the glass nonwoven and the continuous mat are also introduced, advantageously likewise from above, into the matrix layer to be cured. It has proven advantageous to introduce four individual chopped glass mats one after the other into the matrix layer. For this, a highly uniform distribution of the matrix material is required. If, for example, only one thick chopped glass mat corresponding to four individual mats is introduced, the matrix layer material will be pushed out to the sides and the entire plastic composite will be rejected.
[0178] Finally, a further support film, preferably a PET film, is preferably applied to the matrix layer. This prevents oxygen inhibition during the curing of the matrix material. The entire layer system is calendered to remove trapped air between the PET film and the resin. The matrix material is then heat cured by heating to 90° C. for 30 minutes. The resulting plastic composite is then cooled back down to room temperature. The plastic composite is again irradiated with UV radiation to crosslink the top layer containing urethane acrylate. This can be done, for example, at 400 mJ / cm 2 . 2This can be done with a further, preferably deep-curing UV radiation source configured as a gallium or iron-doped mercury lamp emitting a dose of ±10%. In the production process, this radiation source is arranged below the layer system, so that it irradiates the upper layers directly. The irradiation is therefore carried out from below. The irradiation is preferably carried out for 3 to 30 seconds, more preferably 5 to 15 seconds, even more preferably 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15 seconds. In a final step, the two carrier films which have limited the area of the plastic composite up to this point are removed. The plastic composite is then subjected to a finishing treatment. The plastic composite produced in this way has a tensile strength of 60 N / mm according to DIN EN ISO 527-4 / 2 / 2. 2 and a tensile modulus according to DIN EN ISO 527-4 / 2 / 2 of 6,000 N / mm 2 It turned out to be.
[0179] The plastic composite with the two possible top layer options described herein exhibits significantly improved gloss stability, virtually no yellowing, and improved mechanical properties while achieving a 100 g / m2 coating thickness compared to known fiber-reinforced plastic panels. 2 The plastic composites described herein are advantageous in particular in the architectural sector, where the facades of buildings have to retain an attractive appearance for decades. For example, facade elements can be provided that still look almost new even after decades of weathering outdoors. High erosion resistance. Expensive renovation measures or replacement of facade elements are particularly not necessary. This allows for significant cost savings.
[0180] Advantageously, the term Xeno test is understood to mean a test method carried out in accordance with DIN EN ISO 4892-2-A1, which may also be referred to as accelerated weathering test in accordance with DIN EN ISO 4892-2-A1 or accelerated weathering test method in accordance with DIN EN ISO 4892-2-A1.
[0181] Further advantages, features and configuration options are presented in the following drawing descriptions of example embodiments, which should be understood as non-limiting. [Brief description of the drawings]
[0182] [Figure 1] FIG. 1 shows a test method according to DIN EN ISO 4892-2-A1. [Diagram 2] FIG. 2 is a further diagram showing the test method according to DIN EN ISO 4892-2-A1.
[0183] The data measured using a spectrophotometer as described above for the accelerated weathering test method according to DIN EN ISO 4892-2-A1 are shown in Figures 1 and 2.
[0184] FIG. 1 shows the behavior of a plastic composite as described herein (dashed line) under artificial weathering according to the accelerated weathering test method according to DIN EN ISO 4892-2-A1 as discoloration delta b (yellowing) (y-axis) over time (x-axis). A plastic composite as described herein, preferably having at least 1.5% by weight, and at most 8% by weight, of a pigment, for example titanium dioxide, in the upper layer, preferably configured as a urethane acrylate, in the cured state, is shown by the dashed line. It can be seen that the yellowing increases very slowly over time only to a value of 1.5. This means that there is at most a very slight difference in color, which is not noticeable to the observer himself. By way of comparison, the solid line shows the same plastic composite without any color pigment in the upper layer. It can be seen that the yellowing of the matrix layer occurs particularly quickly.
[0185] FIG. 2 shows the gloss loss (y-axis) over time (x-axis) under artificial weathering according to a test method in accordance with DIN EN ISO 4892-2-A1. A plastic composite as described herein, preferably having at least 1.5% by weight, and at most 8% by weight, of a pigment, for example titanium dioxide, in the top layer, preferably configured as a urethane acrylate, in the cured state, is shown by a solid line. It can be seen that the gloss loss over time is only slightly reduced. After about 9000 hours of test method in accordance with DIN EN ISO 4892-2-A1, the gloss retains about 80% of the original new gloss of 100%. The gloss is determined by measuring the ratio of the incident light to the light reflected from the surface with a reflectometer, taking into account the angle of the specular reflection. Here, a BYK-Gardner "tri-gloss" reflectometer was used as the measuring device, with a measuring angle of 20°. The dotted line shows, for comparison, the same plastic composite with a top layer according to the conventional standard (isophthalic polyester resin with neopentyl glycol). The test method according to DIN EN ISO 4892-2-A1 shows that the gloss reduction is already above 80% after a very short time of about 1000 hours.
[0186] Although the present invention has been shown and described in detail by means of preferred embodiment examples, the present invention is not limited to the disclosed examples. Those skilled in the art can derive other variants therefrom without departing from the scope of protection of the present invention. In particular, the present invention is not limited to the combination of features presented below, but can also form other combinations or subcombinations of the disclosed features that are obvious to those skilled in the art.
Claims
1. 1. A fiber reinforced multi-layer planar plastic composite having improved UV resistance, said composite comprising: a. at least one matrix layer forming a support matrix body; and b. at least one top layer disposed on the matrix layer; the top layer being configured as a surface sealant of the matrix layer and / or as a UV protection layer of the matrix layer, the matrix layer comprising at least one resin from the group of unsaturated polyester resins, vinyl ester resins, epoxy resins, polyurethane resins and / or combinations thereof, the top layer comprising at least one acrylate-based resin, At least the matrix layer is configured to be fiber reinforced; the top layer having a layer thickness in the cured state in the range of 40 to 150 μm, the plastic composite having a Delta E value of <1.0 in the color system L / a / b after 1000 h test according to DIN EN ISO 4892-2-A1 and a Delta E value of <1.7 in the color system L / a / b after 3000 h test according to DIN EN ISO 4892-2-A1.
2. 2. The fiber reinforced multi-layer plastic composite of claim 1, wherein the top layer comprises at least one deep-cure UV initiator.
3. 3. A fiber-reinforced multi-layer plastic composite according to claim 2, characterized in that the at least one deep-cure UV initiator comprises a phosphine oxide group.
4. 4. A fiber-reinforced multilayer plastic composite according to claim 1, characterized in that the matrix layer further comprises at least one type of fiber.
5. 5. The fiber-reinforced multilayer plastic composite according to claim 1, further comprising at least one further separating layer disposed between the top layer and the matrix layer.
6. 6. A fibre-reinforced multi-layer plastic composite according to claim 1, characterized in that the top layer and / or the matrix layer comprises at least one further additive.
7. 7. The fiber-reinforced multilayer plastic composite according to claim 1, characterized in that the composite has a loss of reactive diluent of at most 2% by weight relative to the liquid layer material applied during the manufacturing process.
8. 8. The fiber-reinforced multilayer plastic composite according to claim 1, wherein the top layer has a gloss retention of at least 70% of 100% of the original gloss after 9000 hours of testing according to DIN EN ISO 4892-2-A1.
9. 9. A method for producing a plastic composite according to any one of claims 1 to 8, said method comprising at least a. applying an overlayer material to a substrate surface; b. forming the overlayer material to obtain a layer on the surface of the substrate; c. irradiating the resulting top layer with UV light to deep cure the top layer; d. applying a matrix material to form a matrix layer; e) applying a fiber material to the matrix layer, the fiber material being submerged in the still liquid matrix layer and / or being surrounded by the still liquid matrix layer by capillary forces; f. curing the matrix layer applied to the top layer; g. Removing the support material to obtain the final fiber reinforced multi-layer plastic composite. The method comprising:
10. 10. The method according to claim 9, characterized in that it comprises the further step, at least between steps c) and d), of applying at least one separating layer to the deep-cured top layer.
11. 10. The method according to claim 9, further comprising applying a further support material for covering the matrix layer at least between steps e) and f).
12. 10. The method according to claim 9, characterized in that at least between steps f) and g) a UV post-cure of the top layer from the free back side of the support material is carried out.
13. A fiber reinforced multi-layer plastic composite produced by the method of claim 9.
14. 10. A fibre-reinforced multi-layer plastic composite according to any one of claims 1 to 8, produced by the method according to claim 9.
15. 10. A fiber-reinforced multi-layer planar plastic composite with improved UV resistance produced by at least the method of claim 9, said composite comprising: a. at least one matrix layer forming a support matrix body; and b. at least one top layer disposed on the matrix layer; wherein the top layer is configured as a surface sealant for the matrix layer and / or as a UV protection layer for the matrix layer, the matrix layer comprising at least one resin from the group of unsaturated polyester resins, vinyl ester resins, epoxy resins, polyurethane resins and / or combinations thereof, and the top layer comprising at least one acrylate-based resin.
16. Use of a fiber-reinforced multilayer plastic composite as claimed in any one of claims 1 to 8 as sheet elements for the interior and / or exterior of vehicles, aircraft, trains, ships, caravans or camper vans, as sheet elements for logistics and transport, for example for lorry superstructures, as facade elements in the building industry and / or use of a fiber-reinforced multilayer plastic composite as claimed in any one of claims 1 to 8 and / or produced by the method as claimed in claim 9.
Citation Information
Patent Citations
Transparent coated molded article and its production
JP1999077877A
Blush-resistant marine gel coat composition
US20070001343A1
Curable compositions with outdoor performances
WO2020260608A1