Hot melt adhesive composition having a styrene block copolymer
A styrene block copolymer and wax-based adhesive composition addresses high viscosity and temperature issues in absorbent articles, ensuring effective adhesion and cohesion with improved processability and substrate compatibility.
Patent Information
- Application Number
- JP2024534104
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2021-12-07
- Filing Date
- 2022-12-05
- Publication Date
- 2024-11-28
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing hot melt adhesives with high styrene content have high viscosity, making them difficult to apply and potentially damaging to substrates, and require high application temperatures, which is problematic for absorbent articles like diapers.
A hot melt adhesive composition comprising 22% to 60% styrene block copolymer and 0.1% to 5% wax with specific viscosity ranges, ensuring good adhesion and cohesive properties while maintaining processability.
The adhesive composition provides effective adhesion and cohesion, maintaining the integrity of absorbent cores in absorbent articles, even under wet conditions, with improved processability and reduced substrate damage.
Smart Images

Figure 2024544225000001 
Figure 2024544225000002 
Figure 2024544225000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a hot melt adhesive composition comprising a styrenic block copolymer and a wax.
[0002] The present invention also relates to the use of said hot melt adhesive composition as a core stabilizing adhesive. [Background technology]
[0003] Absorbent articles such as diapers, adult incontinence products, sanitary napkins, and the like are well known staple products, and many attempts have been made to provide a good overall fit and high absorbency.
[0004] A typical absorbent article comprises an absorbent core sandwiched between a topsheet and a backsheet. The absorbent core generally comprises an absorbent polymer material capable of storing large amounts of body fluids, such as urine in the case of a diaper. The absorbent core also comprises an adhesive that allows for fixation of the core structure. These adhesives are different from the adhesives used to attach the absorbent core to the topsheet and backsheet of the absorbent article.
[0005] Absorbent articles are generally disposable products that can be worn for extended periods of time, either dry or wet. In order to provide good comfort when worn, it is important to keep the absorbent material / network of the absorbent core contained in a diaper or other absorbent article in place, both when the article is dry, or during expansion when the core is fully / partially wetted (with urine or other body fluids).
[0006] Hot melt adhesive compositions are often used to bond substrates together or to improve the integrity and functionality of disposable absorbent articles. Some attempts have been made to obtain high cohesion of absorbent cores by using styrene block copolymers with high styrene content in hot melt adhesives. However, such hot melt adhesives have high viscosities that make them difficult to apply to substrates (e.g., poor processability), require application at high temperatures that can damage substrates (e.g., thin substrates), and require a lot of energy. Summary of the Invention
[0007] Thus, there is a need to provide hot melt adhesive compositions that have suitable viscosity (including good processability) while exhibiting good adhesive and cohesive properties, especially in absorbent cores. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0008] Hot melt adhesive composition The present invention provides a hot melt adhesive composition comprising: a) 22% to 60% by weight of at least one styrenic block copolymer (A) (designated "SBC(A)"), at least one linear styrene block copolymer (A1), and - optionally at least one styrene diblock copolymer (A2); Including, - a styrene content of 38% by weight or more, based on the total weight of the SBC(A), and - Diblock content ranging from 0% to 10% by weight, based on the total weight of SBC(A) A styrene block copolymer (A) having the formula: b) 0.1% to 5% by weight of at least one wax having a freezing point of 60°C or higher and a needle penetration of 2 dmm or less at 25°C; The hot melt adhesive composition comprises The hot melt adhesive composition has a viscosity of 30,000 mPa·s or more at 120°C and a viscosity of 5,000 mPa·s or less at 177°C.
[0009] Styrene block copolymer (A) Styrenic block copolymer (A), designated "SBC(A)", is: at least one linear styrene block copolymer (A1); optionally with at least one styrene diblock copolymer (A2); comprising, preferably consisting essentially of, and more preferably consisting of, The styrene block copolymer (A) is - a styrene content of 38% by weight or more, based on the total weight of the SBC(A), and - Diblock content ranging from 0% to 10% by weight, based on the total weight of SBC(A) has.
[0010] The styrene block copolymer (A) may comprise only linear styrene block copolymer(s) (A1) and no styrene diblock copolymer (A2), or may comprise a blend of at least one linear styrene block copolymer (A1) and at least one styrene diblock copolymer (A2). The blend may be, for example, two different linear styrene block copolymers (A1) and one styrene diblock copolymer (A2), or three different linear styrene block copolymers (A1) and two different diblock copolymers (A2), or one linear styrene block copolymer (A1) and one styrene diblock copolymer (A2).
[0011] The styrene block copolymer(s) contained in SBC (A), in particular (A1) and optionally (A2), comprises at least one non-elastomeric block A′ which is a styrene-based polymer and at least one elastomeric block X which is a conjugated diene-based block polymer, said conjugated diene-based block polymer being preferably not hydrogenated.
[0012] Linear styrene block copolymer (A1) (“SBC(A1)”) refers to a linear styrene-conjugated diene based block copolymer of at least three blocks.
[0013] In particular, the linear SBC (A1) may be a triblock SBC of formula (1) or a multiblock SBC of formula (2): TIFF2024544225000001.tif14170[In the formula, -A' is a non-elastomeric block of a styrene-based polymer, preferably polystyrene; -X is an elastomeric block of a conjugated diene block polymer, said conjugated diene being preferably selected from butadiene, isoprene, and mixtures thereof; -m is an integer of at least 1].
[0014] The styrene diblock copolymer (A2) ("diblock (A2)") is a styrene-conjugated diene based diblock copolymer, i.e. a diblock copolymer comprising one inelastic block A', which is a styrene based polymer (preferably polystyrene), and one elastomeric block X, which is a conjugated diene based block polymer, said conjugated diene based block polymer being preferably not hydrogenated.
[0015] The styrene diblock copolymer (A2) can be represented by the following formula (3): A'-X (3) [In the formula, -A' is a non-elastomeric block of a styrene-based polymer, preferably polystyrene; -X is an elastomeric block of a conjugated diene block polymer, said conjugated diene being preferably selected from butadiene, isoprene, and mixtures thereof.
[0016] The diblock content in SBC (A) refers to the proportion by weight of the styrene diblock copolymer (A2) contained in SBC (A).
[0017] Preferably, the diblock content is in the range of 0% to 5% by weight, more preferably 0% to 2% by weight, and even more preferably 0% to 1% by weight, based on the total weight of the SBC (A).
[0018] The styrene content in SBC(A) refers to the proportion by weight of the styrene-based polymer block contained in the styrene block copolymer of SBC(A).
[0019] Preferably, SBC (A) has a styrene content in the range of 38% to 70% by weight, more preferably 38% to 60% by weight, and even more preferably 40% to 50% by weight, based on the total weight of SBC (A).
[0020] In one embodiment, the hot melt adhesive composition comprises a mixture of two or more different styrene block copolymers (A).
[0021] In embodiments where the hot melt adhesive composition comprises a mixture of different styrene block copolymers (A) (two or more), the overall styrene content of the mixture may comprise at least 40% by weight, preferably between 40% and 60% by weight, and even more preferably between 42% and 50% by weight, based on the total weight of the mixture.
[0022] In embodiments where the hot melt adhesive composition comprises a mixture of different styrene block copolymers (A) (two or more), the overall diblock content of the mixture may be in the range of 0 wt.% to 5 wt.%, more preferably 0 wt.% to 2 wt.%, and even more preferably 0 wt.% to 1 wt.%, based on the total weight of the mixture.
[0023] The linear styrene block copolymer (A1) may be selected from the following linear triblock copolymers: styrene-butadiene-styrene copolymer (SBS), styrene-isoprene-styrene copolymer (SIS), styrene-ethylene-butylene-styrene copolymer (SEBS), styrene-butadiene-butylene-styrene copolymer (SBBS), styrene-ethylene-propylene-styrene copolymer (SEPS), and any mixtures thereof. Preferably, the linear styrene block copolymer (A1) is selected from the group consisting of styrene-butadiene-styrene copolymer (SBS), styrene-isoprene-styrene copolymer (SIS), and mixtures thereof.
[0024] The diblock styrene copolymer (A2) may be selected from the following diblock copolymers: styrene-butadiene diblock copolymer (SB), styrene-isoprene diblock copolymer (SI), styrene-ethylene-butylene diblock copolymer (SEB), styrene-ethylene-propylene diblock copolymer (SEP), styrene-butylene-butene (SBB), and mixtures thereof.
[0025] It is preferred that the conjugated diene-based block polymer forming the elastic block (corresponding to X in formulae (1), (2) and (3)) of the linear SBC (A1) and the optional diblock (A2) is the same. More preferably, the SBC (A) is styrene-butadiene-based, which means that the conjugated diene-based block polymer forming the elastic block of the linear SBC (A1) and the diblock copolymer (A2) is polybutadiene, and therefore in formulae (3), (4) and (5), B' is an elastic block of polybutadiene.
[0026] The styrene block copolymer (A) preferably has a melt flow index (200° C. / 5 kg) of 20 g / 10 min or more, more preferably 30 g / 10 min or more.
[0027] In embodiments where the hot melt adhesive comprises a mixture of different block copolymers (A), the average melt flow index of the mixture is preferably 20 g / 10 min or more (200° C. / 5 kg), more preferably 30 g / 10 min or more. The average melt flow index of the mixture is calculated relative to the weight percentage of each of the different styrene block copolymers (A) compared to the total weight of the mixture of styrene block copolymers (A).
[0028] The melt flow index can be measured at 200° C. / 5 kg according to ASTM D1238.
[0029] Useful styrenic block copolymers (A) can be prepared by any block polymerization method well known in the art from at least one substituted or unsubstituted styrenic monomer and at least one conjugated diene monomer to form a mixture of linear styrenic block copolymers and optional styrenic diblock copolymers for use in accordance with the present invention.
[0030] Useful SBC(A) are also commercially available. Examples of useful commercially available SBC(A) include, inter alia: - Vector® 4411 (sold by TSRC, a linear styrene-isoprene-styrene block copolymer having a styrene content in the range of 44% by weight and a diblock content of less than 1% by weight); - Kraton® D1162 (sold by KRATON, a linear styrene-isoprene-styrene block copolymer having a styrene content in the range of 43% by weight and a diblock content of less than 1% by weight); - Taipol® 4202 (a linear styrene-butadiene-styrene block copolymer sold by TSRC, having a styrene content of 40% by weight and a diblock content of less than 1% by weight).
[0031] Preferably, the total content of the (one or more) styrene block copolymers (A) is in the range of 25% by weight to 50% by weight, more preferably 25% by weight to 40% by weight, and even more preferably 27% by weight to 37% by weight, based on the total weight of the hot melt adhesive composition.
[0032] wax The hot melt adhesive composition contains 0.1% to 5% by weight, preferably 1% to 5% by weight, more preferably 1.5% to 4.0%, and even more preferably 2.0% to 4.0% by weight of at least one wax described above, based on the total weight of the hot melt adhesive composition.
[0033] The wax is preferably a synthetic wax, more preferably a synthetic wax selected from the group consisting of Fischer-Tropsch wax, polyolefin waxes, and mixtures thereof. Preferably, the wax is a Fischer-Tropsch wax.
[0034] As used herein, the term "synthetic polyolefin wax" refers to polymers or long chain entities composed of olefin monomer units derived from polymerization.
[0035] "Fischer-Tropsch wax" means wax obtained by the so-called Fischer-Tropsch process. The Fischer-Tropsch process involves the conversion of synthesis gas, which mainly contains hydrogen and carbon monoxide, into hydrocarbons. The conversion is typically carried out by contacting the synthesis gas with a Fischer-Tropsch catalyst, such as an iron- or cobalt-based catalyst, in a fixed-bed or slurry-bed reactor under low- or high-temperature Fischer-Tropsch operating conditions. In this way, a mixture of hydrocarbons with different boiling ranges is obtained. From this hydrocarbon mixture, the Fischer-Tropsch wax is then recovered, for example by distillation.
[0036] The wax according to the invention has a freezing point of at least 60° C., preferably at least 65° C., more preferably at least 70° C. and advantageously at least 75° C. The wax according to the invention preferably has a freezing point of at least 80° C.
[0037] The freezing point of the wax may be below 150°C, preferably below 120°C.
[0038] The freezing point of the wax can be determined according to ASTM D 938.
[0039] As used herein, the term "dmm" means decimeters.
[0040] The needle penetration of the wax is 2 dmm or less, preferably 1 dmm or less.
[0041] As used herein, the terms "needle penetration," "needle penetration hardness," and "penetration hardness" are similar.
[0042] Needle penetration of wax can be determined according to ASTM D 1321.
[0043] The wax may have a melting point of 140°C or less, more preferably in the range of 100-120°C.
[0044] The melting point of the wax can be measured according to ASTM method D127-60.
[0045] The wax according to the invention can be a commercially available wax. Examples of commercially available waxes suitable for the present invention include the Fischer-Tropsch wax sold under the trade name SX105 by Shell, with a freezing point of 101-108° C. and a needle penetration of 2 dmm, the Fischer-Tropsch wax sold under the trade name SASOLWAX® H15 by Sasol, with a freezing point of 97° C. and a needle penetration hardness of 1 dmm, or the PE wax sold under the trade name LP1060P by SCG Chemicals, with a freezing point of 116° C. and a needle penetration hardness of 2 dmm.
[0046] Plasticizer The hot melt adhesive composition of the present invention may include a plasticizer, which may be a solid or liquid plasticizer.
[0047] The hot melt adhesive composition may contain about 0% by weight to about 40% by weight, preferably about 5% by weight to about 35% by weight, and more preferably about 10% by weight to about 30% by weight of a plasticizer(s), based on the total weight of the hot melt adhesive composition.
[0048] The plasticizer may be selected from the group consisting of naphthenic and paraffinic oils, olefin oligomers, low molecular weight polymers, glycol benzoates, vegetable and animal oils, and derivatives thereof.
[0049] Naphthenic and paraffinic oils are petroleum-based oils consisting of mixtures of naphthenic hydrocarbons (e.g., aliphatic, saturated or unsaturated, C4-C7 membered hydrocarbon rings; preferably, aliphatic, saturated or unsaturated, C4-C6 membered hydrocarbon rings, including cycloalkanes such as cyclopentane, cyclohexane, cycloheptane, etc.), paraffinic hydrocarbons (saturated, straight or branched chain, alkanes), and aromatic hydrocarbons (aromatic hydrocarbon rings, preferably aromatic C6 membered hydrocarbon rings, which may be monocyclic or polycyclic).
[0050] The classification of naphthenic and paraffinic oils is based on the amount of each type of hydrocarbon in the oil. Typically, paraffinic oils have a paraffinic hydrocarbon content of at least about 50% by weight; naphthenic oils have a naphthenic hydrocarbon content of about 30% to about 50% by weight, based on the total weight of the plasticizer.
[0051] The oligomer can be selected from the group consisting of polypropylene, polybutene, hydrogenated polyisopropene, hydrogenated butadiene, etc., having an average molecular weight of about 100 to about 10,000 g / mol.
[0052] The vegetable and animal oils may be selected from glycerol esters of common fatty acids and their polymerization products.
[0053] In a preferred embodiment, the plasticizer is naphthenic oil.
[0054] Suitable plasticizers are commercially available from Nynas under the trade names Nyflex® 223 and Nyflex® 222B (naphthenic oils), from Sonneborn under the trade names Parol® (paraffin oil), Kaydol® (paraffin oil), from Ergon under the trade name Olympus® L500, from Exxon Mobil under the trade names Primol® 352 and 382, from Calumet under the trade name Calsol® 5550, and from Petrochina Karamay Petrochemical Co.LTD under the trade name Karamay N4010 (naphthenic oil).
[0055] Tackifying Resin The hot melt adhesive composition can include at least one tackifying resin (tackifier).
[0056] The hot melt adhesive composition may comprise 20% to 75% by weight, preferably 30% to 70% by weight, and more preferably 40% to 60% by weight of a tackifying resin(s), based on the total weight of the composition.
[0057] Suitable tackifying resins are those that are compatible with the styrenic block copolymer (A).
[0058] The tackifier resin is - i) homopolymers of terpene resins, preferably having a softening point between 10 ° C and 120 ° C, for example obtained by polymerizing terpene hydrocarbons, such as monoterpenes (or pinene), optionally in the presence of Friedel-Crafts catalysts; - ii) resins obtained by copolymerization of alpha-methylstyrene with other hydrocarbon comonomers, such as styrene, vinyltoluene, and mixtures thereof; - iii) phenol-modified terpene resins, such as resin products obtained from the condensation of terpenes with phenols in an acidic medium; - iv) natural and modified rosins, such as gun rosin, wood rosin, tall oil rosin, distilled rosin, hydrogenated rosin, dimerized rosin, and polymerized rosin; - v) glycerol and pentaerythritol esters of natural and modified rosins, such as the glycerol ester of pale wood rosin, the glycerol ester of hydrogenated rosin, the glycerol ester of polymerized rosin, the pentaerythritol ester of pale wood rosin, the pentaerythritol ester of hydrogenated rosin, the pentaerythritol ester of tall oil rosin, and the phenolic modified pentaerythritol ester of rosin; and - vi) aliphatic and cycloaliphatic petroleum-derived hydrocarbon resins (the latter resins in particular result from the polymerization of monomers consisting mainly of aliphatic or cycloaliphatic olefins and diolefins), which also include hydrogenated aliphatic and cycloaliphatic petroleum hydrocarbon resins; - vii) Aliphatic / aromatic petroleum-derived hydrocarbon resins and their hydrogenated derivatives; - viii) mixtures thereof The compound may be selected from the group consisting of:
[0059] In particular, mention may be made of the following products, of the types defined above: - resins of type i): polyterpene tackifiers sold under the trade names Sylvagum® TR and Sylvares® TR series (7115, 7125, M1115) by Arizone Chemical; - Type ii) resins: Arkon® series from Arakawa and Hikotack® series from Kolon, made from C9 monomers. - resins of type iii) : Dertophene® 1510 sold by DRT, Dertophene® H150 sold by Arizone Chemical, and Sylvarez® TP95 (these are phenolic modified terpene resins); - Type iv) resins: Foral® DX from Pinova Inc. and Foral AX-E from Eastman (these are hydrogenated rosin resins). - resin of type v): Sylvalite® RE 100 (an ester or rosin and pentaerythritol sold by Arizone Chemical); - resins of type vi): Escorez® 5400 (hydrogenated dicyclopentadiene resin sold by Exxon Chemicals with a softening point of 100° C.); Sukorez® SU210 (partially hydrogenated aliphatic and cycloaliphatic petroleum-derived hydrocarbon resin with a softening point of 110° C. sold by Kolon); - Resins of type vii): Quintone® DX390N (non-hydrogenated aliphatic and aromatic petroleum-derived hydrocarbon resin with a softening point of 90° C., sold by Zeon), and Sukorez® SU400 (hydrogenated aliphatic and aromatic petroleum-derived hydrocarbon resin, sold by Kolon).
[0060] In a preferred embodiment, the hot melt adhesive composition does not contain aromatic resins based on pure monomer streams of aromatic monomers such as, for example, vinyl toluene, styrene, alpha-methylstyrene, or indene. Examples of such resins are the Kristalex® or Plastolyn® series sold by Eastman Chemical Co. According to this preferred embodiment, the hot melt adhesive has low odor and reduced VOC emissions due to the absence of these specific tackifying resins, and advantageously exhibits suitable viscosity, adhesion, and mechanical properties.
[0061] Stabilizer The hot melt adhesive composition of the present invention may also contain at least one stabilizer (antioxidant).
[0062] The hot melt adhesive composition comprises from about 0 wt % to about 5 wt %, preferably from 0 wt % to about 3 wt %, more preferably from about 0.1 wt % to about 3 wt %, and even more preferably from about 0.1 wt % to 2 wt % of a stabilizer(s), based on the total weight of the hot melt adhesive composition.
[0063] Suitable stabilizers are typically incorporated to protect the polymers and thereby the entire adhesive system from the effects of thermal and oxidative degradation that typically occur during adhesive manufacture and application, as well as when the final product is typically exposed to the ambient environment.
[0064] Applicable stabilizers include, for example, high molecular weight hindered phenols and polyfunctional phenols such as sulfur- and phosphorus-containing phenols. Hindered phenols are well known to those skilled in the art and can be characterized as phenolic compounds that also contain sterically bulky radicals in close proximity to the phenolic hydroxyl group. In particular, tertiary butyl groups are generally substituted on the benzene ring at least one ortho position relative to the phenolic hydroxyl group. The presence of these sterically bulky substituted radicals in close proximity to the hydroxyl group slows down the stretching frequency of the hydroxyl group and accordingly reduces its reactivity; thus, this steric hindrance provides phenolic compounds with stabilizing properties. Representative hindered phenols include 1,3,5-trimethyl-2,4,6-tris(3-5-di-tert-butyl-4-hydroxybenzyl)benzene; pentaerythritol tetrakis-3(3,5-di-tert-butyl-4-hydroxyphenyl)propionate; n-octadecyl-3(3,5-di-tert-butyl-4-hydroxyphenyl)propionate; 4.4'-methylenebis(4-methyl-6-tert-butylphenol); 2,6-di-tert-butylphenol; 6-(4-hydroxyphenyl)propionate; 2,3,6-tris(4-hydroxy-3,5-di-tert-butyl-phenoxy)-1,3,5-triazine; di-n-octadecyl-3,5-di-tert-butyl-4-hydroxybenzylphosphonate; 2-(n-octyl-thio)ethyl-3,5-di-tert-butyl-4-hydroxybenzoate, and sorbitol hexa-3(3,5-di-tert-butyl-4-hydroxy-phenyl)propionate.
[0065] Suitable antioxidants are commercially available under the trade names Irganox® 1010 (tetrakis(methylene(3,5-di-tert-butyl-4-hydroxyhydrocinnamate))methane), Irgafos® 168 (tris(2,4-ditert-butylphenyl)phosphate) from BASF, and Chinox® 1010 (pentaerythritol tetrakis(3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate)) from Shuangjian, Evernox® 1010 and Everfos® 168 from Everspring Chemical, and Songnox® 10 and 1680 from Songwon.
[0066] Other Additives The hot melt adhesive composition may further comprise at least one additive, preferably in an amount of 0% to 5% of the total weight of the hot melt adhesive composition.
[0067] The additives may be selected from the group consisting of inert colorants (e.g., titanium dioxide), fillers (e.g., talc, calcium carbonate, clay, silica, mica, wollastonite, feldspar, aluminum silicate, alumina, hydrated alumina, glass microspheres, ceramic microspheres, thermoplastic microspheres, and mixtures thereof), surfactants, additional polymers other than styrenic block copolymers, crosslinkers, nucleating agents, reactive compounds, flame retardant mineral or organic agents, ultraviolet (UV) or infrared (IR) light absorbers, and UV or IR fluorescent agents. These optional auxiliary additives are well known in the art.
[0068] The additional polymer may be selected from the group consisting of polyolefins, amorphous poly-alpha-olefins, ethyl vinyl acetate polymers (EVA), polyamides, and mixtures thereof. The hot melt adhesive may comprise from about 0% to about 5% by weight of at least one additional polymer, based on the total weight of the composition.
[0069] Hot melt adhesive composition The viscosity is measured at a temperature of about 177°C or 120°C using a Brookfield viscometer with spindle 27 according to the standard method of ASTM D-3236.
[0070] The hot melt adhesive composition has a viscosity at 120° C. of 30,000 mPa·s or more, preferably 50,000 mPa·s or more, and even more preferably 80,000 mPa·s or more.
[0071] The hot melt adhesive composition has a viscosity at 177°C of 5,000 mPa·s or less, preferably 4,000 mPa·s or less, and even more preferably 3,000 mPa·s or less.
[0072] The hot melt adhesive composition according to the invention advantageously has a sufficient viscosity to be applicable at a suitable temperature, such as for example 160° C. Furthermore, the viscosity is advantageously not too low at 120° C., which allows for better application and better homogeneity of the resulting adhesive structure. Indeed, at too low an application temperature, if the hot melt adhesive becomes too liquid, the rapid cooling process leads to non-uniformity of the adhesive structure.
[0073] The hot melt adhesive composition according to the invention advantageously has good processability (due to the viscosity range at 177°C and 120°C) while exhibiting good adhesion and cohesion. Good adhesion is important to maintain contact between the absorbent material and the substrate. Good internal cohesion ensures that the adhesive does not break during use, especially under external forces. Thus, high internal cohesion advantageously allows the absorbent core to remain together both in the dry state and during expansion while the core is wet.
[0074] These properties make the hot melt adhesive composition advantageously useful as a core stabilizing adhesive (to hold the absorbent material of the core in place and maintain the integrity of the core structure, especially during use of the absorbent article).
[0075] Process for preparing hot melt adhesive composition The present invention also relates to a process for preparing the above-mentioned hot melt adhesive composition.
[0076] The hot melt adhesive composition can be prepared by mixing in the molten state at least one styrenic block copolymer P and at least one Fischer-Tropsch wax. Optional other components or additives of the above-mentioned compositions may be mixed with the above-mentioned components.
[0077] The hot melt adhesive composition of the present invention can be manufactured using any of the techniques known in the art. Preferably, the mixing step is carried out at a temperature of 130° C. to 180° C. The components are preferably mixed for at least several hours, typically at least 4 hours, preferably 4 to 6 hours.
[0078] The hot melt adhesive composition according to the invention can be prepared in the presence of dioxygen (e.g. under an air atmosphere) or, preferably, under an inert atmosphere, such as, for example, under carbon dioxide or nitrogen, to limit potential degradation due to oxidation reactions.
[0079] According to some embodiments, the process for preparing the hot melt adhesive composition according to the present invention comprises the steps of: - a first step of mixing the tackifier resin and the plasticizer(s), preferably together with an antioxidant, if present, at a temperature in the range of 150°C to 180°C for a time at least sufficient for all of the tackifier resin to melt; - a second step of cooling the mixture to a temperature in the range of 130°C to 150°C; - a third step of adding the styrenic block copolymer (A) to the mixture obtained in the previous step while heating at a temperature in the range of 130°C to 150°C under stirring for a time sufficient to melt at least all of the styrenic block copolymer; - A fourth step of adding wax to the mixture obtained in the previous step while heating at a temperature in the range of 130°C to 150°C under stirring for a time sufficient to melt all of the styrenic block copolymer. Includes.
[0080] Additionally, the process of the present invention may include the step of applying a vacuum to remove trapped air within the mixture, before or after any of the foregoing process steps.
[0081] Other useful optional ingredients or additives which may be present in the hot melt adhesive composition according to the invention may be added at any stage of the process according to the invention, as described above.
[0082] use The present invention relates to the use of the hot melt adhesive composition as defined herein in the manufacture of disposable absorbent articles such as, for example, diapers, adult incontinence products, bed pads, sanitary napkins, medical dressings, bandages and the like.
[0083] The present invention relates to the use of the hot melt adhesive composition defined herein as a core stabilizing adhesive.
[0084] The present invention relates to a disposable absorbent article comprising the hot melt adhesive composition defined above. The disposable absorbent article may be selected from the group consisting of diapers, adult incontinence products, bed pads, sanitary napkins, medical dressings, bandages, preferably diapers.
[0085] The disposable absorbent article comprises an absorbent core comprising a core and optionally a core wrap.
[0086] The absorbent cores can be manufactured in-line (i.e., for disposable absorbent articles) on an assembly line, or the cores can be manufactured off-line and rolled or decorated for use at a later date or at another location.
[0087] The core can be of various designs and shapes: rectangular, can be shaped like a dog bone, can be one continuous shape or can be divided into channels formed, for example, by the topsheet and backsheet.
[0088] The absorbent core is generally centrally located within the article and is secured between the topsheet and the backsheet via attachment means (eg, adhesive).
[0089] The core can comprise different layers. The core typically comprises an absorbent material capable of absorbing bodily fluids received from the topsheet. The core can comprise cellulosic fibers (i.e., fluff), wood pulp, cotton, synthetic fibers, nonwovens, tissue, foams, superabsorbent polymers ("SAP"), or other absorbent materials.
[0090] The hot met adhesive composition according to the invention can be applied as a coating (layer) or in the form of a fiber.
[0091] The core wrap can be any material that wraps around the core to hold the core components in place. The core wrap generally wraps the two long sides of the core, leaving both ends open. The core wrap can be selected from the group consisting of nonwovens and tissues.
[0092] The hot melt adhesive composition can be used to hold the absorbent material in place (particularly within the core wrap, if present) and / or to ensure the integrity of the core structure in both the dry (unexpanded) and wet (expanded) states.
[0093] According to the present invention, "included between x and y" or "in the range from x to y" means a range in which the limits x and y are included. For example, the range "included between 1% and 3%" includes in particular 1% and 3%.
[0094] The following examples are given purely for illustrative purposes of the present invention and should not be construed as limiting the scope of the present invention in any circumstances. EXAMPLES
[0095] Experimental part The following materials were used: Plasticizer 1: Nyflex® 223 from Nynas (naphthenic oil); Resin 1: Sukorez® SU 525 from Kolon (partially hydrogenated resin DCPD / C9 with a Ring and Ball softening point of 125° C.); Resin 2: Sukorez® SU 400 from Kolon (partially hydrogenated resin DCPD / C9 with a Ring and Ball softening point of 100° C.); Resin 3: Sukorez® SU 420 from Kolon (partially hydrogenated resin DCPD / C9 with a Ring and Ball softening point of 120° C.); Polymer P1: VECTOR® 4411 from TSRC is a linear SIS copolymer with 44% styrene as styrene blocks and a diblock content of less than 1%; - Polymer P2: TAIPOL® 4202 from TSRC is a linear SBS copolymer with 40% styrene as styrene block and less than 1% diblock content; - Wax 1: SASOLWAX® H1 from SASOL is a Fischer-Tropsch wax with a freezing point of 97°C and a needle penetration of 1 dmm; - antioxidant 1: Irganox® 1010 from BASF (tetrakis(methylene(3,5-di-tert-butyl-4-hydroxyhydrocinnamate))methane); - Antioxidant 2: Irgafos® 168 (tris(2,4-di-tert-butylphenyl)phosphite) from BASF.
[0096] A1: Preparation of hot melt adhesive The hot melt adhesive compositions of Table 1 below are prepared by mixing the ingredients in the following order: The polymer(s) and half of the resin(s) are added and mixed with the plasticizer(s) at 140°C until everything is a homogeneous mixture. Finally, the wax(es) and the remaining half of the resin(s) are added at the same temperature and mixed to obtain the final homogeneous adhesive mixture. Finally, the mixture is cooled and collected for use as is. TIFF2024544225000002.tif119170
[0097] A2: Properties of hot melt adhesive compositions Storage modulus (G'): Dynamic mechanical analysis (DMA) The adhesive was subjected to a shear stress by the rheometer and the resulting strain (shear deformation) response was measured at constant temperature.
[0098] Equipment: TA Instruments DHR-1 rheometer (applying a small oscillatory stress to achieve a constant oscillatory strain within the linear viscoelastic region of the adhesive (e.g. 1%)).
[0099] General protocol: The adhesive was placed between a Peltier plate, which served as the lower fixed plate, and an upper plate with a radius R of 10 mm, connected to the drive shaft of a motor to generate shear stress. The gap between both plates has a height H of 1,000 μm. The Peltier plate controls the temperature of the material (± 0.5 °C).
[0100] Testing: - After GAP 0 is 80°C, set the temperature to the starting temperature (i.e. 150°C); - Place a small amount of adhesive (1 cm3) on the Peltier plate; - Lower the upper plate to the 1,700 μm gap and make contact with the adhesive; - Remove excess material and set the oven temperature to 120°C; - Lower the upper plate to a gap of 1,000 μm; - Set the temperature to a starting temperature of 120℃, a constant measurement strain of 1%, a constant vibration frequency of 1Hz, and a cooling rate of 6℃ / min (120℃~-10℃); - After the test is completed, the adhesive is melted, the upper plate is lifted and the adhesive is removed from both the Peltier plate and the upper plate. - Allow the temperature to return to room temperature.
[0101] Results: The storage modulus was calculated every 30 seconds throughout the cooling process. G' at 21° C. and 60° C. was determined accordingly.
[0102] Brookfield Viscosity The Brookfield viscosity was measured at a temperature of 177° C. using a Brookfield viscometer with spindle 27 according to the method of ASTM standard D-3236.
[0103] result TIFF2024544225000003.tif69170
[0104] N / A: Not applicable because hot melt is not homogenous and cannot be analyzed by the DMA analysis method mentioned above. nd:Not detected
[0105] The results in the table show that the two hot melt adhesive compositions HM1 and HM2 have the advantage that they show a high storage modulus at 21°C (preferably more than 0.150 MPa, even more than 0.2 MPa) while at the same time maintaining a viscosity at 177°C below 3,000 mPa·s, which allows good processability during the application of the hot melt. The hot melt adhesive compositions HM1 and HM2 therefore have the advantage that they allow high internal cohesion and good processability.
[0106] The storage moduli obtained with the comparative compositions HM3 (no wax), HM4 (no wax) and HM5 (10 wt. % wax) are lower than the storage moduli obtained with the inventive hot melt adhesive compositions HM1 and HM2.
[0107] Furthermore, the storage modulus at 60° C. of HM1 and HM2 is also higher than that obtained with the comparative hot melt adhesive compositions HM3, HM4, and HM5.
Claims
1. a) 22% to 60% by weight of at least one styrene block copolymer (A) (designated as “SBC(A)”), at least one linear styrene block copolymer (A1), and optionally at least one styrene diblock copolymer (A2); Includes - a styrene content of 38% by weight or more, based on the total weight of SBC(A); and - a diblock content ranging from 0% to 10% by weight, based on the total weight of the SBC (A); At least one styrene block copolymer (A) having the formula: b) 0.1% to 5% by weight of at least one wax having a freezing point of 60° C. or higher and a needle penetration of 2 dmm or less at 25° C.; A hot melt adhesive composition comprising: The hot melt adhesive composition has a viscosity of 30,000 mPa·s or more at 120°C and a viscosity of 5,000 mPa·s or less at 177°C.
2. 2. The hot melt adhesive composition of claim 1, wherein the diblock content of the styrene block copolymer (A) is in the range of 0 wt.% to 5 wt.%, more preferably 0 wt.% to 2 wt.%, and even more preferably 0 wt.% to 1 wt.%, based on the total weight of the SBC (A).
3. 3. The hot melt adhesive composition according to claim 1 or 2, wherein the styrene block copolymer (A) has a styrene content in the range of 38% by weight to 70% by weight, more preferably 38% by weight to 60% by weight, and even more preferably 40% by weight to 50% by weight, based on the total weight of the styrene block copolymer (A).
4. The hot melt adhesive composition according to any one of claims 1 to 3, wherein the linear styrene block copolymer (A1) is selected from the following linear triblock copolymers: styrene-butadiene-styrene copolymer (SBS), styrene-isoprene-styrene copolymer (SIS), styrene-ethylene-butylene-styrene copolymer (SEBS), styrene-butadiene-butylene-styrene copolymer (SBBS), styrene-ethylene-propylene-styrene copolymer (SEPS), and any mixtures thereof; more preferably, the linear styrene block copolymer (A1) is selected from the group consisting of styrene-butadiene-styrene copolymer (SBS), styrene-isoprene-styrene copolymer (SIS), and mixtures thereof.
5. 5. The hot melt adhesive composition according to claim 1, wherein the diblock styrene copolymer (A2) is selected from the following diblock copolymers: styrene-butadiene diblock copolymer (SB), styrene-isoprene diblock copolymer (SI), styrene-ethylene-butylene diblock copolymer (SEB), styrene-ethylene-propylene diblock copolymer (SEP), styrene-butylene-butene (SBB), and mixtures thereof.
6. 6. The hot melt adhesive composition according to claim 1, wherein the styrene block copolymer (A) has a melt flow index (200° C. / 5 kg) of 20 g / 10 min or more, preferably 30 g / 10 min or more.
7. 7. The hot melt adhesive composition according to any one of claims 1 to 6, wherein the total content of the styrene block copolymer(s) (A) is in the range of 25% to 50% by weight, more preferably 25% to 40% by weight, even more preferably 27% to 37% by weight, based on the total weight of the hot melt adhesive composition.
8. 8. A hot melt adhesive composition according to any one of claims 1 to 7, characterized in that it comprises 1 wt.-% to 5 wt.-%, preferably 1.5% to 4.0%, even more preferably 2.0 wt.-% to 4.0 wt.-% of at least one wax as defined in claim 1, based on the total weight of the hot melt adhesive composition.
9. 9. The hot melt adhesive composition according to any one of claims 1 to 8, wherein the wax is a synthetic wax, preferably the synthetic wax is selected from the group consisting of Fischer-Tropsch wax, polyolefin waxes, and mixtures thereof, more preferably the wax is a Fischer-Tropsch wax.
10. 10. A hot melt adhesive composition according to any one of the preceding claims, wherein the wax has a freezing point of 65°C or higher, preferably 70°C or higher, more preferably 75°C or higher.
11. 11. The hot melt adhesive composition according to any one of claims 1 to 10, wherein the wax has a needle penetration of 1 dmm or less.
12. 12. The hot melt adhesive composition according to any one of claims 1 to 11, characterized in that it comprises from about 0 to about 40% by weight, preferably from about 5 to about 35% by weight, and even more preferably from about 10 to about 30% by weight of plasticizer(s), based on the total weight of the hot melt adhesive composition.
13. At least one tackifying resin, preferably i) homopolymers of terpene resins, preferably having a softening point between 10° C. and 120° C., - ii) resins obtained by copolymerization of alpha-methylstyrene with other hydrocarbon comonomers, such as, for example, styrene, vinyltoluene, and mixtures thereof; - iii) phenol-modified terpene resins; - iv) natural and modified rosins, such as gun rosin, wood rosin, tall oil rosin, distilled rosin, hydrogenated rosin, dimerized rosin, and polymerized rosin; v) glycerol and pentaerythritol esters of natural and modified rosins, such as the glycerol ester of pale wood rosin, the glycerol ester of hydrogenated rosin, the glycerol ester of polymerized rosin, the pentaerythritol ester of pale wood rosin, the pentaerythritol ester of hydrogenated rosin, the pentaerythritol ester of tall oil rosin, and the phenolic modified pentaerythritol ester of rosin, vi) aliphatic and cycloaliphatic petroleum-derived hydrocarbon resins (the latter resulting in particular from the polymerization of monomers consisting mainly of aliphatic or cycloaliphatic olefins and diolefins); vii) aliphatic / aromatic, petroleum-derived hydrocarbon resins and their hydrogenated derivatives; - viii) mixtures thereof At least one tackifying resin selected from the group consisting of:
13. The hot melt adhesive composition according to claim 1, further comprising:
14. 14. The hot melt adhesive composition according to any one of claims 1 to 13, characterized in that it does not contain aromatic resins based on pure monomer streams of aromatic monomers such as, for example, vinyl toluene, styrene, alpha-methyl styrene or indene.
15. 15. A hot melt adhesive composition according to any one of the preceding claims, characterized in that it has a viscosity at 120°C of 50,000 mPa·s or more, more preferably 80,000 mPa·s or more.
16. 16. A hot melt adhesive composition according to any one of the preceding claims, characterized in that it has a viscosity at 177°C of less than or equal to 4,000 mPa·s, more preferably less than or equal to 3,000 mPa·s.
17. 16. Use of the hot melt adhesive composition according to any one of claims 1 to 15 for the manufacture of disposable absorbent articles such as, for example, diapers, adult incontinence products, bed pads, sanitary napkins, medical dressings, bandages, etc.
18. 17. Use of the hot melt adhesive composition according to any one of claims 1 to 16 as a core stabilising adhesive.
19. A disposable absorbent article comprising the hot melt adhesive composition of any one of claims 1 to 16.