Enhanced Selectivity of Silicon Nitride Deposition
The selective deposition of silicon nitride using ammonia plasma pretreatment and periodic treatment during the process addresses the need for additional patterning steps, achieving high selectivity and improved refractive index without additional lithography and etching.
Patent Information
- Application Number
- JP2024534655
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2021-12-15
- Filing Date
- 2022-12-12
- Publication Date
- 2024-11-28
- Estimated Expiration
- 2042-12-12
AI Technical Summary
Existing silicon nitride deposition methods require additional lithography and etching steps to remove undesired areas, increasing fabrication costs and risking lithographic errors in defining the coating area.
A method for selective deposition of silicon nitride using ammonia plasma pretreatment and periodic ammonia plasma treatment during the deposition process, allowing silicon nitride to be deposited only in desired areas, with improved selectivity and refractive index.
Achieves selective deposition of silicon nitride on specific surfaces with high selectivity and improved refractive index, reducing the need for additional patterning steps and minimizing deposition on undesired surfaces.
Smart Images

Figure 2024544253000001_ABST
Abstract
Description
[Technical field]
[0001] Priority claim The present invention claims priority to U.S. Provisional Application No. 63 / 289,714, filed December 15, 2021, which is incorporated herein by reference.
[0002] The present invention relates to a method for the selective deposition of silicon nitride onto specific surfaces of microelectronic devices. [Background technology]
[0003] Silicon nitride is commonly used in the fabrication of integrated circuits. For example, it is often used as an insulating material in the manufacture of various microelectronic devices such as memory cells, logic devices, memory arrays, etc. Conventionally, silicon nitride films are deposited over the entire substrate surface, but deposition may only be required in certain areas. As a result, additional lithography and etching steps are utilized to remove the undesired areas. As a means to reduce the overall cost of fabrication, it is highly desirable to reduce the number of lithography and etching steps involved. Furthermore, if silicon nitride is selectively deposited only where needed, lithography errors will not affect the definition of the coating area. It would therefore be desirable to achieve such enhanced selectivity silicon nitride deposition. Summary of the Invention
[0004] The use of selective deposition of silicon nitride can eliminate traditional patterning steps by allowing silicon nitride to be deposited only in selected desired areas. Using a silicon iodide precursor alternating with a thermal nitrogen source in ALD or pulsed CVD mode, silicon nitride can be preferentially deposited on surfaces such as silicon nitride, silicon dioxide, germanium oxide, SiCO, SiC, SiON, SiOF and low-k substrates with little to no deposition on other exposed surfaces such as titanium nitride, tantalum nitride, aluminum nitride, hafnium oxide, zirconium oxide, aluminum oxide, titanium oxide, tantalum oxide, niobium oxide, lanthanum oxide, yttrium oxide, magnesium oxide, calcium oxide and strontium oxide.
[0005] Furthermore, by both (i) pretreating these surfaces with an ammonia plasma, in conjunction with (ii) periodically treating the substrate directly in the reaction zone with an additional regime of ammonia plasma, selectivity can be maintained throughout the bulk deposition of silicon nitride, and the refractive index of the resulting films can also be improved. [Brief description of the drawings]
[0006] [Figure 1] 1 is a plot of silicon nitride thickness in angstroms versus cycle number for a known method in which a direct ammonia plasma is applied to a substrate in a reaction zone, followed by silicon tetraiodide and ammonia thermal atomic layer deposition. From this plot, it can be observed that initially the method is selective for deposition onto silicon dioxide surfaces, but that this selectivity begins to decrease after about 100 angstroms (10 nm). [Diagram 2]FIG. 1 illustrates results achieved by an embodiment of the invention in which silicon tetraiodide / ammonia atomic layer deposition (silicon tetraiodide / ammonia ALD) is performed with an additional direct ammonia plasma step after each of 200 cycles of silicon tetraiodide / ammonia ALD. In other words, in this method, an ammonia direct plasma is applied, followed by 200 cycles of silicon tetraiodide / ammonia ALD, followed by ammonia direct plasma being reapplied, followed by 200 cycles of silicon tetraiodide / ammonia ALD, etc. [Diagram 3] 13 shows the concomitant improvement in the refractive index of the deposited silicon nitride using various techniques to reapply the ammonia direct plasma to the substrate within the reaction zone. [Figure 4a] Shown is the practical challenge faced when selective deposition of silicon nitride is desired: In Figure 4a, the desired result is to deposit silicon nitride into the well while minimizing deposition on the aluminum oxide sidewalls, thus resulting in "filling." [Figure 4b] Another practical problem faced when selective deposition of silicon nitride is desired is shown in Figure 4b, which shows the opposite problem, i.e., to deposit silicon nitride on the silicon dioxide sidewalls without depositing it on the aluminum oxide bottom. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0007] As used in this specification and the appended claims, the singular forms "a," "an," and "the" include plural referents unless the content clearly dictates otherwise. As used in this specification and the appended claims, the term "or" is generally used in its sense including "and / or" unless the content clearly dictates otherwise.
[0008] The term "about" generally refers to a range of numbers that are considered equivalent to the recited value (e.g., having the same function or result). In many cases, the term "about" can include numbers that are rounded to the nearest significant figure.
[0009] Numeric ranges expressed using endpoints include all numbers subsumed within that range (eg, 1 to 5 includes 1, 1.5, 2, 2.75, 3, 3.80, 4, and 5).
[0010] In a first aspect, the present invention provides a method for depositing silicon nitride on a microelectronic device substrate having multiple surfaces of different composition, comprising: a. contacting the substrate with pulsed silicon tetraiodide or disilicon hexaiodide and a nitrogen-containing co-reactant under deposition conditions at a temperature of about 150° C. to about 400° C. and a pressure of less than about 15 Torr, thereby defining a pulse cycle; Including, b. The substrate is (i) pretreated with ammonia plasma; (ii) the substrate is then periodically further treated with ammonia plasma; A method is provided.
[0011] The present invention provides a method for selective deposition of silicon nitride layers on various microelectronic device substrates. Generally speaking, the present invention allows selective deposition of silicon nitride films over and in the presence of surfaces composed of high-k dielectrics, metals and metal nitride surfaces on microelectronic device substrates having silicon, silicon oxide and / or silicon nitride surfaces. As described above, step b(ii) includes a cyclic treatment with ammonia plasma. By "cyclic" we mean that no ammonia plasma treatment is performed after each pulse cycle of silicon tetraiodide (SiI4) or disilicon hexaiodide (Si2I6) and the nitrogen-containing co-reactant.
[0012] In certain embodiments, the deposition of the present invention is atomic layer deposition (ALD). For the purposes of this specification, ALD is referred to as a chemical vapor deposition mode in which various reactants and co-reactants are separated in space or time such that the substrate is alternatively exposed to one reactant separately from the co-reactant. In other embodiments, the deposition of the present invention is spatial ALD in which film growth is achieved by exposing the substrate to locations containing different precursors. In other embodiments, the deposition conditions include pulsed chemical vapor deposition (Pulsed CVD) conditions, whereby a first reactant, such as silicon tetraiodide or silicon hexaiodide, is introduced sequentially into a reaction zone containing a microelectronic device substrate with pulsed exposure of the substrate to ammonia, each set of pulses defining a cycle by initial pretreatment of the substrate with ammonia plasma. An additional pulse of ammonia plasma is introduced into the reaction zone after a selected number of cycles. In both ALD and pulsed CVD regimes, this periodic introduction of ammonia plasma into the reaction zone occurs after two or more cycles of silicon tetraiodide (or silicon hexaiodide) and ammonia pulses. In certain embodiments, the ammonia plasma is periodically introduced after 3, 5, 10, 50, 100, 150, 200 or 1000 such cycles, or any such pulse cycles in the range of 3 to 1000. In other words, the ammonia plasma is introduced at least once after the initial surface treatment, and may be introduced multiple times at regular or irregular intervals in the range of 3 to 1000 cycles. As shown in the experimental results below, pretreatment of the substrate with ammonia plasma resulted in highly selective deposition of silicon nitride, but this selectivity began to dissipate after achieving a silicon nitride film thickness of about 10 nm (100 Å). Advantageously, treatment with ammonia plasma after every 200 cycles (in the ALD examples herein) significantly improved the selectivity.
[0013] In the practice of the invention, suitable temperatures are from about 150° C. to about 400° C. and pressures are less than about 15 Torr. In other embodiments, the temperature is from about 175° C. to about 350° C., or from about 200° C. to about 250° C. Selective deposition is achieved when a silicon nitride film deposits on some of the exposed surfaces at some manufacturable rate, while other surfaces receive negligible or easily removed amounts of silicon nitride.
[0014] In certain embodiments, one of the microelectronic device surfaces on which silicon nitride deposition is desired (i.e., the "first" surface) comprises a silicon nitride surface. In other embodiments, such a first surface is selected from oxides such as silicon dioxide, germanium oxide, SiOC, SiOF, silicon carbide, silicon oxynitride, and low-k substrates. In some embodiments, the dielectric is a porous material. In some embodiments, the porous dielectric comprises pores that are connected to one another, while in other embodiments, the pores are not connected to one another. In some embodiments, the dielectric comprises a low-k material, which is defined as an insulator having a dielectric value less than about 4.0. In some embodiments, the dielectric value of the low-k material is less than about 3.5, less than about 3.0, less than about 2.5, or less than about 2.3. In some embodiments, the first surface comprises Si-O bonds.
[0015] In certain embodiments, the microelectronic device also has a substrate or surface (i.e., a "second" surface) on which silicon nitride deposition is not desired. In one embodiment, the second surface is aluminum oxide. In other embodiments, the second surface is selected from titanium nitride, tantalum nitride, aluminum nitride, hafnium oxide, zirconium oxide, aluminum oxide, titanium oxide, tantalum oxide, niobium oxide, lanthanum oxide, yttrium oxide, magnesium oxide, calcium oxide, strontium oxide, and combinations thereof.
[0016] In a particular embodiment, the device substrate is comprised of at least one silicon dioxide surface and at least one aluminum oxide surface, whereby silicon nitride is selectively deposited on the aluminum oxide surface.
[0017] In a particular embodiment, the device substrate is comprised of at least one silicon dioxide surface and at least one zirconium dioxide surface, and silicon nitride is selectively deposited on at least one of the zirconium dioxide surfaces.
[0018] In a particular embodiment, the device substrate is comprised of at least one silicon dioxide surface and at least one aluminum oxide surface, and the device surfaces are pretreated with an ammonia plasma and subsequently cyclically treated with an ammonia plasma as described herein, whereby silicon nitride is selectively deposited on the at least one silicon dioxide surface.
[0019] In a particular embodiment, the device substrate is comprised of at least one silicon dioxide surface and at least one hafnium oxide surface, and the device surfaces are pretreated with an ammonia plasma whereby silicon nitride is selectively deposited on the at least one silicon dioxide surface, followed by a cyclic treatment with an ammonia plasma as described herein.
[0020] In a particular embodiment, the device substrate is comprised of at least one silicon dioxide surface and at least one zirconium dioxide surface, and the device surfaces are pretreated with an ammonia plasma whereby silicon nitride is selectively deposited on the at least one silicon dioxide surface, followed by a cyclic treatment with an ammonia plasma as described herein.
[0021] In such embodiments, the term "selectively deposit" or "selectivity" is intended to reflect the preferential deposition of silicon nitride on one surface over another. A numerical definition is given by Gladfelter as the difference in coverage between two surfaces normalized to the sum of the coverage of the same two surfaces [Chem. Mater. 5, 1372 (1993)]. In practice, the selectivity of the method generally depends on the thickness of the film. The present invention allows for selectivity of greater than about 89% at a thickness of 97 Å. In other embodiments, preferential deposition of silicon nitride on one surface over another occurs with an occurrence of greater than 99% at thicknesses of greater than 190 Å.
[0022] This methodology utilizes silicon tetraiodide (SiI4) or disilicon hexaiodide (Si2I6) as one "silicon" precursor and utilizes a nitrogen-containing material as a co-reactant or another precursor. The nitrogen-containing material can be organic (e.g., t-butylhydrazine, methylhydrazine, 1,1-dimethylhydrazine, 1,2-dimethylhydrazine, alkylamines or pyridines) or inorganic (e.g., ammonia or hydrazine). In some embodiments, a mixture of nitrogen-containing materials may be utilized as the ALD precursor, and in other embodiments, only one nitrogen-containing material may be utilized as the ALD precursor (e.g., only ammonia or only t-butylhydrazine). As used herein, the term "nitrogen-containing material" may be utilized to refer to a pure (e.g., completely ammonia or completely t-butylhydrazine) precursor material or may refer to a precursor that contains a "nitrogen-containing material" as part of a mixture of nitrogen-containing materials. In certain embodiments, the deposition of the present invention can be used to form materials that include silicon and nitrogen. Such materials may comprise, consist essentially of, or consist of silicon nitride and / or have other components.
[0023] In one embodiment, microelectronic devices having surfaces or substrates of different composition are pretreated with ammonia plasma, followed by periodic introduction of ammonia plasma after a selected number of cycles or pulses, thereby selectively depositing silicon nitride of about 0.3 to about 5.0 nanometers on silicon dioxide surfaces via nitrogen compounds such as silicon tetraiodide and ammonia, while no or limited deposition is achieved on some metal oxide surfaces (e.g., Al2O3, HfO2, and ZrO2).
[0024] In atomic layer deposition, successive processing steps are generally referred to as "pulses" or cycles. Thus, ALD methods are based on controlled, self-limiting surface reactions of precursor chemicals. The invention can be carried out with fully saturated reactions, or simply separate pulses of precursors and co-reactants, if more manufacturable. Gas-phase reactions are substantially avoided by alternating and sequentially contacting the substrate with the precursors. This can be carried out by moving the substrate from the regions of different reactants and co-reactants, or by alternating gas flows over a stationary substrate. In either case, the gas-phase reactants are separated from each other in time and on the substrate surface, for example, by removing excess reactants and / or reactant by-products from the reaction chamber between reaction pulses. In some embodiments, one or more substrate surfaces are contacted in alternating and sequential fashion with two or more gas-phase precursors or reactants. Contacting the substrate surface with a gas-phase reactant means that the reactant vapor is in contact with the substrate surface for a limited period of time. In other words, it can be understood that the substrate surface is exposed to each gas-phase reactant for a limited period of time.
[0025] Briefly, a substrate including at least a first surface and a second, different surface is heated to a suitable deposition temperature in the range of 150° C. to 400° C. at low pressure, typically less than about 0.5 to 15 Torr. In other embodiments, the temperature is about 175° C. to 350° C. or 200° C. to 250° C. The deposition temperature is generally maintained below the thermal decomposition temperature of the reactants, but high enough to avoid condensation of the reactants and provide activation energy for the desired "selective" surface reactions.
[0026] The surface of the substrate is contacted with the first reactant in the gas phase. In certain embodiments, a pulse of the first reactant in the gas phase is provided to the reaction space containing the substrate. In other embodiments, the substrate is moved into the reaction space containing the first reactant in the gas phase. Conditions are generally selected such that about one or less monolayers of the first reactant are self-limitingly adsorbed on the substrate surface. Appropriate contact times can be readily determined by one of skill in the art based on the particular conditions, substrate and reactor configuration. Excess first reactant and reaction by-products, if present, are removed from the substrate surface, for example by purging with an inert gas or by removing the substrate from the presence of the first reactant.
[0027] By purging, it is meant that the gas phase precursors and / or gas phase by-products are removed from the substrate surface, for example, by evacuating the chamber with a vacuum pump and / or by replacing the gas in the reactor with an inert gas such as argon or nitrogen. In certain embodiments, the purge time is about 0.05-20 seconds, about 1-10 seconds, or about 1-3 seconds. However, other purge times can be utilized as needed, such as when highly conformal step coverage is required for very high aspect ratio structures or other structures with complex surface morphology.
[0028] The surface of the substrate is contacted with a second gaseous reactant in the gas phase. In certain embodiments, a pulse of the second gaseous reactant is provided to the reaction space containing the substrate. In other embodiments, the substrate is moved to a reaction space containing the second reactant in the gas phase. Excess second reactant and gaseous by-products of the surface reaction, if present, are removed from the substrate surface. The contacting and removing steps are repeated until a thin film of desired thickness is selectively formed on the first surface of the substrate, each cycle leaving about one or less molecular monolayers. Additional steps can be included that involve alternating sequential contact of the surface of the substrate with other reactants to form more complex materials, such as ternary materials.
[0029] Each step of each cycle is generally self-limiting. Excess reactant precursor is provided at each step to saturate susceptible structure surfaces. Surface saturation ensures reactant occupation of all available reaction sites (subject to, for example, physical size or "steric hindrance" constraints), thus ensuring excellent step coverage. Typically, less than one molecular layer of material is deposited in each cycle, although in some embodiments, more than one molecular layer is deposited during a cycle.
[0030] Removing excess reactants can include evacuating a portion of the contents of the reaction space and / or purging the reaction space with helium, nitrogen, or another inert gas. In certain embodiments, purging can include turning off the flow of reactive gas while continuing to flow an inert carrier gas through the reaction space. In another embodiment, the purging step can use a vacuum step to remove excess reactants from the surface.
[0031] With respect to the ammonia plasma, the method may include a direct plasma generation method in which the plasma is generated directly in the reactor, or alternatively, a remote plasma generation method in which the plasma is generated "remote" from the reaction zone and the substrate and fed into the reactor. In this regard, an energy source, such as a radio frequency (RF) source, may provide sufficient power to the deposition chamber to ionize the ammonia gas introduced as a pretreatment step and then periodically introduced. In the step of treating with ammonia plasma, the power applied is greater than 200 W, and in certain embodiments, greater than about 250 W, greater than about 275 W, greater than about 300 W, greater than about 325 W, or even greater than about 350 W. For example, the power applied may be in the range of about 250 to about 500 W, in the range of about 300 to about 475 W, in the range of about 350 to about 450 W, or in the range of about 375 to about 425 W. During the step of ammonia plasma treatment, the power applied may optionally be varied, such as by increasing the power over the treatment period.
[0032] Exemplary flow rates of the ammonia plasma are at least 50 sccm, at least about 100 sccm, at least about 150 sccm, or at least about 175 sccm. In more specific aspects, the flow rate of the reducing gas is in the range of about 100 to about 400 sccm, in the range of about 150 to about 300 sccm, or in the range of about 175 to about 275 sccm. The amount of ammonia plasma flowing into the chamber can be optionally expressed in terms of the amount of ammonia plasma relative to the total gas (ammonia plasma and inert gas) flowing into the chamber during the ammonia plasma treatment step. For example, the amount of ammonia plasma can be in the range of about 10% to about 50%, about 15% to about 40%, or about 20% to about 35% of the total amount of gas flowing into the chamber during the ammonia plasma treatment step.
[0033] Reactors that can be used in the method of the present invention include ALD reactors and CVD reactors equipped with appropriate devices and means for providing reactants in a "pulsed" manner. According to certain embodiments, showerhead reactors can be used. Examples of suitable reactors that can be used include commercially available devices, as well as home-built reactors, and are known to those skilled in the art of CVD and / or ALD.
[0034] As used herein, the term "microelectronic device" corresponds to semiconductor substrates, including 3D NAND structures, logic devices, DRAM, power devices, flat panel displays and microelectromechanical systems (MEMS), fabricated for use in microelectronic components, integrated circuits or computer chip applications. It is to be understood that the term "microelectronic device" is not meant to be limiting in any way.
[0035] Insofar as the method of the present invention allows for highly selective deposition of silicon nitride, the resulting microelectronic device substrate is therefore advantageous by minimizing silicon nitride deposited on undesired surfaces.Thus, in a further aspect, the present invention provides a microelectronic device having multiple surfaces of different composition, comprising at least one first surface comprising at least one surface selected from silicon nitride, silicon dioxide, germanium oxide, SiCO, SiC, SiON, SiOF and low-k substrates, and one surface comprising at least one second surface selected from titanium nitride, tantalum nitride, aluminum nitride, hafnium oxide, zirconium oxide, aluminum oxide, titanium oxide, tantalum oxide, niobium oxide, lanthanum oxide, yttrium oxide, magnesium oxide, calcium oxide and strontium oxide.
[0036] In one embodiment, the invention provides a microelectronic device having multiple surfaces of different composition, the microelectronic device comprising at least one first surface comprising at least one surface selected from silicon nitride, silicon dioxide, germanium oxide, SiCO, SiC, SiON, SiOF and a low-k substrate, and a second surface comprising at least one surface selected from titanium nitride, tantalum nitride, aluminum nitride, hafnium oxide, zirconium oxide, aluminum oxide, titanium oxide, tantalum oxide, niobium oxide, lanthanum oxide, yttrium oxide, magnesium oxide, calcium oxide, strontium oxide, the first surface having deposited thereon a silicon nitride film having a thickness of at least 200 Å and the second surface having deposited thereon a silicon nitride film having a thickness of about 3 Å or less.
[0037] In another embodiment, the invention provides a microelectronic device having surfaces of different composition, including at least one surface comprising silicon dioxide and at least one surface comprising aluminum oxide, the surface comprising silicon dioxide having deposited thereon a silicon nitride film having a thickness of at least 200 Å, and the surface comprising aluminum oxide having deposited thereon a silicon nitride film having a thickness of about 3 Å or less.
[0038] The present invention can be further illustrated by the following examples of specific embodiments thereof, however, it will be understood that these examples are included for illustrative purposes only and are not intended to limit the scope of the invention unless specifically stated. EXAMPLES
[0039] [Example 1] In this example, silicon nitride was selectively deposited on a first surface of a substrate relative to a second, third, and fourth distinct surfaces of the substrate. The first surface of the substrate comprised native silicon oxide. The second surface of the substrate comprised Al2O3 deposited by ALD. The third surface of the substrate comprised HfO2 deposited by ALD. The fourth surface of the substrate comprised ZrO2 deposited by ALD. Prior to deposition of silicon nitride, the substrate was subjected to an ammonia plasma treatment method.
[0040] Silicon nitride films were selectively deposited by an ALD method using silicon tetraiodide (SiI4) as the first precursor and ammonia as the second precursor. Silicon tetraiodide was contained in a ProE-Vap ampoule and heated to 100°C. N2 carrier gas flowed over the surface of the solid silicon tetraiodide carrying silicon tetraiodide vapor into the heated chamber with the substrate at a temperature of 200°C and a reaction chamber pressure of 1.5 Torr. Each deposition cycle included a 10 second silicon tetraiodide vapor pulse, a 3 second inert N2 purge, a 10 second ammonia pulse and a 3 second inert N2 purge. With reference to Figure 1, samples were deposited using an ALD method consisting of 100 to 600 deposition cycles and the thickness of the material deposited on the first plasma treated native silicon oxide surface was measured and compared to the thickness of the material deposited on the second, third and fourth plasma treated Al2O3, HfO2 and ZrO2 surfaces. Figure 1 shows that silicon nitride deposition on plasma-treated native silicon oxide surfaces had very high selectivity (selectivity above 95%) compared to plasma-treated Al2O3 surfaces up to 400 cycles. However, plasma-treated HfO2 and ZrO2 surfaces showed the same selectivity of 95% only up to 300 cycles.
[0041] [Example 2] In this example, silicon nitride was selectively deposited on a first surface of a substrate relative to a second, third, and fourth distinct surfaces of the substrate. The first surface of the substrate comprised native silicon oxide. The second surface of the substrate comprised Al2O3 deposited by ALD. The third surface of the substrate comprised HfO2 deposited by ALD. The fourth surface of the substrate comprised ZrO2 deposited by ALD. Prior to deposition of silicon nitride, the substrate was subjected to an ammonia plasma treatment method. After every 200 deposition cycles, the ammonia plasma treatment method was reapplied to all surfaces of the substrate. Referring to FIG. 2, samples were deposited using an ALD method consisting of 200-800 deposition cycles, and the thickness of the material deposited on the first plasma-treated native silicon oxide surface was measured and compared to the thickness of the material deposited on the second, third, and fourth plasma-treated Al2O3, HfO2, and ZrO2 surfaces. Figure 2 shows that silicon nitride deposition on the plasma-treated natural silicon oxide surface had very high selectivity compared to the plasma-treated Al2O3 surface up to 800 cycles (selectivity above 95%). However, the plasma-treated HfO2 and ZrO2 surfaces showed the same selectivity of 95% only up to 600 and 400 cycles, respectively. Comparing Figures 1 and 2, the selectivity between the natural silicon oxide and all the other three surfaces is significantly improved by reapplying the ammonia plasma treatment method.
[0042] [Example 3] In this example, the refractive index (RI) of silicon nitride films deposited using the methods described in Examples 1 and 2 was measured using spectroscopic ellipsometry. The reapplication frequency of different ammonia plasma treatments was varied from every 200 cycles to every 50 cycles. Comparing no reapplication to the RI of the bulk silicon nitride films, reapplication every 50 cycles significantly improved the RI of the deposited silicon nitride films.
[0043] Aspects In a first aspect, the invention provides a method for depositing a silicon nitride film on a microelectronic device substrate having multiple surfaces of differing composition, comprising: a. contacting the substrate with pulsed silicon tetraiodide or disilicon hexaiodide and a nitrogen-containing co-reactant under deposition conditions at a temperature of about 150° C. to about 400° C. and a pressure of less than about 15 Torr, thereby defining a pulse cycle; Including, b. The substrate is (i) pretreated with ammonia plasma; (ii) the substrate is then periodically further treated with ammonia plasma; A method is provided.
[0044] In a second aspect, the present invention provides a method of the first aspect, wherein the substrate is further treated with ammonium plasma at least once within the range of every 10 pulse cycles to every 1000 pulse cycles.
[0045] In a third aspect, the present invention provides a method according to the first or second aspect, wherein the substrate is further treated with an ammonia plasma every 15 pulse cycles.
[0046] In a fourth aspect, the present invention provides a method according to the first or second aspect, wherein the substrate is further treated with an ammonia plasma after every 20 pulse cycles.
[0047] In a fifth aspect, the present invention provides a method of the first or second aspect, wherein the substrate is further treated with an ammonia plasma every 25 pulse cycles.
[0048] In a sixth aspect, the present invention provides a method according to the first or second aspect, wherein the substrate is further treated with an ammonia plasma every 30 pulse cycles.
[0049] In a seventh aspect, the present invention provides a method of the first or second aspect, wherein the substrate is further treated with an ammonia plasma every 35 pulse cycles.
[0050] In an eighth aspect, the present invention provides a method according to the first or second aspect, wherein the substrate is further treated with an ammonia plasma every 40 pulse cycles.
[0051] In a ninth aspect, the present invention provides a method of the first or second aspect, wherein the substrate is further treated with an ammonia plasma every 45 pulse cycles.
[0052] In a tenth aspect, the present invention provides a method of the first or second aspect, wherein the substrate is further treated with ammonia plasma at least once within the range of every 50 pulse cycles to every 200 pulse cycles.
[0053] In an eleventh aspect, the present invention provides a method according to any of the first to tenth aspects, wherein silicon nitride is deposited on a surface selected from silicon nitride, silicon dioxide, germanium oxide, SiCO, SiC, SiON, SiOF and a low-k substrate.
[0054] In a twelfth aspect, the present invention provides a method according to any one of the first to tenth aspects, wherein the silicon nitride film is deposited on a surface selected from silicon nitride, silicon dioxide, germanium oxide, SiCO, SiC, SiON, SiOF and a low-k substrate with a selectivity of about 85 to about 99% over deposition on a surface selected from titanium nitride, tantalum nitride, aluminum nitride, hafnium oxide, zirconium oxide, aluminum oxide, titanium oxide, tantalum oxide, niobium oxide, lanthanum oxide, yttrium oxide, magnesium oxide, calcium oxide, strontium oxide and combinations thereof.
[0055] In a thirteenth aspect, the present invention provides a method of any one of the first to tenth aspects, wherein the device substrate comprises at least one surface comprised of silicon dioxide and at least one surface comprising aluminum oxide, and wherein the method preferentially deposits silicon nitride over silicon dioxide with about 99% selectivity in a silicon nitride film deposited on the silicon dioxide surface, the silicon nitride film having a thickness of about 200 Å.
[0056] In a fourteenth aspect, the invention provides the method of any one of the first to tenth aspects, wherein the device substrate comprises at least one surface comprised of silicon dioxide and at least one surface comprising aluminum oxide, and wherein the method preferentially deposits silicon nitride over silicon dioxide with about 99% selectivity in a silicon nitride film deposited on the silicon dioxide surface, the silicon nitride film having a thickness of at least about 50 Å.
[0057] In a fourteenth aspect, the present invention provides a microelectronic device having multiple surfaces of different composition, the microelectronic device comprising at least one first surface comprising at least one surface selected from silicon nitride, silicon dioxide, germanium oxide, SiCO, SiC, SiON, SiOF and a low-k substrate, and one surface comprising at least one second surface selected from titanium nitride, tantalum nitride, aluminum nitride, hafnium oxide, zirconium oxide, aluminum oxide, titanium oxide, tantalum oxide, niobium oxide, lanthanum oxide, yttrium oxide, magnesium oxide, calcium oxide, strontium oxide, the first surface having deposited thereon a silicon nitride film having a thickness of about 200 Å and the second surface having deposited thereon a silicon nitride film having a thickness of about 3 Å or less.
[0058] In a fifteenth aspect, the present invention provides a microelectronic device having a plurality of surfaces of different composition, including at least one surface comprising silicon dioxide and at least one surface comprising aluminum oxide, the surface comprising silicon dioxide having deposited thereon a silicon nitride film having a thickness of about 200 Å and the surface comprising aluminum oxide having deposited thereon a silicon nitride film having a thickness of about 3 Å or less.
[0059] Having thus described several exemplary embodiments of the present disclosure, those skilled in the art will readily appreciate that still other embodiments may be made and used within the scope of the appended claims. Many advantages of the present disclosure, which are covered by this document, have been set forth in the foregoing description. It will be understood, however, that the present disclosure is in many respects merely illustrative. The scope of the present disclosure is, of course, to be defined in the language in which the appended claims are expressed.
Claims
1. 1. A method for depositing a silicon nitride film on a microelectronic device substrate having multiple surfaces of differing composition, comprising: a. contacting the substrate with pulsed silicon tetraiodide or disilicon hexaiodide and a nitrogen-containing co-reactant under deposition conditions at a temperature between about 150° C. and about 400° C. and a pressure less than about 15 Torr, thereby defining a pulse cycle; Including, b. the substrate has been (i) pretreated with an ammonia plasma; (ii) the substrate is then periodically further treated with an ammonia plasma; method.
2. The method of claim 1 , wherein the substrate is further treated with an ammonia plasma at least once within a range of every 10 pulse cycles to every 1000 pulse cycles.
3. The method of claim 1 , wherein the substrate is further treated with an ammonia plasma every 15 pulse cycles.
4. The method of claim 1 , wherein the substrate is further treated with an ammonia plasma every 20 pulse cycles.
5. The method of claim 1 , wherein the substrate is further treated with an ammonia plasma every 25 pulse cycles.
6. The method of claim 1 , wherein the substrate is further treated with an ammonia plasma every 30 pulse cycles.
7. The method of claim 1 , wherein the substrate is further treated with an ammonia plasma every 35 pulse cycles.
8. The method of claim 1 , wherein the substrate is further treated with an ammonia plasma every 40 pulse cycles.
9. The method of claim 1 , wherein the substrate is further treated with an ammonia plasma every 45 pulse cycles.
10. The method of claim 1 , wherein the substrate is further treated with an ammonia plasma at least once within the range of every 50 pulse cycles to every 200 pulse cycles.
11. 10. The method of claim 1, wherein the silicon nitride is deposited on a surface selected from silicon nitride, silicon dioxide, germanium oxide, SiCO, SiC, SiON, SiOF and a low-k substrate.
12. 2. The method of claim 1, wherein the silicon nitride film is deposited on a surface selected from silicon nitride, silicon dioxide, germanium oxide, SiCO, SiC, SiON, SiOF and low-k substrates with a selectivity of greater than about 85% over deposition on a surface selected from titanium nitride, tantalum nitride, aluminum nitride, hafnium oxide, zirconium oxide, aluminum oxide, titanium oxide, tantalum oxide, niobium oxide, lanthanum oxide, yttrium oxide, magnesium oxide, calcium oxide, strontium oxide and combinations thereof.
13. 10. The method of claim 1, wherein the device substrate comprises at least one surface comprised of silicon dioxide and at least one surface comprising aluminum oxide, and wherein the method preferentially deposits silicon nitride over the silicon dioxide with about 99% selectivity in a silicon nitride film deposited on the silicon dioxide surface, the silicon nitride film having a thickness of at least about 200 Å.
14. 10. The method of claim 1, wherein the device substrate comprises at least one surface comprised of silicon dioxide and at least one surface comprising aluminum oxide, and wherein the method preferentially deposits silicon nitride over the silicon dioxide with about 99% selectivity in a silicon nitride film deposited on the silicon dioxide surface, the silicon nitride film having a thickness of at least about 50 Å.
15. 1. A microelectronic device having a plurality of surfaces of differing composition, the at least one first surface comprising at least one surface selected from silicon nitride, silicon dioxide, germanium oxide, SiCO, SiC, SiON, SiOF and a low-k substrate, and a second surface comprising at least one surface selected from titanium nitride, tantalum nitride, aluminum nitride, hafnium oxide, zirconium oxide, aluminum oxide, titanium oxide, tantalum oxide, niobium oxide, lanthanum oxide, yttrium oxide, magnesium oxide, calcium oxide, strontium oxide, the first surface having a silicon nitride film deposited thereon having a thickness of at least 200 Å and the second surface having a silicon nitride film deposited thereon having a thickness of about 3 Å or less.
16. 1. A microelectronic device having a plurality of surfaces of differing composition, including at least one surface comprising silicon dioxide and at least one surface comprising aluminum oxide, the surface comprising silicon dioxide having a silicon nitride film deposited thereon having a thickness of at least 200 Å, and the surface comprising aluminum oxide having a silicon nitride film deposited thereon having a thickness of about 3 Å or less.
Citation Information
Patent Citations
Selective deposition of silicon nitride
JP2022523159A
Method for selective deposition of silicon nitride layer and structure including selectively-deposited silicon nitride layer
US20200286726A1
Selective deposition of silicon nitride
WO2020167972A1