Compound, rubber blend containing said compound, vehicle tire containing said rubber blend as at least one component, method for producing said compound, and use of said compound as ageing protectant and / or antioxidant - Patents.com

The use of N-(1,3-dimethylbutyl)-9H-carbazol-3-amine as an aging stabilizer and antiozonant in rubber mixtures addresses the health and efficacy issues of traditional stabilizers, providing effective oxidative protection with reduced toxicity and blooming.

JP2024544581AActive Publication Date: 2024-12-03CONTINENTAL REIFEN DEUTSCHLAND GMBH
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2024529490
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2021-12-02
Filing Date
2022-11-02
Publication Date
2024-12-03
Estimated Expiration
2042-11-02

AI Technical Summary

Technical Problem

Existing aging stabilizers for vehicle tires and technical rubber articles, such as aromatic amines, are suspected to be carcinogenic and pose health hazards while providing oxidative protection, and they tend to cause blooming, which affects their effectiveness and safety.

Method used

A compound with the formula N-(1,3-dimethylbutyl)-9H-carbazol-3-amine is used as an aging stabilizer and antiozonant, exhibiting similar protective effects to 6PPD but with lower toxicity and improved solubility in rubber mixtures, thereby reducing health risks and blooming.

Benefits of technology

The compound effectively stabilizes rubber articles against oxidation and ozone, maintaining performance while minimizing health hazards and blooming issues, making it a safer alternative to traditional stabilizers.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024544581000001_ABST
    Figure 2024544581000001_ABST
Patent Text Reader

Abstract

The present invention relates to a compound, a rubber blend containing said compound, a vehicle tire comprising said rubber blend as at least one component, a process for the preparation of said compound, and the use of said compound as an ageing protectant and / or antioxidant. JPEG2024544581000014.jpg35170.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a compound, a rubber mixture containing said compound, a vehicle tire comprising said rubber mixture as at least one component, a process for the preparation of said compound, and the use of said compound as ageing stabilizer and / or antioxidant. [Background technology]

[0002] Vehicle tires and technical rubber articles are known to employ polymeric materials, particularly rubber.

[0003] In case of long-term storage and in the intended application, which is often especially at high temperatures, natural rubber and synthetic polymers (such as IR, BR, SBR, ESBR, etc.), as well as natural and synthetic oils, fats and lubricants, undergo oxidation reactions that adversely affect their original desired properties. Depending on the type of polymer, the polymer chains shorten until the material liquefies or until subsequent hardening of the material occurs.

[0004] Ageing stabilizers therefore play a crucial role in the durability of vehicle tires and other technical rubber articles.

[0005] Known aging stabilizers are aromatic amines, e.g. 6-PPD (N-(1,3-dimethylbutyl)-N'-phenyl-p-phenylenediamine), IPPD (N-isopropyl-N'-phenyl-p-phenylenediamine) or SPPD (N-(1-phenylethyl)-N'-phenyl-p-phenylenediamine).

[0006] These molecules are capable of reacting with oxygen or ozone or with free radicals formed, such as alkyl, alkoxy and alkylperoxy radicals, thereby scavenging them and thus protecting the rubber etc. from further oxidation reactions.

[0007] However, a drawback of this substance class is that they are suspected of being carcinogenic.

[0008] Aging stabilizers that specifically react with ozone to achieve its scavenging are also called "antiozonants." Summary of the Invention [Problem to be solved by the invention]

[0009] The aim of the present invention is to provide new compounds which can be used in particular as ageing stabilizers for vehicle tyres or other technical rubber articles, and which in particular have a lower potential hazard, in combination with a sufficient solubility in the respective matrix, for example in particular in polymers, which are intended to prevent the tendency to blooming whilst maintaining an optimal protection against oxygen and ozone, reducing the hazards to health. [Means for solving the problem]

[0010] This object is achieved by the compounds according to the invention as claimed in claim 1, by rubber mixtures according to the invention which contain the compounds and by vehicle tyres according to the invention which contain a rubber mixture according to the invention in at least one component. The object is further achieved by a process for the preparation of the compounds and by the use of the compounds as ageing stabilizers and / or antioxidants and / or antiozonants.

[0011] The compound of claim 1 has the general formula I: [ka] has.

[0012] Thus, the compound of formula I) is N-(1,3-dimethylbutyl)-9H-carbazol-3-amine, or alternatively designated 3-(1,3-dimethylbutylamino)-9H-carbazole.

[0013] The compounds according to the invention show an ageing stabilizing effect in rubber mixtures similar to that of 6PPD and are therefore suitable as replacements for 6PPD, the degradation products of which are considered to be highly toxic to coho salmon and therefore probably also to other aquatic organisms.

[0014] The compounds according to the invention also surprisingly show very good solubility in rubber mixtures, especially in vehicle tires and other technical rubber articles, which is believed to be due to the 1,3-dimethylbutyl group on the nitrogen atom, although the invention is not bound by any particular mechanism of action or any particular theory. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0015] The present invention includes all advantageous embodiments, in particular those reflected in the claims. The present invention also includes embodiments resulting from combinations of different features having different priorities relative to these features, in particular so that the invention also includes combinations of a first feature described as "preferred" or in the context of an advantageous embodiment with a further feature, for example described as "particularly preferred".

[0016] The compounds of formula I) according to the invention are particularly suitable as ageing stabilizers and / or antiozonants in vehicle tyres and / or other technical rubber articles, such as air springs, bellows, conveyor belts, belts, drive belts, hoses, rubber bands, profiles, seals, membranes, tactile sensors for medical applications or for robotics, or shoe soles or parts thereof, and / or oils and / or lubricants.

[0017] The compounds according to formula I) of the invention are particularly suitable for the manufacture of rubber articles such as air springs, bellows, conveyor belts, belts, drive belts, hoses, rubber bands, profiles, seals, membranes, tactile sensors for medical applications or robotics, or shoe soles or parts thereof.

[0018] In order to use the compounds of formula I) in the articles or materials referred to, said compounds are used in and incorporated into compositions.

[0019] In vehicle tyres or other technical rubber articles, said composition is in particular in a rubber mix.

[0020] The present invention further provides the use of the compounds of the invention of formula I) in oils, lubricants, especially fuels or engine fluids, etc. Thus, the compounds according to the invention may be employed especially in engines.

[0021] As mentioned above, the present invention further provides a rubber mixture.

[0022] The rubber mixtures according to the invention contain a compound of formula I. The rubber mixtures according to the invention may in principle be any rubber mixture in which the novel inventive compound of formula I acts as an ageing stabilizer and / or antiozonant with low toxicity.

[0023] The rubber mixtures of the present invention contain at least one rubber.

[0024] It is preferred if the rubber mixtures according to the invention contain from 0.1 to 10 phr of compounds of formula I), particularly preferably from 0.1 to 6 phr and very particularly preferably from 1 to 5 phr.

[0025] The unit "phr" (parts per 100 parts by weight of rubber) used in this document is the conventional designation of quantities for mixture formulations in the rubber industry. The dosage of parts by weight of individual substances is used in this document to include all high molecular weight (M w based on 100 parts by weight of the total mass of rubber (whose molecular weight exceeds 20,000 g / mol).

[0026] In an advantageous embodiment of the invention, the rubber mixture according to the invention contains at least one diene rubber.

[0027] Thus, the rubber mixture may contain a diene rubber or a mixture of two or more different diene rubbers.

[0028] Diene rubbers are rubbers formed by polymerizing or copolymerizing dienes and / or cycloalkenes and therefore containing C=C double bonds in either the backbone or in side groups.

[0029] The diene rubber is preferably natural polyisoprene (NR), synthetic polyisoprene (IR), epoxidized polyisoprene (ENR), butadiene rubber (BR), butadiene-isoprene rubber, solution polymerized styrene-butadiene rubber (SSBR), emulsion polymerized styrene-butadiene rubber (ESBR), styrene-isoprene rubber, molecular weight M w is selected from the group consisting of liquid rubber having a molecular weight greater than 20,000 g / mol, halobutyl rubber, polynorbornene, isoprene-isobutylene copolymer, ethylene-propylene-diene rubber, nitrile rubber, chloroprene rubber, acrylate rubber, fluororubber, silicone rubber, polysulfide rubber, epichlorohydrin rubber, styrene-isoprene-butadiene terpolymer, hydrogenated acrylonitrile butadiene rubber, and hydrogenated styrene-butadiene rubber.

[0030] Nitrile rubber, hydrogenated acrylonitrile-butadiene rubber, chloroprene rubber, butyl rubber, halobutyl rubber and / or ethylene-propylene-diene rubber are used in particular for the manufacture of technical rubber articles such as belts, drive belts and hoses and / or shoe soles. Mixture compositions known to those skilled in the art for these rubbers, specific in terms of fillers, plasticizers, vulcanization systems and additives, are preferably employed.

[0031] The natural and / or synthetic polyisoprene of all embodiments may be cis-1,4-polyisoprene or 3,4-polyisoprene. However, it is preferred to use cis-1,4-polyisoprene with a cis-1,4 ratio of more than 90% by weight. Firstly, such polyisoprene is accessible by stereospecific polymerization in solution with Ziegler-Natta catalyst or with fine lithium alkyl. Secondly, natural rubber (NR) is such cis-1,4-polyisoprene that the cis-1,4 content in natural rubber is more than 99% by weight.

[0032] Mixtures of one or more natural polyisoprenes and one or more synthetic polyisoprenes are further contemplated.

[0033] In the context of the present invention, the term "natural rubber" should be understood to mean natural rubber that can be obtained from the Hevea rubber tree, and from "non-Hevea" sources, such as the guayule shrub and dandelions, such as TKS (Taraxacum kok-saghyz; Russian dandelion).

[0034] If the rubber mixture of the present invention contains butadiene rubber (i.e. BR, polybutadiene), this may be of any type known to those skilled in the art. These include those called high-cis and low-cis types, where polybutadienes with a cis content of 90% or more by weight are called high-cis types and polybutadienes with a cis content of less than 90% by weight are called low-cis types. An example of a low-cis polybutadiene is Li-BR (lithium catalyzed butadiene rubber) with a cis content of 20% to 50% by weight. With high-cis BR, particularly good properties and low hysteresis are achieved in the rubber mixture.

[0035] The polybutadienes employed may be end-group-modified and / or functionalized along the polymer chain with modifications and functionalizations. The modifications may be selected from modifications with hydroxyl groups and / or ethoxy groups and / or epoxy groups and / or siloxane groups and / or amino groups and / or aminosiloxane and / or carboxyl groups and / or phthalocyanine groups and / or silane-sulfide groups. However, further modifications known to those skilled in the art, also called functionalizations, are also useful. Metal atoms may be constituents of such functionalizations.

[0036] If at least one styrene-butadiene rubber (styrene-butadiene copolymer) is present in the rubber mixture, it may be selected from solution-polymerized styrene-butadiene rubber (SSBR) and emulsion-polymerized styrene-butadiene rubber (ESBR), it being possible to employ a mixture of at least one SSBR and at least one ESBR. The terms "styrene-butadiene rubber" and "styrene-butadiene copolymer" are used synonymously in the context of the present invention.

[0037] The styrene-butadiene copolymers employed may be end-group-modified and / or functionalized along the polymer chain by the modifications and functionalizations mentioned above for polybutadiene.

[0038] The at least one diene rubber is preferably selected from the group consisting of natural polyisoprene (NR, natural rubber), synthetic polyisoprene (IR), butadiene rubber (BR), solution polymerized styrene-butadiene rubber (SSBR), emulsion polymerized styrene-butadiene rubber (ESBR), butyl rubber (IIR) and halobutyl rubber.

[0039] In a particularly preferred embodiment of the present invention, the at least one diene rubber is selected from the group consisting of natural polyisoprene (NR), synthetic polyisoprene (IR), butadiene rubber (BR), solution polymerized styrene-butadiene rubber (SSBR) and emulsion polymerized styrene-butadiene rubber (ESBR).

[0040] In a particularly advantageous embodiment of the invention, the rubber mixture comprises at least one natural polyisoprene (NR), preferably in an amount of 50 to 100 phr, in one particularly advantageous embodiment of the invention in an amount of 80 to 100 phr, very particularly preferably 95 to 100 phr, then preferably 100 phr. Such rubber mixtures exhibit in particular optimized tear and wear properties combined with good processability and reversion stability.

[0041] If the rubber mixture contains less than 100 phr of NR, it preferably contains as further rubber at least one diene rubber selected from the group consisting of synthetic polyisoprene (IR), butadiene rubber (BR), solution polymerized styrene-butadiene rubber (SSBR) and emulsion polymerized styrene-butadiene rubber (ESBR).

[0042] In a further particularly advantageous embodiment of the invention, the rubber mixture comprises at least one natural polyisoprene (NR), preferably in an amount of 5 to 55 phr, and in one particularly advantageous embodiment of the invention in an amount of 5 to 25 phr, very particularly preferably in an amount of 5 to 20 phr. Such rubber mixtures exhibit particularly good processability and reversion stability as well as optimized tear properties and optimal rolling resistance characteristics.

[0043] In a further particularly advantageous embodiment of the invention, the rubber mixture comprises at least one polybutadiene (BR, butadiene rubber), preferably in an amount of 10 to 80 phr, particularly preferably 10 to 50 phr and in a particularly advantageous embodiment of the invention in an amount of 15 to 40 phr, whereby particularly good tear and wear properties as well as optimal braking characteristics of the rubber mixture according to the invention are achieved.

[0044] In a further particularly advantageous embodiment of the present invention, the rubber mixture comprises at least one solution polymerized styrene-butadiene rubber (SSBR), preferably in an amount of 10 to 80 phr, particularly preferably 30 to 80 phr, and in one particularly advantageous embodiment of the present invention in an amount of 50 to 70 phr. This achieves particularly good rolling resistance properties of the rubber mixture according to the invention. In a particularly advantageous embodiment of the present invention, the SSBR is employed in combination with at least one further rubber in order to achieve an optimal and balanced property profile.

[0045] It is preferred if the rubber mixture contains at least one filler, preferably in an amount of 30 to 500 phr, particularly preferably in an amount of 50 to 400 phr, then preferably in an amount of 80 to 300 phr.

[0046] In an advantageous embodiment of the invention, the filler is a reinforcing filler, preferably selected from the group consisting of carbon black and silicon dioxide.

[0047] Suitable carbon blacks include any carbon black type known to those skilled in the art. It is preferred if the carbon black is selected from technical carbon black and pyrolytic carbon black, with technical carbon black being more preferred.

[0048] The carbon black preferably has an iodine value according to ASTM D1510, also known as iodine adsorption, of 30 to 250 g / kg, preferably 30 to 180 g / kg, particularly preferably 40 to 180 g / kg, and further particularly preferably 40 to 130 g / kg, and a DBP value according to ASTM D2414 of 30 to 200 ml / 100 g, preferably 70 to 200 ml / 100 g, and particularly preferably 90 to 200 ml / 100 g.

[0049] The DBP value according to ASTM D2414 determines the specific absorption volume of dibutyl phthalate in carbon black or light colored fillers.

[0050] The use of such types of carbon black in rubber mixtures, particularly for vehicle tires, ensures an optimal compromise between wear resistance and heat storage, which in turn affects the ecologically relevant rolling resistance.

[0051] Particularly suitable and preferred carbon blacks are those having an iodine adsorption number of 80 to 110 g / kg and a DBP number of 100 to 130 ml / 100 g, such as in particular carbon black of type N 339.

[0052] The silicon dioxide is preferably amorphous silicon dioxide, for example precipitated silica, also called precipitated silicon dioxide. However, it is alternatively possible to use, for example, pyrogenic silicon dioxide.

[0053] However, it is particularly preferred to use finely divided precipitated silicas having a nitrogen surface area (BET surface area) (according to DIN ISO 9277 and DIN 66132) of 35 to 400 m2 / g, preferably 35 to 350 m2 / g, more preferably 85 to 320 m2 / g, most preferably 120 to 235 m2 / g and a CTAB surface area (according to ASTM D 3765) of 30 to 400 m2 / g, preferably 30 to 330 m2 / g, more preferably 80 to 300 m2 / g, most preferably 115 to 200 m2 / g. Such silicas result in particularly good physical properties of the vulcanized rubber, for example in rubber mixtures for tire treads. Advantages in the processing of the mixtures due to shortened mixing times can also be obtained while maintaining the same product properties, resulting in improved productivity. The silica used may thus be, for example, Ultrasil® VN3 type (trade name) from Evonik, or highly disperse silica known as HD silica (for example Zeosil® 1165 MP from Solvay).

[0054] In a particularly advantageous embodiment of the invention, the rubber mixture contains at least one silica as filler, preferably in an amount of 30 to 500 phr, particularly preferably in an amount of 50 to 400 phr, then preferably in an amount of 80 to 300 phr.

[0055] In these amounts, silica is especially present as the sole or predominant filler (greater than 50% by weight, based on the total amount of filler).

[0056] In a further advantageous embodiment of the invention, the rubber mixture contains at least one silica as further filler, preferably in an amount of 5 to 100 phr, particularly preferably 5 to 80 phr, then preferably 10 to 60 phr.

[0057] In these amounts, the silica is particularly present as an additional filler, especially in addition to other primary fillers such as carbon black.

[0058] The terms "silicic acid" and "silica" are used synonymously in the context of the present invention.

[0059] In a particularly advantageous embodiment of the invention, the rubber mixture according to the invention contains from 0.1 to 60 phr, preferably from 3 to 40 phr, particularly preferably from 5 to 30 phr and very particularly preferably from 5 to 15 phr of at least one carbon black. In these amounts, the carbon black is in particular present as a further filler, in addition to the main filler, such as silica.

[0060] In a further advantageous embodiment of the invention, the rubber mixture according to the invention contains from 30 to 300 phr, preferably from 30 to 200 phr, particularly preferably from 40 to 100 phr, of at least one carbon black, in these amounts being present alone or as the main filler, optionally in combination with silica in the amounts towards the lower limits mentioned above.

[0061] In a particularly advantageous embodiment of the invention, the rubber mixture contains from 5 to 60 phr, particularly preferably from 5 to 40 phr, of at least one carbon black and from 50 to 300 phr, preferably from 80 to 200 phr, of at least one silica.

[0062] The rubber mixture may further contain further reinforcing or non-reinforcing fillers.

[0063] In the context of the present invention, further (non-reinforcing) fillers include aluminosilicates, kaolin, chalk, starch, magnesium oxide, titanium dioxide, or rubber gels and fibres (eg aramid fibres, glass fibres, carbon fibres, cellulose fibres).

[0064] Further optionally, the reinforcing fillers are carbon nanotubes (CNTs), including, for example, discrete CNTs, so-called hollow carbon fibers (HCFs), and modified CNTs containing one or more functional groups such as hydroxyl, carboxyl, and carbonyl groups, graphite and graphene, and so-called "carbon-silica dual phase fillers."

[0065] In the context of the present invention, zinc oxide is not included in the filler.

[0066] The rubber mixture may further contain conventional additives in conventional parts by weight, which are preferably added in at least one primary mixing stage during the preparation of said mixture. These additives include: a) ageing stabilizers known in the art, For example, p-phenylenediamines, such as N-phenyl-N'-(1,3-dimethylbutyl)-p-phenylenediamine (6PPD), N-(1-phenylethyl)-N'-phenyl-p-phenylenediamine (SPPD), N,N'-diphenyl-p-phenylenediamine (DPPD), N,N'-ditolyl-p-phenylenediamine (DTPD), N-(1,4-dimethylpentyl)-N'-phenyl-p-phenylenediamine (7PPD), N-isopropyl-N'-phenyl-p-phenylenediamine (IPPD), or dihydroquinolines, such as 2,2,4-trimethyl-1,2-dihydroquinoline (TMQ), b) activators, such as zinc oxide and fatty acids (e.g. stearic acid) and / or other activators, such as zinc complexes, such as zinc ethylhexanoate; c) activators and / or agents for binding fillers, in particular carbon black or silica, such as S-(3-aminopropyl)thiosulfate and / or its metal salts (carbon black binding) and silane coupling agents (silica binding); d) antiozonant waxes; e) resins, especially tackifying resins; f) mastication aids, such as 2,2'-dibenzamidodiphenyl disulfide (DBD); g) processing aids, in particular fatty acid esters and metal soaps, for example zinc soaps and / or calcium soaps; h) plasticizers, for example in particular aromatic, naphthenic or paraffinic mineral oil plasticizers, for example MES (Mild Extraction Solvates), preferably having a content of polycyclic aromatic compounds of less than 3% by weight according to method IP 346, or RAE (Residual Aromatic Extract), or TDAE (Processed Distillate Aromatic Extract), or Rubber to Liquid (RTL) oils or Biomass to Liquid (BTL) oils, or triglycerides, for example rapeseed oil or factice, or hydrocarbon resins or liquid polymers with an average molecular weight (determined by GPC = Gel Permeation Chromatography in accordance with BS ISO 11344:2004) of 500 to 20 000 g / mol.

[0067] If a mineral oil is used, it is preferably selected from the group consisting of DAE (distillate aromatic extract), RAE (residual aromatic extract), TDAE (treated distillate aromatic extract), MES (light extract solvate), and naphthenic oils.

[0068] In a particularly advantageous embodiment, the rubber mixture according to the invention does not contain, in addition to the inventive compound of formula I), any ageing stabilizer from the group of p-phenylenediamines, in particular those listed above under a). In a particularly preferred embodiment, the rubber mixture according to the invention contains 0 to 0.1 phr, in particular 0 phr, based on p-phenylenediamine, of a further ageing stabilizer, which is selected from the group comprising, preferably consisting of, N-phenyl-N'-(1,3-dimethylbutyl)-p-phenylenediamine (6PPD), N-(1-phenylethyl)-N'-phenyl-p-phenylenediamine (SPPD), N,N'-diphenyl-p-phenylenediamine (DPPD), N,N'-ditolyl-p-phenylenediamine (DTPD), N-isopropyl-N'-phenyl-p-phenylenediamine (IPPD), N-(1,4-dimethylpentyl)-N'-phenyl-p-phenylenediamine (7PPD).

[0069] The very small amounts, preferably 0-0.1 phr, particularly preferably 0 phr, of the mentioned p-phenylenediamines and the compounds of formula I) present according to the invention make it possible to achieve the same protective effect with lower toxicity.The compounds of formula I) of the invention replace the mentioned p-phenylenediamines known in the prior art.

[0070] In a further advantageous embodiment of the present invention, since at least one further representative of the mentioned p-phenylenediamine aging stabilizers is present, the compounds according to the invention only partially replace the p-phenylenediamines known in the prior art, which also achieves the advantages according to the present invention only to a less than optimal extent.

[0071] In an advantageous embodiment, an ageing stabilizer of the dihydroquinoline type, such as TMQ, is present in the rubber mixture in addition to the compound of formula I) according to the invention. The amount of dihydroquinoline, in particular TMQ, present is preferably from 0.1 to 3, in particular from 0.5 to 1.5 phr.

[0072] The antiozonant waxes (group d above) are considered separately and, in a preferred embodiment of the invention, are present in the rubber mixture regardless of whether or not additional ageing stabilizers a) are present.

[0073] The silane coupling agent may be of any type known to those skilled in the art.

[0074] Additionally, one or more different silane coupling agents may be used in combination with one another, so that a rubber mixture may contain a mixture of different silanes.

[0075] Silane coupling agents react with surface silanol groups or other polar groups of silicon dioxide, especially silica, during mixing of the rubber / rubber mixture (in situ) or in pretreatment (pre-modification) situations, even before the addition of the filler to the rubber.

[0076] Coupling agents known from the prior art are bifunctional organosilanes which have at least one alkoxy, cycloalkoxy or phenoxy group as leaving group on the silicon atom and other functional groups which, possibly after cleavage, are capable of entering into a chemical reaction with the double bonds of the polymer. The latter groups may include, for example, the following chemical groups: -SCN, -SH, -NH2 or -Sx- (wherein x=2 to 8).

[0077] The silane coupling agents which can be used are therefore, for example, 3-mercaptopropyltriethoxysilane, 3-thiocyanatopropyltrimethoxysilane or 3,3'-bis(triethoxysilylpropyl) polysulfides having 2 to 8 sulfur atoms, such as 3,3'-bis(triethoxysilylpropyl)tetrasulfide (TESPT), the corresponding disulfides (TESPD) or other mixtures of sulfides having 1 to 8 sulfur atoms with different sulfides. TESPT can also be added, for example, as a mixture with industrial carbon black (trade name X50S®, manufactured by Evonik).

[0078] Blocked mercaptosilanes, such as known from WO 99 / 09036, can also be used as silane coupling agents. It is also possible to use silanes described in WO 2008 / 083241 A1, WO 2008 / 083242 A1, WO 2008 / 083243 A1 and WO 2008 / 083244 A1. Usable silanes include, for example, those sold by Momentive in the USA in numerous variants under the name NXT, such as in particular 3-octanoylthio-1-propyltriethoxysilane, or those sold by Evonik Industries under the name VP Si 363®.

[0079] The total proportion of further additives is preferably between 3 and 150 phr, more preferably between 3 and 100 phr, most preferably between 5 and 80 phr.

[0080] Zinc oxide (ZnO) may be included in the overall proportion of further additives in the amounts mentioned above.

[0081] This may be any type of zinc oxide known to the person skilled in the art, for example ZnO granules or powder. The zinc oxides normally used generally have a BET surface area of ​​less than 10 m2 / g. However, it is also possible to use zinc oxides with a BET surface area of ​​10 to 100 m2 / g, for example the so-called "nano zinc oxide".

[0082] The rubber mixtures according to the invention are preferably used in vulcanized form, in particular for vehicle tyres or other vulcanized technical rubber articles.

[0083] The terms "vulcanization" and "crosslinking" are used synonymously in the context of the present invention.

[0084] The vulcanization of the rubber mixture of the present invention is preferably carried out in the presence of sulfur and / or sulfur donors with the aid of vulcanization accelerators, some of which can simultaneously act as sulfur donors, selected from the group consisting of thiazole vulcanization accelerators, mercapto vulcanization accelerators, sulfenamide vulcanization accelerators, thiocarbamate vulcanization accelerators, thiuram vulcanization accelerators, thiophosphate vulcanization accelerators, thiourea vulcanization accelerators, xanthogenate vulcanization accelerators and guanidine vulcanization accelerators.

[0085] N-cyclohexyl-2-benzothiazolylsulfenamide (CBS), It is preferred to use a sulfenamide accelerator selected from N,N-dicyclohexylbenzothiazole-2-sulfenamide (DCBS), benzothiazyl-2-sulfene morpholide (MBS), N-tert-butyl-2-benzothiazylsulfenamide (TBBS), and guanidine accelerators such as diphenylguanidine (DPG).

[0086] The sulfur donor material used can be any sulfur donor material known to those skilled in the art.

[0087] Vulcanization retarders may also be present in the rubber mixture.

[0088] In other cases, the preparation of the rubber mixture according to the invention is preferably carried out by processes customary in the rubber industry, which include first preparing a primary mixture in one or more mixing stages, which contains all the components except the vulcanization system (e.g. sulfur and vulcanization-influencing substances), and the final mixture is produced by adding the vulcanization system in the final mixing stage.

[0089] The final mixture may be further processed and formed into a suitable shape, for example by an extrusion operation or by calendering.

[0090] The rubber mixture according to the invention is particularly suitable for use in vehicle tires, especially pneumatic vehicle tires.In principle, its use in all tire components, especially outer components, particularly preferably in the flange profile, tread and / or sidewall, is conceivable.In the case of treads with a cap / base structure, the rubber mixture according to the invention is preferably used at least in the cap.

[0091] For use in vehicle tires, the mixture, as a finished pre-vulcanized mix, is preferably formed into the corresponding shape of the outer component and applied in known manner during the manufacture of green vehicle tires.

[0092] The production of the rubber mixture according to the invention for use as any other body mixture in vehicle tires is carried out as described above. The difference lies in the shaping after the extrusion operation / calendering of the mixture. The shape of the rubber mixture thus obtained, not yet vulcanized, for one or more different body mixtures is then subjected to the production of green tires.

[0093] Here, "body mix" refers essentially to the rubber mix for the inner components of the tire, such as the squeegee, inner liner (inner layer), core profile, belt, shoulder, belt profile, carcass, bead reinforcement, bead profile, flange profile and bandage.

[0094] The green tire, which is not yet cured, is then cured.

[0095] For the use of the rubber mixture of the invention in drive belts and other belts, especially conveyor belts, the extruded, not yet vulcanized mixture is brought into a suitable shape and is often provided, simultaneously or subsequently, with reinforcing elements, such as synthetic fibers or steel cords, usually resulting in a multi-ply structure consisting of one and / or more plies of the rubber mixture, one and / or more plies of identical and / or different reinforcing elements and one and / or more further plies of the same and / or other rubber mixtures.

[0096] The present invention further provides a vehicle tyre comprising a rubber mixture according to the invention containing in at least one of its constituents a compound according to the invention.

[0097] The vulcanized vehicle tire in at least one component contains a vulcanizate of at least one rubber mixture according to the invention. It is known to those skilled in the art that most substances present, such as rubber, may be present already after mixing or only after vulcanization in a chemically modified form.

[0098] In the context of the present invention, "vehicle tires" should be understood as meaning pneumatic vehicle tires and solid rubber tires, including industrial tires, as well as tires for construction site vehicles, trucks, cars and motorcycles.

[0099] It is preferred if the vehicle tyre according to the invention comprises the rubber mixture according to the invention in at least one external component, which external component is preferably the tread, the sidewall and / or the flange profile.

[0100] Thus, the vehicle tyres according to the invention may contain the rubber mixtures according to the invention comprising the inventive compounds of formula I) in several components, optionally in a compatible composition.

[0101] The present invention further provides a process for the production of a compound of formula I), wherein the process comprises at least the following process steps: a1) Substances of formula A1) or A2): [ka] preparing a b1) providing methyl isobutyl ketone (MIBK) and hydrogen or a reducing agent; c1) reacting a compound of formula A1) or formula A2) with the material from step b1) to give a compound of formula I) [ka] The process of obtaining the above.

[0102] Compounds of formula A2) can be prepared as described in M. Takagi, Org. Biomol. Chem., 2019, 17(7), 1791-1795 and as shown in formula R1): [ka]

[0103] Alternatively, the compound of formula A2) can be prepared by nitration of 9H-carbazole (M. Yu, Supramol. Chem., 2008, 20(4), 357-361) to give the compound of formula A1), followed by reduction (M. Takagi, Org. Biomol. Chem., 2019, 17, 1791-1795), as shown in formulas R2) and R3): [ka]

[0104] The compounds of formula A1) can further be prepared by condensation of the corresponding hydrazine with cyclohexyl ketone and subsequent cyclization / aromatization as shown in formula R4) (BA Dalvi, Tet. Lett., 2018, 59, 2145-2149): [ka]

[0105] "Reducing agent" should be understood to mean a compound that allows reduction. As known to those skilled in the art, such agents include hydrides, in particular metal hydrides.

[0106] Suitable reducing agents are, in particular, sodium hydride (NaH), calcium hydride (CaH 2 ), sodium borohydride (NaBH 4 ), NaBH 3 CN, NaBH(OAc) 3 , 2-methylpyridine borane complex.

[0107] In the context of the present invention, hydrogen is explicitly mentioned as an alternative and is therefore not additionally listed as a "reducing agent", however, it will be understood that the term "reducing agent" encompasses any reagent that forms hydrogen in situ and thus performs hydrogenation.

[0108] The use of reducing agents other than hydrogen is especially conceivable when the reaction of step c1) is carried out starting from a compound of formula A2).

[0109] The reaction of step c1) is preferably carried out with hydrogen.

[0110] In reactions using hydrogen, a suitable catalyst is preferably additionally used, which in the context of the present invention is called a "hydrogenation catalyst".

[0111] The hydrogenation catalyst is preferably a noble metal catalyst, in particular palladium (Pd) or platinum (Pt). The noble metal is preferably employed on carbon (C), such as palladium on carbon (Pd / C).

[0112] Additionally, other known catalysts such as Raney nickel or copper chromite may also be used.

[0113] The reaction in step c1) is therefore particularly preferably carried out with hydrogen using a hydrogenation catalyst.

[0114] The reaction in step c1) is preferably carried out at a temperature between 80°C and 150°C, in particular at 120°C for example.

[0115] The reaction mixture is pressurized with hydrogen, preferably at a pressure of 35 to 45 bar, in particular for example 40 bar, and then preferably stirred for 1 to 20 hours, preferably for 3 to 13 hours, particularly preferably for 5 to 13 hours, in particular for example for 10 hours.

[0116] The reaction with hydrogen in step c1) is preferably carried out in a vessel suitable for relatively high pressures, such as in particular in an autoclave or another pressure reactor.

[0117] The reaction in step c1) is particularly preferably carried out with hydrogen using a hydrogenation catalyst at a temperature between 80° C. and 150° C., the reaction mixture is pressurized with hydrogen at a pressure of 25 to 45 bar, and the reaction is carried out in an autoclave or another pressure reactor.

[0118] The solvent in step c1) can be either MIBK, which simultaneously serves as a reactant, or an inert solvent such as toluene or xylene. In the latter case, MIBK is used only in stoichiometric amounts as a reactant. However, it is preferred that MIBK is simultaneously used as a solvent as well. This makes it possible to avoid additional substances such as toluene or xylene. Furthermore, unconverted MIBK can be recovered after the reaction and reused.

[0119] Preferably, step c1) is followed by purification, for example by column chromatography on silica gel.

[0120] As shown, the reaction in step c1) can be carried out starting either from a compound of formula A1) or from a compound of formula A2).

[0121] However, in step c1), it is preferred to directly convert the compound of formula A1) with hydrogen and MIBK, which achieves a relatively high yield.

[0122] The present invention will be more specifically clarified below with reference to examples. EXAMPLES

[0123] Compounds of formula I) were prepared according to the first synthetic route, as depicted in scheme X1), as follows: [ka]

[0124] A stainless steel autoclave equipped with a Teflon inliner was charged with 0.35 g (1.92 mmol, 1 equiv.) of 3-amino-9H-carbazole (compound of formula A2), 0.16 g of palladium on carbon (Pd / C) (5%) (0.4 g for 4.67 mmol of substrate), and 20.0 ml of methyl isobutyl ketone (MIBK). The reaction mixture was then pressurized under 40 bar of hydrogen (H 2 ) and stirred at 120° C. for 10 hours. After completion of the reaction, excess hydrogen was removed and the suspension was filtered through Celite®, followed by washing with ethanol. The filtrate was concentrated to dryness and dried under reduced pressure. The material was purified on silica gel (cyclohexane / ethyl acetate (EA) 10:1): off-white solid; yield 0.38 g (75% of theory). 1H-NMR (Nuclear Magnetic Resonance) (500MHz,DMSO-d6)δ=10.69(s,1H),7.94(dd,J=7.7,1.0Hz,1H),7.36(d,8.1Hz,1H),7.27(ddd,J= 8.2,7.0,1.2Hz,1H),7.24-7.19(m,3H),7.03(ddd,J=7.9,7.0,1.0Hz,1H),6.78(dd,J=8.5,2.3Hz,1H),4.75(d,J =9.0Hz,1H),3.62-3.47(m,1H),1.80(dp,J=13.5,6.7Hz,1H),1.51(dt,J=13.8,7.1Hz,1H),1. 25(dt,J=13.5,6.8Hz,2H),1.13(d,J=6.1Hz,3H),0.96(d,J=6.6Hz,3H),0.91(d,J=6.6Hz,3H). 13 C-NMR(126MHz,DMSO-d6)δ=142.3, 140.6, 132.9, 125.2, 123.6, 122.8, 120 .3, 117.9, 115.4, 111.9, 111.2, 102.1, 47.0, 46.7, 25.1, 23.4, 23.1, 21.3. ESI-MS (electrospray ionization mass spectrometry) [M+H] + =267. Melting point: 107℃

[0125] According to a further synthetic route, as shown in scheme X2), compounds of formula I) were prepared as follows: [ka]

[0126] A stainless steel autoclave equipped with a Teflon inliner was charged with 4.00 g (18.9 mmol, 1 equiv.) of 3-nitro-9H-carbazole (compound of formula A1), 1.60 g of platinum on carbon (Pt / C) (5%) (0.4 g for 4.67 mmol of substrate) and 50.0 ml of methyl isobutyl ketone. The reaction mixture was then pressurized with 40 bar of hydrogen and stirred at 120° C. for 10 h. After completion of the reaction, the excess hydrogen was blown off and the suspension was filtered through Celite®, followed by washing with ethanol. The filtrate was concentrated to dryness and dried under reduced pressure. The material was purified on silica gel (cyclohexane / EE 10:1): off-white solid; yield 4.40 g (88% of theory). <905 1 H-NMR, 13 Analysis of the product including C-NMR, ESI-MS, and melting point: same as above reaction according to Scheme X1).

[0127] For use in rubber mixtures for vehicle tyres, the compounds of formula I) according to the invention are added in one of the mixing stages during the preparation of the rubber mixture in a manner known to those skilled in the art, instead of ageing stabilizers known to those skilled in the art, such as, for example, 6PPD, 7PPD or IPPD.

[0128] Therefore, compounds of formula I) were incorporated in different amounts into exemplary rubber mixtures according to the invention, as shown in Table 1. The resulting examples of the invention are labelled E1 and E2.

[0129] Comparisons were made with rubber mixtures containing 6PPD instead of the compound of formula I) as ageing stabilizer, with the remaining composition being identical and with equimolar substitution of V1 with E1 and V2 with E2 in each case. The amounts in Table 1 are expressed in phr. A reference (Ref.) without ageing stabilizer is also reported.

[0130] In all mixtures, the sum of the amounts of aging stabilizer (6PPD or formula I) and plasticizer oil MES is 10 phr.

[0131] [Table 1]

[0132] The examples of the invention do not show a significant decrease in the ageing stabilization effect, and even show an improvement, compared to the rubber mixtures containing 6PPD.

Claims

1. Formula I): 【Chemistry 1】 Compound.

2. 2. Rubber mixtures containing a compound of formula I) according to claim 1.

3. 3. The rubber mixture according to claim 2, characterized in that it contains at least one diene rubber.

4. 4. The rubber mixture according to claim 3, characterized in that it contains at least one diene rubber selected from the group consisting of natural polyisoprene (NR), synthetic polyisoprene (IR), butadiene rubber (BR), solution polymerized styrene-butadiene rubber (SSBR), emulsion polymerized styrene-butadiene rubber (ESBR), butyl rubber (IIR) and halobutyl rubber.

5. A vehicle tyre comprising in at least one component a rubber mixture according to any one of claims 2 to 4.

6. 6. Vehicle tyre according to claim 5, characterized in that it contains at least one rubber mixture according to any one of claims 2 to 4 in at least one external component, said external component being preferably the tread, the sidewall and / or the flange profile.

7. A method for the preparation of a compound of formula I) according to claim 1, comprising at least the following process steps: a1) A substance of formula A1) or A2): 【Chemistry 2】 preparing a b1) providing methyl isobutyl ketone (MIBK) and hydrogen or a reducing agent; c1) reacting the compound of formula A1) or formula A2) with the material from step b1) to obtain the compound of formula I). 【Chemistry 3】 obtaining The method includes:

8. 8. The process according to claim 7, wherein the reaction in step c1) is carried out using a hydrogenation catalyst and / or with hydrogen at a temperature between 80° C. and 150° C. and / or the reaction mixture is pressurized with hydrogen at a pressure between 25 and 45 bar and the reaction is carried out in an autoclave or another pressure reactor.

9. Use of the compounds of formula I) according to claim 1 as ageing stabilizers and / or antiozonants, in particular in vehicle tyres and / or other technical rubber articles, such as in particular air springs, bellows, conveyor belts, belts, drive belts, hoses, rubber bands, profiles, seals, membranes, tactile sensors for medical applications or robotics, or shoe soles or parts thereof, and / or oils and / or lubricants.

10. Use of a compound of formula I) according to claim 1 for the manufacture of rubber articles, in particular air springs, bellows, conveyor belts, belts, drive belts, hoses, rubber bands, profiles, seals, membranes, tactile sensors for medical applications or robotics, or shoe soles or parts thereof.

11. 2. Use of compounds of formula I) according to claim 1 in oils, lubricants, especially fuels or engine fluids.

Citation Information

Patent Citations

  • Rubber composition and pneumatic tire

    JP2014152323A

  • Stabilization of organic compounds

    US2864676A

  • Rubber having enhanced resistance to degradation

    US2921922A

  • Lubricating grease compositions containing an alkylaminocarbazole

    US2990368A

  • Phenothiazine compound, its preparation and use in rubber blends and vehicle tires, as ageing protectant, antioxidant, antiozonant and colorant

    WO2022069001A1