Method for producing iron phosphate, method for producing lithium iron phosphate

A method for producing iron phosphate from sulfate slag using controlled leaching and calcination enhances metal recovery, addressing the underutilization and pollution issues of sulfate slag, thereby improving resource utilization and economic value.

JP2024544789AActive Publication Date: 2024-12-04HUBEI YUHAO HIGH-TECH NEW MATERIAL CO LTD

Patent Information

Application Number
JP2024537853
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2022-03-30
Filing Date
2022-11-30
Publication Date
2024-12-04
Estimated Expiration
2042-11-30

AI Technical Summary

Technical Problem

The high volume of sulfate slag generated in steel manufacturing is underutilized, leading to environmental pollution and economic inefficiency, with existing methods failing to effectively recover valuable metals and improve resource utilization.

Method used

A method involving the leaching of sulfate slag with phosphoric acid and sodium dihydrogen phosphate under controlled pH and pressure conditions, followed by solid-liquid separation and calcination, to produce iron phosphate and recover cobalt, copper, gold, and silver, enhancing the slag's value.

Benefits of technology

The method significantly increases the leaching rate of iron and recovers valuable metals, improving the resource utilization rate of sulfate slag and reducing environmental impact.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024544789000001_ABST
    Figure 2024544789000001_ABST
Patent Text Reader

Abstract

The present invention provides a method for producing iron phosphate and a method for producing lithium iron phosphate. The method for producing iron phosphate includes the steps of: uniformly mixing sulfate slag and sulfite with water to obtain a first mixture; adding phosphoric acid and a buffer to the first mixture to perform a leaching reaction; performing a first solid-liquid separation on the slurry obtained after the leaching reaction to obtain a first filtrate and a first filter cake; introducing air into the first filtrate to perform a first stirring reaction; performing a second solid-liquid separation on the slurry obtained after the first stirring reaction to obtain a second filtrate and a second filter cake; and calcining the second filter cake, the pressure of the leaching reaction is 0.25-0.5 MPa, the time is 1-2 hours, the pH of the reaction system of the leaching reaction is 1.5-3, and the buffer includes sodium dihydrogen phosphate and / or disodium hydrogen phosphate. The method for producing iron phosphate utilizes an iron source in sulfate slag, which can reduce the production cost of iron phosphate and is simple and easy to operate.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] This application claims priority to a Chinese patent application filed with the State Intellectual Property Office of the People's Republic of China on March 30, 2022, bearing application number 202210328818.0 and entitled "Method for producing iron phosphate and method for producing lithium iron phosphate," the entire contents of which are incorporated herein by reference.

[0002] The present invention relates to the technical field of batteries, and in particular to a method for producing iron phosphate and a method for producing lithium iron phosphate. [Background technology]

[0003] Sulfate slag has a history of more than 100 years as a raw material for steelmaking, etc., and the amount of sulfate slag discharged each year can reach more than 3 million tons, of which only 1 million tons can be rationally utilized, and the rest is discharged into the environment. When piled up, it occupies farmland and pollutes the land, and when discharged into rivers and streams, it pollutes the water.

[0004] Currently, there are many methods for comprehensively utilizing sulfate slag, and most sulfate slag is processed by the method of "sorting iron concentrate and producing bricks from the slag." As a raw material for steelmaking, sorting iron concentrate from sulfate slag with an iron content of 25% or more has a certain economic value, and the sorting process is not significantly different from the general iron ore sorting process. Depending on the specific magnetic coefficient of the iron minerals in the slag, gravity sorting or magnetic sorting can be used. The economic analysis is as follows: If the amount of sulfate slag sorted per year is 20,000 tons, and if the iron grade 60 concentrate is sorted from the iron grade 30 slag (iron grade ≧60% iron concentrate can be used for steelmaking as is), and the yield is 40%, 8,000 tons of iron concentrate can be produced per year. The price of iron grade 60 concentrate (sulfur content ≦0.5) is 110 yuan per ton, the production cost is 70 yuan, and the profit is 40 yuan, and the annual profit is 320,000 yuan. The total investment of one iron sorting plant is about 500,000 yuan, and the entire investment can be recovered in less than two years after starting production. After sorting the iron concentrate, 12,000 tons of slag remain, which can be used to make bricks. The sulfate slag itself does not have adhesive ability, but contains active substances such as SiO2 and AI2O3.

[0005] Sulfate slag can be used as raw material for sintering, and the iron-containing components in it are mainly utilized to reduce the production cost of sintering raw material. However, its poor spheroidization and high water absorption rate affect the sintering production rate. It also has a high sulfur content and contains harmful elements such as Cu, Pb and Zn, which affect the quality of sintering. The amount of sulfate slag added in the sintering material is generally less than 10%. By treating sulfate slag to increase its fineness, improve its iron content and reduce its sulfur content, it can be used as raw material for ore pellets. Some prior art uses a high-temperature chlorination process to chlorinate the metals contained in the slag, and then uses hydrometallurgy to leach precious metals such as gold and silver, and remove the harmful metals in the slag.

[0006] With the development of lithium iron phosphate, cheap iron sources are attracting attention. The price of ferrous sulfate crystals, a by-product of titanium dioxide, has been rising steadily, currently reaching 350 yuan / ton, with freight rates of about 70-90 yuan / ton. With the expansion of the production capacity of lithium iron, the price of ferrous sulfate crystals is rising and becoming more difficult to purchase. Therefore, there is an urgent need to develop a new iron source that is cheap and easy to obtain. The annual production volume of sulfate slag is very large, reaching several million tons, and the recycling rate is low.

[0007] In view of this, the present invention is proposed. Summary of the Invention [Problem to be solved by the invention]

[0008] In view of the above, the present invention aims to provide a method for producing iron phosphate and a method for producing lithium iron phosphate, which is simple and low-cost, and can recover cobalt, copper, gold, silver, sodium sulfate, etc. from sulfate slag, thereby significantly increasing the added value of sulfate slag and improving the resource utilization rate of sulfate slag. [Means for solving the problem]

[0009] The present invention relates to The method includes the steps of: uniformly mixing sulfate slag and sulfite with water to obtain a first mixture; adding phosphoric acid and a buffer to the first mixture to perform a leaching reaction; performing a first solid-liquid separation on a slurry obtained after the leaching reaction to obtain a first filtrate and a first filter cake; introducing air into the first filtrate to perform a first stirring reaction; performing a second solid-liquid separation on the slurry obtained after the first stirring reaction to obtain a second filtrate and a second filter cake; and calcining the second filter cake to obtain iron phosphate, The pressure of the leaching reaction is 0.25 to 0.5 MPa, and the time of the leaching reaction is 1 to 2 hours. The pH of the reaction system of the leaching reaction is 1.5 to 3. The buffer comprises sodium dihydrogen phosphate and / or disodium hydrogen phosphate, thereby providing a method for producing iron phosphate.

[0010] Preferably, the particle size of the sulfate slag is 80 to 120 mesh; Preferably, the molar ratio of the iron element in the sulfate slag to the sulfite, the phosphoric acid, and the buffer is 1:(0.35-0.4):(0.25-0.3):(1.7-1.75); Preferably, the phosphate and the buffer are added to the first mixture within 15 to 30 minutes; Preferably, the ratio of the amount of air introduced into the first filtrate per hour to the amount of ferrous ions in the first filtrate is (8 to 12) m 3 :(28~32) mol.

[0011] The temperature of the leaching reaction is 130 to 170°C. Preferably, the leaching reaction is carried out under stirring conditions.

[0012] Before introducing air into the first filtrate, the first filtrate is heated to 40 to 60° C. under stirring conditions; Preferably, the first stirring reaction is specifically The method includes stirring the first filtrate after the introduction of air until the content of iron element in the supernatant becomes 0.5 g / L or less, heating the first filtrate to 90 to 95°C, and then stirring for an additional 30 to 60 minutes.

[0013] The method further comprises washing and drying the second cake before calcining the second cake; Preferably, the temperature of the washing water for washing is 40 to 50° C., Preferably, washing is performed until the pH of the washing solution becomes 4.5 or more, Preferably, the water content of the second filter cake after drying is 0.5% or less.

[0014] The calcination temperature of the second filter cake is 650 to 680° C., Preferably, the time for calcining the second filter cake is 60 to 90 minutes.

[0015] The method for producing iron phosphate comprises: The method further includes the step of introducing the gas generated in the leaching reaction into a sodium hydroxide solution after the leaching reaction is completed to obtain sodium sulfite.

[0016] The method for producing iron phosphate comprises: The method further includes the steps of: cooling the second filtrate and performing a third solid-liquid separation to obtain sodium sulfate crystals and a mother liquor; adding sodium sulfide to the mother liquor to obtain a third filtrate and a third filter cake; adjusting the pH of the third filtrate to 9 to 10 and performing a fourth solid-liquid separation to obtain a fourth filtrate and a fourth filter cake; calcining the third filter cake and dissolving the calcined third filter cake in sulfuric acid to obtain a second mixture; and extracting, concentrating, and crystallizing the second mixture to obtain crude copper sulfate and crude cobalt sulfate, Preferably, the temperature of the second filtrate after cooling is 5 to 10° C., Preferably, the temperature for firing the third filter cake is 500 to 700 ° C., Preferably, the time for calcining the third filter cake is 2 to 4 hours.

[0017] The method for producing iron phosphate comprises: The method further includes the steps of adding aqua regia to the first filter cake that has been concentrated by flotation to obtain a third mixture, performing a fifth solid-liquid separation on the third mixture to obtain a fifth filtrate, adding sodium chloride to the fifth filtrate and then performing a sixth solid-liquid separation to obtain silver chloride and a sixth filtrate, and adding iron powder to the sixth filtrate to obtain coarse gold powder.

[0018] The present invention provides a method for producing lithium iron phosphate, which includes the above-mentioned method for producing iron phosphate.

[0019] The method for producing the lithium iron phosphate is simple and low cost. Effect of the Invention

[0020] Compared with the prior art, the beneficial effects of the present invention are as follows: (1) The method for producing iron phosphate according to the present invention skillfully utilizes high-pressure reduction leaching to dissolve ferric oxide and red iron oxide, which are difficult to dissolve in acid, and at the same time uses a mixed solution of phosphoric acid and sodium dihydrogen phosphate to leach the reduced iron salt to obtain a ferrous dihydrogen phosphate solution. At the same time, the high pH can prevent the dissolution of some aluminum, calcium, magnesium, etc., and thus greatly improve the iron leaching rate, and the leached iron can be used to produce iron phosphate. (2) The method for producing iron phosphate according to the present invention can also recover cobalt, copper, gold, silver, sodium sulfate, and the like from sulfate slag, thereby significantly increasing the added value of sulfate slag and improving the resource utilization rate of sulfate slag. (3) The method for producing lithium iron phosphate according to the present invention is simple and low cost. [Brief description of the drawings]

[0021] In order to more clearly describe the specific embodiments of the present invention or the technical solutions in the prior art, the drawings necessary for describing the specific embodiments or the prior art will be briefly introduced below. Obviously, the drawings in the following description are only some embodiments of the present invention, and those skilled in the art can further obtain other drawings based on these drawings without creative labor. [Figure 1] FIG. 2 is a diagram showing the results of observing iron phosphate with a scanning electron microscope according to an embodiment of the present invention. [Diagram 2] FIG. 11 is a diagram showing the results of observing iron phosphate with a scanning electron microscope according to another embodiment of the present invention. [Diagram 3] FIG. 13 is a diagram showing the results of particle size distribution of iron phosphate according to yet another embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0022] The technical means of the present invention will be described below clearly and completely with reference to the drawings and specific embodiments. Those skilled in the art should understand that the examples described below are only some of the examples of the present invention, not all of the examples, and are only for illustrating the present invention and do not limit the scope of the present invention. Based on the examples of the present invention, all other examples obtained by those skilled in the art without creative labor are within the scope of protection of the present invention. In the examples, specific conditions are not specified, but are in accordance with normal conditions or conditions proposed by the manufacturer. In the examples, the manufacturers of the reagents or instruments used are not specified, and are all normal products available on the market.

[0023] One aspect of the present invention is The present invention relates to a method for producing iron phosphate, the method including the steps of: uniformly mixing sulfate slag and sulfite with water to obtain a first mixture; adding phosphoric acid and a buffer to the first mixture to perform a leaching reaction; performing a first solid-liquid separation on a slurry obtained after the leaching reaction to obtain a first filtrate and a first filter cake; introducing air into the first filtrate to perform a first stirring reaction; performing a second solid-liquid separation on the slurry obtained after the first stirring reaction to obtain a second filtrate and a second filter cake; and calcining the second filter cake, wherein the pressure of the leaching reaction is 0.25 to 0.5 MPa, the pH of the reaction system of the leaching reaction is 1.5 to 3, and the buffer includes sodium dihydrogen phosphate and / or disodium hydrogen phosphate.

[0024] In some specific embodiments, the pressure of the leaching reaction may be, for example, but not limited to, 0.25 MPa, 0.3 MPa, 0.35 MPa, 0.4 MPa, 0.45 MPa, or 0.5 MPa.

[0025] In some specific embodiments, the pH of the reaction system of the leaching reaction may be, for example, but not limited to, 1.5, 2, 2.5, or 3.

[0026] Sulfate slag is a slag produced by the process of producing sulfuric acid from pyrite, and is also called pyrite tailings or calcined tailings. It is a type of chemical waste. The slag contains iron, so it can be used as a raw material in steel metallurgy. The content of iron-containing oxides (Fe2O3, Fe3O4, FeO) in sulfate slag is about 20-50%, the content of silica is about 15-65%, the content of alumina is about 10%, the content of calcium oxide is about 5%, the content of magnesium oxide is 5% or less, the content of sulfur is about 1-2%, and it usually further contains copper, cobalt, lead, zinc, gold and silver. Triiron tetroxide forms dense triiron tetroxide through the passivation action of sulfuric acid.

[0027] The method for producing iron phosphate according to the present invention skillfully utilizes high-pressure reduction leaching to dissolve triiron tetroxide and red iron oxide, which are difficult to dissolve in acid, and at the same time uses a mixed solution of phosphoric acid and sodium dihydrogen phosphate to leach the reduced iron salt to obtain a ferrous dihydrogen phosphate solution. At the same time, the pH of the leaching reaction system is controlled to 1.5 to 3, which prevents the dissolution of some of the aluminum, calcium, magnesium, etc. and improves the leaching rate of iron.

[0028] Phosphoric acid can supply hydrogen ions, and at the same time, sodium dihydrogen phosphate and disodium hydrogen phosphate are buffer solutions that can replenish hydrogen ions after the hydrogen ions of phosphate ions are consumed, and can prevent the pH of the solution from being too low to leach other impurities.

[0029] The leaching reaction of the present invention is carried out under specific leaching conditions, which greatly improves the leaching rate, and by adding sulfite, it exhibits reductive properties in an acidic environment, reduces trivalent iron ions to divalent iron ions, further improving the leaching rate and finally obtaining ferrous dihydrogen phosphate. At the same time, a ferrous dihydrogen phosphate solution is produced in a weakly acidic environment and in an environment where a large amount of dihydrogen phosphate ions are present.

[0030] Preferably, the sulfite comprises sodium sulfite and / or potassium sulfite.

[0031] Preferably, the particle size of the sulfate slag is 80 to 120 mesh.

[0032] In some specific embodiments, the particle size of the sulfate slag may be, for example, but not limited to, 80 mesh, 90 mesh, 100 mesh, 110 mesh, or 120 mesh.

[0033] Preferably, the molar ratio of the iron element in the sulfate slag, the sulfite, the phosphoric acid, and the buffering agent is 1:(0.35-0.4):(0.25-0.3):(1.7-1.75).

[0034] In some specific embodiments, the molar ratio of the iron element in the sulfate slag to the sulfite, the phosphate, and the buffering agent may be, for example, but not limited to, 1:0.35:0.25:1.7, 1:0.37:0.28:1.173, or 1:0.4:0.3:1.75.

[0035] Preferably, the phosphate and the buffering agent are added to the first mixture system within 15 to 30 minutes (eg, 15 minutes, 20 minutes, 25 minutes, or 30 minutes).

[0036] Preferably, the ratio of the amount of air introduced into the first filtrate per hour to the amount of ferrous ions in the first filtrate is (8 to 12) m 3 :(28~32) mol.

[0037] In some specific embodiments, the ratio of the amount of air introduced into the first filtrate per hour to the ferrous ions in the first filtrate may be, for example, but not limited to, 8:28, 10:30, or 12:32.

[0038] Preferably, the temperature of the leaching reaction is 130 to 170°C.

[0039] In some specific embodiments, the temperature of the leaching reaction may be, for example, but not limited to, 130°C, 140°C, 150°C, 160°C, or 170°C.

[0040] Preferably, the leaching reaction time is 1 to 2 hours.

[0041] In some specific embodiments, the time of the leaching reaction may be, for example, but not limited to, 1 hour, 1.2 hours, 1.4 hours, 1.6 hours, 1.8 hours, or 2 hours.

[0042] Preferably, the leaching reaction is carried out under stirring conditions.

[0043] Preferably, before air is introduced into the first filtrate, the first filtrate is heated to 40 to 60° C. (for example, 40° C., 45° C., 50° C., 55° C., or 60° C.) under stirring.

[0044] Preferably, the first stirring reaction specifically includes stirring the first filtrate after air is introduced until the content of iron element in the supernatant becomes 0.5 g / L or less, heating the first filtrate to 90 to 95°C (e.g., 90°C, 91°C, 92°C, 93°C, 94°C, or 95°C), and then stirring for an additional 30 to 60 min (e.g., 30 min, 35 min, 40 min, 45 min, 50 min, 55 min, or 60 min).

[0045] Preferably, the method further comprises washing and drying the second filter cake before calcining it.

[0046] Preferably, the washing temperature is 40 to 50° C. (eg, 40° C., 42° C., 44° C., 46° C., 48° C., or 50° C.).

[0047] Preferably, washing is performed until the pH of the washing solution becomes 4.5 or higher (eg, 4.5, 4.8, 5, 5.5, 6, or 6.5).

[0048] Preferably, the moisture content of the second filter cake after drying is 0.5% or less (e.g., 0.1%, 0.2%, 0.3%, 0.4% or 0.5%).

[0049] Preferably, the temperature at which the second filter cake is fired is 650 to 680° C. (for example, 650° C., 655° C., 660° C., 665° C., 670° C., 675° C., or 680° C.).

[0050] Preferably, the time for calcining the second filter cake is 60 to 90 minutes (for example, 60 minutes, 65 minutes, 70 minutes, 75 minutes, 80 minutes, 85 minutes, or 90 minutes).

[0051] Preferably, the second filter cake is calcined, then cooled, crushed, sieved, de-ironized and vacuum-packed to obtain anhydrous iron phosphate.

[0052] Preferably, the method for producing iron phosphate further comprises the step of introducing the gas generated in the leaching reaction into a sodium hydroxide solution after the leaching reaction is completed to obtain sodium sulfite for use.

[0053] Preferably, the method for producing iron phosphate further includes the steps of cooling the second filtrate and performing a third solid-liquid separation to obtain sodium sulfate crystals and a mother liquor, adding sodium sulfide to the mother liquor to obtain a third filtrate and a third filter cake, adjusting the pH of the third filtrate to 9 to 10 and performing a fourth solid-liquid separation to obtain a fourth filtrate and a fourth filter cake, calcining the third filter cake and dissolving the calcined third filter cake with sulfuric acid to obtain a second mixture, and extracting, concentrating, and crystallizing the second mixture to obtain crude copper sulfate and crude cobalt sulfate.

[0054] Preferably, the temperature of the second filtrate after cooling is 5 to 10°C (for example, 5°C, 7°C, 8°C, 9°C, or 10°C).

[0055] The second filtrate is mixed with sulfite, then mixed with sodium dihydrogen phosphate, and returned to leach sulfate slag. The second filtrate is recycled three times to be concentrated until the Baume degree is 45-50, then cooled until the temperature of the second filtrate is 5-10°C, centrifuged and dried, and the resulting crystals are sodium sulfate crystals.

[0056] Phosphoric acid and sodium dihydrogen phosphate are added to the fourth filtrate, which is then returned to leach the sulfate slag.

[0057] Preferably, the temperature at which the third filter cake is fired is 500 to 700° C. (for example, 530° C., 560° C., 590° C., 620° C., 650° C., 680° C., or 700° C.).

[0058] Preferably, the time for calcining the third filter cake is 2 to 4 hours (eg, 2 h, 2.5 hours, 3 hours, 3.5 hours, or 4 hours).

[0059] The waste gas produced by calcining the third filter cake is absorbed with sodium hydroxide solution and returned to leach sulfate slag.

[0060] Preferably, the method for producing iron phosphate further includes the steps of adding aqua regia to the first filter cake that has been concentrated by flotation to obtain a third mixture, performing a fifth solid-liquid separation on the third mixture to obtain a fifth filtrate, adding sodium chloride to the fifth filtrate and then performing a sixth solid-liquid separation to obtain silver chloride and a sixth filtrate, and adding iron powder to the sixth filtrate to obtain coarse gold powder.

[0061] The present invention utilizes the iron source in the sulfate slag to produce iron phosphate, and also concentrates the copper and cobalt in the sulfate slag into crude copper sulfate and crude cobalt sulfate, thereby concentrating silver and gold in the sulfate slag.

[0062] Another aspect of the present invention further relates to a method for producing lithium iron phosphate, which includes the method for producing iron phosphate.

[0063] The method for producing lithium iron phosphate is as follows.

[0064] A lithium source, a carbon source and a dopant are added to the anhydrous iron phosphate, pure water is added to form a slurry, the slurry is then pulverized into nano particles and spray-dried, the spray-dried material obtained is fired in an inert atmosphere, and the fired material obtained is pulverized, sieved, de-ironized and vacuum-packaged to obtain lithium iron phosphate.

[0065] The mass ratio of the anhydrous iron phosphate, lithium source, carbon source and dopant is 1:(0.2-0.25):(0.1-0.2):(0.0005-0.005), the lithium source is lithium carbonate or lithium hydroxide, the carbon source is at least one of glucose, sucrose, soluble starch, PEG, citric acid, ascorbic acid and benzoic acid, and the dopant is at least one of titanium compounds, vanadium compounds, magnesium compounds and manganese compounds.

[0066] In the case of nano-pulverization, the slurry is pulverized until the particle size becomes 100 to 600 nm, the inert atmosphere is nitrogen gas, the firing temperature is 600 to 900° C., and the firing time is 5 to 40 hours.

[0067] The method for producing the lithium iron phosphate is simple and low cost. EXAMPLES

[0068] In order to further explain the present invention, a method for producing iron phosphate and a method for producing lithium iron phosphate according to the present invention will be described in detail with reference to examples. However, they should not be construed as limiting the scope of the present invention.

[0069] The method for producing iron phosphate according to this embodiment includes the following steps (1) to (7).

[0070] In step (1), the sulfate slag was ground in a ball mill and then sieved through a 100 mesh sieve. The detection data sampled from the sulfate slag are shown in Table 1.

[0071] Table 1. Specific information of sulfate slag [Table 1]

[0072] In step (2), sulfate slag is added into the autoclave, sodium sulfite solution is added, and the mixture is stirred. A mixed solution of phosphoric acid and sodium dihydrogen phosphate is added into the autoclave by a high-pressure pump. The temperature is raised to 150°C while the mixed solution of phosphoric acid and sodium dihydrogen phosphate is added. The pressure in the autoclave is set to 0.42MPa. The mixed solution of phosphoric acid and sodium dihydrogen phosphate is added for 20 minutes. The mixture is stirred at this temperature and pressure for 1.5 hours to react. The slurry after the reaction is filtered to obtain a first filtrate and a first filter cake. The first filter cake is sampled. The detection data is shown in Table 2.

[0073] Table 2: Specific information of the first filter cake in Example 1 [Table 2]

[0074] The iron leaching rate was greater than 95%, concentrating elements such as gold and silver.

[0075] In step (3), the first filtrate is heated to 50°C under stirring, and then air is introduced and stirred under these conditions until the iron element concentration in the supernatant reaches 0.35g / L. The temperature is then raised to 95°C, and the mixture is stirred for 40 minutes at this temperature for reaction. The mixture is then filtered to obtain a second filtrate and a second filter cake. The second filter cake is washed, dried, and fired in a rotary kiln at a firing temperature of 670°C for a firing time of 80 minutes. The fired material is cooled, crushed, sieved, de-ironized, and vacuum-packed to obtain anhydrous iron phosphate. The detection data of anhydrous iron phosphate is shown in Table 3. The results of observing iron phosphate under a scanning electron microscope are shown in Figures 1 and 2. The particle size distribution of iron phosphate is shown in Figure 3.

[0076] Table 3. Detailed information on anhydrous iron phosphate [Table 3]

[0077] In step (4), the second filtrate is returned to be mixed with sodium dihydrogen phosphate, and then returned to be used to leach sulfate slag; the second filtrate is recycled three times to be concentrated to a Baume degree of 48, then cooled to a temperature of 8°C, centrifuged and dried; the resulting crystals are sodium sulfate crystals; the mother liquor after crystallization is added with sodium sulfide solution and filtered to obtain a third filtrate and a third filter cake; the third filtrate is added with sodium hydroxide to adjust the pH of the solution to 9.5, filtered to obtain a fourth filtrate and a fourth filter cake; the fourth filtrate is returned to be used with a new phosphoric acid solution and sodium dihydrogen phosphate to obtain sodium sulfate crystals with a purity of 98.5% or more.

[0078] The molar ratio of iron element to sodium sulfite to phosphoric acid to sodium dihydrogen phosphate in the sulfate slag was 1:0.37:0.3:1.7, the concentration of the sodium sulfite solution was 2.5 mol / L, and the sum of the molar concentrations of the mixed solutions of phosphoric acid and sodium dihydrogen phosphate was 2 mol / L.

[0079] In step (5), the third filter cake is calcined in a rotary kiln, the calcination temperature is 600°C, and the calcination time is 3 hours. The waste gas generated by calcination is absorbed by sodium hydroxide solution and returned to leach sulfate slag. After calcining the third filter cake, sulfuric acid is added to dissolve it, and cobalt and copper are extracted and separated by P2O4 extractant to obtain a cobalt-copper solution, which is then concentrated and crystallized to obtain crude copper sulfate with a purity of 95.6% and crude cobalt sulfate with a purity of 91.5%.

[0080] In step (6), after the first filter cake is flotation-filtered, the gold and silver are further concentrated, aqua regia is added to dissolve them, and then the mixture is filtered. Sodium chloride is added to the filtrate to precipitate the silver therein and obtain silver chloride. Iron powder is added to the remaining filtrate to replace the gold therein and obtain coarse gold powder.

[0081] In step (7), the gas in the autoclave is introduced into a 2 mol / L sodium hydroxide solution, and nitrogen gas is introduced into the autoclave, so that all of the sulfur dioxide gas is discharged and absorbed into the sodium hydroxide solution, and finally the sodium hydroxide concentration of the absorption liquid becomes less than 0.2 mol / L. The resulting absorption liquid is sodium sulfite, which is returned for reuse, and the flow rate (m ) of the air introduced per hour is reduced. 3 The ratio of the number of moles of ferrous ions in the solution to the total number of moles of ferrous ions in the solution was 20.

[0082] The method for producing lithium iron phosphate is as follows.

[0083] A lithium source, a carbon source and a dopant were added to the above-mentioned anhydrous iron phosphate, and pure water was added to form a slurry. The slurry was then pulverized into nano particles and spray-dried. The spray-dried material obtained was fired in an inert atmosphere, and the fired material obtained was pulverized, sieved, de-ironized and vacuum-packaged to obtain lithium iron phosphate.

[0084] The mass ratio of anhydrous iron phosphate, lithium source, carbon source and dopant was 1:0.23:0.13:0.0015, the lithium source was lithium carbonate, the carbon source was glucose and the dopant was titanium dioxide.

[0085] In the case of nano-pulverization, the slurry was pulverized until the particle size was 320 nm, the inert atmosphere was nitrogen gas, the firing temperature was 780° C., and the firing time was 12 hours.

[0086] The final detection data for lithium iron phosphate is as follows: [Table 4]

[0087] The powder resistivity was measured by the four-point probe method at a pressure of 10 MPa.

[0088] The pressure used to obtain the pressed density was 3T.

[0089] Example 2 The method for producing iron phosphate according to this embodiment includes the following steps (1) to (7).

[0090] Step (1) is the same as in the first embodiment.

[0091] In step (2), sulfate slag was added to the autoclave, potassium sulfite solution was added, and the mixture was stirred. A mixed solution of phosphoric acid and sodium dihydrogen phosphate was added to the autoclave by a high-pressure pump. The temperature was raised to 130°C while the mixed solution of phosphoric acid and sodium dihydrogen phosphate was added. The pressure in the autoclave was set to 0.5 MPa, the time for adding the mixed solution of phosphoric acid and sodium dihydrogen phosphate was set to 15 minutes, and the mixture was stirred at this temperature and pressure for 2 hours to react. The slurry after the reaction was filtered to obtain a first filtrate and a first filter cake.

[0092] In step (3), the first filtrate is heated to 40°C under stirring, and then air is introduced and stirred under these conditions to react until the iron element concentration in the supernatant becomes 0.1 g / L. The temperature is raised to 95°C, and the mixture is stirred at this temperature for 30 minutes to react, filtered, and a second filtrate and a second filter cake are obtained. The second filter cake is washed, dried, and fired in a rotary kiln at a firing temperature of 680°C for a firing time of 60 minutes. The fired material is cooled, crushed, sieved, de-ironized, and vacuum-packed to obtain anhydrous iron phosphate.

[0093] In step (4), the second filtrate is returned to be mixed with sodium dihydrogen phosphate, and then returned to be used to leach sulfate slag; the second filtrate is recycled three times to be concentrated to a Baume degree of 48, then cooled to a temperature of 8°C, centrifuged and dried; the resulting crystals are sodium sulfate crystals; sodium sulfide solution is added to the mother liquor after crystallization, filtered to obtain a third filtrate and a third filter cake; sodium hydroxide is added to the third filtrate to adjust the pH of the solution to 9, filtered to obtain a fourth filtrate and a fourth filter cake; the fourth filtrate is returned to be used with a new phosphoric acid solution and sodium dihydrogen phosphate;

[0094] The molar ratio of iron element to potassium sulfite to phosphoric acid to sodium dihydrogen phosphate in the sulfate slag was 1:0.35:0.25:1.7, the concentration of the potassium sulfite solution was 2.5 mol / L, and the sum of the molar concentrations of the mixed solutions of phosphoric acid and sodium dihydrogen phosphate was 2 mol / L.

[0095] In step (5), the third filter cake is calcined in a rotary kiln, the calcination temperature is 500°C, and the calcination time is 4 hours. The waste gas generated by calcination is absorbed with sodium hydroxide solution and returned to leach sulfate slag. After calcining the third filter cake, sulfuric acid is added to dissolve it, and cobalt and copper are extracted and separated with P204 extractant to obtain a cobalt-copper solution, which is then concentrated and crystallized to obtain crude copper sulfate and crude cobalt sulfate.

[0096] Steps (6) to (7) are the same as in the first embodiment.

[0097] Example 3 The method for producing iron phosphate according to this embodiment includes the following steps (1) to (7).

[0098] Step (1) is the same as in the first embodiment.

[0099] In step (2), sulfate slag was added to the autoclave, sodium sulfite solution was added, and the mixture was stirred. A mixed solution of phosphoric acid and sodium dihydrogen phosphate was added to the autoclave by a high-pressure pump. The temperature was raised to 170°C while the mixed solution of phosphoric acid and sodium dihydrogen phosphate was added. The pressure in the autoclave was set to 0.25 MPa. The time for adding the mixed solution of phosphoric acid and sodium dihydrogen phosphate was set to 30 minutes. The mixture was stirred at this temperature and pressure for 1 hour to react. The slurry after the reaction was filtered to obtain a first filtrate and a first filter cake.

[0100] In step (3), the first filtrate is heated to 60°C while stirring, and then air is introduced and stirred under these conditions to react until the iron element concentration in the supernatant reaches 0.5g / L. The temperature is then raised to 90°C, and the mixture is stirred at this temperature for 60 minutes to react and filtered to obtain a second filtrate and a second filter cake. The second filter cake is washed, dried, and fired in a rotary kiln at a firing temperature of 650°C for 90 minutes. The fired material is cooled, crushed, sieved, de-ironized, and vacuum-packed to obtain anhydrous iron phosphate.

[0101] In step (4), the second filtrate is returned to be mixed with sodium dihydrogen phosphate, and then returned to be used for leaching sulfate slag; the second filtrate is recycled three times to be concentrated to a Baume degree of 48, then cooled to a temperature of 8°C, centrifuged and dried; the resulting crystals are sodium sulfate crystals; sodium sulfide solution is added to the mother liquor after crystallization, filtered to obtain a third filtrate and a third filter cake; sodium hydroxide is added to the third filtrate to adjust the pH of the solution to 10, filtered to obtain a fourth filtrate and a fourth filter cake; the fourth filtrate is returned to be used with a new phosphoric acid solution and sodium dihydrogen phosphate;

[0102] The molar ratio of iron element to sodium sulfite to phosphoric acid to sodium dihydrogen phosphate in the sulfate slag was 1:0.4:0.3:1.75, the concentration of the sodium sulfite solution was 2.5 mol / L, and the sum of the molar concentrations of the mixed solutions of phosphoric acid and sodium dihydrogen phosphate was 2 mol / L.

[0103] In step (5), the third filter cake is calcined in a rotary kiln, the calcination temperature is 700°C, and the calcination time is 2 hours. The waste gas generated by calcination is absorbed with sodium hydroxide solution and returned to leach sulfate slag. After calcining the third filter cake, sulfuric acid is added to dissolve it, and cobalt and copper are extracted and separated with P204 extractant to obtain a cobalt-copper solution, which is then concentrated and crystallized to obtain crude copper sulfate and crude cobalt sulfate.

[0104] Steps (6) to (7) are the same as in the first embodiment.

[0105] Comparative Example 1 The method for producing iron phosphate according to this comparative example differs from Example 1 only in that the pressure for the leaching reaction is 0.1 MPa and the iron leaching rate is 83%.

[0106] Comparative Example 2 The method for producing iron phosphate according to this comparative example differs from Example 1 only in that the pH of the reaction system for the leaching reaction is 1. Detailed information about the obtained first filter cake is shown in Table 4.

[0107] Table 4: Specific information of the first filter cake in Comparative Example 2 [Table 5]

[0108] Comparative Example 3 The method for producing iron phosphate according to this comparative example differs from Example 1 only in that the leaching reaction time is 0.5 hours and the iron leaching rate is 81%.

[0109] By comparing Example 1, Comparative Example 1 and Comparative Example 3, it can be seen that unless the pressure and time of the leaching reaction are within a certain range, the iron leaching effect cannot be guaranteed.

[0110] By comparing Example 1 and Comparative Example 2, it can be seen that when the pH is low, the leaching rate of other impurities is greatly improved, and many impurities are introduced into the iron-containing solution, which affects the iron leaching effect. Unless the pH is within a certain range, the leaching purity of iron cannot be guaranteed.

[0111] Although the present invention has been described with reference to specific embodiments, the above embodiments are merely for illustrating the technical means of the present invention and are not intended to be limiting. It should be understood that a person skilled in the art may modify the technical means described in the above embodiments or make equivalent substitutions for some or all of the technical features thereof without departing from the spirit and scope of the present invention. These modifications and substitutions do not cause the essence of the corresponding technical means to depart from the scope of the technical means of the embodiments of the present invention. Therefore, the appended claims are intended to include all substitutions and modifications that fall within the protection scope of the present invention.

[0112] The above description is merely a preferred embodiment of the present invention, and those skilled in the art may further make various improvements and modifications without departing from the principles described in the present invention, and these improvements and modifications should also be considered as part of the scope of protection of the present invention.

Claims

1. The method includes the steps of: uniformly mixing sulfate slag and sulfite with water to obtain a first mixture; adding phosphoric acid and a buffer to the first mixture to perform a leaching reaction; performing a first solid-liquid separation on a slurry obtained after the leaching reaction to obtain a first filtrate and a first filter cake; introducing air into the first filtrate to perform a first stirring reaction; performing a second solid-liquid separation on the slurry obtained after the first stirring reaction to obtain a second filtrate and a second filter cake; and calcining the second filter cake to obtain iron phosphate, The pressure of the leaching reaction is 0.25 to 0.5 MPa, and the time of the leaching reaction is 1 to 2 hours; The pH of the reaction system of the leaching reaction is 1.5 to 3; The method for producing iron phosphate, wherein the buffer comprises sodium dihydrogen phosphate and / or disodium hydrogen phosphate.

2. The particle size of the sulfate slag is 80 to 120 mesh; Preferably, the molar ratio of iron in the sulfate slag to the sulfite to the phosphoric acid to the buffer is 1:(0.35-0.4):(0.25-0.3):(1.7-1.75); Preferably, the phosphoric acid and the buffer are added to the first mixture within 15 to 30 minutes; Preferably, the ratio of the amount of air introduced into the first filtrate per hour to the amount of ferrous ions in the first filtrate is (8 to 12) m 3 2. The method for producing iron phosphate according to claim 1, wherein the molar ratio is from 28 to 32.

3. The temperature of the leaching reaction is 130 to 170° C. The method for producing iron phosphate according to claim 1, wherein the leaching reaction is preferably carried out under stirring conditions.

4. heating the first filtrate to 40-60° C. under stirring conditions before introducing air into the first filtrate; Preferably, the first stirring reaction is specifically The method for producing iron phosphate according to claim 1, further comprising stirring the first filtrate after the introduction of air until the content of iron element in the supernatant becomes 0.5 g / L or less, heating the first filtrate to 90 to 95° C., and then stirring for an additional 30 to 60 min.

5. The method further comprises washing and drying the second cake before calcining the second cake; Preferably, the temperature of the washing water for washing is 40 to 50° C. Preferably, washing is performed until the pH of the washing solution becomes 4.5 or more, The method for producing iron phosphate according to claim 1, wherein the water content of the second filter cake after the drying is preferably 0.5% or less.

6. The temperature for firing the second filter cake is 650 to 680° C., The method for producing iron phosphate according to claim 1, wherein the time for calcining the second filter cake is preferably 60 to 90 minutes.

7. 2. The method for producing iron phosphate according to claim 1, further comprising the step of: introducing the gas generated in the leaching reaction into a sodium hydroxide solution after the leaching reaction is completed to obtain sodium sulfite.

8. The method further includes the steps of: cooling the second filtrate and performing a third solid-liquid separation to obtain sodium sulfate crystals and a mother liquor; adding sodium sulfide to the mother liquor to obtain a third filtrate and a third filter cake; adjusting the pH of the third filtrate to 9 to 10 and performing a fourth solid-liquid separation to obtain a fourth filtrate and a fourth filter cake; calcining the third filter cake and dissolving the calcined third filter cake with sulfuric acid to obtain a second mixture; and extracting, concentrating, and crystallizing the second mixture to obtain crude copper sulfate and crude cobalt sulfate, Preferably, the temperature of the second filtrate after cooling is 5 to 10° C.; Preferably, the temperature for firing the third filter cake is 500 to 700 ° C., The method for producing iron phosphate according to claim 1, wherein the time for calcining the third filter cake is preferably 2 to 4 hours.

9. 2. The method for producing iron phosphate according to claim 1, further comprising the steps of: adding aqua regia to the first filter cake that has been concentrated by flotation to obtain a third mixture; performing a fifth solid-liquid separation on the third mixture to obtain a fifth filtrate; adding sodium chloride to the fifth filtrate and then performing a sixth solid-liquid separation to obtain silver chloride and a sixth filtrate; and adding iron powder to the sixth filtrate to obtain coarse gold powder.

10. A method for producing lithium iron phosphate, comprising the method for producing iron phosphate according to any one of claims 1 to 9.

Citation Information

Patent Citations

  • Production of phosphate compounds from materials containing phosphorus and at least one of iron and aluminum

    JP2016527162A

Cited By

  • Preparation method of iron-process iron phosphate and preparation method of lithium iron phosphate

    CN122380324A