High-temperature, high-density composite material for nuclear fuel and its manufacturing method

A silicon carbide-based composite material with oxygen-free nuclear fuel particles addresses nuclear fuel's high-temperature irradiation issues, maintaining structural integrity and fission product retention.

JP2024544876AInactive Publication Date: 2024-12-05JOINT STOCK COMPANY ROSENERGOATOM +2
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
JP2024527206
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2021-12-13
Filing Date
2021-12-15
Publication Date
2024-12-05
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing nuclear fuel materials face issues with corrosion cracking, expansion, and structural phase changes under high-temperature irradiation, leading to mechanical deterioration and fuel element rupture, which existing composite materials fail to adequately address.

Method used

A high-temperature, high-density composite material is developed using a silicon carbide-based ceramic matrix with oxygen-free nuclear fuel particles, coated with a dense silicon carbide layer to prevent corrosion and maintain structural integrity.

Benefits of technology

The composite material exhibits high thermal stability and minimal mass loss (≤2%) under extreme conditions, ensuring structural integrity and effective retention of fission products.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024544876000001_ABST
    Figure 2024544876000001_ABST
Patent Text Reader

Abstract

The present invention belongs to nuclear fuel materials and relates to a high-temperature high-density composite material of nuclear fuel and a method for producing the same. The high-temperature high-density composite material of nuclear fuel includes a radioactive inert ceramic matrix in which nuclear fuel particles are dispersed. The matrix is ​​made of a powder of a material mainly composed of silicon carbide. The nuclear fuel particles are oxygen-free nuclear fuel particles. The method for producing the high-temperature high-density composite material of nuclear fuel includes preparing a mixture of nuclear fuel particles and a powder of a radioactive inert ceramic matrix, forming the mixture by pressing, and sintering the formed mixture. The formed mixture is sintered by hot pressing. According to the present invention, a high-temperature high-density composite material of nuclear fuel can be produced with a mass loss of not more than 2% after annealing in a vacuum at a temperature of 0.63 Tmelt for 10 hours.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The invention relates in particular to a nuclear fuel material characterized by high resistance to corrosion cracking under the influence of high-temperature irradiation, stability of the structural phases and an improved ability to retain volatile fission products, as well as to a method for producing a high-temperature, high-density composite material of a nuclear fuel. [Background technology]

[0002] Ensuring the thermal strength of nuclear fuel under irradiation conditions is one of the important issues in the design and operation of nuclear facilities.

[0003] Expansion of nuclear fuel due to irradiation, release of fission products, oxygen and other products of chemical interaction between solids and gases can cause localized stresses and changes in the structural phase state of fuel elements (heat-generating elements) in normal and emergency operating modes, leading to degradation of their mechanical properties and, ultimately, to fuel cracks and rupture of the fuel element shells.

[0004] A method for producing a nuclear fuel composite material comprising a radioactively inert ceramic matrix in which nuclear fuel particles are dispersed is known which comprises preparing a mixture of particles of a nuclear fuel precursor material and a powder of a material for producing the radioactively inert ceramic matrix, shaping the mixture by pressing and sintering the shaped mixture in a reducing atmosphere (GB Patent No. 1 116 663, IPC C01G 43 / 025, C04B 35 / 51, G21C 3 / 62, published 12 June 1968).

[0005] However, composite materials produced in this manner do not solve the problem of expansion of nuclear fuel under irradiation, release of volatile fission products, and localized stresses within the material.

[0006] A method for producing a nuclear reactor fuel composition is known in which finely dispersed fuel is poured into a shell of a given size and shape, the shell is filled with a substance that forms a solid matrix at a temperature above the melting point of the fuel, and the shell filled with finely dispersed fuel and the substance that forms a solid matrix is ​​heated to a temperature above the melting point of the fuel and cooled (Russian Patent No. 2295165 C1, IPC (2006.01) G21C 3 / 02, G21C 3 / 30, G21C 21 / 02, published 10 March 2007). The invention demonstrates the performance and integrity of this fuel composition at cyclical temperature changes from 20 to 1200 °C (100 cycles).

[0007] However, the use of metal nuclear fuel and preceramic polymers in the manufacturing process of the fuel composition limits its performance at high temperatures.

[0008] The closest technically to the high temperature and high density composite material of nuclear fuel and its manufacturing method of the present invention is a composite nuclear fuel material and its manufacturing method, which comprises preparing a mixture of particles of nuclear fuel precursor material and powder of material, pressing the mixture, and sintering the molded mixture in a reducing atmosphere (Russian Patent No. 2175791 C2, IPC (2000.01) G21C 3 / 64, C04B 35 / 51, published on November 10, 2001).

[0009] The material comprises a radioactive inert ceramic matrix in which nuclear fuel particles are dispersed. The size of the gap between the matrix and the particles is 1-10 μm. The thermal expansion coefficient of the matrix is ​​smaller than that of the nuclear fuel particles. The matrix can be made of spinel, magnesium oxide or yttrium oxide. The nuclear fuel particles are particles of UO2 or oxide mixtures with UO2 as the main component.

[0010] However, when the composite material obtained in this way is irradiated at high temperatures, corrosion due to active oxygen in the material and accumulation of internal stress due to changes in the structural phase state of the matrix material during operation occur.

[0011] None of the above materials can simultaneously solve the problems of expansion of nuclear fuel under high temperature irradiation conditions and preservation of the structural phase state of the fuel elements. [Prior art documents] [Patent documents]

[0012] [Patent Document 1] British Patent No. 1116663 [Patent Document 2] Russian Patent No. 2295165 [Patent Document 3] Russian Patent No. 2175791 Summary of the Invention [Problem to be solved by the invention]

[0013] The present invention aims to obtain a new nuclear fuel material that solves the above problems and to create a method for preparing such a nuclear fuel.

[0014] This is achieved by combining a heat-resistant oxygen-free fuel, superior to conventional carbon dioxide fuels in almost all thermophysical parameters, with a dense silicon carbide matrix, which has high heat resistance, high dissociation temperature, high temperature resistance in various environments, does not expand, is almost unaffected by irradiation and has a low thermal neutron capture cross section, which is confirmed by half a century of experience using it as a power layer in the design of micro fuel elements for high-temperature gas-cooled reactors.

[0015] The low chemical activity and high temperature resistance of the high density silicon carbide material ensures gas tightness and stable heat exchange between the fuel elements and the coolant, even under high temperature operating conditions up to 0.63 Tmelt.

[0016] The technical result aimed at by the present invention is the production of a high-temperature, high-density composite material of nuclear fuel, which after annealing in vacuum at a temperature of 0.63 Tmelt for 10 hours has a mass loss of no more than 2%. [Means for solving the problem]

[0017] To achieve this result, a high temperature, high density composite material of nuclear fuel has been proposed which comprises a radioactively inert ceramic matrix in which nuclear fuel particles are dispersed, the matrix being made from a powder of a silicon carbide based material, the nuclear fuel particles being oxygen-free nuclear fuel particles.

[0018] A powder of silicon carbide-based material with submicron dispersion is used.

[0019] As a powder of a material mainly composed of silicon carbide, a Si-C-Al system carborundum powder is used.

[0020] The dispersed particles of oxygen-free nuclear fuel are particles of nitride or carbide or uranium-zirconium carbonitride fuel.

[0021] The proportion and geometric dimensions of the nuclear fuel particles dispersed in the ceramic matrix are determined by the neutron properties of the nuclear power plant core.

[0022] The high temperature, high density composite material of the nuclear fuel is further coated with a cladding layer of high density silicon carbide which retains the fission products.

[0023] The thickness of the high density silicon carbide coating layer is 50-100 μm.

[0024] The shape and geometric dimensions of the hot, dense composite material of nuclear fuel are determined by the neutron properties of the nuclear power plant's core.

[0025] A method for producing high temperature and high density composite material of nuclear fuel is proposed, which includes the steps of preparing a mixture of nuclear fuel particles and a powder of a radioactive inert ceramic matrix, molding the mixture by pressing, and sintering the molded mixture, where the molded mixture is sintered by hot pressing, the matrix is ​​made of a powder of a material mainly composed of silicon carbide, and the nuclear fuel particles are oxygen-free nuclear fuel particles.

[0026] The molded mixture is sintered by hot pressing at a temperature of (0.70-0.85) Tmelt and a pressure of at least 100 MPa.

[0027] The high temperature, high density composite material of the nuclear fuel is coated with a cladding layer of high density silicon carbide which retains the fission products.

[0028] The use of oxygen-free nuclear fuel in a composite material in combination with a high density silicon carbide matrix prevents the occurrence of oxygen corrosion within the material and reduces the rate of expansion of the nuclear fuel, thereby maintaining thermophysical properties and significantly reducing internal stresses associated with changes in the structural phase state of the matrix material during operation. [Brief description of the drawings]

[0029] [Figure 1] FIG. 2 shows the material structure of the high-temperature, high-density composite material of the manufactured nuclear fuel after thermal testing. [Diagram 2] FIG. 2 shows the material structure of the high-temperature, high-density composite material of the manufactured nuclear fuel after thermal testing. [Diagram 3] FIG. 2 shows the material structure of the high-temperature, high-density composite material of the manufactured nuclear fuel after thermal testing. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0030] Example 1 A high-temperature, high-density composite material for nuclear fuel was produced by mixing 2 g of uranium zirconium carbonitride fuel particles with 25 g of powdered silicon carbide material for producing a radioactive inert ceramic matrix, pressing the mixture into a mold, and sintering the pressed mixture by hot pressing in vacuum at a temperature of 0.80 T and a pressure of 400 MPa.

[0031] Figure 1 shows the structure of the high-temperature, high-density composite material of the manufactured nuclear fuel after thermal testing, showing that the mass loss of the material was 0.3% after annealing at a temperature of 0.63 Tmelt for 10 hours under vacuum.

[0032] Example 2 The high-temperature, high-density composite material of nuclear fuel was produced by mixing 3 g of nitride nuclear fuel particles with 50 g of powder of silicon carbide material for producing a radioactive inert ceramic matrix, pressing the mixture, and sintering the pressed mixture by hot pressing in vacuum at a temperature of 0.75 Tmelt and a pressure of 300 MPa.

[0033] Figure 2 shows the structure of the high-temperature, high-density composite material of the manufactured nuclear fuel after thermal testing, showing that the mass loss of the material was 1.7% after annealing at a temperature of 0.63 Tmelt for 10 hours under vacuum.

[0034] Example 3 The high-temperature, high-density composite material of nuclear fuel was produced by mixing 1.5 g of carbide nuclear fuel with 20 g of powder of silicon carbide material for producing a radioactive inert ceramic matrix, pressing the mixture, and sintering the pressed mixture by hot pressing in vacuum at a temperature of 0.85 Tmelt and a pressure of 500 MPa.

[0035] Figure 3 shows the structure of the high-temperature, high-density composite material of the manufactured nuclear fuel after thermal testing, showing that the mass loss of the material was 1.1% after annealing at a temperature of 0.63 Tmelt for 10 hours under vacuum.

[0036] Thus, a high temperature, high density composite material of nuclear fuel has been proposed which comprises a radioactively inert ceramic matrix in which nuclear fuel particles are dispersed, the matrix being made of a powder of a silicon carbide based material, the nuclear fuel particles being oxygen-free nuclear fuel particles.

[0037] Thermal testing of the high-temperature, high-density composite material of the produced nuclear fuel showed that the mass loss of the material after annealing in vacuum at a temperature of 0.63 Tmelt for 10 hours did not exceed 2%.

[0038] The high temperature resistance and structural phase stability of this material were demonstrated at test temperatures 1.5 times higher than similar test temperatures of prototypes and similar products where interaction between the ceramic matrix and nuclear fuel particles was observed.

Claims

1. A high-temperature, high-density composite material of nuclear fuel, a radioactively inert ceramic matrix having nuclear fuel particles dispersed therein; the radiation inert ceramic matrix is ​​made from a powder of a silicon carbide based material; The nuclear fuel particles are oxygen-free nuclear fuel particles. A high-temperature, high-density composite material of nuclear fuel.

2. The powder of the material mainly composed of silicon carbide has submicron dispersion.

2. The high temperature, high density composite material of nuclear fuel according to claim 1.

3. Si-C-Al carborundum powder is used as a powder of a material mainly composed of silicon carbide.

2. The high temperature, high density composite material of nuclear fuel according to claim 1.

4. The oxygen-free nuclear fuel dispersion particles are particles of nitride or carbide or uranium zirconium carbonitride fuel.

2. The high temperature, high density composite material of nuclear fuel according to claim 1.

5. The proportion and geometric dimensions of the nuclear fuel particles dispersed in the ceramic matrix are determined by the neutron properties of the nuclear power plant core.

2. The high temperature, high density composite material of nuclear fuel according to claim 1.

6. Additionally, it is coated with a high density silicon carbide coating layer.

2. The high temperature, high density composite material of nuclear fuel according to claim 1.

7. The thickness of the high density silicon carbide coating layer is 50 to 100 μm.

7. The high temperature, high density composite material of nuclear fuel according to claim 6.

8. The shape and geometric dimensions of the hot, dense composite material of nuclear fuel are determined by the neutron properties of the nuclear power plant core.

2. The high temperature, high density composite material of nuclear fuel according to claim 1.

9. 1. A method for producing high temperature, high density composite material of nuclear fuel, comprising: preparing a mixture of nuclear fuel particles and a powder of a radioactively inert ceramic matrix, compacting the mixture in a press, and sintering the compacted mixture; The molded mixture is sintered by hot pressing. the radiation inert ceramic matrix is ​​made from a powder of a silicon carbide-based material; The nuclear fuel particles are oxygen-free nuclear fuel particles. A method comprising:

10. The molded mixture is sintered by hot pressing at a temperature of (0.70-0.85) Tmelt and a pressure of at least 100 MPa.

10. The method of claim 9.

11. The high temperature, high density composite material of the nuclear fuel is coated with a coating layer of high density silicon carbide.

10. The method of claim 9.

Citation Information

Patent Citations

  • Nuclear fuel for light water reactor

    JP1995209464A

  • Composite material of nuclear fuel and preparation thereof

    JP1997236680A

  • Process for dispersed particle ceramics

    JP2000002779A

  • Complete ceramic nuclear fuel and related methods

    JP2014500496A

  • U3Si2 pellets coated with a coating that is highly resistant to oxidation by water and steam

    JP2020511642A