Cathode catalysts for carbon oxide electrolysers.

By employing catalyst compositions with specific metal catalyst particles and ionomers on conductive support particles, the issues of uniformity and agglomeration in carbon oxide electrolyzers are addressed, resulting in enhanced faradaic efficiency and product selectivity.

JP2024544878APending Publication Date: 2024-12-05TWELVE BENEFIT CORP
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
JP2024527253
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2021-11-09
Filing Date
2022-11-09
Publication Date
2024-12-05

AI Technical Summary

Technical Problem

Existing carbon oxide electrolyzers face challenges in achieving robust catalyst performance due to issues with catalyst uniformity, agglomeration, and impurities, which affect faradaic yield and product mixing at the cathode, particularly in the reduction of carbon monoxide and other carbon-containing products.

Method used

The development of catalyst compositions comprising electrically conductive support particles with metal catalyst particles, characterized by specific size, dispersion, and attachment properties, along with an ionomer, to enhance catalyst uniformity and stability, thereby improving the reduction of carbon oxides.

Benefits of technology

The proposed catalyst compositions achieve improved faradaic efficiency and product selectivity by ensuring uniform distribution and reduced agglomeration of metal catalyst particles, enhancing the performance of carbon oxide electrolyzers.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024544878000001_ABST
    Figure 2024544878000001_ABST
Patent Text Reader

Abstract

Aspects of the present disclosure relate to a catalyst composition comprising electrically conductive support particles; and metal catalyst particles attached to the electrically conductive support particles. The catalyst composition may be used in the cathode of a carbon oxide reduction electrolyzer.
Need to check novelty before this filing date? Find Prior Art

Description

[Background technology]

[0001] Incorporation by Reference The PCT Request Form is being filed contemporaneously herewith as a part of this application. Each application to which this application claims benefit or priority as identified in the contemporaneously filed PCT Request Form is hereby incorporated by reference in its entirety for all purposes. Statement of Government Support

[0002] This invention was made with Government support under U.S. Department of Energy Award No. DE-AC36-08GO28308. The Government has certain rights in this invention.

[0003] Electrolytic carbon oxide reduction reactors require the use of a catalyst to promote the reduction of the carbon oxide reactant. The properties of the catalyst can have a strong influence on the operating voltage of the electrolytic reactor, the faradaic yield, and the mix of products produced at the cathode, including carbon monoxide (CO) and / or other carbon-containing products (CCPs) and hydrogen.

[0004] The background and contextual discussion contained herein is provided solely for the purpose of generally setting forth the context of the present disclosure. Much of the present disclosure presents work of the inventors, and merely because such work is set forth in the background section or is presented as context elsewhere herein does not mean that such work is admitted as prior art. Summary of the Invention

[0005] This Summary is provided to introduce a selection of concepts in a simplified form that are further described below in the Detailed Description. This Summary is not intended to identify key features or essential features of the claimed subject matter, nor is it intended to be used as an aid in determining the scope of the claimed subject matter.

[0006] Aspects of the present disclosure relate to catalyst compositions that include (a) conductive support particles and (b) metal catalyst particles attached to the conductive support particles. The metal catalyst particles can have an average diameter of about 2-100 nm, or about 2-50 nm, or about 2-10 nm. In certain embodiments, the metal catalyst particles have a particle size dispersity of up to about 200%, or up to about 15%. In certain embodiments, the metal catalyst particles have a loading of the catalyst composition of about 20-40% by mass fraction.

[0007] In certain embodiments, at least a portion of the metal catalyst particles attached to the conductive support particles have nearest neighboring metal catalyst particles on the respective conductive support particles to which they are attached, and such metal catalyst particles may be characterized by a spacing between nearest neighboring metal catalyst particles, which spacing may be characterized by a dispersity of about 50% or less.

[0008] In certain embodiments, at least about 80% of the conductive particles are attached to the metal catalyst particles, hi certain embodiments, at least about 95% of the metal catalyst particles are attached to the conductive support particles.

[0009] In certain embodiments, at least about 90% of the metal catalyst particles are single crystal particles.In certain embodiments, at least about 85% of the metal catalyst particles in the composition have a sphericity of at least about 90%.

[0010] In certain embodiments, the conductive support particles have an average diameter of about 10-100 nm, about 20-100 nm, or about 20-50 nm. In certain embodiments, the conductive support particles have a porosity of about 25%-75%. In certain embodiments, the conductive support particles have a porosity of about 25-225 cm. 3 / 100g surface area to volume ratio.

[0011] In certain embodiments, the metal catalyst particles comprise at least about 90% atoms of a metal selected from the group consisting of gold, platinum, rhenium, ruthenium, rhodium, palladium, silver, osmium, and iridium, hi certain embodiments, the metal catalyst particles comprise gold metal.

[0012] In certain embodiments, the metal catalyst particles contain about 200 ppm or less of boron or one or more alkali metals, hi certain embodiments, the metal catalyst particles contain about 20 ppm or less of any transition metal.

[0013] In certain embodiments, the conductive support particles include carbon. In certain embodiments, the conductive support particles include amorphous carbon. In certain embodiments, the conductive support particles include carbon black.

[0014] Some aspects of the present disclosure relate to a cathode catalyst layer comprising: (a) an ionomer; and (b) a catalyst composition, such as one having any one or more of the characteristics identified above. In some embodiments, the ionomer is an anion conducting polymer.

[0015] Some aspects of the present disclosure relate to membrane electrode assemblies that include catalyst layers such as those described above.

[0016] In the above-described embodiments of the present disclosure, any combination of one or more of the sub-features may be realized together or separately when used with the main catalyst composition and membrane electrode assembly embodiments. These and other features of the present disclosure are presented below, and some embodiments are described with reference to the figures. [Brief description of the drawings]

[0017] [Figure 1] A comparison of the size and uniformity of commercially available gold nanoparticles (left panel) and gold particles according to an embodiment of the present disclosure (right panel) is shown.

[0018] [Diagram 2]Two images of commercially available gold nanoparticles are presented, the left panel is of gold nanoparticles with a relatively low loading of nanoparticles, and the right panel is of those nanoparticles with a relatively high loading.

[0019] [Diagram 3] A comparison of the shapes of commercially available gold nanoparticles (left panel) and gold particles according to certain embodiments of the present disclosure (right panel) is shown.

[0020] [Figure 4] 1 shows a comparison of the crystallinity of commercially available gold nanoparticles (left panel) and gold particles of certain embodiments of the present disclosure (right panel).

[0021] [Diagram 5] Included are images of commercially available gold-modified carbon particles (left panel) and gold-modified carbon particles according to an embodiment of the present disclosure (right panel).

[0022] [Figure 6] Also shown are images of commercially available gold-modified carbon particles (left panel) and gold-modified carbon particles according to an embodiment of the present disclosure (right panel).

[0023] [Figure 7] 1 includes images of a commercially available gold-modified carbon particle (left panel) and a gold-modified carbon particle according to an embodiment of the present disclosure (right panel). As shown in the left panel, the gold nanoparticles are closely and non-uniformly clustered with a high degree of aggregation on the carbon particle surface. In contrast, the right panel shows well-spaced gold nanoparticles on the carbon particle surface with a low degree of random aggregation.

[0024] [Figure 8] 1 includes images of gold-modified carbon particles in an ionomer matrix.

[0025] [Figure 9] FIG. 1 shows a schematic diagram of an example of a flow-through system.

[0026] [Figure 10] 1 shows an exemplary system for a carbon oxide reduction reactor that may include a cell including an MEA (membrane electrode assembly).

[0027] [Figure 11] 1 shows an example of an MEA for use in COx reduction. The MEA has a cathode layer and an anode layer separated by an ion-conducting polymer layer. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0028] Introduction and Context Carbon oxide electrolyzers including polymer-based membrane electrode assemblies (MEAs) are designed or configured to produce oxygen from water at the anode and one or more carbon-based compounds through the electrochemical reduction of carbon dioxide or other carbon oxides at the cathode. Various examples of MEAs and MEA-based carbon oxide electrolyzers are described in the following references: PCT Publication No. 2017 / 192788, published on November 9, 2017, entitled "Reactor with Advanced Architecture for Electrochemical Reaction of CO2, CO and Other Chemical Compounds," PCT Publication No. 2019 / 144135, published on July 25, 2019, entitled "System and Method for Carbon Dioxide Reactor Control," and PCT Publication No. 2021 / 108446, published on June 3, 2021, entitled "Membrane Electrode Assembly for COx Reduction," each of which is incorporated herein by reference in its entirety.

[0029] In some cases, the MEA has a bipolar interface, i.e., an interface between a layer of a first ion exchange polymer that is substantially more conductive for anions than for cations, and a layer of a second ion exchange polymer that is substantially more conductive for cations than for anions, hi some cases, the MEA includes only anion exchange polymer or multiple anion exchange polymers (optionally provided as multiple layers).

[0030] The cathode of the MEA, also called the cathode layer or cathode catalyst layer, is x It promotes reduction. x The cathode layer includes a catalyst for the reduction reaction. In some embodiments, it also includes an electronically conductive support particle that provides support for the reduction catalyst particle and / or the ion-conducting polymer. In some embodiments, the reduction catalyst particle is combined with the ion-conducting polymer without a support. In some cases, the cathode layer is porous. Exemplary thicknesses of the cathode layer range from about 80 nm to 300 μm.

[0031] In some examples, the catalyst is a metal particle, such as gold, silver, or copper particles. In some embodiments, the metal catalyst particles have an average size of about 0.1-1000 nm, or about 1-100 nm, or about 0.2-10 nm. In some embodiments, the catalyst can be in the form of a film or nanostructured surface.

[0032] If used, the electronically conductive support in the cathode can be made from a variety of materials and have a variety of forms. For example, the support can include carbon particles, such as carbon black particles. Other exemplary conductive support particles include boron-doped diamond or fluorine-doped tin oxide.

[0033] A single cathode may contain one, two, or more types of catalysts. For example, a cathode may contain one catalyst that is good at one reaction (e.g., CO2 → CO) and a second catalyst that is good at another reaction (e.g., CO → CH4). In such an example, the cathode layer may perform the conversion of CO2 → CH4, but different steps in the reaction occur preferentially over different catalysts.

[0034] In addition to the metal catalyst particles, the cathode ion-conducting polymer, and the electron-conducting support, the cathode catalyst layer may include other additives, such as additives that promote the formation of pores. By way of example, such additives may be PTFE particles or fibers. In some embodiments, void spaces form around such particles. term

[0035] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art. The terms presented immediately below may be more fully understood by reference to other parts of the specification. The following explanations are presented to provide context and introduction to the complex concepts described herein. These explanations are not intended to limit the full scope of the present disclosure.

[0036] Carbon oxides - As used herein, the term carbon oxides refers to carbon dioxide (CO), carbon monoxide (CO), carbonate ion (CO 2- ), hydrogen carbonate ion (HCO3 - ), and any combination thereof.

[0037] Catalyst Particles - Catalyst particles are particles that lower the activation energy of a given reaction, typically a desired reaction such as the reduction of carbon oxide at the cathode of an electrolytic cell. Catalyst particles include a material that catalyzes the reaction. Such a material may be a metal, such as gold, silver, copper, or any other metal capable of catalyzing the desired reaction. The particles may have any of a variety of characteristics, such as composition, physical size, shape, crystallinity, etc. The particles may have a composition that is homogeneous (e.g., substantially pure catalyst material) or non-homogeneous.

[0038] Support particles - In some embodiments, the catalyst particles are provided on support particles. The support particles may hold or have attached thereto one, two, or more catalyst particles. When used in a catalyst layer for an electrolytic cell, the support particles may function to present the catalyst particles in a manner that makes them accessible to reactants such as carbon oxide. The support particles may impart one or more other characteristics to the catalyst layer. For example, the support particles may impart electrical and / or thermal conductivity to the catalyst layer. The electrical conductivity may be for electrons and / or ions.

[0039] Modified Support Particles - Modified support particles are support particles having one or more catalyst particles attached thereto. In some cases, the support particles are, on average, larger than the catalyst particles. As a result, a support particle may, on average, have many (e.g., 5 or more) catalyst particles attached thereto.

[0040] A mixture may contain two or more components and, unless otherwise specified, may contain components other than those identified. Cathode catalyst particle parameters

[0041] The metal particles in the catalyst can be characterized by a variety of parameters. The following discussion identifies some of these parameters. Examples of metal catalyst parameters that can affect cathode performance include size, size distribution, uniformity of coverage on the support particles, shape, loading (characterized as weight of metal / weight of metal+weight of carbon or as mass of particles per geometric area of ​​catalyst layer), surface area (actual metal catalyst surface area per volume of catalyst layer), purity, etc.

[0042] In some cases, the metal particles are gold nanoparticles. In other cases, the particles include different metals, such as different precious metals (e.g., platinum) or transition metals (e.g., copper). In some cases, the metal catalyst nanoparticles include alloys. In some embodiments, the metal nanoparticles are components of a catalyst layer of an MEA. In some cases, the metal nanoparticles are components of a mixture that serves as a precursor to the catalyst layer. For example, the metal nanoparticles may be provided as a mixture that includes substantially only metal nanoparticles. In some cases, the metal nanoparticles are provided with a conductive support material, such as carbon particles. In some cases, the metal nanoparticles are provided in a composition that includes a conductive support material and an ion-conducting matrix, such as an ionomer. Metal particle size

[0043] The size of catalytic metal particles may be characterized by the diameter of a representative sphere of the metal particle. As used herein, particle diameter is a parameter that assumes that the particles are spherical, even if they are not all spherical in reality. As an example, particle size may be determined by high-resolution imaging, for example, using transmission electron microscopy (TEM). The resulting micrograph can be analyzed to determine particle size. Using the number of particles in the micrograph and the total area of ​​all particles in the micrograph, the area per particle can be determined, and the diameter of a spherical particle can then be calculated inversely. In another example, the average area of ​​all particles is determined, and the diameter is calculated assuming the particles are spherical. In some embodiments, the image analysis process limits the size calculation to only particles within a specified range of particle "circularity" or sphericity (e.g., 1 = perfect circle or sphere, and close to 0 = elongated polygon). For example, only particles with a circularity of about 0.3 or higher are considered in the size determination.

[0044] In certain embodiments, the arithmetic mean or other representative (e.g., median) diameter of the metal particles in the carbon oxide electrolyzer cathode catalyst is about 2-100 nm or about 3-5 nm. In certain embodiments, the average diameter of the metal particles is about 2-100 nm, or about 2-50 nm, or about 2-10 nm, or about 3-5 nm. Metal particle size uniformity

[0045] Metal catalyst particles have a distribution of sizes or diameters. In certain embodiments, the distribution is substantially uniform. In some embodiments, the metal particles in the catalyst are characterized by a dispersity (sometimes referred to as a polydispersity index). Dispersity is a measure of the heterogeneity of the size of particles in a mixture. A collection of objects is called homogeneous if the objects have the same size, shape, or mass. A sample of objects with inconsistent size, shape, and mass distribution is called heterogeneous.

[0046] Dispersity is calculated by dividing the sample standard deviation by the mean particle diameter (i.e., s / μ). The sample standard deviation, s, is given by:

number

[0047] In some implementations, the metal catalyst particles have a particle size dispersity of at most about 300%, or at most about 200%, or at most about 100%, or at most about 50%, or at most about 15%.

[0048] The inventors have observed that commercially available gold nanoparticle preparations often have a wide range of particle sizes, e.g., ranging from 3-75 nm, and as a result are very heterogeneous. FIG. 1 shows a comparison of commercially available gold nanoparticles from Premetek of Cherry Hill, NJ (left panel) with gold particles according to embodiments of the present disclosure (right panel). The gold nanoparticles shown in the left panel are very non-uniform, having diameters ranging from about 3-75 nm. The gold nanoparticles shown in the right panel are much more homogeneous, having diameters ranging from about 3-5 nm. Metal filling degree

[0049] In various embodiments, the catalyst comprises metal nanoparticles in combination with electronically conductive support particles, such as carbon particles. The metal nanoparticles may be attached to the support particles. The metal-supported catalyst combination may be characterized by the loading of the metal nanoparticles. The loading may be the mass fraction of the metal in a combination that includes only the metal and the support material (e.g., carbon). It does not include other common components of the catalyst layer, such as ionomers. In certain embodiments, the catalyst particles have a metal loading of about 20-40%. In certain embodiments, the catalyst particles have a metal loading of at least about 30%. In some cases, such loading is achieved with little or no metal particle agglomeration.

[0050] The inventors have observed that commercially available gold nanoparticle compositions having relatively high loadings (eg, greater than 30%) have significant irregularly shaped aggregates of gold particles.

[0051] Figure 2 shows two images of commercially available gold nanoparticles from Premetek. The gold nanoparticles in the left panel have a relatively low loading of nanoparticles, while those in the right panel have a relatively high loading. As shown in the right panel, gold nanoparticles provided at high loading tend to aggregate or agglomerate into undesirable irregularly shaped clumps. Metal particle shape

[0052] In certain embodiments, the catalytic metal nanoparticles have a generally spherical or circular shape. For example, the metal nanoparticles can be close to the shape of a perfect sphere or circle. In certain embodiments, the metal nanoparticles can have other shapes, such as (generally) regular polyhedrons (e.g., cubes, octahedrons, dodecahedrons, etc.), ellipsoids, or wires. In certain embodiments, the catalytic metal particles are characterized by their sphericity or roundness, which is a measure of the degree of sphericity or circularity of an object. The sphericity of a particle is defined as the ratio of the surface area of ​​a sphere of equal volume to the actual surface area of ​​the particle. In certain embodiments, at least about 50% of the metal nanoparticles have a sphericity of at least about 80%, or at least about 70% of the metal nanoparticles have a sphericity of at least about 90%. In certain embodiments, at least about 85% of the metal nanoparticles in the catalyst have a sphericity of at least about 90%.

[0053] Figure 3 shows a comparison of commercially available gold nanoparticles from Premetek (left panel) and gold particles according to certain embodiments of the present disclosure (right panel). The gold nanoparticles shown in the left panel are highly non-spherical, with many non-spherical particles such as triangles, octahedrons, etc. In contrast, the gold nanoparticles shown in the right panel have a much more uniform spherical shape. Crystallinity of metal particles

[0054] In certain embodiments, many or most of the metal particles in the catalyst are single crystal nanoparticles. Single crystal particles are not polycrystalline, e.g., they do not exhibit twinning.

[0055] Catalytic metal particles in a composition such as a catalyst layer may be characterized by a minimum fraction of particles that are single crystal. In some catalysts, at least about 20% of the metal particles are single crystal particles. In some catalysts, at least about 80% of the metal particles are single crystal particles.

[0056] Figure 4 shows a comparison of commercially available gold nanoparticles from Premetek (left panel) and gold particles of certain embodiments of the present disclosure (right panel). The gold nanoparticles shown in the left panel are highly polycrystalline (e.g., twinned) and have well-defined grain boundaries. In contrast, the gold nanoparticles shown in the right panel are single-crystalline nanoparticles. Impurities in metal particles

[0057] In certain embodiments, the metal catalyst nanoparticles have few, if any, impurities. For example, the metal catalyst nanoparticles (e.g., gold nanoparticles) contain about 200 ppm or less of boron or one or more alkali metals (e.g., sodium). In certain embodiments, the metal catalyst nanoparticles (e.g., gold nanoparticles) contain about 20 ppm or less of any transition metal or any other impurity. In some implementations, the metal nanoparticles are produced using equipment that has few or no metal parts in contact with the reactants that produce the metal nanoparticles and / or other components of the catalyst composition. Carbon Particle Size

[0058] In certain embodiments, metal catalyst particles, such as gold nanoparticles, are provided on a substrate or support, which may be an electronically conductive substrate or support. In some cases, the conductive support is a particulate material. In some cases, the metal catalyst particles are attached or bonded to the conductive support. In some cases, some or most of the conductive support particles have a plurality of catalyst particles attached thereto. A conductive support particle having metal catalyst particles attached or bonded thereto may be said to be modified with metal catalyst particles.

[0059] In some embodiments, the conductive support particles are carbon particles. Such particles can be made from carbon with any of a variety of bond types, allotropes, and / or chemical properties. In general, the carbon support can be amorphous carbon or non-amorphous carbon. Examples of non-amorphous carbon include graphite or graphene-containing carbon, fullerenes, or any combination thereof. In certain embodiments, carbon black particles are used as the support. An example of carbon black is Vulcan XC 72R (Cabot Corporation, Boston, Massachusetts). Any of these types of carbon particles can be modified with gold or other metal catalyst particles.

[0060] Various parameters can characterize carbon black or other carbon support particles. Examples of these parameters include carbon particle size, the fraction of carbon particles modified with metal catalyst particles, the bonds between carbon and metal particles, and carbon porosity.

[0061] As with catalyst particles, the size of support particles can be characterized in a variety of ways. For example, the size of a support particle can be characterized by the diameter of a representative sphere of the support particle. In some cases, the diameter of the support particle assumes that the particle is spherical, even if in fact they are not all spherical.

[0062] In certain embodiments, the carbon support particles have an average or other representative (e.g., median) diameter of about 20-50 nm or about 25-35 nm, and in certain embodiments, the conductive support particles have an average diameter of about 10-100 nm, about 20-100 nm, or about 20-50 nm. Coverage of metal catalyst particles on carbon particles

[0063] In some embodiments, all or nearly all of the support particles in the catalyst composition have at least one metal catalyst particle attached thereto, in some embodiments, the minimum fraction of support particles having at least one metal catalyst particle attached thereto is at least about 80% or at least about 90%.

[0064] 5 includes images of commercially available gold-modified carbon particles from Premetek (left panel) and gold-modified carbon particles according to an embodiment of the present disclosure (right panel). As can be seen, the mixture shown in the left panel contains many carbon particles with little or no gold coverage. The gold coverage on the carbon is very inconsistent. In contrast, in the mixture shown in the right panel, the gold coverage on the carbon particles is much more consistent and uniform. There are no carbon particles without gold. Bonds between metal particles and carbon

[0065] Similarly, in some embodiments, all or nearly all of the metal catalyst particles in the catalyst composition are attached to the support particles, e.g., the fraction of the metal catalyst particles that are attached to the support particles is at least about 95% or at least about 98%.

[0066] In some cases, the bond between the metal catalyst particles and the support particles is promoted during manufacture of the modified particles, for example, by modifying the surface energy of the catalyst particles using ligands to improve adhesion to the support particles. In some cases, the modified particles are prepared by mechanically fixing the metal particles to the carbon particles by mixing colloidal metal particles with a solution containing the support particles.

[0067] 6 shows images of commercially available gold-modified carbon particles from Premetek (left panel) and gold-modified carbon particles according to an embodiment of the present disclosure (right panel). The mixture shown in the left panel contains many gold nanoparticles that are not attached to any carbon particles. In contrast, in the mixture shown in the right panel, the attachment of the gold nanoparticles to the carbon particles is much more consistent. There are few, if any, gold particles that are not attached to the carbon particles. Porosity of carbon particles

[0068] Support particles, such as carbon particles, can be characterized by their porosity. The porosity of the support particles, and therefore the cathode layer, can affect the ability of gaseous reactants and products to enter and exit the cathode while removing water. However, the cathode layer should not be so porous that the ionic and / or electrical resistance of the cathode degrades performance.

[0069] In certain embodiments, the porosity of the support particles is about 15% to about 85% or about 25% to about 75%. In some embodiments, the porosity is determined by methods such as mercury porosimetry or image analysis of TEM images. In certain embodiments, the pore volume per mass of the support particles is about 25 to 225 cm. 3 / 100g or about 50~200cm 3 / 100g. Spacing between metal catalyst particles

[0070] In certain embodiments, the catalytic metal particles are substantially uniformly spaced on the support particle surface. In such cases, there is a low probability that the metallic catalyst particles will agglomerate randomly on the support particle surface. This tendency to be uniformly spaced is a property of powders that include support particles with catalyst particles. The uniform spacing may be preserved in the final catalyst layer, which may include an ionomer.

[0071] In certain embodiments, the uniform spacing between individual metal catalyst particles on a support particle is represented by the standard deviation or dispersity of the separation distance between nearest neighbors. For example, the dispersity of the spacing between individual metal nanoparticles (nearest neighbors) is about 50% or less. The dispersity of the spacing of metal nanoparticles on a support particle surface can be defined by dividing the sample standard deviation by the average separation distance between nearest neighbor nanoparticles (s / μ).

[0072] 7 includes images of a commercially available gold-modified carbon particle (left panel) and a gold-modified carbon particle according to an embodiment of the present disclosure (right panel). As shown in the left panel, the gold nanoparticles are closely and non-uniformly clustered with a high degree of aggregation on the carbon particle surface. In contrast, the right panel shows well-spaced gold nanoparticles on the carbon particle surface with a low degree of random aggregation. Ionomer coating uniformity

[0073] Catalyst layers for MEAs may include ion-conducting materials such as anion-conducting polymers as well as conductive support particles modified with metal catalyst particles. In MEA catalyst layers, all or substantially all of the metal catalyst particles may be in contact with an ionomer or other ion-conducting material. For example, within an ionomer matrix, at least about 50% of the catalyst particles are coated with (or in intimate contact with) the ionomer. In some embodiments, at least about 70% of the catalyst particles are coated with (or in intimate contact with) the ionomer.

[0074] Figure 8 includes images of gold modified carbon particles in an ionomer matrix. As shown in the left panel, the ionomer (small light specks or green areas) is inconsistently dispersed. It non-uniformly coats the gold particles (bright or red dots) and does not disperse well. In contrast, as shown in the right panel, the ionomer produces a substantially uniform coating or distribution in all areas of the catalyst layer. The gold particles and carbon particles (large light areas or blue) are well dispersed within the ionomer.

[0075] Although the examples and embodiments described herein generally refer to cathode catalysts for carbon oxide electrolysers, the catalysts and other compositions described herein may be used in other contexts such as in other electrochemical systems such as fuel cells and electrolysers of various substances other than carbon oxides, e.g., MEAs for water electrolysers.

[0076] Furthermore, although the examples and embodiments described herein generally refer to gold particles as a catalyst, other catalysts may be used depending on the electrode and application. For example, precious metals other than gold may be used in the electrolyzer cathode. Such other precious metals include platinum, rhenium, ruthenium, rhodium, palladium, silver, osmium, and iridium. Such metals may be suitable for reducing carbon dioxide to carbon monoxide. In some embodiments, the electrolyzer cathode may use other metal catalysts such as copper, vanadium, chromium, manganese, iron, cobalt, nickel, zirconium, niobium, and molybdenum. Such metals may be suitable for reducing carbon oxides to hydrocarbons (e.g., methane and ethylene), formic acid, alcohols, aldehydes, and the like.

[0077] The supported metal particle catalyst composition may be prepared by a batch or flow-through process. The method involves forming metal nanoparticles by mixing a metal precursor solution with a capping agent solution to form a first mixture, and then adding a reducing agent to reduce the metal precursor to form the metal nanoparticles. The metal nanoparticles are then added to a solution containing suspended support particles. The solutions are mixed to allow the metal nanoparticles to adsorb onto the support particles.

[0078] Any suitable metal-containing compound that can be reduced to form elemental metal can be used. To synthesize gold nanoparticles, examples of metal precursors include gold monoiodide (AuI), gold(I) bromide (AuBr), gold(I) chloride (AuCl), gold(I) fluoride (AuF), gold trichloride (AuCl3), tetrachloroauric acid trihydrate (HAuCl4), gold(I) sulfide autothiopoole, Au m (SCH2CH2Ph) n, AuCl(oleylamine), AuCl(octadecylamine), gold(III) acetate, and gold(III) nitrate. The solid precursors can be dissolved in ultrapure water or other suitable solvents. For the synthesis of nanoparticles of other metals, suitable metal-containing precursors can be used. For example, silver nitrate (AgNO3) can be used to synthesize silver nanoparticles, and copper nitrate (Cu(NO3)2) can be used to synthesize copper nanoparticles.

[0079] Capping agents facilitate the synthesis of metal nanoparticles with controlled size and well-defined shape. Examples include citric acid, sodium citrate, cetrimonium bromide (CTAB), cetrimonium chloride (CTAC), primary amines with short alkyl ligands including hexylamine, nonylamine, and dodecylamine, carboxylic acids, polyethylene glycols (PEG), polyvinyl alcohols, polyvinylpyrrolidones, thiols including dodecanethiol, thiolates, sodium alkyl sulfates including sodium dodecyl sulfate, polysorbates such as Tween 80®, phosphorus ligands, dendrimers, heterocycles, thiolate end-capped polystyrene, thiolate poly(N-isopropylacrylamide) (PNIPAM), thiolate poly(vinylpyridine) (PVP), 5-arm polyethylene glycol-b-poly(ε-caprolactone) (PEG-b-PCL) star block copolymers, polypeptides with disulfide termini, and tetraoctylammonium bromide (TOAB).

[0080] Examples of reducing agents include sodium borohydride, potassium borohydride, ascorbyl ascorbate, polyols, tannic acid, amines including hydroxylamine, aldehydes including formaldehyde, thiols, hydrazines, phosphonic acids, thiosulfates, borohydrides, and aminoboranes.

[0081] Examples of support particles are provided above and include carbon black particles, boron doped diamond, and fluorine doped tin oxide.

[0082] In an example of batch processing, a metal precursor (e.g., HAuCl4 in ultrapure water) is mixed with a capping agent (e.g., trisodium citrate in ultrapure water) in a vessel and the mixture is stirred. A reducing agent solution (e.g., sodium borohydride) is added and the mixture is stirred for several hours. The size of the metal particles can be monitored by UV-visible spectroscopy. The mixture is then pumped into a second vessel containing diluted pre-dissolved carbon support (e.g., Vulcan carbon) and stirred for several days. The supported material can be recovered by decanting and centrifugation.

[0083] FIG. 9 shows a schematic diagram of an example of a flow-through system. The system 900 includes a metal precursor solution reservoir 902, a capping and reducing solution reservoir 904. Solutions containing the metal precursor and the capping and reducing agents are controllably pumped to a junction 908 for mixing. Examples of junctions include Y-junctions, T-junctions, and cable-type junctions followed by a short tube section containing a static mixer. The metal nanoparticle / capping solution mixture flows in a channel 914 to a junction 910. The mixture flows through a channel 916 where the metal precursor and reducing solutions react for a sufficient time to form metal nanoparticles. Once the metal nanoparticles are formed, they can be transferred to a mixing vessel 912 for mixing with the support particles in a suspension solution.

[0084] 9, the metal nanoparticles are flowed directly into the mixing vessel 912. In an alternative embodiment, they can be first collected and added separately to the mixing vessel, with flow synthesis being used to prepare only the metal nanoparticles.

[0085] In some embodiments where the metal nanoparticles are mixed with the support particles without prior collection, the support particle suspension can be added to the mixing vessel from a support particle suspension reservoir (not shown) during the mixing process, which can be useful in preventing agglomeration.

[0086] To scale up production, multiple parallel channels and multiple junctions from each reservoir can be used.

[0087] Parameters that can be used to control particle size and particle size distribution include flow rate, residence time, ratio of capping agent to metal precursor, and concentration of reducing agent. Residence time can be controlled in part by the length of channels 914 and 916. In some embodiments, serpentine channels are used to facilitate long channels. The channels can be provided in a flow field plate. Example channel lengths are 10 meters to 100 meters. Example diameters are 1 mm to 25 mm.

[0088] Residence times vary according to the size of the metal nanoparticles and the channel dimensions. Example residence times are 1-10 minutes. The ratio of capping agent to metal precursor depends on the capping agent used. Example molar ratios are 2:1-20:1. Example reducing and capping agent concentrations are 1 mmol / L-100 mmol / L. Example metal precursor concentrations are 1 mmol / L-100 mmol / L. Higher concentrations produce larger nanoparticles for the same residence time. Example flow rates are 10 mL / min-1000 mL / min for the metal precursor solution. Example flow rates for the reducing and capping agent solutions are 0.1-4 mL / min.

[0089] To help determine parameter values ​​for specific sizes and size distributions, metal nanoparticle sizes can be monitored using in-line UV-visible spectroscopy or dynamic light scattering. Carbon oxide electrolyzer system embodiments

[0090] 10 illustrates an exemplary system 1001 for a carbon oxide reduction reactor 1003 that may include a cell including a membrane electrode assembly (MEA). The reactor may include multiple cells or MEAs arranged in a stack. The system 1001 includes an anode subsystem that interfaces with the anode of the reduction reactor 1003 and a cathode subsystem that interfaces with the cathode of the reduction reactor 1003. The system 1001 is an example of a system that may be used with or implement any of the methods or operating conditions described above.

[0091] As shown, the cathode subsystem includes a carbon oxide source 1009 configured to provide a carbon oxide feed stream to the cathode of the reduction reactor 1003, which during operation may produce an output stream that includes products of the reduction reaction at the cathode. The product stream may include unreacted carbon oxides and / or hydrogen, see 1008.

[0092] The carbon oxide source 1009 is coupled to a carbon oxide flow controller 1013 configured to control a volumetric or mass flow rate of carbon oxide to the reduction reactor 1003. One or more other components may be disposed on the flow path from the flow carbon oxide source 1009 to the cathode of the reduction reactor 1003. For example, an optional humidifier 1004 may be provided on the path and configured to humidify the carbon oxide feed stream. The humidified carbon oxide may wet one or more polymer layers of the MEA, thereby preventing drying of such layers. Another component that may be disposed on the flow path is a purge gas inlet coupled to a purge gas source 1017. In certain embodiments, the purge gas source 1017 is configured to provide purge gas during periods when the current to the cells of the reduction reactor 1003 is suspended. In some implementations, flowing purge gas over the MEA cathode promotes recovery of catalytic activity and / or selectivity. Examples of purge gases include carbon dioxide, carbon monoxide, hydrogen, nitrogen, argon, helium, oxygen, and mixtures of any two or more of these.

[0093] During operation, the output stream from the cathode flows through a conduit 1007 that connects to a backpressure controller 1015 that is configured to maintain the pressure at the cathode side of the cell within a specified range (e.g., about 50-800 psig, depending on system configuration). The output stream may provide reaction products 1008 to one or more components (not shown) for separation and / or concentration.

[0094] In certain embodiments, the cathode subsystem is configured to controllably recycle unreacted carbon oxide from the outlet stream back to the cathode of the reduction reactor 1003. In some implementations, the output stream is treated to remove reduction products and / or hydrogen before recycling the carbon oxide. Depending on the configuration and operating parameters of the MEA, the reduction products may be carbon monoxide, hydrogen, hydrocarbons such as methane and / or ethylene, oxygen-containing organic compounds such as formic acid, acetic acid, and any combination thereof. In certain embodiments, one or more components (not shown) are disposed downstream of the cathode outlet to remove water from the product stream. Examples of such components include a phase separator configured to remove liquid water from the product gas stream and / or a condenser configured to cool the product stream gas and thereby provide dry gas, for example, to a downstream process if required. In some implementations, the recycled carbon oxide may be mixed with fresh carbon oxide from a source 1009 upstream of the cathode.

[0095] As shown in FIG. 10, the anode subsystem is configured to provide an anode feed stream to the anode side of the carbon oxide reduction reactor 1003. In certain embodiments, the anode subsystem includes an anode water source (not shown) configured to provide fresh anode water to a recirculation loop that includes an anode water reservoir 1019 and an anode water flow controller 1011. The anode water flow controller 1011 is configured to control the flow rate of the anode water to or from the anode of the reduction reactor 1003. In the illustrated embodiment, the anode water recirculation loop is coupled to components for adjusting the composition of the anode water. These may include a water reservoir 1021 and / or an anode water additive source 1023. The water reservoir 1021 is configured to provide (and circulate in the anode water recirculation loop) water having a different composition than that in the anode water reservoir 1019. In one example, the water in the water reservoir 1021 is pure water that may dilute solutes or other components in the circulating anode water. The pure water may be conventional deionized water or even ultrapure water, for example having a resistivity of at least about 15 MOhm-cm or greater than 18.0 MOhm-cm. The anode water additive source 1023 is configured to supply solutes, such as salts and / or other components, to the circulating anode water.

[0096] During operation, the anode subsystem may provide water or other reactants to the anode of reactor 1003, which at least partially react to produce oxidation products, such as oxygen. The products, along with any unreacted anode feed material, are provided in the outlet stream of the reduction reactor. Although not shown in FIG. 10, an optional separation component may be provided in the path of the anode outlet stream and configured to condense or separate the oxidation products from the anode product stream.

[0097] Other control functions may be included in the system 1001. For example, a temperature controller may be configured to heat and / or cool the carbon oxide reduction reactor 1003 at appropriate points during operation. In the illustrated embodiment, the temperature controller 1005 is configured to heat and / or cool the anode water provided to the anode water recirculation loop. For example, the temperature controller 1005 may include or be coupled to heaters and / or coolers that may heat or cool the water in the anode water reservoir 1019 and / or the water in the reservoir 1021. In some embodiments, the system 1001 includes a temperature controller configured to directly heat and / or cool components other than the anode water components. Examples of such other components in the cell or stack are carbon oxide flowing to the cathode.

[0098] Depending on the phase of electrochemical operation, including whether or not current flow to the carbon oxide reduction reactor 1003 is suspended, certain components of the system 1001 may operate to control non-electrical operation. For example, the system 1001 may be configured to adjust the flow rate of carbon oxide to the cathode and / or the flow rate of anode feed material to the anode of the reactor 1003. Components that may be controlled for this purpose may include a carbon oxide flow controller 1013 and an anode water controller 1011.

[0099] Also, depending on the phase of the electrochemical operation, including whether or not the current is paused, certain components of the system 1001 may operate to control the composition of the carbon oxide supply stream and / or the anode feed stream. For example, the water reservoir 1021 and / or the anode water additive source 1023 may be controlled to adjust the composition of the anode feed stream. In some cases, the additive source 1023 may be configured to adjust the concentration of one or more solutes, such as one or more salts, in the aqueous anode feed stream.

[0100] In some cases, a temperature controller such as controller 1005 is configured to adjust the temperature of one or more components of system 1001 based on the phase of operation. For example, the temperature of cells 1003 may be increased or decreased during break-in, current suspend during normal operation, and / or storage.

[0101] In some embodiments, the carbon oxide electrolytic reduction system is configured to facilitate removal of the reduction cell from other system components. This can be useful when the cell needs to be removed for storage, maintenance, refurbishment, etc. In the illustrated embodiment, isolation valves 1025a and 1025b are configured to block fluid communication of cell 1003 to the carbon oxide source and to the cathode and back pressure controller 1015, respectively. Additionally, isolation valves 1025c and 1025d are configured to block fluid communication of cell 1003 to the anode water inlet and outlet, respectively.

[0102] The carbon oxide reduction reactor 1003 may operate under the control of one or more power supplies and associated controllers. See block 1033. The power supplies and controllers 1033 may be programmed or otherwise configured to control the current provided to and / or the voltage applied to the electrodes in the reduction reactor 1003. The current and / or voltage may be controlled to implement a current schedule and / or current profile described elsewhere herein. For example, the power supplies and controllers 1033 may be configured to periodically pause the current applied to the anode and / or cathode of the reduction reactor 1003. Any of the current profiles described herein may be programmed into the power supplies and controllers 1033.

[0103] In certain embodiments, the power supply and controller 1033 performs some, but not all, of the operations necessary to achieve a desired current schedule and / or profile in the carbon oxide reduction reactor 1003. A system operator or other responsible person may act in conjunction with the power supply and controller 1033 to completely define the schedule and / or profile of the current applied to the reduction reactor 1003. For example, the operator may institute one or more current pauses in addition to a set of current pauses programmed into the power supply and controller 1033.

[0104] In certain embodiments, the power supply and controller cooperates with one or more other controllers or control mechanisms that interface with other components of the system 1001. For example, the power supply and controller 1033 may cooperate with controllers for controlling the delivery of carbon oxide to the cathode, the delivery of anode water to the anode, the addition of pure water or additives to the anode water, and any combination of these functions. In some implementations, the one or more controllers are configured to control or operate in a coordinated manner to control any combination of the following functions: application of current and / or voltage to the reduction cell 1003, control of backpressure (e.g., via the backpressure controller 1015), supply of purge gas (e.g., using the purge gas component 1017), delivery of carbon oxide (e.g., via the carbon oxide flow controller 1013), humidification of the carbon oxide in the cathode supply stream (e.g., via the humidifier 1004), flow of anode water to and / or from the anode (e.g., via the anode water flow controller 1011), and anode water composition (e.g., via the anode water source 1005, the pure water reservoir 1021, and / or the anode water additive component 1023).

[0105] In the illustrated embodiment, the voltage monitoring system 1034 is used to determine the voltage across the anode and cathode of the MEA cell or across any two electrodes of the cell stack, e.g., across all cells in a multi-cell stack. The voltages thus determined can be used to control the cell voltage during a current pause, inform the duration of the pause, etc. In certain embodiments, the voltage monitoring system 1034 is configured to work in coordination with the power supply 1033 to keep the reduction cell 1003 within a specified voltage range. For example, the power supply 1033 can be configured to apply a current and / or a voltage to the electrodes of the reduction cell 1003 during the current pause to maintain the cell voltage within the specified range. For example, during the current pause, if the open circuit voltage of the cell deviates from the specified range (as determined by the voltage monitoring system 1034), the power supply can be configured to apply a current or a voltage to the electrodes to maintain the cell voltage within the specified range.

[0106] Electrolytic carbon reduction systems such as that shown in Figure 10 may employ a control system including one or more controllers and one or more controllable components such as pumps, sensors, dispensers, valves, and power supplies. Examples of sensors include pressure sensors, temperature sensors, flow sensors, conductivity sensors, voltmeters, ammeters, electrolyte composition sensors including electrochemical instruments, chromatography systems, optical sensors such as absorbance measurement tools, and the like. Such sensors may be coupled to the inlets and / or outlets of the MEA cells (e.g., in the flow field), in reservoirs for holding anode water, pure water, salt solutions, and the like, and / or other components of the electrolytic carbon reduction system.

[0107] Various functions that may be controlled by one or more controllers include applying current and / or voltage to the carbon oxide reduction cells, controlling back pressure on the cathode outlet on such cells, supplying purge gas to the cathode inlet, delivering carbon oxide to the cathode inlet, humidifying carbon oxide in the cathode feed stream, flowing anode water to and / or from the anode, and controlling the anode feed composition. Any one or more of these functions may have a dedicated controller to control that function alone. Any two or more of these functions may share a controller. In some embodiments, a hierarchy of controllers is used, with at least one master controller providing instructions to two or more component controllers. For example, the system may include a master controller configured to provide high-level control instructions to (i) the power supply to the carbon oxide reduction cells, (ii) the cathode feed stream flow controller, and (iii) the anode feed stream flow controller. For example, a programmable logic controller (PLC) may be used to control the individual components of the system.

[0108] In certain embodiments, the control system is configured to apply a current to a carbon oxide reduction cell comprising an MEA according to a current schedule, which may have any of the characteristics described herein. For example, the current schedule may provide periodic pauses in the applied current. In some cases, the control system provides current pauses having a defined profile, such as a ramp and / or step change as described herein.

[0109] In certain embodiments, the control system is configured to control the flow rate of one or more feed streams (e.g., a cathode feed stream, such as a carbon oxide flow, and an anode feed stream) in coordination with the current schedule. For example, the flow of carbon oxide or a purge gas may be switched on, off, or otherwise adjusted when the current applied to the MEA cell is suspended.

[0110] In certain embodiments, a control system may be configured to implement the recovery sequences described herein. Such a control system may be configured to suspend or reduce current, flow recovery gas, flow water or other liquid, dry the cathode, resume normal operation, or any combination thereof. The controller may be configured to control the initialization of the recovery sequence, control the duration of any operation in the recovery sequence, etc.

[0111] The controller may include any number of processors and / or memory devices. The controller may include control logic, such as software or firmware, and / or execute instructions provided from another source. The controller may be integrated with electronics to control the operation of the electrolytic cell before, during, and after carbon oxide reduction. The controller may control various components or subparts of one or more electrolytic carbon oxide reduction systems. The controller may be programmed to control any of the processes disclosed herein, such as gas delivery, temperature settings (e.g., heating and / or cooling), pressure settings, power settings (e.g., voltage and / or current delivered to the electrodes of the MEA cell), liquid flow rate settings, fluid delivery settings, and dosing of purified water and / or salt solutions, depending on the process requirements and / or type of system. These controlled processes may be connected or interfaced with one or more systems that work in concert with the electrolytic carbon oxide reduction system.

[0112] In various embodiments, the controller includes electronics with various integrated circuits, logic, memory, and / or software that receive instructions, issue instructions, and control the operations described herein. The integrated circuits may include chips in the form of firmware that store program instructions, digital signal processors (DSPs), chips defined as application specific integrated circuits (ASICs), and / or one or more microprocessors or microcontrollers that execute the program instructions (e.g., software). The program instructions may be instructions communicated to the controller in the form of various individual settings (or program files) that define the operating parameters for carrying out a process in one or more components of the electrolytic oxidative carbon reduction system. In some embodiments, the operating parameters may be part of a recipe defined by a process engineer to accomplish one or more process steps during the production of a particular reduction product, such as carbon monoxide, hydrocarbons, and / or other organic compounds.

[0113] In some implementations, the controller may be part of or coupled to a computer that is integrated with, coupled to, or otherwise networked to the system, or a combination thereof. For example, the controller may utilize and / or execute instructions stored remotely (e.g., in the "cloud"). The computer may enable remote access to the system to monitor the current progress of the electrolysis operation, examine the history of past electrolysis operations, examine trends or performance metrics from multiple electrolysis operations, and modify parameters of the current process, set process steps to follow the current process, or start a new process. In some examples, a remote computer (e.g., a server) may provide a process recipe to the system over a network, which may include a local network or the Internet. The remote computer may include a user interface that allows for entry or programming of parameters and / or settings, which are then communicated from the remote computer to the system. In some examples, the controller receives instructions in the form of data that specify parameters for each of the process steps to be performed during one or more operations.

[0114] The controller may be distributed, such as by including one or more separate controllers networked together and functioning toward a common purpose, such as application of current to the MEA cells and other process control as described herein. One example of a control system distributed for such purposes includes one or more processors on the system for electrolytic reduction of carbon oxides and one or more processors located remotely (such as at the platform level or as part of a remote computer) that are combined to control the process.

[0115] Any of the controllers and various associated computational elements, including processors, memories, instructions, routines, models, or other components, may, in some cases, be described or claimed as being "configured to" perform one or more tasks. In this context, the phrase "configured to" is used to indicate structure by indicating that a component includes a task or structure (e.g., stored instructions, circuitry, etc.) that, when in operation, performs a task. Thus, a controller and / or associated components may be said to be configured to perform a task even if a particular component is not necessarily currently in operation (e.g., not on).

[0116] Controllers and other components "configured to" perform an operation may be implemented as hardware, including, for example, circuits, memories storing executable program instructions to implement the operation, etc. Additionally, controllers and other components "configured to" perform an operation may be implemented as hardware that is manipulated by software and / or firmware (e.g., an FPGA or a general-purpose processor executing software) to operate in a manner that enables it to perform the described tasks. Additionally, "configured to" may refer to one or more memories or memory elements that store computer-executable instructions to perform the described tasks. Such memory elements may include memory on a computer chip with processing logic.

[0117] Non-computational elements such as reactors, electrolyzers, membrane assemblies, layers, and catalyst particles may also be "configured" to perform a particular function. In this context, "configured to" indicates that the structure being referred to has one or more characteristics that enable it to perform the function. Examples of such characteristics include physical and / or chemical properties such as dimensions, composition, porosity, etc. MEA Embodiments Overview of MEA

[0118] In various embodiments, the MEA includes an anode layer, a cathode layer, an electrolyte, and optionally one or more other layers. The layers may be solids and / or gels. These layers may include polymers, such as ion-conducting polymers.

[0119] In use, the cathode of the MEA is x , CO x By combining three inputs: CO, ions (e.g., protons or hydroxide ions) that react chemically with CO, and electrons. x The anode of the MEA promotes the electrochemical reduction of CO, hydrocarbons, and / or oxygen-containing and hydrogen-containing organic compounds, such as methanol, ethanol, and acetic acid. In use, the anode of the MEA promotes an electrochemical oxidation reaction, such as the electrolysis of water, to produce elemental oxygen and protons. The cathode and anode may each include a catalyst to promote the respective reaction.

[0120] During operation of the MEA, ions move through the polymer electrolyte while electrons flow from the anode through an external circuit to the cathode. In some embodiments, liquids and / or gases move or permeate through the MEA layers. This process may be facilitated by pores within the MEA.

[0121] The composition and organization of the layers within the MEA is x A high yield of reduction products may be promoted. To this end, the MEA may promote any one or more of the following conditions: (a) minimal parasitic reduction reactions (non-CO) at the cathode; x (b) CO reduction to the anode or elsewhere in the MEA x (c) low loss of reactants; (d) physical integrity of the MEA during the reaction (e.g., the MEA layers remain fixed together); x (e) preventing crossover of reduction products; (f) a suitable environment at the cathode for the reduction reaction; (g) a pathway for desired ions to migrate between the cathode and anode while blocking undesired ions; and (h) low voltage operation. COx Reduction Considerations

[0122] Polymer-based membrane assemblies such as MEAs have been used in a variety of electrolysis systems, such as water electrolyzers, and in a variety of galvanic systems, such as fuel cells. x Reduction presents a problem that does not occur, or occurs to a lesser extent, in water electrolysers and fuel cells.

[0123] For example, in many applications, CO x The MEA for reduction requires a life of about 50,000 hours or more (about 5 years of continuous operation), which is significantly longer than the expected life of a fuel cell for automotive use (e.g., about 5,000 hours). x The MEA for reduction uses electrodes with a relatively large surface area compared to the MEAs used in fuel cells for automotive applications. For example, CO x The MEA for reduction should be at least about 500 cm 2 An electrode having a surface area (not considering pores and other non-planar features) of 0.1 mm may be used.

[0124] CO x The reduction reaction may be implemented in an operating environment that facilitates mass transfer of certain reactant and product species and suppresses parasitic reactions. Fuel cell and water electrolyzer MEAs often cannot create such an operating environment. For example, such MEAs may promote undesirable parasitic reactions such as gaseous hydrogen evolution at the cathode and / or gaseous CO production at the anode.

[0125] In some systems, CO x The rate of reduction is determined by the amount of gaseous CO at the cathode. x Limited by the availability of reactants. In contrast, the rate of water electrolysis is not significantly limited by the availability of reactants. Liquid water tends to be readily accessible to the cathode and anode, allowing the electrolyzer to operate near the highest possible current density. MEA Configuration

[0126] In certain embodiments, the MEA has a cathode layer, an anode layer, and a polymer electrolyte membrane (PEM) between the anode layer and the cathode layer. The polymer electrolyte membrane provides ionic transfer between the anode layer and the cathode layer while preventing electronic transfer that would cause a short circuit. The cathode layer includes a reduction catalyst and, optionally, an ion-conducting polymer (sometimes called an ionomer). The cathode layer may also include an electronic conductor and / or an additional ion conductor. The anode layer includes an oxidation catalyst and, optionally, an ion-conducting polymer. The anode layer may also include an electronic conductor and / or an additional ion conductor. The PEM also includes an ion-conducting polymer. In certain embodiments, the MEA has a cathode buffer layer between the cathode layer and the polymer electrolyte membrane. The cathode buffer also includes an ion-conducting polymer.

[0127] Each of the ion-conducting polymers in the PEM, cathode, anode, and cathode buffer layer, if present, may differ from each other in composition, conductivity, molecular weight, or other properties. In some cases, two or more of these polymers are the same. For example, the ion-conducting polymers in the cathode and cathode buffer layer may be the same.

[0128] In certain embodiments, the MEA has an anode buffer layer between the anode layer and the polymer electrolyte membrane. The anode buffer also includes an ion-conducting polymer that may have the same properties as any of the other ion-conducting polymers (e.g., the ion-conducting polymer in the anode). Alternatively, the ion-conducting layer of the anode may be different from all other ion-conducting layers in the MEA.

[0129] With respect to a particular MEA design, there are three available classes of ion conducting polymers: anion conductors, cation conductors, and mixed cation-anion conductors. In certain embodiments, at least two of the first, second, third, fourth, and fifth ion conducting polymers are from different classes of ion conducting polymers. Ion-conducting polymers for MEA layers

[0130] The terms "ion-conducting polymer" or "ionomer" are used herein to describe a polymer that conducts ions (anions and / or cations) and refer to the material being an ion-conducting material or ionomer. In certain embodiments, an MEA includes one or more ion-conducting polymers having a specific conductivity of about 1 mS / cm or greater for anions and / or cations. The term "anion conductor" refers to an ion-conducting polymer that conducts primarily anions (although there may still be some small amount of cation conduction) and has a transport number for the anions greater than about 0.85 at a thickness of about 100 micrometers. The terms "cation conductor" and / or "cation-conducting polymer" refer to an ion-conducting polymer that conducts primarily cations (e.g., there may still be an incidental amount of anion conduction) and has a transport number for the cations greater than about 0.85 at a thickness of about 100 micrometers. For ion-conducting polymers described as conducting both anions and cations ("cation-anion conductors"), neither the anions nor the cations have transport numbers greater than about 0.85 or less than about 0.15 at a thickness of about 100 micrometers. Examples of ion-conducting polymers of each class are provided in Table 1 below. [Table 1] Polymer Structure

[0131] Provided below are examples of polymer structures that may include ionizable or ionic moieties and may be used as ion-conducting polymers (ionomers) in the MEAs described herein. The ion-conducting polymers may be used as appropriate in any of the MEA layers that include ion-conducting polymers. Charge conduction through the material may be controlled by the type and amount of charge provided on the ionizable / ionic moieties (e.g., anionic and / or cationic charges on the polymer structure). The composition may also include polymers, homopolymers, copolymers, block copolymers, polymeric blends, other polymer-based forms, or other useful combinations of monomeric repeat units. As described below, according to various embodiments, the ion-conducting polymer layers may include one or more of bridges, linking moieties, and arylene groups. In some embodiments, two or more ion-conducting polymers (e.g., in two or more ion-conducting polymer layers of an MEA) may be crosslinked.

[0132] Non-limiting monomeric units can include one or more of the following: [ka] where Ar is an optionally substituted arylene or aromatic; Ak is an optionally substituted alkylene, haloalkylene, aliphatic, heteroalkylene, or heteroaliphatic; L is a linking moiety (e.g., any described herein), or -C(R 7 )(R 8 )-. Still other non-limiting monomeric units may include optionally substituted arylene, aryleneoxy, alkylene, or combinations thereof, such as optionally substituted (aryl)(alkyl)enes (e.g., -Ak-Ar- or -Ak-Ar-Ak- or -Ar-Ak-, where Ar is an optionally substituted arylene and Ak is an optionally substituted alkylene). One or more of the monomeric units may be optionally substituted with one or more ionizable or ionic moieties (e.g., as described herein).

[0133] One or more monomer units may be combined to form a polymer unit. Non-limiting polymer units include any of the following: [ka] where Ar, Ak, L, n, and m can be any of those described herein. In some embodiments, each m is independently an integer of 0 or greater than 1. In other embodiments, Ar can include two or more arylene or aromatic groups.

[0134] Other alternative configurations are also encompassed by the compositions herein, such as branched configurations, diblock copolymers, triblock copolymers, random or statistical copolymers, steroblock copolymers, gradient copolymers, graft copolymers, and combinations of any of the blocks or regions described herein.

[0135] Exemplary polymeric structures include those according to any one of formulas (I)-(V) and (X)-(XXXIV) or salts thereof. In some embodiments, the polymeric structure is a copolymer and includes a first polymeric structure selected from any one of formulas (I)-(V) or salts thereof; a second polymeric structure includes an optionally substituted aromatic, an optionally substituted arylene, a structure selected from any one of formulas (I)-(V) and (X)-(XXXIV) or salts thereof.

[0136] In one embodiment, the MW of the ion-conducting polymer is a weight average molecular weight (Mw) of at least 10,000 g / mol or from about 5,000 to 2,500,000 g / mol, in another embodiment, the MW is a number average molecular weight (Mn) of at least 20,000 g / mol or from about 2,000 to 2,500,000 g / mol.

[0137] In any embodiment herein, n, n1, n2, n3, n4, m, m1, m2, or m3 are each independently 1 or more, 20 or more, 50 or more, 100 or more, and 1 to 1,000,000, for example, 10 to 1,000,000, 100 to 1,000,000, 200 to 1,000,000, 500 to 1,000,000, or 1,000 to 1,000,000.

[0138] Non-limiting polymer structures include the following: [ka] or a salt thereof, Here, R 7 , R 8 , R 9 , and R 10 each is independently an electron-withdrawing moiety, H, an optionally substituted aliphatic, alkyl, heteroaliphatic, heteroalkylene, aromatic, aryl, or arylalkylene, where R 7 or R 8 At least one of R may include an electron-withdrawing moiety, or 7 and R 8 or R 9 and R 10 combinations of, taken together, form an optionally substituted cyclic group; Ar is or includes an optionally substituted aromatic or arylene (e.g., any described herein); Each n is independently an integer of 1 or greater; Each of rings a-c can be optionally substituted; Ring a~c, R 7 , R 8 , R 9 and R 10 may optionally include an ionizable or ionic moiety.

[0139] Further non-limiting polymer structures include the following: [ka] or a salt thereof, wherein: R 7 can be any of those described herein (e.g., for formulas (I)-(V)); n is 1 or greater; Each L 8A , L B' , and L B" are independently linking moieties; each X 8A , X 8A' , X 8A" , X B' , and X B" are independently ionizable or ionic moieties.

[0140] Yet another polymer structure is as follows: [ka] [ka] [ka] or a salt thereof, wherein: R 1 , R 2 , R 3 , R 7 , R 8 , R 9 and R 10 each is independently an electron-withdrawing moiety, H, an optionally substituted aliphatic, alkyl, heteroaliphatic, heteroalkylene, aromatic, aryl, or arylalkylene, where R 7 or R 8 At least one of R may include an electron-withdrawing moiety, or 7 and R 8 or R 9 and R 10 combinations of may be taken together to form an optionally substituted cyclic group; each Ak is or includes an optionally substituted aliphatic, alkylene, haloalkylene, heteroaliphatic, or heteroalkylene; each Ar is or includes an optionally substituted arylene or aromatic; L, L 1 , L 2 , L 3 , and L 4 each is independently a linking moiety; each of n, n1, n2, n3, n4, m, m1, m2, and m3 is independently 1 or more integers; q is 0, 1, 2 or greater; Each of rings a-i can be optionally substituted; Rings a~i, R 7 , R 8 , R 9 , and R 10 may optionally include an ionizable or ionic moiety.

[0141] In certain embodiments (e.g., with respect to formula (XIV) or (XV)), each of the nitrogen atoms on ring a and / or ring b is substituted with an optionally substituted aliphatic, alkyl, aromatic, aryl, ionizable or ionic moiety. In some embodiments, one or more hydrogen or fluorine atoms (e.g., in formula (XIX) or (XX)) may be substituted to include an ionizable or ionic moiety (e.g., any of those described herein). In other embodiments, an oxygen atom present in the polymer structure (e.g., in formula (XXVIII)) is substituted with an alkali dopant (e.g., K + ) may be associated with

[0142] In certain examples, Ar, rings a-i (e.g., rings a, b, f, g, h, or i), L, L 1 , L 2 , L 3 , L 4 , Ak, R 7 , R 8 , R 9 and / or R 10 One or more of Ar, a ring (e.g., rings a-i), L, Ak, R may be optionally substituted with one or more ionizable or ionic moieties and / or one or more electron-withdrawing groups. 7 , R8 , R 9 and R 10 Further other non-limiting substituents for include one or more of those described herein, such as, for example, cyano, hydroxy, nitro, and halo, and optionally substituted aliphatic, alkyl, alkoxy, alkoxyalkyl, amino, aminoalkyl, aryl, arylalkylene, aryloyl, aryloxy, arylalkoxy, hydroxyalkyl, and haloalkyl.

[0143] In some embodiments, R 1 , R 2 and R 3 Each of R is independently H, optionally substituted aromatic, aryl, aryloxy, or arylalkylene. In other embodiments (e.g., in Formulas (I)-(V) or (XII)), R 7 In yet another embodiment, R 8 , R 9 and / or R 10 comprises an ionizable or ionic moiety.

[0144] In one case, a polymer subunit may not have an ionic moiety. Alternatively, a polymer subunit may include an ionic moiety that may be incorporated into the Ar group, the L group, both the Ar and L groups, or as part of the L group. Non-limiting examples of ionizable or ionic moieties include cationic groups, anionic groups, and multi-ionic groups described herein.

[0145] In any embodiment herein, the electron withdrawing moiety can be an optionally substituted haloalkyl, cyano (CN), phosphate (e.g., -O(P=O)(OR P1 )(OR P2 ) or -O-[P(=O)(OR P1 )-O] P3 -R P2 ), sulfates (e.g., -OS(=O)2(OR S1)), sulfonate (-SO3H), sulfonyl (e.g., -SO2-CF3)), difluoroboranyl (-BF2), borono (B(OH)2), thiocyanato (-SCN), or piperidinium. Further other non-limiting phosphate groups may include derivatives of phosphoric acid, such as orthophosphate, pyrophosphate, tripolyphosphate, tetrapolyphosphate, trimetaphosphate, and / or phosphoric anhydride, or combinations thereof.

[0146] Further other polymer units include poly(benzimidazole) (PBI), polyphenylene (PP), polyimide (PI), poly(ethyleneimine) (PEI), sulfonated polyimide (SPI), polysulfone (PSF), sulfonated polysulfone (SPSF), poly(ether ether ketone) (PEEK), PEEK with cardo groups (PEEK-WC), polyethersulfone (PES), sulfonated polyethersulfone (SPES), sulfonated poly(ether ether ketone) (SPEEK), SPEEK with cardo groups (SPEEK-WC), poly(p-phenylene oxide) (PPO), sulfonated polyphenylene oxide (SPPO), ethylene tetrafluoroethylene (ETFE), poly These may include tetrafluoroethylene (PTFE), poly(epichlorohydrin) (PECH), poly(styrene) (PS), sulfonated poly(styrene) (SPS), hydrogenated poly(butadiene-styrene) (HPBS), styrene divinylbenzene copolymer (SDVB), styrene-ethylene-butylene-styrene (SEBS), sulfonated bisphenol-A-polysulfone (SPSU), poly(4-phenoxybenzoyl-1,4-phenylene) (PPBP), sulfonated poly(4-phenoxybenzoyl-1,4-phenylene) (SPPBP), poly(vinyl alcohol) (PVA), poly(phosphazene), poly(aryloxyphosphazene), polyetherimide, and combinations thereof. Bipolar MEA for COx reduction

[0147] In certain embodiments, the MEA includes a bipolar interface having an anion conducting polymer on the cathode side of the MEA and an interfacing cation conducting polymer on the anode side of the MEA. In some implementations, the cathode contains a first catalyst and an anion conducting polymer. In certain embodiments, the anode contains a second catalyst and a cation conducting polymer. In some implementations, a cathode buffer layer located between the cathode and the PEM contains an anion conducting polymer. In some embodiments, an anode buffer layer is disposed between the anode and the PEM and includes a cation conducting polymer.

[0148] In embodiments using an anion conducting polymer in the cathode and / or cathode buffer layer, the MEA can reduce or block undesired reactions that produce undesired products and reduce the overall efficiency of the cell, and in embodiments using a cation conducting polymer in the anode and / or anode buffer layer, the MEA can reduce or block undesired reactions that reduce the production of desired products and reduce the overall efficiency of the cell.

[0149] For example, at the level of potential used for cathodic reduction of CO2, hydrogen ions may be reduced to hydrogen gas. This is a parasitic reaction, and the current that could be used to reduce CO2 is instead used to reduce hydrogen ions. Hydrogen ions may be generated by various oxidation reactions carried out at the anode of the CO2 reduction reactor, and may travel across the MEA and reach the cathode, where they can be reduced to produce hydrogen gas. The extent to which this parasitic reaction can proceed is a function of the concentration of hydrogen ions present at the cathode. Thus, the MEA may use anion-conducting materials in the cathode layer and / or cathode buffer layer. The anion-conducting materials at least partially block hydrogen ions from reaching the catalytic sites on the cathode. As a result, the parasitic production of hydrogen gas is reduced and the rate of production of CO or other carbon-containing products is increased.

[0150] Another reaction that may be avoided is the reaction of carbonate or bicarbonate ions at the anode to produce CO2. Aqueous carbonate or bicarbonate ions may be generated from CO2 at the cathode. When such ions reach the anode, they may react with hydrogen ions to produce and release gaseous CO2. As a result, CO2 is net transferred from the cathode to the anode, where it is not reduced and is lost together with the oxidation products. To prevent carbonate and bicarbonate ions generated at the cathode from reaching the anode, the anode and / or anode buffer layer may include a cation-conducting polymer, which at least partially blocks the transport of negative ions, such as bicarbonate ions, to the anode.

[0151] Thus, in some designs, a bipolar membrane structure raises the pH at the cathode to promote CO2 reduction, and a cation-conducting polymer, such as a proton exchange layer, prevents significant amounts of CO2 and CO2 reduction products (e.g., bicarbonate) from passing to the anode side of the cell.

[0152] CO x An example of an MEA 1100 for use in reduction is shown in FIG. The MEA 1100 has a cathode layer 1120 and an anode layer 1140 separated by an ion conducting polymer layer 1160 that provides a path for ions to move between the cathode layer 1120 and the anode layer 1140. In certain embodiments, the cathode layer 1120 comprises an anion conducting polymer and / or the anode layer 1140 comprises a cation conducting polymer. In certain embodiments, the cathode layer and / or the anode layer of the MEA are porous. The pores may facilitate gas and / or fluid transport and may increase the amount of catalyst surface area available for reaction.

[0153] The ion conducting layer 1160 may include two or three sublayers, namely, a polymer electrolyte membrane (PEM) 1165, an optional cathode buffer layer 1125, and / or an optional anode buffer layer 1145. One or more layers of the ion conducting layer may be porous. In certain embodiments, at least one layer is non-porous so that reactants and products of the cathode cannot pass to the anode by gas and / or liquid transport, and vice versa. In certain embodiments, the PEM layer 1165 is non-porous. Examples of properties of the anode and cathode buffer layers are provided elsewhere herein. In certain embodiments, the ion conducting layer is exclusively a single layer or includes two sublayers.

[0154] In some embodiments, the carbon oxide electrolyzer anode comprises a blend of an oxidation catalyst and an ionically conductive polymer. Depending on the reactants and anode catalyst provided to the anode, there are various oxidation reactions that can occur at the anode. In one configuration, the oxidation catalyst is selected from the group consisting of metals and oxides of Ir, Pt, Ni, Ru, Pd, Au and their alloys, IrRu, PtIr, Ni, NiFe, stainless steel, and combinations thereof. The oxidation catalyst may further comprise conductive support particles such as carbon, boron-doped diamond, titanium, and any combination thereof.

[0155] By way of example, the oxidation catalyst may be in the form of a structured mesh or in the form of particles. If the oxidation catalyst is in the form of particles, the particles may be supported by electronically conductive support particles. If the oxidation catalyst is in the form of particles, the particles may be supported by electronically conductive support particles. The conductive support particles may be nanoparticles. The conductive support particles may be compatible with the chemicals present in the electrolytic cell anode when the electrolytic cell is operating that are oxidation stable and do not participate in any electrochemical reactions. This is particularly useful when the conductive support particles are selected with the voltage and reactants at the anode in mind. In some configurations, the conductive support particles are titanium, which is well suited for high voltages. In other configurations, the conductive support particles are carbon, which may be most useful at low voltages. In some embodiments, such conductive support particles are larger than the oxidation catalyst particles, and each conductive support particle may support one or more oxidation catalyst particles. In one configuration, the oxidation catalyst is iridium ruthenium oxide. Examples of other materials that can be used for the oxidation catalyst include, but are not limited to, those listed above. It should be understood that many of these metal catalysts may be in the form of an oxide, particularly under reaction conditions.

[0156] As mentioned, in some embodiments, the anode layer of the MEA includes an ion-conducting polymer. In some cases, the polymer includes one or more covalently bonded negatively charged functional groups configured to transport mobile positively charged ions. Examples of second ion-conducting polymers include ethanesulfonyl fluoride, 2-[1-[difluoro-[(trifluoroethynyl)oxy]methyl]-1,2,2,2-tetrafluoroethoxy]-1,1,2,2,-tetrafluoro-, tetrafluoroethylene, tetrafluoroethylene-perfluoro-3,6-dioxa-4-methyl-7-octanesulfonic acid copolymer, other perfluorosulfonic acid polymers, and blends thereof. Examples of commercially available cation-conducting polymers include, for example, Nafion 115, Nafion 117, and / or Nafion 211. Other examples of cation-conducting ionomers described above are suitable for use in the anode layer.

[0157] There may be a tradeoff in selecting the amount of ion-conducting polymer in the anode. For example, the anode may include enough anode ion-conducting polymer to provide sufficient ion conductivity while being porous to allow easy movement of reactants and products therethrough. The anode may also be fabricated to maximize the amount of catalytic surface area available for reaction. In various configurations, the ion-conducting polymer in the anode comprises between about 10 and 90 wt%, or between about 20 and 80 wt%, or between about 25 and 70 wt% of the total anode mass. By way of example, the ion-conducting polymer may comprise between about 5 and 20 wt% of the anode. In certain embodiments, the anode may be configured to withstand relatively high voltages, such as voltages above about 1.2 V versus the reversible hydrogen electrode. In some embodiments, the anode is porous to maximize the amount of catalytic surface area available for reaction and to facilitate gas and liquid transport.

[0158] In one example of a metal catalyst, Ir or IrOx particles (100-200 nm) and Nafion ionomer form a porous layer about 10 μm thick. The loading of the metal catalyst is about 0.5-3 g / cm. 2 It is. In some embodiments, NiFeOx is used for the basic reaction.

[0159] In some embodiments, the MEA and / or associated cathode layer is designed or configured to accommodate gases generated in situ. Such gases can be generated through a variety of mechanisms. For example, carbon dioxide can be generated when carbonate or bicarbonate ions migrating from the cathode to the anode encounter hydrogen ions migrating from the anode to the cathode. This encounter can occur, for example, at the interface of an anion- and cation-conducting ionomer in a bipolar MEA. Alternatively, or additionally, such contact can occur at the interface of the cathode layer and the polymer electrolyte membrane. For example, the polymer electrolyte membrane can include a cation-conducting ionomer that allows transport of protons generated at the anode. The cathode layer can include an anion-conducting ionomer.

[0160] The production of carbon dioxide or other gases, if left unchecked, can delaminate or otherwise damage the MEA, and it can also prevent some of the reactant gases from being reduced at the anode.

[0161] Locations within or adjacent to MEAs where gases such as carbon dioxide are produced in situ may include one or more structures designed to accommodate such gases and, optionally, prevent the gas from reaching the anode (where it would otherwise be unavailable for reaction).

[0162] In certain embodiments, pockets or voids are provided where gas is generated. These pockets or voids may have associated pathways that allow the generated gas to exit the MEA, and optionally to the cathode (where, for example, carbon dioxide can be electrochemically reduced). In certain embodiments, the MEA includes discontinuities at the interfaces of the anion and cation conducting ionomer layers (such as such interfaces in bipolar MEAs). In some embodiments, the cathode structure is constructed in a manner that includes pores or voids that allow carbon dioxide generated at or near the cathode to retreat into the cathode.

[0163] In some embodiments, such discontinuities or void regions are prepared by separately fabricating the anode and cathode structures and then fabricating the MEA in a manner that sandwiches the two separately fabricated structures together in a manner that creates the discontinuities or voids.

[0164] In some embodiments, an MEA structure is fabricated by depositing copper or other catalytic material onto a porous or fibrous matrix, such as a fluorocarbon polymer, and then coating the resulting structure with an anion-conducting ionomer. In some embodiments, the coated structure is then attached to the remainder of the MEA structure, which may include an anode and a polymer electrolyte membrane, such as a cation-conducting membrane.

[0165] In some embodiments, the cathode has a porous structure and / or an associated cathode buffer layer having a porous structure. The pores may be present in an open cell format that allows produced carbon dioxide or other gases to find their way to the cathode.

[0166] In some MEAs, the interface between the anion conducting layer and the cation conducting layer (e.g., the interface of the cathode buffer layer and the PEM) includes features that resist delamination caused by carbon dioxide, water, or other materials that may form at the interface. In some embodiments, the features provide void space for generated materials to occupy until they exit the MEA. In some instances, natural porosity of a layer, such as an anion conducting layer, provides the necessary void space. An interconnected network of pores may provide an escape route for carbon dioxide or other gases generated at the interface. In some embodiments, the MEA includes an interlocking structure (physical or chemical) at the interface. In some embodiments, the MEA includes discontinuities at the interface. In some embodiments, the MEA includes a fibrous structure in one layer adjacent to the interface. Further description of the interface structure between the anion and cation conducting layers of the MEA is included in PCT Publication No. 2021 / 108446, entitled "Membrane Electrode Assembly for COx Reduction," published June 3, 2021, and incorporated herein by reference in its entirety. Cathode catalyst layer Cathode layer function

[0167] The main function of the cathode catalyst layer is to reduce CO x The purpose of the catalyst is to provide a catalyst for the reduction of CO2 + 2H + +2e - →CO+H2O

[0168] The cathode catalyst layer also x They may have other functions that facilitate conversion. These include water management, gas transport, reactant delivery to the metal catalyst, product removal, stabilization of the particulate structure of the metal catalyst, electronic and ionic conduction to the metal catalyst, and mechanical stability within the MEA.

[0169] Certain features and challenges are unique to carbon oxide electrolysers and are not found in MEA assemblies for other applications such as fuel cells or water electrolysers. These challenges include the cathode catalyst layer of the MEA transporting gas (e.g., CO2 or CO) in and transporting gas (e.g., ethylene, methane, CO) or liquid (e.g., ethanol) out. The cathode catalyst layer may be designed or configured to prevent water accumulation that may block gas transport. Additionally, catalysts for COx reduction are sometimes less stable than catalysts such as platinum that may be used in hydrogen fuel cells. These features, these specific challenges, and how they can be addressed are described below. Water management (cathode catalyst layer)

[0170] The cathode catalyst layer facilitates water movement and prevents water from being trapped in the cathode catalyst layer. Trapped water is then converted into CO x access to the catalyst and / or reaction products from migrating out of the cathode catalyst layer.

[0171] The challenge of water management is in many ways CO x It is inherent to the electrolyser. For example, compared to the oxygen electrode of a PEM fuel cell, the CO x Electrolysers use much lower gas flows. x The electrolyser also uses a lower flow rate to reduce the input CO x High utilization of CO is achievable. Gas phase water removal is determined by the volumetric gas flow rate. x The gas phase water removal performed in the electrolyser is much less. xElectrolysers may operate at higher pressures than fuel cells (e.g., 100 psi to 450 psi), and at higher pressures, the same molar flow rate results in lower volumetric flow rates and less gas phase water removal. For some MEAs, the ability to remove gas phase water is further limited by temperature limitations that are not present in fuel cells. For example, CO2 reduction to CO may be performed at about 50°C, and ethylene and methane production may be performed at 20°C to 25°C. This compares to typical operating temperatures of 80°C to 120°C for fuel cells. The result is more liquid phase water to remove.

[0172] Properties that affect the ability of a cathode catalyst layer to remove water include porosity, pore size, pore size distribution, hydrophobicity, the relative amounts of ion-conducting polymer, metal catalyst particles, and electronically conductive support, the thickness of the layer, the distribution of catalyst throughout the layer, and the distribution of ion-conducting polymer around the catalyst throughout the layer.

[0173] The porous layer allows for an exit path for water. In some embodiments, the cathode catalyst layer has a pore size distribution with some pores having a size of about 1 nm to 100 nm and other pores having a size of at least about 1 micron. This size distribution can aid in the removal of water. The porous structure can be formed by one or more of the following: pores within the carbon support structure (e.g., support particles), pores stacked between stacked carbon nanoparticles, pores stacked secondarily between agglomerated carbon spheres (micrometer scale), or pores introduced with inert fillers (e.g., PTFE), where the interface between PTFE and carbon also creates irregular pores in the range of hundreds of nm to micrometers.

[0174] The thickness of the cathode catalyst layer can contribute to water management. By using a thicker layer, the catalyst, and therefore the reaction, can be dispersed over a larger volume. This spreads out the water distribution and makes it easier to manage. In certain embodiments, the thickness of the cathode layer is about 80 nm to 300 μm.

[0175] Ion-conducting polymers with non-polar hydrophobic backbones may be used in the cathode catalyst layer. In some embodiments, the cathode catalyst layer may include a hydrophobic polymer, such as PTFE, in addition to the ion-conducting polymer. In some embodiments, the ion-conducting polymer may be a component of a copolymer that also includes a hydrophobic polymer. In some embodiments, the ion-conducting polymer has hydrophobic and hydrophilic regions. The hydrophilic regions can support water transport and the hydrophobic regions can support gas transport. Gas transport (cathode catalyst layer)

[0176] The cathode catalyst layer is structured for gas transport. Specifically, CO x is transported to the catalyst and the gas phase reaction products (e.g., CO, ethylene, methane, etc.) are transported out of the catalyst bed.

[0177] A particular challenge associated with gas transportation is the CO x Inherent in the electrolyser. Gases are transported in and out of the cathode catalyst layer. x is pumped in and products such as CO, ethylene, and methane are pumped out. In a PEM fuel cell, gas (O2 or H2) is pumped in and either nothing or product water is pumped out. Also, in a PEM water electrolyser, water is a reactant with the O2 and H2 gas products.

[0178] Operating conditions, including pressure, temperature, and flow rate through the reactor, affect gas transport. Properties of the cathode catalyst layer that affect gas transport include porosity, pore size and distribution, layer thickness, and ionomer distribution. Example values ​​for these parameters are provided elsewhere herein.

[0179] In some embodiments, the contact of the ionomer with the catalyst is minimized. For example, the ionomer may form a continuous network along the surface of the carbon while minimizing contact with the catalyst. The ionomer, support, and catalyst may be designed such that the ionomer has a higher affinity for the support surface than the catalyst surface. This may facilitate gas transport to and from the catalyst that is not blocked by the ionomer, while allowing the ionomer to conduct ions to and from the catalyst. Ionomer (cathode catalyst layer)

[0180] The ionomer may have multiple functions, including holding the particles of the catalyst layer together and allowing the movement of ions through the cathode catalyst layer. In some cases, the interaction of the ionomer with the catalyst surface enhances the CO x It creates an environment that is favorable for reduction, which may increase selectivity to the desired product and / or reduce the voltage required for the reaction. It is important that the ionomer is an ionically conductive polymer that allows the movement of ions through the cathode catalyst layer. For example, hydroxide ions, bicarbonate ions, and carbonate ions are transported through the CO x It moves away from the catalyst surface where reduction occurs.

[0181] In certain embodiments, the ion-conducting polymer of the cathode comprises at least one ion-conducting polymer that is an anion conductor, which may be advantageous since it increases the pH compared to proton conductors.

[0182] A variety of anion conducting polymers have been described above. Many of these have aryl groups in their backbones. Such ionomers may be used in the cathode catalyst layer as described herein. In some embodiments, the ion conducting polymer may include one or more covalently bonded, positively charged functional groups configured to transport mobile negatively charged ions. Examples of such ion conducting polymers include aminated tetramethylpolyphenylene; poly(ethylene-co-tetrafluoroethylene) based quaternary ammonium polymers; quaternized polysulfones, blends thereof, and / or any other suitable ion conducting polymer. The first ion conducting polymer may be configured to solubilize bicarbonate or hydroxide salts.

[0183] In some embodiments, the ion-conducting polymer in the cathode comprises at least one ion-conducting polymer that is a cation and anion conductor. Examples of such ion-conducting polymers include polyethers capable of transporting cations and anions, and polyesters capable of transporting cations and anions. Further examples of such ion-conducting polymers include polyethylene oxide, polyethylene glycol, polyvinylidene fluoride, and polyurethane.

[0184] During use in an electrolyser, the cation and anion conductors can increase the local pH (compared to pure cation conductors). Furthermore, in some embodiments, it may be advantageous to use cation and anion conductors to promote a large amount of acid-base recombination rather than at the two-dimensional interface of the anion conducting polymer and the cation conducting polymer. This can spread out the formation of water and CO2, heat generation, and potentially lower the membrane resistance by reducing the barrier to acid-base reactions. All of these can be advantageous to help avoid product build-up, heat, and may be advantageous to lower resistive losses in the MEA, lowering the cell voltage.

[0185] In certain embodiments, the anion conducting polymer has a polymer backbone with covalently attached positively charged functional groups attached thereto. In some embodiments, these may include positively charged nitrogen groups. In some embodiments, the polymer backbone is non-polar as described above. The polymer may have any suitable molecular weight, for example, from 25,000 g / mol to 150,000 g / mol, although it is understood that polymers outside this range may be used.

[0186] CO x A particular challenge with ion-conducting polymers in electrolysers is that CO2 dissolves in the polymers and / or solubilizes them, reducing their mechanical stability and making them more prone to swelling, allowing the polymer to move more freely. This reduces the mechanical stability of the entire catalyst layer and the polymer electrolyte membrane. In some embodiments, polymers that are less susceptible to CO2 plasticization are used. Also, unlike in water electrolysers and fuel cells, conductive carbonate and bicarbonate ions are key parameters for CO2 reduction.

[0187] The introduction of polar functional groups such as hydroxyl and carboxyl groups that can form hydrogen bonds creates a pseudo-crosslinked network. Crosslinkers such as ethylene glycol and aluminum acetylacetonate can be added to strengthen the anion exchange polymer layer and inhibit CO2 plasticization of the polymer. Additives such as polydimethylsiloxane copolymers can also help mitigate CO2 plasticization.

[0188] According to various embodiments, the ion-conducting polymer may have a bicarbonate ion conductivity of at least 6 mS / cm, or in some embodiments at least 12 mS / cm, is chemically and mechanically stable at temperatures up to 80° C., and is soluble in organic solvents used during manufacture, such as methanol, ethanol, and isoproponol. xIt is stable (chemically stable and has stable solubility) in the presence of reduction products. The ion-conducting polymer may be characterized by its ion exchange capacity, the sum of active sites or functional groups participating in ion exchange, which in some embodiments may range from 2.1 mmol / g to 2.6 mmol / g. In some embodiments, ion-conducting polymers with lower IECs, such as greater than 1 or 1.5 mmol / g, may be used.

[0189] Examples of anion conducting polymers are given above in the table as Class A ion conducting polymers.

[0190] The as-received polymers are cleaved by the formation of anions (e.g., I - , Br - etc.) with bicarbonate.

[0191] Also, as noted above, in certain embodiments, the ionomer may be a cation-anion conducting polymer, with examples shown in the table above as Class B ion conducting polymers.

[0192] There are tradeoffs in selecting the amount of cation-conducting polymer in the cathode. The cathode may contain enough cathode ion-conducting polymer to provide sufficient ionic conductivity, but may be porous enough to allow easy movement of reactants and products therethrough, and to maximize the amount of catalytic surface area available for reaction. In various configurations, the cathode ion-conducting polymer comprises about 10-90 wt%, about 20-80 wt%, or about 30-70 wt% of the material in the cathode layer. Metal catalyst (cathode catalyst layer)

[0193] In certain embodiments, the metal catalyst has one or more of the properties listed above. Generally, the metal catalyst is capable of reacting with one or more of the CO xCatalyzes reduction reactions. Metal catalysts can usually be in the form of nanoparticles, although in some embodiments larger particles, films, and nanostructured surfaces may be used. The particular morphology of the nanoparticles can expose and stabilize active sites with greater activity.

[0194] Examples of materials that can be used for the reduced catalyst particles include, but are not limited to, transition metals such as V, Cr, Mn, Fe, Co, Ni, Cu, Zr, Nb, Mo, Au, Ru, Rh, Pd, Ag, Cd, Hf, Ta, W, Re, Ir, Pt, and Hg, and combinations thereof, and / or any other suitable materials. Other catalyst materials can include alkali metals, alkaline earth metals, lanthanides, actinides, and transition metals such as Sn, Si, Ga, Pb, Al, Tl, Sb, Te, Bi, Sm, Tb, Ce, Nd, and In, and combinations thereof, and / or any other suitable catalyst materials. The choice of catalyst can be based on the CO x It depends on the reaction carried out at the cathode of the electrolytic cell.

[0195] The metal catalyst may be composed of a pure metal (e.g., Cu, Au, Ag), although alloys or bimetallic systems may be used for certain reactions. In some embodiments, the metal catalyst includes a dopant. Examples of dopants include boron, nitrogen, and hydrogen. In some cases, the metal catalyst includes boron-doped copper. The concentration of the dopant may be substantially uniform across the metal particle or may vary as a function of distance from the particle surface. For example, the dopant concentration may decrease with distance from the particle surface.

[0196] The choice of catalyst can be guided by the desired reaction. For example, Au can be used for CO production, while Cu can be used for methane and ethylene production. CO2 reduction has a high overpotential compared to other well-known electrochemical reactions such as hydrogen evolution and oxygen evolution over known catalysts. Small amounts of pollutants can poison the catalyst for CO2 conversion.

[0197] Different metal catalyst materials can be selected based, at least in part, on the desired products and operation of the MEA. For example, 1D nanowires can have higher selectivity for ethylene production, while triangular Cu nanoplates can have higher selectivity for methane. Nanocubes can show good selectivity for ethylene in AEM MEAs. Carrier (cathode catalyst layer)

[0198] As explained above, the support structures can be particles. More generally, however, they can have many different shapes, such as spheres, polygons (e.g., triangles), nanotubes, and sheets (e.g., graphene). Structures with a large surface area relative to volume are useful for providing sites for catalyst particles to attach to. Support structures can also be characterized by their porosity, surface area per volume, electrical conductivity, functional groups (N-doped, O-doped, etc.), and the like. Various properties of particulate support structures are presented above.

[0199] If present, the support of the cathode catalyst particles can have any of a variety of functions. The support of the cathode catalyst layer can stabilize the metal nanoparticles to prevent them from agglomerating and distribute the catalytic sites throughout the volume of the catalyst layer to spread out reactant loss and product formation. The support can also provide a conductive path to the metal nanoparticles. For example, carbon particles are packed together such that contacting carbon particles provide a conductive path. The void spaces between the particles form a porous network through which gases and liquids can pass.

[0200] The support may be hydrophobic and have an affinity for the metal nanoparticles.

[0201] In many cases, the conductive support particles are compatible with the chemistry present at the cathode during operation, are reductively stable, and have a high hydrogen production overpotential so as not to participate in any electrochemical reactions, hi certain embodiments, such conductive support particles are larger than the reduced catalyst particles, and each conductive support particle can support many reduced catalyst particles.

[0202] Examples of carbon black that can be used include: ·Vulcan XC-72R-Density 256mg / cm2, 30~50nm ·Ketjen Black-Hollow structure, density 100~120mg / cm2, 30~50nm Printex carbon, 20~30nm Cathode catalyst layer characteristics

[0203] In certain embodiments, the cathode layer has a porosity of about 15-75%. The porosity of the cathode layer can be determined by a variety of techniques. In one method, the loading of each component (e.g., catalyst, support, and polymer) is multiplied by its respective density. These are summed to determine the thickness of the material that the components occupy. This is then divided by the known total thickness to get the percentage of the layer that is occupied by the material. The resulting percentage is then subtracted from 1 to get the percentage of the layer that is assumed to be void space (e.g., filled with air or other gas or vacuum), i.e., the porosity. In some embodiments, the porosity is determined directly by methods such as mercury porosimetry or image analysis of TEM images.

[0204] The cathode layer can also be characterized by its roughness. The surface properties of the cathode layer can affect the resistance across the membrane electrode assembly. An excessively rough cathode layer can potentially result in interfacial gaps between the catalyst and other electronically conductive support layers, such as the current collector or microporous layer. These gaps impede electron transfer from the current collector to the catalyst area, thus increasing the contact resistance. The interfacial gaps can also serve as a place for water accumulation, which is detrimental to the mass transport of reactants and products. On the other hand, very smooth surfaces can have problems with poor contact between the layers. The roughness of the cathode layer can affect the electrical contact resistance and the concentration polarization losses. Surface roughness can be measured by using different techniques (e.g., mechanical stylus methods, optical profilometry, or atomic force microscopy) and is defined as the high-frequency, short-wavelength component of the actual surface. The arithmetic mean height S ais a parameter commonly used to evaluate surface roughness. It is calculated numerically by integrating the absolute height of the valleys and peaks on the surface relative to the average plane over the entire geometric area of ​​the specimen. Cathode layer S between 0.50-1.10 μm or 0.70-0.90 μm a The value may be used in some embodiments.

[0205] Examples of cathode catalyst layer characteristics for CO, methane, and ethylene / ethanol production CO generation: 4 nm diameter Au nanoparticles supported on Vulcan XC72R carbon and mixed with TM1 anion exchange polymer electrolyte from Orion. The layer was approximately 15 μm thick, with Au / (Au+C)=30%, TM1 to catalyst mass ratio of 0.32, and mass loading of 1.4–1.6 mg / cm. 2 , with an estimated porosity of 0.47. Methane production: Cu nanoparticles with sizes of 20-30 nm are supported on Vulcan XC72R carbon and mixed with FAA-3 anion-exchange solid polymer electrolyte from Fumatech. The mass ratio of FAA-3 to catalyst is 0.18. The estimated Cu nanoparticle loading is in a wider range of 1-100 μg / cm. 2 Within about 7.1 μg / cm 2 It is. Ethylene / ethanol production: Cu nanoparticles with sizes ranging from 25 to 80 nm are mixed with FAA-3 anion-exchange solid polymer electrolyte from Fumatech. The mass ratio of FAA-3 to catalyst is 0.10. They are deposited either on Sigracet39BC GDE for pure AEM or on polymer electrolyte membrane. The estimated Cu nanoparticle loading is 270 μg / cm. 2 It is. Bipolar MEA for methane production: The catalyst ink is made of 20nm Cu nanoparticles supported by Vulcan carbon (Premetek 40% Cu / Vulcan XC-72) mixed with FAA-3 anion exchange solid polymer electrolyte (Fumatech). The mass ratio of FAA-3 to catalyst is 0.18. The cathode is formed by ultrasonic spray deposition of the catalyst ink onto a bipolar membrane containing FAA-3 anion exchange solid polymer electrolyte which is spray coated onto a Nafion (PFSA) 212 (Fuel Cell Etc) membrane. The anode is made of 3mg / cm2 of catalyst ink. 2 The MEA consists of IrRuOx spray-coated on the opposite side of the bipolar membrane with a loading of 1.0 μm. A porous carbon gas diffusion layer (Sigracet 39BB) is sandwiched between the Cu catalyst-coated bipolar membrane to form the MEA. Bipolar MEA for ethylene production: The catalyst ink is made of pure 80 nm Cu nanoparticles (Sigma Aldrich) mixed with FAA-3 anion exchange solid polymer electrolyte (Fumatech). The mass ratio of FAA-3 to catalyst is 0.09. The cathode is formed by ultrasonic spray deposition of the catalyst ink onto a bipolar membrane containing FAA-3 anion exchange solid polymer electrolyte, which is spray coated onto a Nafion (PFSA) 115 (Fuel Cell Etc) membrane. The anode is formed by ultrasonic spray deposition of the catalyst ink onto a bipolar membrane containing FAA-3 anion exchange solid polymer electrolyte, which is spray coated onto a Nafion (PFSA) 115 (Fuel Cell Etc) membrane. 2 The MEA consists of IrRuOx spray-coated on the opposite side of the bipolar membrane with a loading of 1.0 μm. A porous carbon gas diffusion layer (Sigracet 39BB) is sandwiched between the Cu catalyst-coated bipolar membrane to form the MEA. CO generation: Au nanoparticles with a diameter of 4 nm are supported on Vulcan XC72R carbon and mixed with TM1 anion exchange polymer electrolyte from Orion. The layer is about 14 microns thick with Au / (Au+C)=20%. In the catalyst layer, the mass ratio of TM1 to catalyst is 0.32 and the mass loading is 1.4-1.6 mg / cm. 2 , the estimated porosity is 0.54. CO generation: Au nanoparticles with a diameter of 45 nm are supported on Vulcan XC72R carbon and mixed with TM1 anion exchange polymer electrolyte from Orion. The layer is about 11 microns thick with Au / (Au+C)=60%. In the catalyst layer, the mass ratio of TM1 to catalyst is 0.16 and the mass loading is 1.1-1.5 mg / cm. 2 and the estimated porosity is 0.41. CO generation: Au nanoparticles with a diameter of 4 nm are supported on Vulcan XC72R carbon and mixed with TM1 anion exchange polymer electrolyte from Orion. The layer is about 25 microns thick with Au / (Au+C)=20%. In the catalyst layer, the mass ratio of TM1 to catalyst is 0.32 and the mass loading is 1.4-1.6 mg / cm. 2 and the estimated porosity is 0.54. PEM

[0206] The MEA may include a polymer electrolyte membrane (PEM) disposed between and conductively coupled to the anode and cathode catalyst layers. In certain embodiments, the polymer electrolyte membrane has high ionic conductivity (e.g., greater than about 1 mS / cm) and is mechanically stable. Mechanical stability may be demonstrated in a variety of ways, such as high tensile strength, modulus, elongation at break, and tear resistance. Many commercially available membranes may be used for the polymer electrolyte membrane. Examples include, but are not limited to, various Nafion® formulations, GORE-SELECT, FumaPEM® (PFSA) (FuMA-Tech GmbH), and Aquivion® (PFSA) (Solvay).

[0207] In one configuration, the PEM includes at least one ion-conducting polymer that is a cation conductor. The third ion-conducting polymer can include one or more covalently bound negatively charged functional groups configured to transport mobile positively charged ions. The third ion-conducting polymer can be selected from the group consisting of ethanesulfonyl fluoride, 2-[1-[difluoro-[(trifluoroethenyl)oxy]methyl]-1,2,2,2-tetrafluoroethoxy]-1,1,2,2,-tetrafluoro-, tetrafluoroethylene, tetrafluoroethylene-perfluoro-3,6-dioxa-4-methyl-7-octenesulfonic acid copolymer, other perfluorosulfonic acid polymers, and blends thereof. Cathode Buffer Layer

[0208] If the polymer electrolyte membrane is a cation conductor (e.g., it conducts protons), it may contain a high concentration of protons during operation of the CRR, while the cathode may operate better when a low concentration of protons is present. A cathode buffer layer may be provided between the polymer electrolyte membrane and the cathode to provide a transition region from a high concentration of protons to a low concentration of protons. In one configuration, the cathode buffer layer is an ion-conducting polymer that has many of the same properties as the ion-conducting polymer in the cathode. The cathode buffer layer may provide a region for the proton concentration to transition from the polymer electrolyte membrane, which has a high proton concentration, to the cathode, which has a low proton concentration. Within the cathode buffer layer, protons from the polymer electrolyte membrane may encounter anions from the cathode, which may neutralize each other. The cathode buffer layer may help ensure that a detrimental number of protons from the polymer electrolyte membrane do not reach the cathode and increase the proton concentration. If the proton concentration in the cathode is too high, CO x No reduction occurs. A high proton concentration may be a concentration in the range of about 10 to 0.1 molar, and a low proton concentration may be a concentration less than about 0.01 molar.

[0209] The cathode buffer layer can include a single polymer or multiple polymers. When the cathode buffer layer includes multiple polymers, the multiple polymers can be mixed together or can be arranged in separate adjacent layers. Examples of materials that can be used for the cathode buffer layer include, but are not limited to, FumaSep FAA-3, Tokuyama anion exchange membrane material, and polyether-based polymers such as polyethylene oxide (PEO), and blends thereof. Further examples are described above in the description of the cathode catalyst layer.

[0210] The thickness of the cathode buffer layer is determined by the low proton concentration and the CO x The thickness is selected to be sufficient to provide high reduction activity. This sufficiency may vary depending on the material of the cathode buffer layer. In general, the thickness of the cathode buffer layer is between about 200 nm and 100 μm, between 300 nm and 75 μm, between 500 nm and 50 μm, or any suitable range.

[0211] In some embodiments, the cathode buffer layer is less than 50 μm, for example, between 1 and 25 μm, such as between 1 and 5 μm, 5 and 15 μm, or 10 and 25 μm. By using a cathode buffer layer of this range of thickness, the proton concentration in the cathode can be reduced while maintaining the overall conductivity of the cell. In some embodiments, ultra-thin layers (100 nm to 1 μm, and in some embodiments, submicron) may be used. Also, as noted above, in some embodiments, the MEA does not have a cathode buffer layer. In some such embodiments, the anion-conducting polymer in the cathode catalyst layer is sufficient. The thickness of the cathode buffer layer can be characterized relative to that of the PEM.

[0212] Water and CO2 formed at the interface of the cathode buffer layer and the PEM can delaminate the MEA to which the polymer layer is attached. The delamination issue can be addressed by using a cathode buffer layer with inert filler particles and associated pores. One possible explanation for its effectiveness is that the pores create a path for the gaseous carbon dioxide to escape back to the cathode where it can be reduced.

[0213] Suitable materials for the inert filler particles include, but are not limited to, TiO2, silica, PTFE, zirconia, and alumina. In various configurations, the size of the inert filler particles is between 5 nm and 500 μm, between 10 nm and 100 μm, or any suitable size range. The particles may be generally spherical.

[0214] Too much PTFE (or other filler) dilutes the polymer electrolyte to the point where it has low ionic conductivity. Too much polymer electrolyte dilutes the PTFE to the point where it is not useful for porosity. In many embodiments, the polymer electrolyte / PTFE mass ratio is 0.25-2, more specifically 0.5-1. The polymer electrolyte / PTFE volume ratio (or, more generally, polymer electrolyte / inert filler) can be 0.25-3, 0.5-2, 0.75-1.5, or 1.0-1.5.

[0215] In other configurations, porosity is achieved by using certain processing methods when the layers are formed. One example of such a processing method is laser ablation, where nano- to micro-sized channels are formed in the layers. Another example is mechanically drilling holes in the layers to form channels through them.

[0216] In one configuration, the cathode buffer layer has a porosity of 0.01%-95% (e.g., by weight, volume, mass, etc., anywhere therebetween). However, in other configurations, the cathode buffer layer can have any suitable porosity (e.g., 0.01-95%, 0.1-95%, 0.01-75%, 1-95%, 1-90%). In some embodiments, the porosity is 50% or less, e.g., 0.1-50%, 5-50%, 20-50%, 5-40%, 10-40%, 20-40%, or 25%-40%. In some embodiments, the porosity is 20% or less, e.g., 0.1-20%, 1-10%, or 5-10%.

[0217] Porosity may be measured as described above in relation to catalyst layers, including using the mass loading and thickness of components with methods such as mercury porosimetry, X-ray diffraction (SAXS or WAXS), and image processing of TEM images to calculate filled versus empty space. Porosity is measured when the MEA is completely dry, since materials swell to different degrees when exposed to water during operation.

[0218] The porosity of the layers of the MEA, including the cathode buffer layer, is discussed further below. Anode Buffer Layer

[0219] In some CRR reactions, bicarbonate is produced at the cathode. It may be useful to have a polymer present that blocks bicarbonate transport somewhere between the cathode and anode, preventing bicarbonate migration from the cathode. Bicarbonate may pick up some CO2 as it migrates, reducing the amount of CO2 available for reaction at the cathode. In some MEA configurations, the polymer electrolyte membrane contains a polymer that blocks bicarbonate transport. Examples of such polymers include, but are not limited to, Nafion® formulations, GORE-SELECT, FumaPEM® (PFSA) (FuMA-Tech GmbH), and Aquivion® (PFSA) (Solvay). In some MEA configurations, there is an anode buffer layer between the polymer electrolyte membrane and the anode, which blocks bicarbonate transport. If the polymer electrolyte membrane is an anion conductor or does not block bicarbonate transport, an additional anode buffer layer to prevent bicarbonate transport may be useful. Materials that can be used to block bicarbonate transport include, but are not limited to, Nafion® formulations, GORE-SELECT, FumaPEM® (PFSA) (FuMA-Tech GmbH), and Aquivion® (PFSA) (Solvay). Of course, if no bicarbonate is present in the CRR, it is not particularly desirable to include bicarbonate blocking functionality in the ion exchange layer.

[0220] In certain embodiments, the anode buffer layer provides a region for the proton concentration to transition from the polymer electrolyte membrane to the anode. The proton concentration in the polymer electrolyte membrane depends on both its composition and the ions it conducts. For example, a Nafion polymer electrolyte membrane that conducts protons has a high proton concentration. A FumaSep FAA-3 polymer electrolyte membrane that conducts hydroxides has a low proton concentration. For example, if the desired proton concentration at the anode differs from the polymer electrolyte membrane by more than three orders of magnitude, the anode buffer layer may be useful to affect the transition from the proton concentration of the polymer electrolyte membrane to the desired proton concentration of the anode. The anode buffer layer may include a single polymer or multiple polymers. If the anode buffer layer includes multiple polymers, the multiple polymers may be mixed together or may be arranged in separate adjacent layers. Materials that may be useful for providing regions for pH transition include, but are not limited to, Nafion, FumaSep FAA-3, Sustainion®, Tokuyama anion exchange polymers, and polyether-based polymers such as polyethylene oxide (PEO), blends thereof, and / or any other suitable materials. A high proton concentration is considered to be in the range of about 10 to 0.1 molar, and a low concentration is considered to be less than about 0.01 molar. Ion-conducting polymers may be classified into different classes based on the type of ion they conduct. This was discussed in detail above. There are three classes of ion-conducting polymers listed in Table 1 above. In one embodiment of the invention, at least one of the ion-conducting polymers in the cathode, anode, polymer electrolyte membrane, cathode buffer layer, and anode buffer layer is of a different class than at least one of the others. Layer Porosity

[0221] It may be useful if some or all of the following layers are porous: cathode, cathode buffer layer, anode, and anode buffer layer. In some configurations, porosity is achieved by combining inert filler particles with the polymers of these layers. Suitable materials for the inert filler particles include, but are not limited to, TiO2, silica, PTFE, zirconia, and alumina. In various configurations, the size of the inert filler particles is between 5 nm and 500 μm, between 10 nm and 100 μm, or any suitable size range. In other configurations, porosity is achieved by using a particular processing method when the layer is formed. One example of such a processing method is laser ablation, where nano- to micro-sized channels are formed in the layer. Laser ablation can additionally or alternatively achieve porosity in the layer by subsurface ablation. Subsurface ablation can form voids in the layer when a beam is focused at a point in the layer, thereby vaporizing the layer material near that point. This process can be repeated to form voids throughout the layer, thereby achieving porosity in the layer. The volume of the voids is preferably determined by the laser power (e.g., higher laser power corresponds to a larger void volume), but can additionally or alternatively be determined by the focal size of the beam, or any other suitable laser parameter. Another example is mechanically drilling holes in the layer to form channels through the layer. The porosity can have any suitable distribution in the layer (e.g., uniform, an increasing porosity gradient through the layer, a random porosity gradient, a decreasing porosity gradient through the layer, periodic porosity, etc.).

[0222] The porosity of the above and other examples and variations (e.g., the porosity of the cathode buffer layer, the anode buffer layer, the membrane layer, the cathode layer, the anode layer, other suitable layers, etc.) preferably has a uniform distribution, but can additionally or alternatively have any suitable distribution (e.g., a randomized distribution, a gradient of increasing pore size through or across the layer, a gradient of decreasing pore size through or across the layer, etc.). The porosity can be formed by any suitable mechanism, such as inert filler particles (e.g., diamond particles, boron-doped diamond particles, polyvinylidene fluoride / PVDF particles, polytetrafluoroethylene / PTFE particles, etc.), and any other suitable mechanism for forming substantially non-reactive regions within the polymer layer. The inert filler particles can have any suitable size, such as a minimum of about 10 nanometers, a maximum of about 200 nanometers, and / or any other suitable size or size distribution.

[0223] As noted above, the cathode buffer layer preferably has a porosity of about 1-90 volume percent, but can additionally or alternatively have any suitable porosity (e.g., including no porosity). However, in other configurations and examples, the cathode buffer layer can have any suitable porosity (e.g., 0.01-95%, 0.1-95%, 0.01-75%, 1-95%, 1-90%, etc.). In some embodiments, the porosity is 20% or less, e.g., 0.1-20%, 1-10%, or 5-10%.

[0224] In some embodiments, the cathode buffer layer is porous, but at least one layer between the cathode layer and the anode layer is non-porous. This can prevent delamination while preventing the passage of gas and / or bulk liquid between the cathode layer and the anode layer. For example, the non-porous layer can prevent the direct passage of water from the anode to the cathode. Further embodiments and conclusions

[0225] Although omitted for simplicity, system and / or method embodiments may include any combination and permutation of the various system components and various method processes, and one or more examples of the methods and / or processes described herein may be performed asynchronously (e.g., sequentially), simultaneously (e.g., in parallel), or in any other suitable order by and / or using one or more example systems, elements, and / or entities described herein.

[0226] As those skilled in the art will recognize from the foregoing detailed description, drawings and claims, modifications and variations to the preferred embodiments of the invention can be made without departing from the scope of the invention, which is defined in the following claims.

Claims

1. Conductive support particles; and metal catalyst particles attached to said conductive support particles, said metal catalyst particles having an average diameter of about 2-100 nm; A catalyst composition comprising:

2. 10. The catalyst composition of claim 1, wherein the metal catalyst particles have a particle size dispersity of up to about 200%.

3. 3. The catalyst composition of claim 2, wherein the metal catalyst particles have a particle size dispersity of up to about 15%.

4. 2. The catalyst composition of claim 1, wherein at least a portion of the metal catalyst particles attached to the conductive support particles have a nearest neighbor metal catalyst particle on each conductive support particle to which they are attached, and the spacing between the nearest neighbor metal catalyst particles has a dispersion of about 50% or less.

5. The catalyst composition according to claim 1, wherein the metal catalyst particles are loaded in the catalyst composition at a mass fraction of about 10 to 80%.

6. 10. The catalyst composition of claim 1, wherein at least about 80% of the conductive particles are attached to the metal catalyst particles.

7. 10. The catalyst composition of claim 1, wherein at least about 95% of said metal catalyst particles are attached to said conductive support particles.

8. 10. The catalyst composition of claim 1, wherein at least about 50% of said metal catalyst particles are single crystal particles.

9. 10. The catalyst composition of claim 1, wherein at least about 85% of the metal catalyst particles have a sphericity of at least about 90%.

10. 10. The catalyst composition of claim 1, wherein the conductive support particles have an average diameter of about 10 to 100 nm.

11. 10. The catalyst composition of claim 1, wherein the conductive support particles have a porosity of about 10% to 80%.

12. The conductive carrier particles have a surface area of ​​about 20 to 2000 cm 3 10. The catalyst composition of claim 1 having a surface area to volume ratio of 100 / 100 g.

13. 10. The catalyst composition of claim 1, wherein the metal catalyst particles comprise at least about 90% atoms of a metal selected from the group consisting of gold, platinum, rhenium, ruthenium, rhodium, palladium, silver, osmium and iridium.

14. 10. The catalyst composition of claim 1, wherein the metal catalyst particles comprise a metal that is gold.

15. 10. The catalyst composition of claim 1, wherein the metal catalyst particles contain about 200 ppm or less of boron or one or more alkali metals.

16. 10. The catalyst composition of claim 1, wherein the metal catalyst particles contain about 20 ppm or less of any transition metal.

17. The catalyst composition of claim 1 , wherein the conductive support particles comprise carbon.

18. 10. The catalyst composition of claim 1, wherein the conductive support particles comprise amorphous carbon.

19. 10. The catalyst composition of claim 1, wherein the conductive support particles comprise carbon black.

20. ionomers; and 20. The catalyst composition according to any one of claims 1 to 19. A cathode catalyst layer comprising:

21. 21. The cathode catalyst layer of claim 20, wherein the ionomer is an anion conducting polymer.

22. A membrane electrode assembly comprising the catalyst layer of claim 20.

Citation Information

Cited By

  • Electrolysis system, reduction electrode, and laminated body

    WO2026177183A1