Silicone Coating for Airbags

A hydrosilylation curable silicone rubber coating with reduced dry coat weight effectively prolongs airbag inflation by using a specific composition, addressing cost and leakage issues in one-piece woven airbags.

JP2024544966APending Publication Date: 2024-12-05DOW SILICONES CORP +1
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2024527812
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2021-11-16
Filing Date
2022-11-10
Publication Date
2024-12-05

AI Technical Summary

Technical Problem

Existing silicone coatings for one-piece woven airbags require high dry coat weights to maintain inflation duration, leading to increased cost and potential gas leakage, while thinner coatings result in rapid deflation during rollover collisions.

Method used

A hydrosilylation curable silicone rubber coating composition with specific components, including an organopolysiloxane polymer, reinforcing fillers, and a hydrosilylation catalyst, is applied to achieve a reduced average dry coat weight of 45-62 g/m², maintaining high gas retention and preventing rapid deflation.

Benefits of technology

The composition ensures the airbag remains inflated for a longer duration, reducing material costs and preventing gas leakage, while maintaining flexibility and thermal stability, thus enhancing occupant protection during rollover accidents.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024544966000001
    Figure 2024544966000001
  • Figure 2024544966000002
    Figure 2024544966000002
  • Figure 2024544966000003
    Figure 2024544966000003
Patent Text Reader

Abstract

The present disclosure relates to integral woven airbags coated with the cured product of a hydrosilylation curable silicone rubber coating composition, and to a process for coating the integral woven airbags with the hydrosilylation curable silicone rubber coating composition. The resulting integral woven airbags coated with the cured product of the hydrosilylation curable silicone rubber coating composition are of reduced average dry coat weight while maintaining the properties of previous integral woven airbags coated with standard thicker coatings.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to integral woven airbags coated with the cured product of a hydrosilylation curable silicone rubber coating composition, and to a process for coating the integral woven airbags with the hydrosilylation curable silicone rubber coating composition. The resulting integral woven airbags coated with the cured product of the hydrosilylation curable silicone rubber coating composition are of reduced average dry coat weight while maintaining the properties of previous integral woven airbags coated with standard thicker coatings. [Background technology]

[0002] Airbags generally consist of a textile bag (sometimes called a cushion), a sensor, and an inflation means. If the sensor detects a crash, the inflator triggers effective instantaneous inflation of the airbag. In the event of an accident, a sensor in the vehicle measures abnormal deceleration and triggers the inflator. Inflation gas from the fill travels through a conduit and fills the airbag, which typically inflates instantly in front of the driver and passengers to protect them from harmful impact with the interior of the car due to the release of gas. Airbags and / or airbag fabrics can be made from woven or knitted fabrics made of synthetic fibers, e.g., polyamides such as nylon-6,6, or polyesters such as polyethylene terephthalate. They can be made from flat pieces of fabric that are coated and then sewn together to provide sufficient mechanical strength, or they can be woven together with an integral woven seam (commonly referred to as "integral weave"). Sewn flat fabric airbags are generally assembled with a coated fabric surface on the inside of the airbag. One-piece woven airbags are coated on the outside of the airbag and tend to be used in airbags that are better able to retain gas pressure after deployment and are therefore designed to remain inflated for a longer period of time after a crash or the like, e.g., side curtain airbags.

[0003] Various airbags are utilized as inflatable safety restraint devices and are designed to inflate and deploy in a crash situation, most notably in a vehicle. Today, it is generally mandatory to have several airbags in a vehicle as a means of providing safety to the occupants in the event of a crash. These include front airbags, front center airbags, side airbags, side curtain airbags, thorax airbags, and / or knee airbags. Typically, the airbags are hidden within the vehicle trim so that they are not visible during normal vehicle operation. For example, front airbags may be installed in the steering wheel on the driver's side of the car and in the dashboard on the passenger's side of the car. They are provided to act as a cushion at the point of impact, especially during a collision with the front or rear of the vehicle. They exhibit a relatively high air permeability, allowing the inflated airbag to rapidly deflate after the initial impact. Typically, these airbags are flat pieces of fabric sewn together.

[0004] Side curtain airbags are increasingly being utilized, and are most often mounted in the headliner above the doors and windows, and deploy from near the ceiling along the side windows to protect vehicle occupants from side impacts and resulting rollover events (where the vehicle rolls on its side, upside down, or flips over two or more times). However, side curtain airbags are primarily designed to protect occupants during rollover collisions by retaining their inflated state for long durations (e.g., exhibiting at least 50% retention of initial pressure after 5 seconds of high pressure inflation), and generally deploy from packing containers stored in the roof line along the side windows of the automobile (thus having only a rear and a front side). Thus, side curtain airbags not only provide a cushioning effect, but also provide protection from broken glass and other debris. Thus, as mentioned above, it is essential that side curtain airbags remain inflated for several seconds until the end of the rollover period resulting from the collision, i.e., they need to retain a large volume of gas as well as a high gas pressure for a longer period of time throughout the potential rollover. Side curtain airbag fabrics, which include sewn or sealed woven blanks, are subject to potentially high gas leakage, especially at and around the seams, and therefore, to accomplish this, they are coated with very large amounts of a silicone sealing material.

[0005] One-piece woven type airbags do not tend to suffer from leakage to the same extent as flat fabric sewn airbags, and are therefore currently commonly used for side curtain airbags in combination with a silicone sealant coating to provide the low permeability (and therefore longer gas leakage time) required for side curtain airbags. The use of one-piece woven (OPW) type airbags allows complex side curtain airbag structures with woven seams to be manufactured with great flexibility in creating patterns and designs. For example, side curtain airbags activated by side impacts are shaped according to the interior contours of the particular car in which they are to be installed. The method of manufacturing such airbags as well as their shape and structure are created at the weaving stage. As a result, no subsequent sewing operations are required. To effectively protect the occupants in a rollover situation, OPW side curtain airbags must remain inflated for several seconds. However, even one-piece woven (OPW) type airbags generally require a 65 g / m2 or higher fabric pressure to achieve this. 2 A silicone coating having an average dry coat weight of at least 100 g is required.

[0006] Silicone coatings are not only designed to prevent air leakage, but also to keep the airbag flexible and resistant to temperature fluctuations, aging, and wear. They require such properties because, for example, airbags can remain unused for long periods of time before a crash triggers deployment. This requires the silicone coatings to be very stable over time to prevent the airbag from sticking and ensure smooth deployment even after many years. Furthermore, inflators are typically designed to emit very hot gases during inflation, and they require good thermal stability to prevent or at least significantly reduce the possibility that the fabric on which the coating is coated will catch fire on the occupant, which could otherwise cause burns to the occupant. Unfortunately, silicone airbag coatings, due to their low permeability properties, require low add-on coating weights, i.e., the aforementioned 65 g / m2 on the target airbag fabric surface.2 Further, while traditionally utilized silicone airbag coatings offer the advantages of excellent durability, aging, and processability, they also tend to exhibit very low tensile strength and elongation at break properties that do not readily withstand high pressure inflation unless very thick coatings are utilized.

[0007] Also, by using an integral woven airbag, the possibility of coating both the front and back of each individual fabric panel has been eliminated. Therefore, there is a greater need to form a relatively thin coating layer only on the outer panel (i.e., the front) of such an article, which has led the industry to understand that without such a heavy coating, the airbag will likely deflate too quickly and therefore not function properly during a rollover collision. These heavy coatings add significant costs to the overall manufacture of the airbag. However, when using a conventionally known curable silicone rubber composition for coating woven fabric to reduce the amount of coating of the curable silicone rubber composition applied to the woven fabric in order to reduce the weight and cost of the curtain airbag, there is a problem that the inflation duration of the airbag becomes too short.

[0008] Thus, a need exists to produce a one-piece woven airbag that uses a silicone airbag coating that has a less expensive (i.e., lower average dry coat weight) silicone airbag coating without losing the aging, moisture, and permeation properties necessary to function properly upon deployment, allowing a manufacturer to reduce their overall total cost of ownership due to a reduction in the amount of silicone coating required, while having the ability to sustain a sufficiently long inflation time, similar to existing materials, to allow the airbag to protect the occupant throughout the duration of the impact. Summary of the Invention

[0009] In this specification, 45 to 62 g / m2 tested according to ISO 3801 21. An integrally woven airbag comprising a coating having an average dry coat weight of a) an organopolysiloxane polymer having a viscosity of 100 to 200,000 mPa.s (inclusive) at 25°C and at least two unsaturated groups per molecule, the unsaturated groups being selected from alkenyl or alkynyl groups; b) reinforcing fillers including fumed silica, precipitated silica and / or calcium carbonate; c) organosilicon compounds having at least two, alternatively at least three, Si-H groups per molecule; d) a hydrosilylation curing catalyst; e) one or more substantially non-functional organosilicon compounds, (i) a silicone resin selected from T silicone resins (silsesquioxanes), DT silicone resins, MQ silicone resins, MDT silicone resins, MTQ silicone resins, QDT silicone resins, or mixtures thereof; and / or (ii) trialkyl-terminated polydiorganosiloxanes; f) one or more monoacrylates, diacrylates or methacrylates, epoxy-containing alkoxysilanes, alkoxysilanes containing methacryl or acrylic groups, and i) one or more alkoxysilanes having an epoxy group in the molecule; ii) a linear organopolysiloxane oligomer containing at least one alkenyl group and at least one hydroxy or alkoxy group per molecule; and iii) an adhesion promoter selected from mixtures and / or reaction products of an organometallic condensation reaction catalyst comprising an organoaluminum compound or an organozirconium compound, or mixtures thereof; the coating has a loss tangent (tan δ) value of at least 0.175 at an angular frequency of 500 rad / sec; tan δ=G” / G'=dynamic loss modulus / dynamic storage modulus, A one-piece woven airbag is provided, as determined by the rheological test method disclosed herein.

[0010] A method for preparing the coated integrally woven airbag described herein above, comprising the steps of: a) an organopolysiloxane polymer having a viscosity of 100 to 200,000 mPa.s (inclusive) at 25°C and at least two unsaturated groups per molecule, the unsaturated groups being selected from alkenyl or alkynyl groups; b) a reinforcing filler comprising fumed silica and / or precipitated silica; c) organosilicon compounds having at least two, alternatively at least three, Si-H groups per molecule; d) a hydrosilylation curing catalyst; e) one or more substantially non-functional organosilicon compounds, (i) a silicone resin selected from T silicone resins (silsesquioxanes), DT silicone resins, MQ silicone resins, MDT silicone resins, MTQ silicone resins, QDT silicone resins, or mixtures thereof; and / or (ii) trialkyl-terminated polydiorganosiloxanes; f) one or more monoacrylates, diacrylates or methacrylates, epoxy-containing alkoxysilanes, alkoxysilanes containing methacryl or acrylic groups, and i) one or more alkoxysilanes having an epoxy group in the molecule; ii) a linear organopolysiloxane oligomer containing at least one alkenyl group and at least one hydroxy or alkoxy group per molecule; iii) mixing the components of a hydrosilylation-curable silicone coating composition comprising an adhesion promoter selected from mixtures and / or reaction products of an organometallic condensation reaction catalyst comprising an organoaluminum compound or an organozirconium compound, or mixtures thereof; Upon curing, the one-piece woven airbag has a hardness of 45-62 g / m2 as determined in accordance with ISO 3801. 2 and coating the integrally woven airbag to have an average dry coat weight of the coating has a loss tangent (tan δ) value of at least 0.175 at an angular frequency of 500 rad / sec; tan δ=G” / G'=dynamic loss modulus / dynamic storage modulus, Methods are also provided, as determined by the rheological test methods disclosed in the Examples herein.

[0011] Preferably, in each of the above cases, the integrally woven airbag, when coated, also has an internal pressure retention characteristic of greater than 60% retained 6 seconds after deployment as determined using a cold gas inflation system capable of pre-holding a predetermined volume of gas or blend of gases to which the airbag is secured, commercially available from Microsys Technologies Inc. At the start of the test, the retained pressure is released from the retention reservoir into the bag. The highest pressure response measured after pressure release is considered the "peak" pressure achieved in the airbag. At the start of the test (P Osec The difference in pressure observed from the target test duration to the pressure hold is commonly referred to as the "pressure hold," with a standard test duration of 6 seconds (P 6sec ) is used.

[0012] The cured product of the hydrosilylation-curable silicone coating composition described herein and coated as described herein above, a monolithic woven airbag has a coating hardness of 45 to 62 g / m2 as determined according to ISO 3801. 2 , 50~62g / m 2In the case of a one-piece woven airbag having an average dry coat weight of 1000g, it is possible to maintain the inflation time of the inflated one-piece woven airbag for a long time even if the coating amount of the composition applied to the woven fabric is reduced for the purpose of reducing weight and cost. Furthermore, the one-piece woven airbag coated with the cured liquid curable silicone rubber composition is excellent for producing curtain airbags. The fact that the loss tangent (tan δ) value of the cured product of the composition is greater than that of the analogue not filled with component (e) suggests that it is more robust and therefore may reduce the amount of damage sustained during the deployment of the airbag. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0013] The composition utilized to prepare the coating includes the following components: Component (a) of the hydrosilylation curable silicone coating composition is one or more organopolysiloxane polymers having a viscosity of 100 to 200,000 mPa.s (inclusive) at 25°C and at least two unsaturated groups per molecule, the unsaturated groups being selected from alkenyl or alkynyl groups. Each organopolysiloxane of component (a) contains a plurality of siloxy units of formula (I): R' a SiO (4-a) / 2 (I) The subscript "a" is 0, 1, 2, or 3.

[0014] The siloxy units may be described by the shorthand nomenclature "M", "D", "T", and "Q", where R' is as above or, alternatively, an alkyl group, typically a methyl group. M units are siloxy units where a=3, i.e., R'SiO 1 / 2 and D units are siloxy units where a=2, i.e., R'SiO 2 / 2 where T units are siloxy units where a=1, i.e., R'1SiO 3 / 2 and Q units are siloxy units where a=0, i.e., SiO 4 / 2The organopolysiloxane polymer of component (a) is substantially linear, but may contain a certain percentage of branching due to the presence of T units (described above) within the molecule, such that the average value of a in structure (I) is about 2.

[0015] The unsaturated groups of component (a) may be located at either the terminal or pendant positions of the organopolysiloxane polymer, or at both positions. The unsaturated groups of component (a) may be alkenyl or alkynyl groups as described above. Each alkenyl group, if present, may contain, for example, 2 to 30, alternatively 2 to 24, alternatively 2 to 20, alternatively 2 to 12, alternatively 2 to 10, alternatively 2 to 6 carbon atoms. If present, the alkenyl groups may be exemplified by, but not limited to, vinyl, allyl, methallyl, propenyl, and hexenyl, and cyclohexenyl groups. Each alkynyl group, if present, may have 2 to 30, alternatively 2 to 24, alternatively 2 to 20, alternatively 2 to 12, alternatively 2 to 10, alternatively 2 to 6 carbon atoms. Examples of alkynyl groups may be exemplified by, but are not limited to, ethynyl, propynyl, and butynyl groups. Preferred examples of unsaturated groups in component (a) include vinyl, propenyl, isopropenyl, butenyl, allyl, and 5-hexenyl.

[0016] In formula (I), each R' other than the above unsaturated groups is independently selected from an aliphatic hydrocarbyl group, a substituted aliphatic hydrocarbyl group, an aromatic group, or a substituted aromatic group. Each aliphatic hydrocarbyl group may be exemplified by, but is not limited to, an alkyl group having 1-20 carbons per group, alternatively 1-15 carbons per group, alternatively 1-12 carbons per group, alternatively 1-10 carbons per group, alternatively 1-6 carbons per group, or a cycloalkyl group such as cyclohexyl. Specific examples of alkyl groups include methyl, ethyl, propyl, pentyl, octyl, undecyl, and octadecyl groups, alternatively methyl and ethyl groups. The substituted aliphatic hydrocarbyl group is preferably a non-halogenated substituted alkyl group.

[0017] Aliphatic non-halogenated organyl groups are exemplified by, but not limited to, the above alkyl groups with suitable nitrogen-containing groups such as amide groups, imide groups, etc.; oxygen-containing groups such as polyoxyalkylene groups, carbonyl groups, alkoxy groups, and hydroxyl groups. Further organyl groups may include sulfur-containing groups, phosphorus-containing groups, and boron-containing groups. Examples of aromatic or substituted aromatic groups are phenyl groups and substituted phenyl groups with the above-mentioned substituents.

[0018] Component (a) may be selected, for example, from polydimethylsiloxanes, alkylmethylpolysiloxanes, alkylarylpolysiloxanes, or copolymers thereof (reference to alkyl means any suitable alkyl group, alternatively an alkyl group having 2 or more carbons), provided that each polymer has the viscosity of the organopolysiloxane polymer (a), which should be between 100 and 200,000 mPa.s (inclusive) at 25°C.

[0019] Thus, component (a) may, for example, be: dialkylalkenyl-terminated polydimethylsiloxanes, such as dimethylvinyl-terminated polydimethylsiloxanes, dialkylalkenyl-terminated dimethylmethylphenylsiloxanes, such as dimethylvinyl-terminated dimethylmethylphenylsiloxanes, trialkyl-terminated dimethylmethylvinylpolysiloxanes, dialkylvinyl-terminated dimethylmethylvinylpolysiloxane copolymers, dialkylvinyl-terminated methylphenylpolysiloxanes, dialkylalkenyl-terminated methylvinylmethylphenylsiloxanes, dialkylalkenyl-terminated methylvinyldiphenylsiloxanes, dialkylalkenyl-terminated methylvinylmethylphenyldimethylsiloxanes, trimethyl-terminated methylvinylmethylphenylsiloxanes, trimethyl-terminated methylvinyldiphenylsiloxanes, or trimethyl-terminated methylvinylmethylphenyldimethylsiloxanes.

[0020] In each case, the viscosity of component (a) organopolysiloxane polymer (a) should be from 100 to 200,000 mPa.s (inclusive) at 25° C., alternatively from 1000 to 150,000 mPa.s at 25° C., alternatively from 1000 mPa.s to 125,000 mPa.s, alternatively from 1000 mPa.s to 70,000 mPa.s at 25° C. Unless otherwise indicated, all viscosity measurements given are zero shear viscosities (η ) obtained by extrapolating values ​​taken at low shear rates to zero (or simply taking the average of the values), insofar as the viscosity-shear rate curve is rate independent. o ) value, which is test method independent, provided a suitable and properly operating rheometer is used. For example, the zero shear viscosity of a material at 25°C can be measured in 0.01 s without exceeding the torque limit of the transducer. -1 , 0.1 seconds -1 , and 1.0 seconds -1 Viscosity measurements may be obtained using a commercially available rheometer such as an Anton-Parr MCR-301 rheometer or a TA Instruments AR-2000 rheometer equipped with a cone and plate fixture of suitable diameter to generate an appropriate torque signal over a range of low shear rates such as 0.1 to 10 seconds on a 25 mm cone and plate. Alternatively, viscosity measurements may be obtained using an ARES-G2 rotational rheometer commercially available from TA Instruments, with a 25 mm cone and plate. -1 If the zero shear plateau region cannot be observed at the shear rates available to the rheometer or viscometer, we use a steady rate sweep of 0.1 s at 25° C. -1 Viscosity measured at a standard shear rate of 100 is reported.

[0021] Typically, the alkenyl and / or alkynyl content, e.g., vinyl content, of the polymer is 0.01 to 3 weight percent of component (a) for each organopolysiloxane containing at least two silicon-bonded alkenyl groups per molecule, alternatively 0.01 to 2.5 weight percent of component (a), alternatively 0.001 to 2.0 weight percent, alternatively 0.01 to 1.5 weight percent of component (a) for each organopolysiloxane containing at least two unsaturated groups per molecule, the unsaturated groups being selected from alkenyl or alkynyl groups per molecule of component (a). The alkenyl / alkynyl content of component (a) is determined using quantitative infrared analysis according to ASTM E168.

[0022] Component (a) may be present in the composition in an amount of from 40% to about 80% by weight of the composition, alternatively from 45 to 80% by weight of the composition, alternatively from 50 to 80% by weight of the composition. Typically, component (a) is present in an amount that is the difference between 100% by weight and the cumulative weight % of the other components / ingredients of the composition.

[0023] Ingredient (b) Component (b) of the hydrosilylation-curable silicone coating composition is a reinforcing filler comprising fumed silica and / or precipitated silica. Finely divided forms of silica are preferred. Reinforcing filler (b), for example, has a relatively high surface area, typically at least 50 m 2 / g (BET method according to ISO9277:2010) is used. For example, 50 to 450 m 2 / g, alternatively 50-400m 2 / gm 2 / g, alternatively 50-300m 2 / g, alternatively 100-300m 2 A filler (e.g., fumed silica) having a surface area of ​​0.1 g / g (BET method according to ISO 9277:2010) is typically used.

[0024] Typically, the reinforcing fillers (b) are naturally hydrophilic (e.g., untreated) silica fillers and are therefore treated with a treating agent to render them hydrophobic. These surface-modified reinforcing fillers (b) do not aggregate and can be homogeneously incorporated into the organopolysiloxane polymer (a) described below, since the surface treatment allows the fillers to be easily wetted by the organopolysiloxane polymer (a).

[0025] Typically, reinforcing filler (b) can be surface-treated with any low molecular weight organosilicon compound disclosed in the art that can be applied to prevent creping of organosiloxane composition during processing.For example, organosilanes, polydiorganosiloxanes, or organosilazanes such as hexaalkyldisilazanes, short-chain siloxane diols, or fatty acid esters such as fatty acid or stearic acid esters can be used to make the filler hydrophobic, thus making it easier to handle and obtain a homogeneous mixture with other components. Specific examples include, but are not limited to, silanol-terminated trifluoropropylmethylsiloxane, silanol-terminated vinylmethylsiloxane, tetramethyldi(trifluoropropyl)disilazane, tetramethyldivinyldisilazane, silanol-terminated MePh siloxane, liquid hydroxyl-terminated polydiorganosiloxane containing an average of 2 to 20 repeating units of diorganosiloxane in each molecule, hexaorganodisiloxane, and hexaorganodisilazane. A small amount of water may be added together with the silica treatment agent as a processing aid.

[0026] The reinforcing silica filler (b) may be pretreated prior to introduction into the hydrosilylation-curable silicone coating composition, or may be treated in situ (i.e., in the presence of at least a portion of the other components of the hydrosilylation-curable silicone coating composition herein) by blending these components together at room temperature or above until the filler is completely treated. Typically, untreated reinforcing filler (b) is treated with a treating agent in situ in the presence of organopolysiloxane polymer (a), thereby resulting in the preparation of a silicone rubber-based material that can later be mixed with the other components.

[0027] The reinforcing filler (b) is present in the composition in an amount from 1.0 to 50% by weight of the composition, alternatively from 1 to 30% by weight of the composition, alternatively from 5.0 to 25% by weight of the composition.

[0028] Ingredient (c) Component (c) functions as a crosslinking agent and is provided in the form of an organosilicon compound having at least two, alternatively at least three, Si-H groups per molecule. Component (c) usually contains three or more silicon-bonded hydrogen atoms so that the hydrogen atoms can react with the unsaturated groups (alkenyl and / or alkynyl groups) of component (a) and / or the rest of the composition to form a network structure, thereby curing the composition. Alternatively, some or all of component (c) may have two silicon-bonded hydrogen atoms per molecule. However, such molecules are used as the only crosslinking agents only when, for example, polymer (a) has more than two unsaturated groups per molecule, in which case a network can be generated during the curing process. Otherwise, when component (c) partially contains a molecule having two silicon-bonded hydrogen atoms per molecule, the molecule may function as a chain extender.

[0029] The molecular architecture of the organosilicon compound (c) having at least two, alternatively at least three, Si-H groups per molecule is not particularly limited and can be a silane, or a linear, branched (linear chain with some branching through the presence of T units), or cyclic polymer, or silicone resin based.

[0030] The molecular weight of component (c) is not particularly limited, but the viscosity may be measured in any suitable manner, and may be determined as the zero shear viscosity (η o ) values.

[0031] The silicon-bonded organic group used in component (c) may be exemplified by alkyl groups such as methyl, ethyl, propyl, n-butyl, t-butyl, pentyl, hexyl, etc.; aryl groups such as phenyl, tolyl, xylyl, or similar aryl groups; 3-chloropropyl, 3,3,3-trifluoropropyl, or similar halogenated alkyl groups, and may preferably be an alkyl group having 1 to 6 carbons, particularly a methyl, ethyl, or propyl group, or a phenyl group. Preferably, the silicon-bonded organic group used in component (c) is an alkyl group, alternatively a methyl, ethyl, or propyl group.

[0032] Examples of organosilicon compounds (c) having at least two, alternatively at least three, Si-H groups per molecule include, but are not limited to, the following: (a) trimethylsiloxy-terminated methylhydrogenpolysiloxane, (b) trimethylsiloxy-terminated polydimethylsiloxane-methylhydrogensiloxane; (c) dimethylhydrogensiloxy-terminated dimethylsiloxane-methylhydrogensiloxane copolymer; (d) dimethylsiloxane-methylhydrogensiloxane cyclic copolymers; (e)(CH3)2HSiO 1 / 2 Unit: (CH3)3SiO 1 / 2 Units, and SiO 4 / 2 copolymers and / or silicone resins consisting of units; (f)(CH3)2HSiO 1 / 2 Units and SiO 4 / 2 copolymers and / or silicone resins consisting of units; (g) methylhydrogensiloxane cyclic homopolymers having 3 to 10 silicon atoms per molecule; Alternatively, the crosslinker, component (c), can be a filler, such as silica treated with one of the above, and mixtures thereof.

[0033] In one embodiment, component (c) is selected from a methylhydrogenpolysiloxane having both molecular terminals blocked with trimethylsiloxy groups; a copolymer of methylhydrogensiloxane and dimethylsiloxane having both molecular chain terminals blocked with trimethylsiloxy groups; a dimethylsiloxane having both molecular chain terminals blocked with dimethylhydrogensiloxy groups; and a copolymer of methylhydrogensiloxane and dimethylsiloxane having both molecular chain terminals blocked with dimethylhydrogensiloxy groups.

[0034] The crosslinker (c) is generally present in the hydrosilylation curable silicone coating composition such that the molar ratio of silicon-bonded hydrogen atoms in component (c) to the total unsaturated groups selected from alkenyl and / or alkynyl groups in the composition is 0.5:1 to 20:1.If this ratio is less than 0.5:1, a sufficiently cured composition is not obtained.If this ratio is more than 20:1, the hardness of the cured composition tends to increase when heated.

[0035] The molar ratio of silicon-bonded hydrogen atoms in component (c) to the total unsaturated groups selected from alkenyl and / or alkynyl groups in organopolysiloxane (a) is preferably at least 1:1 and can be up to 8:1 or 10:1. Most preferably, the molar ratio of Si-H groups to aliphatic unsaturated groups is in the range of from 1.1:1 to 5:1.

[0036] The silicon-bonded hydrogen (Si-H) content of component (c) is determined using quantitative infrared analysis according to ASTM E168. In the present invention, the ratio of silicon-bonded hydrogen to alkenyl (vinyl) and / or alkynyl is important when relying on a hydrosilylation cure process. Generally, this is determined by calculating the total weight percent of alkenyl groups in the composition, e.g., vinyl [V], and the total weight percent of silicon-bonded hydrogen [H] in the composition, where the molecular weight of hydrogen is 1 and the molecular weight of vinyl is 27, resulting in a molar ratio of silicon-bonded hydrogen to vinyl of 27 [H] / [V].

[0037] Typically, component (c) is present in an amount from 0.1 to 10% by weight of the hydrosilylation curable silicone coating composition, alternatively from 0.1 to 7.5% by weight of the hydrosilylation curable silicone coating composition, alternatively from 0.25 to 7.5% by weight, further alternatively from 0.25% to 5% by weight of the hydrosilylation curable silicone coating composition, alternatively from 0.25% to 5% by weight of the hydrosilylation curable silicone coating composition, depending on the number of unsaturated groups in component (a) and the remainder of the composition, and the number of Si-H groups in component (c).

[0038] (d) Hydrosilylation catalyst Component (d) of the hydrosilylation curable silicone coating composition is a hydrosilylation catalyst that comprises or consists of platinum group metals or their compounds.They are usually selected from catalysts of platinum group metals (platinum, ruthenium, osmium, rhodium, iridium, and palladium) or one or more compounds of such metals.Alternatively, platinum and rhodium compounds are preferred due to the high activity level of these catalysts in hydrosilylation reactions, with platinum compounds being the most preferred.In hydrosilylation (or addition) reactions, hydrosilylation catalysts such as component (d) herein catalyze the reaction between unsaturated groups, usually alkenyl groups, such as vinyl, and Si-H groups.

[0039] The hydrosilylation catalyst of component (d) may be a platinum group metal, a platinum group metal deposited on a support, such as activated carbon, a metal oxide such as aluminum oxide or silicon dioxide, silica gel or powdered charcoal, or a compound or complex of a platinum group metal. Preferably, the platinum group metal is platinum.

[0040] Examples of preferred hydrosilylation catalysts of component (d) are platinum-based catalysts such as platinum black, platinum oxide (Adams' catalyst), platinum on various solid supports, chloroplatinic acid such as hexachloroplatinic acid (Pt oxidation state IV) (Speier's catalyst), chloroplatinic acid in a solution of an alcohol such as isooctanol or amyl alcohol (Lamoreaux's catalyst), and complexes of chloroplatinic acid with ethylenically unsaturated compounds such as olefins and organosiloxanes containing ethylenically unsaturated silicon-bonded hydrocarbon groups, such as tetra-vinyl-tetramethylcyclotetrasiloxane-platinum complex (Ashby's catalyst). Usable soluble platinum compounds include, for example, platinum-olefin complexes of the formulae (PtCl2.(olefin)2 and H(PtCl3.olefin), in which in this context it is preferred to use alkenes having 2 to 8 carbon atoms, such as ethylene, propylene, isomers of butene and isomers of octene, or cycloalkanes having 5 to 7 carbon atoms, such as cyclopentene, cyclohexene and cycloheptene. Other soluble platinum catalysts are, for example, platinum-cyclopropane complexes of the formula (PtCl2C3H6)2, hexachloroplatinic acid and alcohols, ethers, etc. and platinum-cyclopropane complexes of formula (PtCl2C3H6)2, which are reaction products of hexachloroplatinic acid and / or its conversion products with vinyl-containing siloxanes such as methylvinylcyclotetrasiloxane in the presence of sodium bicarbonate in an ethanolic solution. Platinum catalysts with phosphorus, sulfur, and amine ligands, such as (Ph3P)2PtCl2, and complexes of platinum with vinyl siloxanes such as sym-divinyltetramethyldisiloxane (Karstedt's catalyst), may also be used.

[0041] Therefore, specific examples of suitable platinum-based catalysts of component (d) include: (i) Complexes of chloroplatinic acid with organosiloxanes containing ethylenically unsaturated hydrocarbon groups, as described in U.S. Pat. No. 3,419,593; (ii) Chloroplatinic acid, either in its hexahydrate or anhydrous form; (iii) platinum-containing catalysts obtained by a process comprising reacting chloroplatinic acid with an aliphatically unsaturated organosilicon compound, such as divinyltetramethyldisiloxane; (iv) alkene-platinum-silyl complexes as described in U.S. Pat. No. 6,605,734, such as (COD)Pt(SiMeCl2)2, where "COD" is 1,5-cyclooctadiene, and / or (v) Karstedt's catalyst, which is a platinum divinyltetramethyldisiloxane complex, typically containing about 1% by weight of platinum in a vinylsiloxane polymer. Historically, solvents such as organic solvents such as toluene have been used as alternatives, but the use of vinylsiloxane polymers is a much more preferred choice. These are described in U.S. Pat. Nos. 3,715,334 and 3,814,730. In a preferred embodiment, component (d) can be selected from platinum coordination compounds. In one embodiment, hexachloroplatinic acid and its conversion products with vinyl-containing siloxanes, Karstedt's catalyst, and Speier's catalyst are preferred.

[0042] The catalytic amount of the hydrosilylation catalyst is generally 0.01 ppm to 10,000 ppm, alternatively 0.01 to 5000 ppm, alternatively 0.01 to 3,000 ppm, alternatively 0.01 to 1,000 ppm, based on the weight of the composition in parts by weight of platinum group metal per million (ppm). In certain embodiments, the catalytic amount of the catalyst may range from 0.01 to 1,000 ppm, alternatively 0.01 to 750 ppm, alternatively 0.01 to 500 ppm, alternatively 0.01 to 100 ppm, based on the weight of the composition. The ranges may relate to only the metal content in the catalyst, or to the entire catalyst (including its ligands), as specified, but typically these ranges relate to only the metal content in the catalyst. The catalyst may be added as a single species or as a mixture of two or more different species. Typically, depending on the form / concentration in which the catalyst is provided, for example in the polymer or solvent, the amount of component (d) present will be in the range of 0.001 to 3.0% by weight of the composition, alternatively 0.001 to 1.5% by weight of the composition, alternatively 0.01 to 1.5% by weight, alternatively 0.01 to 0.1.0% by weight of the hydrosilylation curable silicone coating composition.

[0043] (e) one or more substantially non-functional organosilicon compounds The one or more substantially non-functional organosilicon compounds of component (e) in the hydrosilylation-curable silicone coating composition are (i) a silicone resin selected from T silicone resins (silsesquioxanes), DT silicone resins, MQ silicone resins, MDT silicone resins, MTQ silicone resins, QDT silicone resins, or mixtures thereof; and / or (ii) trialkyl-terminated polydiorganosiloxanes.

[0044] Such resins of component (e)(i) using the MDTQ designation are Q type (SiO 4 / 2 ) Siloxane unit, T type (R 2 1SiO 3 / 2 ) Siloxane unit, D type (R 2 1SiO 3 / 2 ) siloxane unit, and R2 3SiO 1 / 2 (M) siloxane units. These resins can be divided into two broad categories: silsesquioxanes and silicates. Silsesquioxane or T resins consist primarily of T units and can be synthesized by hydrolysis and condensation of alkoxysilanes, chlorosilanes, or mixtures thereof. Silicate or MQ resins consist primarily of M and Q units and can be synthesized through hydrolysis and condensation of alkoxysilanes and chlorosilanes. Alternatively, MQ resins can be synthesized through polymerization of aqueous alkaline silicates in the presence of acid, followed by reaction with triorganoalkoxysilanes, triorganochlorosilanes, hexaorganodisiloxanes, or mixtures thereof.

[0045] Typically, the MQ resin of component (e)(i) is SiO 4 / 2 (Q) Siloxane unit and R 2 3SiO 1 / 2 (M) a siloxane unit, wherein each 2 are the same or different and represent monovalent radicals selected from hydrocarbon radicals having 1 to 20 carbon atoms, alternatively 1 to 12 carbon atoms. 2 Exemplary groups include alkyl groups such as methyl, ethyl, propyl, pentyl, octyl, undecyl, and octadecyl; alicyclic groups such as cyclohexyl; aryl groups such as phenyl, tolyl, xylyl, benzyl, α-methylstyryl, and 2-phenylethyl; alternatively, R 2 The group is a methyl group, an ethyl group, or a phenyl group, for example the preferred non-reactive R 2 3SiO 1 / 2 An example of an (M) siloxane unit is MeSiO 1 / 2 , PhMe2SiO 1 / 2 , and PhMeSiO 1 / 2 Hereinafter, Me refers to methyl, and hereafter, Ph refers to phenyl. The silicone resin may alternatively be referred to as silsesquioxane. The silicone resin may be a single silicone resin or a mixture that includes two or more different silicone resins, each of which may be as described above.

[0046] As specified above, the silicone resin of (e)(i) is substantially non-functional. Substantially non-functional means that the silicone resin of (e)(i) does not have any chemically available groups that can chemically participate in the curing process. Thus, in particular, the substantially non-functional silicone resin of (e)(i) does not contain silicon-bonded hydrogen groups and silicon-bonded alkenyl groups. In the most preferred embodiment, the resin of (e)(i) contains less than 0.035 moles of hydroxyl per mole of Si and does not contain silicon-bonded hydrogen groups and silicon-bonded alkenyl groups. This can be confirmed by infrared analysis according to ASTM E168. The silicone resin of (e)(i) also contains less than 0.06 moles of hydroxyl per mole of silicon (Si), alternatively less than 0.05 moles of hydroxyl per mole of Si, alternatively less than 0.04 moles of hydroxyl per mole of Si, alternatively less than 0.035 moles of hydroxyl per mole of Si, which are: 29 Quantified by Si NMR. Any residual silanols present are sterically inaccessible and cannot participate in subsequent reactions, so that the resin cannot covalently bond to other components in the formulation or to the substrate surface.

[0047] The non-functional silicone resin of (e)(i) is mainly composed of R 2 3SiO 1 / 2 (M) Siloxane unit and SiO 4 / 2 (Q) units. In addition, silicone resins may contain residual OZ, where OZ may represent hydrogen or an alkyl group. OZ remains on the Q component after the synthesis of the silicone MQ resin, indicating incomplete condensation during the reaction to produce the MQ resin, provided that the OZ content meets the above hydroxyl per mole Si requirement. Residual OZ is inherent to the process and reaction utilized to make the MQ resin. Non-functional silicone MQ resins may also undergo a subsequent silylation reaction to further minimize residual OZ.

[0048] The silicone resin (e)(i) is typically supplied in a hydrocarbon or silicone solvent, and the solvent-free silicone resin is typically a solid, but preferably herein the silicone resin (e)(i) is supplied in a silicone solvent such as a non-functional polydimethylsiloxane, e.g., component (e)(ii), or a polydimethylsiloxane containing two or more alkenyl groups per molecule, e.g., sample component (a) herein.

[0049] For example, any suitable MQ resin may be utilized as component (e)(i). The molar ratio of M siloxane units to Q siloxane units has a value from 0.5:1 to 1.2:1, alternatively from 0.6:1 to 1.1:1, alternatively from 0.8:1 to 1.1:1, alternatively from 0.9:1 to 1.1:1. In one embodiment, the MQ resin (e)(i) has a molar ratio of M siloxane units to Q siloxane units of from 0.5:1 to 1.2:1, alternatively from 0.6:1 to 1.1:1, alternatively from 0.8:1 to 1.1:1, alternatively from 0.9:1 to 1.1:1. 4 / 2 siloxane units (i.e., Q units), each of which is bonded to at least one other SiO 4 / 2 The resin comprises a resin portion bonded to a siloxane unit. The molar ratio of M units to Q units is from 0.5:1 to 1.2:1, alternatively from 0.6:1 to 1.1:1, alternatively from 0.8:1 to 1.1:1, alternatively from 0.9:1 to 1.1:1. Such MQ resins suitable as component (e)(i) may have a number average molecular weight (Mn) of from 2000 to 50,000 g / mol, alternatively from 3,000 to 30,000 g / mol. In one embodiment, the silicone resin may be described in terms of mole fraction as an MQ silicone resin having the formula: (R 4 3SiO 1 / 2 ) u (SiO 4 / 2 ) v In the formula, R 4 C1-C without aliphatic unsaturation 10 is a hydrocarbon group, u is from 0.3 to 0.6, alternatively from 0.37 to 0.52, v is from 0.4 to 0.7, alternatively from 0.48 to 0.63, and the value of u+v is 1.0.

[0050] Methods for preparing silicone resins are well known in the art. For example, they can be made by treating a resin copolymer produced by a silica hydrosol capping process with an alkyl and / or alkenyl-containing endblocking agent. This preferably involves reacting a silica hydrosol with a hydrolyzable triorganosilane, such as trimethylchlorosilane, a siloxane, such as hexamethyldisiloxane, and combinations thereof, under acidic conditions, and then reacting the silica hydrosol with an M(RSiO)-based siloxane having 0.07 to 0.2 moles of hydroxyl per mole of silicon (Si). 1 / 2 ) units and Q(SiO 4 / 2 and recovering the copolymer having 1,2-dihydroxyl (OH) units. The copolymer may be further reacted with an endblocking agent containing a saturated organic group to achieve less than 0.06 moles of hydroxyl per mole of Si. Suitable endblocking agents include silazanes, siloxanes, silanes, and combinations thereof.

[0051] The trialkyl terminated polydiorganosiloxane of (e)(ii) may be of any suitable viscosity, for example, from 1000 to 100,000 mPa.s at 25° C., alternatively from 5000 to 80,000 mPa.s at 25° C., alternatively from 10,000 to 70,000 mPa.s at 25° C. Each alkyl end group may be the same or different and have from 1 to 20 carbons, alternatively from 1 to 15 carbons, alternatively from 1 to 12 carbons, alternatively from 1 to 10 carbons. Specific examples of alkyl groups include methyl, ethyl, propyl, pentyl, octyl, undecyl, and octadecyl groups, alternatively methyl and ethyl groups. Preferably, they are methyl groups. The organic groups of the trialkyl-terminated polydiorganosiloxane of (e)(ii) are the same as R' except for the unsaturated groups described above for component (a), i.e., selected from aliphatic hydrocarbyl groups, substituted aliphatic hydrocarbyl groups, aromatic groups, or substituted aromatic groups. Each aliphatic hydrocarbyl group may be exemplified by, but is not limited to, alkyl groups having 1-20 carbons per group, alternatively 1-15 carbons per group, alternatively 1-12 carbons per group, alternatively 1-10 carbons per group, alternatively 1-6 carbons per group, or cycloalkyl groups such as cyclohexyl. Specific examples of alkyl groups include methyl, ethyl, propyl, pentyl, octyl, undecyl, and octadecyl groups, alternatively methyl and ethyl groups. The substituted aliphatic hydrocarbyl groups are preferably non-halogenated substituted alkyl groups. As indicated above, unless otherwise indicated, all viscosity measurements given are based on the zero shear viscosity (η o ) value.

[0052] Component (e) may be present in the composition in an amount of from 1 to 60% by weight, alternatively from 1 to 40% by weight, and is preferably, in the case of (e)(i), in the form of an MQ resin.

[0053] Components (a), (c), (e)(i) and (e)(ii) always consist of a mixture of macromolecular species with different degrees of polymerization and therefore different molecular weights. There are different types of average polymer molecular weights, which can be measured in different experiments. The two most important are the number average molecular weight (Mn) and the weight average molecular weight (Mw). The Mn and Mw of silicone polymers and / or resins can be determined by gel permeation chromatography (GPC) using polystyrene calibration standards. This technique is standard and gives the Mw, Mn and polydispersity index (PI). The degree of polymerisation (DP) = Mn / Mu, where Mn is the number average molecular weight from the GPC measurement and Mu is the molecular weight of the monomer units. PI = Mw / Mn. DP is related to the viscosity of the polymer by Mw, the higher the DP the higher the viscosity. The silicone resin typically has a weight average molecular weight (M) of 2,000 to 50,000 Daltons, alternatively 3,000 to 40,000, alternatively 3,000 to 30,000, alternatively 4,000 to 30,000, alternatively 5,000 to 25,000. w ), which is determined by a triple detector system, including a light scattering detector, a refractive index detector, and / or a viscosity detector, and gel permeation chromatography using polystyrene standards.

[0054] (f) Adhesion promoter The hydrosilylation curable silicone coating composition used to prepare the coating for the integral woven airbag additionally comprises an adhesion promoter (f). The adhesion promoter (f) can be any suitable adhesion promoter that is not detrimental to the physical properties of the cured coating on the airbag. For example, one or more monoacrylates, diacrylates, or methacrylates. Examples include C acrylates such as hexanediol diacrylate, heptanediol diacrylate, octanediol diacrylate, nonanediol diacrylate, and / or undecanediol diacrylate. 4~20Diacrylates may be included, such as alkanediol diacrylates. Examples of monoacrylates include alkoxysilanes containing methacryl or acryl groups, such as methacryloxymethyl-trimethoxysilane, 3-methacryloxypropyl-trimethoxysilane, 3-methacryloxypropyl-methyldimethoxysilane, 3-methacryloxypropyl-dimethylmethoxysilane, 3-methacryloxypropyl-triethoxysilane, 3-methacryloxypropyl-methyldiethoxysilane, 3-methacryloxyisobutyl-trimethoxysilane, or similar methacryloxy-substituted alkoxysilanes, and 3-acryloxypropyl-trimethoxysilane, 3-acryloxypropyl-methyldimethoxysilane, 3-acryloxypropyl-dimethyl-methoxysilane, 3-acryloxypropyl-triethoxysilane, or similar acryloxy-substituted alkyl-containing alkoxysilanes.

[0055] Examples of epoxy-containing alkoxysilanes that may be used as adhesion promoters may include 3-glycidoxypropyltrimethoxysilane, 3-glycidoxypropyltriethoxysilane, 3-glycidoxypropylmethyldimethoxysilane, 4-glycidoxybutyltrimethoxysilane, 5,6-epoxyhexyltriethoxysilane, 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, or 2-(3,4-epoxycyclohexyl)ethyltriethoxysilane.

[0056] The adhesion promoter (f) may alternatively include alkoxysilanes containing methacryl or acryl groups, such as methacryloxymethyl-trimethoxysilane, 3-methacryloxypropyl-trimethoxysilane, 3-methacryloxypropyl-methyldimethoxysilane, 3-methacryloxypropyl-dimethylmethoxysilane, 3-methacryloxypropyl-triethoxysilane, 3-methacryloxypropyl-methyldiethoxysilane, 3-methacryloxyisobutyl-trimethoxysilane, or similar methacryloxy-substituted alkoxysilanes; 3-acryloxypropyl-trimethoxysilane, 3-acryloxypropyl-methyldimethoxysilane, 3-acryloxypropyl-dimethyl-methoxysilane, 3-acryloxypropyl-triethoxysilane, or similar acryloxy-substituted alkyl-containing alkoxysilanes.

[0057] The adhesion promoter (f) may alternatively be i) one or more alkoxysilanes having an epoxy group in the molecule; ii) a linear organopolysiloxane oligomer containing at least one alkenyl group and at least one hydroxy or alkoxy group per molecule; iii) Adhesion promoters including mixtures and / or reaction products of organometallic condensation reaction catalysts including organoaluminum compounds or organozirconium compounds.

[0058] In such a case, (f)(i) the one or more alkoxysilanes having an epoxy group in the molecule may be 3-glycidoxypropyltrimethoxysilane, 3-glycidoxypropyltriethoxysilane, 3-glycidoxypropylmethyldimethoxysilane, 4-glycidoxybutyltrimethoxysilane, 5,6-epoxyhexyltriethoxysilane, 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, or 2-(3,4-epoxycyclohexyl)ethyltriethoxysilane, and (f)(ii) the linear organopolysiloxane oligomer containing at least one alkenyl group and at least one hydroxy group or alkoxy group per molecule may be, for example, a methylvinylpolysiloxane having dimethylhydroxysiloxy units at both molecular terminals, or a copolymer of methylvinylsiloxane and dimethylsiloxane units having dimethylhydroxysiloxy units at both molecular terminals. The oligomeric organopolysiloxane can be a mixture of organopolysiloxane molecules, some of which have silanol end groups at both ends of the molecular chain and some of which have only one silanol group, such as a dimethylhydroxysiloxy end unit, where the other end units are, for example, dimethylmethoxysiloxy, trimethylsiloxy or dimethylvinylsiloxy units. Preferably, more than 50% by weight of the oligomeric organopolysiloxane, more preferably between 60 and 100%, comprises molecules having silanol end groups at both ends of the molecular chain.

[0059] The oligomeric organopolysiloxane preferably contains at least 3% by weight, more preferably at least 5% by weight, of vinyl groups, and may contain up to 35 or 40% by weight of vinyl groups. Most preferably, the oligomeric organopolysiloxane contains 5 to 30% by weight of vinyl groups. The oligomeric organopolysiloxane preferably has a molecular weight of 1000 to 10000. The oligomeric organopolysiloxane preferably has a viscosity of 0.1 to 300 mPa·s, alternatively 0.1 to 200 mPa·s, alternatively 1 to 100 mPa·s. (Measured at 25° C. using a Brookfield DV 3T Rheometer). Component (f)(ii) may be present in the composition in an amount of 0.1 to 5% by weight of the composition, alternatively 0.1 to 3% by weight of the composition, alternatively 0.1 to 2% by weight of the composition.

[0060] The third part of the adhesion promoter, (f)(iii), is an organometallic condensation reaction catalyst comprising an organoaluminum or organozirconium compound that can be used to catalyze the reaction of the other components of the adhesion promoter, i.e., (f)(i) and (ii), and is used to activate and / or accelerate the reaction between them. The condensation catalyst can be selected from organometallic catalysts comprising zirconates, organoaluminum chelates, and / or zirconium chelates.

[0061] Zirconate-based catalysts have the general formula: Zr[OR 5 ]4, where each R5 may be the same or different and represents a monovalent, primary, secondary, or tertiary aliphatic hydrocarbon group, which may be linear or branched, containing 1 to 20 carbon atoms, alternatively 1 to 10 carbon atoms. Optionally, the zirconate may contain partially unsaturated groups. R 5 Preferred examples of R include, but are not limited to, methyl, ethyl, propyl, isopropyl, butyl, tertiary butyl, and branched secondary alkyl groups, such as 2,4-dimethyl-3-pentyl. 5 is the same, preferably, R 5is an isopropyl group, a branched secondary alkyl group or a tertiary alkyl group, in particular a tertiary butyl group. Specific examples include zirconium tetrapropylate and zirconium tetrabutylate, tetra-isopropyl zirconate, zirconium(IV) tetraacetylacetonate (sometimes called zirconium AcAc4), zirconium(IV) hexafluoroacetylacetonate, zirconium(IV) trifluoroacetylacetonate, tetrakis(ethyltrifluoroacetylacetonate)zirconium, tetrakis(2,2,6,6-tetramethylheptanethionate)zirconium. , zirconium(IV) dibutoxybis(ethylacetonate), zirconium tributoxyacetylacetate, zirconium butoxyacetylacetonate bisethylacetoacetate, zirconium butoxyacetylacetonate bisethylacetoacetate, diisopropoxybis(2,2,6,6-tetramethyl-heptanethionate)zirconium, or similar zirconium complexes with β-diketones (including their alkyl- and fluorine-substituted forms) used as ligands.

[0062] Suitable aluminum-based condensation catalysts include Al(OC3H7)3, Al(OC3H7)2(C3COCH2COC 12 H 25 ), Al(OC3H7)2(OCOCH3), and Al(OC3H7)2(OCOC 12 H 25 ) may include, but are not limited to, one or more of:

[0063] Component (f)(iii) may be present in the composition in an amount from 0.1 to 5% by weight of the composition, alternatively from 0.1 to 3% by weight of the composition, alternatively from 0.1 to 2% by weight of the composition. When adhesion promoter (f) is the cumulative amount of (f)(i), (ii), and (iii), it may comprise about 0.3 to 6% by weight of the composition, alternatively from 0.3 to 4% by weight of the composition.

[0064] The adhesion promoter provides strong bonding capabilities between the resulting coating and textile substrates, including woven fabrics.

[0065] Additional Optional Ingredients Additional optional ingredients may be present in the liquid silicone rubber composition, depending on its intended end use. Examples of such optional ingredients include cure inhibitors, thermally conductive fillers, pot life extenders, flame retardants, lubricants, non-reinforcing fillers, pigments and / or colorants, fungicides, wetting agents, heat stabilizers, compression set additives, plasticizers, and mixtures thereof.

[0066] When the hydrosilylation curable silicone coating composition described herein above is cured via addition / hydrosilylation reaction, an inhibitor can be utilized to inhibit the curing of the composition. These inhibitors are utilized to retard or inhibit the activity of the catalyst, thereby preventing premature curing during storage, and / or to provide a longer working time or pot life for the hydrosilylation curing composition. Inhibitors of hydrosilylation catalyst (d), such as platinum metal-based catalysts, are well known in the art and can include hydrazines, triazoles, phosphines, mercaptans, organic nitrogen compounds, acetylene alcohols, silylated acetylene alcohols, maleates such as dibutyl maleate, fumarates, ethylenically or aromatically unsaturated amides, ethylenically unsaturated isocyanates, olefinic siloxanes such as tetramethyltetrazinylcyclotetrasiloxane, unsaturated hydrocarbon monoesters and diesters, conjugated ene-ynes, hydroperoxides, nitriles, and diaziridines. Alkenyl-substituted siloxanes such as those described in US Pat. No. 3,989,667 may also be used, of which cyclic methylvinyl siloxanes are preferred.

[0067] One class of known inhibitors for hydrosilylation catalysts such as platinum catalysts (d) includes the acetylenic compounds disclosed in U.S. Patent No. 3,445,420. Acetylenic alcohols such as 2-methyl-3-butyn-2-ol constitute a preferred class of inhibitors that suppress the activity of platinum-containing catalysts at 25° C. Typically, compositions containing these inhibitors must be heated to temperatures of 70° C. or higher in order to cure at a practical rate.

[0068] Examples of acetylenic alcohols and their derivatives include 1-ethynyl-1-cyclohexanol (ETCH), 2-methyl-3-butyn-2-ol, 3-butyn-1-ol, 3-methylbutynol, 3-butyn-2-ol, propargyl alcohol, 2-phenyl-2-propyn-1-ol, 3,5-dimethyl-1-hexyn-3-ol, 1-ethynylcyclopentanol, 1-phenyl-2-propynol, 3-methyl-1-penten-4-yn-3-ol, and mixtures thereof. In one alternative, the inhibitor is selected from one or more of 1-ethynyl-1-cyclohexanol (ETCH), tetramethyltetrazinylcyclotetrasiloxane, 3-methylbutynol, and / or dibutyl maleate.

[0069] When present, in some cases, inhibitor concentrations as low as 1 mole of inhibitor per mole of metal of catalyst (d) provide sufficient storage stability and cure speed. In other cases, inhibitor concentrations of up to 500 moles of inhibitor per mole of metal of catalyst (d) are required. The optimum concentration for a given inhibitor in a given hydrosilylation-curable silicone coating composition herein is easily determined by routine experimentation. Mixtures of the above may also be used. Depending on the concentration and form in which the selected inhibitor is commercially provided / available, when present in the composition, the inhibitor is typically present in an amount of 0.0001-10% by weight, alternatively 0.001-5% inhibitor, alternatively 0.0125-5% by weight of the composition.

[0070] A pot life extender, such as a triazole, may be used but is not considered essential within the scope of the present invention, and thus the liquid curable silicone rubber composition may be free of a pot life extender.

[0071] Examples of flame retardants include aluminum trihydrate, chlorinated paraffins, hexabromocyclododecane, triphenyl phosphate, dimethylmethylphosphonate, tris(2,3-dibromopropyl)phosphate (brominated tris), and mixtures or derivatives thereof.

[0072] Examples of lubricants include tetrafluoroethylene, resin powder, graphite, fluorinated graphite, talc, boron nitride, fluorine oil, silicone oil, molybdenum disulfide, and mixtures or derivatives thereof.When present in the composition, the flame retardant is typically present in an amount of 0.1 to 5% by weight of the composition.

[0073] Non-reinforcing fillers may include ground quartz, diatomaceous earth, barium sulfate, iron oxide, titanium dioxide, and carbon black, talc, wollastonite. Other fillers that may be used alone or in addition to the above include aluminite, calcium sulfate (anhydrite), gypsum, calcium sulfate, magnesium carbonate, clays such as kaolin, aluminum trihydroxide, magnesium hydroxide such as hydrotalcite, graphite, copper carbonate such as malachite, nickel carbonate such as zarachite, barium carbonate such as witherite, and / or strontium carbonate such as strontium oresite.

[0074] Other fillers may include silicates from the group consisting of aluminum oxide, olivine family, garnet family, aluminosilicates, ring silicates, chain silicates, and layer silicates. The olivine family includes silicate minerals such as, but not limited to, forsterite and Mg2SiO4. The garnet family includes red garnet; Mg3Al2Si3O 12 ; green garnet; and Ca2Al2Si3O 12The aluminosilicates include, but are not limited to, ground silicate minerals such as sillimanite, Al2SiO5, mullite, 3Al2O3.2SiO2, kyanite, and Al2SiO5. Cyclic silicates may be utilized as non-reinforcing fillers, and these include cordierite and Al3(Mg,Fe)2[Si4AlO 18 The chain silicate family includes ground silicate minerals such as wollastonite and Ca[SiO3]. Layered silicates may alternatively or additionally be used as non-reinforcing fillers, suitable groups include silicate minerals such as mica; K2Al 14 [Si6Al2O 20 ](OH)4;phyllite;Al4[Si8O 20 ](OH)4;Talc, Mg6[SiO 20 ](OH)4; serpentine, e.g. asbestos; kaolinite; Al4[Si4O 10

[0036] (OH)8; and vermiculite. In one alternative, the filler is selected from one or more of fumed silica, precipitated silica, calcium carbonate, talc, mica, quartz, and aluminum oxide.

[0075] Examples of pigments include titanium dioxide, chromium oxide, bismuth vanadium oxide, iron oxide, and mixtures thereof.

[0076] Examples of colorants that may be utilized in the hydrosilylation curable silicone coating composition include pigments, vat dyes, reactive dyes, acid dyes, chrome dyes, disperse dyes, cationic dyes, and mixtures thereof. The dual moisture curable organopolysiloxane composition described herein may further include one or more pigments and / or colorants that may be added as needed. The pigments and / or colorants may be colored, white, black, metallic effect, and luminescent, such as fluorescent and phosphorescent. The pigments are utilized as needed to color the composition. Any suitable pigment may be utilized as long as it is compatible with the compositions herein. In the dual moisture curable organopolysiloxane composition, pigments and / or colored (non-white) fillers, such as carbon black, may be used in the catalyst package to color the end sealant product.

[0077] Suitable white pigments and / or colorants include titanium dioxide, zinc oxide, lead oxide, zinc sulfide, lithopone, zirconium oxide, and antimony oxide.

[0078] Suitable non-white inorganic pigments and / or colorants include, but are not limited to, iron oxide pigments such as goethite, lepidocrite, hematite, maghemite, and magnetite, black iron oxide, yellow iron oxide, brown iron oxide, and red iron oxide; blue iron pigments; chromium oxide pigments; cadmium pigments such as cadmium yellow, cadmium red, cadmium cinnabar; bismuth pigments such as bismuth vanadate and bismuth molybdate vanadate; mixed metal oxide pigments such as cobalt titanate green; chromate and molybdate pigments such as chrome yellow, molybdate red, and molybdate orange; ultramarine pigments; cobalt oxide pigments; nickel antimony titanate; lead chromium; carbon black; lamp black, and metallic effect pigments such as aluminum, copper, copper oxide, bronze, stainless steel, nickel, zinc, and brass.

[0079] Suitable organic non-white pigments and / or colorants include phthalocyanine pigments such as phthalocyanine blue and phthalocyanine green; monoarylide yellow, diarylide yellow, benzimidazolone yellow, heterocyclic yellow, DAN orange, quinacridone pigments such as quinacridone magenta and quinacridone violet; organic reds including metallized azo reds and non-metallized azo reds and other azo pigments, monoazo pigments, diazo pigments, azo pigment lakes, β-naphthol pigments, naphthol AS pigments, benzimidazolone pigments, diazo condensed pigments, isoindolinone and isoindoline pigments, polycyclic pigments, perylene and perinone pigments, thioindigo pigments, anthrapyrimidone pigments, flavanthrone pigments, anthanthrone pigments, dioxazine pigments, triarylcarbonium pigments, quinophthalone pigments, and diketopyrrolopyrrole pigments.

[0080] Typically, the pigment and / or colorant, when particulate, has an average particle size in the range of 10 nm to 50 μm, preferably in the range of 40 nm to 2 μm. When present, the pigment and / or colorant is present in a range of from 2 wt % of the catalyst package composition, alternatively from 3 wt %, alternatively from 5 wt % to 20 wt %, alternatively up to 15 wt % of the catalyst package composition, alternatively up to 10 wt % of the catalyst package composition.

[0081] In a preferred embodiment of the present invention, the pigment and dye are used in the form of a pigment master batch constituted by dispersing them in the component (a) at a ratio of 25:75 to 70:30.

[0082] The hydrosilylation curable silicone coating composition can be a heat-stabilized hydrosilylation curable silicone coating composition.Examples of heat stabilizers can include metal compounds, such as red iron oxide, yellow iron oxide, ferric hydroxide, cerium oxide, cerium hydroxide, lanthanum oxide, copper phthalocyanine, aluminum hydroxide, fumed titanium dioxide, iron naphthenate, cerium naphthenate, cerium dimethyl polysilanolate, and acetylacetone salts of metals selected from copper, zinc, aluminum, iron, cerium, zirconium, titanium, etc.Other examples of heat stabilizers can include suitable antioxidants or metal scavengers, such as salicyloylaminotriazole, 1,2-bis(3,5-di-tert-butyl-4-hydroxylhydrocinnamoyl)hydrazine, 2-hydroxy-N-1H-1,2,4-triazol-3-ylbenzamide, and N'1,N'12-bis(2-hydroxybenzoyl)dodecane dihydrazide. When present, the amount of heat stabilizer in the hydrosilylation-curable silicone coating composition can range from 0.01 to 1.0 percent by weight of the total composition.

[0083] In one embodiment, the thickness is 45 to 62 g / m2 as determined according to ISO 3801. 2 The integrally woven airbag includes a coating having an average dry coat weight of a) an organopolysiloxane polymer (a) having a viscosity of from 100 to 200,000 mPa.s (inclusive) at 25° C., alternatively from 1000 to 150,000 mPa.s at 25° C., alternatively from 1000 mPa.s to 125,000 mPa.s, alternatively from 1000 mPa.s to 70,000 mPa.s at 25° C., and having at least two unsaturated groups per molecule selected from alkenyl and / or alkynyl groups, in an amount of from 40% to about 80% by weight of the composition, alternatively from 45 to 80% by weight of the composition, alternatively from 50 to 80% by weight of the composition; b) a reinforcing filler comprising fumed silica and / or precipitated silica, the filler having a viscosity of at least 50 ml2 / g (BET method according to ISO 9277:2010), alternatively 50-450m 2 / g, alternatively 50-400m 2 / gm 2 / g, alternatively 50-300m 2 / g, alternatively 100-300m 2 / g (BET method according to ISO 9277:2010), said reinforcing fillers (b) typically being treated to render them hydrophobic and present in an amount of 1.0 to 50% by weight of the composition, alternatively 1 to 30% by weight of the composition, alternatively 5.0 to 25% by weight based on the weight percent of the composition; and c) an organosilicon compound having at least two, alternatively at least three, Si-H groups per molecule, preferably wherein the molar ratio of silicon-bonded hydrogen atoms in component (c) to the total unsaturated groups selected from alkenyl and / or alkynyl groups in the composition is from 0.5:1 to 20:1, or alternatively wherein the molar ratio of silicon-bonded hydrogen atoms in component (c) to the total unsaturated groups selected from alkenyl and / or alkynyl groups in organopolysiloxane (a) is preferably at least 1:1, and can be up to 8:1 or 10:1. Most preferably, the molar ratio of Si-H groups to aliphatically unsaturated groups ranges from 1.1:1 to 5:1 and the organosilicon compound having at least two, alternatively at least three, Si-H groups per molecule is present in an amount from 0.1 to 10% by weight of the hydrosilylation curable silicone coating composition, alternatively from 0.1 to 7.5% by weight of the hydrosilylation curable silicone coating composition, alternatively from 0.5 to 7.5% by weight, and further alternatively from 0.5% to 5% by weight of the hydrosilylation curable silicone coating composition. Component (c) functions as a crosslinker. d) a hydrosilylation cure catalyst, wherein the catalytic amount of the hydrosilylation catalyst is from 0.01 ppm to 10,000 parts by weight of platinum group metal per million parts (ppm) based on the weight of the composition, alternatively from 0.01 to 5000 ppm, alternatively from 0.01 to 3,000 ppm, alternatively from 0.01 to 1,000 ppm, alternatively from 0.01 to 750 ppm, alternatively from 0.01 to 500 ppm, alternatively from 0.01 to 100 ppm of metal based on the weight of the composition, where the amount of component (d) present ranges from 0.001 to 3.0% by weight of the composition, alternatively from 0.001 to 1.5% by weight of the composition, alternatively from 0.01 to 1.5% by weight, alternatively from 0.01 to 0.1.0% by weight of the hydrosilylation curable silicone coating composition, depending on the form / concentration in which the catalyst is provided, for example, in a polymer or solvent; e) one or more substantially non-functional organosilicon compounds, (i) a silicone resin selected from T silicone resins (silsesquioxanes), DT silicone resins, MQ silicone resins, MDT silicone resins, MTQ silicone resins, QDT silicone resins, or mixtures thereof; and / or (ii) trialkyl-terminated polydiorganosiloxanes; an organosilicon compound in an amount of 1 to 60% by weight of the composition, alternatively 1 to 40% by weight; f) one or more monoacrylates, diacrylates or methacrylates, epoxy-containing alkoxysilanes, alkoxysilanes containing methacryl or acrylic groups, and i) one or more alkoxysilanes having an epoxy group in the molecule in an amount of 0.1 to 5% by weight of the composition, alternatively 0.5 to 3% by weight of the composition, alternatively 0.5 to 2% by weight of the composition; ii) a linear organopolysiloxane oligomer containing at least one alkenyl group and at least one hydroxy or alkoxy group per molecule in an amount from 0.1 to 5% by weight of the composition, alternatively from 0.1 to 3% by weight of the composition, alternatively from 0.1 to 2% by weight of the composition; and iii) an adhesion promoter selected from mixtures and / or reaction products of an organometallic condensation reaction catalyst comprising an organoaluminum compound or an organozirconium compound, or mixtures thereof, in an amount from 0.1 to 5% by weight of the composition, alternatively from 0.1 to 3% by weight, alternatively from 0.1 to 2% by weight of the composition; wherein the adhesion promoter (f) is typically present in the composition in a cumulative amount of (f)(i), (ii), and (iii) from about 0.3 to 6 alternatively 0.3 to 4 weight percent of the composition, and the composition can be any combination of the above ranges, with the total weight percent being 100 weight percent.

[0084] Typically, prior to use, compositions utilized to make integral woven airbag coatings are stored in two parts, Part A and Part B, to keep components (c) (crosslinker) and (d) hydrosilylation cure catalyst separate to prevent premature cure. Typically, Part A compositions include components (a) polymer, (b) reinforcing filler, and (d) hydrosilylation cure catalyst, and Part B includes components (a), (b), and (c) crosslinker, and inhibitors, if present. Both of the above components (e)(i) and / or (ii) may be present in either or both Part A and Part B. When utilizing the reaction product of (f)(i), (f)(ii), and (f)(iii) with respect to adhesion promoters, component (f)(iii) is typically stored in Part A and components (f)(i) and (ii) in Part B to prevent premature reaction.

[0085] When present, additives in the composition can be present in either Part A or Part B, so long as they do not adversely affect the properties of any other components (e.g., catalyst deactivation). Parts A and B of the hydrosilylation-curable silicone coating composition described herein are mixed together immediately prior to use to initiate the cure of the entire composition into a silicone elastomeric material. The composition can be designed to be mixed in any suitable ratio, for example, Part A:Part B can be mixed together in a ratio of 10:1 to 1:10, alternatively 5:1 to 1:5, alternatively 2:1 to 1:2, but most preferably in a 1:1 ratio.

[0086] Each component of Part A and / or Part B may be mixed together individually, or may be introduced into the composition in a pre-prepared combination, for example to facilitate mixing of the final composition. For example, components (a) and (b) are often mixed together to form an LSR polymer base or masterbatch, prior to addition with the other components. These may then be mixed directly with the other components of the part being manufactured, or may be used to make pre-prepared concentrates, commonly referred to in the industry as masterbatches.

[0087] In this case, to facilitate mixing of the components, one or more masterbatches may be utilized to facilitate mixing of the components to form the Part A and / or Part B compositions. For example, a "fumed silica" masterbatch may be prepared, which is effectively an LSR silicone rubber base with silica treated in situ.

[0088] The A and B parts of the composition can be prepared by combining all of the respective components at ambient temperature. Any mixing technique and equipment described in the prior art can be used for this purpose. The specific equipment used will be determined by the viscosity of the components and the final composition. Suitable mixers include, but are not limited to, paddle-type mixers, such as planetary mixers, and kneader-type mixers. It may be desirable to cool the components during mixing to avoid premature hardening of the composition.

[0089] Prior to use, the respective Part A and Part B components are mixed together in the desired ratio.

[0090] As part of the method herein, the coating composition described herein above can be applied to a fabric substrate, typically an integrally woven airbag substrate, by any suitable known technique. These include spraying, gravure coating, bar coating, knife-over-roll coating, knife-over-air coating, padding, dipping, and screen printing. The coating composition can be applied to an airbag fabric that is cut into pieces and sewn to assemble an airbag, or to an integrally woven airbag, but is especially suitable for use in an integrally woven airbag, designed to hold the airbag in an inflated form for several seconds after impact, and therefore considering that side curtain airbags, which are generally integrally woven, are much better designed to avoid gas leakage / permeability after deployment, and are the type that are primarily maintained in an inflated state for a critical few seconds immediately after impact to protect the occupants of a vehicle, etc.

[0091] Curing of the hydrosilylation-curable silicone coating composition of the present invention that has been applied to the woven fabric is typically carried out by heating the composition at a temperature of 150-200° C. for a period of 1-2 minutes.

[0092] Although not preferred, it is possible to apply the composition in multiple layers, which together have the above average dry coat weight. If deemed necessary, it is also possible to apply an additional compatible coating to the coating composition, for example, of a material that provides low friction.

[0093] This disclosure applies to a fiber size range of 45-62 g / m2 determined according to ISO 3801. 2and a method for preparing the coated integrally woven airbag. The integrally woven airbag may be made from any suitable woven fabric, particularly a plain weave fabric, but may be, for example, a knitted or nonwoven fabric. The fabric may be made from synthetic fibers or blends of natural and synthetic fibers, such as polyamides such as nylon 6, nylon 66, nylon 46, polyester fibers such as polyethylene terephthalate, polybutylene terephthalate, polyimide, polyethylene, polypropylene, polyester-cotton, polyacrylonitrile fiber fabrics, aramid fiber fabrics, polyetherimide fiber fabrics, polysulfone fiber fabrics, carbon fiber fabrics, rayon fiber fabrics, and / or glass fibers. For applications requiring high strength, such as, for example, an integrally woven airbag for an automobile, it is preferable to use polyamide fiber fabrics or polyester fiber fabrics. Before coating with the liquid curable silicone rubber composition of the present invention, the woven fabric is preferably washed with water and dried.

[0094] For use as integral woven airbag fabrics, the fabric should be sufficiently flexible to be able to fold into a relatively small volume, but also have sufficient strength to withstand high speed deployment, e.g., under the influence of an explosive charge. Polyamide and polyester fibers are particularly preferred for making airbag textiles. However, it can be difficult to adhere coatings to polyamide and polyester airbags, and hence the need for adhesion promoters, such as component (f) in the above compositions as the coating compositions described hereinabove must have good adhesion to plain woven nylon and polyester fabrics. Thus, the coating compositions described herein are designed to have particularly good adhesion and film-forming properties immediately upon contact with the fabric, such that the film formation on the surface of the fabric being coated is uniform. Preferably, they also have a lower than normal adhesion and film-forming properties, e.g., 45-62 g / m2, as determined according to ISO 3801, while unexpectedly obtaining a cured coating having a loss tangent (tan δ) value of at least 0.175. 2 Alternatively, 50-62g / m2 It also has good penetration into fabrics due to its ability to achieve an average dry coat weight of

[0095] The loss tangent (tan δ) value represents the ability of the cured product of the compositions described herein to dissipate energy versus its ability to store energy. Because the cured coating is viscoelastic, when a deformation such as shear occurs (or in this case when the airbag deploys due to a crash), some of the energy is stored elastically (represented by G') and the rest is dissipated as heat (represented by G"). A higher loss tangent (tan δ) value is better at absorbing the energy of the impact and reducing the amount of damage sustained during deformation, and therefore a more dissipative material will not sustain as much damage during the deployment of an integrally woven airbag.

[0096] Additionally, preferably such airbags, when coated with the compositions described herein, avoid immediate deflation and have greater than 60% internal pressure retention after 6 seconds of deployment, alternatively 62% or greater internal pressure retention after 6 seconds, using the test method described above. Despite having a thinner coating on the integral woven airbag than conventional coatings for side curtain airbags, reduced gas permeability and / or good air tightness can be maintained for a period of time in the curtain airbag after a crash and subsequent rollover, e.g., about 6 seconds, thus avoiding complete deflation and providing protection to the occupant during the critical period of the first few seconds after a crash.

[0097] The coated integral woven airbag obtained by coating the hydrosilylation curable silicone coating composition described herein on the uncoated integral woven airbag has at least one coating layer formed from the cured product from the hydrosilylation curable silicone coating composition described herein.However, if necessary, one or more additional layers can be provided on the coated woven fabric.Such additional layers are typically applied to improve the feel of the surface of the coated woven fabric, improve the abrasion resistance of the surface of the coated woven fabric, and / or improve the strength of the coated woven fabric.The additional coating layer can be exemplified by a coating layer formed from a plastic film, a woven fabric, a nonwoven fabric, or an elastic coating material other than the cured silicone rubber of the present invention.Preferably, no additional layer is required or desired.

[0098] This technology can be used in any suitable integral woven airbag application, particularly in the automotive market, but also as an escape chute from an aircraft, for example. The airbag coated with the cured product of the curable silicone composition can be coated with a lower average dry coat weight than existing materials when coated on an integral woven airbag. As a result, this provides an overall lower total cost of ownership for manufacturers due to the reduction in the amount of silicone coating required, as well as achieving a reduction in mass for vehicle weight reduction considerations. Advantageously, this reduction in average dry coat weight is achieved by the coated airbag having the ability to sustain a sufficiently long inflation time, allowing the integral woven airbag to protect the occupant throughout the duration of the impact encountered, for example, in a vehicle rollover accident. EXAMPLES

[0099] In the following examples, compositions are defined in weight percent (wt%) unless otherwise specified.

[0100] The vinyl and Si-H group contents were determined by infrared spectroscopy according to ASTM E168 using the standards of carbon double bond stretching and silicon-hydrogen bond stretching, respectively.

[0101] Viscosity determination Unless otherwise indicated, all viscosity measurements given are zero shear viscosities (η ) obtained by extrapolating values ​​taken at low shear rates to zero (or simply taking the average of the values) insofar as the viscosity-shear rate curve is rate independent. o ) values, which are test method independent, provided that a suitable and properly operating rheometer is used. Viscosity measurements were taken using an ARES-G2 rotational rheometer available from TA Instruments, over a 25 mm cone and plate at 0.1 to 10 seconds. -1 When the zero shear plateau region could not be observed at the shear rates available to the rheometer or viscometer, we used a steady rate sweep of 0.1 s at 25°C. -1 Viscosity measured at a standard shear rate of 100 is reported.

[0102] M vi A comparative example was prepared that included Q resin, and two examples according to the compositions described above were also prepared using the compositions provided in Table 1. The compositions were prepared as binary compositions.

[0103] [Table 1]

[0104] [Table 2]

[0105] Polymer 1 was a dimethylvinylsiloxy-terminated dimethylsiloxane having a vinyl content of 0.085% by weight and a viscosity of 57,000 mPa.s at 25°C. The treated filler in Polymer 1 was 29.8 wt. % CAB-0-SIL™ MS-75D fumed silica (commercially available from Cabot Corporation), which was treated in situ with hexamethyldisilazane (HMDZ). Polymer 2 was a dimethylvinylsiloxy-terminated dimethylsiloxane having a vinyl content of 0.42 wt % and a viscosity of 400 mPa.s at 25°C. Polymer 3 was a trimethyl-terminated polydimethylsiloxane having a viscosity of 60,000 mPa.s at 25°C. The crosslinker was a trimethylsiloxy-terminated dimethylmethylhydrogensiloxane having a Si-H content of 0.46 wt % and a viscosity of 5.3 mPa.s. The catalyst used was Karstedt's catalyst. M in polymer 1 vi Q resin is 27% by weight of M in polymer 1. vi The MQ resin had dimethylvinyl M groups in a mixture with the Q resin, and the blend had a combined vinyl content of 0.66 wt %. The MQ resin in polymer 1 has the formula (molar fraction): (MeSiO 1 / 2 ) u (SiO 4 / 2 ) v where Me is methyl, u is 0.3-0.6, v is 0.4-0.7, and the value of u+v is 1.0. The MQ resin was present in the mixture with Polymer 1 in an amount of 45 wt %. Adhesive package component 1 was gamma-glycidoxypropyltrimethoxysilane. Adhesive package component 2 was a dimethylhydroxy terminated dimethylmethylvinylsiloxane having a vinyl content of 11.2% by weight and a viscosity of 23 mPa.s at 25°C. Adhesive package component 3 was a mixture of 50% by weight zirconium acetylacetonate in polymer 2. The heat stabilizing additive was 2-hydroxy-N-1H-1,2,4-triazol-3-ylbenzamide.

[0106] Preparation process As a first step, an in-situ treated fumed silica masterbatch was prepared in a Kneader mixer by mixing the ingredients shown in Table 1 and removing residual water and treating agents. The ingredients identified in Table 1 were then used to prepare each of the Part A and Part B compositions, where additional ingredients were introduced into the silicone rubber base of the treated filler in Polymer 1. Each of the Part A and Part B compositions were then mixed together and the resulting compositions were either coated onto integral woven airbags or prepared for physical property testing as described below.

[0107] Method for measuring mechanical properties of silicone rubber The physical properties of the comparative and example samples and the corresponding cured samples were prepared and analyzed, and the results are shown in Table 2 below.

[0108] In each case, for this analysis, the liquid curable silicone rubber composition was subjected to a press cure at 120° C. under a pressure of 30 tons for 10 minutes to obtain a 2 mm thick cured silicone rubber specimen. The hardness of the silicone rubber was measured by a Shore A durometer in accordance with ASTM D 2240. The tensile strength, elongation at break, and modulus results of the dumbbell specimen (No. 7) were measured in accordance with Japanese Industrial Standard JIS K 6251 using an MTS™ Criterion Model C41 available from MTS Systems equipped with a 500 N load cell, and the nominal strain and elongation were measured by the crosshead distance based on an initial gauge length of 40 mm.

[0109] [Table 3]

[0110] The loss tangent (tan δ) values ​​were then analyzed for each example, and the coating compositions of each example and comparative example were coated onto a one-piece woven airbag in an amount that resulted in the average dry coat weight described herein above, and analyzed for internal pressure retention properties.

[0111] Method for measuring loss tangent (tan δ) values: Part A composition and Part B composition were mixed in a high speed mixer in a 1:1 weight ratio. The materials were loaded into an Anton Paar MCR-301 rheometer with 25 mm aluminum parallel plates. The temperature was increased from 23°C to 150°C using a Peltier heating device (5°C / min ramp rate) under constant normal force, constant oscillatory strain of 0.1% and constant angular frequency of 1 rad / sec. The temperature was then held for 20 minutes to cure the composition. Afterwards, the temperature was reduced to 23°C and held for another 20 minutes. The elastic modulus and tan δ were then measured as a function of angular frequency (0.01 rad / sec to 500 rad / sec) by a frequency sweep process (oscillating strain of 0.1% and angular frequency of 1 rad / sec).

[0112] Internal pressure retention characteristics The Part A composition and the Part B composition were mixed in a high-speed mixer in a 1:1 weight ratio. The final compositions of C.1, Example 1, and Example 2 were each coated onto the same integral woven airbag made of PET (woven polyethylene terephthalate) by knife coating. The coated fabric was then cured at 196°C for 1 minute.

[0113] The airbag was then tested using a commercially available cold gas inflation system from Microsys Technologies Inc., which is capable of pre-holding a predetermined volume of gas or blend of gases to which the airbag is secured. At the start of the test, a predetermined pressure is released from the holding reservoir into the bag. The internal space of the resulting coated hollow woven fabric was inflated by blowing compressed gas under a pressure of 165 kPa through a gas inlet to adjust the internal pressure to 70 kPa. The highest pressure response measured after pressure release is considered the "peak" pressure achieved in the airbag. The start of the test (P Osec ) to target test duration 6 seconds (P 6sec The pressure difference observed from 0.01 to 0.25 mm was measured, and the resulting pressure retention was measured. The results are shown in Table 2b.

[0114] [Table 4]

[0115] From the examples herein, it may be seen that there are significantly better loss tangent (tan δ) values.

Claims

1. 45-62 g / m2 determined according to ISO 3801 2 1. An integrally woven airbag comprising a coating having an average dry coat weight of a) an organopolysiloxane polymer having a viscosity of 100 to 200,000 mPa.s (inclusive) at 25° C. and at least two unsaturated groups per molecule, the unsaturated groups being selected from alkenyl or alkynyl groups; b) reinforcing fillers including fumed silica, precipitated silica and / or calcium carbonate; c) organosilicon compounds having at least two, alternatively at least three, Si—H groups per molecule; d) a hydrosilylation curing catalyst; e) one or more substantially non-functional organosilicon compounds, (i) a silicone resin selected from T silicone resin (silsesquioxane), DT silicone resin, MQ silicone resin, MDT silicone resin, MTQ silicone resin, QDT silicone resin, or a mixture thereof; and / or (ii) trialkyl-terminated polydiorganosiloxanes; f) one or more monoacrylates, diacrylates or methacrylates, epoxy-containing alkoxysilanes, alkoxysilanes containing methacryl or acryl groups, and i) one or more alkoxysilanes having an epoxy group in the molecule; ii) a linear organopolysiloxane oligomer containing at least one alkenyl group and at least one hydroxy or alkoxy group per molecule; and iii) an adhesion promoter selected from mixtures and / or reaction products of an organometallic condensation reaction catalyst comprising an organoaluminum compound or an organozirconium compound, or mixtures thereof; 1. A one-piece woven airbag, wherein the coating has a loss tangent (tan δ) value of at least 0.175 at an angular frequency of 500 rad / sec, where tan δ=G″ / G′=Dynamic Loss Modulus / Dynamic Storage Modulus, as determined by the rheology test method disclosed herein.

2. 50-62 g / m2, determined according to ISO 3801 2 2. The one-piece woven airbag of claim 1, wherein said average dry coat weight is

3. 3. The one-piece woven airbag of claim 1 or 2, wherein the one-piece woven airbag also has an internal pressure retention characteristic of greater than 60% retained 6 seconds after deployment using the test method described in the Examples herein.

4. The integrally woven airbag of any one of claims 1 to 3, wherein component (e) is a non-functional silicone resin selected from silsesquioxane or MQ silicone resins.

5. The non-functional silicone resin of component (e)(i) has the formula: (R 4 3 SiO 1/2 ) u (SiO 4/2 ) v is an MQ silicone resin having In the formula, R 4 but does not contain aliphatic unsaturation 1 ~C 10 5. The integrally woven airbag of claim 1, wherein u is a hydrocarbon group, u is between 0.3 and 0.6, v is between 0.4 and 0.7, and the value of u+v is 1.

0.

6. The integrally woven airbag according to any one of claims 1 to 5, wherein the integrally woven airbag is a curtain airbag.

7. The integrally woven airbag of any one of claims 1 to 6, wherein the non-functional silicone resin of component (e)(i) is free of alkenyl and / or alkynyl groups and Si-H bonds.

8. 1. A method for preparing a coated integrally woven airbag, comprising: a) an organopolysiloxane polymer having a viscosity of 100 to 200,000 mPa.s (inclusive) at 25° C. and at least two unsaturated groups per molecule, the unsaturated groups being selected from alkenyl or alkynyl groups; b) reinforcing fillers, including fumed silica and / or precipitated silica; c) organosilicon compounds having at least two, alternatively at least three, Si—H groups per molecule; d) a hydrosilylation curing catalyst; e) one or more substantially non-functional organosilicon compounds, (i) a silicone resin selected from T silicone resin (silsesquioxane), DT silicone resin, MQ silicone resin, MDT silicone resin, MTQ silicone resin, QDT silicone resin, or a mixture thereof; and / or (ii) trialkyl-terminated polydiorganosiloxanes; f) one or more monoacrylates, diacrylates or methacrylates, epoxy-containing alkoxysilanes, alkoxysilanes containing methacryl or acryl groups, and i) one or more alkoxysilanes having an epoxy group in the molecule; ii) a linear organopolysiloxane oligomer containing at least one alkenyl group and at least one hydroxy or alkoxy group per molecule; iii) mixing the components of a hydrosilylation-curable silicone coating composition comprising an adhesion promoter selected from the mixture and / or reaction product of an organometallic condensation reaction catalyst comprising an organoaluminum compound or an organozirconium compound, or a mixture thereof; Upon curing, the one-piece woven airbag has a hardness of 45-62 g / m2 as determined in accordance with ISO 3801. 2 and coating the integrally woven airbag to have an average dry coat weight of said coating having a loss tangent (tan δ) value of at least 0.175 at an angular frequency of 500 rad / sec; tan δ=G″ / G′=Dynamic Loss Modulus / Dynamic Storage Modulus, as determined by the Rheological Test Method disclosed in the Examples herein.

9. 9. The method for preparing a coated, integrally woven airbag according to claim 8, wherein the non-functional silicone resin of component (e)(i) is selected from a silsesquioxane or an MQ silicone resin.

10. The non-functional silicone resin of component (e)(i) has the formula: (R 4 3 SiO 1/2 ) u (SiO 4/2 ) v is an MQ silicone resin having In the formula, R 4 but does not contain aliphatic unsaturation 1 ~C 10 10. The method for preparing a coated integrally woven airbag according to claim 8 or 9, wherein u is a hydrocarbon group, u is 0.3 to 0.6, v is 0.4 to 0.7, and the value of u+v is 1.

0.

11. 11. The method for preparing a coated, integrally woven airbag according to claim 8, 9 or 10, wherein the non-functional silicone resin of component (e)(i) is free of alkenyl and / or alkynyl groups and Si-H bonds.

12. 12. The method of preparing a coated integrally woven airbag according to claim 8, 9, 10, or 11, wherein the adhesion promoter (f) is present in the composition in a cumulative amount of (f)(i), (ii), and (iii) of typically about 0.3-6% by weight of the composition.

13. 13. A method of coating a textile with the hydrosilylation-curable silicone coating composition of any one of claims 8, 9, 10, 11, or 12, wherein the textile is coated by spraying, gravure coating, bar coating, knife-over-roller coating, knife-over-air coating, padding, dipping, and screen printing.

14. 1. Use of a hydrosilylation-curable silicone coating composition, comprising: a) an organopolysiloxane polymer having a viscosity of 100 to 200,000 mPa.s (inclusive) at 25° C. and at least two unsaturated groups per molecule, the unsaturated groups being selected from alkenyl or alkynyl groups; b) reinforcing fillers, including fumed silica and / or precipitated silica; c) organosilicon compounds having at least two, alternatively at least three, Si—H groups per molecule; d) a hydrosilylation curing catalyst; e) one or more substantially non-functional organosilicon compounds, (i) a silicone resin selected from T silicone resin (silsesquioxane), DT silicone resin, MQ silicone resin, MDT silicone resin, MTQ silicone resin, QDT silicone resin, or a mixture thereof; and / or (ii) trialkyl-terminated polydiorganosiloxanes; f) one or more monoacrylates, diacrylates or methacrylates, epoxy-containing alkoxysilanes, alkoxysilanes containing methacryl or acryl groups, and i) one or more alkoxysilanes having an epoxy group in the molecule; ii) a linear organopolysiloxane oligomer containing at least one alkenyl group and at least one hydroxy or alkoxy group per molecule; iii) an adhesion promoter selected from mixtures and / or reaction products of an organometallic condensation reaction catalyst comprising an organoaluminum compound or an organozirconium compound, or a mixture thereof; 45-62 g / m2 determined according to ISO 3801 2 2. producing a coated integrally woven airbag having an average dry coat weight of said coating having a loss tangent (tan δ) value of at least 0.175 at an angular frequency of 500 rad / sec; tan δ=G″ / G′=Dynamic Loss Modulus / Dynamic Storage Modulus, as determined by the Rheological Test Method disclosed herein.

15. 15. The use of the hydrosilylation-curable silicone coating composition of claim 14, wherein the integrally woven airbag also has an internal pressure retention property of greater than 60% retained 6 seconds after deployment according to the method described herein.

Citation Information

Patent Citations

  • Liquid silicone rubber coating composition for curtain air bag, curtain air bag, and manufacturing method therefor

    JP2009007468A

  • Liquid curable silicone rubber composition, and textiles coated with the cured product of the composition.

    JP2013531695A

  • Manufacturing method of silicone rubber coating base fabric for air bag, ultraviolet curable air bag coating agent and base fabric for air bag

    JP2018003194A

  • Silicone coating for airbags

    JP2022542153A

  • Silicone composition for coating textile material substrates

    US6511754B1