Phosphorus-containing silicone core acrylic shell impact modifier
Patent Information
- Application Number
- JP2024532305
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2021-12-09
- Filing Date
- 2022-12-07
- Publication Date
- 2024-12-05
Smart Images

Figure 2024545033000001_ABST
Abstract
Description
[Technical Field]
[0001] The present invention relates generally to phosphorus-containing multi-stage polymer compositions useful as impact modifiers. More specifically, the compositions relate to multi-stage polymer compositions having a silicone core and an acrylic shell in the multi-stage polymer. [Background technology]
[0002] In manufacturing products, it is generally desirable to achieve ease of manufacturing as well as light weight, i.e., a reduction in the weight of the product. Both of these objectives are achieved through the use of plastics relative to the use of metals or ceramics. On the other hand, it is generally desirable for the manufactured article to have low to no flammability, which is provided by the use of metals or ceramics and generally not provided by the use of plastics.
[0003] Recently, plastic formulations with improved (i.e., lower) levels of flammability have been developed. Typically, these formulations contain high levels of flame retardant additives in addition to drip-proofing additives. These formulations can achieve certain standards specified by UL (Underwriters Laboratories), allowing them to be used in the manufacture of electrical appliances and articles for use under the hood of automobiles.
[0004] These plastic formulations generally have a requirement for substantial impact strength. However, additives used to achieve lower flammability typically reduce the impact strength of the molded product. It is very common to add core-shell polymer impact modifiers to these formulations to achieve the required level of impact strength. However, the polymers used to make these core-shell impact modifiers can be highly flammable and can increase the flammability of the formulation in direct correlation with the amount utilized in the formulation. Therefore, there is a problem in the field of plastic formulations to achieve the appropriate balance between impact strength and flammability.
[0005] U.S. Patent No. 5,219,907 discloses the use of core-shell emulsion polymers containing phosphate monomers as part of the shell, which can be used in polycarbonate formulations. The core comprises an elastomer selected from polybutadiene or crosslinked polyacrylate rubber.
[0006] EP 0663410 discloses the use of high concentrations of phosphorus monomers located in a graft polymer on a rubbery substrate, the rubbery substrate being an alkyl acrylate rubber or an olefin rubber, to provide improved flammability.
[0007] There is a need to develop new processes and impact modifier polymer compositions containing silicone cores that have improved flammability. Summary of the Invention
[0008] One aspect of the present invention provides a multi-stage polymer composition comprising: (a) a core comprising a silicone polymer; and (b) a shell comprising an acrylic polymer, wherein at least one of the silicone polymer in the core and the acrylic polymer in the shell comprises polymerized units derived from an organophosphorus monomer.
[0009] In another aspect, the present invention provides a matrix resin composition comprising: (A) a multi-stage polymer composition comprising: (i) a core comprising a silicone polymer; and (ii) a shell comprising an acrylic polymer; and (B) one or more matrix resins, wherein at least one of the silicone polymer in the core and the acrylic polymer in the shell comprises polymerized units derived from an organophosphorus monomer. [Brief explanation of the drawings]
[0010] [Figure 1] 1 is a graph of burn times of resin compositions according to embodiments of the present invention. DETAILED DESCRIPTION OF THE INVENTION
[0011] The present inventors have surprisingly found that organophosphorus monomers can be incorporated into silicone core / acrylic shell multistage polymers to enhance the flame resistance of the multistage polymers.
[0012] As used herein, the term "polymer" refers to a polymeric compound prepared by polymerizing monomers, whether of the same or different types. The general term "polymer" includes the terms "homopolymer," "copolymer," "terpolymer," and "resin." As used herein, the term "polymerized units derived from" refers to a polymer molecule synthesized according to polymerization techniques in which the product polymer contains "polymerized units derived from" the constituent monomers that are the starting materials for the polymerization reaction. As used herein, the term "(meth)acrylate" refers to either acrylate or methacrylate, or a combination thereof, and the term "(meth)acrylic" refers to either acrylic or methacrylic, or a combination thereof. As used herein, the term "substituted" refers to having at least one attached chemical group, such as an alkyl group, an alkenyl group, a vinyl group, a hydroxyl group, a carboxylic acid group, other functional groups, and combinations thereof.
[0013] As used herein, the term "organophosphate" refers to an organic compound containing phosphorus. As used herein, the term "phosphate" refers to an anion composed of a phosphorus atom and an oxygen atom, where phosphorus is in the +5 oxidation state. Orthophosphate (PO4 -3 ), polyphosphate (P n O 3n+1 -(n+2) , where n is 2 or more), and metaphosphates (formula P m O 3m -mwhere m is 2 or greater). As used herein, "alkali phosphate" refers to a salt of an alkali metal cation and a phosphate anion. Alkali phosphates include alkali metal orthophosphates, alkali metal polyphosphates, and alkali metal metaphosphates. Alkali phosphates also include partially neutralized salts of phosphate acids, including, for example, partially neutralized salts of orthophosphate acids, such as, for example, monosodium dihydrogen phosphate and disodium hydrogen phosphate. As used herein, the term "phosphonate" refers to an anion composed of phosphorus and oxygen atoms, where phosphorus is in the +3 oxidation state.
[0014] As used herein, the term "multi-stage polymer" refers to a polymer made by forming (i.e., polymerizing) a first polymer, referred to as the "first stage" or "first stage polymer," which forms the core of the multi-stage polymer. A second polymer, referred to as the "second stage" or "second stage polymer," is then formed in the presence of the first stage, which may be an intermediate or final stage of the multi-stage polymer. A multi-stage polymer may also contain additional stages, which may be formed before or after the second stage polymer. Each intermediate stage is formed in the presence of the polymer resulting from the polymerization of the stage immediately preceding it. In such embodiments, where each subsequent stage forms a partial or complete shell around each particle remaining from the previous stage, the resulting multi-stage polymer is known as a "core / shell" polymer, where the first stage polymer comprises the core and each subsequent stage comprises a shell on the preceding stage, with the final stage forming the outermost shell. Thus, the second stage polymer constitutes at least a portion of the shell in the multi-stage polymer.
[0015] As used herein, "weight average molecular weight" or "M wThe term "weight of polymer" refers to the weight average molecular weight of the polymer as measured by gel permeation chromatography (GPC) for acrylic acid polymers against polystyrene calibration standards according to ASTM D5296-11(2011) and using tetrahydrofuran (THF) as the mobile phase and diluent. As used herein, the term "weight of polymer" means the dry weight of the polymer.
[0016] As used herein, "glass transition temperature" or "T g The term "glass transition temperature" refers to the temperature at or above which a glassy polymer undergoes segmental motion of the polymer chains. The glass transition temperature of a copolymer can be estimated by the Fox equation (Bulletin of the American Physical Society, 1(3) p. 123 (1956)) as follows: 1 / T g =w1 / T g(1) +w2 / T g(2)
[0017] For copolymers, w1 and w2 refer to the weight fractions of the two comonomers, and T g(1) and T g(2) refers to the glass transition temperature of two corresponding homopolymers made from a monomer. For polymers containing three or more monomers, additional terms are added (w n / T g(n) The glass transition temperatures of homopolymers can be found, for example, in "Polymer Handbook" edited by J. Brandrup and E.H. Immergut (Interscience Publishers). g can also be measured by a variety of techniques, including, for example, differential scanning calorimetry (DSC). As used herein, "calculated T" refers to a temperature at which the gThe phrase "glass transition temperature" is intended to mean the glass transition temperature as calculated by the Fox equation. g When two or more T g can be observed. T observed in one stage of a multi-stage polymer g is a characteristic of the polymer that forms the step, T g (i.e., the T observed when the polymer forming that stage is formed and measured separately from other stages. g ) can be identical to the monomer T g When a homopolymer made from that monomer is said to have that T g It means having.
[0018] A compound is considered "water-soluble" herein if the amount of the compound that can be dissolved in water at 20° C. is 5 g or more per 100 mL of water. A compound is considered "water-insoluble" herein if the amount of the compound that can be dissolved in water at 20° C. is 0.5 g or less per 100 mL of water. A compound is considered "partially water-soluble" herein if the amount of the compound that can be dissolved in water at 20° C. is 0.5 g to 5 g per 100 mL of water.
[0019] As used herein, when it is said that a "polymeric composition contains little or no particular substance," it means that the polymeric composition does not contain any of that substance, or, if any of that substance is present in the composition, the amount of that substance is 1 wt. % or less, based on the weight of the polymeric composition. Among embodiments described herein as having "little or no" particular substances, embodiments are contemplated in which none of the particular substances are present.
[0020] The multistage polymers of the present invention comprise a core and a shell. The core comprises a silicone polymer and the shell comprises an acrylic polymer. One or both of the silicone polymer and the acrylic polymer contain polymerized units derived from organophosphorus monomers.
[0021] Silicone (i.e., polysiloxane) polymers can be synthesized using either linear organosiloxanes or cyclic organosiloxanes. Cyclic organosiloxanes are particularly preferred. Of these, 3- to 7-membered cyclic organosiloxanes are preferred. Specific examples include, but are not limited to, hexamethylcyclotrisiloxane, octamethylcyclotetrasiloxane, decamethylcyclopentasiloxane, dodecamethylcyclohexasiloxane, trimethyltriphenylcyclotrisiloxane, tetramethyltetraphenylcyclotetrasiloxane, and octaphenylcyclotetrasiloxane. These may be used alone or in combination of two or more. Of these, it is preferred to use octamethylcyclotetrasiloxane as the monomer.
[0022] The silicone polymer preferably contains a siloxane crosslinker for better elasticity and impact strength. The siloxane crosslinker is preferably selected from those having a siloxy group. By using the siloxane crosslinker, a polyorganosiloxane having a crosslinked structure can be obtained. Specific examples of the siloxane crosslinker include trifunctional or tetrafunctional silane crosslinkers such as trimethoxymethylsilane, triethoxyphenylsilane, tetramethoxysilane, tetraethoxysilane, tetra-n-propoxysilane, and tetrabutoxysilane. Among them, tetrafunctional crosslinkers are preferred, and tetraethoxysilane is more preferred.
[0023] The silicone polymer may also contain one or more polymerized units of graft linkers. The graft linker is a monomer that can be bonded to both the (meth)acrylic polymer and the silicone polymer through the reaction with (meth)acrylate and siloxane. Preferred graft linkers include siloxane compounds that have a polymerizable vinyl functional group and can be bonded to dimethylsiloxane through a siloxane bond.
[0024] Examples of siloxanes having a polymerizable vinyl functional group include (meth)acryloyloxyethyldimethoxymethylsilane, γ-(meth)acryloyloxypropyldimethoxymethylsilane, γ-(meth)acryloyloxypropylmethoxydimethylsilane, γ-(meth)acryloyloxypropyltrimethoxysilane, γ-(meth)acryloyloxypropylethoxydiethylsilane, γ-(meth)acryloyloxypropyldiethoxymethylsilane, and δ-(meth)acryloyloxybutyldiethoxymethylsilane. vinyl siloxanes such as p-vinylphenyldimethoxymethylsilane; mercaptosiloxanes such as γ-mercaptopropyldimethoxymethylsilane and γ-mercaptopropyltrimethoxysilane; and disiloxanes such as 1,3-bis(3-methacryloyloxypropyl)tetramethyldisiloxane and 1,3-bis(3-mercaptopropyl)tetramethyldisiloxane, but are not limited to these.
[0025] In the multi-stage polymer, one or both of the silicone polymer in the core and the acrylic polymer in the shell comprise polymerized units derived from an organophosphorus monomer. Thus, the multi-stage polymer may comprise a phosphorus-containing silicone polymer in the core and an acrylic polymer in the shell, a silicone polymer in the core and a phosphorus-containing acrylic polymer in the shell, or a phosphorus-containing silicone polymer in the shell and a phosphorus-containing acrylic polymer in the shell.
[0026] When the silicone polymer comprises polymerized units derived from an organophosphorus monomer, the organophosphorus monomer may be selected from phospho-silane monomers. Phospho-silane monomers have the formula Si(OR 2 )3-R 3 -P(O)(OR 4 R 2 and R 4 are independently hydrogen and C1 to C 12 R may be selected from alkyl groups.3 is C1~C 12 Preferably, R 2 , R 3 , and R 4 are independently selected from C1 to C6 alkyl groups.
[0027] When the silicone polymer in the core contains polymerized units derived from a phosphosilane monomer, the phosphosilane monomer may be present in an amount ranging from 0.1 to 20 wt. % based on the total weight of the silicone polymer. For example, the phosphosilane monomer may be present in an amount of at least 0.25 wt. %, at least 0.5 wt. %, or at least 1 wt. % based on the total weight of the silicone polymer. The phosphosilane monomer may be present in an amount of, for example, 15 wt. % or less, 10 wt. % or less, or 5 wt. % or less based on the total weight of the silicone polymer.
[0028] The multi-stage polymer may contain silicone polymer in an amount of, for example, 2% by weight or more, 5% by weight or more, 10% by weight or more, 20% by weight or more, or 50% by weight or more, based on the total weight of the multi-stage polymer. The multi-stage polymer may contain silicone polymer in an amount of 98% by weight or less, or 95% by weight or less, or 90% by weight or less, based on the total weight of the multi-stage polymer.
[0029] The multi-stage polymers of the present invention contain an acrylic polymer in the shell. The acrylic polymer may include polymerized units derived from one or more monomers selected from substituted and unsubstituted alkyl (meth)acrylate monomers.
[0030] Suitable alkyl groups in the at least one alkyl (meth)acrylate monomer include linear or branched C1-C 12 The alkyl group includes methyl, ethyl, propyl, butyl, hexyl, 2-ethylhexyl, and octyl groups. Preferably, the alkyl (meth)acrylate monomer comprises methyl methacrylate.
[0031] The acrylic polymer may further include polymerized units derived from other monomers, such as, for example, styrene monomers.
[0032] When the acrylic polymer in the shell comprises polymerized units derived from an organophosphorus monomer, examples of the organophosphorus monomer include:
[0033] [ka] wherein R is an organic group containing an acryloxy, methacryloxy, or vinyl group, and R' and R" are independently selected from H and a second organic group. The second organic group can be saturated or unsaturated. Suitable organophosphorus monomers include dihydrogen phosphate functional monomers, such as dihydrogen phosphate esters of alcohols that also contain polymerizable vinyl or olefinic groups, such as allyl phosphate, monophosphate or diphosphate of bis(hydroxy-methyl) fumarate or itaconate, derivatives of (meth)acrylic acid esters, such as phosphates of hydroxyalkyl (meth)acrylates, including 2-hydroxyethyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, and the like.
[0034] Other suitable organophosphorus monomers are those having the formula: 5 is H or -CH 3 , R 6 = alkyl, and n = 1-5, such as the methacrylates SIPOMER™ PAM-100, SIPOMER™ PAM-200, SIPOMER™ PAM-400, SIPOMER™ PAM-600 and the acrylate SIPOMER™ PAM-300, available from Solvay. 5 )-C(O)-O-(R 6 O) n -P(O)(OH)2.
[0035] Other suitable organophosphorus monomers are the phosphonate-functional monomers disclosed in WO 99 / 25780 A1, including vinylphosphonic acid, allylphosphonic acid, 2-acrylamido-2-methylpropanephosphonic acid, α-phosphonostyrene, 2-methylacrylamido-2-methylpropanephosphonic acid. Further suitable organophosphorus monomers are the 1,2-ethylenically unsaturated (hydroxy)phosphinylalkyl(meth)acrylate monomers disclosed in U.S. Pat. No. 4,733,005, including (hydroxy)phosphinylmethyl methacrylate.
[0036] Preferably, the organophosphorus monomer has the formula CH═C(R 5 )-C(O)-O-(R 6 O) n More preferably, R 5 is -CH3 and R 6 is an alkyl group containing 1 to 6 carbon atoms and n=1.
[0037] The acrylic polymer in the shell may contain polymerized units derived from at least one organophosphorus monomer in an amount of 0.25 wt.% or more, or 0.5 wt.% or more, based on the total weight of the acrylic polymer. The second stage polymer may contain polymerized units derived from at least one organophosphorus monomer in an amount of 20 wt.% or less, 15 wt.% or less, or 10 wt.% or less, based on the total weight of the acrylic polymer. Preferably, the acrylic polymer contains polymerized units derived from at least one organophosphorus monomer in an amount ranging from 0.5 to less than 20 wt.%, based on the total weight of the acrylic polymer. More preferably, the acrylic polymer contains polymerized units derived from at least one organophosphorus monomer in an amount ranging from 2 to less than 10 wt.%, based on the total weight of the acrylic polymer.
[0038] The acrylic polymer may further include additional components, for example, the acrylic polymer may include one or more of a crosslinking agent, a chain transfer agent, or a functional monomer.
[0039] Acrylic polymers are used at temperatures above 50°C or above 90°C. g The final stage polymer may have a T g may have:
[0040] The multi-stage polymer may contain, for example, 2% by weight or more, or 10% by weight or more, or 20% by weight or more of the acrylic polymer, based on the total weight of the multi-stage polymer. The multi-stage polymer may contain, for example, 98% by weight or less, 80% by weight or less, 70% by weight or less, or 60% by weight or less of the acrylic polymer, based on the total weight of the multi-stage polymer.
[0041] Preferably, the acrylic polymer has a T of 50° C. or greater in an amount of 50 wt. % or greater, or 75 wt. % or greater, or 90 wt. % or greater, based on the total weight of the acrylic polymer. g The polymerized units are derived from a monomer having the formula:
[0042] The multi-stage polymer may contain one or more interstage polymers in the shell in addition to the acrylic polymer. The total interstage polymers may be present in an amount of 1% by weight or more, or 2% by weight or more, or 5% by weight or more, or 10% by weight or more, based on the total weight of the multi-stage polymer. The total interstage polymers may be present in an amount of 60% by weight or less, or 2% by weight or less, or 5% by weight or less, or 10% by weight or less, based on the total weight of the multi-stage polymer. As with the acrylic polymer in the shell of the multi-stage polymer, the one or more interstage polymers may also contain polymerized units derived from one or more organophosphorus monomers.
[0043] Multistage polymers can be prepared by any conventional method. For example, silicone polymers can be prepared by acid-catalyzed aqueous emulsion polymerization. Acrylic polymers can be prepared by radical aqueous emulsion polymerization. In aqueous emulsion polymerization, water forms the continuous medium in which polymerization occurs. The water may or may not be mixed with one or more additional compounds that are miscible with or dissolved in water. The continuous medium may contain 30% or more water by weight, 50% or more water by weight, 75% or more water by weight, or 90% or more water by weight, based on the weight of the continuous medium. Emulsion polymerization of siloxane monomers is catalyzed by acid. Examples of acid catalysts used in the polymerization of siloxane mixtures include, but are not limited to, sulfonic acids such as aliphatic sulfonic acid, aliphatic-substituted benzenesulfonic acid, and aliphatic-substituted naphthalenesulfonic acid, as well as mineral acids such as sulfuric acid, hydrochloric acid, and nitric acid. These compounds may be used alone or in combination of two or more of them.
[0044] The emulsion polymerization of (meth)acrylic polymers involves the presence of one or more initiators. An initiator is a compound that forms one or more free radicals that can start the polymerization process. The initiator is usually water-soluble. Some suitable initiators form one or more free radicals when heated. Some suitable initiators are oxidizing agents that form one or more free radicals when mixed with one or more reducing agents, or when heated, or a combination thereof. Some suitable initiators form one or more free radicals when exposed to radiation, such as ultraviolet light or an electron beam. Combinations of suitable initiators are also suitable.
[0045] Preferably, the multi-stage polymer is prepared in the form of a latex. As used herein, the term "latex" refers to the physical form of a polymer in which the polymer exists in the form of small polymer particles dispersed in water. The latex may have, for example, an average particle size of 50 nm or more, or 100 nm or more. The latex may have an average particle size of 1,000 nm or less, or 800 nm or less, or 600 nm or less.
[0046] The emulsion polymerization may include the use of at least one organophosphorus soap containing an anionic phosphate surfactant. Each anionic phosphate surfactant has a cation associated therewith, forming an alkali metal salt of the phosphate surfactant, including, for example, alkyl phosphate salts and alkylaryl phosphate salts. Suitable cations include, for example, ammonium, alkali metal cations, and mixtures thereof. Suitable alkali metal salts of phosphate surfactants include, for example, polyoxyalkylene alkylphenyl ether phosphate salts, polyoxyalkylene alkyl ether phosphate salts, polyoxyethylene alkylphenyl ether phosphate salts, and polyoxyethylene alkyl ether phosphate salts. The alkali metal salt of the phosphate surfactant may include polyoxyethylene alkyl ether phosphate salts. The weight of the phosphate surfactant present during the emulsion polymerization of the multistage polymer, characterized by the weight of the phosphate surfactant based on the weight of the total monomers added to the polymerization, may range from 0.5% by weight or more, preferably 1.0% by weight or more, and more preferably 1.5% by weight or more. The weight of the phosphate surfactant present during the emulsion polymerization of the multi-stage polymer, characterized by the weight of the phosphate surfactant based on the total monomer weight added to the polymerization, can be in the range of 5% by weight or less, preferably 4% by weight or less, and more preferably 3% by weight or less. In addition to the anionic phosphate surfactant described above, one or more anionic surfactants can be utilized in the emulsion polymerization. Suitable additional anionic surfactants include, for example, carboxylates, sulfosuccinates, sulfonates, and sulfates.
[0047] In the process of the present invention, the multi-stage polymer latex can be isolated by coagulation or spray drying to retain the organophosphorus soap on the surface of the multi-stage polymer. Suitable coagulation methods include, for example, coagulation with divalent cations.
[0048] Suitable divalent cations include, for example, divalent metal cations and alkaline earth cations. Suitable divalent cations include, for example, calcium(+2), cobalt(+2), copper(+2), iron(+2), magnesium(+2), zinc(+2), and mixtures thereof. Preferably, the multivalent cation is selected from calcium(+2) and magnesium(+2). More preferably, any divalent cations present are calcium(+2), magnesium(+2), or mixtures thereof. Even more preferably, the divalent cation comprises calcium(+2). The divalent cation may be present in an amount of 10 ppm or more, or 30 ppm or more, or 100 ppm or more, based on the dry weight of the multistage polymer. The divalent cation may be present in an amount of 3 wt. % or less, or 1 wt. % or less, or 0.3 wt. % or less, based on the dry weight of the multistage polymer.
[0049] Preferably, most or all of the divalent cations present in the composition are in the form of water-insoluble phosphate salts. The molar amount of polyvalent cations present in the form of water-insoluble phosphate salts can be 80% or more, or 90% or more, or 95% or more, or 98% or more, or 100%, based on the total moles of divalent cations present in the composition.
[0050] Preferably, most or all of the water remaining with the isolated polymer is removed from the isolated polymer by one or more of the following procedures: filtration (including, for example, vacuum filtration) and / or centrifugation. The isolated polymer may optionally be washed with water one or more times. It is known that coagulated polymers have complex structures, and water cannot easily access every part of the coagulated polymer. While not wishing to be bound by theory, it is contemplated that significant amounts of divalent cations and residual organophosphate soaps are left behind. Therefore, the compositions of the present invention may contain organophosphate soaps in an amount of 50 ppm or more, or 100 ppm or more, or 500 ppm or more, based on the dry weight of the multistage polymer. The compositions of the present invention may contain organophosphate soaps in an amount of 10,000 ppm or less, or 7,500 ppm or less, or 5,000 ppm or less, based on the dry weight of the multistage polymer.
[0051] Preferably, the dried multi-stage polymer has a moisture content of less than 1.0% by weight, based on the weight of the dried multi-stage polymer.
[0052] The polymer composition of the present invention may also contain a flow aid. The flow aid is a hard material in the form of a powder (average particle size of 1 micrometer to 1 mm). Suitable flow aids are, for example, hard polymers (i.e., polymers with a T of 80° C. or higher). g Polymers having the formula (I) or minerals (e.g., silica).
[0053] The polymer composition of the present invention may also contain a stabilizer. Suitable stabilizers include, for example, radical scavengers, peroxide decomposers, and metal deactivators. Suitable radical scavengers include, for example, hindered phenols (e.g., those having a tertiary butyl group attached to each carbon atom of the aromatic ring adjacent to the carbon atom to which a hydroxyl group is attached), secondary aromatic amines, hindered amines, hydroxylamines, and benzofuranones. Suitable peroxide decomposers include, for example, organic sulfides (e.g., divalent sulfur compounds, such as esters of thiopropionic acid), esters of phosphorous acid (HPO), and hydroxylamines. Suitable metal deactivators include, for example, chelating agents (e.g., ethylenediaminetetraacetic acid).
[0054] In the process of the present invention, the multi-stage polymer latex may be isolated by coagulation or spray drying. Suitable coagulation methods include, for example, coagulation with divalent cations.
[0055] Preferably, most or all of the water remaining with the isolated polymer is removed from the isolated polymer by one or more of the following operations: filtration (including, for example, vacuum filtration) and / or centrifugation. The isolated polymer may optionally be washed one or more times with water.
[0056] Preferably, the dried multi-stage polymer has a moisture content of less than 1.0% by weight, based on the weight of the dried multi-stage polymer.
[0057] The polymer composition of the present invention may also contain a flow aid. The flow aid is a hard material in the form of a powder (average particle size of 1 micrometer to 1 mm). Suitable flow aids are, for example, hard polymers (i.e., polymers with a T of 80° C. or higher). g Polymers having the formula (I) or minerals (e.g., silica).
[0058] The polymer composition of the present invention may also contain a stabilizer. Suitable stabilizers include, for example, radical scavengers, peroxide decomposers, and metal deactivators. Suitable radical scavengers include, for example, hindered phenols (e.g., those having a tertiary butyl group attached to each carbon atom of the aromatic ring adjacent to the carbon atom to which a hydroxyl group is attached), secondary aromatic amines, hindered amines, hydroxylamines, and benzofuranones. Suitable peroxide decomposers include, for example, organic sulfides (e.g., divalent sulfur compounds, such as esters of thiopropionic acid), esters of phosphorous acid (HPO), and hydroxylamines. Suitable metal deactivators include, for example, chelating agents (e.g., ethylenediaminetetraacetic acid).
[0059] As noted above, one aspect of the present invention utilizes the polymer composition described herein as an impact modifier in a matrix resin composition containing a multi-stage polymer composition and a matrix resin. After the mixture of multi-stage polymer and matrix resin is mixed, melted, and molded into a solid product, the impact resistance of the product will be better than the same solid product made using a matrix resin that is not mixed with the multi-stage polymer. The multi-stage polymer can be provided in a solid form, such as pellets or powder, or a mixture thereof. The matrix resin can also be provided in a solid form, such as pellets or powder, or a mixture thereof. The solid multi-stage polymer can be mixed with the solid matrix resin at room temperature (20°C) or at an elevated temperature (e.g., 30°C to 90°C). Alternatively, the solid multi-stage polymer can be mixed with the molten matrix resin in, for example, an extruder or other melt mixer. The solid multi-stage polymer can also be mixed with the solid matrix resin, the solid mixture then heated sufficiently to melt the matrix resin, and the mixture can be further mixed, for example, in an extruder or other melt processing device.
[0060] The weight ratio of matrix resin to the multi-stage polymer of the present invention can be in the range of, for example, 1:1 or more, or 1.1:1 or more, or 2.3:1 or more, or 4:1 or more, or 9:1 or more, or 19:1 or more, or 49:1 or more, or 99:1 or more.
[0061] Suitable matrix resins include, for example, polyolefins, polystyrene, styrene copolymers, poly(vinyl chloride), poly(vinyl acetate), acrylic polymers, polyethers, polyesters, polycarbonates, polyurethanes, and polyamides. Preferably, the matrix resin contains at least one polycarbonate. Suitable polycarbonates also include, for example, homopolymers of polymerized units derived from bisphenol A ("Bisphenol A, BPA"), and copolymers containing polymerized units of BPA together with one or more other polymerized units.
[0062] The matrix resin may include at least one polyester. Suitable polyesters include, for example, polyethylene terephthalate and polybutylene terephthalate.
[0063] The matrix resin may comprise a blend of polymers. Suitable blends of polymers include, for example, blends of polycarbonate and styrene resins, and blends of polycarbonate and polyester. Suitable styrene resins include, for example, polystyrene and copolymers of styrene with other monomers, such as acrylonitrile / butadiene / styrene (ABS) resins.
[0064] The matrix resin composition containing the multi-stage polymer and the matrix resin may contain one or more additional materials added to the mixture. Any one or more of such additional materials can be added to the multi-stage polymer or the matrix resin before forming the final mixture of all materials. When the matrix resin is in solid or molten form, each of the additional materials (if used) can be added to the matrix resin (singly or in combination with each other and / or in combination with the multi-stage polymer). Suitable additional materials include, for example, dyes, colorants, pigments, carbon black, fillers, fibers, lubricants (e.g., montan wax), flame retardants (e.g., borates, antimony trioxide, or molybdates), and other impact modifiers that are not the multi-stage polymers of the present invention.
[0065] The matrix resin composition can be used to form useful articles by, for example, film blowing, profile extrusion, molding, other methods, or combinations thereof. Molding methods include, for example, blow molding, injection molding, compression molding, other molding methods, and combinations thereof.
[0066] The multi-stage polymers of the present invention can provide significant improvements in the flammability of matrix resin compositions.
[0067] Some embodiments of the present invention are described in detail in the following examples. [Example]
[0068] Particle size measurement The particle size of the oligomers was measured with a Malvern Zetasizer Nano S90 particle size analyzer.
[0069] Representative core-shell polymer synthesis Representative silicone core emulsion synthesis (S1) A 5-liter, four-necked round-bottom flask equipped with a mechanical stirrer, thermometer, condenser, and electric heating mantle was charged with 2000 g of deionized water and 10 g of dodecylbenzenesulfonic acid. The reactor contents were heated to 85°C. In a separate vessel, 650 g of deionized water, 975 g of octamethylcyclotetrasiloxane, 20 g of tetraethoxysilane, 5 g of methacryloxypropyldimethoxymethylsilane, and 4.4 g of sodium dodecylbenzenesulfonate were mixed. The monomer mixture was then added to the kettle over 60 minutes. When the monomer feed was completed, the reaction mixture was stirred at 85°C for an additional 3 hours. After the hold, the batch was cooled to 40°C and held at that temperature for 4 hours before being cooled to room temperature. The batch was stirred at room temperature for an additional 18 hours and then neutralized with 45 g of 5% aqueous sodium hydroxide. The emulsion was characterized as having a particle size of 170 nm and a solids content of 23.5%.
[0070] Silicone Core Acrylic Shell Emulsion Polymer Synthesis (Sample 2) To 2785 parts of the 23.5% solids silicone emulsion (S1) prepared above, 285 parts of deionized water were added, and the mixture was heated to 60°C. At 60°C, 4.1 parts of Rhodafac® RS-610, 3.2 parts of sodium formaldehyde sulfoxylate (5% aqueous solution), and 2.3 parts of tert-butyl hydroperoxide (5% aqueous solution) were added. Subsequently, a monomer mixture of 106 parts of methyl methacrylate, 44 parts of styrene, and 14.32 parts of PAM600 was added over 1 hour. Simultaneously with the start of the monomer mixture feed, 16 parts of sodium formaldehyde sulfoxylate (5% aqueous solution) and 11 parts of tert-butyl hydroperoxide (5% aqueous solution) were fed over 240 minutes while maintaining the reaction temperature at 60°C. After all feeds were completed, 22.4 parts of Rhodafac® RS-610 was added. The reaction mixture was then cooled to room temperature and determined to have a solids content of 24.3%.
[0071] Representative procedure for clotting (Sample 2) Emulsion preparation The Sample 2 emulsion was neutralized with sodium phosphate solution to a pH of 6.9. 5297 g of the neutralized Sample 2 emulsion was stirred and held at 57°C.
[0072] coagulation To a 5-gallon coagulation vessel, 16.6 g of solid calcium chloride and 7203.4 g of deionized water were added. The contents of the vessel were heated to 57°C while stirring at 500 rpm. Once the contents reached 57°C, the preheated emulsion described above was slowly added to the vessel. Coagulation was completed by adding 49.7 g of calcium chloride dissolved in 200 g of deionized water. The mixture was then heated to 90°C and held at 90°C for 30 minutes. After holding, the mixture was cooled, dewatered, and washed in a Buchner funnel. The sample was washed with deionized water until the conductivity of the filtrate was less than 30 μS / m and then dewatered again. After dewatering and washing, the sample was dried in a vacuum oven at 65°C for 24 hours. The particle size of the coagulated slurry was measured using a Malvern Mastersizer 2000.
[0073] compound Polycarbonate formulations according to Table 1 were compounded in an extruder to make pellets for injection molding.
[0074] [Table 1]
[0075] PC Lexan 141: Polycarbonate manufactured by SABIC MBS: FR MBS powder of Example 1 or M732 powder of the comparative example FR-2025a: 100% potassium perfluorobutanesulfonate manufactured by 3M INP449: A blend of 50% polytetrafluoroethylene and 50% SAN manufactured by SABIC IRGANOX® 1076 and IRGANOX® 168: antioxidants manufactured by BASF
[0076] The polycarbonate formulations were injection molded to form double-end gated 1.0 mm ASTM burn bars for flammability testing using the UL 94 flammability test method.
[0077] [Table 2]
[0078] [Table 3]
[0079] [Table 4]
[0080] Samples 1-10 were also tested for flame retardancy using the UL-94 flammability test. Each sample demonstrated excellent flame retardancy (V-0). As shown in Figure 1, the inventive samples also demonstrated superior burn times compared to the non-phosphorus-containing samples. The comparative examples contained a commercially available silicone polymer in the core (C1 had a core / shell weight ratio of 70 / 30, and C2 had a core / shell weight ratio of 80 / 20). There was no phosphorus in the core / shell polymer.
Claims
1. 1. A multi-stage polymer composition comprising: (a) a core comprising a silicone polymer; (b) a shell comprising an acrylic polymer; A multi-stage polymer composition wherein at least one of said silicone polymer in said core and said acrylic polymer in said shell comprises polymerized units derived from an organophosphorus monomer.
2. 10. The polymer composition of claim 1, wherein the organophosphorus monomer comprises a phosphate or phosphonate functional group.
3. The polymer composition of claim 1 or 2, wherein the silicone polymer in the core comprises polymerized units derived from phospho-silane monomers.
4. The polymer composition of claim 3, wherein the phospho-silane monomer is present in the silicone polymer in an amount ranging from 0.1 to 10 weight percent, based on the total weight of the silicone polymer.
5. The phospho-silane monomer has the formula Si(OR 2 ) 3 -R 3 -P(O)(OR 4 ) 2 wherein R 2 and R 4 are independently hydrogen or C 1 ~C 12 alkyl group; R 3 is C 1 ~C 12 5. The polymer composition according to claim 3 or 4, wherein the alkyl group is selected from the group consisting of aryl, ... and alkyl groups.
6. R 2 , R 3 , and R 4 is independently 1 ~C 6 The polymer composition of claim 5 , wherein the alkyl group is selected from the alkyl groups.
7. The polymer composition of any one of claims 1 to 6, wherein the acrylic polymer in the shell comprises units derived from an organophosphorus monomer.
8. 8. The polymer composition of claim 7, wherein the organophosphorus monomer is present in the acrylic polymer in an amount ranging from 0.5 to 20 weight percent, based on the total weight of the acrylic polymer.
9. 9. The polymer composition of claim 8, wherein the organophosphorus monomer is present in the acrylic polymer in an amount ranging from 2 to 10 weight percent, based on the total weight of the acrylic polymer.
10. The organophosphorus monomer in the acrylic polymer in the shell has the formula CH 2 = C(R 5 )-C(O)-O-(R 6 O) n -P(O)(OH) 2 wherein R 5 is H or -CH 3 and R 6 10. The polymer composition according to any one of claims 7 to 9, wherein n is alkyl and n=1 to 5.
11. R 5 But -CH 3 and R 6 But, C 1 ~C 6 The polymer composition of claim 9, wherein the alkyl group is an alkyl group.
12. 12. The polymer composition of any one of claims 1 to 11, wherein the silicone polymer is present in an amount of from 2 to 98 weight percent, based on the total weight of the multi-stage polymer, and the acrylic polymer is present in an amount of from 2 to 98 weight percent, based on the total weight of the multi-stage polymer.
13. A matrix resin composition comprising mixing one or more matrix resins with the multi-stage polymer composition of any one of claims 1-12.
Citation Information
Patent Citations
Aqueous polymer dispersions and processes for making same
JP2021524522A
Aqueous dispersion of polymeric composite microspheres
WO2020092138A1