Selective Etching Solution for 3D NAND Structure Sheets
Patent Information
- Application Number
- JP2024536427
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2022-10-10
- Filing Date
- 2023-03-23
- Publication Date
- 2024-12-05
- Estimated Expiration
- 2043-03-23
Smart Images

Figure 2024545274000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention is in the field of electronic chemicals, and specifically relates to selective etchants for silica and silicon nitride. [Background technology]
[0002] 3D NAND is a key process technology for flash memory chips, which uses vertical stacking technology to build more storage units in a smaller space so that more storage data units can be obtained, which is three times that of similar NAND technology and is also the mainstream trend of current development.
[0003] However, in the process of etching the 192-layer 3D NAND structure with an etching solution, because it is a structure of alternating layers of silica and silicon nitride, while etching silicon nitride, it also causes a certain degree of etching of silica. Therefore, the etching solution is required to have high selectivity to silica, so that while etching silicon nitride, it also slightly etches silicon oxide. In the etching process, as the content of silicic acid in the solution increases, when a certain silicon content is reached, silicon redeposition is formed on the silica layer, and at the same time, it increases the grain size on the surface of the wafer, which causes the electrical performance of the final product to be unqualified and reduces the chip yield.
[0004] In order to solve the above problem, it is necessary to add a composite additive into phosphoric acid, which can inhibit and stabilize the etching of silica with increasing silicon content, reduce the re-deposition of silica on the surface, and at the same time maintain the etching rate of silicon nitride. Summary of the Invention
[0005] The technical problem that the present invention aims to solve is to provide a selective etching solution for silica and silicon nitride, which can inhibit and stabilize the etching of silica with increasing silicon content, reduce the surface redeposition of silica, and at the same time maintain the etching rate of silicon nitride, and is applicable to NAND structures.
[0006] In one aspect, the present invention relates to a selective etching solution for silica and silicon nitride, the composition of the etching solution being 1.5 to 2.0 mass % of silane additive 1, 2.0 to 2.5 mass % of silane additive 2, 83 to 86 mass % of phosphoric acid, and the remainder being water.
[0007] In the selective etching solution according to the present invention, the silane coupling agent 1 is any one of 3-glycidyloxypropyltrimethoxysilane, diethoxy(3-glycidyloxypropyl)methylsilane, and triethoxy(3-epoxypropyloxypropyl)silane.
[0008] The main function of silane coupling agent 1 is to adjust the selectivity of silicon nitride and silica, and its mechanism of action is the hydrolysis of silane coupling agent in phosphoric acid, so that the chemical bond of silicon-oxy-silicon structure can be attached to the surface of silica; at the same time, the larger the terminal group, the greater the steric hindrance effect, so that it can prevent the etching of silica surface by phosphoric acid and water, and thus the synergistic effect of the two effects inhibits the etching of silica.
[0009] In the selective etching solution according to the present invention, the silane coupling agent 2 is any one of 2-cyanoethyltriethoxysilane, 3-isocyanatopropyltriethoxysilane, and 3-ureidopropyltriethoxysilane.
[0010] The main function of silane coupling agent 2 is to prevent silicic acid from re-adhering to the surface of silica. Through hydrolysis of carbon-nitrogen bonds, chemical bonds such as hydroxyl groups and carboxyl groups, which are highly water-soluble, are formed, so that silane coupling agent 2 can bond with silicic acid and prevent it from re-adhering to the surface of silica. Silane coupling agent 1 can effectively adhere to the surface of silica, so that after bonding with silicic acid, it is easy to adhere to the surface of silica. In addition, silane coupling agent 2 can interact with silane coupling agent 1 to reduce its ability to adhere to the surface of silica. When the silicon content in the solution is high, the etching of silica can also reach the effect of positive etching.
[0011] In the etching solution of the present invention, the content of phosphoric acid and water has a great impact on the initial etching rate of silica and silicon nitride, that is, the higher the content of phosphoric acid, the lower the water content, and the faster the etching rate of silica.However, if the concentration of phosphoric acid is too high, it is easy to cause dehydration and carbonization of silane coupling agent, so it is ineffective, and the etching rate of silica increases quickly, and if the concentration of phosphoric acid is too low, it cannot meet the need for stable content of high-temperature etching water.
[0012] The mass ratio of phosphoric acid to water in the etching solution according to the present invention is 6 to 8, and preferably 7 to 7.5.
[0013] The 3D NAND structure sheet has a laminated structure of a silica film and a silicon nitride film, the silicon nitride film layer has a thickness of 500 to 1000 Å, the silica film layer has a thickness of 50 to 500 Å, and the number of layers in the laminated structure is 150 to 250.
[0014] In another aspect, the present invention provides a method for preparing a selective etching solution for 3D NAND structure sheets, by uniformly mixing silane coupling agents A and B at room temperature, and adding them together into phosphoric acid solution to obtain an etching solution.
[0015] The phosphoric acid solution is preheated to a temperature of 80 to 100°C, and silane coupling agents A and B are mixed uniformly. Both are then added to the phosphoric acid solution at 80 to 100°C. The solution is then heated again to 110 to 120°C, kept at that temperature for 0.5 to 1 hour, and cooled to room temperature to obtain an etching solution.
[0016] In the preparation process, when the preparation is performed under room temperature conditions, the gel lump phenomenon is easily realized, and after the silane coupling agents A and B are mixed uniformly, they are added to the phosphoric acid aqueous solution at room temperature, and then slowly heated to 80-100 ° C, more preferably 80 ° C, 90 ° C, or 100 ° C, the formed gel lump may not completely disappear and may be mixed into the formed mixture. After further increasing to 110-120 ° C, it is ensured that the formed etching solution is completely dissolved, and the temperature is further increased to 110 ° C or 120 ° C.
[0017] The mass content of the silane coupling agent A is 1.5 to 2.0%.
[0018] The mass content of the silane coupling agent B is 2.0 to 2.5%.
[0019] The mass content of phosphoric acid is 83 to 86%, with the remainder being water, and the mass content ratio of phosphoric acid to water in the etching solution is 6 to 8, and preferably 7 to 7.5.
[0020] The silane additive 1 is any one of 3-glycidyloxypropyltrimethoxysilane, diethoxy(3-glycidyloxypropyl)methylsilane, and triethoxy(3-epoxypropyloxypropyl)silane.
[0021] The silane additive 2 is any one of 2-cyanoethyltriethoxysilane, 3-isocyanatopropyltriethoxysilane, and 3-ureidopropyltriethoxysilane.
[0022] The 3D NAND structure sheet has a laminated structure of a silica film and a silicon nitride film, the silicon nitride film layer has a thickness of 500 to 1000 Å, the silica film layer has a thickness of 50 to 500 Å, and the number of layers in the laminated structure is 150 to 250.
[0023] In another aspect, the present invention provides a method for etching a 3D NAND structure sheet using a selective etching solution for the 3D NAND structure sheet, which is characterized in that a laminated structure of a silica film and a silicon nitride film is etched in the selective etching solution at an operating temperature of 156 to 164°C, more preferably 160±0.5°C. With the etching solution of the present invention, as the temperature increases, the etching rates of both silicon nitride and silica increase, but the etching rate of silica increases more than that of silicon nitride, and the etching selectivity decreases. As the temperature decreases, the selectivity increases, but silica becomes more likely to reattach.
[0024] The selective etchant contains the following ingredients:
[0025] The mass content of the silane coupling agent A is 1.5 to 2.0%.
[0026] The mass content of the silane coupling agent B is 2.0 to 2.5%.
[0027] The mass content of phosphoric acid is 83 to 86%, with the remainder being water, and the mass content ratio of phosphoric acid to water in the etching solution is 6 to 8, and preferably 7 to 7.5.
[0028] The silane additive 1 is any one of 3-glycidyloxypropyltrimethoxysilane, diethoxy(3-glycidyloxypropyl)methylsilane, and triethoxy(3-epoxypropyloxypropyl)silane.
[0029] The silane additive 2 is any one of 2-cyanoethyltriethoxysilane, 3-isocyanatopropyltriethoxysilane, and 3-ureidopropyltriethoxysilane.
[0030] The 3D NAND structure sheet has a laminated structure of a silica film and a silicon nitride film, the silicon nitride film layer has a thickness of 500 to 1000 Å, the silica film layer has a thickness of 50 to 500 Å, and the number of layers in the laminated structure is 150 to 250.
[0031] The silicon content in the etching process is 0 to 500 ppm.
[0032] When the content of added silicon in the etching solution is 0 ppm, the etching rate of silicon nitride is more than 2000 Å / 30 min, the etching rate of silica is less than 0.8 Å / 30 min, and the etching rate selectivity of silicon nitride / silica is more than 2500.
[0033] When the content of additional silicon in the etching solution is 300 ppm, the etching rate of silicon nitride exceeds 1800 Å / 30 min, and the etching rate of silica exceeds 0.3 Å / 30 min.
[0034] In the present invention, etching experiments are carried out by slicing silica and silicon nitride in order to verify the etching effect of a selective etching solution.
[0035] In the present invention, in order to verify the etching effect of the selective etching solution, etching experiments are performed by slicing silica and silicon nitride.
[0036] All of the reagents and raw materials used in the present invention can be purchased commercially.
[0037] In accordance with common knowledge in the art, the above-mentioned preferred conditions can be combined to provide a more excellent example of the etching effect of the present invention.
[0038] The advantage of the present invention, compared to the prior art, is that the present invention provides an etching solution that is selective to silicon nitride and silica and inhibits etching of silica while at the same time having a high etching life.
[0039] (1) The initial etching rate of the etching solution of the present invention for silicon nitride exceeds 2000 Å / 30 min, and the etching selectivity exceeds 2500.
[0040] (2) The etching solution of the present invention extends the window of the etching service life and silicon content of the solution through the hydrolyzable group with good water solubility, and achieves a positive etching effect of silica mainly by preventing the re-deposition of silicic acid. The etching rate of silicon nitride at a silicon content of 300 ppm is more than 1800 Å / 30 min, and the etching rate of silica is more than 0.3 Å / 30 min.
[0041] (3) The etching solution of the present invention is used to etch a 192-layer 3D NAND structure sheet, and the toothed structure is clear and complete, there is no adhesion between layers, and there is no re-deposition on the silica layer with a silicon content of 300 ppm. [Brief description of the drawings]
[0042] [Figure 1] FIG. 1 is a SEM image of the 3D NAND structure sheet of Example 3 after etching when the silicon content is 0 ppm.
[0043] [Diagram 2] FIG. 2 is a SEM image of the 3D NAND structure sheet of Example 3 after etching when the silicon content is 100 ppm.
[0044] [Diagram 3] FIG. 3 is a SEM image of the 3D NAND structure sheet of Example 3 after etching when the silicon content is 200 ppm.
[0045] [Figure 4] FIG. 4 is a SEM image of the 3D NAND structure sheet of Example 3 after etching when the silicon content is 300 ppm.
[0046] [Diagram 5] FIG. 5 is a SEM image of the 3D NAND structure sheet of Comparative Example 1 after etching when the silicon content is 300 ppm. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0047] The technical solutions in the embodiments of the present invention are described below in a clear and complete manner in conjunction with the specific embodiments of the present invention, and the above embodiments are only some of the embodiments of the present invention, not all of the embodiments. All other embodiments that can be obtained by those skilled in the art based on the embodiments of the present invention without any creative efforts belong to the protection scope of the present invention.
[0048] 1. Preparation of etching solution
[0049] Mix silane coupling agents 1 and 2 homogeneously at room temperature, add them to an aqueous solution of phosphoric acid with a concentration of about 86.5% at 80°C, completely dissolve the silane coupling agent in the phosphoric acid, heat to 120°C, keep at that temperature for 1 hour, and finally cool to room temperature.
[0050] 2. Etching experiment
[0051] 2.1 Method for detecting etching rate
[0052] Wafer etching: The deposition thicknesses of the two film materials on the silicon semiconductor wafer, silica film and silicon nitride film, are 300 Å and 1000 Å respectively, and the wafer is sliced into strips of 1.5 cm*3 cm when the experiment is carried out.
[0053] Etching temperature: 160±0.5℃.
[0054] Etching time: the silica film is etched for 3600 s, and the silicon nitride film is etched for 300 s.
[0055] Etching rate calculation method: Using ellipsometry, detect the thickness of the silica film and silicon nitride film before and after etching, and divide the difference between the initial film thickness and the film thickness after etching by the etching time, i.e., the etching rate. The etching selectivity is the ratio of the silicon nitride etching rate (SiN E / R) to the silica etching rate (SiO E / R).
[0056] 2.2 Method for detecting etching service life
[0057] By etching the silicon nitride layer, the silicon content in the etching solution is gradually increased, and the etching of silica and silicon nitride is inhibited.The initial silicon content of the etching solution is 0 ppm, and silicon nitride is dissolved therein to prepare etching solutions with silicon contents of 100 ppm, 200 ppm, and 300 ppm, and the etching rates and selectivities of silica and silicon nitride are tested respectively, so as to characterize the service life of the etching solution.
[0058] 2.3 Etching test of laminated structure
[0059] Etching experiment: The 3D NAND structure sheet is etched with etching solutions having silicon contents of 0 ppm, 100 ppm, 200 ppm, and 300 ppm, respectively. The etching conditions are the same as those of the speed detection, and the etching time is 20 min.
[0060] Detection method: The etching effect and redeposition situation are analyzed by taking high-resolution SEM images of the cross section of the 3D NAND structure sheet.
[0061] Examples 1 to 11 and Comparative Examples 1 to 7 are shown in Table 1, where the contents of phosphoric acid and silane coupling agent are expressed as mass percent, with the remainder being water.
[0062] [Table 1] TIFF2024545274000002.tif210170
[0063] When the initial silicon content was set to 0 ppm, the etching rates and selectivity ratios of the etching solutions in Examples 1 to 11 and Comparative Examples 1 to 7 for the silica film and silicon nitride film are shown in Table 2.
[0064] [Table 2] TIFF2024545274000003.tif114170
[0065] In the experiment of Example 11, the boiling point is low, the boiling conditions are unstable, and the heating time is long, and at the same time, part of the water evaporates, and the experimental conditions do not reach a stable state. The initial selection ratio of Example 10 does not meet the corresponding requirements. It is more preferable to use the ratio of Example 1, and the entire experiment is mainly centered on the ratio of Example 1.
[0066] When the silicon content was set to 100 ppm, the etching rates and selectivity ratios of the etching solutions in Examples 1 to 9 and Comparative Examples 1 to 7 for the silica film and silicon nitride film are shown in Table 3.
[0067] [Table 3] TIFF2024545274000004.tif103170
[0068] When the silicon content was set to 200 ppm, the etching rates and selectivity ratios of the etching solutions in Examples 1 to 9 and Comparative Examples 1 to 7 for the silica film and silicon nitride film are shown in Table 4.
[0069] [Table 4] TIFF2024545274000005.tif103170
[0070] NOTE: Negative numbers indicate the rate at which the silica film thickens when the silicon content is high.
[0071] When the silicon content was set to 300 ppm, the etching rates and selectivity ratios of the etching solutions in Examples 1 to 9 and Comparative Examples 1 to 7 for the silica film and silicon nitride film are shown in Table 4.
[0072] [Table 5] TIFF2024545274000006.tif103170
[0073] From the above experimental data, it can be seen that the silane coupling agent 1 in Comparative Examples 1-3 has high initial selectivity, but with the continuous increase in silicon content, its silica etching rate quickly decreases, and when the silicon content reaches 300ppm, redeposition phenomenon occurs; the silane coupling agent 2 in Comparative Examples 4-6 does not have good initial selectivity, but with the continuous increase in silicon content, positive etching is maintained; Examples 1-9 combine the advantages of two silane coupling agents, and when the silicon content is 0-300ppm, the silica etching rate is maintained at 0.3-0.8Å / 30min, and the silicon nitride etching rate is maintained at 1800-2100Å / 30min, and redeposition phenomenon does not occur. Examples 10 and 11 are the cases where the mass fraction ratio of phosphoric acid to water is adjusted. When the mass content ratio of phosphoric acid to water is less than 7, the phenomenon occurs in Example 11 that the solution boiling state during the etching process is unstable, which is not good for practical manufacture. When the mass content ratio of phosphoric acid to water is more than 8, the etching speed of silica in Example 10 is too fast, and the selectivity cannot meet the requirements of the present invention. Therefore, the ratio is preferably 7 to 7.5 to stabilize the etching result.
[0074] From the SEM image of the structure sheet, it can be seen that in Example 3, when the silicon content is 300 ppm, the 192-layer 3D NAND structure sheet after etching appears as a transparent toothed structure without adhesion, and there is no re-deposition reduction on the silica layer, which is obviously improved compared with the result of pure phosphoric acid etching. In addition, the other examples can achieve similar etching effects on the structure sheet when the silicon content is 0 to 300 ppm. The figures of Examples 1, 2, and 3 to 9 are similar to the figure of Example 3. The figures of Comparative Examples 1 to 3 when the silicon content is 300 ppm are similar to the figure of Comparative Example 1.
[0075] The selective etching solution for silica and silicon nitride of the present invention has been described in detail above, but the above content is merely a specific embodiment of the present invention and is not intended to limit the scope of protection of the present invention, and it is obvious to those skilled in the art that some modifications or improvements can be made to it based on the present invention. Therefore, as long as they do not deviate from the gist of the present invention, all of these modifications and improvements belong to the scope of protection claimed by the present invention.
Claims
1. In parts by weight 1.5-2.0% silane additive 1, 2.0-2.5% silane additive 2, A selective etching solution for 3D NAND structure sheets, comprising 83-86% phosphoric acid and the remainder water.
2. 2. The selective etching solution for a 3D NAND structure sheet according to claim 1, wherein the silane additive 1 is any one of 3-glycidyloxypropyltrimethoxysilane, diethoxy(3-glycidyloxypropyl)methylsilane, and triethoxy(3-epoxypropyloxypropyl)silane.
3. 2. The selective etching solution for 3D NAND structure sheets according to claim 1, wherein the silane additive 2 is any one of 2-cyanoethyltriethoxysilane, 3-isocyanatopropyltriethoxysilane, and 3-ureidopropyltriethoxysilane.
4. The selective etching solution for 3D NAND structure sheets according to claim 1, wherein the mass ratio of phosphoric acid to water in the etching solution is 6-8, preferably 7-7.
5.
5. 2. The selective etching solution for a 3D NAND structure sheet according to claim 1, wherein the 3D NAND structure sheet has a laminated structure of a silica film and a silicon nitride film, the silicon nitride film layer has a thickness of 500 to 1000 Å, the silica film layer has a thickness of 50 to 500 Å, and the number of layers in the laminated structure is 150 to 250.
6. A method for preparing a selective etching solution for a 3D NAND structure sheet, comprising: uniformly mixing silane coupling agents A and B at room temperature, and adding them together into a phosphoric acid solution to obtain an etching solution.
7. The method according to claim 6, characterized in that the phosphoric acid solution is preheated to a temperature of 80-100°C, the silane coupling agents A and B are mixed uniformly, and then both are added to the phosphoric acid solution at 80-100°C, and then the mixture is heated again to 110-120°C, kept at the temperature for 0.5-1 hour, and cooled to room temperature to obtain the etching solution.
8. The mass content of the silane coupling agent A is 1.5 to 2.0%; The mass content of the silane coupling agent B is 2.0 to 2.5%; The mass content of phosphoric acid is 83 to 86%, and the remainder is water, and the mass ratio of phosphoric acid to water in the etching solution is 6 to 8, preferably 7 to 7.5; The silane additive 1 is any one of 3-glycidyloxypropyltrimethoxysilane, diethoxy(3-glycidyloxypropyl)methylsilane, and triethoxy(3-epoxypropyloxypropyl)silane; 8. The method of claim 7, wherein the silane additive 2 is one of 2-cyanoethyltriethoxysilane, 3-isocyanatopropyltriethoxysilane, and 3-ureidopropyltriethoxysilane.
9. 9. The method of claim 8, wherein the 3D NAND structure sheet is a laminated structure of a silica film and a silicon nitride film, the silicon nitride film layer has a thickness of 500-1000 Å, the silica film layer has a thickness of 50-500 Å, and the number of layers in the laminated structure is 150-250 layers.
10. A method for etching a 3D NAND structure sheet with a selective etching solution, comprising: etching a laminated structure of a silica film and a silicon nitride film in the selective etching solution at an operating temperature of 156-164°C.
11. Selective etchants include: The silane coupling agent A has a mass content of 1.5 to 2.0%; A silane coupling agent B having a mass content of 2.0 to 2.5%; The raw materials are phosphoric acid with a mass content of 83-86%, and the rest water. The mass ratio of phosphoric acid to water in the etching solution is 6 to 8, preferably 7 to 7.5; The silane additive 1 is any one of 3-glycidyloxypropyltrimethoxysilane, diethoxy(3-glycidyloxypropyl)methylsilane, and triethoxy(3-epoxypropyloxypropyl)silane; The silane additive 2 is any one of 2-cyanoethyltriethoxysilane, 3-isocyanatopropyltriethoxysilane, and 3-ureidopropyltriethoxysilane; 11. The method of claim 10, wherein the 3D NAND structure sheet is a laminated structure of a silica film and a silicon nitride film, the silicon nitride film layer has a thickness of 500-1000 Å, the silica film layer has a thickness of 50-500 Å, and the number of layers in the laminated structure is 150-250 layers.
12. 12. The method of claim 11, wherein the 3D NAND structure sheet is a laminated structure of a silica film and a silicon nitride film, the silicon nitride film layer has a thickness of 500-1000 Å, the silica film layer has a thickness of 50-500 Å, and the number of layers in the laminated structure is 150-250 layers.
13. The silicon content in the etching process is 0-500 ppm; When the content of additional silicon in the etching solution is 0 ppm, the etching rate of silicon nitride is more than 2000 Å / 30 min, the etching rate of silica is less than 0.8 Å / 30 min, and the etching rate selectivity of silicon nitride / silica is more than 2500; 13. The method of claim 12, wherein when the content of additional silicon in the etching solution is 300 ppm, the etching rate of silicon nitride is greater than 1800 Å / 30 min and the etching rate of silica is greater than 0.3 Å / 30 min.
Citation Information
Patent Citations
Insulation layer etchant composition and method of forming pattern using the same
CN110157434A
Composition for silicon nitride film etching
JP2018182312A
Silicon nitride etchant composition
JP2020145343A
Etching composition for silicon nitride and method for manufacturing semiconductor device
JP2022048714A
Silicon nitride film etching composition
JP2022520655A