Curable resin composition and polymer optical waveguide
The curable resin composition with a fluorine-containing polymer and cyclic ether structure addresses the trade-off between heat and bending resistance, providing enhanced performance for polymer optical waveguides.
Patent Information
- Application Number
- JP2025069660
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2025-04-21
- Publication Date
- 2026-11-02
AI Technical Summary
Existing polymer optical waveguides face a trade-off between heat resistance and bending resistance, making them unsuitable for practical applications where both properties are required, especially in high-temperature environments and flexible devices.
A curable resin composition containing a fluorine-containing polymer, a polymerization initiator, and a compound with a cyclic ether structure, which enhances both heat resistance and bending resistance after curing.
The composition achieves excellent heat resistance and bending resistance, maintaining optical properties over time and flexibility, suitable for polymer optical waveguides.
Smart Images

Figure 2026174993000001 
Figure 2026174993000002 
Figure 2026174993000003
Abstract
Description
[Technical Field]
[0001] The present invention relates to a curable resin composition and a polymer optical waveguide. [Background technology]
[0002] In the field of telecommunications equipment, expectations are rising for the use of polymer optical waveguides made of resin for signal transmission, as devices become smaller and communication speeds increase. Well-known resin materials include norbornene resin and siloxane resin. However, these resins have drawbacks, such as poor transparency in wavelength ranges used in optical communications, for example, 1260-1360 nm (O-band) and 1530-1565 nm (C-band).
[0003] Recently, the use of fluorine-containing polymers as polymer optical waveguide materials has attracted attention. For example, Patent Document 1 discloses that by using a resin in which monomers or oligomers are partially fluorinated as an optical waveguide, optical properties can be maintained for a long time. [Prior art documents] [Patent Documents]
[0004] [Patent Document 1] International Publication No. 2008 / 017318 [Overview of the project] [Problems that the invention aims to solve]
[0005] In order to commercialize such polymer optical waveguides, not only transparency but also heat resistance is required. This is because, for example, temperatures of around 260°C may be applied during reflow assembly, and the practical conditions may reach high temperatures of around 150°C. However, no studies on heat resistance for practical application, as described above, had been conducted.
[0006] The inventors investigated and found that adding monomers with a more rigid structure to improve heat resistance resulted in a loss of flexibility in the cured resin composition, making it prone to cracking when bent. In other words, there is a trade-off between heat resistance and bending resistance after curing, and it is difficult to achieve both. The bending resistance of the cured material is an important characteristic from the perspective of flexible optical waveguides.
[0007] Therefore, the present invention aims to provide a curable resin composition that achieves both excellent heat resistance and bending resistance after curing. Furthermore, it also aims to provide a polymer optical waveguide using the cured product of the above curable resin composition. [Means for solving the problem]
[0008] As the inventors further investigated the above-mentioned problems, they conceived the idea that by adding a compound having a cyclic ether structure to a fluorine-containing polymer, it is possible to create a curable resin composition that exhibits excellent heat resistance and bending resistance after curing, thus completing the present invention.
[0009] In other words, the gist of this embodiment is as follows.
[0010] [1] A curable resin composition containing 100 parts by mass of a fluorine-containing polymer (A), 0.5 to 4 parts by mass of a polymerization initiator (B), and 2 to 30 parts by mass of a compound (C) having a cyclic ether structure. [2] The compound (C) having the cyclic ether structure is a 4- to 6-membered ring, and contains one or more oxygen atoms and one or more carbon atoms as atoms forming the skeleton of the 4- to 6-membered ring, At least one of the carbon atoms forming the 4- to 6-membered ring skeleton has a substituent, At least one of the substituents is a C2-C10 alkyl group, cycloalkyl group, ether group, aryl group, or heteroaryl group having a functional group. The curable resin composition according to [1], wherein the functional group is at least one selected from the group consisting of an acryloyl group, a methacryloyl group, a thionyl group, an allyl group, a vinyl group, an acetylene group, and a stynyl group. [3] The curable resin composition according to [1] or [2] above, wherein the fluorine-containing polymer (A) is a condensation reaction product of a fluorine-containing aromatic compound (X) represented by the following general formula (1), at least one of a compound having a crosslinkable functional group and a phenolic hydroxyl group (Y-1) and a compound having a crosslinkable functional group and a fluorine atom-substituted aromatic ring (Y-2), and a compound having three or more phenolic hydroxyl groups (Z).
[0011] [ka]
[0012] (In the formula, n represents an integer from 0 to 3, a and b each independently represent an integer from 0 to 3, and Rf 1 and Rf 2 Each of these independently represents a fluorine-containing alkyl group with 8 or fewer carbon atoms, and the F within the aromatic ring indicates that all hydrogen atoms in that aromatic ring are replaced by fluorine atoms.
[0013] [4] The curable resin composition according to any one of [1] to [3], wherein the change in transmittance at a wavelength of 1310 nm after the film is further held at 150°C for 1000 hours with respect to the transmittance at a wavelength of 1310 nm when the curable resin composition is cured to form a film with a thickness of 0.3 mm is 5% or less. [5] The curable resin composition according to any one of [1] to [4], wherein the change in refractive index at a wavelength of 1310 nm of the cured product obtained by curing the curable resin composition, after the cured product is further held at 150°C for 1000 hours, is within 3%. [6] The curable resin composition according to any one of [1] to [5] above, wherein the curable resin composition is cured by ultraviolet irradiation and heating at 190°C for 1 hour to form a film with a thickness of 0.1 mm, and the minimum bending radius is 5 mm or less. [7] The curable resin composition according to any one of the above [1] to [6], which is used for members for optical communication applications by being cured. [8] A polymer optical waveguide, wherein a cured product of the curable resin composition according to any one of the above [1] to [7] is used for at least one of a core and a cladding. [Advantageous Effects of Invention]
[0014] According to the present embodiment, it is possible to provide a curable resin composition that achieves both excellent heat resistance and bending resistance after curing. It is also possible to provide a polymer optical waveguide having heat resistance and bending resistance. [Description of Embodiments for Carrying Out the Invention]
[0015] Hereinafter, the present invention will be described in detail. However, the present invention is not limited to the following embodiments, and can be arbitrarily modified and implemented without departing from the gist of the present invention. In the present specification, "~" indicating a numerical range is used to mean that the numerical values described before and after it are included as the lower limit value and the upper limit value.
[0016] 《Curable Resin Composition》 The curable resin composition according to the present embodiment contains a fluorine-containing polymer (A), a polymerization initiator (B), and a compound (C) having a cyclic ether structure. Since the compound (C) has a cyclic ether structure, it is possible to obtain a curable resin composition that is excellent in both heat resistance and bending resistance after curing, which were conventionally difficult to achieve simultaneously due to a trade-off relationship.
[0017] The curable resin composition according to the present embodiment preferably contains 2 to 30 parts by mass of the compound (C) having a cyclic ether structure relative to 100 parts by mass of the fluorine-containing polymer (A), and more preferably further contains 0.5 to 4 parts by mass of the polymerization initiator (B).
[0018] <Fluorine-containing Polymer (A)> The fluorine-containing polymer (A) in the present embodiment is not particularly limited as long as it has fluorine atoms. For example, a fluorine-containing polymer used for polymer optical waveguides is preferred, more preferably one having a crosslinkable functional group, and still more preferably one that crosslinks and cures by at least one of light irradiation and heat.
[0019] The fluorine-containing polymer (A) in the present embodiment is preferably, for example, a condensation reaction product of the below-described fluorine-containing aromatic compound (X), at least one of the compound (Y-1) having a crosslinkable functional group and a phenolic hydroxyl group and the compound (Y-2) having a crosslinkable functional group and a fluorine atom-substituted aromatic ring, and the compound (Z) having 3 or more phenolic hydroxyl groups.
[0020] The number average molecular weight of the fluorine-containing polymer (A) in the present embodiment is not particularly limited, and is, for example, preferably 1×10 3 ~5×10 5 . Here, from the viewpoints of coating properties and heat resistance of the curable resin composition, bending resistance after curing, solvent resistance and the like, the number average molecular weight is preferably 1×10 3 or more, more preferably 1.5×10 3 or more, and is preferably 5×10 5 or less, more preferably 1×10 5 or less.
[0021] ·Fluorine-containing aromatic compound (X) The fluorine-containing aromatic compound (X) is a compound represented by the following general formula (1).
[0022]
Chemical Formula
[0023] (In general formula (1), n represents an integer of 0 to 3, a and b each independently represent an integer of 0 to 3, Rf 1 and Rf 2 each independently represent a fluorine-containing alkyl group having 8 or less carbon atoms, and F in the aromatic ring represents that all hydrogen atoms on the aromatic ring are substituted with fluorine atoms.)
[0024] In general formula (1), Rf 1 and Rf 2 The group is a fluorine-containing alkyl group, but its carbon number is 8 or less, preferably 3 or less. Among these, perfluoroalkyl groups are preferred from the viewpoint of heat resistance. Specific examples include perfluoromethyl group, perfluoroethyl group, perfluoropropyl group, perfluorobutyl group, perfluorohexyl group, and perfluorooctyl group.
[0025] In general formula (1), a and b are each independent integers from 0 to 3, but from the viewpoint of ease of manufacture, 0 to 2 is preferred, 0 to 1 is more preferred, and 0 is the most preferred. Note that if a and b are 2 or more, there are multiple Rf 1 , Rf 2 The structures of each may be the same or different.
[0026] In general formula (1), n is an integer between 0 and 3, preferably between 1 and 3. The fluorine-containing aromatic compound (X) in general formula (1) is preferably perfluorobenzene, perfluorotoluene, or perfluoroxylene when n=0; perfluorobiphenyl when n=1; perfluoroterphenyl when n=2; and perfluoro(1,3,5-triphenylbenzene) or perfluoro(1,2,4-triphenylbenzene) when n=3, with perfluorotoluene, perfluoro(1,3,5-triphenylbenzene), perfluoro(1,2,4-triphenylbenzene), or perfluorobiphenyl being particularly preferred. If n is 2 or 3, the n structures within the parentheses may be identical or different.
[0027] The fluorine-containing aromatic compound (X) may be used alone or in a mixture of two or more types. In general formula (1), when n=3, a branched structure is introduced into the fluorine-containing polymer (A), which improves heat resistance. Perfluorobiphenyl is the most preferred fluorine-containing aromatic compound (X) because it offers an excellent balance between dielectric constant and heat resistance of the resulting cured product, as well as high flexibility.
[0028] ·Compound (Y-1) Compound (Y-1) in this embodiment is a compound having a crosslinkable functional group and a phenolic hydroxyl group. Because compound (Y-1) has a crosslinkable functional group, when cured, a cured product is obtained that simultaneously satisfies low dielectric constant, low water absorption, and high heat resistance.
[0029] Examples of compound (Y-1) include phenols having reactive double bonds such as 4-hydroxystyrene and 4-acetoxystyrene; ethynylphenols such as 3-ethynylphenol, 4-phenylethynylphenol, and 4-(4-fluorophenyl)ethynylphenol; bis(phenylethynyl)dihydroxybiphenyls such as 2,2'-bis(phenylethynyl)-5,5'-dihydroxybiphenyl and 2,2'-bis(phenylethynyl)-4,4'-dihydroxybiphenyl; and dihydroxydiphenylacetylenes such as 4,4'-dihydroxytran and 3,3'-dihydroxytran. These may be used individually or in combination of two or more. Among these, phenols having a reactive double bond are preferred from the viewpoint of reaction efficiency with fluorine-containing aromatic compounds (X), and 4-acetoxystyrene is more preferred.
[0030] ·Compound (Y-2) Compound (Y-2) in this embodiment is a compound having a crosslinkable functional group and a fluorine atom-substituted aromatic ring. Because compound (Y-2) has a crosslinkable functional group, when cured, a cured product is obtained that simultaneously satisfies low dielectric constant, low water absorption, and high heat resistance.
[0031] Examples of compound (Y-2) include fluorine-containing aryl compounds having reactive double bonds such as pentafluorostyrene, pentafluorobenzyl acrylate, pentafluorobenzyl methacrylate, pentafluorophenyl acrylate, pentafluorophenyl methacrylate, perfluorostyrene, pentafluorophenyl trifluorovinyl ether, and 3-(pentafluorophenyl)pentafluoropropene-1; fluorine-containing aryl compounds having cyano groups such as pentafluorobenzonitrile; fluorine-containing arylacetylene compounds having triple bonds such as pentafluorophenylacetylene and nonafluorobiphenylacetylene; and fluorine-containing diarylacetylene compounds such as phenylethynylpentafluorobenzene, phenylethynylnonafluorobiphenyl, and decafluorotran. These may be used individually or in mixtures of two or more. Fluorine-containing aryl compounds having reactive double bonds and fluorine-containing arylacetylene compounds having triple bonds are preferred because the crosslinking reaction proceeds at relatively low temperatures and the resulting fluorine-containing polymer (A) has high heat resistance.
[0032] While at least one of the above compounds (Y-1) and (Y-2) may be used, it is preferable to use compound (Y-1) from the viewpoint of ease of manufacture.
[0033] Compounds having three or more phenolic hydroxyl groups (Z) In this embodiment, compound (Z) is a compound having three or more phenolic hydroxyl groups. By using a compound (Z) having three or more phenolic hydroxyl groups, a branched structure is introduced into the polymer chain, making the molecular structure three-dimensional. This is preferable because, when the resulting curable resin composition is cured, the free volume of the polymer is increased, resulting in lower density, i.e., lower dielectric constant. Furthermore, while linear polymers having aromatic rings are generally prone to molecular orientation due to stacking of the aromatic rings, in the curable resin composition according to this embodiment, molecular orientation is suppressed by introducing a branched structure, resulting in reduced birefringence.
[0034] The number of phenolic hydroxyl groups in compound (Z) may be three or more, preferably three to six, more preferably three or four, and even more preferably three. Since compound (Z) does not have a crosslinking functional group, it can be clearly distinguished from compound (Y-1).
[0035] Examples of compound (Z) include trihydroxybenzene, trihydroxybiphenyl, trihydroxynaphthalene, 1,1,1-tris(4-hydroxyphenyl)ethane, tris(4-hydroxyphenyl)benzene, tetrahydroxybenzene, tetrahydroxybiphenyl, tetrahydroxybinaphthyl, and tetrahydroxyspiroindanes. Since the flexibility of the film when the curable resin composition is cured is increased, compound (Z) is preferably a compound having three phenolic hydroxyl groups, and among these, trihydroxybenzene and 1,1,1-tris(4-hydroxyphenyl)ethane are more preferred, and trihydroxybenzene is even more preferred, because they result in a lower dielectric constant of the cured product.
[0036] Method for producing fluorine-containing polymer (A) In this embodiment, when using a condensation reaction product of a fluorine-containing polymer (A) represented by general formula (1), a compound (X), a compound having a crosslinkable functional group and a phenolic hydroxyl group (Y-1), a compound having a crosslinkable functional group and a fluorine atom-substituted aromatic ring (Y-2), and a compound (Z) having three or more phenolic hydroxyl groups, a commercially available product or a manufactured product may be used. The above-mentioned fluorine-containing polymer (A) can be produced, for example, by at least one of the following methods (i) and (ii).
[0037] (i) A method for condensing a fluorine-containing aromatic compound (X) represented by general formula (1), a compound (Z) having three or more phenolic hydroxyl groups, and a compound (Y-1) having a crosslinkable functional group and a phenolic hydroxyl group, in the presence of a HF removal agent. (ii) A method for condensing a fluorine-containing aromatic compound (X) represented by general formula (1), a compound (Z) having three or more phenolic hydroxyl groups, and a compound (Y-2) having a crosslinkable functional group and a fluorine atom-substituted aromatic ring in the presence of a fluorine removal agent.
[0038] Furthermore, when producing the fluorine-containing polymer (A) by both methods (i) and (ii) above, the fluorine-containing aromatic compound (X), compound (Z), compound (Y-1), and compound (Y-2) are subjected to a condensation reaction in the presence of a fluorine-removing agent.
[0039] In either method (i) or (ii) above, the condensation reaction may be carried out in a single step or in multiple steps. Alternatively, a specific compound may be reacted preferentially first, followed by the reaction of other compounds. When a condensation reaction is carried out in multiple steps, the intermediate products obtained during the process may be separated from the reaction system, purified, and then used in subsequent reactions (condensation reactions). The starting compounds may be added all at once, continuously, or intermittently during the reaction.
[0040] As a dehydrogenase agent, basic compounds are preferred, and alkali metal carbonates, bicarbonates, or hydroxides are particularly preferred. Specifically, examples include sodium carbonate, potassium carbonate, sodium bicarbonate, potassium bicarbonate, sodium hydroxide, potassium hydroxide, and the like.
[0041] <Polymerization initiator (B)> The polymerization initiator (B) in this embodiment is not particularly limited once the polymerization reaction has started. When the curable resin composition according to this embodiment is cured by light irradiation, the photosensitive agent that acts as a polymerization initiator preferably contains one or more selected from the group consisting of benzoin alkyl ether derivatives, benzophenone derivatives, α-aminoalkylphenone derivatives, oxime ester derivatives, thioxanthone derivatives, anthraquinone derivatives, acylphosphine oxide derivatives, glyoxyester derivatives, organic peroxide derivatives, trihalomethyltriazine derivatives, and titanocene derivatives, and among these, oxime ester derivatives are more preferred from the viewpoint of radical generation efficiency.
[0042] Suitable commercially available α-aminoalkylphenone-based products include IRGACURE 907 and IRGACURE 369 from Ciba Specialty Chemicals. Suitable commercially available oxime ester derivatives include IRGACURE OXE01, IRGACURE OXE02, and IRGACURE OXE04 from Ciba Specialty Chemicals. Suitable commercially available acylphosphine oxide derivatives include DAROCUR® TPO manufactured by Ciba Specialty Chemicals. Polymerization initiator (B) may be used alone or in combination of two or more types.
[0043] When the curable resin composition according to this embodiment is cured by heat, examples of thermosetting accelerators that act as polymerization initiators include azobisisobutyronitrile, benzoyl peroxide, tert-butyl hydroperoxide, cumene hydroperoxide, di-tert-butyl peroxide, and dicumyl peroxide.
[0044] <Compounds having a cyclic ether structure (C)> Compound (C) in this embodiment has a cyclic ether structure. A cyclic ether structure is a ring structure containing oxygen atoms, that is, a ring containing oxygen atoms. The ring in the above cyclic ether structure may be saturated or unsaturated.
[0045] In the above cyclic ether structure, the ring is preferably a 4- to 6-membered ring, and more preferably a saturated cyclic structure with a 4- to 6-membered ring. Furthermore, it is preferable that the atoms forming the 4-6 membered ring skeleton include one or more oxygen atoms and one or more carbon atoms, and it is more preferable that the ring skeleton is formed from only oxygen atoms and carbon atoms.
[0046] Compound (C) in this embodiment may have only one cyclic ether structure or two or more. The number of cyclic ether structures may be, for example, 1 to 4, preferably 1 to 3, and more preferably 1 to 2. If there are two or more cyclic ether structures, they may be directly bonded to each other by sharing one carbon atom, or they may be bonded to each other via substituents.
[0047] The above cyclic ether structure preferably has one or more substituents among the carbon atoms constituting the ring. The number of carbon atoms in the substituent is preferably 1 to 15, and more preferably 2 to 10. The substituents are more preferably alkyl groups, cycloalkyl groups, ether groups, aryl groups, or heteroaryl groups.
[0048] The substituents described above preferably have a functional group. The above functional group is more preferably at least one selected from the group consisting of, for example, acryloyl group, methacryloyl group, thionyl group, allyl group, vinyl group, acetylene group, and stynyl group.
[0049] As a combination of these, for example, the above cyclic ether structure is a 4- to 6-membered ring, preferably a saturated cyclic 4- to 6-membered ring, and it is more preferable that the atoms forming the skeleton of this 4- to 6-membered ring include one or more oxygen atoms and one or more carbon atoms. Furthermore, it is even more preferable that at least one of the carbon atoms forming the skeleton of the 4- to 6-membered ring has a substituent, and at least one of the substituents is a C1-C15 alkyl group, cycloalkyl group, ether group, aryl group, or heteroaryl group having a functional group, and in addition to these, it is even more preferable that the above functional group is at least one selected from the group consisting of acryloyl group, methacryloyl group, thionyl group, allyl group, vinyl group, acetylene group, and stynyl group.
[0050] The following are examples of compounds (C) having a cyclic ether structure in this embodiment, but are not limited to these.
[0051] [ka]
[0052] <Other optional ingredients> The curable resin composition according to this embodiment may further contain other optional components, as long as they do not impair the effects of the present invention. Other optional components include, for example, solvents and additives.
[0053] If the curable resin composition according to this embodiment contains a solvent, the proportion of the solvent to the curable resin composition may be, for example, 0 to 99% by mass or 20 to 85% by mass.
[0054] Additives include, for example, stabilizers such as UV absorbers, antioxidants, thermal polymerization inhibitors, and polymerization inhibitors; surfactants such as leveling agents, defoamers, precipitation inhibitors, and dispersants; plasticizers; thickeners, and various other additives well known in the coating field.
[0055] Furthermore, if the cured film obtained by curing the curable resin composition is a material (straight material) that remains as a functional component in the final product without being removed during the manufacturing process, such as an interlayer insulating film, an adhesion improver such as a silane coupling agent may be added to the curable resin composition.
[0056] If the curable resin composition according to this embodiment contains an additive, the proportion of the additive relative to the curable resin composition may be, for example, 0.1 to 10% by mass.
[0057] <Content ratio> The curable resin composition according to this embodiment preferably contains 2 to 50 parts by mass of a compound having a cyclic ether structure (C) per 100 parts by mass of a fluorine-containing polymer (A), and more preferably contains 0.5 to 5 parts by mass of a polymerization initiator (B).
[0058] From the viewpoint of refractive index, the content of compound (C) having a cyclic ether structure is preferably 2 parts by mass or more, more preferably 5 parts by mass or more, and even more preferably 10 parts by mass or more, per 100 parts by mass of fluorine-containing polymer (A). Furthermore, from the viewpoint of absorption characteristics, the above content is preferably 50 parts by mass or less, more preferably 45 parts by mass or less, and even more preferably 40 parts by mass or less.
[0059] From the viewpoint of light absorption characteristics when the curable resin composition is used as a polymer optical waveguide, the content of the polymerization initiator (B) is preferably 0.5 parts by mass or more, more preferably 0.75 parts by mass or more, even more preferably 1.0 part by mass or more, and also preferably 5 parts by mass or less, more preferably 4.5 parts by mass or less, and even more preferably 4 parts by mass or less, per 100 parts by mass of the fluorine-containing polymer (A).
[0060] <Physical properties / characteristics> The heat resistance of the curable resin composition according to this embodiment after curing can be indicated by changes in transmittance and refractive index. Specifically, the curable resin composition is cured to form a 0.3 mm thick film, and the transmittance at a wavelength of 1310 nm is determined before and after holding the film at 150°C for 1000 hours. The change in transmittance after holding relative to the transmittance before holding is preferably 5% or less, more preferably 2% or less, even more preferably 1% or less, and the smaller the change, the better. The curing conditions for the curable resin composition when measuring the change in transmittance are not particularly limited, but for example, a 0.3 mm thick film is used, which is obtained by dissolving the curable resin composition in a solvent, applying it to a substrate, irradiating it with ultraviolet light, and then curing it by heating it at 190°C for 1 hour.
[0061] Similarly, regarding the change in refractive index, the refractive index at a wavelength of 1310 nm is determined before and after holding the cured product, which is made by curing the curable resin composition, at 150°C for 1000 hours. The change in refractive index after holding relative to the refractive index before holding is preferably 3% or less, more preferably 2% or less, even more preferably 1% or less, and the smaller the change, the better. The curing conditions for the curable resin composition when measuring the refractive index change are not particularly limited, but for example, a 30 μm thick film is used, which is obtained by dissolving the curable resin composition in a solvent, applying it to a substrate, irradiating it with ultraviolet light, and then heating it at 190°C for 1 hour to cure it.
[0062] The bending resistance of the curable resin composition according to this embodiment after curing can be indicated by the minimum bending radius when it is formed into a film. Specifically, the curable resin composition is cured by ultraviolet irradiation and heating at 190°C for 1 hour to obtain a film with a thickness of 0.1 mm. The minimum bending radius of the above film is preferably 5 mm or less, more preferably 3 mm or less, even more preferably 2 mm or less, and even more preferably 1 mm or less. Here, the minimum bending radius is the bending radius at which cracks appear on the surface of the bent portion when the hardened film is bent, and it is an indicator of the bending limit. The bending radius is synonymous with the radius of curvature. The above minimum bending radius is measured in accordance with JIS K 7171:2016.
[0063] <Application> The curable resin composition according to this embodiment can be suitably used in optical communication components such as waveguides and lenses after curing. In particular, it is preferable to use it as a polymer optical waveguide by curing it, and it may be used in at least one of the core and cladding.
[0064] 《Cured film》 A cured film obtained by curing the curable resin composition described above in "Curable Resin Composition" in film form is suitable, for example, as a polymer optical waveguide. Specifically, at least one of the core and cladding constituting the polymer optical waveguide is made of a cured product of the curable resin composition described above. A preferred embodiment of this curable resin composition is the same as the preferred embodiment described above.
[0065] Polymer optical waveguides consist of a core and a cladding with a lower refractive index than the core. When using the cured product of the curable resin composition described above for both the core and the cladding, the refractive index can be adjusted by adjusting the mixing ratio of the fluorine-containing polymer (A), polymerization initiator (B), compound having a cyclic ether structure (C), and other optional components, or by adding additives as appropriate.
[0066] The method for producing the cured film described above is not particularly limited, but for example, it can be obtained by dissolving a curable resin composition in a solvent, applying it to a substrate, and curing it by light irradiation or heating. Light irradiation and heating may be performed sequentially or simultaneously to cure the curable resin composition. Furthermore, when using polymer optical waveguides, methods such as the replication (stamper) method, direct exposure method, a combination of reactive ion etching (RIE) and photolithography process, injection molding-based method, photobleaching method, direct writing method, and self-forming method can be employed.
[0067] When curing a coating film of a curable resin composition by heating, the heating temperature may be, for example, 100 to 350°C or 150 to 250°C.
[0068] When curing a coating film of a curable resin composition by light irradiation, for example, ultraviolet light is used for irradiation (exposure). In this case, pre-baking may be performed at 40-100°C, followed by light irradiation, and then final baking. The heating temperature for final baking is, for example, 100-350°C.
[0069] The thickness of the cured film can be appropriately selected depending on the application and is not particularly limited. For example, when used as a core or cladding for polymer optical waveguides, a thickness of 0.1 to 100 μm is acceptable, or 1 to 50 μm. Alternatively, the thickness of the cured film can be 0.1 μm to 1 mm. [Examples]
[0070] The present invention will be described more specifically by reference to examples and comparative examples, but the present invention is not limited thereto, and various modifications are possible as long as the essence of the invention is not altered. Examples 1 to 4 are examples, while Examples 5 and 6 are comparative examples.
[0071] [Example Test] <Example 1> In an N,N-dimethylacetamide (hereinafter referred to as "DMAc") solvent, perfluorobiphenyl (225 g) and 1,3,5-trihydroxybenzene (40 g) were reacted at 40°C for 6 hours in the presence of potassium carbonate. Subsequently, 4-acetoxystyrene (30 g) was reacted in the presence of a 48% by mass potassium hydroxide aqueous solution to synthesize a fluorine-containing polymer. The obtained fluorine-containing polymer was reprecipitated and purified by adding the DMAc solution to an aqueous hydrochloric acid solution (3.5% by mass aqueous solution), and then vacuum-dried to obtain a powdered fluorine-containing polymer (A).
[0072] To the solvent propylene glycol monomethyl ether acetate (PGMEA), 100 parts by mass of the fluorine-containing polymer (A) obtained above, 2 parts by mass of polymerization initiator (B) (CIBA Specialty Chemicals, IRGACURE OXE01), 20 parts by mass of compound (C-1) having a cyclic ether structure represented by the following formula, and 4-tert-butylcatechol (TBC) as a polymerization inhibitor were added and mixed at room temperature for 48 hours using a mixing rotor to obtain a curable resin composition.
[0073] [ka]
[0074] <Example 2> A curable resin composition was obtained in the same manner as in Example 1, except that a compound having a cyclic ether structure (C-2), represented by the following formula, was used instead of a compound having a cyclic ether structure (C-1).
[0075] [ka]
[0076] <Example 3> A curable resin composition was obtained in the same manner as in Example 1, except that a compound having a cyclic ether structure (C-3), represented by the following formula, was used instead of a compound having a cyclic ether structure (C-1).
[0077] [ka]
[0078] <Example 4> A curable resin composition was obtained in the same manner as in Example 1, except that a compound having a cyclic ether structure (C-4), represented by the following formula, was used instead of a compound having a cyclic ether structure (C-1).
[0079] [ka]
[0080] <Example 5> A curable resin composition was obtained in the same manner as in Example 1, except that a compound represented by the following formula (C'-5) was used instead of a compound having a cyclic ether structure (C-1).
[0081] [ka]
[0082] <Example 6> A curable resin composition was obtained in the same manner as in Example 1, except that a compound represented by the following formula (C'-6) was used instead of a compound having a cyclic ether structure (C-1).
[0083] [ka]
[0084] "evaluation" <Heat resistance; change in transmittance> The curable resin compositions obtained in each example were dissolved in PGMEA, applied to a substrate, and cured by UV irradiation followed by heating at 190°C for 1 hour to obtain a cured film with a thickness of 0.3 mm. Using test pieces cut from this film to a size of 1 cm × 1 cm, the transmittance at a wavelength of 1310 nm was measured before and after holding at 150°C for 1000 hours. The change in transmittance (%) after holding was calculated using the transmittance at a wavelength of 1310 nm before holding as a baseline. The results are shown in Table 1 under "Heat Resistance; Transmittance Change." "○" indicates that the calculated transmittance change is within 5%, meaning the heat resistance is good, while "×" indicates that the calculated transmittance change is greater than 5%, meaning the heat resistance is poor.
[0085] <Heat resistance; refractive index change> The curable resin compositions obtained in each example were dissolved in PGMEA, applied to a substrate, and cured by UV irradiation followed by heating at 190°C for 1 hour to obtain a cured film with a thickness of approximately 30 μm. Using test pieces cut from this film to a size of 1 cm × 1 cm, the refractive index at a wavelength of 1310 nm was measured before and after holding at 150°C for 1000 hours. The refractive index change (%) after holding was calculated using the refractive index at 1310 nm before holding as the baseline. The results are shown in Table 1 under "Heat Resistance; Refractive Index Change." "○" indicates that the calculated refractive index change was within 3%, meaning the heat resistance was good, while "×" indicates that the calculated refractive index change was greater than 3%, meaning the heat resistance was poor.
[0086] <Bending resistance> The curable resin compositions obtained in each example were dissolved in PGMEA and applied to a substrate. Subsequently, the mixture was cured by UV irradiation and heating at 190°C for 1 hour to obtain a cured film with a thickness of 0.1 mm. A bending test was performed on the above film in accordance with JIS K 7171:2016 to determine the minimum bending radius. The results are shown in Table 1 under "Bending Resistance." "○" indicates that the minimum bending radius is 5 mm or less, and that the bending resistance is good, while "×" indicates that the minimum bending radius is greater than 5 mm, and that the bending resistance is poor.
[0087] [Table 1]
[0088] The results of Example 5 show that cured resin compositions containing a compound with an ether structure (C'-5) exhibit excellent flexural resistance but poor heat resistance. On the other hand, as can be seen from the results of Example 6, using a compound with a hydrocarbon ring structure (C'-6) resulted in a cured product with good heat resistance but poor flexural resistance. Thus, simply adding compounds with ether or ring structures did not allow for a balance between heat resistance and flexural resistance in cured resin compositions. In contrast, the curable resin composition according to this embodiment, by containing a compound (C) having a cyclic ether structure, was able to achieve both good heat resistance and bending resistance after curing.
Claims
1. A curable resin composition containing 100 parts by mass of a fluorine-containing polymer (A), 0.5 to 4 parts by mass of a polymerization initiator (B), and 2 to 30 parts by mass of a compound (C) having a cyclic ether structure.
2. The compound (C) having the cyclic ether structure has a 4- to 6-membered ring, and contains one or more oxygen atoms and one or more carbon atoms as atoms forming the skeleton of the 4- to 6-membered ring. At least one of the carbon atoms forming the 4- to 6-membered ring skeleton has a substituent, At least one of the substituents is a C2-C10 alkyl group, cycloalkyl group, ether group, aryl group, or heteroaryl group having a functional group. The curable resin composition according to claim 1, wherein the functional group is at least one selected from the group consisting of an acryloyl group, a methacryloyl group, a thionyl group, an allyl group, a vinyl group, an acetylene group, and a stynyl group.
3. The curable resin composition according to claim 1 or 2, wherein the fluorine-containing polymer (A) is a condensation reaction product of a fluorine-containing aromatic compound (X) represented by the following general formula (1), at least one of a compound (Y-1) having a crosslinkable functional group and a phenolic hydroxyl group, and a compound (Y-2) having a crosslinkable functional group and a fluorine atom-substituted aromatic ring, and a compound (Z) having three or more phenolic hydroxyl groups. 【Chemistry 1】 (In the formula, n represents an integer from 0 to 3, a and b each independently represent an integer from 0 to 3, and Rf 1 and Rf 2 Each of these independently represents a fluorine-containing alkyl group with 8 or fewer carbon atoms, and the F within the aromatic ring indicates that all hydrogen atoms in that aromatic ring are replaced by fluorine atoms.
4. The curable resin composition according to claim 1 or 2, wherein the change in transmittance at a wavelength of 1310 nm after the film is further held at 150°C for 1000 hours, relative to the transmittance at a wavelength of 1310 nm when the curable resin composition is cured to form a film with a thickness of 0.3 mm, is within 5%.
5. The curable resin composition according to claim 1 or 2, wherein the change in refractive index at a wavelength of 1310 nm of the cured product obtained by curing the curable resin composition, after the cured product is further held at 150°C for 1000 hours, is within 3%.
6. The curable resin composition according to claim 1 or 2, wherein when the curable resin composition is cured by ultraviolet irradiation and heating at 190°C for 1 hour to form a film with a thickness of 0.1 mm, the minimum bending radius is 5 mm or less.
7. A curable resin composition according to claim 1 or 2, which, when cured, is used in components for optical communication applications.
8. A polymer optical waveguide in which at least one of the core and the cladding is a cured product of the curable resin composition according to claim 1 or 2.
Citation Information
Patent Citations
Optical device and polymer material with nonlinear optical properties
WO2008017318A1