Methods for producing polymers and metal-polymer composites
By using activated metal surfaces to initiate polymerization of monomers directly on metals, the method addresses the challenges of conventional bonding techniques, achieving efficient and cost-effective production of metal-polymer composites with enhanced properties.
Patent Information
- Application Number
- JP2021532539
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2018-08-16
- Filing Date
- 2019-08-16
- Publication Date
- 2024-09-17
- Estimated Expiration
- 2039-08-16
AI Technical Summary
Conventional methods for bonding polymers to metals, such as steel, face challenges due to differences in chemical and physical properties, requiring surface preparation, volatile organic compounds, and high energy consumption, and often involve expensive and time-consuming processes under inert atmospheres.
A method involving the use of activated metal surfaces to initiate polymerization of polymerizable monomers directly on the metal surface, eliminating the need for external initiators and solvents, and allowing for the formation of metal-polymer composites through direct attachment.
This approach enables efficient and cost-effective production of metal-polymer composites with high bonding strength, reducing environmental hazards and energy consumption while providing lightweight, durable materials with excellent insulation and soundproofing properties.
Smart Images

Figure 0007551133000081 
Figure 0007551133000101 
Figure 0007551133000073
Abstract
Description
[Technical field]
[0001] The present invention relates to methods of making polymers and metal-polymer composites. The present invention also relates to polymer and metal-polymer composites, including those made by the methods described above. [Background technology]
[0002] Metal-polymer composites, such as steel-polymer composites, are widely used in the automotive, construction, thermal insulation, acoustic insulation, marine, and appliance industries due to their high strength-to-weight ratio, high impact resistance, excellent corrosion resistance, and / or design flexibility.
[0003] Bonding polymers to metals such as steel can be difficult due to differences in the chemical and physical properties of metals and polymers. Traditional joining techniques (i.e., adhesive bonding, mechanical fastening, welding, and injection molding) used for metal-polymer composites such as steel-polymer composites have several drawbacks, including the need for surface treatment, emission of volatile organic compounds, generation of stress concentrations, high energy consumption, limited bonding area, and / or the need for specific types of polymers.
[0004] Traditionally, polymers have been prepared in the presence of a catalyst, which typically requires an inert atmosphere. This type of system can be expensive and time consuming to implement. Traditional polymerizations also typically require organic solvents, which can raise health and safety concerns due to their toxicity and volatility.
[0005] There continues to be a need for other polymerization methods and other methods for preparing metal-polymer composites, such as steel-polymer composites. Summary of the Invention [Problem to be solved by the invention]
[0006] It is an object of the present invention to at least in some way meet this need; and / or at least provide the public and / or industry with a useful option. Other objects of the present invention will become apparent from the following description which is given by way of example only.
[0007] Where references are made herein to external sources, including patents and other documents, this is generally for the purpose of providing a context for discussing features of the present invention. Unless otherwise expressly stated, the references to such sources should not be construed as an admission that such sources are prior art in any jurisdiction or as forming part of the common general knowledge in the art.
[0008] Any documents referenced herein, including, but not limited to, patents, patent applications, journal articles, books, and the like, are hereby incorporated by reference in their entirety. All section headings used herein are for organizational purposes only and should not be construed as limiting the subject matter described. [Means for solving the problem]
[0009] In a first aspect, the present invention provides a method for producing a polymer comprising: providing one or more polymerizable monomers; providing a substrate comprising an activated metal surface, the activated metal surface comprising one or more compounds capable of initiating polymerization of one or more polymerizable monomers; contacting the activated metal surface with one or more polymerizable monomers to polymerize the one or more polymerizable monomers, thereby producing a polymer; The present invention relates to a method comprising the steps of:
[0010] In another aspect, the present invention relates to a method for preparing a metal-polymer composite, comprising the steps described in the first aspect. In another aspect, the invention relates to a polymer prepared by the method of the invention.
[0011] In another aspect, the present invention relates to a metal-polymer composite prepared by the method of the present invention. In another aspect, the invention relates to a polymer formed by polymerizing one or more polymerizable monomers.
[0012] In another aspect, the invention relates to a metal-polymer composite comprising a polymer directly attached to the metal surface of a substrate. In another aspect, the present invention relates to a metal-polymer composite having a peel strength of about 1.5 to about 5 MPa, preferably about 2.5 to about 5 MPa.
[0013] The embodiments described below may relate to only one of the above aspects, or to any combination of two or more of them. In some embodiments, the activated metal surface, when contacted with an aqueous solution of 30.096 μM terephthalic acid and 0.001 mol / L NaOH and irradiated with 365 nm light from a 15 W light source for 1 hour at room temperature, exhibits a concentration of 2-hydroxyterephthalic acid of at least 0.0001, 0.0002, 0.0003, 0.0004, 0.0005, 0.0006, 0.0007, 0.0009, 0.100, 0.200, 0.300, 0.400, 0.500, 0.600, 0.700, 0.800, 0.900, 1000, 1100, 1200, 1300, 1400, 1500, 1600, 1700, 1800, 1900, 2000, 21000, 2200, 2300, 2400, 2500, 2600, 2700, 2800, 2900, 3000, 3100, 3200, 3300, 3400, 3500, 3650, 3700, 3800, 3900, 4000, 4100, 4250, 4300, 4400, 4500, 4600, 4700, 4800, 4900, 5000, 5100, 5200, 5300, 5400, 5500, 5600, 5700, 5800 0.08, 0.0009, 0.001, 0.0015, 0.002, 0.0025, 0.003, 0.0035, 0.004, 0.0045, 0.005, 0.0055, 0.006, 0.0065, 0.007, 0.0075, 0.008, 0.0085, 0.009, 0.0095, 0.01, 0.0105, 0.011, 0.0115, 0.012, 0.0125, or 0.013 μM / mm of geometric area of activated surface 2and useful ranges can be selected from any of these values, for example, 0.0001 to 0.013, preferably at least 0.0001, preferably at least 0.0005, preferably at least 0.001, preferably at least 0.005, preferably at least 0.01 μM / mm 2 Geometric area of activated surface (μmolL -1 / mm 2 ).
[0014] In some embodiments, the activated metal surface, when tested according to the procedure described in Example 1.7, produces 2-hydroxyterephthalic acid at concentrations as defined in the previous embodiment.
[0015] In some embodiments, the activated surface can be produced by treating a metal surface of a substrate comprising a metal surface; or the method of the present invention further comprises providing a substrate comprising a metal surface and producing the activated metal surface by treating the substrate comprising a metal surface.
[0016] In some embodiments, the activated surface can be generated during formation of the substrate, for example, by forming the substrate at an elevated temperature. In some embodiments, the methods of the present invention may be for producing a metal-polymer composite by polymerizing one or more polymerizable monomers onto and / or at an activated metal surface to produce a metal-polymer composite.
[0017] In some embodiments, the polymer may be attached directly to the metal surface of the substrate. In some embodiments, the polymer can form a coating on a substrate surface.
[0018] In some embodiments, the activated metal surface can include one or more metal oxides capable of generating hydroxyl radicals. In some embodiments, the metal oxide may be selected from the group consisting of magnesium oxide, lead oxide, zinc oxide, copper oxide, titanium dioxide, silver oxide, tin oxide, aluminum oxide, cadmium oxide, iron oxide, and nickel oxide, or a combination of any two or more thereof.
[0019] In some embodiments, the metal oxide may be selected from the group consisting of lead oxide, zinc oxide, copper oxide, titanium dioxide, silver oxide, tin oxide, aluminum oxide, cadmium oxide, iron oxide, and nickel oxide, or a combination of any two or more thereof.
[0020] In some embodiments, the metal oxide can be selected from the group consisting of zinc oxide, titanium oxide, and aluminum oxide, or a combination of any two or more thereof. In some embodiments, the metal oxide can be zinc oxide or titanium oxide, or a combination thereof.
[0021] In some embodiments, the metal oxide can be zinc oxide. In some embodiments, the metal oxide can be selected from magnesium oxide, copper oxide, zinc oxide, titanium oxide, and aluminum oxide, or a combination of any two or more thereof.
[0022] In some embodiments, the metal surface can include one or more metals, the oxides of which are capable of generating hydroxyl radicals. In some embodiments, the metal surface can include magnesium, zinc, titanium, aluminum, lead, copper, titanium, silver, tin, cadmium, iron, or nickel, or a combination of any two or more thereof.
[0023] In some embodiments, the metal surface can include zinc, titanium, aluminum, lead, copper, titanium, silver, tin, cadmium, iron, or nickel, or a combination of any two or more thereof.
[0024] In some embodiments, the metal surface may comprise zinc, titanium, or aluminum, or a combination of any two or more thereof. In some embodiments, the metal surface may include zinc or titanium, or a combination thereof.
[0025] In some embodiments, the metal surface may include zinc. In some embodiments, the metal surface can include magnesium, copper, zinc, titanium, or aluminum, or a combination of any two or more thereof.
[0026] In some embodiments, the activated metal surface is or comprises an anodized surface, including, for example, titanium, aluminum, and magnesium.
[0027] In some embodiments, the substrate comprising a metal surface is a substrate comprising a galvanized surface. In some embodiments, one or more metal oxides may be produced by treating the metal surface; alternatively, the methods of the present invention may include treating the metal surface to produce one or more metal oxides.
[0028] In some embodiments, the methods of the present invention can include contacting an activated metal surface and one or more polymerizable monomers and irradiating with light, preferably light including UV light.
[0029] In some embodiments, the polymerization can be carried out in the absence of an external or exogenous initiator. In some embodiments, the substrate can be a monolithic structure having at least one dimension greater than 100 nm, preferably greater than 1 mm.
[0030] In some embodiments, the metal surface and / or substrate can comprise, consist of, or consist essentially of galvanized steel, electrogalvanized steel, Galfan steel, zinc metal, aluminum metal, titanium metal, zinc-aluminum alloy coated steel (referred to herein as zincalume), zinc-magnesium coated steel, or zinc-aluminum-magnesium coated steel, or a combination of any two or more thereof.
[0031] In some embodiments, the metal surface and / or substrate can include, consist of, or consist essentially of galvanized steel. In some embodiments, the metal surface and / or substrate may comprise, consist of, or consist essentially of hot-dip galvanized steel.
[0032] In some embodiments, the substrate can be selected from the group consisting of particles, fibers, sheets, blocks, wires, mesh, panels, slabs, plates, poles, columns, rods, round bars, beams, foil, joists, laminates, barrier fences, pipes, chains, fabrics, roofing materials, coatings, or any combination of two or more thereof.
[0033] In some embodiments, treating the metal surface to produce an activated surface can include one or more of heating the metal surface at an elevated temperature (e.g., in an oven, with a laser, or by other suitable methods), passing an electric current through the metal surface (e.g., an anodization step), subjecting the metal surface to a chemical treatment (e.g., a treatment to produce hydroxyl groups on the metal surface, an alkaline treatment (e.g., an alkali metal hydroxide treatment), or an acid treatment), subjecting the metal surface to a plasma treatment (e.g., an oxygen plasma treatment), or exposing the metal surface to UV light.
[0034] In some embodiments, treating the metal surface can include heating the metal surface at an elevated temperature to produce an activated metal surface. In some embodiments, the metal surface is heated by a laser or other heat source capable of rapidly heating the metal surface, such as a plasma.
[0035] In some embodiments, the one or more monomers can be contacted with the activated surface immediately after the activated surface is generated, for example by spraying. In some embodiments, heating the metal surface can include heating to a temperature of at least about 100°C to about 600°C, preferably at least about 300°C to about 600°C, and more preferably at least about 300°C to about 400°C.
[0036] In some embodiments, heating the metal surface can include heating for at least about 1, 2, 3, 4, 5, 6, 7, 8, 9, 10 hours, or more, such as from about 1 to about 10 hours, preferably at least about 1 hour, and more preferably at least about 2 hours.
[0037] In some embodiments, the activated metal surface can be contacted with one or more polymerizable monomers within less than about 72, 48, 24, 12, 6, 5, 4, 3, 2, or 1 hours after formation, preferably within less than about 72 hours, preferably within less than about 24 hours, and more preferably within about 2 hours.
[0038] In some embodiments, the activated metal surface may be cooled prior to contacting with the one or more polymerizable monomers, preferably to a temperature below the boiling point at atmospheric pressure of the one or more polymerizable monomers.
[0039] In some embodiments, the activated surface can be generated when the substrate is formed. In some embodiments, one or more of the polymerizable monomers can be photoactive monomers.
[0040] In some embodiments, the one or more polymerizable monomers can be monoolefinically unsaturated monomers, preferably monoethylenically unsaturated monomers; or polyolefinically, preferably diolefinically unsaturated monomers, preferably polyethylenically unsaturated monomers; preferably diethylenically unsaturated monomers.
[0041] In some embodiments, one or more of the polymerizable monomers can be unsaturated, preferably olefinically unsaturated, preferably ethylenically unsaturated. In some embodiments, the one or more polymerizable monomers can be selected from the group consisting of vinyl monomers, preferably acrylic acid esters or methacrylic acid esters.
[0042] In some embodiments, the one or more polymerizable monomers have Formula I:
[0043] [ka]
[0044] (In the formula, R 1 is C(O)OR 3 , CO(O)R 4 , aryl, or NR 20 ;R 2 is H or C1-4 alkyl, preferably H or CH3; R 3 is C1-10 alkyl or (CH2CH2O) n CH3, preferably C1-4 alkyl; R 4 is C1-10 alkyl, preferably C1-4 alkyl; n is an integer selected from 1 to 20; R 20 may be a monomer of H or an alkyl group, preferably H or C1-10 alkyl, preferably H).
[0045] In some embodiments, the one or more polymerizable monomers have Formula II:
[0046] [ka]
[0047] (In the formula, X is independently O or NR 20 and; R 20 is H or an alkyl group, preferably H or a C1-10 alkyl group, preferably H; R 5 and R 6 are each independently H or C1-5 alkyl, preferably H or CH3; Y is preferably a linking group that may include a linear chain having at least 2, 5, 10, 15, 20, 25, 30, 35, 40, 45, 50, 55, 60, 65, 70, 75, 80, 85, 90, 95, 100, or more atoms selected from C, N, O, and S).
[0048] In some embodiments, the linking group has the formula (CR 30 R 40 ) q or formula (CR 50 R 60 O) r (CR 70 R 80 ) group, where R 30 , R 40 , R 50 , R 60 , R 70 , and R 80 are each independently H or alkyl, preferably C1-10 alkyl, and q and r are each independently an integer from 1 to 40.
[0049] In some embodiments, Y is (CH) m , CH2CH2CH(CH3), (CH2CH2O) p (CH2CH2), and formula IIA:
[0050] [ka]
[0051] (In the formula, m and p each independently represent an integer of 1 to 40, preferably about 1 to about 10; R 7 , R 8 , R 9 , and R 10 are each independently selected from H and C1-5 alkyl.
[0052] In some embodiments, the one or more polymerizable monomers have Formula III:
[0053] [ka]
[0054] (In the formula, R 11 and R 12 are each independently H or:
[0055] [ka]
[0056] and R 5 is as defined herein). In some embodiments, each X can be O. In some embodiments, one or more polymerizable monomers can be a monomer of formula II having a linking group of formula IIA.
[0057] In some embodiments, R 5 and R 6 may both be methyl. In some embodiments, R 7 and R 9can both be methyl, R 8 and R 10 are each independently selected from the group consisting of H and CH3, preferably R 8 and R 10 One of them is H and R 8 and R 10 The other is CH3, and preferably, R 7 and R 9 are both methyl, and R 8 and R 10 exists as a 1:1 mixture of H and CH3.
[0058] In some embodiments, the one or more polymerizable monomers may be selected from the group consisting of methyl acrylate, methyl methacrylate, butyl methacrylate, diurethane dimethacrylate, poly(ethylene glycol) methyl ether methacrylate, butyl acrylate, styrene, and vinyl acetate.
[0059] In some embodiments, the one or more polymerizable monomers can be diurethane dimethacrylate, CAS number 72869-86-4. In some embodiments, the activated metal surface can be contacted with one or more different types of polymerizable monomers.
[0060] In some embodiments, the activated metal surface can be contacted with one or more polymerizable monomers for a first period of time followed by a second period of time. In some embodiments, the methods of the present invention can include contacting an activated metal surface and one or more polymerizable monomers and irradiating with light having a wavelength of about 10, 50, 100, 150, 200, 250, 300, 350, 400, 450, 500, 550, 600, 650, 700, 750, 800, 850, 900, 950, 1000, 1050, 1100, 1150, 1200, 1250 nm or greater, with useful ranges being any of these. The optical fiber length can be selected from the following values, for example, about 10 to 400, 50 to 400, 100 to 400, 150 to 400, 200 to 400, 10 to 700, 50 to 700, 100 to 700, 150 to 700, 200 to 700, 300 to 700, 400 to 700, 10 to 1000, 50 to 1000, 100 to 1000, 150 to 1000, 200 to 1000, 300 to 1000, 400 to 1000, 500 to 1000, 600 to 1000, or 700 to 1000 nm.
[0061] In some embodiments, the light comprises, consists essentially of, or consists of light at a wavelength that optimizes the generation of hydroxyl radicals and / or electrons by one or more compounds capable of initiating polymerization at the activated surface.
[0062] In some embodiments, the power of the light can be at least about 1, 1.5, 2, 2.5, 3, 3.5, 4, 4.5, 5, 5.5, 6, 6.5, 7, 7.5, 8, 8.5, 9, 9.5, 10, 10.5, 11, 11.5, 12, 12.5, 13, 13.5, 14, 14.5, 15, 15.5, 16, 16.5, 17, 17.5, 18, 18.5, 19, 19.5, 20, 25, 30, 35, 40, 45, 50, 55, 60, 65, 70, 75, 80, 85, 90, 95, 100, 105, 110, 115, 120, 125, 130 W.
[0063] In some embodiments, the intensity of the light is determined by the amount of light emitted from the activated surface (m 2 ) is at least 1, 2, 3, 4, 5, 6, 7, 8, 9, or 10 W per In some embodiments, the activated metal surface can be contacted with one or more polymerizable monomers for a first period of time followed by a second period of time characterized by different temperature and / or irradiation.
[0064] In some embodiments, the activated metal surface may be contacted with one or more polymerizable monomers at a first temperature for a first period of time and at a second temperature for a second period of time, where the first temperature is different from the second temperature, preferably the first temperature is higher than the second temperature, and preferably the second temperature is higher than the first temperature.
[0065] In some embodiments, contacting the activated metal surface with the one or more polymerizable monomers can be performed under irradiation with light for only a first period of time. In some embodiments, the activated metal surface can be contacted with one or more polymerizable monomers for a first period of time at a temperature of at least about 10, 15, 20, 25, 30, 35, 40, 45, 50, 55, 60, 65, 70, 75, 80, or 85°C, with suitable ranges selected from any of these values, such as from about 10°C to about 85°C, more preferably from 50 to 85°C, more preferably from 20 to 50°C.
[0066] In some embodiments, the activated metal surface can be contacted with one or more polymerizable monomers for a second period of time at a temperature of at least about 10, 15, 20, 25, 30, 35, 40, 45, 50, 55, 60, 65, 70, 75, 80, or 85°C, with suitable ranges selected from any of these values, e.g., from about 10°C to about 85°C, from about 50 to about 85°C, preferably at least about 20°C, preferably at least about 50°C, preferably at least 85°C.
[0067] In some embodiments, the first period of time can be at least about 30 seconds, 1, 5, 10, 15, 30, or 60, 70, 80, 90, 100, 110, or 120 minutes, preferably from about 30 seconds to about 120 minutes, and more preferably from about 30 seconds to about 60 minutes.
[0068] In some embodiments, the second period of time can be less than about 72, 48, 36, 24, 12, 11, 10, 9, 8, 7, 6, 5, 4, 3, 2, or 1 hour, preferably less than about 5 hours, and more preferably less than about 1 hour.
[0069] In some embodiments, the number average molecular weight of the polymer is at least about 500,000, 550,000, 600,000, 650,000, 700,000, 750,000, 800,000, 850,000, 900,000, 950,000, 1,000,000, 1,050,000, 1,100,000, 1,150,000, 1,200,000, 1,250,00, 1,500,000, 2,000,000, 3,000,000, 4,000,000, or 5,000,000 g / mol, and useful ranges can be selected from any of these values, for example, from about 500,000 to about 5,000,000 g / mol.
[0070] In some embodiments, the number average molecular weight of the polymer is at least about 2,000, 10,000, 50,000, 100,000, 150,000, 200,000, 250,000, 300,000, 350,000, 400,000, 450,000, 500,000, 550,000, 600,000, 650,000, 700,000, 750 The molecular weight may be 2,000, 800,000, 850,000, 900,000, 950,000, 1,000,000, 1,050,000, 1,100,000, 1,150,000, or 1,200,000 g / mol, and a useful range may be selected from any of these values, for example, from about 2,000 to about 1,200,000 g / mol.
[0071] In some embodiments, the polydispersity index of the polymer is at least about 1, 1.05, 1.1, 1.15, 1.2, 1.25, 1.3, 1.35, 1.4, 1.45, 1.5, 1.55, 1.6, 1.65, 17, 1.75, 1.8, 1.85, 1.9, 1.95, 2, 2.05, 2.1, 2.15, 2.2, 2.25, 2.3, 2.35, 2.4, 2.45, 2.5, 2.55, 2.6, 2.65, 2.7, 2.75, 2.8, 2.95, 2.9, 2.95, 3, 3.05, 3.1, 3.15, 3.2, 3.25, 3.3, 3.35, 3.4, 3.45, The molecular weight may be 3.5, 3.55, 3.6, 3.65, 3.7, 3.75, 3.8, 3.85, 3.9, 3.95, 4, 4.05, 4.1, 4.15, 4.2, 4.25, 4.3, 4.35, 4.4, 4.45, 4.5, 4.5, 4.55, 4.6, 4.65, 4.7, 4.75, 4.8, 4.85, 4.9, 4.95, or 5, and useful ranges may be selected from any of these values, for example, about, preferably at least about 1.05 to about 2.5, preferably at least about 1.05 to about 1.5, and more preferably at least about 1.05 to about 1.2.
[0072] In various embodiments, the metal polymer composite has a tape test rating of at least 2B, preferably 3B, preferably 4B as measured by AST D3359.
[0073] In some embodiments, the metal-polymer composite has a peel strength as measured by ASTM D4541-09 of about 1.5, 1.6, 1.7, 1.8, 1.9, 2.0, 2.1, 2.2, 2.3, 2.4, 2.5, 2.6, 2.7, 2.8, 2.9, 3.0, 3.1, 3.2, 3.3, 3.4, 3.5, 3.6, 3.7, 3.8, 3.9, 4, 4.1, 4.2, 4.3, 4.4, 4.5, 4.6, and greater than 4.7, 4.8, 4.9, 5, 5.5, 6, 6.5, 7, 7.5, 8, 8.5, 9, 9.5, or 10 MPa, and useful ranges can be selected from any of these values, for example, about 1.5 to 10, 2.5 to 10, 1.5 to 7.5, 2.5 to 7.5, 1.5 to 5, or 1.5 to 4 MPa, preferably about 2.5 to about 5 MPa.
[0074] In some embodiments, the direct attachment can comprise, consist of, or consist essentially of a non-covalent bond between the polymer and the metal surface, hi some embodiments, the non-covalent bond comprises, consists of, or consists essentially of a hydrogen bond.
[0075] In some embodiments, the one or more polymerizable monomers can be photochemically polymerized. In some embodiments, the one or more polymerizable monomers can be polymerized in the absence of an electric current, an applied voltage, or an externally applied potential difference.
[0076] In some embodiments, the one or more polymerizable monomers may be polymerized in a liquid medium comprising less than 90, 85, 80, 75, 70, 65, 60, 55, 50, 45, 40, 35, 30, 25, 20, 15, 10, 5, 4, 3, 2, or 1 vol.% solvent, preferably less than 90 vol.%, preferably less than 50 vol.%, preferably less than 10 vol.% solvent, preferably the one or more polymerizable monomers are polymerized in the absence of solvent.
[0077] In some embodiments, the one or more polymerizable monomers may be polymerized in air and / or in the presence of air or other oxygen-containing atmosphere. In some embodiments, the metal surface may be subjected to one or more pre-treatment steps, such as one or more physical, mechanical and / or chemical treatments, such as plasma treatment or surface roughening, such as surface roughening by etching and / or patterning, prior to undergoing the treatment to produce the activated metal surface.
[0078] In some embodiments, the metal surface is subjected to a pretreatment step, such as a surface roughening step, that increases the surface area of the metal surface. In some embodiments, the metal surface is subjected to a pretreatment step, e.g., a plasma, laser, chemical, or other pretreatment step, that increases the wettability and / or free energy of the surface and / or modifies the morphology of the surface to enhance bonding (e.g., mechanical bonding) between the polymer and the surface.
[0079] Other aspects of the present invention will become apparent from the following description, given by way of example only, and with reference to the accompanying drawings. Reference to a numerical range disclosed herein (e.g., 1-10) is intended to encompass reference to every rational number within that range (e.g., 1, 1.1, 2, 3, 3.9, 4, 5, 6, 6.5, 7, 8, 9, and 10), as well as any range of rational numbers within that range (e.g., 2-8, 1.5-5.5, and 3.1-4.7), and therefore, every subrange of every range explicitly disclosed herein is also expressly disclosed thereby. These are merely examples of what is specifically intended, and all possible combinations of numerical values between the minimum and maximum values recited are also considered to be expressly set forth in this application.
[0080] The present invention may also be broadly described as consisting of the parts, components, and features referred to or indicated in the specification of this application, either individually or collectively, and any combination of any two or more of said parts, components, or features, and where a specific whole having known equivalents in the art to which the invention pertains is described in this specification, such known equivalents are also deemed to be incorporated in this specification as if they were individually set forth.
[0081] The invention will now be described, by way of example only, with reference to the drawings in which: [Brief description of the drawings]
[0082] [Figure 1] Graph showing thermogravimetric analysis / derivative thermogravimetric (TGA / DTG) curves of basic zinc carbonate powder when heated in air at a rate of 10° C. per minute. (Weight is plotted against the right y-axis and is expressed as the percentage of weight loss at a particular temperature. Derivative weight is plotted against the left y-axis and represents the differential weight loss. Differential weight loss corresponds to the percentage of weight loss as a function of temperature. Temperature is represented in degrees Celsius (° C.) on the x-axis.) [Diagram 2] X-ray diffraction patterns of basic zinc carbonate powder that was not annealed (bottom curve) and basic zinc carbonate powders that were annealed at different heat treatment temperatures of 100, 200, 300, and 400 °C (from the bottom curve to the second top curve, respectively) (markers in the shape of ◆, ▽, and ◇ are used to indicate signals corresponding to specific chemical species, where ◆ represents the peak corresponding to ZnO, ▽ represents the peak corresponding to ZnCO3, and ◇ represents the peak corresponding to Zn5(CO3)2(OH)6. The y-axis of Figure 2 represents intensity in absorbance units (au) and the x-axis represents 2θ (°). [Figure 3a] XPS spectrum of C 1s of annealed ZnO powder for reference (the spectrum shows peaks at various binding energies (eV) and signals (peaks) corresponding to specific chemical species are identified in each figure). [Figure 3b] X-ray photoelectron spectroscopy (XPS) spectrum of O 1s of annealed ZnO powder for reference (the spectrum shows peaks at various binding energies (eV) and signals (peaks) corresponding to specific chemical species are identified in each figure). [Figure 3c] X-ray photoelectron spectroscopy (XPS) spectrum of Zn 2p3 / 2 from annealed ZnO powder for reference (the spectrum shows peaks at various binding energies (eV) and signals (peaks) corresponding to specific chemical species are identified in each figure). [Figure 3d] X-ray photoelectron spectroscopy (XPS) spectrum of annealed ZnO powder Zn L3M45M45 for reference (the spectrum shows peaks at various binding energies (eV) and signals (peaks) corresponding to specific chemical species are identified in each figure). [Figure 4a] C 1s spectrum of basic zinc carbonate powder for reference (signals corresponding to specific chemical species are identified. The spectrum shows peaks at various binding energies (eV) and signals (peaks) corresponding to specific chemical species are identified). [Figure 4b] Reference O 1s spectrum of basic zinc carbonate powder (signals corresponding to specific chemical species are identified. The spectrum shows peaks at various binding energies (eV) and signals (peaks) corresponding to specific chemical species are identified). [Figure 4c] Spectrum of Zn 2p3 / 2 of basic zinc carbonate powder for reference (signals corresponding to specific chemical species are identified. The spectrum shows peaks at various binding energies (eV), and signals (peaks) corresponding to specific chemical species are identified). [Figure 4d] Spectrum of basic zinc carbonate powder Zn L3M45M45 (Figure 4(d)) for reference (signals corresponding to specific chemical species are identified. The spectrum shows peaks at various binding energies (eV), and signals (peaks) corresponding to specific chemical species are identified). [Diagram 5]XPS spectra obtained from (a) untreated galvanized steel (UTGS), (b) heat-treated galvanized steel heat-treated at 400 °C (TTGS(400)), and (c) heat-treated galvanized steel heat-treated at 600 °C (TTGS(600)). The spectra show peaks at various binding energies (eV) and signals (peaks) corresponding to specific chemical species are identified in each spectrum. [Figure 6] C 1s spectra obtained from (a) UTGS, (b) TTGS(400), and (c) TTGS(600). The spectra show peaks at various binding energies (eV), and signals (peaks) corresponding to specific chemical species are identified in each spectrum. [Figure 7] O 1s spectra obtained from (a) UTGS, (b) TTGS(400), and (c) TTGS(600). The spectra show peaks at various binding energies (eV), and signals (peaks) corresponding to specific chemical species are identified in each spectrum. [Figure 8] Zn 2p3 / 2 spectra acquired from (a) UTGS, (b) TTGS(400), and (c) TTGS(600). [Figure 9] Zn L3M45M45 spectra obtained from (a) UTGS, (b) TTGS(400), and (c) TTGS(600). [Figure 10] Scanning electron microscope (SEM) secondary electron images (SEI) of (a) UTGS, (b) TTGS(400), and (c) TTGS(600) (scale bars in each of these figures correspond to 100 μm). [Figure 11] (a) SEI of a small hole on the UTGS surface (scale bar is 2 μm) and (a1) SEI of a small hole further enlarged (scale bar is 500 nm), and (b) SEI of a small hole on the UTGS surface and (b1) SEI of a small hole further enlarged. [Figure 12](a) SEI of a small hole on the TTGS(400) surface and (a1) SEI of the small hole further enlarged, (b) SEI of the TTGS(400) surface of the substrate (scale bar corresponds to 2 μm) and (bl) SEI of the substrate further enlarged (scale bar corresponds to 500 nm). [Figure 13] (a) SEI of a small hole on the surface of TTGS(600) (scale bar corresponds to 2 μm) and (a1) SEI of a small hole further enlarged (scale bar corresponds to 500 nm), (b) SEI of a small hole on the surface of TTGS(600) and (bl) SEI of a small hole further enlarged, and (c) SEI of a small hole on the surface of TTGS(600) and (c1) SEI of a small hole further enlarged. [Figure 14] SEM backscattered electron images (BSE) of (a) UTGS, (b) TTGS(400), and (c) TTGS(600). [Figure 15] Graph showing the production of 2-hydroxyterephthalic acid (TAOH) from terephthalic acid (TA) measured by fluorescence spectroscopy after 1 hour of UV irradiation in the presence and absence of UTGS, TTGS(400), and TTGS(600), plotted as a function of the fluorescence intensity of the signal at each wavelength (nm) in absorbance units (au). In the legend, from the top, TA (dotted line): the spectrum obtained from the control sample terephthalic acid (TA) (TA in the absence of UTGS, TTGS(400), and TTGS(600)) is shown at the bottom curve, TA+UV (solid line): the spectrum of TA obtained in the presence of ultraviolet (UV) light only, TA+UV+UTGS (dash-dotted line): the spectrum of TA obtained in the presence of UV and UTGS, TA+UV+TTGS(400) (dashed line): the spectrum of TA obtained in the presence of UV and TTGS(400), and TA+UV+TTGS(600) (dash-dotted line): the spectrum of TA obtained in the presence of UV and TTGS(600). [Figure 16] Graph showing the calibration curve of fluorescence intensity in absorbance units (au) at various TAOH concentrations (μM) (the equation constructed from the measured points on the curve was: y=10.19643+120.297x+9.453x2, resulting in an R2 value of 0.994). [Figure 17]Kinetic plot versus time showing the rate of monomer consumption (i.e., the rate of conversion of polymerizable monomers to the corresponding polymer) as a function of reaction time for the polymerization reaction of methyl methacrylate (MMA) using TTGS(600) as initiator (y-axis corresponds to ln([M0] / [Mt]) determined as described herein and x-axis corresponds to time in hours (h)). [Figure 18] Plot of molecular weight (solid symbols ▲) and polydispersity index (PDI) (open symbols △) of polymers obtained from the polymerization reaction of MMA using TTGS(600) as initiator (monomer conversion (i.e., the percentage of the total amount of polymerizable monomers that is converted into the corresponding polymer) is taken on the x-axis, molecular weight (Mn) expressed as Mn / 104 is taken on the left y-axis, and PDI is taken on the right y-axis). [Figure 19A] Photograph of a block copolymer of MMA and butyl methacrylate (BMA) obtained according to an embodiment of the method described herein (showing a layer of poly(methyl methacrylate) (PMMA) (first layer) formed on a TTGS(600) surface, on which a second PMMA layer is visible. To facilitate identification of the different blocks, red-brown and green dyes were added to the different monomers, producing light and dark layers). [Figure 19B] Photograph of a block copolymer of MMA and butyl methacrylate (BMA) obtained according to an embodiment of the method described herein (showing a PMMA layer (first layer) formed on a TTGS(600) surface, on top of which is a second layer (PBMA copolymer of butyl methacrylate and methyl methacrylate). To facilitate identification of the different blocks, red-brown and green dyes were added to the different monomers, resulting in light and dark layers). [Figure 20]Graph showing the formation of TAOH from TA when irradiated with UV light for 1 hour in the presence and absence of untreated zinc-aluminum alloy coated steel (herein referred to as zincalum) as defined herein (UTZnAl), UTGS, heat treated zincalum heat treated at 600°C (TTZnAl(600)), and heat treated galvanized steel heat treated at 600°C (TTGS(600)), as measured by fluorescence spectroscopy. In the legend, from top to bottom, (the bottom curve on the graph) TA (dashed line): the spectrum obtained for the control sample TA (TA in the absence of light (UV), UTGS, UTZnAl, TTGS, and TTZnAl), TA+UV (short dotted line): TA in the presence of various wavelengths of light (nm) (in the absence of UTGS, UTZnAl, TTGS, and TTZnAl), TA+UTZnAl (short dashed line): TA in the presence of light (UV) and UTZnAl, TA+UTGS (solid line): TA in the presence of light (UV) and UTGS, TA+TTZnAl (jump dotted line): TA in the presence of light (UV) and TTZnAl (600), (the top curve on the graph) TA+TTGS (long dashed line): TA in the presence of light (UV) and TTGS (600). [Figure 21] Figure 1 shows a kinetic plot of monomer consumption (i.e., conversion of polymerizable monomer to corresponding polymer) as a function of reaction time for the polymerization reaction of MMA using heat-treated galvanized steel (TTGS(600)) heat treated at 600°C (dotted line) and heat-treated zincalan (TTZnAl) heat treated at 600°C (solid line). The y-axis corresponds to ln([M0] / [Mt]) determined as described herein and the x-axis corresponds to time in hours (h). [Figure 22]1 is a plot of the molecular weight (solid symbols) and polydispersity index (PDI) (open symbols) of the polymers obtained by polymerization of MMA using heat-treated galvanized steel (TTGS(600)) heat-treated at 600°C (represented by filled and open triangles) and heat-treated zincalan (TTZnAl(600)) heat-treated at 600°C (represented by filled and open squares). The monomer conversion (i.e., the percentage of the total amount of polymerizable monomers that is converted to the corresponding polymer) is plotted on the x-axis, the molecular weight (Mn) in Mn / 104 is plotted on the left y-axis, and the PDI is plotted on the right y-axis. [Figure 23] A graph showing the effect of UV light of different power (6 W is represented by the dotted line and 15 W is represented by the solid line) on the amount of TAOH produced from TA, measured as fluorescence intensity (intensity is measured in absorbance units (au) at a wavelength of 425 nm). [Figure 24] A graph showing the effect of time on the amount of TAOH produced from TA when a mixture containing TA is irradiated with 15 W UV light for varying times (from 0 minutes to 60 minutes) (showing the change in fluorescence intensity expressed in absorbance units (au) recorded at a wavelength of 425 nm). In the legend, from top to bottom, dotted line (bottom curve on graph): 0 minutes, solid line: 10 minutes, long dashed line: 20 minutes, dashed line: 30 minutes, short dashed line: 40 minutes, dashed line: 50 minutes, jump dotted line: 60 minutes (top curve on graph). [Diagram 25] FIG. 13 is a graph showing the amount of TAOH produced (μM) as a function of irradiation time (min) using 15 W UV light in the presence of heat-treated galvanized steel (heat-treated at 600 °C) (TTGS(600)). [Figure 26] Kinetic plot showing the monomer consumption rate (i.e., conversion rate of polymerizable monomer to the corresponding polymer) as a function of reaction time for the polymerization reaction of MMA in the presence of TTGS(600) under UV irradiation at 15 W (dashed line) and 6 W (solid line). (The y-axis corresponds to ln([M0] / [Mt]) as described herein and the x-axis corresponds to time in hours (h)). [Figure 27]1 is a kinetic plot showing the monomer consumption rate (i.e., the conversion rate of polymerizable monomers to the corresponding polymer) as a function of reaction time in the polymerization of MMA using TTGS(600) with 15 W UV light for 60 min (dashed line), 50 min (solid line), 40 min (dash-dotted line), and 30 min (dotted line). The y-axis corresponds to ln([M0] / [Mt]) as described herein, and the x-axis corresponds to time in hours (h). [Figure 28] 1 is a kinetic plot showing the monomer consumption rate (i.e., the conversion of polymerizable monomers to the corresponding polymer) as a function of reaction time for the polymerization of MMA using TTGS(600) at different polymerization temperatures: 80° C. (dashed line) and 60° C. (solid line). The y-axis corresponds to ln([M0] / [Mt]) as described herein and the x-axis corresponds to time in hours (h). DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0083] The word "comprising" as used in this specification and the claims means "consisting at least in part of." In interpreting each statement in this specification and the claims containing the word "comprising," there may be features present other than the feature or features that the word precedes. Related words such as "comprise" and "comprises" should be interpreted in the same manner.
[0084] Unless otherwise specified, the singular forms "a," "an," and "the" include plural references. As used herein the term "and / or" means "and" or "or" or both.
[0085] As used herein, "(s)" following a noun refers to the plural and / or singular form of that noun. General chemical names used in the formulas herein have their usual meanings.
[0086] Unless otherwise specified, the nomenclature used to designate chemical groups or moieties used herein follows the convention that the name is read from left to right with the point of attachment to the remainder of the molecule located to the right of the name, e.g., an "arylalkyl" group is attached to the remainder of the molecule at the alkyl terminus.
[0087] The term "alkyl", alone or in combination with other terms, refers to straight or branched chain hydrocarbon groups, unless otherwise specified. In some embodiments, the alkyl group has 1 to 40 carbon atoms. In some embodiments, the alkyl group has 1 to 12, 1 to 10, 1 to 8, 1 to 6, or 1 to 4 carbon atoms. Examples of straight chain alkyl groups include, but are not limited to, methyl, ethyl, n-propyl, n-butyl, n-pentyl, n-hexyl, n-heptyl, and n-octyl. Examples of branched alkyl groups include, but are not limited to, isopropyl, iso-butyl, sec-butyl, tert-butyl, neopentyl, isopentyl, and 2,2-dimethylpropyl.
[0088] The term "aryl", as used herein alone or in combination with other terms, refers to a radical of a cyclic aromatic hydrocarbon group, unless otherwise specified. Aryl groups encompass monocyclic and bicyclic ring systems as well as heteroaryl ring systems. Aryl groups also encompass aromatic-cycloalkyl and aromatic-cycloalkenyl fused ring systems. Examples of aryl groups include, but are not limited to, phenyl, naphthyl, azulenyl, pentalenyl, indenyl, indanyl, dihydronaphthyl, tetrahydronaphthyl, and the like. In some embodiments, an aryl group contains 6 to 10 ring carbon atoms. Groups of this type are sometimes referred to herein as 6 to 10 membered aryl groups. In some embodiments, the aryl group is a phenyl group.
[0089] The term "polymerizable monomer," as used herein, unless otherwise specified, alone or in combination with other terms, refers to a monomer that is capable of combining or being combined to form a polymer.
[0090] As used herein in reference to metal-polymer composites, "direct attachment" and related terms such as "directly attached," either alone or in combination, means that the polymer of the metal-polymer composite is directly attached or bonded to the metal surface, with no intervening layer (e.g., adhesive layer), material, compound, or connecting moiety between the polymer and the metal surface. The direct bond can be mechanical and / or chemical (e.g., non-covalent and / or covalent) in nature.
[0091] As used herein, the term "copolymer" refers to a polymer that contains two or more, e.g., three or more, different monomer units, i.e., two or more monomer units having different structures. A copolymer of two different monomers is sometimes called a bipolymer, and a copolymer of three different monomers is sometimes called a terpolymer. The different monomer units may be randomly distributed throughout the polymer or may be in an ordered arrangement, e.g., in block form, depending on how the copolymer is formed.
[0092] As used herein, the term "unsaturated" as used herein refers to a monomer that contains at least one non-aromatic carbon-carbon double bond or carbon-carbon triple bond.
[0093] Conventional methods for polymerizing monomers to prepare metal-polymer composites typically require exogenous initiators, catalysts, organic solvents, and inert polymerization conditions, which can make conventional polymerization methods, as described herein, expensive to implement and subject to safety concerns, such as exposure of workers and the environment to toxic solvents, as well as the generation of polymerization by-products.
[0094] Surprisingly, the inventors have found that polymerization of monomers and preparation of metal-polymer composites can be carried out using metal surfaces activated as described herein in the absence of exogenous initiators, catalysts, and / or solvents.
[0095] In various embodiments, the one or more polymerizable monomers polymerize in the absence of an electric current, an applied voltage, or an externally applied potential difference. In various embodiments, the one or more polymerizable monomers are polymerized in the absence of an external or exogenous initiator, such as one or more conventional initiators, such as azobisisobutyronitrile (AIBN).
[0096] In various embodiments, the polymerizable monomer or monomers can be polymerized in air and / or in the presence of air or other oxygen-containing atmosphere. In various embodiments, the one or more polymerizable monomers are polymerized in a liquid medium that contains less than 90, 85, 80, 75, 70, 65, 60, 55, 50, 45, 40, 35, 30, 25, 20, 15, 10, 5, 4, 3, 2, or 1% by volume of a solvent, useful ranges can be selected from any of these values, for example, less than 90%, less than 50%, or less than 10% by volume, and most preferably, the one or more polymerizable monomers are polymerized in the absence of a solvent.
[0097] In various embodiments, metal-polymer composites prepared by the methods described herein may have advantages such as light weight, durability, higher bond strength, better thermal and acoustic insulation, and / or better weather resistance compared to conventional metal-polymer composites prepared by adhesive bonding.
[0098] Thus, the present invention relates to polymers, metal-polymer composites, and methods for producing polymers and metal-polymer composites. In particular, the present invention relates to a method for producing a polymer, comprising: Providing one or more polymerizable monomers; Providing a substrate comprising an activated metal surface, the activated metal surface comprises one or more compounds capable of initiating polymerization of one or more polymerizable monomers; contacting the activated metal surface with one or more polymerizable monomers to polymerize the one or more polymerizable monomers, thereby producing a polymer; The present invention relates to a method comprising the steps of:
[0099] Any substrate known in the art can be used in the present invention, provided that the substrate comprises an activated metal surface. Additionally, substrates of any dimensions can be used in the methods described herein.
[0100] In various embodiments, the substrate can be a monolithic structure having at least one dimension (e.g., two or three or more dimensions) greater than about 100 nanometers, e.g., greater than about 0.1, 1, 10, 50, 100, 500, 600, 700, 800, 900, or 1,000, 5,000, 10,000, 100,000 μm, with useful ranges selected from any of these values, e.g., from about 0.1 μm to about 1,000 μm.
[0101] In some embodiments, the substrate may be in granular form, e.g., the substrate may be a powder. In various embodiments, the substrate may be non-granular, e.g., a fiber. In various embodiments, the substrate, e.g., the monolithic structure, comprises an activated surface, which can be produced by treating a metal surface of the substrate as described herein.
[0102] In various embodiments, the substrate can be a monolithic substrate. In various embodiments, the substrate can be, for example, a monolithic structure having a seamless surface and at least one dimension of greater than or equal to about 1, 5, 10, 20, 50, 100, 200, 300, 400, 500, 600, 700, 800, 900, 1000 mm, and useful ranges can be selected from any of these values, for example, about 1 to about 5, 1 to about 10, 1 to about 20, 1 to about 50, 1 to about 100, 1 to about 1000, 5 to about 1000, 10 to about 1000, 100 to about 1000, or 500 to about 1000 mm.
[0103] Those skilled in the art will appreciate that the substrate can be selected based on the intended use of the substrate. With this in mind, it will be apparent to those skilled in the art that substrates having a wide range of lengths, diameters, dimensions, and aspect ratios can be selected, and that all of these parameters will depend on the intended use of the substrate. For example, in some embodiments, the substrate can have at least one dimension that is greater than 0.5, 1, 2, 3, 4, 5, or 10 meters.
[0104] The substrate may comprise a metallic surface and / or an activated surface comprising a metal selected from the group consisting of magnesium, zinc, titanium, aluminum, lead, copper, titanium, silver, tin, cadmium, iron, or nickel, or a combination of any two or more thereof, preferably a metal selected from the group consisting of zinc, titanium, and aluminum, or a combination of any two or more thereof, more preferably the substrate comprises a metallic surface comprising, consisting of, or consisting essentially of zinc.
[0105] In some embodiments, the substrate may be a metallic substrate, or the substrate may include, for example, a non-metallic material having a metallic surface attached thereto. In some embodiments, the metal surface may be a coating or layer, for example, the metal surface may be powder coated or applied by dipping.
[0106] In various embodiments, the metal surface and / or substrate comprises, consists of, or consists essentially of galvanized steel, electrogalvanized steel, Galvanized steel, zinc metal, aluminum metal, titanium metal, zinc-aluminum alloy coated steel (referred to herein as zincalum), zinc-magnesium coated steel, or zinc-aluminum-magnesium coated steel, or a combination of any two or more thereof. Steel is an alloy containing iron and carbon and small amounts of other elements. Galvanized steel comprises steel, the surface of which is coated with zinc.
[0107] The form of the substrate will depend on the intended use of the polymer or metal-polymer composite produced by the methods described herein. For example, the substrate can be selected from the group consisting of particles, fibers, sheets, blocks, wires, webs, panels, slabs, plates, poles, columns, rods, round bars, beams, foils, joists, laminates, barrier fences, pipes, chains, fabrics, roofing materials, coatings, or any combination of two or more thereof, and preferably the substrate is in laminate, sheet, or fiber form.
[0108] The substrate may be a sheet, the metal surface of the sheet and / or the sheet itself comprises, consists of, or consists essentially of galvanized steel, electrogalvanized steel, galvanized steel, zincaluminum steel, zinc potassium, metallic zinc, metallic aluminum, metallic titanium, zinc-magnesium coated steel, or zinc-aluminum-magnesium coated steel, or a combination of any two or more thereof, preferably the metal surface of the sheet and / or the sheet itself comprises, consists of, or consists essentially of galvanized steel, more preferably hot-dip galvanized steel. In various embodiments, the metal surface and / or the substrate comprises, consists of, or consists essentially of galvanized steel, preferably hot-dip galvanized steel.
[0109] One skilled in the art will appreciate that the metal surface and / or substrate can comprise multiple elements and / or compounds. In some embodiments, the metal surface, activated metal surface, and / or substrate can comprise, consist of, or consist essentially of a pure metal or a metal alloy. The substrate can comprise a surface that comprises two or more different metals.
[0110] In some embodiments, the entire substrate surface may include one or more regions corresponding to a metal surface or an activated surface. For example, in some embodiments, the entire substrate surface may include 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 25, 50, 75, 100% or more of the regions that are metal surfaces, and useful ranges may be selected from any of these values, for example, about 1 to about 2, 1 to about 3, 1 to about 4, 1 to about 5, 1 to about 6, 1 to about 7, 1 to about 8, 1 to about 9, 1 to about 10, 1 to about 25, 1 to about 50, 1 to about 75, 1 to about 100, 10 to about 25, 10 to about 50, 10 to about 75, 10 to about 100, 25 to about 50, 25 to about 75, 25 to about 100, 50 to about 75, 50 to about 100, or 75 to about 100 regions that are metal surfaces. In some embodiments, the entire surface of the substrate can be a metal surface or an activated metal surface.
[0111] All or a portion of the substrate surface may be treated. In some embodiments, only a portion of the substrate surface may be treated such that only a portion of the metal surface of the substrate can be converted to its corresponding activated metal surface. For example, a portion of a beam material may be subjected to treatment to convert the metal surface of the beam material to an activated metal surface. The activated metal surface may then be used in the methods of forming the polymers described herein.
[0112] An activated metal surface is an "activated" metal surface, the surface of which is capable of initiating polymerization of one or more monomers provided on the surface. Activation of a metal surface can include treating the metal surface to produce one or more compounds on the surface that can initiate polymerization of one or more monomers provided on the surface, as described below. The metal surface and / or activated metal surface can include any metal known in the art, and one of skill in the art will understand that the metal surface can include more than one metal, and thus, as such, surfaces including mixtures of two or more metals are also contemplated.
[0113] In some embodiments, the metal surface can comprise magnesium, zinc, titanium, aluminum, lead, copper, titanium, silver, tin, cadmium, iron, or nickel, or a combination of any two or more thereof. Preferably, the metal surface comprises zinc, titanium, or aluminum, or a combination of any two or more thereof. In various embodiments, the metal surface comprises zinc or titanium, or a combination thereof, preferably, the metal surface comprises zinc.
[0114] As noted above, the metal surface can occupy all or a portion of the surface of the substrate. For example, the metal surface can be present as part of a larger surface that includes one or more metals, one or more non-metallic materials, such as one or more polymers, or a mixture of one or more metals and one or more non-metallic materials.
[0115] In various embodiments, the metal surface can be treated to generate one or more compounds on the surface that can initiate polymerization. Those skilled in the art will appreciate that in some embodiments, the metal surface prior to treatment may contain a relatively low amount or concentration of compounds that can initiate polymerization. In such embodiments, the metal surface can be treated to increase the amount of compounds that can initiate polymerization on the activated metal surface compared to the metal surface prior to treatment.
[0116] In various embodiments, the activated metal surface can be capable of initiating polymerization of one or more polymerizable monomers at a rate such that the polymerization proceeds to a sufficient degree of completion (e.g., at least 20, 30, 40, 50, 60, 70, 80, or 90% of the starting materials are reacted) within a desired time frame, e.g., less than 0.5, 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, or 12 days. For example, the activated metal surface can be one that allows polymerization at a rate of at least about 0.002, 0.003, 0.004, 0.005, 0.006, 0.007, 0.008, 0.009, 0.01, 0.15, 0.02, 0.025, 0.03, 0.035, 0.04, 0.045, 0.05, 0.055, 0.06, 0.065, 0.07, 0.075, 0.08, 0.085, 0.09, 0.095, 0.1 mol / (L×min) when the UV intensity is 15 W and the irradiation time is 1 hour at 60° C., and a useful range can be selected from any of these values, for example, from about 0.002 to about 0.1 mol / (L×min).
[0117] Those skilled in the art will understand that various parameters, such as temperature, initiator concentration (e.g., concentration of hydroxyl radicals), can affect polymerization. For example, higher temperatures and higher hydroxyl radical concentrations can result in faster polymerization rates. The polymerization rate also depends on the amount or concentration of one or more compounds that can initiate polymerization on the activated surface.
[0118] It has been found that untreated metal surfaces can also initiate polymerization, however, polymerization over such metal surfaces may proceed more slowly. Without wishing to be bound by any particular theory, it is believed that initiation of polymerization may involve, for example, the generation of radicals. In various embodiments, the metal surface can include one or more metals, the oxides of which are capable of generating hydroxyl radicals.
[0119] It will be understood by one of skill in the art that the metal surface can comprise more than one metal, and in some embodiments, the metal surface, the activated surface, and / or the one or more compounds capable of initiating polymerization comprise more than one metal oxide capable of initiating polymerization, for example, two or more oxides of the same metal and / or oxides of two or more different metals.
[0120] The oxide or one of the oxides present on the metal surface and / or the activated metal surface may be selected from the group consisting of magnesium oxide, lead oxide, zinc oxide, copper oxide, titanium dioxide, silver oxide, tin oxide, aluminium oxide, cadmium oxide, iron oxide and nickel oxide or a combination of two or more thereof, preferably the oxide or one of the oxides is selected from the group consisting of zinc oxide, titanium oxide and aluminium oxide or a combination of two or more thereof, preferably zinc oxide and / or titanium oxide, more preferably the oxide is zinc oxide.
[0121] In various embodiments, the activated metal surface can be capable of generating hydroxyl radicals. In some embodiments, the activated metal surface can generate hydroxyl radicals, and upon UV irradiation, the fluorescent 2-hydroxyl terephthalic acid is generated from the non-fluorescent terephthalic acid, as measured at 425 nm.
[0122] In some embodiments, the activated metal surface can be produced by treating a metal surface of a substrate comprising a metal surface, whereby in some embodiments the method can include providing a substrate comprising a metal surface and treating the substrate comprising a metal surface to produce the activated surface.
[0123] In various embodiments, the activated surface can be formed during formation of the substrate. In various embodiments, one or more metal oxides can be generated by treating a metal surface; alternatively, the method of the present invention can include treating a metal surface to generate one or more metal oxides. Treating a metal surface to generate an activated surface can include generating one or more metal oxides capable of generating hydroxyl radicals. Without wishing to be bound by a particular theory, it is believed that the generated hydroxyl radicals may participate in the polymerization process. The amount of hydroxyl radicals generated per unit surface area on the activated surface is in turn dependent on the concentration of one or more compounds capable of initiating polymerization on the activated surface, with the amount of hydroxyl radicals increasing as the concentration of one or more compounds increases.
[0124] The amount of hydroxyl radicals generated on the surface can be measured by various methods known in the art. The results obtained by such methods can be used to estimate the ability of the surface to promote polymerization. In the present specification, the amount or concentration of 2-hydroxyterephthalic acid (TAOH) (determined, for example, based on the fluorescence intensity at 425 nm of a sample in the presence of terephthalic acid (TA), as described in Section 1.7 under the heading "General Procedure for Testing the Generation of TAOH by Activated Metal Surfaces") can be used to indicate the presence of hydroxyl radicals. In some embodiments, when the activated metal surface is contacted with an aqueous solution of 30.096 μM terephthalic acid and 0.001 mol / L NaOH and irradiated with a 15 W light source at 365 nm for 1 hour at room temperature, the 2-hydroxyterephthalic acid is reduced in concentration by at least 0.0001, 0.0002, 0.0003, 0.0004, 0.0005, 0.0006, 0.0007, 0.0009, 0.0001, 0.0002, 0.0003, 0.0004, 0.0005, 0.0006, 0.0007, 0.0008, 0.0009, 0.0001, 0.0002, 0.0003, 0.0004, 0.0005, 0.0006, 0.0007, 0.0001 ...1, 0.0001, 0.0001, 0.0001, 0.0001, 0.0001, 0.0001, 0.0001, 0.000 8, 0.0009, 0.001, 0.0015, 0.002, 0.0025, 0.003, 0.0035, 0.004, 0.0045, 0.005, 0.0055, 0.006, 0.0065, 0.007, 0.0075, 0.008, 0.0085, 0.009, 0.0095, 0.01, 0.0105, 0.011, 0.0115, 0.012, 0.0125, or 0.013 μM / mm of geometric area of activated surface 2 and useful ranges can be selected from any of these values, e.g., 0.0001 to 0.013, preferably at least 0.0001, preferably at least 0.0005, preferably at least 0.001, preferably at least 0.005, preferably at least 0.01 μM / mm of geometric area of activated surface. 2In some embodiments, the activated metal surface produces 2-hydroxyterephthalic acid at such a concentration when tested according to the procedure described in Section 1.7 of the Examples. Unless otherwise specified, when referring to the concentration of 2-hydroxyterephthalic acid produced or capable of being produced from an activated surface by contacting the activated surface with an aqueous solution of 30.096 μM terephthalic acid and 0.001 mol / L NaOH and irradiating with a 15 W light source at 365 nm for 1 hour at room temperature, this concentration refers to the concentration of 2-hydroxyterephthalic acid produced by the activated surface reduced (i.e., after subtraction) by the concentration of 2-hydroxyterephthalic acid produced in a control sample, i.e., the concentration of 2-hydroxyterephthalic acid produced when kept in the aqueous solution in the dark for 1 hour at room temperature in the absence of the activated surface (e.g., as described below in Section 1.7).
[0125] In some embodiments, a method for producing a polymer includes treating a substrate comprising a metal surface to produce an activated metal surface, which can then be contacted with one or more polymerizable monomers to polymerize the one or more polymerizable monomers.
[0126] The treatment of the metal surface to obtain an activated metal surface can be carried out in any suitable manner that produces and / or increases the concentration of one or more compounds capable of initiating polymerization on the surface. The concentration of the one or more initiator compounds on the activated surface can depend on the treatment method used to produce the activated surface and the morphology of the surface. For example, a surface with a high surface area morphology can provide an activated surface with a high concentration of initiator compounds.
[0127] Treating the metal surface to produce an activated surface can include one or more of heating the metal surface to an elevated temperature (e.g., in an oven, with a laser, or by other suitable methods), passing an electric current through the metal surface (e.g., an anodization step), subjecting the metal surface to a chemical treatment (e.g., a treatment to generate hydroxyl groups on the metal surface, an alkali treatment such as an alkali metal hydroxide treatment, or an acid treatment), subjecting the metal surface to a plasma treatment (e.g., an oxygen plasma treatment), or exposing the metal surface to UV light radiation. In some embodiments, treating the metal surface can include heating the metal surface to an elevated temperature to produce an activated surface, passing an electric current through the metal surface, or exposing the metal surface to ultraviolet (UV) radiation.
[0128] The metal surface may be heated to an elevated temperature for a suitable period of time. Those skilled in the art will appreciate that the temperature and time for which the metal surface is heated may be relevant. The temperature will depend on the nature of the metal surface, such as the melting point of the metal. The heating temperature and time will also depend on the method for heating the surface. Metal Surfaces Metal surfaces can be heated to temperatures of at least about 100, 150, 200, 250, 300, 350, 400, 450, 500, 550, 600, 650, 700, 750, 800, 850, 900, 950, 1000, 1050, 1100, 1150, 1200, 1250, 1300, 1350, 1400, 1450, 1500°C, and useful ranges can be selected from any of these values, for example, at least about 200°C to about 600°C, preferably at least about 300°C to about 600°C, and more preferably at least about 300°C to about 400°C.
[0129] In some embodiments, the metal surface may be subjected to more than one treatment step to produce an activated metal surface. For example, in some embodiments, the metal surface may be subjected to a first treatment step and a second treatment step, either sequentially or simultaneously. For example, in some embodiments, the first treatment step may comprise a treatment selected from the group consisting of a plasma treatment, e.g., an oxygen plasma treatment, anodization, an alkali treatment, e.g., an alkali metal hydroxide treatment, or an acid treatment, preferably an alkali treatment, and the second treatment step may comprise heating the metal surface at an elevated temperature (heat treatment).
[0130] In some embodiments, heating the metal surface includes heating for at least about 1, 2, 3, 4, 5, 6, 7, 8, 9, 10 hours, or more, and a useful range can be selected from any of these values, such as at least about 1 to about 10 hours, 2 to about 10, 3 to about 10, 4 to about 10, 5 to about 10, 6 to about 10, 7 to about 10, 8 to about 10, 9 to about 10, 2 to about 9, 3 to about 9, 4 to about 9, 5 to about 9, 6 to about 9, 7 to about 9, 8 to about 9, 2 to about 8, 3 to about 8, 4 to about 8, 5 to about 8, 6 to about 8, 7 to about 8, 1 to about 9, 1 to about 8, 1 to about 7, 1 to about 8, 1 to about 6, 1 to about 5, 1 to about 4, 1 to about 3, or at least about 1 to about 2 hours, preferably at least about 1 hour, and more preferably at least about 2 hours. Heating times of this type may be useful, for example, in embodiments where the entire substrate is subjected to heating, for example, in an oven or furnace.
[0131] In other embodiments, the heating can be carried out for a period of less than 1 hour, such as less than 30, 20, 10, 5, 4, 3, 2, or 1 minute. In some embodiments, the heating is performed for less than 60, 30, 20, 10, 5, 4, 3, 2, 1, 0.5, 0.1, 0.05, or 0.01 seconds. To transfer enough heat to activate the surface in such a short heating time, a laser or other heat source capable of rapidly heating the metal surface, such as a plasma, can be used. The power of the laser and the beam / surface interaction time can be selected and / or varied to achieve the desired degree of activation. The laser rapidly performs localized surface heating, heating a thin layer of the metal surface while the bulk of the substrate remains relatively cool. Such localized heating of the surface can achieve a useful degree of activation, but reduces or prevents deformation or softening of the metal surface and / or substrate, which may occur, for example, when heated at high temperatures for long periods of time in an oven. By using a laser, the time required to generate an activated surface is significantly reduced compared to, for example, using an oven. Laser surface treatment can be performed in a variety of ways. As an example, a continuous wave (CW) laser can be raster scanned over the surface, with the dwell time depending on the power of the laser. In another example, a pulsed laser can be used to create an array of dots on an activated surface, with the laser fired once or multiple times for each dot.
[0132] In some embodiments, the metal surface can be heated at the same temperature throughout the treatment step. In some embodiments, the temperature can be changed during the treatment step. For example, the temperature can be changed during heating in a range of at least about 100°C to about 600°C. The temperature of the treatment step can be monitored manually or automatically, and any temperature changes can be adjusted manually or automatically as needed to adjust the treatment time. The treatment step can include more than one stage, for example, 2, 3, 4, or 5 or more stages, each stage having a different treatment temperature, for example, the temperature is independently selected from at least about 100°C to about 600°C, preferably at least about 200°C to about 600°C, preferably at least about 300°C to about 600°C, more preferably at least about 300°C to about 400°C. In some embodiments, each stage includes heating the metal surface to an elevated temperature above the temperature of the previous stage.
[0133] The activity of the activated surface may decrease over time. However, the activated surface produced by the treatments described herein will usually maintain a suitable degree of activity for a reasonable period of time, for example, about 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16, 17, 18, 19, 20, 21, 22, 23, 24, 25, 26, 27, 28, 29, 30, 31, 32, 33, 34, 35, 36, 37, 38, 39, 40, 41, 42, 43, 44, 45, 46, 47, or 48 hours. A suitable range can be selected from any of these values, for example, about 1 to about 48 hours, about 1 to about 25 hours, or about 1 to about 12 hours. In some embodiments, a useful degree of activity is maintained for at least 12, 24, 48, or 72 hours or more. The decrease in activity of the activated surface may depend on a variety of factors, such as the metal or metals present on the activated surface, the temperature to which the metal surface is heated to activate it, the ambient temperature, and the rate of cooling, e.g., the rate of cooling to room temperature. The rate of cooling, e.g., the rate of cooling to room temperature, will in turn be affected by factors such as the surface area of the activated surface and whether the activated surface is subjected to one or more steps designed to accelerate cooling, e.g., by immersion in a quench bath.
[0134] One skilled in the art will appreciate that metal surfaces can be activated to different degrees, depending, for example, on different amounts or concentrations of one or more compounds capable of initiating polymerization that are present on the surface. For example, an activated surface may have a high degree of activation immediately after treatment. This degree of activation may subsequently decrease at a rate that depends on factors such as those listed above.
[0135] In some embodiments, untreated metal surfaces may be active in the sense that they may contain compounds capable of initiating polymerization, however, as described herein, the amount or concentration of such compounds on an untreated metal surface may be lower than the amount or concentration on a corresponding treated surface.
[0136] To polymerize the one or more polymerizable monomers, the one or more polymerizable monomers may be contacted with the surface while the surface is in an activated state. In some embodiments, the activated surface is contacted with one or more polymerizable monomers within less than about 72, 48, 24, 12, 6, 5, 4, 3, 2, or 1 hour after formation, and useful ranges can be selected from any of these values, such as 72 to about 1, 48 to about 1, 24 to about 1, 12 to about 1, 6 to about 1, 4 to about 1, 3 to about 1, or 2 to about 1 hour, preferably less than about 48 hours, more preferably less than about 24 hours. In some embodiments, contacting of the activated surface with the monomer occurs within less than about 30, 15, 10, 5, 1, or 0.5 minutes, or within less than about 10, 5, or 1 second after formation of the activated surface.
[0137] Contacting the activated surface with one or more polymerizable monomers can, in some embodiments, be carried out at a temperature above the boiling point of the one or more polymerizable monomers, however, contacting at such temperatures can cause the monomers to volatilize, leading to loss of monomers.
[0138] In various embodiments, the activated surface can be cooled, preferably to a temperature lower than the boiling point of the polymerizable monomer or monomers at atmospheric pressure, before contacting with the polymerizable monomer or monomers. Cooling can be achieved, for example, by storing the substrate with the activated surface, for example at room temperature, for a time sufficient to cool the activated surface, or by immersing in a quench bath. The time to cool the activated surface can vary depending on the mechanism by which the surface is cooled. For example, one skilled in the art will understand that cooling the activated surface of a substrate at ambient temperature may require a longer time than cooling the activated surface or substrate, for example, by immersing in a quench bath of cold water or other suitable liquid. Thus, the activated surface may be cooled for less than about 5, 10, 15, 20, 25, 30, 35, 40, 45, 50, 55, 60, 120, 180, 240, 300, 360, 420, 480, 540, or 600 minutes, and suitable ranges may be selected from any of these values, for example, the activated surface may be cooled for about 5 minutes to about 600 minutes, about 5 minutes to about 300 minutes, about 5 minutes to about 120 minutes, about 5 minutes to about 50 minutes, or about 5 minutes to about 30 minutes. In various embodiments, the activated surface may be cooled for less than 10 hours, preferably less than 5 hours, and more preferably less than 2 hours. It will be understood by those skilled in the art that the temperature, time, and subsequent cooling time may be influenced at least in part by factors such as the type of metal surface being heated, particularly the metal present on the metal surface and the size of the metal surface.
[0139] In some embodiments where the metal surface is heated with a laser or other heat source such as a plasma capable of rapidly heating the metal surface to generate the activated surface, one or more monomers can be contacted with the activated surface immediately after the activated surface is generated, for example by spraying. In some embodiments where a laser is used to generate the activated surface (as opposed to using a plasma, for example), the monomers can be contacted before or simultaneously with the generation of the activated surface. This type of embodiment may depend on the power and spot size of the laser. The laser only locally heats the surface in a thin layer, and the absorbed heat is quickly dissipated to the remaining surface and / or the bulk of the substrate. Therefore, the activated surface is cooled very quickly to a temperature suitable for contacting the monomer. In some embodiments, the laser beam (continuous wave or pulsed) moves over the metal surface to generate the activated surface, preferably followed or tracked by a dispensing device such as a nozzle that delivers one or more monomers to the activated surface immediately after activation. In some embodiments, an irradiation source may follow or track the dispensing device, under which polymerization occurs. In some embodiments, the monomer forms a liquid coating on the activated surface, which can prevent or reduce the degree of activity of the activated surface from decreasing before polymerization occurs. In some embodiments, the monomer or monomers and the activated surface are irradiated to induce polymerization immediately upon contact with the activated surface. This type of embodiment using a laser to generate the activated surface can be useful for generating a variety of metal-polymer composites, such as substrates that may be difficult to heat treat, for example in an oven, due to their shape, size, composition, or other characteristics.
[0140] Many substrates with metal surfaces, such as those listed above, can be prepared industrially at high temperatures. For example, substrates such as steel, zinc potassium, and zinc can be prepared from a melt of a metal mixture, which is cast or solidified in various molds that may vary depending on the intended application to obtain the desired shape and / or configuration. The use of high temperatures in the manufacture of such substrates will usually result in a substrate having an activated metal surface. Thus, in some embodiments, the method of the present invention includes providing a substrate with an activated metal surface, which is generated upon forming the substrate.
[0141] In another embodiment, the method of the present invention includes providing a substrate comprising a metal surface and treating the substrate to produce a substrate comprising an activated metal surface. The concept of providing a substrate with an activated metal surface for use in the method of the invention can be illustrated by the example of galvanized steel. The industrial preparation of galvanized steel involves immersing the steel surface in a bath of molten zinc, a process known as hot-dip galvanization, which results in a coating of zinc on the steel surface. By using high temperatures in this process (usually above 400° C.), galvanized steel with an activated surface is produced. Freshly produced galvanized steel can then be used directly in the method of the invention, with or without cooling.
[0142] Galvanized steel may be produced in a batch process, where all of the galvanized steel samples of a particular batch are processed together through each step of the manufacturing process, or it may be produced in a continuous process, where the galvanized steel samples are subjected to all of the processing steps in sequence, with no time or sequence gap between each.
[0143] The methods described herein can be incorporated into both batch and continuous processes for the manufacture of galvanized steel. For example, freshly galvanized steel pieces can be pulled off the line hot and provided hot or after cooling for use in the methods described herein. Thus, the methods described herein can be incorporated into processes currently used in the art for the manufacture of galvanized steel and other substrates described herein.
[0144] As mentioned above, the manufacturing process of substrates such as galvanized steel, electroplated steel, galvanized steel, zinc potassium, metallic zinc, metallic aluminum, metallic titanium, zinc-magnesium coated steel, or zinc-aluminum-magnesium coated steel can be carried out to produce substrates with activated surfaces suitable for use in the method of the present invention. However, many of these substrates may be stored for long periods of time before being shipped and used in their intended applications. In some embodiments where these substrates may be stored for long periods of time before being used in the method of producing the polymers described herein, it may be advantageous to evaluate the activity of the surface before use in the method of the present invention. In some embodiments, it may be desirable to subject the substrate to a treatment step before contacting it with a polymerizable monomer as described herein.
[0145] As described herein, the degree of surface activation can be evaluated, for example, by measuring the hydroxyl radicals generated by the surface of the substrate, as described herein. Monitoring the degree of surface activation can be useful for determining the duration and / or conditions that can be used to contact one or more polymerizable monomers with the activated surface. The degree of activation of the activated surface is indicative of and / or related to the concentration of one or more compounds that can initiate polymerization on the activated surface.
[0146] The one or more polymerizable monomers can be any monomer that can be polymerized, preferably by radical polymerization, for example, polymerization that includes, consists of, or consists essentially of photochemical polymerization. In various embodiments, the one or more monomers can be commercially available monomers that are liquid at room temperature. The use of monomers that are gaseous or solid at room temperature is also contemplated herein.
[0147] In various embodiments, the one or more polymerizable monomers are photoactive monomers. In various embodiments, the one or more polymerizable monomers are unsaturated, preferably olefinically unsaturated, preferably ethylenically unsaturated. In some embodiments, the one or more polymerizable monomers can be esters or amides, preferably esters, of ethylenically unsaturated carboxylic acids having 1 to 15, preferably 1 to 10 carbon atoms, such as esters or amides of acrylic acid and methacrylic acid. In various embodiments, the one or more polymerizable monomers are monoolefinically unsaturated monomers, preferably monoethylenically unsaturated monomers; or polyolefinic, preferably diolefinically unsaturated monomers, preferably polyethylenically unsaturated monomers; preferably diethylenically unsaturated monomers.
[0148] The one or more polymerizable monomers can include at least one polymerizable carbon-carbon double bond. In various embodiments, the at least one carbon-carbon double bond is represented by Formula I:
[0149] [ka]
[0150] or a moiety comprising the structure shown in Formula II:
[0151] [ka]
[0152] or the moiety shown in formula III:
[0153] [ka]
[0154] where R 1 , R 2 , R 5 , R 6 , R 11 , R 12 , X and Y are as defined herein. In some embodiments, the one or more polymerizable monomers can be selected from the group consisting of vinyl monomers, preferably acrylic acid esters or methacrylic acid esters.
[0155] In some embodiments, the one or more polymerizable monomers have Formula I:
[0156] [ka]
[0157] where R 1 and R 2 is as described herein. In some embodiments, the one or more polymerizable monomers have Formula II:
[0158] [ka]
[0159] where R 5 , R 6 , X, and Y are as described herein. In some embodiments, the one or more polymerizable monomers have Formula III:
[0160] [ka]
[0161] where R 5 , R 11 , and R 12 is as described herein. In the monomer of formula II, Y can be a linking group, which can preferably comprise a linear chain containing at least 2, 5, 10, 15, 20, 25, 30, 35, 40, 45, 50, 55, 60, 65, 70, 75, 80, 85, 90, 95, 100 or more atoms selected from carbon, nitrogen, oxygen, and sulfur, with suitable ranges being selected from any of these values, such as a linear chain of about 1 to about 100 atoms, e.g., about 1 to about 100 atoms. In various embodiments, the linking group can comprise an atom selected from the group consisting of carbon, hydrogen, nitrogen, and oxygen. In some embodiments, the linking group may comprise a branched or unbranched, saturated or unsaturated alkyl chain containing about 1, 5, 10, 15, 20, 25, 30, 35, 40, 45, 50, 55, 60, 65, 70, 75, 80, 85, 90, 95, 100 or more atoms, with suitable ranges being selected from any of these values, for example, from about 1 to about 100 atoms. In various embodiments, Y is a linking group. In various embodiments, Y is a group of the formula (CR 30 R 40 ) q or formula (CR 50 R 60 O) r (CR 70 R 80 ) linking group (wherein R 30 , R 40 , R 50 , R 60 , R 70 , and R 80 are each independently H or alkyl, preferably C1-10 alkyl, and q and r are each independently an integer from 1 to 40. In various embodiments, Y is (CH2) m , CH2CH2CH(CH3), (CH2CH2O)p (CH2CH2), and formula IIA:
[0162] [ka]
[0163] wherein R 7 , R 8 , R 9 , R 10 , m and p are as defined herein). In various embodiments, the one or more polymerizable monomers are monomers of formula II. In various embodiments, each X is O. In some embodiments, the one or more polymerizable monomers are monomers of formula II having a linking group of formula IIA.
[0164] In some embodiments, R 5 and R 6 are both methyl. In some embodiments, R 7 and R 9 are both methyl, and R 8 and R 10 are each independently selected from the group consisting of H and CH3, preferably R 8 and R 10 One of them is H and the other is R 8 and R 10 The other is CH3, and preferably R 7 and R 9 are both methyl, and R 8 and R 10 exists as a 1:1 mixture of H and CH3.
[0165] In an exemplary embodiment, the one or more polymerizable monomers is diurethane dimethacrylate, CAS number 72869-86-4. In various embodiments, the one or more polymerizable monomers are monomers of formula III.
[0166] In some embodiments, the one or more polymerizable monomers may be selected from the group consisting of methyl acrylate, methyl methacrylate, butyl methacrylate, poly(ethylene glycol) methyl ether methacrylate, butyl acrylate, styrene, vinyl acetate, diurethane dimethacrylate (DUDMA), ethylene glycol dimethacrylate (EGDMA), 1,3-butanediol dimethacrylate, 1,6-hexanediol dimethacrylate, poly(ethylene glycol) dimethacrylate, di(ethylene glycol) dimethacrylate, and glycerol dimethacrylate.
[0167] In various embodiments, the one or more polymerizable monomers are selected from the group consisting of methyl acrylate, methyl methacrylate, butyl methacrylate, diurethane dimethacrylate, poly(ethylene glycol) methyl ether methacrylate, butyl acrylate, styrene, and vinyl acetate.
[0168] Some of the monomers described herein are commercially available. The polymerizable monomer(s) can be contacted with the activated metal surface in a number of ways, for example, the polymerizable monomer(s) can be contacted with the activated metal surface (or vice versa) by spraying, painting, sputtering, spin coating, immersing, dipping, or otherwise applying the polymerizable monomer(s) to the surface.
[0169] The activated surface may be contacted with one or more monomers of one type to form a homopolymer. For example, the activated surface may be contacted with one or more monomers of formula I, II, or III to form a polymer of the monomers. Conditions for polymerizing the one or more monomers are described herein.
[0170] In other embodiments, the activated metal surface can be contacted with two or more polymerizable monomers (i.e., two or more different types of monomers) to form a copolymer. The activated metal surface can be contacted with one or more polymerizable monomers simultaneously or sequentially. For example, the activated metal surface can be contacted with a first type of monomer and a second type of monomer simultaneously. Alternatively, the first type of monomer can be contacted with the activated surface first, and then the second type of monomer can be contacted with the activated surface. That is, the first type of monomer can be contacted with the activated surface for a period of time to polymerize the monomer before contacting the second type of monomer. In embodiments where the activated surface is contacted with different types of monomers, copolymers of different types of monomers are produced. For example, in embodiments where the first type of monomer is contacted with the activated surface first, and then the second type of monomer is contacted with the activated surface, copolymers of the first and second types of monomers can be produced. As another example, a solution containing a first monomer can be contacted with the activated surface first, followed by a solution containing a second monomer, and this process can be repeated one or more times, for example to produce an alternating polymer. The copolymers produced in the methods described herein can be block, brush, statistical (random) or graft copolymers, preferably block copolymers.
[0171] In various embodiments, the activated surface can be contacted with one or more polymerizable monomers in liquid state (e.g., neat or in solution in a solvent or solvent mixture, e.g., organic solvent and / or aqueous solution) or gaseous state. In some embodiments, the activated surface can be contacted with one or more polymerizable monomers in solid state at room temperature. The solid polymerizable monomer can be heated to a temperature sufficient to melt the polymerizable monomer or to allow the solid polymerizable monomer to dissolve in the solvent. It will be understood by those skilled in the art that in some cases, it may be desirable to use no solvent or a minimal amount of solvent, for example, for cost and / or safety reasons. Thus, in certain preferred embodiments, the one or more monomers are contacted with the activated surface in the absence of a solvent (i.e., neat).
[0172] In other embodiments, the activated surface can be contacted with one or more polymerizable monomers in one or more solvents that have a low propensity for hydrogen transfer reactions (HAT) to carbon-centered radicals (less prone to chain transfer and termination), such as dimethylformamide (DMF) and / or toluene. Without wishing to be bound by theory, the inventors believe that the use of solvents that are prone to HAT can inhibit or prevent chain growth during polymerization.
[0173] It will be understood by those skilled in the art that the state of the polymerizable monomer(s) may depend on factors such as, for example, the nature of the monomer(s), the contact temperature, and the contact pressure. In various embodiments, contact of the activated surface with the polymerizable monomer(s) can be carried out at a temperature near room temperature (20-25° C.) and / or at a pressure near atmospheric pressure (760 mmHg). In other embodiments, contact of the activated surface with the polymerizable monomer(s) can be carried out at elevated temperatures and / or pressures.
[0174] The rate of polymerization and the characteristics of the resulting polymer may depend on the conditions used for polymerization, including, but not limited to, the concentration and nature of the polymerizable monomer(s), the contacting temperature, the contacting pressure, the length of time the contacting step is carried out, and the exposure time to light, e.g., ultraviolet (UV) light, and the power of the light used for irradiation, if used. The rate will also depend on the degree of activation and / or the concentration of compounds capable of initiating polymerization on the activated surface.
[0175] In various embodiments, the activated metal surface and the one or more polymerizable monomers can be contacted for a first period of time at a first temperature. Thus, in various embodiments, the activated metal surface is contacted with the one or more polymerizable monomers for a first period of time at a temperature of at least about 10, 15, 20, 25, 30, 35, 40, 45, 50, 55, 60, 65, 70, 75, 80, or 85° C. or greater, with useful ranges being selected from any of these values, such as from about 10° C. to about 85° C., preferably 20° C., and more preferably 85° C.
[0176] The first period of time can be at least about 30 seconds, 1, 5, 10, 15, 30, or 60, 70, 80, 90, 100, 110, or 120 minutes, and a useful range can be selected from any of these values, such as from about 30 seconds to about 120 minutes, or from about 30 seconds to about 60 minutes. As noted above, one of ordinary skill in the art will appreciate that the first period of time can depend on factors such as, for example, the intensity of the light, preferably UV light, under which the metal surface and the polymerizable monomer are contacted.
[0177] In some embodiments, the activated metal surface can be contacted with one or more polymerizable monomers for a first period of time and then for a second period of time. In various embodiments, the method of producing a polymer can include contacting an activated metal surface with one or more polymerizable monomers and irradiating the surface with light, preferably UV light, for a first period of time. The activated metal surface can be contacted with one or more polymerizable monomers and irradiated with light having a wavelength of about 10, 50, 100, 150, 200, 250, 300, 350, 400, 450, 500, 550, 600, 650, 700, 750, 800, 850, 900, 950, 1000, 1050, 1100, 1150, 1200, 1250 nm or more for a first period of time, and useful ranges can be selected from any of these values, such as about 10 nm to about 1000 nm, about 10 nm to about 700 nm, and preferably about 10 nm to about 400 nm. Further useful ranges are selected from the wavelength values mentioned above, for example, about 10-400, 50-400, 100-400, 150-400, 200-400, 10-700, 50-700, 100-700, 150-700, 200-700, 300-700, 400-700, 10-1000, 50-1000, 100-1000, 150-1000, 200-1000, 300-1000, 400-1000, 500-1000, 600-1000, or 700-1000 nm. The wavelength can be selected based on the metal / metal oxide present on the activated surface. The wavelength and / or power of the light used for irradiation can depend, for example, on the metal in the activated metal surface that is used as an initiator during polymerization. Different metals may also be subjected to different power levels and / or different wavelengths of light, such as UV light, to initiate polymerization.
[0178] The light can be selected to include wavelengths that optimize the generation of hydroxyl radicals by the compound or compounds capable of initiating polymerization on the activated surface. For example, light can be selected to include wavelengths that generate electrons by the compound or compounds capable of initiating polymerization. Suitable wavelengths or wavelength ranges will be apparent to those skilled in the art. In this way, irradiation with other wavelengths of light that may undesirably heat or otherwise interact with the activated surface, the monomer or monomers, or the resulting polymer can be reduced or avoided.
[0179] Polymerization can be initiated and proceeded with relatively low power light, e.g., visible light, such as in sunlight, but faster polymerization rates can be achieved using higher power levels of light, e.g., UV light. Thus, in some embodiments, the power of the light is at least about 1, 1.5, 2, 2.5, 3, 3.5, 4, 4.5, 5, 5.5, 6, 6.5, 7, 7.5, 8, 8.5, 9, 9.5, 10, 10.5, 11, 11.5, 12, 12.5, 13, 13.5, 14, 14.5, 15, 15.5, 16, 16.5, 17, 17.5 , 18, 18.5, 19, 19.5, 20, 25, 30, 35, 40, 45, 50, 55, 60, 65, 70, 75, 80, 85, 90, 95, 100, 105, 110, 115, 120, 125, 130 W, or more, and a useful range can be selected from any of these values, for example, from about 1 to about 130 W. In some embodiments, the light intensity is determined by the amount of light emitted by the irradiated activated surface (m 2 ) is at least 1, 2, 3, 4, 5, 6, 7, 8, 9, or 10 W per 100 W. The amount of hydroxyl radicals generated by the activated surface and / or the degree of conversion of one or more monomers to polymer can be increased in some embodiments by increasing the irradiation intensity. Any suitable light source can be used. Examples of suitable light sources include lamps and lasers of various powers and wavelengths.
[0180] In various embodiments, the activated metal surface can be contacted with one or more polymerizable monomers for a first period of time followed by a second period of time characterized by different temperatures and / or irradiation, e.g., irradiation with UV light. In various embodiments, the activated metal surface can be contacted with one or more polymerizable monomers for a first period of time at a first temperature and for a second period of time at a second temperature, the first temperature being different from the second temperature, and preferably the first temperature being higher than the second temperature. In various embodiments, the contacting of the activated metal surface with the one or more polymerizable monomers can be performed with irradiation with light, e.g., UV light, only for the first period of time. In various embodiments, the method can include contacting the activated metal surface with the one or more polymerizable monomers for a second period of time for polymerization chain propagation, optionally without further irradiation. In various embodiments, the method can include contacting the activated metal surface with the one or more polymerizable monomers for a second period of time for polymerization chain propagation in the absence of light, e.g., UV light. In various embodiments, contacting the activated metal surface with the one or more polymerizable monomers can be carried out for the second period of time at a temperature of at least about 10, 15, 20, 25, 30, 35, 40, 45, 50, 55, 60, 65, 70, 75, 80, or 85°C, preferably from 10°C to about 85°C, and more preferably from 50 to 85°C.
[0181] In some embodiments, contacting the activated metal surface with one or more polymerizable monomers under irradiation with light, e.g., UV light, on an industrial scale may be accomplished by irradiating the substrate with the activated metal surface and the one or more polymerizable monomers in a chamber, e.g., the substrate may be passed through the chamber in the case of a continuous process, or the substrate may be placed in the chamber in the case of a batch process. In other embodiments, a light source for irradiating, e.g., a laser, may be moved over the substrate.
[0182] As mentioned above, the method of the present invention can be incorporated into a continuous process for manufacturing a substrate, for example, a continuous process for manufacturing a galvanized steel substrate. In some embodiments where the method of the present invention is incorporated into a continuous process, the substrate, for example, galvanized steel, may be transported from one stage of the manufacturing process to another, for example, by a conveyor belt. The substrate may be passed through a first treatment stage, for example, a first chamber, which converts the metal surface of the substrate into an activated surface. Alternatively, the substrate may already be provided with an activated surface. The substrate with the activated metal surface may then be passed through a second treatment stage, in which it is contacted with one or more polymerizable monomers for a first period of time in the presence of light, for example, UV light, to initiate polymerization of the one or more polymerizable monomers on or at the activated metal surface.
[0183] Continuing with the continuous process described above, the substrate may be passed through a second processing stage and transitioned to a third processing stage where polymerization chain propagation may occur for a second period of time under conditions described herein. In some embodiments, the third processing stage may be, for example, a chamber, a storage unit, or a shipping container.
[0184] In some embodiments, the activated metal surface and the one or more polymerizable monomers can be contacted at a first temperature for a first period of time, followed by contact at a second temperature for a second period of time. The first temperature can be the same or different than the second temperature, and the first period of time can be the same or different than the second period of time. In some embodiments, after the first period of time, the activated surface and the one or more polymerizable monomers can be heated to a temperature of about 20, 25, 30, 35, 40, 45, 50, 55, 60, 65, 70, 75, 80, or 85° C. or greater for a second period of time, with useful ranges being selected from any of these values, for example, the second period of time can be conducted at a temperature between about 20° C. and about 85° C., preferably between about 50° C. and about 85° C.
[0185] It will be understood by those skilled in the art that the above-mentioned first period of time may depend on the intensity, wavelength, and / or power of the instant light, e.g., UV light, used to irradiate the activated surface and the one or more polymerizable monomers during the first period of time.
[0186] In embodiments where the activated surface and one or more polymerizable monomers are contacted for a first period of time followed by a second period of time, the first period of time can be used to aid in initiation of polymerization and the second period of time can be used to aid chain propagation of the polymerization.
[0187] The second period of time can be less than about 72, 48, 36, 24, 12, 11, 10, 9, 8, 7, 6, 5, 4, 3, 2, or 1 hour, and a useful range can be selected from any of these values, such as from about 1 to about 72 hours, preferably less than about 5 hours, and more preferably less than about 1 hour. In some embodiments, the second period of time does not require the presence of light, i.e., polymerization can be chain-propagated in the dark.
[0188] Without wishing to be bound by any particular theory, the inventors believe that under irradiation with light, e.g., UV light, one or more metals on the activated metal surface can act as a photocatalyst to initiate polymerization of one or more polymerizable monomers at the interface between the activated metal surface (e.g., steel) and the polymer. The inventors believe that under irradiation with light, e.g., light in the UV-visible range, preferably light in the UV range, a metal compound, e.g., a metal oxide, such as zinc oxide, can generate hydroxyl radicals on the activated metal surface as described herein.
[0189] In various embodiments, the characteristics of the polymer or metal-polymer composite produced by the method of the invention can be controlled by the selection of monomers used in the method and by adjusting the conditions used to treat the metal surface to produce an activated metal surface and / or the conditions used to contact the activated metal surface with one or more polymerizable monomers. For example, the molecular weight of the polymer formed by the method, the degree of crosslinking of the polymer, the glass transition temperature (Tg), and the polydispersity index can be controlled. In some embodiments, it may be possible to control the hardness of the polymer. This control may allow the production of polymers and metal-polymer composites tailored for specific applications. In some embodiments, the polymers produced by the method of the invention can have higher molecular weights and narrower polydispersity indexes than polymers produced by prior art polymerization processes that use external or exogenous initiators and / or chain transfer agents.
[0190] In various embodiments described herein, the activated metal surface can act as a polymerization initiator. Thus, for example, the activated surface can be selected to control the molecular weight of the resulting polymer, e.g., to change the mechanical and / or other properties of the resulting polymer, for example, to tailor the resulting polymer to a particular intended application. For example, in some embodiments, heat-treated zinc potassium (TTZnAl) can be used to produce a polymer with a higher molecular weight than a polymer prepared using galvanized steel (TTGS(600)) heat-treated at 600°C. Without wishing to be bound by a particular theory, the inventors believe that the use of different initiators can produce different amounts or concentrations of radicals on their surfaces, which can result in the production of polymer products with different molecular weights.
[0191] It will be appreciated by those skilled in the art that the methods described herein can be used to prepare polymers over a wide range of molecular weights. Moreover, the methods described herein can be used to produce polymers within a specific molecular weight range, for example, to tailor the polymer to one or more intended uses. In various embodiments, the number average molecular weight (Mn) of the polymer is at least about 2,000, 10,000, 50,000, 100,000, 150,000, 200,000, 250,000, 300,000, 350,000, 400,000, 450,000, 500,000, 550,000, 600,000, 650,000, 700,000, 750,000, 800,000, 850,000, 900,000, 950,000, 1,000,000, 1,050,000, 1,100,000, 1,200,000, 1,300,000, 1,400,000, 1,500,000, 2,600,000, 2,700,000, 2,800,000, 3,100,000, 3,200,000, 4,100,000, 4,200,000, 5,300,000, 6,400,000, 7,500,000, 8,500,000, 9,500,000, 10,000,000, 11,000,000, 12,000,000, 13,000,000, 14,000,000, 15,000,000, 16,000,000, 17,000,000, The molecular weight of the polymer can be about 2,000 to about 1,200,000, about 10,000 to about 1,200,000, about 50,000 to about 1,200,000, about 100,000 to about 1,200,000, about 500,000 to about 1,200,000, about 2,000 to about 500,000, about 10,000 to about 500,000, about 50,000 to about 500,000, or about 100,000 to about 500,000 g / mol. In other embodiments, the number average molecular weight of the polymer can be at least about 500,000, 550,000, 600,000, 650,000, 700,000, 750,000, 800,000, 850,000, 900,000, 950,000, 1,000,000, 1,050,000, 1,100,000, 1,150,000, 1,200,000, 1,250,00, 1,500,000, 2,000,000, 3,000,000, 4,000,000, or 5,000,000 g / mol, with useful ranges selected from any of these values, for example, from about 500,000 to about 5,000,000 g / mol.
[0192] The intensity of the light used to initiate polymerization can also affect the molecular weight of the polymer produced. For example, in some embodiments, polymerization using a relatively high intensity light, e.g., a 15 W light source, can produce a lower molecular weight polymer compared to a polymer produced using a lower intensity light, e.g., a 6 W light source.
[0193] In some embodiments, the UV intensity can be substrate dependent. In some embodiments, controlling the irradiation time may allow for control of the molecular weight of the polymer produced. For example, in some embodiments, longer irradiation times may result in the production of polymers with relatively lower molecular weights. Without wishing to be bound by any particular theory, the inventors believe that the irradiation time may affect the amount or concentration of radicals produced by the activated metal surface, which in turn may affect the molecular weight of the resulting polymer.
[0194] Polydispersity index (PDI) can be used as an indicator of the uniformity of particles in a mixture. PDI is another parameter that can be controlled by the method of the present invention. In various embodiments, the method of producing polymers described herein can produce polymers with narrow PDI ranges. In various embodiments, the polydispersity index (PDI) of the polymer is at least about 1, 1.05, 1.1, 1.15, 1.2, 1.25, 1.3, 1.35, 1.4, 1.45, 1.5, 1.55, 1.6, 1.65, 17, 1.75, 1.8, 1.85, 1.9, 1.95, 2, 2.05, 2.1, 2.15, 2.2, 2.25, 2.3, 2.35, 2.4, 2.45, 2.5, 2.55, 2.6, 2.65, 2.7, 2.75, 2.8, 2.95, 2.9, 2.95, 3, 3.05, 3.1, 3.15, 3.2, 3.25, 3.3, 3.35, 3.4, 3.45, The molecular weight may be 3.5, 3.55, 3.6, 3.65, 3.7, 3.75, 3.8, 3.85, 3.9, 3.95, 4, 4.05, 4.1, 4.15, 4.2, 4.25, 4.3, 4.35, 4.4, 4.45, 4.5, 4.5, 4.55, 4.6, 4.65, 4.7, 4.75, 4.8, 4.85, 4.9, 4.95, or 5 or more, and a useful range may be selected from any of these values, for example, from about 1 to about 5, preferably at least about 1.05 to about 2.5, preferably from about 1.05 to about 1.5, and more preferably from about 1.05 to about 1.2.
[0195] In preparing copolymers by the method of the present invention, the feed ratio of monomers may also play a role in determining the characteristics of the resulting copolymer. The feed ratio represents the ratio of each type of monomer in the mixture to the total amount of monomers provided to the activated surface. For example, in producing a copolymer of two types of polymerizable monomers, the feed mixture (mixture of monomers applied to the activated surface) may contain a first type of polymerizable monomer to a second type of polymerizable monomer in a ratio of, for example, 2:1.
[0196] The inventors have found that the method of the present invention can be used to prepare copolymers having glass transition temperatures (Tg) different from that of the corresponding homopolymers, and that the Tg can be controlled by adjusting the monomer feed ratio. The glass transition temperature of the copolymer can be further controlled by adjusting other parameters in carrying out the contacting step, potentially allowing the preparation of copolymers tailored for specific applications.
[0197] As noted above, the polymers and metal-polymer composites of the present invention may be useful in many different applications. In some embodiments, the parameters of the methods for producing the polymers described herein can be adapted to produce polymers suitable for use in a variety of applications.
[0198] As an example of an application of a metal-polymer composite, for example a composite including galvanized steel, may be useful in the construction industry. It may be desirable to use polymer-coated metals in the construction industry because the polymer coating may protect the metal surface from corrosion by acting as a physical barrier that retards the penetration of corrosive electrolytes to the metal surface.
[0199] In various embodiments, the methods described herein can be used to prepare metal-polymer composites that exhibit corrosion resistance. A number of methods can be used to evaluate corrosion resistance, including accelerated corrosion tests, such as the salt spray test of ASTM D610-08. The extent of corrosion can also be evaluated using ASTM D1654-08 as described herein. In some embodiments, the metal-polymer composite has a rust grade, as determined by ASTM D610-08, of at least 2, 3, or 4; and / or a rating number (R ) as determined by ASTM D1654-08. s) is at least 5, 6, or 7. In some circumstances, diffusion of corrosive species to the coating / metal interface can reduce adhesion of the coating, which can reduce the corrosion resistance of the coating over time. Thus, the inventors believe that the adhesive strength of the coating can affect the corrosion resistance of the material. As described herein, the methods of the invention can be tailored to control the adhesive strength of the polymer to the metal surface on which it is formed.
[0200] The methods of producing polymers described herein can be used to produce the polymers or metal-polymer composites of the present invention. It will be appreciated by those skilled in the art that in embodiments making metal-polymer composites, the polymer is typically attached to the metal surface of the substrate. In various embodiments, the polymer can be formed as a coating or layer on the substrate surface.
[0201] In some embodiments, the polymer produced can be recovered from the reaction mixture, e.g., in some embodiments, the polymer can be removed from the substrate surface, if desired.
[0202] In various embodiments, the polymer can be directly attached to the metal surface of the substrate. In various embodiments, the polymer can form a coating on the substrate surface. The coating can have a thickness of about 0.1, 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, 0.7, 0.8, 0.9, 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16, 17, 18, 19, 20, 21, 22, 23, 24, 25, 26, 27, 28, 29, 30, 31, 32, 33, 34, 35, 36, 37, 38, 39, 40, 41, 42, 43, 44, 45, 46, 47, 48, The thickness may be 49, 50, 55, 60, 65, 70, 75, 80, 85, 90, 95, 100, 110, 120, 130, 140, or 150 μm, and a useful range may be selected from any of these values, for example, about 0.1 to 150, 1 to 150, 0.1 to 100, 1 to 100, 5 to 100, 10 to 100, 20 to 100, 1 to 50, 5 to 50, 10 to 50, 20 to 50, or 10 to 30 μm.
[0203] In some embodiments, the methods of the present invention are for producing a metal-polymer composite by polymerizing one or more polymerizable monomers onto and / or at an activated metal surface to produce a metal polymer composite.
[0204] The direct attachment can include mechanical and / or chemical bonding, preferably mechanical and chemical bonding. In various embodiments, the chemical bonding can include one or more different types of chemical bonding. For example, in some embodiments, the chemical bonding can include covalent or non-covalent bonding, or a combination thereof. In some embodiments, the chemical bonding can include van der Waals forces, hydrogen bonding, ionic bonding, or metallic bonding, or a combination of any two or more thereof. Without wishing to be bound by a particular theory, the inventors believe that in various embodiments, the direct attachment can include, consist of, or consist essentially of non-covalent bonding, preferably hydrogen bonding, between the polymer and the metal surface.
[0205] Different types and / or strengths of bond / adhesion may be desired depending, for example, on the application in which the polymer or metal-polymer composite is to be used. In some embodiments, the direct attachment can include a bond that is weak enough to separate the polymer from the activated surface to allow for recovery of the polymer. A weak bond can be desirable, for example, when adapting the polymer for a particular application, such as a biomedical application.
[0206] In some embodiments, the direct attachment can be strong enough to prevent the polymer from separating from the activated surface, resulting in a metal-polymer composite. For example, a strong bond may be desired for materials intended for use in the construction industry. The strength of the bond, i.e., the adhesive strength between the polymer and the activated metal surface, can be measured by a number of methods, for example, using ASTM D439-14, a standard test method for rubber properties (adhesion to hard substrates), or using peel strength tests such as ASTM D4541-09. Other methods of measuring bond strength, such as ASTM D3359 described herein, will be apparent to those skilled in the art.
[0207] The bond strength can be affected by many factors, including, but not limited to, the characteristics of the metal and / or activated surface, such as the presence of irregularities on the metal and / or activated surface, the type of metal or metals present on the metal and / or activated surface, the treatment time and conditions for producing the activated surface from the metal surface, the length of time between the treatment and contacting steps, and the length of time the activated surface is contacted with one or more polymerizable monomers.
[0208] The bond strength between the metal surface and the polymer may also be affected by the type of monomer(s) and / or the concentration of the monomer(s) that are contacted with the activated surface. For example, without wishing to be bound by theory, the inventors believe that monomers that contain a high content of polar groups may increase wettability, which may increase bond strength.
[0209] In various embodiments, the bond between the activated metal surface and the polymer is characterized by a tape adhesion test rating of at least 2B, preferably 3B, preferably 4B, as measured by AST D3359.
[0210] In various embodiments, the bond between the activated metal surface and the polymer has a peel strength as measured by ASTM D4541-09 of about 1.5, 1.6, 1.7, 1.8, 1.9, 2.0, 2.1, 2.2, 2.3, 2.4, 2.5, 2.6, 2.7, 2.8, 2.9, 3.0, 3.1, 3.2, 3.3, 3.4, 3.5, 3.6, 3.7, 3.8, 3.9, 4, 4.1, 4.2, 4.3, 4.4, 4.5, 4.6, 4.7, 4.8, 4.9, 5.0, 5.1, 5.2, 5.3, 5.4, 5.5, 5.6, 5.7, 5.8, 5.9, 5.1, 5.2, 5.3, 5.4, 5.5, 5.6, 5.7, 5.8, 5.9, 5.8, 5.9, 5.1, 5.2, 5.4, 5.5, 5.6, 5.8, 5.9, 5.1, 5.2, 5.4, 5.5, 5.6, 5.9, 5.1, 5.2, 5.5, 5.6, 5.9, 5.1, 5.2, 5.3, 5.4, 5.5, 5.7, 5.8, 5.9, 5.1, 5.2, 5.4, 5.5, 5.8, 5.9, 5.1, 5.2, 5.5, 5.6, 5.7, 5.8, 5.9, 5.1, , 4.9, 5, 5.5, 6, 6.5, 7, 7.5, 8, 8.5, 9, 9.5, or 10 MPa, and useful ranges can be selected from any of these values, such as from about 1.5 to 10, 2.5 to 10, 1.5 to 7.5, 2.5 to 7.5, 1.5 to 5, or 1.5 to 4 MPa, preferably from about 2.5 to about 5 MPa. In other embodiments, where a weak bond may be desired, such as to allow easy removal of the polymer from the activated surface, the metal-polymer composite has a peel strength as measured by ASTM D4541-09 of less than 1.5 MPa, such as less than 1.4, 1.3, 1.2, 1.1, 1.0, 0.9, 0.8, 0.7, 0.6, or 0.5 MPa.
[0211] In some embodiments, the bond strength between the activated surface and the polymer can result in a relatively strong bond, thereby producing a metal-polymer composite, hi some embodiments, the bond between the activated surface and the polymer can be a relatively weak bond, thereby allowing the polymer to be separated from the activated surface.
[0212] The metal surface may be subjected to one or more pre-treatment steps (i.e. steps prior to treating the metal surface) prior to undergoing the above treatment to produce the activated metal surface, such as one or more physical, mechanical and / or chemical treatments, such as plasma treatment or surface roughening, such as by etching and / or patterning, grinding, blasting, phosphating or using photolithography.
[0213] The pretreatment step can be selected to increase or decrease the surface area of the metal surface, as desired. In some embodiments, the surface can be subjected to a surface roughening step to increase the surface area of the metal surface. Examples of suitable surface roughening steps include mechanical treatments (e.g., grinding, sanding, blasting, e.g., sand / grit blasting), chemical treatments (e.g., etching), and plasma treatments. Without wishing to be bound by this, it is believed that increasing the surface area of the metal surface can result in an activated metal surface having a higher concentration of one or more compounds capable of initiating polymerization on the surface compared to a surface that has not been subjected to a pretreatment step to increase the surface area. In this way, the increased concentration of compounds capable of initiating polymerization can allow the desired degree of conversion of one or more monomers to polymer to be achieved more quickly compared to a surface that has not been subjected to a pretreatment step. Additionally or alternatively, increasing the surface area of the metal surface can reduce the time required to produce an activated surface having a desired concentration of one or more compounds capable of initiating polymerization compared to the absence of the surface area-increasing pretreatment step. Additionally or alternatively, increasing the surface area of the metal surface can produce an activated surface having a surface morphology that enhances mechanical bonding with the polymer formed during the contacting step.
[0214] Prior to subjecting the metal surface to treatment to produce an activated surface, the metal surface may be pretreated to modify the characteristics of the metal surface, for example to enhance or weaken (as desired) the bonding of the polymer formed during the contacting step.
[0215] In some embodiments, the metal surface can be modified to enhance the bonding of the polymer produced in the contacting step in order to produce a metal-polymer composite. In other embodiments, the metal surface can be modified to weaken the bonding of the polymer produced in a subsequent contacting step in order to produce a polymer that can be removed after polymerization from the activated metal surface, e.g., a polymer that has a relatively low peel strength as measured by ASTM D4541-09.
[0216] In various embodiments, the metal surface can be modified by physical, physicochemical, and / or chemical methods. The metal surface can be subjected to a pretreatment step, e.g., a plasma, laser, chemical, or other pretreatment step, to increase the wettability and / or free energy of the metal surface and / or modify the surface morphology to enhance bonding (e.g., mechanical bonding) between the polymer and the surface.
[0217] Surface roughening, e.g., by etching, heat treatment, and / or patterning, can be used to modify the surface properties of the metal surface and to enhance the bonding of the polymer to the metal surface, e.g., by enhancing the mechanical bond between the polymer and the metal surface.
[0218] In various embodiments, the metal surface can be modified by plasma treatment. In some embodiments, the plasma treatment can improve the wettability, free energy, and / or surface morphology of the metal surface. Without wishing to be bound by a particular theory, the inventors believe that the improved wettability, free energy, and / or surface morphology may be due to the generation of oxygen-containing functional groups, such as hydroxyl groups, by plasma treating the metal surface. Many plasma treatment methods are known in the art, including, for example, atmospheric pressure plasma treatment. Other plasma treatments will be apparent to one of ordinary skill in the art.
[0219] In various embodiments, the metal surface may be subjected to a cleaning step as a pretreatment step prior to carrying out the treatment step. Cleaning may be carried out, for example, using a solvent such as methanol or ethanol, or using a mild soap, ammonia, or phosphate solution.
[0220] In some embodiments, the metal surface may be modified by more than one method (pre-treatment step) before performing the treatment step. In some embodiments, the metal surface may be modified by two, three, four, five or more methods before performing the treatment step. The methods may be the same or different. For example, the metal surface may be cleaned and then modified by plasma treatment, or the metal surface may be subjected to two cleaning steps and then modified by a plasma treatment step. EXAMPLES
[0221] Unless otherwise stated, Materials and Methods Section 1 below applies to all examples. 1. Materials and Methods 1.1 Reagents and equipment Unless otherwise specified, all monomers, polymers, and other reagents used in this study were purchased from Sigma-Aldrich and used as received.
[0222] The galvanized steel and zinc aluminium were purchased from New Zealand Steel. The galvanized steel had a zinc coating of approximately 20-25 μm and the zinc aluminium had a coating of 55% Zn and 45% Al, approximately 35-40 μm thick.
[0223] Methyl methacrylate (MMA, 99%, Sigma-Aldrich), butyl methacrylate (BMA, 99%, Sigma-Aldrich), methyl acrylate (MA, 99%, Sigma-Aldrich), and butyl acrylate (BA, 99%, Sigma-Aldrich) were purified and stored in a nitrogen atmosphere in a cool place until use. UV lamps (6 W (UV 1) and 15 W (UV 2)) were obtained from UVTech Systems, Inc. A 15 W UV lamp (365 nm) and a 6 W UV lamp (365 nm) were obtained from UVTech Systems, Inc. 1.2 Monomer purification Methyl methacrylate (MMA), butyl methacrylate (BMA), methyl acrylate (MA), and butyl acrylate (BA) were washed three times with 10 wt% sodium hydroxide (NaOH), followed by deionized water until the monomers were neutral, then dehydrated overnight with sodium sulfate (Na2SO4), and distilled under reduced pressure.
[0126] The purified monomers were stored refrigerated at 4 °C under nitrogen until use. Poly(ethylene glycol) methyl ether methacrylate (PEGMEMA) and diurethane dimethacrylate (DUDMA) were used as received. 1.3 Heat treatment of galvanized steel substrate The substrates, in the form of sheets with a thickness of 0.5 mm, were all placed in a 15 mm × 15 mm square tube (geometric area 225 mm 2 The substrates were then ultrasonically cleaned in ethanol and distilled water.
[0224] Heat treatment of each substrate was carried out at 400° C. or 600° C. under ambient atmosphere for 2 hours. 1.4 General Procedure for Polymerizing Vinyl Monomers Homopolymerization Homopolymerization of methyl methacrylate (MMA) was carried out as follows: MMA (9.4 g, 0.094 mol) and heat-treated substrate (15 mm × 15 mm) were placed in a 20 mL vial, and the reaction mixture was irradiated with UV light (6 W or 15 W, λ = 350 nm) for 1 h under ambient atmosphere.
[0225] The vials were sealed and kept in a constant temperature (60°C) oven for varying times (0-48 hours). Approximately 10 mg of sample was periodically removed to measure the monomer conversion. 1 Detected by 1 H NMR.
[0226] Polymerizations of the other monomers (MA / BMA / BA / DUDMA / PEGMEMA) were carried out following the same procedure as described above for MMA. copolymerization The copolymerization procedure of vinyl monomers was carried out as follows: Mixtures of methyl methacrylate and butyl methacrylate in different ratios were charged into 20 mL vials, and the reaction mixtures were irradiated with UV light (15 W, λ = 350 nm) for 1 h.
[0227] The vials were sealed and kept in a constant temperature (60°C) oven for varying times (8-48 h). Block Copolymerization The procedure for block copolymerization of vinyl monomers is as follows: After polymerization of MMA (described in section 1.4 above), the resulting polymer (PMMA) was charged into fresh monomer solution (MM or BMA) and the reaction mixture was kept at 60°C for different times to obtain the block copolymers. 1.5 Characterization Method The chemical composition of the substrate surface was measured by X-ray photoelectron spectroscopy (XPS).
[0228] Investigation of the surface morphology and qualitative elemental chemical analysis of the substrates were carried out by scanning electron microscopy (SEM) coupled with energy dispersive X-ray spectroscopy (EDS). Characterization of the crystallinity and the crystalline phases present in the substrates was carried out by X-ray diffraction (XRD).
[0229] The production of radicals was measured by fluorescence spectroscopy (FL) using terephthalic acid (TA) as a probe. The changes of chemical species during polymerization were monitored by Fourier transform infrared spectroscopy (FTIR).
[0230] The structures of the monomers and polymers were determined by nuclear magnetic resonance (NMR) spectroscopy using CDCl3 as the solvent. The molecular weight and molecular weight distribution of the polymer were determined by size exclusion chromatography (SEC).
[0231] The glass transition temperatures of the polymer samples were measured by temperature modulated differential scanning calorimetry (MDSC). The degradation properties of the polymers were measured by thermogravimetric analysis (TGA).
[0232] Details of these characterization techniques and experimental parameters are provided below. X-ray photoelectron spectroscopy (XPS) The chemical composition of the substrate surface before and after the heat treatment was analyzed by XPS using a Kratos Axis DLD X-ray photoelectron spectrometer at the University of Auckland. -9 Analyzed in torr.
[0233] The modified Auger parameter for Zn (α'Zn) was measured and compared with literature values from C.D. Wagner, Analytical Chemistry, 44 (1972) 967-973 to identify the zinc compounds present. A 150 W monochromated Al(Κα) X-ray source (1486.6 eV) was used for collection of the XPS data, with pass energies of 160 eV for survey spectra and 20 eV for high-resolution spectra.
[0234] All XPS analyses were performed using an attached charge neutralizer. The C 1s peak of natural carbon at 284.8 eV was used as the reference and for charge correction of all spectra. Data were processed using Casa XPS: peak areas were measured and normalized using linear or Shirley background subtraction and Scofield relative response factors. Energy Dispersive X-ray Spectroscopy (EDS) Surface morphology and qualitative elemental chemical analysis of the substrates were performed by scanning electron microscopy (SEM) equipped with energy dispersive X-ray spectroscopy (EDS) using a Field Electron and Ion (FEI) Quanta 200 field emission SEM-EDS. A platinum thin film was formed on the substrate by physical vapor deposition (PVD) under vacuum. The substrates were then observed in secondary electron mode at an accelerating voltage of 10 kV and in backscattered electron mode at an accelerating voltage of 20 kV. X-ray diffraction Characterization of the crystallinity and the crystalline phases present in the substrates was carried out using X-ray diffraction (XRD).
[0235] The change in the crystal characteristics of the reference basic zinc carbonate powder after heat treatment was investigated using XRD. XRD patterns of the basic zinc carbonate powder before and after heat treatment were collected using an X-ray diffractometer (Bruker D8) equipped with a Cu-Kα radiation source (wavelength = 1.5418 Å). The spectra were collected with a scan angle (2θ) range of 10 to 80°, a step angle (2θ) of 0.05°, and a measurement time of 10 s / step. Fourier Transform Infrared Spectroscopy (FTIR) The changes in the compounds during polymerization were monitored by Fourier transform infrared spectroscopy (FTIR).
[0236] Attenuated total reflectance (ATR)-FTIR (ATR-FTIR) was used to measure the residual double bonds to determine the degree of completion of the reaction from monomer to polymer. ATR-FTIR was performed on a Nicolet 8700 FTIR spectrometer using a diamond crystal ATR attachment. -1 The spectra were recorded with a resolution of 4 cm -1 The number of calculations was set to 64. nuclear magnetic resonance (NMR) The structure of the monomer used in the reaction and the resulting polymer are 1 The reaction completion and consumption of monomer during polymerization were also analyzed by H NMR spectroscopy. 1 The polymerization was monitored by H-NMR spectroscopy. The reaction completion was calculated by measuring the methylene (=CH2) protons remaining after polymerization. The monomer consumption rate was calculated by comparing the integral ratio of the methylene (=CH2) protons to the methoxyl (-OCH3) protons of the polymer. 1 H-NMR spectra were recorded on a Bruker Advance 400 MHz spectrometer using CDCl3 as the solvent. Chemical shifts were determined relative to tetramethylsilane (TMS) as an internal standard. Size Exclusion Chromatography (SEC) The molecular weight, molecular weight distribution, and polydispersity index (PDI) of the polymers were measured by size-exclusion chromatography (SEC) using a Waters model 510 pump, a Waters model 486 refractive index detector, and two Styragel HR 4.5 μm columns. THF was used as the eluent at 30 °C with a flow rate of 1.0 mL / min, and the columns were calibrated with polystyrene standards obtained from Polymer Laboratories. Samples were filtered through a 0.2 μm pore size microfilter before injection. Modulated Temperature Differential Scanning Calorimetry (MDSC) Thermal analysis of polymer samples was performed by temperature modulated differential scanning calorimetry (MDSC) using a TA Instruments model Q1000. Heat flow curves were normalized to the polymer mass only, not the total sample mass. Two heating scans and one cooling scan were performed from 35 to 250 °C at a rate of 2.5 °C / min, with a modulation temperature amplitude of ±1 °C and a modulation period of 60 s. The sample mass was approximately 7-8 mg, and the cell was purged with nitrogen gas at 50 mL / min during the scans.
[0237] A second heating scan was used to determine the glass transition data from the reversible heat flow curves so that all samples were subjected to a similar thermal history. The glass transitions (Tg) reported were determined from the half-height temperature of the transition step, i.e., by identifying the temperature range corresponding to the transition from the glassy to the rubbery state and taking the midpoint of this temperature range. Thermogravimetric analysis (TGA) The decomposition characteristics of the polymer were measured by thermogravimetric analysis (TGA) using a TGA Q(5000) instrument. The measurements were performed under a nitrogen atmosphere, with a temperature range of 35–600°C and a heating rate of 20°C min -1 The maximum process rate (Tmax) and weight loss (Dm) were determined using TA Instruments Universal Analysis 2000 software. Fluorescence spectroscopy (FL) Without wishing to be bound by any particular theory, the inventors believe that terephthalic acid (TA) reacts with hydroxyl radicals to produce a highly fluorescent product, 2-hydroxyterephthalic acid (TAOH) [1]. TAOH exhibits a characteristic fluorescence peak at around 425 nm. The intensity of this fluorescence peak is proportional to the amount of hydroxyl radicals produced in solution [2]. Thus, the production of this radical can be determined by fluorescence spectroscopy using terephthalic acid (TA) as a probe for hydroxyl radical detection.
[0238] The fluorescence spectra of each sample tested were recorded on a PerkinElmer LS 55 fluorescence spectrophotometer. 1.6 General procedure for constructing a TAOH calibration curve To determine the relationship between TAOH concentration and fluorescence intensity measured for a particular sample, a calibration curve was constructed as follows: Aqueous solutions of 2-hydroxyterephthalic acid (TAOH) with known concentrations between 0.5 and 4 mM (solutions 1–8) were prepared in aqueous NaOH (0.001 mol / L, pH=11, in distilled water) as described below.
[0239] Solution 1: 1.457 mg of TAOH was dissolved in NaOH solution in a 2000 mL volumetric flask. This solution corresponds to a 4 μM TAOH solution (calculated based on the following information [M(TAOH)=182.13 g.mol-1], i.e. (0.001457 g / 182.13) / 2 x 1000,000). 20 mL of this TAOH solution 1 was added to a small container (flask, vial).
[0240] Solution 2: 10 mL of solution 1 (4 μM) was placed in another small container and diluted with 10 mL of NaOH solution to prepare a final solution with a TAOH concentration of 2 μM. Solution 3: 10 mL of solution 2 (2 μM) was placed in another small container and diluted with 10 mL of NaOH solution to prepare a final solution with a TAOH concentration of 1 μM.
[0241] Solution 4: 10 mL of solution 3 (1 μM) was placed in another small container and diluted with 10 mL of NaOH solution to prepare a final solution with a TAOH concentration of 0.5 μM. Solution 5: A final solution with a TAOH concentration of 3 μM was prepared by placing 10 mL of solution 1 (4 μM) and 10 mL of solution 2 (2 μM) in a small container.
[0242] Solution 6: 10 mL of solution 5 (3 μM) was placed in another small container and diluted with 10 mL of NaOH solution to prepare a solution with a TAOH concentration of 1.5 μM. Solution 7: 10 mL of solution 3 (2 μM) and 10 mL of solution 5 (3 μM) were placed in a small container to prepare a final solution with a TAOH concentration of 2.5 μM.
[0243] Solution 8: 10 mL of solution 1 (4 μM) and 10 mL of solution 5 (3 μM) were placed in a small container to prepare a final solution with a TAOH concentration of 3.5 μM. The fluorescence (FL) instrument measured the emission wavelength at 315 nm for each of solutions 1-8, and the FL intensity was measured at 425 nm, starting with the least concentrated solution, using a PerkinElmer LS 55 fluorescence spectrophotometer.
[0244] For each of solutions 1 to 8, the fluorescence intensity values measured at 425 nm were plotted on a graph, with fluorescence intensity (measured in absorbance units (au)) on the y-axis and the solution concentration corresponding to the fluorescence intensity measurement values on the x-axis, to create the calibration curve shown in Figure 16. 1.7 General procedure for testing the generation of TAOH by activated metal surfaces Step 1 Terephthalic acid (TA) stock solution was prepared in dilute NaOH aqueous solution (0.001 mol / L, in distilled water) to ensure dissolution. The pH value of the NaOH solution was 11. TA stock solution was prepared by dissolving 5 mg of TA in NaOH solution in a 1 L volumetric flask, and the resulting TA stock solution was stored in the dark at room temperature (20-25 °C) until use. The TA concentration of the stock solution was 30.096 μM (0.005 g in 1 L), calculated based on the following information: [M (TA) =166.13 g.mol -1 ], or (0.005g / 166.13) x 1000,000. Step 2 A control sample was prepared by adding 15 mL of TA stock solution (prepared as described in step 1 above) to an empty container.
[0245] The control sample was then left for 1 hour in the dark at room temperature. After 1 hour, 2 mL of the control sample was withdrawn and analyzed using a PerkinElmer LS 55 fluorescence spectrophotometer. The excitation spectrum was monitored at 315 nm and the emission spectrum was measured at 425 nm. The fluorescence intensity at 425 nm generated by the control sample was recorded and used in step 5 described below. Step 3 The substrates, in the form of sheets with a thickness of 0.5 mm, were all placed in a 15 mm × 15 mm square tube (geometric area 225 mm 2 The substrates were then ultrasonically cleaned in ethanol and distilled water.
[0246] The heat treated substrates were heat treated in a furnace at 400° C. or 600° C. under ambient atmosphere for 2 hours. Step 4 To test the ability of the substrate surface to generate TAOH in the presence of TA, 15 mL of TA stock solution (prepared as described in step 1 above) was added to a substrate sample (prepared as described in step 3 above) in a vial.
[0247] The sample was left in the dark at room temperature for 1 hour and then irradiated with UV (365 nm, 15 W) at room temperature (20-25 °C). After 1 hour, 2 mL of the reaction solution was withdrawn and analyzed using a PerkinElmer LS 55 fluorescence spectrophotometer. The excitation spectrum was monitored at 315 nm, and the emission spectrum was measured at 425 nm. The fluorescence intensity at 425 nm generated from the substrate sample was recorded and used in step 5 described below. Step 5 The 425 nm fluorescence intensity of the control sample (measured in step 2) was subtracted from the 425 nm fluorescence intensity of the substrate sample measured in step 4 to obtain the corrected 425 nm fluorescence intensity of the substrate sample. "Corrected fluorescence intensity" is the fluorescence intensity of the substrate after correction for the background fluorescence intensity, i.e., the fluorescence intensity of the control sample that does not contain a substrate with an activated surface.
[0248] The corrected fluorescence intensity at 425 nm of the substrate sample is shown by the markers on the calibration curve in Figure 16 (obtained as described in section 1.6 above). The concentration of TAOH corresponding to the fluorescence intensity was read off the calibration curve. The concentration of TAOH generated in the presence of TA on the surface of this substrate sample (prepared and tested as described in steps 3-5 above) is the background corrected concentration of TAOH in the control sample that does not contain a substrate with an activated surface. 2. Example 1 - Heat treatment and property evaluation of galvanized steel 2.1 Overview Galvanized steel is steel coated with a zinc-containing layer to protect it from corrosion. Without wishing to be bound by any particular theory, the inventors believe that zinc carbonate and basic zinc carbonate may form on the surface of galvanized steel when the zinc layer comes into contact with atmospheric oxygen, carbon dioxide, and water. Heat treatment of galvanized steel and other substrates with coatings containing zinc can produce ZnO, for example, by oxidizing metallic zinc and / or decomposing zinc carbonate or basic zinc carbonate that may be present in the zinc layer.
[0249] This example describes conditions that can be used to produce ZnO. To determine the heat treatment temperature, pyrolysis of reference basic zinc carbonate powder was carried out.
[0250] The chemical composition of the galvanized steel surface before and after heat treatment was investigated by XPS. The modified Auger parameter for Zn (α'Zn) was measured and compared with literature values to identify the zinc compounds present. [3] The surface morphology and qualitative elemental chemistry of the substrates were also detected by SEM-EDS. 2.2 Experimental Method Heat treatment and characterization of galvanized steel was carried out as described in sections 1.4 and 1.6. Thermal decomposition of reference basic zinc carbonate was carried out by heat treatment of basic zinc carbonate powder at different selected temperatures (100°C, 200°C, 300°C, and 400°C) for 2 h.
[0251] Thermogravimetric analysis of basic zinc carbonate powder was carried out using a TGA Q 500 instrument in air flow (50 mL / min). Approximately 15 mg of sample was heated to 600 °C at a rate of 10.0 °C / min in an open platinum crucible. DTG curves were also recorded to further analyze the decomposition process of basic zinc carbonate. The products of thermal decomposition were investigated by XRD analysis. 2.3 Results and Discussion 2.3.1 Chemical species present on the substrate surface To investigate the effect of heat treatment temperature on the formation of ZnO, the thermal decomposition of reference basic zinc carbonate powder was carried out.
[0252] The decomposition reaction of basic zinc carbonate to produce solid zinc oxide and gaseous carbon dioxide is shown in the following equation (1), with the theoretical maximum weight loss being 25.9%.[4][5][6] Zn5(CO3)2(OH)6→5ZnO+2CO2+3H2O (1) Figure 1 shows the TGA-DTG curves of basic zinc carbonate pyrolyzed in air at a rate of 10°C / min. The curves show that basic zinc carbonate pyrolyzed in two stages, with the weight loss rates maximizing at 46°C and 262°C. The small weight loss up to 100°C may be due to the loss of physically adsorbed water. The further weight loss starting at about 210°C may be due to the loss of water from basic zinc carbonate as well as the loss of carbon dioxide. Without wishing to be bound by any particular theory, the inventors believe that the final remaining solid material may be zinc oxide that did not decompose. The total mass loss from pyrolysis was 24.6±0.1%, which is in good agreement with the theoretical value of 25.9% determined above.
[0253] Selected basic zinc carbonate samples annealed at different temperatures (100-400°C) were analyzed by powder X-ray diffraction (Figure 2). The diffraction patterns of basic zinc carbonate powders annealed at 100°C and 200°C shown in Figure 2 indicated the presence of zinc oxide (Joint Committee on Powder Diffraction Standards (JCPDS) 36-1451), zinc carbonate (JCPDS 83-1765), and basic zinc carbonate phases (JCPDS 19-1458). The diffraction patterns of basic zinc carbonate powders annealed at 300°C and 400°C shown in Figure 2 were consistent with the diffraction pattern of zinc oxide (JCPDF 36-1451), which suggested that the powders annealed at 300°C and 400°C were ZnO powders with a hexagonal wurtzite structure phase.
[0254] TGA-DTG and XRD analyses showed that basic zinc carbonate decomposed in a two-step process by heat treatment in air, with the decomposition product being ZnO. The first step was the loss of physically adsorbed water at about 100°C. The majority of the decomposition occurred in the second step, with simultaneous dehydration and decarbonation from about 210°C, and the maximum weight loss reached 24.6% at about 400°C. Accordingly, heat treatment was carried out at or above 400°C for 2 hours under ambient atmosphere to produce heat-treated galvanized steel (TTGS) and heat-treated zinc potassium (TTZnAl). 2.3.2 Characterization of galvanized steel XRD was performed to determine the crystalline phases of galvanized steel before and after heat treatment. Comparison of the measured XRD spectra with reference spectra from the JCPDS database showed that only metallic zinc (JCPDS 4-831) was detected in both UTGS and TTGS(600). After heat treatment, the zinc (201) peak on UTGS disappeared, while a new zinc (004) peak was detected on TTGS(600). This result therefore suggests that the growth direction of Zn changed due to heat treatment. The finding that the only detectable phase was Zn is consistent with other findings. Neither zinc oxide, zinc carbonate, nor basic zinc carbonate was detected by XRD in either untreated or heat-treated galvanized steel. It is still possible that these compounds are present on the galvanized steel surface, but are not detectable by XRD, possibly because they are present in relatively small amounts at the surface or are not highly crystalline.
[0255] Since the zinc compounds on the galvanized surface may be too thin for bulk-sensitive methods, sophisticated surface analytical techniques such as XPS were employed to investigate the chemical composition of the galvanized steel before and after heat treatment. XPS spectra of reference ZnO and basic zinc carbonate compounds were collected. The reference ZnO powder was annealed immediately before analysis to reduce residual zinc carbonate interference with the ZnO signal.
[0256] The XPS C 1s spectra obtained from the reference ZnO and basic zinc carbonate compounds are shown in Figures 3(a) and 4(a), respectively. Table 1 shows the relative atomic composition of the C 1s components based on these spectra. The peaks at 284.8 eV in Figures 3(a) and 4(a) were both assigned to naturally deposited carbon, which was used to correct the binding energies (BE) of the other components. The peaks at 286.1 eV in Figures 3(a) and 4(a) were both assigned to CO bonds due to contamination. The higher binding energy peaks of 288.7 eV and 289.7 eV in Figure 4(a) were in good agreement with the reported values for carbonate and hydroxide carbonate, respectively. The peak at 291 eV was assigned to adsorbed CO2. It is noteworthy that carbonate peaks were also found to appear in the annealed reference ZnO (Figure 3(a)).
[0257] [Table 1]
[0258] Figures 3(b) and 4(b) show the XPS O 1s spectra of the reference ZnO and basic zinc carbonate compounds, respectively. Referring to Figure 3(b), the peak at 529.9 eV is assigned to oxygen of zinc oxide, which is in good agreement with the literature value. The peaks at 530.7 eV and 531.7 eV (Figures 3(b) and 4(b)) are assigned to carbonate and basic carbonate, respectively, based on the literature value. The peak at 532.6 eV (Figure 3(b)) can be assigned to hydroxide.
[0259] The most intense peaks of the annealed ZnO reference sample were ZnO peaks, while the most intense peaks of the zinc basic carbonate reference sample corresponded to zinc carbonate and zinc basic carbonate in the O 1s spectrum of Figure 4(b). The O 1s spectrum of the ZnO reference (shown in Figure 3(b)) further supports the presence of Zn2CO3 and Zn5(CO3)2(OH)6 in the annealed ZnO reference powder.
[0260] XPS spectra of the reference zinc oxide powder and the reference basic zinc carbonate powder, Zn 2p 3 / 2; and Zn L3M45M45, were also recorded and are shown in Figures 3(c), 3(d), and 4(c), 4(d), respectively.
[0261] Table 2 shows the relative elemental composition of the O 1s components based on ZnO and basic zinc carbonate for reference.
[0262] [Table 2]
[0263] Without wishing to be bound by any particular theory, the inventors believe that the binding energy shift of the Zn 2p3 / 2 orbitals of zinc species is very small, and therefore it may be difficult to distinguish between different Zn species. Therefore, it is preferred to use the modified Auger parameter (α') for the identification of Zn species.
[0264] Binding energies of the Zn 2p 3 / 2 peaks of ZnO and basic zinc carbonate for reference, Zn L3M 45 M 45 The kinetic energies of the Auger peaks, along with the corresponding modified Auger parameters (α'), are compared with the data in the NIST XPS database in Table 3. The modified Auger parameters for the reference ZnO and basic zinc carbonate compound were 2010.2 eV and 2009.3 eV, respectively. The modified Auger parameters (α') of the reference samples were very close to those reported in the NIST XPS database and other literature.
[0265] [Table 3]
[0266] The reference spectra described above were used as a baseline for peak deconvolution of the galvanized steel samples. That is, to increase the accuracy of the curve fitting and chemical characterization, the spectra of the pure reference compounds were used for fitting and characterization of the experimental XPS spectra. The XPS surveys of untreated galvanized steel (UTGS), galvanized steel heat treated at 400°C (TTGS(400)), and galvanized steel heat treated at 600°C (TTGS(600)) are shown in Figure 5.
[0267] Table 4 shows the elemental composition of the galvanized steel surface before and after heat treatment. Along with carbon, oxygen, and zinc, small amounts of chromium, phosphorus, and calcium were also detected on the steel sample surface. The signals of Zn and O were found to increase with the annealing temperature. In contrast, the intensity of the C signal decreased with the annealing temperature.
[0268] [Table 4]
[0269] For UTGS, TTGS(400), and TTGS(600), C 1s, O 1s, Zn 2p 3 / 2, and Zn L3M 45 M 45 A higher resolution spectrum of was recorded. The C 1s and O 1s spectra are shown in Figures 6 and 7, respectively. Peak positions determined from reference spectra of ZnO and basic zinc carbonate samples were used in fitting the data.
[0270] The C 1s and O 1s spectra of the galvanized steel samples with fitted compositions are in good agreement with those of the reference ZnO and basic zinc carbonate samples. The most intense peaks in the C 1s spectra of UTGS, TTGS(400), and TTGS(600) are likely due to naturally deposited carbon, a common surface contaminant. The C 1s spectra indicate the presence of zinc carbonate and basic zinc carbonate on the surface of UTGS and TTGS(400), while only naturally deposited carbon was detected in TTGS(600). The signal intensity of zinc carbonate decreased with increasing annealing temperature, suggesting the decomposition of zinc carbonate compounds on the galvanized steel surface.
[0271] In the O 1s spectra shown in Fig. 7, most of the peaks in UTGS and TTGS(400) were derived from zinc carbonate and basic zinc carbonate. The relative elemental ratios of O 1s in Fig. 7(b) indicated that about 6% and 38% of oxygen existed as ZnO in TTGS(400) and TTGS(600), respectively. These results indicated the presence of basic zinc carbonate on the surface of all galvanized steel substrates, and also indicated the formation of ZnO on the surface of TTGS(400) and TTGS(600).
[0272] Table 5 shows the relative elemental composition of the C 1s components based on UTGS, TTGS(400), and TTGS(600).
[0273] [Table 5]
[0274] Table 6 shows the relative elemental composition of the O 1s components based on UTGS, TTGS(400), and TTGS(600).
[0275] [Table 6]
[0276] [Table 7]
[0277] The modified Auger parameters (α') of Zn on untreated and heat-treated galvanized steel are shown in Table 7. The modified Auger parameters were compared with data from the NIST XPS database and our reference samples (Table 3). The small shift in binding energy of the Zn 2p3 / 2 orbitals and the Zn L3M 45 M 45 In the spectra, the quantification of the mixture of metals, metal oxides, and metal carbonates was difficult because of the overlapping spectra. 45 M 45 The most intense peaks of each were used for the calculation. The modified Auger parameter of UTGS was 2009.2 eV, which was consistent with the values of Zn5(CO3)2(OH)6 from our reference and the NIST XPS database. This agreement suggested the presence of Zn5(CO3)2(OH)6 on the surface of UTGS.
[0278] The modified Auger parameter of TTGS(400) was 2009.5 eV, which was intermediate between the α' of ZnO (2010.2 eV) and that of Zn5(CO3)2(OH)6 (2009.3 eV). This value could be attributed to a mixture of ZnO and Zn5(CO3)2(OH)6 on the surface of TTGS(400). However, the modified Auger parameter value of TTGS(400) did not allow for unambiguous identification of zinc compounds on the surface.
[0279] The modified Auger parameter of TTGS(600) is 2010.0 eV, which is in good agreement with the reference ZnO sample, indicating the presence of ZnO on TTGS(600).
[0280] From the analysis of XPS spectra and modified Auger parameters, it was concluded that zinc carbonate and basic zinc carbonate were present on the surface of all galvanized steel samples and it was suggested that both heat-treated galvanized steel surfaces contained a complex mixture of zinc compounds with some ZnO present. The amount of ZnO on the heat-treated galvanized steel surfaces increased with the heat treatment temperature, while the carbonate compounds decreased with increasing temperature. 2.3.3 Morphology of galvanized steel samples before and after heat treatment The morphology and qualitative elemental composition of the galvanized steel before and after heat treatment were analyzed by SEM-EDS. Secondary electron images (SEI) of the galvanized steel before and after heat treatment are shown in Figure 10.
[0281] The UTGS sample exhibits a typical corrugated morphology, consisting of plateaus, valleys, and dispersed pores (Fig. 10(a)). The surface topography of TTGS(400) is similar as shown in Fig. 10(b), but it has more pores than UTGS. A dramatic change was observed after heat treatment at 600 °C; TTGS(600) contained grains in the range of 1–5 μm (Fig. 10(c)). This change may be due to the thermal decomposition of zinc compounds and the oxidation of zinc on the galvanized steel surface.
[0282] To further investigate the pore structure, secondary electron images (SEI) of the grains and substrate of both untreated and heat-treated galvanized steel were taken at higher magnification. As shown in Figure 11 (UTGS) and Figure 12 (TTGS(400)), both UTGS and TTGS(400) showed irregular micrometer-scale pores, with no detectable nanostructures inside the pores. Single and aggregated spherical nanoscale grains were observed in both UTGS and TTGS(400), with no significant difference in shape and size. SEM images of galvanized steel annealed at 600°C (Figure 13) showed that TTGS(600) was composed of pebble-shaped, aggregated spherical, and needle-shaped grains of nanoscale size.
[0283] To analyze the elemental composition of the samples, backscattered electron images and corresponding EDS spectra were taken from different regions of the samples. Backscattered electron images and corresponding EDS spectra of UTGS, TTGS(400), and TTGS(600) (see FIG. 14). From this analysis, it was found that the surfaces of all three substrates were mainly composed of zinc with trace amounts of Fe, Pb, Al, Cr, and Ca, as shown in Table 8 below.
[0284] [Table 8]
[0285] The Fe concentration (15%) in the TTGS(600) sample was higher than that in the UTGS (1%) and TTGS(400) (1%) samples. Also, the C concentration (5%) in the UTGS sample was higher than that in the TTGS(400) (4%) and TTGS(600) (1%) samples. Conversely, the O concentration increased with increasing annealing temperature. These results are consistent with the results of XPS analysis, which may suggest that basic zinc carbonate on the galvanized steel surface was decomposed to form ZnO. 2.4 Conclusion A comparative study of the surface chemistry of galvanized steel before and after heat treatment was carried out using XPS and SEM-EDS. An investigation of the thermal decomposition of reference basic zinc carbonate powder showed that ZnO was produced by thermal decomposition of basic zinc carbonate. This was used to determine the temperatures that can be used for the heat treatment of galvanized steel substrates.
[0286] XPS spectra and modified Auger parameters indicate the presence of zinc carbonate and basic zinc carbonate on the surface of all galvanized steel samples, and confirm that both heat-treated galvanized steel surfaces (TTGS(400) and TTGS(600)) contain a complex mixture of zinc compounds with some ZnO present.
[0287] The XPS results also showed that the amount of carbonate compounds decreased and the amount of ZnO increased with increasing heat treatment temperature, which may be due to the thermal decomposition of zinc carbonate and basic zinc carbonate or the oxidation of metallic zinc to form ZnO.
[0288] SEM results showed that the morphology of galvanized steel changed upon heat treatment. More pores were observed on the surface of TTGS(400) than UTGS, and no nanostructure was found inside the pores. Single and aggregated nanoscale spherical particles were observed on the untreated and heat-treated galvanized steel substrates. Heat treatment at 600°C showed a more obvious morphological change. TTGS(600) consisted of nanoscale sized pebble-shaped particles, aggregated spherical particles, and needle-shaped particles. 3. Example 2 - Investigation of surface-initiated controlled radical polymerization (CRP) of vinyl monomers using galvanized steel as a photoinitiator The above examples have demonstrated the formation of ZnO on the heat-treated galvanized steel surface. In this example, the photoinitiation efficiency of ZnO on the heat-treated galvanized steel (TTGS) surface was investigated.
[0289] Polymerization of several vinyl monomers was carried out using TTGS substrate as photoinitiator. The polymerization mechanism was elucidated through a series of experiments. To understand the polymerization kinetics, the monomer consumption during polymerization was monitored. Some of the important properties of the resulting polymers were measured. 3.1 Experiments 3.1.1 Materials Methyl methacrylate (MMA), butyl methacrylate (BMA), methyl acrylate (MA), and butyl acrylate (BA) were purified and stored refrigerated at 4° C. under nitrogen until use. Purification of the monomers was performed as described in section 1.3 above.
[0290] Poly(ethylene glycol) methyl ether methacrylate (PEGMEMA), diurethane dimethacrylate (DUDMA), chloroform-D (CDCl3), tetrahydrofuran (THF), terephthalic acid (TA), and 2-hydroxyterephthalic acid (TAOH) were used as received.
[0291] UTGS, TTGS(400), and TTGS(600) sheets were ultrasonically cleaned in distilled water. A 15 W UV lamp (365 nm) was obtained from UVTech Systems, Inc. 3.1.2 General procedure for homopolymerization Vinyl monomers (MMA / MA / BMA / BA / DUDMA / PEGMEMA) (0.1 mol) and galvanized steel substrates (UTGS / TTGS(400) / TTGS(600)) were added to a 20 mL vial and the reaction mixture was irradiated with UV light (15 W, λ = 350 nm) at room temperature for 1 h. The vials were sealed and kept in a constant temperature (60 °C) oven for different times (0 to 48 h). 3.1.3 General procedure for obtaining block copolymers After polymerization of MMA, the resulting polymer (PMMA) was poured into a fresh monomer solution (MMA or BMA) and the reaction mixture was kept at 60°C for different times to obtain block copolymers. 3.1.4 Characterization Fluorescence spectroscopy was used to detect hydroxyl radicals generated on UV-irradiated UTGS, TTGS(400), and TTGS(600) photoinitiators.
[0292] The changes in the compounds during polymerization were monitored by ATR-FTIR. The molecular weight and polydispersity index (PDI) of the resulting polymer were measured by size exclusion chromatography (SEC).
[0293] Monomer consumption and structural changes during polymerization 1 The reaction was monitored by 1 H NMR spectroscopy. 3.2 Results and Discussion Initial investigations determined the ability of galvanized steel surfaces to photoinitiate polymerization under UV irradiation. Since the system does not contain a catalyst that requires an inert atmosphere to maintain activity, all polymerizations were carried out under ambient atmosphere to simplify the reaction set-up.
[0294] First, the polymerization of methyl methacrylate (MMA) was carried out at 60 °C without UV irradiation or with UV irradiation for 1 h without the use of any initiator or additional materials, and the polymerization of MMA monomer was also carried out at 60 °C without UV irradiation using UTGS, TTGS(400), or TTGS(600) as photoinitiator.
[0295] Polymerization of MMA was carried out using UTGS, TTGS(400), or TTGS(600) as photoinitiator under UV irradiation for 1 h, and the reaction mixture was then left in the dark at 60 °C for 48 h. The presence of clear solid polymer indicated that polymerization had occurred and PMMA polymer had been synthesized.
[0296] The obtained material 1 The detailed reaction conditions and the observation results of the obtained materials are listed in Table 9.
[0297] [Table 9]
[0298] The obtained polymers were also characterized by ATR-FTIR. The spectra of the polymers prepared with MMA monomer and UTGS showed a peak at 1640 cm -1 The characteristic absorption band around this wavelength was assigned to carbon double bonds (C=C). The presence of a large amount of double bonds remaining in the polymer prepared using UTGS was interpreted as indicating that the polymerization was incomplete. On the other hand, the polymers prepared using TTGS(400) and TTGS(600) showed the same wavenumber (1640 cm -1The disappearance of the carbon double bond peak confirmed that polymerization had occurred using TTGS(400) and TTGS(600) as photoinitiators to synthesize PMMA polymer.
[0299] Subsequent investigations focused on elucidating the polymerization mechanism. Without wishing to be bound by any particular theory, the inventors believe that this mechanism may involve the formation of a ZnO photocatalyst on the galvanized steel surface and the photoexcitation of the ZnO to generate hydroxyl radicals that can initiate the polymerization. The inventors believe that irradiating the ZnO photocatalyst with UV light can increase the number of conduction band electrons (e cb - ) and simultaneously, the valence band hole (h vb - ) may also be generated. These electrons and holes can react with atmospheric oxygen and water, respectively, to generate hydroxyl radicals. To verify this proposed mechanism, the generation of hydroxyl radicals on a galvanized steel surface was investigated.
[0300] To evaluate the photocatalytic activity of galvanized steel surfaces, fluorescence spectroscopy was used to detect hydroxyl radicals generated on UV-irradiated UTGS, TTGS(400), and TTGS(600). Terephthalic acid (TA), which reacts with hydroxyl radicals to produce the highly fluorescent product 2-hydroxyterephthalic acid (TAOH), was used as a fluorescent probe for hydroxyl radicals. The intensity of the fluorescence peak is proportional to the amount of hydroxyl radicals generated in solution.
[0301] Figure 15 shows the formation of TAOH in NaOH solution after 1 hour of UV irradiation. The TA control and UV only spectra did not show a peak at 425 nm, indicating that UV irradiation alone does not produce TAOH. A small peak appeared in the spectrum of UTGS, and the peak intensity of UTGS was slightly higher than the background of the TA control. This small peak can be attributed to the small amount of TAOH present in the solution. The spectra of TTGS(400) and TTGS(600) showed a strong peak at 425 nm corresponding to TAOH.
[0302] In order to calculate the TAOH concentration produced from each sample tested from the fluorescence intensity measured above and shown in Figure 15, a calibration curve was created using the fluorescence intensity (au) measured for TAOH solutions of known concentrations (μM) (prepared and measured as described in Section 1.6). The resulting calibration curve is shown in Figure 16.
[0303] The TAOH concentration produced from each sample was calculated based on the calibration curve in FIG. 16 using the fluorescence intensity at 425 nm of each substrate tested (UTGS, TTGS(400), and TTGS(600)) (described in Section 1.7).
[0304] The following Table 10 shows the fluorescence intensity at 425 nm shown in FIG. 15 for each substrate tested. TAOH concentration shown in Table 10 * is the corrected TAOH concentration, i.e., the TAOH concentration after correction for the TAOH concentration of the background TA control sample (TA only, no UV and no substrate sample). TAOH concentration * As described in Section 1.7, the surface area is 15 mm × 15 mm (geometric area 225 mm 2 ) based on the substrate with TAOH concentration ** has a geometric area of 1 mm 2 is the TAOH concentration corrected based on the substrate.
[0305] [Table 10]
[0306] The concentration of TAOH in TTGS(400) was found to be lower than that in TTGS(600). Without wishing to be bound by any particular theory, the inventors believe that the lower TAOH concentration measured for TTGS(400) may correspond to a lower amount of ZnO on the TTGS(400) surface. This result is consistent with the XPS analysis. These observations indicate that both the untreated and heat-treated substrates generate hydroxyl radicals, with the heat-treated substrate generating a higher proportion.
[0307] The inventors believe that, among all the compounds present on galvanized steel surfaces, ZnO is the most likely photocatalyst for the generation of hydroxyl radicals. The generation of hydroxyl radicals indicated that the polymerization of vinyl monomers initiated by heat-treated galvanized steel may proceed via free radical polymerization. Taking the polymerization of methyl methacrylate as an example, the inventors believe that the polymerization may involve the generation of hydroxyl radicals, with the reaction of a monomer molecule with a hydroxyl radical generating an initiating radical. The initiating radical can then continue to react, adding monomer, to generate a chain-propagating radical. Once a chain-propagating radical is generated, the chain can then propagate until the monomer is consumed or termination / chain transfer occurs.
[0308] The structure of PMMA / PMA / PBMA / PBA obtained by the above reaction and the monomer reaction rate during polymerization are also shown. 1 It was analyzed by 1 H NMR spectroscopy. The monomer reaction rate can be expressed by Equation 2:
[0309]
number
[0310] (where [M0] is the amount of starting monomer and [M t] is the concentration of the monomer at time t. The conversion degree of the MMA / MA / BMA / BA reaction was calculated by the integral of the vinyl peak area of the monomer (I CH2= ) to the integral value of the methoxy peak area (I O-CH3 ) [7].
[0311]
number
[0312] The reaction completion of the resulting polymers is summarized in Table 11. It was found that UTGS was able to photoinitiate polymerization with a reaction completion of 6.19%, but the polymerization rate was slow. The reaction completion of MMA on TTGS(400) and TTGS(600) was determined to be 95.6% and 97.9%, respectively, as shown in Table 11 below.
[0313] The reaction completion of MA, BMA, and BA is shown in Table 11 below.
[0314] [Table 11]
[0315] 1 The heat-treated galvanized steel sheets were investigated in more detail using H NMR spectroscopy. PMMA prepared by reaction with TTGS(400) and TTGS(600) photoinitiators for 36 h was 1 H NMR showed that the vinyl peaks of the monomer (6.1 ppm and 5.5 ppm) were dramatically reduced, and new methyl (-CH3) and methylene (-CH2-) signals appeared at 0.5-1.8 ppm. In addition, a new signal was detected around 3.6 ppm, which could be assigned to the methoxy of the polymer. The results indicated that polymerization took place in the presence of heat-treated galvanized steel sheet as a photoinitiator to produce PMMA.
[0316] The molecular weight and polydispersity index (PDI) of the obtained PMMA were measured by size exclusion chromatography (SEC). The SEC charts showed narrow monomodal distributions for both polymers with short retention times. Table 12 shows that both polymers prepared by TTGS(400) and TTGS(600) have high number average molecular weights (Mn) (1,181,000 and 956,000 g / mol, respectively) and narrow molecular weight distributions (PDI=1.11 and 1.14, respectively). In contrast, the PDI values of commercial polymers are usually in the range of 2-5.
[0317] [Table 12]
[0318] In summary, both TTGS(400) and TTGS(600) photoinitiators were demonstrated to be effective in achieving controlled radical polymerization of MMA with high reaction completion, high molecular weight, and low PDI.
[0319] The control of chain propagation by the TTGS(600) photoinitiator may be due to the presence of low concentrations of hydroxyl radicals and the absence of solvent and organic initiator in the system.
[0320] Without wishing to be bound by any particular theory, the inventors believe that the concentration of hydroxyl radicals generated in the TTGS(600) sample may have been low enough to allow chain propagation on the one hand and reduce chain termination on the other hand. Chain termination is the quenching of the activity of the chain radicals by coupling or disproportionation of the propagating radicals. Low concentrations of hydroxyl radicals may result in a relatively small number of propagating radicals, thus reducing chain termination. Furthermore, the absence of solvent and organic initiators prevents chain transfer to solvents and organic initiators. The reduced chain termination and chain transfer may have allowed the precision polymerization of the heat-treated galvanized steel photoinitiator system to be achieved.
[0321] To investigate the effectiveness of heat-treated galvanized steel in the photoinitiated polymerization of acrylic monomers, methyl acrylate (MA), butyl acrylate (BA), butyl methacrylate (BMA), poly(ethylene glycol) methyl ether methacrylate (PEGMEMA), and diurethane dimethacrylate (DUDMA) were also polymerized using TTGS(600) as a photoinitiator.
[0322] Table 13 shows the degree of reaction completion of the resulting polymer. It was found that the TTGS(600) photoinitiator is capable of photoinitiating polymerization with a high degree of reaction completion (>95%). 1 H NMR spectra were analyzed. The reduction in vinyl peaks and the increase in polymeric methyl or methylene peaks were interpreted as indicating that polymerization had occurred and that a polymer was obtained as a result. These results confirmed that heat-treated galvanized steel was capable of photoinitiating the polymerization of acrylic monomers.
[0323] [Table 13]
[0324] The above obtained polymers are classified into three types: linear polymers, branched polymers, and cross-linked polymers. Poly(methyl methacrylate) (PMMA), poly(methyl acrylate) (PMA), poly(butyl acrylate) (PBA), and poly(butyl methacrylate) (PBMA) are amorphous thermoplastic linear polymers. These polymers are believed to contain long chains that are densely packed. Without wishing to be bound by a particular theory, the inventors believe that as a result of this dense packing, these linear polymers have relatively high tensile strength and relatively high melting points. These polymers also have a relatively low average density. Thus, linear polymer-steel composites can be a lightweight alternative to metal alloys.
[0325] Poly[poly(ethylene glycol) methyl ether methacrylate] (PPEGMA) is a branched polymer that can be used, for example, in anti-biofouling materials because its hydrophilic side chains can prevent bacterial adhesion.
[0326] Poly(diurethane dimethacrylate) (PDUDMA) is a cross-linked polymer. The double bonds at both ends of PDUDMA can react with each other to form a cross-linked structure. The molecular weight and polydispersity index (PDI) of the resulting polymer were then measured by size exclusion chromatography (SEC). The size exclusion chromatography (SEC) results in Table 14 show that all linear acrylic monomers produced polymers with relatively high molecular weights (Mn>845,000g / mol) and low PDIs (PDI<1.3). These results indicate that TTGS(600) is an efficient photoinitiator for achieving precise polymerization of acrylic monomers.
[0327] [Table 14]
[0328] To further gain insight into the polymerization kinetics, we measured the monomer consumption during polymerization. 1 The polymerization rate (R p ) can be regarded as the rate of monomer consumption versus time, which is defined as follows in Equation 4 [8]:
[0329]
number
[0330] Integrating with respect to time gives Equation 5 [9]:
[0331]
number
[0332] where k p is the propagation rate constant, [M]0 is the amount of monomer at the start, and [M] t is the monomer concentration at time t and [P·] is the concentration of active propagating species. Without wishing to be bound by any particular theory, we believe that in controlled / living polymerizations, the number of propagating species remains constant and the logarithm of the monomer concentration is a linear function of time.
[0333] ln[M]0 / [M] t To obtain a plot of time versus time, 10 mg of sample was prepared using TTGS(600). 1 H NMR spectra were recorded at regular time intervals. The consumption rate of methyl methacrylate monomer (i.e., the reaction rate of polymerizable monomer to the corresponding polymer) was calculated by comparing the ratio of the integrals of methylene (=CH2) protons to methoxy (-OCH3) protons. The kinetic plot of TTGS(600) in FIG. 17 shows linear behavior, indicating that precise polymerization was achieved. Control of chain propagation was established by minimizing termination and eliminating chain transfer. Without wishing to be bound by a particular theory, the inventors believe that by reducing the concentration of hydroxyl radicals, the number of propagating radicals can be made relatively small, and therefore chain termination reactions are less likely to occur. Since there is no solvent or organic initiator, chain transfer to them can be eliminated.
[0334] Without wishing to be bound by any particular theory, the inventors believe that in controlled / living polymerizations, chain termination and chain transfer are minimized or do not occur, so that each activated species (initiating radical) is responsible for one chain. The inventors also believe that this mechanism results in a higher average degree of polymerization (DP n ), the number average molecular weight of the polymer can therefore be predicted by calculating the ratio of monomer consumption to active species. The average degree of polymerization is given by Equation 6
[10] :
[0335]
number
[0336] therefore,
[0337]
number
[0338] Here, M n is the number average molecular weight, M0 is the molecular weight of the monomer unit, [I]0 is the concentration of active species (primary radicals), and [M]0 is the amount of monomer at the start. According to Equation 7, the number average molecular weight increases linearly with the reaction rate in controlled / living polymerizations.
[0339] To investigate whether the polymerization reactions described above have the characteristics of precise / living polymerization, the evolution of molecular weight and PDI as a function of monomer conversion was monitored by SEC. In Figure 18, the molecular weight values increased linearly with monomer conversion, demonstrating the control of TTGS(600). It was also found that the PDI values gradually decreased with increasing monomer conversion. Furthermore, the SEC results in Table 15 showed a unimodal distribution of polymers, with the molecular weight values shifting to higher values with increasing monomer conversion. These results further demonstrate the control of both the molecular weight and molecular weight distribution of the resulting polymers by the TTGS(600) photoinitiator.
[0340] [Table 15]
[0341] The polymerization kinetics and the evolution of molecular weight with monomer conversion revealed that the polymer had the characteristics of controlled / living polymerization. Without wishing to be bound by a particular theory, the inventors believe that living polymerization may allow efficient resumption of polymerization. To investigate the resumption ability of the obtained polymer, a series of block polymerizations were carried out. Poly(methyl methacrylate) (PMMA) obtained by the above process was introduced into vials containing various monomers (MMA and BMA), and the mixture was then left in the dark at 60° C. until the monomers were consumed.
[0342] [Table 16]
[0343] The successful block copolymerization confirmed the ability of the precursor polymer to reinitiate polymerization. The resulting block copolymer was a transparent, rigid polymer. To facilitate the identification of the different blocks, red-brown and green dyes were added to the additional monomers, respectively. As shown in Figure 19A and B, two distinct layers are visible, the first of which corresponds to the original PMMA homopolymer. The presence of two layers suggests that it may be possible to resume the polymerization to create a multilayer polymer. 3.3 Summary and conclusions We successfully polymerized various monomers using the surface-initiated controlled radical polymerization (GSM-SICRP) technique via galvanized steel. The control of polymer molecular weight and molecular weight distribution was achieved, suggesting that this could be a versatile platform for synthesizing various polymers with designed molecular weights and well-defined structures.
[0344] The first-order reaction rate equation and the increase in molecular weight with monomer conversion are characteristic of living polymerization. By GSM-SICRP, we successfully synthesized block copolymers with controlled molecular weight and narrow molecular weight distribution.
[0345] The GSM-SICRP technique works without the use of solvents, initiators (apart from metal surfaces, e.g., galvanized steel), catalysts, or additives. The absence of solvents and initiators in this system allows for the production of products of high purity. Furthermore, the above examples show that the GSM-SICRP system does not contain a catalyst that requires an inert atmosphere to maintain its activity, so the polymerization can be carried out in an ambient atmosphere.
[0346] The GSM-SICRP system is capable of polymerizing a wide range of monomers. Without wishing to be bound by any particular theory, the inventors believe that monomers that can be polymerized by conventional free radical polymerization may also be polymerized by GSM-SICRP. The examples provided herein demonstrate that some activated monomers, such as acrylates and methacrylates, can be polymerized by GSM-SICRP.
[0347] GSM-SICRP can be used to tailor the chemical and physical properties of substrates without damaging the metal substrate. The GSM-SICRP technique may require less surface treatment compared to surface-initiated graft polymerization, activation of the metal surface can be achieved by heat treatment, and the above examples show that the activated metal surface can initiate polymerization under UV irradiation. Compared to electrochemically or photoelectrochemically induced surface-initiated polymerization, GSM-SICRP may be more economical due to the absence of an electrical driving force. 4. Example 3 - Effect of polymerization conditions on polymerization rate and polymer properties In this example, the effect of polymerization conditions on the polymerization rate and polymer properties was investigated, with emphasis on the analysis of the effect of photoinitiator, irradiation parameters, polymerization temperature, and monomer feed ratio on the polymerization rate and the properties of the resulting polymer.
[0348] To evaluate the ability of different galvanized steels to polymerize the vinyl monomer methyl methacrylate (MMA), two different types of heat-treated galvanized steels (hot-dip galvanized steel and zinc potassium) were used as photoinitiators and polymerizations were carried out under identical experimental conditions. MMA was then polymerized using TTGS(600) photoinitiator under different UV intensities, exposure times, and temperatures. The properties of the resulting polymers were also evaluated. To gain further insight into the polymerization kinetics, the monomer consumption during polymerization was also measured. 1 The reaction was monitored by 1 H NMR spectroscopy.
[0349] The monomer feed ratio is increased to the glass transition temperature (T g To investigate the effect of methyl methacrylate and butyl methacrylate on the copolymerization of ethylenediaminetetraacetate (FDPA), methyl methacrylate and butyl methacrylate were copolymerized in different ratios. The resulting copolymers were then characterized. 4.1 Experiments 4.1.1 Materials Methyl methacrylate (MMA) and butyl methacrylate (BMA) were purified and stored refrigerated at 4 °C under nitrogen until use. Chloroform-D (CDCl3), tetrahydrofuran (THF), terephthalic acid (TA), and 2-hydroxyterephthalic acid (TAOH) were used as received.
[0350] Sheets of untreated galvanized steel (UTGS), untreated zincalum (UTZnAl), heat-treated galvanized steel (TTGS(600)) treated at 600°C, and heat-treated zincalum (TTZnAl(600)) treated at 600°C were ultrasonically cleaned in distilled water. A 15W UV lamp (365nm) and a 6W UV lamp (365nm) were obtained from UVTech Systems, Inc. 4.1.2 Homopolymerization Methyl methacrylate (MMA) (9.4 g, 0.094 mol) and photoinitiator (TTGS(600) or TTZnAl(600)) were charged in a 20 mL vial, and the reaction mixture was irradiated with UV light (6 W or 15 W, λ = 350 nm) for different times (0-60 min). The vial was sealed and kept in a constant temperature (60 °C or 80 °C) oven for different times (0-48 h). 4.1.3 Copolymerization Mixtures of different ratios of methyl methacrylate (MMA) and butyl methacrylate (BMA) were placed in 20 mL vials and the reaction mixtures were irradiated with UV light (15 W, λ=350 nm) for 1 h. The vials were sealed and kept at 60° C. for 48 h. 4.1.4 Characterization Fluorescence spectroscopy was used to investigate the generation of hydroxyl radicals on UV-irradiated UTGS, UTZnAl, TTGS(600), and TTZnAl(600) photoinitiators. The structures of the monomers and polymers were 1 The molecular weight and molecular weight distribution of the polymer were measured by SEC. MDSC was used to measure the glass transition temperature of the obtained polymer. 4.2 Results and Discussion 4.2.1 Effect of photoinitiators The above examples demonstrate that the polymer molecular weight and molecular weight distribution can be controlled by using TTGS(600) as a photoinitiator.
[0351] To investigate the effect of the photoinitiator on the properties of the final polymer, polymerizations were carried out using zinc potassium (ZnAl) (steel with a coating of 55% zinc and 45% aluminum) as photoinitiator. The chemical composition of UTGS, TTGS(600), UTZnAl, and TTZnAl(600) was investigated by X-ray photoelectron spectroscopy (XPS). The zinc compounds present were identified by measuring the modified Auger parameter of Zn (α'Zn) and comparing it with literature values. The XPS results of UTGS and TTGS(600) shown in Tables 17 and 18 are identical to those shown in Example 1.
[0352] This α′Zn indicated the presence of basic zinc carbonate on the surface of the UTZnAl substrate and confirmed the formation of ZnO on the TTZnAl(600) (Table 17). XPS survey spectra confirmed that the zinc concentration on the TTZnAl(600) surface was lower than that of TTGS(600), which corresponds to a lower amount of zinc than that of the initial untreated substrate (Table 18).
[0353] [Table 17]
[0354] [Table 18]
[0355] Before carrying out the polymerization, the photocatalytic activity of all the photoinitiators was investigated using fluorescence spectroscopy as follows. 15 mL of TA stock solution and different substrates: untreated galvanized steel (UTGS), galvanized steel heat-treated at 400 °C (TTGS400), galvanized steel heat-treated at 600 °C (TTGS600), untreated zincalum (UTZnAl), and zincalum heat-treated at 600 °C (TTZnAl600) were prepared as described in section 1.7 above. The samples thus prepared were left in the dark at room temperature for 1 h. The samples were then irradiated with UV (365 nm, 15 W) at room temperature (20-25 °C). A control sample was also prepared as described in section 1.7. After 1 h, 2 mL of the reaction solution was withdrawn and analyzed using a PerkinElmer LS 55 fluorescence spectrophotometer. The excitation spectrum was monitored at 315 nm and the emission spectrum was measured at 425 nm.
[0356] Fluorescence spectra confirmed the generation of hydroxyl radicals in both the untreated and heat-treated photoinitiators (Figure 20). The rate of hydroxyl radical generation in the untreated photoinitiator was slower than that with the heat-treated photoinitiator. The rate of hydroxyl radical generation in TTZnAl(600) was 0.92 μM / h / cm 2TTGS(600) (1.34 μM / h / cm 2 ) was slower than
[0357] The concentration of TAOH produced by each sample subjected to the test was calculated from the fluorescence intensity measured above and shown in FIG. 20, using the calibration curve shown in FIG. 16, as described in Section 1.7. The following Table 19 shows the fluorescence intensity at 425 nm shown in FIG. 20 for each substrate tested. TAOH concentration shown in Table 19 * is the corrected TAOH concentration, i.e., the TAOH concentration after correcting for the background TAOH concentration of the TA control sample (TA only, no UV and no substrate sample). * The substrate has a surface area of 15 mm × 15 mm (geometric area 225 mm) as described in Section 1.7. 2 ) based on TAOH concentration ** has a geometric area of 1 mm 2 is the corrected TAOH concentration based on the substrate.
[0358] [Table 19]
[0359] Methyl methacrylate (MMA) was polymerized under the same experimental conditions using UTGS, UTZnAl, TTGS(600), and TTZnAl(600) as photoinitiators. The polymerization conditions and some characterization results are summarized in Table 20.
[0360] [Table 20]
[0361] As can be seen, when UTGS and UTZnAl were used as initiators, the reaction completion was low (5.44-6.19%) and slow polymerization occurred (Table 20, Test No. 1, Test No. 2).
[0362] Both TTGS(600) and TTZnAl(600) were demonstrated to be effective in achieving controlled radical polymerization of MMA with high reaction completion (95.6-97.9%) and low PDI (1.11-1.14). The SEC chart showed that using TTZnAl(600) as the photoinitiator resulted in a higher molecular weight (Mn=1,164,000 g / mol) than TTGS(600) (Mn=956,000 g / mol), indicating that a lower concentration of hydroxyl radicals resulted in a higher molecular weight. The number of initiated chains decreased with the decrease in the hydroxyl radical concentration. Therefore, the increase in molecular weight could be attributed to the decrease in the number of initiated chains.
[0363] To gain further insight into the polymerization kinetics, we measured the consumption of monomer during polymerization. 1 The reaction was monitored by 1 H NMR spectroscopy. TTGS(600) and TTZnAl(600) photoinitiators were each placed in a 20 mL vial containing 0.094 mol of MMA, and the reaction mixture was irradiated with UV light (15 W, λ=350 nm) for 60 min under ambient atmosphere. The sealed vial was then kept at 60 °C. Approximately 10 mg of sample was periodically withdrawn and 1 The conversion and consumption of monomer were monitored by 1 H NMR analysis.
[0364] As can be seen from Figure 21, the kinetic plots of TTGS(600) and TTZnAl(600) show linear behavior, indicating that precise polymerization was achieved. The slope of the kinetic plot of TTGS(600) is larger, indicating that TTGS(600) had a higher polymerization rate than TTZnAl(600), which may be due to the higher concentration of hydroxyl radicals.
[0365] The evolution of molecular weight and PDI as a function of monomer conversion was also monitored by SEC as shown in Figure 23. The molecular weight values increased linearly with monomer conversion, confirming their control by TTGS(600) and TTZnAl(600). It was also found that the PDI values gradually decreased with increasing monomer conversion for both photoinitiator systems (Tables 21 and 22).
[0366] [Table 21]
[0367] [Table 22]
[0368] Furthermore, the SEC charts showed that the polymers had a unimodal distribution and that the molecular weight values shifted to higher values with increasing monomer conversion. Collectively, these results further demonstrate that TTGS(600) and TTZnAl(600) photoinitiators control both molecular weight and molecular weight distribution. The polymerization rate with TTGS(600) photoinitiator was faster than that with TTZnAl(600). However, polymerization with TTZnAl(600) photoinitiator gave polymers with higher molecular weight. 4.2.2 Influence of irradiation parameters The results presented in the above section indicate that the nature of the photoinitiator influences the generation of hydroxyl radicals and therefore the polymerization kinetics and thus the properties of the polymer. Therefore, the effect of the irradiation parameters on the amount of hydroxyl radicals generated was also investigated.
[0369] To prepare each test sample, 15 mL of TA stock solution (prepared as described in section 1.7) and a sample of galvanized steel (TTGS600) heat treated at 600 °C (prepared as described in section 1.7) were added to a vial. The test samples thus prepared were then left in the dark at room temperature for 1 hour. After this time, each sample was irradiated with different intensities of UV (UV1: 365 nm, 6 W and UV2: 365 nm, 15 W) at room temperature (20-25 °C). A control sample was also prepared (see section 1.7). After 1 hour, 2 mL of each test sample was withdrawn and analyzed using a Perkin Elmer LS 55 fluorescence spectrophotometer. The excitation spectrum was monitored at 315 nm and the emission spectrum was measured at 425 nm.
[0370] FIG. 23 shows the fluorescence spectra of TTGS600 solution irradiated with 6 W and 15 W of UV light. The 425 nm fluorescence intensity results shown in Figure 23 and Table 23 below were then corrected (taking into account the fluorescence intensity of the control TA sample without UV irradiation as described in section 1.7). The corrected TAOH concentration for each sample was then calculated based on the sample's corrected fluorescence intensity at 425 nm using the calibration curve shown in Figure 16. The corrected TAOH concentration for each sample is shown in Table 23 below.
[0371] The results showed that the rate of hydroxyl radical production (assessed based on fluorescence intensity at 425 nm) was higher when high-intensity (15 W) UV light was used than when low-intensity (6 W) UV light was used.
[0372] [Table 23]
[0373] The effect of UV irradiation time on the rate of hydroxyl radical generation was also investigated as follows: 15 mL of TA stock solution (prepared as described in section 1.7 above) and galvanized steel heat-treated at 600°C (TTGS600) prepared as described in section 1.7 were placed in a vial. Six samples were prepared in this way.
[0374] Each sample was left in the dark at room temperature for 1 hour. After this time, each sample was irradiated with UV light (365 nm, 15 W) at room temperature (20-25 °C). 2 mL of reaction solution was withdrawn from each sample at 10 min intervals (i.e., 10, 20, 30, 40, 50, and 60 min) and analyzed using a PerkinElmer LS 55 fluorescence spectrophotometer. A control sample containing TA was also prepared (see section 1.7) and analyzed as the 0 min sample. Excitation spectra were monitored at 315 nm and emission spectra were measured at 425 nm.
[0375] The fluorescence spectra of samples exposed to UV for different times are shown in Figures 24 and 25. The fluorescence intensity results shown in Figures 24 and 25 were then corrected (taking into account the fluorescence intensity of the control TA sample that was not exposed to UV irradiation as described in section 1.7). The corrected TAOH concentration of each sample was then calculated based on the corrected fluorescence intensity of the sample at 425 nm using the calibration curve shown in Figure 16. The results for samples after 20 to 60 minutes are shown in Table 24 below.
[0376] Based on the results, the amount of hydroxyl radicals produced (assessed based on the fluorescence intensity at 425 nm) increased with irradiation time. Analysis of the data showed that the higher the irradiation intensity and the longer the irradiation time, the faster the rate of hydroxyl radical production.
[0377] [Table 24]
[0378] SEC charts were also recorded for PMMA prepared at various irradiation times (30, 40, 50 and 60 min). The SEC charts showed that the molecular weight of the resulting polymer decreased with irradiation time. The concentration of hydroxyl radicals increased with irradiation time. We believe that this may be a result of an increase in the number of initiated chains. Thus, the decrease in molecular weight may be due to an increase in the number of initiated chains.
[0379] To investigate the effect of irradiation parameters on the polymer properties, polymerizations were carried out using different UV intensities and irradiation times. The total polymerization time for each experiment was 48 hours. As shown in Table 25, a lower molecular weight (956,000 g / mol) was obtained by using a higher UV intensity (15 W), which we believe may correspond to a higher concentration of hydroxyl radicals. Furthermore, the molecular weight of the resulting polymer decreased with irradiation time. The concentration of hydroxyl radicals increased with irradiation time, thus increasing the number of initiated chains. Thus, the decrease in molecular weight may be due to an increase in the number of initiated chains.
[0380] [Table 25]
[0381] To further investigate the polymerization kinetics, the monomer consumption was monitored with different UV irradiation intensities and UV irradiation times. Figures 26 and 27 report the monomer consumption rate as a function of reaction time with different UV intensities and irradiation times, respectively. The higher UV intensity resulted in a faster polymerization rate, as shown by the higher slope of the polymerization kinetic plot with 15 W UV. The polymerization kinetic plot with 15 W UV shown in Figure 26 shows that the polymerization rate increased with irradiation time.
[0382] Overall, these results demonstrate that higher UV intensity and longer exposure time lead to faster polymerization rates, however polymerizations using higher UV intensity and longer exposure time led to lower molecular weight polymers. 4.2.3 Effect of polymerization temperature The effect of temperature on the rate of hydroxyl radical generation was investigated by irradiating TA at different temperatures for 60 min in the presence of TTGS photoinitiator. The temperature was kept constant in all cases under UV irradiation and in the dark. The fluorescence spectra obtained show that the rate of hydroxyl radical generation was not affected by temperature.
[0383] Table 26 lists the conditions used for the polymerization of MMA at different temperatures and some characterization results. The molecular weight results indicate that the molecular weight of the polymer did not show a significant temperature dependence.
[0384] [Table 26]
[0385] To investigate the dependence of polymerization kinetics on polymerization temperature, the monomer consumption at different temperatures was monitored. Figure 28 shows the monomer consumption as a function of reaction time for different polymerization temperatures. As can be seen, the polymerization rate increased with increasing polymerization temperature. From the analysis of molecular weight and polymerization kinetics, it can be concluded that the polymerization rate became faster by increasing the polymerization temperature, but the molecular weight of the polymer did not show a significant temperature dependence. 4.2.4 Effect of monomer feed ratio Glass transition temperature (T g ) is the temperature range where the polymer transitions from a glassy to a rubbery material. T g is an important feature that can affect the material properties of a polymer and its potential applications. g One way to tailor the glass transition temperature is by copolymerizing monomers in specific ratios. The Gordon-Taylor equation8 predicts the glass transition temperature of random copolymers
[11] :
[0386]
number
[0387] (In the formula, T g,mix is the glass transition temperature of the copolymer, and T g,1 and T g,2 is the glass transition temperature of each homopolymer, and ω iis the weight fraction of component i, and K is an adjustable fitting parameter)
[12] . According to the Gordon-Taylor equation 8, the T g,mix is T g,1 and T g,2 Between the actual T g,mix The value depends on the ratio of the monomers.
[0388] To investigate the effect of the monomer feed ratio on the glass transition temperature, methyl methacrylate (MMA) and butyl methacrylate (BMA) were copolymerized at different ratios. The initial butyl methacrylate ratio was 0.5 (f BMA ) and the chemical composition of the obtained copolymer was detected by ATR-FTIR.
[0389] FTIR spectra of MMA monomer, BMA monomer, and copolymers of MMA and BMA were also recorded. The spectra of MMA and BMA monomers contain a 1640 cm -1 A characteristic absorption band appeared near (C=C). However, no absorption peak appeared at the same wavenumber in the copolymer. The disappearance of the C=C peak in the copolymer spectrum confirmed that the copolymerization was complete.
[0390] Homopolymers of MMA and BMA were prepared as described in section 4.1.2 above. The glass transition temperatures of the homopolymers and the resulting copolymers were measured by MDSC. The DSC curves of PMMA and PBMA, respectively, prepared in the presence of TTGS(600) showed that the T of PBMA was g (31.8℃) is the T of PMMA g This indicates that the temperature is lower than the normal range (108.9℃).
[0391] DSC curves of the copolymers prepared in the presence of TTGS(600) were recorded. In Table 27, the Tg values of the copolymers are summarized along with the concentrations of MMA and BMA used in the preparation of each copolymer. The glass transition temperatures of the prepared copolymers varied from 52.3 to 68.4°C depending on the monomer feed ratio. Increasing the proportion of BMA in the initial monomer mixture decreased the glass transition temperature. Thus, the glass transition temperature of the resulting copolymers can be tailored by adjusting the monomer feed ratio.
[0392] [Table 27]
[0393] 4.3 Conclusion This example demonstrates the influence of photoinitiator, irradiation parameters, polymerization temperature, and monomer feed ratio on the polymerization kinetics and the resulting polymer properties.
[0394] The molecular weight of the polymer is affected by the concentration of hydroxyl radicals (assessed based on the fluorescence intensity at 425 nm). Using TTZnAl(600) photoinitiator, polymers with higher molecular weight were produced than using TTGS(600), which we believe may correspond to the lower concentration of hydroxyl radicals.
[0395] Polymerizations carried out with higher UV intensities resulted in lower molecular weights, which is believed to correspond to higher concentrations of hydroxyl radicals.
[0396] The molecular weight of the resulting polymer decreased with irradiation time. This decrease may be due to the increase in the concentration of hydroxyl radicals with irradiation time. Furthermore, the rate of hydroxyl radical production was not affected by temperature. In other words, the molecular weight of the polymer did not show a significant temperature dependence. This result indicates that the molecular weight of the polymer was dependent on the concentration of hydroxyl radicals.
[0397] The results indicate that the concentration of hydroxyl radicals and reaction temperature affect the polymerization kinetics. The use of TTGS(600) photoinitiator, which has a higher concentration of hydroxyl radicals, resulted in a faster polymerization rate than that of TTZnAl(600). Higher irradiation intensity and longer irradiation time resulted in higher concentration of hydroxyl radicals and faster polymerization rate. Furthermore, higher polymerization temperature resulted in a faster polymerization rate. Thus, higher hydroxyl radical concentration (assessed based on the fluorescence intensity at 425 nm) and higher reaction temperature resulted in a faster polymerization rate.
[0398] The glass transition temperature of the copolymer was influenced by the initial comonomer composition. The glass transition temperature of the copolymer produced in this example was between the glass transition temperatures of the respective homopolymers and depended on the ratio of the monomers. The higher the ratio of the homopolymer with the lower Tg, the lower the glass transition temperature of the copolymer.
[0399] The successful production of polymers and copolymers with a range of molecular weights and glass transition temperatures suggested that polymer properties could be tailored by adjusting reaction conditions and monomer feed ratios. 5. Example 4 - Adhesion and corrosion resistance GSM-SICRP has the potential to produce metal-polymer composites in a variety of configurations, such as laminated steel-polymer, steel fiber reinforced polymer, woven steel fabric-polymer, and steel-polymer composites such as polymer-coated galvanized steel.
[0400] Polymer-coated galvanized steel composites and laminated galvanized steel-polymer composites have been successfully fabricated using the GSM-SICRP technique. Composite analysis and design may include testing of composite performance, such as environmental corrosion resistance and mechanical, electromagnetic, and thermal transport properties.
[0401] This example measures the adhesive strength and corrosion resistance of a polymer coating on a galvanized steel surface. The polymer chosen for this example was poly(diurethane dimethacrylate) (PDUDMA), which is both crosslinkable and flexible.
[0402] The adhesive strength of the PDUDMA coatings applied to different galvanized steels was evaluated by a pull-off adhesion test (described below). As a control experiment, a pull-off adhesion test of epoxy resin on galvanized steel was performed. Epoxy resin was chosen because it is a commonly used adhesive for joining dissimilar materials.
[0403] The adhesion strength of the PDUDMA coating to a galvanized steel substrate was also measured using a tape adhesion test (described below). There are several points where the PDUDMA / galvanized steel system can fail. The failure morphology at the interface was investigated. The corrosion resistance of the PDUDMA / galvanized steel was also evaluated by salt spray testing. 5.1 Experiments 5.1.1 Materials Diurethane dimethacrylate (DUDMA) and sodium chloride (NaCl) were used as received. UTGS, TTGS(400), and TTGS(600) sheets were cut into square slides with dimensions of 100 mm × 100 mm and then ultrasonically cleaned in ethanol and distilled water. A 15 W UV lamp (365 nm) was obtained from UVTech Systems, Inc. 5.1.2 Spin coating A spin coater (WS-400 Lite Series, Laurell Technologies, USA) was used for spin coating. UTGS, TTGS(400), and TTGS(600) sheets with a thickness of 0.5 mm and dimensions of 100 mm × 100 mm were used as substrates.
[0404] The DUDMA monomer was applied to a galvanized steel substrate at room temperature, and the substrate was then spun horizontally at 2000 rpm for 60 seconds. The deposited sample was irradiated with UV light (15 W, λ = 350 nm) for 1 h and then kept at constant temperature (60 °C) for 48 h before being cooled to room temperature.
[0405] After the reaction was completed, a solid polydiurethane dimethacrylate (PDUDMA) coating was obtained on the galvanized steel substrate, the thickness of which was approximately 30 μm as measured by a coating thickness gauge (Elcometer Limited, UK, model number: Elcomete 355).
[0406] The chemical changes during polymerization were monitored by ATR-FTIR. 5.1.3 Pull-off test The adhesion strength of PDUDMA coatings to galvanized steel substrates was measured using a direct pull-off adhesion test. The pull-off adhesion test was performed using a pull-off adhesion tester (DeFelsko Corporation, USA, model No: PosiTest AT-M Manual) according to ASTM D4541-09 (Standard Test Method for the Peel Strength of Coatings Using a Portable Adhesion Tester)
[13] . Heavy-duty super-strength epoxy (3M, USA) was used as the adhesive. Five specimens for each coating system were tested and the corresponding average peel strengths were calculated. A combination of SEM / EDS and XPS was applied to investigate the failure morphology to obtain high-resolution physical and chemical information. The failure of the substrates and the corresponding test dollies after the pull-off adhesion test were examined using a stereomicroscope (Nikon Corporation, Japan, model No: MSZ 18). The interface failure area was calculated using image analysis software (ImageJ). 5.1.4 Tape adhesion test The adhesion strength of the PDUDMA coatings to galvanized steel substrates was measured using a tape adhesion test. Tape adhesion tests were performed according to ASTM D3359-17 (Standard Test Method for Grading Adhesion by Tape Adhesion Test) using 3M Transparent Duct Tape 2120 (25 mm) and Scotch Blue 2090 Painter's Tape (24 mm). A razor blade was used as the incision tool. PDUDMA coatings with dry film thicknesses between 50 μm and 125 μm were used. Six incisions of approximately 20 mm length and 2 mm spacing were made in the first direction and six incisions (of equal length and spacing) were made in the second direction perpendicular to the first direction to generate a checkerboard pattern of 2 × 2 mm squares (five rows and five columns). The incision pressure was sufficient to just reach the edge of the blade into the substrate. The center of the tape was placed over the square and within the area of the square, smoothed to ensure uniform contact between the tape's adhesive and the coating surface. 90 seconds after application, the tape was quickly removed from the square area and inspected for peeling of the coating from the substrate. 5.1.5 Salt spray test Salt spray tests were performed in a salt spray chamber (Caliber Plastics Ltd, New Zealand) according to ASTM B117-16 (Standard Practice for Operating Salt Spray Apparatus)
[14] . Three types of uncoated galvanized steel sheets and three types of galvanized steel sheets with a PDUDMA coating were tested. Accelerated aging of scribed specimens was also performed according to ASTM D1654-08 (Standard Test Method for Evaluating Painted or Coated Specimens Exposed to Corrosive Environments)
[15] . Six specimens were manually scribed using a sharp cutting tool. Two perpendicular scribe marks on each specimen penetrated the coating to expose the steel substrate. Each scribe was 7 cm long. The end of the scribe was 1.5 cm from the edge of the sheet. The sides of all specimens were sealed with a waterproof silicone sealant (Cerise, New Zealand). Three samples of each type of specimen were tested.
[0407] The environmental conditions for both salt spray tests are given in Table 28 below. The specimens were placed in the chamber at an angle of 80°. The total salt spray test time for the unnotched specimens was 672 hours. The specimens were inspected after 72, 408, and 672 hours of exposure to the corrosive environment. The total test time for the notched specimens was 312 hours. The specimens were inspected after 144, 216, and 312 hours of exposure to the corrosive environment. After each experiment, the salt on the specimens was carefully washed off with running water and immediately dried in warm ambient air. The corroded and damaged areas of the notched specimens were calculated using image analysis software (ImageJ).
[0408] [Table 28]
[0409] The corrosion resistance of the test specimens was evaluated by the Rating Number (RN) method according to ASTM D610-08 (Standard Method for Evaluating the Degree of Rust on Painted Steel Surfaces)
[16] . This method provides a standardized method for quantifying the degree of surface rust on a scale of 0 to 10 based on the percentage of surface rust that is visible. Table 29 lists the rust scale according to ASTM D610-08.
[0410] [Table 29]
[0411] The damaged area on the notched specimens was measured and graded in terms of ASTM D1654-08
[15] . The average width of the blister originating from the notch was measured in millimeters. The average blister severity originating from the notch was rated based on the blister width using a scale of 0 to 10 as specified in Table 30.
[0412] [Table 30]
[0413] 5.2 Results and Discussion 5.2.1 PDUDMA Coverage The chemical structures of the DUDMA monomer and the PDUDMA coating were characterized by ATR-FTIR. -1 and 1530cm -1 Characteristic absorption peaks corresponding to C=O stretching and NH stretching were observed at 1640 cm -1 The characteristic peak was assigned to the carbon double bond (C=C)
[0113] . -1 The absorption peak of 1,2-dichloro-1,3-tetrafluoroethylene (PDUDMA) was not observed in the PDUDMA coating. The disappearance of the carbon double bond peak confirmed that polymerization had occurred to give a PDUDMA polymer. 5.2.2 Adhesion test A pull-off adhesion test was used to measure the adhesive strength of the epoxy resin and PDUDMA coatings on galvanized steel substrates. The results of the pull-off adhesion measurements are shown in Table 31 below, along with the average adhesive strength of the test specimens.
[0414] The average bond strength of the epoxy systems was in the range of 1.88-1.98 MPa, while the bond strength of the PDUDMA coating system was higher, in the range of 2.40-2.48 MPa. Without wishing to be bound by any particular theory, the inventors believe that the peel strength of polymer-coated steel depends on the properties of the polymer and the substrate, and is typically in the range of 1.5-5 MPa. The peel strength of the PDUDMA coating system is in this range, indicating that the PDUDMA coating system is comparable to conventional adhesively bonded coating systems. Unlike adhesively bonded coating systems, the bond strength of the PDUDMA coating system was achieved without any specific pretreatment.
[0415] [Table 31]
[0416] In addition to measuring the adhesive strength, the failure modes of the epoxy and PDUDMA coatings were also investigated. Two experiments were set up. In the first experiment, a test cylinder was directly attached to a galvanized steel surface specimen (i.e., steel with a layer of zinc on its surface) using an epoxy adhesive. In the second experiment, a test cylinder was attached to the PDUDMA coated surface of a galvanized steel substrate specimen (i.e., steel substrate with a layer of zinc on its surface).
[0417] Adhesive failure may occur at the interface between the two phases. In this case, adhesive failure may occur at the epoxy-substrate interface, the epoxy-test cylinder interface, the epoxy-PDUDMA interface, or the PDUDMA-substrate interface. Without wishing to be bound by a particular theory, the inventors believe that adhesive failure may indicate poor interfacial bonding. Unlike adhesive failure, cohesive failure occurs within the bulk of the epoxy or the bulk of the PDUDMA coating. This failure is usually the desired failure mode, since it can be interpreted as meaning that the polymer / galvanized steel interface bond is stronger than the internal strength of the polymer.
[0418] Optical microscopy, SEM / EDS, and XPS were used in combination to identify the type of failure at the interface. Optical microscopy determined the domain failure mode primarily at the interface. To further understand the failure mode, the components on the surfaces of the substrate and test cylinder were observed.
[0419] Without wishing to be bound by any particular theory, the inventors believe that adhesive failure at the epoxy / test cylinder interface can be demonstrated by the presence of epoxy residue on the galvanized steel substrate and the absence of epoxy on the test cylinder. The presence of epoxy or PDUDMA on the test cylinder and the absence of polymer (epoxy or PDUDMA) residue may indicate that adhesive failure occurred at the epoxy / substrate or PDUDMA / substrate interface. The presence of epoxy or PDUDMA coating on both the galvanized steel substrate side and the test cylinder side may indicate that cohesive failure occurred within the bulk of the polymer coating.
[0420] Using optical images of one of five pull-off adhesion test areas for epoxy resin and PDUDMA coating systems, the areas of residual epoxy and PDUDMA were calculated using image analysis software (ImageJ) (see results in Tables 32 and 33, respectively). For UTGS-epoxy, TTGS(400)-epoxy, and TTGS(600)-epoxy samples, most of the residual epoxy was located on the test cylinder side. Failure occurred primarily at the epoxy / zinc interface (85%, 81%, and 78% for UTGS-epoxy, TTGS(400)-epoxy, and TTGS(600)-epoxy samples, respectively, as shown in Table 32), indicating relatively low adhesive strength.
[0421] [Table 32]
[0422] In the PDUDMA system, noticeable residual PDUDMA was found on both the substrate side and the test cylinder side. Failure of the PDUDMA coating system occurred primarily as a cohesive failure within the epoxy and PDUDMA coating.
[0423] The percentage of cohesive failure for the epoxy and PDUDMA coatings of UTGS-PDUDMA, TTGS(400)-PDUDMA, and TTGS(600)-PDUDMA was 51%, 75%, and 73%, respectively. The percentage of cohesive failure for the heat-treated galvanized steel-PDUDMA coated samples (75%, 73%) was higher than that of the UTGS-PDUDMA sample (51%). The increased area of cohesive failure may be due to the increased surface roughness caused by the heat treatment.
[0424] Without wishing to be bound by any particular theory, the inventors believe that the heat treated galvanized steel substrate is able to initiate more PDUDMA chains than the untreated substrate. Therefore, another reason for the increased bond strength of the heat treated samples may be that more PDUDMA chains are attached to the surface of the heat treated galvanized steel than the untreated steel. The fact that the failure occurs primarily at the polymer coating rather than the polymer steel interface may suggest that the bond between PDUDMA and galvanized steel is stronger than the epoxy system (where the test cylinder was attached directly to the galvanized steel surface using an epoxy adhesive).
[0425] [Table 33]
[0426] Since optical microscopy only provides an approximate area failure mode, SEM / EDS and XPS were performed to obtain physical and chemical insights of the fracture interface. Elemental mapping analysis revealed the location of the polymer residue on the galvanized steel. The presence of C and Zn in the images indicated that the failure mainly occurred as a mixture of cohesive and adhesive failure.
[0427] The galvanized steel substrate side and the corresponding test cylinder side of the same cohesively / adhesively failed area were analyzed using XPS. Zinc was present on both the galvanized steel side and the test cylinder side. Tin (Sn) was detected on both surfaces. The Sn element was attributed to the tin complex catalyst (tin(II) 2-ethylhexanoate or tin(II) octoate or stannous octoate (Sn(Oct)2)) from the PDUDMA coating. The presence of zinc and the PDUDMA coating on both sides further suggested a possible mixture of cohesive failure within the zinc layer, cohesive failure within the PDUDMA coating, and adhesive failure at the PDUDMA / zinc interface.
[0428] The relative elemental composition of the steel side and the test cylinder side of the samples were also analyzed, and the results are shown in Table 34 below.
[0429] [Table 34]
[0430] Overall, the bond strength of the PDUDMA coating system was comparable to that of coating systems bonded with conventional adhesives. The joining technique described herein (GSM-SICRP) can be utilized without the need for costly and potentially toxic adhesives, solvents, or other additives. The absence of additives can make the technique described herein more environmentally friendly and potentially more cost-effective than adhesive bonding. Additionally, the GSM-SICRP technique can require reduced surface preparation compared to adhesive bonding. 5.2.3 Tape adhesion test The adhesion strength of the PDUDMA coating to a galvanized steel substrate was measured using a tape adhesion test. The results of the adhesion test were graded near 4B (see Table 34a), which corresponds to less than 5% of the area of the checkerboard coating being removed from the substrate after the tape adhesion test, indicating good adhesion between the PDUDMA coating and the substrate.
[0431] [Table 35]
[0432] 5.2.4 Salt spray test The appearance of uncoated and coated galvanized steel samples before and after salt spray test for different time periods (h) is shown in Table 35.
[0433] [Table 36]
[0434] Corrosion was observed on the UTGS surface after 408 h of exposure, whereas corrosion products did not begin to form on the UTGS-PDUDMA surface until 672 h. For the TTGS(400) sample, some white rust was observed on the TTGS(400) surface after 72 hours. This white rust may be derived from simoncolite (Zn5(OH)8Cl2) and hydrozinsite (Zn5(CO3)2(OH)6). After 408 hours of exposure, the white rust spread over the entire surface of TTGS(400). In contrast, no obvious global corrosion occurred on the TTGS(400)-PDUDMA sample even after 408 hours of exposure. After 672 hours of exposure, white rust started to form on the TTGS(400)-PDUDMA surface.
[0435] For the TTGS(600) sample, the surface was completely covered with red rust after 72 h exposure, which may be due to the presence of iron oxide (Fe2O3), while the TTGS(600)-PDUDMA sample showed no obvious red rust up to 408 h exposure.
[0436] These observations suggest that galvanized steel sheets with a PDUDMA coating may be more corrosion resistant than uncoated galvanized steel sheets. Furthermore, the corrosion rate of galvanized steel increased with heat treatment temperature. Without wishing to be bound by any particular theory, the inventors believe that the heat treatment removed the passivation layer (zinc carbonate or basic zinc carbonate) and changed the surface morphology. The removal of the passivation layer and the change in surface morphology may facilitate the penetration of corrosive electrolytes into the zinc layer of the steel substrate.
[0437] After 672 hours of salt spray testing, the specimens were given their corresponding corrosion resistance rating numbers, which are listed in Table 36.
[0438] [Table 37]
[0439] The galvanized steel sheets with PDUDMA coating had a higher rust rating (R) than the corresponding uncoated galvanized steel sheets, suggesting that the galvanized steel sheets with PDUDMA coating may have a better corrosion inhibition performance than the uncoated steel samples.
[0440] Among the galvanized steel samples with PDUDMA coating, the TTGS(400)-PDUDMA sample had the least corrosion and the highest rust rating (R). The corrosion resistance of TTGS(400)-PDUDMA was higher than that of UTGS-PDUDMA, which may be due to the better protection of the coating, which the inventors believe may be due to the higher bond strength.
[0441] TTGS(400)-PDUDMA had higher corrosion resistance than TTGS(600)-PDUDMA, which may be due to the better corrosion resistance of the zinc layer.
[0442] The corrosion resistance of the TTGS(400)-PDUDMA sample may result from a combination of protection from the polymer coating and secondary protection from the zinc layer. The corrosion behavior of the notched specimens was also investigated. Table 37 shows the rust intensity of notched galvanized steel sheets with and without PDUDMA coating after exposure to a corrosion accelerating medium for different times up to 312 hours.
[0443] [Table 38]
[0444] Table 38 shows the rust degree (R) corresponding to the test piece and the rust degree (R) of the area where the notch was made. s ) are listed.
[0445] [Table 39]
[0446] As shown in Table 38, corrosion products did not begin to form on the UTGS and UTGS-PDUDMA samples until 216 hours of exposure. TTGS(400) and TTGS(400)-PDUDMA began to form corrosion products on the surface after 144 hours of exposure.
[0447] After 312 hours, more corrosion products and wider scratches were observed on TTGS(400) and TTGS(400)-PDUDMA compared to the untreated ones. Furthermore, the rust intensity of the TTGS(400)-PDUDMA specimen (R=1) was higher than that of the TTGS(400) specimen (R=0), indicating that the former had less corrosion products than the latter. The TTGS(600) surface was completely covered with corrosion products after 144 hours of exposure, indicating a more severe attack by corrosion.
[0448] The corrosion products of TTGS(600)-PDUDMA were less and the corresponding rust degree (R) was higher than that of TTGS(600), indicating that the corrosion resistance of TTGS(600)-PDUDMA was higher than that of TTGS(600). These observations were in good agreement with the unnotched specimens, and also demonstrated that the galvanized steel with PDUDMA coating exhibited higher corrosion inhibition performance compared to the uncoated specimen.
[0449] Among all the specimens with notched coating, the UTGS-PDUDMA specimen showed the least corrosion and the highest rust level (R). The TTGS-PDUDMA specimen showed more corrosion than the corresponding untreated specimen, which may be due to the faster corrosion of the zinc layer caused by the penetration of corrosive electrolyte through the linear scratches, which resulted in the degradation of the polymer coating. In summary, the salt spray test results of the unnotched and notched specimens showed that the galvanized steel with PDUDMA coating had better corrosion resistance than the specimen without PDUDMA coating. 5.3 Conclusion This example demonstrates the adhesion properties of the PDUDMA coating as well as the corrosion resistance of the PDUDMA coating on different galvanized steel substrate surfaces.
[0450] The adhesive strength of PDUDMA / galvanized steel and epoxy / galvanized steel was evaluated by pull-off adhesion testing. Failure occurred primarily within the polymer rather than at the polymer / zinc layer interface for the PDUDMA system, suggesting increased bond strength compared to that of the epoxy system. The higher peel strength values for the PDUDMA system compared to the epoxy system indicated higher bond strength.
[0451] These results indicated that the bond strength of PDUDMA / galvanized steel was higher than that of the epoxy system. The percentage of cohesive failure of the heat-treated galvanized steel-PDUDMA coated samples was higher than that of the UTGS coated system, which also suggested that the bond strength of the heat-treated galvanized steel-PDUDMA coated system may be higher compared to that of the untreated samples.
[0452] The adhesive strength of PDUDMA / galvanized steel was evaluated by tape adhesion test, and the results showed good adhesion between the PDUDMA coating and the substrate. The corrosion resistance of different galvanized steel specimens and galvanized steel specimens with corresponding PDUDMA coating was investigated by salt spray test. The appearance of galvanized steel specimens with and without notches with PDUDMA coating after salt spray test showed improved corrosion resistance compared to that of uncoated specimens. Furthermore, the corrosion rate of uncoated galvanized steel was found to increase with heat treatment temperature. The decrease in corrosion resistance of heat treated specimens may be due to the removal of passivation layer and change in surface morphology, which may facilitate the penetration of corrosive electrolytes into the zinc layer and steel substrate. 6. Example 5 - Polymerization of methyl methacrylate (MMA) initiated by heat-treated titanium (Ti) substrates This example demonstrates the ability of heat-treated titanium (TTTi) substrates to photoinitiate polymerization under UV irradiation. 6.1 Experiments Methyl methacrylate (MMA) (99%, Sigma-Aldrich, containing ≦30 ppm Mequinol (4-methoxyphenol (MEHQ) as an inhibitor) was purified by washing three times with 10 wt% NaOH, followed by washing with deionized water until the monomer was neutral, then drying overnight over Na2SO4, followed by distillation under reduced pressure. The purified monomer was stored refrigerated at 4 °C under a nitrogen atmosphere until use.
[0453] Titanium (Ti) substrates in the form of 0.5 mm thick sheets were cut into square slides with dimensions of 15 mm×15 mm, then ultrasonically cleaned in ethanol and distilled water. Heat treatment was carried out at 400° C. for 2 hours under ambient atmosphere to obtain heat-treated titanium substrates (TTTi).
[0454] In each experiment, methyl methacrylate (MMA) (9.4 g, 0.094 mol) and heat-treated titanium substrate (TTTi) (15 mm × 15 mm) were charged into a 20 mL vial, and the reaction mixture was irradiated with UV light (6 W or 15 W, λ = 350 nm) for 1 h. The vials were sealed and kept in a constant temperature (60 °C) oven for different times (0 to 48 h). The changes in chemical species during polymerization were monitored by Fourier transform infrared spectroscopy (FTIR). 6.2 Results and Discussion Since the mixture of methyl methacrylate (MMA) and heat-treated titanium substrate (TTTi) does not contain a catalyst that requires an inert atmosphere to maintain its activity, all polymerizations were carried out under ambient atmosphere to simplify the reaction setup.
[0455] Polymerization of methyl methacrylate (MMA) was first carried out at 60° C. without UV irradiation or with UV irradiation for 1 hour without the use of any initiator or additional materials. MMA monomer was also polymerized by using TTTi substrate as photoinitiator at 60° C. without UV irradiation. Table 39 lists the detailed reaction conditions and the observations of the resulting materials.
[0456] [Table 40]
[0457] As shown in Table 39, no polymerization occurred in the absence of UV irradiation and TTTi photoinitiator. In contrast, in the presence of TTTi, a clear solid polymer was formed in the reaction mixture containing MMA. The resulting polymer was characterized by ATR-FTIR. The spectrum of MMA monomer showed a peak at 1640 cm -1A characteristic absorption band was observed around 1640 cm, which was assigned to a carbon-carbon double bond (C=C). The polymer prepared with TTTi had an absorption peak at the same wavenumber (1640 cm). -1 ) was not observed. The disappearance of the carbon-carbon double bond peak confirmed that polymerization occurred using TTTi as a photoinitiator, and PMMA polymer was synthesized. 7. Example 6 - Polymerization of MMA initiated by different metal initiators 7.1 Experiments This example demonstrates the ability of different initiators to photoinitiate polymerization under UV irradiation. 7.1.1 Materials Methyl methacrylate (MMA) was purified and kept refrigerated at 4 °C under nitrogen atmosphere until use. ZnCO3, ZnO, basic zinc carbonate (Zn5(CO3)2(OH)6), and TiO2 powders were used as received. Al foil, zinc potassium sheet, and Cu sheet were cut into square slides with dimensions of 15 mm × 15 mm, and then ultrasonically cleaned with ethanol and distilled water. Heat treatment was carried out at 400 °C for 2 h under ambient atmosphere to obtain heat-treated metal substrates. 7.1.2 Homopolymerization Methyl methacrylate (MMA) (9.4 g, 0.094 mol) and heat-treated metal substrate (15 mm × 15 mm) / powder 0.5 wt% were placed in a 20 mL vial and the reaction mixture was irradiated with UV light (15 W, λ = 350 nm) for 1 h. The vial was sealed and kept in a constant temperature (60 °C) oven for 48 h. 7.2 Results and Discussion First, the polymerization of methyl methacrylate (MMA) was carried out without any initiator or additional materials at 60° C. without UV irradiation or with UV irradiation for 1 h. Also, MMA monomer was polymerized at 60° C. without UV irradiation using different photoinitiators.
[0458] Table 40 lists the detailed reaction conditions and observations of the resulting materials. The subsequent polymerization of MMA was carried out by UV irradiation for 1 h using TT zinc potassium, ZnO powder, and TiO2 powder as photoinitiators. The reaction mixture was then left in the dark at 60 °C for 48 h. A large amount of transparent solid polymer was produced, indicating that polymerization had occurred and PMMA polymer had been synthesized.
[0459] In no case did polymerization occur. On the other hand, when TT Al foil, ZnCO3, and Zn5(CO3)2(OH)6 were used as photoinitiators under the same conditions, no polymerization to obtain a solid phase occurred.
[0460] [Table 41]
[0461] 8. Example 7 - Polymerization of DUDMA by surface initiated polymerization on metal substrates 8.1 Experiments This example illustrates the preparation of PDUDMA coatings on different substrates by spin coating. 8.1.1 Materials Diurethane dimethacrylate (DUDMA) was used as received. All metal substrates (galvanized steel (GS), titanium (Ti), Al 5251 sheet (Al), anodized Al sheet (anodized Al), copper sheet (Cu)) were in sheet form and were cut into square slides with dimensions 100 mm x 100 mm and then washed with ethanol and distilled water. Heat treatment was carried out at 400 °C for 2 hours under ambient atmosphere to obtain heat treated substrates. 8.1.2 General Procedure for Preparing PDUDMA Coatings on Substrates by Spin Coating A spin coater (WS-400 Lite Series, Laurell Technologies, USA) was used for spin coating. The DUDMA monomer was placed on the metal substrate at room temperature. The substrate was then spun horizontally at speeds of 1000, 2000, and 3000 rpm for 2 min. The deposited samples were then irradiated with UV light (15 W, λ=350 nm) for 2 h, then held at constant temperatures (60 °C and 80 °C) for various times until a solid PD-UDMA coating was obtained, and then cooled to room temperature. 8.1.3 Characterization of PDUDMA Coatings The coating thickness was measured using a film thickness gauge (Elcometer Limited, UK, model No: Elcomete 355). Chemical changes during polymerization were monitored by ATR-FTIR.
[0462] The chemical structures of the DUDMA monomer and the PDUDMA coating were characterized by ATR-FTIR. 8.2 Results and Discussion The observed results of the coatings obtained by initiation with different metal initiators are shown in Table 41. Polymerization was carried out using heat treated galvanized steel, Ti, Al, anodized Al, and copper as photoinitiators to synthesize PDUDMA coatings.
[0463] The polymerization rate using TTGS and TTTi was faster (6 to 7 days) than using other metal substrates (approximately 12 days).
[0464] [Table 42]
[0465] From ATR-FTIR, 1725cm -1 and 1530cm -1 The characteristic absorption peaks associated with C=O stretching and NH stretching were observed at 1640 cm and 1650 cm, respectively. -1A characteristic peak appeared at 1640 cm, which was assigned to a carbon-carbon double bond (C=C). -1 ) was not seen in the spectrum of the PDUDMA coating. The disappearance of the carbon double bond peak confirmed that polymerization had occurred to give the PDUDMA polymer. 9. Example 8 - Molecular weight measurement of polymers by SEC-MALS 9.1 Experiments A 20 mL vial was charged with methyl methacrylate (MMA) (9.4 g, 0.094 mol) and the heat-treated substrate (15 mm x 15 mm), and the reaction mixture was irradiated with UV light (15 W, λ = 350 nm) for 1 h. The vial was sealed and kept in a constant temperature (60 °C) oven for different times (0-48 h). Polymerization of other monomers (MA / BMA / BA) was carried out following the same procedure. 9.1.1 Materials The acrylic monomers were purified and refrigerated at 4 °C under nitrogen atmosphere until use. Hot-dip galvanized steel samples with a zinc coating of approximately 20–25 μm in thickness were ultrasonically cleaned in deionized water. Heat treatment was carried out at 400 °C (TTGS(400)) and 600 °C (TTGS(600)) for 2 h under ambient atmosphere to prepare heat-treated galvanized steel. 9.1.2 Characterization of polymers by SEC-MALS The molecular weight and polydispersity index of the polymers were determined by size-exclusion chromatography (SEC) coupled with multi-angle light scattering (MALS). SEC was performed using THF as the eluent at 30 °C with a flow rate of 1.0 mL / min. Data acquisition and processing were performed using ASTRA 4 software (Wyatt Technologies Corporation). 9.2 Results and Discussion The molecular weight and polydispersity of the resulting PMMA / PMA / PBMA / PBA were measured by size exclusion chromatography coupled with multi-angle light scattering analysis (SEC-MALS). The polymer properties are listed in Table 42.
[0466] [Table 43]
[0467] The SEC chart of the obtained PMMA showed a unimodal distribution with high molecular weight (Mn=2,270k) and low polydispersity (PDI=1.12), indicating that TTGS(400) photoinitiator can produce high molecular weight and narrow molecular weight distribution in one initiation route. To investigate the efficiency of TTGS(400) to synthesize acrylic polymers with high molecular weight structure with low PDI, methyl acrylate (MA), butyl acrylate (BA), and butyl methacrylate (BMA) were also polymerized using TTGS(400) as initiator. The SEC results showed that all acrylic monomers produced high molecular weight polymers (Mn>1,993k) with low PDI (PDI<1.2). These results indicate that TTGS(400) is a highly efficient photoinitiator for synthesizing acrylic polymers with high molecular weight and narrow molecular weight distribution. 10. Example 9 - Measurement of PMMA polymer hardness The hardness of the PMMA polymer produced as described herein by the method of the present invention was measured using an Elcometer 3092 Sclerometer Hardness Tester (pencil hardness test). No deformation of the polymer coating was observed even when the maximum force (20N) was applied. Thus, the hardness of the PMMA polymer was greater than 20N. 11. Example 10 - Polymerization of DUDMA on Heat Treated Magnesium Substrates Polymerization of DUDMA on heat treated magnesium substrates was carried out as described herein in accordance with the method of the present invention, and a PDUDMA coating was observed after a curing time of 12 days. References [1] Linxiang, L. et al., "An HPLC assay of hydroxyl radicals by the hydroxylation reaction of terephthalic acid," Biomedical Chromatography, 2004, Vol. 18, No. 7, pp. 470-474. [2] Ishibashi, K.-i. et al., "Detection of active oxidative species in TiO2 photocatalysis using the fluorescence technique," Electrochemistry Communications, 2000, Vol. 2, No. 3, pp. 207-210. [3] Wagner, C. D., "Auger lines in X-ray photoelectron spectrometry," Analytical Chemistry, Vol. 44, No. 6, 1972, pp. 967-973. [4] Dollimore, D. et al., "Kinetic aspects of the thermal decomposition of zinc carbonate," Thermochimica Acta, 1980, Vol. 36, No. 3, pp. 343-349 [5] Hutera, B. et al., "Synthesis of ZnO nanoparticles by thermal decomposition of basic zinc carbonate," Archives of Metallurgy and Materials, 2013, Vol. 58, No. 2, pp. 489-491. [6] Kanari, N. et al., "Thermal decomposition of zinc carbonate hydroxide," Thermochimica Acta, 2004, Vol. 410, No. 1, pp. 93-100. [7] Moad, G. and D. H. Solomon, "The chemistry of radical polymerization", Elsevier, 2006. [8] Matyjaszewski, K. and T. P. Davis, Handbook of radical polymerization, John Wiley & Sons, 2003. [9] Buback, M. and A. M. van Herk, Radical Polymerization: Kinetics and Mechanism, John Wiley & Sons, 2007.
[10] Jagur-Grodzinski, J., Living and controlled polymerization: synthesis, characterization, and properties of the respective polymers and copolymers, Nova Publishers, 2006.
[11] Jagur-Grodzinski, J., Living and controlled polymerization: synthesis, characterization, and properties of the respective polymers and copolymers, Nova Publishers, 2006.
[12] Odian, G., "Principles of Polymerization," John Wiley & Sons, 2004.
[13] ASTM,D.,4541, "Standard Test Method for Pull-Off Strength of Coatings Using Portable Adhesion Testers", ASTM International, USA, 2009.
[14] ASTM,B.,117, "Standard Practice for Operating Salt Spray (Fog) Apparatus", ASTM International (1997 Edition), 2011.
[15] Paint, ACD-o., M. Related Coatings, and Applications, Standard Test Method for Evaluation of Painted or Coated Specimens Subjected to Corrosive Environments, 2008, ASTM International.
[16] D610-08,A, Standard Practice for Evaluating Degree of Rusting on Painted Steel Surfaces, ASTM international, 2008. The following numbered paragraphs define certain aspects of the embodiments of the invention described herein: 1. A method for producing a polymer, comprising: Providing one or more polymerizable monomers; providing a substrate comprising an activated metal surface, the activated metal surface comprising one or more compounds capable of initiating polymerization of one or more polymerizable monomers; contacting the activated metal surface with one or more polymerizable monomers to polymerize the one or more polymerizable monomers, thereby producing a polymer; The method includes: 2. The activated metal surface, when contacted with an aqueous solution of 30.096 μM terephthalic acid and 0.001 mol / L NaOH and irradiated with 365 nm light from a 15 W light source for 1 hour at room temperature, exhibited concentrations of 2-hydroxyterephthalic acid of at least 0.0001, 0.0002, 0.0003, 0.0004, 0.0005, 0.0006, 0.0007, 0.0008, 0.0009, 0.10, 0.20, 0.30, 0.40, 0.50, 0.60, 0.70, 0.80, 0.90, 1.00, 1.10, 1.20, 1.30, 1.40, 1.50, 1.60, 1.70, 1.80, 1.90, 1.80, 1.90, 1.90, 1.10, 1.20, 1.40, 1.50, 1.80, 1.90, 1.10, 1.20, 1.40, 1.50, 1.60, 1.80, 1.9 ... 0009, 0.001, 0.0015, 0.002, 0.0025, 0.003, 0.0035, 0.004, 0.0045, 0.005, 0.0055, 0.006, 0.0065, 0.007, 0.0075, 0.008, 0.0085, 0.009, 0.0095, 0.01, 0.0105, 0.011, 0.0115, 0.012, 0.0125, or 0.013 μM / mm of geometric area of activated surface 2 The method according to claim 1, wherein 3. The activated metal surface, when tested according to the procedure described in Example 1.7, is capable of absorbing at least 0.0001, 0.0002, 0.0003, 0.0004, 0.0005, 0.0006, 0.0007, 0.0008, 0.0009, 0.001, 0.0015, 0.002, 0.0025, 0.00 3, 0.0035, 0.004, 0.0045, 0.005, 0.0055, 0.006, 0.0065, 0.007, 0.0075, 0.008, 0.0085, 0.009, 0.0095, 0.01, 0.0105, 0.011, 0.0115, 0.012, 0.0125, or 0.013 μM / mm of geometric area of activated surface 2 3. The method according to claim 1 or 2, wherein the concentration of 4. The method according to any one of claims 1 to 3, wherein the activated surface is produced by treating a metal surface of a substrate comprising a metal surface; or the method further comprises: providing a substrate comprising a metal surface; and treating the substrate comprising a metal surface to produce an activated metal surface. 5. The method according to any one of claims 1 to 4, wherein the method is for producing a metal-polymer composite, and wherein one or more polymerizable monomers are polymerized onto and / or at the activated metal surface, thereby producing a metal polymer composite. 6. The method of any one of claims 1 to 5, wherein the polymer is attached directly to the metal surface of the substrate. 7. The method of any one of claims 1 to 6, wherein the polymer forms a coating on the surface of the substrate. 8. The method of any one of claims 1 to 7, wherein the activated metal surface comprises one or more metal oxides capable of generating hydroxyl radicals. 9. The method of claim 8, wherein the metal oxide is selected from the group consisting of magnesium oxide, lead oxide, zinc oxide, copper oxide, titanium dioxide, silver oxide, tin oxide, aluminum oxide, cadmium oxide, iron oxide, and nickel oxide, or any combination of two or more thereof. 10. The method according to claim 8 or 9, wherein the metal oxide is selected from the group consisting of lead oxide, zinc oxide, copper oxide, titanium dioxide, silver oxide, tin oxide, aluminum oxide, cadmium oxide, iron oxide, and nickel oxide, or a combination of two or more thereof. 11. The method according to any one of items 8 to 10, wherein the metal oxide is selected from the group consisting of zinc oxide, titanium oxide, and aluminum oxide, or a combination of two or more of these. 12. The method according to any one of claims 8 to 11, wherein the metal oxide is zinc oxide or titanium oxide or a combination thereof. 13. The method of any one of claims 8 to 11, wherein the metal oxide is zinc oxide. 14. The method according to claim 8 or 9, wherein the metal oxide is selected from the group consisting of magnesium oxide, copper oxide, zinc oxide, titanium oxide, and aluminum oxide, or a combination of two or more thereof. 15. The method of any one of claims 1 to 14, wherein the metal surface comprises one or more metals, the oxides of which are capable of generating hydroxyl radicals. 16. The method of any one of paragraphs 1 to 15, wherein the metal surface comprises magnesium, zinc, titanium, aluminum, lead, copper, titanium, silver, tin, cadmium, iron, or nickel, or a combination of any two or more thereof. 17. The method of any one of claims 1 to 16, wherein the metal surface comprises zinc, titanium, aluminum, lead, copper, titanium, silver, tin, cadmium, iron, or nickel, or a combination of any two or more thereof. 18. The method of any one of paragraphs 1 to 17, wherein the metal surface comprises zinc, titanium, or aluminum, or a combination of any two or more of these. 19. The method of any one of claims 1 to 18, wherein the metal surface comprises zinc or titanium or a combination thereof. 20. The method of any one of claims 1 to 19, wherein the metal surface comprises zinc. 21. The method of any one of paragraphs 1 to 20, wherein the metal surface comprises magnesium, copper, zinc, titanium, or aluminum, or a combination of two or more thereof. 22. The method according to any one of paragraphs 8 to 21, wherein the one or more metal oxides are produced by treating the metal surface; or the method comprises treating a metal surface to produce one or more metal oxides. 23. The method of any one of claims 1 to 22, wherein the method comprises contacting an activated metal surface and one or more polymerizable monomers and irradiating with light, preferably light comprising UV light. 24. The process according to any one of claims 1 to 23, wherein the polymerization is carried out in the absence of an external or exogenous initiator. 25. The method of any one of claims 1 to 24, wherein the substrate is a monolithic structure having at least one dimension greater than 100 nm, preferably greater than 1 mm. 26. The method of any one of clauses 1 to 25, wherein the metal surface and / or substrate comprises, consists of, or consists essentially of galvanized steel, electrogalvanized steel, Galfan steel, metallic zinc, metallic aluminum, metallic titanium, zinc-aluminum alloy coated steel, zinc-magnesium coated steel, or zinc-aluminum-magnesium coated steel, or a combination of two or more thereof. 27. The method of any one of claims 1 to 26, wherein the metal surface and / or substrate comprises, consists of or consists essentially of galvanized steel. 28. The method of any one of claims 1 to 27, wherein the metal surface and / or substrate comprises, consists of or consists essentially of hot-dip galvanized steel. 29. The method of any one of paragraphs 1 to 28, wherein the substrate is selected from the group consisting of particles, fibers, sheets, blocks, wires, mesh, panels, slabs, plates, poles, columns, bars, round bars, beams, foil, joists, laminates, fences, pipes, chains, fabrics, roofing materials, coatings, or any combination of two or more thereof. 30. The method of any one of clauses 4 to 29, wherein the treatment of the metal surface to produce an activated surface comprises one or more of: heating the metal surface at an elevated temperature (e.g. in an oven, with a laser or by other suitable method); passing an electric current through the metal surface (e.g. an anodization step); subjecting the metal surface to a chemical treatment (e.g. a treatment to produce hydroxyl groups on the metal surface, an alkaline treatment (e.g. an alkali metal hydroxide treatment) or an acid treatment), subjecting the metal surface to a plasma treatment (e.g. an oxygen plasma treatment) or exposing the metal surface to UV light. 31. The method of any one of claims 4 to 30, wherein treating the metal surface comprises heating the metal surface at an elevated temperature to produce an activated metal surface. 32. The method according to paragraph 31, wherein the metal surface is heated by a laser or other heat source capable of rapidly heating the metal surface, such as a plasma. 33. The method according to paragraph 31 or 32, wherein heating the metal surface comprises heating to a temperature of at least about 100°C to about 600°C, preferably at least about 300°C to about 600°C, more preferably at least about 300°C to about 400°C. 34. The method of claim 31 or 33, wherein heating the metal surface comprises heating for at least about 1, 2, 3, 4, 5, 6, 7, 8, 9, 10 hours or more, for example, from about 1 to about 10 hours, preferably at least about 1 hour, more preferably at least about 2 hours. 35. The method of any one of paragraphs 1 to 34, wherein the activated metal surface is contacted with one or more polymerizable monomers within less than about 72, 48, 24, 12, 6, 5, 4, 3, 2, or 1 hours after formation, preferably within less than about 72 hours, preferably within less than about 24 hours, more preferably within about 2 hours. 36. The method according to any one of claims 1 to 35, wherein the activated metal surface is cooled, preferably to a temperature below the boiling point at atmospheric pressure of the one or more polymerizable monomers, before being contacted with the one or more polymerizable monomers. 37. The method of any one of claims 1 to 36, wherein the activated surface is generated when the substrate is formed. 38. The method of any one of paragraphs 1 to 37, wherein the one or more polymerizable monomers are photoactive monomers. 39. The method according to any one of paragraphs 1 to 38, wherein the one or more polymerizable monomers are monoolefinically unsaturated monomers, preferably monoethylenically unsaturated monomers; or polyolefinically, preferably diolefinically unsaturated monomers, preferably polyethylenically unsaturated monomers; preferably diethylenically unsaturated monomers. 40. The method of any one of paragraphs 1 to 39, wherein the one or more polymerizable monomers are unsaturated, preferably olefinically unsaturated, preferably ethylenically unsaturated. 41. The method according to any one of paragraphs 1 to 40, wherein the one or more polymerizable monomers are selected from the group consisting of vinyl monomers, preferably acrylic acid esters or methacrylic acid esters. 42. The one or more polymerizable monomers are represented by formula I:
[0468] [ka]
[0469] (In the formula, R 1 is C(O)OR 3 , CO(O)R 4 , aryl, or NR 20 and; R 2 is H or C1-4 alkyl, preferably H or CH3; R 3 is C1-10 alkyl or (CH2CH2O) n CH3, preferably C1-4 alkyl; R 4 is C1-10 alkyl, preferably C1-4 alkyl; n is an integer selected from 1 to 20; R 20 42. The method according to any one of items 1 to 41, wherein is a monomer of H or an alkyl group, preferably H or C1-10 alkyl, preferably H. 43. The one or more polymerizable monomers are represented by formula II:
[0470] [ka]
[0471] (In the formula, X is independently O or NR 20 and; R 20 is H or an alkyl group, preferably H or a C1-10 alkyl group, preferably H; R 5 and R6 are each independently H or C1-5 alkyl, preferably H or CH3; 42. The method of any one of claims 1 to 41, wherein Y is a monomer of a linking group, which may include a linear chain having at least 2, 5, 10, 15, 20, 25, 30, 35, 40, 45, 50, 55, 60, 65, 70, 75, 80, 85, 90, 95, 100 or more atoms selected from C, N, O, and S. 44. The linking group is represented by the formula (CR 30 R 40 ) q or formula (CR 50 R 60 O) r (CR 70 R 80 ) group, where R 30 , R 40 , R 50 , R 60 , R 70 , and R 80 Item 44. The method according to item 43, wherein each of x, y, y and r is independently H or alkyl, preferably C1-10 alkyl, and q and r are each independently an integer of 1 to 40. 45.Y is (CH2) m , CH2CH2CH(CH3), (CH2CH2O) p (CH2CH2), and formula IIA:
[0472] [ka]
[0473] (In the formula, m and p each independently represent an integer of 1 to 40, preferably about 1 to about 10; R 7 , R 8 , R 9 , and R 10 are each independently selected from H and C1-5 alkyl). 46. The one or more polymerizable monomers are represented by formula III:
[0474] [ka]
[0475] (In the formula, R 11 and R 12 are each independently H or:
[0476] [ka]
[0477] and R 5 42. The method according to any one of claims 1 to 41, wherein said monomer is as defined in any one of claims 1 to 45. 47. The method of any one of paragraphs 1 to 41 or 43 to 45, wherein each X is O. 48. The method of any one of paragraphs 1-41, 43-45, or 47, wherein the one or more polymerizable monomers are monomers of formula II having a linking group of formula IIA. 49.R 5 and R 6 and are both methyl. 50.R 7 and R 9 are both methyl, and R 8 and R 10 are each independently selected from the group consisting of H and CH3, preferably R 8 and R 10 One of them is H and R 8 and R 10 The other is CH3, and preferably, R 7 and R 9 are both methyl, and R 8 and R 10 50. The method of any one of paragraphs 45 or 47-49, wherein is present as a 1:1 mixture of H and CH3. 51. The method of any one of paragraphs 1 to 45 or 47 to 50, wherein the one or more polymerizable monomers are selected from the group consisting of methyl acrylate, methyl methacrylate, butyl methacrylate, diurethane dimethacrylate, poly(ethylene glycol) methyl ether methacrylate, butyl acrylate, styrene, and vinyl acetate. 52. The method of any one of paragraphs 1 to 45, 43, 45, or 47 to 51, wherein the one or more polymerizable monomers are diurethane dimethacrylates having CAS number 72869-86-4. 53. The method of any one of claims 1 to 52, wherein the activated metal surface is contacted with one or more different types of polymerizable monomers. 54. The method of any one of claims 1 to 53, wherein the activated metal surface is contacted with one or more polymerizable monomers for a first period of time and then for a second period of time. 55. Contacting an activated metal surface and one or more polymerizable monomers and irradiating with light of a wavelength of about 10, 50, 100, 150, 200, 250, 300, 350, 400, 450, 500, 550, 600, 650, 700, 750, 800, 850, 900, 950, 1000, 1050, 1100, 1150, 1200, 1250 nm or greater, useful ranges can be selected from any of these values, for example, about 10 55. The method according to any one of items 1 to 54, wherein the wavelength is from 1 to 400 nm, 50 to 400 nm, 100 to 400 nm, 150 to 400 nm, 200 to 400 nm, 10 to 700 nm, 50 to 700 nm, 100 to 700 nm, 150 to 700 nm, 200 to 700 nm, 300 to 700 nm, 400 to 700 nm, 10 to 1000 nm, 50 to 1000 nm, 100 to 1000 nm, 150 to 1000 nm, 200 to 1000 nm, 300 to 1000 nm, 400 to 1000 nm, 500 to 1000 nm, 600 to 1000 nm, or 700 to 1000 nm. 56. The method according to any one of claims 1 to 55, comprising contacting the activated metal surface with one or more polymerizable monomers and irradiating the surface with light having a wavelength of about 10, 50, 100, 150, 200, 250, 300, 350, 400, 450, 500, 550, 600, 650, 700, 750, 800, 850, 900, 950, 1000, 1050, 1100, 1150, 1200, 1250 nm or greater, for example, light having a wavelength of about 10 nm to about 1000 nm, about 10 nm to about 700 nm, preferably about 10 nm to about 400 nm. 57. The method of any one of claims 23 to 56, wherein the light comprises, consists essentially of, or consists of light of a wavelength that optimizes the generation of hydroxyl radicals and / or electrons by one or more compounds capable of initiating polymerization at the activated surface. 58. The method of any one of claims 1-57, wherein the power of the light is at least about 1, 1.5, 2, 2.5, 3, 3.5, 4, 4.5, 5, 5.5, 6, 6.5, 7, 7.5, 8, 8.5, 9, 9.5, 10, 10.5, 11, 11.5, 12, 12.5, 13, 13.5, 14, 14.5, 15, 15.5, 16, 16.5, 17, 17.5, 18, 18.5, 19, 19.5, 20, 25, 30, 35, 40, 45, 50, 55, 60, 65, 70, 75, 80, 85, 90, 95, 100, 105, 110, 115, 120, 125, 130 W. 59. The intensity of the light is determined by the amount of light emitted from the activated surface (m 2 Item 29. The method of any one of items 23 to 58, wherein the Watts per second is at least 1, 2, 3, 4, 5, 6, 7, 8, 9, or 10 W per second. 60. The method according to any one of claims 1 to 59, wherein the activated metal surface is contacted with one or more polymerizable monomers for a first period of time and then for a second period of time characterized by different temperature and / or irradiation. 61. The method of any one of paragraphs 1 to 60, wherein the activated metal surface is contacted with one or more polymerizable monomers at a first temperature for a first period of time and at a second temperature for a second period of time, the first temperature being different from the second temperature, and preferably the first temperature being higher than the second temperature. 62. The method according to any one of claims 1 to 61, wherein the contacting of the activated metal surface with the one or more polymerizable monomers is carried out under irradiation with light for a first period only. 63. The method according to any one of paragraphs 1 to 62, wherein the activated metal surface is contacted with one or more polymerizable monomers for a first period of time at a temperature of at least about 10, 15, 20, 25, 30, 35, 40, 45, 50, 55, 60, 65, 70, 75, 80, or 85°C, a suitable range may be selected from any of these values, for example, from about 10°C to about 85°C, more preferably from 50 to 85°C, more preferably from 20 to 50°C. 64. The method of any one of paragraphs 1 to 63, wherein the activated metal surface is contacted with one or more polymerizable monomers for a second period of time at a temperature of at least about 10, 15, 20, 25, 30, 35, 40, 45, 50, 55, 60, 65, 70, 75, 80, or 85°C, a suitable range may be selected from any of these values, for example, from about 10°C to about 85°C, from about 50 to about 85°C, preferably at least about 20°C, preferably at least about 50°C, preferably at least 85°C. 65. The method of any one of paragraphs 54 to 64, wherein the first period of time is at least about 30 seconds, 1, 5, 10, 15, 30, or 60, 70, 80, 90, 100, 110, or 120 minutes, preferably from about 30 seconds to about 120 minutes, more preferably from about 30 seconds to about 60 minutes. 66. The method of any one of paragraphs 1 to 65, wherein the second period of time is less than about 72, 48, 36, 24, 12, 11, 10, 9, 8, 7, 6, 5, 4, 3, 2, or 1 hour, preferably less than about 5 hours, more preferably less than about 1 hour. 67. The number average molecular weight of the polymer is at least about 500,000, 550,000, 600,000, 650,000, 700,000, 750,000, 800,000, 850,000, 900,000, 950,000, 1,000,000, 1,050,000, 1,100,000, 1,150,000, 1,200,000 67. The method of any one of claims 1 to 66, wherein the molecular weight of the polymer is 1,250,000, 1,500,000, 2,000,000, 3,000,000, 4,000,000, or 5,000,000 g / mol, and a useful range can be selected from any of these values, for example, from about 500,000 to about 5,000,000 g / mol. 68. The number average molecular weight of the polymer is at least about 2,000, 10,000, 50,000, 100,000, 150,000, 200,000, 250,000, 300,000, 350,000, 400,000, 450,000, 500,000, 550,000, 600,000, 650,000, 700,000, 750,000, 800,000, 850,000, 900,000, 950,000, 1,000,000, 1,050,000, 1,100,000, 1,150,000, or 1,200,000 g / mol, and a useful range can be selected from any of these values, for example, from about 2,000 to about 1,200,000 g / mol. 69. The polydispersity index of the polymer is at least about 1, 1.05, 1.1, 1.15, 1.2, 1.25, 1.3, 1.35, 1.4, 1.45, 1.5, 1.55, 1.6, 1.65, 17, 1.75, 1.8, 1.85, 1.9, 1.95, 2, 2.05, 2.1, 2.15, 2.2, 2.25, 2.3, 2.35, 2.4, 2.45, 2.5, 2.55, 2.6, 2.65, 2.7, 2.75, 2.8, 2.95, 2.9, 2.95, 3, 3.05, 3.1, 3.15, 3.2, 3.25, 3.3, 3.35, 3.4, 3.5, 3.6, 3.7, 3.8, 3.9, 3.10, 3.11, 3.12, 3.13, 3.14, 3.15, 3.16, 3.17, 3.18, 3.19, 3.20, 3.21, 3.22, 3.23, 3.24, 3.25, 3.26, 3.27, 3.28, 3.29, 3.30, 3.31, 3.32, 3.33, 3.34, 3.35, 3.35, 3.36, 3.37, 3.38, 3.39, 3.40, 3.41, 3.42, 3. 69. The method of any one of claims 1 to 68, wherein the MnO2 content is 0.45, 3.5, 3.55, 3.6, 3.65, 3.7, 3.75, 3.8, 3.85, 3.9, 3.95, 4, 4.05, 4.1, 4.15, 4.2, 4.25, 4.3, 4.35, 4.4, 4.45, 4.5, 4.5, 4.55, 4.6, 4.65, 4.7, 4.75, 4.8, 4.85, 4.9, 4.95, or 5, and is preferably at least about 1.05 to about 2.5, preferably at least about 1.05 to about 1.5, and more preferably at least about 1.05 to about 1.2. 70. The method of any one of paragraphs 1 to 69, wherein the metal polymer composite has a tape adhesion rating of at least 2B, preferably 3B, preferably 4B as measured by AST D3359. 71. Metal-polymer composites have peel strengths as measured by ASTM D4541-09 of approximately 1.5, 1.6, 1.7, 1.8, 1.9, 2.0, 2.1, 2.2, 2.3, 2.4, 2.5, 2.6, 2.7, 2.8, 2.9, 3.0, 3.1, 3.2, 3.3, 3.4, 3.5, 3.6, 3.7, 3.8, 3.9, 4, 4.1, 4.2, 4.3, 4.4, 4.5, 4.6, 4.7, 4.8, 4.9, 5.0, 5.1, 5.2, 5.3, 5.4, 5.5, 5.6, 5.7, 5.8, 5.9 ...8, 5.9, 5.1, 5.2, 5.4, 5.5, 5.6, 5.9, 5.1, 5.3, 5.4, 5.5, 5.7, 5.8, 5.9, 5.1, 5.2, 5.3, 5.4, 5.5, 5.8, 5.9, 5.1, 5.2, 5.4, 5.5, 5.6, 5.8, 5.9, 5.1, 5.2, 5.4, 5.5, 5.8, 5.9, 5.1, 5.2, 71. The method according to any one of claims 1 to 70, wherein the pressure is greater than 9, 5, 5.5, 6, 6.5, 7, 7.5, 8, 8.5, 9, 9.5, or 10 MPa, and a useful range can be selected from any of these values, for example about 1.5 to 10, 2.5 to 10, 1.5 to 7.5, 2.5 to 7.5, 1.5 to 5, or 1.5 to 4 MPa, preferably about 2.5 to about 5 MPa. 72. The method of any one of paragraphs 1 to 71, wherein the metal-polymer composite has a peel strength of greater than about 1.5, 1.6, 1.7, 1.8, 1.9, 2.0, 2.1, 2.2, 2.3, 2.4, 2.5, 2.6, 2.7, 2.8, 2.9, 3.0, 3.1, 3.2, 3.3, 3.4, 3.5, 3.6, 3.7, 3.8, 3.9, 4, 4.1, 4.2, 4.3, 4.4, 4.5, 4.6, 4.7, 4.8, 4.9, 5 MPa, preferably from about 2.5 to about 5 MPa, as measured by ASTM D4541-09. 73. The method of any one of paragraphs 1 to 72, wherein the direct attachment comprises, consists of, or consists essentially of a non-covalent bond between the polymer and the metal surface. 74. The method of claim 73, wherein the non-covalent bond comprises, consists of, or consists essentially of a hydrogen bond. 75. The method of any one of claims 1 to 74, wherein the one or more polymerizable monomers are photochemically polymerized. 76. The method of any one of paragraphs 1 to 75, wherein the one or more polymerizable monomers are polymerized in the absence of electric current, applied voltage, or externally applied potential difference. 77. The method of any one of the preceding claims, wherein the one or more polymerizable monomers are polymerized in a liquid medium comprising less than 90, 85, 80, 75, 70, 65, 60, 55, 50, 45, 40, 35, 30, 25, 20, 15, 10, 5, 4, 3, 2, or 1 vol.% of solvent, preferably less than 90 vol.%, preferably less than 50 vol.%, preferably less than 10 vol.% of solvent, preferably the one or more polymerizable monomers are polymerized in the absence of solvent. 78. The method of any one of paragraphs 1 to 77, wherein the one or more polymerizable monomers are polymerized in air and / or in the presence of air or other oxygen-containing atmosphere. 79. A method according to any one of claims 4 to 78, wherein the metal surface is subjected to one or more pretreatment steps, such as one or more physical, mechanical and / or chemical treatments, such as plasma treatment or surface roughening, such as surface roughening by etching and / or patterning, prior to carrying out said treatment to produce said activated metal surface. 80. The method according to paragraph 79, wherein the metal surface is subjected to a pretreatment step, such as a surface roughening step, which increases the surface area of the metal surface. 81. A method according to any one of paragraphs 79 or 80, wherein the metal surface is subjected to a pretreatment step, e.g. a plasma, laser, chemical or other pretreatment step, which increases the wettability and / or free energy of the surface and / or modifies the morphology of the surface in order to enhance bonding (e.g. mechanical bonding) between the polymer and the surface. 82. The method of any one of claims 1 to 81, wherein the polymer is removed from the surface of the substrate. 83. The method of any one of paragraphs 1 to 82, wherein contacting the activated surface with the monomer occurs within less than about 30, 15, 10, 5, 1, or 0.5 minutes, or within less than about 10, 5, or 1 seconds, after the activated surface is generated. 84. The method of any one of paragraphs 1 to 83, wherein the activated metal surface is an anodized surface or comprises an anodized surface, for example an anodized surface including titanium, aluminum, and magnesium. 85. A method according to any one of claims 4 to 84, wherein the substrate having a metal surface is a substrate having a zinc-plated surface. 86. A polymer prepared by the method of any one of paragraphs 1 to 85. 87. The polymer according to paragraph 86, wherein the polymer is a block copolymer. 88. A metal-polymer composite prepared by the method of any one of paragraphs 1 to 85. 89. A metal-polymer composite according to paragraph 88, wherein the polymer of the metal-polymer composite is a block copolymer. 90. A polymer produced by polymerizing the monomer according to any one of items 1 to 85. 91. A metal-polymer composite comprising a polymer directly attached to the metal surface of a substrate. 92. A metal-polymer composite having a peel strength of about 1.5 to about 5 MPa, preferably about 2.5 to about 5 MPa. 93. A polymer or metal-polymer complex according to any one of paragraphs 85 to 92, wherein the number average molecular weight of the polymer is in the range of at least about 2,000 to 1,200,000 g / mol. 94. A polymer or metal-polymer complex according to any one of items 85 to 93, wherein the polydispersity index of the polymer is at least about 1 to about 5, preferably at least about 1.05 to about 2.5, preferably at least about 1.05 to about 1.5, more preferably at least about 1.05 to about 1.2. 95. The metal-polymer complex of any one of paragraphs 88, 89, or 91-94, wherein the direct attachment comprises, consists of, or consists essentially of a non-covalent bond. 96. The metal-polymer complex according to paragraph 95, wherein the non-covalent bond comprises, consists of, or consists essentially of hydrogen bonds. 97. The metal-polymer composite of any one of paragraphs 88, 89, or 91-96, wherein the substrate is a monolithic structure, the monolithic structure having at least one dimension greater than 100 nanometers. 98. The metal-polymer composite of any one of claims 88, 89, or 91-97, wherein the metal surface and / or substrate comprises, consists of, or consists essentially of galvanized steel, electrogalvanized steel, Galfan steel, metallic zinc, metallic aluminum, metallic titanium, zinc-aluminum alloy coated steel, zinc-magnesium coated steel, or zinc-aluminum-magnesium coated steel, or a combination of two or more thereof. 99. The metal-polymer composite of any one of paragraphs 88, 89, or 91-98, wherein the metal surface and / or substrate comprises, consists of, or consists essentially of galvanized steel. 100. The metal-polymer composite of any one of paragraphs 88, 89, or 91-99, wherein the metal surface and / or substrate comprises, consists of, or consists essentially of hot-dip galvanized steel. 101. The metal-polymer composite of any one of paragraphs 88, 89, or 91-100, wherein the substrate is selected from the group consisting of particles, fibers, sheets, blocks, wires, mesh, panels, slabs, plates, poles, columns, rods, round bars, beams, foil, joists, laminates, barrier fences, pipes, chains, fabrics, roofing materials, coatings, or any combination of two or more thereof. 102. A polymer or metal-polymer composite according to any one of claims 1 to 101, wherein the polymer is a block copolymer.
Claims
1. 1. A method for producing a polymer comprising: Providing one or more radical initiated polymerizable monomers; providing a substrate comprising a metal surface that has been activated by one or more of treating the metal surface with an elevated temperature, passing an electric current through the metal surface, subjecting the metal surface to a chemical treatment, subjecting the metal surface to a plasma treatment, or exposing the metal surface to light, wherein the activated metal surface comprises one or more metal compounds capable of initiating polymerization of the one or more radically initiated polymerizable monomers; contacting the activated metal surface with one or more radically initiated polymerizable monomers to polymerize the one or more radically initiated polymerizable monomers, thereby producing the polymer in the absence of an exogenous initiator.
2. The activated metal surface, when contacted with an aqueous solution of 30.096 μM terephthalic acid and 0.001 mol / L NaOH and irradiated with 365 nm light from a 15 W light source for 1 hour at room temperature, exhibits a concentration of 2-hydroxyterephthalic acid of at least 0.0001, 0.0002, 0.0003, 0.0004, 0.0005, 0.0006, 0.0007, 0.0008, 0.0009, 0.100, 0.200, 0.300, 0.400, 0.500, 0.600, 0.700, 0.800, 0.900, 1.000, 1.100, 1.200, 1.300, 1.400, 1.500, 1.600, 1.700, 1.800, 1.9 ... 0009, 0.001, 0.0015, 0.002, 0.0025, 0.003, 0.0035, 0.004, 0.0045, 0.005, 0.0055, 0.006, 0.0065, 0.007, 0.0075, 0.008, 0.0085, 0.009, 0.0095, 0.01, 0.0105, 0.011, 0.0115, 0.012, 0.0125, or 0.013 μM / mm of geometric area of activated surface 2 The method of claim 1, wherein the
3. 3. The method of claim 1 or 2, wherein the method is for producing a metal-polymer composite, and the one or more radical initiated polymerizable monomers are at least one of polymerized toward and at the activated metal surface, thereby producing the metal polymer composite.
4. The method of any one of claims 1 to 3, wherein the polymer is attached directly to the metal surface of the substrate.
5. The method according to any one of claims 1 to 4, wherein the activated metal surface contains one or more metal oxides capable of generating hydroxyl radicals.
6. 6. The method of any one of claims 1 to 5, wherein the metal surface comprises magnesium, zinc, titanium, aluminum, lead, copper, titanium, silver, tin, cadmium, iron, or nickel, or a combination of any two or more thereof.
7. 7. The method according to any one of claims 1 to 6, comprising the step of contacting the activated metal surface and one or more radically initiated polymerizable monomers and irradiating with light, preferably light comprising UV light.
8. 8. The method of any one of claims 1 to 7, wherein treating the metal surface at an elevated temperature comprises heating the metal surface at an elevated temperature to produce the activated metal surface.
9. 9. The method of claim 8, wherein heating the metal surface comprises heating to a temperature of at least about 100°C to about 600°C, preferably at least about 300°C to about 600°C, and more preferably at least about 300°C to about 400°C.
10. 10. The method of any one of claims 1 to 9, wherein the activated metal surface is contacted with the one or more radical initiated polymerizable monomers within less than about 72, 48, 24, 12, 6, 5, 4, 3, 2, or 1 hours after formation, preferably within less than about 72 hours, preferably within less than about 24 hours, more preferably within about 2 hours.
11. 11. The method according to any one of claims 1 to 10, wherein the one or more radically initiated polymerizable monomers are monoolefinically unsaturated monomers, preferably monoethylenically unsaturated monomers; or polyolefinically, preferably diolefinically unsaturated monomers, preferably polyethylenically unsaturated monomers; preferably diethylenically unsaturated monomers.
12. The method includes contacting the activated metal surface and one or more radical initiated polymerizable monomers and irradiating with light having a wavelength of about 10, 50, 100, 150, 200, 250, 300, 350, 400, 450, 500, 550, 600, 650, 700, 750, 800, 850, 900, 950, 1000, 1050, 1100, 1150, 1200, 1250 nm or greater, and useful ranges can be selected from any of these values, e.g.
12. The method of claim 1, wherein the diameter of the nanoparticles is about 10-400, 50-400, 100-400, 150-400, 200-400, 10-700, 50-700, 100-700, 150-700, 200-700, 300-700, 400-700, 10-1000, 50-1000, 100-1000, 150-1000, 200-1000, 300-1000, 400-1000, 500-1000, 600-1000, or 700-1000 nm.
13. 13. The method of any one of claims 1 to 12, wherein the light comprises, consists essentially of, or consists of at least one of light at a wavelength that optimizes the generation of hydroxyl radicals and electrons by the one or more compounds capable of initiating polymerization at the activated surface.
14. The intensity of the light is determined by the irradiated metal surface (m 2 14. The method of any one of claims 1 to 13, wherein the power consumption is at least 1, 2, 3, 4, 5, 6, 7, 8, 9, or 10 W per 100 W.
15. 15. The method according to any one of claims 1 to 14, wherein the activated metal surface is contacted with the one or more radically initiated polymerizable monomers for a first period of time and then for a second period of time characterized by different at least one of temperature and irradiation.
16. The number average molecular weight of the polymer may be at least about 500,000, 550,000, 600,000, 650,000, 700,000, 750,000, 800,000, 850,000, 900,000, 950,000, 1,000,000, 1,050,000, 1,100,000, 1,150,000, 1,200,000, , 250,000, 1,500,000, 2,000,000, 3,000,000, 4,000,000, or 5,000,000 g / mol, and useful ranges can be selected from any of these values, for example, from about 500,000 to about 5,000,000 g / mol.
17. The polydispersity index of the polymer is at least about 1, 1.05, 1.1, 1.15, 1.2, 1.25, 1.3, 1.35, 1.4, 1.45, 1.5, 1.55, 1.6, 1.65, 1.7, 1.75, 1.8, 1.85, 1.9, 1.95, 2, 2.05, 2.1, 2.15, 2.2, 2.25, 2.3, 2.35, 2.4, 2.45, 2.5, 2.55, 2.6, 2.65, 2.7, 2.75, 2.8, 2.85, 2.9, 2.95, 3, 3.05, 3.1, 3.15, 3.2, 3.25, 3.3, 3.35, 3.4 , 3.45, 3.5, 3.55, 3.6, 3.65, 3.7, 3.75, 3.8, 3.85, 3.9, 3.95, 4, 4.05, 4.1, 4.15, 4.2, 4.25, 4.3, 4.35, 4.4, 4.45, 4.5, 4.55, 4.6, 4.65, 4.7, 4.75, 4.8, 4.85, 4.9, 4.95, or 5, preferably at least about 1.05 to about 2.5, preferably at least about 1.05 to about 1.5, more preferably at least about 1.05 to about 1.
2.
18. The method of claim 4, wherein the direct attachment of the polymer to the metal surface comprises, consists of, or consists essentially of a non-covalent bond between the polymer and the metal surface.
19. 19. The method of any one of claims 1 to 18, wherein the one or more radically initiated polymerizable monomers are polymerized in a liquid medium comprising less than 90, 85, 80, 75, 70, 65, 60, 55, 50, 45, 40, 35, 30, 25, 20, 15, 10, 5, 4, 3, 2, or 1 vol.% of solvent, preferably less than 90 vol.%, preferably less than 50 vol.%, preferably less than 10 vol.% of solvent, preferably the one or more radically initiated polymerizable monomers are polymerized in the absence of solvent.
20. The method according to any one of the preceding claims, wherein the metal surface is subjected to one or more pretreatment steps.
21. The method of any one of claims 1 to 20, wherein the polymer is removed from the surface of the substrate.
22. A polymer prepared by the method of any one of claims 1 to 21.
Citation Information
Patent Citations
Surface-modified metal and method for modifying metal surface
JP2017042415A