Pearl colored scale-like particles, inks, and coatings
Optimizing the thickness of zinc sulfide and magnesium fluoride layers in a three-layer structure addresses the issues of pearl pigments in inkjet printing, achieving superior pearl coloring and smooth appearance.
Patent Information
- Application Number
- JP2021167844
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2021-10-13
- Publication Date
- 2024-09-18
- Estimated Expiration
- 2041-10-13
AI Technical Summary
Existing pearl pigments, such as ZnS/MgF2 three-layer flakes, are not suitable for inkjet printing due to poor ejection stability and lack of optimization in layer thickness, leading to issues with pearl coloring and graininess.
Optimizing the thickness of each layer in a three-layer structure of a first zinc sulfide layer, a magnesium fluoride layer, and a second zinc sulfide layer, with specific thickness ranges and a cumulative 50% volume particle diameter of 1.8 μm or less, to enhance pearl coloring and suitability for inkjet printing.
The optimized three-layer structure provides excellent pearl coloring and seamless, moist appearance in inkjet-printed applications, overcoming the limitations of conventional flakes.
Smart Images

Figure 0007551985000022 
Figure 0007551985000027 
Figure 0007551985000030
Abstract
Description
[Technical field]
[0001] The present invention relates to pearlescent colored scaly particles, ink, and coating film. [Background technology]
[0002] Conventionally, various light interference pearl pigments have been used in the fields of paints, plastics, printing inks, cosmetics, etc. Known examples of the pearl pigments include those in which the surface of a scaly powder base material is coated with titanium oxide, iron oxide, etc.
[0003] In addition, Patent Document 1 describes ZnS / MgF 2 It is disclosed that optically variable flakes having a three-layer structure of ZnS / MgF exhibit pearl coloring (see paragraph
[0010] , Table 1). 2 It is disclosed in Patent Document 1 that the total average thickness of the three layers of ZnS / MgF is 0.5 μm (500 nm) or less, and the average particle size of the flakes is within the range of 2 μm to 20 μm (see paragraph
[0037] ). 2 It is disclosed that the deposition method and the sputtering method can be used as a method for forming the three-layer structure of ZnS / ZnS (see paragraph
[0024] ). [Prior art documents] [Patent documents]
[0004] [Patent Document 1] Japanese Patent Application Publication No. 8-58224 Summary of the Invention [Problem to be solved by the invention]
[0005] However, the ZnS / MgF 2Flakes with a three-layer structure of ZnS / MgF are mainly used for anti-counterfeit cards, and the ink is applied by bar coat printing, screen printing, etc. (see paragraph
[0037] ), but is not used for inkjet printing. When inkjet printing is performed using ink containing flakes with an average particle size of 2 μm to 20 μm as in Patent Document 1, the ejection stability may be extremely poor due to the size of the nozzle diameter of the inkjet printer head and the influence of dispersion stability. Furthermore, the ZnS / MgF in Patent Document 1 2 It is stated that the flakes consisting of three layers of ZnS / ZnS have a total average thickness of the three layers of 0.5 μm (500 nm) or less, but there is no description of the average thickness of each of the three layers, and no attempt has been made to optimize the thickness of each of the three layers to suit pearl coloring.
[0006] The present invention aims to solve the above-mentioned problems in the prior art and to achieve the following objectives: That is, the present invention aims to provide pearlescent coloring scaly particles, ink, and coating film that can realize excellent pearlescent coloring by optimizing the thickness of each layer in a three-layer structure having a first zinc sulfide layer, a magnesium fluoride layer, and a second zinc sulfide layer in this order. [Means for solving the problem]
[0007] The means for solving the above problems are as follows. <1> A first zinc sulfide layer, a magnesium fluoride layer, and a second zinc sulfide layer in this order; The first zinc sulfide layer has an average thickness of 30 nm or more, The magnesium fluoride layer has an average thickness of 25 nm or more, The second zinc sulfide layer has an average thickness of 30 nm or more; The pearlescent colored scaly particles are characterized in that the total average thickness of the three layers, the first zinc sulfide layer, the magnesium fluoride layer, and the second zinc sulfide layer, is 330 nm or less. <2> The first zinc sulfide layer has an average thickness of 30 nm or more and 130 nm or less, The average thickness of the magnesium fluoride layer is 25 nm or more and 60 nm or less, The average thickness of the second zinc sulfide layer is 30 nm or more and 190 nm or less. <1> The pearl-colored scale-like particles are as described in 1. <3> Cumulative 50% volume particle size D 50 is 1.8 μm or less. <1> from <2> The pearlescent colored scale-like particles according to any one of claims 1 to 5, <4> The ink jet printing method according to the present invention <1> from <3> The pearlescent colored scale-like particles according to any one of claims 1 to 5, <5> The above <1> from <4> 1. An ink comprising the pearlescent colored scaly particles according to any one of claims 1 to 9. <6> The above <1> from <4> 2. A coating film comprising the pearl-colored scale-like particles according to claim 1. Effect of the Invention
[0008] According to the present invention, the above-mentioned problems in the prior art can be solved and the above-mentioned object can be achieved, and by optimizing the thickness of each layer in a three-layer structure having a first zinc sulfide layer, a magnesium fluoride layer, and a second zinc sulfide layer in this order, it is possible to provide pearlescent coloring flake particles, ink, and coating film that can realize excellent pearlescent coloring. [Brief description of the drawings]
[0009] [Figure 1] FIG. 1 is a schematic diagram showing an example of the pearlescent colored scale-like particle of the present invention. [Diagram 2] FIG. 2 is a front view of the coating film of configuration 1. [Diagram 3] FIG. 3 is a perspective view of the coating film of configuration 1. [Figure 4] FIG. 4 is a front view of the coating film of configuration 2. [Diagram 5] FIG. 5 is a front view of the coating film of configuration 3. [Figure 6] FIG. 6 is a front view of the coating film of configuration 4. [Figure 7]FIG. 7 is a diagram showing a method for measuring the absolute reflectance in the 5° specular reflection direction and the absolute reflectance in the 45° specular reflection direction for the evaporated films of Configurations 1 to 4. [Figure 8] FIG. 8 is a graph showing the results of simulation and actual measurement of the 5° regular reflectance of the evaporated film of configuration 1. [Figure 9] FIG. 9 is a graph showing the results of simulation and actual measurement of the 5° regular reflectance of the evaporated film of configuration 2. [Figure 10] FIG. 10 is a graph showing the results of simulation and actual measurement of the 5° regular reflectance of the evaporated film of configuration 3. [Figure 11] FIG. 11 is a graph showing the results of simulation and actual measurement of the 5° regular reflectance of the evaporated film of configuration 4. [Figure 12] FIG. 12 is a graph showing the results of simulation and actual measurement of the 45° regular reflectance of the evaporated film of configuration 1. [Figure 13] FIG. 13 is a graph showing the results of simulation and actual measurement of the 45° regular reflectance of the evaporated film of configuration 2. [Figure 14] FIG. 14 is a graph showing the results of simulation and actual measurement of the 45° regular reflectance of the evaporated film of configuration 3. [Figure 15] FIG. 15 is a graph showing the results of simulation and actual measurement of the 45° regular reflectance of the evaporated film of configuration 4. [Figure 16] FIG. 16 is a graph showing the results of a simulation of the 5° regular reflectance of Example 1, Example A, Example D, Example E, Comparative Example F, Comparative Example G, Comparative Example H, and Comparative Example I. [Figure 17] FIG. 17 is a graph showing the results of a simulation of the 5° specular reflectance of Comparative Example A, Comparative Example B, Comparative Example C, Comparative Example D, and Comparative Example E. [Figure 18] FIG. 18 is a graph showing the relationship between the total average thickness of the first to third layers and the cumulative 50% volume particle size D50 after fine pulverization. [Figure 19] FIG. 19 is a schematic diagram showing a method for taking a photograph of the appearance of a coating film. [Figure 20]FIG. 20 shows photographs of the appearance of the coating films of Configurations 1 to 4, the coating films of Configurations 5 to 8, and a coating film of a competitor's product. [Figure 21] FIG. 21 shows cross-sectional SEM images of scaly particles obtained by pulverizing the vapor-deposited films of Configurations 1 to 4, scaly particles obtained by pulverizing the vapor-deposited films of Configurations 5 to 8, and a competitor's powder. [Figure 22] FIG. 22 is an enlarged cross-sectional SEM photograph of scaly particles obtained by pulverizing the vapor-deposited film of Configuration 2. [Figure 23] FIG. 23 is an enlarged cross-sectional SEM photograph of scaly particles obtained by pulverizing the vapor-deposited film of Configuration 7. [Figure 24] FIG. 24 is an enlarged cross-sectional SEM photograph of the powder of a competitor's product (SXB). [Diagram 25] FIG. 25 shows SEM photographs of the particle shapes of the finely pulverized scaly particles of Configurations 1 to 4, the finely pulverized scaly particles of Configurations 5 to 8, and a competitor's product. [Figure 26] FIG. 26 is a graph showing the particle size distribution of the finely pulverized scaly particles of Configurations 1 to 4. [Figure 27] FIG. 27 is a diagram showing the particle size distribution of the finely pulverized scaly particles of Compositions 5 to 8 and particles of a competitor's product. [Figure 28] FIG. 28 is a diagram showing the 5° specular reflection spectrum of each coating film of Configurations 1 to 4. [Figure 29] FIG. 29 is a diagram showing the 45° specular reflection spectrum of each coating film of Configurations 1 to 4. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] (Pearl-colored scale-like particles) The pearlescent colored scaly particles of the present invention have a first zinc sulfide layer, a magnesium fluoride layer, and a second zinc sulfide layer in this order, the first zinc sulfide layer having an average thickness of 30 nm or more, the magnesium fluoride layer having an average thickness of 25 nm or more, the second zinc sulfide layer having an average thickness of 30 nm or more, and the total average thickness of the three layers, the first zinc sulfide layer, the magnesium fluoride layer, and the second zinc sulfide layer, being 330 nm or less.
[0011] Conventionally, pearl pigments have been produced by, for example, coating the surface of mica or glass flakes with a metal oxide (TiO 2 etc.) coated flakes or TiO 2 / SiO 2 / TiO 2 Examples include scale-like particles having a three-layer structure (high refractive index layer / low refractive index layer / high refractive index layer). The surface of the mica or glass flakes is treated with a metal oxide (TiO 2 Flakes coated with metal oxides (TiO etc.) have a large thickness, and it is difficult to make them fine enough for inkjet printing, resulting in a noticeable graininess. 2 The flakes coated with ZnS / MgF 2 However, there is a problem that the seamless feeling and moist feeling that can be obtained by finely grinding the evaporated film of the three-layer structure of ZnS and ZnS flake particles cannot be achieved.
[0012] The present invention relates to ZnS / MgF 2 The three-layered TiO / ZnS scale-like particles are 2 / SiO 2 / TiO 2 This is because the crystal structure of the deposited film obtained by deposition is similar to that of TiO 2 / SiO 2 / TiO 2 Since ZnS / MgF has an amorphous structure, its refractive index is lower than that of the bulk. 2 Since / ZnS has a crystalline structure, the refractive index is close to the literature value, resulting in a large refractive index difference, high reflectance, and good pearl coloring.
[0013] Therefore, according to the present invention, a first zinc sulfide (ZnS) layer and a magnesium fluoride (MgF 2 ) layer and a second zinc sulfide (ZnS) layer in this order, and by optimizing the average thickness of each of the three layers, it is possible to realize scale-like particles that exhibit good pearl coloring within the visible light wavelength range.
[0014] As shown in FIG. 1, the pearlescent colored scaly particle 10 of the present invention has a three-layer structure in which a first zinc sulfide layer 1, a magnesium fluoride layer 2, and a second zinc sulfide layer 3 are laminated in this order. The average thickness of each layer is designed to obtain good pearlescent coloring, and the cumulative 50% volume particle diameter D is suitable for inkjet printing. 50 It is finely ground into
[0015] <First zinc sulfide layer and second zinc sulfide layer> The content of zinc sulfide (ZnS) in the first and second zinc sulfide layers is preferably 98 mass % or more, more preferably 99 mass % or more, and even more preferably 99.9 mass % or more. The zinc sulfide content in the first and second zinc sulfide layers can be measured by, for example, X-ray fluorescence analysis (XRF).
[0016] The average thickness of the first zinc sulfide layer is 30 nm or more, preferably 30 nm or more and 130 nm or less, and more preferably 30 nm or more and 120 nm or less. The average thickness of the second zinc sulfide layer is 30 nm or more, preferably 30 nm or more and 190 nm or less, and more preferably 30 nm or more and 170 nm or less.
[0017] The average thickness of the first and second zinc sulfide layers, for example, when produced by a physical vapor phase method, is the same as the average deposition thickness obtained by measuring the thickness at 5 to 10 points on the first and second zinc sulfide layers and averaging them. Examples of methods for measuring the average thickness of the first and second zinc sulfide layers include scanning electron microscope (SEM) observation, X-ray fluorescence analysis (XRF), and ultraviolet-visible spectroscopy. When the average thickness is determined by the scanning electron microscope (SEM) observation, a cross-section of a vapor-deposited film or a scaly particle containing the first and second zinc sulfides is observed using the scanning electron microscope (SEM), the thicknesses of the first and second zinc sulfide layers are measured at 5 to 10 locations, and the average vapor deposition thickness is taken as the average thickness. When the average thickness is determined by the X-ray fluorescence analysis (XRF), the thicknesses of the first and second zinc sulfide layers are measured at 5 to 10 locations by quantitative analysis, and the average value can be used as the average thickness.
[0018] <Magnesium fluoride layer> Magnesium fluoride (MgF 2 The content of ) is preferably 98% by mass or more, more preferably 99% by mass or more, and even more preferably 99.9% by mass or more. The content of magnesium fluoride in the magnesium fluoride layer can be measured, for example, by X-ray fluorescence analysis (XRF). The average thickness of the magnesium fluoride layer is 25 nm or more, preferably 25 nm or more and 60 nm or less, and more preferably 35 nm or more and 50 nm or less.
[0019] The total average thickness of the three layers, ie, the first zinc sulfide layer, the magnesium fluoride layer, and the second zinc sulfide layer, is 330 nm or less, and preferably 130 nm or more and 290 nm or less.
[0020] <Other layers> The other layers include, for example, a release layer for releasing the laminate consisting of the first and second zinc sulfide layers and the magnesium fluoride layer from the substrate by dissolving.
[0021] The pearlescent coloring particles of the present invention having the magnesium fluoride layer between the first zinc sulfide layer and the second zinc sulfide layer are scaly particles, and may also be called thin plate-like particles, flat particles, flake-like particles, etc. In the present invention, the scale-like particles refer to particles having a substantially flat surface and a substantially uniform thickness in the direction perpendicular to the substantially flat surface. The shape of the approximately flat surface is not particularly limited and can be appropriately selected depending on the purpose. Examples of the shape include polygonal shapes such as approximately circular, approximately elliptical, approximately triangular, approximately rectangular, approximately pentagonal, approximately hexagonal, approximately heptagonal, and approximately octagonal, and random, indefinite shapes.
[0022] The cumulative 50% volume particle diameter D of the pearl-colored scale-like particles 50 is preferably 1.8 μm or less, more preferably 0.8 μm or more and 1.8 μm or less, further preferably 0.7 μm or more and 1.7 μm or less, and particularly preferably 0.5 μm or more and 1.6 μm or less. The cumulative 50% volume particle diameter D 50 is the particle size equivalent to 50% of the cumulative volume distribution of the particle size distribution curve obtained by the laser diffraction method, and is the average length of the long and short axes of the non-spherical scale-like particles when the non-spherical scale-like particles are measured assuming that they are perfect spheres. However, the actual scale-like particles are not spherical, but have a scale shape with long and short sides. Therefore, the above D 50 is a value different from the actual length in the long side direction (long diameter) and the actual length in the short side direction (short diameter) of the scale-like particle. An example of the means using the laser diffraction method is a laser diffraction / scattering type particle size distribution measuring instrument.
[0023] The ratio of the scale-like particles (cumulative 50% volume particle diameter D 50 The average thickness (nm) of the three layers is preferably 5 or more, and more preferably 10 or more. In addition, in the present invention, "D 50 The ratio of "(nm) / total average thickness of three layers (nm)" is the D measured using a laser diffraction method. 50 is a ratio calculated by dividing the average thickness obtained by scanning electron microscope (SEM) observation or fluorescent X-ray analysis. 50 The ratio of "(nm) / average thickness (nm)" is different from the parameter generally called the aspect ratio.
[0024] <Method of manufacturing pearl-colored scale-like particles> The method for producing pearlescent colored scaly particles of the present invention includes forming a release layer on a substrate, forming a first zinc sulfide layer on the release layer by a vapor phase method, forming a magnesium fluoride layer on the first zinc sulfide layer by a vapor phase method, forming a second zinc sulfide layer on the magnesium fluoride layer by a vapor phase method to obtain a laminate, peeling the laminate from the substrate, and pulverizing the laminate. This allows for efficient production of pearlescent colored scaly particles 10 as shown in FIG. 1.
[0025] The method for producing pearlescent colored scaly particles of the present invention specifically includes a peeling layer forming step, a first zinc sulfide layer forming step, a magnesium fluoride layer forming step, a second zinc sulfide layer forming step, a peeling step, and a pulverizing step, and may further include other steps as necessary.
[0026] <Release layer formation process> The release layer forming step is a step of providing the release layer on the substrate.
[0027] -Base material- The substrate is not particularly limited as long as it has a smooth surface, and various substrates can be used. Among these, a resin film, a metal, or a composite film of a metal and a resin film having flexibility, heat resistance, solvent resistance, and dimensional stability can be appropriately used. Examples of the resin film include a polyester film, a polyethylene film, a polypropylene film, a polystyrene film, and a polyimide film. Examples of the metal include copper foil, aluminum foil, nickel foil, iron foil, and alloy foil. The composite film of the metal and the resin film may be a film obtained by laminating the resin film and the metal.
[0028] -Release layer- The peeling layer can be made of various organic substances that can be dissolved in the subsequent peeling step, or solvents such as water, etc. In addition, by appropriately selecting an organic material constituting the peeling layer, the organic substances attached to or remaining on the magnesium fluoride layer or the first and second zinc sulfide layers can be made to function as a protective layer for the scale-like particles, which is preferable. The protective layer has a function of suppressing aggregation, oxidation, elution into a solvent, etc. of the scale-like particles. In particular, by utilizing the organic material used in the release layer as the protective layer, it is preferable since it becomes unnecessary to provide a separate surface treatment step. Examples of the organic material constituting the release layer that can be used as the protective layer include cellulose acetate butyrate (CAB), other cellulose derivatives, polyvinyl alcohol, polyvinyl butyral, polyethylene glycol, polyacrylic acid, polyacrylamide, acrylic acid copolymers, modified nylon resins, etc. These may be used alone or in combination of two or more. Among these, cellulose acetate butyrate (CAB) is preferred from the viewpoint of high functionality as the protective layer.
[0029] The method for forming the release layer is not particularly limited and can be appropriately selected depending on the purpose, and examples thereof include an inkjet method, a blade coating method, a gravure coating method, a gravure offset coating method, a bar coating method, a roll coating method, a knife coating method, an air knife coating method, a comma coating method, a U comma coating method, an AKKU coating method, a smoothing coating method, a microgravure coating method, a reverse roll coating method, a four-roll coating method, a five-roll coating method, a dip coating method, a curtain coating method, a slide coating method, a die coating method, etc. These methods may be used alone or in combination of two or more.
[0030] <First zinc sulfide layer forming process> The first zinc sulfide layer forming step is a step of forming a first zinc sulfide layer on the release layer by a vapor phase method.
[0031] The vapor phase method includes a deposition method and a sputtering method, which are generally called physical vapor deposition (PVD).
[0032] <Magnesium fluoride layer forming process> The magnesium fluoride layer forming step is a step of forming a magnesium fluoride layer on the first zinc sulfide layer by a vapor phase method.
[0033] The vapor phase method includes a deposition method and a sputtering method, which are generally called physical vapor deposition (PVD).
[0034] <Second zinc sulfide layer forming process> The second zinc sulfide layer forming step is a step of forming a second zinc sulfide layer on the magnesium fluoride layer by a vapor phase method. As a result of the above, a laminate is formed in which the first zinc sulfide layer, the magnesium fluoride layer, and the second zinc sulfide layer are laminated in this order on the release layer of the substrate.
[0035] The vapor phase method includes a deposition method and a sputtering method, which are generally called physical vapor deposition (PVD).
[0036] <Peeling process> The peeling step is a step of peeling off the laminate by dissolving the release layer. The solvent capable of dissolving the release layer is not particularly limited as long as it is capable of dissolving the release layer, and may be appropriately selected depending on the purpose.
[0037] The solvent capable of dissolving the release layer is not particularly limited and can be appropriately selected depending on the purpose. For example, alcohols such as methanol, ethanol, propanol, isopropanol, butanol, octanol, dodecanol, ethylene glycol, and propylene glycol; ethers such as tetrahydrone; ketones such as acetone, methyl ethyl ketone, and acetylacetone; esters such as methyl acetate, ethyl acetate, butyl acetate, and phenyl acetate; ethyl cellosolve, butyl cellosolve, ethyl carbitol, butyl carbitol, ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, ethylene glycol monoisopropyl ether, ethylene glycol monobutyl ether, ethylene glycol monohexyl ether, ethylene glycol monophenyl ether, diethylene glycol monomethyl ether, diethylene glycol monoethyl ether, diethylene glycol monobutyl ether, diethylene glycol dimethyl ether, diethylene glycol diethyl ether, triethylene glycol Examples of the alkoxysilane include glycol ethers such as glycol monomethyl ether, triethylene glycol monoethyl ether, triethylene glycol monobutyl ether, propylene glycol monomethyl ether, propylene glycol monoethyl ether, dipropylene glycol monomethyl ether, dipropylene glycol monoethyl ether, and diethylene glycol monomethyl ether acetate; phenols such as phenol and cresol; aliphatic or aromatic hydrocarbons such as pentane, hexane, heptane, octane, dodecane, tridecane, tetradecane, pentadecane, hexadecane, octadecane, octadecene, benzene, toluene, xylene, trimesine, nitrobenzene, aniline, and methoxybenzene; aliphatic or aromatic chlorinated hydrocarbons such as dichloromethane, chloroform, trichloroethane, chlorobenzene, and dichlorobenzene; sulfur-containing compounds such as dimethyl sulfoxide; nitrogen-containing compounds such as dimethylformamide, dimethylacetamide, acetonitrile, propionitrile, and benzonitrile; and water. These may be used alone or in combination of two or more.
[0038] <Crushing process> The pulverization step is a step of pulverizing the laminate peeled off from the substrate in the peeling step. By carrying out this pulverization step, the pearlescent colored scale-like particles of the present invention can be obtained.
[0039] The method used in the pulverization step is not particularly limited and can be appropriately selected depending on the purpose. Examples of the method include a jet mill, a ball mill, a bead mill, a vibration mill, and an ultrasonic homogenizer. Furthermore, if necessary, various treatments may be carried out to recover the pearlescent colored scaly particles or adjust their physical properties. For example, the particle size of the pearlescent colored scaly particles may be adjusted by classification, the scaly particles may be recovered by centrifugation, suction filtration, or the solid content concentration of the dispersion may be adjusted. In addition, solvent replacement may be carried out, and viscosity adjustment may be carried out using additives.
[0040] <Other processes> Examples of the other steps include a step of extracting the pulverized pearl colored scale-like particles as a dispersion liquid, and a step of recovering the scale-like particles from the dispersion liquid.
[0041] <Dispersion> The dispersion used in the present invention contains the pearlescent colored scaly particles of the present invention, and preferably contains an organic solvent and water, and further contains other components as required. The dispersion may be either aqueous or solvent-based, but is preferably aqueous from the standpoint of environmental friendliness.
[0042] The content of the pearlescent colored scale-like particles is preferably 0.1% by mass or more and 50% by mass or less based on the total amount of the dispersion liquid.
[0043] -Organic solvents- The organic solvent is not particularly limited and can be appropriately selected depending on the purpose, and examples thereof include polyhydric alcohols, polyhydric alcohol alkyl ethers, polyhydric alcohol aryl ethers, nitrogen-containing heterocyclic compounds, amides, amines, sulfur-containing compounds, etc. These may be used alone or in combination of two or more.
[0044] Examples of the polyhydric alcohols include ethylene glycol, diethylene glycol, 1,2-propanediol, 1,3-propanediol, 1,2-butanediol, 1,3-butanediol, 1,4-butanediol, 2,3-butanediol, 3-methyl-1,3-butanediol, triethylene glycol, polyethylene glycol, polypropylene glycol, 1,2-pentanediol, 1,3-pentanediol, 1,4-pentanediol, and 1,5-pentanediol. Examples of suitable hexanediols include 2,4-pentanediol, 1,5-pentanediol, 1,2-hexanediol, 1,6-hexanediol, 1,3-hexanediol, 2,5-hexanediol, 1,5-hexanediol, glycerin, 1,2,6-hexanetriol, 2-ethyl-1,3-hexanediol, ethyl-1,2,4-butanetriol, 1,2,3-butanetriol, and 2,2,4-trimethyl-1,3-pentanediol.
[0045] Examples of the polyhydric alcohol alkyl ethers include ethylene glycol monoethyl ether, ethylene glycol monobutyl ether, diethylene glycol monomethyl ether, diethylene glycol monoethyl ether, diethylene glycol monobutyl ether, tetraethylene glycol monomethyl ether, and propylene glycol monoethyl ether.
[0046] Examples of the polyhydric alcohol aryl ethers include ethylene glycol monophenyl ether and ethylene glycol monobenzyl ether.
[0047] Examples of the nitrogen-containing heterocyclic compound include 2-pyrrolidone, N-methyl-2-pyrrolidone, N-hydroxyethyl-2-pyrrolidone, 1,3-dimethyl-2-imidazolidinone, ε-caprolactam, and γ-butyrolactone.
[0048] Examples of the amides include formamide, N-methylformamide, N,N-dimethylformamide, 3-methoxy-N,N-dimethylpropionamide, and 3-butoxy-N,N-dimethylpropionamide.
[0049] Examples of the amines include monoethanolamine, diethanolamine, and triethylamine. Examples of the sulfur-containing compound include dimethyl sulfoxide, sulfolane, and thiodiethanol.
[0050] -Other ingredients- The other components are not particularly limited and can be appropriately selected depending on the purpose. Examples of the other components include water, polymers, crosslinking agents, antioxidants, fillers, polymerization inhibitors, surface conditioners, antistatic agents, antifoaming agents, viscosity modifiers, light resistance stabilizers, weather resistance stabilizers, heat resistance stabilizers, antioxidants, leveling agents, antiseptics / fungal agents, rust inhibitors, and pH adjusters.
[0051] -water- As the water, for example, pure water such as ion-exchanged water, ultrafiltered water, reverse osmosis water, distilled water, or ultrapure water can be used.
[0052] (ink) The ink of the present invention contains the pearlescent colored scaly particles of the present invention, and preferably contains a binder, and further contains other components as required. The ink of the present invention may be either water-based or solvent-based.
[0053] -Pearl-colored scale-like particles- The content of the pearlescent colored scaly particles relative to the total amount of the ink is not particularly limited, and can be appropriately selected depending on the purpose. The ink of the present invention may contain other luster pigments other than the pearlescent colored scaly particles, as necessary. Examples of the other luster pigments include metallic pigments (e.g., aluminum pigments), pigments obtained from natural mica (e.g., pearl pigments), and glass flake pigments.
[0054] -binder- The binder is not particularly limited and can be appropriately selected depending on the purpose. Examples of the binder include polyurethane resin, polyester resin, acrylic resin, vinyl acetate resin, styrene resin, butadiene resin, styrene-butadiene resin, vinyl chloride resin, acrylic-styrene resin, acrylic-silicone resin, polyvinyl alcohol resin, polyether resin, alkyd resin, polyvinylpyrrolidone, and cellulose. When the ink contains the binder, an ink having excellent fixability and dispersibility can be obtained. The content of the binder is not particularly limited and can be appropriately selected depending on the purpose.
[0055] The organic solvent and water in the ink may be the same as those in the dispersion.
[0056] -Other ingredients- The other components are not particularly limited and may be appropriately selected depending on the purpose. Examples of the other components include surfactants, antifoaming agents, antiseptic and antifungal agents, rust inhibitors, and pH adjusters.
[0057] The ink of the present invention can be used for coating methods such as, for example, the inkjet method, gravure coating method, screen printing method, spray coating method, spin coating method, blade coating method, gravure offset coating method, bar coating method, roll coating method, knife coating method, air knife coating method, comma coating method, U comma coating method, AKKU coating method, smoothing coating method, microgravure coating method, reverse roll coating method, four-roll coating method, five-roll coating method, dip coating method, curtain coating method, slide coating method, die coating method, etc. Among these, the inkjet method, bar coating method, spray coating method, gravure coating method, and screen printing method are preferred.
[0058] (Paint film) The coating film of the present invention contains the pearlescent colored scaly particles of the present invention, and preferably contains a binder, and further contains other components as required. The coating film may be used alone, but may also be a coated product formed on a substrate by the above-mentioned coating method using the ink of the present invention. The substrate is not particularly limited and can be appropriately selected depending on the purpose. Examples of the substrate include plain paper, glossy paper, special paper, cloth, film, OHP sheet, general-purpose printing paper, automobile window glass and film, building window glass and film, agricultural film, and the like.
[0059] <Application> The pearlescent colored scaly particles of the present invention can realize excellent pearlescent coloring and can be used in a wide variety of fields, such as paints, plastics, printing, food, cosmetics, and automobiles. EXAMPLES
[0060] Examples of the present invention will be described below, but the present invention is not limited to these examples.
[0061] (Experimental Example 1) <Simulation of ZnS / MgF 2 / Optimization of the average thickness of each layer in the 3-layer structure of ZnS> ZnS / MgF with compositions 1 to 4 that produce good pearl coloring 2 The optimum average thickness of each layer in the ZnS / ZnS three-layer structure was found by simulation. The results are shown in Table 1. The reflectance was calculated by simulating the optical thin film design software (TFV ver.3, manufactured by Nally Software) as a simulator. The color tone was evaluated based on the obtained reflectance spectrum using the CIE Lab color system.
[0062] [Table 1]
[0063] (Experimental Example 2) <Preparation of pearl-colored scale-like particles> (1) As described above, a simulation of a deposition film with a three-layer structure was performed, and the lower limit of the average thickness of each layer of configurations 1 to 4 was determined. As described later, it has been confirmed that the optical characteristics (reflection spectrum) of the simulation and the actually manufactured sample are almost identical. Therefore, there is no problem in optimally designing the average thickness of each layer by simulation.
[0064] (2) ZnS / MgF determined by simulation 2 Using the average thickness of each layer of the three-layer structure of ZnS / ZnS, compositions 1 to 4 of the evaporated film having a three-layer structure were actually produced. Specifically, a solution containing 5% by mass of cellulose acetate butyrate (CAB) was applied at a rate of 0.06 g / m2 onto a polyethylene terephthalate (PET) film having an average thickness of 25 μm by gravure coating. 2 ±0.01g / m 2 The coating was dried at 110° C. or more and 120° C. or less to form a release layer. Next, zinc sulfide was deposited on the release layer by vacuum deposition to form a first zinc sulfide layer having an average thickness of 40 nm. The average thickness of the first zinc sulfide layer was determined by measuring the thickness of the first zinc sulfide layer at five locations by quantitative analysis using X-ray fluorescence analysis (XRF) and averaging the measured values. Next, magnesium fluoride was deposited on the first zinc sulfide layer by vacuum deposition to form a magnesium fluoride layer having an average thickness of 50 nm. Next, a second zinc sulfide layer having an average thickness of 40 nm was formed on the magnesium fluoride layer by the same method as for the first zinc sulfide layer. As a result, a vapor-deposited film having a configuration 1 was obtained in which a release layer, a first zinc sulfide layer, a magnesium fluoride layer, and a second zinc sulfide layer were laminated in this order on a PET film. The deposition films of configurations 2 to 4 were also prepared in the same manner as above.
[0065] (3) Each deposition film is pulverized (pulverized as finely as possible) for inkjet printing, and the cumulative 50% volume particle diameter D 50 The pearlescent colored scale-like particles of Configurations 1 to 4 were obtained. Specifically, butyl acetate was sprayed onto the PET film surface on which the vapor-deposited film was formed to dissolve the release layer, and the vapor-deposited film was scraped off with a doctor blade. Next, the mixture of the vapor-deposited film and butyl acetate was subjected to a fine pulverization process to adjust the particle size, and the target cumulative 50% volume particle size D 50 was ground to a particle size of 1.8 μm or less.
[0066] (4) The above pearlescent coloring scale-like particles were dispersed in butyl acetate to prepare pearlescent coloring inks of compositions 1 to 4. (5) The pearl coloring inks of compositions 1 to 4 were applied onto a polyethylene terephthalate (PET) film (transparent) using a bar coater. (6) Black tape was attached to half of the surface of the PET film opposite the ink-coated surface, and the coating films of Configurations 1 to 4 were visually observed and various data were measured.
[0067] Here, Fig. 2 is a front view of the coating film of configuration 1. Fig. 3 is an oblique view of the coating film of configuration 1. As shown in Figs. 2 and 3, when the viewing angle is changed from the front to an oblique direction, it is recognized that the peak wavelength of the reflected light of the pearl color shifts and the color changes. FIG. 4 is a front view of the coating film of Configuration 2, and the left side shows a coating film coated with a bar coater using pearlescent ink in which the solid content of the pearlescent colored scaly particles is high. FIG. 5 is a front view of the coating film of Configuration 3, and the left side shows a coating film coated with a bar coater using pearl coloring ink in which the solid content concentration of the pearl coloring scaly particles is high. FIG. 6 is a front view of the coating film of Configuration 4, and the left side shows a coating film coated with a bar coater using pearl coloring ink in which the solid content concentration of the pearl coloring scaly particles is high.
[0068] (Experimental Example 3) <Comparison between simulation and actual measurement (evaporated film)> -simulation- As a simulator, optical thin film design software (TFV ver.3, manufactured by Nally Software) was used to obtain simulated values of reflectance. The reflectance is the absolute reflectance in the 5° regular reflection direction when light is incident at an angle of 5° from the normal direction of each film. The absolute reflectance is calculated using the following formula. Absolute reflectance = (amount of light reflected by the sample / amount of light used) x 100 Absolute reflectance is the reflectance when the reflectance of air is taken as 100%.
[0069] -Actual measurement (evaporated film)- When the reflectance was actually measured, the reflectance of a sample in which a black tape 12 was provided on the back of a vapor-deposited film 11 as shown in FIG. 7 was measured. The reflectance was measured using an ultraviolet-visible-near infrared spectrophotometer (SolidSpec-3700, manufactured by Shimadzu Corporation). As shown in Fig. 7, the absolute reflectance in the 5° specular reflection direction when light was incident at an angle tilted by 5° from the normal direction of each of the evaporated films of the above configurations 1 to 4, and the absolute reflectance in the 45° specular reflection direction when light was incident at an angle tilted by 45° from the normal direction of each of the evaporated films of the above configurations 1 to 4 were measured. The results are shown in Figs. 8 to 15. From the results of Figs. 8 to 15, it was found that the simulation and actual measurements (evaporated film) were almost in agreement in the reflection spectrum in visible light wavelengths, and the average thickness of each layer could be optimally designed by simulation.
[0070] (Examples 1 to 4, Examples A to D, and Comparative Examples A to I) <Setting the lower limit of the average thickness of each of the three layers through simulation (evaporated film)> For Examples 1, A, D, E, F, G, H, and I in which the average thicknesses of the three layers were changed as shown in Table 2, the visual color was evaluated, and the results of a simulation of the 5° regular reflectance are shown in Table 2 and FIG. 16. For Comparative Examples A, B, C, D, and E in which the average thickness of each of the three layers was changed as shown in Table 2, the visual color was evaluated, and the results of a simulation of the 5° regular reflectance are shown in Table 2 and FIG. 17.
[0071] -Visual color- The visual color was evaluated using the reflectance spectrum obtained from a simulation and the CIE Lab color system, and was judged according to the following criteria. [Evaluation Criteria] OK: Visual color is good NG: Poor visual color
[0072] [Table 2]
[0073] Next, the results of a simulation of 5° regular reflection for Example 1 (Configuration 1), Example A (lower limit of Configuration 1), Example E, and Comparative Examples A to I are shown in Tables 3-1 to 3-3. The lower limit of the average thickness of each of the three layers in the blue region must satisfy both (1) and (2) below. (1) The value of (maximum reflectance in the wavelength range of 380 nm to 530 nm) / (minimum reflectance in the wavelength range of 420 nm to 630 nm) is 3.0 or more. (2) In the reflectance spectrum ranging from 380 nm to 780 nm, the minimum reflectance is in the range from 420 nm to 630 nm. By simultaneously satisfying the above (1) and (2), the color is easily recognized as blue by the naked eye.
[0074] [Table 3-1]
[0075] [Table 3-2]
[0076] [Table 3-3]
[0077] From the results in Tables 3-1 to 3-3, it was found that between Comparative Example I and Example E there was a boundary for the lower limit of the average thickness of each of the three layers.
[0078] (Experimental Example 4) <Setting the upper limit of the average thickness of the three layers> The cumulative 50% volume particle size D that can be used for inkjet printing by pulverizing each deposition film 50 The upper limit of the total average thickness of the three layers was set so as to fall within the range. The results are shown in FIG. The average thickness of each layer was calculated by measuring the thickness of each layer at five locations by quantitative analysis using X-ray fluorescence spectrometry (XRF) and averaging the measured values.
[0079] [Table 4]
[0080] [Table 5]
[0081] From the results of FIG. 18 and Tables 4 and 5, it was found that the upper limit of the total average thickness of the three layers was 330 nm or less. The total average thickness of the three layers and the cumulative 50% volume particle size after fine grinding D 50 The relationship between is thought to be independent of the material of each layer. The thicker the total average thickness of the three layers, the less fine the particles will be even after pulverization. In the range indicated by A in FIG. 18, head clogging occurred when printing was performed with an inkjet printer.
[0082] (Experimental Example 5) <Appearance of coating film> ZnS / MgF 2 Structures 1 to 4 are coatings using three layers of finely ground scaly particles of TiO 2 / SiO 2 / TiO 2 Compositions 5 to 8, which are coatings using three layers of finely ground scaly particles, and a product from a different company (Nihon Koken Kogyo Co., Ltd., natural mica with TiO 2 As shown in Fig. 19, external photographs of the coating films of the embedded samples (SXB, YXB) were taken with an iPhone (registered trademark) (manufactured by Apple Inc.) at a light source of D65 and an angle perpendicular to the photograph. The results are shown in Fig. 20. Note that the left half of each photograph in Fig. 20 corresponds to the left half in Fig. 19, and the right half of each photograph in Fig. 20 corresponds to the right half in Fig. 19. From the results in Figure 20, it can be seen that the TiO 2 The embedded products (SXB, YXB) are large flake powders, not finely ground particles, and therefore have a grainy (rough) texture visible in the coating film, which is undesirable. In contrast, the coating films made by the bar coating method in configurations 1 to 8 have a moist visibility.
[0083] (Experimental Example 6) <SEM observation of powder cross section> ZnS / MgF 2 / ZnS three-layer deposition film, 2 / SiO 2 / TiO 2 Configurations 5 to 8, which are three-layered evaporated films of TiO on natural mica, and a product from another company (Nihon Koken Kogyo Co., Ltd.) 2 The cross sections of the powders (embedded specimens, SXB, and YXB) were observed using a scanning electron microscope (SEM) HITACHI S-4700 (manufactured by Hitachi, Ltd.). The results are shown in FIG. An enlarged cross-sectional SEM photograph of scaly particles obtained by pulverizing the vapor-deposited film of Configuration 2 is shown in Figure 22. An enlarged cross-sectional SEM photograph of scaly particles obtained by pulverizing the vapor-deposited film of Configuration 7 is shown in Figure 23. An enlarged cross-sectional SEM photograph of the powder of a competitor's product (SXB) is shown in Figure 24. From the results in Figs. 21 to 24, ZnS / MgF 2 / ZnS and TiO 2 / SiO 2 / TiO 2 It can be seen from the cross section that it has a three-layer structure, and that the three-layer vapor deposition film was pulverized into powder. In contrast, the competitor's product has no cross section, and it can be seen that the entire powder surface is uniformly coated. Figure 24 shows an enlarged SEM image of a competitor's powder. 2 This photo was taken where a part of the mica had peeled off, revealing the mica inside. Competitor products use large-grain mica as a post-processing coating on the entire surface, so the mica basically becomes large in size (it is not crushed after coating). And ZnS / MgF 2 / ZnS and TiO 2 / SiO 2 / TiO 2 It can be seen that the powders of Configurations 1 to 8 obtained by pulverizing the evaporated films of the three layers have a smaller particle size when the total thickness of the three layers is smaller.
[0084] (Experimental Example 7) <SEM observation of powder shape> ZnS / MgF2 Compositions 1-4 are finely ground scaly particles of three layers of TiO 2 / SiO 2 / TiO 2 Compositions 5 to 8, which are three-layer finely ground scaly particles, and a competitor's product (Nihon Koken Kogyo Co., Ltd., natural mica with TiO 2 The powder shape of the flakes (embedded sample, SXB, and YXB) was observed using a scanning electron microscope (SEM) HITACHI S-4700 (manufactured by Hitachi, Ltd.). The results are shown in FIG. From the results in Figure 25, ZnS / MgF 2 In the three-layer structure of ZnS / ZnS, even though the first and second zinc sulfide layers have different thicknesses, no curling due to film stress is observed, and it is clear that the shape is flaky.
[0085] (Experimental Example 8) <Measurement of particle size distribution> ZnS / MgF 2 Compositions 1-4 are finely ground scaly particles of three layers of TiO 2 / SiO 2 / TiO 2 Compositions 5 to 8, which are three-layer finely ground scaly particles, and a competitor's product (Nihon Koken Kogyo Co., Ltd., natural mica with TiO 2 The particle size distribution of the flakes (embedded sample, SXB, and YXB) was measured using a laser diffraction / scattering particle size distribution analyzer (LSM-2000e, manufactured by Seishin Enterprise Co., Ltd.), and the cumulative 10% volume particle diameter D 10 , cumulative 50% volume particle diameter D 50 , and cumulative 90% volume particle diameter D 90 The results are shown in Figures 26 and 27. From the results of Figures 26 and 27, the finely ground scaly particles consisting of a three-layer structure of ZnS / MgF2 / ZnS have a cumulative 50% volume particle diameter D 50 It can be seen that the particle size is 1.8 μm or less.
[0086] (Experimental Example 9) <Optical data of coating film> 0.40 g of the finely pulverized scaly particles of compositions 1 to 4, 0.04 g of binder (S-LEC B, manufactured by Sekisui Chemical Co., Ltd.), and 3.64 g of butyl acetate were mixed using a mixer (rotation-revolution type mixer ARE-310, manufactured by Thinky Corporation) to prepare inks of compositions 1 to 4. Next, each ink was applied to a polyethylene terephthalate (PET) film with an average thickness of 100 μm using an applicator so that the average thickness was 5 μm or less. After natural drying at room temperature, the film was dried at 120°C for 3 minutes using a dryer to produce each coating film of Compositions 1 to 4.
[0087] [Table 6]
[0088] Next, the coating films of the obtained compositions 1 to 4 were measured using an ultraviolet-visible-near infrared spectrophotometer (SolidSpec-3700, manufactured by Shimadzu Corporation) under the following measurement conditions at absolute reflectance of 5° and 45°. * a * b * , Y, x, and y were measured. The results are shown in Table 7. [Measurement conditions] Lighting: D65 Field of view: 2 degrees In addition, the 5° specular reflection spectra of the coating films of Configurations 1 to 4, measured using an ultraviolet-visible-near-infrared spectrophotometer (SolidSpec-3700, manufactured by Shimadzu Corporation), are shown in Figure 28, and the 45° specular reflection spectra of the coating films of Configurations 1 to 4 are shown in Figure 29.
[0089] [Table 7]
[0090] From the results in Table 7, Figure 28, and Figure 29, when the absolute reflectance was measured by irradiating light at angles inclined at 5° and 45° with respect to the normal direction of each coating film, it was found that the reflected wavelength and absorbed wavelength were different at 5° and 45°, and that the wavelength at 45° was shifted to the shorter wavelength side. [Explanation of symbols]
[0091] 1 First zinc sulfide layer 2. Magnesium fluoride layer 3 Second zinc sulfide layer 10 Pearl colored scale-like particles
Claims
1. The coating film has a three-layer structure including a first zinc sulfide layer, a magnesium fluoride layer, and a second zinc sulfide layer in this order, The first zinc sulfide layer has an average thickness of 30 nm or more and 130 nm or more; The magnesium fluoride layer has an average thickness of 25 nm or more and 60 nm or less, The average thickness of the second zinc sulfide layer is 30 nm or more and 190 nm or less, The cumulative 50% volume particle size D 50 is 1.8 μm or less; the first zinc sulfide layer, the magnesium fluoride layer, and the second zinc sulfide layer are all vapor-deposited films; A pearlescent colored scaly particle, characterized in that the total average thickness of the three layers, namely, the first zinc sulfide layer, the magnesium fluoride layer and the second zinc sulfide layer, is 330 nm or less.
2. 2. The pearlescent colored scaly particles according to claim 1, which are for inkjet printing.
3. 3. An ink comprising the pearlescent colored scaly particles according to claim 1.
4. A coating film comprising the pearlescent colored scale-like particles according to claim 1 or 2.
Citation Information
Patent Citations
Preparation of pigment flake
JP1990173162A
Data carrier member
JP1996058224A
Multilayered film-coated powder
JP1998001701A
Multilayered film-coated powder and method for producing the same
JP2001271006A
All-dielectric light-diffractive pigment
JP2005528503A